Expanded thermoplastic polyurethane for special molding process

The use of a thermoplastic elastomer and thermoplastic polymer composition with specific dielectric properties, fused using an electromagnetic field, addresses the inefficiencies of traditional molding methods by enhancing mechanical properties and energy distribution, resulting in improved thermoplastic polyurethane bead foams.

WO2024200654A1PCT designated stage expired Publication Date: 2024-10-03BASF SE

Patent Information

Application Number
PCT/EP2024/058487
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-28
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Current methods for molding expanded thermoplastic polyurethane bead foams, such as steam molding, face inefficiencies due to high energy requirements and unsatisfactory heat distribution, leading to poor mechanical properties and increased cycle times, while electromagnetic field-based methods struggle with uniform heating and material conductivity issues.

Method used

A process using a composition of thermoplastic elastomer and thermoplastic polymer with specific dielectric properties, where the JDIM factor is between 0.3 and 3, allowing for efficient energy distribution through an electromagnetic field to fuse expanded particles without melting the central area, resulting in improved mechanical properties and reduced cycle times.

Benefits of technology

The process achieves better tensile strength and mechanical properties by ensuring uniform heating and energy distribution within the molded body, overcoming the limitations of traditional methods by using a specific composition and electromagnetic field energy.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure IMGF000004_0001
    Figure IMGF000004_0001
  • Figure IMGF000005_0001
    Figure IMGF000005_0001
  • Figure IMGF000007_0001
    Figure IMGF000007_0001
Patent Text Reader

Abstract

The present invention is directed to a molded body comprising expanded particles fused using an electromagnetic field, the expanded particles comprising a composition (C1) comprising a thermoplastic elastomer (TPE1) as component (M) and a thermoplastic polymer (TP1) as component (B1), wherein the composition (C1) has a factor JDIM in the range of from 0.3 to 3, defined by the melting point of the composition (C1) and the loss factor tanδ of the components of the composition (C1). The present invention is also directed to a process for the preparation of a molded body comprising expanded particles comprising a composition (C1), comprising the steps of loading the expanded particles comprising composition (C1) into a mold, and fusing the expanded particles comprising a thermoplastic elastomer by supplying energy at least partially through an electromagnetic field, wherein the composition (C1) has a factor JDIM in the range of from 0.3 to 3. The invention is further directed to the use of the molded body in shoe soles, part of shoe soles, shoe intermediate soles, shoe insoles, damping elements, cushioning elements, underlays, grips, flooring, mattresses, sporting goods, bicycle saddles, tires and in automotive interiors and exteriors.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Expanded thermoplastic polyurethane for special molding process

[0002] The present invention is directed to a molded body comprising expanded particles fused using an electromagnetic field, the expanded particles comprising a composition (C1) comprising a thermoplastic elastomer (TPE1) as component (M) and a thermoplastic polymer (TP1) as component (B1), wherein the composition (C1) has a factor JDIM in the range of from 0.3 to 3, defined by the melting point of the composition (C1) and the loss factor tan5 of the components of the composition (C1). The present invention is also directed to a process for the preparation of a molded body comprising expanded particles comprising a composition (C1), comprising the steps of loading the expanded particles comprising composition (C1) into a mold, and fusing the expanded particles comprising a thermoplastic elastomer by supplying energy at least partially through an electromagnetic field, wherein the composition (C1) has a factor JDIM in the range of from 0.3 to 3. The invention is further directed to the use of the molded body in shoe soles, part of shoe soles, shoe intermediate soles, shoe insoles, damping elements, cushioning elements, underlays, grips, flooring, mattresses, sporting goods, bicycle saddles, tires and in automotive interiors and exteriors.

[0003] The preparation of expanded thermoplastic elastomer bead foams is described within WO2014 / 198779 A1 using the extrusion technology while the preparation of parts out of the expanded thermoplastic elastomer beads is not explained.

[0004] WO2015 / 052265 also describes the preparation of expanded beads out of thermoplastic elastic polymers using an autoclave to impregnate the compact material. Afterwards, the impregnated beads can be foamed and in a special case directly molded to a part reducing the pressure within the autoclave. In another possibility, the impregnated beads are taken out and heated to the foaming temperature in a separate machinery. In case, single foamed beads are achieved, the part preparation is not further described.

[0005] Bead foams, such as polypropylene or polystyrene bead foams, typically are fused together with superheated water vapor in automatic molding machines to form shaped parts for the packaging industry for example. TPU bead foams can be further processed not only by superheated steam fusion but also by in situ foaming or adhering with reactive polyurethane systems. Since superheated steam fusion has very high energy requirements, alternatives are sought. Fusion by means of hot air is possible in principle, but does not as yet yield satisfactory parts owing to unsatisfactory distribution, and requires long cycle times because of the low energy content of hot air and the poor thermal conduction of closed-cell foams. The molding of expanded thermoplastic polyurethane bead foams is described in DE102013110242 A1. Here, different variations on filling the mold are explained all with the intention to have a fully filled cavity. Therefore, filling under pressure or with crack that is closed before molding are mentioned. Within all these variants, the filling is occurred by pressing more material into the cavity increasing the overall weight and density of the part. Regarding molding steam molding is used.

[0006] Using electromagnetic radiation or an electromagnetic field to provide the energy for molding is described in general in EP3698949 A1 and WO2017 / 125410 A1 for different expanded thermoplastic beads. Especially in W02017 / 125410 A1 it is shown thata homogeneous foamed part can be achieved using an electromagnetic field to apply the energy.

[0007] Improving the molding by using electromagnetic fields, a special mold design is described in EP3808522 A1. Here, the mold is separated in cavities to adjust the electromagnetic field and improve homogeneity of molding.

[0008] Foam moldings comprising expanded thermoplastic polyurethane are widely used for sports apparel, shoes, and shoe parts as well as for cushioning elements.

[0009] A way of bonding the foam beads together thermally is by high-frequency fusion as described inter alia in WO 2001 / 64414. In high-frequency fusion, the foamed beads, in particular of expandable polystyrene (EPS), expanded polypropylene (EPP) or expandable polyethylene terephthalate (EPET) which are to be fused together are surrounded with a liquid medium absorbing electromagnetic radiation, water for example, and then joined together by applying a form of electromagnetic radiation such as, for example, microwaves. Owing to the water imbibition due to the higher polarity of thermoplastic polymers, this process is only marginally possible for foam beads comprising thermoplastic elastomers. In addition, the 100°C temperature attainable on boiling water under atmospheric pressure is usually insufficient to fuse the elastomer beads together. The water imbibition allows the water to penetrate excessively into the beads, and the heating is effective not just at the points of contact but also within the beads. As a result, the beads may collapse prior to being fused.

[0010] DE 102013 012 515 A1 describes a process for joining foam beads, in particular EPP or EPS, together thermally by inductive heating with an improved energy balance. However, the production of shaped parts by inductive heating presupposes some electrical conductivity on the part of the beads, at least at the surfaces to be joined together. This is attainable by coating with electrically conductive fillers such as, for example, metallic powder or carbon black, nanotubes.

[0011] Spraying is an example of a possible way to coat the beads.

[0012] WO 2019 / 162172 A1 discloses a method for producing bead foams from foam beads based on thermoplastic elastomers, which comprises foam beads being wetted with a polar liquid and joined together thermally in a mold via high-frequency electromagnetic radiation. The use of additives in the molding process makes the process less efficient and increases the costs.

[0013] WO 2017 / 125410 A1 relates to a method for producing a particle foam part wherein foam particles are heated in a mold such that they weld together. This foam particles are made from polyurethane (Pll), polylactide (PLA), polyethylene block amide (PEBA) or from polyethylene terephthalate (PET). The heat is guided by means of electromagnetic RF radiation to the foam particles. In case of large or thick particle foam parts it is described that they heat up more strongly in the middle than in the edge region. An increase of the energy input by the electromagnetic field leads to a complete melting of the foam particles in the central area of the particle foam part.

[0014] The problem addressed by the present invention was that of remedying the disadvantages mentioned and of providing a method for producing molded bodies in a simple cost efficient process.

[0015] According to the present invention, this problem is solved by a molded body comprising expanded particles fused using an electromagnetic field, the expanded particles comprising a composition (C1) comprising a thermoplastic elastomer (TPE1) as component (M) and a thermoplastic polymer (TP1) as component (B1), wherein the composition (C1) has a factor JDIM:

[0016] 15000 v-

[0017] JDIM— — * > (tan 6t — 0,06) * ct where i is the index for the components in the composition in the range of from 0.3 < JDIM< 3, wherein Tmis the melting temperature of (M) determined via DSC, measured based on DIN EN ISO 11357-3:2013 with a heating rate of 20 K / min and drying of test specimen for 10 minutes at 100°C under nitrogen before measurement start, determined in the first heating cycle at the point of max enthalpy at the first peak, tanb is the energy dielectric loss factor measured at 27 MHz at 80°C of the components of the composition in according to DIN EN I EC 62631-2-2:2022, c is the concentration of the components of the composition as weight percentage. Due to the heat distribution in the mold, fusing the expanded particles using an electromagnetic field results in a different structure within the molded body in comparison to a molded body obtained by fusing expanded particles applying heat by different means such as for example using steam. In the latter case (steam molding) the heat is primarily applied to the surface of the molded body which results in stronger fusing in near the surface compared to the inner parts of the molded body.

