High entropy oxides and method of preparation by electric arc fusion

The electric arc fusion method addresses the challenge of scalable bulk production of high entropy oxides by achieving stable lattice formation in high entropy oxides, enabling their application in abrasives and refractories through equi-atomic mixing and fusion at high temperatures, resulting in a stable fluorite crystal structure.

WO2024201532A1PCT designated stage expired Publication Date: 2024-10-03CARBORUNDUM UNIVERSAL LIMITED

Patent Information

Application Number
PCT/IN2024/050339
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2024-03-30
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Existing methods for synthesizing high entropy oxides face challenges in achieving scalable bulk production while maintaining a stable, single-phase structure, as high temperature diffusion methods are difficult to scale and can result in non-stoichiometric oxides due to exposure to the atmosphere, disrupting lattice formation.

Method used

The electric arc fusion method is used to synthesize high entropy oxides by mixing ceramic oxides in equi-atomic quantities, followed by pelletization, air drying, and fusion in an electric arc furnace at temperatures exceeding 2000°C, allowing for stable lattice formation and scalability to commercial bulk production.

Benefits of technology

This method promotes homogeneity and stability of the high entropy oxide phase, enabling its use in abrasive and refractory applications, with the ability to maintain a stable fluorite crystal structure across different cooling modes and heat treatments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure IN2024050339_03102024_PF_FP_ABST
    Figure IN2024050339_03102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention provides high entropy oxide (HEO) and a method for preparing the same by electric arc fusion method. HEO prepared by this invention may be used in abrasive industry, coated and bonded, blasting abrasive applications and for high temperature thermal resistance coating applications.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] HIGH ENTROPY OXIDES AND METHOD OF PREPARATION BY

[0002] ELECTRIC ARC FUSION

[0003] TECHNICAL FIELD

[0004] The present application relates to multi-component oxide for abrasive applications designed and synthesized using high entropy concept. The application also relates to the bulk powder synthesis of high entropy oxide (HEO) powders by electric arc fusion route.

[0005] BACKGROUND AND PRIOR ART

[0006] Discovering new material systems to cater the advanced application needs has always been the fundamental driving force in the material science field. The most traditional method of making new materials is by mixing two components or alloying. The mixture can yield properties average or superior than the individual components or it can show complete new set of properties. The discovery of high entropy alloys (HEAs) proposed by Yeh et al in Advanced Engineering Materials, 6 (2004) 299-303 opened richer compositional space to design and develop new materials. HEAs generally have five or more principal elements with equi-atomic or newer equi-atomic concentrations and therefore associated with larger configurational entropy. In multicomponent systems like HEA, high entropy can lead to unique attributes including stabilisation of single -phase solid solution with simple crystal structure and collection of properties surpassing the individual constituents in the system.

[0007] High entropy ceramics (HEC) are derived from the field of HEAs. Like HEAs, HECs are also composed of multiple component elements which form a single phase, and their formation is due to their high conformational entropy. The advantage of HECs is their structural diversity. HECs have a crystal structure composted of a cation sub-lattice and an anion sub-lattice, which enables the coexistence of cations and anions in the same crystal structure, thereby increasing configurational entropy. However, HECs gained much attention when High Entropy Oxide system (Mg, Co, Ni, Cu, Zn)O with high configurational entropy with single phase rock salt crystal structure was prepared. Since then, borides, carbides, silicides, zirconates, phosphates, and niobates have been extensively investigated. HEO basically contains one cation sub-lattice with five or more metals and oxygen sub-lattice which together form single phase oxide solid solution. HEOs have severe lattice distortion and lattice defects due to the non-stoichiometry in oxygen sub-lattice. This reduces thermal conductivity and increases the toughness of the material. Hence, HEOs are considered for high temperature applications.

[0008] Although theoretically HEC sound very tempting it has its own challenges when it comes to synthesis. To achieve a single -phase solid solution of HEC, diffusion at the atomic scale is very much essential. Diffusivity of the atoms exponentially increases with the temperature. Generally, the constituent elements in HEC systems are ceramics which possess very high melting points. Therefore, to achieve high diffusion rate in these systems high temperature is needed. The most common synthesis methods of HEC reported so far are solid state reaction, wet chemical route for powder synthesis and solidification, field assisted sintering or spark plasma sintering to make sintered compacts. In wet chemical synthesis flame pyrolysis, hydrothermal synthesis, sol-gel method, combustion synthesis are widely used. In solid state synthesis, the most used process is ball milling of the powders followed by spark plasma sintering or conventional sintering at high temperatures.

