Binder powder for nonaqueous secondary battery electrode, mixture powder composition, method for producing electrode for nonaqueous secondary battery, and nonaqueous secondary battery

The binder powder with controlled particulate polymer characteristics addresses the low adhesive strength issue in non-aqueous secondary battery electrodes by forming a composite powder composition that significantly enhances the bonding between the current collector and electrode active material layer, improving the battery's mechanical and operational performance.

WO2024203750A1PCT designated stage expired Publication Date: 2024-10-03ZEON CORP
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/011099
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-21
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Non-aqueous secondary battery electrodes manufactured using a dry process often exhibit low adhesive strength between the current collector and the electrode active material layer, necessitating a solution to enhance this bonding.

Method used

A binder powder with specific particulate polymer characteristics, including a controlled average primary particle size and particle size distribution, is developed to form a composite powder composition that improves the adhesive strength between the current collector and the electrode active material layer.

Benefits of technology

The use of the binder powder and composite powder composition results in electrodes with enhanced adhesive strength, reducing peeling and maintaining mechanical integrity, thereby improving the performance of non-aqueous secondary batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
  • Figure JPOXMLDOC01-APPB-T000003
    Figure JPOXMLDOC01-APPB-T000003
Patent Text Reader

Abstract

A binder powder for a nonaqueous secondary battery electrode containing a particulate polymer with an average primary particle size of 0.3 μm or more, wherein the ratio of particles with a particle size greater than 250 μm is 10 wt% or less.
Need to check novelty before this filing date? Find Prior Art

Description

Binder powder for non-aqueous secondary battery electrodes, composite powder composition, electrode for non-aqueous secondary battery and method for manufacturing the same, and non-aqueous secondary battery

[0001] The present invention relates to a binder powder for a non-aqueous secondary battery electrode, a composite powder composition, an electrode for a non-aqueous secondary battery and a method for producing the same, and a non-aqueous secondary battery.

[0002] Electrodes for non-aqueous secondary batteries such as non-aqueous lithium-ion secondary batteries have generally been produced by a wet process using a liquid material containing a solvent. For example, an electrode mixture containing an electrode active material and a binder is mixed with a solvent to prepare a slurry composition, and the slurry composition is then applied to a current collector and dried to produce an electrode (Patent Document 1).

[0003] However, in recent years, attention has been drawn to the production of electrodes by dry processes using powdered materials. As such methods for producing electrodes by dry processes, for example, the methods disclosed in Patent Documents 2 and 3 are known.

[0004] International Publication No. 2018 / 034093 (corresponding publication: U.S. Patent Application Publication No. 2020 / 0052270) Japanese Patent No. 6327249 U.S. Patent Application Publication No. 2020 / 0144591

[0005] However, electrodes for non-aqueous secondary batteries manufactured by dry processes tend to have low adhesive strength between the current collector and the electrode active material layer, and therefore there is a need to develop a technology to improve the adhesive strength between the current collector and the electrode active material layer.

[0006] The present invention has been made in view of the above-mentioned problems, and aims to provide: a binder powder and composite powder composition for non-aqueous secondary battery electrodes, which enable the production of electrodes for non-aqueous secondary batteries having excellent adhesive strength between the current collector and the electrode active material layer; an electrode for non-aqueous secondary batteries having excellent adhesive strength between the current collector and the electrode active material layer, and a method for producing the same; and a non-aqueous secondary battery comprising the electrode for non-aqueous secondary batteries.

[0007] The present inventors have conducted extensive research to solve the above-mentioned problems. As a result, the present inventors have found that the above-mentioned problems can be solved by a binder powder containing a particulate polymer having a specific average primary particle size, in which the content ratio of particles having particle sizes equal to or larger than a predetermined value is within a predetermined range, and have completed the present invention. That is, the present invention includes the following.

[0008] [1] A binder powder for a non-aqueous secondary battery electrode, comprising a particulate polymer having an average primary particle size of 0.3 μm or more, wherein the proportion of particles having a particle size exceeding 250 μm is 10% by weight or less. [2] The binder powder for a non-aqueous secondary battery electrode according to [1], wherein the proportion of particles having a particle size exceeding 74 μm is 10% by weight or less. [3] The binder powder for a non-aqueous secondary battery electrode according to [1] or [2], wherein the average primary particle size of the particulate polymer is 0.5 μm or more and 15 μm or less. [4] The binder powder for a non-aqueous secondary battery electrode according to any one of [1] to [3], wherein the particulate polymer has a glass transition temperature of 35° C. or more and 100° C. or less. [5] A composite powder composition comprising the binder powder for a non-aqueous secondary battery electrode according to any one of [1] to [4] and an electrode active material. [6] An electrode for a non-aqueous secondary battery, comprising a current collector and an electrode active material layer formed on the current collector using the composite powder composition according to [5]. [7] An average particle diameter D of the particulate polymer contained in the electrode active material layer is B and the average particle size D of the electrode active material A Relative to D B / D A is 0.01 or more and 1.0 or less. [8] A nonaqueous secondary battery comprising the electrode for a nonaqueous secondary battery according to [6] or [7]. [9] A method for producing an electrode for a nonaqueous secondary battery, comprising a step of forming an electrode active material layer from the composite powder composition according to [5] by a dry process.

[0009] According to the present invention, it is possible to provide a binder powder and composite powder composition for a non-aqueous secondary battery electrode, which can provide an electrode for a non-aqueous secondary battery having excellent adhesive strength between the current collector and the electrode active material layer; an electrode for a non-aqueous secondary battery having excellent adhesive strength between the current collector and the electrode active material layer and a method for producing the same; and a non-aqueous secondary battery including the electrode for a non-aqueous secondary battery.

[0010] The present invention will be described in detail below with reference to embodiments and examples. However, the present invention is not limited to the embodiments and examples described below, and may be modified and implemented as desired within the scope of the claims and their equivalents.

[0011] In the following description, unless otherwise specified, an electrode active material layer refers to a layer containing an electrode active material, a positive electrode active material layer refers to an electrode active material layer for a positive electrode, and a negative electrode active material layer refers to an electrode active material layer for a negative electrode.

[0012] In the following description, unless otherwise specified, the term "(meth)acrylic acid" includes acrylic acid, methacrylic acid, and combinations thereof. Furthermore, unless otherwise specified, the term "(meth)acrylate" includes acrylate, methacrylate, and combinations thereof. Furthermore, unless otherwise specified, the term "(meth)acrylonitrile" includes acrylonitrile, methacrylonitrile, and combinations thereof.

[0013] <Binder Powder> The binder powder according to one embodiment of the present invention contains a particulate polymer. This binder powder may contain only a particulate polymer. The binder powder may be a dry powder and may have a powdery form in a room temperature environment (generally, a 25°C environment).

[0014] The particulate polymer contained in the binder powder may be primary particles in which the particulate polymer particles are not aggregated, or may be secondary particles formed by aggregation of multiple particulate polymer particles, or may be a combination of these primary particles and secondary particles. In general, particulate polymers may have a particle size distribution depending on characteristics such as the particle size and aggregation state of each primary particle. Therefore, the binder powder containing the particulate polymer may also have a particle size distribution.

