Gel material having four-branched crosslinking points at which strain-induced crystallization is developed
The gel composition, featuring a polymer network with specific functional groups and molecular weights, overcomes the low toughness of existing four-branched gels by inducing crystallization, achieving a breaking stress of 1 MPa or more through elongation-induced crystallization.
Patent Information
- Application Number
- PCT/JP2024/010379
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-29
- Filing Date
- 2024-03-15
- Publication Date
- 2024-10-03
AI Technical Summary
Current polymer gels with four-branched crosslinking points do not exhibit elongation-induced crystallization, resulting in low mechanical toughness, with breaking stress during uniaxial extension tests being less than 1 MPa.
A gel composition comprising a first polymer with an electrophilic functional group and a polyethylene glycol backbone, and a second polymer with a nucleophilic functional group, both being four-branched or linear, forming a polymer network with a solvent, where the total polymer content is 30% by weight or more and the molecular weight between crosslinking points is 10,000 or more, facilitating elongation-induced crystallization.
The gel composition achieves significant toughness with a breaking stress of 1 MPa or more during uniaxial stretching, enhancing mechanical reliability through elongation-induced crystallization.
Smart Images

Figure JPOXMLDOC01-APPB-C000001 
Figure JPOXMLDOC01-APPB-C000002 
Figure JPOXMLDOC01-APPB-C000003
Abstract
Description
Gel material with four-branched crosslinks exhibiting elongation-induced crystallization
[0001] The present invention relates to a gel material containing a polymer network formed by crosslinking a four-branched polymer.
[0002] Materials in which a solvent is trapped within a crosslinked polymer network are called polymer gels. Hydrogels using water as the solvent are expected to be used in biomedical materials such as artificial joints, while ion gels using ionic liquids as the solvent are expected to be used as electrolytes in wearable devices. To realize these applications, the mechanical toughness of polymer gels must be improved. Recently, the use of stretch-induced crystallization, in which oriented polymers crystallize during stretching to prevent breakage, has attracted attention as a method for toughening polymer gels. In 2021, a report was published showing that in slide-ring hydrogels in which polyethylene glycol (PEG) chains are crosslinked with cyclic molecules, the sliding freedom of the cyclic molecules causes uniform orientation of the PEG chains, resulting in stretch-induced crystallization, thereby achieving significant toughness (Non-Patent Document 1). We have also found that stretch-induced crystallization occurs in slide-ring ion gels using ionic liquids and salts as solvents, and have filed a patent application for this finding (Patent Document 1). In addition, in 2022, it was reported that stretch-induced crystallization occurred in a PEG hydrogel with three cross-linking branching points, a cross-link network consisting only of polymer chains without using cyclic molecules, leading to excellent extensibility (Non-Patent Document 2). Cross-linking branching points are known to inhibit polymer chain crystallization because they prevent polymer chains from approaching each other. It is believed that the minimal number of branching points in the three-branched hydrogel led to the efficient stretch-induced crystallization.
[0003] On the other hand, the development of 4-arm cross-linked PEG hydrogels and ion gels has been reported in previous papers and patents, but in none of them did strain-induced crystallization occur, and the breaking stress in uniaxial strain tests was less than 1 MPa (Non-Patent Documents 3 and 4).
[0004] Patent Application No. 2022-113741 (National University Corporation, University of Tokyo) 07.15.2022
[0005] Liu, C., Morimoto, N., Jiang, L., Kawahara, S., Noritomi, T., Yokoyama, H., Mayumi, K., Ito, K. “Tough hydrogels with rapid self-reinforcement”, Science, 372, 1078-1081 (2021).Fujiyabu, T., Sakumichi, N., Katashima, T., Liu, C., Mayumi, K., Chung, U. I., Sakai, T. “Tri-branched gels: Rubbery materials with the lowest branching factor approach the ideal elastic limit”, Science Advances, 8, eabk0010 (2022).Sakai, T., Matsunaga, T., Yamamoto, Y., Ito, C., Yoshida, R., Suzuki, S., Sasaki, N., Shibayama, M., Chung, U. I., “Design and fabrication of a high-strength hydrogel with ideally homogeneous network structure from tetrahedron-like macromonomers”, Macromolecules, 41, 5379-5384 (2008).Tosa, M., Hashimoto, K., Kokubo, H., Ueno, K., Watanabe, M. “Effect of network homogeneity on mechanical, thermal and electrochemical properties of solid polymer electrolytes prepared by homogeneous 4-arm poly (ethylene glycols)”, Soft Matter, 16, 4290-4298 (2020).
[0006] The problem to be solved by the present invention is to provide a gel composition having four-branched crosslinking points that exhibits stretch-induced crystallization.
[0007] The present invention includes the following embodiments: Item 1. A gel composition comprising a polymer network formed by crosslinking a first polymer, which is a tetra-branched or linear polymer having electrophilic functional groups and a polyethylene glycol backbone, and a second polymer, which is a tetra-branched or linear polymer having nucleophilic functional groups and a polyethylene glycol backbone, wherein one or both of the first polymer and the second polymer are tetra-branched polymers, and a solvent, wherein the total amount of the first polymer and the second polymer relative to the amount of the gel composition is 30% by weight or more, and wherein the molecular weight between crosslinking points of the polymer network is 10,000 or more.
[0008] Item 2. The gel composition according to Item 1, wherein the electrophilic functional group of the first polymer is an active ester group, a maleimidyl group, a carboxyl group, an N-hydroxy-succinimidyl group, a sulfosuccinimidyl group, a phthalimidyl group, or a nitrophenyl group.
[0009] Item 3. The gel composition according to Item 1, wherein the nucleophilic functional group of the second polymer is an amino group, a thiol group, or —CO2PhNO2 (wherein Ph is an o-, m-, or p-phenylene group).
[0010] Item 4. The gel composition according to Item 1, wherein the solvent comprises at least one selected from the group consisting of water, an organic solvent, and an ionic liquid.
[0011] Item 5. The gel composition according to Item 1, wherein crystals of the polyethylene glycol skeleton are formed by uniaxial stretching.
[0012] Item 6. The gel composition according to Item 1, wherein a gel sheet made of the gel composition according to Item 1 is punched into a dumbbell shape having a thickness of 1 mm in accordance with JIS K 6251 No. 3 and is uniaxially stretched at an elongation rate of 12.5% / sec, and the measured breaking stress is 1 MPa or more.
