Binder composition for nonaqueous secondary battery negative electrodes, slurry composition for nonaqueous secondary battery negative electrodes, negative electrode for nonaqueous secondary batteries, and nonaqueous secondary battery
The use of a graft copolymer binder composition with specific structural units in non-aqueous secondary battery negative electrodes addresses capacity reduction issues by dispersing stress from expansion and contraction, enhancing cycle characteristics and mechanical strength.
Patent Information
- Application Number
- PCT/JP2024/010695
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-29
- Filing Date
- 2024-03-19
- Publication Date
- 2024-10-03
AI Technical Summary
Non-aqueous secondary batteries, such as lithium-ion batteries, experience capacity reduction due to repeated charging and discharging cycles, necessitating a technology that can suppress this capacity degradation.
A binder composition for non-aqueous secondary battery negative electrodes is developed, comprising a graft copolymer with a backbone polymer containing hydroxyl groups, a monomer unit with an anionic group, and a water-soluble monomer unit, which provides excellent cycle characteristics by dispersing stress caused by the expansion and contraction of the negative electrode active material.
The binder composition effectively suppresses the disconnection of conductive paths and maintains high mechanical strength in the negative electrode composite layer, leading to improved cycle characteristics and capacity retention in non-aqueous secondary batteries.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002
Abstract
Description
Binder composition for non-aqueous secondary battery negative electrode, slurry composition for non-aqueous secondary battery negative electrode, non-aqueous secondary battery negative electrode, and non-aqueous secondary battery
[0001] The present invention relates to a binder composition for a non-aqueous secondary battery negative electrode, a slurry composition for a non-aqueous secondary battery negative electrode, a non-aqueous secondary battery negative electrode, and a non-aqueous secondary battery.
[0002] Non-aqueous secondary batteries such as lithium-ion secondary batteries (hereinafter sometimes abbreviated as "secondary batteries") are small, lightweight, have high energy density, and can be repeatedly charged and discharged, and are therefore used in a wide range of applications. Therefore, in recent years, improvements to battery components such as electrodes have been investigated with the aim of further improving the performance of secondary batteries.
[0003] Electrodes used in secondary batteries such as lithium-ion secondary batteries typically include a current collector and an electrode mixture layer (positive electrode mixture layer or negative electrode mixture layer) formed on the current collector. The electrode mixture layer is formed, for example, by applying a slurry composition containing an electrode active material and a binder composition containing a binder onto the current collector and then drying the applied slurry composition (Patent Document 1).
[0004] International Publication No. 2020 / 080246
[0005] In general, the capacity of a secondary battery decreases with repeated charge and discharge cycles. From the viewpoint of improving battery performance, there is a need to develop a technology that can suppress the capacity decrease caused by repeated charge and discharge cycles.
[0006] The present invention has been made in view of the above-mentioned problems, and has an object to provide a binder composition for a non-aqueous secondary battery negative electrode, a slurry composition for a non-aqueous secondary battery negative electrode, and a non-aqueous secondary battery negative electrode, which can provide a non-aqueous secondary battery with excellent cycle characteristics; and a non-aqueous secondary battery with excellent cycle characteristics.
[0007] The present inventors have conducted extensive research to solve the above-mentioned problems. As a result, the present inventors have found that the above-mentioned problems can be solved when a graft copolymer containing a specific structural unit is used as a binder for a negative electrode, and have completed the present invention. That is, the present invention includes the following.
[0008] [1] A binder composition for a non-aqueous secondary battery anode, comprising a graft copolymer, wherein the graft copolymer comprises a trunk polymer containing a hydroxyl group, and a branch polymer comprising a monomer unit containing an anionic group and a water-soluble monomer unit not containing an anionic group, both bonded to the trunk polymer. [2] The binder composition for a non-aqueous secondary battery anode according to [1], wherein the weight ratio of the monomer unit containing an anionic group to the water-soluble monomer unit not containing an anionic group (monomer unit containing anionic group / water-soluble monomer unit not containing an anionic group) is 10 / 90 or more and 50 / 50 or less. [3] The binder composition for a non-aqueous secondary battery anode according to [1] or [2], wherein the proportion of the trunk polymer relative to 100% by weight of the graft copolymer is 3.0% by weight or more and 20% by weight or less. [4] The binder composition for a non-aqueous secondary battery anode according to any one of [1] to [3], wherein the trunk polymer contains a hydroxyl group-containing unsaturated aliphatic unit. [5] The binder composition for a non-aqueous secondary battery anode according to any one of [1] to [4], wherein the branch polymer contains an ethylenically unsaturated monocarboxylic acid unit. [6] The binder composition for a non-aqueous secondary battery anode according to any one of [1] to [5], wherein the branch polymer contains an unsaturated carboxylic acid amide unit. [7] The binder composition for a non-aqueous secondary battery anode according to any one of [1] to [6], comprising water. [8] A slurry composition for a non-aqueous secondary battery anode, comprising a negative electrode active material and the binder composition for a non-aqueous secondary battery anode according to any one of [1] to [7]. [9] The slurry composition for a non-aqueous secondary battery anode according to [8], wherein the negative electrode active material contains a silicon-based negative electrode active material.
[10] A negative electrode for a non-aqueous secondary battery, comprising a negative electrode mixture layer containing a negative electrode active material and a graft copolymer, wherein the graft copolymer contains a trunk polymer containing a hydroxyl group, and a branch polymer containing a monomer unit containing an anionic group and a water-soluble monomer unit not containing an anionic group, both bonded to the trunk polymer.
[11] A non-aqueous secondary battery, comprising a positive electrode, the negative electrode for a non-aqueous secondary battery according to
[10] , and an electrolyte solution.
[0009] According to the present invention, it is possible to provide a binder composition for a non-aqueous secondary battery negative electrode, a slurry composition for a non-aqueous secondary battery negative electrode, and a non-aqueous secondary battery negative electrode, which can provide a non-aqueous secondary battery with excellent cycle characteristics; and a non-aqueous secondary battery with excellent cycle characteristics.
[0010] The present invention will be described in detail below with reference to embodiments and examples. However, the present invention is not limited to the embodiments and examples described below, and can be implemented with any modifications within the scope of the claims and their equivalents.
[0011] In a polymer produced by copolymerizing multiple types of monomers, the ratio of structural units formed by polymerizing a certain monomer in the polymer usually coincides with the ratio (feed ratio) of the certain monomer to all the monomers used in the polymerization of the polymer, unless otherwise specified.
[0012] The structure of a molecule or a part thereof, such as a structural unit, is not limited by its production method. For example, an anionic monomer unit is a unit having a structure formed by polymerization of an anionic monomer, but the anionic monomer unit also includes units formed by other formation methods that have the same structure as the structure formed by polymerization of an anionic monomer.
[0013] In the following description, unless otherwise specified, the term "(meth)acrylic acid" includes acrylic acid, methacrylic acid, and mixtures thereof. Furthermore, unless otherwise specified, the term "(meth)acrylate" includes acrylate, methacrylate, and mixtures thereof. Furthermore, unless otherwise specified, the term "(meth)acrylamide" includes acrylamide, methacrylamide, and mixtures thereof.
[0014] In the following description, unless otherwise specified, a substance being "water-soluble" means that when 0.5 g of the substance is dissolved in 100 g of water at 25° C., the insoluble content is less than 0.5 wt %. Furthermore, a substance being "water-insoluble" means that when 0.5 g of the substance is dissolved in 100 g of water at 25° C., the insoluble content is 90 wt % or more.
[0015] <Outline of binder composition for non-aqueous secondary battery negative electrode> A binder composition for non-aqueous secondary battery negative electrode according to one embodiment of the present invention (hereinafter sometimes abbreviated as "binder composition") contains a graft copolymer. This graft copolymer contains a trunk polymer as a polymer that forms the trunk portion of the graft copolymer, and a branch polymer as a polymer that is bonded to the trunk polymer to form the branch portion of the graft copolymer. The trunk polymer contains hydroxyl groups. Furthermore, the branch polymer contains a combination of a monomer unit containing an anionic group and a water-soluble monomer unit that does not contain an anionic group. Hereinafter, a "monomer unit containing an anionic group" may be referred to as an "anionic monomer unit," and a "water-soluble monomer unit that does not contain an anionic group" may be referred to as a "non-anionic water-soluble monomer unit."
[0016] The binder composition according to this embodiment can be used to form a negative electrode of a non-aqueous secondary battery. Specifically, the binder composition can be used to manufacture a slurry composition for a non-aqueous secondary battery negative electrode (hereinafter, sometimes abbreviated as "slurry composition"). This slurry composition can also be used to manufacture a negative electrode for a non-aqueous secondary battery (hereinafter, sometimes abbreviated as "negative electrode"). This negative electrode can then be used to manufacture a non-aqueous secondary battery. This non-aqueous secondary battery can have excellent cycle characteristics. Furthermore, the binder composition according to this embodiment can generally produce a negative electrode composite layer with excellent mechanical strength. Without being bound by any particular theory, the inventors speculate that the mechanism by which the above-described effects are obtained is as follows. However, the technical scope of the present invention is not limited to the mechanism described below.
