Positive-electrode mix, production method for positive-electrode mix, and lithium-ion battery
The combination of titanium polysulfide with a glass-ceramic solid electrolyte in the positive electrode composite material enhances lithium ion battery discharge capacity and conductivity, addressing limitations in existing titanium polysulfide-based batteries.
Patent Information
- Application Number
- PCT/JP2024/010947
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-29
- Filing Date
- 2024-03-21
- Publication Date
- 2024-10-03
AI Technical Summary
Lithium ion batteries using titanium polysulfide as the positive electrode material have limited discharge capacity, and existing solutions with solid electrolytes either have low ionic conductivity or structural limitations that hinder further improvements.
A positive electrode composite material is developed by combining titanium polysulfide with a specific glass-ceramic solid electrolyte, which includes a sulfide solid electrolyte with a diffraction peak at 2θ = 20.1±0.4° in X-ray diffraction, and optimized composition ratios of titanium sulfide, sulfide solid electrolyte, and conductive additives to enhance lithium ion conductivity and discharge capacity.
The composite material significantly increases the discharge capacity of lithium ion batteries compared to similar solid electrolytes, maintaining high ionic conductivity and structural integrity, leading to a more efficient energy storage solution.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002 
Figure 00000030_0000
Abstract
Description
Positive electrode mixture, method for producing the positive electrode mixture, and lithium ion battery
[0001] The present invention relates to a positive electrode composite, a method for producing the positive electrode composite, and a lithium ion battery.
[0002] In order to increase the energy density of lithium-ion batteries, the use of sulfur as a positive electrode active material has been investigated. Since sulfur is an insulating material, a technique for providing electronic conductivity by compounding it with a metal sulfide has been investigated. For example, titanium polysulfide (TiS), which is a compound of titanium disulfide and sulfur, has been investigated. x : 2<x<10) has been developed as a positive electrode active material for lithium secondary batteries (Patent Document 1).
[0003] It is also known that titanium polysulfide and a solid electrolyte are combined to enhance the lithium ion conductivity of the positive electrode. Sulfide solid electrolytes have been investigated as a composite solid electrolyte (Patent Document 1 and Non-Patent Document 1). Because sulfide solid electrolytes are softer than oxide solid electrolytes, compacting the electrode layer and solid electrolyte layer can form a low-resistance electrode-electrolyte interface.
[0004] JP 2014-093210 A
[0005] Solid State Ionics 262 (2014) 143-146
[0006] Lithium-ion batteries using titanium polysulfide in the positive electrode do not have a large discharge capacity, and further improvement is required.
[0007] One object of the present invention is to provide a positive electrode mixture using titanium polysulfide that can provide a lithium ion battery with a large discharge capacity.
[0008] The present inventors discovered that a lithium-ion battery with a large discharge capacity can be obtained by using a cathode composite that combines titanium polysulfide with a specific glass-ceramic solid electrolyte, and completed the present invention. The use of the specific glass-ceramic solid electrolyte results in a lithium-ion battery with a large discharge capacity, even compared to solid electrolytes with the same specific element composition or solid electrolytes with the same ionic conductivity.
[0009] According to the present invention, the following positive electrode mixtures can be provided: 1. Titanium sulfide TiS x 1. A cathode composite comprising at least one of titanium sulfide (2<x<10) and a discharge product of the titanium sulfide, and a sulfide solid electrolyte having a diffraction peak at 2θ of 20.1±0.4° in X-ray diffraction using CuKα radiation. 2. The cathode composite according to 1, wherein the sulfide solid electrolyte contains lithium, phosphorus, sulfur, and a halogen as constituent elements. 3. The cathode composite according to 1 or 2, wherein a content of lithium relative to all constituent elements of the sulfide solid electrolyte is 35 to 45 mol%. 4. The cathode composite according to any one of 1 to 3, wherein a content of the titanium sulfide, b content of the sulfide solid electrolyte, and c content of the conductive additive satisfy the following formulas (1) to (3): 10% by mass≦a≦90% by mass (1) 0% by mass<b≦65% by mass (2) 0% by mass≦c≦40% by mass (3) (a+b+c is 100% by mass). 5. The positive electrode composite according to any one of 1 to 4, having, in X-ray diffraction using CuKα rays, a diffraction peak at 2θ of 20.1±0.4°, a diffraction peak at 2θ of 34±1°, and one or more diffraction peaks at 2θ selected from 15.5±1°, 44±1°, and 54±1°. 6. The positive electrode composite according to 4, wherein the content c of the conductive additive is 0% by mass. 7. A titanium sulfide TiS that satisfies the following (A): x (2<x<10) with a sulfide solid electrolyte that satisfies the following (B): (A) In X-ray diffraction using CuKα radiation, the sulfide solid electrolyte has a diffraction peak at 2θ of 34±1° and one or more diffraction peaks at 2θ selected from 15.5±1°, 44±1°, and 54±1°. (B) In X-ray diffraction using CuKα radiation, the sulfide solid electrolyte has a diffraction peak at 2θ of 20.1±0.4°. 8. The manufacturing method according to 7, wherein the sulfide solid electrolyte has an average particle size of 10 μm or less. 9. The manufacturing method according to 7 or 8, comprising a step of mechanically mixing sulfur and titanium disulfide to synthesize the titanium sulfide. 10. A cathode mixture obtained by the manufacturing method according to any one of 7 to 9. 11. A cathode comprising the cathode mixture according to any one of 1 to 6 and 10. 12. A lithium ion battery comprising the cathode according to 11.
[0010] According to the present invention, it is possible to provide a positive electrode mixture using titanium polysulfide, which can provide a lithium ion battery with a large discharge capacity.
[0011] 1 shows X-ray diffraction (XRD) charts of sulfide solid electrolyte powder A, the cathode composite of Example 1, sulfide solid electrolyte powder C, and the cathode composite of Comparative Example 2. 1 shows XRD charts of sulfide solid electrolyte powder B and the cathode composite produced in Comparative Example 1. 1 shows XRD charts of the cathode composite produced in Example 2. 1 shows XRD charts of sulfur, titanium disulfide, cathode active material B, and cathode active material C. 1 shows XRD charts of sulfide solid electrolyte powder D. 1 shows XRD charts of the cathode composite produced in Example 3. 1 shows XRD charts of the cathode composite produced in Example 4. 1 shows XRD charts of the cathode composites produced in Examples 5 to 7.
