Composition for forming negative electrode active material layer for lithium-ion secondary battery

The composition of a negative electrode active material layer with carbon nanotubes and a specific formula addresses the issue of uneven reaction distribution in lithium-ion batteries, enhancing cycle characteristics and lifespan by ensuring uniform reactions and maintaining electrode strength.

WO2024203706A1PCT designated stage expired Publication Date: 2024-10-03KRI INC
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/010981
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2024-03-21
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Lithium-ion batteries face significant challenges in extending their operational lifespan due to factors like oxidation, lithium ion insertion and desorption, electrolyte decomposition, and uneven reaction distribution within the electrode, leading to premature capacity loss and resistance increase, which is exacerbated by overvoltage conditions and the lack of effective methods to homogenize reactions.

Method used

A composition for forming a negative electrode active material layer that includes a negative electrode active material and carbon nanotubes, with a specific formula (2.15M1 + 0.00454(M2 × D^2) + 6.54 ≤ 7.40, where M1 is the binder content, M2 is the thickener and/or dispersant content, and D is the average particle diameter, to ensure uniform reaction distribution and maintain electrode strength, thereby enhancing charge-discharge cycle characteristics.

Benefits of technology

The solution effectively homogenizes reactions within the battery, significantly improving charge-discharge cycle characteristics and extending the battery's lifespan by reducing uneven reaction distribution and maintaining sufficient electrode strength, even under high load conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-C000002
    Figure JPOXMLDOC01-APPB-C000002
  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000003
    Figure JPOXMLDOC01-APPB-T000003
Patent Text Reader

Abstract

This composition for forming a negative electrode material layer for a lithium-ion secondary battery can be used to produce a battery in which reactions within the battery become more uniform and the charge / discharge cycle characteristics are superior. The composition for forming a negative electrode material layer contains at least a negative electrode active material and carbon nanotubes, and satisfies formula (1): (1) 2.15M1 + 0.00454 (M2 × D2) + 6.54 ≤ 7.40 (In the formula: M1 represents the content (mass%) of a binder; M2 represents the content (mass%) of a thickener and / or a dispersant; and D represents the average particle size (μm) of the negative electrode active material.)
Need to check novelty before this filing date? Find Prior Art

Description

Composition for forming negative electrode active material layer for lithium ion secondary battery

[0001] The present invention relates to a composition for forming a negative electrode active material layer for a lithium ion secondary battery.

[0002] The lithium-ion battery (LIB) business has achieved dramatic growth thanks to relentless technological development aimed at miniaturizing and lightening mobile devices and enhancing their functionality (pursuing convenience) by leveraging the battery's high energy density, high voltage, and safety characteristics. With global environmental and resource issues now in the spotlight, policies such as promoting eco-cars and shifting to renewable energy are expected to continue to drive the growth of the LIB market. Meanwhile, if LIBs are adopted for personal electric vehicles (EVs) and stationary energy storage (e.g., for renewable energy leveling), the number of LIBs needed by 2030 is estimated to be approximately 10 times that of 2018. This could lead to economically unfavorable situations for users, such as a sharp rise in battery costs due to resource shortages. Therefore, research and development into reuse and recycling, both from the perspective of extending the life of a single battery, has become active. Extending battery life is also effective from the perspective of life cycle assessment (LCA).

[0003] Furthermore, new proposals have been made regarding the future of mobility, including EVs. CASE and MaaS, which aim to further improve user convenience, are becoming a reality, and there are signs that mobility, including EVs, will shift from individual ownership to sharing in the future. Amid this trend, AIEVs (Artificial Intelligence Electric Vehicles), which are expected to be deployed in the market in the future, are EVs equipped with AI, with automated driving, shared vehicles, and vehicles managed by a management company rather than by individuals. The management company provides mobility services (CASE) and various services required by users within the vehicle (MaaS). Furthermore, since the management company can also perform driving control and charging / discharging control, operation can also take into consideration battery life, safety, etc. Furthermore, vehicle sharing can reduce the user's burden to approximately one-fifth of that of individual ownership, making it economically advantageous. In other words, in the future, replacing private cars, which are currently mainly gasoline-powered, with AIEVs (sharing cars) is expected to contribute to the global environment, reduce traffic accidents and congestion, provide a new means of transportation in aging and depopulated areas, reduce personal expenses, and make effective use of travel time. Furthermore, AIEVs will be able to function as huge energy storage systems, automatically charging electricity generated from highly fluctuating renewable energy sources through a management company's management system and discharging it as needed.

[0004] However, to achieve this, it will be necessary to reconsider the development direction of lithium-ion batteries, which are currently the mainstream (Figure 1).

[0005] In particular, dramatically extending the lifespan of batteries installed in electric vehicles is essential. To realize AIEVs, unlike privately owned vehicles, a total vehicle mileage of, for example, 500,000 km or more is required. If the battery life remains at the current level, multiple battery replacements will be necessary, undermining economic viability and leaving resource issues unresolved. The required battery performance emphasizes battery life over the currently mainstream requirements of energy density (mileage) and rapid charging. Specifically, the energy density must be at least 400 Wh / L for a single cell, and the vehicle mileage is 200-300 km with a 20-30 kWh battery installed. However, the target practical operating life must be at least five times longer than the current level.

[0006] Although various studies have been conducted to extend the life of batteries, if the target is to extend the practical operating life by at least five times the current life, a new perspective is required. In the present invention, the inventors have focused on the overvoltage factor, in contrast to the many degradation factors that have been studied in the past, such as degradation due to oxidation and reduction of active materials and components, degradation associated with the insertion and desorption of lithium ions into and from active materials, consumption of lithium ions due to decomposition of the electrolyte, and degradation due to loosening of electrodes.

[0007] The present inventors have explained phenomena such as low-temperature degradation and secondary degradation by defining a new degradation mechanism called "degradation due to overvoltage factor (current × resistance)." Degradation due to overvoltage factor is defined as a degradation factor affected by load current and battery resistance (DC resistance). For example, degradation during low-temperature cycling can be explained as being caused by an increase in resistance at low temperatures, and degradation due to rapid charging can be explained as being caused by an increase in load current. Furthermore, as battery resistance increases with degradation, and as capacity decreases, the load on the active material (apparent load) increases when the same current as the initial current is applied. Furthermore, if gas accumulates within the electrode group, the gas does not allow ions to pass through, so load is placed on the electrode parts and active material other than the gas accumulation. From this perspective, one factor affecting battery life as an overvoltage factor is uneven reaction distribution within the electrode. If the reaction does not occur uniformly within the electrode, some active materials used in the electrode will accumulate stress over the long term of the battery. For example, in the case of the negative electrode, this can lead to localized strong reduction, resulting in the consumption of lithium ions. In the worst case, this can lead to lithium electrodeposition. This often results in a sudden drop in capacity and a rapid increase in resistance (secondary degradation) after repeated charge-discharge cycles. By uniforming the electrode reaction and preventing uneven reaction distribution within the battery, this secondary degradation (sudden capacity drop) can be prevented, dramatically extending battery life. Therefore, it is important to uniformize the reaction within the battery, but little effort has been made to achieve this.

