Solid electrolyte and lithium ion battery
The solid electrolyte composition, featuring specific metal and anion combinations, addresses stability and reduction resistance issues, resulting in improved performance and safety for lithium ion batteries by enhancing ionic conductivity and energy density.
Patent Information
- Application Number
- PCT/JP2023/012625
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-28
- Publication Date
- 2024-10-03
AI Technical Summary
Solid electrolytes used in lithium ion batteries face challenges with stability and reduction resistance, leading to decomposition and low moisture resistance, which affects the safety and energy density of all-solid-state batteries.
A solid electrolyte composition including Li, Mα, Mβ, Mγ, and Cl, where Mα is Zr or Hf, Mβ is Ta, and Mγ is Gd, Yb, Dy, Er, or Sc, combined with anions such as OH^- , AlO_2^-, SO_4^2-, and TFSI^- , which provides high ionic conductivity and stability, and is represented by the formula Li_(6-(4+a-b)(1+c)(Mα_(1-a-b)Mβ_aMγ_b)_1+cCl_6*n(Mδ_xA_y), optimizing the valence and molar ratios to enhance reduction resistance.
The optimized solid electrolyte achieves high ionic conductivity, stability, and improved reduction resistance, leading to enhanced safety and energy density in all-solid-state lithium ion batteries.
Smart Images

Figure JP2023012625_03102024_PF_FP_ABST
Abstract
Description
Solid Electrolyte and Lithium-Ion Batteries
[0001] The present invention relates to a solid electrolyte and a lithium-ion battery.
[0002] In recent years, there has been a strong demand for smaller size and improved reliability (safety) of batteries that serve as power sources for electronic devices. Therefore, all-solid-state batteries using solid electrolytes have attracted attention. Halides are known as sulfur-free solid electrolytes, and Li 3 YCl 6 exhibits high Li ion conductivity at room temperature (see, for example, Japanese Patent No. 6934626 (Reference 1)). In addition, in International Publication No. 2020 / 070956 (Reference 2), Li 6-4b+ab (Zr 1-a M a ) b X 6 Here, M is at least one element selected from the group consisting of Al, Ga, Bi, Sc, Sm, and Sb, X is a halogen element, and 0<a<1 and 0<b<1.5 are satisfied.
[0003] As mentioned above, Li 3 YCl 6 Chloride electrolytes such as Li2O4 and Li2O5 exhibit high ionic conductivity at room temperature, but no information is disclosed regarding their stability. The present inventors prepared the solid electrolytes disclosed in the above-mentioned documents 1 and 2 and left them in a dry room with a controlled dew point of -40°C. However, they found that the electrolyte decomposed and could not maintain its initial ionic conductivity, i.e., its stability (or moisture resistance) was low. Therefore, in order to improve the stability of chloride electrolytes, the present inventors have investigated the use of Li2O4 and Li2O5 as the solid electrolytes. x MCl 6 In this study, materials were prepared by combining various cations (M) to search for combinations of cations with high stability. As a result, as described below in the related art, a combination of cations exhibiting high ionic conductivity and high stability was identified. Meanwhile, in all-solid-state batteries, it is also necessary to improve the reduction resistance of the solid electrolyte in order to increase the energy density.
[0004] The present invention is directed to a solid electrolyte, and has an object to provide a solid electrolyte having excellent reduction resistance.
[0005] A first aspect of the present invention is a solid electrolyte comprising Li, Mα, Mβ, Mγ, Cl, and A, wherein Mα is at least one element selected from the group consisting of Zr and Hf, Mβ is at least one element selected from the group consisting of Ta and Nb, Mγ is at least one element selected from the group consisting of Gd, Yb, Dy, Er, Ho, Eu, and Sc, and A is selected from the group consisting of OH. - , AlO 2 - , S.O. 3 - , S.O. 4 2- , SiO 3 2- , SiO 4 4- , Si 2 O 7 6- , CO 3 2- , P.O. 4 3- , P 2 O 7 4- , B.O. 2 - , B.O. 3 3- , P.O. 3 - , NO 3 - , B.F. 4 - , P.F. 6 - , ClO 4 - , B(C 2 O 4 ) 2- , C.H. 3 COO - , TFSI - and FSI - At least one selected from the group consisting of:
[0006] According to the present invention, a solid electrolyte having excellent reduction resistance can be provided.
