Functional particle-carrying fiber

Functional particle-supported fibers with a binder resin and graft-bonded compounds improve particle retention on natural fibers, addressing the sustainability issues during bleaching and washing, ensuring effective functional expression and durability.

WO2024203542A1PCT designated stage expired Publication Date: 2024-10-03KURABO INDUSTRIES LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/010566
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-27
Filing Date
2024-03-18
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Existing methods for imparting functionality to fibers, such as embedding functional substances, often result in reduced functional expression and poor sustainability against chemical or physical loads, especially when using natural fibers like cotton and rayon, which face challenges during bleaching and washing treatments.

Method used

The use of functional particle-supported fibers with a binder resin and a compound having multiple acrylic or methacrylic groups, where the compound is graft-bonded to the fiber or binder resin, enhancing the retention of functional particles on the fiber surface through crosslinking and hydrophobic interactions, thereby improving their durability against chemical and physical loads.

Benefits of technology

This approach significantly enhances the retention of functional particles on natural fibers, ensuring they withstand bleaching and washing treatments, maintaining their functionality and structural integrity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-C000001
    Figure JPOXMLDOC01-APPB-C000001
  • Figure JPOXMLDOC01-APPB-C000002
    Figure JPOXMLDOC01-APPB-C000002
  • Figure JPOXMLDOC01-APPB-C000003
    Figure JPOXMLDOC01-APPB-C000003
Patent Text Reader

Abstract

Provided is a functional particle-carrying fiber in which functional particles are carried on a fiber (F) derived from at least one natural material selected from a natural fiber and a regenerated cellulose-based fiber. The functional particle-carrying fiber contains a binder resin that is fixed to the fiber (F) and a compound that is bound to the fiber (F) or the binder resin through a graft bond and has two or more, per molecule, of at least one group selected from an acryl group and a methacryl group, wherein the functional particles are carried on the fiber (F) thorough the binder resin or the graft-bound compound. The fiber (F) is preferably cotton, the binder resin is preferably an acrylic resin, and the compound is preferably an acrylic-modified organopolysiloxane.
Need to check novelty before this filing date? Find Prior Art

Description

Functional particle-supported fibers

[0001] The present invention relates to a functional particle-supported fiber, a method for producing the same, a functional particle-supported spun yarn or a functional particle-supported fiber structure containing the functional particle-supported fiber, etc.

[0002] When imparting some functionality to fibers, in the case of synthetic fibers, functionality is imparted by embedding a functional substance in the raw resin (Patent Document 1). Another method is to support the functional substance on the fiber surface. In this case, a binder component is generally used to support the functional substance on the fiber surface. For example, in Patent Document 2, an infrared blocking agent is fixed to the fiber material using a binder resin or the like.

[0003] JP 2016-196715 A Japanese Patent No. 4080106 A

[0004] However, when a functional substance is loaded by kneading, the functional substance is embedded inside the fiber, which is less effective than loading it on the fiber surface. Furthermore, when loading a functional substance using only a binder component, there is an issue with the durability of the functional substance loading against chemical or physical stress during bleaching (de-sizing, scouring, bleaching) and washing. In addition, there is a strong demand for products containing fibers derived from natural materials such as cotton and rayon, particularly when producing fabrics for underwear. The present invention provides a functional particle-loaded fiber that has a high retention of loaded functional particles on fibers derived from natural materials, and a spun yarn and fiber structure that include the functional particle-loaded fiber.

[0005] In one aspect, the present invention relates to a functional particle-supported fiber in which functional particles are supported on fibers (F) derived from at least one type of natural material selected from natural fibers and regenerated cellulose-based fibers, the functional particle-supported fiber comprising: a binder resin fixed to the fibers (F); and a compound graft-bonded to the fibers (F) or the binder resin, the compound having two or more groups of at least one type selected from acrylic groups and methacrylic groups in one molecule, the functional particles being supported on the fibers (F) via the binder resin or the graft-bonded compound.

[0006] In one aspect, the present invention relates to a functional particle-supported spun yarn comprising the functional particle-supported fiber of the present invention.

[0007] In one aspect, the present invention relates to a functional particle-supported fiber structure comprising the functional particle-supported spun yarn of the present invention.

[0008] In one aspect, the present invention relates to a method for producing a functional particle-supported fiber in which functional particles are supported on a fiber (F) derived from at least one type of natural material selected from natural fibers and regenerated cellulose-based fibers, the method comprising: impregnating the fiber (F) with a treatment liquid obtained by mixing a compound having two or more groups of at least one type selected from acrylic groups or methacrylic groups in one molecule, a binder resin, functional particles, and water; and curing the binder resin impregnated into the fiber (F) to graft-bond the compound to the fiber (F) or the binder resin.

[0009] In one aspect, the present invention relates to a method for producing a functional particle-supported fiber structure in which functional particles are supported on a fiber structure containing fibers (F) derived from at least one type of natural material selected from natural fibers and regenerated cellulose-based fibers, the method comprising: impregnating the fiber structure with a treatment liquid obtained by mixing a compound having two or more groups of at least one type selected from acrylic groups or methacrylic groups in one molecule, a binder resin, functional particles, and water; and curing the binder resin impregnated into the fiber structure, thereby graft-bonding the compound to the fibers (F) of the fiber structure or the binder resin.

[0010] The present invention provides a functional particle-supported fiber that has a high retention force of supported functional particles on the fiber, and a functional particle-supported spun yarn and a functional particle-supported fiber structure that include the functional particle-supported fiber, by using a compound that has two or more groups of at least one type selected from acrylic groups or methacrylic groups in one molecule in combination with a binder resin.

[0011] The present inventors have conducted extensive research into improving the retention of functional particles on fibers (F) derived from at least one natural material selected from natural fibers and regenerated cellulose fibers. As a result, they have discovered that by using a compound (hereinafter sometimes abbreviated as "compound") containing two or more groups selected from acrylic groups (CH2CHCOO-) or methacrylic groups (CH2C(CH3)COO-) in one molecule in combination with a binder resin and graft-bonding the compound to the fibers (F) or the binder resin, the detachment of functional particles from the fibers (F) due to chemical or physical stress is suppressed, and the retention of the supported functional particles on the fibers (F) is improved. The acrylic group is also called an acryloyloxy group, and the methacrylic group is also called a methacryloyloxy group. Grafting the compound onto the fiber (F) or the binder resin includes grafting the compound onto both the fiber (F) and the binder resin.

