Thermoelectric conversion material and method for producing thermoelectric conversion material
The development of a thermoelectric conversion material with a skutterudite structure and optimized intergranular layer composition enhances electrical conductivity and reduces thermal conductivity, addressing the limitations of current materials and achieving higher ZT values for efficient energy conversion.
Patent Information
- Application Number
- PCT/JP2024/006812
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-02-26
- Publication Date
- 2024-10-03
AI Technical Summary
Current thermoelectric conversion materials face challenges in achieving a high dimensionless figure of merit ZT, which limits their efficiency in converting thermal energy into electrical energy, due to the correlation between electrical and thermal conductivity, making it difficult to increase ZT beyond a certain threshold.
A thermoelectric conversion material with a skutterudite crystal structure containing Yb, Co, and Sb, featuring a secondary intergranular layer with a specific atomic ratio of O to Yb between 0.4 and 1.5, and a method involving rapid solidification, heat treatment, and pressure sintering to optimize the material's properties, including the introduction of Yb oxides and CoSb2 crystals, is developed to enhance electrical conductivity while reducing thermal conductivity.
The approach results in a thermoelectric conversion material with a higher dimensionless figure of merit ZT, improving energy conversion efficiency and reliability, and allowing for the effective utilization of waste heat energy.
Smart Images

Figure JP2024006812_03102024_PF_FP_ABST
Abstract
Description
Thermoelectric conversion material and method for producing the same
[0001] The present invention relates to a thermoelectric conversion material and a method for producing a thermoelectric conversion material.
[0002] Currently, huge amounts of thermal energy are emitted from large-scale power generation systems such as thermal power plants, steel furnaces, waste incinerators, and automobiles powered by fossil fuel engines. Some of the emitted thermal energy is used as a heat source for hot water and heating, but most is discarded unused. Waste thermal energy that is discarded unused is called unused waste thermal energy. If unused waste thermal energy could be efficiently utilized and recovered, it would lead to a reduction in energy consumption throughout the entire social system, and would make a significant contribution to solving energy problems and environmental issues such as global warming.
[0003] Thermoelectric power generation systems, which convert thermal energy into electrical energy, have attracted attention for their potential to recycle unused waste heat. A thermoelectric power generation system uses a thermoelectric module with multiple elements: n-type thermoelectric materials, which have electrons as carriers, and p-type thermoelectric materials, which have holes as carriers, connected via a conductive material. When a temperature gradient occurs between one side of the thermoelectric module and the other, electrons are excited in the high-temperature region of the n-type thermoelectric material, increasing the concentration of free electrons (carrier concentration). In the low-temperature region, the carrier concentration is low, so free electrons diffuse to the low-temperature region. As a result, a potential difference occurs between the high-temperature and low-temperature regions, resulting in a high potential on the high-temperature side. Meanwhile, in p-type thermoelectric materials, holes are excited in the high-temperature region, which migrate to the low-temperature region, generating thermoelectric power, resulting in a high potential on the low-temperature side. When n-type and p-type thermoelectric materials are connected via a conductive material, an electric current flows between them (known as the Seebeck effect), behaving like a battery. A thermoelectric power generation system supplies the electrical energy obtained in this way.
[0004] In other words, the thermoelectric materials used in thermoelectric conversion modules directly exchange energy in a solid state, do not emit carbon dioxide, and do not require cooling using refrigerants such as fluorocarbon gas. Therefore, their value has been reassessed in recent years as an energy technology that coexists with the environment.
[0005] Techniques relating to thermoelectric conversion materials are disclosed in, for example, Patent Documents 1 and 2.
[0006] Patent Document 1 describes a method for producing a filled skutterudite alloy, which comprises melting an alloy raw material consisting of a rare earth metal R (where R is at least one of La, Ce, Pr, Nd, Sm, Eu, and Yb), a transition metal T (where T is at least one of Fe, Co, Ni, Os, Ru, Pd, Pt, and Ag), and metal antimony (Sb), and then rapidly solidifying the molten metal by strip casting. Patent Document 1 also describes that a substantially uniform filled skutterudite alloy can be easily mass-produced by a casting method using strip casting. Patent Document 1 also describes that the produced filled skutterudite alloy can be used directly in a thermoelectric conversion element without the need for milling and sintering, thereby significantly reducing the production cost of the thermoelectric conversion element.
[0007] In addition, Patent Document 2 discloses Yb x Co 4 Sb 12 The article describes a method for producing a filled-skutterudite alloy, which is characterized by melting alloy raw materials expressed in a ratio of: 1000 to 10000, rapidly solidifying the molten metal by strip casting, and heat-treating the heat-treated raw material powder in hydrogen and then sintering it immediately to precipitate a non-stoichiometric Yb-O compound. It also describes that this treatment results in higher thermoelectric performance than materials that are not treated in hydrogen.
[0008] JP 2004-76046 A International Publication No. 2019 / 139168
[0009] The performance of thermoelectric conversion materials is evaluated by a quantity called the dimensionless figure of merit ZT, and a ZT greater than 1 is considered a benchmark for practical use. It is said that a thermoelectric conversion material with a ZT ≒ 1 has a theoretical power generation efficiency of approximately 9%.
[0010] ZT = S 2 σT / κ (1) In the formula (1), S is the Seebeck coefficient, σ is the electrical conductivity, κ is the thermal conductivity, and T is the absolute temperature.
[0011] As shown in the formula (1) above, a thermoelectric conversion material with good performance, i.e., high efficiency, is a material with a large electrical conductivity σ and a large Seebeck coefficient S, and a small thermal conductivity κ. However, in general, there is a correlation between thermoelectric conversion materials such that the higher the electrical conductivity σ of a material, the higher the thermal conductivity κ, and the lower the electrical conductivity σ of a material, the lower the thermal conductivity κ, so it is difficult to increase the dimensionless figure of merit ZT.
[0012] Furthermore, although the thermoelectric conversion material containing the Yb—O compound described in Patent Document 2 is designed to have a high dimensionless figure of merit ZT, it is desirable to further increase this figure.
[0013] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a thermoelectric conversion material that has a higher dimensionless figure of merit ZT and high reliability, and a method for manufacturing such a thermoelectric conversion material.
[0014] The object of the present invention is achieved by the following means: A thermoelectric conversion material according to the present invention has oxide crystals formed in secondary intergranular layers present between crystal grains in polycrystalline grains having a skutterudite-type crystal structure containing Yb, Co, and Sb, in which the atomic ratio of O to Yb is greater than 0.4 and not more than 1.5.
[0015] The thermoelectric conversion material according to the present invention comprises a crystal having Yb oxide formed in a secondary intergranular layer present between crystal grains in a polycrystalline grain having a skutterudite-type crystal structure containing Yb, Co, and Sb, and a CoSb 2 and has crystals of.
[0016] a mixing step of melting and mixing the raw materials; a ribbon production step of rapidly solidifying the molten raw materials by a liquid rapid solidification method to produce a ribbon; a step of heat treating the produced ribbon in an inert atmosphere having an adjusted oxygen concentration; and a pulverization step, and the method further comprises a first heat treatment step of obtaining polycrystalline grains; a second heat treatment step of heat treating the polycrystalline grains again in an inert atmosphere having an adjusted oxygen concentration in order to adjust the oxygen concentration in the polycrystalline grains heat-treated in the first heat treatment step; a reducing atmosphere pressure heat treatment step of pressure-heat treating the polycrystalline grains heat-treated in the second heat treatment step in a reducing atmosphere; and a pressure sintering step of pressure-sintering the polycrystalline grains pressure-heat-treated in the reducing atmosphere pressure heat treatment step in an inert atmosphere to produce a thermoelectric conversion material.
[0017] According to the present invention, it is possible to provide a thermoelectric conversion material having a higher dimensionless figure of merit ZT and high reliability, and a method for producing such a thermoelectric conversion material.
[0018] 1B is a schematic diagram illustrating the structure of a thermoelectric conversion material 1 according to the present embodiment.
[0024] FIG. 1B is a schematic diagram illustrating the structure of a thermoelectric conversion material 1 according to the present embodiment, clearly showing the interior of a polycrystalline grain 11. It is an enlarged view of the ic portion of FIG. 1B. It is a schematic diagram illustrating the structure of a thermoelectric conversion material 1 according to the present embodiment before the reducing-atmosphere pressure heat treatment step S6 (a structure not subjected to the reducing-atmosphere pressure heat treatment step S6). It is an SEM image of a sample (comparative example) of a sintered material that was subjected to the pressure sintering step S7 without the reducing-atmosphere pressure heat treatment step S6 after the second heat treatment step S5. The scale bar in the figure indicates 10 μm. It is an SEM image of a sample (comparative example) of a sintered material that was subjected to the pressure sintering step S7 without the reducing-atmosphere pressure heat treatment step S6 after the second heat treatment step S5, showing the interfaces of polycrystalline grains 11. The scale bar in the figure indicates 10 μm.