[0009] The first ever patent application on high entropy alloys was US20020159914 filed by Yeh Jien-Wei which defined high entropy multicomponent alloys and explained the concept of high entropy. High entropy multi-component alloy was made using 5 to 11 metallic elements from beryllium, magnesium, aluminium, scandium, titanium, vanadium, chromium, manganese, iron, cobalt, nickel, copper, zinc, yttrium, zirconium, niobium, molybdenum, ruthenium, rhodium, palladium, silver, hafnium, tantalum, tungsten, platinum, gold, lanthanum, cerium, praseodymium, neodymium, samarium, europium, gadolinium and terbium. The alloy was melted in an electric arc furnace followed by a rapid solidification process. According to the claims, the basic characteristic of the high entropy alloy was very high hardness, very high heat resistance and very high corrosion resistance.

[0010] Chinese patent no. CN113185305B, has disclosed preparation of high temperature heat insulation high entropy oxide preparation by sol-gel chemical synthesis. The chemical formula of the system is (Hf Zr Ce T Al) which has good high temperature thermal stability, phase stability and heat insulating property. The method includes preparation of precursor followed by drying to make a gel and heat treatment of the gel at 900-1600°C for 24 hours to obtain HEO. The molar ratio of hafnium tetrachloride to zirconium oxychloride octahydrate to cerium nitrate hexahydrate to yttrium nitrate hexahydrate to an aluminium source is 0.15-0.3: 0.15-0.3: 0.15-0.3: 0.05-0.3: 0.05-0.3.

[0011] Prior art US20220134616, Chou et al, reported synthesis of high surface area of HEO using sol-gel method. The composition of the HEO contains metal cations from the first row of the transition metals with oxygen anions in equi-molar ratio. In this sol-gel method, polymeric complex agent is dissolved in water to form aqueous solution. Then the metal salts are dissolved in the aqueous solution followed by drying to form a gel. The gel is subjected to calcination in oxygen atmosphere to form high surface area HEO in a single-phase fluorite lattice structure.

[0012] CN 112340787 discloses a formation of single -phase spinel type high entropy using sol-gel combustion method. The high entropy oxide material system used in this invention contains five transition metals Co, Cr, Fe, Mn, Ni and Zn is used to replace any one of the Co, Cr, Fe, Mn, Ni metal cations. In the preparation method, five out of the six nitrides are taken in equal quantity and mixed with glycine followed by blast drying in oven to form a viscous gel. Then the gel is heat treated in a muffle furnace at 850°C to obtain single phase spinel type HEO. CN 115093214 discloses a high entropy oxide method by ball milling and sintering route. In this invention, ultra-fast synthesis of HEO is reported using joule heating device which has an extremely high heating rate and very high temperature upper limit. The material system taken was widely studied among the HEO system, i.e. (Mgo.2Coo.2Nio.2Cuo.2Zno.2)02. Prior to the sintering, all the metal oxides are subjected to ball milling for 2 hours for homogenisation of the powders.

[0013] CN109987935 discloses synthesis of fluorite type (Zr Hf Ce Ti Zn)O2 HEO system by ball milling and sintering route. According to the invention, the first step is to mix the all five oxide powders in equi-molar ratio and subjected to high energy ball mill for 10-30 hours. In the second step the powder is filled in a graphite mould and subjected to sintering at 1200-1600°C in a discharge plasma furnace to obtain a high-energy ceramic block.

[0014] CN 114618503 discloses a HEO material designed for oxygen storage material. The HEO precursor material is synthesized by hydrothermal method. To prepare the precursor, all the metal nitrates are mixed with a complex agent preferably citric acid. The metal nitrates include rare earth nitrates and / or transition metal nitrates. The hydrothermal reaction of the prepared solution is carried out at 100-120°C for 1-5 hours. Finally, the reacted solution was subjected to calcination at 400-600°C to obtain a high entropy oxide oxygen storage material. In the second part of the invention, it is claimed that the synthesized HEO mainly composed of meso-pores which is very beneficial for heterogenous catalytic reaction.

[0015] Though the prior arts disclose single phase HEO by sintering methods which involves solid to solid high temperature diffusion, it is difficult to scale such methods to bulk production. Moreover, HEO systems contains anions and cations in which during fusion, due to the exposure to atmosphere, some of the oxides can evaporate based on the local partial pressure. It can create non stoichiometric oxides with oxygen vacancies. These changes during fusion may disrupt the single crystal lattice formation. Hence, the HEO system must be chosen to from a single high entropy oxide phase after solidification.