[0012] Hereinafter, an embodiment of the present invention (hereinafter, sometimes referred to as "the present embodiment") will be described. In this specification, the upper and lower limit values of a range expressed as "greater than or equal to," "less than or equal to," and "to" can be arbitrarily combined, and the numerical values in the examples can also be used as the upper and lower limit values.
[0013] 1. Positive Electrode Composite The positive electrode composite according to one embodiment of the present invention is made of titanium sulfide TiS x (2<x<10) and at least one of the discharge products of the titanium sulfide (hereinafter, titanium sulfide and its discharge products may be collectively referred to as titanium polysulfide), and a sulfide solid electrolyte having a diffraction peak at 2θ of 20.1±0.4° in X-ray diffraction using CuKα rays.
[0014] The sulfide solid electrolyte is a glass ceramic that exhibits a peak at a predetermined position in powder X-ray diffraction (XRD) measurement. By combining the sulfide solid electrolyte with titanium polysulfide, a cathode composite is obtained that can be used to obtain a lithium-ion battery with a large discharge capacity. The components of the cathode composite of this embodiment are described below.
[0015] [Sulfide Solid Electrolyte] The sulfide solid electrolyte used in this embodiment is a glass ceramic having a diffraction peak at 2θ of 20.1±0.4° in XRD measurement. In the present application, a glass ceramic solid electrolyte refers to a solid electrolyte in which a peak derived from the solid electrolyte is observed in XRD measurement, regardless of whether or not a peak derived from the raw material of the solid electrolyte is present. That is, a glass ceramic solid electrolyte includes a crystalline structure derived from the solid electrolyte, and the crystalline structure may be partially or entirely derived from the solid electrolyte. Furthermore, as long as the glass ceramic solid electrolyte has the X-ray diffraction pattern described above, it may also contain an amorphous component (also referred to as a "glass component") in part. The glass ceramic solid electrolyte includes so-called glass ceramics obtained by heating an amorphous solid electrolyte (glass component) above its crystallization temperature.
[0016] In this embodiment, the peak attributable to the solid electrolyte is a diffraction peak at 2θ = 20.1 ± 0.4°. In addition, diffraction peaks at 2θ = 23.5 ± 0.4°, 37.1 ± 0.8°, and 40.7 ± 0.8° can also be used as peaks attributable to the solid electrolyte to identify a sulfide solid electrolyte. Note that it is not necessary to observe all of the above peaks; the solid electrolyte may be identified by the diffraction peak at 2θ = 20.1 ± 0.4° and at least one other peak.
[0017] In one embodiment, the sulfide solid electrolyte contains lithium, phosphorus, sulfur, and a halogen as constituent elements. The halogen (X) preferably contains one or more selected from fluorine (F), chlorine (Cl), bromine (Br), and iodine (I), and more preferably contains Br or I. The halogen (X) preferably contains I.
[0018] The types and molar ratios of the constituent elements of the sulfide solid electrolyte can be confirmed, for example, by an ICP atomic emission spectrometer. The molar ratio of the constituent elements of the sulfide solid electrolyte can be adjusted by controlling the raw material blending. The molar ratio of the constituent elements in the raw materials is approximately equal to the molar ratio of the constituent elements of the resulting sulfide solid electrolyte.
[0019] The sulfide solid electrolyte of the present embodiment can be produced, for example, by mixing and pulverizing starting materials for a known lithium ion sulfide solid electrolyte so that the molar ratios of the constituent elements satisfy a predetermined range, vitrifying the mixture, and further converting the mixture into a ceramic by heat treatment.
[0020] As raw materials for the sulfide solid electrolyte, two or more compounds or simple substances containing lithium, phosphorus, sulfur, and a halogen as constituent elements can be used in combination, and any compound or simple substance can be used without particular limitation as long as it exhibits ionic conductivity due to the contained metal atoms.
[0021] Examples of raw materials containing lithium (Li) include lithium sulfide (Li 2 S), lithium oxide (Li 2 O), lithium carbonate (Li 2 CO 3 Among these, lithium compounds are preferred, and lithium sulfide is more preferred.
[0022] The lithium sulfide can be used without any particular limitation, but high purity lithium sulfide is preferred. Lithium sulfide can be produced by the methods described in, for example, JP-A-7-330312, JP-A-9-283156, JP-A-2010-163356, and JP-A-2011-84438.
[0023] Specifically, lithium hydroxide and hydrogen sulfide are reacted in a hydrocarbon organic solvent at 70°C to 300°C to produce lithium hydrosulfide, and then this reaction solution is dehydrosulfided, thereby synthesizing lithium sulfide (JP 2010-163356 A).
[0024] Alternatively, lithium sulfide can be synthesized by reacting lithium hydroxide with hydrogen sulfide in an aqueous solvent at 10°C to 100°C to produce lithium hydrosulfide, and then dehydrosulfiding the reaction solution (JP 2011-84438 A).
[0025] Examples of raw materials containing phosphorus (P) include diphosphorus trisulfide (P 2 S 3 ), diphosphorus pentasulfide (P 2 S5 ) and other phosphorus sulfides, sodium phosphate (Na 3 P.O. 4 Among these, phosphorus sulfide is preferred, and diphosphorus pentasulfide (P 2 S 5 ) is more preferred. 2 S 5 The phosphorus compounds such as ammonium nitrate, ...
[0026] The raw material containing halogen (X) preferably contains, for example, a halogen compound represented by the following formula: l -X m
[0027] In the formula, M represents sodium (Na), lithium (Li), boron (B), aluminum (Al), silicon (Si), phosphorus (P), sulfur (S), germanium (Ge), arsenic (As), selenium (Se), tin (Sn), antimony (Sb), tellurium (Te), lead (Pb), bismuth (Bi), or any of these elements bonded to an oxygen element or a sulfur element, and is preferably lithium (Li) or phosphorus (P), and more preferably lithium (Li).
[0028] X is a halogen element selected from fluorine (F), chlorine (Cl), bromine (Br), and iodine (I).
[0029] Furthermore, l is an integer of 1 or 2, and m is an integer of 1 to 10. When m is an integer of 2 to 10, that is, when there are multiple Xs, the Xs may be the same or different. For example, in the case of SiBrCl 3 In the formula, m is 4 and X is composed of two different elements, Br and Cl.
