Stretched film and method for manufacturing same
A polyethylene-based stretched film with specific density and heat shrinkage characteristics addresses the recyclability and heat resistance challenges in conventional laminates, offering improved heat resistance and transparency.
Patent Information
- Application Number
- PCT/JP2024/006925
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-30
- Filing Date
- 2024-02-27
- Publication Date
- 2024-10-03
AI Technical Summary
Conventional laminated packaging films with different resin materials face challenges in recyclability due to material separation difficulties and high heat shrinkage rates, leading to wrinkles and poor appearance during heat sealing.
A stretched film with a polyethylene main component, having a density of 0.950 g/cm³ and a heat shrinkage rate of 3% or less at 120°C, produced by stretching a raw film containing high-density polyethylene with a melting point between 130 to 140°C and ultra-high molecular weight polyethylene, ensuring improved heat resistance and recyclability.
The solution provides a film with excellent heat resistance, high recyclability, and improved transparency, addressing the issues of heat shrinkage and material separation in conventional laminates.
Smart Images

Figure JP2024006925_03102024_PF_FP_ABST
Abstract
Description
Stretched film and method for producing same
[0001] The present invention relates to a stretched film used for packaging films and the like, and a method for producing the same.
[0002] Conventionally, as packaging films used for pouches and the like, a laminate has been used in which, for example, a base film made of a resin material and a sealant film made of a material different from the resin material that makes up the base film are laminated together.
[0003] There is a demand for reducing the environmental impact of plastics in general, and packaging films are also required to be recyclable. However, in the case of laminates in which films made of the above-mentioned different materials are stacked, there is a problem in that it is difficult to separate the materials, making recycling difficult.
[0004] Therefore, in recent years, there has been an active movement toward mono-material packaging films, which are made from a single material. Examples of resins used in mono-material packaging films include polyethylene, polypropylene, and polyethylene terephthalate. Of these, polyethylene is the most widely used material in existing packaging films, and is particularly sought after as a mono-material.
[0005] As a packaging film using this polyethylene, for example, a laminate has been proposed, which includes a base film and a sealant film, both made of polyethylene, and the base film has been subjected to a stretching treatment. It is described that such a configuration can provide a laminate having high recyclability, printability, and strength, and in which the transparency of the base film is improved (see, for example, Patent Document 1).
[0006] JP 2019-171860 A
[0007] Here, various functions are required for packaging films, but it is known that stretching the film causes thermal shrinkage. The packaging film described in Patent Document 1 has a density of 0.950 g / cm 3Because the main component is polyethylene of less than 100%, the heat shrinkage rate is large, and there was a problem that the base film shrinks during the heat sealing performed during bag production, causing wrinkles and poor appearance.
[0008] The present invention has been made in view of the above problems, and has an object to provide a stretched film having excellent heat resistance.
[0009] In order to achieve the above object, the stretched film of the present invention has a density of 0.950 g / cm 3 A stretched film containing polyethylene as a main component, and having a density of 0.950 g / cm3 or more relative to the entire stretched film 3 The polyethylene content is more than 50% by mass, and the heat shrinkage rate when heated at 120°C for 10 minutes in the stretching direction of the film is 3% or less.
[0010] In addition, the method for producing a stretched film of the present invention is also advantageous in that the density is 0.950 g / cm 3 A method for producing a stretched film, comprising at least the steps of preparing a raw film containing the above polyethylene as a main component and stretching the raw film, wherein the raw film has a density of 0.950 g / cm3 as a whole. 3 The polyethylene content is more than 50% by mass, and the stretching temperature in the stretching treatment is 125°C or higher and lower than 130°C.
[0011] According to the present invention, it is possible to provide a stretched film having excellent heat resistance.
[0012] 1 is a cross-sectional view illustrating a laminate using a stretched film of the present invention, and FIG. 2 is a plan view illustrating a laminate using a stretched film of the present invention.
[0013] The stretched film of the present invention will be specifically described below. Note that the present invention is not limited to the following embodiments, and can be appropriately modified and applied within the scope of the present invention.
