Thermoplastic resin composition, molded article using the same, and method for producing thermoplastic resin composition

The thermoplastic resin composition, with ionic liquids and donor-acceptor compounds bonded to cellulose fibers, addresses the aging issue of antistatic properties in molded products, ensuring continuous antistatic and antifouling performance by preventing their loss, thus effectively reducing dust adhesion and maintaining surface resistivity.

WO2024201660A1PCT designated stage expired Publication Date: 2024-10-03MITSUBISHI ELECTRIC CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2023/012240
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-27
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Existing thermoplastic resin compositions used for molded products, such as OA equipment, fail to maintain excellent antistatic properties over time due to aging deterioration of antistatic agents, leading to reduced antifouling properties and dust adhesion issues.

Method used

A thermoplastic resin composition comprising a thermoplastic resin, an ionic liquid, a donor-acceptor compound, cellulose fibers, and a compatibilizing resin, where the ionic liquid and donor-acceptor compound are bonded to the cellulose fibers, preventing their loss and maintaining antistatic and antifouling properties.

Benefits of technology

The composition continuously exhibits excellent antistatic and antifouling properties by preventing the disappearance of ionic liquids and donor-acceptor compounds, reducing dust adhesion, and maintaining surface resistivity within desired ranges even after accelerated testing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-C000001
    Figure JPOXMLDOC01-APPB-C000001
  • Figure JPOXMLDOC01-APPB-C000002
    Figure JPOXMLDOC01-APPB-C000002
  • Figure JPOXMLDOC01-APPB-T000003
    Figure JPOXMLDOC01-APPB-T000003
Patent Text Reader

Abstract

This thermoplastic resin composition includes: a thermoplastic resin (A); at least one of an ionic liquid (B) and a donor-acceptor compound (C); cellulose fibers (D); and a compatibilizing resin (E). The thermoplastic resin (A) is at least one of an olefin resin and a styrene resin. The ionic liquid (B) is a phosphonium salt. The cellulose fibers (D) have an average fiber diameter of 3 nm to 50 μm and an average fiber length of 100 nm to 400 μm. The compatibilizing resin (E) is a different resin from the thermoplastic resin (A), and is a resin for compatibilizing the thermoplastic resin (A) and the cellulose fibers (D).
Need to check novelty before this filing date? Find Prior Art

Description

Thermoplastic resin composition, molded article using the same, and method for producing thermoplastic resin composition

[0001] The present disclosure relates to a thermoplastic resin composition, a molded article using the same, and a method for producing the thermoplastic resin composition.

[0002] Molded articles of thermoplastic resin compositions based on olefin-based resins, styrene-based resins, polycarbonate-based resins, etc. are used for housings and parts of home appliances and office automation equipment such as copiers and computers. Examples of thermoplastic resins include olefin-based resins such as polypropylene (abbreviated as PP) and polyethylene (abbreviated as PE), styrene-based resins such as high-impact polystyrene (abbreviated as HIPS) and general-purpose polystyrene (abbreviated as GPPS), and acrylonitrile-based resins such as acrylonitrile-butadiene-styrene (abbreviated as ABS) and acrylonitrile-styrene (abbreviated as AS). Most of the thermoplastic resins used for the housings and parts of office automation equipment are acrylonitrile-based resins (such as ABS and AS), polycarbonate (PC)-based resins, polycarbonate / acrylonitrile-based resins, or flame-retardant resins.

[0003] In order to impart antistatic properties to a resin composition containing a thermoplastic resin, an antistatic agent may be added to the resin composition. For example, Patent Document 1 (JP-A-7-18137) discloses the addition of an antistatic agent that is a phosphonium sulfonate salt to a resin composition used for a molded product that may be susceptible to dust or the like. Patent Document 2 (JP-A-2020-50857) and Patent Document 3 (JP-A-2021-193169) disclose resin compositions containing a donor-acceptor antistatic agent.

[0004] Japanese Patent Application Laid-Open No. 7-18137 Japanese Patent Application Laid-Open No. 2020-50857 Japanese Patent Application Laid-Open No. 2021-193169

[0005] Development of molded articles imparted with antifouling properties has been progressing in order to keep molded articles clean and to make them easier to clean. By using a resin composition containing an antistatic agent, it is possible to impart antifouling properties to molded articles that inhibit the adhesion of dust and the like. To ensure that the antifouling properties of molded articles are maintained, it is necessary for the molded articles to maintain their excellent antistatic properties. However, Patent Documents 1 to 3 do not consider the deterioration of the antistatic properties of molded articles over time, and it is thought that the antifouling properties of molded articles are difficult to maintain.

[0006] An object of the present disclosure is to provide a thermoplastic resin composition that can continuously exhibit excellent antistatic properties.

[0007] The thermoplastic resin composition of the present disclosure comprises a thermoplastic resin (A), at least one of an ionic liquid (B) and a donor-acceptor compound (C), cellulose fibers (D), and a compatibilizing resin (E).

[0008] The thermoplastic resin (A) is at least one of an olefin-based resin and a styrene-based resin. The ionic liquid (B) is a phosphonium salt. The cellulose fibers (D) have an average fiber diameter of 3 nm or more and 50 μm or less and an average fiber length of 100 nm or more and 400 μm or less. The compatibilizing resin (E) is a resin different from the thermoplastic resin (A) and serves to compatibilize the thermoplastic resin (A) and the cellulose fibers (D).

[0009] According to the thermoplastic resin composition of the present disclosure, it is possible to provide a molded article that continuously exhibits excellent antistatic properties.

[0010] Embodiment 1 (Thermoplastic Resin Composition) The thermoplastic resin composition of this embodiment (hereinafter sometimes referred to as "the composition") includes a thermoplastic resin (A), at least one of an ionic liquid (B) and a donor-acceptor compound (C), cellulose fibers (D), and a compatibilizing resin (E). The thermoplastic resin (A) is at least one of an olefin-based resin and a styrene-based resin. The ionic liquid (B) is a phosphonium salt. The cellulose fibers (D) have an average fiber diameter of 3 nm or more and 50 μm or less and an average fiber length of 100 nm or more and 400 μm or less. The compatibilizing resin (E) is a resin different from the thermoplastic resin (A) and serves to compatibilize the thermoplastic resin (A) and the cellulose fibers (D).

[0011] The ionic liquid (B) and the donor-acceptor compound (C) can impart antistatic properties to molded articles formed using the composition. The ionic liquid (B) and the donor-acceptor compound (C) can impart excellent antistatic properties to molded articles even at low contents. Therefore, the addition of the ionic liquid (B) and the donor-acceptor compound (C) can prevent the physical properties of the thermoplastic resin (A) from deteriorating.

[0012] The antistatic properties of the molded article can prevent dust from adhering to the molded article, and the molded article can also have excellent antifouling properties. Molded articles formed using the present composition are resistant to the adhesion of hydrophilic dust such as sand and dirt, as well as hydrophobic dust such as oily smoke.