[0016] Thus, it is an object of the present invention to provide for a method which offers more homogeneity and is scalable to commercial bulk manufacturing. It is also an object of the present invention to provide for high entropy oxide which form a stable, single high entropy phase after fusion.

[0017] SUMMARY OF THE INVENTION

[0018] Accordingly, the present invention provides high entropy oxide (HEO) and a method for preparing the same by electric arc fusion method.

[0019] BRIEF DESCRIPTION OF ACCOMPANYING DRAWINGS

[0020] The various aspects of the present invention will be apparent and more readily appreciated from the following description of the example embodiment taken in conjunction with the accompanying drawings in which:

[0021] Figure 1 represents the particle size distribution of the raw materials used in the present invention;

[0022] Figure 2 represents the X-ray diffraction patters of the a) raw material and HEO in ultra-fast, fast and normal modes; b) HEO heat treated samples.

[0023] Figure 3 represents the BSE-SEM image taken on the polished grain surface of the samples a) HEO-pot mode; b) HEO heat treated at 1600°C for 5 hours.

[0024] DETAILED DESCRIPTION OF INVENTION

[0025] For the purposes of the following detailed description, it is to be understood that the invention may assume various alternative variations and step sequences, except where expressly specified to the contrary. Moreover, other than in any operating examples, or where otherwise indicated, all numbers expressing, for example, quantities of ingredients used in the specification are to be understood as being modified in all instances by the term "about”. It is noted that, unless otherwise stated, all percentages given in this specification and appended claims refer to percentages by weight of the total composition.

[0026] The use of examples anywhere in this specification including examples of any terms discussed herein is illustrative only, and in no way limits the scope and meaning of the invention or of any exemplified term. Likewise, the invention is not limited to various embodiments given in this specification.

[0027] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. In the case of conflict, the present document, including definitions will control. It must be noted that, as used in this specification and the appended claims, the singular forms “a, ” “an" and “the" include plural referents unless the content clearly dictates otherwise. Thus, for example, reference to a “solvent" may include two or more such solvents. The terms “preferred" and “preferably ” refer to embodiments of the invention that may afford certain benefits, under certain circumstances. However, other embodiments may also be preferred, under the same or other circumstances. Furthermore, the recitation of one or more preferred embodiments does not imply that other embodiments are not useful, and is not intended to exclude other embodiments from the scope of the invention.

[0028] As used herein, the terms “comprising", “including", “having", “containing", “involving", and the like are to be understood to be open-ended, i.e., to mean including but not limited to.

[0029] Unless defined otherwise, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which the invention pertains. It is also to be understood that the terminology used herein is for the purpose of describing a particular embodiment of the invention only, and is not intended to limit the scope of the invention in any manner. Thus, before describing the present invention in detail, it is to be understood that this invention is not limited to the following embodiment. The description of a particular embodiment and examples provided herein are only for the purpose of illustration and does not limit the scope of the invention to a particular embodiment.

[0030] In one aspect, the present invention provides a multicomponent High Entropy Oxide (HEO) having high configurational entropy, said HEO comprises at least one or more individual ceramic oxide selected from the group comprising Alumina (AI2O3), Zirconium oxide (ZrO2), Titanium oxide (TiO2), Yttrium oxide (Y2O3), chromium oxide (CT2O3). silicon dioxide (SiO2) and Hafnium oxide (HfO2). The HEO has equi-atomic or near equi-atomic concentrations of the individual ceramic oxide.

[0031] Fig.l and table 1 shows the particle distribution and chemistry of the individual ceramic oxides. HEO has fluorite-type crystal structure in which said structure is a face-centered cubic structure with cations occupying the regular sites and oxygen anions occupying tetrahedral voids. HEO is represented by the molecular formula AlZrTiYCr)O. This high entropy ceramic oxide may have applications in abrasives and refractories.

[0032] In another aspect, the present invention provides for A process for preparing a multicomponent High Entropy Oxide (HEO) having high configurational entropy, comprising the steps of - a) mixing one or more individual ceramic oxides in equi-atomic quantities; b) pelletizing the mix of 3-5 mm size with addition of water and air drying for 12 hours at 150°C in hot air dryer c) electric arc fusion of the pelletised raw material mixture.

