Biaxially oriented polyamide film
A biaxially stretched polyamide film with specific composition and orientation enhances bending pinhole resistance, puncture strength, and ethanol permeability, addressing the challenges of existing films by incorporating a resin with a large dispersion diameter and controlled crystallinity, suitable for food and alcohol transpiration packaging.
Patent Information
- Application Number
- PCT/JP2024/011079
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-30
- Filing Date
- 2024-03-21
- Publication Date
- 2024-10-03
AI Technical Summary
Biaxially stretched polyamide films used for food packaging and alcohol transpiration agents face challenges with balancing bending pinhole resistance, puncture strength, dimensional stability, and ethanol permeability, with existing films often compromising on strength or permeability.
A biaxially stretched polyamide film with polyamide 6 as the main component, incorporating a resin with a maximum dispersion diameter of 1 μm or more, and a specific planar orientation, achieving excellent bending pinhole resistance, puncture strength, and ethanol permeability by controlling crystallinity and layer composition.
The film exhibits improved bending pinhole resistance, puncture strength, and ethanol permeability, maintaining dimensional stability while ensuring sufficient mechanical strength and ethanol transmission for food packaging and transpiration applications.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002 
Figure JPOXMLDOC01-APPB-T000003
Abstract
Description
Biaxially oriented polyamide film
[0001] The present invention relates to a biaxially oriented polyamide film suitable for use as a food packaging film, a packaging material for alcohol-evaporating agents, etc.
[0002] Biaxially stretched films made of aliphatic polyamides, such as polyamide 6, have excellent impact resistance and pinhole resistance due to bending, and are widely used as various packaging film materials. Patent Documents 1 and 2 disclose that polyamide films generally have high alcohol permeability, and are therefore also used as base films for packaging bags for alcohol-evaporating agents and freshness-preserving packaging bags, which require specific gas permeability. Patent Document 3 discloses that desired gas permeability can be obtained by reducing the thickness of the biaxially stretched polyamide film.
[0003] JP 2003-211604 A JP 2002-204652 A JP 2010-167652 A
[0004] Although Patent Document 3 shows that reducing the thickness of a nylon film is effective in improving ethanol permeability, the inventors have found that reducing the film thickness leads to problems such as reduced pinhole resistance and puncture strength. Patent Document 3 also found that there is room for improvement in the dimensional stability of the film.
[0005] An object of the present invention is to provide a biaxially oriented polyamide film that is excellent in flexural pinhole resistance, puncture strength, dimensional stability, and ethanol permeability.
[0006] The present inventors conducted extensive research to achieve the above object and discovered that by dispersing a resin other than polyamide 6 having a maximum dispersion diameter of 1 μm or more in a polyamide 6 resin in a biaxially oriented polyamide film and imparting a specific degree of planar orientation and a specific degree of crystallinity, a biaxially oriented polyamide film with good bending pinhole resistance, puncture strength, dimensional stability, and ethanol permeability can be obtained. After further research and improvements, the inventors have completed the following representative inventions.
[0007] [1] A biaxially stretched polyamide film containing polyamide 6 as a main constituent, having an ethanol permeability of 6000 to 10000 g μm / m 2a biaxially oriented polyamide film having a thickness of 15 μm or less, a thermal shrinkage of 2.0% or less in both the machine direction and the width direction of the film when heat-treated at 160°C for 10 minutes, a surface crystallization parameter of 1.0 to 1.5, and a puncture strength of 6.0 N or more after 24 hours (50% RH / 40°C); [2] The biaxially oriented polyamide film according to [1], which has at least one layer containing 60% to 99% by mass of polyamide 6 resin (a) and 2% to 40% by mass of resin (b) other than polyamide 6. [3] The biaxially oriented polyamide film according to [2], wherein the resin (b) other than polyamide 6 is at least one selected from the group consisting of thermoplastic elastomers such as polyolefins, ionomer polymers, polyester elastomers, polyamide elastomers, polyolefin elastomers, polystyrene elastomers, polyurethane elastomers, and polyvinyl chloride elastomers, aliphatic polyester resins, aliphatic-aromatic polyester resins, aliphatic polyamide resins, and aliphatic-aromatic polyamide resins. [4] The biaxially oriented polyamide film according to [2] or [3], wherein the aliphatic-aromatic polyester resin is polybutylene adipate terephthalate resin. [5] The biaxially oriented polyamide film according to [2], wherein the resin (b) other than polyamide 6 is biomass-derived and is at least one polyamide selected from the group consisting of polyamide 11, polyamide 410, polyamide 610, and polyamide 1010. [6] The biaxially stretched polyamide film according to any one of [2] to [5], wherein the maximum dispersed diameter of the resin (b) other than polyamide 6 is 1 μm or more. [7] The biaxially stretched polyamide film according to any one of [1] to [6], wherein the stress at 5% elongation in both the machine direction and the width direction of the film is 70.0 MPa or less. [8] The biaxially stretched polyamide film according to any one of [1] to [7], wherein the degree of planar orientation (ΔP) is 0.050 or more.[9] The biaxially oriented polyamide film according to any one of [1] to [8], wherein a laminate film of the biaxially oriented polyamide film and a 40 μm-thick polyethylene film is prepared, and when the laminate film is subjected to 1,000 flexing treatments using a Gelbo flex tester in an atmosphere at a temperature of 1° C., the number of pinholes that develops is 20 or less.
[10] A food packaging material comprising the biaxially oriented polyamide film according to any one of [1] to [9] and a sealant film.
[11] A packaging material for an ethanol-transporting agent, comprising a laminate including the biaxially oriented polyamide film according to any one of [1] to [9] and at least two layers of a breathable resin film or a nonwoven fabric.
[0008] The present invention provides a biaxially oriented polyamide film that is excellent in bending pinhole resistance, puncture strength, dimensional stability, and ethanol permeability, as well as a food packaging material and an ethanol-transpirable agent packaging material that use the biaxially oriented polyamide film.
[0009] 1 is a transmission electron microscope photograph showing the dispersion state of polyamide 6 resin (a) and resin other than polyamide 6 (b) contained in a film.
[0010] The biaxially stretched polyamide film of the present invention will be described in detail below. In this specification, a numerical range expressed using "to" means a range that includes the numerical values written before and after "to" as the lower and upper limits.
