Sicn film-forming method and plasma processing apparatus
The PEALD method for SiCN film formation inherits Si-C and Si-N bonds from precursor gases using UHF or VHF plasma, addressing the challenge of low-temperature film quality and etching resistance, resulting in high-density and etching-resistant SiCN films for electronic device manufacturing.
Patent Information
- Application Number
- PCT/JP2024/009913
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-28
- Filing Date
- 2024-03-14
- Publication Date
- 2024-10-03
AI Technical Summary
Existing methods for forming SiCN films at low temperatures struggle to inherit Si-C bonds from precursor gases, leading to poor film quality and etching resistance, as high-temperature processes break these bonds, resulting in films with reduced etching resistance and composition changes during manufacturing.
A plasma enhanced atomic layer deposition (PEALD) method using a precursor gas with Si-N and Si-C bonds, where UHF or VHF plasma is used to form a SiCN film without breaking these bonds, inheriting Si-C and Si-N bonds from the adsorption layer, and controlling the substrate temperature below 450°C to maintain film quality and etching resistance.
The method effectively forms SiCN films with high density and etching resistance by inheriting Si-C and Si-N bonds, improving film quality and maintaining etching resistance at low temperatures, suitable for electronic device manufacturing.
Smart Images

Figure JP2024009913_03102024_PF_FP_ABST
Abstract
Description
SiCN film forming method and plasma processing apparatus
[0001] The present disclosure relates to a method for forming a SiCN film and a plasma processing apparatus.
[0002] For example, U.S. Patent No. 6,277,949 discloses a method for depositing a silicon carbide film on a substrate surface. The method includes, for example, the use of a gas-phase carbosilane precursor and employs a plasma-enhanced atomic layer deposition (PEALD) process by an ALD (atomic layer deposition) method. It is described that the method may be carried out at a temperature below 600°C, for example, between about 23°C and about 200°C, or about 100°C.
[0003] For example, Patent Documents 2 and 3 disclose a method for forming a silicon-containing film by using a deposition method selected from an ALD deposition process or a cyclic CVD deposition process, in which a substrate is placed in a reactor, heated to, for example, 700° C., and Si—N bonds, Si—Si bonds, and Si—H bonds are formed. 2 The method discloses a method of introducing at least one silane-based precursor having a group, purging unreacted materials, providing a reducing agent (hydrogen plasma) to react with the precursor to deposit a silicon-containing film, and then purging unreacted materials, and repeating this process.
[0004] For example, U.S. Patent No. 6,277,663 discloses a method for forming a silicon nitride film on a substrate at low temperatures. The method includes supplying a gas containing precursor gas molecules having unstable Si—N, Si—C, or N—C bonds, and forming a precursor material layer on the substrate by preferentially breaking the unstable bonds. The method also discloses that, when forming the precursor material layer on the substrate, activated precursor gas molecules bond with the surface of the substrate at the one or more reaction sites, and performing a plasma treatment process on the precursor material layer to form a conformal silicon nitride film.
[0005] US Patent Application Publication No. 2012 / 0122302 JP 2014-013888 A JP 2015-15465 A JP 2015-507362 A
[0006] The present disclosure provides techniques that allow the Si—C bonds of the precursor gas to be transferred to the film formed on the substrate.
[0007] According to one aspect of the present disclosure, there is provided a method for forming a SiCN film, the method comprising: (a) preparing a substrate in a processing vessel; (b) supplying a first gas into the processing vessel, the first gas including a precursor gas having Si—N bonds and Si—C bonds, to form an adsorption layer on the substrate, wherein the Si—N bonds and Si—C bonds are not activated in the formation of the adsorption layer; (c) a first purging step of purging the processing vessel after the step (b); (d) supplying a second gas including hydrogen gas and VHF or UHF wave power into the processing vessel to generate plasma, and exposing the substrate to the plasma to react with the adsorption layer, thereby forming a SiCN film, wherein the SiCN film retains at least a portion of the Si—C bonds and Si—N bonds of the adsorption layer; and (e) a second purging step of purging the processing vessel after the step (d), the method comprising repeating the steps (b) to (e).
[0008] According to one aspect, the Si—C bonds of the precursor gas can be inherited by the film formed on the substrate.
[0009] FIG. 1 is a schematic cross-sectional view showing an example of the configuration of a plasma processing apparatus according to an embodiment; FIG. 2 is a diagram for explaining a precursor gas having Si—C bonds and the inheritance of bonds in a film; FIG. 3 is a diagram showing an example of a precursor gas; FIG. 4 is a diagram showing an example of a precursor gas; FIG. 5 is a diagram showing an example of a precursor gas; FIG. 6 is a diagram showing an example of a precursor gas; FIG. 7 is a diagram showing an example of a precursor gas; FIG. 8 is a diagram showing an example of a precursor gas; FIG. 9 is a flowchart showing an example of a method for forming a SiCN film according to an embodiment; FIG. 10 is a diagram showing a modified example of the method for forming a SiCN film according to an embodiment; FIG. 11 is a diagram showing an example of an experiment result of the composition and pressure dependence of a SiCN film; FIG. 12 is a diagram showing the relationship between the carbon concentration in a SiCN film and the film density; FIG. 13 is a diagram showing an example of an XPS measurement result of a SiCN film; H 2 Plasma and N 2The present invention relates to a method for forming a SiCN film using a plasma, ...
[0010] Hereinafter, embodiments of the present disclosure will be described with reference to the drawings. In the drawings, the same components are denoted by the same reference numerals, and redundant explanations may be omitted.
[0011] [Plasma Processing Apparatus] A configuration example of a plasma processing apparatus that performs the film forming method according to this embodiment will be described with reference to Fig. 1. Fig. 1 is a diagram showing a configuration example of a plasma processing apparatus 1 that is equipped with a UHF wave plasma source according to one embodiment.