[0013] Item 7. The first polymer is a compound represented by the following formula (I) or a compound represented by formula (II): (In formula (I), n1 to n4 may be the same or different, and n1 to n4 are integers of 5 to 300; A is a maleimidyl group, an N-hydroxy-succinimidyl group, a sulfosuccinimidyl group, a phthalimidyl group, an imidazoyl group, an acryloyl group, or a nitrophenyl group; R 1 ~R 4 may be the same or different, and each represents an alkylene group having 1 to 7 carbon atoms, an alkenylene group having 2 to 7 carbon atoms, or —NH—R 5 -, -CO-R 5 -, -R 6 -OR 7 -, -R 6 -NH-R 7 -, -R 6 -COO-R 7 -, -R 6 -COO-NH-R 7 -, -R 6 -CO-R 7 -, -R 6 -NH-CO-R 7 - or -R 6 -CO-NH-R 7 - where R 5 represents an alkylene group having 1 to 7 carbon atoms, and R 6 represents an alkylene group having 1 to 3 carbon atoms, and R 7 represents an alkylene group having 1 to 5 carbon atoms.) (In formula (II), n 12 is an integer from 1 to 10000, B is a maleimidyl group, an N-hydroxy-succinimidyl group, a sulfosuccinimidyl group, a phthalimidyl group, an imidazoyl group, an acryloyl group, or a nitrophenyl group, and R 11 represents an alkylene group having 1 to 7 carbon atoms, an alkenylene group having 2 to 7 carbon atoms, -NH-R 13 -, -CO-R 13 -, -R 14 -OR 15 -, -R 14 -NH-R 15 -, -R 14 -COO-R 15-, -R 14 -COO-NH-R 15 -, -R 14 -CO-R 15 -, R 14 -NH-CO-R 15 -or-R 14 -CO-NH-R 15 - where R 13 represents an alkylene group having 1 to 7 carbon atoms, and R 14 represents an alkylene group having 1 to 3 carbon atoms, and R 15 represents an alkylene group having 1 to 5 carbon atoms, and R 12 represents an alkylene group having 1 to 7 carbon atoms, an alkenylene group having 2 to 7 carbon atoms, -NH-R 16 -, -CO-R 16 -, -R 17 -OR 18 -, -R 17 -NH-R 18 -, -R 17 -COO-R 18 -, -R 17 -COO-NH-R 18 -, -R 17 -CO-R 18 -, R 17 -NH-CO-R 18 -or-R 17 -CO-NH-R 18 - where R 16 represents an alkylene group having 1 to 7 carbon atoms, and R 17 represents an alkylene group having 1 to 3 carbon atoms, and R 18 represents an alkylene group having 1 to 5 carbon atoms.) The gel composition according to item 1, wherein the second polymer is a compound represented by the following formula (III) or a compound represented by formula (IV): (In formula (III), n 21 ~n 24 may be the same or different, and n 21 ~n 24 is an integer of 25 to 250, D is a thiol group, an amino group, or -COOPhNO2 (Ph represents an o-, m-, or p-phenylene group), and R 21 ~R 24may be the same or different, and each represents an alkylene group having 1 to 7 carbon atoms, an alkenylene group having 2 to 7 carbon atoms, or —NH—R 25 -, -CO-R 25 -, -R 26 -OR 27 -, -R 26 -NH-R 27 -, -R 26 -COO-R 27 -, -R 26 -COO-NH-R 27 -, -R 26 -CO-R 27 -, R 26 -NH-CO-R 27 -or-R 26 -CO-NH-R 27 - where R 25 represents an alkylene group having 1 to 7 carbon atoms, and R 26 represents an alkylene group having 1 to 3 carbon atoms, and R 27 represents an alkylene group having 1 to 5 carbon atoms.) (In formula (IV), n 32 is an integer of 1 to 10000, E is a thiol group, an amino group, or -COOPhNO2 (Ph represents an o-, m-, or p-phenylene group), and R 31 represents an alkylene group having 1 to 7 carbon atoms, an alkenylene group having 2 to 7 carbon atoms, -NH-R 33 -, -CO-R 33 -, -R 34 -OR 35 -, -R 34 -NH-R 35 -, -R 34 -COO-R 35 -, -R 34 -COO-NH-R 35 -, -R 34 -CO-R 35 -, R 34 -NH-CO-R 35 -or-R 34 -CO-NH-R 35 - where R 33 represents an alkylene group having 1 to 7 carbon atoms, and R 34 represents an alkylene group having 1 to 3 carbon atoms, and R 35 represents an alkylene group having 1 to 5 carbon atoms, and R32 represents an alkylene group having 1 to 7 carbon atoms, an alkenylene group having 2 to 7 carbon atoms, -NH-R 36 -, -CO-R 36 -, -R 37 -OR 38 -, -R 37 -NH-R 38 -, -R 37 -COO-R 38 -, -R 37 -COO-NH-R 38 -, -R 37 -CO-R 38 -, R 37 -NH-CO-R 38 -or-R 37 -CO-NH-R 38 - where R 36 represents an alkylene group having 1 to 7 carbon atoms, and R 37 represents an alkylene group having 1 to 3 carbon atoms, and R 38 represents an alkylene group having 1 to 5 carbon atoms.)
[0014] Item 8. A gel sheet formed from the gel composition according to any one of items 1 to 7.
[0015] Overview of gel compositions according to embodiments of the present invention. (A) Stress-extension curves for three types of 4-branched hydrogels with different molecular weights between crosslinks (all PEG concentrations of 40 wt%). (B)-(D) Wide-angle X-ray scattering (WAXS) images at maximum extension ratios: (B) Molecular weight between crosslinks of 5kJ (Tetra 10kJ + Tetra 10kJ), (C) Molecular weight between crosslinks of 10kJ (Tetra 20kJ + Tetra 20kJ), (D) Molecular weight between crosslinks of 30kJ (Linear 20kJ + Tetra 20kJ). Extension and vertical WAXS one-dimensional profiles (λ = 10, 11) of the WAXS image in Figure 2(C). Extension and vertical WAXS one-dimensional profiles of the WAXS image in Figure 2(D). (A) Stress-extension curves for three types of 4-branched hydrogels with different PEG concentrations (Linear 20k + Tetra 20k, all with molecular weights between crosslinks of 30k). (B)-(D) Wide-angle X-ray scattering at the maximum extension ratio. (B) PEG concentration 10 wt%, (C) PEG concentration 20 wt%, (D) PEG concentration 40 wt%. (A) WAXS image of a 4-branched ionic gel under extension, (B) ionic liquid, and (C) one-dimensional WAXS profile perpendicular to the extension direction. WAXS images of 4-branched hydrogels obtained using four different ionic liquids: [C2mim][NTf2], Li[NTf2], [Li(G3)][NTf2], and [Li(G4)][NTf2].
[0016] As used herein, the singular forms (a, an, the) include both the singular and the plural unless otherwise expressly stated herein or clearly contradicted by context.
[0017] In this specification, the term "comprise" is a concept that encompasses "consist essentially of" and "consist only of."
[0018] In the numerical ranges described in stages in this specification, the upper or lower limit of a certain numerical range can be arbitrarily combined with the upper or lower limit of another numerical range. Furthermore, in the numerical ranges described in this specification, the upper or lower limit of the numerical range may be replaced with a value shown in an example or a value that can be unambiguously derived from an example. Furthermore, in this specification, a numerical value connected with "to" means a numerical range that includes the numbers before and after "to" as the upper and lower limits.
[0019] In the present invention, we discovered that stretch-induced crystallization occurs in a four-branch crosslinked polymer gel, which has a more common crosslinked structure, and found that excellent toughness can be achieved.
[0020] According to one aspect of the present invention, there is provided a gel composition comprising a polymer network formed by crosslinking a first polymer, which is a tetra-branched or linear polymer having electrophilic functional groups and a polyethylene glycol backbone, and a second polymer, which is a tetra-branched or linear polymer having nucleophilic functional groups and a polyethylene glycol backbone, wherein one or both of the first polymer and the second polymer are tetra-branched polymers; and a solvent; wherein the total amount of the first polymer and the second polymer relative to the amount of the gel composition is 30% by weight or more; and wherein the molecular weight between crosslinking points of the polymer network is 10,000 or more.
[0021] A "tetra-branched polymer with a polyethylene glycol backbone" is a hydrophilic polymer having a structure in which four polyethylene glycol chains branch from the center. Gels consisting of such a tetra-branched polyethylene glycol backbone are generally known as Tetra-PEG gels.
[0022] A polymer network is constructed by an AB cross-end coupling reaction between two four-branched polymers: the first polymer has electrophilic functional groups and the second polymer has nucleophilic functional groups (Matsunaga et al., Macromolecules, Vol. 42, No., pp. 1344-1361, 2009).
[0023] Tetra-PEG gels can be easily prepared in situ by simply mixing two polymer solutions, and the gelation time can be controlled by adjusting the pH and ionic strength during gel preparation. Furthermore, because this gel is primarily composed of PEG, it is also highly biocompatible.
[0024] When the total amount of the first polymer and the second polymer relative to the amount of the gel composition is 30% by weight or more and the molecular weight between crosslinking points of the polymer network is 10,000 or more, stretch-induced crystallization occurs, resulting in a toughened gel composition. When the total amount of the first polymer and the second polymer relative to the amount of the gel composition is less than 30% by weight or when the molecular weight between crosslinking points of the polymer network is less than 10,000, stretch-induced crystallization does not occur even when the gel composition is stretched to break.
[0025] The tetra-branched polymer used as the first polymer preferably has one or more electrophilic functional groups on the side chain or at the end, and the tetra-branched polymer used as the second polymer preferably has one or more nucleophilic functional groups on the side chain or at the end.