[0011] The biaxially oriented polyamide film of the present invention preferably contains polyamide 6 as a major component. Here, "containing polyamide 6 as a major component" means that the content of this component in the polyester resin composition constituting the film is 50% by mass or more, preferably 60% by mass or more, more preferably 70% by mass or more, and even more preferably 80% by mass or more, based on 100% by mass of all components of the polyester resin. The biaxially oriented polyamide film of the present invention is preferably a biaxially oriented polyamide film having a functional layer laminated on at least one side of a substrate layer. The biaxially oriented polyamide film of the present invention is preferably a film having at least two layers: a substrate layer and a functional layer. It may have a two-layer structure of substrate layer / functional layer or a three-layer structure of functional layer / substrate layer / functional layer. Details of each layer are described below.
[0012] [Substrate Layer A] The first resin composition forming the substrate layer contains at least a polyamide 6 resin (a). The first resin composition preferably contains 60% by mass or more of polyamide 6, more preferably 80% by mass or more, and even more preferably 85% by mass or more, based on 100% by mass of the first resin composition. A polyamide 6 content below 60% may result in a decrease in impact resistance and a significant increase in gas permeability. By containing 80% by mass or more of polyamide 6, a polyamide film having mechanical strength such as impact strength and gas barrier properties can be obtained. The upper limit of the polyamide 6 content is preferably 98% by mass or less, more preferably 97% by mass or less, based on 100% by mass of the first resin composition. That is, the polyamide 6 content is preferably 60 to 98% by mass, more preferably 80 to 98% by mass, and even more preferably 85 to 97% by mass. Note that, in this specification, the upper and lower limits of the numerical ranges may be appropriately combined to obtain a suitable numerical range (the same applies hereinafter to the numerical ranges).
[0013] The first resin composition forming the base layer contains at least one resin (b) other than polyamide 6. The resin (b) is a substance that is effective in imparting flexibility to the base layer and is not particularly limited as long as it is incompatible with polyamide 6, but is preferably at least one selected from the group consisting of thermoplastic elastomers such as polyolefins, ionomer polymers, polyester-based elastomers, polyamide-based elastomers, polyolefin-based elastomers, polystyrene-based elastomers, polyurethane-based elastomers, and polyvinyl chloride-based elastomers, aliphatic polyester resins, aliphatic-aromatic polyester resins, aliphatic polyamide resins, and aliphatic-aromatic polyamide resins.
[0014] Examples of polyolefins include olefin homopolymers, copolymers of olefins with other monomers, and mixtures thereof, as well as polyolefins graft-polymerized with unsaturated carboxylic acids. Examples of olefin homopolymers include polyethylene (high density, low density) and polypropylene. Examples of copolymers of olefins with other monomers include ethylene-vinyl acetate copolymer, ethylene-propylene copolymer, ethylene-butene copolymer, ethylene-acrylic acid copolymer, and ethylene-methacrylic acid copolymer. Examples of unsaturated carboxylic acids used in polyolefins graft-polymerized with unsaturated carboxylic acids include acrylic acid, methacrylic acid, maleic acid, fumaric acid, itaconic acid, citraconic acid, and other carboxylic acids, as well as acid anhydrides such as maleic anhydride, citraconic anhydride, and itaconic anhydride. Unsaturated carboxylic acids may be used alone or in combination.
[0015] An ionomeric polymer is a polymer composed of a polyolefin and an α,β-ethylenically unsaturated monomer having a carboxyl moiety, the carboxyl moiety being neutralized with a metal ion having a valence of 1 to 3. Examples of polyolefins include copolymers of polyethylene or ethylene with at least one α-olefin having typically 3 to 8 carbon atoms and a diolefin, such as 1,4-hexadiene. Examples of α,β-ethylenically unsaturated monomers having a carboxyl moiety include methacrylic acid, acrylic acid, maleic acid, maleic anhydride, and fumaric acid. Examples of metal ions include zinc ions, sodium ions, lithium ions, potassium ions, and magnesium ions. Ionomeric polymers are produced by a direct synthesis method in which an α-olefin and an olefin monomer having a carboxyl moiety are polymerized, or by a grafting method in which a monomer having a carboxyl moiety is added to the olefin backbone.
[0016] Examples of thermoplastic elastomers include thermoplastic elastomers such as polyolefins, ionomer polymers, polyester elastomers, polyamide elastomers, polyolefin elastomers, polystyrene elastomers, polyurethane elastomers, and polyvinyl chloride elastomers, as well as aliphatic polyester resins, aliphatic aromatic polyester resins, aliphatic polyamide resins, and aliphatic aromatic polyamide resins. For example, polyamide elastomers, polyester elastomers, polyurethane elastomers, acrylic thermoplastic elastomers, polystyrene elastomers, and hydrogenated products thereof may also be used.
[0017] Examples of polyamide elastomers include polyether amides, polyether ester amides, and polyester amides. The polyamide elastomers may be copolymerized with dicarboxylic acids such as dodecanedicarboxylic acid, adipic acid, and terephthalic acid as optional components.
[0018] The polyester elastomer refers to a block copolymer composed of a crystalline hard segment and a flexible soft segment. Among them, a block copolymer having a hard segment made of a cyclic polyester and a soft segment made of a polyalkylene ether, and a block copolymer having a hard segment made of a cyclic polyester and a soft segment made of a linear aliphatic polyester are preferred, and a cyclic polyester-polyalkylene ether block copolymer is more preferred. In the present invention, the term "cyclic polyester" refers to a raw material containing a dicarboxylic acid or an alkyl ester thereof having a cyclic structure.
[0019] From the viewpoint of moldability, examples of polyurethane-based thermoplastic elastomers include those having a hard segment composed of a diisocyanate compound and a glycol having a molecular weight of approximately 50 to 500, and a soft segment composed of a diisocyanate compound and a long-chain glycol. Examples of the long-chain glycol include polyether-based compounds such as polyalkylene glycols having a molecular weight of approximately 500 to 10,000, and polyester-based compounds such as polyalkylene adipate, polycaprolactone, and polycarbonate. Examples of diisocyanate compounds include phenylene diisocyanate, triisocyanate, xylene diisocyanate, 4,4-diphenylmethane diisocyanate, and hexamethylene diisocyanate. The diisocyanate compounds in the soft and hard segments may be the same or different.
[0020] Examples of acrylic thermoplastic elastomers include ethylene-acrylic ester copolymer elastomers, ethylene-methacrylic ester copolymer elastomers, and acrylic ABA triblock copolymers composed of acrylic esters and methacrylic esters.