[0012] The plasma processing apparatus 1 includes a processing vessel 10 and a plasma source 2. The processing vessel 10 is airtight, has a generally cylindrical shape, is made of a metal material such as aluminum, and is grounded. The plasma source 2 generates plasma by introducing UHF wave power into the processing vessel 10. The ceiling wall 10a of the processing vessel 10 is configured by a metal main body into which dielectric members (hereinafter referred to as dielectric windows 56) connected to multiple radiation mechanisms 42 are fitted. As a result, the plasma source 2 introduces UHF waves into the processing vessel 10 through the multiple dielectric windows 56 in the ceiling wall 10a.
[0013] However, the configuration of the ceiling wall 10a of the processing vessel 10 is not limited to a configuration in which a dielectric member connected to multiple radiation mechanisms 42 is fitted into a metal main body. For example, a dielectric member may be provided to cover the surface of the ceiling wall 10a facing the substrate W, and UHF wave power may be introduced from one radiation mechanism 42, or a configuration having a shower structure in which a predetermined gas is supplied in a shower-like manner to the surface of the ceiling wall 10a facing the substrate W may be used. Furthermore, the power introduced into the processing vessel 10 is not limited to UHF waves, and may be VHF wave power. The frequency of the VHF waves or UHF waves is within the range of 100 MHz to 3 GHz.
[0014] The plasma processing apparatus 1 has a control device 130. The control device 130 is, for example, a computer, and has a program storage unit (not shown). The program storage unit stores a program for controlling the processing of a substrate W, such as a semiconductor wafer, in the plasma processing apparatus 1. The program may be recorded on a computer-readable storage medium, such as a computer-readable hard disk (HD), flexible disk (FD), compact disk (CD), magnetic optical disk (MO), or memory card, and may be installed into the control device 130 from the storage medium.
[0015] A mounting table 11 for horizontally supporting a substrate W is provided within the processing vessel 10 and is supported by a cylindrical support member 12 that stands via an insulating member 12a at the center of the bottom of the processing vessel 10. The mounting table 11 and the support member 12 are made of a material such as a metal such as aluminum whose surface has been anodized (anodized), or an insulating material (ceramics, etc.) that has a high-frequency electrode inside.
[0016] Although not shown, the mounting table 11 is also provided with a temperature control mechanism, a gas flow path for supplying a gas for heat transfer to the rear surface of the substrate W, and lifting pins for lifting and lowering to transport the substrate W. Furthermore, an electrostatic chuck for electrostatically attracting the substrate W may be provided.
[0017] An RF bias power supply 14 is electrically connected to the mounting table 11 via a matching box 13. When RF bias power is supplied from the RF bias power supply 14 to the mounting table 11, ions in the plasma are attracted to the substrate W side, which contributes to improving film quality and in-plane uniformity.
[0018] An exhaust pipe 15 is connected to the side of the bottom of the processing vessel 10, and an exhaust device 16 including a vacuum pump is connected to the exhaust pipe 15. By operating the exhaust device 16, the processing vessel 10 can be evacuated and the pressure inside the processing vessel 10 can be reduced to a predetermined value. In addition, a side wall 10b of the processing vessel 10 is provided with a loading / unloading port 17 for loading / unloading the substrate W, and a gate valve 18 for opening / closing the loading / unloading port 17.
[0019] The plasma processing apparatus 1 also has a first gas shower section 21 for discharging a predetermined gas into the processing vessel 10 from the ceiling wall 10a of the processing vessel 10, and a second gas shower section 22 for introducing gas from a position between the ceiling wall 10a and the mounting table 11.
[0020] 1, the first gas shower unit 21 and the second gas shower unit 22 are shown at radially offset positions for convenience, but are actually provided alternately on the same circle. The first gas shower unit 21 supplies gas carried from a first gas supply unit 81 through a gas line 83 from the rear surface of the ceiling wall 10a. The second gas shower unit 22 has a nozzle hanging down from the rear surface of the ceiling wall of the processing vessel 10, and supplies gas carried from a second gas supply unit 82 through a gas line 84 from the tip of the nozzle to a position between the ceiling wall 10a and the mounting table 11.
[0021] The plasma source 2 includes a UHF wave output unit 30 that distributes UHF waves to multiple paths and outputs them, and a UHF wave transmission unit 40 that transmits the UHF waves output from the UHF wave output unit 30. The UHF wave output unit 30 includes a UHF wave power supply, a UHF wave oscillator, an amplifier, and a distributor. The UHF wave power supply supplies power to the UHF wave oscillator. The UHF wave oscillator generates UHF waves at a predetermined frequency, for example, by PLL oscillation. The amplifier amplifies the oscillated UHF waves. The distributor distributes the UHF waves amplified by the amplifier while matching the impedance between the input and output sides to minimize loss of the UHF waves. The frequency of the UHF waves is within the range of 300 MHz to 3 GHz.
[0022] The UHF wave transmission unit 40 has a plurality of amplifier units 41 and a plurality of radiation mechanisms 42 provided corresponding to the amplifier units 41. The radiation mechanisms 42 are arranged, for example, one at the center of the top wall 10a and six at equal intervals on a circumference centered on the central one, for a total of seven. In this example, the radiation mechanisms 42 are arranged so that the distance between the central radiation mechanism 42 and the outer peripheral radiation mechanisms 42 is equal to the distance between the outer peripheral radiation mechanisms 42.
[0023] The amplifier unit 41 guides the UHF waves distributed by the distributor to each radiation mechanism 42. The radiation mechanism 42 includes a coaxial tube 51. The coaxial tube 51 has a coaxial UHF wave transmission line consisting of a cylindrical outer conductor 51a and a rod-shaped inner conductor 51b disposed at the center of the outer conductor 51a. The radiation mechanism 42 includes a power feeding antenna (not shown) that feeds the UHF waves amplified by the amplifier unit 41 to the coaxial tube 51. The radiation mechanism 42 further includes a tuner that matches the impedance of the load to the characteristic impedance of the UHF wave power source, and an antenna that radiates the UHF waves from the coaxial tube into the processing chamber 10.