[0017] Generally, the negative electrode active material contained in the negative electrode mixture layer expands and contracts during charging and discharging. In particular, silicon-based negative electrode active materials can achieve high capacity, but the degree of expansion and contraction is large. Conventionally, when the negative electrode active material expands and contracts, the binder is stretched during expansion, which can lead to rupture of the binder. When the binder is ruptured, the conductive path is broken, resulting in a decrease in discharge capacity and a decrease in the mechanical strength of the negative electrode mixture layer.
[0018] In contrast, the graft copolymer contained in the binder composition according to this embodiment has a branched structure including a trunk polymer and a branch polymer bonded to the trunk polymer. This branched structure allows for the dispersion of stress during expansion of the negative electrode active material. Therefore, the graft copolymer can function as a binder that is highly resistant to the expansion and contraction of the negative electrode active material, thereby suppressing the disconnection of the conductive path and the decrease in discharge capacity, thereby achieving excellent cycle characteristics. Furthermore, because the graft copolymer can disperse stress, the negative electrode composite layer containing the graft copolymer can have high resistance to stress and therefore typically achieve high mechanical strength.
[0019] <Graft Copolymer> The graft copolymer has a branched molecular structure including a trunk polymer and branch polymers bonded to the trunk polymer. The trunk polymer contains a hydroxyl group. Preferably, the trunk polymer includes a structural unit containing a hydroxyl group. Hereinafter, the structural unit containing a hydroxyl group may be referred to as a "hydroxyl group-containing unit."
[0020] The hydroxyl group-containing unit typically has a structure formed by polymerizing a hydroxyl group-containing monomer. The hydroxyl group-containing monomer can be a compound containing a hydroxyl group and a polymerizable group, and examples thereof include hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl acrylate, 2-hydroxymethacrylate, 2-hydroxypropyl acrylate, 2-hydroxypropyl methacrylate, hydroxybutyl acrylate, hydroxybutyl methacrylate, 3-chloro-2-hydroxypropyl methacrylate, di-(ethylene glycol) maleate, di-(ethylene glycol) itaconate, 2-hydroxyethyl maleate, bis(2-hydroxyethyl) maleate, and 2-hydroxyethyl methyl fumarate; and hydroxyl group-containing unsaturated aliphatic compounds such as allyl alcohol and vinyl alcohol. Typically, the hydroxyl group-containing monomer is water-soluble, and polymers (homopolymers, copolymers, etc.) of such monomers can also be water-soluble. Therefore, a trunk polymer containing a hydroxyl group-containing unit corresponding to the hydroxyl group-containing monomer can typically be water-soluble.
[0021] The backbone polymer may contain only one type of hydroxyl group-containing unit, or may contain two or more types in combination.
[0022] Among the above-mentioned hydroxyl group-containing monomers, hydroxyl group-containing unsaturated aliphatic compounds are preferred. Therefore, it is preferred that the backbone polymer of the graft copolymer contains a hydroxyl group-containing unsaturated aliphatic unit. The "hydroxyl group-containing unsaturated aliphatic unit" refers to a structural unit having a structure formed by polymerizing a hydroxyl group-containing unsaturated aliphatic compound.
[0023] The proportion of the hydroxyl group-containing units relative to 100% by weight of the total trunk polymer is preferably 60% by weight to 99% by weight, more preferably 70% by weight to 99% by weight, and even more preferably 80% by weight to 99% by weight. When the proportion of the hydroxyl group-containing units is within this range, a secondary battery with particularly excellent cycle characteristics can be obtained, and typically, a negative electrode mixture layer with excellent mechanical strength can also be obtained. When the trunk polymer is produced by polymerizing a hydroxyl group-containing monomer, the proportion of the hydroxyl group-containing units relative to 100% by weight of the total trunk polymer usually corresponds to the weight proportion of the hydroxyl group-containing monomer relative to 100% by weight of the total weight of the monomers used to produce the trunk polymer.
[0024] Polyvinyl alcohol is particularly preferred as the trunk polymer. Polyvinyl alcohol can be produced, for example, by saponifying polyvinyl acetate. The range of the saponification degree of the polyvinyl alcohol thus produced can be the same as the range of the ratio of the hydroxyl group-containing units to 100% by weight of the total trunk polymer.
[0025] The degree of polymerization of the trunk polymer is preferably 800 or more, more preferably 1000 or more, even more preferably 1200 or more, and is preferably 3000 or less, more preferably 2800 or less, even more preferably 2600 or less. When the degree of polymerization of the trunk polymer is within the above range, a secondary battery having particularly excellent cycle characteristics can be obtained, and furthermore, a negative electrode composite layer having excellent mechanical strength can usually be obtained.
[0026] The trunk polymer may contain any structural unit that does not contain a hydroxyl group in combination with the hydroxyl group-containing unit. For example, when polyvinyl alcohol is used as the trunk polymer, the polyvinyl alcohol as the trunk polymer may contain, as an optional structural unit, a vinyl acetate unit that remains unsaponified (a structural unit having a structure formed by polymerizing vinyl acetate). The trunk polymer may contain only one type of any structural unit, or may contain two or more types in combination.
[0027] The ratio of the trunk polymer to 100% by weight of the graft copolymer is preferably within a specific range. Specifically, the range of the trunk polymer ratio is preferably 3.00% by weight or more, more preferably 3.10% by weight or more, even more preferably 3.22% by weight or more, and preferably 20.00% by weight or less, more preferably 18.00% by weight or less, and even more preferably 15.00% by weight or less. When the trunk polymer ratio is within the above range, a secondary battery with particularly excellent cycle characteristics can be obtained, and further, a negative electrode mixture layer with excellent mechanical strength can usually be obtained. The ratio of the trunk polymer to 100% by weight of the graft copolymer usually corresponds to the ratio of the trunk polymer used to produce the graft copolymer to the total amount (100% by weight) of the monomers and polymers used to produce the graft copolymer.
[0028] The branch polymer of the graft copolymer contains an anionic monomer unit (a monomer unit containing an anionic group). The anionic group contained in the anionic monomer unit represents a group capable of generating an anion in water. Examples of this anionic group include a phosphate group, a sulfonic acid group, and a carboxylic acid group. The anionic monomer unit may contain one type of anionic group or two or more types of anionic groups. Among these, a carboxylic acid group is preferred.
[0029] The anionic monomer unit may be a structural unit having a structure formed by polymerizing a monomer containing an anionic group. Hereinafter, a "monomer containing an anionic group" may be referred to as an "anionic monomer." Anionic monomers are typically water-soluble, and polymers (homopolymers, copolymers, etc.) of the anionic monomers may also be water-soluble. Therefore, branch polymers and graft copolymers containing anionic monomer units corresponding to the anionic monomers are typically water-soluble. The anionic monomer may be a compound containing an anionic group and a polymerizable group, such as a phosphate group-containing monomer containing a phosphate group, a sulfonic acid group-containing monomer containing a sulfonic acid group, or a carboxylic acid group-containing monomer containing a carboxylic acid group.
[0030] Among anionic monomers, carboxylic acid group-containing monomers are preferred, and ethylenically unsaturated carboxylic acid monomers are more preferred. Examples of ethylenically unsaturated carboxylic acid monomers include ethylenically unsaturated monocarboxylic acids and their derivatives, ethylenically unsaturated dicarboxylic acids and their acid anhydrides, and their derivatives. Examples of ethylenically unsaturated monocarboxylic acids include acrylic acid, methacrylic acid, and crotonic acid. Examples of derivatives of ethylenically unsaturated monocarboxylic acids include 2-ethylacrylic acid, isocrotonic acid, α-acetoxyacrylic acid, β-trans-aryloxyacrylic acid, α-chloro-β-E-methoxyacrylic acid, and β-diaminoacrylic acid. Examples of ethylenically unsaturated dicarboxylic acids include maleic acid, fumaric acid, and itaconic acid. Examples of acid anhydrides of ethylenically unsaturated dicarboxylic acids include maleic anhydride, acrylic anhydride, methylmaleic anhydride, and dimethylmaleic anhydride. Examples of derivatives of ethylenically unsaturated dicarboxylic acids include substituted maleic acids such as methylmaleic acid, dimethylmaleic acid, phenylmaleic acid, chloromaleic acid, dichloromaleic acid, and fluoromaleic acid; and maleic acid esters such as methylallyl maleate, nonyl maleate, decyl maleate, dodecyl maleate, octadecyl maleate, and fluoroalkyl maleate. Among these, ethylenically unsaturated monocarboxylic acids are preferred, and (meth)acrylic acid is more preferred. Therefore, it is preferable that the branch polymer of the graft copolymer contains an ethylenically unsaturated monocarboxylic acid unit. The term "ethylenically unsaturated monocarboxylic acid unit" refers to a structural unit having a structure formed by polymerizing an ethylenically unsaturated monocarboxylic acid.
[0031] The branch polymer may contain only one type of anionic monomer unit, or may contain two or more types in combination.