[0030] Specific examples of the halogen compounds represented by the above formula include sodium halides such as NaI, NaF, NaCl, and NaBr; lithium halides such as LiF, LiCl, LiBr, and LiI; and BCl. 3 , BBr 3 , B.I. 3 Boron halides such as AlF 3, AlBr 3 , AlI 3 , AlCl 3 aluminum halides such as SiF 4 , SiCl 4 , SiCl 3 , Si 2 Cl 6 , SiBr 4 , SiBrCl 3 , SiBr 2 Cl 2 , SiI 4 Silicon halides such as PF 3 , P.F. 5 , PCl 3 , PCl 5 , POCl 3 , PBr 3 , POBr 3 , P.I. 3 , P 2 Cl 4 , P 2 I 4 Phosphorus halides such as SF 2 , SF 4 , SF 6 , S 2 F 10 , SC1 2 , S 2 Cl 2 , S 2 Br 2 sulfur halides such as GeF 4 , GeCl 4 , GeBr 4 , GeI 4 , GeF 2 , GeCl 2 , GeBr 2 , GeI 2 Germanium halides such as AsF 3 , AsCl 3 , AsBr 3 , AsI 3 , AsF 5 arsenic halides such as SeF 4 , SeF 6 , SeCl 2 , SeCl 4 , Se 2 Br 2 , SeBr 4 selenium halides such as SnF4 , SnCl 4 , SnBr 4 , SnI 4 , SnF 2 , SnCl 2 , SnBr 2 , SnI 2 tin halides such as SbF 3 , SbCl 3 , SbBr 3 , SbI 3 , SbF 5 , SbCl 5 antimony halides such as TeF 4 , Te 2 F 10 , TeF 6 , TeCl 2 , TeCl 4 , TeBr 2 , TeBr 4 , TeI 4 Tellurium halides such as PbF 4 , PbCl 4 , PbF 2 , PbCl 2 , PbBr 2 , PbI 2 Lead halides such as BiF 3 , BiCl 3 , BiBr 3 , BiI 3 and the like.
[0031] Among these, lithium halides such as lithium chloride (LiCl), lithium bromide (LiBr), and lithium iodide (LiI), phosphorus pentachloride (PCl), 5 ), phosphorus trichloride (PCl 3 ), phosphorus pentabromide (PBr 5 ), phosphorus tribromide (PBr 3 Among them, lithium halides such as LiCl, LiBr, and LiI, PBr 3 is preferred, and lithium halides such as LiCl, LiBr, and LiI are more preferred, with LiI and LiBr being more preferred.
[0032] The halogen compound may be one of the above compounds alone or a combination of two or more of them, i.e., at least one of the above compounds can be used.
[0033] In this embodiment, the raw material contains a lithium compound, a phosphorus compound, and one or more halogen compounds, and at least one of the lithium compound and the phosphorus compound preferably contains elemental sulfur, and more preferably a combination of lithium sulfide, phosphorus sulfide, and one or more lithium halides.
[0034] For example, when lithium sulfide, diphosphorus pentasulfide, and lithium halide are used as raw materials for the sulfide solid electrolyte, the molar ratio of lithium sulfide to diphosphorus pentasulfide in the molar ratio of the input raw materials is preferably 65 to 85:15 to 35, more preferably 70 to 80:20 to 30, still more preferably 72 to 78:22 to 28, and particularly preferably 75:25.
[0035] In addition, the sulfide solid electrolyte is Li 2 S, P 2 S 5 When LiX is used as the raw material, the total content of lithium sulfide and diphosphorus pentasulfide ([Li 2 S+P 2 S 5 ]×100 / [Li 2 S+P 2 S 5 +LiX]) is preferably 60 to 95 mol %, more preferably 65 to 90 mol %, and even more preferably 70 to 85 mol %.
[0036] In one embodiment, the sulfide solid electrolyte has a lithium content of 35 to 45 mol % relative to all constituent elements, resulting in a cathode composite that can provide a battery with a large discharge capacity despite having a lower lithium content than a solid electrolyte having an argyrodite-type crystal structure, for example.
[0037] In this embodiment, mechanical stress is applied to the raw materials to cause a reaction and produce an intermediate (glass-like powder). Here, "applying mechanical stress" means mechanically applying shear force, impact force, or the like. Examples of means for applying mechanical stress include grinders such as planetary ball mills, vibration mills, and tumbling mills, and kneaders. The raw material powder is ground and mixed by applying strong mechanical stress until at least a portion of the powder can no longer maintain its crystallinity.
[0038] As for the conditions for pulverization and mixing, for example, when a planetary ball mill is used as the pulverizer, the rotation speed may be set to several tens to several hundreds of revolutions per minute, and the processing time may be set to 0.5 to 100 hours. More specifically, in the case of the planetary ball mill (manufactured by Fritsch: Model No. P-7) used in the examples of the present application, the rotation speed of the planetary ball mill is preferably 100 rpm or more and 500 rpm or less, and more preferably 150 rpm or more and 450 rpm or less. When zirconia balls are used as the pulverization media, for example, their diameter is preferably 0.2 to 20 mm. The temperature during pulverization is not particularly specified, but 200°C or less is preferred to prevent the solid electrolyte itself from crystallizing and hardening.
[0039] The intermediate produced by pulverization and mixing is subjected to a heat treatment. Specifically, the heating temperature of the intermediate is determined by subjecting the intermediate to simultaneous differential thermal and thermogravimetric analysis (TGDTA) at a temperature increase rate of 10°C / min using a TGDTA apparatus, and determining the peak top temperature (T c1 ) as a starting point, the temperature is preferably 5°C or lower, more preferably 10°C or lower, and even more preferably 15°C or lower, and there is no particular restriction on the lower limit, but it may be about −10°C or higher than the peak top temperature of the exothermic peak observed at the lowest temperature side. By setting the temperature in this range, the sulfide solid electrolyte (glass ceramic solid electrolyte) used in this embodiment can be obtained more efficiently.
[0040] The heating temperature for obtaining the glass ceramic solid electrolyte of this embodiment cannot be generally defined, but is generally preferably 250°C or lower, more preferably 225°C or lower, and even more preferably 200°C or lower. There is no particular lower limit, but the temperature is preferably 100°C or higher, more preferably 110°C or higher, and even more preferably 120°C or higher.
