Improved tyre tread composition comprising silanes

The tyre tread composition combines diene rubber with carbon black or silica and a mercapto-sulphide silane blend to enhance abrasion and tear resistance, winter traction, and reduce rolling resistance, addressing the trade-offs in existing compositions and improving tyre mileage.

WO2024201514A1PCT designated stage expired Publication Date: 2024-10-03APOLLO TYRES LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
PCT/IN2024/050318
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-27
Filing Date
2024-03-26
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Current tyre tread compositions face a trade-off between abrasion resistance, cut and tear resistance, and rolling resistance coefficient (RRC), where improvements in one characteristic often deteriorate others, and there is a need for a composition that enhances mileage, abrasion resistance, cut and tear resistance, and winter traction performance without increasing RRC.

Method used

A tyre tread composition incorporating a combination of diene rubber, carbon black or silica as reinforcing fillers, and a specific blend of mercapto silane and sulphide silane coupling agents, with a silanes loading range of 1-8 phr, where 40-90% of the silanes are mercapto silane, to improve interaction between rubber and fillers, reducing hysteresis loss and maintaining low RRC.

Benefits of technology

The composition achieves improved mechanical properties, enhanced cut and tear performance, winter traction, and abrasion resistance while maintaining a low RRC, thereby increasing tyre mileage and performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure IMGF000008_0001
    Figure IMGF000008_0001
  • Figure IMGF000009_0001
    Figure IMGF000009_0001
  • Figure IMGF000009_0002
    Figure IMGF000009_0002
Patent Text Reader

Abstract

The present invention provides a tyre tread composition comprising a combination of at least a diene rubber, reinforcing fillers, and a combination of silanes consisting of at least a mercapto silane and at least a sulfide silane, which, at a particular loading dosage ratio improves the cut & tear performance, winter traction performance, and abrasion resistance of the tyre tread composition.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] IMPROVED TYRE TREAD COMPOSITION COMPRISING SILANES

[0002] FIELD OF THE INVENTION

[0003] The present invention relates to the field of rubber technology, in particular, a tyre tread composition comprising a combination of silanes as coupling agents.

[0004] BACKGROUND OF THE INVENTION

[0005] This section is intended to provide information relating to the field of the invention and thus, any approach or functionality described below should not be assumed to be qualified as prior art merely by its inclusion in this section.

[0006] Mileage of a tyre depends on its design, construction and compounding approaches. Tyre tread performance comprises different performance parameters such as, abrasion resistance, traction performance, and fuel efficiency, which collectively os called the “magic triangle” of a tyre. In addition, cut and tear performance is also a crucial parameter for predicting tyre life. With simultaneous improvement of abrasion resistance and cut and chip resistance, the overall mileage performance of a tyre increases. But there is a trade-off among these characteristics. Improvement in one particular characteristic causes a decrease in the other. A tyre tread composition possesses better abrasion resistance when its reinforcing index is higher, however it is detrimental to better cut and chip resistance. Thus, there is a requirement of higher cut and tear resistant compounds along with higher abrasion resistance without affecting the traction performance and fuel efficiency performance.

[0007] A reinforcing material is used in tyre tread compositions for improving the mechanical properties of the tyre. As a greener technology, silica as as carbon black substitute as a reinforcing filler has been used extensively in tyre compositions to improve the fuel efficiency of the tyre. However, silica alone as a filler is not effective in reduction of RRC (Rolling Resistance Coefficient) of the tyre tread due to the mismatch in polarity between rubber and silica. Hence, a coupling agent is required for interaction between rubber and silica filler. Silanes are one such coupling agents, which act as a bridging material as it has two reactive sites. One of the reactive sites (polar alkoxy group) interacts with the polar silica filler and another site (hydrocarbon part) interacts with the rubber. Therefore, due to an improvement in rubber to filler interaction mediated by the coupling agent, hysteresis loss is reduced for the rubber compound and fuel efficiency is increased. However, reduction of hysteresis loss is detrimental for better cut and tear performance . Generally, an improved cut and tear resistant compound has higher hysteresis loss, which increases the RRc level of tyre. Similar behavior is observed between traction performance and RRc, wherein improvement in traction performance deteriorates the RRc level.

[0008] Traditionally high surface area carbon black is used to improve the abrasion properties of tyre tread, but beyond the optimum loading of filler tear performance of the tyre deteriorates. However, it leads to higher hysteresis loss that in turn increases the rolling resistance of tyre. Furthermore, replacement of carbon black with silica filler reduces the abrasion resistance of tyre tread, while reduction in rolling resistance eventually favors better fuel efficiency. Another approach to improve tyre performance is reduction of crosslink density with smart compounding of curatives. But with this technology optimized performance level is not achieved in abrasion resistance that in turn affects the mileage of the tyre. Thus, an improved tyre tread composition with adequate selection of polymer, filler and coupling agents improves the cut & tear performance, and winter traction performance, without affecting the RRc.