[0024] The antenna unit is provided at the lower end of the coaxial tube 51 and is fitted into a metal portion of the ceiling wall 10a of the processing vessel 10. The antenna unit has a dielectric window 56, and a surface wave plasma is generated directly below the dielectric window 56 in the processing vessel 10 by the UHF wave that has passed through the dielectric window 56.
[0025] The plurality of dielectric windows 56 are provided in the center of the ceiling and six on the periphery. Each of the plurality of dielectric windows 56 can independently control the UHF wave power supplied from the plasma source 2. The UHF wave power supplied from the dielectric window 56 on the periphery may be higher than or the same as the UHF wave power supplied from the dielectric window 56 in the center.
[0026] The plasma processing apparatus 1 has an ion trap function in the processing chamber 10, and generates hydrogen plasma (H 2 In the case of plasma, hydrogen radicals may be irradiated onto the substrate.
[0027] [Outline of SiCN Film Formation] In the method of forming a SiCN film according to the present disclosure, a plasma-enhanced atomic layer deposition (PEALD) process using an ALD method is carried out in a plasma processing apparatus 1 .
[0028] A precursor gas, which is a raw material gas, is supplied from the second gas shower unit 22. For example, when forming a SiCN film, a first gas containing a precursor gas having Si—N bonds and Si—C bonds is supplied from the second gas shower unit 22 to form an adsorption layer on the substrate W. In the step of forming the adsorption layer, no power is supplied and no plasma is used. By supplying the precursor gas to a position closer to the substrate W, dissociation of the precursor gas is suppressed, and the precursor gas is adsorbed onto the substrate W. Furthermore, in the step of forming the adsorption layer, the Si—N bonds and Si—C bonds are not activated. Therefore, the Si—N bonds and Si—C bonds in the adsorption layer are not broken.
[0029] The precursor gas may be selected from one of HMCTS, HMCTZ, TMSI, BTBAMS, BSBAMS, BTBAES, and BTBAVS (see FIGS. 3A-3G). The precursor gas may have at least Si—N and Si—C bonds, but may not have Si—Si bonds.
[0030] The first gas may contain a carrier gas such as He gas. The first gas may also contain an inert gas such as Ar gas as a dilution gas. The carrier gas and dilution gas contained in the first gas may be supplied from the first gas shower unit 21. However, the dilution gas contained in the first gas may also be supplied from the second gas shower unit 22.
[0031] H 2 The second gas containing hydrogen gas is supplied from the first gas shower unit 21. 2 The gas is activated by plasma (plasma excitation). Optionally, RF bias power may be supplied from an RF bias power supply 14. The C atoms other than the Si—C bond contained in the precursor gas are included in a group R that is easily broken with Si. The substrate W is then heated to a plasma-excited state of H. 2 Gas (H 2 By exposing the adsorbed layer to a plasma, H2 The plasma can break the bonds of the group R. This causes the group R, which deteriorates the properties of the SiCN film, to be desorbed from the adsorption layer, while at least some of the Si—N bonds and Si—C bonds of the adsorption layer are inherited by the SiCN film. This method allows the SiCN film to be formed while the temperature of the substrate W is controlled to a low temperature of 450° C. or less, and further allows the Si—C bonds to be inherited by the SiCN film, thereby improving the film quality.
[0032] The second gas may include an inert gas, such as Ar gas, He gas, or N 2 The inert gas contained in the second gas may be supplied from the first gas shower section 21 and / or the second gas shower section 22.
[0033] a step of supplying a first gas containing a precursor gas to form an adsorption layer on the substrate W; 2 A second gas containing H 2 A purge step is provided between the step of exposing the adsorbed layer to plasma to react with the adsorbed layer and forming the SiCN film.
[0034] In the purge step, an inert gas such as Ar gas is supplied from the first gas shower unit 21 and / or the second gas shower unit 22. The purge step performed before the step of supplying a first gas containing a precursor gas into the processing vessel 10 to form an adsorption layer on the substrate W (hereinafter referred to as the "step of forming an adsorption layer") is referred to as the second purge step. 2 A second gas containing H 2 The purging process performed before the process of exposing the substrate to plasma to react with the adsorption layer to form a SiCN film (hereinafter referred to as the "process of forming a SiCN film") and after the process of forming the adsorption layer is called the first purging process.
[0035] In the first and second purge steps, the gas inside the processing vessel 10 is replaced by supplying Ar gas or the like, and the gas supplied in the previous step is exhausted to the outside of the processing vessel 10 by the exhaust device 16 .
[0036] The first purging step, the adsorption layer forming step, the second purging step, and the SiCN film forming step are repeatedly performed, thereby enabling the ALD method to form a SiCN film on the substrate W while controlling the substrate W to a temperature of 450° C. or less using the plasma processing apparatus 1 shown in FIG.
[0037] [Low-Temperature Formation of SiCN Film] SiN films are easily etched when exposed to etching liquids such as hydrofluoric acid used in the manufacturing process of electronic devices. Therefore, in recent years, SiCN films have been used as films with high wet-etching resistance in the manufacturing process of electronic devices. In particular, with the increasing integration of devices, there is a demand for SiCN films with high wet-etching resistance to be formed at low temperatures (e.g., 450°C or lower).
[0038] As shown on the right side of FIG. 2( a), when the substrate temperature during film formation is 600° C. or higher, Si contained in the gas bonds with C, forming Si—C bonds during film formation, making it possible to form a desired SiCN film with improved film quality.