[0018] The present invention is also directed to a process for the preparation of a molded body comprising expanded particles comprising composition (C1), comprising the steps of

[0019] (i) loading the expanded particles comprising composition (C1) into a mold,

[0020] (ii) fusing the expanded particles comprising a thermoplastic elastomer by supplying energy at least partially through an electromagnetic field, wherein the composition (C1) comprises a thermoplastic elastomer (TPE1) as component (M) and a thermoplastic polymer (TP1) as component (B1), wherein the composition (C1) has a factor JDIM:

[0021] 15000 v-

[0022] JDIM— — * > (tan 6t — 0,06) * ct where i is the index for the components in the composition in the range of from 0.3 < JDIM< 3, wherein Tmis the melting temperature of (M) determined via DSC, measured based on DIN EN ISO 11357-3:2013 with a heating rate of 20 K / min and drying of test specimen for 10 minutes at 100°C under nitrogen before measurement start, determined in the first heating cycle at the point of max enthalpy at the first peak, tanb is the energy dielectric loss factor measured at 27 MHz at 80°C of the components of the composition in according to DIN EN I EC 62631-2-2:2022, c is the concentration of the components of the composition as weight percentage.

[0023] The dielectric properties define the interaction of the RF field with the material. Higher losses will lead to a higher increase in temperature and thereby directly influence the molding performance. The dielectric characteristics are described by the real and imaginary part of the relative permittivity £r= £‘r- j £“r. The real part corresponds to the ability of the material to store the energy of the electric field, whereas the imaginary part corresponds to the dielectric losses. The so called loss factor tan(5) is defined as the ratio of the imaginary and real part of permittivity (£“rI £‘r). The practical meaning becomes clear when comparing an ideal and real capacitor. For an ideal capacitor, the current and voltage will have a phase delay of 90°. This phase delay is smaller than 90° by the loss angle 5.

[0024] There are multiple ways to measure the dielectric properties of a material. The methodological choice depends on the required frequency, the sample geometry and expected dielectric parameters. For solid dielectrics measurement guidelines are described in DIN EN IEC 62631-2- 2:2022. Unless otherwise noted, for the values stated in the present invention, measurements were performed with an impedance analyzer (Keysight E4991 B) and a dedicated sample test fixture (16453A) that allows dielectric evaluation from 1MHz-1GHz in a temperature range from - 55°C to +150°C. The test fixture was placed in a laboratory oven to perform the dielectric characterization in the temperature range that is expected to occur during the molding process. Prior to the measurement the system was calibrated using an open, short, load (with PTFE) compensation.

[0025] It has been surprisingly found that the use of a composition comprising a thermoplastic elastomer with a defined ratio of the melting temperature of the composition and the loss factor tan 5 allows to fuse the foamed particles and to obtain molded bodies with improved mechanical properties. It has been found that the temperature increase which occurs by the stimulation of the thermoplastic elastomer with energy at least partially through an electromagnetic field is sufficient to result in thermally molding the particles without melting of the foamed particles in the central area of the particle. The stimulation of the thermoplastic elastomer with energy at least partially through an electromagnetic field allows for a better energy distribution in the fusion step which in turn results in better mechanical properties such as for example better tensile strength of the molded body.

[0026] According to the present invention, the specific adjustment of the melting temperature and the dielectric properties of the composition, result in improved fusing in a process using an electromagnetic field and improved properties of the molded bodies obtained when using stimulation through an electromagnetic field. It has surprisingly been found that the melting temperature of the composition is strongly dependent on the melting temperature of the thermoplastic elastomer used as component (M) and the dielectric loss factor depends on the dielectric properties of the component (M) and (B1) present in the composition. Thus, according to the present invention, it is possible to adjust the properties of the composition using different combinations of components and adjusting the amounts based on the formula as defined above. According to the present invention, the composition (C1) comprises at least one thermoplastic elastomer (TPE1) as component (M) and a thermoplastic polymer (TP1) as component (B1). The composition may comprise further components or additives. Typically, the composition (C1) comprises the thermoplastic elastomer (TPE1) in an amount of 50% by weight to 100% by weight based on the weight of the composition (C1), preferably in an amount of from 60 to 99% by weight, more preferably in an amount of from 70 to 98% by weight, in particular in the range of from 85 to 97 % by weight, more preferable in an amount in the range of from 90 to 95% by weight based on the weight of the composition (C1). llseful thermoplastic elastomers include, for example, thermoplastic polyurethanes (TPU), thermoplastic polyester elastomers (e.g., polyether esters and polyester esters), thermoplastic copolyamides (e.g., polyether copolyamides) or thermoplastic styrene-butadiene block copolymers. Foam beads based on thermoplastic polyurethane (TPU) are particularly preferred.

[0027] According to the present invention, the composition (C1) has a factor JDIM:

[0028] 15000 v-

[0029] JDIM— — * > (tan 6t — 0,06) * ct where i is the index for the components in the composition in the range of from 0.3 < JDIM< 3, wherein Tmis the melting temperature of (M) determined via DSC, measured based on DIN EN ISO 11357-3:2013 with a heating rate of 20 K / min and drying of test specimen for 10 minutes at 100°C under nitrogen before measurement start, determined in the first heating cycle at the point of max enthalpy at the first peak, tanb is the energy dielectric loss factor measured at 27 MHz at 80°C of the components of the composition in according to DIN EN I EC 62631-2-2:2022, c is the concentration of the components of the composition as weight percentage.

[0030] Typically, the melting temperature of composition (C1) is in the range of from 90°C to 170°C, more preferable in the range of from 100°C to 160°C, in particular in the range of from 110°C to 140°C.

[0031] The thermoplastic elastomers employed to produce the foam beads preferably have a Shore hardness in the range from 70A to 92A, preferably in the range from 75A to 90A and more preferably in the range from 80A to 90A, determined by DIN ISO 48-4:2021-02 (average value; indentation of 3s) using samples that were tempered after preparation at 100 °C for 20 h. The bulk density of the foam beads used is preferably in the range from 30 to 250 kg / m3.

[0032] Expanded thermoplastic polyurethane beads according to the present invention belong to the group of particle foams, which are also referred to as foamed pellets (or bead foams, particle foam, expanded thermoplastic elastomer particles or expanded thermoplastic polyurethane beads). Particle foams and moldings (also referred to as molded article) made therefrom, based on thermoplastic polyurethanes or other thermoplastic elastomers, are known (for example WO 94 / 20568A1 , WO 2007 / 082838 A1 , WO2017 / 030835 A1 , WO 2013 / 153190 A1 , WO 2010 / 010010 A1) and can be used in many ways.

[0033] A foamed pellet or also a particle foam or bead foam in the sense of the present invention refers to a foam in the form of a particle, the average length of the particles preferably being in the range of 1 to 15 mm, determined according to DS / ISO 13322-2: 2021. In the case of non-spherical, e.g., oval particles average length means the longest dimension by length, (determined by 3D evaluation of the granules, for example by means of dynamic image analysis with an optical measuring device named “PartAn 3D”, Microtrac).

[0034] The single foam granules according to the present invention preferably have an average mass in the range of 0.1 to 50 mg, preferable in the range between 0.5 and 45 mg. The average mass means in this context the arithmetic mean based on a sample size of 10 different particles wherein each particle is weighted three times.

[0035] The foamed pellets according to the invention usually have a bulk density of 30 g / l to 250 g / l, preferably 50 g / l to 200 g / l, more preferably 70 g / l to 180 g / l. The bulk density is measured analogously to DIN ISO 60:1999, wherein the determination of the above values in contrast to the standard, a vessel with 10 I volume is used instead of a vessel with 0.1 I volume, since especially for the foam particles with low density and low mass a measurement with only 0.1 I volume is too inaccurate.

[0036] The particle foam according to the present invention can optionally be optimized by additives such as for example dyes, process aids, nucleating agents or stabilizers. The additives may be added during the generation of the precursor of the particle foam or during the foaming step. A precursor is a polymer composition that is used as input material for foaming.

[0037] Suitable additives may be present in the composition in an amount of from 0.01 % by weight to 15 % by weight, preferably in an amount of from 0.1 % by weight to 10 % by weight, in particular in an amount of from 0.5 % by weight to 5 % by weight, in each case based on the weight of the composition (C1).

[0038] In another embodiment of the present invention, the particle foams can be coated.

[0039] In a preferred embodiment for the particle foam molding according to the invention expanded thermoplastic polyurethane beads of the same composition and the same average mass are used.

[0040] In a preferred embodiment the particle foam molding consists of expanded thermoplastic polyurethane beads.

[0041] According to a further aspect, the present invention is also directed to the process as disclosed above, wherein the thermoplastic elastomer is a thermoplastic polyurethane.

[0042] In a preferred embodiment the dielectric loss factor of the thermoplastic polymer, in particular the thermoplastic polyurethane present in the composition as component (M), at 27 MHz and 80°C is in the range from 0.04 to 0.2. The dielectric loss factor of the thermoplastic polymer (TP1) or further additives may vary in wide ranges. For example the dielectric loss factor of thermoplastic polymers such as polystyrene or polyolefins is about 0.

[0043] In the context of the present invention, unless otherwise noted, the dielectric loss factor is determined using the compact material, i.e. the material before a foaming step or the individual materials of the foam beads after melting the foams beads and annealing and thus obtaining a compact material. The dielectric loss factor can be measured using a dielectric material test fixture named Keysight as described above. For this purpose, small and compact plates have to be generated by injection molding and, afterwards, cut into pieces which can be placed in the dielectric test fixture.

[0044] According to the present invention, the expanded particles are fused by supplying energy at least partially through an electromagnetic field. The thermal energy which results from the stimulation of the thermoplastic elastomer is sufficient to result in the thermal joining of the foam beads.