[0012] The mechanism by which the above effects are exhibited is not clear, but is assumed as follows: Note that the scope of the present invention is not limited by the assumption below.

[0013] The functional particle-supported fiber of the present invention is manufactured using a treatment solution containing the compound, a binder resin, functional particles, and water, and the functional particles are believed to be supported on the fiber (F) via the grafted compound or the binder resin fixed to the fiber (F) (hereinafter, this treatment will also be referred to as "particle-supporting processing"). More specifically, when the compound is grafted, radicals are generated, and the compound becomes entangled with the fiber (F) and the binder resin fixed to the fiber (F) through graft polymerization, and a crosslinking reaction between the compounds proceeds, firmly fixing the compound to the fiber (F) and the binder resin. The functional particles are structurally entangled with the grafted compound, or are supported by the compound through hydrophobic interactions, or are supported on the fiber (F) via the binder resin. From the above, it is presumed that in the functional particle-carrying fiber of the present invention, the grafted compound and the binder resin each carry functional particles, and that the combined use of the compound and the binder resin increases the adhesive strength of one to the other, and the other to the fiber (F), thereby increasing the retention strength of the functional particles and suppressing the detachment of the functional particles due to chemical or physical stress during bleaching treatments (de-sizing, refining, bleaching), washing, etc.

[0014] In the functional particle-supported fiber of the present invention (hereinafter sometimes abbreviated as "particle-supported fiber"), the natural fiber is preferably one or more natural fibers selected from the group consisting of cotton, hemp, kapok, silk, wool, angora, and mohair, and among these, cotton, which is a cellulosic fiber, is preferred. Rayon is an example of a regenerated cellulosic fiber, and its material may be either wood pulp or cotton linter. Among rayons, Modal (registered trademark), which is made from beech pulp, is preferred.

[0015] The compound is preferably an acrylic-modified organopolysiloxane or a polyfunctional acrylate. The compound has two or more acrylic groups in one molecule, which participates in graft bonding and is effective in supporting functional fine particles.

[0016] The acrylic-modified organopolysiloxane is not particularly limited, but examples include acrylic-modified organopolysiloxanes having units represented by the following general formula (1) in the molecule and having two or more acrylic groups in one molecule.

[0017]

[0018] In the general formula (1), R 1 are the same or different substituted or unsubstituted monovalent hydrocarbon groups having 1 to 18 carbon atoms, R 2 is a hydrogen atom, m is an integer of 1 to 8, a and b are positive numbers that satisfy the relationship a+b≦3. The substituted or unsubstituted monovalent hydrocarbon group having 1 to 18 carbon atoms is not particularly limited, but examples thereof include alkyl groups such as methyl, ethyl, propyl, and butyl groups, alkenyl groups such as vinyl and allyl groups, aryl groups such as phenyl and tolyl groups, and groups in which some or all of the hydrogen atoms bonded to the carbon atoms of these groups have been substituted with halogen atoms, cyano groups, or the like, such as chloromethyl groups, trifluoropropyl groups, and cyanoethyl groups. In the general formula (1), R 1 is more preferably a methyl group.

[0019] The acrylic-modified organopolysiloxane preferably has a viscosity at 25° C. in the range of 50 to 5,000 mPa·s, more preferably 100 to 1,000 mPa·s, for reasons of ease of adhesion to the fibers (F) and ease of preparation of the treatment liquid. The acrylic-modified organopolysiloxane may be a single acrylic-modified organopolysiloxane, or a mixture of multiple acrylic-modified organopolysiloxanes differing in degree of polymerization or amount of functional groups.

[0020] Examples of polyfunctional acrylates include trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol tri(meth)acrylate, dipentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, etc. The polyfunctional acrylates may be used alone or in combination of two or more.

[0021] Examples of binder resins include urethane resins, acrylic resins, polyamide resins, and polyester resins, with acrylic resins being preferred. The acrylic resin is preferably a styrene-acrylic acid ester copolymer. A binder resin that is cured by heat is usually used.

[0022] Examples of functional particles include inorganic particles, which are fine particles of inorganic elements or inorganic compounds. Specific examples of inorganic fine particles include at least one inorganic fine particle selected from the group consisting of silver (Ag), palladium (Pd), rhodium (Rh), ruthenium (Ru), nickel (Ni), copper (Cu), cobalt (Co), silica, titanium oxide, zinc oxide, cerium oxide, zirconium oxide, and magnesium oxide. For example, titanium oxide has heat-shielding, light-shielding, and stain-resistant properties, making it suitable for clothing applications, particularly underwear. Silver also has antibacterial properties, while zinc oxide, magnesium oxide, zirconium oxide, and silica have cool-to-the-touch properties and anti-transparency properties. These inorganic fine particles may be used alone or in combination of two or more.

[0023] The inorganic fine particles preferably have an average particle diameter of 1 μm or less, more preferably 0.6 μm or less. There is no particular lower limit, but from the viewpoint of suppressing aggregation of the fine particles, a diameter of 0.2 μm or more is preferred. The average particle diameter here refers to the volume average particle diameter.

[0024] In the particle-supported fiber of the present invention, the content of functional particles may be determined appropriately depending on the type of functional particles, the application of the particle-supported fiber, etc., and is not particularly limited. In the particle-supported fiber of the present invention, the content of binder resin may be determined appropriately depending on the type and content of functional particles, the application of the particle-supported fiber, etc., but from the viewpoint of achieving both good functional particle support and good texture, it is preferably 0.1 to 10 mass% and more preferably 0.2 to 4 mass% when the particle-supported fiber is taken as 100 mass%. In the particle-supported fiber of the present invention, from the viewpoint of achieving both good functional particle support and good texture, the content ratio (mass ratio) of the binder resin and the compound in terms of non-volatile content of each component is preferably binder resin:compound = 1:0.5 to 1:15, more preferably 1:0.5 to 1:12, even more preferably 1:1 to 1:12, and even more preferably 1:2 to 1:12.

[0025] In one embodiment, the particle-supported fiber of the present invention may further contain an amino-modified organopolysiloxane having one or more amino groups in one molecule, represented by the following general formula (2), in order to increase the flexibility of the fiber, as long as the effects of the present invention are not impaired.

