Ar device

The laminate structure in AR devices, featuring a light guide plate and low refractive index layer with specific thickness and refractive index, addresses issues of light leakage and color unevenness, achieving transparency and thinness while enhancing durability.

WO2024203072A1PCT designated stage expired Publication Date: 2024-10-03NITTO DENKO CORP
View PDF 13 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/008520
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-06
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

AR devices with an air layer between the light guide plate and optical plate are prone to damage from external forces and suffer from light leakage when exposed to water or dirt, while eliminating the air layer to prevent damage results in thicker designs and color unevenness due to interference between the light guide plate and low refractive index layers.

Method used

A laminate structure comprising a light guide plate and a low refractive index layer with a refractive index of 1.25 or less, and a thickness between 1.5 μm and 10 μm, disposed on both sides of the light guide plate, along with an adhesive and base material layer, to suppress light leakage and color unevenness, maintaining transparency and thinness.

Benefits of technology

The laminate structure effectively prevents light leakage, suppresses color unevenness, and maintains excellent transparency and thinness, ensuring the AR device's optical performance and durability without the need for an air layer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024008520_03102024_PF_FP_ABST
    Figure JP2024008520_03102024_PF_FP_ABST
Patent Text Reader

Abstract

This AR device comprises a laminate (1), and the laminate (1) has a light guide plate (2) and a low-refractive-index layer (3) disposed on at least one side of the light guide plate (2) in the thickness direction. Further, the refractive index of the low-refractive-index layer (3) is 1.25 or less, and the thickness of the low-refractive-index layer (3) is 1.5-10 μm.
Need to check novelty before this filing date? Find Prior Art

Description

AR device

[0001] The present invention relates to an AR device.

[0002] In recent years, AR (Augmented Reality) technology has been attracting attention, and development of AR devices (for example, AR glasses and head-mounted displays) used in AR has been progressing.

[0003] One such AR device known is AR glasses that include an image generating device and a lens portion. Specifically, light emitted from the image generating device is incident on a light guide plate provided in the lens portion, where it is repeatedly totally reflected and emitted toward the user's eyes, thereby displaying an image. Typically, the lens portion is provided with an optical plate (e.g., transparent glass) that protects the light guide plate to prevent damage to the light guide plate. Furthermore, because the light incident on the light guide plate needs to be totally reflected in the lens portion, it has been proposed to form an air layer between the light guide plate and the optical plate (see, for example, Patent Document 1 below).

[0004] JP 2011-221129 A

[0005] However, in an AR device that includes an air layer between the light guide plate and the optical plate, as in Patent Document 1, if an external force is applied directly to the optical plate, the light guide plate may be damaged. On the other hand, while such damage can be prevented by increasing the thickness of the air layer, this has the disadvantage of making the lens portion thicker.

[0006] Furthermore, in an AR device such as that disclosed in Patent Document 1, which includes an air layer between the light guide plate and the optical plate, there is a problem in that light leakage occurs when water or dirt adheres to the light guide plate.

[0007] Therefore, it has been considered to solve the above-mentioned problems by using a laminate having a light guide plate and a low refractive index layer without an air layer in the lens portion.

[0008] However, in such a laminate, the light reflected by the light guide plate and the light reflected by the low refractive index layer interfere with each other, causing color unevenness on the surface of the laminate and resulting in poor transparency.

[0009] The present invention provides an AR device that can be made thin, can suppress light leakage from a light guide plate, can suppress color unevenness on the surface, and has a laminate with excellent transparency.

[0010] The present invention [1] includes an AR device comprising a laminate having a light guide plate and a low refractive index layer disposed on at least one side of the light guide plate in a thickness direction, wherein the refractive index of the low refractive index layer is 1.25 or less, and the thickness of the low refractive index layer is 1.5 μm or more and 10 μm or less.

[0011] The present invention [2] includes the AR device according to the above [1], wherein the standard deviation in thickness of the low refractive index layer is 10% or less.

[0012] The present invention [3] includes the AR device according to the above [1] or [2], wherein the thickness of the light guide plate is 0.3 mm or more and 5 mm or less.

[0013] The present invention [4] includes the AR device according to any one of the above [1] to [3], which includes a laminate further having a pressure-sensitive adhesive layer disposed on at least one side of the light guide plate in the thickness direction.

[0014] The present invention [5] includes the AR device according to any one of the above [1] to [4], which includes a laminate further having a base material layer arranged on at least one side of the light guide plate in the thickness direction.

[0015] The present invention [6] includes the AR device according to any one of [1] to [5] above, in which, in the following color unevenness evaluation test, no color unevenness is visually observed on the surface of the laminate when observed from a 0° position on one side of the thickness direction of the laminate. [Color Unevenness Evaluation Test] A 100 mm x 100 mm laminate is placed flat and visually observed from a 0° position on one side of the thickness direction of the laminate (a position at the center of the laminate, perpendicular to the surface direction), and a photograph is taken from the same position. The visual observation and the photograph are checked to evaluate the presence or absence of color unevenness.

[0016] The AR device of the present invention includes a laminate having a light guide plate and a low-refractive index layer disposed on at least one side of the light guide plate in the thickness direction. The refractive index of the low-refractive index layer is 1.25 or less, and the thickness of the low-refractive index layer is 1.5 μm or more and 10 μm or less. Since the laminate does not include an air layer, the AR device of the present invention can be made thin and light leakage from the light guide plate can be suppressed. Furthermore, since the low-refractive index layer has a specific thickness, color unevenness on the surface can be suppressed, and the device has excellent transparency.

[0017] FIG. 1 shows an overall configuration diagram of one embodiment of an AR device of the present invention. FIG. 2 shows a cross-sectional view of a first embodiment of a laminate included in the AR device shown in FIG. 1. FIG. 3 is a schematic view showing one embodiment of a method for manufacturing a laminate included in the AR device shown in FIG. 1. FIG. 3A shows a first step of preparing a light guide plate. FIG. 3B shows a step of arranging a low refractive index layer on one thickness-wise surface of the light guide plate. FIG. 3C shows a second step of arranging an adhesive layer on one thickness-wise surface of the low refractive index layer. FIG. 3D shows a step of arranging a base layer on one thickness-wise surface of the adhesive layer. FIG. 4 shows a cross-sectional view of a second embodiment of a laminate included in the AR device shown in FIG. 1. FIG. 5 shows a cross-sectional view of a third embodiment of a laminate included in the AR device shown in FIG. 1.

[0018] Referring to FIG. 1, one embodiment of the AR device of the present invention will be described.

[0019] <AR Device> An example of the AR device 10 is AR glasses.

[0020] As shown in FIG. 1, an AR device 10 (AR glasses) includes a lens portion 11, and also includes, for example, an image generating device 12 and a wearing portion 13.

[0021] The lens portion 11 includes a laminate 1, which will be described later.

[0022] The mechanism of the AR device 10 is, for example, to display an image by making light emitted from the image generating device 12 enter the lens portion 11, causing it to be totally reflected by the light guide plate of the lens portion 11, and then emitting it toward the user's eyes.

[0023] Next, a first embodiment of the laminate 1 included in the AR device 10 will be described with reference to FIG.

[0024] 2, the up-down direction of the paper surface is the up-down direction (thickness direction, first direction), the upper side of the paper surface is the upper side (one side in the thickness direction, one side in the first direction), and the lower side of the paper surface is the lower side (the other side in the thickness direction, the other side in the first direction). In addition, the left-right direction and the depth direction of the paper surface are surface directions perpendicular to the up-down direction.