[0041] The heating time is not particularly limited as long as it is a time that allows a desired glass ceramic solid electrolyte to be obtained, but is, for example, preferably 10 minutes or more, more preferably 30 minutes or more, even more preferably 60 minutes or more, and even more preferably 2 hours or more. The upper limit of the heating time is not particularly limited, but is preferably 10 hours or less, more preferably 8 hours or less, even more preferably 6 hours or less, and even more preferably 4 hours or less.
[0042] The atmosphere for the heat treatment is not particularly limited, and may be a hydrogen sulfide atmosphere, an inert gas atmosphere such as nitrogen or argon, or a vacuum atmosphere.
[0043] [Titanium sulfide TiS x (2<x<10)] The titanium sulfide is not particularly limited, and known substances can be used. Specifically, crystalline TiS as a raw material disclosed in Patent Document 1 can be used. 2 and sulfur, and then mixing and pulverizing them by mechanical milling.
[0044] In one embodiment, the titanium sulfide is amorphous or crystalline. Crystalline titanium sulfide has, in X-ray diffraction using CuKα radiation, a diffraction peak at 2θ of 34±1° and one or more diffraction peaks at 2θ selected from 15.5±1°, 44±1°, and 54±1°. The diffraction peaks are derived from titanium disulfide crystals, and TiS 2 The diffraction peaks are at a diffraction angle of 2θ = 15.5 ± 1 ° based on the (001) plane of the crystal, at a diffraction angle of 2θ = 34 ± 1 ° based on the (011) plane, at a diffraction angle of 2θ = 44 ± 1 ° based on the (102) plane, and at a diffraction angle of 2θ = 54 ± 1 ° based on the (110) plane. The synthesis of titanium sulfide will be described later.
[0045] During the battery reaction, part or all of the titanium sulfide is converted into a discharge product. Therefore, in one embodiment, a titanium sulfide discharge product is present in the positive electrode composite (positive electrode). Examples of the titanium sulfide discharge product include a substance containing Li as an element, in which titanium sulfide is lithiated.
[0046] [Others] In one embodiment of the present invention, the positive electrode composite preferably further contains a conductive additive. The conductive additive may be any material that has electron conductivity. The conductive additive preferably has a large specific surface area and a plurality of pores. A carbon material having pores is particularly preferred. Carbon materials have high conductivity and are lighter than other conductive materials, so the output density and electrical capacity per unit weight of the battery can be increased.
[0047] The specific surface area of the conductive additive is 0.1 m 2 / g or more 5000m 2 / g or less, and more preferably 1m 2 / g or more 4000m 2 / g or less, and more preferably 1m 2 / g or more 3000m 2 / g or less, and most preferably 10m 2 / g or more 3000m 2 / g or less.
[0048] The pore volume of the conductive additive is preferably 0.1 cc / g or more and 5.0 cc / g or less. The pores of the conductive additive preferably have an average diameter of 0.1 nm or more and 40 nm or less, more preferably 0.5 nm or more and 40 nm or less, even more preferably 0.5 nm or more and 20 nm or less, and most preferably 1 nm or more and 20 nm or less.
[0049] The specific surface area, pore volume, and pore diameter of the conductive additive can be determined using a nitrogen adsorption isotherm obtained by adsorbing nitrogen gas to the conductive additive at liquid nitrogen temperature. Specifically, the specific surface area can be calculated using the nitrogen adsorption isotherm by the Brenauer-Emmet-Telle (BET) multipoint method. Furthermore, the pore volume and pore diameter can be determined using the nitrogen adsorption isotherm by the Barret-Joyner-Halenda (BJH) method. As a measuring device, for example, a specific surface area and pore distribution measuring device (Autosorb-3) manufactured by Quantacrome can be used for measurement.
[0050] The carbon material is not particularly limited, but examples thereof include carbon black such as ketjen black, acetylene black, denka black, thermal black, and channel black, mesoporous carbon, activated carbon, amorphous carbon, carbon nanotubes, vapor-grown carbon fiber (VGCF), and carbon nanohorns. Examples of conductive carbon materials include fullerene, carbon fiber, natural graphite, artificial graphite, graphene, graphene oxide, and reduced graphene oxide. Of these, activated carbon is preferred. These may be used alone or in combination of two or more. Composites of these may also be used.
[0051] In one embodiment, it is preferable that the titanium sulfide content a, the sulfide solid electrolyte content b, and the conductive additive content c in the positive electrode composite satisfy the following formulas (1) to (3): 10 mass%≦a≦90 mass% (1), 0 mass%<b≦65 mass% (2), and 0 mass%≦c≦40 mass% (3) (a+b+c is 100 mass%).
[0052] By satisfying formulas (1) to (3), a battery with a larger discharge capacity can be obtained. The titanium sulfide content a is more preferably 30% by mass or more, and even more preferably 60% by mass or more. Also, it is more preferably 85% by mass or less. The sulfide solid electrolyte content b is more preferably 10% by mass or more, and even more preferably 15% by mass or more. Also, it is more preferably 50% by mass or less. The conductive additive content c is more preferably 30% by mass or less, and even more preferably 10% by mass or less. It may also be 0% by mass. In other words, a high-performance positive electrode composite can be obtained without using a conductive additive.
[0053] In one embodiment, the positive electrode composite may or may not contain components other than the titanium polysulfide, sulfide solid electrolyte, and conductive additive described above. The other components are not particularly limited, and examples thereof include a binder, a solvent, and a dispersant. The positive electrode composite according to this embodiment can be produced, for example, by the method described below.
[0054] 2. Method for Producing a Positive Electrode Composite A method for producing a positive electrode composite according to one embodiment of the present invention comprises producing a titanium sulfide TiS that satisfies the following (A): x (2<x<10) with a sulfide solid electrolyte that satisfies the following (B): (A) In X-ray diffraction using CuKα radiation, the sulfide solid electrolyte has a diffraction peak at 2θ of 34±1° and one or more diffraction peaks at 2θ selected from 15.5±1°, 44±1°, and 54±1°. (B) In X-ray diffraction using CuKα radiation, the sulfide solid electrolyte has a diffraction peak at 2θ of 20.1±0.4°.
[0055] As described above, (A) above means that the titanium sulfide contains titanium disulfide crystals. (B) above means that the sulfide solid electrolyte is a predetermined glass ceramic. In this embodiment, by mixing the titanium sulfide and sulfide solid electrolyte described above, a positive electrode composite that can be used to obtain a lithium ion battery with a large discharge capacity can be produced.