[0008] To achieve uniform reactions within a battery, it is important to create an electrode structure that allows for uniform ion migration within the electrode. To achieve this, efforts have been made to increase the electrode porosity or reduce the electrode's basis weight. However, these methods result in a decrease in energy density (mileage), and these methods alone are limited in terms of achieving the 400 Wh / L level. Furthermore, eliminating factors that can inhibit ion migration within the electrode—specifically, electrode constituent materials such as binders typically used to strengthen the electrode, thickeners used to stabilize the electrode slurry, and dispersants—is also considered effective in achieving uniform ion migration within the electrode. However, reducing or eliminating these constituent materials significantly reduces the electrode's strength, making it unable to adapt to volumetric changes during charging and discharging, and reducing its lifespan due to factors such as a lack of current collection paths.

[0009] In addition, reducing the particle size of the negative electrode active material is also considered to uniformize the reaction within the battery. Reducing the particle size of the negative electrode active material increases the reaction area, thereby reducing the lithium ion flux per unit area. This reduces the risk of lithium precipitation, particularly under high-load conditions or long-term use, and is expected to improve battery life. However, according to research by the inventors, simply reducing the particle size of the negative electrode active material accelerates deterioration due to decomposition of the electrolyte due to the increased reaction area. Furthermore, the number of interfaces between the negative electrode active material particles increases, increasing the number of starting points for structural collapse. This requires a large amount of binder, thickener, dispersant, etc. to maintain the strength of the electrode. As a result, the reaction within the battery cannot be uniformized, and battery life does not improve.

[0010] The present invention is intended to solve the above-mentioned problems, and has an object to provide a composition for forming a negative electrode active material layer that can make the reaction in a battery more uniform and produce a battery with excellent charge-discharge cycle characteristics.

[0011] In view of the above-mentioned problems, the present inventors have conducted extensive research. As a result, they have found that by adjusting the content of the binder, the content of the thickener and / or dispersant, and the average particle size of the negative electrode active material so as to satisfy a predetermined mathematical formula, the electrode has sufficient strength to maintain its shape, the reaction within the battery is made uniform, and excellent charge-discharge cycle characteristics are achieved. Based on this finding, the present invention has been completed through further research. That is, the present invention includes the following configurations.

[0012] Item 1. A negative electrode active material containing at least a negative electrode active material and carbon nanotubes, and a negative electrode active material having the following formula (1): 2.15M 1 +0.00454(M 2 ×D 2 )+6.54≦7.40 (1) [wherein, M 1 indicates the content (mass%) of the binder. 2 represents the content (% by mass) of the thickener and / or dispersant, and D represents the average particle size (μm) of the negative electrode active material.

[0013] Item 2. The composition for forming a negative electrode active material layer for a lithium ion secondary battery according to Item 1, wherein, based on 100% by mass of the total amount of the composition, the content of the negative electrode active material is 96.6 to 99.9% by mass, the content of the carbon nanotubes is 0.01 to 1.4% by mass, the content of negative electrode constituent materials other than the negative electrode active material and the carbon nanotubes is 0 to 2.0% by mass, and the average particle size of the negative electrode active material is 0.1 to 30.0 μm.

[0014] Item 3. The composition for forming a negative electrode active material layer for a lithium ion secondary battery according to Item 1 or 2, wherein the negative electrode active material is a material capable of absorbing and releasing lithium ions.

[0015] Item 4. The composition for forming a negative electrode active material layer for a lithium ion secondary battery according to any one of Items 1 to 3, wherein the carbon nanotubes are single-walled carbon nanotubes.

[0016] Item 5. The composition for forming a negative electrode active material layer for a lithium ion secondary battery according to any one of Items 1 to 4, which is used to reduce uneven distribution of reactions in a lithium ion secondary battery.

[0017] Item 5-1: Use of the composition for forming a negative electrode active material layer for a lithium ion secondary battery according to any one of Items 1 to 4, for reducing uneven distribution of a reaction in the lithium ion secondary battery.

[0018] Item 6. The composition for forming a negative electrode active material layer for a lithium ion secondary battery according to any one of Items 1 to 5, which is for a lithium ion secondary battery used in an electric vehicle for car sharing.

[0019] Item 6-1. Use of the composition for forming a negative electrode active material layer for a lithium ion secondary battery according to any one of Items 1 to 5 in a lithium ion secondary battery used in an electric vehicle for car sharing.

[0020] Item 7. A negative electrode active material layer for a lithium ion secondary battery, comprising the composition for forming a negative electrode active material layer for a lithium ion secondary battery according to any one of Items 1 to 6.

[0021] Item 8. The negative electrode active material layer for a lithium ion secondary battery according to Item 7, which is for a lithium ion secondary battery used in an electric vehicle for car sharing.

[0022] Item 8-1. Use of the negative electrode active material layer for a lithium ion secondary battery according to Item 7 in a lithium ion secondary battery used in an electric vehicle for car sharing.

[0023] Item 9. A negative electrode for a lithium ion secondary battery, comprising the negative electrode active material layer for a lithium ion secondary battery according to Item 7 or 8.

[0024] Item 10. The negative electrode for a lithium ion secondary battery according to Item 9, which is for a lithium ion secondary battery used in an electric vehicle for car sharing.

[0025] Item 10-1. Use of the negative electrode for a lithium ion secondary battery according to Item 9 in a lithium ion secondary battery used in an electric vehicle for car sharing.

[0026] Item 11. A lithium ion secondary battery comprising the negative electrode for a lithium ion secondary battery according to Item 9 or 10.

[0027] Item 12. The charging rate SOC is defined by the following formula (2): SOC (%) = remaining capacity (Ah) / full charge capacity (Ah) × 100 (2), and after discharging from an SOC of 100% to an SOC of 90% under conditions of 25°C and 3.0C, a 10-minute pause is performed to measure the rise in voltage during the pause, and from the measured voltage rise, the reaction resistance is separated into two components, a resistance DCR (0.3s) due to reaction inhibition and a resistance DCR (0.3s-10min) due to ion migration inhibition, and the resistance DCR (0.3s) is calculated, and the resistance DCR (0.3s) due to reaction inhibition is calculated by the following formula (3): 2.15M 1 +0.00454(M 2 ×D 2 )+5.00≦DCR(0.3s)≦2.15M 1 +0.00454(M 2 ×D 2 )+7.40 (3) [wherein, M 1 indicates the content (mass%) of the binder. 2 Item 12. The lithium ion secondary battery according to Item 11, wherein ≡100 μm represents the content (mass%) of the thickener and / or dispersant, and D represents the average particle diameter (μm) of the negative electrode active material.

[0028] Item 13. The lithium ion secondary battery according to Item 11 or 12, which is used in an electric vehicle for car sharing.

[0029] Item 13-1. Use of the lithium ion secondary battery according to Item 11 or 12 in an electric vehicle for car sharing.

[0030] According to the present invention, by adjusting the content of the binder, the content of the thickener and / or dispersant, and the average particle size of the negative electrode active material so as to satisfy a predetermined mathematical formula, the electrode has sufficient strength to maintain its shape, the reaction within the battery is made uniform, and excellent charge-discharge cycle characteristics are achieved.

[0031] 1 is a schematic diagram showing the direction of development of lithium-ion batteries, keeping in mind a worldview in which the use and operation of automobiles will change dramatically. 2 is a diagram showing an outline of a method for analyzing resistance resulting from reaction inhibition in the high-load rest method. 3 is a graph showing an outline of an analysis method for AC impedance measurement in Test Example 1. 4 is a graph showing the results of AC impedance measurement in Test Example 1. 5 is a diagram showing the correlation between the calculated value of reaction resistance DCR (0.3 s) using a calculation formula and the actually measured value of DCR (0.3 s) in Test Example 2.