[0032] The ratio of the anionic monomer units relative to 100 wt% of the graft copolymer is preferably 15 wt% or more, more preferably 18 wt% or more, even more preferably 20 wt% or more, and preferably 30 wt% or less, more preferably 28 wt% or less, and even more preferably 26 wt% or less. When the ratio of the anionic monomer units is within this range, a secondary battery with particularly excellent cycle characteristics can be obtained, and further, a negative electrode composite layer with excellent mechanical strength can usually be obtained. The ratio of the anionic monomer units relative to 100 wt% of the graft copolymer usually corresponds to the weight ratio of the anionic monomer relative to 100 wt% of the total weight of the monomers and polymers used to produce the graft copolymer.
[0033] The proportion of the anionic monomer units relative to 100% by weight of the entire branch polymer is preferably 10% by weight or more, more preferably 15% by weight or more, even more preferably 20% by weight or more, and preferably 40% by weight or less, more preferably 35% by weight or less, and even more preferably 30% by weight or less. When the proportion of the anionic monomer units is within the above range, a secondary battery with particularly excellent cycle characteristics can be obtained, and furthermore, a negative electrode mixture layer with excellent mechanical strength can usually be obtained. The proportion of the anionic monomer units relative to 100% by weight of the entire branch polymer usually corresponds to the weight proportion of the anionic monomer relative to 100% by weight of the total weight of the monomers used to produce the branch polymer.
[0034] The weight ratio of the anionic monomer units to the non-anionic water-soluble monomer units (anionic monomer units / non-anionic water-soluble monomer units) contained in the graft copolymer is preferably 10 / 90 or more, more preferably 15 / 85 or more, even more preferably 20 / 80 or less, and preferably 50 / 50 or less, more preferably 40 / 60 or less, and even more preferably 30 / 70 or less. When the weight ratio is within the above range, a secondary battery with particularly excellent cycle characteristics can be obtained, and furthermore, a negative electrode mixture layer with excellent mechanical strength can usually be obtained. The weight ratio usually corresponds to the weight ratio of the anionic monomer to the non-anionic water-soluble monomer used in the production of the branch polymer. The term "non-anionic water-soluble monomer" refers to a water-soluble monomer that does not contain an anionic group.
[0035] The amount of the anionic monomer unit per 100 parts by weight of the trunk polymer is preferably 50 parts by weight or more, more preferably 100 parts by weight or more, even more preferably 200 parts by weight or more, and preferably 900 parts by weight or less, more preferably 850 parts by weight or less, even more preferably 800 parts by weight or less. When the amount of the anionic monomer unit per 100 parts by weight of the trunk polymer is within the above range, a secondary battery with particularly excellent cycle characteristics can be obtained, and further, a negative electrode mixture layer with excellent mechanical strength can usually be obtained. The amount of the anionic monomer unit per 100 parts by weight of the trunk polymer usually corresponds to the amount of the anionic monomer per 100 parts by weight of the trunk polymer used in the production of the graft copolymer.
[0036] The branch polymer of the graft copolymer contains a non-anionic water-soluble monomer unit (a water-soluble monomer unit not containing an anionic group). The non-anionic water-soluble monomer unit may be a structural unit having a structure formed by polymerizing a water-soluble monomer not containing an anionic group (i.e., a non-anionic water-soluble monomer). Since non-anionic water-soluble monomers are generally water-soluble, polymers (homopolymers, copolymers, etc.) of the non-anionic water-soluble monomers may also be water-soluble. Therefore, branch polymers and graft copolymers containing non-anionic water-soluble monomer units corresponding to the non-anionic water-soluble monomers are generally water-soluble. The non-anionic water-soluble monomer may be a water-soluble compound that does not contain an anionic group but contains a polymerizable group, such as an unsaturated carboxylic acid amide.
[0037] Among non-anionic water-soluble monomers, unsaturated carboxylic acid amides are preferred. Therefore, it is preferable that the branch polymer of the graft copolymer contains an unsaturated carboxylic acid amide unit. The term "unsaturated carboxylic acid amide unit" refers to a structural unit having a structure formed by polymerizing an unsaturated carboxylic acid amide. Examples of unsaturated carboxylic acid amides include acrylamide, methacrylamide, N-methylolacrylamide, N-methylolmethacrylamide, N,N-dimethylacrylamide, and hydroxyethylacrylamide. Among these, (meth)acrylamide is more preferred.
[0038] The branch polymer may contain only one type of non-anionic water-soluble monomer unit, or may contain two or more types in combination.
[0039] The proportion of the non-anionic water-soluble monomer units relative to 100% by weight of the graft copolymer is preferably 40% by weight or more, more preferably 50% by weight or more, even more preferably 60% by weight or more, and preferably 90% by weight or less, more preferably 80% by weight or less, and even more preferably 75% by weight or less. When the proportion of the non-anionic water-soluble monomer units is within this range, a secondary battery with particularly excellent cycle characteristics can be obtained, and furthermore, a negative electrode mixture layer with excellent mechanical strength can usually be obtained. The proportion of the non-anionic water-soluble monomer units relative to 100% by weight of the graft copolymer usually corresponds to the weight proportion of the non-anionic water-soluble monomer relative to 100% by weight of the total weight of the monomers and polymers used to produce the graft copolymer.
[0040] The proportion of the non-anionic water-soluble monomer units relative to 100% by weight of the entire branch polymer is preferably 60% by weight or more, more preferably 65% by weight or more, even more preferably 70% by weight or more, and preferably 90% by weight or less, more preferably 85% by weight or less, and even more preferably 80% by weight or less. When the proportion of the non-anionic water-soluble monomer units is within the above range, a secondary battery with particularly excellent cycle characteristics can be obtained, and furthermore, a negative electrode mixture layer with excellent mechanical strength can usually be obtained. The proportion of the non-anionic water-soluble monomer units relative to 100% by weight of the entire branch polymer usually corresponds to the weight proportion of the non-anionic water-soluble monomer relative to 100% by weight of the total weight of the monomers used to produce the branch polymer.
[0041] The amount of the non-anionic water-soluble monomer unit per 100 parts by weight of the trunk polymer is preferably 100 parts by weight or more, more preferably 200 parts by weight or more, even more preferably 300 parts by weight or more, and preferably 2900 parts by weight or less, more preferably 2700 parts by weight or less, and even more preferably 2500 parts by weight or less. When the amount of the non-anionic water-soluble monomer unit per 100 parts by weight of the trunk polymer is within the above range, a secondary battery with particularly excellent cycle characteristics can be obtained, and further, a negative electrode mixture layer with excellent mechanical strength can usually be obtained. The amount of the non-anionic water-soluble monomer unit per 100 parts by weight of the trunk polymer usually corresponds to the amount of the non-anionic water-soluble monomer per 100 parts by weight of the trunk polymer used in the production of the graft copolymer.
[0042] The branch polymer may contain any structural unit other than the anionic monomer unit and the non-anionic water-soluble monomer unit, as long as the effects of the present invention are not significantly impaired. Examples of the optional structural unit include a water-insoluble monomer unit (a structural unit having a structure formed by polymerizing a water-insoluble monomer). In the branch polymer, the proportion of the optional structural unit is preferably small. Furthermore, it is more preferable that the branch polymer does not contain any optional structural unit.
[0043] The ratio of the branch polymer to 100% by weight of the graft copolymer is preferably within a specific range. Specifically, the range of the branch polymer ratio is preferably 80.00% by weight or more, more preferably 82.00% by weight or more, even more preferably 85.00% by weight or more, and preferably 97.00% by weight or less, more preferably 96.90% by weight or less, and even more preferably 96.78% by weight or less. When the branch polymer ratio is within the above range, a secondary battery with particularly excellent cycle characteristics can be obtained, and further, a negative electrode mixture layer with excellent mechanical strength can usually be obtained. The ratio of the branch polymer to 100% by weight of the graft copolymer usually corresponds to the ratio of the monomers and polymers used to form the branch polymer to the total amount (100% by weight) of the monomers and polymers used to produce the graft copolymer.
[0044] When a viscosity measurement test is performed to measure the viscosity of a 4 wt % aqueous solution of the graft copolymer, the viscosity is preferably within a specific range. The viscosity of the 4 wt % aqueous solution correlates with the molecular weight of the graft copolymer, and the viscosity can indirectly represent the molecular weight of the graft copolymer. The specific viscosity range of the 4 wt % aqueous solution of the graft copolymer is preferably 200 mPa·s or more, more preferably 1000 mPa·s or more, even more preferably 2000 mPa·s or more, and preferably 8000 mPa·s or less, more preferably 7000 mPa·s or less, and even more preferably 6000 mPa·s or less. When the viscosity of the 4 wt % aqueous solution of the graft copolymer is within the above range, a secondary battery with particularly excellent cycle characteristics can be obtained, and a negative electrode composite layer with excellent mechanical strength can also be obtained.
[0045] The viscosity of a 4 wt % aqueous solution of the graft copolymer can be measured using a Brookfield viscometer at a temperature of 25° C., a rotation speed of 60 rpm, and a rotation time of 60 seconds. Specific measurement conditions may be those described in the "Method for measuring the viscosity of a 4 wt % aqueous solution of a polymer" section of the Examples section described later.
