Metal member, battery, method for manufacturing same, and mold

The described manufacturing method for metal members, with a specific punch and die configuration, addresses the challenge of forming thin-walled safety valves in metal battery cases by reducing the load on both the material and the mold, enhancing efficiency and reducing costs.

WO2024202912A1PCT designated stage expired Publication Date: 2024-10-03NIPPON STEEL CORPORATION
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/007656
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-27
Filing Date
2024-02-29
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Conventional methods for forming thin-walled safety valves in metal battery cases, particularly using steel plates, require high loads that can damage molds and are inefficient due to the need for multiple processing steps, making it difficult to reduce the load on both the material and the mold.

Method used

A manufacturing method involving a punch and die configuration where the punch shoulder and die shoulder have specific geometric relationships, allowing for the formation of thin-walled portions with reduced load requirements, enabling the use of harder materials like steel with lower surface pressure and fewer processing steps.

Benefits of technology

This method allows for the easy formation of thin-walled parts with lower loads, reducing the risk of mold damage and decreasing the number of processing steps, thus improving efficiency and reducing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024007656_03102024_PF_FP_ABST
    Figure JP2024007656_03102024_PF_FP_ABST
Patent Text Reader

Abstract

This method for manufacturing a metal member (20) comprises: a step for preparing a starting material (40); and a step for placing the starting material (40) between a punch (31) including a punch top surface (311), a punch shoulder (312), and a punch side surface (313), and a die (32) including a die flange surface (321), a die shoulder (322), and a die side surface (323), bringing the punch (31) and the die (32) close to one another, and sandwiching and compressing the starting material (40) between the punch shoulder (312) and the die shoulder (322), thereby forming a thin-walled portion (231) in the starting material (40). Parts of the punch shoulder (312) and the die shoulder (322) that form the thin-walled portion (231) in the starting material (40) have an arc shape or a tapered shape in a cross-sectional view, and are configured so as to satisfy Cpd ≤ 1.00, 0.10×Cpd ≤ w1, and w1 < w2.
Need to check novelty before this filing date? Find Prior Art

Description

Metallic member, battery, manufacturing method thereof, and mold

[0001] The present disclosure relates to a metal member, a battery, and a manufacturing method thereof. The present disclosure also relates to a mold, and more particularly to a mold for manufacturing a metal member.

[0002] Conventionally, in sealed batteries, a safety valve is provided in the lid of a metal battery case. The safety valve includes a valve body and an annular portion provided around the valve body. The annular portion includes a thin-walled portion that is thinner and weaker than the other portions of the lid. When the internal pressure of the battery case reaches or exceeds a predetermined pressure, the thin-walled portion can rupture before the other portions. When the thin-walled portion ruptures, the pressure inside the battery case is released, preventing the battery case from bursting.

[0003] Patent Document 1 discloses a method for forming a safety valve by coining (local crushing) a stainless steel sheet. In Patent Document 1, for example, multiple coining processes are performed. In each coining process, a punch and a die each having an annular protrusion are used, and a thin-walled annular portion is formed in the steel sheet by clamping a portion of the steel sheet between the annular protrusions of the punch and the die. The width of the annular protrusions of the punch and the die becomes smaller in later coining processes.

[0004] Patent Document 2 discloses a method for forming a safety valve by shearing a metal plate, such as an aluminum alloy plate, in which a punch and a die partially overlap, and a thin annular portion is formed in the metal plate by compressing a portion of the metal plate at the overlapping portion of the punch and the die.

[0005] JP 2013-151024 A JP 2015-85356 A

[0006] Patent Document 1 describes that because the annular protrusions of the punch and the die are pressed against both sides of the steel sheet, the amount of machining performed by each annular protrusion is reduced, and the machining load on each annular protrusion is also reduced. Patent Document 1 also describes that by forming a thin-walled annular portion through multiple coining processes, the machining load on each annular protrusion can be further reduced. However, in Patent Document 1, because multiple coining processes are performed, the number of steps and costs required to manufacture the metal member that will become the lid of the battery case increase.

[0007] In Patent Document 2, the overlapping portion of the punch and die compresses a portion of the metal plate until it undergoes work hardening. Patent Document 2 also describes that if the overlapping amount between the punch and die is set to a value close to the minimum overlapping amount at which the annular portion does not break, a thin-walled portion of a set thickness can be formed with a light processing load. However, in Patent Document 2, since the flat surfaces of the punch and die overlap, it is difficult for material to flow out of the overlapping portion, making it difficult to sufficiently reduce the load required to form the thin-walled annular portion. In particular, when a steel plate is used as the raw material instead of an aluminum alloy plate in the method described in Patent Document 2, reducing the load may be more difficult.

[0008] An object of the present disclosure is to provide a method for manufacturing a metal member that can form a thin-walled portion more easily and with a lower load on a material made of a metal plate.

[0009] A method for manufacturing a metal member according to the present disclosure includes the steps of: preparing a material made of a metal plate; placing the material between a punch including a punch top surface, a punch shoulder, and punch lateral surfaces; and a die including a die flange surface, a die shoulder, and a die lateral surfaces; bringing the punch and die relatively close to each other; and sandwiching and compressing a portion of the material between the punch shoulder and the die shoulder, thereby forming a thin-walled portion in the material that is thinner than other portions. The punch shoulder is continuous with the outer periphery of the punch top surface. The punch lateral surfaces are connected to the punch top surface via the punch shoulder. The die flange surface has an annular shape. The die shoulder is continuous with the inner periphery of the die flange surface. The die lateral surfaces are connected to the die flange surface via the die shoulder. The punch top surface is located inside the die flange surface when viewed along a direction of relative approach between the punch and die. The punch shoulder faces the die shoulder in the approach direction. The punch lateral surfaces are located outside the die lateral surfaces when viewed along the approach direction. The punch shoulder and die shoulder portions that form the thin-walled portion in the material each have an arc shape or a tapered shape in the cross-sectional view of the punch and die, and are configured to satisfy the following formulas (1), (2), and (3): Cpd≦1.00 (1) 0.10×Cpd≦w1 (2) w1<w2 (3) where Cpd is the distance [mm] from the boundary between the punch shoulder and the punch side surface to the boundary between the die shoulder and the die side surface in the cross-section of the punch and die. w1 is the radius of curvature [mm] of the punch shoulder when the punch shoulder has an arc shape in the cross-section of the punch, and is the length [mm] of the punch shoulder in the direction perpendicular to the approach direction when the punch shoulder has a tapered shape in the cross-section of the punch. w2 is the radius of curvature [mm] of the die shoulder when the die shoulder has an arc shape when viewed in the cross section of the die, or the length [mm] of the die shoulder in the direction perpendicular to the approach direction when the die shoulder has a tapered shape when viewed in the cross section of the die.

[0010] According to the method for manufacturing a metal component according to the present disclosure, a thin-walled portion can be formed more easily and with a lower load on a material made of a metal plate.

[0011] FIG. 1 is a perspective view schematically showing the configuration of a battery according to the first embodiment. FIG. 2 is a cross-sectional view taken along line II-II of FIG. 1. FIG. 3 is a cross-sectional view of a mold used in the manufacturing method of a metal member according to the first embodiment. FIG. 4A is a schematic view illustrating the manufacturing method of a metal member according to the first embodiment. FIG. 4B is a schematic view illustrating the manufacturing method of a metal member according to the first embodiment. FIG. 4C is a schematic view illustrating the manufacturing method of a metal member according to the first embodiment. FIG. 4D is a schematic view illustrating the manufacturing method of a metal member according to the first embodiment. FIG. 4E is a schematic view illustrating the manufacturing method of a metal member according to the first embodiment. FIG. 5 is a cross-sectional view of a mold used in the manufacturing method of a metal member according to the second embodiment. FIG. 6 is a cross-sectional view of a mold according to a modification of the first embodiment. FIG. 7 is a cross-sectional view of a mold according to a modification of the second embodiment. FIG. 8 is a cross-sectional view of a metal member according to a modification of each embodiment. FIG. 9 is a cross-sectional view of a metal member according to another modification of each embodiment.

