Solid electrolyte and lithium ion battery
The solid electrolyte composition with specific cations and oxygen improves stability and conductivity, addressing the limitations of existing electrolytes by maintaining high ionic conductivity and safety in lithium ion batteries without heat treatment.
Patent Information
- Application Number
- PCT/JP2023/012623
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-28
- Publication Date
- 2024-10-03
AI Technical Summary
Existing solid electrolytes for lithium ion batteries exhibit low stability and moisture resistance, which affects their ionic conductivity and reliability, particularly at room temperature.
A solid electrolyte composition containing lithium (Li), Zr or Hf, Ta, Gd, Yb, Dy, Er, or Sc, and oxygen, with specific molar ratios, is developed to enhance both ionic conductivity and stability, using a combination of tetravalent, pentavalent, and trivalent cations along with chlorine and oxygen, which is synthesized through mechanochemical milling.
The electrolyte achieves high initial ionic conductivity and stability without requiring heat treatment, maintaining conductivity and safety in dry environments, suitable for all-solid-state lithium ion batteries.
Smart Images

Figure JP2023012623_03102024_PF_FP_ABST
Abstract
Description
Solid Electrolyte and Lithium-Ion Batteries
[0001] The present invention relates to a solid electrolyte and a lithium-ion battery.
[0002] In recent years, there has been a strong demand for smaller size and improved reliability (safety) of batteries that serve as power sources for electronic devices. Therefore, all-solid-state batteries using solid electrolytes have attracted attention. Halides are known as sulfur-free solid electrolytes, and Li 3 YCl 6 exhibits high Li ion conductivity at room temperature (see, for example, Japanese Patent No. 6934626 (Reference 1)). In addition, in International Publication No. 2020 / 070956 (Reference 2), Li 6-4b+ab (Zr 1-a M a ) b X 6 A halide solid electrolyte material represented by the formula (I) is disclosed. Here, M is at least one element selected from the group consisting of Al, Ga, Bi, Sc, Sm, and Sb, and X is a halogen element, and 0<a<1 and 0<b<1.5 are satisfied. Furthermore, WO 2021 / 250985 (Document 3) discloses a solid electrolyte material containing Li, M, O, and X. Here, M is at least one element selected from the group consisting of Ti, Zr, and Hf, and X is at least one element selected from the group consisting of Cl, Br, and I.
[0003] As mentioned above, Li 3 YCl 6 Chloride electrolytes such as Li2O4 and Li2O5 exhibit high ionic conductivity at room temperature, but no information is disclosed regarding their stability. The present inventors prepared the solid electrolytes disclosed in the above-mentioned documents 1 to 3 and placed them in a dry room with a controlled dew point of -40°C. However, they found that the electrolyte decomposed and could not maintain its initial ionic conductivity, i.e., its stability (or moisture resistance) was low. Therefore, in order to improve the stability of chloride electrolytes, the present inventors have investigated the use of Li2O4 and Li2O5 as the solid electrolytes. x MCl 6In this study, materials were prepared by combining various cations (M) to search for combinations of cations with high stability. As a result, as described below in the related art, combinations of cations exhibiting high initial conductivity and high stability were identified. However, the ionic conductivity and stability of solid electrolytes in the related art are not necessarily sufficient.
[0004] The present invention is directed to a solid electrolyte, and has an object to provide a solid electrolyte having high ionic conductivity and high stability.
[0005] A first aspect of the invention is a solid electrolyte comprising Li, Mα, Mβ, Mγ, Cl, and O, wherein Mα is at least one element selected from the group consisting of Zr and Hf, Mβ is at least one element selected from the group consisting of Ta and Nb, and Mγ is at least one element selected from the group consisting of Gd, Yb, Dy, Er, Ho, Eu, and Sc.
[0006] According to the present invention, it is possible to provide a solid electrolyte having high ionic conductivity and high stability.
[0007] A second aspect of the present invention is the solid electrolyte of the first aspect, in which Mα includes Zr.
[0008] A third aspect of the present invention is the solid electrolyte of the first or second aspect, in which Mβ contains Ta.
[0009] A fourth aspect of the present invention is the solid electrolyte according to any one of the first to third aspects, in which Mγ includes Gd, Yb, or Er.
[0010] A fifth aspect of the present invention is the solid electrolyte of any one of the first to fourth aspects, which is represented by the following composition formula (1): Li6-(4+a-b)(1+c)(Mα (1-a-b) Mβ a Mγ b ) 1+c Cl 6-2d O d ...(1) 0<a, 0<b, a+b<1, -0.2≦c≦0.2, and 0<d<3 are satisfied.