[0007] A second aspect of the present invention is the solid electrolyte of the first aspect, in which Mα includes Zr.
[0008] A third aspect of the present invention is the solid electrolyte of the first or second aspect, in which Mβ contains Ta.
[0009] A fourth aspect of the present invention is the solid electrolyte according to any one of the first to third aspects, in which Mγ includes Gd, Yb, or Er.
[0010] A fifth aspect of the present invention is the solid electrolyte according to any one of the first to fourth aspects, wherein A is SO 4 2- , CO 3 2- , P.O. 4 3- , B.O. 2 - , B.O. 3 3- , P.O. 3 - , NO 3 - or TFSI - Includes:
[0011] A sixth aspect of the present invention is the solid electrolyte of any one of the first to fifth aspects, which is represented by the following formula (1): Li6-(4+a-b)(1+c)(Mα (1-a-b) Mβ a Mγ b ) 1+c Cl 6 n (Mδ x A y ) (1) When 0<a, 0<b, a+b<1, −0.2≦c≦0.2, 0<n, 0<x, and 0<y are satisfied, and when the valence of Mδ is s and the valence of A is t, s×x=t×y is satisfied, and Mδ is at least one element selected from the group consisting of Li, Zr, Hf, Ta, Nb, Gd, Yb, Dy, Er, Ho, Eu, and Sc.
[0012] A seventh aspect of the invention is a lithium ion battery including the solid electrolyte of any one of the first to sixth aspects.
[0013] The above and other objects, features, aspects and advantages will become more apparent from the following detailed description of the invention which proceeds with reference to the accompanying drawings.
[0014] FIG. 1 is a longitudinal sectional view showing an all-solid-state lithium ion secondary battery.
[0015] First, a solid electrolyte according to a related art of the present invention will be described. The solid electrolyte according to the related art is a lithium (Li) ion conductive material that contains lithium (Li), three other metal elements (Mα, Mβ, Mγ) that become cations, and chlorine (Cl).
[0016] Mα is an element that becomes a tetravalent cation and is at least one element selected from the group consisting of zirconium (Zr) and hafnium (Hf). Mβ is an element that becomes a pentavalent cation and is at least one element selected from the group consisting of tantalum (Ta) and niobium (Nb). Mγ is an element that becomes a trivalent cation and is at least one element selected from the group consisting of gadolinium (Gd), ytterbium (Yb), dysprosium (Dy), erbium (Er), holmium (Ho), europium (Eu), and scandium (Sc). The solid electrolyte containing at least one trivalent, tetravalent, and pentavalent element in addition to Li as a cation achieves high ionic conductivity and high stability.
[0017] A preferred example of the solid electrolyte according to the related art is a compound represented by the following composition formula: Li6-(4+a-b)(1+c)(Mα (1-a-b) Mβ a Mγ b ) 1+c Cl 6 The conditions 0<a, 0<b, a+b<1, and −0.2≦c≦0.2 are satisfied.
[0018] Next, a solid electrolyte according to one embodiment of the present invention will be described. The solid electrolyte is a Li ion conductive material, and is a composite of the solid electrolyte according to the related art described above and a metal salt of an anion described below. The solid electrolyte is used, for example, in the manufacture of an all-solid-state secondary battery. The solid electrolyte contains Li, three other metal elements (Mα, Mβ, Mγ) that serve as cations, Cl, and A as an anion. The solid electrolyte may consist only of Li, Mα, Mβ, Mγ, Cl, and A.
[0019] As in the solid electrolyte according to the related art, Mα is an element that becomes a tetravalent cation and is at least one element selected from the group consisting of Zr and Hf. Mβ is an element that becomes a pentavalent cation and is at least one element selected from the group consisting of Ta and Nb. Mγ is an element that becomes a trivalent cation and is at least one element selected from the group consisting of Gd, Yb, Dy, Er, Ho, Eu, and Sc. Since the solid electrolyte according to the present embodiment contains at least one trivalent, one tetravalent, and one pentavalent element in addition to Li as a cation, high ionic conductivity and high stability are also achieved.