[0032] In this specification, the term "containing" is a concept that encompasses all of "comprise," "consist essentially of," and "consist only of."

[0033] In addition, in this specification, the expression "A to B" means "A or more and B or less."

[0034] 1. Composition for Forming a Negative Electrode Active Material Layer for Lithium-Ion Secondary Batteries Generally, the negative electrode active material layer in a negative electrode often contains a significant amount of other negative electrode constituent materials, such as binders (e.g., binders, thickeners, dispersants), in addition to the negative electrode active material. Because these other negative electrode constituent materials are impermeable to lithium ions, the presence of a significant amount of other negative electrode constituent materials inhibits the migration of lithium ions, preventing uniform charge and discharge. When lithium ion migration is inhibited, the reaction concentrates in areas where the migration of lithium ions is less inhibited, resulting in lithium electrodeposition and other problems. On the other hand, simply reducing the amount of other negative electrode constituent materials does not provide sufficient strength to maintain the shape of the negative electrode. This leads to deterioration of current collection, such as expansion and contraction during charge and discharge, destruction of the electrode structure, and reduced conductivity within the electrode, resulting in a decrease in the cycle and life characteristics of the battery. Therefore, simply reducing the amount of other negative electrode constituent materials cannot simultaneously alleviate the uneven reaction distribution and improve the cycle and life characteristics. Although a positive electrode can function even if the amount of positive electrode constituent materials other than the positive electrode active material is reduced, in the case of a negative electrode, as described above, the battery life characteristics are reduced due to current collection degradation such as breakdown of the negative electrode structure and reduced conductivity within the negative electrode, and therefore it has been common technical knowledge that the amount of negative electrode constituent materials other than the negative electrode active material cannot be significantly reduced. Furthermore, depending on the particle size of the negative electrode active material, the interface between negative electrode active material particles may change, which may increase the number of starting points for structural collapse, and therefore it has not been possible to simultaneously alleviate uneven reaction distribution and improve cycle characteristics and life characteristics by simply significantly reducing the amount of negative electrode constituent materials other than the negative electrode active material.

[0035] In contrast, the composition for forming a negative electrode active material layer for a lithium ion secondary battery of the present invention contains at least a negative electrode active material and carbon nanotubes, and has a structure represented by the following formula (1): 2.15M 1 +0.00454(M 2 ×D 2 )+6.54≦7.40 (1) [wherein, M 1 indicates the content (mass%) of the binder. 2 indicates the content (mass %) of the thickener and / or dispersant, and D indicates the average particle diameter (μm) of the negative electrode active material.]

[0036] By adopting such a configuration, the content of the binder, the content of the thickener and / or the dispersant, and the average particle size of the negative electrode active material are appropriately adjusted, so that the reaction in the battery is made uniform while maintaining the strength sufficient to maintain the shape of the electrode, and the cycle characteristics and life characteristics are significantly improved. In other words, the composition for forming a negative electrode active material layer for a lithium ion secondary battery of the present invention can be used to reduce uneven reaction in a lithium ion secondary battery.

[0037] (1-1) Negative Electrode Active Material The negative electrode active material is not particularly limited, and any material that can be used as a negative electrode active material in a lithium ion secondary battery, that is, any material that can absorb and release lithium ions, can be used. Examples of the negative electrode active material include carbon materials such as natural graphite, artificial graphite, and amorphous carbon; metal materials that can be alloyed with lithium, such as Si, Al, Sn, Pb, Zn, Bi, In, Mg, Ga, Si alloys, Sn alloys, and Al alloys; and SiO. x (0<x<2), SnO x (0<x<2), lithium titanium composite oxide (Li 2 TiO 3 Examples of the negative electrode active material include metal oxides capable of absorbing and releasing lithium ions, such as vanadium oxide, and composite materials containing a metal material and a carbon material, such as Si-C composites and Sn-C composites. These negative electrode active materials can be used alone or in combination of two or more. In particular, when a conductive material, such as a carbon material, is used as the negative electrode active material, the negative electrode active material also functions as a conductive material, making it particularly easy to reduce the content of substances that inhibit the movement of lithium ions.

[0038] The shape of the negative electrode active material is not particularly limited, and various shapes such as spheres, scales, chunks, fibers, whiskers, and crushed shapes can be used. A combination of negative electrode active materials of different shapes can also be used. The spherical shape may be a perfect sphere or an elliptical shape.

[0039] The composition for forming a negative electrode active material layer for a lithium ion secondary battery of the present invention has an appropriate binder content, a thickener and / or dispersant content, and an average particle size of the negative electrode active material, so that the reaction within the battery is uniform while maintaining a strength sufficient to maintain the shape of the electrode, thereby significantly improving cycle characteristics and life characteristics. From the above formula (1), it can be seen that a smaller average particle size of the negative electrode active material is preferable, but from the viewpoints of easily suppressing aggregation, reducing the flux of lithium ions per unit area, easily reducing reaction resistance, and easily improving cycle characteristics and life characteristics, a particle size of 0.1 to 30.0 μm is preferred, 0.5 to 20.0 μm is more preferred, and 1.0 to 13.0 μm is even more preferred. In the composition for forming a negative electrode active material layer for a lithium ion secondary battery of the present invention, when no negative electrode constituent material other than the negative electrode active material and carbon nanotubes described below is contained, the average particle size of the negative electrode active material is not particularly affected, whereas when even a small amount of a negative electrode constituent material other than the negative electrode active material and carbon nanotubes described below is contained, the average particle size of the negative electrode active material is preferably 0.1 to 20.0 μm, more preferably 0.5 to 13.0 μm, and even more preferably 1.0 to 10.0 μm. The average particle size of the negative electrode active material is measured by a laser diffraction / scattering method.

[0040] The composition for forming a negative electrode active material layer for a lithium ion secondary battery of the present invention has an appropriate binder content, a thickener and / or dispersant content, and an average particle size of the negative electrode active material. As a result, the reaction within the battery is uniform while maintaining sufficient strength to maintain the electrode shape, resulting in significantly improved cycle characteristics and life characteristics. To facilitate these adjustments, the content of the negative electrode active material is preferably 96.6 to 99.9 mass%, more preferably 97.6 to 99.8 mass%, and even more preferably 98.2 to 99.7 mass%. When multiple negative electrode active materials are used, it is preferable to adjust their total amount so that it falls within the above range. In the composition for forming a negative electrode active material layer for a lithium ion secondary battery of the present invention, the total amount of the negative electrode active material, carbon nanotubes, and negative electrode constituent materials other than the electrode active material and carbon nanotubes (total amount of the composition) is 100 mass%.

[0041] (1-2) Carbon Nanotubes The composition for forming a negative electrode active material layer for a lithium ion secondary battery of the present invention has an appropriate binder content, a thickener and / or dispersant content, and an average particle size of the negative electrode active material, and as a result, the composition maintains a strength sufficient to maintain the shape of the electrode while uniformly promoting reactions within the battery, resulting in significantly improved cycle characteristics and life characteristics. On the other hand, even if the particle size of the negative electrode active material is reduced to increase the number of interfaces between the negative electrode active material particles and thereby increase the number of starting points for structural collapse, the composition is likely to have sufficient strength to maintain the shape of the negative electrode even when the amount of negative electrode constituent materials other than the negative electrode active material is reduced, uniformly promoting reactions within the battery, and improving cycle characteristics and life characteristics.