[0011] A sixth aspect of the invention is a lithium ion battery including the solid electrolyte of any one of the first to fifth aspects.
[0012] The above and other objects, features, aspects and advantages will become more apparent from the following detailed description of the invention which proceeds with reference to the accompanying drawings.
[0013] FIG. 1 is a longitudinal sectional view showing an all-solid-state lithium ion secondary battery.
[0014] First, a solid electrolyte according to a related art of the present invention will be described. The solid electrolyte according to the related art is a lithium (Li) ion conductive material that contains lithium (Li), three other metal elements (Mα, Mβ, Mγ) that become cations, and chlorine (Cl).
[0015] Mα is an element that becomes a tetravalent cation and is at least one element selected from the group consisting of zirconium (Zr) and hafnium (Hf). Mβ is an element that becomes a pentavalent cation and is at least one element selected from the group consisting of tantalum (Ta) and niobium (Nb). Mγ is an element that becomes a trivalent cation and is at least one element selected from the group consisting of gadolinium (Gd), ytterbium (Yb), dysprosium (Dy), erbium (Er), holmium (Ho), europium (Eu), and scandium (Sc). The solid electrolyte containing at least one trivalent, tetravalent, and pentavalent element in addition to Li as a cation achieves high initial conductivity and high stability.
[0016] A preferred example of the solid electrolyte according to the related art is a compound represented by the following composition formula: Li6-(4+a-b)(1+c)(Mα (1-a-b) Mβ a Mγ b ) 1+c Cl 6 The conditions 0<a, 0<b, a+b<1, and −0.2≦c≦0.2 are satisfied.
[0017] Next, a solid electrolyte according to one embodiment of the present invention will be described. The solid electrolyte is a Li ion conductive material, and is obtained by adding oxygen (O) to the solid electrolyte according to the related art. The solid electrolyte is used, for example, in the manufacture of an all-solid-state secondary battery. The solid electrolyte contains Li, three other metal elements (Mα, Mβ, Mγ) that become cations, Cl, and O. The solid electrolyte may be composed only of Li, Mα, Mβ, Mγ, Cl, and O.
[0018] As with the solid electrolytes according to the related art, Mα is an element that forms a tetravalent cation and is at least one element selected from the group consisting of Zr and Hf. Mβ is an element that forms a pentavalent cation and is at least one element selected from the group consisting of Ta and Nb. Mγ is an element that forms a trivalent cation and is at least one element selected from the group consisting of Gd, Yb, Dy, Er, Ho, Eu, and Sc. A solid electrolyte containing at least one trivalent, one tetravalent, and one pentavalent element in addition to Li as a cation, and further containing Cl and O, as described below, achieves higher ionic conductivity and higher stability than solid electrolytes according to the related art. Furthermore, since this solid electrolyte does not generate hydrogen sulfide gas, it is possible to provide an all-solid-state secondary battery that is highly safe.
[0019] In order to more reliably achieve high ionic conductivity and high stability in the solid electrolyte according to this embodiment, Mα preferably contains Zr, and Mα may consist of only Zr. Furthermore, Mβ preferably contains Ta, and Mβ may consist of only Ta. Furthermore, Mγ preferably contains Gd, Yb, or Er, and Mγ may consist of only Gd, Yb, or Er. Mγ may contain two or more elements of Gd, Yb, and Er. The amount of substance of Li is, for example, greater than the amount of substance of any of Mα, Mβ, and Mγ, and preferably greater than the total amount of substance of Mα, Mβ, and Mγ. The amount of substance of Cl is, for example, greater than the total amount of substance of Li, Mα, Mβ, and Mγ. The amount of substance of O is, for example, less than half the amount of substance of Cl, and preferably less than one-quarter the amount of substance of Cl.
[0020] A preferred solid electrolyte is a compound represented by the following composition formula (1): Li6-(4+a-b)(1+c)(Mα (1-a-b) Mβ a Mγ b ) 1+c Cl 6-2d O d ... (1) 0<a, 0<b, a+b<1, -0.2≦c≦0.2, and 0<d<3 are satisfied. Regarding a and b, 0.1≦a≦0.5 and 0.1≦b≦0.4 may be satisfied. Furthermore, 0.2≦a+b≦0.8 may be satisfied. Regarding the relationship between a and b, a≧b is, for example, a<b, but a<b may also be satisfied. Regarding c, -0.1≦c≦0.1 may be satisfied, or c may be 0. Regarding d, 0<d<1 may be satisfied. Preferably, 0<d<0.5 is satisfied, and more preferably, 0<d≦0.4 is satisfied. The lower limit of d may be 0.1. The solid electrolyte may be crystalline or amorphous.