[0009] There are traditionally known approaches to improve only the cut and tear performance like using higher reinforcing filler but with this approach hysteresis loss is increased in the rubber compound, which increases the RRc level thereby dropping the fuel efficiency in its service. Another approach is reduction of crosslink density with smart compounding of curatives. But with this technology, optimized performance level is not achieved in abrasion resistance that affects the mileage of the tyre. One of the approaches for providing an improved tyre tread composition is by the modification of cure technology. Although rubber compounds vulcanized by smart soft cure process provides tyre tread with improved cut and tear performance, however it increases the RRc. Another approach is using blends of elastomer matrices with conventional fillers. However, blending with synthetic rubber leads to the improvement in mileage with a known drawback of increasing RRc and reduction of cut & tear performance.

[0010] US20210363333 discloses a sulfiir-crosshnkable rubber mixture comprising a rubber blend composed of at least one solution-polymerized diene polymer A of high molecular weight and at least one solution-polymerized polymer B of low molecular weight; and a vulcanization system comprising at least one accelerator and elemental sulfur and / or at least one sulfur donor substance. The composition of the rubber mixture comprises a silane coupling agent, wherein the silane is either a mercapto silane (NXT) or a sulfide silane (TESPD).

[0011] US11261312 discloses a sulfur-crosslinkable rubber mixture comprising a rubber blend of a diene polymer A of high molecular weight and a polymer B of low molecular weight, at least one silica, and 1 to 20 phr of at least a silane coupling agent. The said rubber composition comprises either TESPT or TESPD as the silane coupling agent.

[0012] US20200377702A1 discloses a rubber mixture comprising at least one diene rubber, at least one silica, 1 to 30 phr of at least one silane A, and 0.5 to 30 phr of one silane B. The patent application discloses that silane A bonds to polymers on account of the polysulfidic Sx group or the reactive S-X group, while silane B has no sulfur atoms. Further, the rubber composition comprises 2 to 100 phr of natural rubber and the rubber composition thus disclosed improves the rolling resistance of the tyre.

[0013] US11015041B2 discloses a rubber blend comprising a solution-polymerized diene polymer A of high molecular weight, a solution-polymerized polymer B of low molecular weight, and fdlers. The patent discloses that the rubber mixture comprises a mixture of different silanes, wherein the silane coupling agents used may be 3 -mercaptopropyltriethoxy silane, TESPT, TESPT etc. The rubber composition comprises at least one blocked and / or unblocked mercaptosilane. Further, the patent discloses that the amount of coupling agent is preferably 0.1 to 20 phr.

[0014] There remains an unmet need to develop a tyre tread composition with a low rolling resistance coefficient that provides enhanced mileage and better performance of the tyres by improving the abrasion resistance, cut and tear resistance, and winter performance of the tyres.

[0015] SUMMARY OF THE INVENTION

[0016] This section is intended to introduce certain aspects of the disclosed method in a simplified form and is not intended to identify the key advantages or features of the present disclosure.

[0017] In an aspect of the present invention, there is provided a tyre tread composition comprising: at least a diene rubber selected from the group consisting of natural rubber, synthetic rubber, and combinations thereof; at least a reinforcing filler selected from the group consisting of carbon black, silica, and combinations thereof; and silanes comprising a combination of at least a mercapto silane and at least a sulphide silane, wherein silanes loading is in the range of 1-8 phr, and 40-90% of the silanes is at least a mercapto silane.

[0018] In another aspect of the present invention, there is provided a tyre comprising a tyre tread composition, said composition comprising: at least a diene rubber selected from the group consisting of natural rubber, synthetic rubber, and combinations thereof; at least a reinforcing filler selected from the group consisting of carbon black, silica, and combinations thereof; and silanes comprising a combination of at least a mercapto silane and at least a sulphide silane, wherein silanes loading is in the range of 1-8 phr, and 40-90% of the silanes is at least a mercapto silane.

[0019] DETAILED DESCRIPTION OF THE INVENTION

[0020] In the following description, for the purposes of explanation, various specific details are set forth in order to provide a thorough understanding of the embodiments of the present invention. It will be apparent, however, that the embodiments of the present invention may be practiced without these specific details. Several features described hereafter can each be used independently of one another or with any combination of other features. An individual feature may address only one of the problems discussed above. Some of the problems discussed above might not be fully addressed by any of the features described herein.

[0021] Definitions:

[0022] The following acronyms are used in the present description.

[0023] “CB” refers to Carbon Black;

[0024] “RRc” refers to Rolling Resistance Coefficient;

[0025] “NR” refers to natural rubber; and

[0026] “Tan5 / E” (Winter Traction Performance)”.