[0025] <Laminate> As shown in FIG. 2, the laminate 1 extends in a plane direction perpendicular to the thickness direction, and has a flat upper surface (one surface in the thickness direction) and a flat lower surface (the other surface in the thickness direction).

[0026] 2 , the laminate 1 of the first embodiment has a light guide plate 2, and a low refractive index layer 3, a pressure-sensitive adhesive layer 4, and a base layer 5, which are arranged on one and the other thickness-wise sides of the light guide plate 2. Specifically, the laminate 1 has the light guide plate 2, and on one thickness-wise side of the light guide plate 2, the low refractive index layer 3, the pressure-sensitive adhesive layer 4, and the base layer 5, which are arranged in this order toward one thickness-wise side, and further has the low refractive index layer 3, the pressure-sensitive adhesive layer 4, and the base layer 5, which are arranged in this order toward the other thickness-wise side of the light guide plate 2.

[0027] In other words, since the laminate 1 does not have an air layer, it can be made thin, and further, since the low refractive index layer 3 is arranged on one thickness-wise surface and the other thickness-wise surface of the light guide plate 2, it is possible to prevent water or dirt from adhering to the light guide plate 2 and to prevent light leakage from the light guide plate 2.

[0028] The total light transmittance of the laminate 1 is, for example, 60% or more, preferably 70% or more, more preferably 80% or more, and even more preferably 90% or more, and for example, 99% or less, preferably 98% or less, and more preferably 97% or less.

[0029] When the total light transmittance of the laminate 1 is within the above range, the laminate 1 has excellent transparency.

[0030] The haze of the laminate 1 is, for example, 0.1% or more, preferably 0.2% or more, more preferably 0.3% or more, and for example, 3% or less, preferably 2.5% or less, more preferably 2% or less.

[0031] When the haze of the laminate 1 is within the above range, the laminate 1 has excellent transparency.

[0032] The thickness of the laminate 1 is, for example, 4.8 mm or less, preferably 3.8 mm or less, more preferably 2.8 mm or less, and for example, 0.35 mm or more, preferably 0.55 mm or more, more preferably 0.75 mm or more.

[0033] When the thickness of the laminate 1 is equal to or less than the upper limit, it can be made thinner. When the thickness of the laminate 1 is equal to or greater than the lower limit, it has sufficient strength.

[0034] [Light Guide Plate] The light guide plate 2 is configured so that incident light undergoes repeated total reflections, propagates, and is emitted in a predetermined direction at a predetermined position. Specifically, in the AR device 10, light emitted from the image generation device 12 enters the lens portion 11. The light that enters the lens portion 11 propagates, undergoing repeated total reflections within the light guide plate 2, and is emitted toward the user's pupil. As a result, the image from the image generation device 12 is visually recognized by the user of the AR device 10.

[0035] Examples of materials for the light guide plate 2 include transparent glass and plastic.

[0036] The refractive index of the light guide plate 2 is, for example, 1.4 or more, preferably 1.6 or more, more preferably 1.8 or more, even more preferably 2.0 or more, and for example, 2.5 or less, preferably 2.4 or less, more preferably 2.3 or less.

[0037] If the refractive index of the light guide plate 2 is within the above range, light can be efficiently incident from the image generating device 12 and emitted to the user's pupil, and further, the light incident within the light guide plate 2 can be reliably totally reflected.

[0038] The Abbe number of the light guide plate 2 is in the range of, for example, 10 or more, or preferably 15 or more, and for example, 80 or less, or preferably 70 or less.

[0039] The total thickness variation (TTV) on one surface and the other surface in the thickness direction of the light guide plate 2 is, for example, 5 μm or less, preferably 3 μm or less, and more preferably 1 μm or less. The smaller the thickness variation, the better.

[0040] If the thickness variation of the light guide plate 2 is equal to or less than the above upper limit, distortion of the optical path within the light guide plate 2 can be reduced.

[0041] The thickness unevenness can be measured using a reflective interference film thickness meter (Optical NanoGauge Film Thickness Meter, manufactured by Hamamatsu Photonics KK).

[0042] The surface roughness Ra of the light guide plate 2 on one surface in the thickness direction and on the other surface in the thickness direction is, for example, 10 nm or less, preferably 5 nm or less, more preferably 1 nm or less, and for example, 0.1 nm or more.

[0043] If the surface roughness Ra of the light guide plate 2 is equal to or less than the above upper limit, the haze of the laminate 1 can be reduced.

[0044] The surface roughness Ra of the light guide plate 2 can be adjusted, for example, by polishing the surface of one side in the thickness direction and the surface of the other side in the thickness direction of the light guide plate 2 .

[0045] The surface roughness Ra is the arithmetic mean roughness based on JIS B 0601.

[0046] The light guide plate 2 may be used alone or in a stack of a plurality of sheets.

[0047] The thickness of the light guide plate 2 is, for example, 0.3 mm or more, preferably 0.4 mm or more, more preferably 0.5 mm or more, and for example, 5.0 mm or less, preferably 4.0 mm or less, more preferably 3.8 mm or less, and even more preferably 3.6 mm or less.

[0048] When a plurality of light guide plates 2 are stacked, the thickness of the light guide plate 2 refers to the total thickness.

[0049] [Low Refractive Index Layer] The low refractive index layer 3 is a layer having a lower refractive index than the light guide plate 2, the pressure-sensitive adhesive layer 4 described later, and the base layer 5 described later. The low refractive index layer 3 allows light incident on the laminate 1 to be totally reflected within the light guide plate 2.

[0050] The low refractive index layer 3 is disposed on one surface and the other surface of the light guide plate 2 in the thickness direction.

[0051] The low refractive index layer 3 is formed, for example, by applying and drying a low refractive index layer coating liquid. Specifically, the low refractive index layer 3 is a dried product of the low refractive index layer coating liquid.

[0052] The low refractive index layer coating liquid contains, for example, particles and a dispersion medium.

[0053] The shape of the particles is not particularly limited, and examples thereof include spherical, plate-like, needle-like, string-like, and bunch-of-grapes shapes. Examples of string-like particles include particles in which a plurality of spherical, plate-like, or needle-like particles are strung together like beads, short fiber-like particles (e.g., short fiber-like particles described in JP 2001-188104 A), and combinations thereof. Examples of bunch-of-grapes-like particles include particles in which a plurality of spherical, plate-like, and needle-like particles are aggregated to form a bunch of grapes.

[0054] The shape of the particles can be confirmed by observation using, for example, a transmission electron microscope.

[0055] Examples of the particles include hollow particles (e.g., hollow nanosilica / nanoballoon particles), porous particles, and nanofibers (e.g., cellulose nanofibers, alumina nanofibers, silica nanofibers). Preferably, porous particles are used. The particles can be used alone or in combination of two or more types.

[0056] Examples of materials for the porous particles include organic and inorganic materials. Preferably, inorganic materials are used. The materials for the porous particles can be used alone or in combination of two or more.

[0057] Examples of organic materials include polymerizable monomers (for example, (meth)acrylic monomers and styrene monomers) and curable resins (for example, (meth)acrylic resins, fluorine-containing resins, and urethane resins).

[0058] Examples of inorganic substances include silicon compounds containing Si, magnesium compounds containing Mg, aluminum compounds containing Al, titanium compounds containing Ti, zinc compounds containing Zn, and zirconium compounds containing Zr. Silicon compounds are preferred.

[0059] Examples of silicon compounds include silica-based compounds (e.g., hydrolyzable silanes, their partial hydrolysates and dehydration condensates), and silicon compounds containing silanol groups (e.g., activated silica obtained by contacting silicate with acid or ion exchange resin).Preferably, silicon compounds containing silanol groups are used.