[0021] When determining whether an unknown solid electrolyte is the solid electrolyte according to the present embodiment, chemical analysis is performed on the unknown solid electrolyte to determine whether the constituent elements are Li, Mα, Mβ, Mγ, Cl, and O. When determining whether the unknown solid electrolyte is of the composition formula (1), Li, Mα, Mβ, and Mγ can be quantified, for example, by ICP-emission spectroscopy. Cl can be quantified, for example, by ion chromatography. O can be quantified, for example, by ONH analysis using an oxygen, nitrogen, and hydrogen analyzer.
[0022] The molar ratio of Li, Mα, Mβ, Mγ, Cl, and O in the composition formula (1) is Li:Mα:Mβ:Mγ:Cl:O=6-(4+a-b)(1+c):(1-a-b)(1+c):a(1+c):b(1+c):6-2d:d. In the molar ratio determined by analysis of an unknown solid electrolyte, if the Li value is 0.90 × {6-(4+a-b)(1+c)} or more and 1.10 × {6-(4+a-b)(1+c)} or less, it is considered that the Li satisfies the composition formula (1). It is more preferable that the Li value is 0.95 × {6-(4+a-b)(1+c)} or more and 1.05 × {6-(4+a-b)(1+c)} or less. The same applies to Mα, Mβ, Mγ, Cl, and O.
[0023] The solid electrolyte according to this embodiment is manufactured, for example, by the following method. First, a powder of a compound containing Li, a powder of a compound containing Mα, a powder of a compound containing Mβ, and a powder of a compound containing Mγ are prepared. Some of these compounds are chlorides, and the remaining compounds are oxides. Oxides and chlorides containing the same metal element may be prepared. The chloride containing Li is, for example, LiCl, and the oxide containing Li is, for example, Li 2 O. Chlorides containing Mα are, for example, MαCl 4 and the oxide containing Mα is, for example, MαO 2 The chloride containing Mβ is, for example, MβCl 5 and the oxide containing Mβ is, for example, Mβ 2 O 5 The chloride containing Mγ is, for example, MγCl 3 and the oxide containing Mγ is, for example, Mγ 2 O 3 These powders are weighed and mixed to obtain a predetermined molar ratio.
[0024] Next, the mixture is milled (mechanochemical milling). Here, a planetary ball mill is used as an example of the milling process. In a planetary ball mill, the pot rotates on its axis while the stage carrying the pot revolves, making it possible to generate very high impact energy. The milling process may also be performed using other types of grinders. The solid electrolyte according to this embodiment is obtained by the milling process. This solid electrolyte is used to manufacture the positive electrode layer 112, the negative electrode layer 122, or the electrolyte layer 13 in the all-solid-state secondary battery 1 (see FIG. 1 ), which will be described later. In this example, the milling process is performed at room temperature, but the temperature and other conditions may be changed as appropriate. The solid electrolyte according to this embodiment may also be manufactured by a process other than milling, such as firing.
[0025] FIG. 1 is a longitudinal cross-sectional view showing an all-solid-state lithium-ion secondary battery 1 (hereinafter simply referred to as "all-solid-state secondary battery 1"). The all-solid-state secondary battery 1 uses a solid electrolyte according to the present embodiment. The all-solid-state secondary battery 1 includes, from top to bottom in FIG. 1 , a positive electrode 11, an electrolyte layer 13, and a negative electrode 12. That is, the electrolyte layer 13 is provided between the positive electrode 11 and the negative electrode 12. The electrolyte layer 13 is a solid electrolyte layer and also serves as a separator layer. The electrolyte layer 13 is made of or includes the solid electrolyte according to the present embodiment. The positive electrode 11 includes a current collector 111 and a positive electrode layer 112. The positive electrode layer 112 includes a positive electrode active material. The negative electrode 12 includes a current collector 121 and a negative electrode layer 122. The negative electrode layer 122 includes a negative electrode active material.
