Copper alloy sheet material, method for producing same, and current-carrying component
The Cu-Fe-P copper alloy plate material, with a tailored composition and manufacturing process, addresses the trade-off between strength and bendability, achieving superior performance and cost-effectiveness for board-to-board connectors by ensuring high strength, conductivity, and bending workability.
Patent Information
- Application Number
- PCT/JP2024/005028
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-29
- Filing Date
- 2024-02-14
- Publication Date
- 2024-10-03
AI Technical Summary
Current Cu-Fe-P copper alloy materials for board-to-board connectors face a trade-off between strength, conductivity, and bendability, failing to meet the demanding requirements of smaller, lower-profile connectors with higher current capacities.
A Cu-Fe-P copper alloy plate material with specific chemical composition (Fe: 0.05-1.10%, P: 0.02-0.50%, Mg: 0-0.50%, Ni: 0-0.80%, Sn: 0-0.80%, Zn: 0-0.80%, and a crystallite size of 30 nm or less, manufactured through hot rolling, intermediate cold rolling, intermediate heat treatment, and finishing heat treatment, ensuring high strength, conductivity, and improved bending workability.
The alloy achieves excellent strength, conductivity, and bending workability, reducing manufacturing costs and enhancing the performance of board-to-board connectors, while maintaining high electrical conductivity and resistance to cracking during bending.
Smart Images

Figure JP2024005028_03102024_PF_FP_ABST
Abstract
Description
Copper alloy sheet material, its manufacturing method and current-carrying component
[0001] The present invention relates to a Cu-Fe-P-based copper alloy sheet suitable for a connector for connecting board-to-board (sometimes referred to as "BtoB" or "BTB"), a method for manufacturing the same, and an electrically conductive component using the copper alloy sheet.
[0002] Among copper alloys used in current-carrying components such as connectors, Cu-Fe-P copper alloys are available that can be strengthened by Fe-P precipitates. Patent Document 1 describes a Cu-Fe-P copper alloy material that combines strength, electrical conductivity, and drawability by enhancing the orientation of the {220} plane. It describes that the material is manufactured by repeatedly performing hot rolling, cold rolling, and recrystallization annealing, followed by stress relief annealing after the final cold rolling.
[0003] Patent No. 5467163
[0004] In connectors, continuity between paired pins (current-carrying components) is ensured by fitting the bent portions of both pins together. Board-to-board connectors are composed of many pins, each with a complex bend. When inserting or removing a board-to-board connector, some pins may be subjected to significant stress depending on slight misalignment between the boards and the method of insertion / removal (handling). For this reason, it is extremely important that the bent portions of each pin are quality-controlled to ensure they are in a sound state without cracks. It is also important that the connectors have high strength and high conductivity.
[0005] In recent years, as board-to-board connectors have become smaller, thinner, and have become larger in current, the materials used therein are required to have higher levels of strength, conductivity, and bending workability than ever before. According to the technology of Patent Document 1, a Cu-Fe-P-based copper alloy sheet material with excellent strength and conductivity can be obtained. However, since there is generally a trade-off between strength and bending workability, there remains room for improvement in providing excellent bending workability that can meet the strict requirements of today's board-to-board connectors.
[0006] An object of the present invention is to provide a Cu-Fe-P based copper alloy sheet having excellent strength and electrical conductivity and an improved level of bending workability.
[0007] In order to achieve the above object, the present specification discloses the following invention: [1] A steel sheet having a chemical composition, in mass %, of 0.05 to 1.10% Fe, 0.02 to 0.50% P, 0 to 0.50% Mg, 0 to 0.80% Ni, 0 to 0.80% Sn, 0 to 0.80% Zn, a total of elements other than Fe, P, Mg, Ni, Sn, Zn, and Cu: 0 to 0.10%, and the balance being Cu, wherein the crystallite size measured by the Halder-Wagner method based on the integral width of the peak in an X-ray diffraction pattern using CuKα radiation on the sheet surface is 30 nm or less, and the 0.2% proof stress in the direction perpendicular to the rolling direction is 450 N / mm 2 [2] In an observation plane parallel to the sheet surface, the number density of precipitate particles having a major axis of 10 to 100 nm is 50 particles / μm 2 [3] The copper alloy sheet according to the above [1] or [2], having an electrical conductivity of 50% IACS or more. [4] The copper alloy sheet according to any one of the above [1] to [3], having a ratio MBR / t of the minimum bending radius MBR at which cracks do not occur to the sheet thickness t in a 90°L bending test with the bending axis parallel to the rolling direction (B.W.) of 0.7 or less.
