Mixture of cyclic acid anhydrides, method for producing same, curable resin composition, and cured products of these

A mixture of cyclic acid anhydrides with optimized peak area ratios, produced via an addition reaction, addresses the challenges of slow crystallization and low thermal stability in curable resin compositions, achieving enhanced heat resistance and handling properties for carbon fiber reinforced materials.

WO2024203425A1PCT designated stage expired Publication Date: 2024-10-03NIPPON KAYAKU CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/010149
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2024-03-15
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Cyclic acid anhydrides used in curable resin compositions for applications like carbon fiber reinforced materials face issues with slow crystallization rates, poor handling properties, and low heat resistance, which affect their thermal and dimensional stability.

Method used

A mixture of cyclic acid anhydrides with specific peak area ratios, produced through an addition reaction between 1,3-p-mentadiene and maleic anhydride, is formulated to enhance crystallization rates and thermal stability, allowing for improved handling and processing into forms like pellets or marbles, and inclusion in a curable resin composition with an epoxy resin and curing accelerator.

Benefits of technology

The resulting curable resin composition exhibits excellent heat resistance and dimensional stability, suitable for carbon fiber reinforced composite materials, with an inexpensive production method and improved handling properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024010149_03102024_PF_FP_ABST
    Figure JP2024010149_03102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention provides: a mixture of cyclic acid anhydrides having excellent heat resistance and dimensional stability; a curable resin composition; and a method for producing the mixture of cyclic acid anhydrides. This mixture of cyclic acid anhydrides comprises a cyclic acid anhydride represented by formula (A-a), a cyclic acid anhydride represented by formula (A-b) and a cyclic acid anhydride represented by formula (A-c). If the total peak area for cyclic acid anhydrides represented by the formulae (A-a) to (A-c) is taken to be 100% when the mixture of cyclic acid anhydrides is analyzed using gas chromatography, the peak area of the cyclic acid anhydride represented by the formula (A-a) is 0.1-1.0%, the peak area of the cyclic acid anhydride represented by the formula (A-b) is 98.0-99.0%, and the peak area of the cyclic acid anhydride represented by the formula (A-c) is 0.1-1.0%.
Need to check novelty before this filing date? Find Prior Art

Description

Cyclic acid anhydride mixture, method for producing the same, curable resin composition, and cured product thereof

[0001] The present invention relates to a mixture of cyclic acid anhydrides, a curable resin composition, and a cured product thereof, which are suitable for use in electrical and electronic components such as semiconductor encapsulants, printed wiring boards, and build-up laminates, lightweight, high-strength materials such as carbon fiber reinforced plastics and glass fiber reinforced plastics, 3D printing applications, and adhesives.

[0002] Epoxy resins are widely used in various fields due to their excellent mechanical strength, heat resistance, adhesiveness, gas barrier properties, etc. It has been well known that acid anhydrides are effective as curing agents for epoxy resins, and acid anhydrides have been used in applications such as small-scale casting, large-scale casting, impregnation molding, and powder coatings because they are less toxic and odorous than amine-based curing agents, and they generate less heat and shrink less during curing.

[0003] Many of the hardeners used, such as epoxy resins and acid anhydrides, have been derived from petroleum. However, in recent years, concerns have arisen about the depletion of petroleum resources, and methods of recycling many of these materials, such as using renewable resources such as plants, or decomposing the hardened materials, are being considered.

[0004] JP 55-118920 A JP 01-167326 JP 07-018059 JP 2014-025036

[0005] Patent Documents 1 to 4 describe 1-isopropyl-4-methyl-bicyclo[2.2.2]oct-5-ene-2,3-dicarboxylic anhydride, which is synthesized by an addition reaction of 1,3-p-menthadiene, a renewable resource such as a plant, with maleic anhydride. The applicant of the present application produced 1-isopropyl-4-methyl-bicyclo[2.2.2]oct-5-ene-2,3-dicarboxylic anhydride using the method described in these documents, but found that the crystallization rate was slow.

[0006] When the crystallization rate is slow, the liquid is generally placed in a container such as a drum and allowed to crystallize over time, after which it is crushed from the outside of the drum or container with a hammer or the like, or heated and melted in an oven or the like before use, which makes it very difficult to handle.