[0026] The positive electrode active material of the positive electrode layer 112 preferably contains a lithium composite oxide. A preferred positive electrode active material is a lithium composite oxide having a layered rock salt structure, such as NCM (Li(Ni, Co, Mn)O 2 The positive electrode active material may be other lithium composite oxides, for example, NCA (Li(Ni, Co, Al)O) having a layered rock salt structure. 2 ), LCO (LiCoO 2 ), LNMO (LiNi) having a spinel structure 0.5 Mn 1.5 O 4 ), LFP (LiFePO) having an olivine structure4 ) or the like. The positive electrode layer 112 includes the solid electrolyte according to the present embodiment in addition to the positive electrode active material. The positive electrode layer 112 may further include an electron conduction assistant (carbon black, etc.). An example of the positive electrode layer 112 is one in which these materials are integrated by applying pressure or heat.
[0027] The negative electrode active material of the negative electrode layer 122 is, for example, LTO (Li 4 Ti 5 O 12 ), NTO(Nb 2 TiO 7 ), TiO 2 Examples of the materials include compounds such as titanium oxide (TiO 2 ), graphite, and SiO 2 (silicon monoxide). The anode layer 122 includes the solid electrolyte according to this embodiment in addition to the anode active material. The anode layer 122 may further include an electron conduction aid (carbon black, etc.). An example of the anode layer 122 is one in which these materials are integrated by applying pressure or heat. The configurations and materials of the positive electrode 11 and the negative electrode 12 of the all-solid-state secondary battery 1 are not limited to those described above, and various other configurations and materials can be used.
[0028] Next, examples and comparative examples of solid electrolytes will be described. Tables 1 to 5 show the compositions and evaluation results of the solid electrolytes of Examples 1 to 8 and Comparative Examples 1 to 6. The solid electrolytes of Comparative Examples 1 and 3 to 6 are solid electrolytes according to the related art described above.
[0029]
[0030]
[0031]
[0032]
[0033]
[0034] Example 1 [Preparation of Electrolyte] In an argon atmosphere having a dew point of −60° C. or less, LiCl, ZrCl 4 , TaCl 5 and Gd 2 O 3 LiCl:ZrCl 4 : TaCl5 : Gd 2 O 3 The raw material powders were weighed to have a molar ratio of 1.7:0.5:0.4:0.05, and then pulverized and mixed in a mortar. The resulting mixed powder was placed in a zirconia pot and milled at 300 rpm for 20 hours using a planetary ball mill to obtain a solid electrolyte powder.
[0035] [Exposure Test] The solid electrolyte powder was placed in a petri dish and allowed to stand (expose) for 16 hours in a dry room controlled at a dew point of -40°C.
[0036] [Conductivity Measurement] The solid electrolyte powder was placed in a mold consisting of a resin sleeve and upper and lower punches made of stainless steel (SUS), and uniaxial press molding was performed under a pressure of 150 MPa. Lead wires were connected to the upper and lower punches, and impedance measurements were performed at room temperature to calculate the lithium ion conductivity (hereinafter also simply referred to as "ionic conductivity").
[0037] [Stability Evaluation] The impedance of the solid electrolyte powder immediately after milling in a planetary ball mill (after synthesis) and the solid electrolyte powder exposed to a dry room for 16 hours was measured, and the ionic conductivity was calculated. In Table 1, the ionic conductivity of the solid electrolyte powder immediately after milling (i.e., initial conductivity) is shown in the "After Synthesis" column, and the ionic conductivity of the solid electrolyte powder exposed to a dry room for 16 hours is shown in the "16-Hour Exposure" column (similar to Tables 2 to 5). In addition, the stability evaluation involved calculating the ionic conductivity retention rate. The ionic conductivity retention rate after 16 hours of exposure was calculated by (100 × (ionic conductivity after 16 hours of exposure) / (ionic conductivity after synthesis)). It can be said that the higher the retention rate, the higher the stability (moisture resistance).
[0038] Example 2 In the electrolyte preparation of Example 1, LiCl, Li 2 O, ZrCl 4 , TaCl 5 and Gd 2 O 3 But LiCl:Li 2 O: ZrCl 4 : TaCl 5 : Gd 2 O 3An electrolyte was prepared in the same manner as in Example 1 except that the components were weighed out so as to have a molar ratio of 1.4:0.15:0.5:0.4:0.05, and then tested and evaluated.