[0014] FIG. 1 is a cross-sectional view showing a laminate using the stretched film of the present invention.
[0015] The laminate 1 includes a polyethylene film (stretched film) 3 that serves as a base film, and a sealant film 2 laminated on the polyethylene film 3 .
[0016] <Sealant Film> From the viewpoint of mono-material, the sealant film 2 of the present invention is preferably a polyethylene-based resin. More specifically, examples thereof include high-density polyethylene (HDPE), medium-density polyethylene (MDPE), low-density polyethylene (LDPE), and linear low-density polyethylene (LLDPE).
[0017] From the viewpoint of improving heat sealability, it is preferable to use low density polyethylene (LDPE) or linear low density polyethylene (LLDPE) having a melting point lower than that of the base film in order to provide a difference in melting point with respect to the base film.
[0018] The polyethylene content in the sealant film 2 is preferably 70% or more, more preferably 90% or more, even more preferably 95% or more, and most preferably 100%.
[0019] The thickness of the sealant film 2 is preferably 20 μm to 200 μm, and more preferably 30 μm to 150 μm.
[0020] Furthermore, the sealant film 2 may contain components other than the polyethylene resin described above, as long as the properties of the sealant film 2 are not impaired.
[0021] Other components include olefin resins, amide antiblocking agents (such as stearic acid amide), plasticizers, ultraviolet absorbers, antioxidants, weather stabilizers, antistatic agents, colorants, antifogging agents, metal soaps, waxes, mildew inhibitors, antibacterial agents, nucleating agents, flame retardants, and lubricants.
[0022] <Polyethylene Film> The polyethylene film 3 of the present invention is composed mainly of high density polyethylene (HDPE). In the present invention, the density of the high density polyethylene is 0.950 g / cm 3 This is because the density is 0.950 g / cm3 If the melting point of polyethylene is less than 1000 kJ / cm, the melting point of polyethylene will be low, resulting in an increase in the heat shrinkage rate, a decrease in heat resistance, and a decrease in film strength.
[0023] The density of high-density polyethylene is 0.970 g / cm 3 This is preferably less than 0.970 g / cm 3 In the above cases, the film becomes hard and easily torn, which may make it difficult to produce a stretched film.
[0024] The melting point of the high-density polyethylene is preferably in the range of 130 to 140° C., more preferably 132 to 140° C. If the melting point is less than 130° C., stretching at a temperature equal to or higher than the stretching temperature (125° C.) described below may not be possible, and the heat resistance of the stretched film may decrease.
[0025] The "melting point" mentioned above is measured in accordance with JIS K 7121:1987, and is determined by measuring the temperature at which the main endothermic peak appears using a differential scanning calorimeter (DSC).
[0026] The melt mass flow rate (MFR) of the high-density polyethylene is preferably 0.01 to 3.00 g / 10 min, more preferably 0.02 to 2.50 g / 10 min, and even more preferably 0.1 to 2.00 g / 10 min. This is because a melt mass flow rate (MFR) of 0.01 g / 10 min or more allows molding using a general-purpose extruder without using special equipment, and a melt mass flow rate (MFR) of 3.00 g / 10 min or less allows sufficient film strength to be imparted.
[0027] The melt mass flow rate can be obtained by measuring in accordance with the provisions of JIS K7210:1999.
[0028] From the viewpoint of further improving heat resistance, the content of high-density polyethylene in the entire polyethylene film is more than 50% by mass, preferably 70% by mass or more, based on 100% by mass of the polyethylene film.
[0029] The polyethylene film 3 of the present invention may contain ultra-high molecular weight polyethylene (UHMWPE) in addition to the high-density polyethylene that is the main component. By using a mixture of high-density polyethylene that is the main component and ultra-high-molecular-weight polyethylene as the polyethylene that constitutes the polyethylene film 3, it becomes possible to perform stretching at a higher temperature without causing melting of the film, thereby further improving heat resistance.