[0039] On the other hand, as shown on the left side of Figure 2(a), when the substrate temperature is lower than 600°C (for example, 450°C), the Si contained in the gas preferentially bonds with the N in the processing vessel 10, making it difficult to bond Si and C at low temperatures, and low-temperature synthesis of Si-C bonds does not proceed. This poses the problem that the desired SiCN film cannot be formed and the film quality does not improve. In particular, when plasma is used, the ion energy breaks the Si-C bonds, and ultimately, C disappears from the composition of the adsorption layer, resulting in a film that is almost entirely SiN.
[0040] Therefore, in the method for forming a SiCN film of this embodiment, a precursor gas having an Si-C bond is used, and the Si-C bond of the precursor gas is inherited by the SiCN film without being broken. Furthermore, a precursor gas having not only an Si-C bond but also an Si-N bond is used, and the Si-N bond of the precursor gas is inherited by the SiCN film without being broken. In order to inherit the Si-C bond and Si-N bond in the precursor gas to the SiCN film, a source gas having the following characteristics (1) to (3) is used as the precursor gas. (1) There is an Si-C bond. (2) There is an Si-N bond. (3) C other than the Si-C bond and the Si-N bond is included in a group (sometimes represented by the group R, such as "R" or "R'") that is easily broken with Si.
[0041] Regarding (3), for example, Si—NH—R, Si—NR 2 , Si-NRR' has C other than Si-C bond and Si-N bond in "R" and "R'". For example, CH 3 The carbon-containing groups that have a negative effect on the SiCN film, such as the above, are included in group R that is easily cut off from Si.
[0042] The bond energy of Si—N is about 400 kJ / mol, and the N—R of Si—NH—R is about 200 to 300 kJ / mol, and N—R is more easily broken than Si—N. 2 By reacting with plasma, Si—N of Si—NH—R remains, R is broken, Si—C bond and Si—N bond are inherited, and C in the set R, which has a negative effect on the SiCN film, is removed.
[0043] If the Si-C bond is not inherited, the adsorption layer does not contain Si-C bonds, as shown in FIG. 2(c), and a SiCN film cannot be formed when the temperature of the substrate W is controlled to 450°C or less. On the other hand, if the Si-C bond is inherited, the adsorption layer contains Si-C bonds, as shown in FIG. 2(d), and a SiCN film of high film quality can be formed. Furthermore, by using high-frequency plasma with a high plasma density using the plasma processing apparatus 1 of FIG. 1, film quality can be further improved. Note that, to improve film quality using high-density plasma, high-frequency plasma with a VHF or UHF wave frequency in the range of 100 MHz to 3 GHz is used.
[0044] As described above, in the SiCN film formation method of this embodiment, the Si—C bonds of the adsorption layer are inherited by the SiCN film. The Si—N bonds of the adsorption layer are also inherited by the SiCN film. This method allows a high-density SiCN film with high etching resistance to be formed while the temperature of the substrate W is controlled to 450° C. or less.
[0045] Examples of precursor gases having the above characteristics (1) to (3) include the following: Aminosilanes: R I R II N-R 2-x SiH x -NR III R IV (x is an integer between 0 and 1, R is C n H m group, R I , R II , R III , R IV are the same or different C n H m group or H). R I , R II , R III , R IV is an example of a group R where C other than Si-C bonds and Si-N bonds is easily broken with Si. Silazanes: Cyclic [-(CH 3 ) 2 Si—NH—] n , cyclic [-(CH 3 ) SiH—NH—] n , cyclic [-(CH 3 )SiH—N(CH 3 )-] n , for example, n=4 to 6.
[0046] 2,2,4,4,6,6-hexamethylcyclotrisilazane (see Figure 3A HMCTS), linear (CH 3 ) 3 Si-NH-Si(CH 3 ) 3 , (CH 3 ) 3 Si-[NH-Si(CH 3 ) 2 ] n -Si(CH 3 )3 , for example, n=1 to 3, is an example of a precursor gas containing Si—C bonds and Si—N bonds. Note that if there are Si—C bonds, some or all of the CH 3 But H and C x H y Silyl imidazoles: trimethylsilylimidazole (see Figure 3C TMSI).
[0047] The precursor gas may be selected from one of HMCTS (FIG. 3A), HMCTZ (FIG. 3B), TMSI (FIG. 3C), BTBAMS (FIG. 3D), BSBAMS (FIG. 3E), BTBAES (FIG. 3F), BTBAVS (FIG. 3G).
[0048] [Method of Forming SiCN Film] A method of forming a SiCN film according to one embodiment will be described with reference to Fig. 4, Fig. 5A, and Fig. 5B. Fig. 4 is a flowchart showing an example of a method of forming a SiCN film according to one embodiment. Fig. 5A is a diagram showing an example of a method of forming a SiCN film according to one embodiment. Fig. 5B is a diagram showing a modified example of a method of forming a SiCN film according to one embodiment.
[0049] The method for forming the SiCN film is, for example, an atomic layer deposition (ALD) process performed in the plasma processing apparatus 1 of Fig. 1 and is controlled by the control device 130. In the method for forming the SiCN film according to one embodiment shown in Fig. 4, in step S1, the control device 130 opens the gate valve 18, loads the substrate W into the processing chamber 10 of the plasma processing apparatus 1 through the load / unload port 17, and places the substrate W on the mounting table 11.
[0050] Next, in step S3, the control device 130 purges the processing vessel 10 (FIG. 5A, purge step ST1). The control device 130 supplies an inert gas, such as Ar gas, into the processing vessel 10 and controls the exhaust device 16 to purge the processing vessel 10 for 0.1 to 60 seconds while exhausting the gas within the processing vessel 10. This allows the conditions within the processing vessel 10 to be adjusted by exhausting the gas within the processing vessel 10. This purge step is performed from the second time onwards of the repeated process described below, and is referred to as "H 2This is an example of a second purge step for purging the inside of the processing vessel 10 after the "plasma treatment step (ST4)" and before the "precursor gas adsorption step (ST2)". The "precursor gas adsorption step (ST2)" is an example of a "step for forming an adsorption layer", and is a step for forming an adsorption layer by "H 2 The plasma treatment process (ST4) is an example of a process for forming a SiCN film.