[0039] Example 3 In the electrolyte preparation of Example 1, LiCl, Li 2 O, ZrCl 4 , TaCl 5 and Gd 2 O 3 But LiCl:Li 2 O: ZrCl 4 : TaCl 5 : Gd 2 O 3 An electrolyte was prepared in the same manner as in Example 1 except that the components were weighed so as to have a molar ratio of 1.0:0.35:0.5:0.4:0.05, and then tested and evaluated.
[0040] Example 4 In the electrolyte preparation of Example 1, LiCl, Li 2 O, ZrCl 4 , TaCl 5 and Gd 2 O 3 But LiCl:Li 2 O: ZrCl 4 : TaCl 5 : Gd 2 O 3 An electrolyte was prepared in the same manner as in Example 1 except that the components were weighed so as to have a molar ratio of 0.5:0.6:0.5:0.4:0.05, and tests and evaluations were carried out.
[0041] Example 5 In the electrolyte preparation of Example 1, LiCl and ZrCl were used as raw material powders. 4 , TaCl 5 , GdCl 3 and Gd 2 O 3 LiCl:ZrCl 4 : TaCl 5 : GdCl 3 : Gd 2 O 3 An electrolyte was prepared in the same manner as in Example 1 except that the components were weighed out so as to have a molar ratio of 2.0:0.6:0.2:0.1:0.05, and then tested and evaluated.
[0042] Example 6 In the electrolyte preparation of Example 1, LiCl and ZrCl were used as raw material powders. 4 , TaCl 5 and Gd 2 O 3 LiCl:ZrCl 4 : TaCl 5 : Gd 2 O 3 An electrolyte was prepared in the same manner as in Example 1 except that the components were weighed so as to have a molar ratio of 1.9:0.5:0.3:0.1, and then tested and evaluated.
[0043] Example 7 In the electrolyte preparation of Example 1, LiCl, Li 2 O, ZrCl 4 , TaCl 5 and YbCl 3 But LiCl:Li 2 O: ZrCl 4 : TaCl 5 : YbCl 3 An electrolyte was prepared in the same manner as in Example 1 except that the components were weighed out so as to have a molar ratio of 1.7:0.15:0.6:0.2:0.2, and then tested and evaluated.
[0044] Example 8 In the electrolyte preparation of Example 1, LiCl, Li 2 O, ZrCl 4 , TaCl 5 and ErCl 3 But LiCl:Li 2 O: ZrCl 4 : TaCl 5 : ErCl 3 An electrolyte was prepared in the same manner as in Example 1 except that the components were weighed out so as to have a molar ratio of 1.15:0.3:0.25:0.5:0.25, and then tested and evaluated.
[0045] Comparative Example 1 In the electrolyte preparation of Example 1, LiCl, ZrCl 4 , TaCl 5 and GdCl 3 LiCl:ZrCl 4 : TaCl 5 : GdCl 3An electrolyte was prepared in the same manner as in Example 1 except that the components were weighed so as to have a molar ratio of 1.7:0.5:0.4:0.1, and then tested and evaluated.
[0046] Comparative Example 2 In the electrolyte preparation of Example 1, LiCl and ZrCl were used as raw material powders. 4 and TiO 2 LiCl:ZrCl 4 : TiO 2 An electrolyte was prepared in the same manner as in Example 1 except that the components were weighed so as to have a molar ratio of 2.0:0.7:0.3, and then tested and evaluated.
[0047] Comparative Example 3 In the electrolyte preparation of Example 1, LiCl and ZrCl were used as raw material powders. 4 , TaCl 5 and GdCl 3 LiCl:ZrCl 4 : TaCl 5 : GdCl 3 An electrolyte was prepared in the same manner as in Example 1 except that the components were weighed so as to have a molar ratio of 2.0:0.6:0.2:0.2, and then tested and evaluated.
[0048] Comparative Example 4 In the electrolyte preparation of Example 1, LiCl, ZrCl 4 , TaCl 5 and GdCl 3 LiCl:ZrCl 4 : TaCl 5 : GdCl 3 An electrolyte was prepared in the same manner as in Example 1 except that the components were weighed out so as to have a molar ratio of 1.9:0.5:0.3:0.2, and then tested and evaluated.
[0049] Comparative Example 5 In the electrolyte preparation of Example 1, LiCl, ZrCl 4 , TaCl 5 and YbCl 3 LiCl:ZrCl 4 : TaCl 5 : YbCl 3 An electrolyte was prepared in the same manner as in Example 1 except that the components were weighed so as to have a molar ratio of 2.0:0.6:0.2:0.2, and then tested and evaluated.
