Binder package

The packaging system for binder compositions, featuring a container with a liquid feeding adapter and particulate polymers, addresses the issue of quality deterioration and contamination, enhancing the performance and reliability of secondary batteries by maintaining the integrity of the binder composition during storage.

WO2024203512A1PCT designated stage expired Publication Date: 2024-10-03ZEON CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/010451
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-18
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

The quality of binder compositions for secondary batteries, such as lithium ion batteries, deteriorates during storage, leading to poor coating and decreased battery performance due to contamination and aggregation of particles, which existing packaging methods fail to adequately prevent.

Method used

A specialized packaging system for binder compositions that includes a container with a liquid feeding adapter and pipe, a stopper, and a connector, which maintains a high contact angle with the binder composition to minimize adhesion to the container walls, and incorporates a particulate polymer with a core-shell structure and an anti-drying agent to reduce particle aggregation and contamination.

Benefits of technology

The packaging system effectively suppresses the deterioration of the binder composition during storage, preventing particle aggregation and contamination, thereby ensuring better battery performance and reducing defects in the final battery product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024010451_03102024_PF_FP_ABST
    Figure JP2024010451_03102024_PF_FP_ABST
Patent Text Reader

Abstract

This binder package comprises: a container; and a binder composition for secondary batteries which is accommodated in an internal space of the container. The container comprises an accommodation part, a liquid feed adapter, a liquid feed pipe, and a plug. The liquid feed adapter is provided to be engaged with an opening of the accommodation part. The liquid feed pipe has a top-side terminal engaged with the liquid feed adapter. The liquid feed adapter and the liquid feed pipe constitute a liquid guiding path which connects an opening of the bottom-side terminal of the liquid feed pipe and the top side of the container. The plug is provided to be attachably / detachably engaged with the liquid feed adapter and to seal the liquid guiding path. The contact angle θB between the binder composition and the inner wall surface of the container is 30° or more.
Need to check novelty before this filing date? Find Prior Art

Description

Binder packaging

[0001] The present invention relates to a package for a binder for a secondary battery, and more particularly to a package in which a binder for a secondary battery is packaged in a state suitable for storage and use.

[0002] Binders are used as materials for manufacturing batteries such as lithium-ion secondary batteries. Binders can be used in the electrodes (positive or negative electrodes) of batteries as materials for bonding active material particles that constitute the electrodes and as materials for bonding layered structures such as electrodes and separators together.

[0003] In many cases, the binder is prepared as a binder composition in a liquid state such as a slurry, which contains a fine particulate polymer that functions as a binder and a dispersion medium. The prepared binder composition may be used immediately after preparation, but in many cases, it is packaged in a container and stored until use.

[0004] Because the binder is a substance that constitutes the internal structure of a battery, its quality can significantly affect the battery's performance. In particular, in the case of secondary batteries such as lithium-ion secondary batteries, improved performance is required for smooth charging and discharging, and therefore high-quality binders are also required. Therefore, the packaging of the binder composition is required to be able to store the binder composition without damaging its quality. Various packaging materials for binder compositions have been proposed (e.g., Patent Documents 1 to 3).

[0005] Patent Document 1: JP 2011-098736 A, International Publication No. 2022 / 071523 (corresponding publication: US Patent Application Publication No. 2023 / 331976), International Publication No. 2015 / 029835

[0006] Compared to preparing a binder composition for a secondary battery and using it immediately when needed, if a binder composition for a secondary battery is prepared, stored, and then used to manufacture a battery, problems such as poor coating of the binder composition, decreased battery performance, etc. The occurrence of such problems is thought to be due to deterioration in the quality of the binder composition due to storage, but conventional binder composition packaging has not been able to sufficiently suppress such deterioration in quality.

[0007] Therefore, an object of the present invention is to provide a package of a binder composition that can suppress deterioration of the quality of the binder composition due to storage, that allows the binder composition to be easily taken out when used, and that can effectively suppress the occurrence of defects in the resulting battery.

[0008] The present inventors conducted extensive research to solve the above-mentioned problems. During the research, the inventors discovered that deterioration of the quality of binder compositions is largely due to the incorporation of coarse particles from the environment when the binder composition is transferred from a container to a coating device, and the formation of aggregates due to evaporation of the dispersion medium and contact of the binder composition with the inner wall of the container while the binder composition is stored in the container. The inventors further discovered that the formation of granular components such as coarse particles and aggregates due to these causes can be effectively suppressed by using a specific packaging material for the binder composition, and thus completed the present invention. Specifically, the present invention provides the following:

[0009] (1) A binder package including a container and a binder composition for a secondary battery contained in an internal space of the container, wherein the container includes a storage section, a liquid feed adapter, a liquid feed tube, and a stopper, wherein the container has an opening at its top, the liquid feed adapter is provided to engage with the opening of the container, the bottom end of the liquid feed tube is close to the bottom of the internal space of the container and the top end is engaged with the liquid feed adapter, the liquid feed adapter and the liquid feed tube form a liquid-conducting path that connects the opening at the bottom end of the liquid feed tube with the top side of the container, and the stopper is provided to detachably engage with the liquid feed adapter to seal the liquid-conducting path, and a contact angle θ between the binder composition and an inner wall surface of the container B (2) The binder package according to (1), wherein the liquid supply adapter has an engaging portion connectable to a connector that delivers the binder composition to the outside of the container. (3) The binder package according to (1) or (2), wherein the binder composition contains a particulate polymer having a glass transition temperature of 40°C or higher and 200°C or lower. (4) The binder package according to (1) or (2), wherein the binder composition contains a particulate polymer having a core-shell structure with a core portion and a shell portion covering the outer surface of the core portion, and wherein the glass transition temperature of the shell portion is 40°C or higher and 200°C or lower. (5) The binder package according to (4), wherein the binder composition further contains an auxiliary particulate polymer that is a non-core-shell particulate polymer, and wherein the content of the auxiliary particulate polymer in 100% by mass of the binder composition is 5% by mass or lower. (6) The binder package according to (1) or (2), wherein the binder composition contains a particulate polymer, and the particulate polymer consists solely of a particulate polymer having a core-shell structure including a core portion and a shell portion covering the outer surface of the core portion. (7) The binder composition contains a particulate polymer, an anti-drying agent, and water, and the contact angle θ between the inner wall surface of the container and water is W(8) The binder package according to any one of (1) to (7), wherein the binder composition contained in the binder package, after being stored for 6 months in an environment of 5°C to 40°C, has a concentration of granular components having a sphere volume equivalent diameter of 5 μm or more of 1000 ppm or less.

[0010] According to the present invention, there is provided a package of a binder composition that can suppress deterioration of the quality of the binder composition due to storage, that allows the binder composition to be easily taken out when in use, and that can effectively suppress the occurrence of defects in the resulting battery.

[0011] Fig. 1 is a longitudinal cross-sectional view schematically showing an example of the binder package of the present invention and a container which is a component thereof. Fig. 2 is a partial longitudinal cross-sectional view schematically showing an example of a state in which a liquid supply adapter and a connector are connected to deliver the binder composition from the binder package of the present invention.

[0012] The present invention will be described in detail below with reference to embodiments and examples. However, the present invention is not limited to the embodiments and examples shown below, and can be modified and implemented as desired without departing from the scope of the claims of the present invention and their equivalents. The components of the embodiments shown below can be combined as appropriate. In addition, in the drawings, the same components are designated by the same reference numerals, and their description may be omitted.

[0013] In the following description, a "long" substrate refers to a substrate having a length that is 5 times or more, preferably 10 times or more, the width, and specifically refers to a substrate having a length that can be wound into a roll for storage or transportation. There is no particular upper limit to the length of the substrate, and it can be, for example, 100,000 times or less the width.

[0014] (Binder Package: Shape of Container) The binder package of the present invention includes a container and a binder composition for a secondary battery housed in the internal space of the container.

[0015] Fig. 1 is a longitudinal cross-sectional view schematically illustrating an example of a binder package according to the present invention and a container as a component thereof. In Fig. 1, the container 100 includes a storage section 110, a liquid supply adapter 120, a liquid supply tube 130, and a stopper 140. The storage section 110 has an opening 111 at its top.

[0016] The liquid supply adapter 120 is provided so as to engage with the opening 111 of the storage section 110. In this example, the liquid supply adapter 120 and the storage section 110 are engaged with each other by screwing together at a threaded section 191 where a male thread near the opening 111 of the storage section 110 engages with a female thread on a corresponding portion of the liquid supply adapter 120.

[0017] In the present application, the engagement of the components constituting the container may be a sealed engagement that can block the inflow and outflow of fluid at the engagement portion. For example, the engagement between the storage portion 110 and the liquid feed adapter 120, the engagement between the liquid feed adapter 120 and the liquid feed tube 130, the detachable engagement between the liquid feed adapter 120 and the stopper 140, and the engagement between the liquid feed adapter 120 and a connector (described later) may be a sealed engagement that can block the inflow and outflow of fluid at the engagement portion. Engagements that are not limited to detachable engagements may be detachable engagements or non-detachable engagements. Furthermore, the engagement of multiple components may be a mechanical engagement such as screwing, or may be integrated by gluing multiple components together.

[0018] The liquid supply adapter 120 has a through-hole 121. The through-hole 121 is a hole that communicates from a bottom-side opening 121L to a top-side opening 121H. The bottom-side opening 121L is an opening that opens toward the container internal space 101, and the top-side opening 121H is an opening that opens toward the outside of the container.