[0046] The graft copolymer is usually water-soluble, and therefore, when the binder composition according to this embodiment contains water, the graft copolymer is usually dissolved in water.
[0047] There are no particular limitations on the method for producing the graft copolymer. For example, the graft copolymer may be produced by a method including preparing a trunk polymer and a branch polymer, and then polymerizing and bonding the trunk polymer and the branch polymer. Alternatively, the graft copolymer may be produced by polymerizing a branch polymer monomer onto the trunk polymer. Because graft copolymers are typically water-soluble, polymerization is carried out by solution polymerization using water as the reaction solvent. Therefore, it is preferable to use a water-soluble initiator as the polymerization initiator. Examples of water-soluble initiators include persulfates such as ammonium persulfate, potassium persulfate, and sodium persulfate; water-soluble peroxides such as hydrogen peroxide; water-soluble azo compounds such as 2,2'-azobis(2-methylpropionamidine hydrochloride); and oxidation-reduction (redox) initiators combining an oxidizing agent such as a persulfate with a reducing agent such as sodium bisulfite, ammonium bisulfite, sodium thiosulfate, and hydrosulfite. The polymerization temperature may be set depending on factors such as the polymerization conversion rate and the viscosity of a 4 wt % aqueous solution of the graft copolymer. In one example, the polymerization temperature is preferably 40° C. or higher, more preferably 50° C. or higher, and preferably 90° C. or lower, more preferably 80° C. or lower. The polymerization is preferably carried out in an inert atmosphere such as a nitrogen atmosphere.
[0048] The amount of the graft copolymer in the binder composition according to this embodiment is not particularly limited. For example, when the binder composition contains the graft copolymer and a solvent, the amount of the graft copolymer relative to 100% by weight of the binder composition is preferably 2% by weight or more, more preferably 10% by weight or more, and even more preferably 30% by weight or more. The upper limit is not particularly limited, and may be, for example, 90% by weight or less, 80% by weight or less, or 70% by weight or less.
[0049] <Optional Components That May Be Included in the Binder Composition> The binder composition according to this embodiment may contain optional components in combination with the graft copolymer.
[0050] The binder composition usually contains a solvent in combination with the graft copolymer. One type of solvent may be used alone, or two or more types may be used in combination. The graft copolymer may be dissolved in the solvent, or may not be dissolved but may be dispersed in the solvent as particles. From the viewpoint of significantly obtaining the effects of the present invention, it is preferable that the graft copolymer is dissolved in the solvent. Since the graft copolymer is usually water-soluble, water is preferred as the solvent.
[0051] The binder composition may contain a pH adjuster. Examples of the pH adjuster include alkali metal compounds such as lithium hydroxide, sodium hydroxide, and potassium hydroxide; alkaline earth metal compounds such as calcium hydroxide and magnesium hydroxide; and ammonia. One type of pH adjuster may be used alone, or two or more types may be used in combination.
[0052] The binder composition may contain optional additives. Examples of optional additives include antioxidants, preservatives, antifoaming agents, and binders other than the above-mentioned graft copolymers. One type of optional additive may be used alone, or two or more types may be used in combination.
[0053] <Characteristics of Binder Composition> The binder composition according to the present embodiment may be a solid composition, but is preferably a liquid composition. When the binder composition is a liquid composition, the liquid composition may be a solution in which components other than the solvent are dissolved in the solvent, or a dispersion in which components other than the solvent are dispersed in the solvent.
[0054] The binder composition preferably has a pH within a specific range. The pH range of the binder composition is preferably 6.0 or higher, more preferably 7.0 or higher, even more preferably 7.5 or higher, and preferably 13.0 or lower, more preferably 10.0 or lower, and even more preferably 9.0 or lower. When the binder composition has a pH within the above range, a secondary battery having particularly excellent cycle characteristics can be obtained, and furthermore, a negative electrode mixture layer having excellent mechanical strength can usually be obtained. The pH can be adjusted, for example, by mixing the above-mentioned pH adjuster or a solution thereof with the binder composition.
[0055] <Method for producing binder composition> The binder composition according to this embodiment can be produced by mixing each component that can be contained in the binder composition. From the viewpoint of reducing the number of steps and achieving efficient production, it is preferable to produce the binder composition by a method including a step of obtaining a solution of the graft copolymer by solution polymerization and a step of mixing the solution with any component.
[0056] <Slurry Composition for Non-Aqueous Secondary Battery Negative Electrode> A slurry composition according to one embodiment of the present invention (slurry composition for non-aqueous secondary battery negative electrode) contains a negative electrode active material and the binder composition described above.
[0057] The amount of binder composition in the slurry composition is not particularly limited, but it is preferable to set the amount of graft copolymer per 100 parts by weight of negative electrode active material so that it falls within a specific range. Specifically, the amount of graft copolymer per 100 parts by weight of negative electrode active material is preferably 0.5 parts by weight or more, more preferably 1 part by weight or more, even more preferably 2 parts by weight or more, and preferably 15 parts by weight or less, more preferably 10 parts by weight or less, even more preferably 7 parts by weight or less. When the amount of graft copolymer is within the above range, a secondary battery with particularly excellent cycle characteristics can be obtained, and further, a negative electrode composite layer with excellent mechanical strength can usually be obtained.
[0058] The negative electrode active material is not particularly limited, and any known negative electrode active material used in secondary batteries can be used. For example, negative electrode active materials that can be used in lithium ion secondary batteries, which are an example of secondary batteries, include carbon-based negative electrode active materials, metal-based negative electrode active materials, and negative electrode active materials that are combinations of these.
[0059] The carbon-based negative electrode active material refers to a negative electrode active material having a carbon skeleton that can insert (also referred to as "doping") lithium. Examples of the carbon-based negative electrode active material include carbonaceous materials such as coke, mesocarbon microbeads (MCMB), mesophase pitch-based carbon fiber, pyrolytic vapor-grown carbon fiber, phenolic resin calcined body, polyacrylonitrile-based carbon fiber, pseudoisotropic carbon, furfuryl alcohol resin calcined body (PFA), and hard carbon; and graphitic materials such as natural graphite and artificial graphite.
[0060] The amount of the carbon-based negative electrode active material relative to 100% by weight of the total negative electrode active material is preferably 70% by weight or more, more preferably 75% by weight or more, and is preferably 99% by weight or less, more preferably 95% by weight or less, and even more preferably 90% by weight or less.
[0061] The metal-based negative electrode active material refers to a negative electrode active material containing a metal. The metal-based negative electrode active material usually contains an element capable of intercalating lithium in its structure. When lithium is intercalated, the theoretical electric capacity per unit weight of the metal-based negative electrode active material is usually 500 mAh / g or more. Examples of metal-based negative electrode active materials include lithium metal, elemental metals capable of forming lithium alloys (e.g., Ag, Al, Ba, Bi, Cu, Ga, Ge, In, Ni, P, Pb, Sb, Si, Sn, Sr, Zn, Ti, etc.), as well as oxides, sulfides, nitrides, silicides, carbides, and phosphides thereof. Further examples include oxides such as lithium titanate.
[0062] The negative electrode active material preferably includes a metal-based negative electrode active material, and more preferably includes a silicon-based negative electrode active material. The silicon-based negative electrode active material refers to a negative electrode active material containing silicon. The silicon-based negative electrode active material enables a secondary battery to have a high capacity. Furthermore, silicon-based negative electrode active materials generally undergo a large degree of expansion and contraction upon charging and discharging, and thus have traditionally tended to have poor cycle characteristics. In contrast, the binder composition according to this embodiment can effectively improve the poor cycle characteristics due to such expansion and contraction. Therefore, when a silicon-based negative electrode active material is used, the effects of the present invention can be effectively utilized.
[0063] Examples of silicon-based negative electrode active materials include silicon (Si); alloys of silicon with any metal such as cobalt, nickel, or iron; SiO; 2 , SiO x and composites in which Si-containing materials are coated with or composited with conductive carbon. Among these, silicon oxides are preferred.
[0064] Among silicon oxides, SiO x is SiO and SiO 2 and Si. x is usually a number of 0.01 or more and less than 2. SiO x can be produced, for example, by utilizing the disproportionation reaction of silicon monoxide (SiO). x can be produced by heat treating SiO, optionally in the presence of a polymer such as polyvinyl alcohol, to produce silicon and silicon dioxide. The heat treatment may be carried out in an inert gas atmosphere after grinding and mixing SiO and, optionally, the polymer.
[0065] An example of a composite of a Si-containing material and conductive carbon is a compound obtained by heat-treating a pulverized mixture of SiO, a polymer such as polyvinyl alcohol, and optionally a carbon material under an inert gas atmosphere. When the temperature during heat treatment of the pulverized mixture is high, a composite (Si-SiOx-C composite) is produced in which SiOx produced by the disproportionation reaction of SiO is dispersed in a conductive carbon matrix composed of a carbonized polymer and an optional carbon material. When the temperature during heat treatment of the pulverized mixture is relatively low, a composite (SiO-C) is produced in which a portion of the Si in SiO is substituted with conductive carbon.