[0060] If the silicon compound is a trifunctional silane, a low refractive index layer 3 having a particularly low refractive index can be formed. If the silicon compound is a tetrafunctional silane, a low refractive index layer 3 having excellent scratch resistance can be formed.

[0061] That is, the particles are preferably porous particles of a silicon compound. Such porous particles of a silicon compound can be obtained, for example, by gelling a silicon compound in a hydrophilic medium, aging the obtained gel-like silicon compound, and pulverizing the gel-like silicon compound after aging.

[0062] Examples of silicon compounds include tris(hydroxy)methylsilane and trimethoxy(methyl)silane. Tris(hydroxy)methylsilane can be obtained by hydrolyzing trimethoxy(methyl)silane, and is a precursor of the gel silicon compound described below.

[0063] Examples of hydrophilic media include isopropyl alcohol (IPA), ethanol, methanol, butanol, acetone, dimethylformamide (DMF), and dimethyl sulfoxide (DMSO). Preferably, IPA and DMSO are used. The hydrophilic media can be used alone or in combination of two or more. The hydrophilic medium may also be mixed with water.

[0064] The gelation of silicon compounds is achieved, for example, by a dehydration condensation reaction between silicon compounds, which is preferably carried out in the presence of a catalyst.

[0065] Examples of catalysts include acid catalysts and base catalysts. Examples of acid catalysts include hydrochloric acid, oxalic acid, and sulfuric acid. Examples of base catalysts include ammonia, potassium hydroxide, sodium hydroxide, and ammonium hydroxide.

[0066] The aging temperature of the obtained gel silicon compound is, for example, 20° C. or higher and, for example, 50° C. or lower. The aging time is, for example, 10 hours or higher, preferably 15 hours or higher.

[0067] The method of pulverizing gel silicon compound after aging is not particularly limited, and can be pulverized by known method.As pulverization method, for example, can be pulverized by using pulverizer that utilizes cavitation phenomenon such as ultrasonic homogenizer, high-speed rotation homogenizer, etc.Specifically, can be pulverized by high-pressure medialess pulverization that uses homogenizer.

[0068] This makes it possible to obtain a sol liquid in which porous particles of a silicon compound are dispersed in a hydrophilic medium.

[0069] The low refractive index layer coating liquid can be obtained by replacing the hydrophilic medium contained in the sol liquid with a dispersion medium.

[0070] Examples of the dispersion medium include alcohols, esters, ethers, ketones, and aromatic hydrocarbons, with alcohols and ethers being preferred.

[0071] Examples of alcohols include ethanol, isopropyl alcohol, butanol, t-butanol, isobutyl alcohol, and 2-methoxyethanol (methyl cellosolve), with isobutyl alcohol being preferred. Examples of esters include ethyl acetate and butyl acetate. Examples of ethers include diisopropyl ether, diethylene glycol methyl ethyl ether, and propylene glycol monomethyl ether, with diethylene glycol methyl ethyl ether being preferred. Examples of ketones include acetone, methyl ethyl ketone, and methyl isobutyl ketone. Examples of aromatic hydrocarbons include toluene.

[0072] The dispersion medium may be used alone or in combination of two or more kinds, and preferably, isobutyl alcohol and diethylene glycol methyl ethyl ether are used in combination.

[0073] The method for replacing the hydrophilic medium with a dispersion medium is not particularly limited, and examples thereof include decantation, cross-flow filtration, and dynamic filtering. These replacements are preferably performed multiple times. If necessary, the blending ratio of the particles can be adjusted using the dispersion medium.

[0074] The mixing ratio of the particles in the low refractive index layer coating liquid is, for example, 0.1 parts by mass or more, preferably 0.5 parts by mass or more, and for example, 50 parts by mass or less, preferably 30 parts by mass or less, per 100 parts by mass of the dispersion medium.

[0075] The viscosity of the low refractive index layer coating liquid is, for example, 0.1 mPa·s or more, preferably 1.0 mPa·s or more, and for example, 2000 mPa·s or less, preferably 200 mPa·s or less.

[0076] The viscosity can be calculated using a rheometer manufactured by Anton-Paar.

[0077] In this manner, a coating liquid for a low refractive index layer can be obtained.

[0078] When the low refractive index layer coating liquid contains porous particles of a silicon compound, it is possible to stably produce a laminate 1 having desired optical properties.

[0079] In the low refractive index layer coating liquid, the volume average particle diameter of the particles is, for example, 0.10 μm or more, preferably 0.20 μm or more, more preferably 0.40 μm or more, and for example, 2.00 μm or less, preferably 1.50 μm or less, more preferably 1.00 μm or less.

[0080] In the low refractive index layer coating liquid, the particle size distribution of the particles is such that the proportion of particles having a particle size of 0.4 μm to 1 μm relative to the total amount of particles is, for example, 50 mass% or more, preferably 80 mass% or more, more preferably 90 mass% or more, and for example, 99.9 mass% or less, preferably 99.8 mass% or less, more preferably 99.7 mass% or less.

[0081] In the low refractive index layer coating liquid, the particle size distribution of the particles is, for example, 0.1 mass % or more, preferably 0.2 mass % or more, more preferably 0.3 mass % or more, and for example, 50 mass % or less, preferably 20 mass % or less, more preferably 10 mass % or less, such that the ratio of particles having a particle diameter of 1 μm to 2 μm to the total amount of particles is, for example, 0.1 mass % or more, preferably 0.2 mass % or more, more preferably 0.3 mass % or more, and for example, 50 mass % or less, preferably 20 mass % or less, more preferably 10 mass % or less.

[0082] The particle size distribution can be measured, for example, by a particle size distribution evaluation device such as a dynamic light scattering method or a laser diffraction method, or by an electron microscope such as a scanning electron microscope (SEM) or a transmission electron microscope (TEM). The volume average particle size is an index of the variation in particle size of the pulverized body.

[0083] By adjusting the volume average particle size and particle size distribution of the particles in the low refractive index layer coating liquid, it is possible to adjust the porosity and refractive index of the low refractive index layer 3, which will be described later. In other words, as long as the volume average particle size and particle size distribution of the particles are within the above ranges, the desired porosity and refractive index of the low refractive index layer 3 can be obtained.

[0084] The low refractive index layer 3 can be obtained by applying the low refractive index layer coating liquid and drying it.

[0085] The low refractive index layer 3, which is a dried product of such a low refractive index layer coating liquid, has, for example, voids inside.

[0086] There are no particular limitations on the method for forming voids in the low refractive index layer 3. For example, porous particles are chemically bonded to each other to form a porous body, and voids are formed within the porous body. Specifically, when the porous particles are porous particles of a silicon compound, a silicone porous body is formed.

[0087] The form of chemical bond (chemical bond) between the porous particles is not particularly limited, and examples thereof include cross-linking, covalent bonding, and hydrogen bonding. Specifically, when the porous particles are porous particles of a silicon compound, the porous particles of the silicon compound are bonded by siloxane bonding.

[0088] When a silicone porous material is formed in the low refractive index layer 3, the proportion of unbonded silicon atoms (i.e., residual silanols) among all silicon atoms contained in the silicone porous material is, for example, less than 50%, preferably 30% or less, and more preferably 15% or less.

[0089] The porous particles are chemically bonded to each other, for example, by the action of a catalyst, light irradiation, heating, etc. They may also be bonded via a small amount of a binder component (for example, a binder component equal to or less than the mass of the particles).