[0026]

[0027] In the general formula (2), R 3 are the same or different substituted or unsubstituted monovalent hydrocarbon groups having 1 to 18 carbon atoms, hydroxyl groups, alkoxy groups, or amino groups. 4 are the same or different substituted or unsubstituted monovalent hydrocarbon groups having 1 to 18 carbon atoms, or amino groups. 3 and R 4At least one of the groups is an amino group. n is a positive number, and preferably n is 1 or more and 1000 or less. The substituted or unsubstituted monovalent hydrocarbon group having 1 to 18 carbon atoms is not particularly limited, but examples thereof include alkyl groups such as methyl, ethyl, propyl, and butyl groups, alkenyl groups such as vinyl and allyl groups, aryl groups such as phenyl and tolyl groups, and groups in which some or all of the hydrogen atoms bonded to the carbon atoms of these groups have been substituted with halogen atoms, cyano groups, or the like, such as chloromethyl groups, trifluoropropyl groups, and cyanoethyl groups. In the general formula (2), R 3 and R 4 The amino group represented by the formula (3) is not particularly limited, but examples thereof include amino groups represented by the following general formula (3):

[0028]

[0029] In the general formula (3), R 5 represents a substituted or unsubstituted divalent hydrocarbon group having 1 to 8 carbon atoms, R 6 , R 7 and R 8 are each a hydrogen atom, a substituted or unsubstituted monovalent hydrocarbon group having 1 to 4 carbon atoms, or —CHCH(OH)CHOH, and c is an integer from 0 to 4. Examples of the substituted or unsubstituted divalent hydrocarbon group having 1 to 8 carbon atoms include alkylene groups such as ethylene, trimethylene, tetramethylene, hexamethylene, and isobutylene, as well as methylenephenylene and methylenephenylenemethylene groups, with trimethylene being preferred. Examples of the substituted or unsubstituted monovalent hydrocarbon group having 1 to 4 carbon atoms include alkyl groups such as methyl, ethyl, propyl, and butyl, alkenyl groups such as vinyl and allyl, and groups in which the hydrogen atoms bonded to the carbon atoms of these groups are partially substituted with halogen atoms, with methyl being particularly preferred from the standpoints of water repellency, smoothness, and flexibility.

[0030] The amino-modified organopolysiloxane preferably has a viscosity at 25° C. in the range of 50 to 5,000 mPa·s, and more preferably in the range of 100 to 1,000 mPa·s, because it adheres easily to natural fibers and the treatment liquid can be easily prepared. The amino-modified organopolysiloxane may be a single acrylic-modified organopolysiloxane, or a mixture of multiple acrylic-modified organopolysiloxanes having different degrees of polymerization or amounts of functional groups.

[0031] [Functional particle-supported spun yarn] In one aspect, the present invention relates to a functional particle-supported spun yarn (hereinafter sometimes abbreviated as "particle-supported spun yarn") comprising the particle-supported fiber of the present invention. The particle-supported spun yarn may be a blended spun yarn or a core-sheath spun yarn that further comprises unprocessed fiber from the viewpoint of improving the strength of the spun yarn. Here, unprocessed fiber refers to fiber that has not been subjected to the particle-supporting processing described above, or fiber that has not been subjected to graft polymerization for other functions such as moisture absorption and heat generation. The blend ratio of particle-supported fiber may be adjusted appropriately depending on the application. The unprocessed fiber is preferably a natural fiber or a regenerated cellulose fiber, and cotton is preferred, but it may also be a synthetic fiber such as polyester fiber, nylon fiber, acrylic fiber, or spandex. From the viewpoint of being able to control the amount of functional particles (amount of particles carried) depending on the mixing ratio of particle-carrying fibers and from the viewpoint of the strength of the particle-carrying spun yarn, the mass proportion of particle-carrying fibers is preferably 5 to 50 mass%, more preferably 5 to 40 mass%, and the mass proportion of unprocessed fibers is preferably 50 to 95 mass%, more preferably 60 to 95 mass%.

[0032] [Functional particle-supported fiber structure] In one aspect, the present invention provides a functional particle-supported fiber structure (hereinafter sometimes abbreviated as "particle-supported fiber structure") in which functional particles are supported on a fiber structure containing fiber (F) derived from at least one natural material selected from natural fibers and regenerated cellulose-based fibers. The particle-supported fiber structure is preferably a fabric, more preferably a knitted or woven fabric, and is useful for clothing, towels, bedding, etc. Knitted fabrics in particular are stretchable and soft, making them suitable for innerwear. The particle-supported fiber structure of the present invention may be one produced using the particle-supported spun yarn of the present invention, or may be one produced by impregnating a fabric containing the fiber (F) with the treatment liquid, curing the binder resin, and grafting the compound having two or more acrylic groups per molecule to support the functional particles.

[0033] The fabric containing the fiber (F) may be made of 100% natural fibers such as cotton, but may also contain synthetic fibers such as polyester fibers, nylon fibers, acrylic fibers, and spandex. The mass proportion of the particle-supported fiber in the particle-supported fiber structure is preferably 2 to 50 mass%, more preferably 5 to 40 mass%, from the viewpoints of the ability to control the amount of functional particles (supported amount) depending on the blend ratio and the strength of the particle-supported fiber structure. The mass proportion of the unprocessed fiber is preferably 50 to 98 mass%, more preferably 60 to 95 mass%. The particle-supported fiber structure of the present invention may be made solely from spun yarn containing the particle-supported fiber of the present invention, or may be made by mixing spun yarn containing the particle-supported fiber with yarn that has not been processed to support particles, i.e., by interweaving or interknitting these yarns. For example, one spun yarn containing the particle-supported fiber may be used with one or two unprocessed yarns. More specifically, preferably, three repeating units of yarn are used, one of which is a blended spun yarn containing 30% by mass of functional particle-supported fiber, and the other two are yarns that have not been processed to support particles, and when the fabric is taken as 100% by mass, a fabric containing 10% by mass of particle-supported fiber is obtained. By changing the usage ratio of the particle-supported fiber to the yarn that has not been processed to support particles in this way, the amount of functional particles incorporated (amount supported) can be controlled depending on the usage ratio.

