Resin, paste composition, inorganic sintered body, electronic device, and solar panel

The resin, with its specific structural units and mercaptan derivatives, addresses the limitations of existing binder resins by enhancing thixotropy and thermal decomposition, improving the printability and performance of inorganic sintered bodies in electronic devices and solar panels.

WO2024203009A1PCT designated stage expired Publication Date: 2024-10-03MITSUBISHI CHEM CORP

Patent Information

Application Number
PCT/JP2024/008189
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-27
Filing Date
2024-03-05
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Existing binder resins for inorganic sintered bodies in electronic devices and solar panels lack high thixotropy and solvent solubility, and their thermal decomposition properties are not adequately adjustable, which affects the printability and performance of these components.

Method used

A resin with structural units derived from (meth)acrylic acid esters and mercaptans, having a high weight average molecular weight to number average molecular weight ratio, and incorporating specific mercaptan structures, which enhances thixotropy and thermal decomposition while allowing for adjustable viscosity and solvent solubility.

Benefits of technology

The resin provides excellent solvent solubility, thermal decomposition properties, and high thixotropy, improving screen printability and post-printing leveling, making it suitable for internal and external electrode layers of electronic devices and solar panels.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
Patent Text Reader

Abstract

Provided are: a resin having excellent solvent solubility and thermal decomposition properties and high thixotropic properties; a paste composition; an inorganic sintered body; an electronic device; and a solar panel. A resin according to the present invention has a constituent unit derived from a (meth)acrylic acid ester and a chemical structure derived from mercaptan having two or more SH groups, and the ratio Mw / Mn of the weight-average molecular weight (Mw) to the number-average molecular weight (Mn) is 5.0 or more.
Need to check novelty before this filing date? Find Prior Art

Description

Resins, paste compositions, inorganic sintered bodies, electronic devices and solar panels

[0001] The present invention relates to a resin, a paste composition, an inorganic sintered body, an electronic device, and a solar panel. This application claims priority based on Japanese Patent Application No. 2023-049200, filed on March 27, 2023, the contents of which are incorporated herein by reference.

[0002] Inorganic molded bodies and patterns formed from such molded bodies (e.g., wiring patterns, insulating patterns, etc.) are sometimes used in internal electrode layers and external electrodes of multilayer electronic components such as multilayer ceramic capacitors, solar cell electrodes, etc. A known method for forming such molded bodies or patterns is to mix an inorganic compound such as a metal powder, a metal oxide powder, a fluorescent powder, or a glass frit with a binder resin to prepare a paste composition, mold this paste composition into a predetermined shape to form a molded body or a pattern, and then bake the paste composition to thermally decompose the binder resin.

[0003] The binder resin used in this process improves processability during molding and binds the inorganic compounds together to prevent damage during transport. Because this binder resin is removed by thermal decomposition when the inorganic compounds are sintered before becoming the final product, it is required to have high thermal decomposition properties and excellent workability during each processing step. Furthermore, the binder resin for this application is required to be a solvent-free solid that is easily soluble in solvents, allowing for easy adjustment of the viscosity range by adjusting the amount added during compounding and a wide range of solvent options.

[0004] Known methods for processing a paste composition include screen printing, forming into a sheet using a doctor blade or the like, dipping, and dispensing. When applying the screen printing method, the higher the thixotropy of the paste composition, the better the printability and leveling properties after printing. Therefore, when screen printing is performed, a paste composition with high thixotropy is required.

[0005] As a binder resin, for example, Patent Document 1 discloses crosslinked fine particles that are (meth)acrylic resins containing 20 to 55 mass% of structural units derived from a monofunctional (meth)acrylic ester having 1 to 4 carbon atoms in the ester moiety and 45 to 80 mass% of structural units derived from a polyfunctional (meth)acrylic ester having an alkylene glycol moiety having 2 to 4 carbon atoms, and have an average particle size of 0.1 to 0.5 μm, and that leave a heating residue of 0.3 mass% or less when heated to 500°C at 5°C / min in an air atmosphere. Patent Document 2 discloses a binder resin for conductive pastes that is excellent in thixotropy and thermal decomposition properties due to a polymer of a specific structure having a hydroxyurethane structure.

[0006] Japanese Patent Publication No. 2021-017478 International Publication No. 2020 / 152939

[0007] However, the paste composition obtained using the crosslinked fine particles described in Patent Document 1 does not provide high thixotropy suitable for screen printing. Furthermore, the binder resin for conductive paste described in Patent Document 2 is not solid, and there are issues with solvent selectivity and adjusting the viscosity range. An object of the present invention is to provide a resin, paste composition, inorganic sintered body, electronic device, and solar panel that have excellent solvent solubility and thermal decomposition properties and high thixotropy.

[0008] The present invention is summarized in the following [1] to

[16] . [1] A resin having a structural unit derived from a (meth)acrylic acid ester and a chemical structure derived from a mercaptan having two or more SH groups, wherein the ratio Mw / Mn of the weight average molecular weight (Mw) to the number average molecular weight (Mn) is 5.0 or more. [2] The resin of [1] above, wherein the resin is a solid binder for firing. [3] The resin of [1] or [2] above, wherein the mass average particle diameter is greater than 100 μm and not greater than 1500 μm. [4] The resin of any of [1] to [3] above, wherein the acid value is 0 to 50 mgKOH / g. [5] The resin of any of [1] to [4] above, further having a chemical structure derived from a mercaptan having one SH group. [6] The resin of any of [1] to [5] above, further having a structural unit derived from a monomer having two or more polymerizable double bonds. [7] The resin of any of [1] to [6] above, wherein the structural units derived from a monomer having two or more polymerizable double bonds account for 0.1 to 5.0 mass% of the structural units derived from all monomers in the resin. [8] The resin of any of [1] to [7] above, wherein the thermal weight loss rate determined under the following measurement conditions is 95.0% or more. <Measurement conditions for thermal weight loss rate> Using a differential thermal balance (TG-DTA), 5 mg of a measurement sample is heated in a nitrogen atmosphere from a starting temperature of 30°C to 500°C at a rate of 10°C / min, and the mass of the residue upon reaching 450°C is measured, and the thermal weight loss rate is calculated using the following formula (1). Thermal loss rate (%) = {(mass (mg) of measurement sample - mass (mg) of residue) / mass (mg) of measurement sample} × 100 ... (1) [9] The resin of any of [1] to [8] above, wherein a resin solution containing 30 mass% of the resin, obtained by dissolving the resin in terpineol, satisfies the following formula (2): η1 / η1000 ≧ 1.5 ... (2) Here, η1 and η1000 are the viscosity (Pa s) of the resin solution measured using a viscoelasticity measuring device under conditions of a cone plate 1.0° / 20 mm and a measurement temperature of 23°C, η1 is the viscosity (Pa s) at a shear rate of 1 (1 / s), and η1000 is the viscosity (Pa s) at a shear rate of 1000 (1 / s).

[10] The resin according to any one of [1] to [9] above, having a weight average molecular weight of 10,000 to 1,000,000.

[11] The resin of any one of [1] to

[10] above, having a water content of 0.01 to 10 mass% relative to the total mass of the resin.

[12] A paste composition comprising the resin of any one of [1] to

[11] above, a metal or inorganic compound, and an organic solvent.

[13] The paste composition of

[12] above, wherein the boiling point of the organic solvent is 180°C or higher.

[14] An inorganic sintered body obtained by firing the paste composition of

[12] or

[13] above.

[15] An electronic device having the inorganic sintered body of

[14] above.

[16] A solar panel having the inorganic sintered body of

[14] above.

[0009] According to the present invention, it is possible to provide a resin, a paste composition, an inorganic sintered body, an electronic device, and a solar panel that have excellent solvent solubility, thermal decomposition property, and high thixotropy.