[0045] Typically, the thermal joining of the foam beads is effected in a mold via high-frequency electromagnetic radiation, especially via microwaves. High-frequency is to be understood as referring to electromagnetic radiation having frequencies of not less than 100 MHz. The electromagnetic radiation used is generally in the frequency range between 100 MHz and 300 GHz. Preference is given to using microwaves in the frequency range between 0.5 and 100 GHz, more preferably 0.8 to 10 GHz and irradiation times between 0.1 to 15 minutes. The frequency range of the microwave is preferably aligned with the absorption behavior of the thermoplastic elastomer, or conversely the thermoplastic elastomer is selected on the strength of its absorption behavior in relation to the frequency range of the microwave appliance used.

[0046] The method of the present invention makes it possible to fuse the foam beads together across a very wide frequency range.

[0047] The energy may be supplied by electromagnetic induction. For this purpose, a dielectric molding-tool is placed in between at least two capacitor plates which generate at least one dielectric field. The expanded foam beads are loaded into the cavity of the molding tool and are heated by applying the dielectric field. As a result, the surface of the foam beads is partially molten and, therefore the beads become fused and form the molded part. To preserve the foam morphology and melt the bead surface only, the process is adapted in accordance with the used materials and the design of the molded article. Typically, the temperature within the mold is in the range of from 40°C below the melting temperature of the composition (C1) to 20°C above the first melting temperature of the composition (C1), preferably in the range of from 20°C below the melting temperature of the composition (01) to 10°C above the first melting temperature of the composition (01), in particular in the range of from 10°C below the melting temperature of the composition (01) to 5°C above the first melting temperature of the composition (01). The temperature within the mold can for example be measured using an optical sensor.

[0048] In general, the energy input is controlled and adjusted by the applied voltage, the irradiation time, and the amount of material. Before the molded part can be removed from the molding tool, it must be stabilized and cooled down. The stabilization can be achieved by stopping the active heating or by means of an active cooling-procedure, such as for example described in EP3405322.

[0049] Fusing by energetic radiation is generally carried out in the microwave-frequency range of 300 MHz - 300 GHz or in the radio-frequency range of 30 kHz - 300 MHz. Microwaves are preferably applied in the frequency range between 0.5 and 100 GHz, especially preferably in the range between 0.8 and 10 GHz and irradiation times between 1 s and 15 min are used. Radio waves are preferably applied in the frequency range between 500 kHz and 100 MHz, especially preferably in the range between 1 MHz and 100 MHz and irradiation times between 1 s and 30 min are used. According to a further aspect, the present invention is also directed to the process as disclosed above, wherein in step (ii) the frequency of the electromagnetic field is in the range from 1 MHz to 100 MHz, in particular in the range of from 25 to 30 MHz. Typically, irradiation times in step (ii) are in the range of from 1 to 300 s.

[0050] According to the present invention, the molded body typically has an average thickness in the range of from 0.01 to 30 cm, preferably in the range of from 0.1 to 15 cm, more preferable in the range of from 0.5 to 10 cm, in particular in the range of from 1 to 5 cm.

[0051] Typically, the conditions in step (ii), for example the material of the mold, the distance of the plates and the frequency range used are adapted to result in an electric field of about 0.2 to 3 kV / cm.

[0052] The properties of the composition (C1) and the thermoplastic elastomer and thermoplastic polymers used may vary in broad ranges as long as JDIM is in the range as defined above. Suitable thermoplastic elastomers may for example have a molecular weight Mw in the range of from 50 to 250 kg / mol are used. Preferably, the molecular weight Mw is in the range of from 60 to 200 kg / mol, in particular in the range of from 100 to 180 kg / mol.

[0053] Unless otherwise noted, the molecular weight Mw of the thermoplastic elastomer is determined using GPC in the context of the present invention. Unless otherwise stated in the context of the present invention the determination of the weight average molecular weights Mw of the thermoplastic elastomers, dissolved in HFIP (hexafluoroisopropanol), is effected by means of GPC using the thermoplastic elastomers, dissolved in HFIP (hexafluoroisopropanol). Determination of the molecular weight is effected by means of two GPC columns arranged in series (PSS-Gel; 100A; 5p; 300*8 mm, Jordi-Gel DVB; MixedBed; 5p; 250*10 mm; column temperature 60° C.; flow 1 mL / min; Rl detector). Calibration is performed with polymethyl methacrylate (EasyCal; from PSS, Mainz) and HFIP is used as eluent.

[0054] Expanded particles comprising a thermoplastic elastomer and methods for the preparation thereof are in principle known from the state of the art. In particular expanded particles comprising a thermoplastic polyurethane are known from the state of the art.

[0055] Typically, the molecular weight can be adjusted by methods known to the person skilled in the art, for example by adjusting the process parameters in the preparation process, the ratios of the starting materials used or also the reactivity of the starting materials used. Thermoplastic polyurethanes usually are prepared using at least one polyisocyanate, at least one polyol and usually at least one chain extender. Suitable components for the preparation of thermoplastic polyurethanes are in principle known to the person skilled in the art.

[0056] Suitable isocyanates within the context of the present invention are in particular diisocyanates, in particular aliphatic or aromatic diisocyanates, more preferably aliphatic diisocyanates.

[0057] In addition, within the context of the present invention, pre-reacted products may be used as isocyanate components, in which some of the OH components are reacted with an isocyanate in a preceding reaction step. The products obtained are reacted with the remaining OH components in a subsequent step, the actual polymer reaction, thus forming the thermoplastic polyurethane.

[0058] Aliphatic diisocyanates typically used are customary aliphatic and / or cycloaliphatic diisocyanates. Suitable aromatic diisocyanates are also known to the person skilled in the art.

[0059] Mixtures can in principle also be used. Examples of mixtures are mixtures comprising at least one further methylene diphenyl diisocyanate besides methylene diphenyl 4,4’-diisocyanate. The term “methylene diphenyl diisocyanate” here means diphenylmethane 2,2’-, 2,4’- and / or 4,4’- diisocyanate or a mixture of two or three isomers. It is therefore possible to use as further isocyanate, for example, diphenylmethane 2,2’- or 2,4’-diisocyanate or a mixture of two or three isomers. In this embodiment, the polyisocyanate composition can also comprise other abovementioned polyisocyanates.

[0060] If further isocyanates are used, these are present in the isocyanate composition (IC) preferably at an amount in the range from 0.1 % to 20% by weight, further preferably in the range from 0.1 % to 10% by weight and particularly preferably at an amount in the range from 0.5% to 5% by weight.

[0061] Preferred examples of higher-functionality isocyanates are triisocyanates, for example triphenylmethane 4,4',4"-triisocyanate, and also the cyanurates of the aforementioned diisocyanates, and the oligomers obtainable by partial reaction of diisocyanates with water, for example the biurets of the aforementioned diisocyanates, and also oligomers obtainable by controlled reaction of semiblocked diisocyanates with polyols having an average of more than two and preferably three or more hydroxyl groups. Organic isocyanates that can be used are aliphatic, cycloaliphatic, araliphatic and / or aromatic isocyanates.

[0062] Crosslinkers can additionally also be used, for example the previously mentioned higher-functionality polyisocyanates or polyols, or else other higher-functionality molecules having a plurality of isocyanate-reactive functional groups. It is likewise possible within the context of the present invention to achieve crosslinking of the products through an excess of the isocyanate groups used in proportion to the hydroxyl groups. Examples of higher-functionality isocyanates are triisocyanates, for example triphenylmethane 4,4',4"-triisocyanate and isocyanurates, and also the cyanurates of the aforementioned diisocyanates, and the oligomers obtainable by partial reaction of diisocyanates with water, for example the biurets of the aforementioned diisocyanates, and also oligomers obtainable by controlled reaction of semiblocked diisocyanates with polyols having an average of more than two and preferably three or more hydroxyl groups.

[0063] Here, within the context of the present invention, the amount of crosslinker, that is to say of higher-functionality isocyanates and higher-functionality polyols or higher-functionality chain extenders, is no greater than 3% by weight, preferably less than 1% by weight, further preferably less than 0.5% by weight, based on the total mixture of the components.

[0064] The polyisocyanate composition may also comprise one or more solvents. Suitable solvents are known to those skilled in the art. Suitable examples are nonreactive solvents such as ethyl acetate, methyl ethyl ketone and hydrocarbons.

[0065] A polyol composition (PC) may be used according to the invention. According to the invention, the polyol composition (PC) may comprise at least one polyol. Suitable polyols are known in principle to those skilled in the art and described for example in "Kunststoffhandbuch [Plastics Handbook], volume 7, Polyurethane [Polyurethanes]”, Carl Hanser Verlag, 3rd edition 1993, chapter 3.1. Particular preference is given to using, as polyol, polyesterols or polyetherols as polyols. It is likewise possible to use polycarbonates. Copolymers may also be used in the context of the present invention. Polyether polyols are particularly preferred. The number-average molecular weight of the polyols used according to the invention is preferably in the range from 500 to 5000 g / mol, by way of example in the range from 550 g / mol to 2000 g / mol, preferably in the range from 600 g / mol to 1500 g / mol, especially between 650 g / mol and 1000 g / mol. According to the present invention, the polyols used can be fossil based or non-fossil based.

[0066] Polyetherols, but also polyesterols, block copolymers and hybrid polyols such as for example poly(ester / amide), are suitable according to the invention. According to the invention, preferred polyetherols are polyethylene glycols, polypropylene glycols. Suitable polyols may also be selected from polyadipates, polycarbonates, polycarbonate diols and polycaprolactone.

[0067] In a further embodiment, the present invention accordingly relates to foamed pellets as described previously, wherein the polyol composition comprises a polyol selected from the group consisting of polyetherols, polyesterols, such as polycaprolactone polyols, and polycarbonate polyols.