[0090] Furthermore, the low refractive index layer 3 preferably has an open-cell structure in which the pores of the porous particles are continuous. The open-cell structure means, for example, that the pore structure of a porous body is connected three-dimensionally, and the internal voids of the pore structure are continuous. When the porous body has an open-cell structure, the porosity can be increased.

[0091] If the particles are closed-cell particles (particles having individual pore structures) such as hollow silica, an open-cell structure cannot be formed. On the other hand, if the particles are porous particles of a silicon compound, they have a three-dimensional dendritic structure, and therefore, when a low refractive index layer coating liquid is applied to form a coating film, the porous particles of the silicon compound settle and deposit, making it possible to easily form an open-cell structure.

[0092] The low refractive index layer 3 preferably has a monolithic structure in which the open-cell structure includes a plurality of pore distributions. The monolithic structure refers to, for example, a hierarchical structure including a structure in which nano-sized fine voids (nanovoids) exist and an open-cell structure in which the nanovoids are aggregated. When forming a monolithic structure, for example, the fine voids can provide film strength, while the coarse open-cell structure can provide high porosity, thereby achieving both film strength and high porosity. Such a monolithic structure is preferably formed by controlling the pore distribution of the resulting void structure in the porous particles of the silicon compound. Furthermore, for example, the monolithic structure can be formed by controlling the particle size distribution of the porous particles of the silicon compound to a desired size.

[0093] The porosity of the low refractive index layer 3 is, for example, 35 vol% or more, preferably 38 vol% or more, more preferably 40 vol% or more, and for example, 90 vol% or less, preferably 75 vol% or less.

[0094] If the porosity of the low refractive index layer 3 is equal to or greater than the lower limit, the layer 3 can contain a large amount of air, thereby lowering the refractive index. If the porosity of the low refractive index layer 3 is equal to or less than the upper limit, the layer 3 can ensure sufficient strength.

[0095] The porosity can be determined by calculating the porosity from the refractive index measured with an ellipsometer using the Lorentz-Lorenz's formula.

[0096] The size of the voids (holes) in the low refractive index layer 3 is not particularly limited and is, for example, 2 nm or more, preferably 5 nm or more, more preferably 10 nm or more, and even more preferably 20 nm or more, and for example, 500 nm or less, preferably 200 nm or less, and more preferably 100 nm or less.

[0097] The size of the voids (pores) refers to the diameter of the major axis of the voids (pores), and can be quantified by the gas adsorption method (BET method).

[0098] The refractive index of the low refractive index layer 3 is 1.25 or less, preferably 1.20 or less, more preferably 1.18 or less, even more preferably 1.16 or less, particularly preferably 1.14 or less, and for example, 1.05 or more, preferably 1.08 or more, more preferably 1.10 or more.

[0099] If the refractive index of the low refractive index layer 3 is equal to or less than the upper limit, the light incident on the light guide plate 2 can be reliably totally reflected.

[0100] The refractive index of the low refractive index layer 3 can be measured using, for example, an ellipsometer under the conditions of, for example, a wavelength of 550 nm and an incident angle of 50 to 80 degrees.

[0101] The total light transmittance of the low refractive index layer 3 is, for example, 85% or more, preferably 87% or more, more preferably 89% or more, and for example, 99% or less, preferably 98% or less, more preferably 97% or less.

[0102] When the total light transmittance of the low refractive index layer 3 is within the above range, excellent transparency can be ensured.

[0103] The haze of the low refractive index layer 3 is, for example, less than 5%, preferably less than 3%, and is, for example, 0.1% or more.

[0104] When the haze of the low refractive index layer 3 is less than the upper limit, excellent transparency can be ensured.

[0105] The haze of the low refractive index layer 3 can be measured using a haze meter (HM-150, manufactured by Murakami Color Research Laboratory Co., Ltd.). The haze value is calculated using the following formula: Haze (%) = (Diffuse transmittance (%) / Total light transmittance (%)) × 100 (%)

[0106] The thickness of the low refractive index layer 3 is 10 μm or less, preferably 8 μm or less, more preferably 6 μm or less, and 1.5 μm or more, preferably 1.8 μm or more, more preferably 2.0 μm or more, even more preferably 2.5 μm or more, particularly preferably 3.0 μm or more, and most preferably 3.5 μm or more.

[0107] The thickness of the low refractive index layer 3 mentioned above indicates the total thickness of the low refractive index layer 3 arranged on either one side or the other side of the thickness direction of the light guide plate 2 in the laminate 1 .

[0108] When the thickness of the low refractive index layer 3 is equal to or less than the above upper limit, the low refractive index layer 3 can be made thin, and the laminate 1 has excellent manufacturability. When the thickness of the low refractive index layer 3 is equal to or greater than the above lower limit, interference between the light reflected by the light guide plate 2 and the light reflected by the low refractive index layer 3 can be suppressed, and color unevenness can be suppressed on the surface of the laminate 1. Consequently, the laminate 1 has excellent transparency.

[0109] The standard deviation of the thickness of the low refractive index layer 3 is, for example, 10% or less, preferably 9% or less, more preferably 8% or less, and for example, 1% or more, preferably 3% or more, more preferably 5% or more.

[0110] If the standard deviation of the thickness of the low refractive index layer 3 is within the above range, color unevenness on the surface of the laminate 1 can be suppressed.

[0111] [Adhesive Layer] The adhesive layer 4 is a layer that bonds the low refractive index layer 3 and the substrate layer 5 described below, and has a buffering function (cushioning function) against external forces.

[0112] The adhesive layer 4 is arranged on one thickness-wise surface of the low refractive index layer 3 on one thickness-wise side of the light guide plate 2, and is arranged on the other thickness-wise surface of the low refractive index layer 3 on the other thickness-wise side of the light guide plate 2.

[0113] The pressure-sensitive adhesive layer 4 has a hardness that does not allow it to penetrate into the voids in the low refractive index layer 3. That is, the shear storage modulus of the pressure-sensitive adhesive layer 4 at 23° C. is, for example, 0.2×10 5 (Pa) or more, preferably 0.5 × 10 5 (Pa) or more, more preferably 0.8 × 10 5 (Pa) or more, more preferably 1.0 × 10 5 (Pa) or more, particularly preferably 1.2 × 10 5 From the viewpoint of durability, the shear storage modulus of the pressure-sensitive adhesive layer 4 at 23°C is, for example, 5.0 × 10 7 (Pa) or less, preferably 3.0 × 107 (Pa) or less, more preferably 1.0 × 10 7 (Pa) or less, more preferably 5.0 × 10 6 (Pa) or less, particularly preferably 3.0 × 10 6 (Pa) or less, most preferably 1.0 × 10 6 (Pa) or less.

[0114] If the shear storage modulus of the pressure-sensitive adhesive layer 4 is within the above range, it has a buffering function (cushioning function) against external forces and is soft enough to prevent damage to the low refractive index layer 3 .

[0115] The shear storage modulus is determined by reading the value at 23°C when measured at a temperature rise rate of 5°C / min in the range of -50°C to 150°C under a frequency of 1 Hz in accordance with the method described in JIS K 7244-1 "Plastics - Testing methods for dynamic mechanical properties."

[0116] The pressure-sensitive adhesive layer 4 is made of a pressure-sensitive adhesive (pressure-sensitive adhesive composition), and the pressure-sensitive adhesive (pressure-sensitive adhesive composition) is not particularly limited. Specifically, the pressure-sensitive adhesive may be an acrylic pressure-sensitive adhesive (acrylic pressure-sensitive adhesive composition).

