Resin composition and molded body

The combination of a norbornene polymer and plate-like fillers in the resin composition significantly improves the thermal dimensional stability of molded articles, addressing the limitations of conventional compositions by reducing linear expansion and weld formation while ensuring surface quality and water resistance.

WO2024203486A1PCT designated stage expired Publication Date: 2024-10-03ZEON CORP

Patent Information

Application Number
PCT/JP2024/010372
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-15
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Conventional resin compositions used for molded articles lack sufficient thermal dimensional stability, which affects their performance under heat variations.

Method used

A resin composition containing a norbornene polymer and a plate-like filler, such as boehmite or mica, with a specific aspect ratio and content, is used to enhance the thermal dimensional stability of molded articles.

Benefits of technology

The resin composition achieves excellent thermal dimensional stability, reducing linear expansion coefficients and suppressing the occurrence of welds during molding, while maintaining surface smoothness and water resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
Patent Text Reader

Abstract

The resin composition contains a polymer containing a structural unit derived from a norbornene monomer, and a plate-like filler.
Need to check novelty before this filing date? Find Prior Art

Description

Resin composition and molded article

[0001] The present invention relates to a resin composition and a molded article.

[0002] BACKGROUND ART Fillers have conventionally been blended into resin compositions that are the materials for molded articles in order to reinforce the molded articles or to impart various functions to the molded articles.

[0003] For example, Patent Document 1 proposes a resin composition containing a resin and composite particles composed of two types of inorganic fine particles, and according to Patent Document 1, by using this resin composition, a molded article having a low linear expansion coefficient can be produced.

[0004] International Publication No. 2010 / 137437

[0005] However, the conventional resin compositions described above have room for improvement in terms of further improving the dimensional stability of the molded articles against heat (hereinafter, sometimes referred to as "thermal dimensional stability").

[0006] Therefore, an object of the present invention is to provide a molded article having excellent dimensional stability against heat, and a resin composition capable of forming such a molded article.

[0007] The present inventors have conducted extensive research to solve the above-mentioned problems, and have found that a molded article having excellent thermal dimensional stability can be formed by using a resin composition containing a polymer including structural units derived from a norbornene-based monomer (hereinafter, may be referred to as a "norbornene-based polymer") and a plate-like filler, thereby completing the present invention.

[0008] That is, the present invention aims to advantageously solve the above problems, and provides the following resin compositions [1] to [6] and the following molded articles [7] to

[12] .

[0009] [1] A resin composition comprising a polymer containing structural units derived from a norbornene-based monomer and a flake-like filler. Thus, by using a resin composition containing a norbornene-based polymer and a flake-like filler, a molded article with excellent thermal dimensional stability can be produced. In this specification, "norbornene-based monomer" refers to a monomer having a norbornene skeleton. In this specification, "flake-like filler" refers to a filler having two opposing main surfaces and an aspect ratio, calculated as the ratio of the maximum diameter of the main surfaces to the thickness (the distance between the two main surfaces), of 13 or more. Here, "two main surfaces" refers to the two surfaces of the filler that have the largest areas. Furthermore, the shape of the two main surfaces of the flake-like filler, i.e., the planar shape of the flake-like filler, can be any shape. The two main surfaces may be flat or curved, and do not necessarily have to have the same shape. In this specification, the shapes of various fillers can be observed using an electron microscope.

[0010] [2] The resin composition according to [1], wherein the platy filler is at least one of boehmite and mica. By using boehmite and / or mica as the platy filler, the thermal dimensional stability of the resulting molded article can be further improved.

[0011] [3] The resin composition according to [1], wherein the platy filler is boehmite. By using boehmite as the platy filler, the thermal dimensional stability of the resulting molded article can be further improved.

[0012] [4] The resin composition according to any one of [1] to [3], wherein the content of the platy filler is 10 to 60 parts by mass per 100 parts by mass of the polymer. By using a resin composition having a platy filler content within the above range, the thermal dimensional stability of the resulting molded article can be further improved. Furthermore, when producing a molded article by injection molding, the occurrence of weak welds at the merging points of molten resins in the mold can be suppressed.

[0013] [5] The resin composition according to any one of [1] to [4], further comprising a granular filler. By using a resin composition containing the granular filler in addition to the norbornene-based polymer and the flake-like filler, the fluidity of the resin composition can be improved, and the occurrence of welds during the production of a molded product can be suppressed.

[0014] [6] The resin composition according to [5], wherein the ratio of the average particle size of the granular filler to the average particle size of the platy filler is 1 / 10 or less. If the ratio of the average particle size of the granular filler to the average particle size of the platy filler is equal to or less than the above value, the fluidity of the resin composition can be further improved, and the occurrence of welds during the production of a molded product can be further suppressed. In this specification, the "average particle size" of the platy filler and the granular filler means the arithmetic mean diameter determined by observation with an electron microscope, and can be measured in more detail using the method described in the Examples.

[0015] [7] A molded article obtained by molding the resin composition according to any one of [1] to [6] above. The molded article obtained by molding any one of the above-mentioned resin compositions has excellent thermal dimensional stability.

[0016] [8] The molded article according to [7] above, wherein the linear expansion coefficient in the MD direction and the linear expansion coefficient in the TD direction are both 40 ppm / K or less. A molded article having a linear expansion coefficient in both the MD direction and the TD direction that is equal to or less than the above-mentioned value is said to have particularly excellent thermal stability and is therefore preferred. In this specification, the MD (machine direction) direction refers to the direction parallel to the flow of the resin composition when producing the molded article, and the TD (transverse direction) direction refers to the direction perpendicular to the MD direction. The MD direction and the TD direction can be identified by observing the molded article itself. For example, when a gate mark is found in a molded article that is approximately rectangular in plan view, the extension direction of the side where the gate mark exists when the molded article is viewed in plan can be identified as the TD direction, and the direction perpendicular to the TD direction can be identified as the MD direction. Furthermore, for example, when a gate mark is found in a molded body of a substantially circular shape (such as a lens shape), when the molded body is laid flat, the tangential direction of the substantially circle at the center of the gate mark can be specified as the TD direction, and the direction perpendicular to the TD direction can be specified as the MD direction. In this specification, the "linear expansion coefficient" in the MD direction and the TD direction of the molded body can be measured using the method described in the Examples.