[0027] The present invention provides a tyre tread composition comprising: at least a diene rubber selected from the group consisting of natural rubber, synthetic rubber, and combinations thereof; at least a reinforcing filler selected from the group consisting of carbon black, silica, and combinations thereof; and silanes comprising a combination of at least a mercapto silane and at least a sulphide silane, wherein silanes loading is in the range of 1-8 phr, and 40-90% of silanes is at least a mercapto silane.

[0028] In an embodiment, 60-80% of silanes in the tyre tread composition is at least a mercapto silane. In a preferred embodiment, about 66% of silanes in the tyre tread composition is at least a mercapto silane. In a preferred embodiment, the ratio of loading amount of at least a mercapto silane to at least a sulphide silane is 2: 1. In an embodiment, silanes loading in the tyre tread composition is in the range of 2-5 phr. In a preferred embodiment, silanes loading in the tyre thread composition is 3 phr. In a preferred embodiment, mercapto silanes loading in the tyre tread composition is 2 phr and sulphide silanes loading in the tyre tread composition is 1 phr.

[0029] In an embodiment, the tyre tread composition comprises a combination of natural rubber and synthetic rubber, whereby, the synthetic rubber loading in the composition is in the range of 10 to 30 phr, and natural rubber loading in the composition is in the range of 70 to 90 phr. In a preferred embodiment, synthetic rubber loading in the composition is in the range of 10 to 20 phr, and natural rubber loading in the composition is in the range of 80 to 90 phr.

[0030] In embodiment, the reinforcing fdler, silica has BET surface of at least 75m2 / g. In an embodiment, reinforcing fdler carbon black has nitrogen surface area (N2SA) in the range of 40 to 145 m2 / g and Oil Absorption Number (OAN) in the range of 110 and 140 ml / lOOg. In another embodiment, the reinforcing fdler in the tyre tread composition is carbon black. In an embodiment, the reinforcing fdler in the tyre tread composition is silica. In an embodiment, the reinforcing fdler in the tyre tread composition is a combination of carbon black and silica. In an embodiment, carbon black loading in the tyre tread composition is in the range of 20 to 40 phr. In an embodiment, silica loading in the tyre tread composition is in the range of 20 to 40 phr. In an embodiment, where the reinforcing fdler is a combination of carbon black and silica, the ratio of carbon black to silica loading amount is 1 : 1. In an embodiment, where the reinforcing fdler is a combination of carbon black and silica, the ratio of carbon black to silica loading amount is > 1 : 1. In an embodiment, where the reinforcing fdler is a combination of carbon black and silica, the ratio of carbon black to silica loading amount is <1: 1.

[0031] In an embodiment, the mercapto silane is selected from the group consisting of Si363, 3- Octanoylthio-l-propyltriethoxysilane (NXT), and combinations thereof. In a preferred embodiment, the mercapto silane is Si363. In an embodiment, the sulphide silane is selected from the group consisting of bis(triethoxysilylpropyl) disulfide (TESPD), bis (triethoxysilylpropyl) tetrasulfide (TESPT), and combinations thereof. In a preferred embodiment, the sulfide silane is TESPD.

[0032] In a preferred embodiment, the tyre tread composition comprises natural rubber, carbon black, silica, at least a mercapto silane, and at least a sulphide silane. Carbon black loading in the tyre tread composition is 30 phr. Silica loading in the tyre tread composition is 20 phr. Silanes loading the tyre tread composition is 3 phr. The ratio of mercapto silane to sulphide silane loading in the tyre tread composition is 2: 1. The mercapto silane in the tyre tread composition is Si363. The sulphide silane in the tyre tread composition is TESPD.

[0033] In a preferred embodiment, the tyre tread composition comprises natural rubber, synthetic rubber, carbon black, silica, at least a mercapto silane, and at least a sulphide silane. Natural rubber loading in the tyre tread Composition is 90 phr. Synthetic rubber loading in the tyre tread composition is 10 phr. The synthetic rubber is polybutadiene rubber. Carbon black loading in the tyre tread composition is 30 phr. Silica loading in the tyre tread composition is 20 phr. Silanes loading the tyre tread composition is 3 phr. The ratio of mercapto silane to sulphide silane loading in the tyre tread composition is 2: 1. The mercapto silane in the tyre tread composition is Si363. The sulphide silane in the tyre tread composition is TESPD.

[0034] In a preferred embodiment, the tyre tread composition comprises natural rubber, synthetic rubber, carbon black, silica, at least a mercapto silane, and at least a sulphide silane. Natural rubber loading in the tyre tread Composition is 90 phr. Synthetic rubber loading in the tyre tread composition is 10 phr. The synthetic rubber is styrene butadiene rubber. Carbon black loading in the tyre tread composition is 30 phr. Silica loading in the tyre tread composition is 20 phr. Silanes loading the tyre tread composition is 3 phr. The ratio of mercapto silane to sulphide silane loading in the tyre tread composition is 2: 1. The mercapto silane in the tyre tread composition is Si363. The sulphide silane in the tyre tread composition is TESPD.