[0021] Examples of polystyrene elastomers include styrene-butadiene copolymer rubber and styrene-isoprene copolymer rubber.
[0022] As the aliphatic polyester resin, polybutylene succinate and polybutylene succinate adipate are preferably used. As the aliphatic aromatic polyester resin, an aliphatic aromatic polyester resin containing an adipic acid component is preferred, and polybutylene adipate terephthalate is particularly preferred. More preferred is an aliphatic or aliphatic aromatic polyester resin having a glass transition temperature (Tg) of -30°C or less. By using a polyester copolymer having a glass transition temperature of -30°C or less, excellent pinhole resistance can be achieved even in a freezing environment.
[0023] Preferred aliphatic polyamide resins include polyamide 11, polyamide 610, polyamide 1010, and polyamide 410. Furthermore, polyamide resins may be made from at least a portion of biomass-derived raw materials. By incorporating a polyamide resin containing biomass-derived raw materials, flex pinhole resistance can be further improved. Aliphatic aromatic polyamide resins include polymetaxylylene adipamide (MXD6), polyamide 6T, polyamide 6I, polyamide 6T6I, and polyamide 9T. Among these, MXD6 is preferred from the viewpoint of improving stretchability and adhesiveness.
[0024] The content of the resin (b) other than polyamide 6 contained in the first resin composition forming the base layer is preferably 2% by mass or more to 40% by mass or less, or 20% by mass or less, and more preferably 4% by mass or more to 15% by mass, based on 100% by mass of the first resin composition. By including 2% by mass or more of the resin (b) other than polyamide 6, the effect of pinhole resistance can be obtained. By including 40% by mass or less, preferably 20% by mass or less, of the resin (b) other than polyamide 6, the film becomes soft, preventing a decrease in puncture strength and impact strength. Furthermore, the film becomes more stretchable, preventing pitch deviation during processing such as printing.
[0025] The first resin composition forming the base layer may contain a thermoplastic resin other than polyamide 6 resin, provided that the object of the present invention is not impaired. Examples include polyamide-based resins such as polyamide 12 resin, polyamide 66 resin, polyamide 6-12 copolymer resin, polyamide 6-66 copolymer resin, polyamide MXD6 resin, polyamide MXD10 resin, and polyamide 11-6T copolymer resin. If necessary, a thermoplastic resin other than polyamide may be contained, such as a polyester-based polymer such as polyethylene terephthalate, polybutylene terephthalate, or polyethylene-2,6-naphthalate, or a polyolefin-based polymer such as polyethylene or polypropylene.
[0026] The substrate layer may contain various additives such as other thermoplastic resins, lubricants, heat stabilizers, antioxidants, antistatic agents, anti-fogging agents, ultraviolet absorbers, dyes, and pigments, as required.
[0027] [Functional Layer B] The second resin composition forming the functional layer preferably contains at least polyamide 6. The second resin composition preferably contains 70% by mass or more of polyamide 6, more preferably 80% by mass or more, and particularly preferably 90% by mass or more, based on 100% by mass of the second resin composition. By including 70% by mass or more of polyamide 6, a polyamide film having mechanical strength such as impact strength and gas barrier properties can be obtained. The upper limit of the polyamide 6 content is preferably 99% by mass or less, more preferably 96% by mass or less, based on 100% by mass of the first resin composition. That is, the polyamide 6 content is preferably 70 to 99% by mass, more preferably 80 to 96% by mass, and even more preferably 90 to 96% by mass. The polyamide 6 may be the same as the polyamide 6 used in the first resin composition.
[0028] The second resin composition forming the functional layer may contain a polyamide-based resin other than polyamide 6. Examples of polyamide-based resins other than polyamide 6 include polyamide MXD6 resin, polyamide 11, polyamide 12, and polyamide 66. When the second resin composition contains a polyamide-based resin other than polyamide 6, the content thereof is preferably 1% by mass or more and 30% by mass or less, more preferably 3% by mass or more and 20% by mass or less, and particularly preferably 5% by mass or more and 10% by mass or less, based on 100% by mass of the second resin composition. By containing 1% by mass or more, slip properties of the film can be imparted. On the other hand, if the content is more than 30% by mass, the effect of improving the slip properties of the film may become saturated. As the polyamide-based resin other than polyamide 6, polyamide MXD6 resin is preferably used.
[0029] The second resin composition forming the functional layer may contain fine particles, an organic lubricant, or the like as a lubricant to improve the film's slipperiness. By improving the slipperiness, the film's handling properties are improved and the breakage of the packaging bag due to friction can be reduced.
[0030] The fine particles can be appropriately selected from inorganic fine particles such as silica, kaolin, zeolite, etc., and polymeric organic fine particles such as acrylic and polystyrene fine particles, etc. From the viewpoints of transparency and lubricity, it is preferable to use silica fine particles.
[0031] The average particle size of the fine particles is preferably 0.5 μm or more and 5.0 μm or less, more preferably 1.0 μm or more and 3.0 μm or less. When the average particle size is 0.5 μm or more, good slip properties can be expected, and when it is 5.0 μm or less, it can be expected to prevent poor appearance due to increased surface roughness of the film.
[0032] When silica fine particles are used as the fine particles, the pore volume of the silica is preferably in the range of 0.5 ml / g to 2.0 ml / g, more preferably 0.8 ml / g to 1.6 ml / g.
[0033] The organic lubricant can be a fatty acid amide and / or a fatty acid bisamide. Examples of the fatty acid amide and / or a fatty acid bisamide include erucamide, stearamide, ethylene bisstearamide, ethylene bisbehenamide, and ethylene bisoleamide. The content of the fatty acid amide and / or fatty acid bisamide contained in the second resin composition forming the functional layer is preferably 0.01% by mass or more and 0.40% by mass or less, and more preferably 0.05% by mass or more and 0.30% by mass or less, based on 100% by mass of the second resin composition. A content of 0.01% by mass or more can be expected to provide a slipperiness effect. A content of 0.40% by mass or less can ensure wettability of the printing ink when a printing layer is provided on the functional layer side.
[0034] The functional layer may contain various additives such as other thermoplastic resins, lubricants, heat stabilizers, antioxidants, antistatic agents, anti-fogging agents, ultraviolet absorbers, dyes, and pigments.
[0035] [Biaxially oriented polyamide film] The biaxially oriented polyamide film of the present invention is preferably a film having at least two layers: a substrate layer and a functional layer, and may have a two-layer structure of substrate layer / functional layer or a three-layer structure of functional layer / substrate layer / functional layer.