[0117] The acrylic pressure-sensitive adhesive composition contains, for example, a (meth)acrylic polymer as a main component (base polymer). The main component means a component contained in an amount of 50 mass % or more relative to the total amount of solids in the acrylic pressure-sensitive adhesive composition.

[0118] The (meth)acrylic polymer is contained in an amount of, for example, 50 mass % or more, preferably 70 mass % or more, or more preferably 90 mass % or more, relative to the total amount of solids in the acrylic pressure-sensitive adhesive composition.

[0119] A (meth)acrylic polymer is a polymer of a monomer component. The monomer component contains alkyl (meth)acrylate as a main component. The main component means a component that accounts for 50% by mass or more of the total amount of the monomer components. Furthermore, (meth)acrylate refers to acrylate and / or methacrylate.

[0120] The alkyl (meth)acrylate has, for example, a linear or branched alkyl group having 1 to 18 carbon atoms, and preferably has a linear or branched alkyl group having 3 to 9 carbon atoms.

[0121] Examples of alkyl(meth)acrylates include propyl(meth)acrylate, isopropyl(meth)acrylate, butyl(meth)acrylate, isobutyl(meth)acrylate, sec-butyl(meth)acrylate, t-butyl(meth)acrylate, pentyl(meth)acrylate, neopentyl(meth)acrylate, isopentyl(meth)acrylate, hexyl(meth)acrylate, octyl(meth)acrylate, and 2-ethylhexyl(meth)acrylate. Butyl(meth)acrylate is preferred.

[0122] The alkyl (meth)acrylates can be used alone or in combination of two or more kinds.

[0123] Examples of the monomer component include, in addition to alkyl (meth)acrylates, comonomers such as carboxyl group-containing (meth)acrylates, hydroxyl group-containing (meth)acrylates, amide group-containing (meth)acrylates, aromatic ring-containing (meth)acrylates, and heterocycle-containing (meth)acrylates. Preferred are hydroxyl group-containing (meth)acrylates and heterocycle-containing (meth)acrylates.

[0124] The hydroxyl group-containing (meth)acrylate is not particularly limited as long as it has a polymerizable functional group and a hydroxyl group. Examples of the hydroxyl group-containing (meth)acrylate include hydroxyalkyl (meth)acrylate.

[0125] Examples of hydroxyalkyl (meth)acrylates include 2-hydroxyethyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, and 10-hydroxydecyl (meth)acrylate. Preferably, 2-hydroxybutyl (meth)acrylate is used.

[0126] Examples of heterocycle-containing (meth)acrylates include N-acryloylmorpholine, N-acryloylpiperidine, N-methacryloylpiperidine, and N-acryloylpyrrolidine, with N-acryloylmorpholine being preferred.

[0127] If the monomer component contains a heterocycle-containing (meth)acrylate, it is possible to improve both the heat resistance and the moisture resistance when the pressure-sensitive adhesive layer 4 is made thinner.

[0128] The acrylic pressure-sensitive adhesive composition may contain, for example, additives. Examples of additives include a silane coupling agent and a crosslinking agent. Examples of silane coupling agents include an epoxy group-containing silane coupling agent. Examples of crosslinking agents include an isocyanate-based crosslinking agent and a peroxide-based crosslinking agent.

[0129] The method for polymerizing the monomer components in the pressure-sensitive adhesive (pressure-sensitive adhesive composition) is not particularly limited, and examples of the method for polymerizing the monomer components include solution polymerization.

[0130] Examples of solvents used in solution polymerization include ethyl acetate and toluene.

[0131] Details of such an acrylic pressure-sensitive adhesive composition are described in, for example, Japanese Patent No. 4140736.

[0132] The pressure-sensitive adhesive layer 4 has a thickness of, for example, 3 μm or more, preferably 5 μm or more, more preferably 8 μm or more, and for example, 100 μm or less, preferably 50 μm or less, more preferably 30 μm or less.

[0133] The thickness of the pressure-sensitive adhesive layer 4 mentioned above indicates the total thickness of the pressure-sensitive adhesive layer 4 disposed on either one side or the other side of the light guide plate 2 in the thickness direction of the laminate 1 .

[0134] When the thickness of the pressure-sensitive adhesive layer 4 is equal to or greater than the above-mentioned lower limit, it is possible to suppress damage to the light guide plate 2, and as a result, it is possible to maintain good optical properties of the laminate 1. When the thickness of the pressure-sensitive adhesive layer 4 is equal to or less than the above-mentioned upper limit, it is possible to reduce the thickness of the laminate 1, and further, it is possible to suppress the production cost.

[0135] The pressure-sensitive adhesive layer 4 has, for example, a higher refractive index than the low-refractive index layer 3. The difference between the refractive index of the pressure-sensitive adhesive layer 4 and the low-refractive index layer 3 (refractive index of the pressure-sensitive adhesive layer 4 - refractive index of the low-refractive index layer 3) is, for example, 0.05 or more, preferably 0.1 or more, more preferably 0.3 or more, even more preferably 0.5 or more, and particularly preferably 0.8 or more.

[0136] The refractive index of the pressure-sensitive adhesive layer 4 is, for example, 1.3 or more, preferably 1.5 or more, more preferably 1.8 or more, even more preferably 2.0 or more, and for example, 2.5 or less, preferably 2.4 or less, more preferably 2.3 or less.

[0137] [Base Layer] The base layer 5 is a layer that improves the strength of the laminate 1 and protects the light guide plate 2 .

[0138] The base layer 5 is arranged on one thickness-wise surface of the adhesive layer 4 on one thickness-wise side of the light guide plate 2, and is arranged on the other thickness-wise surface of the adhesive layer 4 on the other thickness-wise side of the light guide plate 2.

[0139] The base layer 5 is, for example, a polymer film.

[0140] Examples of materials for the polymer film include (meth)acrylic resins, cellulose resins, cycloolefin resins, olefin resins, ester resins, polyamide resins, polycarbonate resins, and copolymer resins thereof. Ester resins are preferred. The (meth)acrylic resin is an acrylic resin and / or a methacrylic resin.

[0141] Examples of cellulose resins include diacetyl cellulose and triacetyl cellulose. Examples of cycloolefin resins include norbornene resin. Examples of olefin resins include polypropylene. Examples of ester resins include polyethylene terephthalate resin.

[0142] That is, the base layer 5 is, for example, a polymer film, preferably a polymer film made of an ester resin, and more preferably a polyethylene terephthalate film.

[0143] The thickness of the base layer 5 is, for example, 10 μm or more, preferably 20 μm or more, more preferably 30 μm or more, even more preferably 40 μm or more, and for example, 200 μm or less, preferably 150 μm or less, more preferably 100 μm or less, even more preferably 80 μm or less, and particularly preferably 60 μm or less.

[0144] The thickness of the base material layer 5 mentioned above indicates the total thickness of the base material layers 5 arranged on either one side or the other side of the light guide plate 2 in the thickness direction in the laminate 1 .

[0145] If the thickness of the base layer 5 is within the above range, the AR device 10 has excellent surface protection performance, and damage to the light guide plate 2 can be suppressed.

[0146] The Young's modulus of the base layer 5 at 23°C is, for example, 2 GPa or more, preferably 2.5 GPa or more, more preferably 3 GPa or more, even more preferably 3.5 GPa or more, and for example, 10 GPa or less, preferably 8 GPa or less, more preferably 6 GPa or less.

[0147] If the Young's modulus of the base layer 5 is within the above range, the AR device 10 has excellent surface protection performance, and damage to the light guide plate 2 can be suppressed.