[0012] For example, aluminum alloy plates are generally used for battery cases of lithium-ion secondary batteries. To improve the space efficiency of a battery, it is conceivable to use a higher-strength steel plate as the battery case material instead of the aluminum alloy plate, thereby making the battery case thinner than conventional battery cases. However, because the specific gravity of steel is greater than that of aluminum alloys, if it is necessary to avoid an increase in the weight of the battery due to the use of steel plates, the battery case must be significantly thinner. More specifically, because the specific gravity of steel is approximately three times that of aluminum alloys, the thickness of a battery case made of steel plates must be approximately one-third or less of the thickness of a battery case made of aluminum alloy plates. Such thinning is required not only for the battery case but also for the lid attached to the battery case.

[0013] Steel plate is a harder material than aluminum alloy plate. When steel plate is subjected to plastic working, it becomes even harder due to work hardening. Therefore, when compressing steel plate in its thickness direction, a larger load is required compared to aluminum alloy plate. However, when a die is brought into contact with the steel plate over a small area and a high load is applied locally from the die to the steel plate, the surface pressure at the contact surface between the die and the steel plate becomes very high. As a result, the surface pressure may exceed the compressive strength of the die, causing damage to the die. In particular, when forming a thin-walled portion of a safety valve in a steel plate, the thickness of the steel plate needs to be compressed to approximately several tens of μm, requiring an excessively large load.

[0014] In view of the above circumstances, the present inventors have investigated a method for forming a thin-walled portion with a low load even when using a hard material such as a steel plate, and as a result, have completed a method for manufacturing a metal member according to an embodiment.

[0015] A method for manufacturing a metal component according to an embodiment includes the steps of: preparing a material made of a metal plate; placing the material between a punch including a punch top surface, a punch shoulder, and punch lateral surfaces; and a die including a die flange surface, a die shoulder, and a die lateral surfaces; bringing the punch and die relatively close to each other; and sandwiching and compressing a portion of the material between the punch shoulder and the die shoulder, thereby forming a thin-walled portion in the material that is thinner than other portions. The punch shoulder is continuous with the outer periphery of the punch top surface. The punch lateral surfaces are connected to the punch top surface via the punch shoulder. The die flange surface has an annular shape. The die shoulder is continuous with the inner periphery of the die flange surface. The die lateral surfaces are connected to the die flange surface via the die shoulder. The punch top surface is located inside the die flange surface when viewed along a direction of relative approach between the punch and die. The punch shoulder faces the die shoulder in the approach direction. The punch lateral surfaces are located outside the die lateral surfaces when viewed along the approach direction. The punch shoulder and die shoulder portions that form the thin-walled portion in the material each have an arc shape or a tapered shape in a cross-sectional view of the punch and die, and are configured to satisfy the following formulas (1), (2), and (3) (first configuration): Cpd≦1.00 (1) 0.10×Cpd≦w1 (2) w1<w2 (3) where Cpd is the distance [mm] from the boundary between the punch shoulder and the punch side surface to the boundary between the die shoulder and the die side surface in the cross-section of the punch and die. w1 is the radius of curvature [mm] of the punch shoulder when the punch shoulder has an arc shape in the cross-section of the punch, and is the length [mm] of the punch shoulder in the direction perpendicular to the approach direction when the punch shoulder has a tapered shape in the cross-section of the punch. w2 is the radius of curvature [mm] of the die shoulder when the die shoulder has an arc shape when viewed in the cross section of the die, or the length [mm] of the die shoulder in the direction perpendicular to the approach direction when the die shoulder has a tapered shape when viewed in the cross section of the die.

[0016] In the manufacturing method according to the first aspect, the punch top surface is disposed inside the annular die flange surface when viewed along the direction of relative approach between the punch and die, and does not overlap with the die flange surface. Meanwhile, the punch shoulder faces the die shoulder when viewed along the direction of relative approach between the punch and die, and overlaps with the die shoulder when viewed along the direction of approach. Therefore, in the process of forming the thin-walled portion, the material is not constrained by the punch top surface and the die flange surface, and a portion of the material is sandwiched between the punch shoulder and the die shoulder. In this case, the portion of the material that is sandwiched and compressed between the punch shoulder and the die shoulder flows along the die shoulder toward the side of the die. This allows the thin-walled portion to be formed in the material with a relatively low load.

[0017] Furthermore, in the manufacturing method according to the first aspect, at least the portion of the punch shoulder and die shoulder that forms the thin-walled portion has an arc-shaped or tapered cross section. At least the portion of the punch shoulder and die shoulder that forms the thin-walled portion, the overlap amount between the punch and die and the proportion of the punch shoulder to this overlap amount are specified (Cpd≦1.00, and 0.10×Cpd≦w1). Furthermore, at least the portion of the punch shoulder and die shoulder that forms the thin-walled portion also has a specified dimensional relationship (w1<w2). This further reduces the load when forming the thin-walled portion in the blank. In the manufacturing method according to the first aspect, there is no need to perform the forming process using the punch and die multiple times, and the thin-walled portion can be formed in the blank in a single forming process.

[0018] Therefore, according to the manufacturing method of the metal member of the first aspect, it is possible to form a thin-walled portion in a material made of a metal plate more easily and with a lower load. By reducing the load required to form a thin-walled portion in the material, it is possible to reduce the load on the mold and suppress damage to the mold.

[0019] In the manufacturing method according to the first aspect, the material may have a thickness of 0.3 mm or more and 2.0 mm or less. In this case, in the forming step, a thin-walled portion having a thickness of 60 μm or less may be formed in the material (second aspect).

[0020] According to the manufacturing method of the embodiment, a portion of the raw material is clamped and compressed between the punch shoulder and the die shoulder, and the material in the compressed portion is allowed to escape along the die shoulder to the side of the die to form the thin-walled portion. Therefore, even when compressing a raw material having a thickness of 0.3 mm to 2.0 mm to a thickness of 60 μm or less, as in the second configuration, the load when forming the thin-walled portion is unlikely to be high, and the load on the mold can be reduced.

[0021] In the manufacturing method according to the first or second aspect, the metal plate may be a steel plate (third aspect).

[0022] In the manufacturing method according to the embodiment, when forming a thin-walled portion in a blank, the material of the blank that is sandwiched between the punch shoulder and the die shoulder flows out along the die shoulder toward the side of the die. This allows the thin-walled portion to be formed in the blank with a low load, even when a blank made of a relatively hard steel plate is used, as in the third configuration. Therefore, the load on the die can be reduced.

[0023] In the manufacturing method according to the third aspect, the steel sheet may be a plated steel sheet (fourth aspect).

[0024] In the manufacturing method according to the third or fourth aspect, the material may have a Rockwell hardness of 45 or more (fifth aspect).

[0025] A method for manufacturing a battery according to an embodiment includes the steps of manufacturing a metal member using a manufacturing method according to any one of the first to fifth configurations, preparing a cylindrical battery case, and attaching the metal member to the battery case to seal the opening of the battery case (sixth configuration).