[0030] The ultra-high molecular weight polyethylene is a solid powder, and one having a viscosity-average molecular weight (Mv) of 500,000 to 3,000,000 can be used. This is because if the viscosity-average molecular weight (Mv) is less than 500,000, the melt tension will be small, and the effect obtained by mixing the ultra-high molecular weight polyethylene (i.e., the effect of being able to perform stretching at a higher temperature without causing film melting) may be reduced. On the other hand, if the viscosity-average molecular weight (Mv) is greater than 3,000,000, the ultra-high molecular weight polyethylene may not melt and may not mix with the high-density polyethylene (resulting in gelation during kneading and molding).
[0031] As the ultra-high molecular weight polyethylene, for example, a commercially available product such as Hi-Zex Million 030S (manufactured by Mitsui Chemicals, Inc., viscosity average molecular weight: 500,000) can be used.
[0032] Furthermore, cross-linked polyethylene cross-linked by a cross-linking agent or electron beam irradiation, or a polymerized polyethylene (synthesized polyethylene) having a viscosity average molecular weight of 500,000 to 3,000,000 may also be used.
[0033] The "viscosity average molecular weight" is calculated in accordance with JIS K 7367-3:1999.
[0034] The ultra-high molecular weight polyethylene preferably has a melting point in the range of 130 to 140°C after recrystallization, more preferably 132 to 140°C.
[0035] Furthermore, when ultra-high molecular weight polyethylene is used, the content of the ultra-high molecular weight polyethylene relative to the total mass of the polyethylene film is preferably more than 0 mass% and not more than 30 mass% based on 100 mass% of the polyethylene film, because if the content of the ultra-high molecular weight polyethylene is more than 30 mass%, the transparency of the film may decrease.
[0036] Furthermore, the content of polyethylene (i.e., high-density polyethylene and ultra-high molecular weight polyethylene) in the entire polyethylene film is preferably 90% by mass or more, and more preferably 95% by mass or more, based on 100% by mass of the polyethylene film. When the polyethylene content is more than 90% by mass, the entire laminate 1 can be considered to be a single material made of polyethylene, thereby improving recyclability.
[0037] <Other Components> The polyethylene film may contain components other than the high-density polyethylene and ultra-high-molecular-weight polyethylene described above, as long as the heat resistance of the polyethylene film is not impaired.
[0038] Other components include olefin resins, amide antiblocking agents (such as stearic acid amide), plasticizers, ultraviolet absorbers, antioxidants, weather stabilizers, antistatic agents, colorants, antifogging agents, metal soaps, waxes, mildew inhibitors, antibacterial agents, nucleating agents, flame retardants, and lubricants.
[0039] <Method for Producing Laminate> Next, an example of a method for producing a laminate using the stretched film of the present invention will be described in detail.
[0040] First, the raw material containing the above-mentioned high-density polyethylene is formed into a film using an extruder to produce a polyethylene film.
[0041] More specifically, high-density polyethylene and, if necessary, other components such as the above-mentioned ultra-high molecular weight polyethylene are mixed in a predetermined blending ratio, and the mixture is melt-extruded in an extruder equipped with a T-die to form a film, thereby obtaining a raw film before stretching.
[0042] As with the content of the polyethylene film as a whole described above, the content of high-density polyethylene in the entire raw film is more than 50 mass% out of 100 mass% of the raw film, and the content of ultra-high molecular weight polyethylene in the entire raw film is more than 0 mass% and not more than 30 mass% out of 100 mass% of the raw film.
[0043] The raw film is then subjected to uniaxial stretching to produce a stretched film that will become the polyethylene film 3 shown in Figures 1 and 2. The stretching method is not particularly limited, and examples thereof include roll stretching and tenter stretching.
[0044] The uniaxial stretching treatment described above refers to a stretching treatment performed in either the machine axis (longitudinal) direction of the film (hereinafter referred to as "MD") or the direction perpendicular to the MD (hereinafter referred to as "TD") as shown in Figure 2. Note that a biaxial stretching treatment in which stretching treatment is performed in both the MD and TD directions may also be performed.