[0015] In the binder powder according to this embodiment, the proportion of particles exceeding 250 μm in the particle size distribution is within a specific range. Hereinafter, particles exceeding 250 μm in the binder powder may be referred to as "first coarse particles." The proportion of first coarse particles exceeding 250 μm in the particle size distribution is expressed as the proportion of residual components (i.e., binder powder remaining on the sieve) remaining on the sieve when the binder powder is subjected to a sieve test in which the binder powder is passed through a sieve with a mesh size of 250 μm. Hereinafter, this proportion may be referred to as the "sieve residue rate." Unless otherwise specified, the "mesh size" refers to the opening width of the sieve. In a sieve test using a sieve with a mesh size of 250 μm, the sieve residue rate of the binder powder is typically 10% by weight or less, preferably 8% by weight or less, more preferably 6% by weight or less, and even more preferably 5% by weight or less. The lower limit of the sieve residue is usually 0% by weight or more, and may be 0.1% by weight or more, 0.5% by weight or more, etc. The first coarse particles may include both primary particles and aggregates formed by agglomeration of a plurality of the primary particles. The binder powder may contain, as particles, a particulate polymer and particles of any component other than the particulate polymer. Generally, all or most of the particles contained in the binder powder are particulate polymers. Therefore, the range of the sieve residue in a sieve test using a sieve with an opening of 250 μm may correspond to the range of the proportion of particulate polymers (which may include both primary particles and aggregates) having a particle size greater than 250 μm relative to 100% by weight of the total amount of particulate polymer contained in the binder powder.

[0016] Furthermore, in the binder powder according to this embodiment, it is preferable that the proportion of particles exceeding 74 μm in the particle size distribution be within a specific range. Hereinafter, particles exceeding 74 μm in the binder powder may be referred to as "second coarse particles." The proportion of second coarse particles exceeding 74 μm in the particle size distribution is expressed as the proportion of residual components (i.e., binder powder remaining on the sieve) remaining on the sieve when the binder powder is subjected to a sieve test in which the binder powder is passed through a sieve with a mesh size of 74 μm. The sieve residue of the binder powder in the sieve test using a sieve with a mesh size of 74 μm is typically 10% by weight or less, preferably 8% by weight or less, more preferably 6% by weight or less, and even more preferably 5% by weight or less. The lower limit of the sieve residue is typically 0% by weight or more, and may be 0.1% by weight or more, 0.5% by weight or more, etc. The second coarse particles may include both primary particles and aggregates formed by aggregation of multiple primary particles. Generally, all or most of the particles contained in the binder powder are particulate polymers, and therefore, the range of the sieve-on-sieve residue rate in a sieve test using a sieve with a mesh size of 74 μm can correspond to the range of the proportion of particulate polymers (which can include both primary particles and aggregates) having particle sizes exceeding 74 μm relative to 100% by weight of the total amount of particulate polymers contained in the binder powder.

[0017] The sieve residue rate of the binder powder can be measured by the following method. A sample of binder powder with a weight W(0) is sieved. Then, the weight W(1) of the binder powder (residual component) remaining on the sieve is measured. The sieve residue rate can be calculated using the following formula (M1). At this time, by measuring the sieve residue rate using a sieve with a mesh size of 250 μm, the proportion of first coarse particles with a particle size exceeding 250 μm can be measured. Also, by measuring the sieve residue rate using a sieve with a mesh size of 74 μm, the proportion of second coarse particles with a particle size exceeding 74 μm can be measured. A specific measurement method can be the method described in the "Method for measuring the sieve residue rate of binder powder" in the examples below. Sieve residue rate (%) = W(1) / W(0) × 100 (M1)

[0018] The sieve retention rate of the binder powder can be adjusted, for example, by classification. Specifically, after producing the particulate polymer, the sieve retention rate of the binder powder can be adjusted by classifying the produced particulate polymer using a sieve with appropriate openings.

[0019] The average primary particle diameter of the particulate polymer according to this embodiment is within a specific range. Specifically, the average primary particle diameter of the particulate polymer is usually 0.3 μm or more, preferably 0.5 μm or more, and more preferably 0.8 μm or more. The upper limit of the average primary particle diameter of the particulate polymer can be set within the range in which the sieve retention rate of the binder powder falls within the above range, and is preferably 30 μm or less, more preferably 15 μm or less, and even more preferably 10 μm or less.

[0020] The average primary particle size of the particulate polymer can be measured by the following method. A 1% aqueous solution of linear alkylbenzenesulfonate sodium is mixed with the particulate polymer and dispersed using ultrasound to obtain a dispersion in which the primary particles of the particulate polymer are dispersed. The cumulative particle size distribution of this dispersion is measured using a Coulter counter. The particle size at which the integrated value, calculated from the small diameter side of this cumulative particle size distribution, reaches 50% can be obtained as the volume-based average primary particle size of the particulate polymer. A specific measurement method that can be used is the method described in "Method for measuring the average primary particle size of the particulate polymer contained in the binder powder" in the Examples below.

[0021] The average primary particle size of the particulate polymer can be adjusted, for example, by the type and amount of metal hydroxide used in producing the particulate polymer, and the method and conditions for producing the particulate polymer.

[0022] The binder powder according to this embodiment, which satisfies the above-described requirements, can provide an electrode for a non-aqueous secondary battery that has excellent adhesive strength between the current collector and the electrode active material layer. Without being bound by any particular theory, the inventors speculate that the mechanism by which such excellent effects are obtained is as follows. However, the technical scope of the present invention is not limited by the mechanism described below.

[0023] The binder powder according to this embodiment has a low content of excessively large coarse particles (such as first coarse particles and second coarse particles), as represented by the sieve retention rate. Furthermore, the binder powder according to this embodiment has a low content of excessively small fine particles, as represented by the average primary particle diameter of the particulate polymer. Therefore, the particle diameters of the particulate polymer particles (including primary particles, secondary particles, and combinations thereof) contained in the binder powder are highly uniform. Therefore, when an electrode active material layer containing the particulate polymer is formed, the composition of the electrode active material layer can be highly uniform. Therefore, when stress is applied to separate the current collector and the electrode active material layer in the electrode, the occurrence of points where the stress concentrates is suppressed. Therefore, peeling originating from these points is suppressed, thereby achieving high adhesive strength.

[0024] The particulate polymer preferably has a glass transition temperature Tg within a specific range. The range of the glass transition temperature Tg of the particulate polymer is preferably 10° C. or higher, more preferably 20° C. or higher, and even more preferably 35° C. or higher, and is preferably 130° C. or lower, more preferably 120° C. or lower, and even more preferably 100° C. or lower. When the glass transition temperature Tg of the particulate polymer is within the above range, the adhesive strength between the current collector and the electrode active material layer of an electrode produced using the binder powder can be effectively increased.

[0025] The glass transition temperature Tg of the particulate polymer can be measured using a differential scanning calorimeter at a temperature rise rate of 20°C / min in accordance with JIS K 7121: 1987. As a specific measurement method, the method described in <Method for measuring glass transition temperature> in the examples described later can be adopted.

[0026] The particulate polymer preferably contains an aromatic monovinyl monomer unit. The aromatic monovinyl monomer unit refers to a structural unit having a structure formed by polymerizing an aromatic monovinyl monomer. Examples of aromatic monovinyl monomers include styrene, α-methylstyrene, and vinyltoluene. Among these, styrene is preferred. The particulate polymer may contain one type of aromatic monovinyl monomer unit alone or two or more types in combination.