[0034] The fabric containing the fiber (F) may also contain elastic yarn, which is preferably at least one selected from polyurethane yarn and conjugate yarn obtained by conjugate spinning at least two polymers with different shrinkage rates. The polyurethane elastic yarn may be any type, but is not particularly limited, as long as it is made from a polymer diol and a diisocyanate as starting materials. The conjugate yarn is a conjugate yarn obtained by conjugate spinning at least two polymers with different shrinkage rates. The conjugate yarn exhibits crimp (crimp) even in the raw yarn stage, but exhibits even greater crimp (crimp) upon application of heat. Specifically, a conjugate yarn (bicomponent yarn) of polyethylene terephthalate (PET) and polytrimethylene terephthalate (PTT) is preferred. Examples of such latent crimp-type stretch yarns include "Lycra T400" manufactured by Toray Opelontex, "Spandy" manufactured by KB Seiren, and "Z10" manufactured by Unitika Ltd. A commonly used elastic thread is a polyurethane thread.

[0035] When the fabric is taken as 100% by mass, the ratio of fiber (F) (when the synthetic fiber is contained, the total amount of fiber (F) and the synthetic fiber) to elastic yarn is preferably 88:12 to 94:6, more preferably 90:10 to 95:5, by mass.

[0036] The mass per unit area of ​​the fabric is 80 to 300 g / m 2 is preferable, and more preferably 90 to 250 g / m 2 and more preferably 100 to 200 g / m 2 If it is in the above range, it is suitable for use as innerwear.

[0037] The garment sewn using the particle-supported fiber structure (fabric) of the present invention is preferably a so-called one-way stretch fabric in which the elastic yarns are arranged in the circumferential direction of the body. The circumferential direction of the body refers to the circumferential direction of the torso and the circumferential direction of the arms. This results in an inner garment that is comfortable to wear and does not lose its shape even after repeated washing. The garment is preferably a shirt or pants. In the garment, preferably, the fiber (F) derived from at least one natural material selected from cotton and rayon accounts for 85% by mass or more, more preferably 88% by mass or more, and even more preferably 90% by mass or more of the main fiber, and even more preferably, cotton accounts for 85% by mass or more, even more preferably 88% by mass or more, and even more preferably 90% by mass or more. The particle-supported fiber structure (fabric) of the present invention is preferably a fabric for inner garments that is gentle on the skin.

[0038] [Method for producing functional particle-supported fiber] Next, an example of a method for producing the functional particle-supported fiber of the present invention will be described. In one embodiment, the method for producing the functional particle-supported fiber of the present invention includes the following steps (1) and (2). (1) A treatment liquid obtained by mixing a compound having two or more groups of at least one type selected from acrylic groups or methacrylic groups per molecule, a binder resin, functional particles, and water is impregnated into fibers (F) derived from at least one natural material selected from natural fibers and regenerated cellulosic fibers, and the fibers (F) impregnated with the treatment liquid are then dried. (2) The fibers (F) impregnated with the treatment liquid and then dried are heated to cure the binder resin and graft-bond the compound to the fibers (F) or the binder resin.

[0039] The above-mentioned fiber (F) is preferably in a cotton-like form, and a fiber bundle such as a sliver is preferred, from the viewpoint of improving the retention of the supported functional particles on the fiber and of being able to control the amount of functional particles (supported amount) depending on the blending ratio of the fiber (F) in the spun yarn or fiber structure. Furthermore, a fiber bundle allows for continuous processing, which is convenient for later blending with an unprocessed fiber bundle by aligning them or for forming a core-sheath structure. Therefore, the fiber (F) is preferably a natural fiber that can be processed to support particles in the sliver state, and more preferably cotton.

[0040] The treatment liquid may contain other textile chemicals, such as anti-wrinkle agents, flame retardants, antistatic agents, heat-resistant agents, and the amino-modified organopolysiloxane, as long as the effects of the present invention are not impaired.

[0041] In preparing the treatment liquid, the compound may be emulsified using water as a dispersion medium and then mixed with water. When the compound is the acrylic-modified organopolysiloxane, the emulsified compound is preferably mixed with water. The viscosity of the emulsion (25°C) is preferably 1 to 1,000 mPa·s. For this emulsification, nonionic surfactants, anionic surfactants, cationic surfactants, amphoteric surfactants, etc. can be used. Examples of nonionic surfactants include polyoxyethylene alkyl ethers, polyoxyethylene alkylphenyl ethers, sorbitan alkylates, and polyoxyethylene sorbitan alkylates. Examples of anionic surfactants include alkylbenzene sulfonates and alkyl phosphates. Examples of cationic surfactants include quaternary ammonium salts and alkylamine salts. Examples of amphoteric surfactants include alkyl betaines and alkyl imidazolines. These surfactants may be used alone or in combination. The surfactant preferably has an HLB (Hydrophilic-Lipophilic Balance) of 11 to 18, more preferably 13 to 16, because it is easily emulsified.

[0042] The amount of the surfactant used is preferably 5 to 50 parts by mass, more preferably 10 to 30 parts by mass, per 100 parts by mass of the silicone component, i.e., the acrylic-modified organopolysiloxane, or per 100 parts by mass of the mixture of the acrylic-modified organopolysiloxane and the amino-modified organopolysiloxane. The amount of water used during emulsification may be any amount, but is generally such that the concentration of the acrylic-modified organopolysiloxane, or the total concentration of the acrylic-modified organopolysiloxane and the amino-modified organopolysiloxane, in the treatment liquid is 1 to 60% by mass, preferably 1 to 20% by mass. To emulsify the acrylic-modified organopolysiloxane, or the acrylic-modified organopolysiloxane and the amino-modified organopolysiloxane, a surfactant is mixed and the mixture is emulsified using an emulsifier such as a homomixer, homogenizer, colloid mill, or line mixer.

[0043] In one embodiment of the present invention, when both the acrylic-modified organopolysiloxane and the amino-modified organopolysiloxane are used as the silicone component, the components may be mixed in advance and then emulsified, or the components may be individually emulsified in advance and then mixed.

[0044] In preparing the treatment liquid, the binder resin may be dispersed in water to form an aqueous emulsion and then mixed with water.

[0045] Since oils (such as cotton wax) in the greige fabric or cotton prevent the treatment solution from penetrating, the treatment solution may contain a penetrating agent to promote penetration. Examples of penetrating agents include INVADINE 650 (manufactured by Huntsman Japan Co., Ltd.). The amount of penetrating agent added is preferably 0.1 to 2% by mass.