[0066] The amount of the silicon-based negative electrode active material relative to 100% by weight of the total negative electrode active material is preferably 1% by weight or more, more preferably 5% by weight or more, and even more preferably 10% by weight or more, and is preferably 30% by weight or less, and more preferably 25% by weight or less.
[0067] The negative electrode active material may be used alone or in combination of two or more. Among these, a carbon-based negative electrode active material and a metal-based negative electrode active material are preferably used in combination, and a carbon-based negative electrode active material and a silicon-based negative electrode active material are more preferably used in combination. In a negative electrode active material containing a carbon-based negative electrode active material and a silicon-based negative electrode active material in combination, Li insertion and desorption into and from the silicon-based negative electrode active material occur at high potential and Li insertion and desorption into and from the carbon-based negative electrode active material occur at low potential. This suppresses expansion and contraction of the negative electrode active material as a whole, thereby further improving the cycle characteristics of the lithium-ion secondary battery.
[0068] When a carbon-based negative electrode active material and a silicon-based negative electrode active material are combined, a mixture of the carbon-based negative electrode active material and the silicon-based negative electrode active material may be used as the negative electrode active material. As a preferred example, a mixture obtained by grinding and mixing a carbon-based negative electrode active material such as a carbonaceous material or a graphite material with a silicon-based negative electrode active material such as silicon or a silicon oxide, optionally in the presence of a polymer such as polyvinyl alcohol, may be used as the negative electrode active material.
[0069] The negative electrode active material is usually contained in the slurry composition and the negative electrode composite layer in the form of particles. The volume average particle diameter of the negative electrode active material is not particularly limited, but is preferably 0.1 μm or more, more preferably 1 μm or more, even more preferably 5 μm or more, and is preferably 100 μm or less, more preferably 50 μm or less, and even more preferably 20 μm or less. The average particle diameter of the particles can be measured as the particle diameter at which the cumulative volume calculated from the smallest diameter side becomes 50% by measuring the particle size distribution using a laser diffraction particle size distribution measuring device ("SALD-3100" manufactured by Shimadzu Corporation).
[0070] The amount of the negative electrode active material is preferably 30% by weight or more, more preferably 35% by weight or more, and even more preferably 40% by weight or more, and is preferably 50% by weight or less, and more preferably 45% by weight or less, based on 100% by weight of the slurry composition.
[0071] The amount of the negative electrode active material is preferably 70% by weight or more, more preferably 80% by weight or more, even more preferably 90% by weight or more, and even more preferably 95% by weight or more, relative to 100% by weight of the total amount of components other than the solvent contained in the slurry composition (i.e., the entire solid content). The upper limit can be, for example, 99% by weight or less, 98% by weight or less, etc.
[0072] The slurry composition may contain any component other than those described above. For example, the slurry composition may contain any component that the binder composition may contain. Typically, the slurry composition contains the same solvent as the binder composition. Furthermore, the optional components that the slurry composition may contain may include, for example, a dispersant, a viscosity modifier (thickener), a phosphite-based antioxidant, a metal capture agent, a conductive material, etc. One type of optional component may be used alone, or two or more types may be used in combination.
[0073] The slurry composition is usually a liquid composition. It is preferable that this slurry composition has a viscosity within a specific range. The viscosity of the slurry composition is preferably 2000 mPa·s or more, more preferably 2500 mPa·s or more, even more preferably 3000 mPa·s or more, and preferably 8000 mPa·s or less, more preferably 7000 mPa·s or less, even more preferably 6000 mPa·s or less. The viscosity of the slurry composition can be measured using a Brookfield viscometer at a temperature of 25°C and a rotation speed of 60 rpm.
[0074] The method for producing the slurry composition is not particularly limited. The slurry composition can be produced, for example, by mixing a binder composition, a negative electrode active material, and optional components as necessary. The mixing method is not particularly limited, and mixing may be performed using an appropriate stirrer or disperser. From the viewpoint of improving the dispersibility of the negative electrode active material, kneading may be performed at a relatively low solid content concentration, and then a solvent may be further mixed to lower the solid content concentration.
[0075] <Negative electrode for non-aqueous secondary battery> A negative electrode (negative electrode for non-aqueous secondary battery) according to one embodiment of the present invention includes a negative electrode mixture layer containing a negative electrode active material and a graft copolymer. This negative electrode mixture layer is typically formed using the above-described slurry composition, and specifically, may be formed from a dried product of the above-described slurry composition. Therefore, the negative electrode mixture layer may contain components (solids) other than the solvent among the components contained in the slurry composition. Therefore, the negative electrode mixture layer may further contain any component in combination with the negative electrode active material and the graft copolymer. The quantitative ratio of each component contained in the negative electrode mixture layer is typically the same as the quantitative ratio of each component in the slurry composition.
[0076] The amount per unit area of the negative electrode mixture layer is not particularly limited, but is preferably 7.0 mg / cm 2 More preferably, 7.2 mg / cm 2 More preferably, 7.4 mg / cm 2 or more, preferably 7.6 mg / cm 2 The following is the result.
[0077] The density of the negative electrode mixture layer is not particularly limited, but is preferably 1.60 g / cm 3 More preferably, 1.62 g / cm 3 More preferably, 1.65 g / cm 3 or more, preferably 1.70 g / cm 3 or less, more preferably 1.68 g / cm 3 More preferably, 1.66 g / cm or less 3 The following is the result.
[0078] The thickness of the negative electrode mixture layer is not particularly limited, but is preferably 46.3 μm or less, more preferably 45.8 μm or less, even more preferably 44.8 μm or less, preferably 43.6 μm or less, more preferably 44.0 μm or less, even more preferably 44.5 μm or less.
[0079] Typically, a negative electrode composite layer containing the above-described graft copolymer can have high mechanical strength. In one example, when a strength measurement test described below is performed, the composite layer strength of the negative electrode composite layer is preferably 50 N / m or more, more preferably 100 N / m or more, and even more preferably 150 N / m or more. The upper limit of the composite layer strength is not particularly limited, but can be, for example, 900 N / m.
[0080] In the strength measurement test, one side of the negative electrode composite layer is attached to a flat support surface of a test table via double-sided adhesive tape with sufficiently high adhesive strength. Then, a rectangular adhesive tape with sufficiently high adhesive strength is attached to the other side of the negative electrode composite layer. One end of the rectangular adhesive tape is pulled perpendicularly to the support surface and peeled off. The stress generated when peeling off the rectangular adhesive tape is the stress required for delamination of the negative electrode composite layer, and thus corresponds to the stress required to destroy the negative electrode composite layer. Therefore, the stress can be measured as the composite layer strength, which represents the mechanical strength of the negative electrode composite layer. Specifically, the strength measurement test can be performed using the method described in the "Method for Measuring Composite Layer Strength" section of the Examples below.
[0081] Typically, the negative electrode includes a current collector, and a negative electrode composite layer is formed on the current collector. The current collector is preferably made of a material that is electrically conductive and electrochemically durable. Examples of materials for the current collector include iron, copper, aluminum, nickel, stainless steel, titanium, tantalum, gold, and platinum. These materials may be used alone or in combination of two or more. Among these, the negative electrode current collector is preferably made of copper.
[0082] The negative electrode can be produced, for example, by the following methods: (1) applying a slurry composition to the surface of a current collector and then drying it; (2) immersing a current collector in a slurry composition and then drying it; and (3) applying a slurry composition to a release substrate and drying it to produce a negative electrode composite layer, and transferring the resulting negative electrode composite layer to the surface of a current collector.
[0083] Among these, the method (1) is preferred because it is easy to control the thickness of the negative electrode composite layer. Specifically, the method (1) includes a step of applying a slurry composition onto a current collector (application step), and a step of drying the slurry composition applied onto the current collector to form a negative electrode composite layer (drying step).
[0084] Examples of methods for applying the slurry composition onto the current collector include a doctor blade method, a dipping method, a reverse roll method, a direct roll method, a gravure method, an extrusion method, a brush coating method, etc. The slurry composition may be applied to only one surface or both surfaces of the current collector.
[0085] Examples of methods for drying the slurry composition applied to the current collector include drying with warm air, hot air, or low-humidity air; vacuum drying; and drying by irradiation with energy rays such as infrared rays and electron beams. By drying the slurry composition on the current collector, a negative electrode mixture layer can be formed on the current collector, thereby obtaining a negative electrode.
[0086] The method for producing a negative electrode may further include any optional step. For example, the method for producing a negative electrode may include a step of applying pressure to the negative electrode mixture layer after forming the negative electrode mixture layer on the current collector. The pressure treatment may be performed, for example, by a mold press or a roll press. The pressure treatment can improve the adhesion between the negative electrode mixture layer and the current collector or increase the density of the negative electrode mixture layer. Furthermore, when the negative electrode mixture layer contains a polymerizable component, the method for producing a negative electrode may include polymerizing the polymerizable component after forming the negative electrode mixture layer.