[0042] Carbon nanotubes are hollow carbon materials in which graphite sheets (i.e., carbon atom planes of a graphite structure or single-layer graphene sheets) are closed in a tubular shape, with a diameter on the nanometer scale and a graphite wall structure. Carbon nanotubes with a tubular wall structure consisting of a single graphite sheet (single-layer graphene sheet) are called single-walled carbon nanotubes. On the other hand, carbon nanotubes in which multiple graphite sheets are closed in a tubular shape and nested are called nested multi-walled carbon nanotubes. In the present invention, both single-walled carbon nanotubes and multi-walled carbon nanotubes can be used, but single-walled carbon nanotubes are preferred because they tend to have sufficient strength to maintain the shape of the negative electrode, facilitate current collection between negative electrode active materials, and are less likely to inhibit the movement of lithium ions, making it easier to uniformize reactions within the battery and extend the life of the battery.

[0043] Such carbon nanotubes can be used alone or in combination of two or more kinds.

[0044] A small average outer diameter of the carbon nanotubes is preferable from the viewpoints of easily increasing the number of carbon nanotubes per volume, reducing the carbon nanotube content required to maintain the shape of the negative electrode, and minimizing the inhibition of lithium ion migration. Therefore, the average outer diameter of the carbon nanotubes is preferably 0.43 to 20 nm, more preferably 0.43 to 10 nm. The average outer diameter of the carbon nanotubes is measured by observation with a transmission electron microscope (TEM). For carbon nanotubes having such an average outer diameter, the average inner diameter is set according to the average outer diameter.

[0045] The longer the average length of the carbon nanotubes, the more likely they are to have sufficient strength to maintain the shape of the electrode and to facilitate current collection between the negative electrode active materials. On the other hand, from the viewpoints of improving dispersibility and preventing the movement of lithium ions, a shorter average length of the carbon nanotubes is preferable. Therefore, the average length of the carbon nanotubes is preferably 0.5 to 200 μm, more preferably 1 to 50 μm. The average length of the carbon nanotubes is measured by observation with a scanning electron microscope (SEM).

[0046] The average aspect ratio of the carbon nanotubes, defined as the ratio of the average length to the average outer diameter of the carbon nanotubes, is preferably 25 to 200,000, more preferably 100 to 50,000, from the viewpoints that the higher the average aspect ratio, the easier it is to have a strength sufficient to maintain the shape of the electrode with a smaller carbon nanotube content, the easier it is to collect current between negative electrode active materials, and the less it is to inhibit the movement of lithium ions, making it easier to make the reaction within the battery uniform and making it easier to extend the life of the battery.

[0047] In the present invention, the carbon nanotubes may be either individual or bundled carbon nanotubes, which are easily strong as a bundle. Whichever type of carbon nanotube is used, current collection between active material particles and maintenance of the negative electrode shape are facilitated, and the amount of negative electrode constituent material other than the negative electrode active material can be reduced. As a result, the negative electrode has sufficient strength to maintain its shape and is less likely to inhibit the movement of lithium ions, which makes the reaction within the battery uniform and increases the battery life.

[0048] Furthermore, it is considered preferable that the graphene structure of the carbon nanotubes has few defects, i.e., a high G / D ratio in the Raman spectrum, from the viewpoint of suppressing the reactivity between the carbon nanotubes and the electrolyte solution. For this reason, in the present invention, the carbon nanotubes preferably have a G / D ratio in the Raman spectrum of 1 to 200, more preferably 50 to 150.

[0049] The composition for forming a negative electrode active material layer for a lithium ion secondary battery of the present invention appropriately adjusts the binder content, thickener and / or dispersant content, and average particle size of the negative electrode active material, thereby maintaining a strength sufficient to maintain the electrode shape while uniformly facilitating reactions within the battery and significantly improving cycle and life characteristics. On the other hand, even a small amount of carbon nanotubes facilitates current collection between active material particles and maintaining the electrode shape. Even when the particle size of the negative electrode active material is reduced, increasing the number of interfaces between the negative electrode active material particles and increasing the number of starting points for structural collapse, the composition is strong enough to maintain the shape of the negative electrode even when the amount of negative electrode constituent materials other than the negative electrode active material is reduced, thereby uniformizing reactions within the battery and improving cycle and life characteristics. To facilitate these adjustments, the carbon nanotube content is preferably 0.01 to 1.4% by mass, more preferably 0.1 to 1.2% by mass, and even more preferably 0.2 to 1.0% by mass. When multiple carbon nanotubes are used, it is preferable to adjust the total amount so that it is within the above range. In the composition for forming a negative electrode active material layer for a lithium ion secondary battery of the present invention, the total amount of the negative electrode active material, the carbon nanotubes, and the negative electrode constituent materials other than the electrode active material and the carbon nanotubes (total amount of the composition) is 100 mass%.

[0050] (1-3) Negative Electrode Structural Materials Other Than Negative Electrode Active Material and Carbon Nanotubes The composition for forming a negative electrode active material layer for a lithium ion secondary battery of the present invention has an appropriate adjustment of the binder content, the thickener and / or dispersant content, and the average particle size of the negative electrode active material, so that the reaction within the battery is made uniform while maintaining a strength sufficient to maintain the shape of the electrode, and the cycle characteristics and life characteristics are significantly improved.

[0051] In the present invention, the negative electrode constituent materials other than the negative electrode active material and the carbon nanotubes are a general term that includes substances (binders) that have adhesive properties with the negative electrode active material and the negative electrode current collector, as well as conductive materials other than carbon nanotubes such as carbon black, and substances that inhibit the migration of lithium ions other than carbon nanotubes (lithium ion migration inhibiting substances) such as thickeners and dispersants.

[0052] Examples of negative electrode constituent materials other than the negative electrode active material and carbon nanotubes in the present invention include conductive materials such as carbon blacks such as acetylene black, furnace black, and ketjen black; flake graphite; graphene; and amorphous carbon obtained by heat-treating organic materials. Binders are used as emulsions when preparing electrode slurries, and examples include polyolefin resins (styrene-butadiene copolymer resins, ethylene-vinyl alcohol copolymer resins, etc.), synthetic rubbers (styrene-butadiene rubber, acrylonitrile-butadiene rubber, ethylene-propylene-diene rubber, etc.), and acrylic resins. Thickeners or dispersants are used as solutions when preparing electrode slurries, and have a thickening or dispersing function. Examples include fluorine-based polymers (polyvinylidene fluoride resins, polytetrafluoroethylene resins, vinylidene fluoride-hexafluoropropylene copolymers, etc.), polyamides, polyimides, polyacrylic acids, polyacrylic acid esters, polyvinyl ethers, carboxymethyl cellulose, carboxymethyl cellulose sodium salt, carboxymethyl cellulose ammonium, hydroxypropyl cellulose, hydroxyethyl cellulose, and methyl cellulose. These negative electrode active materials and negative electrode constituent materials other than carbon nanotubes can be used alone or in combination of two or more.

[0053] The composition for forming a negative electrode active material layer for a lithium ion secondary battery of the present invention has an appropriate binder content, a thickener and / or dispersant content, and an average particle size of the negative electrode active material, and as a result, the reaction within the battery is made uniform while maintaining a strength sufficient to maintain the shape of the electrode, thereby significantly improving cycle characteristics and life characteristics. From the above formula (1), it can be seen that a small binder content and a small thickener and / or dispersant content are both preferable, but since the contents of negative electrode constituent materials other than the negative electrode active material and carbon nanotubes are also relevant, it is preferable that the composition does not contain negative electrode constituent materials other than the negative electrode active material and carbon nanotubes, or if it does contain them, the contents are small.