[0019] The liquid supply tube 130 is a hollow tube with openings on both ends. One end of the liquid supply tube 130, the bottom end 131L, is close to the bottom of the internal space 101 of the container 100. The other end of the liquid supply tube 130, the top end 131H, engages with the bottom opening 121L of the liquid supply adapter. As a result, the liquid supply adapter 120 and the liquid supply tube 130 form a liquid-conducting path that connects the opening of the bottom end 131L of the liquid supply tube with the outside of the container.

[0020] The liquid supply adapter 120 further has an air supply hole 129 in addition to the through-hole 121. The air supply hole 129 is a hole that communicates from a bottom opening 129L to a top opening 129H.

[0021] The liquid supply adapter 120 further has, near its top side, a connector engaging portion 123 including a recess 122. The connector engaging portion 123 functions when engaging the liquid supply adapter 120 with a connector (described below).

[0022] The stopper 140 is provided so as to be detachably engaged with the fluid supply adapter 120. In this example, the stopper 140 and the fluid supply adapter 120 are detachably engaged with each other by threading them together at a threaded portion 192 where a male thread near the top of the fluid supply adapter 120 engages with a female thread at a corresponding portion of the stopper 140. Through this engagement, the stopper 140 seals the fluid guide path at its opening on the top side (top opening 121H of the fluid supply adapter 120 in this example). Furthermore, through this engagement, the stopper 140 also seals top opening 129H of the air supply hole 129.

[0023] 1 has such a structure, the internal space 101 can be made airtight. Therefore, a liquid binder composition for a secondary battery can be stored inside the container 100, thereby forming the binder package of the present invention.

[0024] When the binder composition is to be discharged from the binder package of the present invention for use, the plug is removed from the liquid supply adapter, and the connector is connected to the liquid supply adapter.

[0025] FIG. 2 is a partial vertical cross-sectional view schematically illustrating an example of a state in which a liquid-feeding adapter and a connector are connected to deliver the binder composition from the binder package of the present invention. FIG. 2 illustrates a state in which a stopper 140 is removed from the liquid-feeding adapter 120 of a container 100 of the binder package, and then a connector 150 is connected to the liquid-feeding adapter 120. The connector 150 has a connecting portion 153 shaped to fit into the recess 122 of the connector mating member 123 of the liquid-feeding adapter 120. Therefore, simply plugging the connector 150 onto the liquid-feeding adapter 120 allows for easy connection. In this example, the connector 150 has an opening 151L located at a position corresponding to the top opening 121H of the through-hole 121, allowing it to receive the binder composition flowing out of the container 100's liquid-inlet path and deliver it to a device for using the binder composition. In this example, the binder composition can be delivered by suctioning it using a pump upstream of the connector 150.

[0026] In this way, the container includes a liquid supply adapter that engages with the opening of the container portion, and further includes a liquid supply tube that engages with the liquid supply adapter, the bottom end of which is adjacent to the bottom of the container's interior space and the top end of which engages with the liquid supply adapter. This allows the binder composition, including any remaining at the bottom of the container, to be easily dispensed from the container during use. Furthermore, connection to the connector for this dispensing can be easily achieved by opening only the small top opening of the liquid supply adapter and immediately closing it with the connector, without opening the container portion. This makes it possible to easily and significantly reduce the contamination of coarse particles from the environment when dispensing the binder composition from the container to the coating device. Therefore, the adoption of this mechanism provides advantageous effects in terms of both ease of binder composition removal and suppression of deterioration of the binder composition, compared to conventional mechanisms that require opening the container opening and inserting a liquid supply tube into the opening from the outside to dispense the binder composition.

[0027] In addition, the connector 150 has an opening 159L that is opened at a position corresponding to the top opening 129H of the air supply hole 129. This makes it possible to introduce gas into the container 100 from the opening 159L of the connector 150. The gas introduced into the container 100 from the opening 159L can be a gas with a low concentration of coarse particles derived from the environment. For example, gas obtained by filtering outside air or gas with a low concentration of coarse particles that has been stored in a tank in advance can be used. Such gas with a reduced concentration of coarse particles contains no coarse particles at all or has a coarse particle count of 3,000 particles / m3 captured by a mesh filter with a mesh size of 5 μm. 3 It can be the following gases:

[0028] (Contact Angle) In the binder package of the present invention, the contact angle θ between the binder composition and the inner wall surface of the container B is a large value equal to or greater than a specific value. B is 30° or more, preferably 60° or more. B The upper limit is not particularly limited, and can be less than 180°.

[0029] According to the inventors' findings, the specific value of the contact angle θ B By having this, deterioration of the quality of the binder composition during storage of the binder package can be significantly suppressed. Without being bound by a particular theory, it is believed that such an effect is due to the suppression of aggregation of the dispersed matter in the binder composition on the inner wall surface of the container. In other words, during storage of the binder package, the binder composition is stored in the internal space of the container at a position lower than a certain level of the liquid surface. Due to a decrease in the shaking of the container, etc., a portion of such binder composition may adhere to the inner wall surface of the container at a position higher than the liquid surface. Contact angle θ B If the contact angle θ is small, the binder composition adhering to the inner wall surface of the container will remain adhering for a long time, and the dispersion medium will partially volatilize, which may increase the concentration of the dispersed matter (microparticulate polymer, etc.) in the binder composition. In this case, aggregation of the dispersed matter in the binder composition will easily occur, resulting in the generation of aggregated particles. BIt is considered that the aggregation of such dispersions is suppressed and the generation of aggregate particles is suppressed by the contact angle θ being a specific high value. In addition, it is considered that the binder composition interacts with the inner wall surface of the container at a position lower than the liquid level of the stored binder composition, which may cause the dispersion to become unstable and aggregation of the dispersion to occur. B It is believed that when ρ is a specific high value, such destabilization is suppressed and the generation of coarse molecules due to aggregation is suppressed.

[0030] Explaining again with reference to the example of FIG. 1 , in the container 100, the binder composition is stored in contact with the inner wall surface 102 of the storage portion 100, and therefore the contact angle between the inner wall surface 102 of the storage portion 100 and the binder composition is set to a large value equal to or greater than a specific value. Such a contact angle can be obtained by appropriately selecting a material for the storage portion 100 that provides such a contact angle in relation to the binder composition. Specifically, when a binder composition using water as the main dispersion medium is used, preferred examples of materials constituting the storage portion 100 include high-density polyethylene (HDPE), polyethylene, polypropylene, polyethylene terephthalate, polyamide, polyester, polyvinyl alcohol, and the like.

[0031] Contact angle θ B The contact angle θ can also be changed by appropriately adjusting the components and their ratios of the binder composition. For example, by appropriately adjusting the ratio of components such as a dispersant contained in the binder composition, B can be adjusted.

[0032] In the binder package of the present invention, the contact angle θ between water and the inner wall surface of the container W It is preferable that the contact angle θ is a large value equal to or greater than a specific value. W is preferably 80° or more, and more preferably 100° or more. W There is no particular upper limit to the contact angle θ and it can be less than 180°. As the binder composition, various types of so-called aqueous binder compositions (i.e., binder compositions containing water as a dispersion medium) are known.W By having the above, it is possible to obtain a binder package that can satisfactorily obtain the effects of the present invention using a common container for any of various aqueous binder compositions.

[0033] (Binder Composition) The binder composition packaged as a component of the binder package of the present invention will be described below. The binder composition is used as a material for manufacturing secondary batteries such as lithium-ion secondary batteries. The binder composition may contain a particulate polymer and a dispersion medium. From the viewpoints of ease of handling and reducing environmental impact, the dispersion medium preferably contains water. Furthermore, from the viewpoint of reducing the generation of aggregate particles, the binder composition preferably contains a drying inhibitor.

[0034] In a preferred example, the binder composition includes a particulate polymer, an anti-drying agent, and water, and has a contact angle θ W The angle between the binder composition and the binder is preferably 80° or more. By adopting such a configuration, the binder composition can be made easier to handle, the environmental impact of using the binder composition can be reduced, the generation of aggregate particles can be reduced, and the performance of a battery obtained using the binder composition can be improved.

[0035] In a preferred example, the binder composition can be a coating liquid for coating by an inkjet method. In the case of a coating liquid for inkjet printing, problems such as nozzle clogging due to granular components such as coarse particles and aggregate particles contained in the coating liquid can be problematic. However, the binder composition stored in the binder package of the present invention can reduce such problems, which is particularly preferred.

[0036] In the present application, the granular components in the binder composition may be defined as granular components having a sphere volume equivalent diameter of 5 μm or more. The concentration of such granular components in the binder composition may be measured by filtering the binder composition through a nylon mesh filter with a mesh size of 5 μm and weighing the collected material on the filter. Such granular components include particles resulting from aggregation of the dispersed particles in the binder composition and foreign matter introduced from the external environment during handling of the binder composition. Therefore, in the present application, granular components having a sphere volume equivalent diameter of 5 μm or more may be simply referred to as "granular components," and particulate polymers and the like contained as components of the binder composition are not included in the category of "granular components."

[0037] (Binder composition: particulate polymer) The particulate polymer can function in a battery electrode (positive electrode or negative electrode) as a material for adhering active material particles constituting the electrode and as a material for adhering layer structures such as an electrode, a separator, etc. The binder composition may contain only one type of particulate polymer, or may contain two or more types of particulate polymers.

[0038] The content of the particulate polymer in the binder composition is preferably 1% by mass or more, more preferably 3% by mass or more, and preferably 15% by mass or less, based on the total amount of the binder composition. If the content of the particulate polymer is equal to or greater than the lower limit, the adhesion between electrode members of a secondary battery can be improved. On the other hand, if the content of the particulate polymer is equal to or less than the upper limit, the inkjet ejection characteristics can be improved.