[0010] The present invention will be described in further detail below with reference to preferred embodiments of the invention. However, the following description is merely an example of an embodiment of the present invention, and the present invention is not limited to the following description as long as it does not depart from the gist of the invention. In the present invention, "(meth)acrylic" is a general term for acrylic and methacrylic. "(meth)acrylate" is a general term for acrylate and methacrylate. "(meth)acryloyl" is a general term for acryloyl and methacryloyl. In the present invention, "polymerizable double bond" means a double bond capable of radical polymerization. In the present invention, "room temperature" means 5 to 30°C. In the present invention, the "to" symbol indicating a numerical range means that the numerical values ​​before and after it are included as the lower and upper limits.

[0011] [Resin] One embodiment of the resin of the present invention will be described below. The resin of this embodiment has a structural unit (a1) derived from a (meth)acrylic acid ester (hereinafter also referred to as "monomer (a1)") and a chemical structure (b1) derived from a mercaptan having two or more SH groups, and the ratio Mw / Mn of the weight average molecular weight (Mw) to the number average molecular weight (Mn) is 5.0 or more. In order to obtain good solvent solubility and thixotropy, the ratio Mw / Mn of the weight average molecular weight (Mw) to the number average molecular weight (Mn) is preferably 5.5 or more, more preferably 10 or more, even more preferably 15 or more, particularly preferably 30 or more, and most preferably 35 or more. Furthermore, it is preferably 100 or less, more preferably 80 or less, even more preferably 60 or less, and particularly preferably 40 or less. The above upper and lower limits can be combined arbitrarily. For example, it may be 5.0 to 100, 5.5 to 100, 10 to 100, 30 to 100, 35 to 100, 5.0 to 80, 10 to 80, 15 to 80, 30 to 80, 35 to 80, 5.0 to 60, 10 to 60, 15 to 60, 30 to 60, 35 to 60, 5.0 to 40, 10 to 40, 15 to 40, 30 to 40, or 35 to 40. Within the above ranges, an increase in the proportion of low molecular weight components improves solvent solubility, thermal decomposition, and thixotropy. As a method for adjusting the ratio Mw / Mn of the weight average molecular weight (Mw) to the number average molecular weight (Mn) of the resin, for example, the ratio Mw / Mn can be increased by increasing the proportion of the structural unit (a2) relative to all structural units of the resin. Alternatively, the ratio Mw / Mn can be decreased by decreasing the proportion of the structural unit (a2) relative to all structural units of the resin. The weight average molecular weight (Mw) and number average molecular weight (Mn) of the resin are values ​​calculated in terms of standard polystyrene measured by gel permeation chromatography (GPC). Detailed measurement conditions are as described in the Examples below.

[0012] In addition to the structural unit (a1) and chemical structure (b1), the resin preferably further comprises at least one of a structural unit (a2) derived from a monomer having two or more polymerizable double bonds (hereinafter also referred to as "monomer (a2)") and a chemical structure (b2) derived from a mercaptan having one SH group. The resin may further comprise a structural unit (a3) ​​derived from a monomer other than the monomer (a1) and the monomer (a2) (hereinafter also referred to as "monomer (a3)").

[0013] <Monomer (a1)> The monomer (a1) is a (meth)acrylic acid ester. The monomer (a1) is a monofunctional monomer having one polymerizable double bond, specifically one (meth)acryloyl group as the functional group having the polymerizable double bond. Examples of the monomer (a1) include alkyl (meth)acrylates having a linear or branched hydrocarbon skeleton, such as methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, i-propyl (meth)acrylate, n-butyl (meth)acrylate, i-butyl (meth)acrylate, t-butyl (meth)acrylate, n-pentyl (meth)acrylate, i-pentyl (meth)acrylate, n-hexyl (meth)acrylate, n-octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, lauryl (meth)acrylate, stearyl (meth)acrylate, isostearyl (meth)acrylate, and 4-t-butylcyclohexyl (meth)acrylate; Alkyl (meth)acrylates having an alicyclic skeleton, such as cyclohexyl (meth)acrylate, isobornyl (meth)acrylate, adamantyl (meth)acrylate, tricyclodecanyl (meth)acrylate, dicyclopentadienyl (meth)acrylate, and dicyclopentanyl (meth)acrylate; (meth)acrylic acid esters having a glycidyl group, such as glycidyl (meth)acrylate and hydroxybutyl (meth)acrylate glycidyl ether; (meth)acrylic acid esters having an aromatic ring, such as phenoxy (meth)acrylate, benzyl (meth)acrylate, phenyl (meth)acrylate, phenoxyethyl (meth)acrylate, phenoxy polyethylene glycol (meth)acrylate, nonylphenol EO adduct (meth)acrylate, and o-biphenyloxyethyl (meth)acrylate; (meth)acrylic acid salts, such as ammonium (meth)acrylate, sodium (meth)acrylate, and potassium (meth)acrylate; (Meth)acrylates having a cyclic ether, such as tetrahydrofurfuryl (meth)acrylate; (meth)acrylates having an amino group, such as N-dimethylaminoethyl (meth)acrylate and N-diethylaminoethyl (meth)acrylate;(Meth)acrylamide derivatives such as (meth)acrylamide, (meth)acrylamide diacetone acrylamide, N-methylol (meth)acrylamide, N-methoxymethyl (meth)acrylamide, N-ethoxymethyl (meth)acrylamide, N-butoxymethyl (meth)acrylamide, and (meth)acryloylmorpholine; monomers having a phosphate group such as 2-(meth)acryloyloxyethyl acid phosphate, 2-(meth)acryloyloxyethyl acid phosphate monoethanolamine salt, diphenyl ((meth)acryloyloxyethyl) phosphate, (meth)acryloyloxypropyl acid phosphate, 3-chloro-2-acid phosphooxypropyl (meth)acrylate, acid phosphooxypolyoxyethylene glycol mono(meth)acrylate, and acid phosphooxypolyoxypropylene glycol (meth)acrylate; Hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 1,2-dihydroxyethyl (meth)acrylate, 1,2-dihydroxypropyl (meth)acrylate, 1,2-dihydroxybutyl (meth)acrylate, 1,2-dihydroxy-5-ethylhexyl (meth)acrylate, 1,1-dihydroxyethyl (meth)acrylate, 1,1-dihydroxypropyl (meth)acrylate, 1,1-dihydroxybutyl (meth)acrylate, 1,2,3-trihydroxypropyl (meth)acrylate, 1,2,3-trihydroxybutyl (meth)acrylate, 1,1,2-trihydroxypropyl (meth)acrylate, and 1,1,2-trihydroxybutyl (meth)acrylate; hydroxy(meth)acrylates having an aromatic ring, such as 2-hydroxy-3-phenoxypropyl(meth)acrylate;Hydroxypolyethylene oxide mono(meth)acrylate, hydroxypolypropylene oxide mono(meth)acrylate, hydroxy(polyethylene oxide-polypropylene oxide) mono(meth)acrylate, hydroxy(polyethylene oxide-propylene oxide) mono(meth)acrylate, hydroxy(polyethylene oxide-polytetramethylene oxide) mono(meth)acrylate, hydroxy(polyethylene oxide-tetramethylene oxide) mono(meth)acrylate, hydroxy(polypropylene oxide-polytetramethylene oxide) mono(meth)acrylate, hydroxy(polypropylene oxide-polytetramethylene oxide) mono(meth)acrylate, 1,2-dihydroxypolyethyl oxide (meth)acrylate, 1,2-dihydroxypolypropylene oxide (meth)acrylate, polyhydroxyalkyl (meth)acrylate; hydroxypolyalkylene oxide (meth)acrylates such as 1,2,3-trihydroxypropylene glycol (meth)acrylate and 1,1,2-trihydroxypropylene glycol (meth)acrylate; Examples of the monomer (a1) include (meth)acrylates having a carboxyl group, such as acrylic acid, methacrylic acid, mono(2-(meth)acryloyloxyethyl succinate), and ω-carboxy-polycaprolactone mono(meth)acrylate. From the viewpoint of thermal decomposition properties, alkyl(meth)acrylates having a linear or branched hydrocarbon skeleton are preferred, and from the viewpoint of versatility in particular, methyl(meth)acrylate, ethyl(meth)acrylate, n-propyl(meth)acrylate, i-propyl(meth)acrylate, n-butyl(meth)acrylate, i-butyl(meth)acrylate, t-butyl(meth)acrylate, 2-ethylhexyl(meth)acrylate, and lauryl(meth)acrylate are more preferred. One type of monomer (a1) may be used alone, or two or more types may be used in combination.