[0036] The ethanol permeability of the biaxially stretched polyamide film of the present invention is 6000 g μm / m 2 Preferably, the permeability is 24 hours (50% RH / 40°C) or more. When the biaxially stretched polyamide film of the present invention is used as a packaging material for an ethanol evaporative agent, the ethanol impregnated into the nonwoven fabric as an ethanol evaporative agent slowly evaporates, and a sufficient ethanol gas concentration can be obtained to maintain the freshness of food in the food packaging. The ethanol permeability is 6000 g μm / m 2 If the temperature is lower than 24 hours (50% RH / 40°C), the permeation of the alcohol gas evaporating from the alcohol evaporating agent is inhibited, and it may not be possible to obtain a sufficient alcohol gas concentration to maintain the freshness of the food inside the food packaging, which is not preferable. 224 hours (50% RH / 40°C) or less is preferable. 2 By keeping the temperature at 50% RH / 40°C or less for 24 hours, it is possible to prevent condensation of ethanol inside the package, which would occur if the amount of ethanol permeated were large.
[0037] The thickness of the biaxially oriented polyamide film of the present invention is preferably 15 μm or less, more preferably 5 to 12 μm. A thickness of 15 μm or less provides excellent alcohol permeability and contributes to resource conservation and waste reduction. A thickness of 5 μm or more is preferred because it provides sufficient mechanical strength required for secondary processing such as lamination, coating, and slitting.
[0038] The thickness of the substrate layer is preferably 50% to 90% and particularly preferably 60% to 80% of the total thickness of the substrate layer and the functional layer (when a plurality of substrate layers and functional layers are present, the total thickness of each). By making the thickness of the substrate layer 50% or more, bending pinhole resistance can be imparted. By making the thickness of the substrate layer 90% or less, friction pinhole resistance in the functional layer can be imparted.
[0039] The biaxially stretched polyamide film of the present invention preferably has an F5 value, i.e., a stress at 5% elongation obtained by a tensile test in the machine direction and width direction of the film, of 70 MPa or less. It is more preferably 60 MPa or less, and even more preferably 50 MPa or less. By keeping the F5 value at 70 MPa or less, the film becomes flexible and less susceptible to breakage due to flex fatigue. The lower limit of the F5 value is preferably 20 MPa or more. An F5 value of 20 MPa or more is preferable in terms of preventing print pitch deviation due to film elongation during secondary processing. That is, the F5 value is preferably 20 to 70 MPa, more preferably 20 to 60 MPa, and even more preferably 20 to 50 MPa. Methods for achieving an F5 value of 20 MPa or more and 70 MPa or less include low-magnification stretching, high-temperature stretching, and the addition of a resin other than nylon 6. From the viewpoint of productivity, the addition of a resin other than nylon 6 is preferred.
[0040] The biaxially stretched polyamide film of the present invention has excellent pinhole resistance when subjected to a twist bending test using a Gelbo flex tester 1,000 times at a temperature of 1° C., and the number of pinhole defects is 1,520 or less, more preferably 15 or less, and even more preferably 10 or less. The fewer the number of pinhole defects after the bending test, the better the pinhole resistance when bending. If the number of pinholes is preferably 1,520 or less, more preferably 15 or less, a packaging bag that is less likely to develop pinholes even when a load is applied to the packaging bag during transportation, etc. can be obtained.
[0041] The biaxially stretched polyamide film of the present invention has a peak at 1200 cm in the spectrum obtained by ATR measurement of FT-IR. -1 Nearby and 1370 cm -1 The crystallization parameter (1200 cm) calculated from the intensity ratio of the peaks around -1 / 1370cm -1 ) is preferably 1.0 or more. -1 The peak at 1370 cm is the absorption due to the α crystal of nylon 6. -1 is absorption unrelated to crystallization. Dimensional stability can be obtained by setting this crystallization parameter in the range of 1.0 to 1.5. Dimensional stability is improved by setting the crystallization parameter to 1.0 or more. Mechanical strength can be maintained by setting the crystallization parameter to 1.5 or less.
[0042] The biaxially stretched polyamide film of the present invention preferably has a heat shrinkage rate at 160°C for 10 minutes in the machine direction (hereinafter sometimes abbreviated as MD direction) and the width direction (hereinafter sometimes abbreviated as TD direction) of 0.6% to 3.0%, more preferably 0.5% to 2.0%. A heat shrinkage rate of 3.0% or less can suppress curling and shrinkage when heat is applied in subsequent processes such as lamination and printing. A heat shrinkage rate of 0.6% or more is preferred in terms of excellent impact resistance.
[0043] The planar orientation (ΔP) of the biaxially stretched polyamide film of the present invention is preferably 0.050 to 0.070. Planar orientation can be determined by measuring birefringence with a refractometer and using the following formula, where Nx is the refractive index in the machine direction, Ny is the refractive index in the width direction, and Nz is the refractive index in the thickness direction: ΔP = (Nx + Ny) / 2 - Nz. Planar orientation can be increased by increasing the biaxial stretching ratio, particularly the stretching ratio in the TD direction. A planar orientation of 0.05 or more ensures the film's mechanical strength, such as puncture resistance. Furthermore, a planar orientation of 0.07 or less can prevent a decrease in productivity.
[0044] The impact strength of the biaxially stretched polyamide film of the present invention is preferably 0.6 J or more, more preferably 0.7 J or more.
[0045] The puncture strength of the film of the present invention is preferably 6.0 N or more. By setting the puncture strength to 6.0 N or more, even when filled with solid contents, it is possible to prevent the contents from puncturing the bag and causing a hole in the bag, or to prevent the bag from being caused by external factors during transportation. The upper limit of the puncture strength is not particularly limited, but it may be 100 N or less, or may be 50 N or less.
[0046] The maximum dispersion diameter of the resin (b) other than polyamide 6 contained in the base layer is preferably 1.0 μm or more. Here, the maximum dispersion diameter refers to the longest length (unit: μm) of the resin (b) dispersed in the base layer when the base layer is observed with a transmission electron microscope (TEM). An example is shown in Figure 1. Figure 1 is a photograph of a cross section of the film in the machine direction observed with a transmission electron microscope at 2000x magnification, and the darkly stained domains are resin (b). When the dispersion diameter of resin (b) is 1.0 μm or more, good bending pinhole resistance and ethanol permeability are obtained. The reason for good bending pinhole resistance is believed to be that the dispersion of flexible resin (b), which is incompatible with polyamide 6, improves the overall flexibility of the film, making it less susceptible to fracture due to bending fatigue. The reason for good ethanol permeability is believed to be that the incompatible dispersion of resin (b) in polyamide 6 forms an interface with weak adhesion between polyamide 6 and resin (b), allowing ethanol to permeate the film through this interface. If the maximum dispersed diameter of resin (b) is less than 1.0 μm, compatibility is promoted and the characteristics of the base material, polyamide 6, become apparent, resulting in a decrease in pinhole resistance and ethanol permeability.