[0026] The metal member according to the embodiment comprises a valve body, an annular portion, and a member body. The annular portion is arranged to surround the valve body. The member body is arranged around the annular portion. The member body is connected to the valve body via the annular portion. The annular portion includes a thin-walled portion. The thin-walled portion has a thickness smaller than that of the valve body and the member body. The thin-walled portion is formed continuously on one surface of the member body in the thickness direction. The valve body is arranged on the opposite side of the member body in the thickness direction relative to the thin-walled portion. In a cross-sectional view of the metal member, the valve body has a curved shape that is convex on the opposite side of the member body in the thickness direction. Alternatively, in a cross-sectional view of the metal member, the valve body has an undulating shape that undulates in the thickness direction (seventh configuration).

[0027] A battery according to an embodiment includes the metal member according to the seventh configuration and a battery case. The battery case has a cylindrical shape. The opening of the battery case is sealed by the metal member (eighth configuration).

[0028] A mold according to an embodiment is a mold for manufacturing a metal member. The mold includes a punch and a die. The punch includes a punch top surface, a punch shoulder, and a punch side surface. The punch shoulder is continuous with the outer peripheral edge of the punch top surface and has an arc-shaped or tapered shape in cross-sectional view. The punch side surface is connected to the punch top surface via the punch shoulder. The die includes a die flange surface, a die shoulder, and a die side surface. The die flange surface has an annular shape. The die shoulder is continuous with the inner peripheral edge of the die flange surface and has an arc-shaped or tapered shape in cross-sectional view. The die side surface is connected to the die flange surface via the die shoulder. When the punch and die are coaxially arranged so that the punch top surface faces the opening of the die flange surface, as viewed along the axial direction of the punch and die, the punch top surface is located inside the die flange surface, the punch shoulder faces the die shoulder, and the punch side surface is located outside the die side surface. The punch and die are configured to satisfy the following formulas (1), (2), and (3) (ninth configuration). Cpd≦1.00 (1) 0.10×Cpd≦w1 (2) w1<w2 (3) where Cpd is the distance [mm] from the boundary between the punch shoulder and punch side surface to the boundary between the die shoulder and die side surface in a direction perpendicular to the axial direction in the cross sections of the punch and die. w1 is the radius of curvature [mm] of the punch shoulder when the punch shoulder is arc-shaped in the cross section of the punch, and is the length [mm] of the punch shoulder in a direction perpendicular to the axial direction when the punch shoulder is tapered in the cross section of the punch. w2 is the radius of curvature [mm] of the die shoulder when the die shoulder is arc-shaped in the cross section of the die, and is the length [mm] of the die shoulder in a direction perpendicular to the axial direction when the die shoulder is tapered in the cross section of the die.

[0029] Hereinafter, embodiments of the present disclosure will be described with reference to the drawings. In each drawing, the same or equivalent components are designated by the same reference numerals, and the same description will not be repeated.

[0030] 1 is a perspective view schematically illustrating the configuration of a battery 100 according to this embodiment. Although not particularly limited, the battery 100 is, for example, a lithium-ion secondary battery. The battery 100 includes a battery case 10 and a metal member 20.

[0031] In this embodiment, the battery case 10 has a cylindrical shape with a bottom. That is, the battery case 10 includes a peripheral wall 11 and a bottom plate 12. The peripheral wall 11 has a cylindrical shape. In the example shown in FIG. 1 , the peripheral wall 11 has a rectangular cylindrical shape. However, the peripheral wall 11 may have a polygonal cylindrical shape or a cylindrical shape other than a rectangular cylindrical shape. The bottom plate 12 closes one axial end of the peripheral wall 11.

[0032] The metal member 20 is a lid for the battery case 10. The metal member 20 seals the opening of the battery case 10. That is, the metal member 20 seals the end of the peripheral wall 11 opposite the bottom plate 12 in the axial direction. The metal member 20 is joined to the battery case 10 by, for example, welding.

[0033] The metal member 20 includes a member main body 21, a valve body 22, and an annular portion 23. The annular portion 23 has an annular shape and is provided so as to surround the valve body 22. In other words, the valve body 22 is disposed inside the annular portion 23. The member main body 21 is provided around the annular portion 23. The member main body 21 is connected to the valve body 22 via the annular portion 23. The member main body 21, the valve body 22, and the annular portion 23 are integrally formed.

[0034] When the metal member 20 is a lid for the battery case 10 as in this embodiment, the member body 21 has a substantially flat plate shape. In the example of FIG. 1 , the member body 21 corresponds to the shape of the battery case 10 and has a substantially rectangular shape in a plan view. However, the shape of the member body 21 is not limited to this. The member body 21 can have various shapes depending on the shape of the battery case 10, for example.

[0035] In this embodiment, the valve body 22 has a substantially circular shape in a plan view of the metal member 20. The annular portion 23 has a substantially circular ring shape in a plan view of the metal member 20. However, the shapes of the valve body 22 and the annular portion 23 are not limited to these. For example, the valve body 22 may have an elliptical shape, an oval track shape, or the like, or a polygonal shape, such as a square shape. The annular portion 23 may have an elliptical ring shape, a polygonal ring shape, or the like, corresponding to the valve body 22.

[0036] Both the battery case 10 and the metal member 20 are made of metal. Examples of the metal that makes up the battery case 10 and the metal member 20 include steel. Examples of steel include plated steel and stainless steel. The battery case 10 and the metal member 20 are preferably made of nickel-plated steel. However, the battery case 10 and the metal member 20 may be made of a metal other than steel. The metal that makes up the battery case 10 and the metal member 20 may be, for example, aluminum, titanium, copper, or an alloy thereof. The material of the metal member 20 is typically the same as the material of the battery case 10, but may be different from the material of the battery case 10.

[0037] 2 is a cross-sectional view (cross-sectional view taken along II-II in FIG. 1) of the metal member 20 cut at the position of the central axis of the valve body 22. In this embodiment, the cross-sectional shape of the metal member 20 is symmetrical with respect to the central axis, and therefore, in FIG. 2, only one side of the cross section of the metal member 20 about the central axis is shown.

[0038] 2 , the annular portion 23 includes a thin-walled portion 231. The thin-walled portion 231 is a portion of the annular portion 23 that has a thickness smaller than that of the member body 21 and the valve body 22. The thin-walled portion 231 is formed continuously with one of the surfaces 211, 212 in the thickness direction (plate thickness direction) of the member body 21. In the metal member 20, the thin-walled portion 231 is connected to the end face of the member body 21 on the valve body 22 side, offset in the thickness direction of the member body 21. The valve body 22 is formed continuously with the thin-walled portion 231.

[0039] The valve body 22 is disposed on the opposite side of the member body 21 with respect to the thin-walled portion 231 in the thickness direction of the member body 21. The valve body 22 is disposed inside the annular portion 23 and bulges out relative to the thin-walled portion 231 and the member body 21. A bulging height H of the valve body 22 is, for example, equal to or greater than the thickness t1 of the member body 21. The bulging height H is the maximum distance in the thickness direction of the member body 21 between the surface 211 of the member body 21 and the surface 221, of both surfaces 221, 222 of the valve body 22, that is connected to the surface 211 of the member body 21.

[0040] The valve body 22 has a curved shape that is convex on the side opposite to the member body 21 when viewed in a cross section including its central axis. In the example of this embodiment, the valve body 22 is curved as a whole when viewed in a cross section of the metal member 20. The valve body 22 has a substantially arc shape when viewed in a cross section of the metal member 20.