[0008] The copper alloy sheets [1] to [4] above can be produced by the following method. [5] A hot rolling process in which a cast slab having a chemical composition consisting of, in mass%, Fe: 0.05 to 1.10%, P: 0.02 to 0.50%, Mg: 0 to 0.50%, Ni: 0 to 0.80%, Sn: 0 to 0.80%, Zn: 0 to 0.80%, the total of elements other than Fe, P, Mg, Ni, Sn, Zn, and Cu: 0 to 0.10%, and the balance being Cu, is rolled at a rolling reduction rate of 70% or more in a temperature range of 950°C or less and 650°C or more, and then rolled at a rolling reduction rate of 60% or more in a temperature range of less than 650°C and 350°C or more; an intermediate cold rolling process in which cold rolling at a rolling reduction rate of 30% or more is performed; and an intermediate heat treatment process in which the material obtained in the intermediate cold rolling process is heat treated by holding it at a temperature of 400°C or more and 700°C or less for 1 hour or more. A method for producing a copper alloy sheet, comprising, in the order mentioned, a finish cold rolling step of cold rolling the material obtained in the intermediate heat treatment step at a rolling reduction rate of 80% or more, and a finish heat treatment step of heating the material obtained in the finish cold rolling step to a temperature range of 180° C. to 500° C. [6] The method for producing a copper alloy sheet according to the above [5], wherein in the finish heat treatment step, a material is obtained having a crystallite size of 30 nm or less as determined by the Halder-Wagner method based on the integral width of a peak in an X-ray diffraction pattern using CuKα radiation on the sheet surface.
[0009] The present invention also provides the following: [7] An electric component using the copper alloy sheet material according to any one of [1] to [4] above.
[0010] In this specification, the notation "n1 to n2" indicating a numerical range means "greater than or equal to n1 and less than or equal to n2." Here, n1 and n2 are values that satisfy n1 < n2. "Plate" refers to a sheet-like metal material formed by utilizing the malleability of metal. Thin sheet-like metal materials are sometimes called "foils," and such "foils" are also included in the term "plate" here. Long sheet-like metal materials wound into a coil are also included in the term "plate." In this specification, the thickness of a sheet-like metal material is referred to as the "plate thickness." The "plate surface" is the surface perpendicular to the thickness direction of the plate material. The "plate surface" is also sometimes called the "rolled surface." The "major axis" of a particle is defined as the diameter of the smallest circle surrounding the particle. The "number density of precipitate particles with a major axis of 10 to 100 nm" can be determined as follows.
[0011] [Method of determining the number density of precipitate particles] The plate surface was electrolytically polished under the following electrolytic polishing conditions, and then ultrasonically cleaned in ethanol for 20 minutes using an ultrasonic cleaner. The surface obtained was observed using an FE-SEM (field emission scanning electron microscope) at an acceleration voltage of 15 kV and a magnification of 100,000 times, and an observation field in which some or all of the particles with a major axis of 1.0 μm or more were not included was randomly set. In the observation field, the number of precipitate particles with a major axis of 10 to 100 nm was counted among the particles whose entire outlines were visible. This operation was repeated for multiple observation fields with no overlapping areas, with a total observation area of 10 to 100 μm. 2 The total number of counts in the entire observed field of view was divided by the total area of the observed field of view, and the value was determined as the number density of precipitate particles (particles / μm 2 (Electrolytic polishing conditions) Electrolytic solution: Distilled water, phosphoric acid, ethanol, and 2-propanol mixed in a volume ratio of 10:5:5:1. Solution temperature: 20°C. Voltage: 15V. Electrolytic time: 20 seconds.
[0012] The rolling ratio in a certain process is calculated by the following formula (1): Rolling ratio (%) = [(t 0 -t 1 ) / t 0 ]×100…(1) t 0 t: Plate thickness before rolling in that process (mm) 1 : Plate thickness after rolling in that process (mm)
[0013] According to the present invention, a Cu-Fe-P-based copper alloy sheet material has been realized that combines high levels of strength, electrical conductivity, and bending workability. This sheet material uses relatively inexpensive additive elements and can be manufactured using a process that does not require solution treatment or repeated cold rolling and recrystallization annealing, making it advantageous in terms of manufacturing cost compared to high-strength sheet materials of the same or other copper alloys. The present invention contributes to improving the performance and reducing the cost of board-to-board connectors, which are becoming increasingly miniaturized.
[0014] A laser microscope photograph of the outer surface of a bent portion of a sheet material sample (intermediate product) after finish cold rolling, which is an intermediate stage in the production of Invention Example No. 2, subjected to a 90°L bending test at B.W. with an R / t of about 0.6. A laser microscope photograph of the outer surface of a bent portion of a sheet material sample (finished product) after finish heat treatment obtained in Invention Example No. 2, subjected to a 90°L bending test at B.W. with an R / t of about 0.6.