[0013] If the ionic liquid (B) and the donor-acceptor compound (C) disappear from the molded article, the antistatic properties of the molded article will decrease, and the antifouling properties will also decrease. If the ionic liquid (B) and the donor-acceptor compound (C) present near the surface of the molded article disappear due to cleaning such as wiping the molded article or due to changes over time, the antistatic properties of the molded article may decrease. Because the composition contains cellulose fibers (D), it is possible to suppress the disappearance of the ionic liquid (B) and the donor-acceptor compound (C) from the molded article and provide a molded article that can continuously exhibit excellent antistatic properties.

[0014] The reason for this is presumed to be as follows. The ionic liquid (B) and the donor-acceptor compound (C) have anionic and cationic components. The cellulose fiber (D) exhibits hydrophilicity due to the bonding of hydroxyl groups in the cellulose skeleton. The hydrophilic cellulose fiber (D) has excellent affinity with the ionic liquid (B) and the donor-acceptor compound (C), and the two are easily bonded by electrostatic attraction. The thermoplastic resin (A) and the cellulose fiber (D) are thought to be well mixed due to the presence of the compatibilizing resin (E). Because the ionic liquid (B) and the donor-acceptor compound (C) are bonded to the cellulose fiber (D) in this state, it is thought that the ionic liquid (B) and the donor-acceptor compound (C) are more likely to remain within the molded article. In addition, the cellulose fiber (D) in the molded article acts as a barrier, preventing the ionic liquid (B) and the donor-acceptor compound (C) from leaking from the surface of the molded article. From these points, it is presumed that a molded article formed using the present composition is unlikely to lose the ionic liquid (B) and the donor-acceptor compound (C) even when its surface is cleaned by wiping or the like, or when it changes over time, and therefore can continuously exhibit excellent antistatic properties and antifouling properties.

[0015] Because the ionic liquid (B) and the donor-acceptor compound (C) have low molecular weights, their presence near the surface of a molded article or their bleeding onto the surface of the molded article can improve the antistatic properties and antifouling properties of the molded article. Even in such cases, by using the present composition, it is expected that the ionic liquid (B) and the donor-acceptor compound (C) will not easily disappear, and that a molded article that can continuously exhibit excellent antistatic properties and antifouling properties can be obtained.

[0016] The present composition can be used to form a molded article as described below. The present composition preferably contains an olefin-based resin or a styrene-based resin as the thermoplastic resin (A). The present composition may contain at least one of an ionic liquid (B) and a donor-acceptor compound (C), or may contain both an ionic liquid (B) and a donor-acceptor compound (C). The present composition may contain other components in addition to the above-mentioned components. Specific examples of the composition will be described later.

[0017] When a flat plate having a size of 100 mm length x 100 mm width x 2 mm thickness is formed using this composition, the surface resistivity of the flat plate at a temperature of 23°C and a relative humidity of 50% is preferably 1.0 x 10 12 Ω / sq or less, more preferably 1.0×10 11 Ω / sq or less, and 5.0 × 10 10 The surface resistivity of the flat plate may be 1.0×10 Ω / sq or less. 7 Ω / sq or more. The surface resistivity of the flat piece referred to here is the initial surface resistivity before the flat piece is subjected to the accelerated test described below. When the initial surface resistivity of the flat piece is within the above range, the molded article obtained using the present composition can be inhibited from adhering to dust and can have excellent anti-fouling properties. The initial surface resistivity can be adjusted, for example, by the type and content of the ionic liquid (B) and donor-acceptor compound (C) contained in the present composition. The above flat piece can be prepared by the method described in the Examples described below. The initial surface resistivity can be measured by the method described in the Examples described below.

[0018] After the accelerated test, the surface resistivity of the flat plate at a temperature of 23°C and a relative humidity of 50% is preferably 1.0 x 10 12 Ω / sq or less, more preferably 5.0 × 10 11 Ω / sq or less, and 1.0 × 10 11 The surface resistivity of the flat plate after the accelerated test is usually 1.0×10 8Ω / sq or more. When the surface resistivity of the flat plate after the accelerated test is within the above range, the molded article obtained using the composition can continuously suppress the adhesion of dust and continuously exhibit excellent antifouling properties. The surface resistivity after the accelerated test can be adjusted, for example, by the type and content of the ionic liquid (B) and donor-acceptor compound (C) contained in the composition, and the type and content of the cellulose fiber (D). The surface resistivity after the accelerated test can be measured by the method described in the Examples below. The accelerated test is a test that simulates an actual use environment and can be performed by the method described in the Examples below.

[0019] Each component contained in the present composition will be described in detail below. (Thermoplastic Resin (A)) The thermoplastic resin (A) is the base resin of the present composition. The thermoplastic resin (A) is at least one of an olefin-based resin and a styrene-based resin, and is preferably an olefin-based resin or a styrene-based resin. The thermoplastic resin (A) may be a recycled thermoplastic resin recovered from molded articles such as housings or parts of used home appliances and office automation equipment such as copiers and computers.

[0020] An olefin resin is a resin having an olefin unit as a repeating structural unit. The olefin resin is a resin composed only of carbon (C) and hydrogen (H) and containing olefin units in a total amount of more than 50 mol% to 100 mol% or less of all structural units constituting the molecular chain. The olefin unit is a structural unit of a polymer obtained by polymerizing an olefin monomer. The thermoplastic resin (A) may contain one or more olefin resins.

[0021] Examples of the olefin resin include one or more selected from the group consisting of polyethylene resins such as homopolyethylene and ethylene-α-olefin copolymers (excluding those containing propylene units as a repeating structural unit); and polypropylene resins such as homopolypropylene, propylene-ethylene block copolymer, propylene-butene block copolymer, propylene-α-olefin block copolymer, propylene-ethylene random copolymer, propylene-butene random copolymer, propylene-α-olefin random copolymer, and propylene-α-olefin graft copolymer. The olefin resin is preferably a polypropylene resin.

[0022] A styrene-based resin is a resin having a styrene-based unit as a repeating structural unit. A styrene-based resin refers to a resin containing a total of more than 50 mol% to 100 mol% of styrene-based units relative to all structural units constituting the molecular chain. A styrene-based unit refers to a structural unit of a polymer obtained by polymerizing a styrene-based monomer having a skeleton in which one hydrogen atom on the benzene ring is substituted with a vinyl group. In the styrene-based monomer, the hydrogen atoms on the benzene ring other than the hydrogen atom substituted with the vinyl group may be substituted with a functional group. The thermoplastic resin (A) may contain one or more styrene-based resins.

[0023] Examples of styrene-based resins include at least one selected from the group consisting of polymers obtained by polymerizing monovinyl aromatic monomers such as styrene, α-methylstyrene, p-methylstyrene, and p-tert-butylstyrene; rubber-modified styrene-based polymers produced by dissolving rubber-like substances such as polybutadiene (PBD) and styrene-butadiene copolymer (SBR) in styrene-based monomers and subjecting them to bulk polymerization or bulk suspension polymerization; and polymers obtained by polymerizing vinyl cyanide monomers such as acrylonitrile.