[0039] The particulate polymer preferably contains a polymer having a glass transition temperature of 40°C or higher. When the particulate polymer contains a polymer having a glass transition temperature of 40°C or higher, inkjet ejection characteristics can be improved. Furthermore, when the glass transition temperature of the particulate polymer is higher than a certain level, the generation of aggregates inside the container can be suppressed, thereby further enhancing the effects obtained when the contact angle θB is within a specific range. It is preferable that at least a portion of the surface of the particulate polymer is composed of the polymer. Here, the glass transition temperature of the polymer is preferably 50°C or higher, more preferably 80°C or higher, and preferably 200°C or lower, and more preferably 120°C or lower. When the glass transition temperature of the polymer is above the lower limit, inkjet ejection characteristics can be further improved. On the other hand, when the glass transition temperature of the polymer is below the upper limit, the particulate polymer becomes appropriately soft, allowing the formation of an adhesive layer that more firmly bonds battery components together, even when pressurized at room temperature. The glass transition temperature of the polymer can be adjusted, for example, by changing the type and ratio of monomers used in preparing the polymer.

[0040] The volume average particle diameter of the particulate polymer is preferably 100 nm or more, more preferably 200 nm or more, even more preferably 400 nm or more, even more preferably 500 nm or more, and preferably 1500 nm or less, more preferably 900 nm or less, even more preferably 800 nm or less, and even more preferably 700 nm or less. When the volume average particle diameter of the particulate polymer is within the above range, aggregation of the particulate polymer can be effectively suppressed, thereby improving the performance of a secondary battery obtained by using the binder composition. Additionally, when the volume average particle diameter of the particulate polymer is equal to or greater than the above lower limit, deterioration of battery characteristics due to an increase in the resistance of the secondary battery caused by obstruction of the path of the electrode or separator can be suppressed. On the other hand, when the volume average particle diameter of the particulate polymer is equal to or less than the above upper limit, nozzle clogging can be further suppressed when the binder composition is applied by an inkjet method, thereby improving inkjet ejection characteristics. In this specification, the term "volume average particle size" refers to the particle size at which the cumulative volume calculated from the smallest diameter side becomes 50% in a volume-based particle size distribution measured by a laser diffraction method, and can be measured using the measurement method described in the examples of this specification.

[0041] The particulate polymer may be a particle made of a single polymer, or may be a particle made of a composite of multiple polymers (a particle formed by physical or chemical bonding of two or more polymers). Among these, from the viewpoint of being able to exhibit multiple properties, the particulate polymer is preferably a particle made of a composite of multiple polymers, and more preferably a particle having a core-shell structure comprising a core and a shell covering at least a portion of the outer surface of the core; a particle having a side-by-side structure in which two or more polymers are juxtaposed; a particle having a structure in which a portion of the central polymer is exposed to the outer shell; or a particle having a structure in which another type of polymer particle is embedded and integrated into the surface of a spherical polymer particle, and even more preferably a particle having a core-shell structure. By employing a particulate polymer having a core-shell structure, both high adhesive performance and dispersion stability can be achieved, which is particularly preferred. Hereinafter, a particulate polymer having a core-shell structure will be described as an example.

[0042] (Particulate polymer having a core-shell structure) The particulate polymer having a core-shell structure has a core portion and a shell portion covering the outer surface of the core portion. By using the particulate polymer having a core-shell structure, it is possible to improve inkjet ejection characteristics.

[0043] Here, the shell portion may cover the entire outer surface of the core portion or may cover only a portion of the outer surface of the core portion. Even if the outer surface of the core portion appears to be completely covered by the shell portion, the shell portion is considered to be a shell portion that partially covers the outer surface of the core portion as long as it has holes that communicate between the inside and outside of the shell portion.

[0044] The particulate polymer may have any constituent element other than the core and shell portions described above, as long as the intended effect is not significantly impaired. Specifically, for example, the particulate polymer may have a portion formed of a polymer different from the core portion inside the core portion. As a specific example, seed particles used when producing the particulate polymer by seed polymerization may remain inside the core portion. However, from the viewpoint of significantly exhibiting the intended effect, it is preferable that the particulate polymer has only the core portion and the shell portion.

[0045] (Core Portion) The glass transition temperature of the polymer of the core portion of the particulate polymer is preferably −50°C or higher, more preferably −45°C or higher, preferably 60°C or lower, more preferably 35°C or lower, even more preferably 0°C or lower, and even more preferably −15°C or lower. When the glass transition temperature of the polymer of the core portion is above the lower limit, inkjet ejection characteristics can be improved. On the other hand, when the glass transition temperature of the polymer of the core portion is below the upper limit, the polymer of the core portion can exhibit good adhesive properties, and an adhesive layer that more firmly bonds battery components together can be formed even when pressurized at room temperature. Furthermore, when the glass transition temperature of the polymer of the core portion is below the upper limit, detachment of components contained in the adhesive layer (so-called powder fall) can be sufficiently suppressed. The glass transition temperature of the polymer of the core portion can be adjusted, for example, by changing the type and ratio of monomers used to prepare the polymer of the core portion.

[0046] Examples of monomers used to prepare the core polymer include vinyl chloride monomers such as vinyl chloride and vinylidene chloride; vinyl acetate monomers such as vinyl acetate; aromatic vinyl monomers such as styrene, α-methylstyrene, styrene sulfonic acid, butoxystyrene, and vinylnaphthalene; vinylamine monomers such as vinylamine; vinylamide monomers such as N-vinylformamide and N-vinylacetamide; methyl acrylate, ethyl acrylate, butyl acrylate, 2-ethylhexyl acrylate, and methyl methacrylate. Examples of suitable (meth)acrylic acid ester monomers include fluorine-free (meth)acrylic acid ester monomers such as ethyl methacrylate, butyl methacrylate, and cyclohexyl methacrylate; (meth)acrylamide monomers such as acrylamide and methacrylamide; (meth)acrylonitrile monomers such as acrylonitrile and methacrylonitrile; fluorine-containing (meth)acrylic acid ester monomers such as 2-(perfluorohexyl)ethyl methacrylate and 2-(perfluorobutyl)ethyl acrylate; maleimide; and maleimide derivatives such as phenylmaleimide. These may be used alone or in combination of two or more types in any ratio. In the present invention, (meth)acrylic refers to acrylic and / or methacrylic, and (meth)acrylonitrile refers to acrylonitrile and / or methacrylonitrile.

[0047] Among these monomers, the monomer used to prepare the core polymer is preferably at least a (meth)acrylic acid ester monomer, from the viewpoint of further firmly bonding the battery components together via the adhesive layer. A combination of a (meth)acrylic acid ester monomer and an aromatic vinyl monomer, or a combination of a (meth)acrylic acid ester monomer and a (meth)acrylonitrile monomer, is more preferred. That is, the core polymer preferably contains at least a (meth)acrylic acid ester monomer unit, and more preferably contains a (meth)acrylic acid ester monomer unit and an aromatic vinyl monomer unit or a (meth)acrylonitrile monomer unit. In the present invention, "containing a monomer unit" means that "the polymer obtained using the monomer contains a repeating unit derived from the monomer." Furthermore, in the present invention, "(meth)acrylic acid ester monomer" refers to a monofunctional (meth)acrylic acid ester monomer having only one polymerization reactive group.

[0048] From the viewpoint of further firmly bonding the battery components together via the adhesive layer, the proportion of the (meth)acrylic acid ester monomer units in the core polymer is preferably 5% by mass or more, more preferably 10% by mass or more, and particularly preferably 20% by mass or more, with the total repeating units (total monomer units) in the particulate polymer being 100% by mass, and is preferably 98% by mass or less, and more preferably 96% by mass or less.

[0049] When the core polymer contains a (meth)acrylic acid ester monomer unit and an aromatic vinyl monomer unit, from the viewpoint of further firmly bonding the battery components together via the adhesive layer, the proportion of the (meth)acrylic acid ester monomer unit in the core polymer is preferably 5% by mass or more, more preferably 10% by mass or more, and particularly preferably 20% by mass or more, and is preferably 80% by mass or less, more preferably 75% by mass or less, and even more preferably 70% by mass or less, based on 100% by mass of all repeating units (total monomer units) in the particulate polymer. Furthermore, the proportion of the aromatic vinyl monomer unit in the core polymer is preferably 15% by mass or more, more preferably 20% by mass or more, and particularly preferably 25% by mass or more, and is preferably 90% by mass or less, more preferably 80% by mass or less, and particularly preferably 70% by mass or less, based on 100% by mass of all repeating units (total monomer units) in the particulate polymer.

[0050] When the core polymer contains (meth)acrylic acid ester monomer units and (meth)acrylonitrile monomer units, from the viewpoint of further firmly bonding the battery components together via the adhesive layer, the proportion of the (meth)acrylic acid ester monomer units in the core polymer is preferably 70% by mass or more, more preferably 80% by mass or more, particularly preferably 85% by mass or more, and preferably 98% by mass or less, and more preferably 96% by mass or less, with the total repeating units (total monomer units) in the particulate polymer being 100% by mass. Furthermore, the proportion of the (meth)acrylonitrile monomer units in the core polymer is preferably 1% by mass or more, more preferably 1.5% by mass or more, preferably 10% by mass or less, and more preferably 5% by mass or less, with the total repeating units (total monomer units) in the particulate polymer being 100% by mass.

[0051] The core polymer may contain an acid group-containing monomer unit. Examples of the acid group-containing monomer include a monomer having an acid group, such as a monomer having a carboxylic acid group, a monomer having a sulfonic acid group, or a monomer having a phosphoric acid group.