[0045] When the polyethylene film 3 is composed of only high-density polyethylene, the stretching temperature in the uniaxial stretching treatment is 125° C. or higher and lower than 129° C., and preferably 127° C. or higher and lower than 129° C. This is because a stretching temperature lower than 125° C. may increase the heat shrinkage rate and reduce heat resistance, while a stretching temperature of 129° C. or higher may cause the film to melt and break.
[0046] That is, if the stretching temperature is within the above range, the effect of heat setting is increased, so that the heat shrinkage rate at high temperatures (120° C.) is reduced, and heat resistance can be improved.
[0047] Furthermore, when the polyethylene film 3 is composed of high-density polyethylene and ultra-high-molecular-weight polyethylene, the temperature is 125° C. or higher and lower than 130° C., and preferably 127° C. or higher and lower than 130° C. By mixing ultra-high-molecular-weight polyethylene with high-density polyethylene, it becomes possible to perform stretching at a higher temperature without causing melting of the film, and the heat resistance can be further improved.
[0048] The stretching ratio in the uniaxial stretching treatment is 4 times or more and 10 times or less. This is because if the stretching ratio is less than 4 times, unstretched portions will remain, which may result in a decrease in transparency. If the stretching ratio is more than 10 times, the film may break. From the viewpoint of improving transparency and preventing film breakage, the stretching ratio is preferably 5 times or more and 8 times or less.
[0049] The polyethylene film produced by the above-mentioned stretching treatment has a density of 0.950 g / cm 3 The film is mainly composed of the above-mentioned high-density polyethylene, and because the melting point of the high-density polyethylene is high, it is possible to suppress an increase in the heat shrinkage rate. When heated at 120°C for 10 minutes in the stretching direction of the film, the heat shrinkage rate is 3% or less, which improves dimensional stability during heat treatment and makes it possible to obtain excellent heat resistance.
[0050] From the viewpoint of improving heat resistance, the heat shrinkage rate of the polyethylene film is preferably 2% or less, and more preferably 1% or less.
[0051] The above-mentioned "thermal shrinkage rate" can be determined by the method described in the examples below.
[0052] Furthermore, the polyethylene film of the present invention has a haze of 20% or less, making it possible to obtain excellent transparency.
[0053] From the viewpoint of further improving transparency, the haze of the polyethylene film is preferably 10% or less, more preferably 7% or less, and even more preferably 5% or less.
[0054] The term "haze" used herein refers to an index of cloudiness measured in accordance with JIS K 7361.
[0055] The polyethylene film of the present invention preferably has a tensile breaking stress of 100 MPa or more in at least one of the MD and TD directions. A tensile breaking stress of 100 MPa or more improves transparency and provides a polyethylene film having sufficient strength as a base film.
[0056] From the viewpoint of further improving transparency, the tensile breaking stress of the polyethylene film is preferably 200 MPa or more.
[0057] The "tensile breaking stress" refers to the stress measured in accordance with JIS K 7127.
[0058] The thickness of the raw film before stretching is preferably 100 μm or more and 300 μm or less, more preferably 100 μm or more and 250 μm or less. If the thickness of the raw film is 100 μm or more, it can obtain strength that can withstand the stress during stretching. If the thickness of the raw film is 300 μm or less, it can obtain sufficient transparency after stretching.
[0059] The thickness of the polyethylene film after stretching is preferably 10 μm or more and 50 μm or less, and more preferably 20 μm or more and 40 μm or less. If the thickness of the polyethylene film after stretching is 10 μm or more, sufficient strength as a base film can be obtained. If the thickness of the polyethylene film after stretching is 50 μm or less, sufficient transparency can be obtained.
[0060] According to the above method, in the present invention, it is possible to obtain a polyethylene film having excellent heat resistance, strength and transparency.