[0017] [9] The molded article according to [7] or [8], wherein the ratio of the linear expansion coefficient in the MD direction to the linear expansion coefficient in the TD direction is 0.8 or more and 1.2 or less. A molded article having a ratio of the linear expansion coefficient in the MD direction / linear expansion coefficient in the TD direction within the above range is preferred because it has small anisotropy in thermal dimensional stability.

[0018]

[10] The molded article according to any one of [7] to [9] above, which has a water absorption rate of 0.05% by mass or less after immersion in water at 23°C for 24 hours as measured in accordance with ASTM D 570. A molded article having the water absorption rate of the above value or less is preferable because it has excellent water absorption resistance.

[0019]

[11] The molded article according to any one of [7] to

[10] above, having an arithmetic surface roughness Ra of 10 nm or less. A molded article having an arithmetic surface roughness Ra of the above value or less is preferable because it has excellent surface smoothness. In this specification, the "arithmetic surface roughness Ra" of the molded article can be measured using the method described in the examples.

[0020]

[12] The molded article according to any one of [7] to

[11] above, which is for use in a mirror.

[0021] According to the present invention, a resin composition capable of forming a molded article having excellent thermal dimensional stability can be provided. Also, according to the present invention, a molded article having excellent thermal dimensional stability can be provided.

[0022] Hereinafter, embodiments of the present invention will be described in detail. The resin composition of the present invention can be used to produce the molded article of the present invention. Furthermore, the molded article of the present invention can be used, without particular limitation, as a mirror to be mounted on a projector, a head-up display, or the like.

[0023] (Resin Composition) The resin composition of the present invention must contain a norbornene-based polymer and a flake-like filler, and may contain optional components as required.

[0024] Furthermore, since the resin composition of the present invention contains a norbornene-based polymer and a flake-like filler, the use of this resin composition makes it possible to produce a molded article having excellent thermal dimensional stability.

[0025] <Norbornene-Based Polymer> The norbornene-based polymer is a polymer obtained by polymerizing a norbornene-based monomer, which is a monomer having a norbornene skeleton, or a hydrogenated product thereof.

[0026] Examples of norbornene-based polymers include ring-opening polymers of norbornene-based monomers, ring-opening polymers of norbornene-based monomers and other monomers copolymerizable therewith, hydrogenated products of these ring-opening polymers, addition polymers of norbornene-based monomers, and addition polymers of norbornene-based monomers and other monomers copolymerizable therewith.The norbornene-based polymers may be used singly or in combination of two or more.

[0027] Norbornene-based monomers include bicyclo[2.2.1]hept-2-ene (common name: norbornene) and its derivatives (those having a substituent on the ring), tricyclo[4.3.0]hept-2-ene (common name: norbornene), and 1,6 .1 2,5]deca-3,7-diene (trivial name: dicyclopentadiene) and its derivatives (those having a substituent on the ring), tetracyclo[9.2.1.0 2,10 .0 3,8 ]tetradeca-3,5,7,12-tetraene, (methanotetrahydrofluorene: also called 1,4-methano-1,4,4a,9a-tetrahydrofluorene) and its derivatives (those having a substituent on the ring), tetracyclo[4.4.1 2,5 .1 7,10 .0]dodec-3-ene (common name: tetracyclododecene) and its derivatives (those having a substituent on the ring). Examples of the substituent include an alkyl group, an alkylene group, a vinyl group, an alkoxycarbonyl group, an alkylidene group, etc. Examples of the norbornene-based monomer having a substituent include 8-methoxycarbonyl-tetracyclo[4.4.0.1 2,5 .1 7,10 ] dodec-3-ene, 8-methyl-8-methoxycarbonyl-tetracyclo[4.4.0.1 2,5 .1 7,10 ] dodec-3-ene, 8-ethylidene-tetracyclo[4.4.0.1 2,5 .1 7,10 ]dodec-3-ene, and the like, but are not limited thereto.

[0028] Other monomers that can be ring-opening copolymerized with norbornene-based monomers include monocyclic olefin-based monomers such as cyclohexene, cycloheptene, cyclooctene, and derivatives thereof (having a substituent on the ring). Examples of the substituents include the same as those shown as the substituents on norbornene-based monomers.

[0029] Other monomers that can be addition-copolymerized with norbornene-based monomers include α-olefins having 2 to 20 carbon atoms, such as ethylene, propylene, 1-butene, 1-pentene, and 1-hexene, and derivatives thereof (having a substituent); cycloolefins and derivatives thereof (having a substituent on the ring), such as cyclobutene, cyclopentene, cyclohexene, and cyclooctene; and non-conjugated dienes, such as 1,4-hexadiene, 4-methyl-1,4-hexadiene, 5-methyl-1,4-hexadiene, and 1,7-octadiene. Among these, α-olefins are preferred, and ethylene is particularly preferred. Examples of the substituents include the same as those shown as the substituents for norbornene-based monomers.

[0030] Ring-opening polymers of norbornene-based monomers or ring-opening polymers of norbornene-based monomers and other monomers copolymerizable therewith can be synthesized by polymerizing the monomer components in the presence of a known ring-opening polymerization catalyst. Examples of the ring-opening polymerization catalyst include catalysts comprising a halide of a metal such as ruthenium or osmium, a nitrate or an acetylacetone compound, and a reducing agent, and catalysts comprising a halide or an acetylacetone compound of a metal such as titanium, zirconium, tungsten, or molybdenum, and an organoaluminum compound.

[0031] The hydrogenated ring-opened polymer of a norbornene monomer can usually be obtained by adding a known hydrogenation catalyst containing a transition metal such as nickel or palladium to a polymerization solution of the ring-opened polymer and hydrogenating the carbon-carbon unsaturated bonds. The hydrogenation rate is preferably 90% or more, more preferably 95% or more, and even more preferably 99% or more. In this specification, the "hydrogenation rate" can be measured using the method described in the Examples.