[0025] FIG. 4 is a perspective view illustrating the configuration of a thermoelectric conversion module 10 according to the present embodiment. It shows a state before the upper substrate 6 is attached. 1 is a perspective view showing the configuration of a thermoelectric conversion module 10 according to the present embodiment. FIG. 5 shows a state after the upper substrate 6 has been attached. FIG. 6 is a flowchart showing the details of a manufacturing method for a thermoelectric conversion material 1 according to the present embodiment. FIG. 7 is a graph showing the measurement temperature dependence of the dimensionless figure of merit (ZT) for samples (Nos. 1 to 3 (all examples)) and samples (Nos. 11 and 10 (all comparative examples)). FIG. 8 is a graph showing the measurement temperature dependence of the dimensionless figure of merit (ZT) for samples (Nos. 8, 7, 6, and 9 (all examples)) and samples (Nos. 11 and 10 (all comparative examples)). 1 is a graph showing the measurement temperature dependence of lattice thermal conductivity for samples (Nos. 1 to 3 (all examples)) and samples (Nos. 11 and 10 (all comparative examples)). 2 is a graph showing the measurement temperature dependence of lattice thermal conductivity for samples (Nos. 4, 2, and 5 (all examples)) and samples (Nos. 11 and 10 (all comparative examples)). 3 is an SEM image of sample No. 5 (example).13A is a phase image of EBSD (electron backscatter diffraction) at portion xiib shown in FIG. 12A. FIG. 12B is a diagram showing the types of phases confirmed in FIG. 12B. FIG. 13C is a STEM dark field image of portion xiii of FIG. 1C, which schematically illustrates the structure of thermoelectric conversion material 1 according to the example. The scale bar in the image represents 1 μm. FIG. 13A is a STEM dark field image at position b. The scale bar in the image represents 0.1 μm. FIG. 13A is a STEM dark field image at position c. The scale bar in the image represents 0.1 μm. FIG. 13A is a STEM dark field image at position d. The scale bar in the image represents 0.1 μm. FIG. 13A is a STEM dark field image at position e. The scale bar in the image represents 0.1 μm.
[0019] Next, an embodiment of the thermoelectric conversion material 1 and a method for manufacturing the thermoelectric conversion material 1 according to the present invention will be described in detail with reference to the drawings as appropriate.
[0020] [Thermoelectric Conversion Material 1] FIG. 1A is a schematic diagram illustrating the structure of thermoelectric conversion material 1 according to this embodiment. FIG. 1B is a schematic diagram illustrating the structure of thermoelectric conversion material 1 according to this embodiment, clearly showing the inside of polycrystalline grain 11. FIG. 1C is an enlarged view of portion ic in FIG. 1B. Note that FIGS. 1A, 1B, and 1C are schematic illustrations based on phase map images obtained by scanning electron microscope (SEM) and electron backscatter diffraction (EBSD). FIG. 2 is a schematic diagram illustrating the structure of thermoelectric conversion material 1 according to this embodiment before the reducing atmosphere pressure heat treatment step S6 described later is performed (a structure that has not been subjected to the reducing atmosphere pressure heat treatment step S6).
[0021] As shown in FIG. 1A , the thermoelectric conversion material 1 according to this embodiment has: (1) a secondary intergranular layer 13 present between crystal grains 15 in polycrystalline grains 11 having a skutterudite-type crystal structure containing Yb, Co, and Sb; and oxide crystals (grain boundary precipitates 16 (see FIG. 1C )) having an atomic ratio of O to Yb of more than 0.4 and not more than 1.5. As will be described later, the polycrystalline grains 11 are pulverized grains produced during the manufacturing process, and the thermoelectric conversion material 1 according to this embodiment is a sintered body obtained by pressure sintering the polycrystalline grains 11. The thermoelectric conversion material 1 according to this embodiment also has: (2) a secondary intergranular layer 13 present between crystal grains 15 in polycrystalline grains 11 having a skutterudite-type crystal structure containing Yb, Co, and Sb; and (3) a secondary intergranular layer 13 present between crystal grains 15 in polycrystalline grains 11 having a skutterudite-type crystal structure containing Yb, Co, and Sb; and (4) a secondary intergranular layer 13 present between crystal grains 15 in polycrystalline grains 11 having a skutterudite-type crystal structure containing Yb, Co, and Sb; 2 Crystals of and can coexist.
[0022] It is believed that the thermoelectric conversion material 1 according to this embodiment can achieve the desired effect by having at least one of the above-described structures (1) and (2) for reasons described below. At present, it is not necessarily clear which of these structures functions more effectively in achieving the desired effect, but it has been confirmed by analysis, etc., described below, that the thermoelectric conversion material 1 has these structures.
[0023] The thermoelectric conversion material 1 having such a configuration can be suitably obtained by the manufacturing method of the thermoelectric conversion material 1 described below. The intergranular layers 12 are introduced by heat treatment, but some of the intergranular layers 12 also extend between the crystals inside the polycrystalline grains 11, like grain boundary precipitates 17. By having the above configuration, the thermoelectric conversion material 1 can increase the electrical conductivity σ while decreasing the thermal conductivity κ, for reasons that will be explained in the reducing atmosphere pressure heat treatment step S6 described below, and as a result, it is thought that the dimensionless figure of merit ZT becomes higher.
[0024] The portion where the crystal grain 15 shown in part ic of Fig. 1B is separated from the adjacent crystal by the grain boundary precipitate 16 (Fig. 1C) is formed during the pressure heat treatment in a reducing atmosphere. This portion penetrates from the intergranular layer 12 in Fig. 2 by the pressure heat treatment in a reducing atmosphere to form the secondary intergranular layer 13 (Fig. 1B). Here, Fig. 1C shows the composition of the secondary intergranular layer 13 in detail. The grain boundary precipitate 16 in the secondary intergranular layer 13 shown in Fig. 1C contains Yb, which has a different crystal structure. 2 O 3 , non-stoichiometric Yb 2-α O 3-β (where α and β are arbitrary numbers that make Yb and O non-stoichiometric) and YbO, Yb 3 O 4 and CoSb 2 Includes:
[0025] In addition, if the reducing-atmosphere pressure heat treatment is not performed, the secondary intergranular layer 13 does not exist in the structure, as shown in, for example, part II in FIG. 2 . The secondary intergranular layer 13 is formed by the reducing-atmosphere pressure heat treatment. Furthermore, after the reducing-atmosphere pressure heat treatment, some parts of the intergranular layer 12 are also a mixture of the secondary intergranular layer 13. Furthermore, as shown in FIG. 2 , if the reducing-atmosphere pressure heat treatment is not performed, the polycrystalline grain interface 18 between the polycrystalline grains 11 (see FIG. 3B ) contains the intergranular layer 12 and grain boundary precipitates 17 extending from the intergranular layer 12 to a depth of approximately 3 to 5 grains or less, but does not contain the grain boundary precipitates 16 deeply penetrating and precipitating within the polycrystalline grains 11. In contrast, in the sintered body produced from the raw material after the reducing-atmosphere pressure heat treatment, the grain boundary precipitates 16 deeply penetrating and precipitating within the crystal grains 15 within the polycrystalline grains 11 shown in FIG. 1B (see FIG. 1C ) are present.
[0026] The skutterudite-type crystal structure containing Yb, Co, and Sb has a crystal structure (cubic crystal) in which Co is surrounded by an octahedral structure of Sb sharing the vertices, and the gaps in the crystal structure are filled with Yb (this is called a filled skutterudite structure, etc.). As such a skutterudite-type crystal structure containing Yb, Co, and Sb, the composition formula Yb is preferably used. x Co 4 Sb 12(where x is greater than 0 and 0.3 or less) can be used. Note that x is preferably 0.1 or more, and more preferably 0.2 or more. Also, x is preferably 0.3 or less. The thermoelectric conversion material 1 functions favorably when it has polycrystalline grains 11 configured including crystal grains 15 with such a crystal structure, preferably polycrystalline grains 11 configured including crystal grains 15 with a crystal structure represented by the above composition formula.
[0027] It is preferable that at least one of the thermal conductivity κ and the electrical conductivity σ of this thermoelectric conversion material 1 is anisotropic. Such anisotropy is obtained by polycrystalline grains 11 with different aspect ratios that constitute the thermoelectric conversion material 1 being aligned in a substantially constant direction, as shown in Figure 1A. That is, the anisotropy of the thermal conductivity κ and the electrical conductivity σ is thought to arise because the number of intergranular layers 12 passing per unit path differs due to the anisotropy of the shapes of the polycrystalline grains 11 with different aspect ratios.
[0028] Polycrystalline grains 11 with different aspect ratios can be obtained, for example, by preparing ribbons by a liquid quenching solidification method, pulverizing the ribbons to obtain pulverized polycrystalline grains 11, tapping the polycrystalline grains 11, and then pressure-sintering the pulverized polycrystalline grains 11, as described in the manufacturing method described below. That is, by tapping and then pressure-sintering, the polycrystalline grains 11 can be formed to have different aspect ratios and aligned in a substantially uniform direction. The thermal conductivity κ and the electrical conductivity σ are imparted by the shape of the polycrystalline grains 11 formed by tapping and pressure-sintering and the resulting intergranular layers 12. Therefore, in many cases, the anisotropic directions of the thermal conductivity κ and the electrical conductivity σ coincide. To facilitate the anisotropy, it is preferable to vibrate the polycrystalline grains 11, for example by tapping, to improve their stability, followed by pressure-sintering.
[0029] The size of the polycrystalline grains 11 preferably has a maximum length of, for example, 10 to 500 μm. The maximum length refers to the distance between the two most distant points on one polycrystalline grain 11 in an image taken by an electron microscope or the like. When the size of the polycrystalline grains 11 is within this range, it becomes easier to control the oxygen concentration in the sintered body after pressure sintering. The size of the polycrystalline grains 11 can be controlled, for example, by appropriately changing the crushing time when crushing the ribbon.