[0068] Suitable polyols are for example those having ether and ester blocks, for example polycaprolactone having polyethylene oxide or polypropylene oxide end blocks, or else polyethers having polycaprolactone end blocks. According to the invention, preferred polyetherols are polyethylene glycols and polypropylene glycols. Suitable polyols are for example polytetramethylene gylcole or polytrimenthylene glycole. Polycaprolactone is also preferred. According to the present invention, also polyesterols may be used, in particular non fossil based polyesterols. Suitable polyesterols are for example based on succinic acid. Polyols based on castor oil or lignin based polyols may also be used.

[0069] It is also possible in accordance with the invention to use mixtures of different polyols. The poly- ols / the polyol composition used preferably have / has an average functionality of between 1 .8 and 2.3, preferably between 1.9 and 2.2, in particular 2. The polyols used in accordance with the invention preferably have solely primary hydroxyl groups.

[0070] In an embodiment of the present invention, a polyol composition (PC) is used which comprises at least polytetrahydrofuran. According to the invention, the polyol composition may also comprise further polyols in addition to polytetrahydrofuran.

[0071] Further polyols that are suitable according to the invention are, for example, polyethers, but also polyesters, block copolymers and also hybrid polyols such as for example poly(ester / amide). Suitable block copolymers are for example those having ether and ester blocks, for example polycaprolactone having polyethylene oxide or polypropylene oxide end blocks, or else polyethers having polycaprolactone end blocks. According to the invention, preferred polyetherols are polyethylene glycols and polypropylene glycols. Polycaprolactone is also preferred as a further polyol.

[0072] According to the present invention, it is also possible to use polytetramethylengylcole or polytri- menthylenglycole which are non-fossil based or mixtures of fossil and non-fossil based polyols. In a particularly preferred embodiment, the polytetrahydrofuran has a number-average molecular weight Mn in the range from 500 g / mol to 5000 g / mol, preferably in the range of from 500 g / mol to 2000 g / mol, further preferably in the range from 550 to 2000 g / mol, particularly preferably in the range from 650 to 1400 g / mol.

[0073] Within the context of the present invention, the composition of the polyol composition (PC) can vary within wide ranges. The polyol composition can also comprise mixtures of various polyols.

[0074] According to the invention, the polyol composition may also comprise a solvent. Suitable solvents are known perse to those skilled in the art.

[0075] When polytetrahydrofuran is used, the number-average molecular weight Mn of the polytetrahydrofuran is preferably in the range from 500 to 2000 g / mol. The number-average molecular weight Mn of the polytetrahydrofuran is further preferably within the range from 650 to 1400 g / mol.

[0076] In a further embodiment, the present invention also relates to foamed pellets as described previously, wherein the polyol composition comprises a polyol selected from the group consisting of polytetrahydrofurans having a number-average molecular weight Mn in the range from 500 g / mol to 5000 g / mol.

[0077] In a further embodiment, the present invention accordingly relates to foamed pellets as described previously, wherein the polyol composition comprises a polyol selected from the group consisting of polytetrahydrofurans having a number-average molecular weight Mn in the range from 500 g / mol to 2000 g / mol.

[0078] Mixtures of various polytetrahydrofurans can also be used in accordance with the invention, that is to say mixtures of polytetrahydrofurans having different molecular weights.

[0079] Preferred polyetherols according to the invention are polyethylene glycols, polypropylene glycols and polytetrahydrofurans, and also mixed polyetherols thereof. Mixtures of various polytetrahydrofurans differing in molecular weight may by way of example also be used according to the invention.

[0080] According to the invention, at least one chain extender (CE1) may be used. Suitable chain extenders are known per se to those skilled in the art. By way of example, chain extenders are compounds having two groups which are reactive towards isocyanate groups, in particular those having a molecular weight of less than 500 g / mol. Suitable chain extenders are for example diamines or diols. Diols are more preferred according to the invention. Within the scope of the present invention, mixtures of two or more chain extenders may also be used.

[0081] Suitable diols are known in principle to those skilled in the art. According to the invention, the diol preferably has a molecular weight of < 500 g / mol. According to the invention, aliphatic, arali- phatic, aromatic and / or cycloaliphatic diols having a molecular weight of 50 g / mol to 220 g / mol can be used here as chain extenders, for example. Preference is given to alkanediols having 2 to 10 carbon atoms in the alkylene radical, especially di-, tri-, tetra-, penta-, hexa-, hepta-, octa-, nona- and / or decaalkylene glycols. For the present invention, particular preference is given to 1 ,2-ethylene glycol, propane-1 , 3-diol, butane-1 ,4-diol, pentane-1 ,5-diol, hexane-1 ,6-diol.

[0082] Suitable chain extenders (CE1) within the context of the present invention are also branched compounds such as 1 ,4-cyclohexanedimethanol, 2-butyl-2-ethylpropanediol, neopentyl glycol, 2,2,4-trimethylpentane-1 ,3-diol, pinacol, 2-ethylhexane-1 , 3-diol or cyclohexane-1 ,4-diol.

[0083] In a further embodiment, the present invention accordingly relates to foamed pellets as described previously, wherein the chain extender (CE1) is selected from the group consisting of propane-1 , 3-diol, ethane-1 ,2-diol, butane-1 ,4-diol, pentane-1 ,5-diol, hexane-1 ,6-diol and HQEE.

[0084] According to a further aspect, the present invention is also directed to the process as disclosed above, wherein the thermoplastic polyurethane is obtained or obtainable by reacting at least the components (a) to (c):

[0085] (a) a polyisocyanate composition (IC) comprising an isocyanate selected from the group consisting of methylene diphenyl diisocyanate, hexamethylene diisocyanate and pentameth- lyene diisocyanate;

[0086] (b) at least one chain extender (CE1),

[0087] (c) a polyol composition (PC).

[0088] The properties, in particular the molecular weight of the thermoplastic polyurethane obtained may for example be adjusted by adjustment of the temperature applied in the preparation process. Typically, a lower temperature results in lower molecular weight. Furthermore, the use of a suitable catalyst and the amount of catalyst used may have an influence on the molecular weight of the thermoplastic polyurethane obtained. The molecular weight of the thermoplastic polyurethane obtained may also be adjusted by the ratio of the components used, in particular the ratio of NCO groups and the groups which are reactive towards isocyanate groups. The quantitative ratios of the components used are preferably selected here such that a hard segment content in the range from 5% to 80% is obtained, preferably in the range of from 10% to 55%, in particular in the range of from 13% to 45%, more preferable in the range of from 15% to 35%. The hard segment content calculated according to the formula (I) unless otherwise noted:

[0089] It has been found that thermoplastic polyurethanes having a molecular weight Mw in the range of from 50 to 250 kg / mol and a hard segment content of the thermoplastic polyurethane in the range of from 15% to 50% are particularly suitable for the preparation of molded bodies.

[0090] According to a further aspect, the present invention is also directed to the process as disclosed above, wherein the hard segment content of the thermoplastic polyurethane is in the range of from 15% to 50%, calculated according to the formula (I):

[0091] (I).

[0092] Furthermore, it has been found that the crystallinity of the thermoplastic elastomers may have an influence on the properties of the mold obtained. It has been found that thermoplastic elastomers, in particular thermoplastic polyurethanes having a low crystallinity are particularly suitable for the preparation of molded bodies. The crystallinity can be determined by DSC measurement according to DIN EN ISO 11357-3:2018 including a drying step within the measurement system of 10 minutes at 100 °C before starting the measurement from below 0 °C to 250 °C with a cooling rate of 20 K / min to the start temperature of the measurement and a heating rate of 10 K / min from the start temperature up to the 250°C.

[0093] According to the present invention, composition (C1) further comprises at least one thermoplastic polymer (TP1) as component (B1). Composition (C1) may also comprise further components, for example further thermoplastic polymers (TP2) or (TP3) as components (B2) and (B3). Suitable thermoplastic polymers are in principle known to the person skilled in the art. Suitable are for example thermoplastic polymers such as polyamides, styrene polymers or polyolefins, such as polyethylene or polypropylene. According to a further embodiment, the present invention is also directed to the process as disclosed above, wherein the thermoplastic polymer (TP1) is selected from the group consisting of polyolefins, polyamides and polystyrenes.

[0094] Suitable polyamides are commercially available polyamides and are in principle known to the person skilled in the art.

[0095] Suitable styrene polymers may be standard polystyrene. The term “standard polystyrene” here embraces preferably atactic, syndiotactic or isotactic polystyrene, more preferably atactic polystyrene. Atactic polystyrene of the invention, which is amorphous, has a glass transition temperature in the range of 100°C ± 20°C (determined according to DIN EN ISO 11357-1 , February 2017 / DIN EN ISO 11357-2, July 2014, Inflection point method). Syndiotactic and isotactic polystyrene of the invention are each semicrystalline and have a melting point in the region respectively of 270°C and 240°C (DIN EN ISO 11357-1 , February 2017 / DIN EN ISO 11357-3, April 2013, peak melting temperature). The polystyrenes used typically have a modulus of elasticity in tension of more than 2500 (DIN EN ISO 527-1 / 2, June 2012).

[0096] The production and processing of the polystyrenes of the invention is described extensively in the literature, for example in Kunststoff-Handbuch Band 4, "Polystyrol" [Plastics handbook, vol. 4, “Polystyrene”], by Becker / Braun (1996).