[0047] [Method for Producing Biaxially Stretched Polyamide Film] The method for producing the biaxially oriented polyamide film of the present invention will be described below. First, the raw material resin is melt-extruded using an extruder, extruded into a film form through a T-die, and cast onto a cooling roll and cooled to obtain an unstretched film laminated with at least a substrate layer and a functional layer. To obtain an unstretched laminated film, a co-extrusion method using a feed block or multi-manifold is preferred. In addition to co-extrusion, dry lamination, extrusion lamination, etc. can also be selected. When laminating by co-extrusion, it is desirable to minimize the difference in melt viscosity between the first resin composition forming the substrate layer and the second resin composition forming the functional layer.
[0048] The melting temperature of the resin is preferably 220°C or higher and 350°C or lower. If the temperature is lower than this range, unmelted material may be generated, resulting in defects and other poor appearance. If the temperature is higher than this range, resin degradation may be observed, resulting in a decrease in molecular weight and a deterioration in appearance. The die temperature is preferably 250°C or higher and 350°C or lower. The chill roll temperature is preferably -30°C or higher and 80°C or lower, more preferably 0°C or higher and 50°C or lower. To obtain an unstretched film by casting and cooling a film-like molten material extruded from a T-die onto a rotating cooling drum, methods such as using an air knife or an electrostatic adhesion method in which an electrostatic charge is applied are preferably used. It is also preferable to cool the surface of the cast unstretched film opposite the chill roll. For example, it is preferable to use a combination of methods such as contacting the surface of the unstretched film opposite the chill roll with a cooling liquid in a tank, applying a vaporizing liquid with a spray nozzle, or spraying a high-speed fluid for cooling. The unstretched film thus obtained is biaxially stretched to obtain the biaxially stretched polyamide film of the present invention.
[0049] The stretching method may be either a simultaneous biaxial stretching method or a sequential biaxial stretching method. The sequential biaxial stretching method is preferred because it has the advantages of increasing the degree of planar orientation and making it easier to obtain puncture strength, easily adjusting the crystallization parameters to obtain the desired dimensional stability, and increasing the film production speed, making it easier to reduce production costs. In either case, multi-stage stretching such as one-stage stretching or two-stage stretching can be used as the MD stretching method. As will be described later, multi-stage MD stretching such as two-stage stretching is preferred over single-stage stretching in terms of physical properties and uniformity of physical properties in the MD and TD directions (isotropy). Roll stretching is preferred for MD stretching in the sequential biaxial stretching method.
[0050] The lower limit of the MD stretching temperature is preferably 50°C, more preferably 55°C, and even more preferably 60°C. If the temperature is below 50°C, the resin does not soften and stretching may be difficult. The upper limit of the MD stretching temperature is preferably 120°C, more preferably 115°C, and even more preferably 110°C. If the temperature exceeds 120°C, the resin may become too soft and stable stretching may not be possible. Stretching at 120°C or less is preferred in terms of preventing sticking to the roll and breakage. That is, the MD stretching temperature is preferably 50 to 120°C, more preferably 55 to 115°C, and even more preferably 60 to 110°C.
[0051] The lower limit of the stretching ratio in the MD direction (when stretching is performed in multiple stages, the total stretching ratio obtained by multiplying each stretching ratio) is preferably 2.2 times, more preferably 2.5 times, and even more preferably 2.8 times. If it is less than 2.2 times, the thickness accuracy in the MD direction will decrease, and the crystallinity will become too low, which may result in a decrease in impact strength. The upper limit of the stretching ratio in the MD direction is preferably 5.0 times, more preferably 4.5 times, and most preferably 4.0 times. A stretching ratio of 5.0 times or less is preferable from the viewpoint of achieving both productivity and film formation stability. That is, the stretching ratio in the MD direction is preferably 2.2 to 5.0 times, more preferably 2.5 to 4.5 times, and even more preferably 2.8 to 4.0 times.
[0052] Furthermore, when stretching in the MD direction is performed in multiple stages, the above-mentioned stretching is possible in each stretching, but it is preferable to adjust the stretching ratio so that the product of all stretching ratios in the MD direction is 5.0 or less. For example, in the case of two-stage stretching, it is preferable that the first-stage stretching is 1.5 to 2.1 times, and the second-stage stretching is 1.5 to 1.8 times.
[0053] The film stretched in the MD direction is stretched in the TD direction using a tenter, heat-set, and then relaxed (also referred to as relaxation treatment). The lower limit of the TD stretching temperature is preferably 50°C, more preferably 55°C, and even more preferably 60°C. If the temperature is below 50°C, the resin does not soften, making stretching difficult. The upper limit of the TD stretching temperature is preferably 190°C, more preferably 185°C, and even more preferably 180°C. Setting the TD stretching temperature to 190°C or less is preferable from the viewpoint of suppressing film crystallization and preventing breakage. That is, the TD stretching temperature is preferably 50 to 190°C, more preferably 55 to 185°C, and even more preferably 60 to 180°C.
[0054] The lower limit of the stretching ratio in the TD direction (when stretching in multiple stages, the total stretching ratio obtained by multiplying each stretching ratio) is preferably 2.8 times, more preferably 3.2 times, even more preferably 3.5 times, and particularly preferably 3.8 times. If it is less than 2.8 times, the thickness accuracy in the TD direction will decrease, and the crystallinity will be too low, which may result in a decrease in impact strength. The upper limit of the stretching ratio in the TD direction is preferably 5.5 times, more preferably 5.0 times, even more preferably 4.7 times, particularly preferably 4.5 times, and most preferably 4.3 times. A stretching ratio of 5.5 times or less in the TD direction is preferable from the viewpoint of preventing breakage. That is, the stretching ratio in the TD direction is preferably 2.8 to 5.5 times, more preferably 3.2 to 5.0 times, even more preferably 3.5 to 4.7 times, particularly preferably 3.8 to 4.5 times, and most preferably 3.8 to 4.3 times.