[0032] An addition polymer of a norbornene-based monomer or an addition polymer of a norbornene-based monomer and another monomer copolymerizable therewith can be synthesized by polymerizing the monomer components in the presence of a known addition polymerization catalyst, such as a catalyst comprising a titanium, zirconium, or vanadium compound and an organoaluminum compound.

[0033] From the viewpoint of further improving the thermal dimensional stability of the resulting molded article, the proportion of the norbornene-derived structural units contained in the norbornene-based polymer is preferably 50% by mass or more and 100% by mass or less, more preferably 60% by mass or more and 100% by mass or less, and even more preferably 70% by mass or more and 100% by mass or less, where the total amount of all structural units contained in the norbornene-based polymer is 100% by mass.

[0034] The weight-average molecular weight (Mw) of the norbornene-based polymer is not particularly limited, but is preferably 1,000 or more, more preferably 2,000 or more, even more preferably 10,000 or more, and particularly preferably 20,000 or more, and is preferably 1,000,000 or less, and more preferably 500,000 or less. The molecular weight distribution (Mw / Mn) of the norbornene-based polymer is not particularly limited, but is preferably 1.0 or more and 4.0 or less, more preferably 1.5 or more and 3.5 or less. In this specification, the "weight-average molecular weight (Mw)" and "number-average molecular weight (Mn)" of a polymer such as a norbornene-based polymer can be measured using the method described in the Examples.

[0035] <Flat-like filler> As described above, the platy filler is a filler having an aspect ratio of 13 or more. Here, the average aspect ratio of the platy filler is preferably 16 or more, more preferably 20 or more, preferably 80 or less, more preferably 75 or less, even more preferably 60 or less, still more preferably 45 or less, and particularly preferably 30 or less. If the average aspect ratio of the platy filler is within the above-mentioned range, the thermal dimensional stability of the obtained molded body can be further improved. Note that the "average aspect ratio" of the platy filler means the arithmetic mean diameter determined by observation with an electron microscope, and can be measured in more detail using the method described in the examples.

[0036] The average particle size of the platy filler is preferably 1 μm or more, more preferably 2 μm or more, and is preferably 30 μm or less, more preferably 20 μm or less, and even more preferably 10 μm or less. If the average particle size of the platy filler is within the above-mentioned range, the thermal dimensional stability of the obtained molded article can be further improved.

[0037] Here, the shape of the flake-like filler in plan view is not particularly limited as described above, and may be, for example, a polygon, a circle, an ellipse, or a shape similar to any of these shapes.

[0038] The flake-like filler preferably has a hexagonal shape in plan view. The hexagonal shape in plan view is not limited to a regular hexagon, and any approximate hexagon that is recognized as having six corners will suffice, and as long as it has little anisotropy, the lengths of the sides connecting the corners may be slightly different, or at least one of the sides may be curved.

[0039] From the viewpoint of improving the thermal dimensional stability of the resulting molded body, preferred examples of the plate-like filler include boehmite and mica, with boehmite being more preferred. These may be used alone or in combination of two or more. From the viewpoint of maintaining the granulated shape, it is preferable to use boehmite that has been subjected to a granulation process in which a binder resin is molded and solidified. As the binder resin used in the granulation process, it is preferable to use a polyacrylic acid-based resin or a stearic acid-based resin.

[0040] The content of the platy filler in the resin composition of the present invention is preferably 10 parts by mass or more, more preferably 20 parts by mass or more, even more preferably 30 parts by mass or more, particularly preferably 40 parts by mass or more, and is preferably 60 parts by mass or less, more preferably 55 parts by mass or less, and even more preferably 50 parts by mass or less, per 100 parts by mass of the norbornene-based polymer. If the content of the platy filler is 10 parts by mass or more per 100 parts by mass of the norbornene-based polymer, the thermal dimensional stability of the obtained molded article can be further improved. On the other hand, if the content of the platy filler is 60 parts by mass or less per 100 parts by mass of the norbornene-based polymer, the occurrence of welds during the production of the molded article can be suppressed.

[0041] <Optional Components> Components that the resin composition may optionally contain in addition to the norbornene-based polymer and the flaky filler are not particularly limited, and may include other additives such as fillers other than the above-mentioned flaky fillers (other fillers), antioxidants, moisture-resistant agents, mold release agents, flame retardants, antibacterial agents, wood flour, coupling agents, plasticizers, colorants, lubricants, silicone oils, foaming agents, surfactants, thermoplastic elastomers, infrared absorbers, and light stabilizers. These other components may be used alone or in combination of two or more.

[0042] The other fillers are not particularly limited as long as they have a shape other than a plate shape, and may have any shape such as a granular or needle shape.

[0043] In order to prevent welds from occurring when a molded article is produced, the resin composition preferably contains a granular filler. In this specification, the term "granular filler" refers to a filler having an aspect ratio, calculated as the ratio of the maximum diameter to the minimum diameter, of less than 13.

[0044] Here, the average aspect ratio of the granular filler is preferably 5 or less, more preferably 3 or less, and even more preferably 2 or less. If the aspect ratio of the granular filler is the above value or less, the occurrence of welds in the molded body can be further suppressed. Furthermore, the aspect ratio of the granular filler is 1 or more, and may be greater than 1. In this specification, the "average aspect ratio" of the granular filler means the arithmetic mean diameter determined by observation with an electron microscope, and more specifically, it can be measured using the method described in the examples.

[0045] The granular filler is not particularly limited, and carbon-based granular fillers and non-carbon-based granular fillers can be used. Examples of carbon-based granular fillers include graphite such as artificial graphite, flake graphite, exfoliated graphite, natural graphite, acid-treated graphite, expandable graphite, and expanded graphite; carbon black; and the like. Examples of non-carbon-based granular fillers include titanium oxide, alumina, talc, calcium carbonate, and zinc oxide. These granular fillers can be used alone or in combination of two or more.