[0015] [Chemical Composition] The present invention is directed to a Cu-Fe-P based copper alloy. Hereinafter, "%" relating to alloy components means "mass %" unless otherwise specified.
[0016] Iron (Fe) contributes to improving strength by forming compounds with P and finely precipitating them in the matrix (the metal base of the copper alloy). To fully utilize this effect, the Fe content must be 0.05% or more. Excessive Fe content can cause a decrease in electrical conductivity, so the Fe content must be 1.10% or less. 0.90% or less is more preferable, 0.50% or less is even more preferable, and 0.30% or less may be acceptable.
[0017] P (phosphorus) generally serves as a deoxidizer for copper alloys, but in the present invention, it forms fine precipitates of Fe-P compounds, or even Mg-P compounds, thereby contributing to improved strength. To fully exert this effect, the P content must be 0.02% or more. 0.03% or more is more preferable, and 0.05% or more is even more preferable. Since a high P content makes hot tearing more likely to occur, the P content is set to 0.50% or less. 0.30% or less is more preferable, and it may be controlled to 0.15% or less.
[0018] Cu-Fe-P-based copper alloys may contain one or more of Mg (magnesium), Ni (nickel), Sn (tin), and Zn (zinc) as needed. Like Fe, Mg forms compounds with P, contributing to improved strength. When Mg is added, a content of 0.03% or more is more effective. Since a high Mg content increases the likelihood of Mg oxide entrapment during hot rolling, the Mg content is set to 0.50% or less. It is more preferable that the Mg content be 0.30% or less, and even more preferable that the Mg content be 0.20% or less. It is also preferable to set the Mg content so that the total content of Fe and Mg is 1.10% or less. The (Fe + Mg) / P ratio, which represents the mass ratio of the total content of Fe and Mg to the P content, is preferably in the range of 0.4 to 13.0, and more preferably in the range of 0.5 to 12.5.
[0019] Ni, Sn, and Zn dissolve in the matrix and contribute to improving heat resistance. When one or more of these elements are contained, from the viewpoint of maintaining high electrical conductivity, the content of each of Ni, Sn, and Zn is allowed up to 0.80%, and it is more preferable that each content be 0.50% or less, and each may be controlled to a content range of 0.30% or less. When one or more of Ni, Sn, and Zn are contained, it is effective to set the content of each of these elements to 0.001% or more, and it is more effective to set each to 0.002% or more.
[0020] Other elements are permitted to be included to the extent that they do not impair the objective of the present invention (high levels of strength, conductivity, and bending workability). Specifically, the total content of elements other than Fe, P, Mg, Ni, Sn, Zn, and Cu (copper) may be controlled to 0.10% or less. For example, depending on the application, one or more of Al (aluminum), B (boron), Co (cobalt), Cr (chromium), Mn (manganese), Pb (lead), S (sulfur), Si (silicon), Te (tellurium), Ti (titanium), and Zr (zirconium) may be included so that the total content of these elements is 0.10% or less. Furthermore, when one or more of Al, B, Co, Cr, Mn, Pb, S, Si, Te, Ti, and Zr are included, the content of each of these elements may be, for example, 0.001% or more.
[0021] An example of an alloy composition in which the total content of elements other than Fe, P, Mg, Ni, Sn, Zn, and Cu is 0.10% or less is "a chemical composition consisting of, by mass, 0.05-1.10% Fe, 0.02-0.50% P, 0-0.50% Mg, 0-0.80% Ni, 0-0.80% Sn, 0-0.80% Zn, 0-0.10% total of Al, B, Co, Cr, Mn, Pb, S, Si, Te, Ti, and Zr, with the balance being Cu and unavoidable impurities." In this case, unavoidable impurities refer to elements other than those listed above that are inevitably mixed in during manufacturing.
[0022] [Crystallite size] The inventors have found that by reducing the crystallite size, bending workability can be significantly improved while maintaining high strength and high conductivity. Specifically, it is extremely effective for the crystallite size to be 30 nm or less, and more preferably 25 nm or less, as determined by the Halder-Wagner method based on the integral width of the peak in the X-ray diffraction pattern using CuKα radiation on the plate surface. Although there is no particular lower limit for the crystallite size, according to previous studies, it is considered that the crystallite size can be adjusted to, for example, a range of 10 to 30 nm, and may also be controlled to a range of 15 to 25 nm.