[0030] The polycrystalline grains 11 are formed as a metal structure containing numerous crystal grains 15 with the aforementioned skutterudite-type crystal structure containing Yb, Co, and Sb. Because the atomic arrangement of each crystal grain 15 is different from that of the others, a region where the atomic arrangement of the crystal structure is disordered, i.e., a grain boundary (crystal grain boundary), is formed between adjacent crystal grains 15. The secondary intergranular layer 13 is formed to surround each crystal grain 15. The maximum length of the crystal grains 15 constituting the polycrystalline grains 11 is preferably, for example, 1 to 50 μm, but is not limited to this range. A maximum length of the crystal grains 15 within this range can achieve high density. The maximum length of the crystal grains 15 can be controlled, for example, by appropriately changing the quenching rate in the ribbon preparation step S3 and the heat treatment temperatures in the first heat treatment step S4, the second heat treatment step S5, the reducing atmosphere pressure heat treatment step S6, and the pressure sintering step S7.
[0031] The thermoelectric conversion material 1 may also have crystals (grain boundary precipitates 16) with an atomic ratio of O to Yb greater than 0.4 and not greater than 1.5 between polycrystalline grains 11 of a structure having crystals (grain boundary precipitates 16) formed in secondary intergranular layers 13 present between crystal grains 15 within polycrystalline grains 11 having a skutterudite-type crystal structure containing Yb, Co, and Sb. In this way, the thermoelectric conversion material 1 can increase the electrical conductivity σ while decreasing the thermal conductivity κ for reasons that will be explained in the reducing atmosphere pressure heat treatment step S6 described below, and as a result, the dimensionless figure of merit ZT is thought to be higher.
[0032] The thermoelectric conversion material 1 has the numerous polycrystalline grains 11 described above and intergranular layers 12 present between adjacent polycrystalline grains 11 and having crystals (grain boundary precipitates 16) with an atomic ratio of O to Yb exceeding 0.4 and not more than 1.5. The secondary intergranular layers 13 precipitated in the intergranular layers 12 preferably have an atomic ratio of O to Yb of not more than 1.5. Furthermore, the thermoelectric conversion material 1 may be a mixture of these Yb oxides and a Co—Sb-based alloy.
[0033] In this embodiment, the thermoelectric conversion material 1 may have a secondary intergranular layer 13 in which the atomic ratio of O to Yb is greater than 0.4 and not greater than 1.5, and may further have an intergranular layer 12. In other words, the atomic ratio of O to Yb contained in the intergranular layer 12 does not have to be entirely within the above-mentioned range. The thermoelectric conversion material 1 may contain, in the crystals precipitated in the intergranular layer 12, a mixture of crystals in which the atomic ratio of O to Yb is 0.4 or less, or a mixture of crystals in which the atomic ratio of O to Yb is greater than 1.5.
[0034] The raw material thus formed with the intergranular layer 12 is subjected to a reducing atmosphere pressure heat treatment to form the secondary intergranular layer 13. Furthermore, by activating the reducing atmosphere gas at the treatment temperature, the crystals (grain boundary precipitates 16) precipitated in the secondary intergranular layer 13 form precipitates of various chemical forms. Furthermore, the generation of conduction electrons due to deviation from the stoichiometric composition suppresses a decrease in electrical conductivity, making it possible to maintain low thermal conductivity. This is believed to enable the thermoelectric conversion material 1 to have a low thermal conductivity κ while increasing its electrical conductivity σ, thereby further increasing the dimensionless figure of merit ZT.
[0035] 3A and 3B are electron microscope (SEM) images of a sample (comparative example) of a sintered body that was subjected to the pressure sintering step S7 without the reducing atmosphere pressure heat treatment step S6 after the second heat treatment step S5 (described later). Note that FIG. 3B illustrates the SEM image with reference numerals. As shown in FIG. 3B, ribbon grain boundaries 14, polycrystalline grain boundaries 18, and precipitated intergranular layers 12 can be seen in this sample. Note that the ribbon grain boundaries refer to grain boundaries formed after rapid cooling, heat treatment, and pulverization. As shown in FIG. 3B, the components of the intergranular layers 12 at the polycrystalline grain boundaries 18 penetrate into the polycrystalline grains 11, but the distance is limited to approximately 2.5 μm.
[0036] The raw material used for the thermoelectric conversion material 1 according to this embodiment preferably has an oxygen concentration of 1200 mass ppm or more before the reducing-atmosphere pressure heat treatment. This allows many intergranular layers 12 to be introduced into the raw material after the reducing-atmosphere pressure heat treatment, and allows the secondary intergranular layers 13 shown in FIG. 1 to be introduced at many locations. Even when the oxygen concentration of the raw material before the reducing-atmosphere pressure heat treatment is 1200 mass ppm or more, the thermoelectric conversion material 1 produced by the method for producing the thermoelectric conversion material 1 described below has an overall oxygen concentration of 1200 mass ppm or less. When the overall oxygen concentration is 1200 mass ppm or less, the crystals (grain boundary precipitates 16) precipitated in the secondary intergranular layers 13 are likely to form precipitates of various chemical forms. Therefore, it is believed that the thermoelectric conversion material 1 can have a low thermal conductivity κ while a high electrical conductivity σ, thereby achieving a high dimensionless figure of merit ZT.
[0037] The thicknesses of the intergranular layer 12 and the secondary intergranular layer 13 are preferably 5 nm or more and 1 μm or less. When the thicknesses of the intergranular layer 12 and the secondary intergranular layer 13 are within this range, the thermal conductivity κ of the thermoelectric conversion material 1 decreases, and the dimensionless figure of merit ZT can be further increased. From the viewpoint of further increasing the electrical conductivity between the crystal grains 15, the thicknesses of the intergranular layer 12 and the secondary intergranular layer 13 are more preferably 5 nm or more and 100 nm or less. The thicknesses of the intergranular layer 12 and the secondary intergranular layer 13 can be controlled, for example, by appropriately changing the quenching rate in the ribbon preparation step S3 or the heat treatment temperature in the pressure sintering step S7. The maximum length of the polycrystalline grains 11, the maximum length of the crystal grains 15, the maximum length of the grain boundary precipitates 16, the thickness of the intergranular layer 12, and the thickness of the secondary intergranular layer 13 can be observed and measured, for example, using a scanning electron microscope (SEM) or a transmission electron microscope (TEM).
[0038] The thermoelectric conversion material 1 according to this embodiment can achieve the same effect even if an active material such as Ba, La, or Sr is incorporated. The thermoelectric conversion material 1 according to this embodiment may contain impurities as long as they do not adversely affect thermoelectric conversion.
[0039] The thermoelectric conversion material 1 according to the present embodiment described above has oxide crystals (grain boundary precipitates 16) in which the atomic ratio of O to Yb is greater than 0.4 and not greater than 1.5 in the secondary intergranular layers 13 present between the crystal grains 15 in the polycrystalline grains 11 having a skutterudite-type crystal structure containing Yb, Co, and Sb. Alternatively, the thermoelectric conversion material 1 has crystals (grain boundary precipitates 16) having Yb oxide and CoSb in the secondary intergranular layers 13 present between the crystal grains 15 in the polycrystalline grains 11 having a skutterudite-type crystal structure containing Yb, Co, and Sb. 2 The thermoelectric conversion material 1 has a crystal structure of the above formula. It is believed that the thermoelectric conversion material 1 can have a small thermal conductivity κ and a high electrical conductivity σ, and as a result, the dimensionless figure of merit ZT becomes higher.
[0040] [Thermoelectric Conversion Module 10] Next, the thermoelectric conversion module 10 according to this embodiment will be described. Figures 4 and 5 are perspective views showing the configuration of the thermoelectric conversion module 10 according to this embodiment. Figure 4 shows the state before the upper substrate 6 is attached, and Figure 5 shows the state after the upper substrate 6 is attached.
[0041] As shown in FIGS. 4 and 5 , the thermoelectric conversion material 1 according to the present embodiment can be mounted on a thermoelectric conversion module 10. The thermoelectric conversion module 10 includes a plurality of elements 4, each of which includes a columnar thermoelectric conversion material 1 and a columnar thermoelectric conversion material 2 of opposite phase to the thermoelectric conversion material 1, connected at its ends via a conductive material 3. Although not particularly limited, the elements 4 may be configured such that the thermoelectric conversion material 1 and the opposite-phase thermoelectric conversion material 2 are alternately and electrically connected in series via the conductive material 3, as shown in FIGS. 4 and 5 . The elements 4, each of which includes the thermoelectric conversion material 1, the opposite-phase thermoelectric conversion material 2, and the conductive material 3, are disposed between a lower substrate 5 and an upper substrate 6 (see FIG. 5 ). Among the conductive materials 3, the first conductive material 3 a is connected to the thermoelectric conversion material 1, and the second conductive material 3 b is connected to the thermoelectric conversion material 2. The first conductive material 3 a is connected to a voltage-drawing wiring 7, and the second conductive material 3 b is connected to a voltage-drawing wiring 8.