[0056] In one embodiment, the titanium sulfide is synthesized by combining sulfur and titanium disulfide (TiS 2 The process includes mechanically mixing the TiS 2There is no particular limitation on TiS, and any commercially available TiS 2 It is particularly preferable to use high purity sulfur. There is no particular limitation on the sulfur used as a raw material, and sulfur of any crystal system can be used as long as it is solid at room temperature and normal pressure. TiS 2 The ratio of titanium to sulfur is set to be the same as the element ratio of titanium to sulfur in the target titanium polysulfide. x In the formula, x is preferably 3 or more or 4 or more, and is preferably 9 or less or 8 or less. More preferably, TiS x Mix so that x is 4 to 6.
[0057] The mechanical milling method can be carried out by mixing and grinding the raw materials using a mechanical grinding device such as a ball mill, a rod mill, a vibration mill, a disk mill, a hammer mill, a jet mill, a VIS mill, etc. In the mechanical milling method, TiS is obtained without proceeding to complete amorphization. 2 The treatment is carried out until a small amount of fine TiS crystals remain. 2 The crystalline state of can be confirmed by the position and half-width of the diffraction peak in XRD measurement.
[0058] In one embodiment, the active material-conductive additive composite material may be formed from the titanium sulfide and conductive additive described above, and then the sulfide solid electrolyte and the active material-conductive additive composite material may be mechanically mixed.
[0059] In this embodiment, the active material or the active material-conductive additive composite material and the sulfide solid electrolyte are mechanically mixed to form a positive electrode mixture. The active material, the active material-conductive additive composite material, and the sulfide solid electrolyte may be partially pulverized by this step.
[0060] For example, in the case of a planetary ball mill (manufactured by Fritsch: Model No. P-7), the rotation speed of the planetary ball mill is preferably 50 rpm or more and 500 rpm or less, and more preferably 80 rpm or more and 400 rpm or less. When zirconia balls are used as the grinding media, their diameter is preferably 0.2 to 20 mm.
[0061] In one embodiment, the sulfide solid electrolyte has an average particle size of 10 μm or less. This allows for sufficient ion conduction paths to be formed in the positive electrode, resulting in a battery with a large discharge capacity. The average particle size is more preferably 6 μm or less, and particularly preferably 3 μm or less. The average particle size refers to the median diameter (d50).
[0062] In one embodiment, it is preferable to adjust the titanium sulfide content a, the sulfide solid electrolyte content b, and the conductive additive content c in the positive electrode composite so as to satisfy the following formulas (1) to (3): 10 mass%≦a≦90 mass% (1) 0 mass%<b≦65 mass% (2) 0 mass%≦c≦40 mass% (3) (a+b+c is 100 mass%). By satisfying formulas (1) to (3), a battery with a larger discharge capacity can be obtained.
[0063] 3. Positive Electrode and Lithium-Ion Battery A positive electrode or lithium-ion battery according to one embodiment of the present invention includes the above-described positive electrode composite of the present invention. For example, an all-solid-state lithium-ion battery can be manufactured by using a solid electrolyte instead of a liquid electrolyte. By using the positive electrode composite of the present invention, an all-solid-state lithium-ion battery with a large discharge capacity can be manufactured.
[0064] An all-solid-state lithium-ion battery mainly comprises a positive electrode layer, a negative electrode layer, and an electrolyte layer, and the positive electrode composite of the present invention is suitable as a constituent material of the positive electrode layer. The negative electrode layer and the electrolyte layer can be manufactured by known methods. In addition to the positive electrode layer, the negative electrode layer, and the electrolyte layer, a current collector is preferably used, and a known current collector is also used. The solid electrolyte is not particularly limited, and a known solid electrolyte can be used.
[0065] The present invention will be specifically described below based on examples. The present invention is not limited to these examples. The evaluation methods for the samples prepared in each example are as follows. (1) Ion conductivity A 10 mm diameter (cross-sectional area S: 0.785 cm) sample was taken from the solid electrolyte. 2), and a height (L) of 0.1 to 0.3 cm were molded into a circular pellet to prepare a sample. Electrode terminals were attached to the top and bottom of the sample, and measurements were made at 25°C using an AC impedance method (frequency range: 1 MHz to 1 Hz, amplitude: 10 mV) to obtain a Cole-Cole plot. The real part Z' (Ω) at the point where -Z'' (Ω) is minimum near the right end of the arc observed in the high-frequency region was taken as the bulk resistance R (Ω) of the electrolyte, and the ionic conductivity σ (S / cm) was calculated according to the following formula: R = ρ (L / S) σ = 1 / ρ
[0066] (2) X-ray Diffraction (XRD) Measurement The properties of the sample and the presence or absence of diffraction peaks were analyzed by powder XRD measurement. If there were no diffraction peaks or only peaks derived from the raw materials, the sample was judged to be amorphous, and if there were diffraction peaks other than those derived from the raw materials, the sample was judged to be crystalline. Specifically, the sample powder was filled into a groove with a diameter of 20 mm and a depth of 0.2 mm and leveled with glass to prepare a sample. This sample was sealed with Kapton film for XRD and measured without exposing it to air. XRD measurement was performed using a powder X-ray diffractometer D2 PHASER manufactured by BRUKER Co., Ltd. under the following measurement conditions. [Measurement conditions] Tube voltage: 30 kV Tube current: 10 mA X-ray wavelength: Cu-Kα ray (1.5418 Å) Optical system: focusing method Slit configuration: Soller slit 4° (on both the incident and receiving sides), divergence slit 1 mm, Kβ filter (Ni plate 0.5%), air scatter screen 3 mm) Detector: semiconductor detector Measurement range: 2θ = 10-60 deg Step width, scan speed: 0.05 deg, 0.05 deg / sec
[0067] (3) Average Particle Size The median diameter (d50) of the solid electrolyte powder was measured using a laser diffraction / scattering particle size distribution analyzer (LA-960, manufactured by Horiba, Ltd.).
[0068] Example 1 (1) Preparation of Positive Electrode Active Material Powder (Titanium Sulfide) Titanium disulfide (TiS) was dissolved in a glove box under an argon atmosphere. 2The cation (C) powder and sulfur (S) powder were weighed out to a molar ratio of 1:2 and placed in a 45 mL zirconia pot together with 90 g of zirconia balls with a diameter of 4 mm. The pot was placed in a planetary ball mill (P7 Classic Line, manufactured by Fritsche), and mechanical milling was performed at 510 rpm for 50 hours to obtain a positive electrode active material powder A.