[0023] The Halder-Wagner method is based on the integral width β of each of the multiple diffraction peaks in the X-ray diffraction pattern, with the horizontal axis being β / (tan θ × sin θ) and the vertical axis being (β / tan θ). 2 The method involves plotting the data on coordinates such that the crystallite size D is calculated from the slope of the line Kλ / D (β / tan θ) by drawing an approximation line of the following equation (2) for the plots. 2 =(Kλ / D)×[β / (tanθ×sinθ)]+16ε 2 ... (2) where β is the integral width of the diffraction peak, θ is the Bragg angle of the diffraction peak, K is the Scherrer constant, λ is the X-ray wavelength (nm), D is the crystallite size (nm), and ε is the lattice distortion. Here, the integral width β is measured for four diffraction peaks resulting from the (111), (200), (220), and (311) crystal planes, whose diffraction angles 2θ are in the range of 30 to 150°, and the Halder-Wagner method is applied.
[0024] [Number Density of Precipitate Particles] Precipitate particles with a major axis of 10 to 100 nm contribute to improving the strength of the copper alloy sheet material. The number density of precipitate particles with a major axis of 10 to 100 nm is 50 particles / μm. 2 The upper limit of the number density is not particularly limited, but the number density is usually 200 particles / μm 2 less than 150 particles / μm 2 It may be managed as follows:
[0025] [0.2% Yield Strength] In order to meet the needs for miniaturization and thinning of current-carrying components, it is important to maintain a high strength level. Considering the use in board-to-board connectors, the 0.2% yield strength of copper alloy sheet material in the transverse direction (TD) of rolling is 450 N / mm 2 It is desirable that the strength is 500 Nmm or more. 2 More preferably, it is 550 N / mm or more. 2 The 0.2% yield strength of the copper alloy sheet material of the present invention is usually 900 N / mm 2 It can be adjusted within the following range: 700N / mm 2 It may be managed as follows:
[0026] [Conductivity] Considering the use of current-carrying parts such as connectors, the conductivity of the copper alloy sheet is preferably 50% IACS or more, more preferably 65% IACS or more. It can also be adjusted to 70% IACS or more. In the copper alloy sheet having the above-mentioned composition range, the conductivity is usually 90% IACS or less, and may be controlled to 85% IACS or less.
[0027] [Bending workability] Considering the use of board-to-board connectors, which are subjected to complex bending processes, the ratio MBR / t of the minimum bending radius MBR at which cracks do not occur to the sheet thickness t in a 90°L bending test in which the bending axis is parallel to the rolling direction (B.W.) of the copper alloy sheet material is preferably 0.7 or less, and more preferably 0.5 or less. According to the manufacturing method described below, it is also possible to adjust the MBR / t to 0.3 or less, which is an extremely excellent level of bending workability for a Cu-Fe-P based copper alloy.
[0028] [Manufacturing Method] The copper alloy sheet material described above can be obtained, for example, by the following manufacturing process: Melting / casting → Hot rolling → Intermediate cold rolling → Intermediate heat treatment → Finish cold rolling → Finish heat treatment. Although not described in the above processes, facing is performed as needed after hot rolling, and pickling, polishing, or further degreasing is performed as needed after each heat treatment. Each process will be described below.
[0029] [Melting and Casting] A copper alloy having the above-described chemical composition is melted to obtain a cast piece. As a casting method, a known method such as a semi-continuous casting method or a continuous casting method can be applied. An ingot (slab) obtained by an ingot-making method is also included in the term "cast piece" as used in this specification.
[0030] [Hot Rolling] After heating the slab, it is hot rolled. The heating temperature of the slab is preferably 850 to 1000°C. The holding time within the above temperature range is preferably 0.3 hours or more, and more preferably 0.5 to 10 hours. This heating and holding promotes homogenization of the cast structure (mitigation of solidification segregation) and promotes the solid solution of coarse Fe—P-based compounds and Mg—P-based compounds.
[0031] The heated slab is removed from the furnace and hot rolling begins. Hot rolling is performed according to a pass schedule in which rolling is performed at a reduction rate of 70% or more in a temperature range of 950°C or lower and 650°C or higher, followed by rolling at a reduction rate of 60% or more in a temperature range of lower than 650°C and 350°C or higher. The rolling temperature in each rolling pass can be monitored by the surface temperature of the material immediately after it leaves the work rolls of the hot rolling mill. "Rolling at a reduction rate of 70% or more in a temperature range of 950°C or lower and 650°C or higher" means that the plate thickness (slab thickness) before the start of the first rolling pass, in which the rolling temperature is 950°C or lower, is reduced by h 0 (mm), the plate thickness after the last rolling pass at a rolling temperature of 650°C or higher is h 1 (mm), [(h 0 -h 1 ) / h 0 ]×100(%) means that the rolling ratio is 70% or more. In addition, "rolling is performed at a temperature range of less than 650°C and not less than 350°C" means that the thickness before the start of the first rolling pass at a rolling temperature of less than 650°C is reduced by h 1 (mm), the plate thickness after the last rolling pass at a rolling temperature of 350°C or higher is h 2 (mm), [(h 1 -h 2 ) / h 1 ] × 100(%) is 60% or more.