[0042] Here, the reversed-phase thermoelectric conversion material 2 is, for example, n-type when the thermoelectric conversion material 1 is p-type, and p-type when the thermoelectric conversion material 1 is n-type. Examples of the conductive material 3 include thin plates, films, thin films, etc. made of copper, silver, gold, platinum, aluminum, or an alloy of any one of these metals. The conductive material 3 is only required to have conductivity, and is not limited to the metals or forms described above. For example, if it is placed on the low-temperature side, a film made of a conductive polymer can be used as the conductive material 3. The lower substrate 5 and the upper substrate 6 can be made of, for example, aluminum nitride (AlN) or silicon nitride (Si 3 N 4 ), alumina oxide (Al 2 O 3 ) or the like can be used.
[0043] The thermoelectric conversion module 10 of the above-described embodiment can generate a temperature gradient in the same direction for the thermoelectric conversion material 1 and the opposite-phase thermoelectric conversion material 2 by, for example, heating the upper substrate 6 or bringing it into contact with a high-temperature area. This causes thermoelectric power to be generated in the thermoelectric conversion material 1 and the opposite-phase thermoelectric conversion material 2 due to the Seebeck effect. At this time, thermoelectric power is generated in the thermoelectric conversion material 1 and the opposite-phase thermoelectric conversion material 2 in the opposite direction to the temperature gradient, and the thermoelectric powers are added together rather than being canceled out. This allows the thermoelectric conversion module 10 to generate a large thermoelectric power. In addition to the above-described embodiment, the temperature gradient can also be generated by bringing the lower substrate 5 into contact with a cooled or low-temperature area. Furthermore, the upper substrate 6 may be brought into contact with a heated or high-temperature area while the lower substrate 5 is brought into contact with a cooled or low-temperature area.
[0044] The thermoelectric conversion module 10 according to the present embodiment described above uses the thermoelectric conversion material 1 according to the present embodiment described above. Therefore, for the same reasons as those described for the thermoelectric conversion material 1 according to the present embodiment, the thermoelectric conversion module 10 according to the present embodiment has a higher dimensionless figure of merit ZT and is also highly reliable.
[0045] [Method for manufacturing thermoelectric conversion material 1] Next, a method for manufacturing the thermoelectric conversion material 1 according to this embodiment will be described. Fig. 6 is a flowchart showing the details of the method for manufacturing the thermoelectric conversion material 1 according to this embodiment (hereinafter, sometimes simply referred to as the present manufacturing method). This manufacturing method is, for example, a method for manufacturing the thermoelectric conversion material 1 according to this embodiment described above.
[0046] As shown in Figure 6, this manufacturing method includes a weighing step S1, a mixing step S2, a ribbon-making step S3, a first heat treatment step S4, a second heat treatment step S5, a reducing-atmosphere pressure heat treatment step S6, and a pressure sintering step S7. In this manufacturing method, it is desirable to avoid contact with an oxidizing atmosphere (e.g., air) between the first heat treatment step S4 and the second heat treatment step S5, which are performed before the pressure sintering step S7, and between the reducing-atmosphere pressure heat treatment step S6 and the pressure sintering step S7, in order to control the structure. Preferably, the reducing-atmosphere pressure heat treatment step S6 and the pressure sintering step S7 are performed using an airtight furnace. These steps will be described in order below.
[0047] (Weighing Step S1) The weighing step S1 is a step of weighing each of the raw materials containing Yb, the raw material containing Co, and the raw material containing Sb. These raw materials can be weighed using a general weighing machine. The raw materials may be in any form. That is, the raw materials may be, for example, ores, scrap materials, or pre-purified, highly pure products. Here, the contents of Yb, Co, and Sb contained in each raw material are analyzed in advance, and based on the analysis, it is determined that the composition formula of the raw materials after weighing is Yb. x Co 4 Sb 12 (where x is greater than 0 and 0.3 or less).
[0048] Furthermore, weighing is preferably performed in a sealed working apparatus, such as a glove box, that allows work to be performed in an environment isolated from the outside air. It is preferable to use a sealed working apparatus that can supply an inert gas, such as nitrogen or argon, to the inside. It is more preferable to perform weighing in a sealed working apparatus with an oxygen concentration of 0.1 to 100 ppm by mass. The raw materials weighed in the sealed working apparatus are preferably placed in a heat-resistant container, such as a graphite crucible. Furthermore, the raw materials weighed in the sealed working apparatus are preferably placed in a quartz container or the like and vacuum-sealed. While any one of these methods can prevent excessive (more than necessary) oxidation of the raw materials, it is preferable to perform all of them. As will be described later, in this embodiment, excessive oxidation is not preferable. However, after partially oxidizing only the surface of the ribbon, a heat treatment is performed in the second heat treatment step S5 to precipitate a portion of Yb oxide in the intergranular layer 12 at a preferable concentration, and then a reducing atmosphere pressure heat treatment step S6 is performed to change the structure to a preferable one.
[0049] (Mixing Step S2) The mixing step S2 is a step of melting and mixing the raw materials. The raw materials are melted, for example, at 1020°C or higher, preferably 1050°C or higher. From the standpoint of cost and heating device maintenance, the raw materials are melted at 1300°C or lower, more preferably 1100°C or lower. The raw materials are preferably melted at the above temperature for several hours to several tens of hours, followed by rapid cooling. For example, the raw materials are preferably melted at the above temperature for 20 hours, followed by rapid cooling in water cooled to 20°C or lower. If a large amount of raw material is used, slow cooling may be employed. After rapid cooling, the ingot is preferably removed from the quartz container in an inert atmosphere and loaded into a heat-resistant container such as a graphite crucible. For a short period of time, within one hour, the ingot can be removed in air and loaded into a heat-resistant container. The ingot is then reheated, for example, to 1100°C in a high-frequency heating furnace to form a molten metal.
[0050] (Ribbon Production Step S3) The ribbon production step S3 is a step in which the molten metal of the raw materials described above is rapidly solidified by a liquid rapid solidification method to produce a ribbon. The liquid rapid solidification method is a method in which molten metal (molten metal) is dropped onto a rotating metal roll and rapidly cooled at a rate faster than the rate of crystal nucleation, thereby producing a ribbon of amorphous metal. The thickness of the ribbon obtained in the ribbon production step S3 is preferably 10 to 200 μm. If the ribbon thickness is within this range, the uniformity of the structure is high and the degree of oxidation is easy to control. The ribbon production step S3 is also carried out in an inert atmosphere, as described above.
[0051] (First Heat Treatment Step S4) The first heat treatment step S4 includes a step of heat treating the produced ribbon in an inert atmosphere with an adjusted oxygen concentration (not shown in FIG. 6 ) and a step of pulverizing the ribbon (not shown in FIG. 6 ), thereby obtaining pulverized polycrystalline grains 11. That is, the first heat treatment step S4 may involve heat treating the ribbon in an inert atmosphere with an adjusted oxygen concentration, and then pulverizing the ribbon to obtain pulverized polycrystalline grains 11. Alternatively, the first heat treatment step S4 may involve pulverizing the ribbon to obtain pulverized polycrystalline grains 11, and then heat treating the polycrystalline grains 11 in an inert atmosphere with an adjusted oxygen concentration. Alternatively, the first heat treatment step S4 may involve adjusting the flow rate of an inert gas such as nitrogen or argon, which serves as an oxygen carrier, to control the frequency of contact between oxygen and the polycrystalline grains 11.
[0052] Before heat treatment, it is preferable to reload the mixture into a heat-resistant container such as a graphite crucible in a sealed working device (oxygen concentration 0.1 to 100 mass ppm) and cover it with a lid. It is preferable to use a lid for the heat-resistant container with a deep depth, as this allows the oxygen concentration in the heat-resistant container to be low. The depth of the lid for the heat-resistant container is preferably 5 to 10 cm, for example. It is also preferable to load a getter material such as metallic Ti into the heat-resistant container in order to lower the oxygen concentration.
[0053] The oxygen concentration in the inert atmosphere in the first heat treatment step S4 is preferably 10 mass ppm or less, and more preferably 5 mass ppm or less. This allows only the ribbon surface to be slightly oxidized. While excessive oxidation is undesirable in this embodiment, treatment in such an atmosphere can slightly oxidize only the ribbon surface or the surfaces of the polycrystalline grains 11. Furthermore, increasing the oxygen concentration in the material to approximately 1000 ppm in the second heat treatment step S5 performed later facilitates obtaining the structure of the thermoelectric conversion material 1 according to this embodiment in the subsequent reducing atmosphere pressure heat treatment step S6. Therefore, by performing this step, the Yb oxides in the crystals (grain boundary precipitates 16) precipitated in the secondary intergranular layers 13 through the reducing atmosphere pressure heat treatment can be effectively precipitated, thereby reducing thermal conduction. Furthermore, this allows the precipitation of multiple oxides in the grain boundary precipitates 16 precipitated in the secondary intergranular layers 13, with an atomic ratio of O to Yb exceeding 0.4 and not exceeding 1.5. In addition, it is possible to precipitate a plurality of types of non-stoichiometric oxides having the same crystal structure in which the atomic ratio of O to Yb in the grain boundary precipitates 16 precipitated in the secondary intergranular layer 13 is greater than 1.0 and is not more than 1.5. Furthermore, it is possible to precipitate a plurality of types of oxides having the same crystal structure in which the atomic ratio of O to Yb in the grain boundary precipitates 16 precipitated in the secondary intergranular layer 13 is greater than 0.4 and is not more than 1.5, and at the same time, it is possible to precipitate CoSb 2 Crystals of the above-described oxides and crystals can also be precipitated in the secondary intergranular layers 13. The grain boundary precipitates 16, oxides, crystals, and the like described above can also be precipitated in the intergranular layers 12. By having such a configuration, the thermoelectric conversion material 1 can increase the electrical conductivity σ while decreasing the thermal conductivity κ, and can further increase the dimensionless figure of merit ZT.