[0014] The proportion of the structural unit (a1) in the resin, when the total of all structural units constituting the resin is 100% by mass, is preferably 70.0 to 100% by mass, more preferably 90.0 to 99.9% by mass, even more preferably 95.0 to 99.7% by mass, particularly preferably 97.0 to 99.5% by mass, and most preferably 99.0 to 99.5% by mass. If the proportion is equal to or greater than the lower limit, the thermal decomposition property of the resin is further improved. If the proportion is equal to or less than the upper limit, the thixotropy of the resin is further improved.

[0015] <Monomer (a2)> The monomer (a2) is a monomer having two or more polymerizable double bonds. Examples of the monomer (a2) include a polyfunctional monomer having two or more (meth)acryloyl groups as functional groups having a polymerizable double bond. Examples of the monomer (a2) include polyfunctional alkyl (meth)acrylates having a linear or branched hydrocarbon skeleton, such as ethylene glycol di(meth)acrylate, 1,3-butanediol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, 1,10-decanediol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, and dipentaerythritol hexa(meth)acrylate; Polyfunctional polyalkoxylene (meth)acrylates such as polyethylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, polytetramethylene glycol di(meth)acrylate, ethoxylated trimethylolpropane tri(meth)acrylate, propoxylated trimethylolpropane tri(meth)acrylate, and ethoxylated glycerin tri(meth)acrylate; polyfunctional (meth)acrylates having a hydroxy group such as 2-hydroxy-3-acryloyloxypropyl (meth)acrylate and pentaerythritol tri(meth)acrylate; polyfunctional (meth)acrylates having an ester skeleton such as hydroxypivalic acid neopentyl glycol di(meth)acrylate; and polyfunctional glycerin (meth)acrylates such as glycerin tri(meth)acrylate and ethoxylated glycerin tri(meth)acrylate.From the viewpoint of thermal decomposition property, polyfunctional alkyl(meth)acrylates having a linear or branched hydrocarbon skeleton are preferred, and from the viewpoint of crosslink density in particular, ethylene glycol di(meth)acrylate, 1,3-butanediol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, and dipentaerythritol hexa(meth)acrylate are more preferred. Monomer (a2) may be used alone or in combination of two or more.

[0016] The proportion of the structural unit (a2) in the resin is preferably 0 to 20% by mass, more preferably 0.01 to 20% by mass, even more preferably 0.1 to 10% by mass, particularly preferably 0.1 to 6% by mass, especially preferably 0.1 to 5.0% by mass, and most preferably 0.3 to 5.0% by mass, when the total of all structural units constituting the resin is taken as 100% by mass. If the proportion is equal to or greater than the lower limit, the thixotropy when the resin is dissolved in a solvent is further improved. If the proportion is equal to or less than the upper limit, the solvent solubility of the resin is further improved. If the proportion is within the above range, the resin will have an appropriate degree of crosslinking, resulting in good thixotropy and solvent solubility.

[0017] <Monomer (a3)> The monomer (a3) ​​is a monomer other than the monomer (a1) and the monomer (a2). The monomer (a3) ​​is not particularly limited as long as it is copolymerizable with at least the monomer (a1), and examples thereof include aromatic vinyl monomers such as styrene, α-methylstyrene, p-methylstyrene, vinyltoluene, and chlorostyrene; cyanide vinyl monomers such as acrylonitrile, methacrylonitrile, α-cyanoacrylate, dicyanovinylidene, and fumaronitrile; monomers having a carboxyl group such as crotonic acid, isocrotonic acid, cinnamic acid, itaconic acid, maleic acid, fumaric acid, citraconic acid, mesaconic acid, and glutaconic acid; monomers having a sulfonic acid group such as vinyl sulfonic acid and 2-acrylamido-2-methylpropanesulfonic acid; polyfunctional monomers such as divinylbenzene, divinylnaphthalene, and divinyl ether; vinyl monomers such as vinyl acetate and vinyl propionate; and conjugated diene monomers such as 1,3-butadiene, isoprene, 2-chloro-1,3-butadiene, and chloroprene. The monomer (a3) ​​may be used alone or in combination of two or more kinds.

[0018] The proportion of the structural unit (a3) ​​in the resin is preferably 0 to 15% by mass, and more preferably 0 to 9.5% by mass, when the total of all structural units constituting the resin is 100% by mass. If it is equal to or greater than the lower limit, the thixotropy of the resin when dissolved in a solvent is further improved. If it is equal to or less than the upper limit, the thermal decomposition property of the resin is further improved. If it is within the above range, the resin will have an appropriate degree of crosslinking, resulting in good thixotropy and thermal decomposition property of the resin.

[0019] <Mercaptan Having Two or More SH Groups> Mercaptans having two or more SH groups play the role of a chain transfer agent in the polymerization reaction. When producing a resin, by using a mercaptan having two or more SH groups as a chain transfer agent in the polymerization reaction, the mercaptan having two or more SH groups becomes the initiation point of polymerization, and a chemical structure (b1) derived from the mercaptan having two or more SH groups is introduced into the resin. In addition, by introducing the chemical structure (b1) derived from the mercaptan having two or more SH groups into the resin, a spherical resin with an introduced branched structure is obtained, and entanglement between side chains between resin particles is reduced. Therefore, even at high molecular weights, thixotropy is improved, and stringiness associated with entanglement between polymers can be improved.

[0020] Mercaptans having two or more SH groups are compounds having two or more mercapto groups in a single molecule. Examples of mercaptans having two or more SH groups include mercaptans having a linear or branched hydrocarbon skeleton, such as 1,2,3-trimercaptopropane, 2,2-bis(mercaptomethyl)-1-mercaptobutane, 1,2,3,4-tetramercaptobutane, and 2,2-bis(mercaptomethyl)-1,3-dimercaptopropane; mercaptans having a 3-mercaptopropionate structure, such as glycerin tris(3-mercaptopropionate), trimethylolpropane tris(3-mercaptopropionate), pentaerythritol tetrakis(3-mercaptopropionate), dipentaerythritol hexakis(3-mercaptopropionate), and tetraethylene glycol bis(3-mercaptopropionate); Mercaptans having a thioglycolate structure, such as glycerin tris(thioglycolate), trimethylolpropane tris(thioglycolate), pentaerythritol tetrakis(thioglycolate), dipentaerythritol hexakis(thioglycolate), and tetraethylene glycol bis(thioglycolate); Monomers having a 2-mercaptobutyrate structure, such as glycerin tris(2-mercaptobutyrate), trimethylolpropane tris(2-mercaptobutyrate), pentaerythritol tetrakis(2-mercaptobutyrate), dipentaerythritol hexakis(2-mercaptobutyrate), and tetraethylene glycol bis(2-mercaptobutyrate); Monomers having a 3-mercaptobutyrate structure, such as 1,4-bis(3-mercaptobutyryloxy)butane, glycerin tris(3-mercaptobutyrate), trimethylolpropane tris(3-mercaptobutyrate), pentaerythritol tetrakis(3-mercaptobutyrate), dipentaerythritol hexakis(3-mercaptobutyrate), and tetraethylene glycol bis(3-mercaptobutyrate); and monomers having an isocyanate structure, such as tris-[(3-mercaptopropionyloxy)-ethyl]-isocyanurate and tris-[(3-mercaptobutyloxy)-ethyl]-isocyanurate.From the viewpoint of reactivity, mercaptans having a 3-mercaptopropionate structure and mercaptans having a thioglycolate structure are preferred, and trimethylolpropane tris(3-mercaptopropionate), pentaerythritol tetrakis(3-mercaptopropionate), trimethylolpropane tris(thioglycolate), and pentaerythritol tetrakis(thioglycolate) are more preferred from the viewpoints of high reactivity and polymerization stability as chain transfer agents and easy availability. Mercaptans having two or more SH groups may be used alone or in combination of two or more.