[0020] Anion A is OH - , AlO 2 - , S.O. 3 - , S.O. 4 2- , SiO 3 2- , SiO 4 4- , Si 2 O 7 6- , CO 3 2- , P.O. 4 3- , P 2 O 7 4- , B.O. 2 - , B.O. 3 3- , P.O. 3 - , NO 3 - , B.F. 4 - , P.F. 6 - , ClO 4 - , B(C 2 O 4 ) 2- , C.H. 3 COO - , TFSI - and FSI -The anion A is at least one selected from the group consisting of: anion A is also called a polyanion; a solid electrolyte containing anion A has high reduction resistance, as described below; the metal element of the metal salt of anion A is preferably at least one element selected from the group consisting of Li, Zr, Hf, Ta, Nb, Gd, Yb, Dy, Er, Ho, Eu, and Sc; the metal element of the metal salt may be another element; even when anion A contains sulfur (S), anion A is stable, and therefore hydrogen sulfide gas is not generated in the solid electrolyte; therefore, a highly safe all-solid-state secondary battery can be provided.
[0021] In the solid electrolyte according to this embodiment, in order to more reliably achieve high reduction resistance, Mα preferably contains Zr, and Mα may consist of only Zr. Furthermore, Mβ preferably contains Ta, and Mβ may consist of only Ta. Furthermore, Mγ preferably contains Gd, Yb, or Er, and Mγ may consist of only Gd, Yb, or Er. Mγ may contain two or more elements of Gd, Yb, and Er. The amount of substance of Li is, for example, greater than the amount of substance of any of Mα, Mβ, and Mγ, and is preferably greater than the sum of the amounts of substance of Mα, Mβ, and Mγ. The amount of substance of Cl is, for example, greater than the sum of the amounts of substance of Li, Mα, Mβ, and Mγ.
[0022] Anion A is SO 4 2- , CO 3 2- , P.O. 4 3- , B.O. 2 - , B.O. 3 3- , P.O. 3 - , NO 3 - or TFSI - and preferably contains SO 4 2- , CO 3 2- , P.O. 4 3- , B.O. 2 - , B.O. 3 3-, P.O. 3 - , NO 3 - or TFSI - The anion A may contain two or more of these anions. The molar amount of the anion A is smaller than the molar amount of Li, for example.
[0023] A preferred solid electrolyte is a compound represented by the following formula (1): Li6-(4+a-b)(1+c)(Mα (1-a-b) Mβ a Mγ b ) 1+c Cl 6 n (Mδ x A y ) ... (1) 0 < a, 0 < b, a + b < 1, -0.2 ≦ c ≦ 0.2, 0 < n, 0 < x, and 0 < y are satisfied. Furthermore, when the valence of Mδ is s and the valence of A is t, s × x = t × y is satisfied. Furthermore, Mδ is at least one element selected from the group consisting of Li, Zr, Hf, Ta, Nb, Gd, Yb, Dy, Er, Ho, Eu, and Sc. Regarding a and b, 0.1 ≦ a ≦ 0.5 and 0.1 ≦ b ≦ 0.4 may be satisfied. Furthermore, 0.2 ≦ a + b ≦ 0.8 may be satisfied. The relationship between a and b may be a ≧ b or a < b. Regarding c, -0.1 ≦ c ≦ 0.1 may be satisfied, or c may be 0. Regarding n, 0 < n ≦ 3 or 0 < n ≦ 2 may be satisfied. The solid electrolyte may be crystalline or amorphous.
[0024] When confirming whether an unknown solid electrolyte is the solid electrolyte according to the present embodiment, chemical analysis is performed on the unknown solid electrolyte to confirm whether the constituent elements are Li, Mα, Mβ, Mγ, Cl, and the constituent element of A. In confirming whether the unknown solid electrolyte satisfies the above formula (1), Li, Mα, Mβ, and Mγ can be quantified, for example, by ICP-emission spectroscopy. Cl can be quantified, for example, by ion chromatography. A measurement method capable of quantifying the constituent elements of the anion A is appropriately selected. O, N, and H can be quantified, for example, by ONH analysis using an oxygen, nitrogen, and hydrogen analyzer, and F can be quantified, for example, by ion chromatography. C can be quantified, for example, by a carbon and sulfur analyzer (CS meter), and other elements can be quantified by ICP-emission spectroscopy.