[0007] On the other hand, if the crystallization rate is fast, it becomes possible to process the material into pellets, granules, or marbles, which significantly improves handling.Furthermore, if the crystallization rate is fast, it becomes possible to process the material into granules or marbles by dropping the liquid droplets onto a conveyor and cooling them during transport.

[0008] Furthermore, it has become clear that the curable resin composition containing the acid anhydride has a problem in that the heat resistance (Tg) of the cured product is low and the linear expansion coefficient is large, resulting in thermal shrinkage when the cured product is removed from the mold and cooled to room temperature. Therefore, in order to use the curable resin composition in a carbon fiber reinforced composite material, it is necessary to improve the thermal stability and dimensional stability.

[0009] The present invention has been made in view of the above-mentioned problems, and aims to provide a cyclic acid anhydride mixture, a curable resin composition, and a method for producing the cyclic acid anhydride mixture, which are excellent in heat resistance and dimensional stability.

[0010] That is, the present invention provides the following [1] to [7]. In the present invention, "(Numerical value 1) to (Numerical value 2)" indicates that the upper and lower limits are included. [1] A mixture of cyclic acid anhydrides comprising a cyclic acid anhydride represented by the following formula (A-a), a cyclic acid anhydride represented by the following formula (A-b), and a cyclic acid anhydride represented by the following formula (A-c), wherein, when the sum of the peak areas of the cyclic acid anhydrides represented by the formulas (A-a) to (A-c) is taken as 100% when the mixture of cyclic acid anhydrides is analyzed by gas chromatography, the peak area of ​​the cyclic acid anhydride represented by the formula (A-a) is 0.1% to 1.0%, the peak area of ​​the cyclic acid anhydride represented by the formula (A-b) is 98.0% to 99.0%, and the peak area of ​​the cyclic acid anhydride represented by the formula (A-c) is 0.1% to 1.0%.

[0011]

[0012] [2] The cyclic acid anhydride mixture according to the preceding item [1], which, after dissolving at 80°C, crystallizes in 0.1 to 1.5 hours when allowed to stand at 10°C. [3] The cyclic acid anhydride mixture according to the preceding item [1] or [2], is in the form of pellets, granules, or marbles. [4] A curable resin composition comprising the cyclic acid anhydride mixture according to any one of the preceding items [1] to [3], an epoxy resin, and a curing accelerator. [5] A cured product obtained by curing the curable resin composition according to the preceding item [4]. [6] A carbon fiber reinforced composite material obtained by curing the curable resin composition according to the preceding item [4]. [7] A method for producing the cyclic acid anhydride mixture according to any one of the preceding items [1] to [3], by reacting 1,3-p-menthadiene, maleic anhydride, and a solvent at 40 to 80°C, and then concentrating the solvent.

[0013] According to the present invention, it is possible to provide a cyclic acid anhydride mixture and a curable resin composition having excellent heat resistance and dimensional stability, and also to provide an inexpensive method for producing the cyclic acid anhydride mixture.

[0014] The cyclic acid anhydride mixture of this embodiment comprises a cyclic acid anhydride represented by the following formula (A-a), a cyclic acid anhydride represented by the following formula (A-b), and a cyclic acid anhydride represented by the following formula (A-c). When analyzed by gas chromatography, when the sum of the peak areas of the cyclic acid anhydrides represented by formulas (A-a) to (A-c) is taken as 100%, the peak area of ​​the cyclic acid anhydride represented by formula (A-a) is 0.1% to 1.0%, the peak area of ​​the cyclic acid anhydride represented by formula (A-b) is 98.0% to 99.0%, and the peak area of ​​the cyclic acid anhydride represented by formula (A-c) is 0.1% to 1.0%. The cyclic acid anhydride mixture has a fast crystallization rate and can be provided in the form of pellets, granules, or marbles. Furthermore, it can be used for carbon fiber reinforced composite materials with high heat resistance and dimensional stability.

[0015]

[0016] When the mixture of cyclic acid anhydrides is analyzed by gas chromatography, the peak area of ​​the cyclic acid anhydride represented by formula (A-a) is preferably 0.1% or more and 1.0% or less, more preferably 0.1% or more and 0.8% or less, and particularly preferably 0.1% or more and 0.5% or less, when the sum of the peak areas of the cyclic acid anhydrides represented by formulas (A-a) to (A-c) is taken as 100%.