[0041] The member body 21 can have a substantially or roughly uniform thickness t1. The thickness t1 of the member body 21 is, for example, 0.3 mm or more and 2.0 mm or less. The valve body 22 can have a thickness t2 that is substantially equal to the thickness t1 of the member body 21. That is, the thickness t2 of the valve body 22 may be 0.3 mm or more and 2.0 mm or less, similar to the member body 21. When the metal member 20 is made of steel, the thickness t1 of the member body 21 and the thickness t2 of the valve body 22 are preferably 0.8 mm or less from the viewpoint of reducing the weight of the metal member 20. The thickness t1 of the member body 21 and the thickness t2 of the valve body 22 can be measured at a position sufficiently separated from the thin-walled portion 231.

[0042] The thin-walled portion 231 functions as a safety valve together with the valve body 22. The thickness t3 of the thin-walled portion 231 is significantly smaller than the thickness t1 of the member main body 21 and the thickness t2 of the valve body 22 so that the thin-walled portion 231 can rupture before the member main body 21 when the internal pressure of the battery case 10 ( FIG. 1 ) reaches or exceeds a predetermined pressure. The thickness t3 of the thin-walled portion 231 is, for example, 20% or less of the thickness t1 of the member main body 21 and the thickness t2 of the valve body 22. The thickness t3 of the thin-walled portion 231 may be 60 μm or less. The thickness t3 of the thin-walled portion 231 is, for example, 10 μm or more. The thickness t3 of the thin-walled portion 231 is the minimum thickness of the metal member 20.

[0043] The entire annular portion 23 may be the thin-walled portion 231, or only a portion of it may be the thin-walled portion 231. That is, the annular portion 23 may have a thickness t3 along the entire circumference that allows it to be torn when the internal pressure of the battery case 10 ( FIG. 1 ) reaches or exceeds a predetermined pressure, or may have thickness t3 only along a portion of the circumference. When a portion of the annular portion 23 is the thin-walled portion 231 having thickness t3, the thickness of the remaining portion of the annular portion 23 may be substantially equal to the thickness t1 of the member main body 21 and the thickness t2 of the valve body 22, or may be smaller than the thickness t1 of the member main body 21 and the thickness t2 of the valve body 22 but larger than the thickness t3 of the thin-walled portion 231. The thickness of the annular portion 23 does not necessarily have to be constant along the entire circumference.

[0044] When the metal member 20 is made of steel, the Rockwell hardness of the metal member 20 is, for example, 45 or more (45HR30TSm or more). The Rockwell hardness (Rockwell superficial hardness) of the metal member 20 can be obtained by performing a Rockwell hardness test in accordance with JIS Z 2245:2021 on a 30T scale at an arbitrary measurement position on the surface 211 or the surface 212 of the member body 21. The measurement position for the Rockwell hardness is preferably a position on the surface 211 or the surface 212 of the member body 21 that is sufficiently away from the thin-walled portion 231.

[0045] [Method for manufacturing metal member] (Mold) A method for manufacturing the metal member 20 will now be described. First, a mold 30 for manufacturing the metal member 20 will be described with reference to Fig. 3. As shown in Fig. 3, the mold 30 includes a punch 31 and a die 32. The mold 30 may further include a holder 33.

[0046] The punch 31 and the die 32 are arranged coaxially during use. The punch 31 and the die 32 are configured to be able to move closer to and away from each other along the axial direction. The punch 31 and the die 32 are attached to, for example, a known press machine. For example, the punch 31 may be attached to a slide of the press machine and moved up and down together with the slide, thereby moving closer to and away from the die 32. Alternatively, the die 32 may be attached to a slide of the press machine and moved up and down together with the slide, thereby moving closer to and away from the punch 31. Hereinafter, the direction of relative approach between the punch 31 and the die 32, in other words, the axial direction of the punch 31 and the die 32 when the mold 30 is in use, will be referred to as the press direction P.

[0047] The punch 31 includes a punch top surface 311, a punch shoulder 312, and a punch side surface 313. The punch top surface 311 is a surface that intersects with the press direction P. The punch top surface 311 may be a surface that is substantially perpendicular to the press direction P. The punch top surface 311 is, for example, a substantially flat surface over its entirety. The punch top surface 311 has a shape that corresponds to the valve body 22 ( FIGS. 1 and 2 ) of the metal member 20 when viewed along the press direction P. That is, the punch top surface 311 can have a circular, elliptical, polygonal, or other shape in a plan view, corresponding to the valve body 22.

[0048] The punch shoulder 312 is continuous with the outer peripheral edge of the punch top surface 311. The punch shoulder 312 has an annular shape when viewed along the press direction P. When viewed along the press direction P, the punch top surface 311 is disposed inside the annular punch shoulder 312. When viewed along the press direction P, the punch shoulder 312 has a shape corresponding to the annular portion 23 ( FIGS. 1 and 2 ) of the metal member 20. That is, the punch shoulder 312 can have a circular, elliptical, or polygonal annular shape in plan view, corresponding to the annular portion 23.

[0049] In this embodiment, the punch shoulder 312 has an arc shape when viewed in a cross section including the central axis of the punch 31. The punch shoulder 312 has an arc shape that convex outward from the punch 31 when viewed in a cross section of the punch 31. The punch shoulder 312 has a radius of curvature w1. The annular punch shoulder 312 when viewed along the pressing direction P may have a constant radius of curvature w1 over its entire circumference, or may have a predetermined radius of curvature w1 partially. The shape and dimensions of the punch shoulder 312 do not necessarily have to be constant over its entire circumference.

[0050] The punch shoulder 312 is a corner portion between the punch top surface 311 and the punch side surface 313. The punch side surface 313 is connected to the punch top surface 311 via the punch shoulder 312. The punch side surface 313 is continuous around the entire circumference of the annular punch shoulder 312 when viewed along the press direction P. The punch side surface 313 extends in the press direction P when viewed in a cross section including the central axis of the punch 31. The punch side surface 313 may be parallel to the press direction P when viewed in a cross section of the punch 31, or may be slightly inclined with respect to the press direction P.

[0051] The die 32 includes a die flange surface 321, a die shoulder 322, and a die side surface 323. The die flange surface 321 is a surface that intersects with the press direction P. It may also be a surface that is substantially perpendicular to the press direction P. The die flange surface 321 is, for example, a substantially flat surface over its entirety.

[0052] The die flange surface 321 has an annular shape when viewed along the press direction P. That is, the die flange surface 321 has an opening 321a in its center. When the mold 30 is in use, the punch top surface 311 faces the opening 321a of the die flange surface 321. When viewed along the press direction P, the punch top surface 311 is disposed inside the die flange surface 321. Therefore, the punch top surface 311 does not face the die flange surface 321 in the press direction P.

[0053] The die shoulder 322 is continuous with the inner peripheral edge of the die flange surface 321. The die shoulder 322 has an annular shape when viewed along the press direction P. The die shoulder 322 has a shape corresponding to that of the punch shoulder 312 when viewed along the press direction P. That is, the die shoulder 322 can have a circular, elliptical, or polygonal annular shape in plan view, corresponding to the punch shoulder 312.

[0054] When the die 30 is in use, the punch shoulder 312 faces the die shoulder 322 in the press direction P. Like the punch shoulder 312, the die shoulder 322 has an arc shape when viewed in a cross section including the central axis of the die 32. The die shoulder 322 has an arc shape that protrudes outward from the die 32 when viewed in a cross section of the die 32. The die shoulder 322 has a radius of curvature w2. The annular die shoulder 322 when viewed along the press direction P may have a constant radius of curvature w2 throughout its entire circumference, or may have a predetermined radius of curvature w2 partially. The shape and dimensions of the die shoulder 322 do not necessarily have to be constant throughout its entire circumference. The die shoulder 322 has a radius of curvature w2 at least at the position where the punch shoulder 312 has a radius of curvature w1. That is, the punch 31 and the die 32 have a cross section where the punch shoulder 312 has a radius of curvature w1 and the die shoulder 322 has a radius of curvature w2.