[0035] In an embodiment, the tyre tread composition is characterized by having Tan5 / E’ (Winter Traction Performance) value at - 25° C in the range of 0.80-1.20. In an embodiment, the tyre tread composition is characterized by having an abrasion loss of less than 0.30 mg / m. In an embodiment, the tyre tread composition is characterized by having a maximum strength for the Constrained Path Tear of up to 90N. In an embodiment, the tyre tread composition is characterized by having Tan5 / E’ (Winter Traction Performance) value at - 25° C in the range of 0.80-1.20, abrasion loss of less than 0.30 mg / m, and maximum strength for the Constrained Path Tear of up to 90N.

[0036] The present invention also provides a tyre comprising a tyre tread composition as substantially described herein. In an embodiment, the tyre is characterized by having RRc (Rolling Resistance Coefficient) value of less than or equal to 3.5n / kN.

[0037] While the preferred embodiments of the present invention have been described hereinabove, it should be understood that various changes, adaptations, and modifications may be made therein without departing from the spirit of the invention and the scope of the appended claims. It will be obvious to a person skilled in the art that the present invention may be embodied in other specific forms without departing from its spirit or essential characteristics. The described embodiments are to be considered in all respects only as illustrative and not restrictive.

[0038] The tyre tread composition of the present invention provides at least one or more of the following advantages:

[0039] Improvement in mechanical properties;

[0040] Better reinforcement; - Improved cut & tear performance, winter traction performance, abrasion resistance; and

[0041] Better Winter traction indicator

[0042] EXAMPLES The rheological and mechanical properties of the tyre tread composition of the present invention over conventional tyre tread compositions was evaluated based on the following tests and procedures as shown in Table 1 below.

[0043] Table 1: Tests and procedures.

[0044] Various different tyre tread formulations were prepared based on the process steps as shown in Table 2 below. Briefly, Step 1 involves preparation of master batch 1 comprising the following steps: addition of base rubber components in a mixer followed by mastication and mixing for 60s; addition of silica and silanes followed by mixing for 180s;

[0045] - maintaining the temperature for 330s followed by dumping the mixture to obtain master batch 1.

[0046] Step 2 involves preparation of master batch 2 comprising the following steps: addition of master batch 1 to a mixer followed by mixing for 45s; addition of carbon black fdler and mixing from 180s;

[0047] - mixing for 21 Os to obtain master batch 2.

[0048] Step 3 involves preparation of the final batch mix comprising the following steps: addition of curatives (sulfur, accelerator, retarder) to master batch 2 followed by mixing for 30s; dumping the final mixture and mixing for 180s to obtain the desired tyre tread composition.

[0049] Table 2:

[0050] Experiment 1 A reference tyre tread composition coded as R-NR-1 was prepared comprising natural rubber (NR) as the base rubber along with fdlers (carbon black and silica), and mercapto silane (Si363). The rheological properties, physical properties, and the constrained path tear strength of the said tyre tread composition was determined. For evaluation of the rheological and physical properties, the sample were cured at 160°C for 15 minutes. For evaluation of constrained path tear strength, the sample was cured at 160°C for 20 minutes.

[0051] Table 3: Tyre tread composition (reference) (R-NR-1)

[0052] Table 4: Rheological properties of R-NR-1

[0053] Table 5: Physical properties of R-NR-1

[0054] Table 6: Constrained path tear strength of R-NR-1

[0055] Experiment 2

[0056] A reference tyre tread composition coded as R-NR-2 was prepared comprising natural rubber (NR) as the base rubber along with fdlers (carbon black and silica), and sulfide silane (TESPD). The rheological properties, physical properties, and the constrained path tear strength of the said tyre tread composition was determined For evaluation of the rheological and physical properties, the sample was cured at 160°C for 15 minutes. For evaluation of constrained path tear strength, the sample was cured at 160°C for 20 minutes. Table 7: Tyre tread composition (reference) (R-NR-2)

[0057] Table 8: Rheological properties of R-NR-2

[0058] Table 9: Physical properties of R-NR-2 Table 10: Constrained path tear strength of R-NR-2

[0059] Experiment 3

[0060] A tyre tread composition coded as T-NR-1 was prepared comprising natural rubber (NR) as the base rubber along with fdlers (carbon black and silica), and a combination of mercapto silane (Si363) and sulfide silane (TESPD), whereby the loading ratio of mercapto silane to sulphide silane is in a ratio of 2: 1. The rheological properties, physical properties, and the constrained path tear strength of the said tyre tread composition were determined. For evaluation of the rheological and physical properties, the sample was cured at 160°C for 15 minutes. For evaluation of constrained path tear strength, the sample was cured at 160°C for 20 minutes.