[0017] When the mixture of cyclic acid anhydrides is analyzed by gas chromatography, the peak area of ​​the cyclic acid anhydride represented by formula (A-b) is preferably 98.0% or more and 99.0% or less, more preferably 98.5% or more and 99.0% or less, and particularly preferably 98.8% or more and 99.0% or less, when the sum of the peak areas of the cyclic acid anhydrides represented by formulas (A-a) to (A-c) is taken as 100%.

[0018] When the mixture of cyclic acid anhydrides is analyzed by gas chromatography, the peak area of ​​the cyclic acid anhydride represented by formula (A-c) is preferably 0.1% or more and 1.0% or less, more preferably 0.1% or more and 0.8% or less, and particularly preferably 0.1% or more and 0.5% or less, when the sum of the peak areas of the cyclic acid anhydrides represented by formulas (A-a) to (A-c) is taken as 100%.

[0019] The gas chromatography analysis was carried out under the following conditions: Gas chromatography (GC) measurement apparatus: 8890GC System (manufactured by Agilent Technologies) Column: HP-5MS (manufactured by Agilent Technologies) Column flow rate: 1.2 ml / min Oven: 100°C (2 min) - 5°C / min - 300°C (3 min) Injection port: 300°C, injection amount 1.0 μl Detector: FID (300°C)

[0020] The cyclic acid anhydride mixture of this embodiment can be easily obtained by addition reaction of 1,3-p-menthadiene with maleic anhydride. The addition reaction conditions are the same as those of a typical Diels-Alder reaction. In other words, the reaction ratio is preferably approximately a molar equivalent of 1,3-p-menthadiene to maleic anhydride, or a slight excess.

[0021] The reaction may be carried out using a suitable solvent for the reaction system, such as an aromatic hydrocarbon or an alicyclic hydrocarbon (e.g., n-heptane, benzene, toluene, xylene, cyclohexane, etc.). The reaction temperature is preferably 40 to 80°C, more preferably 40 to 70°C, and particularly preferably 45 to 65°C.

[0022] The cyclic acid anhydride mixture of this embodiment may be in any state, such as a solid, molten, or solution, but is preferably in a solid state, and more preferably in the form of pellets, granules, or marbles, from the viewpoint of uniform crystallization and ease of handling.

[0023] The method for forming into pellets, granules, or marbles is not particularly limited, but examples of pellet manufacturing equipment include a belt drum flaker manufactured by Nippon Coke Engineering Co., Ltd., a steel belt conveyor manufactured by Nippon Steel Conveyor Co., Ltd., and a flaker manufactured by Mitsubishi Material Techno Corp. The size of the pellets, granules, or marbles is not particularly limited, but taking into consideration handling during the manufacturing process and secondary molding, a size of 0.1 mm to 10 mm is preferred, and 1 mm to 5 mm is more preferred.

[0024] The melting point of the cyclic acid anhydride mixture of this embodiment is preferably 60 to 80° C., more preferably 61.5 to 80° C. The crystallization rate measured under the following conditions is preferably 0.1 to 1.5 hours, more preferably 0.5 to 1.5 hours.

[0025] The crystallization rate in this embodiment was measured under the following conditions: <Crystallization rate measurement conditions> The cyclic acid anhydride mixture was left to dissolve in an oven at 80°C for 1 hour, and then 0.02 g of the solution of the dissolved cyclic acid anhydride mixture was dropped into a tray maintained at 10°C and left to stand, and the time until the transparent liquid crystallized and completely turned cloudy and solidified was measured.

[0026] The curable resin composition of this embodiment contains the cyclic acid anhydride mixture, an epoxy resin, and a curing accelerator. The epoxy resin is not particularly limited and can be appropriately selected from commonly used epoxy resins. Among these, an epoxy resin having two or more epoxy groups per molecule is preferred. Examples of epoxy resins having two or more epoxy groups per molecule include various polyfunctional epoxy resins such as naphthalene type, phenol novolac type, cresol novolac type, phenol aralkyl type, biphenyl type, hydroxybenzaldehyde type, dicyclopentadiene type, glycidyl ester type, glycidyl amine type, hydantoin type, and isocyanurate type. These epoxy resins may be used alone or in combination of two or more types.

[0027] The epoxy equivalent of the epoxy resin is not particularly limited. From the viewpoint of the heat resistance and water absorbency of the cured product, it is preferably 100 to 350 (g / eq), and more preferably 150 to 300 (g / eq).