[0024] Examples of polymers obtained by polymerizing monovinyl aromatic monomers include polystyrene (GPPS). Examples of rubber-modified styrene polymers include at least one of high impact polystyrene (HIPS) and medium impact polystyrene (MIPS). Examples of polymers obtained by polymerizing vinyl cyanide monomers include acrylonitrile-styrene resin (AS resin) and acrylonitrile-butadiene-styrene copolymer (ABS resin) obtained by polymerizing acrylonitrile, butadiene, and styrene.

[0025] The content of the thermoplastic resin (A) may be, for example, 30% by weight or more and 95% by weight or less, 40% by weight or more and 90% by weight or less, 50% by weight or more and 85% by weight or less, or 60% by weight or more and 80% by weight or less, relative to the total amount of the composition. When the thermoplastic resin (A) contains two or more thermoplastic resins, the content of the thermoplastic resin (A) refers to the total amount thereof.

[0026] (Ionic Liquid (B)) The ionic liquid (B) is a phosphonium salt, and can impart antistatic properties and antifouling properties to a molded article formed using the present composition. When the present composition contains a donor-acceptor compound (C), the present composition may or may not contain an ionic liquid (B). The present composition can contain one or more types of ionic liquid (B).

[0027] Examples of the ionic liquid (B) include one or more selected from the group consisting of tributyldodecylphosphonium bis(trifluoromethanesulfonyl)imide, trihexyltetradecylphosphonium bis(trifluoromethylsulfonyl)imide, triethylpentylphosphonium bis(trifluoromethylsulfonyl)imide, triethyloctylphosphonium bis(trifluoromethylsulfonyl)imide, tri-n-butylmethylphosphonium bis(trifluoromethylsulfonyl)imide, tributyldodecylphosphonium bromide, tetrabutylphosphonium dodecylbenzenesulfonate, and tetrabutylphosphonium tetraphenylborate. The ionic liquid (B) is preferably one or more selected from the group consisting of tributyldodecylphosphonium bis(trifluoromethanesulfonyl)imide, tributyldodecylphosphonium bromide, and tetrabutylphosphonium dodecylbenzenesulfonate. The present composition containing these compounds can impart excellent antistatic properties and antifouling properties to molded articles.

[0028] As the tributyldodecylphosphonium bis(trifluoromethanesulfonyl)imide, a compound manufactured by Fujifilm Wako Pure Chemical Industries, Ltd. and "IL-AP3" manufactured by Koei Chemical Industry Co., Ltd. can be used. As the tributyldodecylphosphonium bromide, a compound manufactured by Fujifilm Wako Pure Chemical Industries, Ltd. can be used. As the tetrabutylphosphonium dodecylbenzenesulfonate, "Elecut S-418" manufactured by Takemoto Oil & Fat Co., Ltd. can be used.

[0029] The content of ionic liquid (B) in the composition is, for example, 0.5 to 5.0 parts by weight, preferably 0.5 to 4.0 parts by weight, and more preferably 0.5 to 3.0 parts by weight, per 100 parts by weight of thermoplastic resin (A). If the content of ionic liquid (B) exceeds 5.0 parts by weight, the thermal stability in high-temperature environments is significantly reduced, the molded article tends to yellow easily, and the mechanical properties of the molded article may be significantly reduced. If the content of ionic liquid (B) is less than 0.5 parts by weight, dust tends to adhere to the molded article, and the stain resistance of the molded article tends to be reduced. When the composition contains two or more types of ionic liquid (B), the content of ionic liquid (B) refers to the total amount.

[0030] (Donor-acceptor compound (C)) The donor-acceptor compound (C) refers to a compound having both an electron-donating group and an electron-withdrawing group. The donor-acceptor compound (C) can impart antistatic properties and antifouling properties to a molded article formed using the present composition. When the present composition contains an ionic liquid (B), the present composition may or may not contain a donor-acceptor compound (C). The present composition may contain one or more donor-acceptor compounds (C).

[0031] The donor-acceptor compound (C) is not particularly limited as long as it is a compound having an electron-donating group and an electron-withdrawing group, but is preferably a compound represented by formula (1) (hereinafter, sometimes referred to as "compound (1)").

[0032] As the compound (1), "Biomicelle BN-105" (chemical formula: C) manufactured by Boron Laboratory Co., Ltd. 42 H 81 O 8 B.C. 23 H 48 ON 2 As the donor-acceptor compound (C), "Biomicelle BN-77" (chemical formula: C) manufactured by Boron Laboratory Co., Ltd., which has a structure similar to that of compound (1), can be used. 42 H 81 O 8 B.C. 23 H48 The present composition containing these compounds can impart excellent antistatic properties and antifouling properties to molded articles.

[0033] The content of the donor-acceptor compound (C) in the composition is, for example, 0.5 to 5.0 parts by weight, preferably 0.5 to 4.0 parts by weight, and more preferably 0.5 to 3.0 parts by weight, per 100 parts by weight of the thermoplastic resin (A). If the content of the donor-acceptor compound (C) exceeds 5.0 parts by weight, the mechanical properties of the molded article may be significantly reduced. If the content of the donor-acceptor compound (C) is less than 0.5 parts by weight, dust tends to adhere to the molded article, and the stain resistance of the molded article tends to be reduced. When the composition contains two or more donor-acceptor compounds (C), the content of the donor-acceptor compounds (C) refers to the total amount.

[0034] (Cellulose fiber (D)) The cellulose fiber (D) has an average fiber diameter of 3 nm or more and 50 μm or less and an average fiber length of 100 nm or more and 400 μm or less. When the composition contains the cellulose fiber (D), it is thought that the ionic liquid (B) and the donor-acceptor compound (C) are less likely to be lost when the molded article is cleaned by wiping or when the molded article changes over time, and that the excellent antistatic properties and antifouling properties of the molded article are more likely to be maintained.

[0035] The cellulose fibers (D) may contain at least one of nanofibers and microfibers. The cellulose fibers (D) may contain nanofibers, microfibers, or both. The nanofibers have an average fiber diameter of 3 nm to 200 nm and an average fiber length of 100 nm to 1000 nm. The nanofibers may be microfibers (cellulose microfibrils) consisting of bundles of several tens of cellulose molecules. The microfibers have an average fiber diameter of 1 μm to 50 μm and an average fiber length of 10 μm to 400 μm.

[0036] The average fiber diameter and average fiber length of the cellulose fibers (D) can be measured by the methods described in the Examples below. When the nanofibers are microfibers, the average fiber diameter of the microfibers refers to the width (diameter) of a bundle of cellulose molecules.

[0037] The cellulose fibers (D) may have hydroxyl groups on the surface thereof. The crystalline form, degree of crystallization, degree of polymerization, etc. of the cellulose fibers (D) are not particularly limited.

[0038] The cellulose fibers (D) can be obtained by subjecting pulp or the like as a raw material to a fiberization treatment. Examples of the fiberization treatment include mechanical fiberization methods and chemical fiberization methods.