[0027] The proportion of aromatic monovinyl monomer units in the particulate polymer is preferably 45% by weight or more, more preferably 50% by weight or more, even more preferably 55% by weight or more, and is preferably 99.5% by weight or less, more preferably 95% by weight or less, even more preferably 90% by weight or less. The proportion of aromatic monovinyl monomer units in the particulate polymer usually corresponds to the weight ratio of aromatic monovinyl monomers to the total weight of monomers used in producing the particulate polymer (feed ratio of aromatic monovinyl monomers).

[0028] The particulate polymer preferably contains a (meth)acrylic acid alkyl ester monomer unit. The (meth)acrylic acid alkyl ester monomer unit refers to a structural unit having a structure formed by polymerizing a (meth)acrylic acid alkyl ester monomer. The (meth)acrylic acid alkyl ester monomer includes an acrylic acid alkyl ester monomer, a methacrylic acid alkyl ester monomer, and a combination thereof. Examples of the (meth)acrylic acid alkyl ester monomer include acrylic acid alkyl ester monomers such as methyl acrylate, ethyl acrylate, n-propyl acrylate, isopropyl acrylate, n-butyl acrylate, t-butyl acrylate, pentyl acrylate, hexyl acrylate, heptyl acrylate, octyl acrylate, 2-ethylhexyl acrylate, nonyl acrylate, decyl acrylate, lauryl acrylate, n-tetradecyl acrylate, and stearyl acrylate. and alkyl methacrylate monomers such as methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, t-butyl methacrylate, pentyl methacrylate, hexyl methacrylate, heptyl methacrylate, octyl methacrylate, 2-ethylhexyl methacrylate, nonyl methacrylate, decyl methacrylate, lauryl methacrylate, n-tetradecyl methacrylate, and stearyl methacrylate. Among these, alkyl (meth)acrylate monomers in which the alkyl group bonded to the non-carbonyl oxygen atom has 4 or more carbon atoms are preferred, and alkyl (meth)acrylate monomers in which the alkyl group bonded to the non-carbonyl oxygen atom has 6 to 20 carbon atoms are more preferred. The particulate polymer may contain one type of alkyl (meth)acrylate monomer unit alone, or two or more types may be contained in combination.

[0029] The proportion of the (meth)acrylic acid alkyl ester monomer unit in the particulate polymer is preferably 0% by weight or more, more preferably 2% by weight or more, even more preferably 5% by weight or more, and is preferably 55% by weight or less, more preferably 50% by weight or less, even more preferably 45% by weight or less. The proportion of the (meth)acrylic acid alkyl ester monomer unit in the particulate polymer usually coincides with the weight ratio of the (meth)acrylic acid alkyl ester monomer to the total weight of the monomers used in producing the particulate polymer (the charge ratio of the (meth)acrylic acid alkyl ester monomer).

[0030] The particulate polymer preferably contains a crosslinkable monomer unit. The crosslinkable monomer unit refers to a structural unit having a structure formed by polymerizing a crosslinkable monomer. The crosslinkable monomer refers to a monomer that can form a crosslinked structure when polymerized. Examples of the crosslinkable monomer include a monomer having two or more reactive groups per molecule. Specific examples of the crosslinkable monomer include a monofunctional crosslinkable monomer having a thermally crosslinkable crosslinkable group and one olefinic double bond per molecule; and a polyfunctional crosslinkable monomer having two or more olefinic double bonds per molecule.

[0031] Examples of the thermally crosslinkable crosslinkable group possessed by the crosslinkable monomer include an epoxy group, an N-methylolamide group, an oxetanyl group, an oxazoline group, and combinations thereof. Among these, an epoxy group is preferred. Examples of monofunctional crosslinkable monomers having an epoxy group as a thermally crosslinkable crosslinkable group and an olefinic double bond include unsaturated glycidyl ethers such as vinyl glycidyl ether, allyl glycidyl ether, butenyl glycidyl ether, and o-allylphenyl glycidyl ether; diene or polyene monoepoxides such as butadiene monoepoxide, chloroprene monoepoxide, 4,5-epoxy-2-pentene, 3,4-epoxy-1-vinylcyclohexene, and 1,2-epoxy-5,9-cyclododecadiene; 3,4-epoxy ethers such as chloroprene monoepoxide, chloroprene monoepoxide, 4,5-epoxy-2-pentene, 3,4-epoxy-1-vinylcyclohexene, and 1,2-epoxy-5,9-cyclododecadiene; alkenyl epoxides such as 1,2-epoxy-1-butene, 1,2-epoxy-5-hexene, and 1,2-epoxy-9-decene; and glycidyl esters of unsaturated carboxylic acids such as glycidyl acrylate, glycidyl methacrylate, glycidyl crotonate, glycidyl 4-heptenoate, glycidyl sorbate, glycidyl linoleate, glycidyl 4-methyl-3-pentenoate, glycidyl ester of 3-cyclohexenecarboxylic acid, and glycidyl ester of 4-methyl-3-cyclohexenecarboxylic acid. Among these, unsaturated glycidyl ethers and glycidyl esters of unsaturated carboxylic acids are preferred, allyl glycidyl ether and glycidyl methacrylate are more preferred, and glycidyl methacrylate is even more preferred.

[0032] The proportion of the monofunctional crosslinkable monomer unit in the particulate polymer is preferably 0% by weight or more, more preferably 2% by weight or more, even more preferably 5% by weight or more, and preferably 25% by weight or less, more preferably 22% by weight or less, even more preferably 20% by weight or less. The monofunctional crosslinkable monomer unit refers to a structural unit having a structure formed by polymerizing a monofunctional crosslinkable monomer. The proportion of the monofunctional crosslinkable monomer unit in the particulate polymer usually corresponds to the weight ratio of the monofunctional crosslinkable monomer to the total weight of the monomers used in producing the particulate polymer (the charging ratio of the monofunctional crosslinkable monomer).

[0033] Examples of polyfunctional crosslinkable monomers having two or more olefinic double bonds include allyl (meth)acrylate, ethylene di(meth)acrylate, ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, trimethylolpropane-tri(meth)acrylate, dipropylene glycol diallyl ether, polyglycol diallyl ether, triethylene glycol divinyl ether, hydroquinone diallyl ether, tetraallyloxyethane, trimethylolpropane-diallyl ether, allyl or vinyl ethers of polyfunctional alcohols other than those mentioned above, triallylamine, methylenebisacrylamide, and divinylbenzene. Among these, ethylene di(meth)acrylate, ethylene glycol di(meth)acrylate, and divinylbenzene are preferred, ethylene glycol di(meth)acrylate is more preferred, and ethylene glycol dimethacrylate is even more preferred.

[0034] The proportion of the polyfunctional crosslinkable monomer unit in the particulate polymer is preferably 0% by weight or more, more preferably 0.1% by weight or more, even more preferably 0.2% by weight or more, and preferably 10% by weight or less, more preferably 8% by weight or less, even more preferably 5.0% by weight or less. The polyfunctional crosslinkable monomer unit refers to a structural unit having a structure formed by polymerizing a polyfunctional crosslinkable monomer. The proportion of the polyfunctional crosslinkable monomer unit in the particulate polymer usually corresponds to the weight ratio of the polyfunctional crosslinkable monomer to the total weight of the monomers used in producing the particulate polymer (the charge ratio of the polyfunctional crosslinkable monomer).