[0046] The method for impregnating the fibers (F) with the treatment liquid is not particularly limited, but examples thereof include a padding method in which the fibers (F) are immersed in the treatment liquid, the treatment liquid is squeezed using nip rolls, and the treatment liquid is uniformly applied. The impregnation amount (also referred to as application amount) is preferably 40 to 120 mass% relative to 100 mass% of the fibers (F) before impregnation. By setting the impregnation amount within the above range, the adhesion of the functional particles to the fibers (F) can be improved.

[0047] Drying for volatilizing water after the fibers (F) are impregnated with the treatment solution may be carried out, for example, by blowing hot air or using a heating furnace. The drying temperature and time may be set arbitrarily as long as they do not affect the fibers, but for example, a drying temperature of 100 to 180°C and a drying time of 10 seconds to 5 minutes are preferred.

[0048] Next, the fibers (F) that have been impregnated with the treatment liquid and then dried are further heated in a heating furnace or the like to cure the binder resin. The heating temperature may be any temperature within a range that does not affect the type of binder resin used and the fibers, but for example, a heating temperature of 120 to 200°C and a heating time of 30 seconds to 5 minutes are preferred.

[0049] In the production method of the present invention, preferably, the binder resin is cured, and then the compound is grafted to the fiber (F) or the binder resin. The grafting is preferably performed by irradiation with an electron beam, thereby fixing the compound to the fiber (F) or the binder resin. The electron beam irradiation device is not particularly limited, and may be a curtain type, a scan type, or a double scan type. The acceleration voltage of the electron beam for this electron beam irradiation is not particularly limited, but may be, for example, in the range of 100 to 1000 kV from the viewpoint of sufficient energy penetration and economic efficiency. The irradiation dose of the electron beam is not particularly limited, but may be, for example, in the range of 5 to 100 kGy from the viewpoint of suppressing fiber degradation and inducing a good graft reaction.

[0050] The method for producing functional particle-supported fibers of the present invention may include, after the electron beam irradiation, washing the fibers with water to remove unreacted compounds.

[0051] In the method for producing functional particle-supported fibers of the present invention, after the step (2), bleaching treatment (de-sizing, refining, bleaching) may be carried out in a conventional manner.

[0052] [Method for Manufacturing a Functional Particle-Supported Fiber Structure] In one embodiment of the present invention, the target of particle support processing may be a fabric containing natural fibers. The fabric may be either a knitted fabric or a woven fabric. That is, in one embodiment, the present invention is an example of a method for manufacturing a functional particle-supported fiber structure, and includes the following steps (I) and (II): (I) A treatment liquid obtained by mixing a compound having two or more groups of at least one type selected from acrylic and methacrylic groups per molecule, a binder resin, functional particles, and water is impregnated into a fabric containing fibers (F) derived from at least one natural material selected from natural fibers and regenerated cellulose-based fibers, and the fabric impregnated with the treatment liquid is then dried. (II) The fabric impregnated with the treatment liquid and then dried is heated to cure the binder resin and graft-bond the compound to the fibers (F) or the binder resin.

[0053] In the manufacturing method of the present invention, preferably, the binder resin is cured, and then the compound is grafted to the fiber (F) or the binder resin. The grafting is preferably performed by irradiation with an electron beam, and the compound is fixed to the fiber (F) or the binder resin of the fabric. The preparation and impregnation of the treatment solution, drying, curing of the binder resin, irradiation with an electron beam, removal of unreacted compound, and the like performed in the above step (I) or (II) can be performed in the same manner as in the [Method for manufacturing functional particle-supported fibers].

[0054] In the method for producing a functional particle-supported fiber structure of the present invention, after the step (II), bleaching treatment (desizing, refining, bleaching) may be carried out in a conventional manner.

[0055] The present invention will be described in more detail below with reference to examples. However, the present invention is not limited to the following examples. The physical properties in the following examples and comparative examples are shown as values ​​measured by the following test methods.

[0056] [Washing durability] (Initial Si and Ti content) Using a Rigaku ZSX 100e fluorescent X-ray analyzer, the mass of all elements (W0t) and the mass of Si atoms (W0 Si ), mass of Ti atom (W0 Ti ) was measured, and the initial Si content and Ti content were calculated using the following formula: Initial Si content (mass%) = [(W0 Si ) / (W0t)] × 100 Initial Ti content (mass%) = [(W0 Ti ) / (W0t) × 100

[0057] (Si and Ti content after 10 washes) The sample was washed 10 times in accordance with JIS L 0217 103 and dried. After that, the mass of all elements (W10t) and the mass of Si atoms (W10 Si ), and the mass of the Ti atom (W Ti The Si content and Ti content after 10 washes were calculated using the following formula. JAFET was used as the laundry detergent. Si content after 10 washes (mass%) = (W10 Si ) / (W10t)×100 Ti content (mass%) after 10 washes = (W10 Ti ) / (W10t)×100

[0058] (Si and Ti Retention After 10 Washes) The Si and Ti retention after 10 washes was calculated using the following formula: Si Yield After 10 Washes (%) = (W10 Si ) / (W0 Si ) × 100 Ti retention after 10 washes (%) = (W10 Ti ) / (W0 Ti ) x 100

[0059] The yield of acrylic-modified organopolysiloxane after 10 washes can be evaluated from the yield of Si after 10 washes, and the yield of titanium oxide particles after 10 washes can be evaluated from the yield of Ti after 10 washes.

[0060] [Bleaching Durability] (Bleaching Treatment) A sample was treated at 98°C for 30 minutes in a mixture of an aqueous solution of sodium hydroxide (manufactured by Nacalai Tesque, Inc.), 30 wt% hydrogen peroxide (manufactured by Nacalai Tesque, Inc.), and Stabilizer WC (stabilizer) (manufactured by Clariant Co., Ltd.), followed by rinsing with hot water and water (bath ratio 1:15). The mixture contained 3 g / L of sodium hydroxide, 5 mL / L of 30% hydrogen peroxide, and 1 g / L of Stabilizer WC. Next, the sample was treated at 60°C for 10 minutes in a mixture containing acetic acid (manufactured by Nacalai Tesque, Inc.) and sodium thiosulfate pentahydrate (manufactured by Nacalai Tesque, Inc.), followed by rinsing with hot water and water (bath ratio 1:15). The mixture contained 1 mL / L of acetic acid and 3 g / L of sodium thiosulfate pentahydrate.