[0050] Comparative Example 6 In the electrolyte preparation of Example 1, LiCl, ZrCl 4 , TaCl 5 and ErCl 3 LiCl:ZrCl 4 : TaCl 5 : ErCl 3 An electrolyte was prepared in the same manner as in Example 1 except that the components were weighed so as to have a molar ratio of 1.75:0.25:0.5:0.25, and then tested and evaluated.
[0051] As shown in Table 1, the solid electrolytes of Examples 1 to 4, which had the same composition ratio of Li, Zr, Ta, and Gd but different O ratios, all had an ionic conductivity of 9.3 × 10 after synthesis. -4 S / cm or more, and the ionic conductivity after 16 hours of exposure was 2.7 × 10 -4 The ionic conductivity was 1.5 S / cm or more, and the ionic conductivity retention rate was 18% or more. Thus, the solid electrolytes of Examples 1 to 4 containing O are materials that combine high ionic conductivity and high stability. In contrast, the solid electrolyte of Comparative Example 1, which had the same composition ratios of Li, Zr, Ta, and Gd as Examples 1 to 4 but did not contain O, had ionic conductivity after synthesis, ionic conductivity after 16 hours of exposure, and ionic conductivity retention rate lower than the values described above for Examples 1 to 4. Furthermore, the solid electrolyte of Comparative Example 2 contained Li, Zr, Cl, and O but did not contain Mβ or Mγ, and had ionic conductivity after synthesis, ionic conductivity after 16 hours of exposure, and ionic conductivity retention rate lower than the values described above for Examples 1 to 4. Therefore, in order to further increase ionic conductivity and stability, it can be said that it is important to contain at least one trivalent, one tetravalent, and one pentavalent element in addition to Li as a cation, and further contain O.
[0052] Tables 2 to 5 also compare Examples and Comparative Examples having the same composition ratio of Li, Mα, Mβ, and Mγ, and show that the solid electrolytes of Examples containing O had higher ionic conductivity after synthesis, higher ionic conductivity after 16 hours of exposure, and higher ionic conductivity retention rate than the solid electrolytes of Comparative Examples not containing O. Thus, at the same cation ratio, the above characteristics change depending on whether or not O is contained, and it was confirmed that the solid electrolytes containing O improved the above characteristics, although the extent of the improvement varied.
[0053] The reason why ionic conductivity improves after synthesis in solid electrolytes containing O is not entirely clear, but the introduction of O creates defects in the anion sites, causing distortion in the structure. This is thought to expand the paths through which Li ions move, improving ionic conductivity. In addition, the ionic radius of O is 1.40, which is smaller than the ionic radius of Cl, 1.81. The bond distance with cations is shorter for O, which has a smaller ionic radius, and the bonding strength between cations and O is thought to be stronger than the bonding strength between cations and Cl. It is presumed that this improvement in bonding strength improves the stability of the material.
[0054] It is believed that the mechanism by which the ionic conductivity and stability after synthesis are increased is the same regardless of the type of cation. Specifically, it is believed that when Hf, which becomes a tetravalent cation like Zr, is used instead of Zr or together with Zr, the ionic conductivity and stability are improved. The same is true when Nb, which becomes a pentavalent cation like Ta and has the same ionic radius as Ta, is used instead of Ta or together with Ta. Furthermore, the same is true when Dy, Ho, Eu and Sc, which become trivalent cations like Gd, Yb and Er and have ionic radii similar to Gd, Yb or Er, are used instead of Gd, Yb or Er or together with Gd, Yb or Er.
[0055] As described above, the solid electrolyte according to this embodiment contains Li, Mα, Mβ, Mγ, Cl, and O. Mα is at least one element selected from the group consisting of Zr and Hf. Mβ is at least one element selected from the group consisting of Ta and Nb. Mγ is at least one element selected from the group consisting of Gd, Yb, Dy, Er, Ho, Eu, and Sc.
[0056] Here, the solid electrolytes of Comparative Examples 1 and 3 to 6 are solid electrolytes according to the above-mentioned related art, and have an ionic conductivity of, for example, 1.0 × 10 at room temperature after synthesis. -4 When the solid electrolyte is left standing in a dry room for 16 hours, the ionic conductivity decreases, but by subsequent heat treatment at 150°C, the ionic conductivity increases to 1.0 x 10 -4 However, the solid electrolytes of Comparative Examples 1 and 3 to 6 require heat treatment to restore ionic conductivity, which consumes a lot of power during production of the solid electrolyte, resulting in increased production costs.