[0055] The die shoulder 322 is a corner portion between the die flange surface 321 and the die side surface 323. The die side surface 323 is connected to the die flange surface 321 via the die shoulder 322. The die side surface 323 is continuous around the entire circumference of the annular die shoulder 322 when viewed along the press direction P. The die side surface 323 extends in the press direction P when viewed in a cross section including the central axis of the die 32. The die side surface 323 extends from the die shoulder 322 to the opposite side of the punch 31 when viewed in a cross section of the die 32. The die side surface 323 may be parallel to the press direction P when viewed in a cross section of the die 32, or may be slightly inclined with respect to the press direction P.

[0056] When viewed along the press direction P, the punch side surface 313 is disposed outside the die side surface 323. That is, when viewed along the press direction P, the punch side surface 313 is disposed so as to surround the die side surface 323. In this case, the punch 31 and the die 32 partially overlap when viewed along the press direction P. When the overlap amount of the punch 31 and the die 32 is Cpd, the overlap amount Cpd, the radius of curvature w1 of the punch shoulder 312, and the radius of curvature w2 of the die shoulder 322 satisfy the following formulas (1), (2), and (3). Cpd≦1.00 (1) 0.10×Cpd≦w1 (2) w1<w2 (3)

[0057] The overlap amount Cpd is the distance [mm] in a direction perpendicular to the press direction P from a boundary 314 between the punch shoulder 312 and the punch side surface 313 (where the R of the punch shoulder 312 ends on the punch side surface 313 side) to a boundary 324 between the die shoulder 322 and the die side surface 323 (where the R of the die shoulder 322 ends on the die side surface 323 side) in a cross section that includes the central axes of the punch 31 and the die 322 and where the punch shoulder 312 and the die shoulder 322 have radii of curvature w1 and w2, respectively. In each of the above formulas, the unit of the radius of curvature w1 of the punch shoulder 312 and the radius of curvature w2 of the die shoulder 322 is [mm], just like the overlap amount Cpd.

[0058] The holder 33 is disposed so as to face the die flange surface 321 in the press direction P. The holder 33 may have, for example, an annular shape when viewed along the press direction P, similar to the die flange surface 321.

[0059] The holder 33 is configured to be able to move toward and away from the die 32. The holder 33 is attached to, for example, a known press machine together with the punch 31 and the die 32. For example, if the holder 33 is attached to a slide of the press machine together with the punch 31, the holder 33 moves toward and away from the die 32 as the slide moves up and down. Alternatively, if the die 32 is attached to a slide of the press machine, the die 32 moves toward and away from the holder 33 as the slide moves up and down.

[0060] The holder 33 is configured to be movable relative to the punch 31 in the pressing direction P. The holder 33 may be attached to the press via an elastic member, such as a fluid pressure cylinder or a spring, that is expandable and contractable in the pressing direction P. In this case, the holder 33 can be moved relative to the punch 31 in the pressing direction P by expanding and contracting the elastic member.

[0061] 4A to 4E, a method for manufacturing the metal member 20 using the mold 30 will be described. The manufacturing method for the metal member 20 according to this embodiment includes a step of preparing a material 40 (preparation step) and a step of forming a thin-walled portion 231 in the material 40 (forming step).

[0062] 4A , in the preparation step, a material 40 made of a metal plate is prepared. The material 40 may be a metal plate (blank) that has not been subjected to any particular shaping process, or may be a metal plate that has been partially given a shape, such as a concave or convex shape.

[0063] The metal plate constituting the base material 40 is, for example, a steel plate. This steel plate may be a plated steel plate. A plated steel plate is a steel plate including a base steel plate and a plating layer that covers the surface of the base steel plate. A known plated steel plate can be used for the base material 40. When the metal member 20 to be manufactured is a lid body of the battery 100 ( FIG. 1 ), the plated steel plate is preferably a steel plate having a nickel-based plating (nickel-plated steel plate).

[0064] When the material 40 is made of a steel plate, the material 40 can have, for example, a Rockwell hardness of 45 or more (hardness of 45HR30TSm or more). The Rockwell hardness (Rockwell superficial hardness) of the material 40 can be obtained by performing a Rockwell hardness test in accordance with JIS Z 2245:2021 on a 30T scale at any measurement position on the surface of the material 40, as with the metal member 20 (FIGS. 1 and 2). When the material 40 is a steel plate that has been subjected to some processing, a similar Rockwell hardness test may be performed on the surface of the steel plate before processing, and the obtained Rockwell hardness may be used as the Rockwell hardness of the material 40. The Rockwell hardness of the material 40 is the same as the Rockwell hardness of the metal member 20 manufactured from the material 40.

[0065] However, the material 40 does not necessarily have to be made of a steel plate, but may be made of a plate material made of, for example, aluminum, titanium, copper, or an alloy thereof.

[0066] The thickness t4 of the blank 40 is, for example, 0.3 mm or more and 2.0 mm or less. When the blank 40 is made of a steel plate, the thickness t4 of the blank 40 is preferably 0.8 mm or less.

[0067] 4B to 4E , in the forming process, the blank 40 is placed between the punch 31 and the die 32, the punch 31 and the die 32 are brought relatively close to each other, and a portion of the blank 40 is sandwiched and compressed by the punch shoulder 312 and the die shoulder 322, thereby forming a thin-walled portion 231 that is thinner than the other portions of the blank 40. The forming process will be described in more detail below.

[0068] 4B , prior to the start of the forming process, the punch 31 and the die 32 are separated from each other in the pressing direction P. The holder 33 is also separated from the die 32 in the pressing direction P. When the punch 31, the die 32, and the holder 33 are attached to a press machine, the slide of the press machine is positioned at the top dead center to separate the punch 31 and the holder 33 from the die 32. Then, a material 40 is placed between the punch 31 and the holder 33 and the die 32. In this embodiment, the material 40 is placed on the die flange surface 321.

[0069] 4C , next, the punch 31 and the holder 33 are moved relatively closer to the die 32 along the pressing direction P. For example, the punch 31 and the holder 33 or the die 32 are moved in the pressing direction P together with the slide of the press machine, so that the punch 31 and the holder 33 and the die 32 are moved relatively closer to each other. As a result, the material 40 is first sandwiched between the holder 33 and the die flange surface 321.

[0070] With the blank 40 held down by the holder 33, the punch 31 and the die 32 are further brought closer to each other. As a result, the punch top surface 311 comes into contact with the blank 40, as shown in FIG. 4D . As the punch 31 and the die 32 continue to move closer to each other, a portion of the blank 40 is sandwiched between the punch shoulder 312 and the die shoulder 322, as shown in FIG. 4E . The portion of the blank 40 sandwiched between the portions of the punch shoulder 312 and the die shoulder 322 that satisfy the above formulas (1) to (3) is compressed to form a thin-walled portion 231. Furthermore, the portion of the blank 40 that was in contact with the punch top surface 311 separates from the punch top surface 311 and bulges inward toward the die side surface 323, becoming the valve body 22. An annular portion 23 including the thin-walled portion 231 is formed around the valve body 22.

[0071] When the valve body 22 and the annular portion 23 are formed in the blank 40, the punch 31 and the die 32 are stopped from moving closer to each other. Thereafter, the punch 31 and the holder 33 are moved away from the die 32 in the pressing direction P. This produces the metal member 20 including the member main body 21, the valve body 22, and the annular portion 23.