[0061] The polyethylene film serving as the base film may be a single layer or a multi-layer film consisting of two or more layers. When the polyethylene film is a multi-layer film, the compositions and thicknesses of the layers may be the same or different. When the polyethylene film is a multi-layer film, the thickness refers to the total thickness of the multi-layer film.
[0062] Next, a raw material containing a polyethylene resin such as the above-mentioned high density polyethylene (HDPE), medium density polyethylene (MDPE), low density polyethylene (LDPE), and linear low density polyethylene (LLDPE) is prepared, and the raw material is molded into a film using an extruder in the same manner as the above-mentioned polyethylene film, thereby producing sealant film 2.
[0063] Then, for example, the polyethylene film 3 and the sealant film 2 are laminated together via an adhesive to produce the laminate 1 shown in FIG.
[0064] The present invention will be described below based on examples. However, the present invention is not limited to these examples, and these examples can be modified or changed based on the spirit of the present invention, and such modifications are not excluded from the scope of the present invention.
[0065] The materials used to prepare the stretched film are as follows: (1) HDPE1: High density polyethylene (density: 0.951 g / cm 3 (2) HDPE2: High-density polyethylene (density: 0.958 g / cm 3, melting point: 133.6°C, MFR: 1.0 g / 10 min, manufactured by Tosoh Corporation) 3 , melting point: 133°C, MFR: 0.98g / 10min, manufactured by Prime Polymer Co., Ltd., trade name: Hi-Zex 3600F) (3) HDPE3: high-density polyethylene (density: 0.960g / cm 3 , melting point: 135°C, MFR: 1.0 g / 10 min, manufactured by Japan Polyethylene Co., Ltd., trade name: Novatec HY540) (4) MDPE: medium density polyethylene (density: 0.943 g / cm 3 (5) UHMWPE: ultra-high molecular weight polyethylene (viscosity average molecular weight: 500,000, density: 0.949 g / cm 3, melting point: 126°C, MFR: 0.24 g / 10 min, manufactured by Prime Polymer Co., Ltd., trade name: Hi-Zex 5100E) 3 Melting point after recrystallization: 132.8°C, manufactured by Mitsui Chemicals, Inc., product name: Hi-Zex Million 030S)
[0066] (Example 1) <Preparation of Stretched Film> First, the high-density polyethylene shown in Table 1 was prepared. Next, the prepared high-density polyethylene was formed into a film by melt extrusion (extrusion temperature: 200°C) using an extruder (manufactured by LABTECH) equipped with a T-die, and the film was taken up on a take-up roll to obtain a raw film before stretching having the thickness shown in Table 1.
[0067] Then, this raw film was stretched by uniaxial stretching in the MD under the conditions of the stretching temperature and stretch ratio shown in Table 1, and a stretched film (polyethylene film) formed from high-density polyethylene and having the thickness shown in Table 1 was produced.
[0068] <Calculation of Heat Shrinkage> A sample of a predetermined size (7 cm x 7 cm) was cut from the prepared stretched film, and 5 cm long, perpendicular benchmark lines parallel to each side were drawn 1 cm inward from each side of the sample. The sample was placed in a 120°C oven and heated for 10 minutes, then removed and cooled to room temperature. The distance between the benchmark lines in the stretching direction (i.e., MD) of the heat-treated sample was measured, and the heat shrinkage percentage [%] was calculated from the change in the benchmark line distance in the stretching direction before and after heating using the following formula (1), which was used as an index of heat resistance. The results are shown in Table 1.
[0069] Heat shrinkage rate in the stretching direction [%] = [(gauge line distance before heating - gauge line distance after heating) / gauge line distance before heating] × 100 (1)
[0070] <Measurement of Tensile Breaking Stress> The tensile breaking stress [MPa] of the produced stretched film was measured in accordance with JIS K 7127. More specifically, a rectangular test piece measuring 200 mm in the MD direction and 10 mm in the TD direction was prepared, and a tensile test was performed using a tensile tester (manufactured by Shimadzu Corporation, product name: Autograph AG-5000A) at a temperature of 25°C and a pulling rate of 100 mm / min, and the tensile breaking stress [MPa] in the MD and TD was measured. The results are shown in Table 1.