[0051] Next, in step S5, the control device 130 supplies a first gas containing a precursor gas into the processing chamber 10 to be adsorbed onto the substrate W ( FIG. 5A , precursor gas adsorption step ST2). For example, TMCTS is supplied as the precursor gas, and gases other than the precursor gas contained in the first gas, such as Ar gas, He gas, and N gas, are also supplied. 2 At least one of the gases is supplied into the processing chamber 10 for 0.1 to 60 seconds, so that the precursor is adsorbed onto the substrate W, and an adsorption layer having Si—N bonds and Si—C bonds is formed on the substrate W.
[0052] Next, in step S7, the control device 130 purges the inside of the processing vessel 10 (FIG. 5A, purge step ST3). The control device 130 supplies an inert gas, such as Ar gas, into the processing vessel 10 and controls the exhaust device 16 to purge the inside of the processing vessel 10 while exhausting the gas for 0.1 to 60 seconds. This exhausts the gas inside the processing vessel 10, thereby adjusting the condition inside the processing vessel 10. This purge step is performed after the "step of forming an adsorption layer (ST2)" and is performed after the "H 2 This is an example of a first purge step for purging the inside of the processing vessel 10 before the plasma processing step (ST4).
[0053] Next, in step S9, the control device 130 2 A second gas containing the gas is supplied into the processing chamber 10, UHF wave power is supplied, and the substrate W is heated to H 2 The adsorbed layer is exposed to plasma to react with the adsorbed layer to form a SiCN film (Fig. 5A-H). 2 Plasma treatment step ST4). For example, H 2 Gas is supplied, and further, for example, Ar gas, He gas, N 2At least one of the gases is supplied into the processing chamber 10 for 0.1 to 60 seconds. 2 A second gas containing H 2 The adsorption layer is exposed to plasma to react with the adsorption layer, and Si-C bonds and Si-N bonds are inherited to form a SiCN film. 2 The adsorption layer is cut by the ion energy in the plasma. 2 By reacting with plasma, Si—N of Si—NH—R remains, and the set R is broken, and the C contained in the set R is removed. As a result, the SiCN film inherits Si—C bonds and Si—N bonds from the precursor gas, and a high-quality SiCN film can be formed.
[0054] Next, in step S11, the control device 130 determines whether the set number of times has been reached, and repeats steps S3 to S9 until the set number of times n has been reached, and terminates this processing when it determines in step S11 that the set number of times has been reached.
[0055] 5B shows a modified example of the method for forming a SiCN film according to one embodiment. Steps ST1, ST2, ST3-1, and ST4 in FIG. 5B are the same as steps ST1, ST2, ST3, and ST4 in FIG. 5A. In this modified example, in addition to these steps ST, step ST3-2, which is not shown in FIG. 5A, is also performed.
[0056] That is, after the purge step of ST3-1, 2 Before the plasma processing step, a step of evacuating the processing vessel 10 in ST3-2 may be further performed. In the evacuation step, the supply of purge gas is stopped, and the pressure inside the processing vessel 10 is controlled by the exhaust device 16 to a desired vacuum level. Steps ST1, ST2, ST3-1, ST3-2, and ST4 may be repeated a set number of times (e.g., 100 times) (repeated (1) in FIG. 5B). In this case, steps ST3-1 and ST3-2 may be repeated a predetermined number of times (e.g., twice) each time steps ST1, ST2, ST3-1, ST3-2, and ST4 are repeated (repeated (2) in FIG. 5B).
[0057] 5A and 5B, the process conditions for forming the SiCN film are as follows: However, the process conditions shown below are merely examples and are not limited to these.
[0058] [Experiment 1] An experiment was conducted on the quality of the SiCN film formed by the above-described SiCN film forming method, changing the pressure and the type of precursor gas.
[0059] <Process conditions> First gas: HMCTS, HMCTZ, BTBAS-MS, TMSI (precursor gas) Second gas: H 2 Gas, Ar gas, He gas, N 2 At least one of the gases Substrate temperature: 100° C. to 450° C. Pressure in the processing chamber: 10 Pa to 400 Pa Gap between the ceiling wall 10 a and the mounting table 11: 10 mm to 100 mm UHF wave frequency: 40 MHz to 3 GHz UHF wave power: 50 W to 5000 W
[0060] [Experimental Results] The film quality of the SiCN film formed by the SiCN film formation method will be described with reference to Figures 6 to 9. Figure 6 shows an example of experimental results of the composition and pressure dependence of the SiCN film formed using HMCTS as a precursor gas by the SiCN film formation method of Figure 4.
[0061] 6, the horizontal axis represents the pressure inside the processing vessel 10, and the vertical axis represents the composition of the formed SiCN film. The pressure inside the processing vessel 10 was set to 20 Pa, 40 Pa, and 133 Pa in the process of forming an adsorption layer using a first gas containing at least a precursor and the process of forming a SiCN film.
[0062] As a result, it was found that C (carbon) was contained in the film at all pressures of 20 Pa, 40 Pa, and 133 Pa. In the SiCN film formation method shown in Figure 4, C in set R was removed during film formation, and therefore C was present in the film, indicating that the Si-C bond contained in the precursor gas was inherited by the SiCN film.
[0063] It was also found that N (nitrogen) was contained in the film at any pressure of 20 Pa, 40 Pa, and 133 Pa. In other words, it was found that the Si—N bonds contained in the precursor gas were inherited by the SiCN film.