[0021] The proportion of the structural unit (b1) in the resin is preferably 0.1 to 20 parts by mass, more preferably 0.5 to 10 parts by mass, and even more preferably 1 to 6 parts by mass, based on 100 parts by mass of the total of all structural units constituting the resin. If the proportion is equal to or greater than the lower limit, the thixotropy of the resin when dissolved in a solvent is further improved. If the proportion is equal to or less than the upper limit, the solvent solubility and thermal decomposition property of the resin are further improved.

[0022] <Mercaptan Having One SH Group> Mercaptan having one SH group plays the role of a chain transfer agent in the polymerization reaction. When a resin is produced, a mercaptan having one SH group is used as a chain transfer agent in the polymerization reaction in addition to a mercaptan having two or more SH groups, and the mercaptan having one SH group in addition to the mercaptan having two or more SH groups serves as the initiation point for polymerization, and a chemical structure (b2) derived from the mercaptan having one SH group is introduced into the resin.

[0023] A mercaptan having one SH group is a compound having one mercapto group in a single molecule. Examples of mercaptans having one SH group include n-octyl mercaptan, n-dodecyl mercaptan, t-dodecyl mercaptan, n-butyl mercaptan, thioglycolic acid, 3-mercaptopropionic acid, 2-mercaptoethanol, 2-ethylhexyl 3-mercaptopropionate, 2-ethylhexyl thioglycolate, isooctyl 3-mercaptopropionate, isooctyl thioglycolate, and 2-methoxybutyl 3-mercaptopropionate. N-octyl mercaptan, n-dodecyl mercaptan, and t-dodecyl mercaptan are preferred as chain transfer agents because they have high reactivity and polymerization stability and are easily available. A single type of mercaptan having one SH group may be used alone, or two or more types may be used in combination.

[0024] The proportion of the structural unit (b2) in the resin is preferably 0 to 20 parts by mass, more preferably 0 to 10 parts by mass, and even more preferably 0 to 6 parts by mass, relative to 100 parts by mass of the total of all structural units constituting the resin. When the proportion is equal to or less than the upper limit, the thermal decomposition properties of the resin are further improved.

[0025] <Physical Properties> The resin is preferably a sintering binder that is solid at room temperature. When the resin is a sintering binder that is solid at room temperature, the amount added can be easily adjusted when preparing the paste composition described below, making it easy to adjust the viscosity range. In addition, since a variety of solvent types can be selected, it is applicable to various blending compositions. The specific shape of the resin is not particularly limited, but examples include powder-like, plate-like, crushed piece-like, spherical, particulate, granular, and pellet-like solids. Among these, powder-like, crushed piece-like, spherical, particulate, and granular solids are preferred because they are easy to handle when dissolved in a solvent.

[0026] In view of good thermal decomposition properties, the resin of the present invention is preferably a binder for firing. Here, the term "binder for firing" means a material that is used by printing the paste composition of the present invention on a substrate and then heating and firing in a high-temperature furnace for the purpose of forming the electronic circuit of the electronic device of the present invention, the electrode of the solar panel of the present invention, the inorganic sintered body of the present invention, or an electromagnetic wave shielding material having the inorganic sintered body of the present invention.

[0027] The acid value (also referred to as solid acid value) of the resin is not particularly limited, but is preferably 0 to 50 mgKOH / g, more preferably 0 to 43 mgKOH / g, even more preferably 0 to 35 mgKOH / g, particularly preferably 0 to 15 mgKOH / g, and most preferably 1 to 19 mgKOH / g. If the acid value is equal to or less than the above upper limit, the thixotropy of the paste composition obtained using the resin is further improved. The above upper and lower limits can be arbitrarily combined. For example, the acid value may be 1 to 50 mgKOH / g, 1 to 43 mgKOH / g, 1 to 35 mgKOH / g, 1 to 15 mgKOH / g, or 0 to 19 mgKOH / g. The acid value of the resin is a value measured by neutralization titration using a potassium hydroxide (KOH) solution. Detailed measurement conditions are as described in the Examples below.

[0028] The mass average particle diameter of the resin is preferably greater than 100 μm and not greater than 1500 μm, more preferably 110 to 1000 μm, even more preferably 130 to 800 μm, particularly preferably 150 to 340 μm, and most preferably 170 to 280 μm. If the mass average particle diameter is greater than or equal to the lower limit, the risk of dust explosion is suppressed. If the mass average particle diameter is equal to or less than the upper limit, the solvent solubility of the resin is further improved. The above upper and lower limits can be combined in any manner. For example, it may be greater than 100 μm and less than 1000 μm, greater than 100 μm and less than 800 μm, greater than 100 μm and less than 340 μm, greater than 100 μm and less than 280 μm, 110 μm to 1000 μm, 110 μm to 800 μm, 110 μm to 340 μm, 110 μm to 280 μm, 130 μm to 1500 μm, 130 μm to 1000 μm, or 130 μm to 800 μm. The mass average particle size of the resin can be calculated by shaking 20 g of the resin for 5 minutes using a standard sieve and classifying it.

[0029] The thermal weight loss rate of the resin is preferably 95.0% or more, more preferably 99.0% or more, even more preferably 99.8% or more, and particularly preferably 99.9% or more. A higher thermal weight loss rate indicates better thermal decomposition properties. If the thermal weight loss rate is equal to or greater than the lower limit, the amount of impurities in the inorganic sintered body obtained using the resin is suppressed. The upper limit of the thermal weight loss rate of the resin is 100%. The thermal weight loss rate of the resin is determined under the following measurement conditions. That is, using a differential thermobalance (TG-DTA), 5 mg of a measurement sample is heated in a nitrogen atmosphere from a starting temperature of 30°C to 500°C at a rate of 10°C / min, and the mass of the residue when it reaches 450°C is measured, and the thermal weight loss rate is calculated using the following formula (1). Thermal weight loss rate (%) = {(mass (mg) of measured sample - mass (mg) of residue) / mass (mg) of measured sample} × 100 (1) As a method for adjusting the numerical value of the thermal weight loss rate of a resin, for example, the numerical value of the thermal weight loss rate can be reduced by setting the ratio of the structural unit (b1) to all structural units constituting the resin to 0.1 parts by mass or more, relative to a total of 100 parts by mass of all structural units constituting the resin. Furthermore, the numerical value of the thermal weight loss rate can be increased by setting the ratio of the structural unit (b1) to all structural units constituting the resin to 20 parts by mass or less, relative to a total of 100 parts by mass of all structural units constituting the resin.