[0071] <Haze Measurement> Using a spectrophotometer (manufactured by Nippon Denshoku Industries Co., Ltd., trade name: HAZE METER NDH5000), the haze [%] in the visible light region of polyethylene (range of 360 to 750 nm) was measured as an index of the haze of the produced stretched film in accordance with JIS K 7361. The results are shown in Table 1.
[0072] Examples 2 to 7, Comparative Examples 1 to 6 Stretched films were produced by stretching raw films having thicknesses shown in Table 1 in the same manner as in Example 1, except that the composition of the stretched film (i.e., the polyethylene used) and the conditions for the uniaxial stretching treatment were changed to those shown in Table 1.
[0073] Then, the heat shrinkage rate was calculated, the tensile breaking stress was measured, and the haze was measured in the same manner as in Example 1. The results are shown in Tables 1 and 2.
[0074] In Comparative Example 2, the raw film before stretching was composed only of high-density polyethylene, and the stretched film melted because the stretching temperature during film formation in the uniaxial stretching process was 129° C. Therefore, in Comparative Example 2, it was not possible to calculate the heat shrinkage rate, measure the tensile breaking stress, or measure the haze.
[0075] In Comparative Example 4, the raw film before stretching was composed only of medium-density polyethylene, and since polyethylene has a low density (low melting point), the stretched film melted at the stretching temperature (125°C) during film formation in the uniaxial stretching process. Therefore, in Comparative Example 4, it was not possible to calculate the heat shrinkage rate, measure the tensile breaking stress, or measure the haze.
[0076] In Comparative Example 5, the raw film before stretching was composed only of medium-density polyethylene, and since the density of polyethylene is low, the stretched film broke at the stretching ratio (5 times) during film formation in the uniaxial stretching process. Therefore, in Comparative Example 5, it was not possible to calculate the heat shrinkage rate, measure the tensile breaking stress, or measure the haze.
[0077] In Comparative Example 6, the raw film before stretching was composed of high-density polyethylene and ultra-high-molecular-weight polyethylene, and the stretched film melted because the stretching temperature during film formation in the uniaxial stretching process was 130° C. Therefore, in Comparative Example 6, it was not possible to calculate the heat shrinkage rate, measure the tensile breaking stress, or measure the haze.
[0078] (Comparative Example 7) First, two types of polyethylene (the above-mentioned HDPE3 and MDPE) were prepared as shown in Table 3. Next, an extruder (manufactured by LABTECH) equipped with a T-die was used to co-extrude the prepared two types of polyethylene at an extrusion temperature of 200°C to form a three-layer film in which a first base material layer, a second base material layer, and a third base material layer were laminated in this order. The film was then taken up on a take-up roll to obtain a raw film before stretching having the thickness shown in Table 3.
[0079] The raw film was then stretched by uniaxial stretching in the MD under the conditions of the stretching temperature and stretch ratio shown in Table 3, to produce a stretched film (polyethylene film) having a three-layer structure formed from two types of polyethylene and having the thickness shown in Table 3.
[0080] Then, the heat shrinkage rate was calculated, and the tensile breaking stress and haze were measured in the same manner as in Example 1. The results are shown in Table 3.
[0081] (Comparative Example 8) A raw film having a thickness shown in Table 3 was stretched to produce a stretched film in the same manner as in Comparative Example 7 described above, except that the stretching temperature in the uniaxial stretching treatment was changed to the condition shown in Table 3 (125°C).
[0082] In Comparative Example 8, the entire second base layer in the raw film before stretching was made of medium-density polyethylene, which has a low density (low melting point), and therefore the second base layer made of medium-density polyethylene melted at the stretching temperature (125°C) during film formation in the uniaxial stretching process. Therefore, in Comparative Example 8, it was not possible to calculate the heat shrinkage rate, measure the tensile breaking stress, or measure the haze.