[0064] Furthermore, the concentration of C contained in the SiCN film changed depending on the pressure inside the processing vessel 10. From the results shown in Fig. 6, it was found that when the pressure inside the processing vessel 10 was low, about 20 Pa, ions collided with the substrate W in a state of strong ion energy, increasing the probability of breaking Si-C bonds.
[0065] FIG. 7 is a graph showing the relationship between the carbon concentration in the SiCN film and the film density when the SiCN film is formed by the SiCN film forming method of FIG. 4 using HMCTS and other precursor gases.
[0066] 7, the horizontal axis indicates the pressure in the process chamber 10 for each type of precursor gas, the left vertical axis indicates the carbon concentration in the formed SiCN film, and the right vertical axis indicates the film density of the formed SiCN film. The pressure in the process chamber 10 was set to 20 Pa and 40 Pa in the process of forming an adsorption layer using a first gas containing at least a precursor and the process of forming a SiCN film.
[0067] As a result, it was found that regardless of which precursor gas was used, the carbon concentration in the film was higher at 40 Pa than at 20 Pa. In the SiCN film formation method shown in Figure 4, C in set R was removed during film formation, and therefore C was present in the film, indicating that the Si-C bond contained in the precursor gas was inherited by the SiCN film.
[0068] It was also found that, regardless of which precursor gas was used, when the pressure was set to a low pressure (20 Pa), the carbon concentration in the film decreased, and the film density also decreased.
[0069] Therefore, in the process of forming an adsorption layer using a first gas containing a precursor and the process of forming a SiCN film, it is preferable to control the pressure inside the processing vessel 10 within a range of 10 Pa to 400 Pa. This allows at least some of the Si-C bonds and Si-N bonds contained in the precursor gas to be retained. As a result, the presence of Si-C bonds in the SiCN film allows for the formation of a high-quality SiCN film. Furthermore, it is preferable to control the pressure to an appropriate level within the above pressure range and further reduce the ion energy to avoid breaking the Si-C bonds. Furthermore, it is preferable to use a UHF wave frequency of 40 MHz or higher to generate high-density plasma. This further improves the film quality of the SiCN film.
[0070] Fig. 8 shows an XPS spectrum measured by X-ray photoelectron spectroscopy (XPS) of a SiCN film formed using HMCTS as a precursor gas by the SiCN film formation method of Fig. 4. In the experiment of Fig. 8, a SiCN film was formed by the SiCN film formation method of Fig. 4 using the above process conditions.
[0071] 8, the horizontal axis represents binding energy (eV), and the vertical axis represents XPS spectrum intensity (CPS). Line A in the figure represents the state of binding energy in the XPS spectrum of a film, with the SiCN film formed by controlling the pressure inside the processing vessel 10 to 40 Pa as the base. Line B represents the state of binding energy in the XPS spectrum of a SiCN film formed by controlling the pressure inside the processing vessel 10 to 20 Pa. Line C represents the state of binding energy in the XPS spectrum of a SiCN film formed by controlling the pressure inside the processing vessel 10 to 133 Pa.
[0072] According to this, at the bond energy of the XPS spectrum when the inside of the processing vessel 10 of line C is 133 Pa, the peak of the XPS spectrum showing the Si-C bond of the measured SiCN film is at a high position similar to the base of line A, and it was found that many Si-C bonds were inherited in the SiCN film similar to the base of line A. It was also found that the bonding state of C in the SiCN film was mainly Si-C bond, with some being C-C bond and / or C-H bond (C-C(H) in the figure). The C-C(H) peak of the SiCN film of line C was lower than the base of line A, and it was found that the film quality was even better than the base.
[0073] On the other hand, the peaks of the XPS spectrum for line B are low for both the Si-C bond and C-C(H) of the measured SiCN film, and it was found that the number of Si-C bonds inherited in the SiCN film is smaller than those of lines A and C. The results shown in Fig. 8 also show that when the pressure inside the processing vessel 10 becomes low at about 20 Pa, ions collide with the substrate with strong ion energy, increasing the probability of breaking the Si-C bond.
[0074] Fig. 9 is a diagram showing an example of experimental results of the composition and film characteristics of a SiCN film formed using HMCTS as a precursor gas by the SiCN film formation method of Fig. 4. In the experiment of Fig. 9, a SiCN film was formed by the SiCN film formation method of Fig. 4 using the above process conditions.
[0075] 9 shows the pressure inside the processing vessel 10 during film formation, the composition, composition ratio, RI, film density, and WER (wet etch rate) of the SiCN film. As shown in the results of FIG. 9, according to the SiCN film formation method of FIG. 4, the Si-C bonds and Si-N bonds of the precursor gas were inherited by the SiCN film, as shown by the composition and composition ratio of the SiCN film, at all pressures. Furthermore, the RI was roughly the same at all pressures, and did not change.
[0076] Furthermore, when the pressure was 40 Pa and 133 Pa, the C content in the SiCN film was 20% or more, which was more than three times that when the pressure was 20 Pa. Therefore, it was found that while the pressure in the processing vessel 10 during film formation should be controlled within the range of 10 Pa to 400 Pa, it is more preferable to control it to 40 Pa or more.
[0077] Generally, the higher the C content in the SiCN film, the lower the film density. The higher the film density, the better the film quality. For example, in an ALD apparatus that performs batch-type heat treatment, when the C content in the SiCN film is about 12%, the film density is about 2.6. In contrast, in the method of forming the SiCN film shown in FIG. 4, when the pressure inside the processing vessel 10 is 40 Pa and 133 Pa, the film density (g / cm) is about 2.6 even if the C content in the SiCN film is 20% or more. 3 ) was 2.8 or more, and a high-density SiCN film could be produced.
[0078] The WER (wet etch rate) indicates the amount (Å / min) of etching per minute when hydrofluoric acid is used at a concentration of 0.5%. The SiCN film was hardly removed when the pressure inside the processing vessel 10 was 20 Pa, 40 Pa, or 133 Pa. In other words, the SiCN film formed by the SiCN film forming method of FIG. 4 had sufficient film properties, including etching resistance (hydrofluoric acid resistance).