[0039] In mechanical defibration methods, nanofibers and microfibers can be obtained by preparing an aqueous suspension or slurry of raw materials such as pulp and mechanically grinding it using a refiner, high-pressure homogenizer, disc mill (grinder), kneader (extruder), ball mill, bead mill, or the like. Alternatively, the following methods may be used: a freeze-pulverization method in which the aqueous suspension or slurry of the raw materials is frozen and defibrated using a ball mill or the like; an underwater head-on collision method in which raw material suspensions are pressurized and collided with each other at high speed, and defibrated using the collision force, pressure difference, and microcavitation; or a water jet method in which the raw material suspension is pressurized up to 245 MPa and sprayed to create Mach 2 water jets, and these water jets are defibrated by colliding with each other obliquely. When obtaining nanofibers, which are fine fibers, it is preferable to subject the raw materials to a chemical pretreatment, i.e., a refining treatment, before mechanical defibration, in order to prevent damage to the fibers.

[0040] Chemical defibration methods include the phosphate esterification method, in which phosphate groups are introduced to the hydroxyl groups at the 2-, 3-, and 6-positions of cellulose molecules to obtain a highly dispersed liquid due to molecular chain repulsion; and the TEMPO catalytic oxidation method, in which TEMPO (2,2,6,6-tetramethylpiperidine-1-oxy radical) is used as a catalyst to selectively introduce carboxyl groups to the hydroxyl groups at the 6-position in the amorphous regions of cellulose molecules to obtain a highly dispersed liquid due to molecular chain repulsion.

[0041] Alternatively, a raw material such as undried pulp may be chemically treated to make it compatible with the thermoplastic resin (A) by acetylating, silanizing, or urethanizing the hydroxyl group at the 6-position of the cellulose molecule with an isocyanate, and then kneading the resulting material with the thermoplastic resin (A) in an extruder to defibrate the raw material.

[0042] Examples of cellulose fibers (D) that can be used include "Nanoforest" manufactured by Chuetsu Pulp & Paper Co., Ltd., "CellFim P" manufactured by Mori Machinery Corporation, "GS CNF" manufactured by GS Alliance Co., Ltd., and "ARBOCEL" manufactured by Rettenmeyer Japan Co., Ltd.

[0043] The content of cellulose fiber (D) in the present composition is, for example, 1.0 part by weight or more and 50 parts by weight or less, preferably 1.0 part by weight or more and 40 parts by weight or less, and more preferably 1.0 part by weight or more and 30 parts by weight or less, relative to 100 parts by weight of thermoplastic resin (A). When the content of cellulose fiber (D) is within the above range, it is easy to continuously suppress dust adhesion in a molded article, and it is easy to continuously exhibit excellent stain resistance. When the present composition contains two or more types of cellulose fiber (D), the content of cellulose fiber (D) refers to the total amount thereof.

[0044] (Compatibilizing Resin (E)) The compatibilizing resin (E) is a resin different from the thermoplastic resin (A) and serves to compatibilize the thermoplastic resin (A) and the cellulose fibers (D). "Different resins" means that the compositions of the structural units constituting the resins are different from each other. "Compatibilized" means that phase separation between the thermoplastic resin (A) and the cellulose fibers (D) in a molded article formed using the present composition is suppressed more than phase separation between the thermoplastic resin (A) and the cellulose fibers (D) in a molded article formed using a composition that is the same as the present composition except that it does not contain the compatibilizing resin (E). The compatibilizing resin (E) preferably contains an oxygen atom (O) that is compatible with the hydroxyl groups (-OH) of the cellulose fibers (D).

[0045] By including the compatibilizing resin (E) in the present composition, phase separation between the thermoplastic resin (A) and the cellulose fibers (D) in a molded article obtained using the present composition is suppressed, and they are easily mixed homogeneously, thereby preventing a significant decrease in the mechanical properties of the molded article.

[0046] The present composition may contain one or more compatibilizing resins (E). The compatibilizing resin (E) may be selected depending on the type of thermoplastic resin (A). For example, when the thermoplastic resin (A) contains an olefin-based resin, it is preferable to use an olefin-based compatibilizing resin, and when the thermoplastic resin (A) contains a styrene-based resin, it is preferable to use a styrene-based compatibilizing resin.

[0047] The olefin compatibilizing resin is preferably a resin containing at least one of a carboxy group (—CO) and a hydroxyl group (—OH). Examples of the olefin compatibilizing resin include one or more resins selected from the group consisting of acid-modified olefin resins obtained by modifying an olefin resin with an unsaturated carboxylic acid such as maleic anhydride, ethylene vinyl acetate resins, vinyl acetate resins, and polyvinyl alcohol resins.

[0048] The acid-modified olefin resin is a polymer containing an olefin unit and an unsaturated carboxylic acid unit as a constituent unit. Examples of the unsaturated carboxylic acid include maleic acid (anhydride), itaconic acid (anhydride), fumaric acid, and crotonic acid, and maleic acid (anhydride) is preferred. Maleic acid (anhydride) refers to maleic acid or maleic anhydride, and itaconic acid (anhydride) refers to itaconic acid or itaconic anhydride.

[0049] The olefin-based compatibilizing resin is preferably an acid-modified olefin-based resin, more preferably a maleic anhydride-modified polypropylene resin. The maleic anhydride-modified polypropylene resin is preferably at least one of a maleic anhydride-modified polypropylene resin and a maleic anhydride-modified ethylene-propylene resin. Examples of the maleic anhydride-modified polypropylene resin that can be used include "SCONA TSPP 10213" manufactured by BYK Japan K.K., "SCONA TPPP 9212" manufactured by BYK Japan K.K., and "UMEX 1010" manufactured by Sanyo Chemical Industries, Ltd.

[0050] When the thermoplastic resin (A) is a polypropylene-based resin, the compatibilizing resin (E) is preferably an olefin-based compatibilizing resin, more preferably a maleic anhydride-modified polypropylene resin.

[0051] Examples of styrene-based compatibilizing resins include at least one of styrene-based thermoplastic elastomers (TPE-S) and methyl methacrylate-butadiene-styrene copolymers (MBS resins) obtained by polymerizing methyl methacrylate, butadiene, and styrene. Styrenic thermoplastic elastomers have a structure in which "hard segments" that impart strength and "soft segments" that have rubber-like elasticity are bonded together. Examples of styrene-based thermoplastic elastomers include SBS (styrene-butadiene-styrene) resin and SIS (styrene-isoprene-styrene) resin, as well as SEBS (styrene-ethylene-butylene-styrene) resin and SEPS (styrene-ethylene-propylene-styrene) resin, which are hydrogenated from these. The above-mentioned styrene-based thermoplastic elastomers have a polystyrene (PS) structure as the hard segment and a different soft segment structure.

[0052] Examples of styrene-based compatibilizing resins that can be used include "TR2003" manufactured by JSR Corporation, "Asaprene T-438" manufactured by Asahi Kasei Corporation, "Labalon A1801N-K" manufactured by Mitsubishi Chemical Corporation, and "Metablen C323A" manufactured by Mitsubishi Chemical Corporation.

[0053] When the thermoplastic resin (A) is a styrene-based resin, the compatibilizing resin (E) is preferably a styrene-based compatibilizing resin, more preferably a styrene-based elastomer.