[0148] The Young's modulus can be measured in accordance with the method described in JIS K 7127 (1999).

[0149] The moisture permeability of the substrate layer 5 is, for example, 0.1 g / m 2 / 24 hr or more, preferably 0.5 g / m 2 / 24 hr or more, more preferably 1 g / m 2 / 24 hr or more, and for example, 1000 g / m 2 / 24 hr or less, preferably 800 g / m 2 / 24 hr or less, more preferably 500 g / m 2 / 24 hours or less.

[0150] If the moisture permeability of the base layer 5 is within the above range, damage to the light guide plate 2 can be further suppressed.

[0151] The moisture permeability can be measured in accordance with the method described in JIS Z 0208.

[0152] The substrate layer 5 has, for example, a higher refractive index than the low refractive index layer 3. The difference between the refractive index of the substrate layer 5 and the refractive index of the low refractive index layer 3 (refractive index of substrate layer 5 - refractive index of low refractive index layer 3) is, for example, 0.05 or more, preferably 0.1 or more, more preferably 0.3 or more, even more preferably 0.5 or more, and particularly preferably 0.8 or more.

[0153] The refractive index of the substrate layer 5 is, for example, 1.3 or more, preferably 1.5 or more, more preferably 1.8 or more, and even more preferably 2.0 or more, and for example, 2.5 or less, preferably 2.4 or less, and more preferably 2.3 or less.

[0154] <Method for Manufacturing Laminate> A method for manufacturing the laminate 1 will be described with reference to FIG.

[0155] In addition, the manufacturing method of the laminate 1 described below will be described with respect to a laminate 1 having a light guide plate 2, and on one thickness side of the light guide plate 2, a low refractive index layer 3, a pressure-sensitive adhesive layer 4, and a base material layer 5, in that order, toward one thickness side, and further having, on the other thickness side of the light guide plate 2, a low refractive index layer 3, a pressure-sensitive adhesive layer 4, and a base material layer 5, in that order, toward the other thickness side.

[0156] The manufacturing method of the laminate 1 includes a first step of arranging (stacking) a low refractive index layer 3 on one thickness-wise surface and the other thickness-wise surface of the light guide plate 2; a second step of arranging (stacking) an adhesive layer 4 on one thickness-wise surface of the low refractive index layer 3 arranged on one thickness-wise surface of the light guide plate 2 and on the other thickness-wise surface of the low refractive index layer 3 arranged on the other thickness-wise surface of the light guide plate 2; and a third step of arranging (stacking) a base layer 5 on one thickness-wise surface of the adhesive layer 4 arranged on one thickness-wise side of the light guide plate 2 and on the other thickness-wise surface of the adhesive layer 4 arranged on the other thickness-wise side of the light guide plate 2.

[0157] [First Step] First, as shown in FIG. 3A, a light guide plate 2 is prepared, and a low refractive index layer coating liquid is applied to one surface and the other surface in the thickness direction of the light guide plate 2.

[0158] An example of the coating method is spray coating, in which a coating liquid for the low refractive index layer is sprayed onto the light guide plate 2 to form a coating film of the low refractive index layer 3 on the light guide plate 2.

[0159] In the spray coating, the distance (coating distance) between the spray head that sprays the low refractive index layer coating liquid and the light guide plate 2 can be adjusted as needed. By adjusting the distance between the spray head and the light guide plate 2, it is possible to adjust the thickness unevenness and haze of the low refractive index layer 3.

[0160] The distance between the spray head and the substrate (coating distance) is, for example, 50 mm or more, preferably 100 mm or more, and for example, 500 mm or less, preferably 300 mm or less, more preferably 200 mm or less.

[0161] The spray coating is performed by repeating a spraying process in which the spray head sprays the low refractive index layer coating liquid while moving in the X direction, the surface direction of the light guide plate 2, and a moving process in which the spray head moves in the Y direction, the surface direction of the light guide plate 2 (the Y direction is perpendicular to the X direction).

[0162] The atomization pressure in spray coating is, for example, 50 kPa or more, preferably 80 kPa or more, and for example, 1000 kPa or less.

[0163] The application rate of the spray coating is, for example, 0.1 mL / min or more and, for example, 20 mL / min or less.

[0164] The movement speed of the spray head in the spraying step is, for example, 1 mm / sec or more, and, for example, 1000 mm / sec or less, preferably 500 mm / sec or less, more preferably 400 mm / sec or less, and even more preferably 300 mm / sec or less.

[0165] The moving distance of the head in the moving step is, for example, 1 mm or more and, for example, 50 mm or less.

[0166] By adjusting the above-mentioned spray coating conditions (atomization pressure, coating amount, moving speed of the spray head, moving distance of the spray head), the thickness and thickness unevenness of the low refractive index layer 3 can be adjusted.

[0167] The coating of the low refractive index layer 3 is dried by heating as required.

[0168] The heating temperature is, for example, 50° C. or more, preferably 60° C. or more, more preferably 65° C. or more, and for example, 200° C. or less, preferably 120° C. or less, more preferably 100° C. or less. The heating time is not particularly limited as long as the coating film can be sufficiently dried.

[0169] Heat drying causes a crosslinking reaction between the particles contained in the coating film, thereby fixing the three-dimensional basic structure. As a result, the low refractive index layer 3 can maintain sufficient strength and flexibility despite having a void structure.

[0170] As a result of the above, the low refractive index layer 3 is disposed (laminated) on one surface and the other surface in the thickness direction of the light guide plate 2 as shown in FIG. 3B.

[0171] [Step 2] Examples of methods for forming the pressure-sensitive adhesive layer 4 include a method of applying the pressure-sensitive adhesive composition described above to a release-treated separator or the like, forming the pressure-sensitive adhesive layer 4 by removing the solvent, and transferring the pressure-sensitive adhesive layer 4 to the low-refractive index layer 3, and a method of applying the pressure-sensitive adhesive composition to the low-refractive index layer 3, and forming the pressure-sensitive adhesive layer 4 by removing the solvent.

[0172] There are no particular limitations on the method for forming the pressure-sensitive adhesive layer 4. Examples of methods for forming the pressure-sensitive adhesive layer 4 include roll coating, kiss roll coating, gravure coating, reverse coating, roll brushing, spray coating, dip roll coating, bar coating, knife coating, air knife coating, curtain coating, lip coating, and extrusion coating using a die coater or the like.

[0173] As a result of the above, as shown in Figure 3C, the pressure-sensitive adhesive layer 4 is arranged (laminated) on one thickness-wise surface of the low-refractive index layer 3 arranged on one thickness-wise surface of the light guide plate 2, and on the other thickness-wise surface of the low-refractive index layer 3 arranged on the other thickness-wise surface of the light guide plate 2.

[0174] [Third step] As shown in FIG. 3D , a base layer 5 is disposed (laminated) on one thickness-wise surface of the pressure-sensitive adhesive layer 4 disposed on one thickness-wise side of the light guide plate 2, and on the other thickness-wise surface of the pressure-sensitive adhesive layer 4 disposed on the other thickness-wise side of the light guide plate 2.

[0175] In this manner, the laminate 1 can be manufactured.

[0176] <Modification of AR Device> The above-described AR device 10 is AR glasses, but it may also be, for example, a head-mounted display. Although not shown, the head-mounted display is a display that is worn on the head, such as a goggle-type or helmet-type display. The head-mounted display includes, for example, a display portion, an image generating device, and a wearing portion. Furthermore, the display portion includes the above-described laminate 1.