[0025] The molar ratio of Li, Mα, Mβ, Mγ, Cl, Mδ and A in the above formula (1) is Li:Mα:Mβ:Mγ:Cl:Mδ:A = 6-(4+a-b)(1+c):(1-a-b)(1+c):a(1+c):b(1+c):6:nx:ny. In the molar ratio determined by analysis of an unknown solid electrolyte, if the value of Li is 0.90 × {6-(4+a-b)(1+c)} or more and 1.10 × {6-(4+a-b)(1+c)} or less, it is considered that the above formula (1) is satisfied for Li. It is more preferable that the value of Li is 0.95 × {6-(4+a-b)(1+c)} or more and 1.05 × {6-(4+a-b)(1+c)} or less. The same is true for Mα, Mβ, Mγ, Cl, Mδ and A.
[0026] The solid electrolyte according to this embodiment is manufactured, for example, by the following method. First, a powder of a chloride containing Li, a powder of a chloride containing Mα, a powder of a chloride containing Mβ, and a powder of a chloride containing Mγ are prepared. The chloride containing Li is, for example, LiCl. The chloride containing Mα is, for example, MαCl. 4 The chloride containing Mβ is, for example, MβCl 5 The chloride containing Mγ is, for example, MγCl 3These powders are weighed and mixed to obtain a predetermined molar ratio.
[0027] Once the mixture is prepared, it is milled (mechanochemical milling). Here, a planetary ball mill is used as an example of the milling process. In a planetary ball mill, the pot rotates on its axis while the stage carrying the pot revolves, making it possible to generate very high impact energy. The milling process may also be performed using other types of grinders. The above milling process produces a solid electrolyte containing Li, Mα, Mβ, Mγ, and Cl. This solid electrolyte is the solid electrolyte before compounding (the solid electrolyte according to the related art described above), and in the following description, the synthesis of this solid electrolyte is also referred to as "pre-synthesis." In this processing example, the milling process is performed at room temperature, but conditions such as temperature may be changed as appropriate.
[0028] Next, the metal salt of anion A and the pre-synthesized solid electrolyte are weighed and mixed to a predetermined molar ratio. Thereafter, the mixture is milled in the same manner as above to obtain the solid electrolyte according to this embodiment. The solid electrolyte is a composite of the pre-synthesized solid electrolyte and the metal salt of the anion. The solid electrolyte is used to manufacture the positive electrode layer 112, the negative electrode layer 122, or the electrolyte layer 13 in the all-solid-state secondary battery 1 (see FIG. 1 ) described below. In the manufacture of the solid electrolyte according to this embodiment, it is not necessarily necessary to pre-synthesize the solid electrolyte (a solid electrolyte not containing anion A). The raw materials of the solid electrolyte (for example, LiCl, MαCl) used in the pre-synthesis are not necessarily used. 4 , MβCl 5 , MγCl 3 A composite solid electrolyte may be produced without prior synthesis by milling a mixture of anion A and a metal salt of anion A. The solid electrolyte may also be produced by a method other than milling, such as calcination.
[0029] FIG. 1 is a longitudinal cross-sectional view showing an all-solid-state lithium-ion secondary battery 1 (hereinafter simply referred to as "all-solid-state secondary battery 1"). The all-solid-state secondary battery 1 uses a solid electrolyte according to the present embodiment. The all-solid-state secondary battery 1 includes, from top to bottom in FIG. 1 , a positive electrode 11, an electrolyte layer 13, and a negative electrode 12. That is, the electrolyte layer 13 is provided between the positive electrode 11 and the negative electrode 12. The electrolyte layer 13 is a solid electrolyte layer and also serves as a separator layer. The electrolyte layer 13 is made of or includes the solid electrolyte according to the present embodiment. The positive electrode 11 includes a current collector 111 and a positive electrode layer 112. The positive electrode layer 112 includes a positive electrode active material. The negative electrode 12 includes a current collector 121 and a negative electrode layer 122. The negative electrode layer 122 includes a negative electrode active material.