[0061] Table 11: Tyre tread composition (T-NR-1)

[0062] Table 12: Rheological properties of T-NR-1

[0063] Table 13: Physical properties of T-NR-1

[0064] Table 14: Constrained path tear strength of formulation

[0065] Experiment 4

[0066] A tyre tread composition coded as T-NR-2 was prepared comprising natural rubber (NR) as the base rubber along with fillers (carbon black and silica), and a combination of mercapto silane (Si363) and sulfide silane (TESPD), whereby the loading ratio of mercapto silane to sulphide silane is in a ratio of 1:2. The rheological properties, physical properties, and the constrained path tear strength of the said tyre tread composition were determined. For evaluation of the rheological and physical properties, the sample was cured at 160°C for 15 minutes. For evaluation of constrained path tear strength, the sample was cured at 160°C for 20 minutes.

[0067] Table 15: Tyre tread composition (T-NR-2)

[0068] Table 16: Rheological properties of T-NR-2

[0069] As shown in Table 16, scorch time and optimum cure time were determined; and both minimum and maximum torque values have been reported. For evaluation of the different rheological properties, the samples were cured at 160°C for 15 minutes. Optimum cure time and maximum torque are slightly higher than R-NR-1. However, it is comparable to R-NR-2 and T-NR-1.

[0070] Table 17: Physical properties of formulation

[0071] Table 18: Constrained path tear strength of formulation The tyre composition of samples coded as R-NR-1, R-NR-2, T-NR-1, and T-NR-2 are compared side by side in Table 19 below.

[0072] Table 19: Comparison of rubber compound formulations

[0073] The rheological properties of the tyre composition of samples coded as R-NR-1, R-NR-2, T-NR- 1, and T-NR-2 are compared side .by side in Table 20 below.

[0074] Table 20: Comparison of rheological properties of rubber compound formulations

[0075] As seen in Table 20 above, while tyre composition R-NR-1 showed lower maximum torque and optimum cure time, in the case of tyre composition R-NR-2, maximum torque and optimum cure time are slightly increased. Tyre composition T-NR-1 and T-NR-2 both show similar cure characteristics as the reference tyre composition R-NR-2.

[0076] Table 21: Comparison of physical properties of rubber compound formulations

[0077] As seen in Table 21 above, the tyre composition T-NR-1, which has mercapto silane to sulphide silane in 2: 1 loading ratio, shows comparable Modulus as that of tyre composition R-NR-1 (only mercapto silane). Tyre composition T-NR-2, which has mercapto silane to sulphide silane in 1:2 loading ratio, shows marginally lower Modulus as compared to that of tyre composition R-NR-2 compound (only sulfide silane).

[0078] Table 22: Comparison of constrained path tear strength of rubber compound formulations

[0079] As seen in Table 22 above, tyre composition T-NR-1, which has mercapto silane to sulphide silane in 2: 1 loading ratio, shows improved tear strength as compared to tyre composition R-NR-1, which has only mercapto silane. Tyre composition T-NR-1 also shows further improved tear strength as compared to tyre composition R-NR-2, which has only sulphide silane. Unexpectedly and surprisingly, comparing R-NR-1, R-NR-2, and T-NR-1, it can be appreciated that even though sulphide silane in R-NR-2 provides inferior tear strength as compared to mercapto silane in R-NR- 1, partially substituting mercapto silane with sulphide silane provides better tear strength as seen in T-NR-1. Furthermore, unexpectedly and surprisingly, T-NR-1 also shows improved tear strength as compared to tyre composition T-NR-2, which also comprises mercapto silane and sulphide silane, however, the loading ratio is 1:2.

[0080] Table 23: Comparison of dynamic properties of rubber compound formulations at -25°C

[0081] As seen in Table 23 above, reference tyre compound R-NR-2 comprising sulphide silane shows higher E’ index value as compared to that of tyre compound R-NR-1 comprising mercapto silane, suggesting that mercapto silane is a better choice of silane. However, unexpectedly and surprisingly, in tyre compound T-NR-1 comprising mercapto silane and sulphide silane in 2: 1 loading composition, partial replacement of mercapto silane with sulphide silane results in a further decrease in E’ index as compared to tyre compound R-NR-1. This decrease in E’ index is specific to a combination of mercapto silane and sulphide silane where loading ratio of mercapto silane to sulphide silane is >1: 1 as in T-NR-2, where the ratio is <1: 1, particularly 1:2, the E’ index value is considerably higher than even R-NR-2 which only has sulphide silane. A similar pattern can also be seen in the case of Tan5 / E', except that in case of Tan5 / E', a higher value is desirable, which is indicative of superior winter traction performance. Table 24: Comparison of dynamic properties of rubber compound formulations at 70°C

[0082] As seen in Table 24 above, tyre compound T-NR-1 shows improvement (higher) in dynamic modulus as compared to reference tyre compound R-NR-1, and T-NR-2.

[0083] Table 25: Comparison of LAT 100 abrasion resistance of rubber compound formulations

[0084] As seen in Table 25 above, while tyre compound T-NR-1 shows superior LAT 100 index (indicative of tyre service life) as compared to reference tyre compound R-NR-2, and as compared to T-NR-2, however, it is lower than that of reference tyre compound R-NR- 1.