[0032] Dynamic recrystallization is likely to occur in the temperature range of 950°C or lower and 650°C or higher. In order to obtain a structure consisting of fine and highly uniform crystal grains from a coarse and non-uniform cast structure, it is extremely effective to set the rolling reduction ratio in the temperature range of 950°C or lower and 650°C or higher to 70% or higher, and even more effective to set it to 80% or higher. The rolling reduction ratio in the temperature range of 950°C or lower and 650°C or higher may be adjusted to, for example, 92% or lower. On the other hand, in the temperature range of lower than 650°C and 350°C or higher, Fe—P-based compounds and Mg—P-based compounds are likely to precipitate. In order to generate many precipitation nuclei for Fe—P-based compounds and Mg—P-based compounds, it is extremely effective to set the rolling reduction ratio in the temperature range of lower than 650°C and 350°C or higher to 60% or higher. In the temperature range of lower than 650°C and 350°C or higher, it is sufficient to set the rolling reduction ratio in the range of lower than 650°C and 350°C or higher, for example, to 85% or lower, or even 75% or lower. By leaving the material (hot-rolled sheet) after hot rolling in a structural state in which a large amount of precipitation nuclei of the above compounds or extremely fine precipitates resulting from them are present, it becomes possible to rapidly and sufficiently generate fine precipitates of Fe—P compounds and Mg—P compounds in the intermediate heat treatment step described below, which is performed without going through a solution treatment step. The sheet thickness after hot rolling may be adjusted, for example, in the range of 5 to 20 mm, depending on the final target sheet thickness.
[0033] [Intermediate Cold Rolling] The material after hot rolling is subjected to cold rolling at a rolling reduction of 30% or more, more preferably 35% or more, and even more preferably 55% or more. The upper limit of the cold rolling reduction can be set depending on the target plate thickness and the mill power of the cold rolling mill. Typically, a rolling reduction of 95% or less is sufficient, and may be set in the range of 85% or less. Note that, as long as a structure containing a large amount of precipitation nuclei of Fe—P-based compounds or Mg—P-based compounds formed by hot rolling or ultrafine precipitates resulting therefrom is maintained, this intermediate cold rolling may be performed on a material whose plate thickness has been reduced by cold rolling and annealing one or more times, as needed.
[0034] [Intermediate Heat Treatment] The material obtained by the intermediate cold rolling is subjected to a heat treatment in which it is held at a temperature of 400°C or higher and 700°C or lower for 1 hour or longer. Because a large amount of precipitation nuclei of Fe-P compounds and Mg-P compounds or extremely fine precipitates resulting therefrom are formed by the hot rolling, and cold working strain is imparted by the intermediate cold rolling, it is possible to rapidly form a large amount of precipitates consisting of Fe-P compounds and Mg-P compounds by holding the material under heat in a temperature range of 400°C or higher and 700°C or lower. Specifically, the density of precipitates having a particle diameter of 10 to 100 nm is set to 50 particles / μm 2 The temperature can be adjusted to the above range. Furthermore, a fine and highly uniform recrystallized structure can be obtained. If the maximum temperature of the material exceeds 700°C, the recrystallized grains may become coarse. There is no particular upper limit to the holding time at a temperature of 400°C or higher but 700°C or lower, but it is usually sufficient to hold the temperature for no more than 24 hours.
[0035] [Finish Cold Rolling] The material obtained by the above intermediate cold rolling is subjected to cold rolling at a rolling ratio of 80% or more to adjust the final plate thickness and further improve strength. By setting the rolling ratio to 80% or more, a large amount of dislocations can be introduced, which is advantageous for obtaining a structure with a small crystallite size in the finish heat treatment described below. A rolling ratio of 90% or more is more effective, and a rolling ratio of 95% or more is even more effective. The upper limit of the rolling ratio may be set, for example, in the range of 99% or less depending on the mill power.
[0036] [Finish Heat Treatment] The material obtained by the above-mentioned finish cold rolling is subjected to a heat treatment in which it is heated to a temperature range of 180°C to 500°C. Because cold working strain is introduced by the above-mentioned finish cold rolling, even if the temperature is held in the 180°C to 500°C range for a short time, such as a few seconds, it is possible to reduce the crystallite size through dislocation rearrangement. Specific heat treatment conditions may be optimal for the heat treatment furnace, so long as they result in a material with a crystallite size of 30 nm or less. However, the maximum temperature is set to a range of 180°C to 500°C. Either a continuous or batch-type heat treatment furnace may be used as the heat treatment furnace. In the case of a continuous heat treatment furnace, the time during which the material temperature reaches 180°C to 500°C (hereinafter referred to as the "heat treatment time") can be easily set to a range of, for example, 3 to 120 seconds. In the case of a batch-type heat treatment furnace, the heat treatment time can be easily set to a range of, for example, 10 minutes or more. The upper limit of the heat treatment time is not particularly specified, but can be set within the range of, for example, 5 hours or less.