[0028] From the viewpoints of heat resistance, electrical properties, and water absorbency, the epoxy resin is preferably at least one polyfunctional epoxy resin selected from the group consisting of dicyclopentadiene type, o-cresol novolac type, naphthalene type, biphenyl type, phenol aralkyl type, and trisphenolmethane type, and has an epoxy equivalent of 100 to 350 (g / eq), and more preferably at least one polyfunctional epoxy resin selected from the group consisting of dicyclopentadiene type, o-cresol novolac type, naphthalene type, and trisphenolmethane type, and has an epoxy equivalent of 150 to 300 (g / eq).

[0029] The content of the epoxy resin in the curable resin composition is not particularly limited, but from the viewpoint of moldability and heat resistance, it is preferably 10 wt % to 80 wt %, and more preferably 40 wt % to 50 wt %, of the total weight of the curable resin composition.

[0030] In the curable resin composition of this embodiment, the amount of the cyclic acid anhydride mixture used is preferably 0.7 to 1.2 equivalents relative to 1 equivalent of the epoxy group of the epoxy resin. If the amount is less than 0.7 equivalents relative to 1 equivalent of the epoxy group or if it exceeds 1.2 equivalents, curing may be incomplete and good cured physical properties may not be obtained.

[0031] In addition to the cyclic acid anhydride mixture, the curable resin composition may further contain another curing agent as needed. The other curing agent can be appropriately selected from curing agents commonly used in curable resin compositions. Examples of the other curing agent include an acid anhydride compound other than the cyclic acid anhydride mixture, a phenolic resin, etc.

[0032] Examples of acid anhydride compounds other than the mixture of cyclic acid anhydrides include phthalic anhydride, maleic anhydride, trimellitic anhydride, pyromellitic anhydride, hexahydrophthalic anhydride, tetrahydrophthalic anhydride, methylnadic anhydride, nadic anhydride, glutaric anhydride, dimethylglutaric anhydride, diethylglutaric anhydride, succinic anhydride, methylhexahydrophthalic anhydride, methyltetrahydrophthalic anhydride, etc. Among these, at least one selected from the group consisting of phthalic anhydride, trimellitic anhydride, hexahydrophthalic anhydride, tetrahydrophthalic anhydride, methylhexahydrophthalic anhydride, methyltetrahydrophthalic anhydride, glutaric anhydride, dimethylglutaric anhydride, and diethylglutaric anhydride is preferred. Furthermore, from the viewpoint of handling and workability of the curable resin composition, acid anhydride compounds that are solid at room temperature are preferred.

[0033] The gel time of the curable resin composition of this embodiment can also be adjusted by using a curing accelerator. Examples of curing accelerators that can be used include imidazoles such as 2-methylimidazole, 2-ethylimidazole, and 2-ethyl-4-methylimidazole; tertiary amines such as 2-(dimethylaminomethyl)phenol and 1,8-diaza-bicyclo[5.4.0]undecene-7; phosphines such as triphenylphosphine; and metal compounds such as tin octoate. The curing accelerator is used in an amount of 0.01 to 5.0 parts by weight per 100 parts by weight of the epoxy resin, as needed.

[0034] The curable resin composition of the present embodiment may further contain various additives exemplified below as needed. However, the curable resin composition of the present embodiment is not limited to the additives listed below, and may contain various additives well known in the technical field as needed.

[0035] The curable resin composition of this embodiment may further contain a flame retardant, if necessary, to impart flame retardancy. The flame retardant is not particularly limited, and examples thereof include phosphorus compounds such as red phosphorus coated with a thermosetting resin such as a phenolic resin, phosphoric acid esters, and triphenylphosphine oxide; nitrogen-containing compounds such as melamine, melamine derivatives, melamine-modified phenolic resins, compounds having a triazine ring, cyanuric acid derivatives, and isocyanuric acid derivatives; phosphorus and nitrogen-containing compounds such as cyclophosphazene; metal complex compounds such as dicyclopentadienyl iron; zinc compounds such as zinc oxide, zinc stannate, zinc borate, and zinc molybdate; metal oxides such as iron oxide and molybdenum oxide; and metal hydroxides such as aluminum hydroxide and magnesium hydroxide. Examples of the flame retardant include known organic or inorganic compounds and metal hydroxides containing a halogen atom, antimony atom, nitrogen atom, or phosphorus atom.