[0085] Higher sulfide silane and lower mercapto silane is inferior for abrasion resistance. Though tyre compound R-NR-1 having only mercapto silane showed higher LAT 100 index, but dynamic modulus was inferior as compared to T-NR-1. Thus, tyre compound T-NR-1 shows overall better dynamic abrasion properties as against other combination of silanes.

[0086] Experiment 5

[0087] Tyre tread composition coded as T-NR-4 was prepared having composition similar to that of T- NR-1, except for having higher carbon black loading (40 phr instead of 30 phr).

[0088] Table 26: Comparison of rubber compound formulation

[0089] Table 27: Comparison of rheological properties of formulations at 160°C, 15 mins

[0090] As seen from Table 27, higher carbon black loading in tyre compound T-NR-4 results in increase in maximum torque, while the optimum cure time is slightly reduced.

[0091] Table 28: Comparison of constrained path tear strength of rubber formulations (cured at 160°C, 20 mins)

[0092] As seen in Table 28 above, it can be inferred that the cut and tear performance is improved in tyre formulation T-NR-4, which has higher loading of carbon black (30% more) as compared to tyre compound T -NR- 1.

[0093] Table 29: Comparison of LAT 100 abrasion resistance

[0094] As seen from Table 29 above, increased carbon black loading loads to better abrasion resistance, which is likely due to better dispersion of the fdler in the rubber matrix.

[0095] Experiment 6

[0096] The tyre tread composition coded T-NR-3 was prepared having composition comprising natural rubber, carbon black, silica, mercapto silane, and sulphide silane. Compared to tyre compound T- NR-2, which has total fdler loading of 50 phr (30 phr carbon black and 20 phr silica), the tyre compound T-NR-3 has a total filler loading of 60 phr (20 phr carbon black and 40 phr silica). The silanes loading in T-NR-3 is also more. Mercapto silane loading is 2.5 phr, while sulphide silane loading is 3.5 phr (higher amount of sulphide silane than mercapto silane).

[0097] Table 30: Comparison of rubber compound rubber formulation

[0098] Table 31: Comparison of physical properties of rubber formulations

[0099] For evaluation of different physical properties, the tyre compounds were cured at 160°C for 15 minutes. As seen in Table 31, an improvement in hardness and modulus is observed in T-NR-3 compound due to the higher fdler loading. Table 32: Comparison of constrained path tear strength of rubber formulations

[0100] For evaluation of constrained path tear strength to determine the cut and tear performance, the samples were cured at 160°C for 20 minutes. As seen from table 32, it can be inferred that increased sulfide silane and lower mercapto silane dosage reduces the constrained path tear strength.

[0101] The dynamic properties of the rubber formulation T-NR-3 was measured at -25°C at 0.23% dynamic strain, and at 70°C. The dynamic properties of the rubber formulation T-NR-3 were measured at varying temperatures and a comparison of the dynamic properties of T-NR-2 and T- NR-3 has been summarized in Tables 33 and 34 below respectively.

[0102] Table 33: Comparison of dynamic properties of the different rubber formulations at -25°C

[0103] As seen from Table 33 above, the tyre compound T-NR-3 shows higher E’ index value as compared to T-NR-2, which is undesirable. Tyre compound T-NR-3 also shows lower Tan5 / E' value (winter traction performance) than T-NR-2, which is also undesirable.

[0104] Table 33: Comparison of dynamic properties of the different rubber formulations at 70°C

[0105] As seen from Table 34, the tyre compound T-NR-3 shows higher dynamic modulus, which is due to higher fdler loading.

[0106] The abrasion resistance of the rubber compound formulation T-NR-3 was determined and was compared with that of T-NR-2. Table 35 shows a comparison of the abrasion resistance of the two rubber compound formulations.

[0107] Table 35: Comparison of LAT 100 Abrasion resistance of different rubber formulations

[0108] As seen from Table 35, the abrasion resistance property of T-NR-3 is inferior than that of T-NR- 2, likely because of higher dosage of sulphide silane.

[0109] Experiment 7

[0110] 4 different tyre tread composition were prepared, each having a combination of natural rubber (90 pbr loading) and polybutadiene rubber (10 phr loading); carbon black loading of 30 phr, silica loading of 20 phr, and varying silanes.

[0111] Table 36: Comparison of rubber compound formulations comprising natural rubber and polybutadiene rubber

[0112] Table 37: Comparison of rheological properties of rubber compound formulations

[0113] For evaluation of the different rheological properties, the samples were cured at 160°C for 15 minutes. As seen in Table 37 above, the trends with regard to effect to silanes was comparable to compositions comprising only natural rubber, or in other words, change in rubber composition did not affect the effect of silanes on rheological properties of the tyre compounds.