[0035] The particulate polymer may contain one type of crosslinkable monomer unit alone or two or more types in combination.

[0036] The proportion of the crosslinkable monomer unit in the particulate polymer is preferably 0% by weight or more, more preferably 0.1% by weight or more, even more preferably 0.2% by weight or more, and is preferably 25% by weight or less, more preferably 22% by weight or less, even more preferably 20% by weight or less. The proportion of the crosslinkable monomer unit in the particulate polymer usually coincides with the weight ratio of the crosslinkable monomer to the total weight of the monomers used in producing the particulate polymer (the charge ratio of the crosslinkable monomer).

[0037] The particulate polymer may contain an α,β-ethylenically unsaturated nitrile monomer unit. The α,β-ethylenically unsaturated nitrile monomer unit refers to a structural unit having a structure formed by polymerizing an α,β-ethylenically unsaturated nitrile monomer. As the α,β-ethylenically unsaturated nitrile monomer, an α,β-ethylenically unsaturated compound having a nitrile group can be used. Examples of the α,β-ethylenically unsaturated nitrile monomer include acrylonitrile; α-halogenoacrylonitriles such as α-chloroacrylonitrile and α-bromoacrylonitrile; and α-alkylacrylonitriles such as methacrylonitrile. The particulate polymer may contain one type of α,β-ethylenically unsaturated nitrile monomer unit alone, or two or more types may be contained in combination.

[0038] The particulate polymer may contain an ethylenically unsaturated carboxylic acid monomer unit. The ethylenically unsaturated carboxylic acid monomer unit refers to a structural unit having a structure formed by polymerizing an ethylenically unsaturated carboxylic acid monomer. Examples of the ethylenically unsaturated carboxylic acid monomer include acrylic acid, methacrylic acid, maleic acid, fumaric acid, and itaconic acid. The particulate polymer may contain one type of ethylenically unsaturated carboxylic acid monomer unit alone, or two or more types of ethylenically unsaturated carboxylic acid monomer units in combination.

[0039] The proportion of the ethylenically unsaturated carboxylic acid monomer unit in the particulate polymer is preferably 0.1% by weight or more, more preferably 0.5% by weight or more, even more preferably 1% by weight or more, and is preferably 10% by weight or less, more preferably 7% by weight or less, even more preferably 5% by weight or less. The proportion of the ethylenically unsaturated carboxylic acid monomer unit in the particulate polymer is usually equal to the weight ratio of the ethylenically unsaturated carboxylic acid monomer to the total weight of the monomers used when producing the particulate polymer (the charging ratio of the ethylenically unsaturated carboxylic acid monomer).

[0040] The particulate polymer may contain an ethylenically unsaturated amide monomer unit. The ethylenically unsaturated amide monomer unit refers to a structural unit having a structure formed by polymerizing an ethylenically unsaturated amide monomer. Examples of the ethylenically unsaturated amide monomer include (meth)acrylamide, N-methylol(meth)acrylamide, and N,N'-dimethylol(meth)acrylamide. The particulate polymer may contain one type of ethylenically unsaturated amide monomer unit alone, or two or more types of ethylenically unsaturated amide monomer units in combination.

[0041] The shape of the primary particles of the particulate polymer is preferably spherical. The spherical shape of the particles means that the sphericity of the particles is 80% or more. When the primary particles of the particulate polymer are spherical, the binder powder can have high fluidity. The sphericity is expressed as a value expressed by (1-(Ll-Ls) / La) x 100. Furthermore, Ls represents the minor axis diameter, Ll represents the major axis diameter, and La represents (Ls+Ll) / 2. The minor axis diameter Ls and major axis diameter Ll of the particulate polymer can be measured by observing a photographic image taken with a transmission or scanning electron microscope. In this case, it is preferable to use the average values ​​of the major axis diameter and minor axis diameter of 10 to 30 primary particles of the particulate polymer as the above-mentioned Ls and Ll.

[0042] As described above, the particulate polymer contained in the binder powder may be primary particles, secondary particles, or a combination thereof. Therefore, for example, the particulate polymer contained in the binder powder may exist as agglomerates (secondary particles) in the form of a plurality of bonded primary particles. The primary particles of the particulate polymer may exist as individual, independent particles, or a single secondary particle may be formed by a plurality of primary particles being bonded by a bonding force such as an intermolecular force while maintaining their shape. Furthermore, secondary particles formed by a plurality of primary particles may be crushed by an external force, so that the primary particles exist as individual, independent particles. Binder powders containing such particulate polymers as primary particles or secondary particles typically have fluidity.

[0043] The particulate polymer may be water-soluble or water-insoluble. A substance is "water-soluble" when 0.5 g of the substance is dissolved in 100 g of water at 25° C., and the insoluble content is less than 0.5 wt %. A substance is "water-insoluble" when 0.5 g of the substance is dissolved in 100 g of water at 25° C., and the insoluble content is 90 wt % or more.

[0044] All or most of the binder powder is composed of the above-mentioned particulate polymer. Specifically, the amount of the particulate polymer is preferably 95% by weight to 100% by weight, more preferably 97% by weight to 100% by weight, even more preferably 99% by weight to 100% by weight, and particularly preferably 100% by weight, relative to 100% by weight of the total amount of the binder powder. When the content of the particulate polymer in the binder powder is this high, the adhesive strength between the current collector and the electrode active material layer of an electrode manufactured using the binder powder can be effectively increased.

[0045] The binder powder may contain any component other than the particulate polymer as long as it does not significantly impair the effects of the present invention. Examples of the optional component include polymerization additives such as surfactants, emulsifiers, dispersion stabilizers, polymerization initiators, and chain transfer agents used in the polymerization of the particulate polymer. However, it is preferable that the amount of the optional component is small, and it is even more preferable that the binder powder does not contain any optional component.

[0046] The binder powder may or may not contain a solvent. Here, the solvent refers to a component that is liquid in a room temperature environment (generally, a 25°C environment). An example of a solvent is water. Preferably, the binder powder is a dry powder, and therefore preferably does not substantially contain a solvent. The amount of solvent contained in the binder powder is preferably 0% to 5% by weight, more preferably 0% to 1% by weight, even more preferably 0% to 0.5% by weight, and even more preferably 0% to 0.1% by weight, with less than 0.1% by weight being particularly preferred.

[0047] The volatile content of the binder powder at 120°C is preferably less than 1 wt% from the viewpoint of increasing the fluidity of the binder powder and improving the uniformity of the thickness of the electrode active material layer. The volatile content of the binder powder at 120°C can be measured by the following method: The binder powder is placed in an oven set to 120°C. The weight of the binder powder is measured every 10 minutes, and the measurement is stopped when the weight change becomes less than 0.1%. The weight change rate (decrease) from the initial weight of the binder powder to the weight at the end of the measurement can be determined as the volatile content at 120°C.

[0048] There are no particular limitations on the method for producing the binder powder. For example, the binder powder can be produced by a method including a step of producing a particulate polymer and a step of classifying the produced particulate polymer.

[0049] The particulate polymer can be produced by a method including polymerizing a monomer. There is no particular limitation on the method for polymerizing the monomer. Examples of the polymerization method include solution polymerization, suspension polymerization, bulk polymerization, and emulsion polymerization. Among them, suspension polymerization and emulsion polymerization are preferred.