[0087] <Non-aqueous secondary battery> A secondary battery (non-aqueous secondary battery) according to one embodiment of the present invention includes the negative electrode, positive electrode, and electrolyte solution described above. The secondary battery may further include a separator.
[0088] The positive electrode may be a known positive electrode used as a positive electrode for a secondary battery. Specifically, the positive electrode may be, for example, a positive electrode including a current collector and a positive electrode composite layer formed on the current collector. The positive electrode current collector may be, for example, one formed of a metal material such as aluminum. The positive electrode composite layer may be a layer containing a known positive electrode active material, a conductive material, and a binder, and a known polymer may be used as the binder.
[0089] As the electrolyte, an organic electrolyte solution in which a supporting electrolyte is dissolved in an organic solvent is usually used. For example, a lithium salt can be used as the supporting electrolyte of a lithium ion secondary battery. Examples of the lithium salt include LiPF 6 , LiAsF 6 , LiBF 4 , LiSbF 6 , LiAlCl 4 , LiClO 4 , C.F. 3 SO 3 Li, C 4 F 9 SO 3 Li, CF 3 COOLi, (CF 3 CO) 2 NLi, (CF 3 SO 2 ) 2 NLi, (C 2 F 5 SO 2 Among them, LiPF is particularly preferred because it is easily soluble in solvents and shows a high degree of dissociation. 6 , LiClO 4 , C.F. 3 SO 3 Li is preferred. The supporting electrolyte may be used alone or in combination of two or more. Generally, the lithium ion conductivity tends to increase as the supporting electrolyte has a higher degree of dissociation, so the lithium ion conductivity can be adjusted by the type of supporting electrolyte.
[0090] The organic solvent used in the electrolyte is not particularly limited as long as it can dissolve the supporting electrolyte. Suitable examples include carbonates such as dimethyl carbonate (DMC), ethylene carbonate (EC), diethyl carbonate (DEC), propylene carbonate (PC), butylene carbonate (BC), ethyl methyl carbonate (EMC), and vinylene carbonate (VC); esters such as γ-butyrolactone and methyl formate; ethers such as 1,2-dimethoxyethane and tetrahydrofuran; and sulfur-containing compounds such as sulfolane and dimethyl sulfoxide. Mixtures of these solvents may also be used. Among these, carbonates are preferred because of their high dielectric constant and wide stable potential range. Generally, the lower the viscosity of the solvent used, the higher the lithium ion conductivity, so the lithium ion conductivity can be adjusted by the type of solvent. The concentration of the electrolyte in the electrolyte can be adjusted as appropriate. The electrolyte may also contain any additive.
[0091] The separator is not particularly limited, and for example, the one described in JP 2012-204303 A can be used. Among these, a microporous film made of a polyolefin resin (polyethylene, polypropylene, polybutene, polyvinyl chloride) is preferred because it allows the thickness of the entire separator to be thin, thereby increasing the ratio of electrode active material in the secondary battery and increasing the capacity per volume.
[0092] A secondary battery including a negative electrode containing the above-described graft copolymer can achieve excellent cycle characteristics. In one example, when the capacity retention rate ΔC of the secondary battery is measured by the method described in the "Method for Evaluating Cycle Characteristics" in the Examples below, the capacity retention rate ΔC is preferably 75% or more, more preferably 80% or more.
[0093] A secondary battery can be produced, for example, by stacking a positive electrode and a negative electrode with a separator interposed therebetween, rolling or folding the resulting structure as necessary according to the battery shape, placing the resulting structure in a battery container, injecting an electrolyte into the battery container, and sealing the container. The secondary battery may be provided with an overcurrent prevention element such as a fuse or a PTC element, an expanded metal, a lead plate, or the like, as necessary, to suppress an increase in pressure inside the secondary battery and the occurrence of overcharging and overdischarging. The shape of the secondary battery may be any of, for example, a coin type, a button type, a sheet type, a cylindrical type, a rectangular type, a flat type, or the like.
[0094] The present invention will be described in detail below based on examples, but the present invention is not limited to these examples. In the following description, "%" and "parts" representing amounts are by weight unless otherwise specified. Furthermore, the operations described below were carried out in air at room temperature and normal pressure (25°C, 1 atm) unless otherwise specified.
[0095] <Method for measuring viscosity of 4 wt % aqueous polymer solution> An aqueous solution of 4 wt % polymer was prepared. The viscosity of this aqueous solution was measured using a Brookfield viscometer under the conditions of a temperature of 25°C, a rotation speed of 60 rpm, and a rotation time of 60 seconds.
[0096] <Method for measuring composite layer strength> A rectangular test piece measuring 100 mm in length and 10 mm in width was cut out from a negative electrode. Double-sided adhesive cellophane tape (specified in JIS Z 1522) was attached to the surface of the negative electrode composite layer of this test piece. The double-sided adhesive cellophane tape was attached to a test stand to fix the negative electrode composite layer to the test stand. One end of the current collector was pulled vertically at a pulling rate of 50 mm / min and peeled off.
[0097] Thereafter, a rectangular piece of cellophane tape measuring 80 mm in length and 8 mm in width was attached to the negative electrode composite layer remaining on the double-sided adhesive cellophane tape on the test bench. One end of the rectangular cellophane tape was pulled vertically at a pulling speed of 50 mm / min and peeled off, and the stress was measured. This measurement was performed three times, and the average stress value of the three measurements was obtained as the composite layer strength. The obtained composite layer strength was evaluated according to the following criteria. This composite layer strength represents the mechanical strength of the negative electrode composite layer, and the higher the strength, the better. Therefore, A indicates the best composite layer strength, and D indicates the worst composite layer strength. A: Composite layer strength is 150 N / m or more; B: Composite layer strength is 100 N / m or more but less than 150 N / m; C: Composite layer strength is 50 N / m or more but less than 100 N / m; D: Composite layer strength is less than 50 N / m
[0098] <Method for Evaluating Cycle Characteristics> After injecting the electrolyte, the lithium-ion secondary battery was left standing at 25°C for 5 hours. It was then charged to a cell voltage of 3.65 V at 25°C using a constant current method at 0.2 C, and then aged for 12 hours at 60°C. It was then discharged to a cell voltage of 3.00 V using a constant current method at 25°C and 0.2 C. It was then subjected to CC-CV (constant current-constant voltage) charging (upper limit cell voltage: 4.20 V) using a constant current method at 0.2 C, and CC discharged to 3.00 V using a constant current method at 0.2 C, and its initial discharge capacity X1 was measured. Next, 50 cycles of charge / discharge were performed at a temperature of 25°C, with a cell voltage of 4.20-3.00 V and a charge / discharge rate of 1.0 C. Thereafter, the cells were CC-CV charged (cell voltage 4.20 V) at a temperature of 25°C using a constant current method of 0.2 C, and then discharged to a cell voltage of 3.00 V using a constant current method of 0.2 C, and the discharge capacity X2 was measured. The capacity retention rate ΔC was calculated using the formula: ΔC = (X2 / X1) × 100 (%) and evaluated according to the following criteria. A indicates the best cycle characteristics, and D indicates the worst cycle characteristics. A: Capacity retention rate ΔC is 80% or more B: Capacity retention rate ΔC is 75% or more but less than 80% C: Capacity retention rate ΔC is 70% or more but less than 75% D: Capacity retention rate ΔC is less than 70%
[0099] Example 1 (1-1. Preparation of a Binder Composition for a Negative Electrode) 1,250 parts of ion-exchanged water was placed in a 10-L flask equipped with a septum, followed by 3.12 parts of polyvinyl alcohol (degree of polymerization: 1,500, degree of saponification: 88%) as a backbone polymer. The mixture was heated to 80°C to dissolve the polyvinyl alcohol. The flask was then purged with nitrogen gas at a flow rate of 100 mL / min. After the aqueous polyvinyl alcohol solution was returned to 25°C, 0.0208 parts (solids equivalent) of a 0.5% aqueous solution of sodium bisulfite was added to the flask using a syringe. 15 minutes later, 0.07 parts (solids equivalent) of a 0.5% aqueous solution of potassium persulfate as a polymerization initiator was added to the flask using a syringe and stirred at 25°C. Next, 24.22 parts of acrylic acid (AA) as an anionic monomer and 72.66 parts of acrylamide (AAm) as a non-anionic water-soluble monomer were added and stirred. Next, the 10 L flask containing the polyvinyl alcohol, monomer, and polymerization initiator was immersed in a 60°C water bath to initiate the polymerization reaction. After 1.5 hours, 0.25 parts (solids equivalent) of a 2.0% aqueous solution of potassium persulfate and 0.115 parts (solids equivalent) of a 5.0% aqueous solution of sodium bisulfite were added to the flask to further increase the reaction conversion. After another 2 hours, 0.25 parts (solids equivalent) of a 2.0% aqueous solution of ammonium persulfate and 0.115 parts (solids equivalent) of a 5.0% aqueous solution of sodium bisulfite were added to the flask.