[0046] Among the above, carbon black and titanium oxide are preferred as the particulate filler from the viewpoint of sufficiently suppressing the occurrence of welds when producing a molded body, and carbon black is more preferred. Carbon black is also useful when producing a black-colored molded body.

[0047] From the viewpoint of sufficiently suppressing the occurrence of welds when producing a molded body, the granular filler preferably has an average particle size of 0.01 μm or more, more preferably 0.015 μm or more, and preferably 0.1 μm or less, more preferably 0.08 μm or less, and even more preferably 0.07 μm or less.

[0048] The content of the granular filler in the resin composition of the present invention is not particularly limited and is, for example, 0 part by mass or more and 0.6 parts by mass or less per 100 parts by mass of the norbornene-based polymer. From the viewpoint of sufficiently obtaining the above-mentioned weld formation suppression effect, the content of the granular filler in the resin composition is preferably 0.05 part by mass or more, more preferably 0.3 part by mass or more, per 100 parts by mass of the norbornene-based polymer.

[0049] <Method for Preparing Resin Composition> The resin composition of the present invention is not particularly limited and can be prepared, for example, by a method that can satisfactorily mix the above-mentioned essential components, i.e., the norbornene-based polymer and the flake-like filler, and any optional components used as needed. Examples of such methods include a method in which a mixture of the above components is supplied to a melt kneader, and the norbornene-based polymer is melted and kneaded. The obtained resin composition may be molded into pellets or the like by any method.

[0050] For kneading, a melt kneader such as a single-screw extruder, a twin-screw extruder, a Banbury mixer, a kneader, a roll, or a feeder ruder can be used. The kneading temperature is preferably 200° C. or higher, more preferably 240° C. or higher, and preferably 400° C. or lower, more preferably 300° C. or lower. In kneading, the components may be kneaded all at once, or may be kneaded by adding them in several portions.

[0051] (Molded Article) The molded article of the present invention is obtained by molding the resin composition of the present invention described above. That is, the norbornene-based polymer and flake-like filler contained in the molded article of the present invention, as well as the optional components used as needed, are as described above in the "Resin Composition" section. Furthermore, the content relationship (content ratio) and attributes of the norbornene-based polymer, flake-like filler, and optional components contained in the molded article of the present invention are generally the same as the content relationship (content ratio) and attributes of those components in the resin composition. Furthermore, since the molded article of the present invention is formed from the resin composition of the present invention described above, it has excellent thermal dimensional stability.

[0052] The molding method for producing the molded article of the present invention is not particularly limited and can be appropriately selected from known molding methods depending on the desired shape of the molded article. Examples of such known molding methods include extrusion molding, injection molding, inflation molding, blow molding, extrusion blow molding, injection blow molding, press molding, vacuum molding, powder slush molding, calendar molding, foam molding, and thermoforming. Among these, injection molding is preferably used as the molding method.

[0053] Furthermore, a molding method (heat and cool molding) may be employed in which the temperature of the mold cavity during filling is set to a temperature at which the resin composition can undergo plastic deformation, cooling is initiated between the completion of filling and the completion of pressure holding, and the product is removed after it has sufficiently cooled. By performing heat and cool molding, the arithmetic surface roughness Ra of the molded body can be reduced while suppressing the occurrence of welds.

[0054] <Properties of Molded Article> The molded article of the present invention can be formed into any shape depending on its application. The molded article of the present invention can have the following properties, for example.

[0055] <<Linear expansion coefficient>> The linear expansion coefficient of the molded body in the TD direction and MD direction is preferably 40 ppm / K or less, more preferably 37 ppm / K or less, even more preferably 33 ppm / K or less, even more preferably 30 ppm / K or less, and particularly preferably 25 ppm / K or less. A molded body having linear expansion coefficients in both the MD direction and the TD direction that are below the above values ​​is preferred because it has particularly excellent thermal stability. The lower limit of the linear expansion coefficient in the TD direction and the MD direction is not particularly limited, but is, for example, 1 ppm / K or more.

[0056] Furthermore, the ratio of the linear expansion coefficient in the MD direction to the linear expansion coefficient in the TD direction of the molded article is preferably 0.80 or more, more preferably 0.85 or more, and is preferably 1.20 or less, more preferably 1.10 or less. A molded article having a ratio of the linear expansion coefficient in the MD direction to the linear expansion coefficient in the TD direction within the above range is preferred because it has little anisotropy in terms of thermal dimensional stability.

[0057] <<Water Absorption Rate>> The norbornene polymer contained in the resin composition used to prepare the molded article has excellent hydrophobicity, and therefore the molded article has good resistance to water absorption. The molded article of the present invention has a water absorption rate after immersion in water at 23°C for 24 hours, as measured in accordance with ASTM D570, of preferably 0.05% by mass or less, more preferably 0.03% by mass or less, and even more preferably 0.01% by mass or less. The lower limit of the water absorption rate is not particularly limited, but is, for example, 0.001% by mass or more.

[0058] <<Arithmetic Surface Roughness Ra>> The molded body preferably has an arithmetic surface roughness Ra of 10 nm or less, more preferably 8 nm or less. A molded body having an arithmetic surface roughness Ra of the above value or less is preferable because it has excellent surface smoothness. The lower limit of the arithmetic surface roughness Ra is not particularly limited, but is, for example, 1 nm or more.

[0059] The present invention will be specifically described below based on examples, but the present invention is not limited to these examples. In the following description, "%" and "parts" representing amounts are based on mass unless otherwise specified.

[0060] In addition, in a polymer produced by polymerizing a plurality of types of monomers, the ratio of a monomer unit formed by polymerizing a certain monomer in the polymer usually coincides with the ratio (feed ratio) of the certain monomer to all the monomers used in the polymerization of the polymer, unless otherwise specified. In the examples and comparative examples, the hydrogenation rate, molecular weight, and glass transition temperature of the norbornene-based polymer, the properties of the platy filler, the average particle size of the granular filler, the linear expansion coefficient of the molded body, the water absorption rate, the presence or absence of welds, and the arithmetic surface roughness Ra were measured or evaluated by the following methods, respectively.