[0037] The mechanism by which this final heat treatment can produce a structure with a small crystallite size has not been fully elucidated, but it is believed that the intermediate heat treatment produces precipitates with a particle size of 10 to 100 nm at 50 particles / μm. 2 It is presumed that because a large amount of dislocations are formed at a density of 180°C or higher and a large amount of dislocations are introduced by the above-mentioned finish cold rolling, when heated to a temperature range of 180 to 500°C, the pinning effect of the finely dispersed precipitates is exerted, and dislocation rearrangement occurs in a form advantageous for reducing the crystallite size. If the heating temperature is 180°C or higher, it is thought that dislocation rearrangement can be caused, and as a result, the crystallite size can be reduced. It is thought that by controlling the maximum temperature of the material to 500°C or lower, the dislocations introduced by the finish cold rolling can be sufficiently retained, and as a result, softening can be prevented.
[0038] In this manner, a Cu-Fe-P-based copper alloy sheet having excellent strength, electrical conductivity, and bending workability can be obtained. The thickness of the sheet can be, for example, 0.02 to 2.0 mm, preferably 0.04 to 0.8 mm. This Cu-Fe-P-based copper alloy sheet can be used as a raw material to manufacture electrically conductive parts such as connectors by, for example, punching or bending.
[0039] Copper alloys having the chemical compositions shown in Table 1 were melted to obtain cast pieces having a thickness of 215 mm, a width of approximately 500 mm, and a length of approximately 5,500 mm. Samples taken from the cast pieces were quantitatively analyzed using the method described below. As a result, it was found that all of the samples satisfied the requirement of "total of elements other than Fe, P, Mg, Ni, Sn, Zn, and Cu: 0 to 0.10 mass %."
[0040] (Elemental Analysis Method) O (oxygen) and N (nitrogen) were quantified using an oxygen / nitrogen / hydrogen analyzer (ONH-836, manufactured by LECO), H (hydrogen) was quantified using a hydrogen analyzer (EMGA-921, manufactured by Horiba, Ltd.), C (carbon) and S (sulfur) were quantified using a carbon / sulfur analyzer (CS844, manufactured by LECO), elements of the second to sixth periods (excluding C, N, O, Group 17 elements, Group 18 elements, Tc (technetium), Po (polonium), and Pm (promethium)) were quantified using an ICP-MS (7900, manufactured by Agilent), and F (fluorine), Cl (chlorine), and Br (bromine) were quantified using a combustion-ion chromatography apparatus (DIONEX ICS-1600, manufactured by Thermo Scientific). These measurements allow the quantification of virtually all elements that may be contained in the copper alloy.
[0041] The resulting slab was held at 950°C for 4 hours, removed from the furnace, and subjected to hot rolling. The rolling temperature for each rolling pass was recorded by monitoring the material surface temperature at the work roll exit of the hot rolling mill. With the exception of some examples (Comparative Examples Nos. 33 and 39), the pass schedule was set so that the reduction ratio at rolling temperatures of 950°C to 650°C was 87%, and the reduction ratio at rolling temperatures of 650°C to 350°C was 63 to 68%. In Example No. 39, the pass schedule was set so that the reduction ratio at rolling temperatures of 950°C to 650°C was 87%, and the reduction ratio at rolling temperatures of 650°C to 350°C was 50%. The total reduction ratio was 95.1 to 95.8%, and in all examples, the rolling temperature of the final pass was 350°C or higher. In this manner, hot-rolled sheets with thicknesses of 9.5 to 11.0 mm were obtained. In No. 33, cracks occurred in the material during hot rolling, and the subsequent process was discontinued.
[0042] With the exception of some examples (Comparative Example No. 35), the surface oxide film of the obtained hot-rolled sheets was removed by mechanical polishing (surfacing), and then cold-rolled to a rolling ratio of approximately 67 to 98% (intermediate cold-rolling process). Because No. 35 had a large amount of Mg oxide inclusions in the hot-rolled sheet, it was not allowed to proceed to the process after hot rolling. The cold-rolled material was then subjected to heat treatment in a batch-type heat treatment furnace, where it was held at a holding temperature set in the range of 500 to 600°C for 5 to 9 hours (intermediate heat treatment process). Next, with the exception of some examples (Comparative Example No. 41), the material was subjected to cold-rolling to a rolling ratio of approximately 87 to 98% to a sheet thickness of 0.06 to 0.08 mm (finish cold-rolling process). No. 41 was cold-rolled to a rolling ratio of approximately 60% to a sheet thickness of 0.10 mm. Next, with the exception of some examples (Comparative Example No. 40), heat treatment was performed in a continuous or batch heat treatment furnace under conditions of a maximum temperature of 200 to 430°C, and a time (heat treatment time) of 13 seconds to 30 minutes for the material temperature to reach 180°C or higher but below the maximum temperature (final heat treatment step). This heat treatment was omitted for No. 40. In this way, test specimens with final plate thicknesses of 0.06 to 0.10 mm were obtained. The manufacturing conditions are shown in Table 2. The following investigations were carried out on the obtained test specimens.