[0030] The positive electrode active material of the positive electrode layer 112 preferably contains a lithium composite oxide. A preferred positive electrode active material is a lithium composite oxide having a layered rock salt structure, such as NCM (Li(Ni, Co, Mn)O 2 The positive electrode active material may be other lithium composite oxides, for example, NCA (Li(Ni, Co, Al)O) having a layered rock salt structure. 2 ), LCO (LiCoO 2 ), LNMO (LiNi) having a spinel structure 0.5 Mn 1.5 O 4 ), LFP (LiFePO) having an olivine structure 4 ) or the like. The positive electrode layer 112 includes the solid electrolyte according to the present embodiment in addition to the positive electrode active material. The positive electrode layer 112 may further include an electron conduction assistant (carbon black, etc.). An example of the positive electrode layer 112 is one in which these materials are integrated by applying pressure or heat.
[0031] The negative electrode active material of the negative electrode layer 122 is, for example, LTO (Li 4 Ti 5 O 12 ), NTO(Nb 2 TiO 7 ), TiO 2Examples of the materials include compounds such as titanium oxide (TiO 2 ), graphite, and SiO 2 (silicon monoxide). The anode layer 122 includes the solid electrolyte according to this embodiment in addition to the anode active material. The anode layer 122 may further include an electron conduction aid (carbon black, etc.). An example of the anode layer 122 is one in which these materials are integrated by applying pressure or heat. The configurations and materials of the positive electrode 11 and the negative electrode 12 of the all-solid-state secondary battery 1 are not limited to those described above, and various other configurations and materials can be used.
[0032] Next, examples and comparative examples of solid electrolytes will be described. Table 1 shows the compositions and evaluation results of the solid electrolytes of Examples 1 to 10 and Comparative Example 1. The solid electrolyte of Comparative Example 1 is the solid electrolyte according to the related art described above.
[0033]
[0034] Example 1 [Pre-synthesis of solid electrolyte] In an argon atmosphere having a dew point of −60° C. or less, raw material powders of LiCl, ZrCl 4 , TaCl 5 and YbCl 3 LiCl:ZrCl 4 : TaCl 5 : YbCl 3 The raw material powders were weighed to have a molar ratio of 2.0:0.6:0.2:0.2, and then pulverized and mixed in a mortar. The resulting mixed powder was placed in a zirconia pot and milled at 300 rpm for 20 hours using a planetary ball mill to pre-synthesize a chloride-based solid electrolyte.
[0035] [Compositing with Li salt containing polyanion] The solid electrolyte synthesized above was mixed with Li salt in an argon atmosphere having a dew point of −60° C. or less. 2 SO 4 The components were weighed to have a molar ratio of 1:0.15, and then crushed and mixed in a mortar. The resulting mixed powder was placed in a zirconia pot and milled for 20 hours at 300 rpm using a planetary ball mill to obtain a solid electrolyte containing a polyanion.
[0036] [Evaluation of Reduction Stability] A solid electrolyte powder was placed in a mold consisting of a resin sleeve and upper and lower punches made of SUS (stainless steel), and uniaxial press molding was performed under a pressure of 150 MPa. The lower punch was then removed, and Li metal foil was attached to the surface of the powder compact. The lower punch was then reinserted and pressurized at 50 MPa. Lead wires were connected to the upper and lower punches, and cyclic voltammetry measurements were performed at room temperature.
[0037] In the cyclic voltammetry measurements, the scan rate was set to 1 mV / sec, and the working electrode was scanned from the OCV (open circuit voltage) at the time of cell construction to −1.0 V (vs. Li) in the reduction direction. To quantify the stability against the reduction potential, the reduction current per unit area of the working electrode was measured to be −20 μA / cm when scanning from the OCV in the reduction direction. 2 The potential at which the reduction started was determined as the reduction starting potential. In Table 1, the obtained values are shown in the "reduction starting potential" column.