[0061] <Hydrogenation rate> Using deuterated chloroform as a solvent, 1H-NMR measurement was performed, and the hydrogenation rate in the hydrogenation reaction was calculated. <Molecular Weight> Number average molecular weight (Mn) and weight average molecular weight (Mw) were measured as values ​​converted to standard polyisoprene by gel permeation chromatography (GPC) using cyclohexane as a solvent. The molecular weight distribution (Mw / Mn) was calculated from these obtained values. For GPC, an HLC8120GPC manufactured by Tosoh Corporation was used. As standard polyisoprene, a total of 10 standard polyisoprenes manufactured by Tosoh Corporation with Mw = 602, 1390, 3920, 8050, 13800, 22700, 58800, 71300, 109000, and 280000 were used. The measurements were performed using three columns connected in series: TSKgel G5000HXL, TSKgel G4000HXL, and TSKgel G2000HXL manufactured by Tosoh Corporation. The conditions were a flow rate of 1.0 ml / min, a sample injection volume of 100 μml, and a column temperature of 40°C. <Glass Transition Temperature> The glass transition temperature (Tg) was measured using a differential scanning calorimeter (DSC6220, manufactured by SII Nanotechnology) at a heating rate of 10°C / min in accordance with JIS K6911. <Properties of Plate-Like Filler> The resin compositions prepared in the examples and comparative examples were burned at 550°C to remove the resin components, and then a solvent was added to the resulting ash to elute the filler components. The filler components were then applied to the surface of an observation substrate, making them observable. Next, properties such as aspect ratio were confirmed using a scanning electron microscope (SEM) to determine whether the various filler components were plate-like. The maximum diameter and thickness of 50 randomly selected plate-like fillers were measured, and the aspect ratio was calculated. The arithmetic mean value of the maximum diameters of these 50 plate-like fillers was taken as the average particle size, and the arithmetic mean value of the aspect ratios was taken as the average aspect ratio. <Average particle size of granular filler> The resin compositions prepared in the Examples and Comparative Examples were burned at 550 ° C to remove the resin components, and then a solvent was added to the resulting ash to dissolve the granular filler, which was then applied to the surface of an observation substrate, making each granular filler observable. The particle diameters of 50 randomly selected granular fillers were then individually observed using a scanning electron microscope (SEM). A circle was drawn on the image of each granular filler obtained using a planar measurement tool, and the maximum and minimum diameters of the drawn circle were measured by linear measurement.The arithmetic mean value of the maximum and minimum diameters was taken as the particle diameter of the granular filler, and the average value of the particle diameters of 50 granular fillers was taken as the average particle diameter of the granular filler. <Linear Expansion Coefficient> Test pieces measuring 10 cm long x 5 cm wide x 5 cm thick were cut out from the molded bodies produced in the Examples and Comparative Examples, with the 10 cm long direction being the TD direction, and the linear expansion coefficient (ppm / K) specified in ASTM E831 was measured. This measurement was performed a total of three times, and the average of these measurements was taken as the linear expansion coefficient in the TD direction. From the molded bodies produced in the Examples and Comparative Examples, test pieces measuring 10 cm long x 5 cm wide x 5 cm thick were cut out from the molded bodies produced in the Examples and Comparative Examples, with the 10 cm long direction being the MD direction, and the linear expansion coefficient (ppm / K) specified in ASTM E831 was measured. This measurement was performed a total of three times, and the average of these measurements was taken as the linear expansion coefficient in the MD direction. The ratio of the linear expansion coefficient in the MD direction to the linear expansion coefficient in the TD direction was then calculated. <Water Absorption> The water absorption of the molded articles produced in the Examples and Comparative Examples was measured after immersion in water at 23°C for 24 hours in accordance with ASTM D570. <Presence or Absence of Welds> The molded articles produced in the Examples and Comparative Examples were visually inspected to determine whether welds were present. <Arithmetic Surface Roughness Ra> The arithmetic surface roughness Ra of the molded articles produced in the Examples and Comparative Examples was measured using a white light interferometer (ZYGO Corporation, NewView (registered trademark) series). The measurement magnification was adjusted so that the measurement field of view was 1.82 mm x 1.36 mm, and measurements were taken at five arbitrary positions near the center of the measurement sample. The average value was taken as the arithmetic surface roughness Ra. The surface roughness was evaluated according to the following criteria. Note that if the four corners of the three-dimensional image of the measurement results were not flat (the unevenness was greater than that of the center), the results were excluded and the average value was calculated. In addition, to correct for large surface waviness, the analysis was performed in Cylinder mode. A+: Arithmetic surface roughness Ra is 10 nm or less. A: Arithmetic surface roughness Ra is more than 10 nm.