[0050] In the polymerization method, a particulate polymer can generally be produced by polymerizing a monomer composition containing the above-mentioned monomers in a reaction solvent. In this case, the ratio of each monomer in the monomer composition is usually the same as the ratio of the corresponding structural units in the particulate polymer. The polymerization may also be carried out in a reaction system containing polymerization additives such as surfactants, emulsifiers, dispersants, polymerization initiators, and chain transfer agents. Specifically, in suspension polymerization (including microsuspension polymerization), a dispersant such as polyvinyl alcohol or magnesium hydroxide may be used to obtain an aqueous dispersion of the particulate polymer. In emulsion polymerization, a latex (aqueous dispersion) of the particulate polymer may also be obtained using an emulsifier such as sodium dodecylbenzenesulfonate.

[0051] The method for producing a binder powder may include a step of drying the particulate polymer after its production. Preferably, the produced particulate polymer is washed and / or purified by an appropriate method, and then dried. In many cases, polymerization of the particulate polymer is carried out in water, so a drying method that can smoothly remove water is preferred. Furthermore, a drying method that can dry the particulate polymer in a redispersible state without excessive adhesion of the primary particles of the particulate polymer to each other is more preferred. Specific examples of drying methods include a method of spray-drying an aqueous dispersion of the particulate polymer; a method of drying in a rotary evaporator; and the like. Furthermore, after spray-drying or drying in a rotary evaporator as described above, it is more preferred to further dry the particulate polymer under vacuum conditions.

[0052] The drying temperature is preferably lower than the minimum film-forming temperature of the particulate polymer from the viewpoint of preventing excessive adhesion between primary particles of the particulate polymer and drying the particulate polymer in a redispersible state. The minimum film-forming temperature of the particulate polymer is preferably 35°C to 100°C from the viewpoint of drying the particulate polymer in a redispersible state and improving the fluidity of the binder powder.

[0053] The minimum film-forming temperature of a particulate polymer refers to the minimum temperature at which a film of the particulate polymer can be formed. The minimum film-forming temperature can be measured, for example, in accordance with JIS K6828-2 (2003) or ISO 2115. Specifically, an aqueous dispersion of a particulate polymer is coated to a thickness of about 100 μm on a flat plate such as an iron plate having an appropriate temperature gradient and dried, and the boundary temperature between the filmed portion and the non-filmed portion is measured. Here, the filmed portion becomes transparent and the non-filmed portion becomes cloudy, so the boundary between the filmed portion and the non-filmed portion can be visually confirmed. Furthermore, when the flat plate after coating and drying with the aqueous dispersion of the particulate polymer is rubbed, the non-filmed portion powders off, so the boundary between the filmed portion and the non-filmed portion can also be confirmed by the presence or absence of powder fall-off. The minimum film-forming temperature can be measured, for example, by conducting a test in accordance with ISO 2115 using a minimum film-forming temperature measuring device (MFFTB90; manufactured by RHOPOINT).

[0054] The method for producing the binder powder preferably includes a step of producing a particulate polymer, drying it as necessary, and then classifying the particulate polymer. There are no limitations on the classification method, but classification by a filtration method using a filter is preferred. Among these, from the viewpoint of smooth classification, filtration using a vibrating sieve such as an ultrasonic sieve is more preferred.

[0055] <Composition Powder Composition> A composite powder composition according to one embodiment of the present invention includes the binder powder and the electrode active material described above. This composite powder composition can be a dry powder composition and can have a powdery form in a room temperature environment (generally, a 25°C environment). This composite powder composition can provide an electrode for a non-aqueous secondary battery that has excellent adhesive strength between the current collector and the electrode active material layer.

[0056] In the composite powder composition, the particulate polymer and electrode active material contained in the binder powder are both in the form of particles. In the composite powder composition, the particulate polymer and the electrode active material may each exist as individual, independent particles. In addition, in the composite powder composition, one or more particulate polymers may adhere to the surface of a particle of the electrode active material to form a composite particle. Furthermore, in the composite powder composition, a plurality of particles of the particulate polymer and the electrode active material, and the composite particle may be bonded together while maintaining their particle shape to form a secondary particle. Usually, such secondary particles are smoothly crushed when subjected to an external force and can return to individual, independent particles (particulate polymer, electrode active material, or composite particle), so the composite powder composition can have high fluidity.

[0057] The binder powder contained in the composite powder composition is as described above. The amount of the binder powder relative to 100% by weight of the composite powder composition is preferably 0.5% by weight or more, more preferably 1.0% by weight or more, even more preferably 1.5% by weight or more, and is preferably 10% by weight or less, more preferably 6% by weight or less, even more preferably 4% by weight or less. When the amount of the binder powder is within the above range, the adhesive strength between the current collector and the electrode active material layer of the electrode manufactured using the composite powder composition can be effectively increased.

[0058] Also, as mentioned above, all or most of the binder powder is usually particulate polymer, and therefore the range of the amount of particulate polymer per 100 wt% of the composite powder composition can be the same as the range of the amount of binder powder per 100 wt% of the composite powder composition.

[0059] The electrode active material can be selected depending on the type of nonaqueous secondary battery. For example, if the nonaqueous secondary battery is a lithium ion secondary battery, the electrode active material can be one that can reversibly insert or release lithium ions by applying a potential in an electrolyte. Such electrode active materials can be classified into positive electrode active materials as electrode active materials for the positive electrode and negative electrode active materials as electrode active materials for the negative electrode.

[0060] As the positive electrode active material for a lithium ion secondary battery, an active material that can be doped and dedoped with lithium ions is used, and examples thereof include positive electrode active materials made of inorganic compounds, positive electrode active materials made of organic compounds, and composite materials that combine these.

[0061] Examples of the inorganic positive electrode active material include transition metal oxides, transition metal sulfides, and lithium-containing composite metal oxides containing lithium and a transition metal, such as Ti, V, Cr, Mn, Fe, Co, Ni, Cu, and Mo.

[0062] Examples of transition metal oxides include MnO and MnO 2 , V 2 O 5 , V 6 O 13 , TiO 2 , Cu 2 V 2 O 3 , amorphous V 2 O-P 2 O 5 , MoO 3 Among them, MnO, V are preferred in terms of cycle stability and capacity. 2 O 5 , V 6 O 13 and TiO 2 is preferred.

[0063] Examples of transition metal sulfides include TiS 2 , TiS 3 , amorphous MoS 2 , FeS, etc.

[0064] Examples of the lithium-containing composite metal oxide include lithium-containing composite metal oxides having a layered structure, lithium-containing composite metal oxides having a spinel structure, and lithium-containing composite metal oxides having an olivine structure. Examples of the lithium-containing composite metal oxides having a layered structure include lithium-containing cobalt oxide (LiCoO 2 ), lithium-containing nickel oxide (LiNiO 2), Co—Ni—Mn lithium composite oxide, Ni—Mn—Al lithium composite oxide, Ni—Co—Al lithium composite oxide, etc. Examples of lithium-containing composite metal oxides having a spinel structure include lithium manganate (LiMn 2 O 4 ), Li[Mn 3/2 M 1 1/2 ]O 4 (Here, M 1 represents a transition metal other than Mn, such as Cr, Fe, Co, Ni, or Cu. Examples of lithium-containing composite metal oxides having an olivine structure include Li X M 2 P.O. 4 (In the formula, M 2 represents at least one element selected from the group consisting of Mn, Fe, Co, Ni, Cu, Mg, Zn, V, Ca, Sr, Ba, Ti, Al, Si, B, and Mo, and X represents a number satisfying 0≦X≦2.