[0061] (Si and Ti content after bleaching treatment) Using a Rigaku ZSX 100e fluorescent X-ray analyzer, the mass of all elements (Wbt) and the mass of Si atoms (Wb Si ), and the mass of the Ti atom (Wb Ti ) was measured, and the Si content and Ti content after bleaching treatment were calculated using the following formula: Si content after bleaching treatment (mass%) = (Wb Si ) / (Wbt) × 100 Ti content after bleaching (mass%) = (Wb Ti ) / (Wbt)×100

[0062] (Yield of Si and Ti after bleaching treatment) The yield of Si and Ti after bleaching treatment was calculated by the following formula: Yield of Si after bleaching treatment (%) = (Wb Si ) / (W0 Si ) × 100 Ti yield after bleaching (%) = (Wb Ti ) / (W0 Ti ) x 100

[0063] The yield of the acrylic-modified organopolysiloxane after the bleaching treatment can be evaluated from the yield of Si after the bleaching treatment, and the yield of the titanium oxide particles after the bleaching treatment can be evaluated from the yield of Ti after the bleaching treatment.

[0064] 1. Washing durability, treatment solution impregnated target: 100% cotton cloth (woven fabric) Example 1 A treatment solution was prepared by mixing 2.0% by mass of a 50% by mass emulsion of an acrylic-modified organopolysiloxane represented by the following average molecular formula (4) (X-52-8459 manufactured by Shin-Etsu Chemical Co., Ltd., viscosity (25°C): 30 mPa s, non-volatile content 50% by mass), 1.0% by mass of an aqueous emulsion containing a styrene-acrylate resin (manufactured by Matsui Pigment Chemical Industry Co., Ltd., trade name "Matsuminsol MR80", solid content (non-volatile content) 45% by mass), and 4.0% by mass of a titanium oxide paste (solid content 50 to 60% by mass, average particle size: 0.4 μm) with water to obtain a treatment solution.

[0065]

[0066] Next, a 100% by mass bleached cotton fabric (manufactured by Kurabo Industries, Ltd., warp yarn count 20s x weft yarn count 10s, warp yarn density 117 threads ( / inch) x weft yarn density 52 threads ( / inch) 3 / 1 twill, basis weight: 277.5 g / m 2 ) was immersed in the treatment solution, squeezed using a mangle roll at a 60% squeezing rate, and dried at 150°C for 90 seconds. It was then cured at 165°C for 105 seconds and subsequently irradiated with 40 kGy of electron beams at an acceleration voltage of 200 kV under a nitrogen atmosphere using an area beam electron beam irradiation device EC250 / 15 / 180L (manufactured by Iwasaki Electric Co., Ltd.). This resulted in a processed fabric (woven fabric) in which the acrylic-modified organopolysiloxane and styrene-acrylate resin (binder resin) were fixed to the fabric and inorganic fine particles (titanium oxide) were supported. The binder resin content in the functional particle-supported fiber constituting the resulting processed fabric (woven fabric) was 0.27% by mass, based on 100% by mass of the functional particle-supported fiber. Furthermore, the nonvolatile content ratio of the binder resin and the compound having two or more acrylic groups per molecule in the functional particle-supported fiber was 1:2.2.

[0067] Comparative Example 1 A treatment solution was prepared by mixing 1.0% by mass of a styrene-acrylate resin-containing aqueous emulsion (manufactured by Matsui Pigment Chemical Industry Co., Ltd., product name "Matsuminzol MR80", solids (non-volatile content) 45% by mass) and 4.0% by mass of titanium oxide paste (solids content 50 to 60% by mass) with water. Next, a bleached 100% cotton cloth (the same as in Example 1) was immersed in the treatment solution, squeezed using a mangle roll at a squeezing rate of 60%, and dried at 150°C for 90 seconds. The cloth was then cured at 165°C for 105 seconds to obtain a processed cloth (woven fabric) in which the styrene-acrylate resin (binder resin) was fixed to the cloth and inorganic fine particles (titanium oxide) were supported.

[0068] Comparative Example 2 A treatment solution was prepared by mixing 1.0 mass% of a styrene-acrylate resin-containing aqueous emulsion (manufactured by Matsui Pigment Chemical Industry Co., Ltd., product name "Matsuminsol MR80", solids content (non-volatile content) 45 mass%) and 4.0 mass% of a titanium oxide paste (solids content 50 to 60 mass%) with water. Next, a bleached 100 mass% cotton fabric (the same as in Example 1) was immersed in the treatment solution, and then squeezed using a mangle roll at a squeezing rate of 60%, and dried at 150°C for 90 seconds. The fabric was then cured at 165°C for 105 seconds, and subsequently irradiated with 40 kGy of electron beams at an acceleration voltage of 200 kV under a nitrogen atmosphere using an area beam electron beam irradiation device EC250 / 15 / 180L (manufactured by Iwasaki Electric Co., Ltd.) to obtain a processed fabric (woven fabric) in which the styrene-acrylic ester resin (binder resin) was fixed to the fabric and inorganic fine particles (titanium oxide) were supported. The content of the binder resin in the functional particle-supported fibers constituting the obtained processed fabric (woven fabric) was 0.27% by mass, assuming the functional particle-supported fibers to be 100% by mass.

[0069]

[0070] As shown in Table 1, it can be seen that by using a treatment liquid containing a binder resin and an acrylic-modified organopolysiloxane as a compound having two or more groups of at least one type selected from acrylic and methacrylic groups per molecule, and irradiating with an electron beam, it is possible to support inorganic fine particles with high washing durability. The results of Example 1 confirmed that the combined use of a binder resin and the above compound significantly improved the yield of inorganic fine particles (titanium oxide) after 10 washes. It can also be seen from the results of Comparative Example 2 that electron beam irradiation did not contribute to improving the washing durability of the inorganic fine particles supported by the binder resin.