[0052] Examples of monomers having a carboxylic acid group include monocarboxylic acids and dicarboxylic acids. Examples of monocarboxylic acids include acrylic acid, methacrylic acid, and crotonic acid. Examples of dicarboxylic acids include maleic acid, fumaric acid, and itaconic acid. Examples of monomers having a sulfonic acid group include vinyl sulfonic acid, methyl vinyl sulfonic acid, (meth)allyl sulfonic acid, (meth)acrylic acid-2-ethyl sulfonate, 2-acrylamido-2-methylpropanesulfonic acid, and 3-allyloxy-2-hydroxypropanesulfonic acid. Examples of monomers having a phosphate group include 2-(meth)acryloyloxyethyl phosphate, methyl-2-(meth)acryloyloxyethyl phosphate, and ethyl-(meth)acryloyloxyethyl phosphate. In the present invention, (meth)allyl means allyl and / or methallyl, and (meth)acryloyl means acryloyl and / or methacryloyl. Among these, as the acid group-containing monomer, a monomer having a carboxylic acid group is preferred, among which a monocarboxylic acid is preferred, and (meth)acrylic acid is more preferred. Furthermore, the acid group-containing monomer may be used alone or in combination of two or more kinds in any ratio.

[0053] The proportion of the acid group-containing units in the core polymer is preferably 0.1% by mass or more, more preferably 1% by mass or more, and preferably 15% by mass or less, and more preferably 10% by mass or less, based on 100% by mass of all repeating units (total monomer units) in the particulate polymer. By keeping the proportion of the acid group-containing units within the above range, the dispersibility of the core polymer can be improved during preparation of the particulate polymer, and it can be made easier to form a shell portion that partially covers the outer surface of the core polymer.

[0054] The core polymer preferably contains a crosslinkable monomer unit in addition to the above-mentioned monomer units. The crosslinkable monomer is a monomer that can form a crosslinked structure during or after polymerization by heating or irradiation with energy rays.

[0055] Examples of crosslinkable monomers include polyfunctional monomers having two or more polymerization reactive groups. Examples of such polyfunctional monomers include divinyl monomers such as divinylbenzene, 1,3-butadiene, isoprene, and allyl methacrylate; di(meth)acrylic acid ester monomers such as ethylene dimethacrylate, diethylene glycol dimethacrylate, ethylene glycol dimethacrylate, diethylene glycol diacrylate, and 1,3-butylene glycol diacrylate; tri(meth)acrylic acid ester monomers such as trimethylolpropane trimethacrylate and trimethylolpropane triacrylate; ethylenically unsaturated monomers containing epoxy groups such as allyl glycidyl ether and glycidyl methacrylate; γ-methacryloxypropyltrimethoxysilane, N-methylolacrylamide, and the like. Among these, di(meth)acrylic acid ester monomers are more preferred. These may be used alone or in combination of two or more in any ratio.

[0056] The proportion of the crosslinkable monomer units in the core polymer is preferably 0.05% by mass or more, more preferably 0.1% by mass or more, and is preferably 10% by mass or less, more preferably 5% by mass or less, and particularly preferably 3% by mass or less, based on 100% by mass of all repeating units (total monomer units) in the particulate polymer. By keeping the proportion of the crosslinkable monomer units within the above range, the battery components can be more firmly bonded to each other via the adhesive layer.

[0057] (Shell Portion) The glass transition temperature of the polymer of the shell portion of the particulate polymer is preferably 40°C or higher, more preferably 50°C or higher, even more preferably 80°C or higher, and preferably 200°C or lower, more preferably 120°C or lower. If the glass transition temperature of the polymer of the shell portion is above the above lower limit, the generation of aggregates can be suppressed and the inkjet ejection characteristics can be further improved. On the other hand, if the glass transition temperature of the polymer of the shell portion is below the above upper limit, the particulate polymer becomes appropriately soft, and an adhesive layer that more firmly bonds battery components together can be formed even when pressurized at room temperature. The glass transition temperature of the polymer of the shell portion can be adjusted, for example, by changing the type and ratio of monomers used to prepare the polymer of the shell portion.

[0058] The glass transition temperature of the polymer in the shell portion is preferably at least 25°C higher than the glass transition temperature of the polymer in the core portion described above, from the viewpoint of maintaining the shape of the particulate polymer after bonding the battery components together and suppressing an increase in resistance.

[0059] Examples of the monomers used to prepare the shell polymer include the same monomers as those exemplified as the monomers that can be used to produce the core polymer. These monomers may be used alone or in combination of two or more types in any ratio.

[0060] Among these monomers, from the viewpoint of more firmly bonding the battery components together via the adhesive layer, it is more preferable to use at least one of a (meth)acrylic acid ester monomer, an aromatic vinyl monomer, a (meth)acrylonitrile monomer unit, and an acid group-containing monomer as the monomer used to prepare the shell polymer. That is, it is preferable that the shell polymer contains at least one of a (meth)acrylic acid ester monomer unit, an aromatic vinyl monomer unit, a (meth)acrylonitrile monomer unit, and an acid group-containing monomer unit.

[0061] From the viewpoint of bonding the battery components together more firmly via the adhesive layer, the proportion of the (meth)acrylic acid ester monomer units in the polymer of the shell portion is preferably 1% by mass or more, more preferably 1.5% by mass or more, and is preferably 10% by mass or less, and more preferably 6% by mass or less, with the total repeating units (total monomer units) in the particulate polymer being 100% by mass.

[0062] From the viewpoint of bonding battery components together more firmly via the adhesive layer, the proportion of aromatic vinyl monomer units in the polymer of the shell portion is preferably 2% by mass or more, more preferably 3% by mass or more, and is preferably 10% by mass or less, and more preferably 5% by mass or less, where the total repeating units (total monomer units) in the particulate polymer is 100% by mass.

[0063] The proportion of (meth)acrylonitrile monomer units in the polymer of the shell portion is preferably 0.1% by mass or more, more preferably 0.2% by mass or more, and is preferably 2% by mass or less, more preferably 1% by mass or less, and even more preferably 0.5% by mass or less, based on 100% by mass of all repeating units (total monomer units) in the particulate polymer.

[0064] The proportion of the acid group-containing monomer in the polymer of the shell portion is preferably 0.01% by mass or more, more preferably 0.03% by mass or more, and is preferably 1% by mass or less, more preferably 0.5% by mass or less, and even more preferably 0.2% by mass or less, based on 100% by mass of all repeating units (total monomer units) in the particulate polymer.

[0065] (Mass Proportion of Shell Portion to the Total of Core Portion and Shell Portion) The mass proportion of the shell portion to the total of the core portion and shell portion of the particulate polymer is preferably 2 mass% or more, preferably 20 mass% or less, more preferably 15 mass% or less, even more preferably 10 mass% or less, and particularly preferably 5 mass% or less. When the mass proportion of the shell portion is equal to or greater than the lower limit, inkjet ejection characteristics can be further improved. On the other hand, when the mass proportion of the shell portion is equal to or less than the upper limit, an adhesive layer that more firmly bonds battery components together can be formed even when pressurized at room temperature. Here, the mass proportion of the shell portion to the total of the core portion and shell portion is calculated from the ratio of the thickness of the core portion to the shell portion and the specific gravity of the particulate polymer, which will be described later.

[0066] (Method for preparing particulate polymer having core-shell structure) The particulate polymer can be prepared, for example, by using the monomer of the polymer of core part and the monomer of the polymer of shell part, and polymerizing them stepwise while changing the ratio of these monomers over time.Specifically, the particulate polymer can be prepared by a continuous multi-stage emulsion polymerization method and a multi-stage suspension polymerization method, in which the polymer of the previous stage is successively coated with the polymer of the subsequent stage.

[0067] (Particulate polymers other than particulate polymers having a core-shell structure: auxiliary particulate polymers) The binder composition of the present invention may contain other particulate polymers in addition to or instead of the particulate polymers having a core-shell structure described above. For example, by containing other particulate polymers in addition to the particulate polymers having a core-shell structure, it is possible to prevent components contained in the layer formed by the binder composition from falling off from the layer in a secondary battery. This effect is particularly advantageous when an adhesive layer is formed in a secondary battery using the binder composition. Hereinafter, such non-core-shell particulate polymers used auxiliary in addition to the particulate polymers having a core-shell structure will be referred to as "auxiliary particulate polymers" for ease of distinction.

[0068] The auxiliary particulate polymer may be particles obtained by granulating only one type of polymer, or particles obtained by granulating a mixture of multiple types of polymers. The glass transition temperature of the auxiliary particulate polymer is preferably 25° C. or lower, more preferably 10° C. or lower, and even more preferably 0° C. or lower. If the glass transition temperature of the polymer is 25° C. or lower, it is possible to sufficiently suppress the components contained in the adhesive layer from falling off, and it is also possible to improve the adhesion between the battery components of the secondary battery.

[0069] Examples of monomers used to prepare the auxiliary particulate polymer include the same monomers as those exemplified as monomers that can be used to produce the core polymer of the particulate polymer described above. For example, monomers that can be used to prepare the polymer as the auxiliary particulate polymer include (meth)acrylic acid ester monomers, (meth)acrylonitrile monomers, aromatic vinyl monomer units, acid group-containing monomers, (meth)acrylamide monomers, and crosslinkable monomers. Furthermore, as monomers used to prepare the polymer as the auxiliary particulate polymer, for example, (meth)acrylic acid ester monomers having a polar group such as 2-hydroxyethyl (meth)acrylate and 2-hydroxypropyl (meth)acrylate can also be used. Note that the above-mentioned monomers may be used alone, or two or more may be used in combination at any ratio.