[0062] (Preparation of Norbornene-Based Polymer, etc.) <Synthesis of Polymer X> A polymerization reactor whose interior was dried and purged with nitrogen was charged with 7 parts (1% based on the total amount of monomers used in polymerization) of a monomer mixture consisting of 70% methanotetrahydrofluorene (MTF) as norbornene-based monomers, 22% tetracyclododecene (TCD), and 8% norbornene (NB), 1,600 parts of dehydrated cyclohexane, 0.6 parts of 1-hexene, 1.3 parts of diisopropyl ether, 0.33 parts of isobutyl alcohol, 0.84 parts of triisobutylaluminum, and 30 parts of a 0.66% cyclohexane solution of tungsten hexachloride, and the mixture was stirred at 55°C for 10 minutes. Next, while maintaining the reaction system at 55°C and stirring, 693 parts of the monomer mixture and 72 parts of a 0.77% tungsten hexachloride cyclohexane solution were continuously added dropwise to the polymerization reactor over 150 minutes, and after further stirring for 30 minutes after the completion of the dropwise addition, 1.0 part of isopropyl alcohol was added to terminate the polymerization reaction. Measurement of the polymerization reaction solution by gas chromatography revealed that the conversion of the monomer to polymer was 100%. Next, 300 parts of the polymerization reaction solution containing the polymer was transferred to an autoclave equipped with a stirrer, and 100 parts of cyclohexane and 2.0 parts of a diatomaceous earth-supported nickel catalyst (manufactured by JGC Chemical Industries, Ltd.; "T8400RL", nickel support rate 58%) were added. After replacing the atmosphere in the autoclave with hydrogen, the reaction was carried out at 180°C under a hydrogen pressure of 4.5 MPa for 6 hours. After completion of the hydrogenation reaction, the mixture was filtered at a pressure of 0.25 MPa using a pressure filter (Funda Filter, manufactured by IHI Corporation) with diatomaceous earth (Radiolite (registered trademark) #500, manufactured by Showa Chemical Industry Co., Ltd.) as a filter bed to obtain a colorless, transparent solution. To the resulting solution, 0.5 parts of an antioxidant, pentaerythrityl-tetrakis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate] (Irganox (registered trademark) 1010, manufactured by Ciba Specialty Chemicals Inc.), was added and dissolved per 100 parts of the hydrogenated product. This solution was filtered through a filter (Zetaplus (registered trademark) 30H, manufactured by Cuno Filter Co., Ltd., pore size 0.5-1 μm), and the filtrate was then filtered through a metal fiber filter (Nichidai Corporation, pore size 0.4 μm) to remove foreign matter.Next, the filtrate obtained above was subjected to a cylindrical concentrating dryer (manufactured by Hitachi, Ltd.) at a temperature of 260°C and a pressure of 1 kPa or less to remove the cyclohexane solvent and other volatile components from the solution. The filtrate was extruded in a molten state into strands from a die directly connected to the concentrator, cooled with water, and then cut with a pelletizer (manufactured by Nagata Seisakusho Co., Ltd.; "OSP-2") to obtain pellets of Polymer X, a norbornene polymer. This Polymer X had an Mw of 24,000, an Mw / Mn of 1.75, a hydrogenation rate of 99.9%, and a Tg of 140°C. <Synthesis of Polymer Y> A polymerization reactor whose interior had been dried and purged with nitrogen was charged with 960 parts of toluene, 220 parts of tetracyclododecene as a norbornene monomer, and 0.166 parts of 1-hexene, and the solvent temperature was raised to 40°C while stirring at a rotation speed of 300 to 350 rpm. Separately, 23.5 parts of toluene, 0.044 parts of rac-ethylenebis(1-indenyl)zirconium dichloride, and 6.22 parts of a 9.0% toluene solution of methylaluminoxane (TMAO-200 series, manufactured by Tosoh Finechem Corporation) were mixed in a glass container to obtain a catalyst solution. When the solvent temperature in the reactor reached 40°C, the catalyst solution was added to the reactor, and immediately thereafter, ethylene gas at 0.08 MPa was introduced into the liquid phase to initiate polymerization. The ethylene outlet was positioned such that the ratio (B) / (A) of the distance (A) between the bottom of the reactor and the liquid level and the distance (B) between the ethylene outlet and the liquid level was 0.60. Ethylene gas was automatically supplied as ethylene gas was consumed, maintaining a constant ethylene gas pressure. After 30 minutes, the introduction of ethylene gas was stopped, the pressure was released, and then 5 parts of methanol was added to terminate the polymerization reaction. The resulting reaction solution was filtered through Radiolite #800 and poured into isopropanol containing 0.05% hydrochloric acid to precipitate a polymer. The precipitated polymer was separated, washed, and dried under reduced pressure at 100°C for 15 hours. The resulting polymer Y (norbornene-based polymer) had an Mw of 56,000, an Mw / Mn of 2.6, and a Tg of 145°C. <Synthesis of Polymer Z> 76 parts of styrene and 4 parts of isoprene were sealed in a stainless steel pressure vessel whose interior had been dried and substituted with nitrogen, and the mixture was stirred to prepare a monomer mixture.Next, 320 parts of dehydrated cyclohexane, 4 parts of the mixed monomer prepared above, and 0.1 parts of dibutyl ether were charged into a dried, nitrogen-purged stainless steel autoclave equipped with a magnetic stirrer. While stirring at 50°C, 0.18 parts of a hexane solution of n-butyllithium (15% concentration) was added to the autoclave to initiate polymerization. 0.5 hours after the start of the reaction (the conversion rate at this point was 96%), 76 parts of the mixed monomer were continuously added to the polymerization reaction solution over 1 hour, and the polymerization reaction was continued. After a further 0.5 hours had elapsed since the end of the addition (the conversion rate at this point was 95%), 0.1 parts of isopropyl alcohol was added to terminate the polymerization reaction, yielding a reaction solution containing a styrene-isoprene copolymer. To 400 parts of the resulting reaction solution, 8 parts of stabilized nickel hydrogenation catalyst E19Z (manufactured by JGC Chemical Industries, Ltd.; nickel-diatomaceous earth hydrogenation catalyst (nickel content 60%)) were added, and the mixture was charged into a stainless steel autoclave. The autoclave was purged with hydrogen gas, and hydrogen was supplied to maintain the pressure inside the autoclave at 4.5 MPa. The hydrogenation reaction was carried out at 160°C for 6 hours. Next, using a pressure filter (Funda Filter, manufactured by IHI Corporation) with a Radiolite #800 filter bed, the mixture was filtered at 0.25 MPa to obtain a colorless, transparent solution from which the catalyst had been removed. The hydrogenation reaction solution was poured into a mixed solution of 250 parts acetone and 250 parts isopropanol with stirring to precipitate the hydride, which was then recovered by filtration. The recovered hydride was further washed with 200 parts acetone and then dried for 24 hours at 100°C in a vacuum oven evacuated to 1 mmHg or less. The yield of the hydride was 99%. The hydride had a Mw of 91,000, a Mw / Mn of 1.27, and a Tg of 125°C. Hereinafter, the resulting hydride may be referred to as "HPSt."100 parts of the HPSt obtained above was mixed with 0.40 parts of pentaerythritol-tetrakis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate] (manufactured by BASF, product name "Irganox (registered trademark) 1010") as a hindered phenol-based antioxidant using a twin-screw kneader (manufactured by Toshiba Machine Co., Ltd., TEM-35B, screw diameter 37 mm, L / D = 32, screw rotation speed 250 rpm, resin temperature 230°C, feed rate 10 kg / hour), and extruded to obtain a pelletized resin composition. The obtained pellets were heated and dried at 80°C for 4 hours to obtain Polymer Z.