[0026] The electrophilic functional group of the first polymer can be an active ester group. Examples of such active ester groups include maleimidyl groups, carboxyl groups, N-hydroxysuccinimidyl (NHS) groups, sulfosuccinimidyl groups, phthalimidyl groups, imidazoyl groups, acryloyl groups, and nitrophenyl groups. Those skilled in the art can appropriately use any electrophilic functional group known to those skilled in the art. In a preferred embodiment, the electrophilic functional group of the first polymer is selected from the group consisting of an active ester group, a maleimidyl group, a carboxyl group, an N-hydroxysuccinimidyl group, a sulfosuccinimidyl group, a phthalimidyl group, and a nitrophenyl group. In a more preferred embodiment, all of the electrophilic functional groups of the first polymer are active ester groups, a maleimidyl group, a carboxyl group, an N-hydroxysuccinimidyl group, a sulfosuccinimidyl group, a phthalimidyl group, or a nitrophenyl group.
[0027] The electrophilic functional groups of the first polymer may be the same or different, but are preferably the same. The same functional groups ensure uniform reactivity with the nucleophilic functional groups that form crosslinks, allowing a gel with a uniform three-dimensional structure to be obtained.
[0028] The nucleophilic functional group of the second polymer may include an amino group, a thiol group (-SH), or -CO2PhNO2 (Ph represents an o-, m-, or p-phenylene group), and those skilled in the art can appropriately use any nucleophilic functional group known to those skilled in the art. In a preferred embodiment, the nucleophilic functional group of the second polymer is selected from the group consisting of an amino group, a thiol group (-SH), and CO2PhNO2 (Ph represents an o-, m-, or p-phenylene group). In a more preferred embodiment, all of the nucleophilic functional groups of the second polymer are amino groups, a thiol group (-SH), or -CO2PhNO2 (Ph represents an o-, m-, or p-phenylene group).
[0029] The nucleophilic functional groups of the second polymer may be the same or different, but are preferably the same, since the reactivity with the electrophilic functional groups that form crosslinks is uniform, making it easier to obtain a gel with a uniform three-dimensional structure.
[0030] In a preferred embodiment, the first polymer is a compound represented by the following formula (I) or a compound represented by formula (II):
[0031]
[0032] (In formula (I), n1 to n4 may be the same or different, and n1 to n4 are integers of 5 to 300; A is a maleimidyl group, an N-hydroxy-succinimidyl group, a sulfosuccinimidyl group, a phthalimidyl group, an imidazoyl group, an acryloyl group, or a nitrophenyl group; R 1 ~R 4 may be the same or different, and each represents an alkylene group having 1 to 7 carbon atoms, an alkenylene group having 2 to 7 carbon atoms, or —NH—R 5 -, -CO-R 5 -, -R6 -OR 7 -, -R 6 -NH-R 7 -, -R 6 -COO-R 7 -, -R 6 -COO-NH-R 7 -, -R 6 -CO-R 7 -, -R 6 -NH-CO-R 7 - or -R 6 -CO-NH-R 7 - where R 5 represents an alkylene group having 1 to 7 carbon atoms, and R 6 represents an alkylene group having 1 to 3 carbon atoms, and R 7 represents an alkylene group having 1 to 5 carbon atoms.)
[0033]
[0034] (In formula (II), n 12 is an integer from 1 to 10000, B is a maleimidyl group, an N-hydroxy-succinimidyl group, a sulfosuccinimidyl group, a phthalimidyl group, an imidazoyl group, an acryloyl group, or a nitrophenyl group, and R 11 represents an alkylene group having 1 to 7 carbon atoms, an alkenylene group having 2 to 7 carbon atoms, -NH-R 13 -, -CO-R 13 -, -R 14 -OR 15 -, -R 14 -NH-R 15 -, -R 14 -COO-R 15 -, -R 14 -COO-NH-R 15 -, -R 14 -CO-R 15 -, R 14 -NH-CO-R 15 -or-R 14 -CO-NH-R 15 - where R 13 represents an alkylene group having 1 to 7 carbon atoms, and R 14 represents an alkylene group having 1 to 3 carbon atoms, and R 15 represents an alkylene group having 1 to 5 carbon atoms, and R 12represents an alkylene group having 1 to 7 carbon atoms, an alkenylene group having 2 to 7 carbon atoms, -NH-R 16 -, -CO-R 16 -, -R 17 -OR 18 -, -R 17 -NH-R 18 -, -R 17 -COO-R 18 -, -R 17 -COO-NH-R 18 -, -R 17 -CO-R 18 -, R 17 -NH-CO-R 18 -or-R 17 -CO-NH-R 18 - where R 16 represents an alkylene group having 1 to 7 carbon atoms, and R 17 represents an alkylene group having 1 to 3 carbon atoms, and R 18 represents an alkylene group having 1 to 5 carbon atoms.
[0035] In the above formula (I), n1 to n4 may be the same or different. The closer the values of n1 to n4 are, the more uniform the three-dimensional structure of the gel will be, and the stronger the gel will be. It is preferable that they are the same. If the values of n1 to n4 are too high, the strength of the gel will be weak, and if the values of n1 to n4 are too low, the gel will be difficult to form due to steric hindrance of the compound. Therefore, n1 to n4 may be, for example, an integer value of 5 to 300, with 20 to 250 being preferred, 30 to 180 being more preferred, and 45 to 115 being even more preferred. In one embodiment, n1 to n4 are integers of 5 to 300. The molecular weight of the compound represented by formula (I) is 5 x 10 3 ~5×10 4 Da is preferred, 7.5 x 10 3 ~3×10 4 Da is preferred, 1 x 10 4 ~2×10 4 Da is more preferred.
[0036] In the above formula (I), R 1 ~R 4 is the linker moiety connecting the functional group and the core moiety. R 1 ~R 4may be the same or different, but are preferably the same in order to produce a high-strength gel having a uniform three-dimensional structure.
[0037] In the above formula (II), n 12 is, for example, an integer value of 1 to 10,000, preferably 25 to 5,000, more preferably 50 to 2,500, and even more preferably 100 to 1,000. The molecular weight of the compound represented by formula (II) is 1.1 × 10 3 ~2.2×10 5 Da is preferred, 2.2 x 10 3 ~1.1×10 5 Da is preferred, 4.4 x 10 3 ~4.4×10 5 Da is more preferred.
[0038] where R 1 ~R 4 , R 11 , and R 12 With respect to each of the above, examples of the alkylene group having 1 to 7 carbon atoms include a methylene group, an ethylene group, a propylene group, and a butylene group. The alkenylene group having 2 to 7 carbon atoms is a linear or branched alkenylene group having 2 to 7 carbon atoms and having one or more double bonds in the chain, and examples thereof include divalent groups having double bonds formed by removing 2 to 5 hydrogen atoms from adjacent carbon atoms of the alkylene group having 1 to 7 carbon atoms.
[0039] In a preferred embodiment, the second polymer is a compound represented by the following formula (III) or a compound represented by formula (IV):
[0040]
[0041] (In formula (III), n 21 ~n 24 may be the same or different, and n 21 ~n 24 is an integer of 25 to 250, D is a thiol group, an amino group, or -COOPhNO2 (Ph represents an o-, m-, or p-phenylene group), and R 21 ~R 24may be the same or different, and each represents an alkylene group having 1 to 7 carbon atoms, an alkenylene group having 2 to 7 carbon atoms, or —NH—R 25 -, -CO-R 25 -, -R 26 -OR 27 -, -R 26 -NH-R 27 -, -R 26 -COO-R 27 -, -R 26 -COO-NH-R 27 -, -R 26 -CO-R 27 -, R 26 -NH-CO-R 27 -or-R 26 -CO-NH-R 27 - where R 25 represents an alkylene group having 1 to 7 carbon atoms, and R 26 represents an alkylene group having 1 to 3 carbon atoms, and R 27 represents an alkylene group having 1 to 5 carbon atoms.)