[0054] For this reason, in the composition for forming a negative electrode active material layer for a lithium ion secondary battery of the present invention, the content of the negative electrode constituent materials other than the negative electrode active material and the carbon nanotubes is preferably 0 to 2.0 mass%, more preferably 0 to 1.6 mass%, and even more preferably 0 to 1.2 mass%. When a plurality of negative electrode active materials and negative electrode constituent materials other than the carbon nanotubes are used, it is preferable to adjust the total amount thereof to be within the above range. In the composition for forming a negative electrode active material layer for a lithium ion secondary battery of the present invention, the total amount of the negative electrode active material, the carbon nanotubes, and the negative electrode constituent materials other than the electrode active material and the carbon nanotubes (total amount of the composition) is 100 mass%.

[0055] In the composition for forming a negative electrode active material layer for a lithium ion secondary battery of the present invention, the content of the binder is preferably 0 to 0.6 mass%, more preferably 0 to 0.4 mass%, and even more preferably 0 to 0.2 mass%. When multiple binders are used, it is preferable to adjust the total amount thereof to be within the above range. In the composition for forming a negative electrode active material layer for a lithium ion secondary battery of the present invention, the total amount of the negative electrode active material, carbon nanotubes, and negative electrode constituent materials other than the electrode active material and carbon nanotubes (total amount of the composition) is 100 mass%.

[0056] In the composition for forming a negative electrode active material layer for a lithium ion secondary battery of the present invention, the content of the thickener and / or dispersant is preferably 0 to 1.4 mass%, more preferably 0 to 1.2 mass%, and even more preferably 0 to 1.0 mass%. When multiple thickeners and / or dispersants are used, it is preferable to adjust the total amount thereof to be within the above range. In the composition for forming a negative electrode active material layer for a lithium ion secondary battery of the present invention, the total amount of the negative electrode active material, the carbon nanotubes, and the negative electrode constituent materials other than the electrode active material and the carbon nanotubes (total amount of the composition) is 100 mass%.

[0057] (1-4) Composition for forming a negative electrode active material layer for a lithium ion secondary battery As described above, the composition for forming a negative electrode active material layer for a lithium ion secondary battery of the present invention contains a negative electrode active material, carbon nanotubes, and, if necessary, a negative electrode constituent material other than the negative electrode active material and carbon nanotubes. Among these, the content of adhesive, the content of thickener and / or dispersant, and the average particle size of the negative electrode active material are appropriately adjusted. As a result, the reaction within the battery is made uniform while maintaining a strength sufficient to maintain the shape of the electrode, and the cycle characteristics and life characteristics are significantly improved.

[0058] Specifically, the following formula (1): 2.15M 1 +0.00454(M 2 ×D 2 )+6.54≦7.40 (1) [wherein, M 1 indicates the content (mass%) of the binder. 2 represents the content (mass%) of the thickener and / or dispersant, and D represents the average particle diameter (μm) of the negative electrode active material.] and preferably satisfies the following formula (1A): 5.00≦2.15M 1 +0.00454(M 2 ×D 2 ) + 6.54≦7.20 (1A), and more preferably satisfies the following formula (1A1): 5.00≦2.15M 1 +0.00454(M 2 ×D 2 ) + 6.54≦7.00 (1A1) is more preferably satisfied.

[0059] In the composition for forming a negative electrode active material layer for a lithium ion secondary battery of the present invention, when a negative electrode active material, carbon nanotubes, and, if necessary, negative electrode constituent materials other than the negative electrode active material and carbon nanotubes are mixed to form a paste composition for forming a negative electrode active material layer for a lithium ion secondary battery, it is possible to make the composition into a paste by adding one or more organic solvents such as water, alcohol (methanol, ethanol, n-propyl alcohol, isopropyl alcohol, etc.), acetone, N-methylpyrrolidone, dimethyl sulfoxide, dimethylformamide, etc. In this case, the content of each component is a value relative to the total amount of the negative electrode active material, carbon nanotubes, and negative electrode constituent materials other than the electrode active material and carbon nanotubes, i.e., the total amount of solids, which is 100 mass.

[0060] The method for producing the composition for forming a negative electrode active material layer for a lithium ion secondary battery of the present invention is not particularly limited. For example, the composition for forming a negative electrode active material layer for a lithium ion secondary battery of the present invention can be produced by mixing the above-mentioned components by a conventional method. The mixing can be performed by mixing all the components simultaneously or sequentially.

[0061] 2. Negative Electrode Active Material Layer for Lithium Ion Secondary Battery The negative electrode active material layer for a lithium ion secondary battery of the present invention contains the composition for forming a negative electrode active material layer for a lithium ion secondary battery of the present invention.

[0062] The thickness of the negative electrode active material layer for a lithium ion secondary battery of the present invention is not particularly limited, but while a thinner layer is preferable in terms of ensuring lithium ion penetration and electrical conductivity and facilitating uniform reaction, the present invention aims to uniformize the battery reaction to improve cycle characteristics and life characteristics, so a thicker layer is also possible in terms of energy density per electrode. Therefore, the thickness of the negative electrode active material layer for a lithium ion secondary battery of the present invention is preferably 1 to 300 μm, more preferably 10 to 150 μm, and even more preferably 50 to 100 μm.

[0063] The negative electrode active material layer for a lithium ion secondary battery of the present invention can be produced by forming the above-mentioned negative electrode active material layer-forming composition for a lithium ion secondary battery of the present invention into a layer. For example, when the negative electrode active material layer-forming composition for a lithium ion secondary battery of the present invention is used as a paste composition for forming a negative electrode active material layer for a lithium ion secondary battery, the paste composition can be dried by a conventional method and formed into a layer.

[0064] 3. Negative Electrode for Lithium-ion Secondary Battery The negative electrode for a lithium-ion secondary battery of the present invention includes the above-described negative electrode active material layer for a lithium-ion secondary battery of the present invention, and specifically, it preferably includes a negative electrode current collector and a negative electrode active material layer for a lithium-ion secondary battery of the present invention disposed on the negative electrode current collector.

[0065] The negative electrode current collector is preferably made of a material that is electrochemically stable at the potential used and has high electronic conductivity, such as copper, stainless steel, nickel, or a carbon material. This negative electrode current collector can be, for example, a foil-shaped or mesh-shaped member.

[0066] When producing such a negative electrode for a lithium ion secondary battery of the present invention, it can be produced by forming the above-mentioned composition for forming a negative electrode active material layer for a lithium ion secondary battery of the present invention into a layer on a negative electrode current collector. For example, when the composition for forming a negative electrode active material layer for a lithium ion secondary battery of the present invention is used as a paste composition for forming a negative electrode active material layer for a lithium ion secondary battery, the paste composition can be dried by a conventional method and formed into a layer on a negative electrode active material, thereby producing the negative electrode for a lithium ion secondary battery of the present invention.

[0067] 4. Lithium-ion secondary battery The lithium-ion secondary battery of the present invention includes the above-described negative electrode for a lithium-ion secondary battery of the present invention. The lithium-ion secondary battery of the present invention may also include a positive electrode, an electrolyte, and a container for storing these, which are applicable to known lithium-ion secondary batteries, in addition to the negative electrode for a lithium-ion secondary battery of the present invention.

[0068] The positive electrode may be any electrode capable of supplying lithium ions to the negative electrode, and any known positive electrode may be used.