[0054] The inert atmosphere may be, for example, at least one of nitrogen and argon, but is not limited thereto. The oxygen concentration of the inert atmosphere can be adjusted by using, for example, a mixed gas of hydrogen and argon, a mixed gas of hydrogen and nitrogen, or hydrogen alone. The inert atmosphere may contain water vapor, which slightly promotes oxidation.
[0055] The heat treatment conditions for the first heat treatment step S4 can be, for example, a heat treatment temperature of 500 to 850° C. Furthermore, the heat treatment conditions for the first heat treatment step S4 can be, for example, 3 hours or more and less than 168 hours when the heat treatment temperature is 700° C. From the viewpoint of preventing excessive outflow of Yb from the ribbon or polycrystalline grains 11 to the intergranular layers 12, the heat treatment time is preferably 96 hours or less.
[0056] The ribbon is preferably pulverized in a sealed working apparatus (oxygen concentration 0.1 to 100 ppm). The polycrystalline grains 11 obtained by pulverization preferably have a median diameter (d50) of 5 to 100 μm. This facilitates oxygen concentration control through contact with oxygen, making it easier to obtain a dense sintered body by pressure sintering, as described below. The ribbon pulverization process may be performed after the ribbon preparation process S3, the first heat treatment process S4, the second heat treatment process S5, or the reducing atmosphere pressure heat treatment process S6. It may also be performed at two or more of these processes. The ribbon can be pulverized using, for example, a mortar and pestle, a ball mill, a rod mill, a high-pressure grinding roll, a vertical impactor mill, a jet mill, or the like.
[0057] The polycrystalline grains 11 obtained in the first heat treatment step S4 are weighed in a sealed working apparatus, then loaded into a carbon mold (a die made of carbon) in a draft, and introduced into a pressure sintering apparatus such as a hot press.
[0058] (Second Heat Treatment Step S5) The second heat treatment step S5 is a step of heat treating the polycrystalline grains 11 again in an inert atmosphere with an adjusted oxygen concentration in order to adjust the oxygen concentration in the polycrystalline grains 11 heat-treated in the first heat treatment step S4. By performing this second heat treatment step S5, the Yb oxide in the intergranular layer 12 is adjusted to a more preferable concentration. In addition, this second heat treatment step S5 has the effect of spreading the amount of Yb that has seeped out from the polycrystalline grains 11 throughout the intergranular layer 12. By performing this step and then performing the reducing atmosphere pressure heat treatment step S6 described later, multiple types of oxides are precipitated in the crystals (grain boundary precipitates 16) precipitated in the secondary intergranular layer 13, in which the atomic ratio of O to Yb is greater than 0.4 and less than 1.5, and at the same time, CoSb2 can also be precipitated in the intergranular layers 12 and the secondary intergranular layers 13. These precipitates can reduce the thermal conductivity κ of the thermoelectric conversion material 1 while increasing the electrical conductivity σ, thereby further increasing the dimensionless figure of merit ZT.
[0059] The inert atmosphere may be, for example, at least one of nitrogen and argon, but is not limited thereto. It is desirable to measure the oxygen concentration in the ribbon before the second heat treatment step S5. The oxygen concentration of the inert atmosphere can be adjusted by using, for example, a mixed gas of hydrogen and argon, a mixed gas of hydrogen and nitrogen, or hydrogen alone. The inert atmosphere may also contain water vapor, which slightly accelerates oxidation.
[0060] The heat treatment conditions for the second heat treatment step S5 can be, for example, a heat treatment temperature of 300 to 800° C. Furthermore, the heat treatment conditions for the second heat treatment step S5 can be, for example, 3 hours or more and less than 72 hours when the heat treatment temperature is 700° C. From the viewpoint of preventing extreme oxidation of the ribbons or polycrystalline grains 11, the heat treatment time is preferably 48 hours or less.
[0061] (Reducing Atmosphere Pressure Heat Treatment Step S6) The reducing atmosphere pressure heat treatment step S6 is a step of pressure heat treating the polycrystalline grains 11 heat-treated in the second heat treatment step S5 in a reducing atmosphere. By performing this reducing atmosphere pressure heat treatment step S6, a portion of the Yb oxide precipitated in the intergranular layer 12 is reduced, and a portion of the Yb oxide precipitated in the secondary intergranular layer 13 is reduced, thereby facilitating the precipitation of crystals (grain boundary precipitates 16) in the secondary intergranular layer 13. By performing this step followed by the pressure sintering step S7 described later, crystals (grain boundary precipitates 16) of multiple types of oxides in which the atomic ratio of O to Yb is greater than 0.4 and not more than 1.5 are finally precipitated in the secondary intergranular layer 13, or CoSb is precipitated simultaneously with the precipitation of the crystals. 2Crystals of Yb can also be precipitated in the intergranular layer 12 and the secondary intergranular layer 13. In addition, it is possible to precipitate multiple types of non-stoichiometric oxides that have the same crystal structure, in which the atomic ratio of O to Yb in the crystals precipitated in the secondary intergranular layer 13 (grain boundary precipitates 16) is greater than 1.0 and less than 1.5. Furthermore, by performing the reducing atmosphere pressure heat treatment step S6, the ratio of metal Yb is increased while containing Yb oxide, resulting in a non-stoichiometric composition, which increases the electrical conductivity σ, and the thermal conductivity κ can be reduced by the effect of the secondary intergranular layer 13 and the precipitated crystals (grain boundary precipitates 16). The reason for this is not clear, but for example, Yb 2 O 3 Oxygen is removed from the bonds of extremely stable Yb oxides with low electrical conductivity σ and thermal conductivity κ, resulting in stable oxides with oxygen defects and Yb oxides with multiple crystalline structures that remain unreduced. 2 O 3 This is thought to be because multiple types of Yb oxides, such as CoSb, are generated. Furthermore, since the Yb oxides having these defects need to generate electrons to ensure electrical neutrality, it is thought that the electrical conductivity σ is inevitably high. Therefore, the thermoelectric conversion material 1 heat-treated in this reducing atmosphere pressure heat treatment step S6 can have a high electrical conductivity σ while having a low thermal conductivity κ, and as a result, the dimensionless figure of merit ZT is thought to be higher. In other words, the reducing atmosphere pressure heat treatment step S6 is a process in which the crystalline Yb suboxides generated on the surfaces of the polycrystalline grains 11 in the second heat treatment step S5 are heat-treated to a degree that generates conduction electrons to maintain electrical neutrality in part or all of the crystalline Yb suboxides, just before sintering, and multiple types of Yb oxides and CoSb are generated. 2 and the thermal conductivity κ is reduced.
[0062] The reducing atmosphere in the reducing atmosphere pressure heat treatment step S6 may have a hydrogen concentration of 3% or 100% by volume. This reducing atmosphere pressure heat treatment step S6 is also preferably performed in a sealed working apparatus (oxygen concentration 0.1 to 100 ppm). The reducing atmosphere pressure heat treatment step S6 is preferably performed in a pressure sintering apparatus for pressure sintering. This allows the reducing atmosphere pressure heat treatment step S6 and the pressure sintering step S7 to be performed continuously in the same furnace. This prevents excessive oxidation of the polycrystalline grains 11 heat-treated in the reducing atmosphere pressure heat treatment step S6. In this embodiment, the pressure sintering apparatus is preferably evacuated to, for example, approximately 10 Pa, and then replaced with an inert atmosphere. Examples of the inert atmosphere include, but are not limited to, at least one of nitrogen and argon. This process is preferably repeated two or more times, and after the final evacuation, the hydrogen concentration is preferably set to 3% or 100% by volume, as described above. In addition, in the reducing atmosphere pressure heat treatment step S6, it is more preferable to set the hydrogen concentration to 90% by volume in order to accelerate the reaction rate. Then, when the gas pressure in the pressure sintering apparatus reaches a gauge pressure of 0.1 to 0.6 MPa (1 to 6 atmospheres), the mixture is heat treated at about 400 to 600°C for 1 to 6 hours, and then cooled.
[0063] (Pressure Sintering Step S7) The pressure sintering step S7 is a step in which the polycrystalline grains 11 pressure-heat-treated in the reducing atmosphere pressure heat treatment step S6 are pressure-sintered in an inert atmosphere to produce the thermoelectric conversion material 1 according to the present embodiment. That is, the pressure sintering step S7 is a step in which the thermoelectric conversion material 1 according to the present embodiment is produced by pressure sintering without being exposed to an oxidizing atmosphere (e.g., air) after the reducing atmosphere pressure heat treatment step S6 until the pressure sintering step S7 is completed. Note that "inert" means not oxidizing. Such an inert atmosphere can be suitably realized by evacuating the furnace to 10 Pa or less and replacing the atmosphere with Ar gas three times to remove oxygen from the air.
[0064] In this pressure sintering step S7, it is preferable to replace the reducing atmosphere with an inert atmosphere before performing the pressure sintering. For example, as described above, the reducing atmosphere in the pressure sintering apparatus is evacuated with an inert gas or evacuated to approximately 10 Pa, and then replaced with an inert atmosphere. At this time, it is preferable to operate the pressure sintering apparatus without opening it to the atmosphere. Examples of the inert atmosphere include, but are not limited to, at least one of nitrogen and argon. Note that an argon atmosphere is preferable as the inert atmosphere. Furthermore, when replacing the reducing atmosphere with an inert atmosphere, it is preferable to perform the above-mentioned replacement operation two or more times, and more preferably three or more times. For example, a hot press can be used as the pressure sintering apparatus. Note that in this step, it is also possible to open it to the atmosphere for a short period of time, such as two hours, before evacuation.