[0069] (2) Preparation of sulfide solid electrolyte In a glove box under an argon atmosphere, 0.4936 g of lithium sulfide, 0.7959 g of diphosphorus pentasulfide, and 0.2104 g of lithium iodide were placed in a 45 mL zirconia pot along with ten 10 mm diameter zirconia balls. The pot was placed in a planetary ball mill (Fritsche P7 Classic Line) and mechanical milling was performed at 370 rpm for 40 hours to obtain a powder. The obtained powder was heated at 195 ° C for 3 hours to obtain sulfide solid electrolyte powder A (glass ceramic). The ionic conductivity of sulfide solid electrolyte powder A was 3.8 mS cm -1 The average particle size d50 was 6 μm. FIG. 1 shows an XRD chart of sulfide solid electrolyte powder A (electrolyte A). Peaks derived from the solid electrolyte were observed at 2θ = 20.1°, 23.5°, 37.2°, and 40.7°.
[0070] (3) Preparation of Positive Electrode Composite Positive electrode active material powder A and acetylene black were weighed to a mass ratio of 50:50 and mixed for 5 minutes using an agate mortar. The obtained powder was sealed in a 45 mL zirconia pot together with 100 zirconia balls with a diameter of 5 mm and mixed in a planetary ball mill (Fritsche P7 Classic Line) at 370 rpm for 1 hour to obtain a composite of positive electrode active material and conductive additive. Subsequently, sulfide solid electrolyte powder A was added to the pot so that the mass ratio of the positive electrode active material and conductive additive composite was 50:50, and further mixed in a planetary ball mill at 100 rpm for 30 minutes to obtain a positive electrode composite. Figure 1 shows the XRD chart of the positive electrode composite (Example 1).
[0071] (4) All-solid-state lithium-ion battery In the method for producing an all-solid-state lithium-ion battery, a positive electrode composite was used as the working electrode, a sulfide-based solid electrolyte A was used as the electrolyte layer, and a lithium-indium alloy was used as the counter electrode. 5 mg of the positive electrode composite was used as the working electrode.
[0072] Comparative Example 1 (1) Preparation of Sulfide Solid Electrolyte In an argon-filled glove box, 4.1414 g of lithium sulfide, 4.1739 g of diphosphorus pentasulfide, and 1.7514 g of lithium chloride were placed in a 250 mL zirconia pot along with 40 10 mm diameter zirconia balls. The pot was placed in a planetary ball mill (Fritsche P5 Classic Line) and mechanically milled at 220 rpm for 40 hours. The resulting powder was heated at 430 °C for 2 hours. The resulting material was crushed in a mortar and then sieved through a 100 μm mesh size sieve. 2 g of the recovered powder, 18.2 g of toluene, and 34 g of 2 mm diameter zirconia balls were placed in a 45 mL zirconia pot. The pot was placed in a planetary ball mill (P7 Classic Line manufactured by Fritsche) and milled at 150 rpm for 17 minutes to obtain a slurry. The obtained slurry was vacuum dried at 120°C for 2 hours to obtain sulfide solid electrolyte powder B. The ionic conductivity of sulfide solid electrolyte powder B was 4.0 mScm. -1 The average particle size d50 was 6 μm. FIG. 2 shows an XRD chart of sulfide solid electrolyte powder B (electrolyte B). As a result of the XRD measurement, sulfide solid electrolyte powder B was an argyrodite-type sulfide solid electrolyte.
[0073] (2) Preparation of Cathode Composite and All-Solid-State Lithium-Ion Battery A cathode composite and an all-solid-state lithium-ion battery were prepared in the same manner as in Example 1, except that sulfide solid electrolyte A was changed to sulfide solid electrolyte B. FIG. 2 shows the results of XRD measurement of the cathode composite prepared in Comparative Example 1.
[0074] Comparative Example 2 (1) Preparation of Sulfide Solid Electrolyte In a glove box under an argon atmosphere, 0.5742 g of lithium sulfide and 0.9258 g of diphosphorus pentasulfide were sealed in a 45 mL zirconia pot together with ten 10 mm diameter zirconia balls. The pot was placed in a ball mill (Fritsche P7 Classic Line), and mechanical milling was performed at 370 rpm for 40 hours to obtain sulfide solid electrolyte powder C. The ionic conductivity of sulfide solid electrolyte powder C was 0.32 mScm. -1 The average particle size d50 was 6 μm. FIG. 1 shows an XRD chart of sulfide solid electrolyte powder C (electrolyte C). As a result of the XRD measurement, there were no clear diffraction peaks other than those due to the raw materials, and therefore it was confirmed that sulfide solid electrolyte powder C was glass.
[0075] (2) Preparation of Cathode Composite and All-Solid-State Lithium-Ion Battery A cathode composite and an all-solid-state lithium-ion battery were prepared in the same manner as in Example 1, except that the sulfide solid electrolyte A was changed to the sulfide solid electrolyte C. FIG. 1 shows an XRD chart of the cathode composite (Comparative Example 2).
[0076] [Evaluation of Battery Characteristics] The voltage range of the all-solid-state lithium ion batteries produced in the Examples and Comparative Examples was 0.9-2.4 V vs. Li-In, and the current density was 0.064 mA cm -2 The results are shown in Table 1. In the table, the positive electrode composite composition (TiS X : SE: C) represents titanium sulfide: sulfide solid electrolyte: conductive additive (mass ratio).
[0077]
[0078] In Comparative Example 1, sulfide solid electrolyte powder B (argyrodite-type sulfide solid electrolyte) having ionic conductivity equivalent to that of sulfide solid electrolyte powder A (glass ceramic) used in Example 1 was used. Furthermore, in Comparative Example 2, sulfide solid electrolyte powder C (glass) having a similar Li atom ratio was used. As a result, it was confirmed that the discharge capacity per gram of positive electrode composite of the all-solid-state lithium ion battery of Example 1 was large. It is believed that sulfide solid electrolyte powder C (glass) has lower lithium ion conductivity than sulfide solid electrolyte powder A (glass ceramic), resulting in a large lithium ion conduction resistance within the positive electrode composite, resulting in a smaller battery capacity. On the other hand, sulfide solid electrolyte powder B (argyrodite-type sulfide solid electrolyte) had a smaller capacity despite having lithium ion conductivity equivalent to that of the glass ceramic.