[0070] In one embodiment, the monomer used to prepare the polymer as auxiliary particulate polymer can be a combination of (meth)acrylic acid ester monomer, (meth)acrylonitrile monomer, acid group-containing monomer, (meth)acrylamide monomer and crosslinking monomer, or can be a combination of aromatic vinyl monomer, acid group-containing monomer, (meth)acrylic acid ester monomer having polar group and crosslinking monomer.That is, the polymer as auxiliary particulate polymer can comprise (meth)acrylic acid ester monomer unit, (meth)acrylonitrile monomer unit, acid group-containing monomer unit, (meth)acrylamide monomer unit and crosslinking monomer unit, or can comprise aromatic vinyl monomer unit, acid group-containing monomer unit, (meth)acrylic acid ester monomer unit having polar group and crosslinking monomer unit.

[0071] The proportion of the (meth)acrylic acid ester monomer units in the polymer as the auxiliary particulate polymer is not particularly limited, but may be, for example, 40% by mass or more, 50% by mass or more, or 60% by mass or more, and may be, for example, 90% by mass or less, or 85% by mass or less, where the total repeating units (total monomer units) contained in the polymer is 100% by mass.

[0072] The proportion of (meth)acrylonitrile monomer units in the polymer as the auxiliary particulate polymer is not particularly limited, but may be, for example, 1% by mass or more, or 5% by mass or more, or 10% by mass or more, or, for example, 20% by mass or less, or 15% by mass or less, where the total repeating units (total monomer units) contained in the polymer is 100% by mass.

[0073] The proportion of the acid group-containing monomer units in the polymer as the auxiliary particulate polymer is not particularly limited, but may be, for example, 0.5% by mass or more, or 1% by mass or more, or 2% by mass or more, or, for example, 10% by mass or less, or 7% by mass or less, or 5% by mass or less, where the total repeating units (total monomer units) contained in the polymer is 100% by mass.

[0074] The proportion of (meth)acrylamide monomer units in the polymer as the auxiliary particulate polymer is not particularly limited, but may be, for example, 0.1% by mass or more, or 0.5% by mass or more, or 1% by mass or more, or, for example, 5% by mass or less, or 4% by mass or less, or 2% by mass or less, where the total repeating units (total monomer units) contained in the polymer is 100% by mass.

[0075] The proportion of aromatic vinyl monomer units in the polymer as the auxiliary particulate polymer is not particularly limited, but may be, for example, 20% by mass or more, 40% by mass or more, or 55% by mass or more, for example, 80% by mass or less, 70% by mass or less, or 65% by mass or less, where the total repeating units (total monomer units) contained in the polymer is 100% by mass.

[0076] The (meth)acrylic acid ester monomer unit having a polar group in the polymer as the auxiliary particulate polymer is not particularly limited, but may be, for example, 0.1 mass % or more and 0.5 mass % or less, for example, 3 mass % or less, or 1.5 mass % or less, where all repeating units (total monomer units) contained in the polymer are taken as 100 mass %.

[0077] The proportion of crosslinkable monomer units in the polymer as the auxiliary particulate polymer is not particularly limited, but may be, for example, 1% by mass or more, or 2% by mass or more, or 3% by mass or more, or, for example, 50% by mass or less, or 40% by mass or less, or 35% by mass or less, where the total repeating units (total monomer units) contained in the polymer is 100% by mass.

[0078] When the polymer used as the auxiliary particulate polymer contains a crosslinkable monomer unit (meth) and an acrylonitrile monomer unit, the proportion of the crosslinkable monomer unit in the polymer is not particularly limited, but may be, for example, 1% by mass or more, 2% by mass or more, 3% by mass or more, for example, 6% by mass or less, 5% by mass or less, or 4% by mass or less, based on the total repeating units (total monomer units) contained in the polymer being 100% by mass. When the polymer used as the auxiliary particulate polymer contains a crosslinkable monomer unit (meth) and an aromatic vinyl monomer unit, the proportion of the crosslinkable monomer unit in the polymer is not particularly limited, but may be, for example, 10% by mass or more, 20% by mass or more, 30% by mass or more, for example, 50% by mass or less, 40% by mass or less, or 35% by mass or less, based on the total repeating units (total monomer units) contained in the polymer being 100% by mass.

[0079] The volume average particle diameter of the auxiliary particulate polymer is preferably 50 nm or more, more preferably 100 nm or more, and even more preferably 200 nm or more, and is preferably 600 nm or less, more preferably 500 nm or less, and even more preferably 400 nm or less. When the volume average particle diameter of the auxiliary particulate polymer is within the above-mentioned range, the battery components can be more firmly bonded to each other via the adhesive material.

[0080] The blending amount of the auxiliary particulate polymer is not particularly limited, and is preferably 1 part by mass or more, more preferably 5 parts by mass or more, and preferably 20 parts by mass or less, and more preferably 15 parts by mass or less, per 100 parts by mass of the particulate polymer having a core-shell structure. When the blending amount of the auxiliary particulate polymer is within the above range, the components contained in the adhesive layer can be sufficiently prevented from falling off, and the cycle characteristics of the secondary battery can be improved.

[0081] The amount of the auxiliary particulate polymer in the binder composition is not particularly limited, but from the viewpoint of suppressing the occurrence of aggregation, a relatively small amount is preferable. Specifically, the amount of the auxiliary particulate polymer in 100% by mass of the binder composition is preferably 5% by mass or less. When the binder composition contains an auxiliary particulate polymer, the lower limit of the amount can be, for example, 0.2% by mass or more. The binder composition does not need to contain an auxiliary particulate polymer. If the binder composition does not contain an auxiliary particulate polymer, the occurrence of aggregates is effectively suppressed. Furthermore, an increase in internal resistance in the resulting secondary battery can be suppressed, further improving the cycle characteristics.

[0082] The polymer as the auxiliary particulate polymer is not particularly limited, and for example, can be prepared by polymerizing a monomer composition containing the above-mentioned monomer in an aqueous solvent such as water.Here, the ratio of each monomer in the monomer composition is usually the same as the ratio of each monomer unit in the polymer.The polymerization method and polymerization reaction are not particularly limited, and known polymerization methods and polymerization reactions can be used.

[0083] (Dispersion Medium) The binder composition preferably contains water as a dispersion medium, and may further contain a dispersion medium other than water. Examples of dispersion medium other than water include organic solvents such as cyclic aliphatic hydrocarbons such as cyclopentane and cyclohexane, aromatic hydrocarbons such as toluene and xylene, ketones such as ethyl methyl ketone and cyclohexanone, esters such as ethyl acetate, butyl acetate, γ-butyrolactone and ε-caprolactone, nitriles such as acetonitrile and propionitrile, ethers such as tetrahydrofuran, and alcohols such as methanol, ethanol and isopropanol.

[0084] (Anti-drying agent) When the binder composition contains an anti-drying agent, drying of the binder composition can be suppressed during storage of the binder composition in the binder package, and the generation of aggregate particles can be further suppressed.

[0085] A low-molecular-weight polyhydric alcohol compound can be used as the drying inhibitor. A low-molecular-weight polyhydric alcohol compound is a compound having a molecular weight of less than 150 and having two or more hydroxyl groups (—OH) in one molecule. When the binder composition contains a low-molecular-weight polyhydric alcohol compound, it is possible to inhibit the binder composition from drying during storage, and also to improve the ejection characteristics when the binder composition is ejected from an inkjet head.

[0086] Examples of low-molecular-weight polyhydric alcohol compounds include propylene glycol, ethylene glycol, glycerin, 1,3-propanediol, and 1,4-butanediol. Among these, glycerin is preferred. These compounds may be used alone or in combination of two or more in any ratio.

[0087] The content of the low-molecular-weight polyhydric alcohol compound per 100 parts by mass of the particulate polymer is preferably 20 parts by mass or more, more preferably 40 parts by mass or more, even more preferably 50 parts by mass or more, even more preferably 55 parts by mass or more, and is preferably 400 parts by mass or less, more preferably 300 parts by mass or less, even more preferably 250 parts by mass or less, and even more preferably 200 parts by mass or less. When the content of the low-molecular-weight polyhydric alcohol compound is equal to or greater than the lower limit, the generation of aggregate particles can be reduced and the inkjet ejection characteristics can be further improved. On the other hand, when the content of the low-molecular-weight polyhydric alcohol compound is equal to or less than the upper limit, an excessive increase in viscosity of the binder composition can be suppressed, and as a result, the inkjet ejection characteristics can be further improved.

[0088] The content of the low-molecular-weight polyhydric alcohol compound per 100 parts by mass of water as a dispersion medium is preferably 1 part by mass or more, more preferably 2 parts by mass or more, and even more preferably 3 parts by mass or more, and is preferably 80 parts by mass or less, more preferably 50 parts by mass or less, and even more preferably 29 parts by mass or less. When the content of the low-molecular-weight polyhydric alcohol compound is equal to or greater than the lower limit, the generation of aggregate particles can be reduced and the inkjet ejection characteristics can be further improved. On the other hand, when the content of the low-molecular-weight polyhydric alcohol compound is equal to or less than the upper limit, an excessive increase in viscosity of the binder composition can be suppressed, and as a result, the inkjet ejection characteristics can be further improved.

[0089] (Other Components of Binder Composition) The binder composition may contain any components in addition to the components described above. For example, it may contain a dispersant (water-soluble polymer) and a dispersion stabilizer to suppress aggregation. Examples of dispersants include ammonium acrylate polymers (for example, Aron (registered trademark) A-6114, manufactured by Toagosei Co., Ltd.).