[0063] Example 1 Preparation of Resin Composition 100 parts of Polymer X as a norbornene-based polymer and 10 parts of boehmite ("BMF-520" manufactured by Kawai Lime Industry Co., Ltd., average aspect ratio: 20, average particle size: 8 μm) as a plate-like filler were mixed, and then kneaded using a kneader (manufactured by Shibaura Machine Co., Ltd., product name "TEM-37") under conditions of 260°C and 150 rpm to obtain a pelletized resin composition. In the Examples and Comparative Examples, the properties (average aspect ratio, average particle size, etc.) of various fillers in the resin compositions were the same as those at the time of charging. <Preparation of Molded Article> The pelletized resin composition was dried by heating at 80°C for 4 hours, and then placed in an injection molding machine (manufactured by Fanuc Corporation, product name "Roboshot α-100B") and injection molded at a cylinder temperature of 270°C and a mold temperature of 135°C to obtain a flat plate-shaped molded article measuring 90 mm x 55 mm x 5 mm. The linear expansion coefficient, water absorption rate, presence or absence of welds, and arithmetic surface roughness Ra of this molded article were measured or evaluated. The results are shown in Table 1.

[0064] (Examples 2 and 6) Resin compositions and molded articles were prepared and various evaluations were performed in the same manner as in Example 1, except that the amount of boehmite was changed from 10 parts to 60 parts (Example 2) and 45 parts (Example 6) during the preparation of the resin compositions. The results are shown in Table 1.

[0065] (Example 3) A resin composition and a molded product were prepared and various evaluations were performed in the same manner as in Example 1, except that 45 parts of mica ("NK-20G" manufactured by Nihon Koken Kogyo Co., Ltd., average aspect ratio: 75, average particle size: 20 μm) was used as the plate-like filler instead of 10 parts of boehmite during the preparation of the resin composition. The results are shown in Table 1.

[0066] Example 4 A resin composition and a molded product were prepared and various evaluations were performed in the same manner as in Example 1, except that 45 parts of mica ("NK-10G" manufactured by Nihon Koken Kogyo Co., Ltd., aspect ratio: 55, average particle size: 10 μm) was used as the plate-like filler instead of 10 parts of boehmite. The results are shown in Table 1.

[0067] Example 5 A molded body was prepared in the same manner as in Example 1, except that a resin composition prepared as follows was used, and various evaluations were performed. The results are shown in Table 1. <Preparation of Resin Composition> 100 parts of polymer Y as a norbornene-based polymer and 45 parts of boehmite ("BMF-520" manufactured by Kawai Lime Industry Co., Ltd., average aspect ratio: 20, average particle size: 8 μm) as a plate-like filler were mixed, and then kneaded using a kneader (manufactured by Shibaura Machine Co., Ltd., product name "TEM-37") under conditions of 260°C and 150 rpm to obtain a pelletized resin composition.

[0068] Example 7 A molded body was prepared in the same manner as in Example 1, except that a resin composition prepared as follows was used, and various evaluations were performed. The results are shown in Table 1. <Preparation of Resin Composition> 100 parts of Polymer X as a norbornene-based polymer, 45 parts of boehmite as a plate-like filler ("BMF-520" manufactured by Kawai Lime Industry Co., Ltd., average aspect ratio: 20, average particle size: 8 μm), and 0.6 parts of carbon black as a granular filler ("CB #650" manufactured by Mitsubishi Chemical Corporation, average particle size: 0.022 μm) were mixed, and then kneaded using a kneader (manufactured by Shibaura Machine Co., Ltd., product name "TEM-37") at 260°C and 150 rpm to obtain a pelletized resin composition.

[0069] (Example 8) A resin composition and a molded article were prepared and various evaluations were performed in the same manner as in Example 7, except that the amount of carbon black was changed from 0.6 parts to 0.3 parts when preparing the resin composition. The results are shown in Table 1.

[0070] Example 9 A resin composition and a molded product were prepared and various evaluations were performed in the same manner as in Example 1, except that 45 parts of boehmite ("BMT" manufactured by Kawai Lime Industry Co., Ltd., average aspect ratio: 15, average particle size: 3 μm) was used instead of 10 parts of boehmite ("BMF-520" manufactured by Kawai Lime Industry Co., Ltd.) when preparing the resin composition. The results are shown in Table 1.

[0071] (Example 10) A resin composition and a molded product were prepared and various evaluations were performed in the same manner as in Example 8, except that the amount of boehmite was changed from 45 parts to 60 parts when preparing the resin composition. The results are shown in Table 1.

[0072] (Example 11) A resin composition and a molded product were prepared and evaluated in the same manner as in Example 8, except that the amount of boehmite was changed from 45 parts to 10 parts and the amount of carbon black was changed from 0.3 parts to 0.05 parts during the preparation of the resin composition. The results are shown in Table 1.

[0073] (Example 12) A pelletized resin composition was prepared in the same manner as in Example 6. The resulting resin composition was then heated and dried at 80°C for 4 hours, and then a molded body was produced under the following conditions, and various evaluations were carried out. The mold temperature was controlled by cooling at 170°C until filling was complete, and then heat and cool molding was carried out, in which the mold was cooled to 170°C until filling was complete, and then rapidly cooled to 140°C. The results are shown in Table 1. <<Production conditions>> Injection molding machine: Made by Japan Steel Works, Ltd., product name "J-450ADS" Cylinder temperature: 270°C Mold temperature: 170°C at high temperature, 140°C at low temperature Superheated steam rapid heating and rapid cooling device: Made by iTOS, product name "USCOOL"

[0074] Comparative Example 1 A resin composition and a molded product were prepared in the same manner as in Example 1, except that boehmite was not used when preparing the resin composition, and various evaluations were carried out. The results are shown in Table 2.