[0069] Examples of the positive electrode current collector that constitutes the positive electrode include materials that are electrochemically stable at the potential used and have high electronic conductivity, such as aluminum, stainless steel, and carbon materials.

[0070] The positive electrode active material used to form the positive electrode is usually a material capable of absorbing and releasing lithium ions. For example, α-NaFeO 2 Examples of suitable lithium transition metal composite oxides include those having a α-type crystal structure, those having a spinel-type crystal structure, polyanion compounds, chalcogen compounds, and sulfur. 2 As the lithium transition metal composite oxide having a crystalline structure, for example, Li[Li x1 Ni γ1 Mn β1 Co(1-x1-γ1-β1)]O 2 (0≦x1<0.5, 0≦γ1≦1, 0≦β1≦1, 0≦γ1+β1≦1), Li[Li x2 Ni γ2 Co β2 Al(1-x2-γ2-β2)]O 2 (0≦x2<0.5, 0≦γ2≦1, 0≦β2≦1, 0≦γ2+β2≦1). Examples of lithium transition metal oxides having a spinel crystal structure include Li x3 Mn 2 O 4 (0.9≦x3<1.5), Li x4 Ni γ4 Mn (2-γ4) O 4 (0.9≦x4<1.5, 0≦γ4≦2) and the like. Examples of polyanion compounds include LiFePO 4 , LiMnPO 4 , LiNiPO 4 , LiCoPO 4 , Li 3 V 2 (P.O. 4 ) 3 , Li 2 MnSiO 4 , Li 2CoPO 4 Examples of the positive electrode active material include titanium disulfide, molybdenum disulfide, and molybdenum dioxide. The atoms or polyanions in these materials may be partially substituted with atoms or anion species of other elements. These positive electrode active materials may be used alone or in combination of two or more. Among these, the lithium transition metal composite oxides are preferred as the positive electrode active material from the viewpoint of achieving high energy density.

[0071] As the positive electrode constituent material other than the positive electrode active material that constitutes the positive electrode, the same materials as the negative electrode active material and the negative electrode constituent material other than carbon nanotubes in the negative electrode described above can be used, and the content thereof can also be the same as the negative electrode active material and the negative electrode constituent material other than carbon nanotubes in the negative electrode.

[0072] The electrolyte solution is an electrolyte solution in which a salt is dissolved in an aprotic organic solvent, and is placed between the positive electrode and the negative electrode. For example, it is preferable that the electrolyte solution is impregnated and held in a separator made of nonwoven fabric or the like to prevent short-circuiting between the positive electrode and the negative electrode.

[0073] Examples of the aprotic organic solvent that constitutes the above-mentioned electrolytic solution include esters such as ethylene carbonate, propylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, methyl ethyl carbonate, γ-butyrolactone, methyl formate, and methyl acetate; furans such as tetrahydrofuran and 2-methyltetrahydrofuran; ethers such as dioxolane, diethyl ether, dimethoxyethane, diethoxyethane, and methoxyethoxyethane; dimethyl sulfoxide; sulfolanes such as sulfolane and methylsulfolane; acetonitrile, etc. These aprotic organic solvents may be used alone or in combination of two or more.

[0074] On the other hand, examples of salts that can be dissolved in such aprotic organic solvents include lithium salts such as lithium perchlorate, lithium fluoroborate, lithium hexafluorophosphate, lithium hexafluoroarsenate, lithium trifluoromethanesulfonate, lithium halides, lithium chloroaluminate, and lithium bis(fluorosulfonyl)imide. These salts may be used alone or in combination of two or more.

[0075] In the lithium ion secondary battery of the present invention as described above, the resistance DCR (0.3 s) resulting from reaction inhibition can be evaluated as follows.

[0076] First, the state of charge (SOC) is defined by the following formula (2): SOC (%) = remaining capacity (Ah) / full charge capacity (Ah) × 100 (2) After discharging from an SOC of 100% to an SOC of 90% under conditions of 25°C and 3.0C, the battery was put to rest and the increase in voltage during rest was measured.

[0077] As described above, the discharge rate is set to 3.0 C, which is a high load condition at 25° C., because this condition makes it easier to evaluate the uneven distribution of the reaction by setting it to a condition that makes the uneven distribution of the reaction more likely to occur.

[0078] The reason why the SOC at the start of discharge is set to 100% is to ensure that the state before measurement is a state in which no uneven reaction occurs by absorbing lithium ions sufficiently into the negative electrode.

[0079] After discharging under these conditions, the voltage rises by pausing the reaction. The resting time until saturation varies depending on the temperature and discharge rate conditions, and can be set to 10 minutes when the discharge rate is 3.0 C.

[0080] As shown in Figure 2, the voltage rise observed during the pause period includes a voltage rise due to reaction inhibition observed at the very beginning of the pause period and a voltage rise due to ion migration inhibition observed thereafter. The voltage rise due to reaction inhibition is due to the uneven distribution of the reaction at the particle level, and is observed when the reaction is unevenly distributed due to the presence of reaction inhibitors such as the negative electrode active material and negative electrode constituent materials other than carbon nanotubes, and the voltage rises sharply at the very beginning of the pause period. On the other hand, the voltage rise due to ion migration inhibition is due to the uneven distribution of the reaction at the structural level, and is observed when lithium ions move due to the uneven distribution of ion migration inhibitors such as the negative electrode active material and negative electrode constituent materials other than carbon nanotubes, and the voltage rise gradually slows down at periods other than the very beginning of the pause period.

[0081] From the above, the voltage rise due to reaction inhibition can be measured, and the resistance due to reaction inhibition can be calculated using the following formula (3): Resistance due to reaction inhibition DCR (0.3 s) = (voltage rise due to reaction inhibition (V) / current value during discharge (A)) × facing area of ​​positive and negative electrodes (cm 2 ) (3) is calculated as follows.

[0082] As a result, if the resistance value due to reaction inhibition is large, it can be evaluated that the reaction is highly uneven and the cycle characteristics and life characteristics are poor, and if the resistance value due to reaction inhibition is small, it can be evaluated that the reaction is less uneven and the cycle characteristics are excellent and the life is long.

[0083] Specifically, when the composition for forming a negative electrode active material layer for a lithium ion secondary battery of the present invention is used, the resistance due to reaction inhibition calculated as described above under the conditions of 25° C. and 3.0 C is 7.40 Ω cm 2 Preferably, it is 5.00 to 7.20 Ω cm or less. 2 More preferably, 5.00 to 7.00 Ω cm 2 is more preferable.

[0084] As a result of the research by the present inventors, the DCR (0.3 s) obtained in this way was 2.15 M 1 +0.00454(M 2 ×D 2) +6.54. Therefore, the lithium ion secondary battery of the present invention has a capacitance value similar to the following formula (3): 1 +0.00454(M 2 ×D 2 )+5.00≦DCR(0.3s)≦2.15M 1 +0.00454(M 2 ×D 2 )+7.40 (3) [wherein, M 1 indicates the content (mass%) of the binder. 2 represents the content (mass%) of the thickener and / or dispersant, and D represents the average particle diameter (μm) of the negative electrode active material.] and preferably satisfies the following formula (3A): 2.15M 1 +0.00454(M 2 ×D 2 )+5.00≦DCR(0.3s)≦2.15M 1 +0.00454(M 2 ×D 2 )+7.20 (3A) [where M 1 indicates the content (mass%) of the binder. 2 represents the content (mass%) of the thickener and / or dispersant, and D represents the average particle diameter (μm) of the negative electrode active material.], and more preferably satisfies the following formula (3A1): 2.15M 1 +0.00454(M 2 ×D 2 )+5.00≦DCR(0.3s)≦2.15M 1 +0.00454(M 2 ×D 2 )+7.00 (3A1) [wherein, M 1 indicates the content (mass%) of the binder. 2 represents the content (mass %) of the thickener and / or dispersant, and D represents the average particle diameter (μm) of the negative electrode active material.] is more preferably satisfied.