[0065] Examples of the positive electrode active material made of an organic compound include conductive polymers such as polyacetylene and poly-p-phenylene.

[0066] Alternatively, for example, an iron-based oxide may be reduced and fired in the presence of a carbon source to produce a composite material covered with a carbon material, and this composite material may be used as a positive electrode active material. Although iron-based oxides tend to have poor electrical conductivity, such a composite material can be used as a high-performance positive electrode active material.

[0067] The positive electrode active material may be used alone or in combination of two or more. Also, a mixture of the inorganic compound and the organic compound described above may be used as the positive electrode active material.

[0068] Examples of negative electrode active materials for lithium ion secondary batteries include carbonaceous materials such as amorphous carbon, graphite, natural graphite, mesocarbon microbeads, and pitch-based carbon fibers; conductive polymers such as polyacenes; metals or alloys thereof such as silicon, tin, zinc, manganese, iron, and nickel; oxides or sulfates of the above metals or alloys; metallic lithium; lithium alloys such as Li—Al, Li—Bi—Cd, and Li—Sn—Cd; lithium transition metal nitrides; and silicon. Furthermore, materials in which a conductive material is attached to the surface of particles of the negative electrode active material by, for example, mechanical modification, may also be used. The negative electrode active material may be used alone or in combination of two or more.

[0069] Typically, the electrode active material may be particles formed from the above-mentioned materials. The electrode active material preferably has a volume average particle size within a specific range. Specifically, the volume average particle size of the electrode active material is preferably 1 μm or more, more preferably 3 μm or more, even more preferably 5 μm or more, and preferably 50 μm or less, more preferably 40 μm or less, even more preferably 35 μm or less. When the volume average particle size of the electrode active material is within the above range, the adhesive strength between the current collector and the electrode active material layer of the electrode manufactured using the composite powder composition can be effectively increased.

[0070] In addition, the particle size ratio between the average primary particle size of the particulate polymer in the composite powder composition and the volume average particle size of the electrode active material ("average primary particle size of the particulate polymer" / "volume average particle size of the electrode active material") is preferably within a specific range. Specifically, the particle size ratio is preferably 0.01 or more, more preferably 0.03 or more, even more preferably 0.05 or more, and is preferably 1.0 or less, more preferably 0.8 or less, even more preferably 0.5 or less.

[0071] The volume average particle size of the electrode active material can be measured by the following method. The cumulative particle size distribution of the electrode active material is measured in a dry state using a laser diffraction / scattering particle size distribution analyzer. The particle size at which the integrated value of this cumulative particle size distribution, calculated from the small diameter side, is 50% can be obtained as the volume average particle size of the electrode active material. A specific measurement method that can be adopted is the method described in "Method for measuring volume average particle size of electrode active material" in the Examples below.

[0072] The amount of the electrode active material relative to 100% by weight of the composite powder composition is preferably 80% by weight or more, more preferably 85% by weight or more, even more preferably 90% by weight or more, and is preferably 99% by weight or less, more preferably 98.5% by weight or less, even more preferably 98% by weight or less. When the amount of the electrode active material is within the above range, the adhesive strength between the current collector and the electrode active material layer of the electrode produced using the composite powder composition can be effectively increased.

[0073] The composite powder composition may contain any component other than the binder powder and the electrode active material, as long as the effect of the present invention is not significantly impaired. Examples of the optional component include a conductive material. Examples of the conductive material include carbon black such as furnace black, acetylene black, and Ketjen Black (registered trademark); carbon nanotubes; carbon nanohorns; and conductive carbon such as graphene. Among these, carbon black is preferred, and acetylene black is more preferred. One type of conductive material may be used alone, or two or more types may be used in combination.

[0074] The conductive material is generally contained in the composite powder composition in the form of particles.

[0075] The amount of the conductive material is preferably 1 part by weight or more, preferably 10 parts by weight or less, and more preferably 5 parts by weight or less, per 100 parts by weight of the electrode active material.

[0076] The composite powder composition may contain a solvent, or may not contain a solvent. Preferably, the composite powder composition is a dry powder, and therefore preferably does not contain substantially a solvent. The amount of solvent contained in the composite powder composition is preferably 0% to 1% by weight, more preferably 0% to 0.5% by weight, even more preferably 0% to 0.1% by weight, and particularly preferably less than 0.1% by weight.

[0077] There are no particular limitations on the method for producing the composite powder composition. For example, the composite powder composition may be produced by a method including mixing a binder powder, an electrode active material, and, if necessary, optional components such as a conductive material. The mixing is preferably performed by dry mixing. "Dry mixing" refers to mixing in a state that is substantially free of liquid, specifically, mixing at a concentration of solids (components other than liquid) of 99% by weight or more during mixing.

[0078] Specific dry mixing methods include, for example, a container stirring method using a mixing device (e.g., a rocking mixer, a tumbler mixer, etc.) in which the container itself is shaken, rotated, or vibrated to mix; a mechanical stirring method using a mixing device (e.g., a horizontal cylindrical mixer, a V-type mixer, a ribbon mixer, a conical screw mixer, a high-speed fluid mixer, a rotating disk mixer, a high-speed rotating blade mixer, etc.) equipped with a rotating shaft installed horizontally or vertically in the container and an agitator such as a blade, a rotating disk, or a screw attached to the rotating shaft for stirring; and an airflow stirring method in which a swirling airflow caused by compressed gas is used to mix powders in a fluidized bed. These mixing methods may be performed alone or in combination of two or more. Furthermore, after dry mixing, disintegration may be performed using a disintegrator such as a mortar to break up agglomerates. Dry mixing maintains good dispersion of the composite powder composition, thereby improving various physical properties such as coating accuracy.

[0079] <Electrode for non-aqueous secondary battery> An electrode for a non-aqueous secondary battery according to one embodiment of the present invention includes a current collector and an electrode active material layer formed on the current collector using the composite powder composition described above. Therefore, the electrode active material layer typically contains the composite powder composition described above. Hereinafter, the electrode for a non-aqueous secondary battery may be simply referred to as "electrode."

[0080] The current collector material is preferably a material that is electrically conductive and electrochemically durable. Specific examples of the current collector material include metals, carbon, and conductive polymers, with metals being preferred. Examples of metals include copper, aluminum, platinum, nickel, tantalum, titanium, stainless steel, and alloys thereof. Among these, copper, aluminum, and aluminum alloys are preferred in terms of conductivity and voltage resistance. When high voltage resistance is required, high-purity aluminum as disclosed in JP-A-2001-176757 can be preferably used. Among these, aluminum is preferred as the current collector material for the positive electrode, and copper is preferred as the current collector material for the negative electrode. These materials may be used alone or in combination of two or more.

[0081] The current collector generally has a film or sheet shape. The thickness of the current collector may be appropriately selected depending on the intended use, and is preferably 1 μm or more, more preferably 5 μm or more, and even more preferably 10 μm or more, and is preferably 200 μm or less, more preferably 100 μm or less, and even more preferably 50 μm or less.