[0038] In addition, the reduction stability evaluation was performed by calculating the amount of electricity generated by the reductive decomposition. The operating potential (0.1 V vs. Li) of graphite, which is a common negative electrode active material for lithium-ion batteries, was used as a reference, and the amount of electricity (unit: coulomb [C]) was calculated by integrating the reduction current that flowed from the reduction onset potential to 0.1 V, thereby quantitatively evaluating the stability of the negative electrode against potential. In Table 1, the obtained values are shown in the column "Amount of electricity generated by decomposition up to 0.1 V."
[0039] (Example 2) In the process of forming a composite with a Li salt containing a polyanion in the electrolyte preparation of Example 1, a pre-synthesized solid electrolyte and Li 2 SO 4 An electrolyte was prepared in the same manner as in Example 1, except that the amounts were weighed so as to give a molar ratio of 1:0.33, and then the test and evaluation were carried out.
[0040] (Example 3) In the process of forming a composite with a Li salt containing a polyanion in the electrolyte preparation of Example 1, a pre-synthesized solid electrolyte and Li 2 SO 4 An electrolyte was prepared in the same manner as in Example 1, except that the amounts were weighed so as to give a molar ratio of 1:1, and then the test and evaluation were carried out.
[0041] Example 4 In the electrolyte preparation of Example 1, in the process of compounding with a Li salt containing a polyanion, a pre-synthesized solid electrolyte and Li 2 CO 3 An electrolyte was prepared in the same manner as in Example 1, except that the amounts were weighed so as to give a molar ratio of 1:1, and then the test and evaluation were carried out.
[0042] (Example 5) In the process of forming a composite with a Li salt containing a polyanion in the electrolyte preparation of Example 1, a pre-synthesized solid electrolyte and Li 3 P.O. 4 An electrolyte was prepared in the same manner as in Example 1, except that the amounts were weighed so as to give a molar ratio of 1:1, and then the test and evaluation were carried out.
[0043] Example 6 In the electrolyte preparation of Example 1, in the process of complexing with a Li salt containing a polyanion, a pre-synthesized solid electrolyte and Li 3 BO 3 An electrolyte was prepared in the same manner as in Example 1, except that the amounts were weighed so as to give a molar ratio of 1:1, and then the test and evaluation were carried out.
[0044] Example 7 In the electrolyte preparation of Example 1, in the process of compounding with a Li salt containing a polyanion, a pre-synthesized solid electrolyte and LiPO 3 An electrolyte was prepared in the same manner as in Example 1, except that the amounts were weighed so as to give a molar ratio of 1:1, and then the test and evaluation were carried out.
[0045] Example 8 In the process of forming a composite with a Li salt containing a polyanion in the electrolyte preparation of Example 1, a pre-synthesized solid electrolyte and LiBO 2 An electrolyte was prepared in the same manner as in Example 1, except that the amounts were weighed so as to give a molar ratio of 1:1, and then the test and evaluation were carried out.
[0046] Example 9 In the process of forming a composite with a polyanion-containing Li salt in the electrolyte preparation of Example 1, a pre-synthesized solid electrolyte and LiNO 3 An electrolyte was prepared in the same manner as in Example 1, except that the amounts were weighed so as to give a molar ratio of 1:1, and then the test and evaluation were carried out.
[0047] Example 10 An electrolyte was prepared in the same manner as in Example 1, except that in the process of forming a composite with a polyanion-containing Li salt, the pre-synthesized solid electrolyte and LiTFSI were weighed out so as to have a molar ratio of 1:0.5. Tests and evaluations were then carried out.
[0048] Comparative Example 1 Testing and evaluation were performed on a pre-synthesized solid electrolyte, omitting the complexation with the polyanion-containing Li salt.
[0049] As shown in Table 1, the solid electrolytes of Examples 1 to 10, in which a pre-synthesized solid electrolyte was composited with a polyanion (metal salt), showed a decrease in reduction onset potential and a decrease in the amount of electricity required for decomposition up to 0.1 V, compared to the uncomposite solid electrolyte of Comparative Example 1. Thus, it was confirmed that the reductive decomposition reaction of the solid electrolyte was suppressed and the reduction resistance was improved by composited a pre-synthesized solid electrolyte with a polyanion.