[0090] (Properties of the Binder Composition) Before filling the binder composition into a container to prepare the binder package of the present invention, it is preferable to filter out granular components such as coarse particles and aggregate particles to reduce their concentration. Specifically, the concentration of granular components can be preferably 1000 ppm or less, more preferably 800 ppm or less, and even more preferably 500 ppm or less.

[0091] Furthermore, by adopting the above-described configuration, the binder package of the present invention can maintain a low concentration of granular components in the binder composition even after long-term storage. Specifically, the concentration of granular components in the binder composition contained in the binder package stored for 6 months in an environment of 5° C. or higher and 40° C. or lower can be preferably 1000 ppm or lower, more preferably 800 ppm or lower, and even more preferably 500 ppm or lower.

[0092] From the viewpoint of ease of handling, the surface tension of the binder composition is preferably 20 to 60 mN / m.

[0093] (Modifications) The binder package of the present invention is not limited to the above-described examples and may be modified from the above-described examples. For example, while FIG. 1 illustrates a container 100 having a generally round storage section 110, the shape of the storage section is not limited to this and may be rectangular. In the examples of FIGS. 1 and 2, the binder composition is drawn from upstream of the connector 150 by a pump, while the binder composition is discharged by introducing gas from the connector opening 159L into the top opening 129H of the liquid supply adapter 120. However, the discharge operation is not limited to this. For example, instead of the air supply hole 129 communicating with the opening of the connector 150, the container 100 may have a hole communicating with the external environment of the container via a filter, and outside air may be introduced through this hole. Alternatively, the binder composition may be discharged by applying pressure to the storage section 110 from the outside, deforming it to create a positive pressure in the container's internal space 101, thereby pressure-feeding the binder composition. Furthermore, in the examples of Figures 1 and 2, the through hole 121 in the liquid delivery adapter 120 was a hole of a simple shape, but the shape of the through hole is not limited to this and may be equipped with, for example, a pressure reducing valve for facilitating suction by a pump.

[0094] The present invention will be described in detail below with reference to examples. However, the present invention is not limited to the following examples and can be implemented with any modifications within the scope of the claims of the present invention and their equivalents. In the following description, "%" and "parts" representing amounts are by weight unless otherwise specified. Furthermore, the operations described below were carried out under conditions of room temperature and normal pressure unless otherwise specified.

[0095] [Evaluation Method] (Glass Transition Temperature) A measurement sample was prepared by drying an aqueous dispersion of the particulate polymer at a temperature of 130°C for 1 hour. 10 mg of the measurement sample was weighed into an aluminum pan, and measurement was carried out using a differential scanning calorimetry measuring device ("EXSTAR DSC6220" manufactured by SII NanoTechnology Inc.) at a temperature range of -100°C to 200°C at a heating rate of 10°C / min under the conditions specified in JIS Z8703 to obtain a differential scanning calorimetry (DSC) curve. An empty aluminum pan was used as a reference during the measurement. During this heating process, the glass transition temperature (°C) was determined as the intersection point between the baseline immediately before the appearance of the endothermic peak of the DSC curve at which the differential signal (DDSC) was 0.05 mW / min / mg or more and the tangent to the DSC curve at the first inflection point that appeared after the endothermic peak.

[0096] (Volume average particle diameter) The volume average particle diameter of the particulate polymer was measured by a laser diffraction method. Specifically, water was added to the prepared aqueous dispersion solution containing the particulate polymer to adjust the solid content concentration to 0.1 mass % to prepare a sample, and the particle size distribution (volume basis) was determined using a laser diffraction particle size distribution analyzer (manufactured by Beckman Coulter, Inc., product name "LS-13 320"). In the particle size distribution, the particle diameter at which the cumulative volume calculated from the smallest diameter side becomes 50% was determined, and this was taken as the volume average particle diameter D50 (nm).

[0097] (Contact Angle) The same storage section 110 as used in each of the Examples and Comparative Examples was prepared and cut open to form a flat sample. The surface corresponding to the inner wall surface 102 was placed facing upward, and water and the binder composition used in each of the Examples and Comparative Examples were dropped onto the surface to form a droplet. Using a contact angle meter (manufactured by Kyowa Interface Science Co., Ltd., product name "DMs-400"), an image of the droplet taken from the horizontal direction was analyzed based on the tangent method to determine the contact angle.

[0098] (Concentration of granular components) A washed nylon mesh filter with 5 μm openings was weighed. 1 kg of the binder composition to be measured was filtered through the mesh filter, and the collected material was washed with ion-exchanged water and then dried at 80° C. for 3 hours. After drying was completed, the mesh filter with the collected material placed thereon was weighed. The difference between the corrected and uncorrected weighed values ​​was calculated, and this value was used as the amount of granular components to calculate the concentration in the measurement target. The calculated concentration was evaluated according to the following criteria.

[0099] A: Less than 500 ppm. B: 500 ppm or more and less than 800 ppm. C: 800 ppm or more and less than 1000 ppm. D: 1000 ppm or more and less than 3000 ppm. E: 3000 ppm or more.

[0100] (Inkjet Discharge Characteristics) In each of the Examples and Comparative Examples, the binder composition was sucked up from a container and transferred to a coater, and then supplied to the nozzle head of a discharge test kit, where it was continuously discharged. The discharge test kit and nozzle head used were a discharge test kit (IJK-200S, manufactured by Microjet Co., Ltd.) equipped with a high-performance glass nozzle head (IJHD-100, manufactured by Microjet Co., Ltd.). The discharge conditions were a droplet volume of 100 pL and a discharge frequency of 500 kHz. The discharge characteristics were evaluated according to the following criteria.

[0101] A: Continuous ejection was not impossible for a period of less than 12 hours after the start of continuous ejection. B: Continuous ejection became impossible for a period of 9 hours or more but less than 12 hours after the start of continuous ejection. C: Continuous ejection became impossible for a period of 6 hours or more but less than 9 hours after the start of continuous ejection. D: Continuous ejection became impossible for a period of 3 hours or more but less than 6 hours after the start of continuous ejection. E: Continuous ejection became impossible for a period of less than 3 hours after the start of continuous ejection.

[0102] (Dry Adhesion Strength) Under the same conditions as in each Example and Comparative Example, a binder composition was applied to one surface of the pressed negative electrode blank, and a separator was then placed on top of the binder composition. The binder composition was then pressed for 10 seconds at a temperature of 25°C and a pressure of 1 MPa. This resulted in a laminate comprising the negative electrode blank, a binder composition layer, and a separator. The laminate was cut out to obtain numerous elongated rectangular test pieces measuring 500 mm x 200 mm. Cellophane tape was fixed to a horizontal test table with the adhesive side facing up. The test piece was then attached to the cellophane tape with the negative electrode side facing down. The cellophane tape used was specified in JIS Z1522. One end of the separator in the longitudinal direction was pulled vertically upward at a pulling rate of 50 mm / min to peel it off, and the stress during peeling was measured. This measurement was performed a total of six times, and the average stress was calculated. This average was used as the peel strength. The peel strength was evaluated according to the following criteria. The higher the peel strength, the higher the dry adhesion between the electrode and the separator due to the dried product of the coating liquid.

[0103] A: Peel strength is 5.0 N / m or more. B: Peel strength is 4.0 N / m or more and less than 5.0 N / m. C: Peel strength is 3.0 N / m or more and less than 4.0 N / m. D: Peel strength is 1.0 N / m or more and less than 3.0 N / m. E: Peel strength is less than 1.0 N / m.

[0104] (Cycle Characteristics) The lithium ion secondary batteries fabricated in each of the Examples and Comparative Examples were charged to 4.3 V at a constant current and constant voltage (CC CV) in an atmosphere at 25°C. The charged batteries were discharged to 3.0 V at constant currents of 0.2 C and 1 C in an atmosphere at -10°C, and the electric capacity was determined. The discharge capacity retention rate, expressed as the ratio of the electric capacities (= (electric capacity at 1 C / electric capacity at 0.2 C) × 100 (%)), was then determined. These measurements were performed on five lithium ion secondary batteries, and the average of the determined discharge capacity retention rates was calculated as the output characteristics. Next, the lithium ion secondary batteries were clamped with a pressure jig to apply a surface pressure of 1 MPa, and then a cycle test was performed at 45°C. The cycle test conditions were 1 C CC+CV charge (4.3 V, 1 / 50 C cut) and 1 C CC discharge (3.0 V cut), and the charge / discharge cycle was repeated 500 times. Thereafter, the temperature was lowered to 25°C while the pressure jig was still fastened, and the output characteristics were measured in the same manner as above. The resistance retention rate (%) before and after the cycle (= (average discharge capacity retention rate after cycle test / average discharge capacity retention rate before cycle test) x 100) was calculated and evaluated according to the following criteria. The higher the resistance retention rate before and after the cycle, the smaller the increase in resistance in the cycle test, i.e., the more excellent the cycle characteristics. A: Resistance retention rate is 80% or more B: Resistance retention rate is 70% or more and less than 80% C: Resistance retention rate is 60% or more and less than 70% D: Resistance retention rate is 40% or more and less than 60% E: Resistance retention rate is less than 40%

[0105] (Production Example 1) 100 parts of ion-exchanged water and 0.1 parts of ammonium persulfate were fed into a reactor equipped with a stirrer, the gas phase was replaced with nitrogen gas, and the temperature was raised to 80°C. Meanwhile, in a separate container, 40 parts of ion-exchanged water, 0.2 parts of sodium dodecylbenzenesulfonate as an emulsifier, and a core monomer composition were mixed to obtain a core-forming mixture. The core monomer composition used was a composition consisting of 91.1 parts of n-butyl acrylate as a (meth)acrylic acid ester monomer, 1.9 parts of methacrylic acid as an acid group-containing monomer, 0.1 parts of ethylene glycol dimethacrylate as a crosslinkable monomer, and 1.9 parts of acrylonitrile as a (meth)acrylonitrile monomer. This core-forming mixture was continuously added to the reactor over 3 hours, and a polymerization reaction was carried out at a temperature of 80°C. The polymerization was continued until the polymerization conversion rate reached 95%, yielding an aqueous dispersion containing a particulate polymer that constitutes the core. Next, the monomer composition for the shell portion was continuously supplied to this aqueous dispersion over 60 minutes to continue polymerization. As the monomer composition for the shell portion, a composition consisting of 4.75 parts of styrene as an aromatic vinyl monomer and 0.25 parts of methacrylic acid as an acid group-containing monomer was used. When the polymerization conversion rate reached 98%, the reaction was stopped by cooling to prepare an aqueous dispersion containing particulate polymer 1. The volume average particle size and glass transition temperature of the obtained particulate polymer 1 were measured. By observing the cross-sectional structure of particulate polymer 1 using a transmission electron microscope (TEM), it was confirmed that particulate polymer 1 had a core-shell structure in which the shell portion partially covered the outer surface of the core portion.