[0082] The electrode active material layer is formed from the composite powder composition described above. Therefore, this electrode active material layer contains an electrode active material and a particulate polymer, and further contains optional components such as a conductive material, as necessary. In this electrode active material layer, particles of the electrode active material, particles of the conductive material, and particles of the electrode active material and conductive material are bound together by the particulate polymer. In the electrode active material layer, optional components such as the particulate polymer, the electrode active material, and the conductive material may maintain their particle shapes in the composite powder composition, or may be deformed by heat and pressure that may be applied in the process of forming the electrode active material layer. Typically, the electrode active material and the conductive material maintain their particle shapes in the composite powder composition. Furthermore, the particulate polymer may be deformed by heat and pressure.

[0083] The average particle size D of the particulate polymer contained in the electrode active material layer B and the average particle size D of the electrode active material A Relative to D B / D Ais preferably in a specific range. B / D A is preferably 0.01 or more, more preferably 0.03 or more, even more preferably 0.05 or more, and is preferably 1.0 or less, more preferably 0.8 or less, even more preferably 0.5 or less. B / D A When the thickness is within the above range, the adhesive strength between the current collector and the electrode active material layer can be effectively increased.

[0084] Ratio D of the average particle size of the particulate polymer and the electrode active material contained in the electrode active material layer B / D A can be measured by the following method. A cross section is formed in the electrode active material layer. The cross section is observed using a FE-SEM (field emission scanning electron microscope) to obtain a cross-sectional image. In this cross-sectional image of the electrode active material layer, circumscribing circle fitting is performed on the particulate polymer particles (primary particles) in the electrode active material layer to measure the diameter of each of the particulate polymer particles. The average value of the diameters of 50 randomly selected particulate polymer particles is calculated as the average particle diameter D of the particulate polymer in the electrode active material layer. B In addition, in the cross-sectional image, the diameter of each particle of the electrode active material (primary particles) in the electrode active material layer is measured by performing circumscribing circle fitting on the particles. The average value of the diameters of 50 randomly selected particles of the electrode active material is calculated as the average particle diameter D of the electrode active material in the electrode active material layer. A The average particle size D B and D A From the ratio D B / D A As a specific measurement method, the method described later in the Examples section entitled "Method for measuring the ratio of the average particle size of the particulate polymer in the electrode active material layer to the average particle size of the electrode active material" can be adopted.

[0085] The amount of the electrode active material layer per unit area is not particularly limited, but is preferably 10 mg / cm 2 More preferably, 15 mg / cm 2 More preferably, 20 mg / cm 2 or more, preferably 35 mg / cm 2or less, more preferably 30 mg / cm 2 More preferably 25 mg / cm 2 The following is the result.

[0086] The density of the electrode active material layer is not particularly limited, but is preferably 2.5 g / cm 3 More preferably, 3.0 g / cm 3 More preferably, 3.3 g / cm 3 or more, preferably 4.0 g / cm 3 or less, more preferably 3.8 g / cm 3 More preferably, 3.6 g / cm or less 3 The following is the result.

[0087] The thickness of the electrode active material layer is not particularly limited, but is preferably 30 μm or more, more preferably 50 μm or more, and even more preferably 60 μm or more, and is preferably 100 μm or less, more preferably 90 μm or less, and even more preferably 80 μm or less.

[0088] The electrode according to this embodiment exhibits excellent adhesive strength between the current collector and the electrode active material layer. This adhesive strength can be evaluated by the force required to peel the current collector from the electrode active material layer. This force may be referred to as "peel strength" hereinafter. In one example, the peel strength is preferably 10 N / m or more, more preferably 15 N / m or more, and even more preferably 20 N / m or more. The peel strength can be measured by pulling the current collector of an electrode having an electrode active material layer fixed to a flat surface at a pulling rate of 100 mm / min in a direction perpendicular to the flat surface to peel the current collector from the electrode active material layer. A specific method for measuring the peel strength may be the method described in "Method for Evaluating Adhesion Strength Between a Current Collector and an Electrode Active Material Layer" in the Examples below.

[0089] The electrode according to this embodiment can be manufactured by a method including a step of forming an electrode active material layer from the composite powder composition described above. Typically, an electrode active material layer can be formed as a layer of the composite powder composition by forming a layer of the composite powder composition using an appropriate method. The electrode active material layer is preferably formed from the composite powder composition by a dry process. Here, the "dry process" of forming the electrode active material layer from the composite powder composition refers to the formation of the electrode active material layer using a powdered composite powder composition. The composite powder composition may contain a solvent to the extent that the composite powder composition remains in a powdered form. In one example, when forming the electrode active material layer by a dry process, it is preferable to form the electrode active material layer without mixing a liquid such as a solvent into the composite powder composition.

[0090] The electrode manufacturing method may include, for example, a step of forming an electrode active material layer by molding a composite powder composition into a layer, and a step of laminating the resulting electrode active material layer with a current collector. Specifically, the electrode may be manufactured by a method including a step of supplying the composite powder composition to a roll-type pressure molding device equipped with a pair of rolls, and pressure-molding the composite powder composition with the pair of rolls to form an electrode active material layer, and a step of laminating the electrode active material layer with a current collector. As another specific example, the electrode may be manufactured by a method including a step of filling a composite powder composition into a mold, pressure-molding the composite powder composition to form an electrode active material layer, and a step of laminating the electrode active material layer with a current collector. As yet another specific example, the electrode may be manufactured by a method including a step of applying the composite powder composition to a suitable support (e.g., a support sheet), and optionally performing a heat treatment and pressure treatment to form an electrode active material layer, a step of laminating the electrode active material layer with a current collector, and a step of peeling off the support.

[0091] As another specific example, the electrode manufacturing method may include using a roll-type pressure molding apparatus equipped with a pair of rolls, supplying a current collector and a composite powder composition between the pair of rolls, and forming an electrode active material layer on the current collector. In this method, the current collector is fed through the pair of rolls while the composite powder composition is pressure-molded by the pair of rolls to form an electrode active material layer on the current collector. In this case, from the viewpoint of increasing the adhesive strength between the electrode active material layer and the current collector, the roll temperature is preferably Tg + 10°C or higher, more preferably Tg + 30°C or higher, even more preferably Tg + 40°C or higher, and preferably Tg + 120°C or lower, more preferably Tg + 100°C or lower, and even more preferably Tg + 80°C or lower. Here, Tg represents the glass transition temperature of the particulate polymer. In one example, the roll temperature is preferably 25°C or higher, more preferably 50°C or higher, even more preferably 80°C or higher, and preferably 200°C or lower, more preferably 150°C or lower, and even more preferably 120°C or lower. From the viewpoint of improving the uniformity of the thickness of the electrode active material layer, the press linear pressure between the rolls is preferably 10 kN / m or more, more preferably 200 kN / m or more, even more preferably 500 kN / m or more, and is preferably 2000 kN / m or less, more preferably 1500 kN / m or less, even more preferably 1200 kN / m or less. Furthermore, the molding speed during pressure molding is preferably 0.1 m / min or more, more preferably 4 m / min or more, and preferably 20 m / min or less, more preferably 10 m / min or less.