[0042]
[0043] (In formula (IV), n 32 is an integer of 1 to 10000, E is a thiol group, an amino group, or -COOPhNO2 (Ph represents an o-, m-, or p-phenylene group), and R 31 represents an alkylene group having 1 to 7 carbon atoms, an alkenylene group having 2 to 7 carbon atoms, -NH-R 33 -, -CO-R 33 -, -R 34 -OR 35 -, -R 34 -NH-R 35 -, -R 34 -COO-R 35 -, -R 34 -COO-NH-R 35 -, -R 34 -CO-R 35 -, R 34 -NH-CO-R 35 -or-R 34 -CO-NH-R 35 - where R 33 represents an alkylene group having 1 to 7 carbon atoms, and R 34represents an alkylene group having 1 to 3 carbon atoms, and R 35 represents an alkylene group having 1 to 5 carbon atoms, and R 32 represents an alkylene group having 1 to 7 carbon atoms, an alkenylene group having 2 to 7 carbon atoms, -NH-R 36 -, -CO-R 36 -, -R 37 -OR 38 -, -R 37 -NH-R 38 -, -R 37 -COO-R 38 -, -R 37 -COO-NH-R 38 -, -R 37 -CO-R 38 -, R 37 -NH-CO-R 38 -or-R 37 -CO-NH-R 38 - where R 36 represents an alkylene group having 1 to 7 carbon atoms, and R 37 represents an alkylene group having 1 to 3 carbon atoms, and R 38 represents an alkylene group having 1 to 5 carbon atoms.)
[0044] In formula (III), n 21 ~n 24 may be the same or different. 21 ~n 24 The closer the values of n are, the more uniform the three-dimensional structure can be, and the higher the strength. Therefore, in order to obtain a gel with high strength, it is preferable that n be the same. 21 ~n 24 If the value of is too high, the strength of the gel will be weak, and 21 ~n 24 If the value of n is too low, the gel is difficult to form due to the steric hindrance of the compound. 21 ~n 24 is preferably 25 to 250, more preferably 35 to 180, and even more preferably 50 to 120. The molecular weight of the compound represented by formula (III) is 5×10 3 ~5×10 4 Da is preferred, 7.5 x 10 3 ~3×10 4 Da is preferred, 1 x 10 4 ~2×104 Da is more preferred.
[0045] In the above formula (III), R 21 ~R 24 is a linker moiety connecting the functional group and the core moiety. 21 ~R 24 may be the same or different, but are preferably the same in order to produce a high-strength gel having a uniform three-dimensional structure.
[0046] In the above formula (IV), n 32 is, for example, an integer value of 1 to 10,000, preferably 25 to 5,000, more preferably 50 to 2,500, and even more preferably 100 to 1,000. The molecular weight of the compound represented by formula (IV) is 5×10 3 ~5×10 4 Da is preferred, 7.5 x 10 3 ~3×10 4 Da is preferred, 1 x 10 4 ~2×10 4 Da is more preferred.
[0047] where R 21 ~R 24 , R 31 , and R 32 With respect to each of the above, examples of the alkylene group having 1 to 7 carbon atoms include a methylene group, an ethylene group, a propylene group, and a butylene group. The alkenylene group having 2 to 7 carbon atoms is a linear or branched alkenylene group having 2 to 7 carbon atoms and having one or more double bonds in the chain, and examples thereof include divalent groups having double bonds formed by removing 2 to 5 hydrogen atoms from adjacent carbon atoms of the alkylene group having 1 to 7 carbon atoms.
[0048] In another preferred embodiment, the first polymer is a compound represented by formula (I) or a compound represented by formula (II):
[0049]
[0050] (In formula (I), n1 to n4 may be the same or different, and n1 to n4 are integers of 5 to 300; A is a maleimidyl group, an N-hydroxy-succinimidyl group, a sulfosuccinimidyl group, a phthalimidyl group, an imidazoyl group, an acryloyl group, or a nitrophenyl group; R 1 ~R 4 may be the same or different, and each represents an alkylene group having 1 to 7 carbon atoms, an alkenylene group having 2 to 7 carbon atoms, or —NH—R 5 -, -CO-R 5 -, -R 6 -OR 7 -, -R 6 -NH-R 7 -, -R 6 -COO-R 7 -, -R 6 -COO-NH-R 7 -, -R 6 -CO-R 7 -, -R 6 -NH-CO-R 7 - or -R 6 -CO-NH-R 7 - where R 2 represents an alkylene group having 1 to 7 carbon atoms, and R 6 represents an alkylene group having 1 to 3 carbon atoms, and R 7 represents an alkylene group having 1 to 5 carbon atoms.)
[0051]
[0052] (In formula (II), n 12 is an integer from 1 to 10000, B is a maleimidyl group, an N-hydroxy-succinimidyl group, a sulfosuccinimidyl group, a phthalimidyl group, an imidazoyl group, an acryloyl group, or a nitrophenyl group, and R 11 represents an alkylene group having 1 to 7 carbon atoms, an alkenylene group having 2 to 7 carbon atoms, -NH-R 13 -, -CO-R 13 -, -R 14 -OR 15 -, -R 14 -NH-R 15 -, -R 14 -COO-R 15 -, -R14 -COO-NH-R 15 -, -R 14 -CO-R 15 -, R 14 -NH-CO-R 15 -or-R 14 -CO-NH-R 15 - where R 13 represents an alkylene group having 1 to 7 carbon atoms, and R 14 represents an alkylene group having 1 to 3 carbon atoms, and R 15 represents an alkylene group having 1 to 5 carbon atoms, and R 12 represents an alkylene group having 1 to 7 carbon atoms, an alkenylene group having 2 to 7 carbon atoms, -NH-R 16 -, -CO-R 16 -, -R 17 -OR 18 -, -R 17 -NH-R 18 -, -R 17 -COO-R 18 -, -R 17 -COO-NH-R 18 -, -R 17 -CO-R 18 -, R 17 -NH-CO-R 18 -or-R 17 -CO-NH-R 18 - where R 16 represents an alkylene group having 1 to 7 carbon atoms, and R 17 represents an alkylene group having 1 to 3 carbon atoms, and R 18 represents an alkylene group having 1 to 5 carbon atoms; and the second polymer is a compound represented by the following formula (III) or a compound represented by the following formula (IV):
[0053]
[0054] (In formula (III), n 21 ~n 24 may be the same or different, and n 21 ~n 24 is an integer of 25 to 250, D is a thiol group, an amino group, or -COOPhNO2 (Ph represents an o-, m-, or p-phenylene group), and R 21 ~R 24may be the same or different, and each represents an alkylene group having 1 to 7 carbon atoms, an alkenylene group having 2 to 7 carbon atoms, or —NH—R 25 -, -CO-R 25 -, -R 26 -OR 27 -, -R 26 -NH-R 27 -, -R 26 -COO-R 27 -, -R 26 -COO-NH-R 27 -, -R 26 -CO-R 27 -, R 26 -NH-CO-R 27 -or-R 26 -CO-NH-R 27 - where R 25 represents an alkylene group having 1 to 7 carbon atoms, and R 26 represents an alkylene group having 1 to 3 carbon atoms, and R 27 represents an alkylene group having 1 to 5 carbon atoms.)
[0055]
[0056] (In formula (IV), n 32 is an integer of 1 to 10000, E is a thiol group, an amino group, or -COOPhNO2 (Ph represents an o-, m-, or p-phenylene group), and R 31 represents an alkylene group having 1 to 7 carbon atoms, an alkenylene group having 2 to 7 carbon atoms, -NH-R 33 -, -CO-R 33 -, -R 34 -OR 35 -, -R 34 -NH-R 35 -, -R 34 -COO-R 35 -, -R 34 -COO-NH-R 35 -, -R 34 -CO-R 35 -, R 34 -NH-CO-R 35 -or-R 34 -CO-NH-R 35 - where R 33 represents an alkylene group having 1 to 7 carbon atoms, and R 34represents an alkylene group having 1 to 3 carbon atoms, and R 35 represents an alkylene group having 1 to 5 carbon atoms, and R 32 represents an alkylene group having 1 to 7 carbon atoms, an alkenylene group having 2 to 7 carbon atoms, -NH-R 36 -, -CO-R 36 -, -R 37 -OR 38 -, -R 37 -NH-R 38 -, -R 37 -COO-R 38 -, -R 37 -COO-NH-R 38 -, -R 37 -CO-R 38 -, R 37 -NH-CO-R 38 -or-R 37 -CO-NH-R 38 - where R 36 represents an alkylene group having 1 to 7 carbon atoms, and R 37 represents an alkylene group having 1 to 3 carbon atoms, and R 38 represents an alkylene group having 1 to 5 carbon atoms.) and one or both of the first polymer and the second polymer are 4-branched polymers.