[0072] Such a manufacturing method for the metal member 20 may be part of a manufacturing method for the battery 100 shown in Fig. 1. That is, the manufacturing method for the battery 100 may include a step of manufacturing the metal member 20 by a manufacturing method including the above-described preparation step and formation step, a step of preparing the battery case 10, and a step of attaching the metal member 20 to the battery case 10 to seal the opening of the battery case 10. The metal member 20 can seal the opening of the battery case 10 in a state in which the contents necessary for the battery 100, such as an electrode body, are housed therein.

[0073] [Effect] In this embodiment, the mold 30 used to manufacture the metal member 20 is configured so that the punch 31 and the die 32 partially overlap when viewed along the press direction P. The punch shoulder 312 faces the die shoulder 322 in the press direction P and, together with the die shoulder 322, sandwiches and compresses a portion of the blank 40 in the metal member 20. At this time, the material of the portion of the blank 40 compressed by the punch shoulder 312 and the die shoulder 322 flows along the die shoulder 322 into the opening 321a of the die flange surface 321. This makes it possible to form the thin-walled portion 231 in the blank 40 with a relatively low load.

[0074] When the punch top surface 311 and the die flange surface 321, which are substantially flat surfaces in the punch 31 and the die 32, overlap, a portion of the material 40 is constrained by the punch top surface 311 and the die flange surface 321, increasing the load required to form the thin-walled portion 231. That is, when the material 40 is compressed by the punch top surface 311 and the die flange surface 321, the material tends to remain between the punch top surface 311 and the die flange surface 321, resulting in a high forming load. However, in this embodiment, the punch top surface 311 is positioned inside the die flange surface 321 as viewed along the pressing direction P so as not to overlap with the punch top surface 311 and the die flange surface 321, which are substantially flat surfaces. In this case, the material 40 can be sandwiched and compressed only by the punch shoulder 312 and the die shoulder 322, without being constrained by the punch top surface 311 and the die flange surface 321. This makes it easier for the material to flow when forming the thin-walled portion 231 in the material 40. Therefore, the thin-walled portion 231 can be formed in the blank 40 with a lower load. In order to prevent material from flowing between the holder 33 and the die flange surface 321 from the punch shoulder 312 and die shoulder 322 sides and to prevent an increase in the load due to this, it is preferable that the holder 33 is not placed close to the punch 31 but is positioned at a certain distance from the punch 31.

[0075] In this embodiment, at least the portion of the punch shoulder 312 and the die shoulder 322 that forms the thin-walled portion 231 in the material 40 has an arc shape in a cross-sectional view of the punch 31 and the die 32, and is configured to satisfy the above-mentioned formulas (1), (2), and (3). The overlap amount Cpd of the punch 31 and the die 32, the radius of curvature w1 of the punch shoulder 312, and the radius of curvature w2 of the die shoulder 322 are set to satisfy the relationships of formulas (1), (2), and (3). In this case, the load when forming the thin-walled portion 231 in the material 40 can be further reduced.

[0076] In this embodiment, the valve body 22 and the thin-walled portion 231 are formed in a single forming process, which allows the metal member 20 to be manufactured more easily than when multiple forming processes are performed, thereby reducing the number of steps and costs required to manufacture the metal member 20.

[0077] As described above, according to this embodiment, the thin-walled portion 231 can be formed more easily and with a lower load in the raw material 40. For example, even when the raw material 40 is made of a relatively hard steel plate, the thin-walled portion 231 can be formed in the raw material 40 with a lower load. Therefore, the load on the mold 30 can be reduced, and damage to the mold 30 can be suppressed.

[0078] If the overlap amount Cpd between the punch 31 and the die 32 is excessively large, it is not possible to sufficiently reduce the load when forming the thin-walled portion 231 in the blank 40. Therefore, in this embodiment, the overlap amount Cpd is set to 1.00 mm or less. From the viewpoint of further reducing the load, the overlap amount Cpd is preferably 0.90 mm or less, and more preferably 0.80 mm or less.

[0079] If the overlap amount Cpd between the punch 31 and the die 32 is too small, the blank 40 may break when compressed by the punch 31 and the die 32, which may make it difficult to stably form the thin-walled portion 231. Therefore, in this embodiment, the overlap amount Cpd is set to 0.05 mm or more. From the viewpoint of more reliably preventing breakage of the blank 40, the overlap amount Cpd is preferably 0.10 mm or more, and more preferably 0.15 mm or more.

[0080] For example, if the radius of curvature w1 of the punch shoulder 312 is equal to or greater than the radius of curvature w2 of the die shoulder 322, when the thin-walled portion 231 is formed in the blank 40, the portion of the member body 21 adjacent to the thin-walled portion 231 will protrude toward the opposite side of the valve body 22. Such a protruding portion may interfere with other parts or members. On the other hand, in this embodiment, in the portions of the punch shoulder 312 and the die shoulder 322 where the thin-walled portion 231 is formed in the blank 40, the radius of curvature w1 of the punch shoulder 312 is less than the radius of curvature w2 of the die shoulder 322. In this case, when the thin-walled portion 231 is formed in the blank 40, protrusion of the portion of the member body 21 adjacent to the thin-walled portion 231 can be suppressed. Furthermore, since the radius of curvature w2 of the die shoulder 322 is larger than the radius of curvature w1 of the punch shoulder 312, when forming the thin-walled portion 231 in the raw material 40, the material of the portion of the raw material 40 compressed by the punch shoulder 312 and the die shoulder 322 is more likely to flow along the die shoulder 322 toward the opening 321a of the die flange surface 321.

[0081] In this embodiment, the curvature radius w1 of the punch shoulder 312 is, for example, 0.05 mm or more. By ensuring a certain degree of curvature radius w1, for example, when the blank 40 is made of a plated steel sheet, the punch shoulder 312 is less likely to disrupt the plating layer. This prevents a decrease in corrosion resistance due to disruption of the plating layer in the thin-walled portion 231 of the metal member 20, thereby suppressing rusting of the base steel sheet. The curvature radius w1 may be, for example, 1.00 mm or less. The curvature radius w2 of the die shoulder 322 may be larger than the curvature radius w1 of the punch shoulder 312, for example, 0.10 mm or more. The curvature radius w2 of the die shoulder 322 is, for example, larger than the curvature radius w1 of the punch shoulder 312 by 0.05 mm or more. The curvature radius w2 may be, for example, 2.00 mm or less.

[0082] In this embodiment, the thickness t4 of the blank 40 is, for example, 0.3 mm or more and 2.0 mm or less. In the forming process, a thin-walled portion 231 having a thickness t3 of, for example, 60 μm or less is formed in the blank 40. Even when a portion of the blank 40 is machined to be extremely thin in this manner, in this embodiment, the material of the portion of the blank 40 compressed by the punch shoulder 312 and the die shoulder 322 is machined while escaping toward the opening 321 a of the die flange surface 321, thereby enabling machining with a low load. Therefore, the load on the mold 30 can be reduced.

[0083] Second Embodiment Fig. 5 is a cross-sectional view of a mold 30A according to this embodiment. Fig. 5 shows a cross-section of the mold 30A when cut along a plane including the central axes of the punch 31 and the die 32. This embodiment differs from the first embodiment in the configuration of the mold 30A. However, the method for manufacturing the metal member 20 and the battery 100 using the mold 30A, and the configurations of the metal member 20 and the battery 100 obtained by this manufacturing method are similar to those of the first embodiment (Figs. 1, 2, and 4A to 4E).

[0084] 5, the die 30A of this embodiment differs from the die 30 of the first embodiment (FIG. 3) in the shapes of the punch shoulder 312 and the die shoulder 322. In the die 30A, the punch shoulder 312 has a tapered shape when viewed in a cross section including the central axis of the punch 31. The punch shoulder 312 is inclined with respect to the pressing direction P so as to move away from the central axis of the punch 31 as the distance from the punch top surface 311 in the pressing direction P increases.