[0036] The curable resin composition of the present embodiment may further contain an inorganic filler as needed. Specific examples of the inorganic filler include fine powders of fused silica, crystalline silica, glass, alumina, calcium carbonate, zirconium silicate, calcium silicate, silicon nitride, aluminum nitride, boron nitride, beryllia, zirconia, zircon, fosterite, steatite, spinel, mullite, titania, talc, clay, mica, etc., and beads obtained by spheronizing these powders.

[0037] Inorganic fillers having a flame retardant effect may be used, such as aluminum hydroxide, magnesium hydroxide, composite metal hydroxides such as composite hydroxides of magnesium and zinc, and zinc borate.

[0038] When the curable resin composition contains an inorganic filler, its content is not particularly limited as long as the effects of this embodiment can be obtained. The content of the inorganic filler is preferably 50 wt% or more based on the total weight of the curable resin composition, and from the viewpoint of flame retardancy, it is more preferably 60 wt% to 95 wt%, and even more preferably 70 wt% to 90 wt%. By including an inorganic filler, the thermal expansion coefficient, thermal conductivity, elastic modulus, etc. of the cured product can be improved to desired properties. When the content of the inorganic filler is 50 wt% or more, the effect of improving these properties can be more effectively obtained. Furthermore, when it is 95 wt% or less, the increase in viscosity of the curable resin composition is further suppressed, sufficient fluidity is easily obtained, and moldability is further improved.

[0039] The curable resin composition of the present embodiment may further contain an antioxidant as needed. This can prevent oxidation of the cured product of the curable resin composition, and can suppress weight loss of the cured product even when left in a high-temperature environment. Electrical properties are further improved.

[0040] Examples of the antioxidant include phenol-based antioxidants, phosphite-based antioxidants, sulfur-based antioxidants, hindered amine-based antioxidants, etc. These antioxidants may be used alone or in combination of two or more.

[0041] When the curable resin composition contains an antioxidant, the content thereof is not particularly limited as long as the weight loss suppression effect is achieved. From the viewpoint of the heat resistance (high Tg) of the curable resin composition, the content of the antioxidant is preferably 0.5 to 20 parts by weight, and more preferably 1 to 10 parts by weight, of the total amount of antioxidant per 100 parts by weight of the total amount of epoxy resin. By setting the content of the antioxidant to 0.5 parts by weight or more, the weight loss suppression effect of the cured product can be sufficiently obtained, and by setting the content of the antioxidant to 20 parts by weight or less, a decrease in the heat resistance (high Tg) of the cured product can be suppressed.

[0042] The curable resin composition of this embodiment may further contain a coupling agent, if necessary. This further improves the adhesion between the resin component and the inorganic filler, and further improves the electrical properties. The coupling agent can be appropriately selected from commonly used compounds. Examples of the coupling agent include known coupling agents such as various silane-based compounds such as epoxysilane, mercaptosilane, aminosilane, alkylsilane, ureidosilane, vinylsilane, styrylsilane, methacrylsilane, acrylicsilane, and sulfidosilane, titanium-based compounds, aluminum chelate compounds, and aluminum / zirconium-based compounds. Among these, silane-based compounds are preferred. These coupling agents may be used alone or in combination of two or more.

[0043] When the curable resin composition contains a coupling agent, the content thereof is preferably 0.05 to 5.0 parts by weight, and more preferably 0.1 to 4.5 parts by weight, relative to 100 parts by weight of the total amount of the inorganic filler. By making the content 0.05 parts by weight or more, the adhesion to the frame, etc. is further improved.

[0044] The method for preparing the curable resin composition of this embodiment is not particularly limited, and the components may be simply mixed uniformly, or may be prepolymerized. For example, a mixture containing the compound of this embodiment is heated in the presence or absence of a curing accelerator or a polymerization initiator, and in the presence or absence of a solvent, to form a prepolymer. Similarly, compounds such as amine compounds, compounds having ethylenically unsaturated bonds, maleimide compounds, cyanate ester compounds, polybutadiene and its modified products, polystyrene and its modified products, inorganic fillers, and other additives may be added to form a prepolymer. The components may be mixed or prepolymerized using, for example, an extruder, kneader, or rolls in the absence of a solvent, or a reaction kettle equipped with a stirrer in the presence of a solvent.