[0114] Table 38: Comparison of physical properties of rubber formulations

[0115] Forevaluation ofthe different physical properties, the samples were cured at 160°C for 15 minutes. As seen in Table 38 above, tyre formulation R-BR-1 which contains only mercapto silane shows lower hardness and modulus. Tyre formulation R-BR-2 which contains only sulfide silane shows higher hardness and modulus. Tyre compound T-BR-1 (higher mercapto silane and lower sulfide silane), shows an improvement in hardness and modulus compared to tyre formulation R-BR- 1. Tyre compound T-BR-2 shows comparable hardness and M300 modulus to tyre compound R-BR- 2.

[0116] Table 39: Constrained path tear strength of formulation

[0117] For evaluation of constrained path tear strength to determine the cut and tear performance, the samples were cured at 160°C for 20 minutes. As seen from Table 39, it can be readily inferred that a significantly higher cut and tear performance is observed in the case of tyre compound T-BR- Iwhich comprises mercapto silane and sulphide silane in 2: 1 loading ratio. In contrast, tyre compound T-BR-2 compound which contains higher sulfide silane and lower mercapto silane, shows inferior cut and tear performance. Surprisingly, while tyre compound R-BR-1 which has mercapto silane shows a lower tear strength than tyre compound R-RB-2 which has sulphide silane, partial substitution of mercapto silane with sulphide silane as in tyre compound T-BR-1 unexpectedly increases the tear strength even more than that of tyre compound R-BR-2. Further, as seen previously, where the loading ratio of mercapto silane to sulphide silane is < 1: 1 (particularly 1:2), similarly, as seen in tyre formulation T-BR-2, the tear strength characteristic is inferior.

[0118] The dynamic properties of the rubber formulations comprising the combination of synthetic and natural rubber was measured at -25°C at 0.25% dynamic strain, results of which are summarized in Table 40 below.

[0119] Table 40: Comparison of dynamic properties of the different rubber formulations at -25°C

[0120] As seen from Table 40, tyre compound R-BR-1 comprising mercapto silane shows higher Tan5 / E' than tyre compound R-BR-2 comprising sulphide silane. It would be expected that substitution of mercapto silane with sulphide silane would reduce the Tan5 / E' value of R-BR- 1 further. However, unexpectedly and surprisingly, tyre compound T-BR-1, which has mercapto silane and sulphide silane in 2: 1 loading ratio shows higher Tan5 / E'. In contrast, tyre compound T-BR-2, which has mercapto silane and sulphide silane in 1:2 loading ratio shows lower Tan5 / E' than R-BR-1 alone, which has only mercapto silane.

[0121] The abrasion resistance of the different rubber compound formulations was also determined, which is summarized in Table 41 below.

[0122] Table 41: Comparison of LAT 100 Abrasion resistance of different rubber formulations

[0123] As seen from Table 41 above, tyre compound R-BR-1 which has only mercapto silane shows higher LAT 100 index value compared to tyre compound R-BR-2, which has only sulphide silane. It would be expected that replacing mercapto silane of R-BR-1 with sulphide silane would reduce the LAT 100 index value. However, contrary to the expectation, as seen in tyre formulation T-BR- 1, a combination of mercapto silane and sulphide silane at 2: 1 loading ration shows higher LAT 100 index value. In contrast, tyre formulation T-BR-2 which has a combination of mercapto silane and sulphide silane at 1:2 loading ratio does not show a significant increase in LAT 100 index. In fact, it is comparable to tyre formulation R-BR-2.

[0124] Experiment 8

[0125] Similar to Experiment 7, 4 different tyre tread compositions were prepared, the difference being that the synthetic rubber is styrene butadiene rubber.

[0126] Table 42: Comparison of rubber compound formulations comprising natural rubber and styrene butadiene rubber

[0127] Table 43: Comparison of rheological properties of rubber compound formulations

[0128] For evaluation of the different rheological properties, the samples were cured at 160°C for 15 minutes. As per Table 43, the results are similar to that reported for rubber compounds comprising natural rubber and polybutadiene rubber. Table 44: Comparison of Physical properties of rubber formulations

[0129] Forevaluation ofthe different physical properties, the samples were cured at 160°C for 15 minutes.

[0130] As seen in Table 44 above, tyre compound R-SBR-1 compound comprising only mercapto silane shows lower hardness and modulus, whereas R-SBR-2 compound comprising only sulfide silane shows higher hardness and modulus. However, in the case of tyre formulation T-SBR-1, the modulus and hardness is improved as compared to tyre formulation R-SBR-1.

[0131] Table 45: Constrained path tear strength of rubber formulations

[0132] For evaluation of constrained path tear strength to determine the cut and tear performance, the samples were cured at 160°C for 20 minutes. Similar to the trend in the case of tyre compound comprising natural rubber and polybutadiene rubber, in the present instance also, higher cut and tear performance was observed in tyre compound T-SBR-1 compound and lower cut and tear performance in T-SBR-2.