[0177] 4 shows a modified example (second embodiment) of the laminate 1 included in the AR device 10 of the present invention. The laminate 1 of the second embodiment has a light guide plate 2 and a low refractive index layer 3 arranged on one surface of the light guide plate 2 in the thickness direction, and further has a low refractive index layer 3 arranged on the other surface of the light guide plate 2 in the thickness direction.

[0178] The laminate 1 of the first embodiment has a pressure-sensitive adhesive layer 4 and a base layer 5, but like the laminate 1 of the second embodiment, depending on the purpose, it may not have the pressure-sensitive adhesive layer 4 and the base layer 5. Furthermore, although not shown, it may have only either the pressure-sensitive adhesive layer 4 or the base layer 5.

[0179] 5 shows a modified example (third embodiment) of the laminate 1 included in the AR device 10 of the present invention. The laminate 1 of the third embodiment includes a light guide plate 2, and on one thickness-wise side of the light guide plate 2, a pressure-sensitive adhesive layer 4, a base layer 5, and a low-refractive index layer 3, which are arranged in this order toward one thickness-wise side, and further includes, on the other thickness-wise side of the light guide plate 2, a pressure-sensitive adhesive layer 4, a base layer 5, and a low-refractive index layer 3, which are arranged in this order toward the other thickness-wise side.

[0180] Although not shown, the laminate 1 may have a plurality of pressure-sensitive adhesive layers 4 and substrate layers 5 .

[0181] Furthermore, the stacking order of the laminate 1 is not particularly limited to those of the first and third embodiments. Specifically, in the laminate 1, the stacking order of the low refractive index layer 3, the pressure-sensitive adhesive layer 4, and the base material layer 5, which are arranged on one side and the other side in the thickness direction of the light guide plate 2, is not particularly limited.

[0182] In the first, second, and third embodiments described above, the number of layers and the order of layers are the same on one side of the thickness direction of the light guide plate 2 and the other side of the thickness direction of the light guide plate 2, but the number of layers and the order of layers may be different, or the layers may be stacked on only one side of the thickness direction or the other side of the thickness direction.

[0183] Furthermore, the laminate 1 may have layers other than the light guide plate 2, the low refractive index layer 3, the pressure-sensitive adhesive layer 4, and the base layer 5 (for example, a hard coat layer and an anti-reflection layer) as needed.

[0184] <Modification of the method for manufacturing the laminate> The method for manufacturing the laminate 1 is not particularly limited as long as the laminate 1 described above can be manufactured.

[0185] In the above-described method for manufacturing the laminate 1, the low refractive index layer 3, the adhesive layer 4, and the base material layer 5 are laminated in parallel on one thickness side and the other thickness side of the light guide plate 2. However, for example, the low refractive index layer 3, the adhesive layer 4, and the base material layer 5 may be laminated on one thickness side of the light guide plate 2, and then the low refractive index layer 3, the adhesive layer 4, and the base material layer 5 may be laminated on the other thickness side of the light guide plate 2.

[0186] <Effects> The AR device 10 of the present invention includes a laminate 1, which has a light guide plate 2 and a low refractive index layer 3 arranged on at least one side in the thickness direction of the light guide plate 2. The refractive index of the low refractive index layer 3 is 1.25 or less, and the thickness of the low refractive index layer 3 is 1.5 μm or more and 10 μm or less. Therefore, the device can be made thinner, light leakage from the light guide plate 2 can be suppressed, color unevenness on the surface can be suppressed, and transparency is excellent.

[0187] More specifically, the AR device 10 includes a laminate 1 having a low refractive index layer 3. Therefore, even without an air layer, the light incident within the light guide plate 2 can be reliably totally reflected, and further, because no air layer is included, the device can be made thinner and light leakage from the light guide plate 2 can be suppressed.

[0188] The AR device 10 of the present invention also includes the laminate 1 having the low-refractive-index layer 3 of a specific thickness. This suppresses interference between the light reflected by the light guide plate 2 and the light reflected by the low-refractive-index layer 3, thereby suppressing color unevenness on the surface and providing excellent transparency.

[0189] The present invention will be described in more detail below with reference to examples and comparative examples. It should be noted that the present invention is in no way limited to these examples and comparative examples. The specific numerical values ​​of the blending ratios (content ratios), physical property values, parameters, etc. used in the following description can be replaced with the upper limit (a numerical value defined as "equal to or less than") or lower limit (a numerical value defined as "equal to or more than") of the corresponding blending ratios (content ratios), physical property values, parameters, etc. described in the "Description of the Invention" above.

[0190] Example 1 <Preparation of low refractive index layer coating liquid> [Gelling step] 0.95 g of methyltrimethoxysilane (MTMS), a silicon compound, was dissolved in 2.2 g of dimethyl sulfoxide (DMSO) to prepare mixed liquid A. 0.5 g of a 0.01 mol / L aqueous oxalic acid solution (catalyst) was added to this mixed liquid A, and the mixture was stirred at room temperature for 30 minutes to hydrolyze the MTMS, thereby producing mixed liquid B containing tris(hydroxy)methylsilane.

[0191] Next, 0.38 g of 28% by mass aqueous ammonia (catalyst) and 0.2 g of pure water were added to 5.5 g of DMSO, and then the above-mentioned mixed solution B was added. The mixture was stirred at room temperature for 15 minutes to gel the tris(hydroxy)methylsilane, thereby obtaining mixed solution C containing a gel-like silicon compound.

[0192] [Aging Step] The mixed solution C containing the gel silicon compound was incubated at 40° C. for 20 hours for aging treatment.

[0193] [Pulverization step] After the aging treatment, the mixed solution C containing the gel-like silicon compound was subjected to a pulverization treatment (high-pressure media-less pulverization). The pulverization treatment (high-pressure media-less pulverization) was carried out using a homogenizer (trade name "UH-50", manufactured by SMT Corporation). 1.85 g of the gel-like silicon compound in the mixed solution C containing the gel-like silicon compound and 1.15 g of isopropanol (IPA) were weighed into a 5 cc screw bottle, and then pulverized for 2 minutes under conditions of 50 W and 20 kHz.

[0194] The gel silicon compound in the mixed solution C containing the gel silicon compound was pulverized by the pulverization treatment, and a sol solution D of porous particles of the silicon compound was obtained.

[0195] Next, isobutyl alcohol and diethylene glycol methyl ether were added as a dispersion medium to the sol D of porous silicon compound particles, and after light stirring, the mixture was left to stand at room temperature for 6 hours to decant the hydrophilic medium and catalyst in the sol D of porous silicon compound particles. The same decantation process was repeated three times to replace the dispersion medium, thereby obtaining a low refractive index layer coating liquid. The volume average particle size, which indicates the particle size variation of the porous silicon compound particles contained in the low refractive index layer coating liquid, was measured using a dynamic light scattering Nanotrac particle size analyzer (UPA-EX150, manufactured by Nikkiso Co., Ltd.), and was found to be 0.50 μm to 0.70 μm.

[0196] <Production of Laminate> A 100 mm x 100 mm alkali-free glass (product name "Eagle XG", manufactured by Coaning) serving as a light guide plate and the above-described low refractive index layer coating liquid were set in a spray coater (product name "API-240" series, manufactured by Apeiros).

[0197] Next, the low refractive index layer coating liquid was spray-coated onto alkali-free glass (light guide plate) under the following coating conditions to form a low refractive index layer coating film on one surface in the thickness direction of the alkali-free glass. The spray coating was performed by repeatedly performing a spraying process in which the spray head sprayed the paint while moving in the X direction, the surface direction of the light guide plate, and a moving process in which the spray head moved in the Y direction, the surface direction of the light guide plate (the Y direction is perpendicular to the X direction).