[0057] In contrast, in the solid electrolyte according to the present embodiment, by doping with oxygen atoms, the ionic conductivity (initial conductivity) after synthesis is higher than that of the solid electrolytes of Comparative Examples 1 and 3 to 6, and high ionic conductivity (for example, 1.0 × 10 -4 S / cm or more). As described above, the solid electrolyte according to the present embodiment exhibits little conductivity degradation and high stability, eliminating the need for heat treatment to restore ionic conductivity. As a result, lithium ion batteries can be easily manufactured by applying the solid electrolyte to existing battery manufacturing processes carried out in a dry room environment. It has also been confirmed that the ionic conductivity of the solid electrolyte according to the present embodiment is improved by performing the same heat treatment as in Comparative Examples 1 and 3 to 6.
[0058] A preferred solid electrolyte is represented by the following composition formula (1): Li6-(4+a-b)(1+c)(Mα (1-a-b) Mβ a Mγ b )1+c Cl 6-2d O d ... (1) 0<a, 0<b, a+b<1, -0.2≦c≦0.2, and 0<d<3 are satisfied. x MCl 6―2d O d By optimizing the oxygen content d and the type and combination of cations M in the chloride electrolyte represented by the formula (1), it is possible to more reliably realize a solid electrolyte having high ionic conductivity and high stability.
[0059] The solid electrolyte and all-solid-state secondary battery 1 can be modified in various ways.
[0060] The solid electrolyte containing Li, Mα, Mβ, Mγ, Cl, and O may not satisfy the above composition formula (1).
[0061] The solid electrolyte may be mixed with other substances (which may include Li) and used as an electrolyte material. In this case, the solid electrolyte is preferably the component with the largest mass ratio among the components contained in the electrolyte material, i.e., the main component. The mass ratio of the main component in the electrolyte material is preferably 50 mass% or more, more preferably 60 mass% or more, and even more preferably 70 mass% or more.
[0062] The solid electrolyte used in the all solid state secondary battery 1 does not necessarily need to be contained in all of the positive electrode 11, the negative electrode 12, and the electrolyte layer 13, but may be contained in at least one of the positive electrode 11, the negative electrode 12, and the electrolyte layer 13. Furthermore, the solid electrolyte may be used in batteries other than all solid state secondary batteries, and may be used for purposes other than batteries.
[0063] The configurations in the above-described embodiment and each modification may be combined as appropriate as long as they are not mutually contradictory.
[0064] While the invention has been particularly illustrated and described, it should be understood that the foregoing description is illustrative and not restrictive, and that numerous modifications and variations are possible without departing from the scope of the invention.
[0065] 1 All-solid-state lithium-ion secondary battery 11 Positive electrode 12 Negative electrode 13 Electrolyte layer
Claims
1. A solid electrolyte containing Li, Mα, Mβ, Mγ, Cl and O, wherein Mα is at least one element selected from the group consisting of Zr and Hf, Mβ is at least one element selected from the group consisting of Ta and Nb, and Mγ is at least one element selected from the group consisting of Gd, Yb, Dy, Er, Ho, Eu and Sc.
2. The solid electrolyte according to claim 1, wherein Mα contains Zr.
3. The solid electrolyte according to claim 1, wherein Mβ contains Ta.
4. The solid electrolyte according to claim 1, wherein Mγ contains Gd, Yb or Er.
5. The solid electrolyte according to claim 1, which is represented by the following compositional formula (1), Li6-(4 + a - b)(1 + c)(Mα (1-a-b) Mβ a Mγ b )( 1+c Cl 6-2d O d ...(1) A solid electrolyte in which 0 < a, 0 < b, a + b < 1, -0.2 ≤ c ≤ 0.2, and 0 < d < 3 are satisfied.
6. A lithium ion battery comprising the solid electrolyte according to any one of claims 1 to 5.
Citation Information
Patent Citations
Solid electrolyte material and battery
JP6934626B2
Halide solid electrolyte material and battery using this
WO2020070956A1
Solid electrolyte material, and battery in which same is used
WO2021250985A1
Oxide, method of preparing the same, solid electrolyte including the oxide, and electrochemical device including the oxide
US20210043966A1
Solid electrolyte, preparation method thereof, metal air battery including the same, and electrochemical device including the same