[0055] The lower limit of the heat setting temperature is preferably 210°C, more preferably 212°C. If the heat setting temperature is too low, the heat shrinkage rate becomes too large, which tends to deteriorate the appearance after lamination and reduce the laminate strength. The upper limit of the heat setting temperature is preferably 220°C, more preferably 218°C. If the heat setting temperature is too high, the impact strength tends to decrease. The heat setting time is preferably 0.5 to 20 seconds, and even more preferably 1 to 15 seconds. The heat setting time can be adjusted appropriately by balancing the heat setting temperature and the wind speed in the heat setting zone. A heat setting temperature of 220°C or less is preferred from the viewpoint of preventing embrittlement of the film. A heat setting temperature of 210°C or higher is preferred from the viewpoint of improving dimensional stability and laminate strength. That is, the heat setting temperature is preferably 210 to 220°C, more preferably 212 to 218°C.
[0056] Relaxation treatment after heat setting is effective in controlling the heat shrinkage rate. The temperature for the relaxation treatment can be selected within the range from the heat setting temperature to the Tg of the resin, but is preferably between (heat setting temperature (°C) - 10)°C and (Tg (°C) + 10)°C. A relaxation temperature that is too high is undesirable because the shrinkage rate is too fast, causing distortion. Conversely, a relaxation temperature that is too low does not result in relaxation treatment, and the film simply becomes loose, preventing a reduction in the heat shrinkage rate and resulting in poor dimensional stability. The lower limit of the relaxation rate for the relaxation treatment is preferably 0.5%, more preferably 1%. If it is less than 0.5%, the heat shrinkage rate may not be reduced sufficiently. The upper limit of the relaxation rate is preferably 20%, more preferably 15%, and even more preferably 10%. If it exceeds 20%, sagging may occur in the tenter, making production difficult. A relaxation rate of 0.5% or more is preferable in terms of reducing the heat shrinkage rate. A relaxation rate of 20% or less is preferable in terms of preventing film sagging. That is, the relaxation rate is preferably 0.5 to 20%, more preferably 1 to 15%, and even more preferably 1 to 10%.
[0057] Furthermore, the biaxially stretched polyamide film of the present invention can be subjected to heat treatment or humidity conditioning treatment to improve dimensional stability depending on the application. In addition, to improve the adhesiveness of the film surface, it can also be subjected to corona treatment, coating treatment, flame treatment, printing, or vapor deposition of metals, inorganic oxides, etc.
[0058] In one embodiment of the present invention, the biaxially oriented polyamide film of the present invention is processed into a laminated film by laminating a sealant film, thereby providing a packaging material. Examples of sealant films include unstretched linear low-density polyethylene (LLDPE) film, unstretched polypropylene (CPP) film, and ethylene-vinyl alcohol copolymer resin (EVOH) film. The sealant film may be laminated so as to be in direct contact with the biaxially oriented polyamide film, or may be laminated via another layer such as an adhesive layer. The packaging material may include a printed layer. The packaging material of the present invention is made into a bag and processed into a packaging bag.
[0059] Another embodiment of the present invention provides a packaging material for ethanol-transmitting agents, comprising a laminate including at least two layers of the biaxially oriented polyamide film of the present invention and a breathable resin film or nonwoven fabric. The breathable resin film is not particularly limited as long as it is a breathable or ethanol-permeable film, but examples include unstretched linear low-density polyethylene (LLDPE) film, unstretched polypropylene (CPP) film, ethylene-vinyl alcohol copolymer resin (EVOH) film, and ethylene-vinyl acetate copolymer resin (EVA) film. A nonwoven fabric can also be used in place of or in combination with the breathable resin film. Examples of materials that can be used as the nonwoven fabric substrate include polyester, polypropylene, rayon, nylon, biodegradable fibers, pulp, and cotton, with polypropylene being preferred. The nonwoven fabric can be either a short-fiber nonwoven fabric or a long-fiber nonwoven fabric. The nonwoven fabric may also be a paper substrate.
[0060] This application claims the benefit of priority based on Japanese Patent Application No. 2023-055926, filed on March 30, 2023. The entire content of the specification of Japanese Patent Application No. 2023-055926, filed on March 30, 2023, is incorporated herein by reference.
[0061] The film was evaluated by the following measurement methods. Unless otherwise specified, the measurements were carried out in a measurement room at an environment of 23° C. and a relative humidity of 65%.
[0062] (1) Film Thickness The film was divided into 10 equal parts in the TD direction (narrow films were divided so that the width was wide enough to measure the thickness), and 10 100 mm films were cut out in the MD direction, and conditioned for at least 2 hours in an environment at a temperature of 23°C and a relative humidity of 65%. The thickness of the center of each sample was measured using a thickness measuring instrument manufactured by Tester Sangyo, and the average value was taken as the thickness.
[0063] (2) Heat Shrinkage of Film The heat shrinkage was measured according to the dimensional change test method described in JIS C2318 using the following formula, except that the test temperature was 160°C and the heating time was 10 minutes: Heat shrinkage = [(length before treatment - length after treatment) / length before treatment] x 100 (%)
[0064] (3) F5 Value of Film The obtained biaxially stretched polyamide film was left to stand for 2 hours in a room adjusted to 23°C and 50% relative humidity, and then cut into strips of 150 mm in the MD and TD measurement directions (gauge length 100 mm) and 15 mm perpendicular to the measurement direction to obtain samples. Tensile tests were performed at a test speed of 200 mm / min using a tensile tester (Shimadzu AG-1I) equipped with a 1 kN load cell and a sample chuck. The stress at which the sample elongated by 5% from the obtained stress-elongation curve was taken as the F5 value and treated as a substitute for the elastic modulus. Measurements were performed on three samples, and the average value for each was calculated.
[0065] (4) Impact Strength of Film: Measurement was carried out using a film impact tester manufactured by Toyo Seiki Seisakusho Co., Ltd.
[0066] (5) Puncture Strength of Film The puncture strength of film was measured in accordance with "2. Test Method for Strength, etc." in "Specifications and Standards for Foods, Food Additives, etc., Part 3: Apparatus and Containers / Packaging" (Ministry of Health and Welfare Notification No. 20, 1982) under the Food Sanitation Act. A needle with a tip diameter of 0.7 mm was pierced into the film at a piercing speed of 50 mm / min, and the strength at which the needle penetrated the film was measured and taken as the puncture strength. The measurement was carried out at room temperature (23°C), and the obtained value was taken as the puncture strength of the film (unit: N).