[0097] Suitable are also styrene polymers with a modulus of elasticity below 2700 MPa (DIN EN ISO 527-1 / 2, June 2012), preferably styrene block copolymers based on a styrene monomer. Suitbale are for example thermoplastic elastomers based on styrene, and high-impact polystyrenes (HIPS) which by way of example include SEBS, SBS, SEPS, SEPS-V and acrylonitrile-butadi- ene-styrene copolymers (ABS), very particular preference being given here to high-impact polystyrene (HIPS).

[0098] The production and processing of the styrene polymers are described extensively in the literature, for example in Kunststoff-Handbuch Band 4, "Polystyrol" [Plastics handbook, vol. 4, “Polystyrene”], by Becker / Braun (1996).

[0099] Suitable polyolefins are for example homopolypropylene, polyethylene or also mixtures of homopolypropylene and polyethylenes.

[0100] Polyolefins produced both with Ziegler catalysts and with metallocene catalysts are suitable. The crystallite melting point (DIN EN ISO 11357-1 / 3, February 2017 / April 2013, W peak melting temperature) of the polyolefins which can be used according to the invention is generally between 90 and 170°C.

[0101] Suitable polyethylenes may be polyethylene polymers customary for those skilled in the art, for example LD (low density), LLD (linear low density), MD (medium density), or HD (high density), HMW (high molecular weight) or LIHMW (ultra high molecular weight) polyethylenes.

[0102] The thermoplastic polymer (TP1) may be present in the composition in an amount of from 0.01 % by weight to 20 % by weight, preferably in an amount of from 0.1 % by weight to 15 % by weight, in particular in an amount of from 1 % by weight to 10 % by weight, in each case based on the weight of the composition (C1).

[0103] In the context of the present invention it is also possible to use two or more thermoplastic polymers. Preferably, the amount of the sum of thermoplastic polymers in composition (C1) is in the range of from 0.01 % by weight to 20 % by weight, preferably in an amount of from 0.1 % by weight to 15 % by weight, in particular in an amount of from 1 % by weight to 10 % by weight, in each case based on the weight of the composition (C1).

[0104] According to the present invention, the amount of thermoplastic polymer may be adapted to adjust the factor JDIM of the composition. The thermoplastic polymer and the amount used may be chosen depending on the dielectric loss factor of the thermoplastic elastomer (TPE1) and the dielectric loss factor of the thermoplastic polymer (TP1).

[0105] The composition (C1) comprises the thermoplastic elastomer and the thermoplastic polymer but may also comprise further additives in suitable amounts, for example composition (C1) may comprise at least one additive selected from the group of dipropylene glycol and water.

[0106] Suitable additives may also be selected from the group of esters of carboxylic acids and diols or triols, for example glycol esters of acetic or citric acid, glycerol esters of acetic or citric acid or glycols and liquid polyglycols, such as triethylene glycol or tripropylene glycol, for example 1 ,2,3-propanetriol triacetate (triacetin, glycerol triacetate), triethylene glycol or tripropylene glycol.

[0107] These additives may be present in the composition in an amount of from 0.01 % by weight to 10 % by weight, preferably in an amount of from 0.01 % by weight to 5 % by weight, in particular in an amount of from 0.01 % by weight to 25 % by weight, in each case based on the weight of the composition (C1).

[0108] Also metal fibers or carbon fibers may be used as additives in the context of the present invention.

[0109] In one embodiment of the present invention, the particle foams comprise polar additives which increase the dielectric heating effect by absorbing the electromagnetic radiation. Polar additives are preferably selected from the group consisting of inorganic salts, esters of carboxylic acids and diols or triols or glycols, amines, carbamide compounds, polyol, and glycerol.

[0110] It is also possible that the polymeric foam beads are coated with water or other polar liquids or additives comprising functional groups with hydrocarbons (such as carbamide or esters of carboxylic acids and diols or triols or glycols and liquid polyethylene glycols). Preferably the coating is applied in proportions of 0,1 to 10 wt.-%, more preferably in proportions of 1 to 6 wt.-%, based on the used particle foam. In another embodiment of the present invention, the polymeric foam beads are coated with inorganic saline solutions such as for example sodium chloride solution prior to the fusion by means of electromagnetic radiation. Preferably the concentration of the applied saline solutions is in the range between 0,1 to 5 wt.-%, more preferably between 0,1 to 0,8 wt.-%. The above-described functionalization to increase the dielectric heating intensity of nonpolar polymeric foam beads can be carried out in analogy to the methods described in EP3053732 or WO16146537. In general, polar additives are applied for polymeric foam beads which cannot be or not sufficiently be stimulated by electromagnetic radiation and, therefore, cannot be heated up without suitable additives. For this purpose, the frequency range of the applied electromagnetic radiation is adjusted to the absorption behavior of the polar coating or additive or vice versa the polar liquid or additive is selected based on the absorption behavior according to the available frequency range of the used device. Fusing polymeric range of the used device. Fusing polymeric foam beads based on thermoplastic polyurethane (TPU) or thermoplastic polyamides (TPA) with electromagnetic radiation can preferably be achieved in the context of the present invention without the use of polar additives.

[0111] The moldings can be produced by means of molding machines. For this purpose, the foamed particles are conveyed into the shaping tool manually or automated by using pressurized air. The shaping tool also referred to as mold or molding tool comprises two primary components, the injection mold-plate with the filling nozzles, and a counterpart-plate. To generate the molding part, both mold-plates are pressed together so that a cavity in the shape of the molding part is formed. The filling of the mold-cavity can be conducted either by crack filling method or by the pressure filling method. The crack-filling method comprises the following steps:

[0112] (i’) injecting the expanded foam-particles into the mold-cavity without a backpressure of the counterpart-plate,

[0113] (ii’) fusing the particles while closing the plates of the mold mechanically,

[0114] (iii’) cool down the molding part and

[0115] (iv’) demold the produced part, wherein in step (i1) a gap between the injection mold-plate and the counterpart-plate is adjusted which is also referred to as crack-height. The mold-cavity is filled with a predetermined amount of the expanded beads in step (i’). In step (ii’) the volume of the mold-cavity is reduced compared to step (i') , because the two parts of the molding tool are closed tightly and the intermediate gap is, thus, disappeared. This leads to a pressure increase within the mold-cavity. The expanded beads are thus pressed against one another and can therefore become fused to give the molding.

[0116] The degree of compression is one important parameter to control the fusion-quality of the molding. The degree of compression is calculated by dividing the dosage volume per cycle through the volume of the mold cavity adjusted in step (ii’), wherein the dosage volume per cycle is given by the dosage weight per cycle divided through the bulk density of the foamed beads.

[0117] In one embodiment according to the present invention the degree of compression is in the range from 1 .7 to 2.3. Preferably, the degree of compression at the crack-filling method is lower than 2.

[0118] The pressure filling method comprises the following steps:

[0119] (i’) injecting the expanded foam-particles into the mold-cavity by pneumatic pressure while compressing both plates of the mold tightly together,

[0120] (ii’) fusing the particles,

[0121] (iii’) cool down the molding part, (iv’) demold the produced part.

[0122] Since the exerted injection pressure in step (i’) is ceased in step (ii’) the inserted foam beads may further expand and as a result be pressed against one and another and, therefore, become fused and give the molding.

[0123] The fusing in step (ii’) can be induced by means of at least one electromagnetic field, independently of the chosen loading method. According to a further embodiment, the present invention therefore is also directed to a process as disclosed above, wherein in step (i) crack-filling method is used.

[0124] As set out above, the energy is supplied by electromagnetic induction. For this purpose, a dielectric molding-tool is placed in between at least two capacitor plates which generate at least one dielectric field. The expanded foam beads are loaded into the cavity of the molding tool and are heated by applying the dielectric field. As a result, the surface of the foam beads is partially molten and, therefore the beads become fused and form the molded part. To preserve the foam morphology and melt the bead surface only, the process is adapted in accordance with the used materials and the design of the molded article. In general, the energy input is controlled and adjusted by the applied voltage, the irradiation time, and the amount of material. Before the molded part can be removed from the molding tool, it must be stabilized and cooled down. The stabilization can be achieved by stopping the active heating or by means of an active cooling procedure, such as for example described in EP3405322.

[0125] Fusing by energetic radiation is generally carried out in the microwave-frequency range of 300 MHz - 300 GHz or in the radio-frequency range of 30 kHz - 300 MHz. Microwaves are preferably applied in the frequency range between 0,5 and 100 GHz, especially preferably in the range between 0,8 and 10 GHz and irradiation times between 1 s and 15 min are used. Radio waves are preferably applied in the frequency range between 500 kHz and 100 MHz, especially 10 preferably in the range between 1 MHz and 80 MHz and irradiation times between 1 s and 30 min are used.

[0126] The expanded particles comprising a thermoplastic elastomer can be molded without using additional additives which can be stimulated through an electromagnetic field, in particular additives which can be stimulated through an electromagnetic field to increase the temperature within the mold. Preferably, no additives are used in the process according to the present invention which can be stimulated through an electromagnetic field in a way which results in a rise of temperature in the mold.

[0127] According to a further aspect, the present invention is also directed to the process as disclosed above, wherein no additives are added in step (i) or (ii) which can be stimulated through an electromagnetic field in a way which results in a rise of temperature in the mold. According to a further aspect, the present invention is also directed to the use of expanded particles comprising a composition (C1) comprising a thermoplastic elastomer (TPE1) as component (M) and a thermoplastic polymer (TP1) as component (B1), wherein the composition (C1) has a factor JDIM:

[0128] 15000 v-

[0129] JDIM— — * > (tan 6t — 0,06) * ct where i is the index for the components in the composition in the range of from 0.3 < JDIM< 3, wherein Tmis the melting temperature of (M) determined via DSC, measured based on DIN EN ISO 11357-3:2013 with a heating rate of 20 K / min and drying of test specimen for 10 minutes at 100°C under nitrogen before measurement start, determined in the first heating cycle at the point of max enthalpy at the first peak, tanb is the energy dielectric loss factor measured at 27 MHz at 80°C of the components of the composition in according to DIN EN I EC 62631-2-2:2022, c is the concentration of the components of the composition as weight percentage.