[0030] The weight-average molecular weight (Mw) of the resin is preferably 10,000 to 1,000,000, more preferably 50,000 to 500,000, even more preferably 100,000 to 400,000, particularly preferably 150,000 to 350,000, and most preferably 200,000 to 300,000. If the Mw is equal to or greater than the lower limit, the thixotropy of the paste composition obtained using the resin is further improved. If the Mw is equal to or less than the upper limit, the solvent solubility of the resin is further improved.

[0031] The water content of the resin is preferably 0.01 to 10% by mass, more preferably 0.02 to 8.0% by mass, even more preferably 0.1 to 5.0% by mass, and particularly preferably 0.3 to 3.0% by mass, relative to the total mass of the resin. If the water content is equal to or greater than the lower limit, the risk of dust explosion is suppressed. If the water content is equal to or less than the upper limit, the paste composition obtained using the resin exhibits improved film uniformity during screen printing. Specific methods for measuring the water content of the resin are as described in the Examples below.

[0032] A resin solution with a resin concentration of 30% by mass obtained by dissolving a resin in terpineol, i.e., a resin solution containing 30% by mass of resin relative to the total mass of the resin solution, preferably satisfies the following formula (2): η1 / η1000≧1.5 (2) Here, η1 and η1000 are the viscosities (Pa s) of the resin solution measured using a viscoelasticity measuring device under conditions of a cone plate of 1.0° / 20 mm and a measurement temperature of 23°C, η1 is the viscosity (Pa s) at a shear rate of 1 (1 / s), and η1000 is the viscosity (Pa s) at a shear rate of 1000 (1 / s).

[0033] The η1 / η1000 is preferably 1.5 or greater, more preferably 2.0 or greater, and even more preferably 2.3 or greater. If the η1 / η1000 is equal to or greater than the lower limit, the thixotropy is further improved when the resin is dissolved in a solvent. As a result, the printability and leveling properties after printing are further improved when a paste composition obtained using the resin is screen-printed. The upper limit of the η1 / η1000 is not particularly limited, but it is preferable that the η1 / η1000 be 6.0 or less. For example, the η1 / η1000 may be 1.5 to 6.0, 2.0 to 6.0, or 2.3 to 6.0. The η1 / η1000 value can be increased, for example, by adjusting the ratio of the structural unit (b1) to all structural units constituting the resin to 0.1 parts by mass or greater per 100 parts by mass of the total of all structural units constituting the resin. Furthermore, the value of η1 / η1000 can be reduced by setting the ratio of the structural unit (b1) to all structural units constituting the resin to 20 parts by mass or less, relative to 100 parts by mass of the total of all structural units constituting the resin. The terpineol used in viscosity measurement is a mixture of α-terpineol, which is the main component, β-terpineol, and γ-terpineol. Commercially available terpineol can be used, and examples of commercially available products include "TERPINEOL PG" manufactured by Takasago International Corporation, "Terpineol C" manufactured by Nippon Terpene Chemical Co., Ltd., and "Terpineol" manufactured by Nippon Fragrance Pharmaceutical Co., Ltd.

[0034] The resin may be a homopolymer or copolymer of the monomer (a1). In particular, it is preferably a copolymer of the monomer (a1), the monomer (a2), and, if necessary, the monomer (a3). When the resin is a copolymer, the resin may have any structure, such as a random copolymer, a graft copolymer, or a block copolymer.

[0035] <Production Method> The resin can be produced by commonly known polymerization methods such as bulk polymerization, solution polymerization, suspension polymerization, etc., but is not limited to these polymerization methods. Among these, suspension polymerization is preferred because it can produce a resin in the form of spherical particles that are easy to handle. An example of a method for producing a resin by suspension polymerization will be described below. The resin production method of this embodiment preferably includes, in order, a suspension polymerization step, a first dehydration step, a washing step, a second dehydration step, and a drying step, as shown below.

[0036] (Suspension polymerization step) The suspension polymerization step is a step of dispersing the above-mentioned monomer (a1) or a monomer mixture (M1) containing the monomer (a1) and the monomer (a2), and optionally the monomer (a3), in water, and performing suspension polymerization in the presence of a mercaptan having two or more SH groups and, optionally, a mercaptan having one SH group, to obtain a resin. The content of the monomer (a1) relative to the total mass of the monomer mixture (M1) is preferably 70 to 100 mass%, more preferably 90 to 100 mass%, even more preferably 95 to 100 mass%, particularly preferably 97 to 100 mass%, and most preferably 99 to 100 mass%. The content of the monomer (a2) is preferably 0 to 20% by mass, more preferably 0.01 to 20% by mass, even more preferably 0.1 to 10% by mass, particularly preferably 0.1 to 6% by mass, particularly preferably 0.1 to 5% by mass, and most preferably 0.3 to 5% by mass, based on the total mass of the mixture (M2). The content of the monomer (a3) ​​is preferably 0 to 15% by mass, more preferably 0 to 9.5% by mass, based on the total mass of the mixture (M2).

[0037] Known methods can be used for suspension polymerization, such as polymerizing a monomer (a1) or a monomer mixture (M1) in a suspended state in water in the presence of a polymerization aid in a vessel having a polymerization temperature control function and a stirring function. Examples of the polymerization aid include a chain transfer agent, a radical polymerization initiator, a dispersant, and a dispersion aid. However, in this embodiment, at least the above-mentioned mercaptan having two or more SH groups is used as the chain transfer agent. By using a polymerization aid, specifically a mercaptan having two or more SH groups as a chain transfer agent, a resin having chemical structure (b1) can be obtained. By using a mercaptan having one SH group in addition to a mercaptan having two or more SH groups as a chain transfer agent, a resin having chemical structure (b2) can be obtained in addition to chemical structure (b1).

[0038] As the chain transfer agent, the above-mentioned mercaptan having two or more SH groups is used. Furthermore, as the chain transfer agent, in addition to the mercaptan having two or more SH groups, the above-mentioned mercaptan having one SH group may be used in combination. Furthermore, other chain transfer agents other than the mercaptan having one SH group and the mercaptan having two or more SH groups may be further used in combination. Examples of other chain transfer agents include hydrogen, diphenyl disulfide, dibenzyl disulfide, α-methylstyrene dimer, terpenoids, and cobalt chain transfer agents. One type of other chain transfer agent may be used alone, or two or more types may be used in combination.

[0039] The amount of the mercaptan having two or more SH groups used is preferably 0.1 to 20 parts by mass, more preferably 0.5 to 10 parts by mass, and even more preferably 1 to 6 parts by mass, relative to 100 parts by mass of the total of all the monomers used in the suspension polymerization. The amount of the mercaptan having one SH group used is preferably 0 to 20 parts by mass, more preferably 0 to 10 parts by mass, and even more preferably 0 to 6 parts by mass, relative to 100 parts by mass of the total of all the monomers used in the suspension polymerization.

[0040] The radical polymerization initiator is not particularly limited, and examples thereof include organic peroxides and azo compounds. Examples of organic peroxides include t-butyl peroxypivalate, o-methylbenzoyl peroxide, bis-3,5,5-trimethylhexanoyl peroxide, octanoyl peroxide, cyclohexanone peroxide, benzoyl peroxide, methyl ethyl ketone peroxide, dicumyl peroxide, lauroyl peroxide, diisopropylbenzene hydroperoxide, t-butyl hydroperoxide, di-t-butyl peroxide, t-butylperoxy-2-ethylhexanoate, and 1,1,3,3-tetramethylbutylperoxy-2-ethylhexanoate. Examples of azo compounds include 2,2'-azobisisobutyronitrile, 2,2'-azobis(2-methylbutyronitrile), 2,2'-azobis(2,4-dimethylvaleronitrile), and 2,2'-azobis(2,4-dimethyl-4-methoxyvaleronitrile). From the viewpoint of the polymerizability of the monomer, benzoyl peroxide, lauroyl peroxide, 1,1,3,3-tetramethylbutylperoxy-2-ethylhexanoate, 2,2'-azobisisobutyronitrile, 2,2'-azobis(2,4-dimethylvaleronitrile), and 2,2'-azobis(2,4-dimethylvaleronitrile) are preferred. One type of radical polymerization initiator may be used alone, or two or more types may be used in combination. The amount of radical polymerization initiator used is not particularly limited, but from the viewpoint of improving the polymerization rate of the monomers, it is preferably 0.0001 to 10 parts by mass per 100 parts by mass of the total of all the monomers used in suspension polymerization.