[0067] (6) Crystallization parameters FT-IR ATR measurements were performed on the front and back surfaces of the sample under the following conditions: FT-IR device: FTS-60A / 896 manufactured by Bio Rad DIGILAB, single-reflection ATR attachment: golden gate MKII (manufactured by SPECAC), internal reflection element: diamond, incident angle: 45°, resolution: 4 cm -1 Number of times: 128 times Crystallinity is 1200 cm -1 Absorption appearing near 1370 cm -1 The intensity ratio of the absorbance appearing near 1200 cm -1 / 1370cm -1 ) where 1200 cm -1 is the absorption of α-crystal of nylon 6, 11370 cm -1 is an absorption independent of the crystal.
[0068] (7) Planar Orientation Degree of Film The refractive index of a sample in the longitudinal direction (nx), width direction (ny), and thickness direction (nz) of the film was measured using an Abbe refractometer with sodium D line as a light source according to JIS K 7142-1996 Method A, and the planar orientation coefficient was calculated using the formula (1): Planar orientation coefficient (ΔP) = (nx + ny) / 2 - nz
[0069] (8) Ethanol Permeability Absorbent cotton soaked in ethanol was placed in a cup, the cup was covered with a film, and the cup was left to stand for 24 hours under conditions of 50% relative humidity and 40°C, and the ethanol permeability was measured from the weight loss.
[0070] (9) Resin dispersion diameter The film was cut so that cross sections in any direction could be observed and embedded in epoxy resin. Ultrathin sections were prepared from the embedded samples using a microtome equipped with an ultrasonic knife. In order to confirm the dispersion shape of resin (b), appropriate staining treatment was performed according to the type of resin (b). Carbon deposition was performed on the test pieces to prepare samples for TEM observation. Observation and photography were carried out using a JEOL JEM2100 transmission electron microscope at an accelerating voltage of 200 kV. The magnification was adjusted so that the entire substrate layer was included in the photographed area. In the photograph obtained, the longest major axis length of the resin dispersed in the substrate layer was taken as the maximum dispersion diameter.
[0071] (10) Film Bending Pinhole Resistance Using a Gelbo Flex Tester manufactured by Tester Sangyo Co., Ltd., the number of pinholes due to bending fatigue was measured using the following method. Specifically, a polyester-based adhesive was applied to the biaxially oriented polyamide film prepared in the Examples, followed by dry lamination with a 40 μm-thick linear low-density polyethylene film (L-LDPE film: L4102 manufactured by Toyobo Co., Ltd.) and aging for 3 days at 40°C to produce a laminate film. The resulting laminate film was cut into a 12-inch x 8-inch cylindrical shape with a diameter of 3.5 inches. One end of the cylindrical film was fixed to the fixed head of the Gelbo Flex Tester, and the other end was fixed to the movable head, with an initial gripping distance of 7 inches. A bending fatigue test was performed 1,000 times at a speed of 40 times / min, with a 440° twist in the first 3.5 inches of the stroke, followed by a linear horizontal movement for the next 2.5 inches to complete the entire stroke. The number of pinholes that occurred in the laminate film was counted. The measurements were carried out in an environment of 1°C. The test film was placed on filter paper (Advantec, No. 50) with the L-LDPE film side facing downwards, and the four corners were fixed with Cellotape (registered trademark). Ink (Pilot ink (product number INK-350-Blue) diluted five times with pure water) was applied to the test film and spread over the entire surface using a rubber roller. After wiping off any excess ink, the test film was removed and the number of ink dots on the filter paper was counted.
[0072] The following resin compositions were used for the substrate layer and the functional layer. Resin composition constituting substrate layer A: Polyamide 6 (manufactured by Toyobo Co., Ltd., relative viscosity 2.8, melting point 220°C) Resins (b) other than polyamide 6: Polybutylene adipate terephthalate PBAT (manufactured by BASF Ecoflex F-Blend C1200) Polyester elastomer PEE (manufactured by Mitsubishi Chemical Corporation Tefablock TPC A1400N) Polyamide elastomer PAE (manufactured by Arkema PEBAX 4033 SA01) Polyolefin elastomer POE (manufactured by Tosoh Corporation Mersen H6051) Polybutylene succinate PBS (Showa Highpolymer Co., Ltd., Bionolle 1001) Polyamide 11: (manufactured by Arkema Rilsan, melting point 186°C)
[0073] Resin composition constituting functional layer B: 90% by mass of polyamide 6 (manufactured by Toyobo Co., Ltd., relative viscosity 2.8, melting point 220°C); 10% by mass of polyamide MXD6 (manufactured by Mitsubishi Gas Chemical Co., Inc., relative viscosity 2.1, melting point 237°C); 0.54% by mass of porous silica microparticles (manufactured by Fuji Silysia Chemical Ltd., average particle size 2.0 μm, pore volume 1.6 ml / g); 0.15% by mass of fatty acid bisamide (ethene bisstearamide, manufactured by Kyoeisha Chemical Co., Ltd.)
[0074] (Examples 1 to 7) The raw materials for the base layer: Layer A and the functional layer: Layer B were mixed according to the formulation shown in Table 1. Using an apparatus consisting of two extruders and a 380 mm wide co-extrusion T-die, lamination was performed using the feed block method in a configuration of functional layer: Layer B / base layer: Layer A / functional layer: Layer B, and the molten resin of the resin composition shown in Table 1 was extruded from the T-die into a film, which was then cast onto a cooling roll controlled to a temperature of 20°C and electrostatically adhered to obtain an unstretched film having a thickness of 100 to 200 μm.
[0075] The resulting unstretched film was introduced into a roll-type stretching machine, and using the difference in peripheral speed of the rolls, it was stretched 1.73 times in the MD direction at 80 ° C., and then further stretched 1.85 times at 70 ° C. Subsequently, this uniaxially stretched film was introduced into a tenter-type stretching machine, preheated at 60 ° C., and then stretched 1.2 times in the TD direction at 120 ° C., 1.7 times at 130 ° C., and 2.0 times at 160 ° C., heat-set at 218 ° C., then subjected to 7% relaxation at 218 ° C., and corona discharge treatment was performed on one surface to obtain a biaxially stretched polyamide film. The extruder output was adjusted so that the thickness of the base layer was 8 μm and the thickness of the functional layer was 1 μm on each side relative to the thickness of the biaxially stretched polyamide film (10 μm).