[0045] The curable resin composition of the present embodiment can be obtained by uniformly mixing the above-mentioned components. The method for producing the curable resin composition of the present embodiment is not particularly limited, but the composition can be obtained, for example, by thoroughly mixing an epoxy resin with a curing agent, a curing accelerator, an inorganic filler, a mold release agent, a silane coupling agent, additives, etc., using an extruder, kneader, rolls, planetary mixer, etc. until the mixture is uniform.

[0046] The obtained curable resin composition can be molded into various forms such as a resin sheet, a prepreg, etc. A prepreg form can be obtained, for example, by heating and melting the curable resin composition and / or a resin sheet of the present embodiment to reduce the viscosity and impregnating the composition into a fiber substrate.

[0047] The curable resin composition of this embodiment can also be dissolved in a solvent such as toluene, xylene, acetone, methyl ethyl ketone, methyl isobutyl ketone, dimethylformamide, dimethylacetamide, or N-methylpyrrolidone, as needed, to form a varnish-like composition (hereinafter simply referred to as a varnish), which can then be impregnated into a substrate such as glass fiber, carbon fiber, polyester fiber, polyamide fiber, alumina fiber, or paper, and dried by heating to produce a prepreg. In this case, the solvent is used in an amount that accounts for 10 to 70 wt %, preferably 15 to 70 wt %, of the mixture of the curable resin composition of this embodiment and the solvent.

[0048] The prepreg is cut into a desired shape, laminated, and then the epoxy resin composition is heat-cured while applying pressure to the laminate by press molding, autoclave molding, sheet winding molding, etc., to obtain a carbon fiber reinforced plastic (CFRP). Copper foil or an organic film can also be laminated during the lamination of the prepreg.

[0049] In addition to the above-mentioned methods, CFRP can also be obtained by molding using known methods, such as resin transfer molding (RTM), in which a carbon fiber substrate (usually a carbon fiber fabric) is cut, laminated, and shaped to produce a preform (a preform before being impregnated with resin), the preform is placed in a mold, the mold is closed, resin is injected to impregnate the preform, and the resin is cured, and the mold is then opened to remove the molded product. Also usable are types of RTM methods, such as the VaRTM method, the SCRIMP (Seeman's Composite Resin Infusion Molding Process), and the CAPRI (Controlled Atmospheric Pressure Resin Infusion) method, which is described in JP-A-2005-527410, in which a resin supply tank is evacuated to a pressure lower than atmospheric pressure, cyclic compression is used, and the net molding pressure is controlled to more appropriately control the resin injection process, particularly the VaRTM method. Furthermore, a film stacking method in which a fiber substrate is sandwiched between resin sheets (films), a method in which powdered resin is attached to a reinforcing fiber substrate to improve impregnation, a molding method in which a fluidized bed or fluid slurry method is used in the process of mixing resin into a fiber substrate (Powder Impregnated Yarn), and a method in which resin fibers are mixed into a fiber substrate can also be used.

[0050] Examples of carbon fibers include acrylic, pitch, and rayon carbon fibers, and among these, acrylic carbon fibers, which have high tensile strength, are preferably used. The carbon fiber may be in the form of twisted yarn, untwisted yarn, or non-twisted yarn, but untwisted yarn or non-twisted yarn is preferred because it provides a good balance between the formability and strength properties of the fiber-reinforced composite material.

[0051] The cured product of the curable resin composition of the present embodiment can be used for various applications other than the above-mentioned applications such as CFRP, and examples thereof include adhesives, paints, coating agents, molding materials (including sheets, films, CFRP, etc.), encapsulants for semiconductor elements, encapsulants for liquid crystal display elements, encapsulants for organic EL elements, electric and electronic parts such as printed wiring boards (BGA substrates, build-up substrates, etc.), 3D printing, and additives for other resins, etc.

[0052] Examples of the adhesive include adhesives for civil engineering, construction, automobiles, general office use, and medical use, as well as adhesives for electronic materials. Among these, adhesives for electronic materials include interlayer adhesives for multilayer substrates such as build-up substrates, die bonding agents, semiconductor adhesives such as underfills, underfills for reinforcing BGAs, and mounting adhesives such as anisotropic conductive films (ACFs) and anisotropic conductive pastes (ACPs), and are applicable to a variety of uses.