[0033] The reaction temperature during step c) which takes place in an electric arc furnace in which the individual ceramics melt and diffuse in liquid phase at >2000°C at atmospheric air conditions. The mix of different sized cations leads to increase in entropy of the system. Hence, the system tries to stabilize the system by forming a stable lattice structure where the cations occupy random position in the lattice. The mix is fed to the electric arc furnace at an interval of 15 minutes to allow complete fusion of the individual ceramic material. After all the raw material is fed to the furnace the material may be cooled in three different modes. In the first mode, the ultrafast mode, the melted and fused material is solidified within cooling time of about <3-4 minutes in a graphite lined steel ladle, directly quenched in water and solidified into thin slabs of 5 to 10 mm. The cooling rate ranges ~ 1500 °C / min. In the second mode, the fast mode, the melted and fused material is cooled by pouring in the gaps of ~10 mm created by two cast iron blocks resulting in solidification in 15 minutes. When the molten melt comes in contact with the metallic plates, the heat will be quickly transferred to the metallic plate resulting in rapid cooling of the molten melt. In the third mode, the normal mode, the melted and fused material is cooled in that the molten material is left in the crucible for 12-15 hours allowing it to cool naturally. These three different solidification modes were adopted to check the stability of the high entropy phase with various cooling rates.

[0034] Fig 2. Shows the XRD patterns of the individual ceramic oxides and high entropy oxide cooled in three modes. When the solidification starts in molten phase, all the different size cations try to fit in a crystal system to reduce the configurational entropy. In the present system, a fluorite structure was observed after solidification. The fluorite structure is a face centered cubic structure with cations occupying the regular sites and oxygen anions occupy tetrahedral voids. Among the crystal structures of the individual ceramic oxides given in table 2, Y2O3 has cubic phase which might act as parent lattice. The new fluorite crystal systems peaks will be distinct form the individual ceramics oxide peaks (Fig.2a). The high entropy phase peaks are not matched with any individual oxide peaks. It is observed that the high entropy phase was formed in all the three modes of solidification. The high entropy oxide crude solidified by normal mode was taken and crushed to F24 grit abrasive grains. These grains were molded and polished for microstructural investigation. Fig.3a shows the back scattered electron SEM micrograph of high entropy oxide. A unique microstructure was observed. Light grey and dark regions were observed in the microstructure. The light grey phase might contain high atomic numbered ceramic oxides and the dark phase contains lighter atomic numbered ceramic oxides.

[0035] Any material system always tries to reduce its free energy to attain a stable phase. If enough driving force is given the material system tries to reduce its entropy to achieve the stable phase. The stability of the high entropy oxide in the present study is unknown as it is new system. To further understand the phase stability of high entropy oxide, it was subjected to various heat treatments.

[0036] After the solidification and cooling, the crude was crushed using roll crusher. After crushing, the HEO by pot mode was subjected to heat treatment in muffle furnace at 1600°C for 5 hours. After prolonged heat treatment the high entropy oxide phase was present. Cold pressed compact was made from the HEO-pot material and heat treated at 990 °C for 5 hours and quench in water from 990 °C to room temperature. After heat treatment and water quenching the high entropy phase remained unchanged.

[0037] WORKING EXAMPLES

[0038] The present invention is hereinafter illustrated by way of an exemplary embodiments read along with enclosed diagrams for better understanding but is not intended to limit the scope of the disclosure. While they are typical of those that might be used, other procedures, methodologies or techniques known to those skilled in the art may alternatively be used. In this regard, the present example embodiment may have different forms and should not be construed as being limited to the descriptions set forth herein. Accordingly, the example embodiments are merely described below for the purpose of explanation only.

[0039] Example 1 The individual ceramics oxides mentioned in table 1 taken in the wt. % of: AI2O3-

[0040] 14.9, Y2O3 - 33, G2O3 - 22.2, Z1O2 - 18, TiCh - 11.9 each and mixed in Y-blender. After the blending, 50 kg batch powder was taken in barrel mixer and made into pellets using water as binding agent. A 300 kg batch pellets were prepared by mixing individual oxides in stoichiometric quantities. The fusion was taken in an electric arc furnace with 300 kg capacity crucible. The current supplied ranges from 700-1500 A where voltage is 110 V. The electric arc furnace crucible bottom was layered with the raw material pellet mix, then graphitic carbon with 99% purity was added as top layer for arcing. The raw material was fed to the furnace in 15 min intervals with a cooking time of 10 min. After the material is fused well in the furnace, the melt is water quenched to room temperature.