[0130] According to a further aspect, the present invention is also directed to a molded body obtainable or obtained by a process as disclosed above.

[0131] Owing to their elastomeric properties, the bead foams of the present invention are useful for applications in the sports, footwear and packaging sectors, for example as safety footwear or as packaging for electronic components or instruments.

[0132] The invention additionally provides for the use of inventive foamed pellets for the production of a molded body for shoe intermediate soles, shoe insoles, shoe combisoles, bicycle saddles, bicycle tires, damping elements, cushioning, mattresses, underlays, grips, protective films, in components in automobile interiors and exteriors, in balls and sports equipment or as floor covering, especially for sports surfaces, track and field surfaces, sports halls, children's playgrounds and pathways. The invention additionally provides for the use of inventive foamed pellets for the production of consumer goods or industrial goods, parts in the automotive sector or packaging.

[0133] Preference is given to using inventive foamed pellets for the production of a molded body for shoe intermediate soles, shoe insoles, shoe combisoles or a cushioning element for shoes. Here, the shoe is preferably an outdoor shoe, sports shoe, sandals, boot or safety shoe, particularly preferably a sports shoe.

[0134] According to a further aspect, the present invention is also directed to the use of the molded body obtained or obtainable according to the process as disclosed above in shoe soles, part of shoe soles, shoe intermediate soles, shoe insoles, damping elements, cushioning elements, underlays, grips, flooring, mattresses, sporting goods, bicycle saddles, tires and in automotive interiors and exteriors. According to another aspect, the present invention is also directed to the use of the molded body as disclosed above in shoe soles, part of shoe soles, shoe intermediate soles, shoe insoles, damping elements, cushioning elements, underlays, grips, flooring, mattresses, sporting goods, bicycle saddles, tires and in automotive interiors and exteriors.

[0135] Further embodiments of the present invention can be found in the claims and the examples. It will be appreciated that the features of the subject matter / processes / uses according to the invention that are mentioned above and elucidated below are usable not only in the combination specified in each case but also in other combinations without departing from the scope of the invention. For example, the combination of a preferred feature with a particularly preferred feature or of a feature not characterized further with a particularly preferred feature etc. is thus also encompassed implicitly even if this combination is not mentioned explicitly.

[0136] Illustrative embodiments of the present invention are listed below, but these do not restrict the present invention. In particular, the present invention also encompasses those embodiments which result from the dependency references and hence combinations specified hereinafter.

[0137] 1 . Molded body comprising expanded particles fused using an electromagnetic field, the expanded particles comprising a composition (C1) comprising a thermoplastic elastomer (TPE1) as component (M) and a thermoplastic polymer (TP1) as component (B1), wherein the composition (C1) has a factor JDIM:

[0138] 15000

[0139] JDIM— — (tan 6t - 0,06) * ct' where i is the index for the components in the composition in the range of from 0.3 < JDIM< 3, wherein Tmis the melting temperature of (M) determined via DSC, measured based on DIN EN ISO 11357-3:2013 with a heating rate of 20 K / min and drying of test specimen for 10 minutes at 100°C under nitrogen before measurement start, determined in the first heating cycle at the point of max enthalpy at the first peak, tan5 is the energy dielectric loss factor measured at 27 MHz at 80°C of the components of the composition in according to DIN EN I EC 62631-2-2:2022, c is the concentration of the components of the composition as weight percentage.

[0140] 2. The molded body according to embodiment 1 , wherein the thermoplastic elastomer (TPE1) is a thermoplastic polyurethane.

[0141] 3. The molded body according to any one of embodiments 1 or 2, wherein the thermoplastic polymer (TP1) is selected from the group consisting of polyolefins, polyamides an polystyrene, in particular from the group consisting of polyethylene and polystyrene.

[0142] 4. The molded body according to any one of embodiments 1 to 3, wherein the molded body has an average thickness in the range of from 0.1 to 30 cm.

[0143] 5. The molded body according to any one of embodiments 1 to 4, wherein the molded body has a tensile strength of greater than 0.6 MPa, preferably greater than 0.7 MPa, more preferable greater than 0.8 MPa, more preferable greater than 0.85 MPa, more preferable greater than 0.9 MPa, in particular greater than 1 .0 MPa, determined according to ASTM D 5035:2015.

[0144] 6. The molded body according to any one of embodiments 1 to 5, wherein the thermoplastic elastomer is a thermoplastic polyurethane with a Shore hardness in the range of from 70A to 92A.

[0145] 7. Process for the preparation of a molded body comprising expanded particles comprising a composition (C1), comprising the steps of

[0146] (i) loading the expanded particles comprising composition (C1) into a mold,

[0147] (ii) fusing the expanded particles comprising a thermoplastic elastomer by supplying energy at least partially through an electromagnetic field, wherein the composition (C1) comprises a thermoplastic elastomer (TPE1) as component (M) and a thermoplastic polymer (TP1) as component (B1), wherein the composition (C1) has a factor JDIM:

[0148] 15000 v-

[0149] JDIM— — * > (tan 6t — 0,06) * ct where i is the index for the components in the composition in the range of from 0.3 < JDIM< 3, wherein Tmis the melting temperature of (M) determined via DSC, measured based on DIN EN ISO 11357-3:2013 with a heating rate of 20 K / min and drying of test specimen for 10 minutes at 100°C under nitrogen before measurement start, determined in the first heating cycle at the point of max enthalpy at the first peak, tanb is the energy dielectric loss factor measured at 27 MHz at 80°C of the components of the composition in according to DIN EN I EC 62631-2-2:2022, c is the concentration of the components of the composition as weight percentage.

[0150] 8. The process according to embodiment 7, wherein the thermoplastic elastomer (TPE1) is a thermoplastic polyurethane.

[0151] 9. The process according to any one of embodiments 7 or 8, wherein the thermoplastic polymer (TP1) is selected from the group consisting of polyolefins, polyamides an polystyrene, in particular from the group consisting of polyethylene and polystyrene.

[0152] 10. The process according to any one of embodiments 7 to 9, wherein the molded body has a tensile strength of greater than 0.6 MPa, preferably greater than 0.7 MPa, more preferable greater than 0.8 MPa, more preferable greater than 0.85 MPa, more preferable greater than 0.9 MPa, in particular greater than 1.0 MPa, determined according to ASTM D 5035:2015.

[0153] 11. The process according to any one of embodiments 7 to 10, wherein in step (ii) a voltage of 3 to 9 kV is applied for a duration of 1 to 300 seconds.

[0154] 12. The process according to any one of embodiments 7 to 11 , wherein the molded body has an average thickness in the range of from 0.1 to 30 cm. 13. The process according to any one of embodiments 7 to 12, wherein the thermoplastic elastomer is a thermoplastic polyurethane with a Shore hardness in the range of from 70A to 92A.

[0155] 14. The process according to any one of embodiments 7 to 13, wherein in step (i), the crackfilling method is used.

[0156] 15. The process according to any one of embodiments 7 to 14, wherein no additives are added in step (i) or (ii) which can be stimulated through an electromagnetic field in a way which results in a rise of temperature in the mold.

[0157] 16. Use of expanded particles comprising a composition (C1) for the preparation of a molded body by fusing the particles by supplying energy at least partially through an electromagnetic field, wherein the composition (C1) comprises a thermoplastic elastomer (TPE1) as component (M) and a thermoplastic polymer (TP1) as component (B1), wherein the composition (C1) has a factor JDIM:

[0158] 15000

[0159] JDIM— — (tan 6t - 0,06) * ct' where i is the index for the components in the composition in the range of from 0.3 < JDIM< 3, wherein Tmis the melting temperature of (M) determined via DSC, measured based on DIN EN ISO 11357-3:2013 with a heating rate of 20 K / min and drying of test specimen for 10 minutes at 100°C under nitrogen before measurement start, determined in the first heating cycle at the point of max enthalpy at the first peak, tan5 is the energy dielectric loss factor measured at 27 MHz at 80°C of the components of the composition in according to DIN EN I EC 62631-2-2:2022, c is the concentration of the components of the composition as weight percentage.

[0160] 17. The use according to embodiment 16, wherein the thermoplastic elastomer (TPE1) is a thermoplastic polyurethane.

[0161] 18. The use according to any one of embodiments 16 or 17, wherein the thermoplastic polymer (TP1) is selected from the group consisting of polyolefins, polyamides an polystyrene, in particular from the group consisting of polyethylene and polystyrene. 19. The use according to any one of embodiments 16 to 18, wherein the thermoplastic elastomer is a thermoplastic polyurethane with a Shore hardness in the range of from 70A to 92A.

[0162] 20. Molded body obtainable or obtained by a process according to any one of embodiments 7 to 15.