[0053] When the curable resin composition of this embodiment is applied to an encapsulant for semiconductor elements, a lead frame equipped with a semiconductor element or a semiconductor package substrate is placed in a mold, and the curable resin composition of this embodiment is molded by a melt casting method, transfer molding method, injection molding method, compression molding method, or the like, and further heated for 2 to 10 hours at 80 to 200° C. to obtain a cured product. Examples of semiconductor devices manufactured using this encapsulant include potting, dipping, and transfer mold encapsulation for capacitors, transistors, diodes, light-emitting diodes, ICs, and LSIs, potting encapsulation for COB, COF, TAB, and the like for ICs and LSIs, underfill for flip chips, and encapsulation (including reinforcing underfill) when mounting IC packages such as QFP, BGA, and CSP.

[0054] When the curable resin composition of this embodiment is applied to printed wiring boards, it can be heated and melted to reduce viscosity, and then impregnated into reinforcing fibers such as glass fibers and polyamide fibers to obtain a prepreg. Specific examples include, but are not limited to, glass fibers such as E-glass cloth, D-glass cloth, S-glass cloth, Q-glass cloth, spherical glass cloth, NE-glass cloth, and T-glass cloth, and / or organic fibers. The shape of the substrate is not particularly limited, but examples include woven fabric, nonwoven fabric, roving, chopped strand mat, and the like. Known weaving methods for woven fabrics include plain weave, sieve weave, and twill weave, and these known methods can be appropriately selected depending on the intended application and performance. Furthermore, woven fabrics that have been opened or surface-treated with a silane coupling agent or the like are preferably used. The thickness of the substrate is not particularly limited, but is preferably approximately 0.01 to 0.4 mm. Furthermore, a prepreg can be obtained by impregnating reinforcing fibers with the varnish and drying them under heat, and a copper clad laminate (CCL) can be produced from this. A laminate can also be produced using the curable resin composition of this embodiment by hot-press molding the obtained prepreg and CCL. The laminate is not particularly limited as long as it comprises one or more prepregs, and may also have any other layer. Furthermore, a sheet-like adhesive can be obtained by applying the varnish to a release film, removing the solvent under heat, and B-staging the adhesive. This sheet-like adhesive can be used as an interlayer insulating layer in a multilayer substrate or as an adhesive sheet for mounting semiconductors. The curable resin composition of this embodiment can also be suitably used for special substrate materials such as package substrates and HDIs (high density interconnects).

[0055] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. Unless otherwise specified, parts are parts by weight.

[0056] Various analytical methods were performed under the following conditions: GC / MS measurement (EI, CI) Instrument: GC-2020Plus / GCMS-QP2020 (Shimadzu Corporation) Column: HP-5MS (Agilent Technologies) Column flow rate: 1.2 ml / min Oven: 50°C (2 min) - 10°C / min - 300°C (18 min) Mass range: m / z 35-800 Ion source: 230°C Injection port: 320°C, injection volume 1.0 μl

[0057] GC measurement equipment: 8890GC System (Agilent Technologies) Column: HP-5MS (Agilent Technologies) Column flow rate: 1.2 ml / min Oven: 100°C (2 min) - 5°C / min - 300°C (3 min) Injection port: 300°C, injection volume 1.0 μl Detector: FID (300°C)

[0058] Synthesis Example 1 49.1 parts of toluene and 25.8 parts of α-terpinene (1,3-p-menthadiene, manufactured by Guangxi Jie Xin Fragrance Co., Ltd.) were placed in a four-neck flask and stirred while heating to 45°C. To this solution, 16.7 parts of maleic anhydride manufactured by Junsei Chemical Co., Ltd. were added in four portions over a period of 1 hour. After the addition was complete, the mixture was stirred at 45°C for 1 hour. After the reaction was complete, the mixture was concentrated under reduced pressure at 185°C to obtain 37 parts of a cyclic acid anhydride mixture (A-1).

[0059] Synthesis Example 2 35 parts of a cyclic acid anhydride mixture (A-2) was obtained in the same manner as in Synthesis Example 1, except that the reaction temperature was changed to 65°C.

[0060] Synthesis Example 3 37 parts of a cyclic acid anhydride mixture (A-3) was obtained in the same manner as in Synthesis Example 1, except that the reaction temperature was changed to 85° C. and toluene was not used.

[0061] Synthesis Example 4 34 parts of a cyclic acid anhydride mixture (A-4) was obtained in the same manner as in Synthesis Example 1, except that the reaction temperature was changed to 185° C. and toluene was not used.