[0041] Example 2

[0042] The individual ceramics oxides mentioned in table 1 taken in the wt. % of: AI2O3-

[0043] 14.9, Y2O3 - 33, G2O3 - 22.2, Z1O2 - 18, TiCh - 11.9 each and mixed in Y-blender. After the blending, 50 kg batch powder was taken in barrel mixer and made into pellets using water as binding agent. A 300 kg batch pellets were prepared by mixing individual oxides in stoichiometric quantities. The fusion was taken in an electric arc furnace with 300 kg capacity crucible. After the fusion, the molten metal was poured in spaces between the metallic plates knows as book mold across industries. The melt was solidified by quick transfer of heat to the metallic plates.

[0044] Example 3

[0045] The individual ceramics oxides mentioned in table 1 taken in the wt. % of: AI2O3-

[0046] 14.9, Y2O3 - 33, G2O3 - 22.2, Z1O2 - 18, TiCh - 11.9 each and mixed in Y-blender. After the blending, 50 kg batch powder was taken in barrel mixer and made into pellets using water as binding agent. A 300 kg batch pellets were prepared by mixing individual oxides in stoichiometric quantities. The fusion was taken in an electric arc furnace with 300 kg capacity crucible. After the fusion the molten material is allowed to solidify in the crucible for 12-14 hours. The mode of solidification is called pot mode. Example 4

[0047] The multicomponent oxide crude from the pot mode was taken and crushed to make F24 grains. 1 kg of F24 grains was taken and heat treated at 1600°C for 5 hours. Again, the crude from the pot was taken and crushed into fine powder. This fine powder was cold pressed to make a pellet. The cold pressed pellet was heat treated at 990 °C for 5 hours and quenched form that temperature. This was done to check if the oxides segregate back to individual oxides. In other words, to check the stability of the formed high entropy oxide phase. The HEO was found to be stable.

[0048] Example 5

[0049] Phase stability of high entropy oxide:

[0050] The oxide was subjected to various heat treatments. In one heat treatment, pot mode F24 grains were taken and subjected to heat treatment at 1600 °C for 5 hours and furnace cooled to room temperature. (In the abrasive industry, the abrasive grains classified into different sized following FEPA (Federation of European Producers of Abrasives] specification. As per that grit size F24 means 50 % of the grains having size more than 745 microns]. The long holding time at 1600°C gives enough driving force for the diffusion to take place. In another heat treatment process, high entropy oxide crude from normal mode was crushed into fine powders and cold pressed with lOOkN load. The pressed pellet was subjected to heat treatment at 990°C for 5 hours. After the holding time, the pellet was water quenched from 990°C. This heat treatment process will give information about any intermediate phase changes happening at 990°C. The XRD patterns of the heat- treated samples were compared to the non-heat-treated samples in Fig.2b. It is observed that high entropy phase was stable and peaks corresponding to fluorite structure could be seen in the XRD patterns. It is also observed that the intensity of the small secondary peaks was increased from non-heat-treated sample peak intensity. These small secondary peaks were identified as segregated AI2O3, Z1O2 and CnCh peaks. Table 1

[0051] Table 1 provides purity and particle size of raw materials used in the inventions. Table 2

[0052] Table 2 shows structural information of the raw materials. It is to infer that, the irrespective of the stating crystal structure or ionic radii, all the oxides together formed HEO system.

[0053] Advantageously, the electric arc fusion method of preparing the HEO of the present invention promotes homogeneity and allows scalability to commercial bulk production levels. One of the potential applications of the mentioned HEO is abrasive industry. It can be used in coated and bonded, blasting abrasive applications. Apart from this, it is a potential candidate for high temperature thermal resistance coating applications.

[0054] As stated hereinabove, the example embodiments of the present inventive concepts have been described are for illustrative purposes only and cannot limit the scope of the invention. A person skilled in the art will appreciate that various modifications and other equivalent embodiments are possible from those described herein in this document.

Claims

CLAIMS1. A multicomponent High Entropy Oxide (HEO) having high configurational entropy, said HEO comprises at least one or more individual ceramic oxide selected from the group comprising Alumina (AI2O3), Zirconium oxide (ZrO2), Titanium oxide (TiO2), Yttrium oxide (Y2O3), chromium oxide (CT2O3 ), silicon dioxide (SiO2) and Hafnium oxide (HK ).