[0079] [Experiment 2] Next, an experiment was conducted to control the carbon concentration in the SiCN film. Fig. 10 is a flowchart showing an example of a method for forming a SiCN film used in this experiment. Fig. 11 is a diagram showing an example of a method for forming a SiCN film used in this experiment.
[0080] In the method of forming a SiCN film shown in FIG. 10, when ST1 to ST4 in FIG. 11 are repeated a first set number of times, H is applied once every second set number of times, which is less than the first set number of times. 2 After the plasma treatment step (ST4), a purge step (ST5) is performed. 2 The plasma treatment step (ST6) is carried out. 2 The plasma treatment is carried out by placing N 2 A third gas containing a gas and VHF or UHF wave power are supplied to generate plasma, and the substrate W is heated by N 2 This is an example of a modification process in which the material is modified by exposing it to plasma. This modification process is performed at a predetermined frequency while the steps ST1 to ST4 in FIG.
[0081] First, in step S1, the control device 130 opens the gate valve 18, loads the substrate W through the load / unload port 17, and places it on the mounting table 11. Next, in step S3, the control device 130 purges the processing vessel 10 (FIG. 11 ST1). For example, an inert gas such as Ar gas is supplied into the processing vessel 10, and the processing vessel 10 is purged while being evacuated by the exhaust device 16 for 0.1 to 60 seconds. This adjusts the conditions inside the processing vessel 10. This purge step is an example of a second purge step.
[0082] Next, in step S5, the control device 130 supplies a first gas containing a precursor gas into the processing chamber 10 and adsorbs it onto the substrate W (FIG. 11 ST2). For example, TMCTS is supplied as the precursor gas, and at least one of Ar gas, He gas, and N2 gas is supplied into the processing chamber 10 as a gas other than the precursor gas contained in the first gas for 0.1 to 60 seconds. This causes the precursor to be adsorbed onto the substrate W, and an adsorption layer having Si—N bonds and Si—C bonds is formed on the substrate.
[0083] Next, in step S7, the control device 130 purges the processing vessel 10 (ST3 in FIG. 11). For example, an inert gas such as Ar gas is supplied into the processing vessel 10, and the processing vessel 10 is purged while being exhausted by the exhaust device 16 for 0.1 to 60 seconds. This adjusts the conditions inside the processing vessel 10. This purge process is an example of a first purge process.
[0084] Next, in step S9, the control device 130 2 A second gas containing the gas is supplied into the processing chamber 10, UHF wave power is supplied, and the substrate W is heated to H 2 The adsorption layer is reacted with the plasma to form a SiCN film (FIG. 11 ST4). 2 Then, for example, at least one of Ar gas, He gas, and N2 gas is supplied into the processing chamber 10 for 0.1 to 60 seconds. 2 A second gas containing H 2The adsorption layer is exposed to plasma to react with the adsorption layer, and Si-C bonds and Si-N bonds are inherited to form a SiCN film. 2 The adsorption layer is cut by the ion energy in the plasma. 2 By reacting with plasma, Si-N of Si-NH-R remains, R is broken, and C other than Si-C bonds is removed. As a result, carbon in the SiCN film becomes Si-C bonds, and a high-quality SiCN film can be formed.
[0085] Next, in step S13, the control device 130 determines whether the first set number of times has been reached, and if the first set number of times has not been reached, the process immediately returns to step S3, and the processes from step S3 onwards are repeated.
[0086] When the first set number of times is reached in step S13 and the process proceeds to step S15, the control device 130 purges the processing vessel 10 (FIG. 11 ST5). For example, an inert gas such as Ar gas is supplied into the processing vessel 10, and the processing vessel 10 is purged while being exhausted by the exhaust device 16 for 0.1 to 60 seconds. This adjusts the conditions inside the processing vessel 10. This purge process is an example of a third purge process.
[0087] Next, in step S17, the control device 130 2 A third gas containing a gas is supplied into the processing chamber 10, and UHF wave power is supplied to heat the substrate. 2 The SiCN film is modified by exposing it to plasma (FIG. 11 ST6). 2 As a gas other than the gas, for example, at least one of Ar gas, He gas, and N2 gas is supplied into the processing chamber 10 for 0.1 to 60 seconds. 2 A third gas containing N 2 The SiCN film is modified by exposing it to plasma and reacting with the adsorption layer. 2 The plasma is not limited to UHF wave power, but may be VHF wave power, for example.
[0088] Next, in step S19, the control device 130 determines whether the second set number of times has been reached. The second set number of times is set to a number of times less than the first set number of times. As an example, the first set number of times is set to 5 to 300 times, and the second set number of times is set to 1 to 30 times. However, this is not limiting, and step S17 may be executed at a predetermined frequency while the processes of steps S3 to S9 are repeated. If the second set number of times has not been reached, the control device 130 immediately returns to step S3, and repeats the processes from step S3 onwards. If it is determined that the second set number of times has been reached, the process ends.
[0089] The main process conditions for the SiCN film formed by the above-described SiCN film forming method are as follows.
[0090] <Process conditions> First gas: THMCTS, HMCTZ, BTBAS-MS, TMSI (precursor gas) Second gas: H 2 Gas, Ar gas, He gas, N 2 At least one of the gases: a third gas: N 2 Gas Substrate temperature: 100° C. to 450° C. Pressure inside the processing chamber: 10 Pa to 400 Pa Gap between the ceiling wall 10 a and the mounting table 11: 10 mm to 100 mm UHF wave frequency: 40 MHz to 3 GHz UHF wave power: 50 W to 5000 W
[0091] [Experimental Results] FIG. 12 is a graph showing the relationship between the carbon concentration in the SiCN film and the film density of the SiCN film formed by the SiCN film forming method of FIG. 10 using precursor gases of HMCTS, HMCTZ, BTBAS-MS, and TMSI.