[0050] The reason why the reduction resistance of the composite solid electrolyte is improved is not entirely clear, but it is thought that the composite with the polyanion disrupts the crystalline structure of the pre-synthesized solid electrolyte, leading to its amorphization. This disruption of the crystalline structure allows cations to interact not only with Cl but also with the polyanion, resulting in stabilization. It is presumed that this structural change contributes to the improvement of the reduction resistance.
[0051] Furthermore, in Examples 1 to 3, which used the same type of polyanion, the ratio of the amount of substance of the metal salt of the polyanion to the amount of substance of the pre-synthesized solid electrolyte was changed, and it was confirmed that the reduction resistance tended to increase as this ratio increased. Therefore, this ratio is preferably 0.33 or more, and more preferably 0.5 or more. This ratio may be 1 or more, and it is believed that a wide range of added amounts of polyanion are effective in improving reduction resistance. From the perspective of improving reduction resistance, there is no particular upper limit to this ratio, but from the perspective of favorably maintaining the properties of the pre-synthesized solid electrolyte, this ratio is, for example, 3 or less, preferably 2 or less.
[0052] The mechanism by which reduction resistance is improved is thought to be the same regardless of the type of polyanion. - , AlO 2 - , S.O. 3 - , SiO 3 2- , SiO 4 4- , Si 2 O 7 6- , P 2 O 7 4- , B.F. 4 - , P.F. 6 - , ClO 4 - , B(C 2 O 4 ) 2- , C.H. 3 COO - and FSI - It is believed that reduction resistance is improved in either case.
[0053] For pre-synthesized solid electrolytes, it is believed that the reduction resistance is improved when Hf, which is a tetravalent cation like Zr, is used instead of or together with Zr by complexing with a polyanion. The same is true when Nb, which is a pentavalent cation like Ta and has the same ionic radius as Ta, is used instead of or together with Ta. Furthermore, the same is true when Gd, Dy, Er, Ho, Eu, and Sc, which are trivalent cations like Yb and have ionic radii similar to Yb, are used instead of or together with Yb.
[0054] As described above, the solid electrolyte according to this embodiment contains Li, Mα, Mβ, Mγ, Cl, and A. Mα is at least one element selected from the group consisting of Zr and Hf. Mβ is at least one element selected from the group consisting of Ta and Nb. Mγ is at least one element selected from the group consisting of Gd, Yb, Dy, Er, Ho, Eu, and Sc. A is OH. - , AlO 2- , S.O. 3 - , S.O. 4 2- , SiO 3 2- , SiO 4 4- , Si 2 O 7 6- , CO 3 2- , P.O. 4 3- , P 2 O 7 4- , B.O. 2 - , B.O. 3 3- , P.O. 3 - , NO 3 - , B.F. 4 - , P.F. 6 - , ClO 4 - , B(C 2 O 4 ) 2- , C.H. 3 COO - , TFSI - and FSI - In this way, by optimizing the types and combinations of Mα, Mβ, Mγ, and A, a solid electrolyte with excellent reduction resistance can be realized. Since the potential window of this solid electrolyte is wide, when this solid electrolyte is applied to an all-solid-state secondary battery 1, the limitation on the operating voltage is alleviated, and the energy density of the all-solid-state secondary battery 1 can be improved.
[0055] Preferably, A is SO 4 2- , CO 3 2- , P.O. 4 3- , B.O. 2 - , B.O. 3 3- , P.O. 3 - , NO 3 -or TFSI - This makes it possible to more reliably improve the reduction resistance of the solid electrolyte.
[0056] A preferred solid electrolyte is represented by the following formula (1): Li6-(4+a-b)(1+c)(Mα (1-a-b) Mβ a Mγ b ) 1+c Cl 6 n (Mδ x A y ) (1) where 0<a, 0<b, a+b<1, -0.2≦c≦0.2, 0<n, 0<x, and 0<y are satisfied, and where the valence of Mδ is s and the valence of A is t, s×x=t×y is satisfied. Furthermore, Mδ is at least one element selected from the group consisting of Li, Zr, Hf, Ta, Nb, Gd, Yb, Dy, Er, Ho, Eu, and Sc. This makes it possible to more reliably realize a solid electrolyte having excellent reduction resistance.