[0054] The content of the compatibilizing resin (E) in the present composition is, for example, 0.5 to 20 parts by weight, preferably 1.0 to 15 parts by weight, and more preferably 1.0 to 10 parts by weight, per 100 parts by weight of the thermoplastic resin (A). If the content of the compatibilizing resin (E) exceeds 20 parts by weight, the mechanical properties of the molded article may be significantly reduced. If the content of the compatibilizing resin (E) is less than 0.5 parts by weight, the compatibility between the thermoplastic resin (A) and the cellulose fiber (D) may be reduced, and the mechanical properties of the molded article may be significantly reduced. When the present composition contains two or more types of compatibilizing resins (E), the content of the compatibilizing resins (E) refers to the total amount thereof.

[0055] (Other Components) The present composition may contain other components in addition to the components described above. Examples of other components include inorganic fillers, thermoplastic resins other than the thermoplastic resin (A) and the compatibilizing resin (E), heat stabilizers, ultraviolet absorbers, light stabilizers, antistatic agents other than the ionic liquid (B) and the donor-acceptor compound (C), plasticizers, release agents, flame retardants, flame retardant assistants, dyes, pigments, etc. The content of other components in the present composition may be adjusted as appropriate to obtain the desired physical properties.

[0056] Examples of inorganic fillers include one or more selected from the group consisting of talc, mica, wollastonite, calcium carbonate, barium sulfate, magnesium carbonate, clay, alumina, silica, calcium sulfate, carbon fiber, glass fiber, metal fiber, silica sand, silica stone, carbon black, titanium dioxide, zinc oxide, antimony trioxide, magnesium hydroxide, asbestos, zeolite, molybdenum, diatomaceous earth, sericite, shirasu, calcium hydroxide, calcium sulfite, sodium sulfate, bentonite, kaolinite, and graphite.

[0057] The other thermoplastic resin may be any thermoplastic resin other than the thermoplastic resin (A) and the compatibilizing resin (E) contained in the composition. Examples of the other thermoplastic resin include one or more selected from the group consisting of polycarbonate resin, alkyd resin, amino resin, bismaleimide triazine resin, chlorinated polyether, allyl resin, epoxy resin, ethylene-vinyl acetate-vinyl chloride copolymer, ethylene-vinyl chloride copolymer, nitrile resin, olefin-vinyl alcohol copolymer, phenolic resin, polyacetal, polyacrylate, polyallylsulfone, polybenzimidazole, polybutylene terephthalate, polyether ether ketone, polyether ketone, polyether nitrile, polyether sulfone, polyethylene terephthalate, polyketone, methacrylic resin, polymethylpentene, polyphenylene ether, polyphenylene sulfide, polysulfone, polyurethane, polyvinyl acetal, polyvinyl chloride, polyvinylidene chloride, silicone resin, xylene resin, ethylene propylene rubber, chloroprene rubber, butyl rubber, and nitrile rubber.

[0058] A heat stabilizer can be used to improve the thermal stability of the composition. The heat stabilizer is preferably a hindered phenol-based, phosphorus-based, or sulfur-based antioxidant. One or more types of heat stabilizers can be used.

[0059] Examples of hindered phenol antioxidants include 2,6-di-tert-butyl-p-cresol, tetrakis[methylene-3-(3',5'-di-tert-butyl-4'-hydroxyphenyl)propionate]methane, stearyl β-(3',5'-di-tert-butyl-4-hydroxyphenyl)propionate, 3,9-bis[1,1-dimethyl-2-[β-(3-tert-butyl-4-hydroxyphenyl)propionate]

[0033] Examples of the hydroxybenzoates include one or more selected from the group consisting of 1,3,5-trimethyl-2,4,6-tris(3',5'-di-tert-butyl-4-hydroxybenzyl)benzene, 1,3,5-trimethyl-2,4,6-tris(3',5'-di-tert-butyl-4-hydroxybenzyl)benzene, and triethylene glycol bis[3-(3-tert-butyl-5-methyl-4-hydroxyphenyl)propionate].

[0060] From the viewpoint of heat resistance and stability, the hindered phenol-based antioxidant is preferably at least one selected from the group consisting of tetrakis[methylene-3-(3',5'-di-tert-butyl-4'-hydroxyphenyl)propionate]methane, stearyl β-(3',5'-di-tert-butyl-4-hydroxyphenyl)propionate, and 3,9-bis[1,1-dimethyl-2-[β-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionyloxy]ethyl]-2,4,8,10-tetraoxaspiro(5,5)undecane.

[0061] Examples of phosphorus-based antioxidants include tris(2,4-di-tert-butylphenyl)phosphite, diphenyl mono(2-ethylhexyl)phosphite, diphenyl monodecyl phosphite, pentaerythritol bis(2,6-di-tert-butyl-4-phenyl phosphite), 2,2'-methylenebis(4,6-di-tert-butylphenyl)-2-ethylhexyl phosphite, distearyl pentaerythritol diphosphite, tris(mononylphenyl) phosphite, and at least one selected from the group consisting of tetrakis(2,4-tert-butylphenyl)-4,4'-biphenyldiphosphonate, ...

[0062] From the viewpoint of heat resistance stability, the phosphorus-based antioxidant is preferably at least one selected from the group consisting of tris(2,4-di-tert-butylphenyl)phosphite, diphenyl mono(2-ethylhexyl)phosphite, diphenyl monodecyl phosphite, pentaerythritol bis(2,6-di-tert-butyl-4-phenyl phosphite), and 2,2′-methylenebis(4,6-di-tert-butylphenyl)-2-ethylhexyl phosphite.

[0063] Examples of sulfur-based antioxidants include one or more selected from the group consisting of pentaerythritol tetrakis(3-laurylthiopropionate), dilauryl-3,3'-thiodipropionate, and dioctadecyl-3,3'-thiodipropionate. From the viewpoint of heat resistance and stability, the sulfur-based antioxidant is preferably pentaerythritol tetrakis(3-laurylthiopropionate).

[0064] The content of the heat resistance stabilizer in the present composition is preferably 0.05 to 10 parts by weight, more preferably 0.05 to 3 parts by weight, per 100 parts by weight of the thermoplastic resin (A). When the present composition contains two or more types of heat resistance stabilizers, the content of the heat resistance stabilizers refers to the total amount thereof.

[0065] The ultraviolet absorber can be used to suppress yellowing of the molded article due to ultraviolet light when used outdoors, etc. Examples of the ultraviolet absorber include one or more selected from the group consisting of hydroxybis(dimethylbenzyl)phenylbenzotriazole, 2-(2'-hydroxy-5'-tert-octylphenyl)benzotriazole, 2,2'-methylenebis[6-(2H-benzotriazol-2-yl)-4-tert-octylphenol], 2-(2'-hydroxy-5'-methylphenyl)benzotriazole, 2-(2'-hydroxy-3'-tert-butyl-5'-methylphenyl)-5-chlorobenzotriazole, 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5-[2-(2-ethylhexanoyloxy)ethoxy]phenol), and 2,4,6-tris(2-hydroxy-4-hexyloxy-3-methylphenyl)-1,3,5-triazine).