[0085] In addition, during the charging process to achieve a 100% SOC described above, as described above, charging at a high load of 3.0 C may cause lithium electrodeposition at the negative electrode, and therefore it is preferable not to charge under high load conditions. Furthermore, the temperature condition is preferably 20°C or higher, which reduces resistance. Furthermore, since the purpose is to achieve a state without reaction uneven distribution before measurement by sufficiently occluding lithium ions in the negative electrode, it is preferable to charge using constant current constant voltage charging (CCCV charging) up to an upper limit voltage equivalent to a 100% SOC. Furthermore, the charge rate is preferably 0.01 to 1.0 C, more preferably 0.01 to 0.75 C. As described above, the lower limit of the charge rate is preferably 0.01 C, but it is also possible to set the lower limit to 0.02 C, 0.03 C, or the like.

[0086] In the lithium ion secondary battery of the present invention, the negative electrode active material layer-forming composition for a lithium ion secondary battery of the present invention is used in the negative electrode, and the binder content, the thickener and / or dispersant content, and the average particle size of the negative electrode active material are appropriately adjusted, so that the reaction within the battery is made uniform while maintaining a strength sufficient to maintain the shape of the electrode, and the cycle characteristics and life characteristics are significantly improved. Therefore, this lithium ion secondary battery is expected to be deployed in the market in the future, and can be effectively used for car sharing electric vehicles, particularly AIEVs (Artificial Intelligence Electric Vehicles), which are required to have even longer life.

[0087] The present invention will be specifically explained below with reference to examples, but the present invention is not limited to these examples.

[0088] Examples 1 to 5 and Comparative Examples 1 to 5 In the compositions shown in Table 1, graphite particles and single-walled carbon nanotubes (bundled single-walled CNT aggregates; average outer diameter of 2 nm, average length of >5 μm per single-walled CNT, G / D: 80 to 150) were used as the negative electrode active material, and other negative electrode constituent materials such as carbomethyl cellulose (CMC) and styrene butadiene (SBR) were added and kneaded with an appropriate amount of water to form a slurry. This slurry was applied to the copper foil and dried with a doctor blade until the weight per unit area of ​​the negative electrode active material layer was 10.3 to 10.9 mg / cm. 2 After drying at 80°C, the density of the negative electrode active material layer was 1.3 g / cm 3 The graphite particles used were spherical artificial graphite (average particle size 25.0 μm), coated natural graphite (average particle size 17.0 μm), coated natural graphite (average particle size 12.0 μm), or coated natural graphite (average particle size 5.0 μm).

[0089] Examples 6 to 9: Graphite particles as a negative electrode active material, single-walled carbon nanotubes (bundled single-walled CNT aggregates; average outer diameter 2 nm, average length > 5 μm, G / D: 80 to 150 per single-walled CNT), and an appropriate amount of NMP were kneaded to form a slurry with the composition shown in Table 1. This slurry was applied to the copper foil and dried with a doctor blade to form a negative electrode active material layer with a weight per unit area of ​​10.3 to 10.9 mg / cm. 2 After drying at 80°C, the density of the negative electrode active material layer was 1.3 g / cm 3 The graphite particles used were spherical artificial graphite (average particle size 25.0 μm), coated natural graphite (average particle size 17.0 μm), coated natural graphite (average particle size 12.0 μm), or coated natural graphite (average particle size 5.0 μm).

[0090] The compositions of the examples and comparative examples are shown in Table 1.

[0091]

[0092] Production Example: Production of Lithium-Ion Secondary Battery The negative electrodes obtained in Examples 1 to 9 and Comparative Examples 1 to 5 were used as negative electrodes.

[0093] LiNi as a positive electrode active material relative to the total mass of the positive electrode composition 0.8 Co 0.15 Al 0.05 O 2 92.0% by mass of NCA (average particle size 6 μm), 4.0% by mass of polyvinylidene fluoride (PVdF) as other positive electrode constituent materials, 4.0% by mass of acetylene black, and an appropriate amount of N-methyl-2-pyrrolidone (NMP) were mixed and kneaded to form a slurry, which was then applied to an aluminum foil (thickness 17 μm) with a doctor blade to form a positive electrode active material layer having a mass per unit area of ​​20.05 to 21.29 mg / cm after drying. 2 After drying at 100°C, the density of the positive electrode active material layer was 3.0 g / cm 3 The mixture was roll-pressed so that the thickness became 100 μm, and then dried under reduced pressure at 170° C. to obtain a positive electrode.

[0094] The electrolyte solution was a mixture of ethylene carbonate (EC) and methyl ethyl carbonate (MEC) in a volume ratio of 3:7 as a solvent, and 1 mol / L of lithium hexafluorophosphate (LiPF 6 The electrolyte solution was impregnated into a polyethylene porous film, which was used as a separator.

[0095] A lithium ion secondary battery was fabricated using the negative electrode, positive electrode, electrolyte, and separator described above. The opposing area of ​​the positive and negative electrodes of the fabricated lithium ion secondary battery was 2.8 cm 2 It was decided.

[0096] Test Example 1: Measurement of reaction resistance In the lithium ion secondary batteries of each Example and Comparative Example, the charge / discharge reaction of the graphite negative electrode active material:

[0097]

[0098] To measure the resistance to the reaction, AC impedance measurement, a common method for measuring reaction resistance, was carried out.

[0099] The reaction resistance was analyzed by taking the smallest intercept on the Z' axis in the Nyquist plot as the bulk resistance, and subtracting the bulk resistance from the arc termination resistance. Measurement conditions were 25°C, SOC (State of Charge) was 100% based on the cell voltage, amplitude was 10 mV, and frequency was 500 kHz to 0.1 Hz. An outline of the analysis method for AC impedance measurement is shown in Figure 3.

[0100] When the negative electrodes obtained in Examples 6 to 9 were used for measurement, the reaction resistance was 3.61 Ωcm in Example 6. 2 , and 3.56 Ωcm in Example 7 2 , and 3.88 Ωcm in Example 8 2 , and 3.69 Ωcm in Example 9 2 The reaction resistance generally evaluated is an index that does not include the influence of uneven distribution of the reaction, and it is assumed that it is difficult to evaluate uneven distribution of the reaction by measuring ordinary electrode resistance.

[0101] Similarly, the results of measurements using the negative electrodes obtained in each Example and Comparative Example are shown in Figure 4. From these results, it is inferred that the reaction resistance is proportional to the amount of CMC, i.e., the content of the thickener and / or thickener, and proportional to the square of the average particle size of the graphite, i.e., the negative electrode active material. Therefore, a detailed analysis was performed in Test Example 2 below.

[0102] Test Example 2: Internal resistance under high load conditions In order to confirm the degree of reaction unevenness in the lithium ion secondary batteries of each Example and Comparative Example, the resistance due to reaction inhibition was calculated by the high load rest method at room temperature (25°C).