[0043] (Number Density of Precipitate Particles) According to the above-mentioned "Method for Determining Number Density of Precipitate Particles", the number density (particles / μm) of precipitate particles with a major axis of 10 to 100 nm was determined. 2 The electrolytic polishing apparatus used was an ElectroMet4 manufactured by BUEHLER, the ultrasonic cleaner used was a BRANSONIC M2800-J, and the FE-SEM used was a JSM-7200F manufactured by JEOL Ltd.
[0044] (Crystallite size) The X-ray diffraction pattern of the plate surface of the test material was measured using an X-ray diffractometer (Rigaku Corporation, RINT-2000) under the conditions of 2θ / θ method, CuKα ray (λ = 0.1542 nm), tube voltage 40 kV, and tube current 40 mA. Using analysis software (Rigaku Corporation, PDXL2), the Kα1 ray and Kα2 ray were analyzed without separating them, and the integral width β was measured for the four diffraction peaks due to the crystal planes (111), (200), (220), and (311) in the 2θ range of 30 to 150°. The horizontal axis is β / (tanθ × sinθ), and the vertical axis is (β / tanθ). 2 The function (Halder-Wagner equation) expressed by the above formula (2) was determined by fitting each plot with a straight line, and the crystallite size D (nm) was calculated from the slope of the function Kλ / D (K: Scherrer constant, λ: X-ray wavelength, D: crystallite size). Here, the value of the Scherrer constant K was 0.94.
[0045] (0.2% yield strength) A tensile test piece (JIS No. 5) was taken from each test material in the direction perpendicular to the rolling direction (TD), and a tensile test was carried out in accordance with JIS Z2241 to measure the 0.2% yield strength. The 0.2% yield strength was 450 N / mm 2 Those that met the above criteria were judged to be acceptable.
[0046] (Conductivity) The conductivity was determined in accordance with JIS H0505. A sample having a conductivity of 50% IACS or more was judged to be acceptable.
[0047] (Bending workability) Test pieces with a width of 0.3 mm, with the longitudinal direction perpendicular to the rolling direction, were cut out from the test material and subjected to a 90°L bending test with the bending axis parallel to the rolling direction (B.W.). The ratio MBR / t, the minimum bending radius MBR at which cracking did not occur and the plate thickness t, was determined. A test piece with an MBR / t of 0.7 or less was judged to have passed. The results are shown in Table 3.
[0048]
[0049]
[0050]
[0051] All of the Cu-Fe-P based copper alloy sheets of the present invention had a high number density of precipitate particles and a structure with a small crystallite size, and were excellent in strength, electrical conductivity, and bending workability.
[0052] In contrast, the comparative examples showed the following results. No. 31 had poor electrical conductivity due to an excessively high Fe content. No. 32 had low strength due to an excessively low Fe content. No. 33 had cracks during hot rolling due to an excessively high P content. No. 34 had poor strength and electrical conductivity due to an insufficient number density of precipitate particles due to an excessively low P content. Furthermore, it is presumed that the pinning effect of finely dispersed precipitates was not fully exerted due to the small amount of precipitates, and dislocation rearrangement, which is advantageous for reducing crystallite size, did not occur sufficiently. Furthermore, due to the softness of the specimen, bending workability was good. No. 35 had too much Mg content, resulting in a hot-rolled sheet with a large amount of Mg oxide inclusions, and further processing was discontinued. No. 36 had poor electrical conductivity due to an excessively high Ni content. No. 37 had poor electrical conductivity due to an excessively high Sn content. No. 38 had poor electrical conductivity due to an excessively high Zn content. No. 39 had a low rolling reduction in the temperature range of less than 650°C and equal to or greater than 350°C during hot rolling, resulting in an insufficient number density of precipitate particles and poor strength and electrical conductivity. Because the dislocation density was low, even after finish heat treatment, reduction of the crystallite size was not achieved. However, because of its softness, bending workability was good. Because finish heat treatment was omitted in No. 40, the crystallite size could not be reduced, resulting in poor bending workability. Because the rolling reduction in No. 41 during finish cold rolling was low, the crystallite size was small, but the introduction of dislocations was insufficient, resulting in a low strength level.