[0041] The dispersant is not particularly limited, but examples thereof include surfactants that stably disperse monomers in water, and specific examples thereof include copolymers of sodium methacrylate and methacrylic acid, polyvinyl alcohol, polyvinylpyrrolidone, hydroxyethyl cellulose, and hydroxypropyl cellulose. One type of dispersant may be used alone, or two or more types may be used in combination.

[0042] The dispersing aid is not particularly limited, and examples thereof include sodium sulfate, sodium carbonate, sodium dihydrogen phosphate, disodium hydrogen phosphate, potassium chloride, calcium acetate, magnesium sulfate, and manganese sulfate. One type of dispersing aid may be used alone, or two or more types may be used in combination.

[0043] Resins obtained by suspension polymerization are obtained in the form of a slurry, which is then dehydrated to yield resin particles that are usually in the form of beads that are nearly spherical.

[0044] (Dehydration Step) Examples of the dehydration step include a first dehydration step in which the slurry after suspension polymerization is dehydrated using a dehydrator or the like to separate the resin from the reaction liquid, and a second dehydration step in which the resin after the washing step described below is dehydrated using a dehydrator or the like to separate the resin in the form of resin particles from the washing liquid.

[0045] Various types of dehydrators can be used in each dehydration step, and can be appropriately selected from, for example, dehydrators with a filtering mechanism using a filter cloth or the like, centrifugal dehydrators, dehydrators with a mechanism for suctioning and removing water on a porous belt, etc. One dehydrator may be used, or two of the same model may be prepared and used for each dehydration step, or multiple dehydrators of different models may be used. A model can be appropriately selected according to the purpose from the perspectives of product quality, capital investment costs, productivity, operating costs, etc. When emphasis is placed on the balance between product quality and production speed, a dedicated dehydrator may be used for each dehydration step.

[0046] (Washing step) The washing step is a step of washing the resin obtained in the first dehydration step. The purity of the resin is increased by the washing step. Examples of methods for washing the resin include a method in which a washing liquid is added to the resin particles dehydrated in the first dehydration step, the particles are re-slurried, and then stirred and mixed, and a method in which the first dehydration step is performed in a dehydrator with a washing function, and then a washing liquid is added to wash the resin. Furthermore, these washing methods may be combined to wash the resin.

[0047] The type and amount of the cleaning liquid may be selected so as to achieve the purpose of the cleaning step. Examples of the cleaning liquid include water such as ion-exchanged water, distilled water, and purified water; an aqueous solution containing a sodium salt; and alcohol such as methanol. One type of cleaning liquid may be used alone, or two or more types may be used in combination.

[0048] (Drying step) The drying step is a step of drying the resin particles (resin particles) obtained by the second dehydration step. Water remains on the surface of the resin particles after the second dehydration step. When the inside of the resin is in a state close to saturated water absorption, it is preferable to dry the resin in order to further reduce the water content of the resin from the viewpoint of improving the purity of the resin.

[0049] Various dryers can be used to dry the resin, including, for example, a dryer that dries by heating under reduced pressure, a dryer that dries resin particles while air-transporting them through a pipe using heated air, and a dryer that blows heated air into the lower side of a perforated plate and dries the resin particles above while causing them to flow. The drying step is preferably carried out so that the moisture content of the resin, which is the resin particles after the drying step, is 0.01 to 10% by mass relative to the total mass of the resin.

[0050] <Effects> The resin of this embodiment described above is solid and contains the structural unit (a1), and therefore has excellent solvent solubility and thermal decomposition properties. Furthermore, the resin contains the chemical structure (b1) in addition to the structural unit (a1), and therefore has high thixotropy. The reason why a resin has high thixotropy due to the chemical structure (b1) is unclear, but it is thought to be as follows. The chemical structure (b1) allows the resin to have a large number of branched structures rather than a linear structure. Generally, the greater the amount of resin in a resin solution, the more thixotropy is exhibited. However, when the resin has a linear structure, thickening proceeds, making it difficult to increase the amount of high-molecular-weight resin added. On the other hand, when a resin has a branched structure, the chain length is shorter than when it has a linear structure, making it possible to suppress thickening and increase the amount of high-molecular-weight resin added. Therefore, it is believed that the resin has high thixotropy due to the chemical structure (b1).

[0051] In particular, if the resin further contains the structural unit (a2) in addition to the structural unit (a1) and the chemical structure (b1), the thixotropy of the binder resin when dissolved in a solvent is improved.Furthermore, if the resin further contains the chemical structure (b2) in addition to the structural unit (a1) and the chemical structure (b1), the viscosity increase of the resin when dissolved in a solvent is suppressed.

[0052] <Uses> The resin can be used, for example, as a raw material for internal electrode layers or external electrode layers of multilayer electronic components such as electronic devices, solar panels, and multilayer ceramic capacitors, and as a paste raw material for solar cell electrodes.

[0053] [Paste Composition] One embodiment of the paste composition of the present invention will be described below. The paste composition of this embodiment contains the resin of the present invention described above, a metal or inorganic compound, and an organic solvent. The paste composition may further contain components other than the resin, the metal or inorganic compound, and the organic solvent (hereinafter also referred to as "optional components"), as necessary, within a range that does not impair the effects of the present invention.

[0054] The resin content is preferably 0.1 to 20% by mass, more preferably 1 to 10% by mass, based on the total mass of the paste composition. If the resin content is equal to or greater than the lower limit, the moldability of the paste composition is improved. If the resin content is equal to or less than the upper limit, the solid content concentration of components other than the resin in the paste composition can be increased.

[0055] The metal or inorganic compound is not particularly limited, but examples thereof include oxides such as alumina, zirconia, titanium oxide, barium titanate, and calcium oxide; nitrides such as alumina nitride, silicon nitride, and boron nitride; metals such as copper, silver, and nickel; silica-based powders such as low-melting-point glass powder; carbon-based powders such as carbon black; and various phosphors. One type of metal or inorganic compound may be used alone, or two or more types may be used in combination.

[0056] The content of the metal or inorganic compound is preferably 40 to 90 mass % relative to the total mass of the paste composition. If the content is equal to or greater than the lower limit, the molding efficiency of the paste composition is improved. If the content is equal to or less than the upper limit, the moldability of the paste composition is improved.

[0057] The organic solvent is not particularly limited, but an organic solvent having a boiling point of 180°C or higher is preferred, and an organic solvent having a boiling point of 200°C or higher is more preferred. If the boiling point of the organic solvent is equal to or higher than the above lower limit, unevenness in drying of the coating film during screen printing is reduced. There is no particular limit to the upper limit of the boiling point of the organic solvent, but for example, the boiling point of the organic solvent is preferably 400°C or lower. For example, the boiling point of the organic solvent may be 180 to 400°C, or 200 to 400°C.