[0057] That is, the first polymer is a compound represented by formula (I) and the second polymer is a compound represented by formula (III), or the first polymer is a compound represented by formula (I) and the second polymer is a compound represented by formula (IV), or the first polymer is a compound represented by formula (II) and the second polymer is a compound represented by formula (III).
[0058] In a preferred embodiment, the gel composition comprises a hydrogel formed by gelling a polymer network formed by crosslinking a first polymer and a second polymer. In this specification, the term "gel" generally refers to a dispersion system of polymers that is highly viscous and has lost fluidity, and in which the storage modulus G' and loss modulus G" satisfy the relationship G'≧G". A hydrogel refers to a state in which the gel contains a solvent such as water inside.
[0059] The type of solvent constituting the gel composition is not particularly limited, but preferably the solvent includes at least one selected from the group consisting of water, organic solvents, and ionic liquids.
[0060] Organic solvents include alcohols such as methanol and ethanol, DMSO, etc. Preferably, the solvent is water.
[0061] An ionic liquid is formed by bonding between a cation and an anion, and is liquid at room temperature (20° C.) or a temperature around that temperature. As the ionic liquid, various known ionic liquids can be used.
[0062] The cation may be, for example, one or more selected from the group consisting of an imidazolium ion, a pyridinium ion, a tetraalkylammonium ion, a pyrrolidinium ion, a piperidinium ion, a tetraalkylphosphonium ion, a pyrazolium ion, a trialkylsulfonium ion, a morpholium ion, a guanidinium ion, and a lithium ion, each of which may have a substituent. Alternatively, the cation may be a combination of a lithium ion and RO(CH2CHO) n It may also be a complex cation consisting of a glyme represented by -R (R is an alkyl group having 1 to 4 carbon atoms, and n is 2 to 6). Lithium ions and glyme usually form a complex cation in a 1:1 molar ratio.
[0063] The anion may be, for example, a halide ion (fluorine, chlorine, iodine, bromine), a tetrafluoroborate ion (BF4 - ), BF3CF3-, BF3C2F5-, BF3C3F7-, BF3C4F9-, hexafluorophosphate ion (PF6 - ), bis(fluorosulfonyl)amide ion (FSA - ), bis(trifluoromethanesulfonyl)imide ion ((CF3SO2)2N-, NTf2-, TFSA -(also known as fluoromethanesulfonyl)imide ion ((FSO2)2N-), bis(pentafluoroethanesulfonyl)imide ion ((CF3CF2SO2)2N-), perchlorate ion (ClO4-), tris(trifluoromethanesulfonyl)carbonate ion (CF3SO2)3C-), trifluoromethanesulfonate ion (CF3SO3-), dicyanamide ion ((CN)2N-), thiocyanate ion (SCN - ), nitrate ions (NO3 - ), sulfate ions (SO4 2- ), thiosulfate ion (S2O3 2- ), carbonate ions (CO3 2- ), bicarbonate ion (HCO3 - ), phosphate ion, phosphite ion, hypophosphite ion, halogen oxide ion (XO4 - , XO3 - , XO2 - or XO - , where X is fluorine, chlorine, bromine, or iodine), a halogenated acetate ion ((CX n H 3-n )COO - , where X is fluorine, chlorine, bromine or iodine, and n is 1 to 3), tetraphenylborate ion (BPh4 - ) and its derivatives (B(Aryl)4 - ) wherein Aryl is a substituted phenyl group).
[0064] Among these, preferred ionic liquids include those in which the cation is 1-ethyl-3-methylimidazolium ion, [N(CH3)(CH3)(C2H5)(C2H4OC2H4OCH3)]+, [N(CH3)(C2H5)(C2H5)(C2H4OCH3)]+, and the anion is halogen ion, tetrafluoroborate ion, bis(trifluoromethanesulfonyl)imide ion ((CF3SO2)2N - ) can be specifically exemplified, and 1-ethyl-3-methylimidazolium ion and bis(trifluoromethanesulfonyl)imide ion ((CF3SO2)2N -) is particularly preferred.
[0065] Preferred ionic liquids that are in a liquid state at or near room temperature (20°C) include those composed of one or more cations (preferably imidazolium ions and quaternary ammonium ions) represented by the following general formulas (V) to (VIII) and an anion (X-).
[0066]
[0067] In formulas (V) to (VIII), R represents a linear or branched alkyl group having 1 to 12 carbon atoms or a linear or branched alkyl group containing an ether bond and having a total of 3 to 12 carbon atoms and oxygen atoms.
[0068] In formula (V), R 1 represents a linear or branched alkyl group having 1 to 4 carbon atoms or a hydrogen atom. In formula (V), R and R 1 are preferably not the same.
[0069] In formulas (VII) and (VIII), x is an integer of 1 to 4. In formulas (VIII) and (VIII), two R groups may be joined together to form a 3- to 8-membered, preferably 5- or 6-membered, aliphatic saturated cyclic group.
[0070] Examples of linear or branched alkyl groups having 1 to 12 carbon atoms include methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, t-butyl, pentyl, hexyl, heptyl, octyl, nonyl, decyl, undecyl, dodecyl, etc. The number of carbon atoms is preferably 1 to 8, more preferably 1 to 6.
[0071] Examples of the straight-chain or branched alkyl group having 1 to 4 carbon atoms include methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, and t-butyl.
[0072] Examples of linear or branched alkyl groups containing an ether bond and having a total of 3 to 12 carbon atoms and oxygen atoms include CH2OCH3, CH2CH2OCH3, CH2OCH2CH3, CH2CH2OCH2CH3, (CH2)p (OCH2CH2) q OR2 (where p is an integer between 1 and 4, q is an integer between 1 and 4, R 2 represents CH3 or C2H5).
[0073] Anion (X - ) is tetrafluoroborate ion (BF4 - ), BF3CF3 - , BF3C2F5 - , BF3C3F7 - , BF3C4F9 - , hexafluorophosphate ion (PF6 - ), bis(fluorosulfonyl)amide ion (FSA - ), bis(trifluoromethanesulfonyl)imide ion ((CF3SO2)2N-, NTf2-, TFSA - bis(fluoromethanesulfonyl)imide ion ((FSO2)2N - ), bis(pentafluoroethanesulfonyl)imide ion ((CF3CF2SO2)2N - ), perchlorate ion (ClO4 - ), tris(trifluoromethanesulfonyl)carbonate ion (CF3SO2)3C - ), trifluoromethanesulfonate ion (CF3SO3 - ), dicyanamide ion ((CN)N - ), trifluoroacetate ion (CF3COO - ), organic carboxylate ions and halogen ions can be exemplified.
[0074] When the gel composition contains a solvent, the amount of the solvent in the gel composition is not particularly limited, but from the viewpoint of the stretchability and high toughness of the gel composition, it is more preferably 1% by mass or more and 80% by mass or less, and more preferably 1% by mass or more and 60% by mass or less. In a preferred embodiment, the solvent is an ionic liquid. In another preferred embodiment, the solvent is water.
[0075] In the gel composition, the mass ratio of the polymer network to the solvent (polymer network:solvent) is not particularly limited, but is preferably 99:1 to 20:80 from the viewpoints of the stretchability and high toughness of the gel composition, and more preferably 99:1 to 40:60 from the viewpoint of high toughness. In a preferred embodiment, the solvent is an ionic liquid. In another preferred embodiment, the solvent is water.
[0076] When the gel composition contains water, the amount of water in the gel composition may be adjusted by drying the gel composition after production.
[0077] The gel composition may further comprise optional additives.