[0065] After replacing the atmosphere with an inert atmosphere, the temperature inside the pressure sintering apparatus is increased, for example, at a rate of 300 to 600°C / h, and maintained at 600 to 800°C for 1 hour. At this time, pressure is applied at a rate equivalent to the rate of temperature increase so that the applied pressure at the maintained temperature is, for example, 50 to 70 MPa, specifically, 68 MPa. After the holding period is over, the material is cooled at a cooling rate of 500°C / h or less, and the pressure is reduced. Cooling can be performed by allowing the material to cool naturally within the pressure sintering apparatus. By performing the operations up to this point, the thermoelectric conversion material 1 according to the present embodiment described above can be suitably produced.
[0066] (Post-processing) In post-processing, the manufactured thermoelectric conversion material 1 is removed from the pressure sintering apparatus together with the carbon mold, and the thermoelectric conversion material 1 (sintered body) is removed from the heat-resistant container. In post-processing, debris is removed from the surface of the thermoelectric conversion material 1, and then the thermoelectric conversion material 1 is cut into the desired dimensions and shape using a precision processing machine. These operations can be performed in air. The precision processing machine is preferably a processing method that is resistant to oxidation, such as a diamond blade or wire saw. After that, the Seebeck coefficient S, electrical conductivity σ, specific heat, thermal conductivity κ, etc. are measured.
[0067] The manufacturing method of the thermoelectric conversion material 1 according to the present embodiment described above, which includes the weighing step S1 through the pressure-sintering step S7 as described above, can manufacture a thermoelectric conversion material 1 having oxide crystals (grain boundary precipitates 16) with an atomic ratio of O to Yb exceeding 0.4 and not exceeding 1.5 in the secondary intergranular layers 13 present between the crystal grains 15 in the polycrystalline grains 11 having a skutterudite-type crystal structure containing Yb, Co, and Sb. And / or, the manufacturing method of the thermoelectric conversion material 1 according to the present embodiment, which includes the weighing step S1 through the pressure-sintering step S7 as described above, can manufacture a thermoelectric conversion material 1 having oxide crystals (grain boundary precipitates 16) with an atomic ratio of O to Yb exceeding 0.4 and not exceeding 1.5 in the secondary intergranular layers 13 present between the crystal grains 15 in the polycrystalline grains 11 having a skutterudite-type crystal structure containing Yb, Co, and Sb. 2 and a thermoelectric conversion material 1 having the crystals of Yb. Therefore, the method for producing the thermoelectric conversion material 1 according to this embodiment can produce a thermoelectric conversion material 1 having a higher dimensionless figure of merit ZT and high reliability. Furthermore, the method for producing the thermoelectric conversion material 1 according to this embodiment performs the reducing atmosphere pressure heat treatment step S6 in a reducing atmosphere to produce multiple oxides in which the atomic ratio of O to Yb in the crystals (grain boundary precipitates 16) contained in the intergranular layers 12 and the secondary intergranular layers 13 is greater than 0.4 and less than 1.5. This shortens the overall heat treatment time. Therefore, the method for producing the thermoelectric conversion material 1 according to this embodiment is superior in mass productivity compared to conventional methods. The method for producing the thermoelectric conversion material 1 according to this embodiment may also include the introduction of active materials such as Ba, La, and Sr during the production process.
[0068] Next, the thermoelectric conversion material 1 and the method for producing the thermoelectric conversion material 1 according to the present invention will be described in more detail with reference to examples that exhibit the effects of the present invention and comparative examples that do not.
[0069] (Production of Samples According to Comparative Examples) Sample No. 10 shown in Tables 1 to 3 according to comparative examples was produced by carrying out the following steps S1 to S5 and S7. Sample No. 11 shown in Tables 1 to 3 according to comparative examples was produced by carrying out the following steps S1 to S4 and S7. Sample No. 12 shown in Tables 1 to 3 according to comparative examples was produced by carrying out the following steps S1 to S4, S6 and S7.
[0070] [1] (Weighing step S1, Mixing step S2, Ribbon preparation step S3) Prepare raw materials of Sb, Co, and Yb, and 0.2~0.3 Co 4 Sb 12 The raw materials were weighed in a glove box with an oxygen concentration of 0.1 to 100 ppm or less so that the temperature was within the range of 1080°C. The weighed raw materials were loaded into a graphite crucible, and the raw materials were heated to 1080°C. After being held for 0 to 1 hour, they were placed in water cooled to 20°C or less and cooled. After cooling, the ingot was removed from the crucible and loaded into a graphite crucible for quenching. The ingot was then heated to 1100°C in a high-frequency heating furnace and remelted. The molten metal was dropped onto a copper roll by a liquid rapid solidification method, and a quenched ribbon was produced.
[0071] [2-1] (First heat treatment step S4) The quenched ribbon was loaded into a large graphite crucible in a glove box and heat-treated in an annealing furnace at 700° C. for 3 to 168 hours. The heat-treated quenched ribbon was then removed from the glove box and the oxygen concentration was measured.
[0072] [2-2] (Second Heat Treatment Step S5) Next, to adjust the oxygen concentration in the ribbon, the large graphite crucible containing the ribbon was placed in the annealing furnace again. The ribbon was then heat-treated at 700°C for 3 to 168 hours until the oxygen concentration of the material reached approximately 1200 ppm. The heat-treated raw material was then removed from the glove box and crushed using a mortar and pestle or a Dalton hammer crusher to produce polycrystalline grains 11. The resulting polycrystalline grains 11 were weighed in the glove box, loaded into a carbon mold (carbon die) in a draft chamber, and introduced into a hot press.
[0073] [2-3] (Reducing atmosphere pressure heat treatment step S6) The inside of the hot press was evacuated to 15 Pa and replaced with Ar gas. This process was repeated two or more times, and after the final evacuation, 100% by volume hydrogen was introduced as a reducing atmosphere gas. Then, after the gas pressure inside the hot press reached 0.3 MPa (3 atmospheres) in gauge pressure, heat treatment was performed at 400°C for 1 hour, as shown in Table 1. No pressing pressure (pressurizing pressure) was applied during this process.
[0074] [3] (Pressure sintering step S7) After cooling, the hot press was again evacuated to 15 Pa or less without being exposed to the atmosphere, and Ar gas was introduced (gauge pressure: 0 MPa (in this case, no numerical value indicating pressure is shown in Table 1)). The temperature was increased at a rate of 300°C / h in the hot press, and the temperature was held at 750°C for 1 hour. At this time, pressure was applied at a rate equivalent to the temperature increase rate so that the press pressure (pressure pressure) at the kept temperature became 68 MPa. After the holding period was over, the material was cooled at a rate of about 500°C / h, and the pressure was reduced.
[0075] [4] (Post-treatment) The carbon mold was removed from the hot press, and the sintered body was taken out in air. After removing debris from the surface of the sintered body, a rectangular parallelepiped measuring 3 mm square x 10 mm long was cut out using a precision processing machine with a diamond blade, and the Seebeck coefficient S and electrical conductivity σ were measured. In addition, small pieces measuring 2-3 mm square x 2 mm thick and square plates measuring 10 mm square x 1 mm thick were cut out from the same sintered body, and the specific heat and thermal diffusivity of each were measured, and the thermal conductivity κ was calculated.
[0076] [5] (Analysis) (Measurement of Oxygen Concentration) The oxygen concentration of the sintered body was measured using a fusion oxygen concentration analyzer (EMGA-920 manufactured by HORIBA).
[0077] (Analysis of Composition) The composition was analyzed using an ICP inductively coupled plasma analyzer (Shimadzu Corporation, ICPS-8100).
[0078] (Identification of texture and crystalline structure) A scanning electron microscope (SEM) (JEOL JSM-7900F), a transmission electron microscope (TEM) (JEOL JEM-ARM200F), and an X-ray diffractometer (Rigaku Smart Lab) were used in combination to identify the texture and crystalline structure. Measurements with the SEM and TEM were performed by observing a range including the intergranular layer 12 and measuring between any two points where the distance between adjacent polycrystalline grains 11 was the shortest.
[0079] (Textural Analysis) The texture was analyzed using an electron probe microanalyzer (EPMA1610 manufactured by Shimadzu Corporation). The measurement conditions for the electron probe microanalyzer were an acceleration voltage of 15 kV, a current of 100 nA, and a beam diameter of 10 μm, and the average value of five points was calculated.
[0080] (Observation of Phase Map) The structure was observed by electron backscatter diffraction (Aztec HKL Symmetry, manufactured by OIKK Co., Ltd.) Observation was carried out on the structure, phase map, and diffraction plane map.