[0085] The punch shoulder 312 has a taper width w1. The taper width w1 is the length of the punch shoulder 312 in a direction perpendicular to the press direction P when viewed in a cross section including the central axis of the punch 31. The taper width w1 is, for example, 0.05 mm or more. The taper width w1 may be, for example, 1.00 mm or less. The annular punch shoulder 312 when viewed along the press direction P may have a constant taper width w1 over its entire circumference, or may have a predetermined taper width w1 partially. As in the first embodiment, the shape and dimensions of the punch shoulder 312 do not necessarily have to be constant over its entire circumference.

[0086] In the mold 30A, the die shoulder 322 also has a tapered shape when viewed in a cross section including the central axis of the die 32. The die shoulder 322 is inclined with respect to the press direction P so as to approach the central axis of the die 32 as the distance from the die flange surface 321 in the press direction P increases.

[0087] The die shoulder 322 has a taper width w2. The taper width w2 is the length of the die shoulder 322 in a direction perpendicular to the press direction P when viewed in a cross section including the central axis of the die 32. The taper width w2 is, for example, 0.10 mm or more. The taper width w2 may be, for example, 2.00 mm or less. The annular die shoulder 322 when viewed along the press direction P may have a constant taper width w2 over its entire circumference, or may have a predetermined taper width w2 partially. The shape and dimensions of the die shoulder 322 do not necessarily have to be constant over its entire circumference. The die shoulder 322 has the taper width w2 at least at a position where the punch shoulder 312 has the taper width w1.

[0088] The punch 31 and the die 32 have a cross section in which the punch shoulder 312 has a tapered width w1 and the die shoulder 322 has a tapered width w2. In this cross section, the tapered width w1 [mm] of the punch shoulder 312 and the tapered width w2 [mm] of the die shoulder 322, together with the overlap amount Cpd [mm] of the punch 31 and the die 32, satisfy the following formulas (1), (2), and (3). Regarding formula (3), the tapered width w2 of the die shoulder 322 may be larger than the tapered width w1 of the punch shoulder 312 by, for example, 0.05 mm or more. Cpd≦1.00 (1) 0.10×Cpd≦w1 (2) w1<w2 (3)

[0089] In the die 30A of this embodiment, at least the portions of the punch shoulder 312 and the die shoulder 322 that form the thin-walled portion 231 in the blank 40 have a tapered shape in a cross-sectional view of the punch 31 and the die 32, and are configured to satisfy the above-mentioned formulas (1), (2), and (3). Even when the metal member 20 (FIGS. 1 and 2) is manufactured using this die 30A, the same effects as those of the first embodiment can be achieved.

[0090] Although the embodiments of the present disclosure have been described above, the present disclosure is not limited to the above-described embodiments, and various modifications are possible without departing from the spirit of the present disclosure.

[0091] In the above embodiment, the die hole defined by the die side surface 323 does not have a bottom surface. However, as shown in FIGS. 6 and 7 , the die 32 may include a die bottom surface 325 provided in the die hole. The die bottom surface 325 faces the punch top surface 311 in the pressing direction P when the mold 30, 30A is in use. The distance D in the pressing direction P from the die flange surface 321 to the die bottom surface 325 (die hole depth) can be determined as appropriate. However, the die hole depth D is set to a size that does not constrain the material between the punch top surface 311 and the die bottom surface 325. Because the material is not constrained by the die bottom surface 325, the same load reduction effect as in the above embodiment can be achieved even when the die hole has a die bottom surface 325.

[0092] When the die hole has a die bottom surface 325, the shape of the metal member 20 manufactured using the punch 31 and die 32 can be changed. More specifically, as shown in Figures 8 and 9, when the die hole has a die bottom surface 325, the shape of the valve body 22 in the metal member 20 manufactured using the punch 31 and die 32 differs from that when the die hole does not have a die bottom surface 325. Figure 8 is a cross-sectional view of the metal member 20 manufactured using a die 32 with a relatively small die hole depth D, and Figure 9 is a cross-sectional view of the metal member 20 manufactured using a die 32 with a larger die hole depth D than the example in Figure 8.

[0093] When the thin-walled portion 231 of the metal member 20 is formed using a die 32 having no die bottom surface 325 in the die hole and a punch 31 as in the above embodiment, the entire valve body 22 is curved convexly toward the opposite side to the member body 21 in a cross-sectional view of the metal member 20 ( FIG. 2 ). On the other hand, when the thin-walled portion 231 of the metal member 20 is formed using a die 32 having a die bottom surface 325 in the die hole and a punch 31, the valve body 22 has an undulating shape that undulates in the thickness direction of the member body 21, as shown in FIGS. 8 and 9 . In other words, the valve body 22 has a wavy shape at least in part in a cross-sectional view of the metal member 20.

[0094] In the above embodiment, the battery case 10 has a cylindrical shape with a bottom. However, the battery case 10 may have a cylindrical shape without a bottom. In this case, both openings at both ends in the axial direction of the cylindrical battery case 10 may be sealed with the metal member 20, or only one of the openings may be sealed with the metal member 20. When one opening of the battery case 10 is sealed with the metal member 20, the other opening may be sealed with a lid separate from the metal member 20.

[0095] In the above embodiment, the metal member 20 is a lid attached to the battery case 10. However, the metal member 20 does not necessarily have to be a lid for the battery case 10. For example, the metal member 20 may be a cylindrical battery case with or without a bottom. In this case, the valve body 22 and the annular portion 23 may be formed on the bottom plate or the peripheral wall of the battery case. A cylindrical battery case with a bottom can be formed, for example, by drawing a metal plate. Depending on the shape of the battery case, the process of forming the annular portion 23 including the valve body 22 and the thin-walled portion 231 may be performed using a metal plate before being formed into a cylindrical battery case as the raw material 40, or may be performed using a battery case formed into a cylindrical shape from a metal plate as the raw material 40. The metal member 20 may also be part of a pressure vessel such as a boiler.

[0096] In the above embodiment, when forming the thin-walled portion 231 in the blank 40, the die 32 is disposed below the punch 31. However, the arrangement of the punch 31 and the die 32 is not limited to this. For example, the die 32 may be disposed above the punch 31.

[0097] The present disclosure will be described in more detail below with reference to examples, although the present disclosure is not limited to the following examples.

[0098] To confirm the effects of the present disclosure, CAE analysis was performed using commercially available analysis software (MSC.Marc, manufactured by MSC Software Co., Ltd.) to evaluate the forming load for the production of metal parts using a mold having the same shape as the mold 30 described in the first embodiment or the mold 30A described in the second embodiment. In this analysis, a nickel-plated steel sheet with a thickness of 0.3 mm and a Rockwell hardness (HR30TSm): 51 was used as the material, and a thin-walled portion was formed in this material. The conditions and evaluation results for this analysis are shown in Table 1.

[0099]

[0100] In Test Examples 1 to 7, the overlap amount Cpd between the punch and the die, the radius of curvature or taper width w1 of the punch shoulder, and the radius of curvature or taper width w2 of the die shoulder satisfy all of the following formulas (1), (2), and (3). Furthermore, in Test Examples 1 to 7, there is no overlap of the flat surfaces when viewed along the press direction, and the die overlaps with the punch substantially only at the die shoulder. Here, "flat surface overlap" in this analysis (Table 1) refers to the overlap between the punch top surface and the die flange surface. In Test Examples 1 to 7, the punch top surface and the die flange surface, which are substantially flat surfaces, do not overlap, and the material is not restrained by the punch top surface and the die flange surface during the process of forming the thin-walled portion. Cpd≦1.00 (1) 0.10×Cpd≦w1 (2) w1<w2 (3)

[0101] In Test Examples 1 to 7, the load (forming load) when forming a thin-walled portion in the blank was low. However, in Test Examples 8 to 14, the forming load was significantly higher than in Test Examples 1 to 7. In particular, in Test Examples 11 and 12, which did not satisfy formulas (2) and (3) and in which the punch top surface and the die flange surface overlapped, the forming load was significantly higher than in Test Examples 1 to 7. Furthermore, in Test Example 14, which did not satisfy formula (1), the forming load was also significantly higher than in Test Examples 1 to 7.