[0066] From the viewpoint of weather resistance stability, the ultraviolet absorber is preferably one or more selected from the group consisting of 2-(2'-hydroxy-5'-tert-octylphenyl)benzotriazole, 2,2'-methylenebis[6-(2H-benzotriazol-2-yl)-4-tert-octylphenol], 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5-[2-(2-ethylhexanoyloxy)ethoxy]phenol), and 2,4,6-tris(2-hydroxy-4-hexyloxy-3-methylphenyl)-1,3,5-triazine). One or more types of ultraviolet absorbers can be used.

[0067] The content of the ultraviolet absorber in the present composition is preferably 0.05 to 10 parts by weight, more preferably 0.05 to 3 parts by weight, based on 100 parts by weight of the thermoplastic resin (A). When the present composition contains two or more ultraviolet absorbers, the content of the ultraviolet absorbers refers to the total amount thereof.

[0068] The light stabilizer can be used to prevent the molded article from yellowing due to ultraviolet light when used outdoors, etc. Examples of the light stabilizer include one or more selected from the group consisting of tetrakis(1,2,2,6,6-pentamethyl-4-piperidyl)butane-1,2,3,4-tetracarboxylate; tetrakis(2,2,6,6-tetramethyl-4-piperidyl)butane-1,2,3,4-tetracarboxylate; a mixed ester of 1,2,3,4-butanetetracarboxylic acid, 1,2,3,6,6-pentamethyl-4-piperidinol, and 3,9-bis(2-hydroxy-1,1-dimethylethyl)-2,4,8,10-tetraoxaspiro[5.5]undecane; and bis(2,2,6,6-tetramethyl-4-piperidyl)sebacate.

[0069] From the viewpoint of weather resistance stability, the light stabilizer is preferably a mixed ester of 1,2,3,4-butanetetracarboxylic acid, 1,2,3,6,6-pentamethyl-4-piperidinol, and 3,9-bis(2-hydroxy-1,1-dimethylethyl)-2,4,8,10-tetraoxaspiro[5.5]undecane. One or more types of light stabilizers can be used.

[0070] The content of the light stabilizer in the present composition is preferably 0.05 to 10 parts by weight, more preferably 0.05 to 3 parts by weight, based on 100 parts by weight of the thermoplastic resin (A). When the present composition contains two or more light stabilizers, the content of the light stabilizers refers to the total amount thereof.

[0071] Examples of antistatic agents other than the ionic liquid (B) and the donor-acceptor compound (C) include ammonium salt-based ionic liquids such as tributylmethylammonium bis(trifluoromethylsulfonyl)imide (manufactured by 3M Japan Limited, "FC-4400"); pyridinium salt-based ionic liquids such as N-butyl-3-methylpyridinium bis(trifluoromethylsulfonyl)imide (manufactured by Nippon Carlit Co., Ltd., "CIL-312"); imidazolium salt-based ionic liquids; pyrrolidinium salt-based ionic liquids; lithium bistrifluoromethanesulfonylimide / polyether polyol (Sanko Co., Ltd., "Sanko Co., Ltd."); Examples of the other antistatic agents include lithium ionic liquids such as "PEO-20R" manufactured by Taisei Chemical Industry Co., Ltd.; polymeric antistatic agents having a quaternary ammonium salt in the side chain ("1SX-1090" and "1WX-1020-NS" manufactured by Taisei Fine Chemical Co., Ltd.); glycerin fatty acid esters such as diglycerin monolaurate ("Poem DL-100" manufactured by Riken Vitamin Co., Ltd.); and polymeric permanent antistatic agents ("Pelectron HS," "Pelectron AS," and "Pelestat NC6321" manufactured by Sanyo Chemical Industries, Ltd., and "Adekastab AS-302" manufactured by ADEKA Corporation). One or more of the other antistatic agents can be used.

[0072] Examples of the plasticizer include one or more selected from the group consisting of polyethylene glycol, polyamide oligomer, ethylene bisstearamide, phthalate ester, adipate ester, polystyrene oligomer, polyethylene wax, and mineral oil. One or more plasticizers can be used.

[0073] Examples of the release agent include one or more selected from the group consisting of polyethylene wax, silicone oil, stearyl phosphite, long-chain carboxylic acid, metal salt of long-chain carboxylic acid, and higher fatty acid ester of monohydric or polyhydric alcohol. One or more types of the release agent can be used.

[0074] Examples of the flame retardant include one or more selected from the group consisting of phosphorus-based flame retardants such as bisphenol A bis(diphenyl phosphite), tricresyl phosphate, triphenyl phosphate, and tris-3-chloropropyl phosphate; bromine-based flame retardants such as 2,2-bis[4-(3,3-dibromopropoxyl)-3,5-dibromophenyl]propane, bis(3,5-dibromo-4-dibromopropyloxyphenyl)sulfone, ethylene bispentabromobenzene, and hexabromocyclododecane; silicone-based flame retardants; and hydroxide-based flame retardants such as magnesium hydroxide and aluminum hydroxide. One or more types of flame retardants can be used.

[0075] Examples of the flame retardant aid include antimony compounds such as antimony trioxide, etc. One or more types of flame retardant aids may be used.

[0076] The present composition may have the composition shown below. In the following composition, the content of each component may be within the range described above. The present composition shown below may further contain other components described above.

[0077] (Composition 1) The present composition may contain an olefin-based resin as the thermoplastic resin (A), an ionic liquid (B), a compound (1) as the donor-acceptor compound (C), cellulose fibers (D), and an olefin-based compatibilizing resin as the compatibilizing resin (E).

[0078] (Composition 2) The present composition may contain an olefin-based resin as the thermoplastic resin (A), an ionic liquid (B), cellulose fibers (D), and an olefin-based compatibilizing resin as the compatibilizing resin (E).

[0079] (Composition 3) The present composition may contain the thermoplastic resin (A) being an olefin-based resin, the compound (1) as the donor-acceptor compound (C), cellulose fiber (D), and an olefin-based compatibilizing resin as the compatibilizing resin (E).

[0080] (Composition 4) The present composition may contain, relative to 100 parts by weight of an olefin-based resin as the thermoplastic resin (A), 0.5 to 3.0 parts by weight of an ionic liquid (B), 0.5 to 3.0 parts by weight of a compound (1) as the donor-acceptor compound (C), 1.0 to 30 parts by weight of cellulose fiber (D), and 1.0 to 10 parts by weight of an olefin-based compatibilizing resin as the compatibilizing resin (E).

[0081] (Composition 5) The present composition may contain a thermoplastic resin (A) that is a styrene-based resin, an ionic liquid (B), a compound (1) that serves as a donor-acceptor compound (C), cellulose fibers (D), and a styrene-based compatibilizing resin that serves as a compatibilizing resin (E).

[0082] (Composition 6) The present composition may contain a thermoplastic resin (A) that is a styrene-based resin, an ionic liquid (B), cellulose fibers (D), and a styrene-based compatibilizing resin as a compatibilizing resin (E).

[0083] (Composition 7) The present composition may contain a thermoplastic resin (A) that is a styrene-based resin, a compound (1) that serves as a donor-acceptor compound (C), cellulose fibers (D), and a styrene-based compatibilizing resin that serves as a compatibilizing resin (E).