[0083]
[0084]
[0085]
[0086] As shown in Table 1, in the stretched films of Examples 1 to 7, the density was 0.950 g / cm 3 The stretched film contains a high-density polyethylene of the above-mentioned value, the content of the high-density polyethylene in the entire stretched film is more than 50 mass%, and the heat shrinkage rate when heated at 120°C for 10 minutes in the stretching direction of the film is 3% or less, so it is clear that the dimensional stability after heat treatment is high and the heat resistance is excellent.
[0087] In particular, the stretched films of Examples 6 and 7 were composed of high-density polyethylene and ultra-high molecular weight polyethylene with a viscosity average molecular weight (Mv) of 500,000, and the content of ultra-high molecular weight polyethylene in the entire stretched film was 30 mass% or less. Therefore, the film could be stretched at a higher temperature (128 to 129°C) without melting, and the heat shrinkage rate was 1% or less, indicating that the films had excellent heat resistance.
[0088] On the other hand, as shown in Table 2, the stretched film of Comparative Example 1 was stretched at a low temperature of 120° C., so that the heat shrinkage rate was large and the heat resistance was poor.
[0089] The stretched film of Comparative Example 3 was made of only medium-density polyethylene and stretched at a low temperature of 120° C., which resulted in a very large heat shrinkage and poor heat resistance. The haze was also greater than 20%, indicating poor transparency.
[0090] Furthermore, as shown in Table 3, in Comparative Example 7, the stretching temperature was as low as 120° C., so the heat shrinkage rate was large and the heat resistance was poor.
[0091] As described above, the present invention is suitable for stretched films used, for example, as packaging films.
[0092] 1 Laminate 2 Sealant film 3 Polyethylene film (stretched film)
Claims
1. Density is 0.950 g / cm 3 A stretched film mainly composed of polyethylene having a density of 0.950 g / cm3 or more, 3 % by mass of a polyethylene having a molecular weight of 100 or more and a thermal shrinkage rate of 3% or less when heated at 120° C. for 10 minutes in the stretching direction of the film.
2. The density is 0.950 g / cm 3 2. The stretched film according to claim 1, characterized in that it consists solely of polyethylene having the above properties.
3. The stretched film according to claim 1, further comprising ultra-high molecular weight polyethylene having a viscosity average molecular weight (Mv) of 500,000 to 3,000,000, wherein the content of the ultra-high molecular weight polyethylene in the entire stretched film is 30 mass% or less.
4. A laminate comprising the stretched film according to any one of claims 1 to 3, and a sealant film laminated on the stretched film.
5. Density is 0.950 g / cm 3 A method for producing a stretched film, comprising at least a step of preparing a raw film mainly composed of polyethylene having a density of 0.950 g / cm or more and a step of stretching the raw film, 3 and the stretching temperature in the stretching treatment is 125° C. or higher and lower than 130° C.
6. The raw film has a density of 0.950 g / cm 3 6. The method for producing a stretched film according to claim 5, characterized in that the film consists of only polyethylene having the above properties.
7. The method for producing a stretched film according to claim 5, characterized in that the raw film further contains ultra-high molecular weight polyethylene having a viscosity average molecular weight (Mv) of 500,000 to 3,000,000, and the content of the ultra-high molecular weight polyethylene in the entire raw film is 30 mass% or less.
Citation Information
Patent Citations
Laminate and packaging material composed of the laminate
JP2019171860A
Production of drawn polyethylene film
JP1987034928A
Drawn polyethylene film
JP1989141936A
Manufacture of polyolefin molding
JP1998180864A
Method for producing stretched film
JP2007269917A
Cited By
BOPE (Biaxially Oriented Polyethylene) film and preparation method thereof
CN119899444A
Polyethylene composition and biaxially stretched polyethylene film
WO2025177915A1
Polyethylene resin composition and film comprising same
WO2026135028A1
Polyethylene resin composition and film comprising same
WO2026135029A1