[0133] The dynamic properties of the rubber formulations comprising a combination of styrene butadiene rubber and natural rubber was measured at -25 °C, which is summarized in Table 46.

[0134] Table 46: Comparison of dynamic properties of rubber formulations at -25 °C

[0135] As seen in Table 46, the tyre compound T-SBR-1 shows comparable winter tyre performance as tyre compound R-SBR-1, and better than tyre compound R-SBR-2 which comprises only sulphide silane.

[0136] The abrasion resistance of the different rubber compound formulations was also determined. Table 47 shows a comparison of the abrasion resistance of the different rubber compound formulations. Table 47: Comparison of LAT 100 Abrasion resistance of rubber formulations As seen in Table 47 above, tyre formulation T-SBR-1, which comprises higher mercapto silane and lower sulfide silane performed better in abrasion resistance as compared to tyre compound comprising higher sulfide silane and lower mercapto silane (T-SBR-2).

[0137] Overall, these data show that the combination of mercapto silane and sulphide silane, particularly where the loading ratio of mercapto silane to sulphide silane is >1: 1, more particularly 2: 1, unexpectedly and surprisingly shows superior desirable tyre composition characteristics. These effect are not an effect of a mere mixing of silanes as higher loading ratio of sulphide silane over mercapto silane in fact leads to degradation of the characteristics. This enhancement is also apparent over the presence of mercapto silane or sulphide silane alone.

Claims

I / We claim:

1. A tyre tread composition comprising:- at least a diene rubber selected from the group consisting of natural rubber, synthetic rubber, and combinations thereof;- at least a reinforcing filler selected from the group consisting of carbon black, silica, and combinations thereof; and silanes comprising a combination of at least a mercapto silane and at least a sulphide silane, wherein silanes loading is in the range of 1-8 phr, and 40-90% of silanes is at least a mercapto silane.

2. The tyre tread composition as claimed in claim 1, wherein the ratio of loading amount of at least a mercapto silane to at least a sulphide silane is 2: 1.

3. The tyre tread composition as claimed in claim 1, wherein at least a diene rubber comprises a combination of natural rubber and synthetic rubber, the synthetic rubber loading in the composition is in the range of 10 to 30 phr, and natural rubber loading in the composition is in the range of 70 to 90 phr.

4. The tyre tread composition as claimed in claim 3, wherein synthetic rubber loading in the composition is in the range of 10 to 20 phr, and natural rubber loading in the composition is in the range of 80 to 90 phr.

5. The tyre tread composition as claimed in claim 1, wherein silica has BET surface of at least 75m2 / g.

6. The tyre tread composition as claimed in claim 1, wherein carbon black has nitrogen surface area (N2SA) in the range of 40 to 145 m2 / g and Oil Absorption Number (OAN) in the range of 110 and 140 ml / lOOg.

7. The tyre tread composition as claimed in claim 1, wherein the carbon black loading in the composition is in the range of 20 to 40 phr.

8. The tyre tread composition as claimed in claim 1, wherein silica loading in the composition is in the range of 20 to 40 phr.

9. The tyre tread composition as claimed in claim 1, wherein at least a reinforcing fdler comprises a combination of carbon black and silica, and the ratio of carbon black to silica loading amount is one of 1: 1, > 1: 1, or <1: 1.

10. The tyre tread composition as claimed in claim 1, wherein at least a mercapto silane is selected from the group consisting of Si363, 3-Octanoylthio-l-propyltriethoxysilane (NXT), and combinations thereof.

11. The tyre tread composition as claimed in claim 1, wherein at least a sulphide silane is selected from the group consisting of bis(triethoxysilylpropyl) disulfide (TESPD), bis (triethoxysilylpropyl) tetrasulfide (TESPT), and combinations thereof.

12. The tyre tread composition as claimed in claim 1, characterized by at least one of having Tan5 / E’ (Winter Traction Performance) value at - 25° C in the range of 0.80-1 .20; having an abrasion loss of less than 0.30 mg / m; or having a maximum strength for the Constrained Path Tear of up to 90N.

13. A tyre comprising a tyre tread composition as claimed in claim 1.

14. The tyre as claimed in claim 13, characterized by having RRc (Rolling Resistance Coefficient) value of less than or equal to 3.5n / kN.

15. The tyre tread composition as claimed in claim 1 for use in a tyre.

Citation Information

Patent Citations

  • Rubber blend, sulfur-crosslinkable rubber mixture, and vehicle tire

    US11015041B2

  • Rubber blend, sulfur-crosslinkable rubber mixture, and vehicle tire

    US11261312B2

  • Sulfur-crosslinkable rubber mixture, vulcanizate of the rubber mixture, and vehicle tire

    US20200377702A1

  • Rubber blend, sulfur-crosslinkable rubber mixture, and vehicle tire

    US20210363333A1

  • Rubber composition for tire

    EP3470458A1