[0058] Examples of organic solvents having a boiling point of 180° C. or higher include α,β,γ-terpineol, terpineol acetate, dihydroterpineol, dihydroterpineol acetate, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether acetate, diethylene glycol monobutyl ether, diethylene glycol monobutyl ether acetate, diethylene glycol monoisobutyl ether, 2,2,4-trimethyl-1,3-pentanediol monoisobutyrate, and isophorone. , benzyl alcohol, 1-octanol, 1-nonaol, 2-ethyl-1-hexanol, 1-decanol, 1-undecanol, 1,2-ethanediol, 1,2-propanediol, 1,3-propanediol, 1,2-butanediol, 1,3-butanediol, 1,4-butanediol, 1,5-pentanediol, Texanol, butyl lactate, dioctyl phthalate, dioctyl adipate, phenylpropylene glycol, cresol, dimethyl sulfoxide, and N-methylpyrrolidone. More preferred organic solvents are α,β,γ-terpineol, terpineol acetate, dihydroterpineol, dihydroterpineol acetate, diethylene glycol monoethyl ether acetate, diethylene glycol monobutyl ether, diethylene glycol monobutyl ether acetate, diethylene glycol monoisobutyl ether, and 2,2,4-trimethyl-1,3-pentanediol monoisobutyrate, as they have a boiling point of 200°C or higher and are widely used.

[0059] The content of the organic solvent is preferably 9.9 to 50 mass % relative to the total mass of the paste composition. If the content is equal to or greater than the lower limit, the moldability of the paste composition is improved. If the content is equal to or less than the upper limit, the solid content concentration of the paste composition is improved.

[0060] Examples of optional components include plasticizers, dispersing aids, antifoaming agents, resins other than the resin of the present invention, etc. One type of optional component may be used alone, or two or more types may be used in combination.

[0061] The paste composition can be obtained by mixing, for example, a resin, an inorganic compound, an organic solvent, and, if necessary, optional components.

[0062] The paste composition of the present embodiment described above contains the resin of the present invention, and therefore has high thixotropy, and is excellent in both printability when the paste composition is screen printed and leveling property after printing.

[0063] Since the paste composition of this embodiment has excellent printability in screen printing, it is preferable to use screen printing when forming a pattern on a substrate using the paste composition of this embodiment, but methods other than screen printing may also be used. For example, when the viscosity of the paste composition is high, dip coating or dispense coating can be used, and when the viscosity is low, doctor blade coating or cast coating can be used. The substrate on which the paste composition is printed or coated is not particularly limited, but examples include ceramic substrates and capacitors.

[0064] [Inorganic Sintered Body] One embodiment of the inorganic sintered body of the present invention will be described below. The inorganic sintered body of this embodiment is obtained by firing the paste composition of the present invention described above. The firing method is not particularly limited, but an example is a method in which a substrate on which the paste composition has been printed or coated is placed in a high-temperature atmosphere. During the firing process, organic substances such as resins contained in the paste composition are decomposed and removed, and metals or inorganic compounds contained in the paste composition are melted and sintered, thereby obtaining an inorganic sintered body. The firing temperature can be determined appropriately depending on the melting temperature of the substrate, the type of inorganic powder, and the organic substance contained in the paste composition, but is usually about 200 to 1500°C, preferably 300 to 1000°C.

[0065] From the viewpoint of current collection performance, the electronic device of the present invention preferably includes the inorganic sintered body. Examples of the electronic device include semiconductors such as logic circuits, memory circuits, and analog circuits, lithium ion batteries, capacitors, printed circuits, and current collection circuits of solar panels. From the viewpoint of photovoltaic power generation, the solar panel of the present invention preferably includes the inorganic sintered body.

[0066] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited thereto. Various measurement and evaluation methods in the following examples and comparative examples are as follows. In the following description, "parts" means parts by mass and "%" means % by mass unless otherwise specified.

[0067] [Measurement and Evaluation Methods] <Measurement of Mass Average Particle Diameter> The mass average particle diameter was measured by shaking and classifying 20 g of granular resin using a standard sieve for 5 minutes.

[0068] <Measurement of Moisture Content> The moisture content of the granular resin immediately after drying the resin at 105° C. for 2 hours was set to 0%, and the moisture content was calculated from the loss on drying of the mass of the resin before and after drying.

[0069] <Measurement of Weight-Average Molecular Weight (Mw) and Number-Average Molecular Weight (Mn)> The weight-average molecular weight (Mw) and number-average molecular weight (Mn) of the resin were measured by gel permeation chromatography (GPC) and calculated as polystyrene equivalent values ​​using a standard polystyrene calibration curve. To eliminate the influence of unreacted substances, the lower limit of the molecular weight was set to 300. The GPC measurement conditions were as follows. (GPC Measurement Conditions) Apparatus: Tosoh Corporation, product name "HLC-8220GPC". Column: Two Tosoh Corporation, product name "TSKgel Super HZM-H (4.6 mmφ x 150 mm)" columns connected in series. Eluent: Tetrahydrofuran. Sample concentration: 0.27% by mass. Measurement temperature: 40°C. Injection volume: 10 μL. Flow rate: 0.5 mL / min. Detector: RI (built into the device), UV (product name "UV-8220" manufactured by Tosoh Corporation).

[0070] <Measurement of Acid Value> Approximately 0.5 g of resin was accurately weighed into a beaker (α(g)), and 50 mL of a mixed solution of toluene and ethanol (mass ratio 1:1) was added. A few drops of phenolphthalein were added, and neutralization titration was performed with a 0.05 N KOH solution (solvent: ethanol). (Titer amount = β(mL), titer of KOH solution = f). A blank measurement was also performed in the same manner (titer amount = γ(mL)), and the solid acid value was calculated according to the following formula (3): Acid value (mgKOH / g) = {(β - γ) × 0.05 × 56.11 × f} / α (3)

[0071] <Evaluation of Solvent Solubility> 14 g of terpineol (manufactured by Takasago International Corporation, trade name "TERPINEOL PG") was placed into a glass bottle (manufactured by Kakuyo Glass Co., Ltd., trade name "Standard Bottle No. 6") together with a stirrer, and 6 g of resin was added while stirring, and the bottle was capped. The temperature was then maintained at 50°C using a water bath, and the mixture was stirred at 500 rpm using a stirrer for 2 hours. The mixture was then cooled to room temperature to prepare a resin solution containing 30% by mass of resin. The appearance of the obtained resin solution was visually observed, and the solvent solubility was evaluated according to the following evaluation criteria. A: There was no residual dissolution or gelation, and the resin solution was colorless and transparent. B: Although the resin solution was transparent, gelation or the generation of insoluble matter was observed. C: The resin solution was cloudy or resin precipitation was observed.

[0072] <Evaluation of Thermal Decomposition Property> Using a differential thermobalance (TG-DTA) (manufactured by Rigaku Corporation, product name "Thermo plus EVO"), 5 mg of a measurement sample was heated in a nitrogen atmosphere from an initial temperature of 30°C to 500°C at a rate of 10°C / min. The mass of the residue when the temperature reached 450°C was measured, and the thermal weight loss rate (%) was calculated using the following formula (1). A higher value of the thermal weight loss rate indicates better thermal decomposition property. Thermal weight loss rate (%) = {(mass (mg) of measurement sample - mass (mg) of residue) / mass (mg) of measurement sample} × 100 ... (1)

[0073] <Evaluation of Thixotropy> A resin solution containing 30% by mass of resin was prepared in the same manner as in the evaluation of solvent solubility. Using a viscoelasticity measuring device (manufactured by Thermo Fisher Scientific, product name "HAAKE MARS"), the viscosity (Pa s) of the resin solution was measured under conditions of a cone plate of 1.0° / 20 mm and a measurement temperature of 23°C. The viscosity (Pa s) of the resin solution at a shear rate of 1 (1 / s) was defined as η1, and the viscosity (Pa s) at a shear rate of 1000 (1 / s) was defined as η1000. The solvent solubility was evaluated according to the following evaluation criteria. A: The value of η1 / η1000 is 2.3 or more. B: The value of η1 / η1000 is 2.0 or more and less than 2.3. C: The value of η1 / η1000 is 1.5 or more and less than 2.0. D: The value of η1 / η1000 is less than 1.5. E: Unmeasurable