[0078] In the gel composition of the present invention, stretch-induced crystallization occurs upon uniaxial stretching, resulting in the formation of crystals of the polyethylene glycol backbone. Such a gel composition is tougher than a gel composition that does not undergo stretch-induced crystallization.
[0079] In a preferred embodiment, the gel composition has a breaking stress of 1 MPa or more, as measured by deforming a gel sheet made of the gel composition, which has been punched into a dumbbell shape having a thickness of 1 mm in accordance with JIS K 6251 No. 3, by uniaxial stretching at an elongation rate of 12.5% / sec.
[0080] According to another aspect of the present invention, there is also provided a gel sheet, which is a sheet formed from the gel composition of any of the above embodiments.
[0081] An overview of a gel composition according to an embodiment of the present invention is shown in Figure 1. This embodiment of the gel composition of the present invention is a gel material comprising a 4-branched polymer network 1 obtained by mixing and reacting a 4-branched polymer having reactive group A at its terminal, each arm of which has a uniform molecular weight, with a 4-branched polymer or linear polymer having reactive group B in a solvent or a solution containing the solvent 2 so that the molar ratio of the terminals is the same. In this case, reactive group A and reactive group B are electrophilic functional groups and nucleophilic functional groups (in any order), such as active ester and amino terminals, maleimide and thiol terminals, and maleimide and amine terminals (the order of the preceding and succeeding functional groups is not specified). PEG is used as the polymer. The solvent may be a polar solvent or an organic solvent, such as water, an ionic liquid, or a salt. When the PEG concentration in the gel is 40 wt% or more and the PEG molecular weight between crosslinks is 10,000 g / mol or more, stretch-induced crystallization occurs and the gel composition exhibits a large breaking stress of 1 MPa or more when stretched uniaxially, for example, as shown by the arrow in Figure 1. In this specification, the molecular weight between crosslinks is calculated as the sum of the molecular weights of the arms of the tetrabranched polymer having reactive group A and the arms of the tetrabranched polymer having reactive group B, and the molecular weights of the arms of each tetrabranched polymer are measured by gel permeation chromatography (GPC) or matrix-assisted laser desorption / ionization time-of-flight mass spectrometry (MALDI-TOFMS).
[0082] A typical example of a method for producing a gel composition according to an embodiment of the present invention will be described below, although the present invention is not necessarily limited to such a production method.
[0083] A preferred embodiment of the method for producing a gel composition includes a step of crosslinking a first polymer, which is a tetra-branched or linear polymer having electrophilic functional groups and a polyethylene glycol backbone, with a second polymer, which is a tetra-branched or linear polymer having nucleophilic functional groups and a polyethylene glycol backbone, in a solvent to obtain a gel composition, thereby enabling the hydrogel to be obtained in one step.
[0084] The initial concentrations of the first and second polymers are the overlapping concentrations C *less than 1 / 3C * Here, the "overlap concentration" (also called "overlap concentration") refers to the concentration at which polymers in a solvent begin to spatially contact each other, and is generally less than the overlap concentration C * is expressed by the following formula:
[0085]
[0086] (In the formula, M w is the weight average molecular weight of the polymer; α is the specific gravity of the solvent; N A is the Avogadro constant; R g is the radius of gyration of the polymer.
[0087] Overlap density C * For the calculation method, see, for example, Polymer Physics (by M. Rubinstein and R. Colby). Specifically, for example, it can be determined by measuring the viscosity of a dilute solution and using the Flory-Fox equation.
[0088] Furthermore, since this production method involves gelation in one step, the initial concentration of the tetrabranched polymer must be equal to or higher than the critical gelation concentration. Here, the term "critical gelation concentration" refers to the minimum concentration of raw polymers required to achieve gelation in a system in which a three-dimensional gel is constructed by crosslinking raw polymers, and is also referred to as the minimum gelation concentration. In the present invention, the term "critical gelation concentration" includes, for example, in a system in which two or more raw polymers are used, a case in which the total concentration of the raw polymers does not reach a concentration that leads to gelation, as well as a case in which the concentration of only one raw polymer is low, i.e., a case in which gelation does not occur due to an unequal ratio of the raw polymers.
[0089] Generally, the critical gelation concentration (minimum gelation concentration) depends on the type of raw polymer used, but such a concentration is known in the art or can be easily determined experimentally by a person skilled in the art. Typically, it is 0.5 to 5% by weight, with the lower limit being about 1 / 5 of the overlap concentration.
[0090] The crosslinking reaction of the first and second polymers can be carried out by mixing solvents containing the first and second polymers or solutions containing the solvents. The addition rate, mixing rate, and mixing ratio of each solution are not particularly limited, and can be appropriately adjusted by a person skilled in the art.
[0091] The first and second polymer solutions can be mixed using, for example, a two-liquid mixing syringe such as that disclosed in International Publication WO 2007 / 083522. The temperature of the two liquids during mixing is not particularly limited, as long as the first and second polymers are dissolved and each liquid has fluidity. For example, the temperature of the solutions during mixing can be in the range of 1°C to 100°C. The temperatures of the two liquids may be different, but it is preferable that they are the same temperature, as this facilitates mixing of the two liquids.
[0092] Preferably, in the first embodiment of the method for producing a gel composition of the present invention, the final gel composition can be obtained within a reaction time of 2 hours or less, preferably within a reaction time of 1 hour or less.
[0093] Industrial Value of the Invention Compared to previously reported slide-ring gels that exhibit strain-induced crystallization, 4-branched polymer gels can be synthesized simply by mixing macromers, making them easier to synthesize. Although strain-induced crystallization has been reported for tri-branched polymer gels, 4-branched cross-linked polymer gels are more common, offering advantages in expanding the range of applications as a material and reducing manufacturing costs. As noted above, 4-branched gels can be synthesized by combining 4-branched macromers with linear polymers, which allows for a larger proportion of inexpensive linear polymers, bringing production costs closer to those of conventional gels.
[0094] Another important point about this invention is that we discovered strain-induced crystallization using a wide range of polar solvents, including water and ionic liquids. Hydrogels using water as the solvent are expected to be used in biomedical materials, while ionic gels using salts or ionic liquids are expected to be used in electrochemical materials such as wearable devices and soft actuators. These applications require durability against repeated deformation, and this gel can achieve high mechanical reliability by being toughened by strain-induced crystallization.
[0095] 1. Preparation of 4-branched hydrogels. Polymer networks were obtained by reacting 4-branched PEG (TetraPEG) with each other or with linear PEG (LinearPEG) in water. TetraPEG, which has succinimide reactive ends, and either TetraPEG or LinearPEG, which has amine reactive ends, were dissolved in buffer. A succinimide-terminated PEG solution and an amine-terminated PEG solution were prepared, and the gelation reaction was initiated by mixing the two solutions. The end groups were mixed in an equimolar ratio. McIlvaine buffer solution was used. A citric acid solution (0.2 M) and a disodium hydrogen phosphate solution (0.4 M) were prepared to the desired concentrations. These solutions were mixed according to McIlvaine TC (1921). "A buffer solution for colorimetric comparison." J. Biol. Chem. 49 (1): 183-186. The buffer concentration was adjusted by diluting with pure water to obtain a buffer with the desired pH. As shown in Table 1, an appropriate buffer was used according to the molecular weight and concentration of the polymer used, and the reaction was carried out so that the gelation time (the time it takes for the two liquids to lose fluidity after mixing) was about 10 minutes. *Possible combinations of reactive terminals include amine and maleimide, thiol and maleimide, and succinimide and amine.
[0096] For example, the gel sheet of Example 1 was manufactured as follows: Amine-terminated LinearPEG (0.8 g) with a molecular weight of 20 kJ was dissolved in a pH 3.64 buffer (0.720 mL). Succinimide-terminated TetraPEG (0.4 g) with a molecular weight of 20 kJ was dissolved in a pH 3.64 buffer (1.080 mL). At this time, the PEG content was 40 wt% of the total. After mixing the two liquids, the mixture was placed in a Teflon (registered trademark) mold and allowed to stand for approximately one day to produce a 1 mm-thick gel sheet. The resulting gel was punched into a dumbbell shape (JIS K 6251 No. 3) to prepare a tensile test specimen. Gel sheets of Examples 2-3 and Comparative Examples 1-7 were also manufactured in the same manner, and tensile test specimens were prepared from each gel sheet.