2. The multicomponent High Entropy Oxide (HEO) having high configurational entropy as claimed in claim 1 wherein said HEO has equi- atomic or near equi-atomic concentrations of the individual ceramic oxide.

3. The multicomponent High Entropy Oxide (HEO) having high configurational entropy, as claimed in any of the preceding claims wherein said HEO has fluorite-type crystal structure in which said structure is a facecentered cubic structure with cations occupying the regular sites and oxygen anions occupying tetrahedral voids fully or partially.

4. A multicomponent High Entropy Oxide (HEO) having high configurational entropy in which said HEO is represented by the molecular formula AlZrTiYCr)O.

5. A process for preparing a multicomponent High Entropy Oxide (HEO) having high configurational entropy, comprising the steps of - a) mixing one or more individual ceramic oxides in equi-atomic quantities; b) pelletizing the mix of 3-5 mm size with addition of water and drying for12 hours at 150°C in dryer c) electric arc fusion of the pelletised raw material mixture.

6. The process for preparing a multicomponent High Entropy Oxide (HEO) having high configurational entropy as claimed in claim 5, wherein the reaction temperature during step c) which takes place in an electric arc furnace in which the individual ceramics melt and diffuse in liquid phase at >2000°C at atmospheric air conditions.

7. The process for preparing a multicomponent High Entropy Oxide (HEO) having high configurational entropy as claimed in any of claims 5-6 wherein the mix is fed to the electric arc furnace at an interval of 15 minutes to allow complete fusion of the individual ceramic material.

8. The process for preparing a multicomponent High Entropy Oxide (HEO) having high configurational entropy as claimed in claims 5-7, wherein the melted and fused material is solidified by normal mode, fast mode and ultrafast mode.

9. The process for preparing a multicomponent High Entropy Oxide (HEO) having high configurational entropy as claimed in claims 5-7 wherein the melted and fused material is cooled by normal or pot mode in which the molten material is left in the crucible for 12-15 hours allowing it to cool naturally.

10. The process for preparing a multicomponent High Entropy Oxide (HEO) having high configurational entropy as claimed in claims 5-7 wherein the melted and fused material is cooled by fast mode in which the said molten material is poured in the gaps of ~10 mm created by two cast iron blocks resulting in solidification in 15 minutes.

11. The process for preparing a multicomponent High Entropy Oxide (HEO) having high configurational entropy as claimed in claims 5-7, wherein the melted and fused material is solidified by ultrafast mode in which the said molten material is poured in the water resulting in solidification in 3-4 minutes.

12. The process for preparing a multicomponent High Entropy Oxide (HEO) having high configurational entropy as claimed in claim 8-11 in which all three modes of cooling resulted in high entropy oxide with fluorite structure.

13. The process for preparing a multicomponent High Entropy Oxide (HEO) having high configurational entropy as claimed in claim 11 in which after cooling, the crude was crushed and subjected to heat treatment in muffle furnace at about 1600°C for about 5 hours showing no degradation in high entropy phase.

14. The process for preparing a multicomponent High Entropy Oxide (HEO) having high configurational entropy as claimed in claim 9 wherein cold pressed compacts were made and heat treated at 990°C for 5 hours and quenched in water to room temperature denoting that high entropy phase remained unchanged.

15. A high temperature thermal resistance coating incorporating the multicomponent High Entropy Oxide (HEO) as claimed in any of the preceding claims.

Citation Information

Patent Citations

  • Single-phase spinel type high-entropy oxides as well as preparation method and application thereof

    CN112340787A

  • High-temperature heat-insulation high-entropy oxide and preparation method thereof

    CN113185305A

  • High-entropy oxide oxygen storage material as well as preparation method and application thereof

    CN114618503A

  • Ultrafast preparation method of high-entropy oxide

    CN115093214A

  • High-entropy multielement alloys

    US20020159914A1

Cited By

  • Fluorite-pyrochlore double-phase high-entropy oxide ceramic powder and preparation method thereof

    CN119100790A

  • Fluorite-hooperite dual-phase high-entropy oxide ceramic powder and preparation method thereof

    CN119100790B

  • Energy-saving coating applied to large ethylene heating furnace and preparation method of energy-saving coating

    CN119118656A

  • Biphase rare earth metal-based high-entropy oxygen carrier for waste plastic gasification and preparation method and application thereof

    CN121494091A

  • Method for preparing high-density high-entropy rare earth hafnate ceramic through electric arc remelting

    CN122167161A