[0084] (Composition 8) The present composition may contain, relative to 100 parts by weight of a styrene-based resin as a thermoplastic resin (A), 0.5 to 3.0 parts by weight of an ionic liquid (B), 0.5 to 3.0 parts by weight of a compound (1) as a donor-acceptor compound (C), 1.0 to 30 parts by weight of cellulose fiber (D), and 1.0 to 10 parts by weight of an olefin-based compatibilizing resin as a compatibilizing resin (E).

[0085] Embodiment 2 (Molded Article) A molded article of this embodiment is formed using the present composition. As described above, the ionic liquid (B) and the donor-acceptor compound (C) are not easily lost from the molded article due to cleaning such as wiping of the surface or changes over time, and the molded article can continuously exhibit excellent antistatic properties and antifouling properties. The molded article can have antifouling properties in which both hydrophilic and hydrophobic dust particles are resistant to adhesion.

[0086] A molded article can be obtained by melt-kneading the present composition, pelletizing the pelletized product, and molding the resulting product using various molding methods. Alternatively, a molded article can be obtained by molding the melt-kneaded composition using an extruder without pelletizing it. Examples of molding methods include injection molding, injection compression molding, extrusion molding, profile extrusion, transfer molding, blow molding, gas-assisted blow molding, blow molding, in-mold coating (IMC) molding, rotational molding, multilayer molding, two-color molding, insert molding, sandwich molding, foam molding, pressure molding, and combinations of one or more of these.

[0087] The shape of the molded article is not particularly limited and can be selected depending on the application and intended use of the molded article. The shape of the molded article may be, for example, a plate, plate-like, rod-like, sheet-like, film-like, cylindrical, annular, circular, elliptical, polygonal, hollow, frame-like, box-like, panel-like, or a combination of one or more of these. The molded article may be, for example, a housing or part of various devices such as home appliances and office automation equipment, an automobile interior panel, a headlamp lens for automobiles such as motorcycles, or a lighting cover. The surface of the molded article may have a textured surface or a three-dimensional curved surface. The molded article may have a single-layer structure or a multi-layer structure. When the molded article has a multi-layer structure, at least one layer may be formed using the present composition, and all layers may be formed using the present composition.

[0088] Embodiment 3 (Method for Producing Thermoplastic Resin Composition) A method for producing the composition can include a step of kneading the components contained in the composition. The composition includes a thermoplastic resin (A), at least one of an ionic liquid (B) and the donor-acceptor compound (C), cellulose fibers (D), and a compatibilizing resin (E), and may also include other components as required.

[0089] The kneading method is preferably a physical blending method, such as one or more methods selected from the group consisting of melt kneading, solvent cast blending, latex blending, and polymer complexing. The kneading method is more preferably melt kneading. The melt kneading temperature may be selected depending on the components contained in the composition, and may be, for example, 180°C or higher and 320°C or lower.

[0090] The kneading device may be, for example, one or more selected from the group consisting of a tumbler, a Henschel mixer, a rotary mixer, a super mixer, a ribbon tumbler, and a V blender.

[0091] The method for producing the present composition may involve melt-kneading to obtain a kneaded product in which the components contained in the composition are uniformly dispersed, and then pelletizing the kneaded product. For pelletization, for example, one or more devices selected from the group consisting of a single-screw or multi-screw extruder, a Banbury mixer, a roller, a co-kneader, a blast mill, and a Prabender blauthograph may be used. These devices may be operated batchwise or continuously.

[0092] The method for producing the present composition may include a step of mixing pellets of the thermoplastic resin (A), at least one of the ionic liquid (B) and the donor-acceptor compound (C), cellulose fibers (D), and a compatibilizing resin (E), and melt-kneading the mixture in the heating barrel of a molding machine (so-called mold blending).

[0093] Hereinafter, the present disclosure will be described in more detail with reference to examples and comparative examples, but the present disclosure is not limited to these examples.

[0094] [Examples 1 to 13, Comparative Examples 1 to 5] The components were mixed to obtain the compositions shown in Tables 1 to 4, and melt-kneaded at 180 to 220°C using a twin-screw kneading extruder ("TEX-26SX" manufactured by Shibaura Kogyo Co., Ltd.) to obtain 3 to 5 mm long pellets of the thermoplastic resin composition. The pellets were molded using an electric injection molding machine ("NEX110IV-9EG" manufactured by Nissei Plastic Industrial Co., Ltd.) to obtain flat pieces (100 mm long x 100 mm wide x 2 mm thick) as molded products. The injection molding conditions were a resin temperature of 200 to 240°C and a mold temperature of 50°C.

[0095] In Tables 1 to 4, each symbol indicates the following component: (Thermoplastic resin (A)) A-1: ​​Polypropylene resin (Novatec BC03B manufactured by Japan Polypropylene Corporation) A-2: Polypropylene resin (Novatec MA3H manufactured by Japan Polypropylene Corporation) A-3: Styrene resin (PS-J Polystyrene H8672 manufactured by PS Japan Corporation)

[0096] (Ionic Liquid (B)) B-1: Tributyldodecylphosphonium bis(trifluoromethanesulfonyl)imide (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) B-2: Tetrabutylphosphonium dodecylbenzenesulfonate ("Elecut S-418" manufactured by Takemoto Yushi Co., Ltd.) B-3: Tributyldodecylphosphonium bromide (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.)

[0097] (Donor-Acceptor Compound (C)) C-1: Compound (1) ("Biomicelle BN-105" manufactured by Boron Laboratory Co., Ltd.)

[0098] (Cellulose fibers (D)) D-1: "Nanoforest" manufactured by Chuetsu Pulp Industries Co., Ltd. D-2: "CellFim P" manufactured by Mori Machinery Corporation D-3: "GS CNF" manufactured by GS Alliance Co., Ltd. D-4: "ARBOCEL" manufactured by Rettenmeyer Japan Co., Ltd. All of D-1 to D-3 above had an average fiber diameter in the range of 3 nm or more and 200 nm or less and an average fiber length in the range of 100 nm or more and 1000 nm or less, and D-4 above had an average fiber diameter in the range of 1 μm or more and 50 μm or less and an average fiber length in the range of 10 μm or more and 400 μm or less.

[0099] (Compatibilizing resin (E)) E-1: Olefin-based compatibilizing resin ("SCONA TPPP 9212" manufactured by BYK Japan Co., Ltd.) E-2: Olefin-based compatibilizing resin ("UMEX 1010" manufactured by Sanyo Chemical Industries, Ltd.) E-3: Styrenic-based compatibilizing resin ("TR2003" manufactured by JSR Corporation)

[0100] The materials used in the Examples and Comparative Examples, and the flat plates of the resin compositions obtained in the Examples and Comparative Examples, were evaluated according to the following procedures.

[0101] [Measurement of average fiber diameter and average fiber length of cellulose fiber (D)] The flat plate pieces (100 mm length × 100 mm width × 2 mm thickness) prepared in the Examples and Comparative Examples were divided into two or four equal pieces. The divided pieces were freeze-fractured in liquid nitrogen to prepare fracture surfaces. Platinum was vapor-deposited on the fracture surfaces to obtain evaluation test pieces. The vapor-deposited surface of the evaluation test piece was observed using a scanning electron microscope, and the fiber diameters and fiber lengths of 50 or more cellulose fibers within the field of view were measured, and the average values ​​were used to determine the average fiber diameter and average fiber length.