[0198] {Coating conditions} Atomization pressure: 100 kPa Coating amount: 8.6 mL / min Head speed in spraying process: 270 mm / sec Head movement distance in movement process: 15 mm Distance between spray head (nozzle) and alkali-free glass (coating distance): 125 mm

[0199] Next, the low refractive index layer coating on one surface in the thickness direction of the alkali-free glass (light guide plate) was dried at 90°C for 10 minutes and then at 70°C for 24 hours to form a low refractive index layer on one surface in the thickness direction of the light guide plate, thereby obtaining a laminate.

[0200] Example 2 <Production of Pressure-Sensitive Adhesive Layer> A four-necked flask equipped with a stirring blade, a thermometer, a nitrogen gas inlet tube, and a condenser was charged with 90.7 parts by mass of butyl acrylate, 6 parts by mass of N-acryloylmorpholine, 3 parts by mass of acrylic acid, 0.3 parts by mass of 2-hydroxybutyl acrylate, and 0.1 parts by mass of 2,2'-azobisisobutyronitrile as a polymerization initiator, along with 100 g of ethyl acetate. Nitrogen gas was then introduced with gentle stirring to replace the atmosphere with nitrogen, and the liquid temperature in the flask was maintained at around 55°C while carrying out a polymerization reaction for 8 hours to prepare an acrylic polymer solution. An acrylic adhesive solution was prepared by blending 0.2 parts by mass of an isocyanate crosslinker (Coronate L, manufactured by Nippon Polyurethane Industry Co., Ltd., an adduct of trimethylolpropane and tolylene diisocyanate), 0.3 parts by mass of benzoyl peroxide (Niper BMT, manufactured by NOF Corporation), and 0.2 parts by mass of γ-glycidoxypropyl methoxysilane (KBM-403, manufactured by Shin-Etsu Chemical Co., Ltd.) per 100 parts by mass of the solids content of the obtained acrylic polymer solution. Next, the above acrylic adhesive solution was applied to one side of a silicone-treated polyethylene terephthalate (PET) film (manufactured by Mitsubishi Chemical Polyester Film Co., Ltd., thickness: 38 μm) so that the thickness of the adhesive layer after drying would be 10 μm, and the film was dried at 150°C for 3 minutes to form an adhesive layer. The shear storage modulus of the obtained adhesive at 23°C was 1.3 × 10 5 (Pa).

[0201] <Production of Laminate> The above-mentioned pressure-sensitive adhesive layer (thickness: 10 μm, storage modulus: 1.3×10 5 Furthermore, a PET film (manufactured by Mitsubishi Chemical Polyester Film Corporation, thickness 50 μm, Young's modulus at 23° C. 4.0 GPa) was laminated as a base layer on one surface in the thickness direction of the pressure-sensitive adhesive layer. In this way, a laminate of Example 2 was obtained.

[0202] Comparative Example 1 A laminate of Comparative Example 1 was obtained in the same manner as in Example 1, except that the head speed in the spraying step in the production of the laminate was set to 350 mm / sec.

[0203] Comparative Example 2 A laminate of Comparative Example 2 was obtained in the same manner as in Example 1, except that the head speed in the spraying step in the production of the laminate was set to 300 mm / sec.

[0204] Comparative Example 3 A pressure-sensitive adhesive layer and a substrate layer were laminated in this order on one surface in the thickness direction of the laminate of Comparative Example 1 (low refractive index layer) in the same manner as in Example 2, to obtain a laminate of Comparative Example 3.

[0205] Comparative Example 4 A pressure-sensitive adhesive layer and a substrate layer were laminated in this order on one thickness-wise surface of the laminate of Comparative Example 2 (low refractive index layer) in the same manner as in Example 2, to obtain a laminate of Comparative Example 4.

[0206] <Evaluation> [Thickness of low refractive index layer] In Example 1 and Comparative Examples 1 and 2, the film thickness of the low refractive index layer laminated on one surface in the thickness direction of the alkali-free glass (light guide plate) was measured at 10 vertical points and 10 horizontal points at 10 mm intervals, a total of 100 points, using a reflective interference film thickness meter (Optical NanoGauge film thickness meter, manufactured by Hamamatsu Photonics K.K.). The average thickness, maximum thickness, minimum thickness, and standard deviation of the thickness are shown in Table 1.

[0207] [Haze of Low Refractive Index Layer] The low refractive index layers of Example 1 and Comparative Examples 1 and 2 were set in a haze meter (HM-150, manufactured by Murakami Color Research Laboratory Co., Ltd.) and the haze was measured. The results are shown in Table 1. The haze was calculated using the following formula: Haze (%) = (Diffuse transmittance (%) / Total light transmittance (%)) × 100 (%)

[0208] [Color Unevenness] The laminates of each Example and Comparative Example were placed flat and visually observed from the 0° position on one side of the thickness direction of the laminate (a position at the center of the laminate, perpendicular to the surface direction of the laminate), and photographs were taken from the same position. Similarly, the laminates were visually observed from positions on one side of the thickness direction, tilted 30° and 60° in the surface direction from the 0° position, and photographs were taken from the same positions. The visual observations and photographs were checked, and the presence or absence of color unevenness was evaluated according to the following criteria. The results are shown in Tables 2 and 3.

[0209] {Criteria} ◯: No color unevenness is observed visually or in the photograph. ×: Color unevenness is observed visually or in the photograph, at least in one case.

[0210]

[0211]

[0212]

[0213] The above invention is provided as an exemplary embodiment of the present invention, but this is merely an example and should not be interpreted as limiting. Modifications of the present invention that are obvious to those skilled in the art are intended to be included in the scope of the following claims.

[0214] It is used in AR glasses and head-mounted displays that support AR technology.

[0215] REFERENCE SIGNS LIST 1 laminate 2 light guide plate 3 low refractive index layer 10 AR device

Claims

1. An AR device comprising a laminate having a light guide plate and a low refractive index layer arranged on at least one side of the light guide plate in a thickness direction, wherein the refractive index of the low refractive index layer is 1.25 or less, and the thickness of the low refractive index layer is 1.5 μm or more and 10 μm or less.

2. The AR device according to claim 1, wherein the standard deviation in thickness of the low refractive index layer is 10% or less.

3. The AR device according to claim 1, wherein the thickness of the light guide plate is 0.3 mm or more and 5 mm or less.

4. The AR device according to claim 1, comprising a laminate further having an adhesive layer disposed on at least one side of the light guide plate in the thickness direction.

5. An AR device according to any one of claims 1 to 4, comprising a laminate further having a base material layer arranged on at least one side in the thickness direction of the light guide plate.

6. The AR device according to claim 1, wherein in the color unevenness evaluation test described below, no color unevenness is visually observed on the surface of the laminate when observed from a 0° position on one side in the thickness direction of the laminate. [Color unevenness evaluation test] A 100 mm x 100 mm laminate is placed so as to be flat, and is visually observed from a 0° position on one side in the thickness direction of the laminate (a position at the center of the laminate that is perpendicular to the surface direction), and a photograph is taken from the same position. The visual observation and the photograph are checked to evaluate the presence or absence of color unevenness.

Citation Information

Patent Citations

  • Antireflection film, polarizing plate and image display device

    JP2001188104A

  • Head mounted display

    JP2011221129A

  • Method and system for mixing a continuously flowing mass with a gas

    US4140736A

  • Image display optical system and image display apparatus

    JP2006162767A

  • Multilayer laminate

    JP2015171815A