[0062] The structures of the mixtures of cyclic acid anhydrides obtained in Synthesis Examples 1 to 4 were identified by GC / MS measurement, and the results of area percentages, when the sum of the peak areas of the cyclic acid anhydrides represented by formulae (A-a) to (Ac) measured by GC measurement is set to 100%, are shown in Table 1.

[0063] The melting point and crystallization rate were measured under the following conditions. <Conditions for Melting Point Measurement> Differential Scanning Calorimeter: CHIP DSC manufactured by Linseis Gas flow rate: N 2 Gas 50 ml / min Heating rate: 20°C / min Measurement temperature range: 30°C-270°C

[0064] <Conditions for measuring crystallization rate> The mixtures of cyclic acid anhydrides obtained in Synthesis Examples 1 to 4 were allowed to stand in an oven at 80°C for 1 hour to dissolve. 0.02 g of a solution in which the mixture of cyclic acid anhydrides was dissolved was added dropwise to a saucer maintained at 10°C and allowed to stand. The time until the transparent liquid crystallized and completely turned cloudy and solidified was measured.

[0065]

[0066] [Example 1, Comparative Examples 1 and 2] The mixtures of cyclic acid anhydrides obtained in Synthesis Examples 1 to 4, epoxy resins, and curing accelerators were mixed in the weight ratios shown in Table 2, and cured at 120°C for 2 hours, followed by 160°C for 6 hours to produce cured products. Physical properties were evaluated under the following conditions.

[0067] <Conditions for measuring heat resistance (Tg) and linear expansion coefficient> Thermomechanical analyzer: TMA Q400 (TA Instruments) Measurement temperature range: 30 to 350°C Heating rate: 2°C / min Tg: change point of linear expansion coefficient Linear expansion coefficient (CTE): change in unit dimension in the ranges of 50-90°C and 260-290°C Standard: Compliant with JIS K-7244

[0068]

[0069] RE-310S: Bisphenol A type epoxy resin (manufactured by Nippon Kayaku Co., Ltd.) 2E4MZ: 2-ethyl-4-methylimidazole (manufactured by Shikoku Chemicals Co., Ltd.)

[0070] As shown in Tables 1 and 2, the acid anhydride mixture of the present invention has a fast crystallization rate, and the curable resin composition thereof has excellent heat resistance and a low coefficient of linear expansion (dimensional stability), and therefore can be suitably used for carbon fiber reinforced composite materials.

Claims

1. A mixture of cyclic acid anhydrides comprising a cyclic acid anhydride represented by the following formula (A-a), a cyclic acid anhydride represented by the following formula (A-b), and a cyclic acid anhydride represented by the following formula (A-c), wherein, when the sum of the peak areas of the cyclic acid anhydrides represented by the formulas (A-a) to (A-c) is taken as 100% in gas chromatography analysis of the mixture of cyclic acid anhydrides, the peak area of ​​the cyclic acid anhydride represented by formula (A-a) is 0.1% or more and 1.0% or less, the peak area of ​​the cyclic acid anhydride represented by formula (A-b) is 98.0% or more and 99.0% or less, and the peak area of ​​the cyclic acid anhydride represented by formula (A-c) is 0.1% or more and 1.0% or less.

2. The mixture of cyclic acid anhydrides according to claim 1, which is dissolved at 80°C and then allowed to stand at 10°C for 0.1 to 1.5 hours until crystallization.

3. The mixture of cyclic acid anhydrides according to claim 1 in the form of pellets, granules or marbles.

4. A curable resin composition comprising the mixture of cyclic acid anhydrides according to any one of claims 1 to 3, an epoxy resin, and a curing accelerator.

5. A cured product obtained by curing the curable resin composition according to claim 4.

6. A carbon fiber reinforced composite material obtained by curing the curable resin composition according to claim 4.

7. A method for producing a mixture of cyclic acid anhydrides according to any one of claims 1 to 3, which comprises reacting 1,3-p-menthadiene, maleic anhydride and a solvent at 40 to 80°C, and then concentrating the solvent.

Citation Information

Patent Citations

  • Preparation method of seven-membered cyclic carbonate monomer and polycarbonate based on D-A reaction

    CN115703789A

  • Curable epoxy resin composition

    JP1980118920A

  • Compound having lactone structure

    JP2004315465A

  • New lactone compound

    JP2005023063A

  • New alicyclic compound, method for producing the same and polymer composition

    JP2008088154A