[0102] [Accelerated Test] An accelerated test was performed on a flat plate specimen, simulating an actual usage environment. The accelerated test was performed in accordance with JIS K7368:1999. In this JIS standard, when estimating the relationship between life and temperature, the recommended test temperature is set at 100 to 150°C. Therefore, in this test, the test temperature was set at 100°C and the test time was set at 800 hours.

[0103] [Measurement of Surface Resistivity] Using a resistivity meter ("Hiresta UP MCP-HT450" manufactured by Mitsubishi Chemical Analytech Co., Ltd.), the surface resistivity of the flat plate was measured before (initial) and after the accelerated test under the test conditions shown below. The smaller the surface resistivity value, the better the antistatic properties. The results are shown in Tables 1 to 4. (Test conditions) Voltage: 1000 V Time: 60 seconds Temperature: 23°C Relative humidity: 50%

[0104] [Evaluation of Dust Adhesion] For the evaluation of dust adhesion, powders conforming to "Test Powders and Test Particles" of JIS Z8901: 2006 were used. Kanto loam (JIS test powder type 11) was used as the hydrophilic dust, and carbon black (JIS test powder type 12) was used as the hydrophobic dust.

[0105] Using hydrophilic and hydrophobic dusts, the dust adhesion of each plate was evaluated before (initial) and after the accelerated test according to the following procedure. 5 g of dust was sprayed onto the surface (one side) of the plate, and the surface of the plate was observed at 100x magnification using a digital microscope (Keyence Corporation, "VHX-5000"), and the dust adhesion rate (the percentage of the area covered with dust) was determined by image processing. Evaluation criteria (1) and (2) were used to evaluate the dust adhesion rate. The results are shown in Tables 1 to 4.

[0106] (Evaluation Criteria (1)) A: The dust adhesion rate on the surface of the flat plate piece is less than 4%. B: The dust adhesion rate on the surface of the flat plate piece is 4% or more.

[0107] (Evaluation Criteria (2)) A: The dust adhesion rates of hydrophilic and hydrophobic dust on the surface of the flat piece both initially and after the accelerated test are less than 5%. B: The dust adhesion rates of hydrophilic and hydrophobic dust on the surface of the flat piece both initially and after the accelerated test are 5% or more.

[0108]

[0109]

[0110]

[0111]

[0112] It can be seen that the molded articles obtained in Examples 1 to 13 are able to continuously exhibit excellent antistatic properties and antifouling properties. The molded articles obtained in Comparative Examples 1, 2, 4, and 5 were formed using compositions that did not contain cellulose fiber (D), and therefore showed increased surface resistivity and poor dust adhesion evaluations after the accelerated test. The molded article obtained in Comparative Example 3 contained cellulose fiber (D) but did not contain ionic liquid (B) or donor-acceptor compound (C), and therefore showed a high surface resistivity and poor antistatic properties.

[0113] The embodiments and examples disclosed herein should be considered to be illustrative in all respects and not restrictive. The scope of the present disclosure is defined by the claims, not the above description, and is intended to include all modifications within the meaning and scope of the claims.

Claims

1. A thermoplastic resin composition comprising a thermoplastic resin (A), at least one of an ionic liquid (B) and a donor-acceptor compound (C), cellulose fibers (D), and a compatibilizing resin (E), wherein the thermoplastic resin (A) is at least one of an olefin-based resin and a styrene-based resin, the ionic liquid (B) is a phosphonium salt, the cellulose fibers (D) have an average fiber diameter of 3 nm or more and 50 μm or less, and the cellulose fibers (D) have an average fiber length of 100 nm or more and 400 μm or less, and the compatibilizing resin (E) is a resin different from the thermoplastic resin (A) and serves to compatibilize the thermoplastic resin (A) and the cellulose fibers (D).

2. The thermoplastic resin composition according to claim 1, wherein the ionic liquid (B) is one or more selected from the group consisting of tributyldodecylphosphonium bis(trifluoromethanesulfonyl)imide, tributyldodecylphosphonium bromide, and tetrabutylphosphonium dodecylbenzenesulfonate.

3. The thermoplastic resin composition according to claim 1 or 2, wherein the donor-acceptor compound (C) is a compound represented by the following formula (1):

4. The thermoplastic resin composition according to any one of claims 1 to 3, wherein the cellulose fibers (D) include at least one of nanofibers and microfibers, the nanofibers have an average fiber diameter of 3 nm or more and 200 nm or less and an average fiber length of 100 nm or more and 1000 nm or less, and the microfibers have an average fiber diameter of 1 μm or more and 50 μm or less and an average fiber length of 10 μm or more and 400 μm or less.

5. A thermoplastic resin composition according to any one of claims 1 to 4, wherein the thermoplastic resin (A) comprises a polypropylene-based resin, and the compatibilizing resin (E) comprises a maleic anhydride-modified polypropylene resin.

6. The thermoplastic resin composition according to any one of claims 1 to 5, wherein the thermoplastic resin (A) contains a styrene-based resin, and the compatibilizing resin (E) contains a styrene-based elastomer.

7. The surface resistivity of a flat plate piece formed from the above thermoplastic resin composition into a size of 100 mm length × 100 mm width × 2 mm thickness at a temperature of 23°C and a relative humidity of 50% is 1.0 × 10 12 The thermoplastic resin composition according to any one of claims 1 to 6, having a modulus of elasticity of Ω / sq or less.

8. A thermoplastic resin composition according to any one of claims 1 to 7, wherein, relative to 100 parts by weight of the thermoplastic resin (A), when the ionic liquid (B) is contained, the content of the ionic liquid (B) is 0.5 parts by weight or more and 3.0 parts by weight or less, when the donor-acceptor compound (C) is contained, the content of the donor-acceptor compound (C) is 0.5 parts by weight or more and 3.0 parts by weight or less, the content of the cellulose fiber (D) is 1.0 part by weight or more and 30 parts by weight or less, and the content of the compatibilizing resin (E) is 1.0 part by weight or more and 10 parts by weight or less.

9. The thermoplastic resin composition according to any one of claims 1 to 8, comprising both the ionic liquid (B) and the donor-acceptor compound (C).

10. A molded article formed using the thermoplastic resin composition according to any one of claims 1 to 9.

11. A method for producing a thermoplastic resin composition according to any one of claims 1 to 9, comprising melt-kneading the thermoplastic resin (A), at least one of the ionic liquid (B) and the donor-acceptor compound (C), the cellulose fibers (D), and the compatibilizing resin (E).

Citation Information

Patent Citations

  • Exterior part for vehicle

    JP2019064403A

  • Manufacturing method of resin composition, and manufacturing method of molded body using the resin composition

    JP2019189758A

  • Antistatic resin composition, method for producing antistatic resin composition, and electronic component packaging material

    JP2021193169A

  • Method for stabilizing propylene-based resin

    JP2021193182A