[0163] 21. Molded body obtainable or obtained by a process for the preparation of a molded body comprising expanded particles comprising a composition (C1), comprising the steps of

[0164] (i) loading the expanded particles comprising composition (C1) into a mold,

[0165] (ii) fusing the expanded particles comprising a thermoplastic elastomer by supplying energy at least partially through an electromagnetic field, wherein the composition (C1) comprises a thermoplastic elastomer (TPE1) as component (M) and a thermoplastic polymer (TP1) as component (B1), wherein the composition (C1) has a factor JDIM:

[0166] 15000 v-

[0167] JDIM— — * > (tan 6t — 0,06) * ct where i is the index for the components in the composition in the range of from 0.3 < JDIM< 3, wherein Tmis the melting temperature of (M) determined via DSC, measured based on DIN EN ISO 11357-3:2013 with a heating rate of 20 K / min and drying of test specimen for 10 minutes at 100°C under nitrogen before measurement start, determined in the first heating cycle at the point of max enthalpy at the first peak, tanb is the energy dielectric loss factor measured at 27 MHz at 80°C of the components of the composition in according to DIN EN IEC 62631-2-2:2022, c is the concentration of the components of the composition as weight percentage.

[0168] 22. The molded body according to embodiment 21 , wherein the thermoplastic elastomer (TPE1) is a thermoplastic polyurethane.

[0169] 23. The molded body according to any one of embodiments 21 or 22, wherein the thermoplastic polymer (TP1) is selected from the group consisting of polyolefins, polyamides an polystyrene, in particular from the group consisting of polyethylene and polystyrene. 24. The molded body according to any one of embodiments 21 to 23, wherein the molded body has a tensile strength of greater than 0.6 MPa, preferably greater than 0.7 MPa, more preferable greater than 0.8 MPa, more preferable greater than 0.85 MPa, more preferable greater than 0.9 MPa, in particular greater than 1.0 MPa, determined according to ASTM D 5035:2015.

[0170] 25. The molded body according to any one of embodiments 21 to 24, wherein in step (ii) a voltage of 3 to 9 kV is applied for a duration of 1 to 300 seconds.

[0171] 26. The molded body according to any one of embodiments 21 to 25, wherein the molded body has an average thickness in the range of from 0.1 to 30 cm.

[0172] 27. The molded body according to any one of embodiments 21 to 26, wherein the thermoplastic elastomer is a thermoplastic polyurethane with a Shore hardness in the range of from 70 A to 92 A.

[0173] 28. The molded body according to any one of embodiments 21 to 27, wherein in step (i), the crack-filling method is used.

[0174] 29. The molded body according to any one of embodiments 21 to 28, wherein no additives are added in step (i) or (ii) which can be stimulated through an electromagnetic field in a way which results in a rise of temperature in the mold.

[0175] 39. Use of the molded body according to any one of embodiments 1 to 6 or a molded body obtained or obtainable according to the process according to any one of embodiments 7 to 15 in shoe soles, part of shoe soles, shoe intermediate soles, shoe insoles, damping elements, cushioning elements, underlays, grips, flooring, mattresses, sporting goods, bicycle saddles, tires and in automotive interiors and exteriors.

[0176] 40. Molded body comprising expanded particles fused using an electromagnetic field, the expanded particles comprising a composition (C1) comprising a thermoplastic elastomer (TPE1) as component (M) and a thermoplastic polymer (TP1) as component (B1), wherein the composition (C1) has a factor JDIM: 15000

[0177] JDIM— — (tan 6t - 0,06) * ct' where i is the index for the components in the composition in the range of from 0.3 < JDIM< 3, wherein Tmis the melting temperature of (M) determined via DSC, measured based on DIN EN ISO 11357-3:2013 with a heating rate of 20 K / min and drying of test specimen for 10 minutes at 100°C under nitrogen before measurement start, determined in the first heating cycle at the point of max enthalpy at the first peak, tan5 is the energy dielectric loss factor measured at 27 MHz at 80°C of the components of the composition in according to DIN EN IEC 62631-2-2:2022, c is the concentration of the components of the composition as weight percentage, wherein the thermoplastic elastomer (TPE1) is a thermoplastic polyurethane.

[0178] 41. Process for the preparation of a molded body comprising expanded particles comprising a composition (C1), comprising the steps of

[0179] (i) loading the expanded particles comprising composition (C1) into a mold,

[0180] (ii) fusing the expanded particles comprising a thermoplastic elastomer by supplying energy at least partially through an electromagnetic field, wherein the composition (C1) comprises a thermoplastic elastomer (TPE1) as component (M) and a thermoplastic polymer (TP1) as component (B1), wherein the composition (C1) has a factor JDIM:

[0181] 15000

[0182] JDIM— — (tan 8i - 0,06) * ct' where i is the index for the components in the composition in the range of from 0.3 < JDIM< 3, wherein Tmis the melting temperature of (M) determined via DSC, measured based on DIN EN ISO 11357-3:2013 with a heating rate of 20 K / min and drying of test specimen for 10 minutes at 100°C under nitrogen before measurement start, determined in the first heating cycle at the point of max enthalpy at the first peak, tan5 is the energy dielectric loss factor measured at 27 MHz at 80°C of the components of the composition in according to DIN EN IEC 62631-2-2:2022, c is the concentration of the components of the composition as weight percentage, wherein fusing with electromagnetic radiation is achieved without the use of polar additives.

[0183] 42. Process for the preparation of a molded body comprising expanded particles comprising a composition (C1), comprising the steps of

[0184] (i) loading the expanded particles comprising composition (C1) into a mold,

[0185] (ii) fusing the expanded particles comprising a thermoplastic elastomer by supplying energy at least partially through an electromagnetic field, wherein the composition (C1) comprises a thermoplastic elastomer (TPE1) as component (M) and a thermoplastic polymer (TP1) as component (B1), wherein the composition (C1) has a factor JDIM:

[0186] 15000 v-

[0187] JDIM— — * > (tan 6t — 0,06) * ct where i is the index for the components in the composition in the range of from 0.3 < JDIM< 3, wherein Tmis the melting temperature of (M) determined via DSC, measured based on DIN EN ISO 11357-3:2013 with a heating rate of 20 K / min and drying of test specimen for 10 minutes at 100°C under nitrogen before measurement start, determined in the first heating cycle at the point of max enthalpy at the first peak, tanb is the energy dielectric loss factor measured at 27 MHz at 80°C of the components of the composition in according to DIN EN IEC 62631-2-2:2022, c is the concentration of the components of the composition as weight percentage, wherein no additives are added in step (i) or (ii) which can be stimulated through an electromagnetic field in a way which results in a rise of temperature in the mold.

[0188] 43. The process according to any one of embodiments 41 to 42, wherein the thermoplastic elastomer (TPE1) is a thermoplastic polyurethane.

[0189] 44. The process according to any one of embodiments 41 to 43, wherein the thermoplastic polymer (TP1) is selected from the group consisting of polyethylene and polystyrene. 45. The process according to any one of embodiments 41 to 44, wherein in step (ii) a voltage of 3 to 9 kV is applied for a duration of 1 to 300 seconds.

[0190] 46. The process according to any one of embodiments 41 to 45, wherein in step (i), the crackfilling method is used.

[0191] 47. Molded body obtainable or obtained by a process according to any one of embodiments 41 to 46.

[0192] 48. Use of the molded body obtained or obtainable according to the process according to any one of embodiments 41 to 46 in shoe soles, part of shoe soles, shoe intermediate soles, shoe insoles, damping elements, cushioning elements, underlays, grips, flooring, mattresses, sporting goods, bicycle saddles, tires and in automotive interiors and exteriors.

[0193] The invention is further described by examples. The examples relate to practical and in some cases preferred embodiments of the invention that do not limit the scope of the invention.

[0194] EXAMPLES

[0195] 1 Production of samples and reference materials

[0196] 1.1 Materials used

[0197] Blendpartner 1 commercially available polystyrene (PS 158 K by BASF SE)

[0198] Blendpartner 2 commercially available high molecular weight high density polyethylene (Lupolen 4261 AG by Lyondell Basell)

[0199] Blendpartner 3 commercially available polyamide (Ultramid flex F 38 by BASF SE)

[0200] Blendpartner 4 commercially available polyamide (Polyamid flex (PA6636) by BASF SE)

[0201] 1 ,4 BDO 1 ,4 butanediol

[0202] 1 ,6-HDO 1 ,6 hexanediol Xflex 2905 bi-functional cross-linker.

[0203] 1.2 TPU synthesis by extrusion

[0204] Following examples were prepared (see composition table 1):

[0205] The production of examples and references were carried out in a twin-screw extruder, ZSK58 MC, of the company Coperion with a process length of 48D (12 housings). The melt discharge from the extruder was carried out by a gear pump. After melting filtration, the polymer melt was processed by underwater granulation into granules, which were continuously dried in a heating vortex bed, at 40 - 90 ° C.

[0206] Polyol, chain extender and diisocyanate and, if necessary, a catalyst were dosed into the first zone. The supply of further additives, as described above, takes place in zone 8.

[0207] The housing temperatures are in the range 150 - 230 °C. The melt discharge and underwater pelletizing are carried out at melt temperatures of 210 - 245°C. The screw speed is between 180 and 240 1 / min. The throughput is in the range of 180 - 220 kg / h.

[0208] Table 1 : Quantities of the components of the thermoplastic materials dosed in the reaction extruder as example and reference (counterexamples) materials 1.4 TPU blends by compounding

[0209] The preparation of the following blend examples and blend counterexamples as summa- rized in tables 2a and b took place in a single-screw extruder, LabTech LE20-30, of the company LabTech Engineering Company LTD with 3-4 housings. The polymer melt was processed under water to receive a polymer strand.

[0210] The strand was crushed, and the resulting granules were used for injection molding.

[0211] Table 2a: Examples and references TPU blends

[0212] (*) comparative example Table 2b: Examples and references TPU blends

[0213] (*) comparative example

[0214] 1.5 ETPU by extrusion After the production of the starting materials, they were further processed into expanded thermoplastic polyurethane granulates as follows.