[0081] (Performance of Thermoelectric Conversion Material 1) The Seebeck coefficient S and electrical conductivity σ were measured using a ZEM-3 manufactured by Advance Riko Co., Ltd. The measurement conditions for the Seebeck coefficient S and electrical conductivity σ were the standard measurement conditions recommended by the device manufacturer. A sample was processed into a shape with two end faces, and the Seebeck coefficient S was measured by heating the end faces of the sample with a differential heater to create a temperature difference between both ends of the sample, and measuring the temperature difference and electromotive force between probe thermocouples pressed against the side of the sample. Electrical resistance was measured using the DC four-terminal method. The thermal conductivity κ was calculated from the specific heat, thermal diffusivity, and density. The specific heat was measured using a power compensation differential scanning calorimeter, Pyris1 manufactured by Perkin-Elmer, the thermal diffusivity was measured using an LFA467 manufactured by NETZSCH, which performs the laser flash method, and the density was measured using the Archimedes method. The dimensionless figure of merit ZT was calculated from the measured Seebeck coefficient S, thermal conductivity κ, and electrical conductivity σ using the above-mentioned formula (1).
[0082] (Production of Samples According to the Examples) Samples No. 1 to 9 in Tables 1 to 3 according to the examples were produced in the same manner as in the comparative examples, except that the above [2-1], [2-2], [2-3], and [3] were changed to the following [2A] and [3A]. That is, samples No. 1 to 9 in Tables 1 to 3 according to the examples were produced by performing all steps from the weighing step S1 to the pressure sintering step S7.
[0083] [2A] (First Heat Treatment Step S4, Second Heat Treatment Step S5) The quenched ribbon was reloaded into a graphite crucible in a glove box and placed directly in an annealing furnace (without being vacuum-sealed in an ampoule). To reduce the oxygen concentration in the graphite crucible, a deep lid (12 cm deep) was used. The quenched ribbon reloaded into the graphite crucible was heat-treated at 700°C for 24 hours in the first heat treatment step S4 with an argon flow rate of 0.1 to 10 liters / minute, until the oxygen concentration of the material reached approximately 1200 ppm. The quenched ribbon that had undergone the first heat treatment was then further heat-treated at 700°C for 24 hours with an argon flow rate of 1 to 5 liters / minute, until the oxygen concentration of the material reached approximately 1200 ppm. The mixture was then removed from the glove box and pulverized at 1000 rpm using a hammer mill with the atmospheric oxygen concentration adjusted to 0.1 to 20 ppm to produce pulverized powder (polycrystalline particles 11) with a d50 of 10 to 100 μm and an oxygen concentration of approximately 1000 ppm. The resulting polycrystalline particles 11 were weighed in the glove box, loaded into a carbon mold in a draft, and introduced into a hot press machine.
[0084] [3A] (Reducing Atmosphere Pressure Heat Treatment Step S6, Pressure Sintering Step S7) The hot press was evacuated to 10 Pa and replaced with Ar gas. This process was repeated two or more times, and after the final evacuation, 100% by volume hydrogen was introduced as a reducing atmosphere gas. Then, as shown in Table 1, after the gas pressure inside the hot press reached 0.1 to 0.6 MPa (1 to 6 atmospheres) in gauge pressure, the samples were heat-treated at 400 to 600°C for 1 to 6 hours. No pressing pressure (pressure) was applied during this process. After cooling, the hot press was again evacuated to 10 Pa or less without being exposed to the atmosphere, and Ar gas was introduced (gauge pressure of 0 MPa (in this case, no numerical value indicating pressure is shown in Table 1)). When this Ar gas was introduced, a gauge pressure of 0.1 MPa to 0.6 MPa was applied depending on the sample. After the replacement with Ar gas was completed, the temperature was again increased at a rate of 300 to 600°C / h and held at 750°C for 1 hour as shown in Table 1. At this time, pressure was applied at a rate equivalent to the temperature increase rate so that the press pressure (applied pressure) reached 68 MPa at the kept temperature of 750°C. After the holding period was over, the material was cooled at about 500°C / h and decompressed.
[0085] Then, steps (4) and (5) were carried out in the same manner as in the comparative example.
[0086] The dimensionless figure of merit (ZT) of the produced materials is shown in Figures 7, 8, 9, and Tables 2 and 3. Each figure shows the hydrogen treatment temperature and / or hydrogen pressure used in the reducing-atmosphere pressure heat treatment step S6. Figure 7 is a graph showing the temperature dependence of the dimensionless figure of merit (ZT) for samples (Nos. 1 to 3 (all examples)) obtained by pressure-sintering raw material powders that had been hydrogen-treated in 100% hydrogen, at a pressure of 0.2 MPa, and at temperatures ranging from 300 to 500°C in the reducing-atmosphere pressure heat treatment step S6. It also shows the temperature dependence of the dimensionless figure of merit (ZT) for the standard material and samples (Nos. 11 and 10 (all comparative examples)) obtained by pressure-sintering raw material powders that had been heat-treated without hydrogen treatment. In the figures, examples are represented by ◇, □, and △, and comparative examples are represented by ■ and ●. FIG. 8 is a graph showing the measured temperature dependence of the dimensionless figure of merit (ZT) for samples (Nos. 4, 2, and 5 (all examples)) obtained by pressure sintering raw material powders that had been hydrogen-treated in the reducing atmosphere pressure heat treatment step S6 at 100% hydrogen, a treatment temperature of 400°C, and a pressure of 0.1 to 0.3 MPa, and for the standard material and samples (Nos. 11 and 10 (comparative examples)) obtained by pressure sintering raw material powders that had been heat-treated without hydrogen treatment. In the figure, examples are represented by ◇, □, and △, and comparative examples are represented by ■ and ●. FIG. 9 is a graph showing the temperature dependence of the dimensionless figure of merit (ZT) for samples (Nos. 8, 7, 6, and 9 (all examples)) obtained by pressure sintering raw material powders that had been hydrogen-treated in 100% hydrogen, at a treatment temperature of 400°C or 500°C, and at a pressure of 0.3 to 0.6 MPa in the reducing atmosphere pressure heat treatment step S6, as well as the temperature dependence of the dimensionless figure of merit (ZT) for samples (Nos. 11 and 10 (comparative examples)) obtained by pressure sintering a standard material and raw material powders that had been heat-treated without hydrogen treatment. In the figure, examples are represented by ◆, ▲, ◯, and ×, and comparative examples are represented by ■ and ●.
[0087]
[0088]
[0089]
[0090] Note that the "-" in Table 1 indicates that the reducing-atmosphere pressure heat treatment step S6 was not performed and therefore not set. As shown in Figures 7 to 9 and Nos. 10 to 12 in Table 3, the comparative samples, i.e., the standard material (No. 11), the material without hydrogen treatment (No. 10), and the material without the second heat treatment step S5 (No. 12 (not shown in Figures 7 to 9)), did not exhibit the effects of the reducing-atmosphere pressure heat treatment step S6, and the dimensionless figure of merit ZT at 773 K (500 °C) was less than 1.1, resulting in unsatisfactory results. Note that the dimensionless figure of merit ZT of the material without hydrogen treatment (No. 10) was lower than that of the standard material (No. 11) because the total amount of Yb oxide introduced in the first heat treatment step S4 and the second heat treatment step S5 was greater than that of the conventional hydrogen gas pressure heat treatment material, resulting in a lower electrical conductivity σ.
[0091] In contrast, the samples according to the examples, which were subjected to hydrogen treatment at temperatures of 300°C, 400°C, and 500°C and hydrogen pressures of 0.1 MPa, 0.2 MPa, and 0.3 MPa, exhibited the effects of performing the reducing atmosphere pressure heat treatment step S6. Therefore, as shown in Figures 7 and 8 and Nos. 1 to 5 and 8 in Tables 2 and 3, these samples had a dimensionless figure of merit ZT of 1.1 or more at 773 K, which was a good result. Among these, sample No. 5 had a dimensionless figure of merit ZT of 1.3 or more at 673 K and a dimensionless figure of merit ZT of 1.5 or more at 773 K, which was particularly good.
[0092] FIG. 10 is a graph showing the temperature dependence of the lattice thermal conductivity for samples (Nos. 1 to 3 (all examples)) obtained by pressure sintering raw material powders that had been hydrogen-treated in a reducing atmosphere at 100% hydrogen, at temperatures between 300°C and 500°C, and at a pressure of 0.2 MPa in the reducing atmosphere pressure heat treatment step S6, as well as the temperature dependence of the lattice thermal conductivity for samples (Nos. 11 and 10 (all comparative examples)) obtained by pressure sintering a standard material and raw material powders that had been treated without hydrogen treatment. In the figure, examples are represented by ◇, □, and △, and comparative examples are represented by ■ and ●. FIG. 11 is a graph showing the temperature dependence of the lattice thermal conductivity for samples (Nos. 4, 2, and 5 (all examples)) obtained by pressure-sintering raw material powders that had been hydrogen-treated in the reducing-atmosphere pressure heat treatment step S6 under conditions of 100% hydrogen, a treatment temperature of 400°C, and a pressure of 0.1 to 0.3 MPa. It also shows the temperature dependence of the lattice thermal conductivity for samples (Nos. 11 and 10 (comparative examples)) obtained by pressure-sintering a standard material and raw material powders that had been hydrogen-treated without hydrogen treatment. In the figure, examples are represented by ◇, □, and △, and comparative examples are represented by ■ and ●. The effects of the reducing-atmosphere pressure heat treatment step S6 were observed in the samples of the examples, which were hydrogen-treated at temperatures of 300°C, 400°C, and 500°C and under hydrogen pressures of 0.1 MPa, 0.2 MPa, and 0.3 MPa. Therefore, these samples are the same as the samples Nos. 11 and 10 in FIGS. 10 and 11 and Tables 2 and 3. As shown in Figures 1 to 5 and 8, as the temperature increased, the lattice thermal conductivity decreased compared to the standard material (comparison example) and the material not subjected to hydrogen treatment, which was a contribution of the thermal conductivity reduction effect.