[0071] 2. Bleaching durability, treatment solution impregnated subject: 100% cotton cloth (woven fabric) Example 2 A treatment solution was prepared by mixing 2.0% by mass of a 50% by mass emulsion of an acrylic-modified organopolysiloxane represented by the following average molecular formula (4) (X-52-8459 manufactured by Shin-Etsu Chemical Co., Ltd., viscosity (25°C): 30 mPa s, non-volatile content 50% by mass), 1.0% by mass of a styrene-acrylate resin-blended aqueous emulsion (manufactured by Matsui Pigment Chemical Industry Co., Ltd., trade name "MATSUMINZOL MR80", solid content (non-volatile content) 45% by mass), 1.0% by mass of a penetrant (INVANIN 650 manufactured by HUNTDUMAN), and 8.0% by mass of a titanium oxide paste (solid content 50 to 60% by mass) with water. Next, a bleached 100% cotton fabric (same as in Example 1) was immersed in the treatment solution, squeezed using a mangle roll at a 60% squeezing rate, and dried at 150°C for 90 seconds. The fabric was then cured at 165°C for 105 seconds, and subsequently irradiated with an electron beam at an acceleration voltage of 200 kV and a dose of 40 kGy using an area beam electron beam irradiation device EC250 / 15 / 180L (manufactured by Iwasaki Electric Co., Ltd.) under a nitrogen atmosphere to obtain a processed fabric (woven fabric) in which the acrylic-modified organopolysiloxane and styrene-acrylate resin (binder resin) were fixed to the fabric and inorganic fine particles (titanium oxide) were supported. The binder resin content in the functional particle-supported fibers constituting the resulting processed fabric (woven fabric) of Example 2 was 0.27% by mass, based on 100% by mass of the functional particle-supported fibers. Furthermore, in the functional particle-supported fiber, the content ratio of the binder resin and the compound having two or more groups of at least one type selected from acrylic groups or methacrylic groups in one molecule in terms of non-volatile content was 1:2.2.

[0072] The resulting processed fabric was bleached according to the above-mentioned "Bleaching Durability" and then the yield of inorganic fine particles and acrylic-modified organopolysiloxane was checked. The results are shown in Table 2.

[0073] Examples 3 and 4: A bleached processed fabric was obtained in the same manner as in Example 2, except that the concentrations of the styrene-acrylic acid ester resin and the acrylic-modified organopolysiloxane in the treatment solution were changed. The binder resin content in the functional particle-carrying fiber constituting the processed fabric (woven fabric) of Example 3 was 0.54% by mass, based on 100% by mass of the functional particle-carrying fiber. Furthermore, in the functional particle-carrying fiber, the nonvolatile content ratio of the binder resin to the compound having two or more acrylic groups per molecule, at least one type of group selected from acrylic and methacrylic groups, was 1:2.2. The binder resin content in the functional particle-carrying fiber constituting the processed fabric (woven fabric) of Example 4 was 1.08% by mass, based on 100% by mass of the functional particle-carrying fiber. Furthermore, in the functional particle-supported fiber, the content ratio of the binder resin and the compound having two or more groups of at least one type selected from acrylic groups or methacrylic groups in one molecule in terms of non-volatile content was 1:2.2.

[0074]

[0075] Table 2 shows that the processed fabrics of Examples 2 to 4 have high durability against bleaching. It was also confirmed that increasing the concentrations of the binder resin and acrylic-modified organopolysiloxane in the treatment solution improved the retention rate.

[0076] 3. Bleaching durability, treatment solution impregnated object: cotton sliver In Example 5 below, instead of 100% cotton fabric, cotton sliver (mass per unit length, unit grain: 25.0 g / 6 yd (4.6 g / m)) was subjected to functional particle carrying processing.

[0077] Example 5 A treatment solution was prepared by mixing 2.0% by mass of a 50% by mass emulsion of an acrylic-modified organopolysiloxane represented by the average molecular formula (4) below (X-52-8459 manufactured by Shin-Etsu Chemical Co., Ltd., viscosity (25°C): 30 mPa s, non-volatile content 50% by mass), 1.0% by mass of an aqueous emulsion containing a styrene-acrylate resin (manufactured by Matsui Pigment Chemical Industry Co., Ltd., trade name "Matsuminzol MR80", solid content (non-volatile content) 45% by mass), 8.0% by mass of titanium oxide paste (solid content 50 to 60% by mass), and 1.0% by mass of a penetrant (INVANIN 650 manufactured by HUNTDUMAN) with water. A cotton sliver was then immersed in the treatment solution, squeezed using a mangle roll at a squeezing rate of 60%, and dried at 150°C for 90 seconds. The fiber was then cured at 165°C for 105 seconds, and subsequently irradiated with 40 kGy of electron beams at an accelerating voltage of 200 kV under a nitrogen atmosphere using an area beam electron beam irradiation device EC250 / 15 / 180L (manufactured by Iwasaki Electric Co., Ltd.). This resulted in a particle-supported cotton sliver in which the acrylic-modified organopolysiloxane and the styrene-acrylate resin (binder resin) were fixed together and inorganic fine particles (titanium oxide) were supported. The binder resin content of the resulting particle-supported cotton sliver (functional particle-supported fiber) was 0.27% by mass, based on 100% by mass of the functional particle-supported fiber. Furthermore, the non-volatile content ratio of the binder resin to the compound having two or more acrylic groups per molecule in the functional particle-supported fiber was 1:2.2.

[0078] The particle-carrying processed cotton sliver obtained as described above and unprocessed cotton sliver (mass per unit length, unit yarn: 25.0 g / 6 yd (4.6 g / m)) were mixed in a mass ratio of 30:70 to produce a spun yarn (cotton blended yarn) with a cotton count of 25, and the mass per unit area (basis weight) was 170 g / m. 2 This knitted fabric was subjected to the same bleaching treatment as in Example 2, and then the yield of inorganic fine particles and acrylic-modified organopolysiloxane was confirmed.

[0079] Example 6 A treatment solution was prepared by mixing 8.0% by mass of a 50% by mass emulsion of an acrylic-modified organopolysiloxane represented by the average molecular formula (4) below (X-52-8459 manufactured by Shin-Etsu Chemical Co., Ltd., viscosity (25°C): 30 mPa s, non-volatile content 50% by mass), 1.0% by mass of a styrene-acrylate resin-blended aqueous emulsion (manufactured by Matsui Pigment Chemical Industry Co., Ltd., trade name "Matsuminzol MR80", solid content (non-volatile content) 45% by mass), 16.0% by mass of titanium oxide paste (solid content 50 to 60% by mass), and 1.0% by mass of a penetrant (INVANIN 650 manufactured by HUNTDUMAN) with water. A cotton sliver was then immersed in the treatment solution, squeezed using a mangle roll at a squeezing rate of 60%, and dried at 150°C for 90 seconds. The fiber was then cured at 165°C for 105 seconds, and subsequently irradiated with 40 kGy of electron beams at an accelerating voltage of 200 kV under a nitrogen atmosphere using an area beam electron beam irradiation device EC250 / 15 / 180L (manufactured by Iwasaki Electric Co., Ltd.). This resulted in a particle-supported cotton sliver in which the acrylic-modified organopolysiloxane and the styrene-acrylate resin (binder resin) were fixed together and inorganic fine particles (titanium oxide) were supported. The binder resin content of the resulting particle-supported cotton sliver (functional particle-supported fiber) was 0.27% by mass, based on 100% by mass of the functional particle-supported fiber. Furthermore, the non-volatile content ratio of the binder resin to the compound having two or more acrylic groups per molecule in the functional particle-supported fiber was 1:8.9.