[0215] For this purpose, the dried sample and reference materials (see table 2a and b) were used in a twin screw extruder (ZE40, KraussMaffei Berstorff) with further additives (0.05 to 0.15 wt. % based on the weight of the polymer composition talc as nucleating agent and possibly a chain extender (0.6 to 1 .2 wt.% based on the weight of the polymer composition x-Flex 2905 MB, BASF Polyurethanes GmbH) mixed and melted in a temperature range of 160 °C to 220 °C.

[0216] As blowing agents, CO2 (1.1 to 2.2 wt.% based on the weight of the polymer composition) and N2 (0.1 to 0.25 wt.% based on the weight of the polymer composition )were injected into the melt in the extruder and mixed with the thermoplastic polyurethane and the other additives to form a homogenic melt.

[0217] The exact polymer composition of the individual examples and counterexamples is listed in Table 1 & 2. The melting mixture was then pressed via a gear pump (about 160-200 ° C depending on the material composition) into a perforated plate (about 180 - 200 ° C depending on the material composition) and cut in the cutting chamber of the underwater granulating (UWG) to granules and transported off with the tempered and pressurized water and expanded under water.

[0218] After separating the expanded granules from the water by means of a centrifugal dryer, the expanded granules are dried at 60 °C for 2 h. Molding of eTPU

[0219] The bead foams were molded using the Wave Foamer C from company Kurtz at a frequency of 27.14 MHz of the electromagnetic field (radio frequency molding) and a distance of the capacitor plates of 4,5 cm. The mold was prepared out of polyethyleneterephtalate with a length and width of 200 mm each and a variable height that can be set to 10 and 20 mm.

[0220] For molding, the cavity was opened, and the required amount of material (weighted before accurately) was homogeneously placed manually into one half of the open mold. Afterwards, the mold was closed to a height of 10 mm and the molding process started. The foam beads were radiated at a certain voltage for a certain time, afterwards a cooling step was done. Finally, the mold was opened again and the part was demolded.

[0221] The used amount of the bead foams (weight) and the used molding conditions are shown in Table 3. The plates were produced by adjusting the core of the mold to the final volume of 200 x 200 x 10 mm3(volume of 0.4 I). The manufacturing procedure was done as described above. The stabilization of the plates was done by a waiting time (passive cooling) according to the table below. Table 3

[0222] The examples and comparative examples in table 3 show that the molded bodies according to the present invention have a higher tensile strength than the comparative examples.

[0223] In table 4, further examples are summarized which show an effect of the parameter JDIM on the formation of stable molds. Table 4

[0224] 3. Methods used

[0225] 3.1 DSC

[0226] DSC is measured based on DIN EN ISO 11357-3:2013 with a heating rate of 20 K / min (drying of test specimen for 10 minutes at 100°C under nitrogen before measurement start) . The melting temperature is determined in the first heating cycle at the point of max enthalpy at the first peak.

[0227] 3.2 Tensile strength E-TPU

[0228] Measurement according to ASTM D 5035:2015, with test specimen (150X25,4X10 mm; stamped out of plate) at test velocity 100 mm / min.

[0229] 3.3 Part density

[0230] Density of foamed part out of thermoplastic polymer is determined based on DIN EN ISO 845:2009.

[0231] 3.4 Dielectric properties

[0232] For the values stated in the present invention, measurements were performed with an impedance analyzer (Keysight E4991 B) and a dedicated sample test fixture (16453A) that allows dielectric evaluation from 1 MHz-1GHz in a temperature range from -55°C to +150°C according to DIN EN I EC 62631-2-2:2022. The test fixture was placed in a laboratory oven to perform the dielectric characterization in the temperature range that is expected to occur during the molding process. Prior to the measurement the system was calibrated using an open, short, load (with PTFE) compensation. Literature cited

[0233] WO20 14 / 198779 A 1

[0234] WO2015 / 052265 A1

[0235] DE102013110242 A1

[0236] EP3698949 A1

[0237] WO2017 / 125410 A1

[0238] WO2017 / 125410 A1

[0239] EP3808522 A1

[0240] WO 2017 / 125410 A1

[0241] WO 2001 / 64414 A1

[0242] WO 2019 / 162172 A1

[0243] DE 102013 012 515 A1

[0244] WO 94 / 20568A1

[0245] WO 2007 / 082838 A1

[0246] WO20 17 / 030835 A 1

[0247] WO 2013 / 153190 A1

[0248] WO 2010 / 010010 A1

[0249] EP3405322A1

[0250] Kunststoffhandbuch [Plastics Handbook], volume 7, Polyurethane [Polyurethanes]”, Carl Hanser

[0251] Verlag, 3rd edition 1993, chapter 3.1

Claims

Claims1. Molded body comprising expanded particles fused using an electromagnetic field, the expanded particles comprising a composition (C1) comprising a thermoplastic elastomer (TPE1) as component (M) and a thermoplastic polymer (TP1) as component (B1), wherein the composition (C1) has a factor JDIM:15000 v-JDIM— — * (tan 6t - 0,06) * ct' where i is the index for the components in the composition in the range of from 0.3 < JDIM< 3, wherein Tmis the melting temperature of (M) determined via DSC, measured based on DIN EN ISO 11357-3:2013 with a heating rate of 20 K / min and drying of test specimen for 10 minutes at 100°C under nitrogen before measurement start, determined in the first heating cycle at the point of max enthalpy at the first peak, tan5 is the energy dielectric loss factor measured at 27 MHz at 80°C of the components of the composition in according to DIN EN I EC 62631-2-2:2022, c is the concentration of the components of the composition as weight percentage.

2. The molded body according to claim 1, wherein the thermoplastic elastomer (TPE1) is a thermoplastic polyurethane.

3. Process for the preparation of a molded body comprising expanded particles comprising a composition (C1), comprising the steps of(i) loading the expanded particles comprising composition (C1) into a mold,(ii) fusing the expanded particles comprising a thermoplastic elastomer by supplying energy at least partially through an electromagnetic field, wherein the composition (C1) comprises a thermoplastic elastomer (TPE1) as component (M) and a thermoplastic polymer (TP1) as component (B1), wherein the composition (C1) has a factor JDIM:15000JDIM(tanwhere i is the index for the components in the composition in the range of from 0.3 < JDIM< 3, wherein Tmis the melting temperature of (M) determined via DSC, measured based on DIN EN ISO 11357-3:2013 with a heating rate of 20 K / min and drying of test specimen for 10 minutes at 100°C under nitrogen before measurement start, determined in the first heating cycle at the point of max enthalpy at the first peak, tan5 is the energy dielectric loss factor measured at 27 MHz at 80°C of the components of the composition in according to DIN EN I EC 62631-2-2:2022, c is the concentration of the components of the composition as weight percentage.

4. The process according to claim 3, wherein fusing with electromagnetic radiation is achieved without the use of polar additives.

5. The process according to claim 3 or 4, wherein no additives are added in step (i) or (ii) which can be stimulated through an electromagnetic field in a way which results in a rise of temperature in the mold.

6. The process according to any one of claims 3 to 5, wherein the thermoplastic elastomer (TPE1) is a thermoplastic polyurethane.

7. The process according to any one of claims 3 to 6, wherein the thermoplastic polymer (TP1) is selected from the group consisting of polyethylene and polystyrene.

8. The process according to any one of claims 3 to 7, wherein in step (ii) a voltage of 3 to 9 kV is applied for a duration of 1 to 300 seconds.

9. The process according to any one of claims 3 to 8, wherein in step (i), the crack-filling method is used.

10. Use of expanded particles comprising a composition (C1) for the preparation of a molded body by fusing the particles by supplying energy at least partially through an electromagnetic field, wherein the composition (C1) comprises a thermoplastic elastomer (TPE1) as component (M) and a thermoplastic polymer (TP1) as component (B1), wherein the composition (C1) has a factor JDIM:15000JDIM(tanwhere i is the index for the components in the composition in the range of from 0.3 < JDIM< 3, wherein Tmis the melting temperature of (M) determined via DSC, measured based on DIN EN ISO 11357-3:2013 with a heating rate of 20 K / min and drying of test specimen for 10 minutes at 100°C under nitrogen before measurement start, determined in the first heating cycle at the point of max enthalpy at the first peak, tanb is the energy dielectric loss factor measured at 27 MHz at 80°C of the components of the composition in according to DIN EN I EC 62631-2-2:2022, c is the concentration of the components of the composition as weight percentage.

11. Molded body obtainable or obtained by a process according to any one of claims 3 to 9.

12. Use of the molded body according to claim 1 or 2 or a molded body obtained or obtainable according to the process according to any one of claims 3 to 9 in shoe soles, part of shoe soles, shoe intermediate soles, shoe insoles, damping elements, cushioning elements, underlays, grips, flooring, mattresses, sporting goods, bicycle saddles, tires and in automotive interiors and exteriors.

Citation Information

Patent Citations

  • Method for manufacturing interior component of motor vehicle from foam particles, involves applying foam particles from retaining container to cavity, and thermally connecting foam particles with one another by inductive heating

    DE102013012515A1

  • Method for manufacturing molding part, involves conditioning expandable thermoplastic polyurethane-particle, dosing particle, filling mold, evaporating filled particle in mold, and remolding finished molding part

    DE102013110242A1

  • Method for manufacture of a plastic component, plastic component, and shoe

    EP3053732A1

  • Method and device for producing a particle foam part

    EP3405322A1

  • Method for manufacture of a plastic component, plastic component, and shoe

    EP3698949A1

Cited By

  • Method for producing particle foam moulded parts

    EP4729265A1