[0102] Test Examples 9 and 13 are test examples in which, although formulas (1), (2), and (3) are satisfied, a thin-walled portion was formed in the blank with the punch top surface and the die flange surface overlapping. Test Example 13 had a smaller ratio of the thickness t3 of the thin-walled portion to the thickness t4 of the original blank compared to Test Example 9, and the blank was compressed to a significantly thinner thickness. Therefore, Test Example 13 required a significantly higher forming load than Test Examples 1 to 7 and Test Example 9. The forming load of Test Example 9 was lower than that of Test Example 13, but was still higher than that of Test Examples 1 to 7.

[0103] Test Examples 8 and 10 are test examples that satisfy formulas (1) and (2) but do not satisfy formula (3). In Test Example 8, the punch top surface and the die flange surface further overlap. In Test Examples 8 and 10, the forming load was lower than in Test Examples 11 to 14, but higher than in Test Examples 1 to 7.

[0104] This analysis confirmed that the load applied when forming a thin-walled portion in a material is effectively reduced when the overlap amount Cpd of the punch and die, the radius of curvature or taper width w1 of the punch shoulder, and the radius of curvature or taper width w2 of the die shoulder all satisfy the following formulas (1), (2), and (3), and when the punch top surface and the die flange surface do not overlap when viewed along the pressing direction.

[0105] 100: Battery 10: Battery case 20: Metal member 21: Member body 22: Valve body 23: Annular portion 231: Thin-walled portion 30, 30A: Die 31: Punch 311: Punch top surface 312: Punch shoulder 313: Punch side surface 314: Boundary 32: Die 321: Die flange surface 321a: Opening 322: Die shoulder 323: Die side surface 324: Boundary 40: Material

Claims

1. A method for manufacturing a metal member, comprising the steps of: preparing a material made of a metal plate; disposing the material between a punch including a punch top surface, a punch shoulder continuing from the outer periphery of the punch top surface, and a punch side surface connected to the punch top surface via the punch shoulder, and a die including a die flange surface having an annular shape, a die shoulder continuing from the inner periphery of the die flange surface, and a die side surface connected to the die flange surface via the die shoulder; bringing the punch and the die relatively close to each other, and sandwiching and compressing a part of the material between the punch shoulder and the die shoulder, thereby forming a thin-walled portion in the material having a smaller thickness than other parts, wherein the punch top surface is disposed inside the die flange surface when viewed along a relative approach direction of the punch and the die, the punch shoulder faces the die shoulder in the approach direction, and the punch side surface is disposed outside the die side surface when viewed along the approach direction, a punch shoulder and a die shoulder, each of which has an arc shape or a tapered shape in a cross-sectional view of the punch and the die, and is configured to satisfy the following formulas (1), (2), and (3). Cpd≦1.00 (1) 0.10×Cpd≦w1 (2) w1<w2 (3) where Cpd is the distance [mm] in the direction perpendicular to the approach direction from the boundary between the punch shoulder and the punch side surface to the boundary between the die shoulder and the die side surface on the cross sections of the punch and the die, w1 is the radius of curvature [mm] of the punch shoulder when the punch shoulder has an arc shape when viewed on the cross section of the punch, or the length [mm] of the punch shoulder in the direction perpendicular to the approach direction when the punch shoulder has a tapered shape when viewed on the cross section of the punch, and w2 is the radius of curvature [mm] of the die shoulder when the die shoulder has an arc shape when viewed on the cross section of the die, or the length [mm] of the die shoulder in the direction perpendicular to the approach direction when the die shoulder has a tapered shape when viewed on the cross section of the die.

2. A manufacturing method according to claim 1, wherein the material has a thickness of 0.3 mm or more and 2.0 mm or less, and in the forming step, the thin-walled portion having a thickness of 60 μm or less is formed in the material.

3. The manufacturing method according to claim 1 or 2, wherein the metal plate is a steel plate.

4. The manufacturing method according to claim 3, wherein the steel sheet is a plated steel sheet.

5. The manufacturing method according to claim 3, wherein the material has a Rockwell hardness of 45 or more.

6. A method for manufacturing a battery, comprising the steps of: manufacturing a metal member by the manufacturing method described in claim 1; preparing a cylindrical battery case; and attaching the metal member to the battery case to seal an opening of the battery case.

7. A metal member comprising: a valve body; an annular portion arranged to surround the valve body; and a member main body arranged around the annular portion and connected to the valve body via the annular portion, wherein the annular portion has a thickness smaller than that of the valve body and the member main body, and includes a thin-walled portion formed continuously on one side of the member main body in a thickness direction, and the valve body is arranged on the opposite side to the member main body in the thickness direction with respect to the thin-walled portion, and in a cross-sectional view of the metal member, has a convex curved shape on the opposite side to the member main body in the thickness direction or an undulating shape that undulates in the thickness direction.

8. A battery comprising: the metal member according to claim 7; and a cylindrical battery case having an opening sealed by the metal member.

9. A die for manufacturing a metal component, comprising: a punch including a punch top surface, a punch shoulder continuing from the outer peripheral edge of the punch top surface and having an arc-shaped or tapered shape in cross section, and a punch side surface connected to the punch top surface via the punch shoulder; and a die including a die flange surface having an annular shape, a die shoulder continuing from the inner peripheral edge of the die flange surface and having an arc-shaped or tapered shape in cross section, and a die side surface connected to the die flange surface via the die shoulder, wherein when the punch and the die are coaxially arranged so that the punch top surface faces an opening of the die flange surface, when viewed along the axial direction of the punch and the die, the punch top surface is arranged inside the die flange surface, the punch shoulder faces the die shoulder, and the punch side surface is arranged outside the die side surface, and the punch and the die are configured to satisfy the following formulas (1), (2), and (3). Cpd≦1.00 (1) 0.10×Cpd≦w1 (2) w1<w2 (3) where Cpd is the distance [mm] in a direction perpendicular to the axial direction from a boundary between the punch shoulder and the punch side surface to a boundary between the die shoulder and the die side surface in the cross sections of the punch and the die, w1 is the radius of curvature [mm] of the punch shoulder when the punch shoulder has an arc shape in the cross section of the punch, or the length [mm] of the punch shoulder in the direction perpendicular to the axial direction when the punch shoulder has a tapered shape in the cross section of the punch, and w2 is the radius of curvature [mm] of the die shoulder when the die shoulder has an arc shape in the cross section of the die, or the length [mm] of the die shoulder in the direction perpendicular to the axial direction when the die shoulder has a tapered shape in the cross section of the die.

Citation Information

Patent Citations

  • Cold forging method of thin wall part and explosion-proof valve

    JP2015085356A

  • Sealing plate of sealed battery and its manufacture

    JP1999273640A

  • Sealed member attached with safety valve and method for manufacturing the same

    JP2001102023A

  • Flat battery and manufacturing method of the same

    JP2002175789A

  • Safety valve for sealed cylindrical battery, and manufacturing method of the same

    JP2005251447A