[0075] Comparative Example 2 A resin composition and a molded product were prepared and various evaluations were performed in the same manner as in Example 1, except that 45 parts of boehmite ("BMM" manufactured by Kawai Lime Industry Co., Ltd., average aspect ratio: 10, average particle size: 1 μm, no plate-like filler) was used instead of 10 parts of boehmite ("BMF-520" manufactured by Kawai Lime Industry Co., Ltd.) during preparation of the resin composition. The results are shown in Table 2.

[0076] Comparative Example 3 A resin composition and a molded product were prepared and various evaluations were performed in the same manner as in Example 1, except that 45 parts of boehmite ("BMB-03" manufactured by Kawai Lime Industry Co., Ltd., average aspect ratio: 2, average particle size: 1 μm, no plate-like filler) was used instead of 20 parts of boehmite ("BMF-520" manufactured by Kawai Lime Industry Co., Ltd.) when preparing the resin composition. The results are shown in Table 2.

[0077] Comparative Example 4 A resin composition and a molded product were prepared in the same manner as in Example 1, and various evaluations were carried out, except that 45 parts of a needle-shaped filler, boehmite ("BMI" manufactured by Kawai Lime Industry Co., Ltd., average aspect ratio: 40, average particle size: 4 μm, no plate-like filler), was used instead of 20 parts of boehmite ("BMF-520" manufactured by Kawai Lime Industry Co., Ltd.) during the preparation of the resin composition. The results are shown in Table 2. The "average aspect ratio" of the needle-shaped filler was determined by observing each filler in the same manner as in the "average particle size of granular filler," calculating the aspect ratio of 50 randomly selected particles as the ratio of the needle length to the needle width, and then calculating the arithmetic average value of these.

[0078] Comparative Example 5 Preparation of Resin Composition 100 parts of Polymer Z and 45 parts of boehmite ("BMF-520" manufactured by Kawai Lime Industry Co., Ltd., average aspect ratio: 20, average particle size: 8 μm) as a plate-like filler were mixed, and then kneaded using a kneader (manufactured by Shibaura Machine Co., Ltd., product name "TEM-37") at 250°C and 150 rpm to obtain a pelletized resin composition. Production of Molded Article The pelletized resin composition was dried by heating at 80°C for 4 hours and then placed in an injection molding machine (manufactured by Fanuc Corporation, product name "Roboshot α-100B") and injection molded at a cylinder temperature of 260°C and a mold temperature of 135°C to obtain a 90 mm x 55 mm x 5 mm plate-like molded article. The linear expansion coefficient, water absorption, presence or absence of welds, and arithmetic surface roughness (Ra) of this molded article were measured or evaluated. The results are shown in Table 2.

[0079] In Tables 1 and 2 shown below, "plate-like / granular particle size ratio" indicates the ratio of the average particle size of the granular filler to the average particle size of the plate-like filler, "MD" indicates the linear expansion coefficient in the MD direction, and "TD" indicates the linear expansion coefficient in the TD direction. "MD / TD" indicates the ratio of the linear expansion coefficient in the MD direction to the linear expansion coefficient in the TD direction, and "≦0.01" indicates 0.01 mass% or less. In Tables 1 and 2, "MD / TD" is expressed as a value rounded to one decimal place.

[0080]

[0081]

[0082] It can be seen from Tables 1 and 2 that in Examples 1 to 12, which used resin compositions containing a norbornene-based polymer and a flake-like filler, molded articles having excellent thermal dimensional stability could be produced.

[0083] According to the present invention, a resin composition capable of forming a molded article having excellent thermal dimensional stability can be provided. Also, according to the present invention, a molded article having excellent thermal dimensional stability can be provided.

Claims

1. A resin composition comprising a polymer containing structural units derived from a norbornene-based monomer and a flake-like filler.

2. The resin composition according to claim 1, wherein the plate-like filler is at least one of boehmite and mica.

3. The resin composition according to claim 1, wherein the plate-like filler is boehmite.

4. The resin composition according to claim 1, wherein the content of the plate-like filler is 10 parts by mass or more and 60 parts by mass or less per 100 parts by mass of the polymer.

5. The resin composition according to claim 1, further comprising a particulate filler.

6. The resin composition according to claim 5, wherein the ratio of the average particle size of said granular filler to the average particle size of said plate-like filler is 1 / 10 or less.

7. A molded article obtained by molding the resin composition according to any one of claims 1 to 6.

8. The molded article according to claim 7, wherein the linear expansion coefficient in the MD direction and the linear expansion coefficient in the TD direction are both 40 ppm / K or less.

9. The molded article according to claim 7, wherein the ratio of the linear expansion coefficient in the MD direction to the linear expansion coefficient in the TD direction is 0.8 or more and 1.2 or less.

10. The molded article according to claim 7, which has a water absorption rate of 0.05% by mass or less after immersion in water at 23°C for 24 hours as measured in accordance with ASTM D570.

11. The molded article according to claim 7, having an arithmetic surface roughness Ra of 10 nm or less.

12. The molded article according to claim 7, which is for use as a mirror.

Citation Information

Patent Citations

  • Resin composition and process for producing same

    WO2010137437A1

  • Light diffusing resin composition and light diffusing plate using the same

    JP2004175963A

  • Resin composition comprising norbornene-based hydrogenated ring-opened polymer and plate-like filler, and molded article

    JP2008138041A

  • Gas barrier film and backside protective sheet for solar cell using the same

    JP2011252112A

  • Sheet including resin layer

    JP2015147886A

Cited By

  • Resin composition, molded body, and method for producing resin composition

    WO2025115733A1