[0103] Specifically, the lithium ion secondary batteries using the negative electrodes of each Example and Comparative Example were subjected to constant current constant voltage (CCCV) charging at room temperature (25°C) with a charge rate of 0.5C and a cut current of 0.05C up to an upper limit voltage of 4.0V, corresponding to an SOC of 100%. Next, after a 10-minute pause, the batteries were discharged (for 2 minutes) to an SOC of 90% at a discharge rate of 3.0C, and then paused for 10 minutes. The charge rate SOC is defined by the following formula (2): SOC (%) = remaining capacity (Ah) / full charge capacity (Ah) × 100 (2)

[0104] As shown in Figure 2, the voltage rise observed during the pause period includes a voltage rise due to reaction inhibition observed at the very beginning of the pause period and a voltage rise due to ion migration inhibition observed thereafter. The voltage rise due to reaction inhibition is due to the uneven distribution of the reaction at the particle level, and is observed when the reaction is unevenly distributed due to the presence of reaction inhibitors such as the negative electrode active material and negative electrode constituent materials other than carbon nanotubes, and the voltage rises sharply at the very beginning of the pause period. On the other hand, the voltage rise due to ion migration inhibition is due to the uneven distribution of the reaction at the structural level, and is observed when lithium ions move due to the uneven distribution of ion migration inhibitors such as the negative electrode active material and negative electrode constituent materials other than carbon nanotubes, and the voltage rise gradually slows down at periods other than the very beginning of the pause period.

[0105] From the above, the voltage rise due to reaction inhibition was measured from the voltage rise observed at the beginning of the rest period, and the resistance due to reaction inhibition was calculated using the following formula: Resistance due to reaction inhibition DCR (0.3 s) = (voltage rise due to reaction inhibition (V) / current value during discharge "current value at 3.0 C (A)") × opposing area of ​​positive and negative electrodes "2.8 cm 2 ") was calculated.

[0106] The results of these high load resting methods are shown in Table 2.

[0107]

[0108] From the results obtained above, multiple regression analysis was performed to obtain the following formula: DCR (0.3s) = 2.15M 1 +0.00454(M 2×D 2 )+6.54 [wherein, M 1 indicates the content (mass%) of the binder. 2 indicates the content (mass %) of the thickener and / or dispersant, and D indicates the average particle diameter (μm) of the negative electrode active material.]

[0109] The correlation between the calculated value of the reaction resistance DCR (0.3s) using this calculation formula and the measured value of DCR (0.3s) is shown in Figure 5. As a result, the calculated value of the reaction resistance DCR (0.3s) using this calculation formula and the measured value of DCR (0.3s) show a very good correlation, and the statistical coefficient of determination R 2 It can be seen that the value is 0.94, which is very close to 1.

[0110] Test Example 3: Load Cycle Test The lithium ion secondary batteries using the negative electrodes of Examples 1, 3, and 6 to 8 and Comparative Examples 1 to 3 were subjected to constant current charging (CC charging) at a charge rate of 0.75 C to an upper limit voltage of 4.0 V at 0° C., followed by a 10-minute pause, followed by constant current discharging (CC discharging) at a discharge rate of 0.75 C to a lower limit voltage of 2.7 V, followed by a 10-minute pause. These charge and discharge steps constitute one cycle, and a charge and discharge cycle test was performed for 10 cycles.

[0111] The results of the charge-discharge cycle characteristics are shown in Table 3.

[0112]

[0113] As a result, DCR (0.3 s) = 2.15 M 1 +0.00454(M 2 ×D 2 ) + 6.54 is 7.48 or more, the cycle characteristics deteriorate even after only 10 cycles. 1 +0.00454(M 2 ×D 2 ) + 6.54≦7.40 is required.

Claims

1. A negative electrode active material containing at least a negative electrode active material and a carbon nanotube, and having the following formula (1): 2.15M 1 +0.00454(M 2 xD 2 )+6.54≦7.40 (1) [wherein, M 1 indicates the content (mass%) of the binder. 2 represents the content (mass %) of the thickener and / or dispersant, and D represents an average particle size (μm) of the negative electrode active material.

2. The composition for forming a negative electrode active material layer for a lithium ion secondary battery according to claim 1, wherein, assuming a total amount of the composition to be 100% by mass, the content of the negative electrode active material is 96.6 to 99.9% by mass, the content of the carbon nanotubes is 0.01 to 1.4% by mass, the content of negative electrode constituent materials other than the negative electrode active material and the carbon nanotubes is 0 to 2.0% by mass, and the average particle size of the negative electrode active material is 0.1 to 30.0 μm.

3. The composition for forming a negative electrode active material layer for a lithium ion secondary battery according to claim 1 or 2, wherein the negative electrode active material is a material capable of absorbing and releasing lithium ions.

4. The composition for forming a negative electrode active material layer for a lithium ion secondary battery according to any one of claims 1 to 3, wherein the carbon nanotubes are single-walled carbon nanotubes.

5. The composition for forming a negative electrode active material layer for a lithium ion secondary battery according to any one of claims 1 to 4, which is used to reduce uneven distribution of reactions in a lithium ion secondary battery.

6. The composition for forming a negative electrode active material layer for a lithium ion secondary battery according to any one of claims 1 to 5, which is for a lithium ion secondary battery used in an electric vehicle for car sharing.

7. A negative electrode active material layer for a lithium ion secondary battery, comprising the composition for forming a negative electrode active material layer for a lithium ion secondary battery according to any one of claims 1 to 6.

8. The negative electrode active material layer for a lithium ion secondary battery according to claim 7, which is for a lithium ion secondary battery used in an electric vehicle for car sharing.

9. A negative electrode for a lithium ion secondary battery comprising the negative electrode active material layer for a lithium ion secondary battery according to claim 7 or 8.

10. The negative electrode for a lithium ion secondary battery according to claim 9, which is for a lithium ion secondary battery used in an electric vehicle for car sharing.

11. A lithium ion secondary battery comprising the negative electrode for lithium ion secondary batteries according to claim 9 or 10.

12. The charging rate SOC is defined as the following formula (2): SOC (%) = remaining capacity (Ah) / full charge capacity (Ah) × 100 (2), and after discharging from an SOC of 100% to an SOC of 90% under conditions of 25°C and 3.0C, the battery is left at rest for 10 minutes and the increase in voltage during the rest period is measured, and from the measured increase in voltage, the reaction resistance is separated into two components, a resistance DCR (0.3s) due to reaction inhibition and a resistance DCR (0.3s-10min) due to ion migration inhibition, and the resistance DCR (0.3s) is calculated, and the resistance DCR (0.3s) due to reaction inhibition is calculated based on the following formula (3): 2.15M 1 +0.00454(M 2 xD 2 )+5.00≦DCR(0.3s)≦2.15M 1 +0.00454(M 2 xD 2 )+7.40 (3) [wherein, M 1 indicates the content (mass%) of the binder. 2 The lithium ion secondary battery according to claim 11 , wherein R represents the content (mass%) of the thickener and / or dispersant, and D represents an average particle diameter (μm) of the negative electrode active material.

13. The lithium ion secondary battery according to claim 11 or 12, which is used in an electric vehicle for car sharing.

Citation Information

Patent Citations

  • Charger and charging method

    JP2013070500A

  • Electric vehicle

    JP2018121411A

  • Self-supporting electrode and method of manufacturing the same

    JP2019050186A

  • Negative electrode for secondary battery, secondary battery, and manufacturing method of negative electrode for secondary battery

    JP2023126032A

  • Electrode structure

    WO2017199884A1