[0057] The solid electrolyte and all-solid-state secondary battery 1 can be modified in various ways.
[0058] The solid electrolyte containing Li, Mα, Mβ, Mγ, Cl, and A may not satisfy the above formula (1).
[0059] The solid electrolyte may be mixed with other substances (which may include Li) and used as an electrolyte material. In this case, the solid electrolyte is preferably the component with the largest mass ratio among the components contained in the electrolyte material, i.e., the main component. The mass ratio of the main component in the electrolyte material is preferably 50 mass% or more, more preferably 60 mass% or more, and even more preferably 70 mass% or more.
[0060] The solid electrolyte used in the all solid state secondary battery 1 does not necessarily need to be contained in all of the positive electrode 11, the negative electrode 12, and the electrolyte layer 13, but may be contained in at least one of the positive electrode 11, the negative electrode 12, and the electrolyte layer 13. Furthermore, the solid electrolyte may be used in batteries other than all solid state secondary batteries, and may be used for purposes other than batteries.
[0061] The configurations in the above-described embodiment and each modification may be combined as appropriate as long as they are not mutually contradictory.
[0062] While the invention has been particularly illustrated and described, it should be understood that the foregoing description is illustrative and not restrictive, and that numerous modifications and variations are possible without departing from the scope of the invention.
[0063] 1 All-solid-state lithium-ion secondary battery 11 Positive electrode 12 Negative electrode 13 Electrolyte layer
Claims
1. A solid electrolyte comprising Li, Mα, Mβ, Mγ, Cl, and A, where Mα is at least one element selected from the group consisting of Zr and Hf, Mβ is at least one element selected from the group consisting of Ta and Nb, Mγ is at least one element selected from the group consisting of Gd, Yb, Dy, Er, Ho, Eu, and Sc, and A is OH - , AlO 2 - , SO 3 - , SO 4 2- , SiO 3 2- , SiO 4 4- , Si 2 O 7 6- , CO 3 2- , PO 4 3- , P 2 O 7 4- , BO 2 - , BO 3 3- , PO 3 - , NO 3 - , BF 4 - , PF 6 - , ClO 4 - , B(C 2 O 4 ) 2- , CH 3 COO - , TFSI - and FSI - and is at least one selected from the group consisting of a solid electrolyte.
2. The solid electrolyte according to claim 1, wherein Mα is a solid electrolyte containing Zr.
3. The solid electrolyte according to claim 1, wherein Mβ is a solid electrolyte containing Ta.
4. The solid electrolyte according to claim 1, wherein Mγ is a solid electrolyte containing Gd, Yb or Er.
5. The solid electrolyte according to claim 1, wherein A is SO 4 2- , CO 3 2- , PO 4 3- , BO 2 - , BO 3 3- , PO 3 - , NO 3 - or TFSI - and the solid electrolyte contains the same.
6. The solid electrolyte according to claim 1, which is represented by the following formula (1): Li6-(4 + a - b)(1 + c)(Mα (1-a-b) Mβ a Mγ b ) 1+c Cl 6 ·n(Mδ x A y )···(1) 0 < a, 0 < b, a + b < 1, -0.2 ≤ c ≤ 0.2, 0 < n, 0 < x, and 0 < y are satisfied, and when the valence of Mδ is s and the valence of A is t, s × x = t × y is satisfied, and Mδ is a solid electrolyte that is at least one element selected from the group consisting of Li, Zr, Hf, Ta, Nb, Gd, Yb, Dy, Er, Ho, Eu, and Sc.
7. A lithium-ion battery comprising the solid electrolyte according to any one of claims 1 to 6.
Citation Information
Patent Citations
Solid electrolyte material and battery
JP6934626B2
Halide solid electrolyte material and battery using this
WO2020070956A1
Oxide, method of preparing the same, solid electrolyte including the oxide, and electrochemical device including the oxide
US20210043966A1
Solid electrolyte, preparation method thereof, metal air battery including the same, and electrochemical device including the same
US20210167419A1
Solid electrolyte material and battery using same
WO2020188914A1