[0097]
[0098] 2. Preparation of 4-branched ionic gels. The gel sheet (Linear 20k + Tetra 20k) of the hydrogel prepared in Example 1 was immersed in pure water for one day, changing the water several times, to replace the buffer with pure water. The sheet was dried at 100°C under reduced pressure to remove moisture. An ionic liquid (1-ethyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide, [C2mim][NTf2]) was added to the dehydrated sheet to a solid weight fraction of 40 wt%, and the sheet was left at 100°C under reduced pressure for one day. Absorption of all the ionic liquid into the sheet was confirmed visually and by weight measurement, and the final polymer fraction was confirmed to be 40 wt%. The prepared gel was punched into a dumbbell shape (JIS K 6251 No. 3) to prepare a tensile test specimen.
[0099] We also conducted an experiment to directly prepare an ion gel without going through a four-arm hydrogel. TetraPEG, which has a maleimide reactive end, and either TetraPEG or linear LinearPEG, which has an amine reactive end, were used to prepare a gel in a mixed solvent of N,N-dimethylformamide (DMF) and an ionic liquid (1-ethyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide, [C2mim][NTf2]). The DMF was then removed by heating and reducing the pressure to obtain the ion gel.
[0100] Similarly, ion gels were obtained using the following ionic liquids: lithium bis(trifluoromethanesulfonyl)imide (Li[NTf2]), an equimolar mixture of lithium bis(trifluoromethanesulfonyl)imide and triglyme ([Li(G3)][NTf2]), and an equimolar mixture of lithium bis(trifluoromethanesulfonyl)imide and tetraglyme ([Li(G4)][NTf2]).
[0101]
[0102] These ionic liquids are known as solvated ionic liquids, as described in the following literature: Watanabe M et al. (2018). "From Ionic Liquids to Solvate Ionic Liquids: Challenges and Opportunities for Next Generation Battery Electrolytes". Bull. Chem. Soc. Jpn. 91 (11): 1660-1682. For example, the following examples are used: Amine-terminated LinearPEG (0.8 g) with a molecular weight of 20 kJ was added to [C2mim][NTf2] (1.2 g) and DMF (2.1 mL), and the mixture was heated to 60°C to dissolve. Maleimide-terminated TetraPEG (0.2 g) with a molecular weight of 10 kJ was added to [C2mim][NTf2] (0.3 g) and DMF (0.530 mL), and the mixture was heated to 60°C to dissolve. After mixing the two liquids, the mixture was placed in a Teflon (registered trademark) mold and left to stand at 60°C for approximately one day to create a gel sheet with a thickness of 1 mm. The resulting gel sheet was then subjected to reduced pressure at 100°C for one day to remove the DMF, yielding the desired ion gel sheet. At this point, the PEG content was 40 wt% of the total. The resulting gel was punched into a dumbbell shape (JIS K 6251 No. 3) to prepare a tensile test specimen. The same procedure was followed even when the types of the two polymers used were different from those used in this example.
[0103] 3. Evaluation of gel sheets [Measurement / tensile test] Measurements were performed using a precision universal testing machine (Shimadzu Corporation, model number: AG-10kNXPlus). Clamp-type grippers were used. The test specimen was held by tightening a pair of grippers with screws, and the upper gripper was moved vertically upward to uniaxially stretch the test specimen. The extension rate was 0.125 / s, and a stress-strain curve was obtained up to breakage. For hydrogels, measurements were performed in a container filled with liquid paraffin oil that encased the entire jig to prevent water evaporation. For ion gels, measurements were performed in air.
[0104] [Measurement / Wide-Angle Scattering Experiment] Structural changes during uniaxial extension tests were analyzed using wide-angle X-ray scattering (WAXS). When X-rays are irradiated onto a sample, they are scattered by electrons within the sample. The scattered X-rays then interfere with each other, resulting in a scattering pattern consisting of bright and dark areas. The scattering pattern reflects the contrast in electron density within the sample and has a Fourier transform relationship with the electron density distribution in real space. Therefore, if a peak is observed in the scattering pattern, it indicates the presence of a repeating structure with a length corresponding to that scattering angle. WAXS targets small structures of approximately 1-10 Å. Therefore, in this study, a Bragg peak corresponding to PEG crystals was observed.
[0105] Measurements were primarily performed using a NANOPIX (Rigaku, Tokyo, Japan). The wavelength was 1.5 Å, and the camera length was 80 mm. The exposure time for measurements was 5 minutes. The samples used were the same dumbbell-shaped as those used in the uniaxial extension tests. The samples were deformed at a strain rate of approximately 0.125 / sec, and when the desired degree of extension was reached, the deformation was stopped. X-rays were irradiated while the deformation was stopped, and a scattering image was obtained. This was repeated by increasing the degree of extension by 100% in increments until the sample broke. For hydrogels, measurements were performed in a container filled with liquid paraffin oil, enclosing the entire jig, to prevent evaporation of water. For ion gels, measurements were performed in air.
[0106] [Experimental Results of 4-Branched Hydrogels] The strain-induced crystallization behavior of the gel sheets of Examples 1-3 and Comparative Examples 1-7, which are 4-branched hydrogels, is summarized in Table 2. Figure 2(A) shows the stress-strain ratio curves when the polymer concentration was kept constant at 40 wt% and the molecular weight between crosslinks was changed from 5,000 to 30,000. In Tetra10k+Tetra10k (Comparative Example 7) with a molecular weight between crosslinks of 5,000, no stretch-induced crystallization was observed (Fig. 2(B)). However, in Tetra20k+Tetra20k (Example 3) with a molecular weight between crosslinks of 10,000 (Fig. 2(C)), and in Linear 20k+Tetra 20k (molecular weight between crosslinks of 30,000) (Example 1) in which a linear chain was incorporated into the network in addition to the 4-branched macromer, stretch-induced crystallization was observed (Fig. 2(D)). In Linear 20k+Tetra 20k and Tetra20k+Tetra20k in which stretch-induced crystallization occurred, the breaking stress was 1. MPa, indicating that toughening due to elongation-induced crystallization was occurring (FIG. 2(A)). In addition, elongation-induced crystallization was observed in the gel sheets of Examples 2 and 3, but not in the gel sheets of Comparative Examples 1-6.
[0107] The wide-angle X-ray scattering (WAXS) images of the gel sheets shown in Figures 2(C) and 2(D), in which stretch-induced crystallization was observed, show scattering profiles in the direction perpendicular to the stretching direction, as shown in Figures 3 and 4. The results indicated that extended-chain crystals of PEG chains were observed in the gel sheet (Example 3) made using a polymer of Tetra20k+Tetra20k (molecular weight between crosslinks: 10,000, PEG concentration: 40 wt%), while helical-chain crystals of PEG chains were observed in the gel sheet (Example 1) made using a polymer of Linear 20k+Tetra20k (molecular weight between crosslinks: 30,000, PEG concentration: 40 wt%) (indicated by arrows in Figures 3 and 4, respectively).
[0108] Figure 5(A) shows the stress-strain curves for gel sheets made from Linear20k and Tetra20k, which are 4-branched hydrogels with a molecular weight between crosslinks of 30,000. At PEG concentrations of 20 wt% or less (Comparative Examples 1 and 2), no strain-induced crystallization was observed (Figures 5(B) and 5(C)). However, as mentioned above, strain-induced crystallization was observed at a PEG concentration of 40 wt% (Example 1) (Figure 5(D)).
[0109]
[0110] [Experimental Results of 4-Branched Ion Gel] As shown in Figure 6(A), a gel sheet of the 4-branched hydrogel (Linear 20k + Tetra 20k, molecular weight between crosslinks: 30,000, PEG concentration: 40 wt%) prepared in Example 1 was dried and then re-swollen in an ionic liquid (Figure 6(B)). Tensile specimens of the 4-branched ion gel (PEG concentration: 40 wt%) prepared as described in "2. Preparation of 4-branched Gel" were also observed to undergo strain-induced crystallization. The formation of PEG helical chain crystals was confirmed at a strain ratio of λ = 8 (Figure 6(C), indicated by the arrow).