[0092] The horizontal axis of FIG. 12 represents the N concentration for each precursor gas type. 2 The left vertical axis indicates the carbon concentration in the SiCN film formed. The right vertical axis indicates the film density of the SiCN film formed. The modification frequency is calculated by H 2 N for plasma 2 The ratio of the number of times of plasma treatment (second set number of times / first set number of times, see FIG. 10) is 0 (N 2 The first set number of times was set to 1 / 50, 1 / 8, and 1 / 10, respectively. 2The second set number of times is the number of times (1) the plasma treatment step (ST4) is repeated. 2 This is the number of times (2) the plasma treatment step (ST6) is repeated.
[0093] As a result, N 2 It was found that the carbon concentration in the SiCN film can be adjusted and controlled by changing the frequency of the plasma modification treatment.
[0094] Also, N 2 By performing plasma modification treatment (FIG. 10 S17), N 2 The quality of the SiCN film can be improved compared to when the plasma modification treatment is not performed. It was found that these methods can maintain the film quality while controlling the carbon concentration in the SiCN film to a desired concentration.
[0095] As described above, according to the first and second embodiments of the SiCN film formation method, the Si-C bonds in the precursor gas can be inherited by the SiCN film formed on the substrate. This allows a high-quality SiCN film to be formed. Furthermore, by generating a high-frequency plasma with a high plasma density using VHF or UHF waves with a frequency of 100 MHz to 3 GHz, the quality of the SiCN film can be further improved.
[0096] Furthermore, N 2 According to the method for forming a SiCN film by performing a plasma modification treatment, N is applied at a predetermined frequency to adjust the C content in the SiCN film. 2 Plasma processing is performed, which makes it possible to adjust the concentrations of N and C in the SiCN film and to improve the film quality of the SiCN film.
[0097] The SiCN film forming method and plasma processing apparatus according to the presently disclosed embodiments should be considered to be illustrative and not restrictive in all respects. The embodiments can be modified and improved in various ways without departing from the spirit and scope of the appended claims. The matters described in the above embodiments can be configured in other ways as long as they are not inconsistent, and can be combined as long as they are not inconsistent.
[0098] The plasma processing apparatus of the present disclosure can be applied to any type of apparatus, including capacitively coupled plasma (CCP), inductively coupled plasma (ICP), radial line slot antenna (RLSA), electron cyclotron resonance plasma (ECR), and helicon wave plasma (HWP).
[0099] This international application claims priority based on Japanese Patent Application No. 2023-050889, filed on March 28, 2023, the entire contents of which are incorporated herein by reference.
[0100] REFERENCE SIGNS LIST 1 plasma processing apparatus 2 plasma source 10 processing vessel 11 mounting table 130 control device
Claims
(b) supplying a first gas containing a precursor gas having Si-N bonds and Si-C bonds into the processing vessel to form an adsorption layer on the substrate, the Si-N bonds and Si-C bonds not being activated in the formation of the adsorption layer, (c) a first purging step of purging the processing vessel after the step (b), (d) supplying a second gas containing hydrogen gas and VHF or UHF wave power into the processing vessel to generate plasma, and exposing the substrate to the plasma to react with the adsorption layer to form a SiCN film, the SiCN film inheriting at least a portion of the Si-C bonds and Si-N bonds of the adsorption layer, and (e) a second purging step of purging the processing vessel after the step (d), wherein the steps (b) to (e) are repeated.
2. The method for forming a SiCN film according to claim 1, wherein the precursor gas does not have a Si-Si bond.
3. The method for forming a SiCN film according to claim 1, wherein the frequency of the VHF wave or UHF wave is within the range of 100 MHz to 3 GHz.
4. The method for forming a SiCN film according to any one of claims 1 to 3, wherein in steps (b) and (d), the pressure inside the processing vessel is within a range of 10 Pa to 400 Pa.
5. The method for forming a SiCN film according to any one of claims 1 to 3, wherein the second gas includes an inert gas.
6. The inert gas is Ar gas, He gas, N 2 The method for forming a SiCN film according to claim 5 , wherein the gas is selected from at least one of the following gases:
7. The method for forming a SiCN film according to any one of claims 1 to 3, further comprising the step of: (f) evacuating the processing vessel after the step (c) and before the step (d).
8. The method for forming a SiCN film according to claim 7, further comprising repeating steps (c) and (f) a predetermined number of times, and then carrying out step (d).
9. The method for forming a SiCN film according to any one of claims 1 to 3, wherein the precursor gas is selected from one of HMCTS, HMCTZ, TMSI, BTBAMS, BSBAMS, BTBAES, and BTBAVS.
10. The method for forming a SiCN film according to any one of claims 1 to 3, wherein the temperature of the substrate is 450°C or less.
11. A method for forming a SiCN film according to any one of claims 1 to 3, further comprising: (g) a modification step of supplying a third gas containing nitrogen gas and VHF or UHF power into the processing vessel to generate plasma, and exposing the substrate to the plasma for modification.
12. The method for forming a SiCN film according to claim 11, wherein the step (g) is performed at a predetermined frequency while the steps (b) to (e) are repeated.
13. A plasma processing apparatus comprising a processing vessel and a control device, the control device controlling the method of forming a SiCN film according to claim 1.
Citation Information
Patent Citations
Method of forming insulation film and apparatus of forming the insulation film
JP2003179054A
Manufacturing method of semiconductor device, substrate processing apparatus, and program
JP2019110263A
Semiconductor device manufacturing method, substrate processing apparatus, and program
JP2020043281A
Silicon carbonitride gap fillers with tunable carbon content
JP2023507326A
Method for Forming Silicon-Containing Dielectric Film by Cyclic Deposition with Side Wall Coverage Control
US20130330933A1