[0100] The flask was then cooled to 40°C and placed under an air atmosphere. A 5.0% aqueous solution of lithium hydroxide was added to the flask to obtain an aqueous solution of the water-soluble graft copolymer having a pH of 8.0 as a binder composition for a negative electrode of a lithium ion secondary battery. Using this aqueous solution of the water-soluble graft copolymer, the viscosity of a 4 wt% aqueous solution of the water-soluble graft copolymer was measured by the method described above.
[0101] (1-2. Preparation of Negative Electrode Slurry Composition) 77.6 parts of artificial graphite (theoretical capacity: 360 mAh / g) and 19.4 parts of SiO (theoretical capacity: 1240 mAh / g) as negative electrode active materials, and 3.0 parts (solid content equivalent) of the above negative electrode binder composition having a solid content concentration of 4.0% were added to a planetary mixer to obtain a mixture. This mixture was diluted with ion-exchanged water to a solid content concentration of 60%. Thereafter, the mixture was kneaded for 60 minutes at a rotation speed of 45 rpm. Then, ion-exchanged water was added to the kneaded mixture so that the viscosity became 3500±100 mPa·s (measured with a Brookfield viscometer at 60 rpm), and a lithium-ion secondary battery negative electrode slurry composition was obtained. The solid content concentration of the negative electrode slurry composition was 45%.
[0102] (1-3. Preparation of Positive Electrode Slurry Composition) 100 parts of lithium cobalt oxide (theoretical capacity: 160 mAh / g) as a positive electrode active material, 3.16 parts of carbon black as a conductive material, and 2.0 parts (solid content equivalent) of an N-methylpyrrolidone solution of polyvinylidene fluoride (solid content concentration: 5.0%) were added to a planetary mixer to obtain a mixture. This mixture was diluted with ion-exchanged water to a solid content concentration of 60%. The mixture was then kneaded for 60 minutes at a rotation speed of 45 rpm. Ion-exchanged water was then added to the kneaded mixture to obtain a viscosity of 4000±300 mPa·s (measured with a Brookfield viscometer at 60 rpm), thereby obtaining a slurry composition for a lithium-ion secondary battery positive electrode. The solid content concentration of the positive electrode slurry composition was 50%.
[0103] (1-4. Production of Negative Electrode) The above-mentioned negative electrode slurry composition was applied to a copper foil (thickness: 15 μm) as a current collector using a comma coater in an amount of 7.4 mg / cm after drying. 2 ~7.6 mg / cm 2 The copper foil coated with the negative electrode slurry composition was then dried. The drying was carried out by conveying the coated copper foil at a speed of 1.0 m / min for 1 minute in an oven at a temperature of 100°C. The copper foil was then further heat-treated at a temperature of 120°C for 2 minutes to obtain a negative electrode blank. Next, the obtained negative electrode blank was pressed with a roll press to obtain a negative electrode composite layer with a density of 1.60 g / cm. 3 ~1.75g / cm 3The negative electrode was then pressed to obtain a negative electrode having a current collector and a negative electrode composite layer formed on one side of the current collector. The composite layer strength of this negative electrode was evaluated by the method described above.
[0104] (1-5. Preparation of Positive Electrode) The positive electrode slurry composition was applied to an aluminum foil (thickness: 20 μm) as a current collector using a comma coater in an amount of 24.5±0.5 mg / cm after drying. 2 The aluminum foil coated with the positive electrode slurry composition was then dried. The drying was carried out by transporting the aluminum foil coated with the positive electrode slurry composition in an oven at a temperature of 60°C for 2 minutes at a speed of 0.5 m / min. The aluminum foil was then further heat-treated at a temperature of 120°C for 2 minutes to obtain a positive electrode blank. Next, the obtained positive electrode blank was pressed with a roll press to obtain a positive electrode composite layer having a density of 3.10 g / cm. 3 ~3.20 g / cm 3 By pressing the current collector so as to obtain a positive electrode having a positive electrode mixture layer formed on one surface of the current collector.
[0105] (1-6. Preparation of Separator) A single-layer polypropylene separator (width 65 mm, length 500 mm, thickness 25 μm; produced by a dry method; porosity 55%) was prepared and cut into a 5 cm×5 cm square.
[0106] (1-7. Assembly of Lithium-ion Secondary Battery) An aluminum packaging exterior was prepared as the exterior of the battery. Then, the positive electrode was cut into a 4 cm x 4 cm square, and the surface of the positive electrode on the current collector side was placed in contact with the aluminum packaging exterior. Next, the square separator was placed on the surface of the positive electrode on the positive electrode composite layer side. Furthermore, the negative electrode was cut into a 4.2 cm x 4.2 cm square, and placed on the surface of the separator opposite the positive electrode composite layer side, with the surface on the negative electrode composite layer side facing the separator. Thereafter, LiPF 5 with a concentration of 1.0 M was added as an electrolyte. 6A solution (solvent: ethylene carbonate / ethyl methyl carbonate = 3 / 7 (volume ratio), additive: vinylene carbonate 2% (solvent ratio)) was filled into the battery. Next, the aluminum packaging exterior was heat-sealed at 150°C to hermetically close the opening of the aluminum packaging exterior, thereby producing a lithium ion secondary battery. The cycle characteristics of this lithium ion secondary battery were evaluated by the method described above.
[0107] Example 2 In producing the negative electrode binder composition in step (1-1), the amount (solid content equivalent) of a 0.5% aqueous solution of potassium persulfate as a polymerization initiator added before starting the polymerization reaction was changed from 0.07 parts to 0.208 parts, and the amount (solid content equivalent) of a 5.0% aqueous solution of sodium hydrogensulfite was changed from 0.0208 parts to 0.0624 parts. Except for this, a negative electrode binder composition, a negative electrode slurry composition, a positive electrode slurry composition, a negative electrode, a positive electrode, a separator, and a secondary battery were produced and evaluated in the same manner as in Example 1.
[0108] Example 3 In the production of the negative electrode binder composition in step (1-1), the amount (solid content equivalent) of a 0.5% aqueous solution of potassium persulfate as a polymerization initiator added before the polymerization reaction was changed from 0.07 parts to 0.208 parts, and the amount (solid content equivalent) of a 5.0% aqueous solution of sodium hydrogen sulfite was changed from 0.0208 parts to 0.0624 parts. The amounts of the monomers used were changed to 6.25 parts of polyvinyl alcohol (PVA, polymerization degree 1500, saponification degree 88%), 23.44 parts of acrylic acid (AA), and 70.31 parts of acrylamide (AAm). Except for the above, the negative electrode binder composition, negative electrode slurry composition, positive electrode slurry composition, negative electrode, positive electrode, separator, and secondary battery were produced and evaluated in the same manner as in Example 1.
[0109] Example 4 In the production of the negative electrode binder composition in step (1-1), the amount (solid content equivalent) of a 0.5% aqueous solution of potassium persulfate as a polymerization initiator added before the polymerization reaction was changed from 0.07 parts to 0.208 parts, and the amount (solid content equivalent) of a 5.0% aqueous solution of sodium hydrogen sulfite was changed from 0.0208 parts to 0.0624 parts. The amounts of the monomers used were changed to 15.00 parts of polyvinyl alcohol (PVA, polymerization degree 1500, saponification degree 88%), 21.3 parts of acrylic acid (AA), and 63.7 parts of acrylamide (AAm). Except for the above, the negative electrode binder composition, negative electrode slurry composition, positive electrode slurry composition, negative electrode, positive electrode, separator, and secondary battery were produced and evaluated in the same manner as in Example 1.
[0110] Example 5 In producing the negative electrode binder composition in step (1-1), the amount (solid content equivalent) of a 0.5% aqueous solution of potassium persulfate as a polymerization initiator added before starting the polymerization reaction was changed from 0.07 parts to 0.625 parts, and the amount (solid content equivalent) of a 5.0% aqueous solution of sodium hydrogensulfite was changed from 0.0208 parts to 0.186 parts. Except for this, a negative electrode binder composition, a negative electrode slurry composition, a positive electrode slurry composition, a negative electrode, a positive electrode, a separator, and a secondary battery were produced and evaluated in the same manner as in Example 1.
[0111] Example 6 In the production of the negative electrode binder composition in step (1-1), the amount (solid content equivalent) of a 0.5% aqueous solution of potassium persulfate as a polymerization initiator added before the polymerization reaction was changed from 0.07 parts to 0.625 parts, and the amount (solid content equivalent) of a 5.0% aqueous solution of sodium hydrogen sulfite was changed from 0.0208 parts to 0.186 parts. The amounts of the monomers used were changed to 6.25 parts of polyvinyl alcohol (PVA, polymerization degree 1500, saponification degree 88%), 23.44 parts of acrylic acid (AA), and 70.31 parts of acrylamide (AAm). Except for the above, the negative electrode binder composition, negative electrode slurry composition, positive electrode slurry composition, negative electrode, positive electrode, separator, and secondary battery were produced and evaluated in the same manner as in Example 1.