[0080] The particle-carrying processed cotton sliver obtained as described above and unprocessed cotton sliver (mass per unit length, unit yarn: 25.0 g / 6 yd (4.6 g / m)) were mixed in a mass ratio of 30:70 to produce a spun yarn (cotton blended yarn) with a cotton count of 30, and a knitted fabric was produced. This knitted fabric was subjected to the same bleaching treatment as in Example 2, and then the yield of inorganic fine particles and acrylic-modified organopolysiloxane was confirmed. The mass per unit area (basis weight) of the knitted fabric after bleaching was 186 g / m 2 It was.

[0081]

[0082] Table 3 shows that even when cotton sliver is subjected to particle-loading processing and then used to make knitted fabric, it is able to withstand the chemical and physical damage caused by the subsequent bleaching process, and the loading of inorganic microparticles is well guaranteed.

[0083] The present invention can provide a fiber structure such as a woven fabric or a knitted fabric that has various functions depending on the type of functional particles carried thereon and that has good durability of the carrying of the functional particles against chemical or physical stress.Furthermore, the present invention is useful because the amount of functional particles to be incorporated can be controlled depending on the mixing ratio of particle-carrying fibers in the yarn or fiber structure.

Claims

1. A functional particle-supported fiber in which functional particles are supported on fiber (F) derived from at least one type of natural material selected from natural fibers and regenerated cellulose-based fibers, the functional particle-supported fiber comprising: a binder resin fixed to the fiber (F); and a compound graft-bonded to the fiber (F) or the binder resin, the compound having two or more groups selected from acrylic groups and methacrylic groups in one molecule, the functional particles being supported on the fiber (F) via the binder resin or the graft-bonded compound.

2. The functional particle-supporting fiber according to claim 1, wherein the natural fibers include one or more natural fibers selected from the group consisting of cotton, hemp, kapok, silk, wool, angora and mohair, and the regenerated cellulosic fibers include rayon.

3. The functional particle-supporting fiber according to claim 1, wherein the fiber (F) is cotton.

4. The functional particle-supporting fiber according to any one of claims 1 to 3, wherein the binder resin is an acrylic resin.

5. A fiber carrying functional particles according to any one of claims 1 to 4, wherein the functional particles are inorganic fine particles.

6. A functional particle-supporting fiber according to any one of claims 1 to 5, wherein the compound is an acrylic-modified organopolysiloxane or a polyfunctional acrylate.

7. A functional particle-carrying fiber according to any one of claims 1 to 6, wherein the functional particle-carrying fiber is in the form of a sliver (cotton).

8. A functional particle-supported fiber described in any one of claims 1 to 7, wherein the content of the binder resin is 0.1 to 10 mass % when the functional particle-supported fiber is 100 mass %.

9. A functional particle-supporting fiber according to any one of claims 1 to 8, wherein the content ratio of the binder resin to each component of the compound is 1:0.5 to 1:

15.

10. A functional particle-supported spun yarn comprising the functional particle-supported fiber according to any one of claims 1 to 9.

11. The functional particle-supporting spun yarn according to claim 10, which is a blended spun yarn or a sheath-core spun yarn, further comprising unprocessed fibers.

12. A fiber structure carrying functional particles, comprising the functional particle-carrying spun yarn according to claim 10 or 11.

13. A method for producing a functional particle-supported fiber in which functional particles are supported on fiber (F) derived from at least one natural material selected from natural fibers and regenerated cellulose-based fibers, the method comprising the steps of impregnating the fiber (F) with a treatment liquid obtained by mixing a compound having two or more groups of at least one type selected from acrylic groups or methacrylic groups in one molecule, a binder resin, functional particles, and water, and curing the binder resin impregnated into the fiber (F), and graft-bonding the compound to the fiber (F) or the binder resin.

14. A method for producing functional particle-supporting fibers as described in claim 13, wherein after the binder resin is cured, the compound is graft-bonded to the fibers (F) or the binder resin by irradiating the binder resin with an electron beam.

15. The method for producing functional particle-supporting fibers according to claim 14, further comprising a bleaching treatment after the electron beam irradiation.

16. A method for producing functional particle-supported fibers according to any one of claims 13 to 15, wherein the compound is an acrylic-modified organopolysiloxane or a polyfunctional acrylate.

17. A method for producing a functional particle-supported fiber structure in which functional particles are supported on a fiber structure containing fibers (F) derived from at least one natural material selected from natural fibers and regenerated cellulose-based fibers, the method comprising: impregnating the fiber structure with a treatment liquid obtained by mixing a compound having two or more groups of at least one type selected from acrylic groups or methacrylic groups in one molecule, a binder resin, functional particles and water; curing the binder resin impregnated into the fiber structure, and graft-bonding the compound to the fibers (F) or the binder resin of the fiber structure.

18. A method for producing a functional particle-supporting fiber structure as described in claim 17, wherein after the binder resin is cured, the compound is graft-bonded to the fiber (F) or the binder resin by irradiating it with an electron beam.

19. The method for producing a functional particle-supporting fiber structure according to claim 18, further comprising a bleaching treatment after the electron beam irradiation.

20. A method for producing functional particle-supported fibers according to any one of claims 17 to 19, wherein the compound is an acrylic-modified organopolysiloxane or a polyfunctional acrylate.

Citation Information

Patent Citations

  • Fiber having cool feeling

    JP1997170176A

  • Deodorant cellulose fiber structure and manufacturing method thereof as well as deodorant cellulose fiber product using the deodorant cellulose fiber structure

    JP2011219898A

  • Anti-viral member

    WO2010073738A1