[0111] As shown in Figure 7, strain-induced crystallization was also observed in tensile specimens of four-branched ion gels prepared directly from the ionic liquids [C2mim][NTf2], Li[NTf2], [Li(G3)][NTf2], and [Li(G4)][NTf2] without the four-branched hydrogel.
[0112] In the four-branched ion gel prepared with [C2mim][NTf2], the formation of PEG crystals and helical crystals was confirmed at an elongation ratio of λ = 9. In the four-branched ion gel prepared with Li[NTf2], the formation of PEG extended crystals and helical crystals was confirmed at an elongation ratio of λ = 14. In the four-branched ion gels reswollen with [Li(G3)][NTf2] and [Li(G4)][NTf2], the formation of PEG extended crystals was confirmed at an elongation ratio of λ = 14.
Claims
1. A gel composition comprising a polymer network formed by crosslinking a first polymer, which is a 4-branched or linear polymer having electrophilic functional groups and a polyethylene glycol backbone, and a second polymer, which is a 4-branched or linear polymer having nucleophilic functional groups and a polyethylene glycol backbone, wherein one or both of the first polymer and the second polymer are 4-branched polymers; and a solvent; the total amount of the first polymer and the second polymer relative to the amount of the gel composition is 30% by weight or more; and the molecular weight between crosslinking points of the polymer network is 10,000 or more.
2. The gel composition of claim 1, wherein the electrophilic functional group of the first polymer is an active ester group, a maleimidyl group, a carboxyl group, an N-hydroxy-succinimidyl group, a sulfosuccinimidyl group, a phthalimidyl group, or a nitrophenyl group.
3. The gel composition of claim 1, wherein the nucleophilic functional group of the second polymer is an amino group, a thiol group, or -CO2PhNO2 (wherein Ph is an o-, m-, or p-phenylene group).
4. The gel composition of claim 1, wherein the solvent comprises at least one selected from the group consisting of water, an organic solvent, and an ionic liquid.
5. The gel composition according to claim 1, in which crystals of the polyethylene glycol skeleton are formed by uniaxial stretching.
6. The gel composition according to claim 1, wherein a gel sheet made of the gel composition according to claim 1, which is punched into a dumbbell shape having a thickness of 1 mm according to JIS K 6251 No. 3, is deformed by uniaxial stretching at an elongation rate of 12.5% / sec, and the breaking stress measured is 1 MPa or more.
7. The first polymer is a compound represented by the following formula (I) or a compound represented by formula (II): (In formula (I), n1 to n4 may be the same or different, and n1 to n4 are integers from 5 to 300; A is a maleimidyl group, an N-hydroxy-succinimidyl group, a sulfosuccinimidyl group, a phthalimidyl group, an imidazoyl group, an acryloyl group, or a nitrophenyl group; R 1 ~R 4 may be the same or different, and each represents an alkylene group having 1 to 7 carbon atoms, an alkenylene group having 2 to 7 carbon atoms, -NH-R 5 -, -CO-R 5 -, -R 6 -OR 7 -, -R 6 -NH-R 7 -, -R 6 -COO-R 7 -, -R 6 -COO-NH-R 7 -, -R 6 -CO-R 7 -, -R 6 -NH-CO-R 7 - or -R 6 -CO-NH-R 7 - where R 5 represents an alkylene group having 1 to 7 carbon atoms, R 6 represents an alkylene group having 1 to 3 carbon atoms, R 7 represents an alkylene group having 1 to 5 carbon atoms.) (In formula (II), n 12 is an integer from 1 to 10000; B is a maleimidyl group, an N-hydroxy-succinimidyl group, a sulfosuccinimidyl group, a phthalimidyl group, an imidazoyl group, an acryloyl group, or a nitrophenyl group; R 11 represents an alkylene group having 1 to 7 carbon atoms, an alkenylene group having 2 to 7 carbon atoms, -NH-R 13 -, -CO-R 13 -, -R 14 -OR 15 -, -R 14 -NH-R 15 -, -R 14 -COO-R 15 -, -R 14 -COO-NH-R 15 -, -R 14 -CO-R 15 -, R 14 -NH-CO-R 15 -or-R 14 -CO-NH-R 15 - where R 13 represents an alkylene group having 1 to 7 carbon atoms, R 14 represents an alkylene group having 1 to 3 carbon atoms, R 15 represents an alkylene group having 1 to 5 carbon atoms; R 12 represents an alkylene group having 1 to 7 carbon atoms, an alkenylene group having 2 to 7 carbon atoms, -NH-R 16 -, -CO-R 16 -, -R 17 -OR 18 -, -R 17 -NH-R 18 -, -R 17 -COO-R 18 -, -R 17 -COO-NH-R 18 -, -R 17 -CO-R 18 -, R 17 -NH-CO-R 18 -or-R 17 -CO-NH-R 18 - where R 16 represents an alkylene group having 1 to 7 carbon atoms, R 17 represents an alkylene group having 1 to 3 carbon atoms, R 18 represents an alkylene group having 1 to 5 carbon atoms.) The gel composition according to claim 1, wherein the second polymer is a compound represented by the following formula (III) or a compound represented by the following formula (IV). (In formula (III), n 21 ~n 24 may be the same or different, n 21 ~n 24 is an integer from 25 to 250, D is a thiol group, an amino group, or -COOPhNO2 (Ph represents an o-, m-, or p-phenylene group), R 21 ~R 24 may be the same or different, and each represents an alkylene group having 1 to 7 carbon atoms, an alkenylene group having 2 to 7 carbon atoms, -NH-R 25 -, -CO-R 25 -, -R 26 -OR 27 -, -R 26 -NH-R 27 -, -R 26 -COO-R 27 -, -R 26 -COO-NH-R 27 -, -R 26 -CO-R 27 -, R 26 -NH-CO-R 27 -or-R 26 -CO-NH-R 27 - where R 25 represents an alkylene group having 1 to 7 carbon atoms, R 26 represents an alkylene group having 1 to 3 carbon atoms, R 27 represents an alkylene group having 1 to 5 carbon atoms.) (In formula (IV), n 32 is an integer from 1 to 10000, E is a thiol group, an amino group, or -COOPhNO2 (Ph represents an o-, m-, or p-phenylene group), R 31 represents an alkylene group having 1 to 7 carbon atoms, an alkenylene group having 2 to 7 carbon atoms, -NH-R 33 -, -CO-R 33 -, -R 34 -OR 35 -, -R 34 -NH-R 35 -, -R 34 -COO-R 35 -, -R 34 -COO-NH-R 35 -, -R 34 -CO-R 35 -, R 34 -NH-CO-R 35 -or-R 34 -CO-NH-R 35 - where R 33 represents an alkylene group having 1 to 7 carbon atoms, R 34 represents an alkylene group having 1 to 3 carbon atoms, R 35 represents an alkylene group having 1 to 5 carbon atoms; R 32 represents an alkylene group having 1 to 7 carbon atoms, an alkenylene group having 2 to 7 carbon atoms, -NH-R 36 -, -CO-R 36 -, -R 37 -OR 38 -, -R 37 -NH-R 38 -, -R 37 -COO-R 38 -, -R 37 -COO-NH-R 38 -, -R 37 -CO-R 38 -, R 37 -NH-CO-R 38 -or-R 37 -CO-NH-R 38 - where R 36 represents an alkylene group having 1 to 7 carbon atoms, R 37 represents an alkylene group having 1 to 3 carbon atoms, R 38 represents an alkylene group having 1 to 5 carbon atoms.) 8. A gel sheet, which is a sheet formed from the gel composition according to any one of claims 1 to 7.
Citation Information
Patent Citations
Crosslinked polymer composition and method of use
JP2000502380A
Gel fiber and nonwoven fabric thereof
JP2015137430A
Novel low-swellling-degree hydrogel containing temperature -responsive polymer
WO2014157186A1
Hemostatic polymer material kit
WO2021225144A1