[0053] (Test to Confirm the Effect of Finish Heat Treatment) A sheet material sample (0.08 mm thick intermediate product) obtained immediately after the finish cold rolling of the No. 2 example of the present invention and a sheet material sample (0.08 mm thick finished product) subsequently subjected to a finish heat treatment with a maximum temperature of 430°C and a time of 13 seconds to keep the material temperature above 180°C but below the maximum temperature were used to measure crystallite size and 0.2% proof stress using the methods described above. A 90°L bending test was also conducted with a bending radius of R = 0.05 mm, a sheet thickness of t = 0.08 mm, and a BW of R / t = 0.05 / 0.08 ≈ 0.6. The results are shown in Table 4. For reference, Figures 1 and 2 show laser microscope photographs of the outer surface of the bent portion of the sheet material sample after finish cold rolling and after finish heat treatment, respectively, after a 90°L bending test with R / t ≈ 0.6. The width and length of these photographs correspond to approximately 0.26 mm.
[0054]
[0055] Although no difference in electrical conductivity was observed before and after the finish heat treatment, the finish heat treatment improved both strength and bending workability. Although it has generally been said that there is a trade-off between strength and bending workability, the finish heat treatment was able to improve both properties simultaneously. This is presumably due to the effect of the finish heat treatment proceeding with the rearrangement of dislocations and the reduction in crystallite size under conditions in which precipitates are finely dispersed by the manufacturing process according to the present invention.
Claims
1. The chemical composition is, in mass%, Fe: 0.05-1.10%, P: 0.02-0.50%, Mg: 0-0.50%, Ni: 0-0.80%, Sn: 0-0.80%, Zn: 0-0.80%, the total of elements other than Fe, P, Mg, Ni, Sn, Zn, and Cu: 0-0.10%, and the balance is Cu. The crystallite size according to the Halder-Wagner method based on the integral width of the peak in the X-ray diffraction pattern using CuKα rays on the plate surface is 30 nm or less, and the 0.2% proof stress in the direction perpendicular to the rolling direction is 450 N / mm 2 That is all about the copper alloy sheet material.
2. In the observation plane parallel to the plate surface, the number density of precipitate particles with a major axis of 10 to 100 nm is 50 particles / μm 2 The copper alloy sheet material according to claim 1 .
3. The copper alloy sheet material according to claim 1, having an electrical conductivity of 50% IACS or more.
4. The copper alloy sheet material according to claim 1, wherein a ratio MBR / t of the minimum bending radius MBR at which cracks do not occur to the sheet thickness t in a 90°L bending test with the bending axis parallel to the rolling direction (B.W.) is 0.7 or less.
5. A hot rolling process in which a cast slab having a chemical composition consisting of, by mass%, Fe: 0.05-1.10%, P: 0.02-0.50%, Mg: 0-0.50%, Ni: 0-0.80%, Sn: 0-0.80%, Zn: 0-0.80%, the sum of elements other than Fe, P, Mg, Ni, Sn, Zn, and Cu: 0-0.10%, and the balance being Cu, is rolled at a rolling reduction rate of 70% or more in a temperature range of 950°C to 650°C and then rolled at a rolling reduction rate of 60% or more in a temperature range of 350°C to 650°C; an intermediate cold rolling process in which cold rolling at a rolling reduction rate of 30% or more is performed; and an intermediate heat treatment process in which the material obtained in the intermediate cold rolling process is heat treated by holding it at a temperature of 400°C to 700°C for 1 hour or more. a finish cold rolling step of subjecting the material obtained in the intermediate heat treatment step to cold rolling at a rolling ratio of 80% or more; and a finish heat treatment step of subjecting the material obtained in the finish cold rolling step to a heat treatment by heating to a temperature range of 180°C or more and 500°C or less, in the above order.
6. The method for producing a copper alloy sheet according to claim 5, wherein in the finish heat treatment step, a material is obtained having a crystallite size of 30 nm or less as determined by the Halder-Wagner method based on the integral width of a peak in an X-ray diffraction pattern using CuKα radiation on the sheet surface.
7. An electric current-carrying part using the copper alloy sheet material according to any one of claims 1 to 4.
Citation Information
Patent Citations
Copper alloy plate, heat dissipation electronic component equipped therewith, and method for manufacturing the copper alloy plate
JP5467163B1
Method for producing high strength and high conductivity copper alloy
JP2006016687A
Copper alloy having bendability and stress relaxation property
JP2006200036A
Copper alloy containing phosphorus and iron and electrical member using the copper alloy
WO2010103646A1
Covered electric wire, electric wire having terminal, copper alloy wire, copper alloy stranded wire, and production method for copper alloy wire