[0106] (Production Example 2) Particulate polymer 2 was obtained by the same procedure as in Production Example 1, except for the following changes, and the volume average particle diameter and glass transition temperature were measured. - As the core monomer composition, a composition consisting of 3 parts of methacrylic acid, 48 parts of 2-ethylhexyl acrylate, 43.9 parts of styrene, and 0.1 parts of ethylene glycol dimethacrylate was used. - As the shell monomer composition, a composition consisting of 4.7 parts of styrene, 0.05 parts of methacrylic acid, and 0.25 parts of acrylonitrile was used. By observing the cross-sectional structure of the particulate polymer using a transmission electron microscope (TEM), it was confirmed that particulate polymer 2 had a core-shell structure in which the shell part partially covered the outer surface of the core part.

[0107] (Production Example 3) 90 parts of ion-exchanged water, 0.05 parts of sodium dodecylbenzenesulfonate (manufactured by Kao Chemical Corporation, "Neopelex G-15") as an emulsifier, and 0.23 parts of ammonium persulfate were each supplied to a reactor equipped with a stirrer, the gas phase was replaced with nitrogen gas, and the temperature was raised to 70 ° C. Meanwhile, in a separate vessel, 50 parts of ion-exchanged water, 0.1 parts of sodium dodecylbenzenesulfonate as an emulsifier, 2.3 parts of methacrylic acid as an acid group-containing monomer, 12.5 parts of acrylonitrile as a (meth)acrylonitrile monomer, 79.9 parts of n-butyl acrylate as a (meth)acrylic acid ester monomer, 3.8 parts of N-methylolacrylamide as a crosslinkable monomer, and 1.5 parts of acrylamide (AAm) as a (meth)acrylamide monomer were mixed to obtain a monomer composition. This monomer composition was continuously added to the reactor over 4 hours to carry out polymerization. During the addition, the reaction was carried out at 80° C. After the addition was completed, the mixture was further stirred at 80° C. for 3 hours to terminate the reaction, thereby preparing an aqueous dispersion containing particulate polymer 3 having no core-shell structure. The volume average particle size and glass transition temperature of the obtained particulate polymer 3 were measured.

[0108] An overview and evaluation results of Production Examples 1 to 3 are shown in Table 1. The meanings of the abbreviations in Table 1 are as follows: BA: butyl acrylate proportion (%) MAA: methacrylic acid proportion (%) AN: acrylonitrile proportion (%) 2EHA: 2-ethylhexyl acrylate proportion (%) St: styrene proportion (%) NMA: N-methylolacrylamide proportion (%) AAm: acrylamide proportion (%) EDMA: ethylene glycol dimethacrylate proportion (%) Shell proportion: mass proportion (%) of the shell proportion in the total of the core and shell parts

[0109]

[0110] (Example 1) (1-1. Binder Composition) 10 parts in solids equivalent of the aqueous dispersion of particulate polymer 1 obtained in Production Example 1, 1 part in solids equivalent of the aqueous dispersion of particulate polymer 3 obtained in Production Example 3, 10 parts of propylene glycol as a drying inhibitor, and 0.1 part in solids equivalent of an ammonium acrylate polymer (Aron (registered trademark) A-6114, manufactured by Toagosei Co., Ltd.) as a dispersant (water-soluble polymer), were mixed, and ion-exchanged water was further added to adjust the concentration to 11.1 mass% to obtain a mixture. The mixture was filtered through a mesh filter with an opening of 5 μm to obtain a binder composition.

[0111] The concentration of the particulate component in the resulting binder composition was measured and evaluated.

[0112] (1-2. Container) An inkjet coating machine (Konica, KM1024 (shear mode type)) equipped with a container having the structure shown schematically in FIG. 1 and a connector 150 having the structure shown schematically in FIG. 2 was prepared. The container 100 included a 10-liter HDPE (high-density polyethylene) storage section 110, a HDPE liquid supply adapter 120, a HDPE liquid supply tube 130, and a stopper 140. The liquid supply adapter 120 was threadedly engaged with the opening 111 of the storage section 110, and the liquid supply tube 130 was structured to engage with the hand-side opening 121L of the liquid supply adapter 120. The stopper 140 was detachably threadedly engaged near the top of the liquid supply adapter 120. These components formed an airtight internal space 101 within the container 100.

[0113] The contact angle θ of the inner wall surface 102 of the container 100 with water W , and the contact angle θ with the binder composition obtained in (1-1) B was measured.

[0114] (1-3. Binder Package) The stopper 140 was removed from the container 100 obtained in (1-2), and the container 100 was washed to clean the inside. 9 liters of the binder composition immediately after filtration obtained in (1-1) was filled into the internal space 101 of the container 100, and the stopper 140 was screwed back on to seal the container 100, thereby obtaining a binder package. The obtained binder package was stored indoors for 6 months. The room temperature during the storage period was in the range of 5 to 40°C. After the storage period, the stopper 140 was removed from the container 100, a portion of the binder composition was extracted, and the concentration of the granular component was measured and evaluated.

[0115] The connector 150 of the coating machine was connected to the liquid supply adapter 120 of the container 100, and the binder composition was sucked up from the container 100 by the liquid supply pump of the coating machine and sent to the coating machine. 3 The binder composition that reached the inside of the coating machine was extracted, and the concentration of the granular components was measured and evaluated.

[0116] (1-4. Preparation of Negative Electrode Raw Sheet) 33 parts of 1,3-butadiene, 3.5 parts of itaconic acid, 63.5 parts of styrene, 0.4 parts of sodium dodecylbenzenesulfonate as an emulsifier, 150 parts of ion-exchanged water, and 0.5 parts of potassium persulfate as a polymerization initiator were placed in a 5 MPa pressure vessel equipped with a stirrer, and after thorough stirring, the mixture was heated to 50 ° C. to initiate polymerization. When the polymerization conversion rate reached 96%, the mixture was cooled to stop the reaction, and a mixture containing a binder (SBR) for the negative electrode composite layer was obtained. A 5% aqueous sodium hydroxide solution was added to the mixture containing the binder for the negative electrode composite layer, and the pH was adjusted to 8. Unreacted monomers were removed by heated vacuum distillation. The mixture was then cooled to a temperature of 30 ° C. or below to obtain an aqueous dispersion containing the desired binder for the negative electrode composite layer. Next, 100 parts of artificial graphite (volume average particle diameter: 15.6 μm) as the negative electrode active material, 1 part of a 2% aqueous solution of carboxymethylcellulose sodium salt (manufactured by Nippon Paper Industries Co., Ltd., product name "MAC350HC") as a viscosity modifier, in terms of solid content, and ion-exchanged water were mixed to adjust the solid content concentration to 68%, and then further mixed at a temperature of 25 ° C. for 60 minutes. Furthermore, the solid content concentration was adjusted to 62% with ion-exchanged water, and then further mixed at a temperature of 25 ° C. for 15 minutes. To the resulting mixture, 1.5 parts of the aqueous dispersion containing the binder for the negative electrode composite layer and ion-exchanged water were added in terms of solid content, and the final solid content was adjusted to 52%, and then further mixed for 10 minutes. This was degassed under reduced pressure to obtain a nonaqueous secondary battery negative electrode slurry composition with good fluidity. The obtained nonaqueous secondary battery negative electrode slurry composition was applied to both sides of a 20 μm thick long copper foil current collector using a comma coater so that the dried film thickness was approximately 150 μm, and then dried. This drying was performed by conveying the copper foil at a speed of 0.5 m / min through an oven at a temperature of 60 ° C for 2 minutes. Then, the copper foil was heated at a temperature of 120 ° C for 2 minutes to obtain a pre-pressed negative electrode blank. This pre-pressed negative electrode blank was rolled using a roll press to obtain a pre-pressed negative electrode blank with a negative electrode composite layer thickness of 80 μm.