[0112] Example 7 In the production of the negative electrode binder composition in step (1-1), the amount (solid content equivalent) of a 0.5% aqueous solution of potassium persulfate as a polymerization initiator added before the polymerization reaction was changed from 0.07 parts to 0.625 parts, and the amount (solid content equivalent) of a 5.0% aqueous solution of sodium hydrogen sulfite was changed from 0.0208 parts to 0.186 parts. The amounts of the monomers used were changed to 15.00 parts of polyvinyl alcohol (PVA, polymerization degree 1500, saponification degree 88%), 21.3 parts of acrylic acid (AA), and 63.7 parts of acrylamide (AAm). Except for the above, the negative electrode binder composition, negative electrode slurry composition, positive electrode slurry composition, negative electrode, positive electrode, separator, and secondary battery were produced and evaluated in the same manner as in Example 1.
[0113] Example 8 A negative electrode binder composition, a negative electrode slurry composition, a positive electrode slurry composition, a negative electrode, a positive electrode, a separator, and a secondary battery were produced and evaluated in the same manner as in Example 1, except that in producing the negative electrode binder composition in step (1-1), 3.12 parts of polyvinyl alcohol (PVA, degree of polymerization 2500, degree of saponification 88%) was used as the trunk polymer instead of 3.12 parts of polyvinyl alcohol (PVA, degree of polymerization 1500, degree of saponification 88%).
[0114] Example 9 A negative electrode binder composition, a negative electrode slurry composition, a positive electrode slurry composition, a negative electrode, a positive electrode, a separator, and a secondary battery were produced and evaluated in the same manner as in Example 1, except that in producing the negative electrode binder composition in step (1-1), 3.12 parts of polyvinyl alcohol (PVA, degree of polymerization 2500, degree of saponification 98%) was used instead of 3.12 parts of polyvinyl alcohol (PVA, degree of polymerization 1500, degree of saponification 88%) as the trunk polymer.
[0115] Example 10 A negative electrode binder composition, a negative electrode slurry composition, a positive electrode slurry composition, a negative electrode, a positive electrode, a separator, and a secondary battery were produced and evaluated in the same manner as in Example 1, except that 24.22 parts of methacrylic acid (MAA) was used instead of 24.22 parts of acrylic acid (AA) in producing the negative electrode binder composition in step (1-1).
[0116] Comparative Example 1: 1,250 parts of ion-exchanged water was placed in a 10-L flask equipped with a septum and heated to 40°C. The atmosphere in the flask was replaced with nitrogen gas at a flow rate of 100 mL / min. Next, 75.0 parts of acrylamide (AAm) as a non-anionic water-soluble monomer and 25.0 parts of acrylic acid (AA) as an anionic monomer were mixed and injected into the flask with a syringe. Then, 0.07 parts (solids equivalent) of a 0.5% aqueous solution of sodium bisulfite was added to the flask with a syringe. 15 minutes later, 0.02 parts (solids equivalent) of a 0.5% aqueous solution of ammonium persulfate as a polymerization initiator was added to the flask with a syringe to initiate the polymerization reaction. After 2 hours, in order to further increase the reaction conversion rate, 0.25 parts (solids equivalent) of a 2.0% aqueous solution of ammonium persulfate and 0.115 parts (solids equivalent) of a 5.0% aqueous solution of sodium hydrogen sulfite were added to the flask, and the reaction temperature was raised to 55° C. After another 2 hours, 0.25 parts (solids equivalent) of a 2.0% aqueous solution of ammonium persulfate and 0.115 parts (solids equivalent) of a 5.0% aqueous solution of sodium hydrogen sulfite were added to the flask.
[0117] The flask was then cooled to 40°C and placed under an air atmosphere. A 5.0% aqueous solution of lithium hydroxide was added to the flask to obtain an aqueous solution of a water-soluble polymer having a pH of 8.0 as a binder composition for a negative electrode. Using this aqueous solution of the water-soluble polymer, the viscosity of a 4 wt% aqueous solution of the water-soluble polymer was measured by the method described above.
[0118] A slurry composition for an anode, a slurry composition for a cathode, an anode, a cathode, a separator, and a secondary battery were produced and evaluated in the same manner as in Example 1, except that the aqueous solution of the water-soluble polymer produced in Comparative Example 1 was used as the binder composition for an anode instead of the aqueous solution of the water-soluble graft copolymer produced in Example 1.
[0119] Comparative Example 2 A negative electrode binder composition, a negative electrode slurry composition, a positive electrode slurry composition, a negative electrode, a positive electrode, a separator, and a secondary battery were produced and evaluated in the same manner as in Example 1, except that, in producing the negative electrode binder composition in step (1-1), the amount of polyvinyl alcohol (PVA, degree of polymerization 1500, degree of saponification 88%) was changed to 3.22 parts, the amount of acrylic acid (AA) was changed to 96.78 parts, and acrylamide (AAm) was not used.
[0120] Comparative Example 3 A negative electrode binder composition, a negative electrode slurry composition, a positive electrode slurry composition, a negative electrode, a positive electrode, a separator, and a secondary battery were produced and evaluated in the same manner as in Example 1, except that, in producing the negative electrode binder composition in step (1-1), the amount of polyvinyl alcohol (PVA, degree of polymerization 1500, degree of saponification 88%) was changed to 3.22 parts, the amount of acrylamide (AAm) was changed to 96.78 parts, and acrylic acid (AA) was not used.
[0121] Comparative Example 4 A 4 wt % aqueous solution of the water-soluble polymer produced in Comparative Example 1 and polyvinyl alcohol (degree of polymerization 1500, degree of saponification 88%) were mixed in a weight ratio of 96.88:3.12, and then stirred for 20 minutes at 400 rpm in a planetary centrifugal mixer to produce a polymer mixed solution as a binder composition for a negative electrode. Using this polymer mixed solution, the viscosity of a 4 wt % aqueous solution of the polymer was measured by the method described above. In Comparative Example 4, the concentration of the 4 wt % aqueous solution of the polymer, "4%," represents the total concentration of the water-soluble polymer produced in Comparative Example 1 and polyvinyl alcohol.
[0122] A slurry composition for an anode, a slurry composition for a cathode, an anode, a cathode, a separator, and a secondary battery were produced and evaluated in the same manner as in Example 1, except that the polymer mixed solution produced in Comparative Example 4 was used as the binder composition for an anode instead of the aqueous solution of the water-soluble graft copolymer produced in Example 1.
[0123] <Results> The results of the above-mentioned Examples and Comparative Examples are shown in the table below. In the table below, the abbreviations have the following meanings: PVA: Polyvinyl alcohol AA: Acrylic acid MAA: Methacrylic acid AAm: Acrylamide
[0124]
[0125]
Claims
1. A binder composition for a non-aqueous secondary battery negative electrode, comprising a graft copolymer, the graft copolymer comprising a trunk polymer containing a hydroxyl group, and a branch polymer containing a monomer unit containing an anionic group and a water-soluble monomer unit not containing an anionic group, the branch polymer being bonded to the trunk polymer.
2. The binder composition for a non-aqueous secondary battery negative electrode according to claim 1, wherein the weight ratio of the monomer unit containing an anionic group to the water-soluble monomer unit not containing an anionic group (monomer unit containing an anionic group / water-soluble monomer unit not containing an anionic group) is 10 / 90 or more and 50 / 50 or less.
3. The binder composition for a negative electrode of a non-aqueous secondary battery according to claim 1, wherein the ratio of the trunk polymer to 100% by weight of the graft copolymer is 3.0% by weight or more and 20% by weight or less.
4. The binder composition for a negative electrode of a non-aqueous secondary battery according to claim 1, wherein the trunk polymer contains a hydroxyl group-containing unsaturated aliphatic unit.
5. The binder composition for a non-aqueous secondary battery negative electrode according to claim 1, wherein the branch polymer contains an ethylenically unsaturated monocarboxylic acid unit.
6. The binder composition for a non-aqueous secondary battery negative electrode according to claim 1, wherein the branch polymer contains an unsaturated carboxylic acid amide unit.
7. The binder composition for a non-aqueous secondary battery negative electrode according to claim 1, which contains water.
8. A slurry composition for a non-aqueous secondary battery negative electrode, comprising a negative electrode active material and the binder composition for a non-aqueous secondary battery negative electrode according to any one of claims 1 to 7.
9. The slurry composition for a non-aqueous secondary battery negative electrode according to claim 8, wherein the negative electrode active material comprises a silicon-based negative electrode active material.
10. A negative electrode for a non-aqueous secondary battery, comprising a negative electrode mixture layer containing a negative electrode active material and a graft copolymer, the graft copolymer comprising a trunk polymer containing a hydroxyl group, and a branch polymer containing a monomer unit containing an anionic group and a water-soluble monomer unit not containing an anionic group bonded to the trunk polymer.
11. A non-aqueous secondary battery comprising a positive electrode, the negative electrode for a non-aqueous secondary battery according to claim 10, and an electrolyte.
Citation Information
Patent Citations
Composition for power storage device, slurry for power storage device electrode, power storage device electrode, and power storage device
JP2021039861A
Graft copolymer and use thereof
JP2022074127A