[0093] The effects of performing the reducing-atmosphere pressure heat treatment step S6 were also observed in the samples of the example, which were subjected to hydrogen treatment at temperatures of 400°C and 500°C and hydrogen pressures of 0.3 to 0.6 MPa. Therefore, as shown in Figure 9 and Nos. 6, 7, and 9 in Tables 2 and 3, these samples had particularly good results, with a dimensionless figure of merit ZT of 1.3 or more at 773 K. This confirmed that the performance of the material can be improved by performing the first heat treatment step S4, the second heat treatment step S5, the reducing-atmosphere pressure heat treatment step S6, and the pressure sintering step S7.
[0094] Figure 12A is an SEM image of Sample No. 5 (Example), which was subjected to the pressure sintering process S7 on raw material powder subjected to the pressure heat treatment process S6 in a reducing atmosphere at 400°C, 100% hydrogen, and a pressure of 0.3 MPa. Intergranular layers 12 precipitated at the ribbon grain boundaries are visible, but due to the pressure sintering process S7, small amounts of Yb oxide of 2 μm or less have seeped into the polycrystalline grains 11. Figure 12B is an EBSD (electron backscatter diffraction) phase image of the xiib portion shown in Figure 12A. The white imaged areas in Figure 12A indicate the presence of a heavy element, i.e., Yb, in high concentrations. Figure 12B shows the chemical form (phase) of the Yb present. As shown in Figure 12B, the intergranular layers 12 can be confirmed. Figure 12C is a diagram showing the types of phases identified in Figure 12B. The phases identified in Figures 12B and 12C are the main phase and CoSb. 2 12B and 12C, after the first heat treatment step S4, the second heat treatment step S5, and the reducing atmosphere pressure heat treatment step S6, the pressure sintering step S7 was performed to obtain a mixture of multiple types of Yb oxides and CoSb. 2 It was possible to precipitate Yb and reduce the thermal conductivity κ. 2 O 3 The fact that the precipitates are of multiple types is the reason why the thermal conductivity κ can be further reduced.
[0095] 13A to 13D are STEM dark field images of part xiii in FIG. 1C, which schematically illustrates the structure of the thermoelectric conversion material 1 according to the example. Note that FIG. 13A shows the sample (No. 5) subjected to the reducing atmosphere pressure heat treatment step S6 under conditions of a hydrogen treatment temperature of 400°C and a hydrogen pressure of 0.3 MPa. As shown in FIG. 13A, the thermoelectric conversion material 1 according to the example is composed of a main phase (crystal 19) and a CoSb phase formed as a result of Yb seeping out. 2 13A shows the CoSb phase (crystal 20) due to Yb permeating into the secondary intergranular layer 13. 2 is generated, and the CoSb 2 This confirms the existence of the phase.
[0096] Figures 13B, 13C, 13D, and 13E show enlarged views of the secondary intergranular layer 13, showing the analysis positions of the STEM dark field image / EDX. Specifically, Figures 13B, 13C, 13D, and 13E are analysis results of positions b, c, d, and e in Figure 13A, respectively. Precipitates 21 to 33 are shown in Figures 13B, 13C, 13D, and 13E. The analytical values for these crystals 19 and 20 and precipitates 21 to 33 are shown in Table 4. Note that blank cells in Table 4 indicate that the precipitates were not detected in the above analysis.
[0097]
[0098] As shown in Table 4, crystals 19 and 20 and precipitates 21 to 33 shown in FIGS. 13A to 13E contain Yb 0.15 CoSb 3 , CoSb 2 , YbO+CoSb 3 , YbO+CoSb 2 , Yb 2 O 3 +CoSb 3 , YbO+CoSb 6 , Yb 2 O 3 +CoSb 6 , Yb 2 O 3 Various precipitates, such as Yb + CoSb, were identified and quantified. 2 O 3 and YbO (for example, Yb 2 O 3 + CoSb and Yb 2 O 3 +CoSb 3 or YbO+CoSb 3 and YbO + CoSb 2 ). As shown in Table 4, the ratio of Yb to O was not constant but varied. This means that defects such as oxygen vacancies and interstitial atoms cause the Yb oxide to deviate from the stoichiometric composition. Furthermore, as shown in Figure 13D, it was found that the precipitates do not precipitate in the secondary intergranular layer 13 that is continuous with the grain boundaries, but rather that the secondary intergranular layer 13 precipitates partially and precipitates precipitate in that region.
[0099] As can be seen from the results in Table 4, by performing predetermined heat treatments (first heat treatment step S4, second heat treatment step S5, and reducing atmosphere pressure heat treatment step S6) before the pressure sintering step S7, the atomic ratio of O to Yb in the oxide containing Yb can be set to a predetermined range of more than 0.4 and 1.5 or less. 2 and CoSb can be precipitated.
[0100] The thermoelectric conversion material 1 and the method for manufacturing the thermoelectric conversion material 1 according to the present invention have been described in detail above through embodiments and examples. However, the present invention is not limited to the above-described embodiments and examples, and various modifications are included.
[0101] REFERENCE SIGNS LIST 1 thermoelectric conversion material 2 thermoelectric conversion material (reverse phase) 3 conductive material 3a first conductive material 3b second conductive material 4 element 5 lower substrate 6 upper substrate 7, 8 wiring 10 thermoelectric conversion module 11 polycrystalline grain 12 intergranular layer 13 secondary intergranular layer 14 ribbon grain boundary 15 crystal grain 16 grain boundary precipitate 17 crystal grain boundary precipitate 18 polycrystalline grain boundary 19, 20 crystal 21-33 precipitate b-e position S1 weighing step S2 mixing step S3 ribbon production step S4 first heat treatment step S5 second heat treatment step S6 reducing atmosphere pressure heat treatment step S7 pressure sintering step
Claims
1. A thermoelectric conversion material characterized in that the secondary intergranular layers present between crystal grains in a polycrystalline grain having a skutterudite-type crystal structure containing Yb, Co, and Sb have oxide crystals in which the atomic ratio of O to Yb is greater than 0.4 and not greater than 1.
5.
2. A polycrystalline grain having a skutterudite-type crystal structure containing Yb, Co, and Sb, and a secondary intergranular layer existing between crystal grains in the polycrystalline grain having a skutterudite-type crystal structure containing Yb, Co, and Sb. 2 A thermoelectric conversion material comprising:
3. The crystal structure has the composition formula Yb x Co 4 Sb 12 3. The thermoelectric conversion material according to claim 1, wherein x is greater than 0 and is not greater than 0.
3.
4. The crystal grains in the polycrystalline grains having the above crystal structure are CoSb 2 The thermoelectric conversion material according to claim 1 or 2, comprising:
5. A thermoelectric conversion material according to claim 1 or 2, characterized in that the atomic ratio of O to Yb is greater than 0.4 and not more than 1.5 is also present between polycrystalline grains of a structure having crystals formed in secondary intergranular layers present between crystal grains within the polycrystalline grains having the crystal structure.
6. A thermoelectric conversion material according to claim 1 or 2, characterized in that the oxygen concentration is 1,200 pm by mass or less.
7. A thermoelectric conversion material according to claim 1 or 2, characterized in that the thickness of the secondary intergranular layer is 5 nm or more and 1 μm or less.
8. A thermoelectric conversion material according to claim 1 or 2, characterized in that at least one of the thermal conductivity and the electrical conductivity is anisotropic.
9. A method for producing a thermoelectric conversion material, comprising: a weighing step of weighing each of a raw material containing Yb, a raw material containing Co, and a raw material containing Sb; a mixing step of melting and mixing the raw materials; a ribbon production step of rapidly solidifying the molten raw materials by a liquid rapid solidification method to produce a ribbon; a step of heat treating the produced ribbon in an inert atmosphere having an adjusted oxygen concentration; and a grinding step, the method comprising: a first heat treatment step of obtaining polycrystalline grains; a second heat treatment step of heat treating the polycrystalline grains again in an inert atmosphere having an adjusted oxygen concentration in order to adjust the oxygen concentration in the polycrystalline grains heat treated in the first heat treatment step; a reducing atmosphere pressure heat treatment step of pressure heat treating the polycrystalline grains heat treated in the second heat treatment step in a reducing atmosphere; and a pressure sintering step of pressure sintering the polycrystalline grains pressure heat treated in the reducing atmosphere pressure heat treatment step in an inert atmosphere to produce a thermoelectric conversion material.
10. The method for producing a thermoelectric conversion material according to claim 9, characterized in that in the pressure sintering step, the reducing atmosphere is replaced with an inert atmosphere before pressure sintering.
11. The method for producing a thermoelectric conversion material according to claim 9 or 10, characterized in that the heat treatment temperature in the pressure sintering step is 600°C or higher and 800°C or lower.
Citation Information
Patent Citations
Thermoelectric conversion material, method for sintering thermoelectric conversion material, and method for manufacturing thermoelectric conversion material
JP2020057676A
Thermoelectric powder and thermoelectric material prepared using the same
US20180269368A1
Thermoelectric conversion material, thermoelectric conversion module, and method for manufacturing thermoelectric conversion material
WO2019139168A1
Thermoelectric conversion material, thermoelectric conversion module using same, and method of manufacturing thermoelectric conversion material
WO2020067111A1