[0076] (Examples 8 and 9) With the formulation shown in Table 1, biaxially oriented polyamide films were obtained in the same manner as in Examples 1 to 7, except that the feed block configuration and the extrusion rate of the extruder were adjusted so that the total thickness of the biaxially oriented polyamide film was 15 μm, the thickness of the base layer was 12 μm, and the thickness of the functional layer was 1.5 μm on each side.
[0077] (Comparative Examples 1 to 4, 6) Biaxially stretched polyamide films were obtained in the same manner as in Example 1, except that the resin compositions of the substrate layer and the functional layer were changed as shown in Table 2. The evaluation results of the obtained films are shown in Table 2.
[0078] (Comparative Example 5) A biaxially stretched polyamide film was obtained in the same manner as in Examples 1 to 7 and Comparative Examples 1 to 4 and 6, except that the rotation speed of the extruder that extrudes the resin composition that constitutes the base layer was increased within a range that did not increase the target thickness, and the kneading was strengthened.
[0079] The evaluation results of the films obtained in the examples and comparative examples are shown in Table 1.
[0080]
[0081]
[0082]
[0083]
[0084] The films described in Examples 1 to 9 exhibited excellent pinhole resistance, dimensional stability, puncture strength, and ethanol permeability, making them suitable for use in alcohol vaporizers. While the planar orientation degree was 0.5 or higher, indicating high orientation, and the crystallization parameter was 1.0 or higher, indicating high crystallization, the dispersion of resin (b) with a dispersion diameter of 1 μm or larger formed an interface with relatively low adhesion strength with the polyamide resin, and this interface was utilized to improve ethanol permeability. Furthermore, the dispersion of resin (b) improved the flexibility of the base layer A itself, resulting in improved pinhole resistance.
[0085] The film described in Comparative Example 1 was excellent in dimensional stability and puncture strength, but was poor in bending pinhole resistance and ethanol permeability. When the planar orientation ΔP was 0.05 or more and the crystallization parameter was in the range of 1 to 1.5, the dimensional stability and puncture strength were good, but it is believed that the progress of crystallization increased the brittleness of the film, resulting in decreased pinhole resistance and ethanol permeability.
[0086] Although the film described in Comparative Example 2 has a thickness of 15 μm, since the base layer does not contain any resin other than polyamide 6, a dispersion structure due to phase separation does not occur, and ethanol permeation does not occur using the dispersion interface, and the ethanol permeability is not satisfactory for use as an alcohol evaporant.
[0087] The film described in Comparative Example 3 was as thick as 25 μm, and since the base layer contained no resin other than polyamide 6, the pinhole resistance and ethanol permeability were not satisfactory for use as an alcohol vaporizer.
[0088] The film described in Comparative Example 4 had a small amount of PBAT added as resin (b), and the interface between polyamide 6 and PBAT was small, resulting in insufficient ethanol permeability.
[0089] In the film of Comparative Example 5, the maximum dispersed diameter of the resin (b) was as small as 0.5 μm, and compatibility with polyamide 6 progressed, so that good ethanol permeability and good pinhole resistance could not be obtained.
[0090] The film described in Comparative Example 6 contained 40% PBAT, resulting in an ethanol permeability of 16,000 g μm / m2 - The time increased to 24 hours (50% RH / 40°C). As an ethanol evaporant, the ethanol evaporated quickly.
Claims
1. A biaxially oriented polyamide film containing polyamide 6 as the main component, and having an ethanol permeability of 6000 to 10000 g μm / m 2 A biaxially oriented polyamide film having a tensile strength of 24 hr (50% RH / 40°C), a thickness of 15 μm or less, a thermal shrinkage rate of 2.0% or less in both the machine direction and width direction of the film when heat-treated for 10 minutes at 160°C, a surface crystallization parameter in the range of 1.0 to 1.5, and a puncture strength of 6.0 N or more.
2. The biaxially oriented polyamide film according to claim 1, having at least one layer containing 60% by mass or more and 98% by mass or less of polyamide 6 resin (a) and 2% by mass or more and 40% by mass or less of a resin other than polyamide 6 (b).
3. The biaxially oriented polyamide film according to claim 2, wherein the resin (b) other than polyamide 6 is at least one selected from the group consisting of thermoplastic elastomers such as polyolefins, ionomer polymers, polyester-based elastomers, polyamide-based elastomers, polyolefin-based elastomers, polystyrene-based elastomers, polyurethane-based elastomers, and polyvinyl chloride-based elastomers, aliphatic polyester resins, aliphatic-aromatic polyester resins, aliphatic polyamide resins, and aliphatic-aromatic polyamide resins.
4. The biaxially oriented polyamide film according to claim 3, wherein the aliphatic-aromatic polyester resin is a polybutylene adipate terephthalate resin.
5. The biaxially oriented polyamide film according to claim 2, wherein the resin (b) other than polyamide 6 is derived from biomass and is at least one polyamide selected from the group consisting of polyamide 11, polyamide 410, polyamide 610, and polyamide 1010.
6. The biaxially oriented polyamide film according to claim 2, wherein the maximum dispersion diameter of the resin (b) other than polyamide 6 is 1.0 μm or more.
7. The biaxially oriented polyamide film according to claim 1, wherein the stress at 5% elongation in both the machine direction and the width direction of the film is 70.0 MPa or less.
8. The biaxially oriented polyamide film according to claim 1, having a planar orientation degree (ΔP) of 0.050 or more.
9. The biaxially oriented polyamide film according to claim 1, wherein a laminate film of the biaxially oriented polyamide film and a 40 μm-thick polyethylene film is prepared, and is flexed 1,000 times in an atmosphere at a temperature of 1° C. using a Gelbo flex tester. The number of pinholes that are generated is 20 or less.
10. A food packaging material comprising the biaxially oriented polyamide film according to any one of claims 1 to 9 and a sealant film.
11. A packaging material for an ethanol evaporative agent, comprising a laminate including at least two layers of the biaxially oriented polyamide film according to any one of claims 1 to 9 and a breathable resin film or nonwoven fabric.
Citation Information
Patent Citations
Stretched polyamide film and method for producing the same
JP2010158775A
Polyamide laminated film with excellent permeability to water vapor and alcohol
JP2010167652A
Alcohol-permeable polyamide film
JP2010241901A
Polyamide resin film and package using the film
JP2021130770A
Polyamide-based biaxially stretched film and package
JP2022077210A