[0074] Example 1 In a polymerization apparatus equipped with a stirrer, a condenser, and a thermometer, a monomer mixture in which 97.4 parts of i-butyl methacrylate and 2.6 parts of trimethylolpropane triacrylate were uniformly dissolved, 1.9 parts of pentaerythritol tetrakis(thioglycolate), 1.9 parts of n-octyl mercaptan, and 1.9 parts of n-dodecyl mercaptan were added and stirred until uniform. 0.3 parts of 2,2'-azobis(2-methylbutyronitrile) was then added and stirred until uniform. A homogeneous mixture of 145 parts of pure water, 0.15 parts of sodium sulfate, and 0.025 parts by mass of a copolymer of sodium methacrylate and methacrylic acid as a dispersant was then added, and the mixture was purged with nitrogen while stirring. Thereafter, the temperature in the flask was controlled to 80°C to initiate suspension polymerization. After detecting the peak of the polymerization exotherm, the mixture was kept at 85°C for 60 minutes, and then the reaction solution was cooled to 40°C or below to obtain a suspension containing a resin. The resulting suspension was filtered through a filter cloth, and the filtrate was washed with deionized water, dehydrated, and dried at 40°C for 16 hours to obtain a particulate solid resin (A1). The mass average particle size, water content, weight average molecular weight, and acid value of the resulting resin (A1) were measured, and the solvent solubility, thermal decomposition property, and thixotropy were evaluated. The results are shown in Table 1.

[0075] Examples 2 to 8, Comparative Examples 1 to 3 Resins (A2) to (A11) were produced in the same manner as in Example 1, except for using the formulations shown in Table 1, and various measurements and evaluations were carried out. The results are shown in Table 1.

[0076]

[0077] The abbreviations in Table 1 have the following meanings: A blank cell in the table means that the component is not blended (amount blended: 0 parts). IBMA: i-butyl methacrylate (manufactured by Mitsubishi Chemical Corporation, trade name "Acryester IB") MMA: methyl methacrylate (manufactured by Mitsubishi Chemical Corporation, trade name "Acryester M") MAA: methacrylic acid (manufactured by Mitsubishi Chemical Corporation, trade name "methacrylic acid") TMPTA: trimethylolpropane triacrylate (manufactured by Shin-Nakamura Chemical Co., Ltd., trade name "A-TMPT") PETG: pentaerythritol tetrakis(thioglycolate) (manufactured by Yodo Chemical Co., Ltd., trade name "pentaerythritol tetrakisthioglycolate (PETG)") PEMP: pentaerythritol tetrakis(3-mercaptopropionate) (manufactured by SC Organic Chemical Co., Ltd., trade name "PEMP") nDM: n-dodecyl mercaptan (manufactured by Chevron Phillips Chemical Co., Ltd., trade name "n-DM") nOM: n-octyl mercaptan (manufactured by Arkema Inc., trade name "n-OM") AMBN: 2,2'-azobis(2-methylbutyronitrile) (manufactured by Otsuka Chemical Co., Ltd., trade name "AMBN")

[0078] As is clear from Table 1, it was confirmed that the resins (A1) to (A8) obtained in Examples 1 to 8 all exhibited excellent solvent solubility, thermal decomposition, and thixotropy. On the other hand, the resins (A9) and (A10) obtained in Comparative Examples 1 and 2 lacked the chemical structure (b1) derived from a difunctional or higher mercaptan, and therefore exhibited poor thixotropy. Note that the resin in Comparative Example 2 was unable to be measured due to significant gelation. Because of the gelation, the thixotropy rating was E, and the weight-average molecular weight (Mw) and Mw / Mn could not be measured. The resin (A11) obtained in Comparative Example 3 had poor thixotropy because the ratio Mw / Mn of the weight-average molecular weight (Mw) to the number-average molecular weight (Mn) was outside the range specified in the present application.

[0079] The resin of the present invention has excellent solvent solubility, thermal decomposition properties, and high thixotropy, and therefore has excellent screen printability and leveling properties after printing. The resin of the present invention can be used, for example, as a raw material for internal electrode layers or external electrodes of multilayer electronic components such as electronic devices, solar panels, and multilayer ceramic capacitors, and as a paste raw material for solar cell electrodes, and is therefore extremely important from an industrial perspective.

Claims

1. A resin having a structural unit derived from a (meth)acrylic acid ester and a chemical structure derived from a mercaptan having two or more SH groups, and having a ratio Mw / Mn of weight average molecular weight (Mw) to number average molecular weight (Mn) of 5.0 or more.

2. The resin of claim 1, wherein said resin is a solid sintered binder.

3. The resin according to claim 1 or 2, having a mass average particle diameter of more than 100 μm and not more than 1,500 μm.

4. The resin according to claim 1 or 2, having an acid value of 0 to 50 mg KOH / g.

5. The resin according to claim 1 or 2, further having a chemical structure derived from a mercaptan having one SH group.

6. The resin according to claim 1 or 2, further comprising a structural unit derived from a monomer having two or more polymerizable double bonds.

7. The resin according to claim 6, wherein the content of the constituent units derived from the monomer having two or more polymerizable double bonds is 0.1 to 5.0 mass % based on the total monomer-derived constituent units of the resin.

8. The resin according to claim 1 or 2, wherein the thermal weight loss rate determined under the following measurement conditions is 95.0% or more. <Measurement conditions for thermal weight loss rate> Using a differential thermobalance (TG-DTA), 5 mg of a measurement sample is heated in a nitrogen atmosphere from a starting temperature of 30°C to 500°C at a rate of 10°C / min, the mass of the residue when the temperature reaches 450°C is measured, and the thermal weight loss rate is calculated according to the following formula (1): Thermal weight loss rate (%) = {(mass (mg) of measurement sample - mass (mg) of residue) / mass (mg) of measurement sample} x 100 ... (1) 9. The resin according to claim 1 or 2, wherein a resin solution containing 30% by mass of the resin, obtained by dissolving the resin in terpineol, satisfies the following formula (2): η1 / η1000≧1.5 ... (2) Here, η1 and η1000 are the viscosities (Pa·s) of the resin solution measured using a viscoelasticity measuring device under conditions of a cone plate of 1.0° / 20 mm and a measurement temperature of 23° C., η1 is the viscosity (Pa·s) at a shear rate of 1 (1 / s), and η1000 is the viscosity (Pa·s) at a shear rate of 1000 (1 / s).

10. The resin according to claim 1 or 2, having a weight average molecular weight of 10,000 to 1,000,000.

11. The resin according to claim 1 or 2, having a water content of 0.01 to 10% by weight based on the total weight of the resin.

12. A paste composition comprising the resin according to claim 1 or 2, a metal or inorganic compound, and an organic solvent.

13. The paste composition according to claim 12, wherein the boiling point of the organic solvent is 180° C. or higher.

14. An inorganic sintered body obtained by firing the paste composition according to claim 13.

15. An electronic device comprising the inorganic sintered body according to claim 14.

16. A solar panel comprising the inorganic sintered body according to claim 14.

Citation Information

Patent Citations

  • Polymer electrolyte and lithium ion battery

    CN110943249A

  • New block polymer and its production

    JP1995179538A

  • Hot melt resin composition

    JP1996199141A

  • Adhesive composition

    JP1997053059A

  • Adhesive, its production and adhesive cloth

    JP1997241610A

Cited By

  • Slurry composition for electrode for multilayer ceramic capacitor, electrode layer for multilayer ceramic capacitor, and multilayer ceramic capacitor

    WO2026100706A1