[0079] The cause is titanium polysulfide (TiS x The tendency of the solid electrolyte particles to break when combined with TiS and the ratio of Li elements contained in the solid electrolyte are thought to be factors that affect this. A crystalline solid electrolyte having an argyrodite-type crystal structure is composed only of crystalline components. x When stress is applied by the composite with TiS, the impact is uniformly applied to the entire solid electrolyte particle, increasing the stress, causing the solid electrolyte particle to crack and become smaller in particle size. The crystalline solid electrolyte having an argyrodite-type crystal structure with a reduced particle size is x When the lithium ions are combined with TiS, they come into sufficient contact with each other, increasing their reactivity. x In addition, the crystalline solid electrolyte having an argyrodite-type crystal structure has a large proportion of Li element, which increases the reactivity and x This is thought to be due to the supply of lithium ions to the positive electrode, which tends to decrease the lithium ion conductivity, increasing the lithium ion conduction resistance within the positive electrode mixture and reducing the discharge capacity.
[0080] On the other hand, glass ceramic solid electrolytes contain glass components, so TiS xEven if stress is applied to the composite with TiS, the glass component is distorted, so the increase in stress is suppressed and the particle size of the solid electrolyte is maintained. As a result, compared to the case of a crystalline solid electrolyte having an argyrodite-type crystal structure, TiS x Because there is insufficient contact with TiS x Therefore, lithium ion conductivity does not decrease. Furthermore, since the proportion of Li element is small in the glass ceramic solid electrolyte, it is assumed that the reactivity is low and the impact of the decrease in conductivity due to the supply of lithium ions is small. From the above, it is thought that the glass ceramic solid electrolyte suppresses the decrease in lithium ion conductivity and has a larger discharge capacity than a crystalline solid electrolyte with an argyrodite-type crystal structure.
[0081] Example 2 (1) Preparation of Positive Electrode Composite A positive electrode composite was prepared in the same manner as in Example 1, except that the mass ratio of the positive electrode active material powder A to acetylene black was changed to 87:13 to obtain a composite of the positive electrode active material and conductive additive, and the mass ratio of the sulfide solid electrolyte powder A to the composite of the active material and conductive additive was changed to 25:75.
[0082] (2) Fabrication and Evaluation of All-Solid-State Lithium-Ion Battery Except for using the positive electrode composite obtained in (1) above, an all-solid-state lithium-ion battery was fabricated and evaluated in the same manner as in Example 1. FIG. 3 shows an XRD chart of the positive electrode composite fabricated in Example 2.
[0083] Example 3 (1) Preparation of Positive Electrode Active Material Powder (Titanium Sulfide) Positive electrode active material powder B was obtained in the same manner as in Example 1 (1), except that the mechanical milling treatment time was changed to 5 hours. Figure 4 shows an XRD chart of positive electrode active material B (MM treatment for 5 hours). In addition, positive electrode active material C (MM treatment for 1 hour), sulfur (S) and titanium disulfide (TiS), which will be described later, were also prepared. 2 ) is shown in the XRD chart.
[0084] (2) Preparation of sulfide solid electrolyte 2 g of sulfide solid electrolyte powder A obtained in Example 1 (2), 7 g of cyclohexane, 1 g of diisopropyl ether, and 40 g of zirconia balls with a diameter of 0.3 mm were sealed in a 45 mL zirconia pot. The pot was placed in a planetary ball mill (Fritsche P7 Classic Line) and mechanically milled at 500 rpm for 1 hour, then at 150 rpm for 1 hour to obtain a slurry. The obtained slurry was vacuum dried at 120 ° C for 2 hours, and the obtained powder was heat-treated at 180 ° C for 2 hours on a hot plate to obtain sulfide solid electrolyte powder D. The ionic conductivity of sulfide solid electrolyte powder D was 2.9 mS cm -1 The average particle size d50 was 2 μm. FIG. 5 shows an XRD chart of sulfide solid electrolyte powder D. Peaks derived from the solid electrolyte were observed at 2θ = 20.2°, 23.5°, 37.1°, and 40.7°.
[0085] (3) Preparation of Positive Electrode Composite Positive electrode active material powder B and acetylene black were weighed to a mass ratio of 87:13 and mixed for 5 minutes using an agate mortar. The obtained powder was sealed in a 45 mL zirconia pot together with 100 zirconia balls with a diameter of 5 mm and mixed in a planetary ball mill (Fritsche P7 Classic Line) at 370 rpm for 1 hour to obtain a composite of positive electrode active material and conductive additive. Subsequently, sulfide solid electrolyte powder D was added to the pot so that the mass ratio of the positive electrode active material and conductive additive composite (electrolyte powder D: composite) was 25:75, and further mixed in a planetary ball mill at 100 rpm for 30 minutes to obtain a positive electrode composite. Figure 6 shows an XRD chart of the positive electrode composite prepared in Example 3.
[0086] (4) Fabrication and Evaluation of All-Solid-State Lithium-Ion Battery An all-solid-state lithium-ion battery was fabricated and evaluated in the same manner as in Example 1, except that the positive electrode composite obtained in (3) above was used.
[0087] Example 4 (1) Preparation of Positive Electrode Composite A positive electrode composite was obtained in the same manner as in Example 3, except that the sulfide solid electrolyte powder A was used instead of the sulfide solid electrolyte powder D.
[0088] (2) Fabrication and Evaluation of All-Solid-State Lithium-Ion Battery Except for using the positive electrode composite obtained in (1) above, an all-solid-state lithium-ion battery was fabricated and evaluated in the same manner as in Example 1. FIG. 7 shows an XRD chart of the positive electrode composite fabricated in Example 4.
[0089] Example 5 (1) Preparation of Positive Electrode Active Material Powder (Titanium Sulfide) Positive electrode active material powder C was obtained in the same manner as in Example 1(1), except that the time for the mechanical milling treatment was changed to 1 hour.
[0090] (2) Preparation of Positive Electrode Composites and All-Solid-State Lithium-Ion Batteries Positive electrode composites and all-solid-state lithium-ion batteries were prepared in the same manner as in Example 3, except that the positive electrode active material powder B was changed to the positive electrode active material powder C. FIG. 8 shows the XRD charts of the positive electrode composites prepared in Examples 5 to 7.