[0117] (1-5. Preparation of Positive Electrode Raw Sheet) LiCoO having a volume average particle diameter of 12 μm was used as the positive electrode active material. 2100 parts of the above, 2 parts of acetylene black (manufactured by Denka Co., Ltd., product name "HS-100") as a conductive material, 2 parts of polyvinylidene fluoride (manufactured by Kureha Corporation, product name "#7208") as a binder, equivalent to the solid content, and N-methylpyrrolidone as a solvent were mixed to a total solids concentration of 70%. These were mixed using a planetary mixer to obtain a slurry composition for a non-aqueous secondary battery positive electrode. The obtained slurry composition for a non-aqueous secondary battery positive electrode was applied to both sides of a 20 μm thick long aluminum foil current collector using a comma coater so that the film thickness after drying was approximately 150 μm, and then dried. This drying was performed by conveying the aluminum foil at a speed of 0.5 m / min in an oven at a temperature of 60 ° C. for 2 minutes. Thereafter, the aluminum foil was heat-treated at a temperature of 120 ° C. for 2 minutes to obtain a positive electrode blank. The obtained positive electrode blank was then rolled using a roll press to obtain a pressed positive electrode blank having a positive electrode composite layer. The pressed positive electrode blank was then cut into a rectangular shape.

[0118] (1-6. Separator Raw Material) A long separator raw material made of polyethylene (PE) (product name "ND412" manufactured by Asahi Kasei) was prepared.

[0119] (1-7. Laminate for non-aqueous secondary battery) While conveying the pressed negative electrode raw sheet obtained in (1-4) at a speed of 10 m / min, a binder composition was supplied onto one surface of the negative electrode raw sheet, and the separator raw sheet (1-6) was further stacked thereon as a first separator raw sheet and bonded with a pressure roller. The binder composition was supplied by discharging the binder composition drawn up from the container into the coater in (1-3) from the inkjet head of the coater. Subsequently, the binder composition was supplied onto the other surface of the negative electrode raw sheet in the same manner as above from another coater, and another separator raw sheet (1-6) was further stacked thereon as a second separator raw sheet and bonded with a pressure roller to obtain a laminate (a) having a layer structure of (first separator raw sheet) / (layer of binder composition) / (negative electrode raw sheet) / (layer of binder composition) / (second separator raw sheet). The binder composition was supplied from another coater to the surface of the first separator raw sheet side of the laminate (a) in the same manner as above, and a rectangular positive electrode raw sheet was further stacked on top of it and bonded with a pressure roller to obtain a laminate (b) having a layer structure of (rectangular positive electrode) / (layer of binder composition) / (first separator raw sheet) / (layer of binder composition) / (negative electrode raw sheet) / (layer of binder composition) / (second separator raw sheet). Next, the binder composition was supplied from another coater to the surface of the positive electrode side of the laminate (b) in the same manner as above, and the laminate (b) was cut. As a result, a rectangular laminate (c) having a layer structure of (layer of binder composition) / (rectangular positive electrode) / (layer of binder composition) / (first separator) / (layer of binder composition) / (negative electrode) / (layer of binder composition) / (second separator) was obtained. By appropriately adjusting the shape of the applied slurry composition and the cutting shape, portions of the current collectors of the positive and negative electrodes of the laminate (c) where no electrode mixture layer (positive electrode mixture layer or negative electrode mixture layer) was formed were provided, and tabs of the desired size were formed. The positive and negative electrode tabs were arranged to extend from the same side of the rectangular laminate (c). The lamination using the pressure roller described above was performed at a temperature of 25°C and a pressure of 2 MPa.Immediately after each bonding step, the binder composition layer was dried at a drying temperature of 70°C for 1 second using a heat roller as a transport roller for transporting the laminate along the transport path of the long laminate. Each binder composition was applied so that the binder composition formed a uniform dot pattern. The dot size was 100 μm in diameter, and the spacing between dots was 400 μm. The binder composition weight (dry weight per unit area) was 0.2 g / m. 2 It was.

[0120] (1-8. Secondary battery) Five stacks (c) prepared in (1-7) were stacked and pressed at a temperature of 25°C and a pressure of 2 MPa for 10 seconds to obtain a stack (d). The stack (d) was wrapped in an aluminum packaging exterior as an exterior, and an electrolyte solution (solvent: ethylene carbonate / diethyl carbonate / vinylene carbonate = 68.5 / 30 / 1.5 (volume ratio), electrolyte: LiPF with a concentration of 1M) was placed in the exterior. 6 The opening of the exterior was then closed by heat sealing at a temperature of 150°C, to prepare a stacked lithium ion secondary battery with a capacity of 800 mAh. The cycle characteristics of the obtained secondary battery were evaluated.

[0121] (Example 2) In the preparation of the binder composition of (1-1), the same operation as in Example 1 is carried out, except that the particulate polymer 2 obtained in Production Example 2 is used instead of the particulate polymer 1, and then the binder package is obtained and evaluated.

[0122] (Example 3) In the preparation of the binder composition of (1-1), the proportion of the particulate polymer 3 was changed from 10 parts to 5 parts, the proportion of the dispersant (water-soluble polymer) was changed from 0.1 parts to 0.05 parts, and the total concentration of the particulate polymers 1 and 3 was adjusted to 10.5%, and the same operation as in Example 1 was carried out, and a binder package was obtained and evaluated.

[0123] (Example 4) As the storage portion 110 of the container 100, instead of the HDPE one used in Example 1, a polyethylene terephthalate one of the same shape was used, and the same operation as in Example 1 was performed, and a binder package was obtained and evaluated.

[0124] (Example 5) In the preparation of the binder composition (1-1), the same operation as in Example 1 was carried out, except that the mixture obtained by mixing the components was used as the binder composition without filtration, and a binder package was obtained and evaluated.

[0125] (Example 6) In the preparation of the binder composition of (1-1), the aqueous dispersion of particulate polymer 3 is not added, and the concentration is adjusted so that the solid content concentration is 10.1 mass %, so that the same operation as in Example 1 is carried out, and then the binder package is obtained and evaluated.

[0126] Comparative Example 1 A binder package was obtained and evaluated by performing the same operations as in Example 1, except for the following changes: In preparing the binder composition (1-1), the proportion of the dispersant (water-soluble polymer) was changed from 0.1 parts to 0.5 parts. As the storage portion 110 of the container 100, instead of the HDPE one used in Example 1, a polyethylene terephthalate one of the same shape was used.

[0127] (Comparative Example 2) A binder package was obtained and evaluated by performing the same operations as in Example 1, except for the following changes: In (1-2), the liquid supply adapter 120 and the liquid supply pipe 130 were not used, and a container having a structure in which the opening 111 of the storage section 110 was closed with a plug was used. In (1-3), when the binder composition was supplied from the binder package, the plug was removed to open the opening, a pipe was inserted through the opening, and the binder composition was sucked up using the liquid supply pump of the coating machine.

[0128] The outline and results of the Examples and Comparative Examples are shown in Table 2.

[0129]

[0130] 100: Container 101: Container internal space 102: Inner wall surface 110: Storage section 111: Opening 120: Liquid supply adapter 121: Through hole 121H: Top opening 121L: Bottom opening 122: Recess 123: Connector engagement section 129: Air supply hole 129H: Top opening 129L: Bottom opening 130: Liquid supply tube 131H: Top end 131L: Bottom end 140: Plug 150: Connector 153: Connection section 151L: Opening 159L: Opening 191: Screwed section 192: Screwed section

Claims

1. A binder package comprising a container and a binder composition for a secondary battery contained in an internal space of the container, wherein the container comprises a storage section, a liquid delivery adapter, a liquid delivery tube, and a plug, the storage section has an opening at its top, the liquid delivery adapter is provided to engage with the opening of the storage section, the bottom end of the liquid delivery tube is close to the bottom of the internal space of the container and the top end is engaged with the liquid delivery adapter, the liquid delivery adapter and the liquid delivery tube form a liquid-conducting path that connects the opening of the bottom end of the liquid delivery tube with the top side of the container, the plug is provided to detachably engage with the liquid delivery adapter to seal the liquid-conducting path, and a contact angle θ between the binder composition and an inner wall surface of the container B is 30° or more.

2. The binder package according to claim 1, wherein the liquid supply adapter has an engaging portion that can be connected to a connector that delivers the binder composition to the outside of the container.

3. The binder package according to claim 1 or 2, wherein the binder composition contains a particulate polymer having a glass transition temperature of 40°C or higher and 200°C or lower.

4. The binder package according to claim 1 or 2, wherein the binder composition comprises a particulate polymer having a core-shell structure comprising a core portion and a shell portion covering the outer surface of the core portion, and the glass transition temperature of the shell portion is 40°C or higher and 200°C or lower.

5. The binder package described in claim 4, wherein the binder composition further contains an auxiliary particulate polymer which is a non-core-shell particulate polymer, and the content of the auxiliary particulate polymer in 100% by mass of the binder composition is 5% by mass or less.

6. The binder package according to claim 1 or 2, wherein the binder composition contains a particulate polymer, and the particulate polymer consists solely of a particulate polymer having a core-shell structure comprising a core portion and a shell portion covering the outer surface of the core portion.

7. The binder composition contains a particulate polymer, an anti-drying agent, and water, and the contact angle θ between the inner wall surface of the storage portion and water is W 3. The binder package according to claim 1, wherein the angle is 80° or more.

8. A binder package as described in claim 1 or 2, wherein the concentration of granular components having a sphere volume equivalent diameter of 5 μm or more in the binder composition contained in the binder package stored for 6 months in an environment of 5°C or higher and 40°C or lower is 1000 ppm or less.

Citation Information

Patent Citations

  • Liquid container, liquid feeding apparatus using the same, and liquid feeding method

    JP2011098736A

  • Binder product for secondary battery

    US20230331976A1

  • Method for preserving aqueous binder composition for lithium secondary cell

    WO2015029835A1

  • Binder product for secondary batteries

    WO2022071523A1

  • Efficient silicon-carbon negative electrode slurry mixing device

    CN115646281A