[0091] Example 6 (1) Preparation of Positive Electrode Composite Positive electrode active material powder C and sulfide solid electrolyte powder D were weighed out to a mass ratio of 75:25, and then sealed in a 45 mL zirconia pot together with 100 zirconia balls with a diameter of 5 mm. The pot was placed in a planetary ball mill (P7 Classic Line, manufactured by Fritsche), and the mixture was mixed at 100 rpm for 30 minutes to obtain a positive electrode composite.
[0092] (2) Fabrication of All-Solid-State Lithium-Ion Battery An all-solid-state lithium-ion battery was fabricated and evaluated in the same manner as in Example 1, except that the positive electrode composite obtained in (1) above was used.
[0093] Example 7 (1) Preparation of Positive Electrode Composite Positive electrode active material powder C and acetylene black were weighed to a mass ratio of 90:10 and mixed for 5 minutes using an agate mortar. The obtained powder was sealed in a 45 mL zirconia pot together with 100 zirconia balls with a diameter of 5 mm and mixed in a planetary ball mill (Fritsche P7 Classic Line) at 370 rpm for 1 hour to obtain a composite of positive electrode active material and conductive additive. Subsequently, sulfide solid electrolyte powder D was added to the pot so that the mass ratio of the positive electrode active material and conductive additive composite (solid electrolyte powder D: composite) was 17:83, and further mixed in a planetary ball mill at 100 rpm for 30 minutes to obtain a positive electrode composite.
[0094] (2) Fabrication of All-Solid-State Lithium-Ion Battery An all-solid-state lithium-ion battery was fabricated and evaluated in the same manner as in Example 1, except that the positive electrode composite obtained in (1) above was used.
[0095] Example 8 (1) Preparation of Positive Electrode Active Material Powder (Titanium Sulfide) Titanium disulfide (TiS) was dissolved in a glove box under an argon atmosphere. 2 ) powder and sulfur (S) powder were weighed to a molar ratio of 1:4 and sealed in a 45 mL zirconia pot together with 90 g of 4 mm diameter zirconia balls. The pot was placed in a planetary ball mill (Fritsche P7 Classic Line), and mechanical milling was performed at 510 rpm for 1 hour to obtain positive electrode active material powder D. (2) Preparation of positive electrode composite: A positive electrode composite was obtained in the same manner as in Example 7, except that the positive electrode active material powder D obtained in (1) above was used. (3) Preparation of all-solid-state lithium-ion battery: An all-solid-state lithium-ion battery was prepared and evaluated in the same manner as in Example 1, except that the positive electrode composite obtained in (2) above was used.
[0096] The batteries fabricated in Examples 2 to 8 were evaluated in the same manner as in Example 1, and the results are shown in Table 2.
[0097]
[0098] Highly electronically conductive TiS 2 It was confirmed that the use of titanium sulfide with a residual crystalline phase further increased the discharge capacity. Furthermore, because titanium sulfide, the positive electrode active material, itself has electronic and lithium ion conductivity, it was confirmed that the amounts of conductive additives and sulfide solid electrolytes to be mixed into the positive electrode mixture could be reduced.
[0099] The positive electrode composite of the present invention is suitable as a structural material for lithium ion batteries. The lithium ion batteries of the present invention are also suitable for use in, for example, information-related devices and communication devices such as personal computers, video cameras, and mobile phones, and in vehicles such as electric vehicles.
[0100] Although several embodiments and / or examples of the present invention have been described in detail above, those skilled in the art will readily be able to make numerous modifications to these exemplary embodiments and / or examples without substantially departing from the novel teachings and advantages of the present invention. Accordingly, these numerous modifications are within the scope of the present invention. The contents of all documents cited in this specification and of the applications from which this application claims priority under the Paris Convention are incorporated by reference in their entirety.
Claims
1. Titanium sulfide TiS x (2<x<10) and at least one of the discharge products of the titanium sulfide, and a sulfide solid electrolyte having a diffraction peak at 2θ of 20.1±0.4° in X-ray diffraction using CuKα radiation.
2. The positive electrode mixture according to claim 1, wherein the sulfide solid electrolyte contains lithium, phosphorus, sulfur, and a halogen as constituent elements.
3. The positive electrode mixture according to claim 1 or 2, wherein the content of lithium relative to all constituent elements of the sulfide solid electrolyte is 35 to 45 mol %.
4. The positive electrode composite according to any one of claims 1 to 3, wherein the titanium sulfide content a, the sulfide solid electrolyte content b, and the conductive additive content c satisfy the following formulas (1) to (3): 10 mass%≦a≦90 mass% (1) 0 mass%<b≦65 mass% (2) 0 mass%≦c≦40 mass% (3) (a+b+c is 100 mass%).
5. The positive electrode composite according to any one of claims 1 to 4, which has, in X-ray diffraction using CuKα radiation, a diffraction peak having a 2θ of 20.1±0.4°, a diffraction peak having a 2θ of 34±1°, and one or more diffraction peaks having a 2θ of 15.5±1°, 44±1°, and 54±1°.
6. The positive electrode mixture according to claim 4, wherein the content c of the conductive additive is 0 mass %.
7. Titanium sulfide TiS that satisfies the following (A) x A method for producing a positive electrode composite material, comprising the step of mixing a sulfide solid electrolyte having a structure in which the sulfide solid electrolyte satisfies the following (B): (A) in X-ray diffraction using CuKα radiation, the sulfide solid electrolyte has a diffraction peak at 2θ of 34±1° and one or more diffraction peaks at 2θ selected from 15.5±1°, 44±1°, and 54±1°; and (B) in X-ray diffraction using CuKα radiation, the sulfide solid electrolyte has a diffraction peak at 2θ of 20.1±0.4°.
8. The method according to claim 7, wherein the sulfide solid electrolyte has an average particle size of 10 μm or less.
9. The method of claim 7 or 8, further comprising the step of mechanically mixing sulfur and titanium disulfide to synthesize said titanium sulfide.
10. A positive electrode mixture obtained by the manufacturing method according to any one of claims 7 to 9.
11. A positive electrode comprising the positive electrode mixture according to any one of claims 1 to 6 and 10.
12. A lithium ion battery comprising the positive electrode of claim 11.
Citation Information
Patent Citations
Thermal cell
JP2006236993A
All solid secondary battery
JP2019040752A
Manufacturing method for all-solid battery and electrode active material
JP2020064864A