[0092] As another specific example, the electrode manufacturing method may include coating a composite powder composition on a current collector to form an electrode active material layer. Coating of the composite powder composition can be performed, for example, by electrostatic coating. The electrostatic coating method is a method in which a composite powder composition charged by a charging device is coated on a current collector, and the composite powder composition can be efficiently fixed to the current collector by electrostatic attraction. In the electrostatic coating method, the current collector may be earthed or charged with a polarity opposite to that of the composite powder composition in order to increase the electrostatic attraction and efficiently fix the composite powder composition. Furthermore, coating of the composite powder composition is generally performed using a coating device separated from the current collector. For example, the composite powder composition may be applied to the current collector by dropping the composite powder composition from a nozzle installed above the current collector in the direction of gravity. Alternatively, the composite powder composition may be applied to the current collector using an injector (e.g., a spray gun) capable of spraying the composite powder composition by the pressure of a gas such as air. Typically, an electric charge is applied to the composite powder composition in an application device such as the nozzle and injector.

[0093] After the electrode active material layer is formed by coating the composite powder composition on the current collector, a thickness adjustment step may be performed to make the thickness of the electrode active material layer uniform. For example, the electrode active material layer may be smoothed with a blade to make the thickness uniform.

[0094] After the composite powder composition is applied to the current collector to form the electrode active material layer, the current collector and the electrode active material layer may be subjected to a heat treatment. The heat treatment can effectively bond the particulate polymer in the composite powder composition applied to the current collector to any component of the current collector, the electrode active material, and the conductive material, thereby increasing the adhesive strength between the current collector and the electrode active material layer and increasing the mechanical strength of the electrode active material layer.

[0095] After the electrode active material layer is formed by coating the composite powder composition on the current collector, the electrode active material layer may be subjected to a pressure treatment, which can increase the density of the electrode active material layer and thereby increase the capacity of the electrode.

[0096] Typically, the heat treatment and pressure treatment are performed by passing the current collector and the electrode active material layer between a pair of heated rolls. At this time, the heat treatment temperature (roll temperature) is preferably Tg + 10 ° C. or higher, more preferably Tg + 30 ° C. or higher, even more preferably Tg + 40 ° C. or higher, from the viewpoint of increasing the adhesive strength between the electrode active material layer and the current collector, and is preferably Tg + 120 ° C. or lower, more preferably Tg + 100 ° C. or lower, even more preferably Tg + 80 ° C. or lower. Here, Tg represents the glass transition temperature of the particulate polymer. Furthermore, the pressure (linear pressure between the rolls) is preferably 10 kN / m or higher, more preferably 200 kN / m or higher, even more preferably 500 kN / m or higher, and preferably 2000 kN / m or lower, more preferably 1500 kN / m or lower, even more preferably 1200 kN / m or lower, from the viewpoint of improving the thickness uniformity of the electrode active material layer. Furthermore, the running speed of the current collector and the electrode active material layer passing between the rolls is preferably 0.1 m / min or more, more preferably 3 m / min or more, even more preferably 4 m / min or more, and is preferably 50 m / min or less, more preferably 20 m / min or less, even more preferably 10 m / min or less.

[0097] The above-described manufacturing method can produce an electrode including a current collector and an electrode active material layer, but the manufacturing method of the electrode may further include any other steps. For example, from the viewpoint of reducing the variation in the thickness of the electrode or increasing the density of the electrode active material layer to further increase the capacity, a post-pressing treatment may be performed as necessary. The method of the post-pressing treatment is preferably a roll pressing method. In the roll pressing method, the electrode is passed between two rolls placed in parallel to apply pressure to the electrode. In this case, the temperature of the rolls may be adjusted, for example, by heating or cooling, as necessary.

[0098] <Nonaqueous Secondary Battery> A nonaqueous secondary battery according to one embodiment of the present invention includes an electrode according to the above-described embodiment. Typically, such a nonaqueous secondary battery includes a positive electrode, a negative electrode, and a nonaqueous electrolyte solution, and includes an electrode according to the above-described embodiment as at least one of the positive electrode and the negative electrode. Therefore, in the nonaqueous secondary battery, the positive electrode may be the electrode according to the above-described embodiment, the negative electrode may be the electrode according to the above-described embodiment, or both the positive electrode and the negative electrode may be the electrodes according to the above-described embodiment.

[0099] The non-aqueous electrolyte solution may be, for example, an electrolyte solution in which a supporting electrolyte is dissolved in a non-aqueous solvent. The supporting electrolyte is preferably a lithium salt. For example, LiPF 6 , LiAsF 6 , LiBF 4 , LiSbF 6 , LiAlCl 4 , LiClO 4 , C.F. 3 SO 3 Li, C 4 F 9 SO 3 Li, CF 3 COOLi, (CF 3 CO) 2 NLi, (CF 3 SO 2 ) 2 NLi, (C 2 F 5 SO 2 Among them, LiPF6 is easily soluble in solvents and exhibits a high degree of dissociation. 6 , LiClO 4 , C.F. 3 SO 3 Li is preferred. The supporting electrolyte may be used alone or in combination of two or more. In general, the use of a supporting electrolyte with a higher degree of dissociation tends to result in higher ionic conductivity.

[0100] The concentration of the supporting electrolyte is preferably set in the range of 0.5 mol / L to 2.5 mol / L depending on the type of supporting electrolyte, since this range allows for high ionic conductivity and improves the charge and discharge characteristics of the nonaqueous secondary battery.

[0101] The nonaqueous solvent used in the nonaqueous electrolyte solution is not particularly limited as long as it can dissolve the supporting electrolyte. Examples of nonaqueous solvents include carbonate solvents such as dimethyl carbonate (DMC), ethylene carbonate (EC), diethyl carbonate (DEC), propylene carbonate (PC), butylene carbonate (BC), and methyl ethyl carbonate (MEC); ester solvents such as γ-butyrolactone and methyl formate; ether solvents such as 1,2-dimethoxyethane and tetrahydrofuran; sulfur-containing compound solvents such as sulfolane and dimethyl sulfoxide; and ionic liquids that are also used as supporting electrolytes. Among these, carbonate solvents are preferred because of their high dielectric constant and wide stable potential range. One type of nonaqueous solvent may be used alone, or two or more types may be used in combination. Generally, the lower the viscosity of the nonaqueous solvent, the higher the ionic conductivity, and the higher the dielectric constant, the higher the solubility of the supporting electrolyte. However, since there is a trade-off between the two, it is preferable to adjust the ionic conductivity by adjusting the type and mixing ratio of the solvent. The non-aqueous solvent may be used in combination with a solvent in which all or part of the hydrogen atoms are replaced by fluorine atoms, or the entire amount of the solvent may be used.

[0102] The non-aqueous electrolyte may contain any additive in combination with the supporting electrolyte and the non-aqueous solvent. Examples of the optional additive include carbonate compounds such as vinylene carbonate (VC); sulfur-containing compounds such as ethylene sulfite (ES); and fluorine-containing compounds such as fluoroethylene carbonate (FEC). One type of additive may be used alone, or two or more types may be used in combination.

[0103] The nonaqueous secondary battery may further include a separator. Examples of the separator include a microporous membrane or nonwoven fabric formed from a resin such as a polyolefin resin or an aromatic polyamide resin; a porous resin-coated membrane containing an inorganic ceramic powder; and the like. Specific examples of the separator include a microporous membrane formed from a resin such as a polyolefin polymer (e.g., polyethylene, polypropylene, polybutene, polyvinyl chloride) or a mixture or copolymer thereof; a microporous membrane formed from a resin such as polyethylene terephthalate, polycycloolefin, polyethersulfone, polyamide, polyimide, polyimideamide, polyaramid, polycycloolefin, nylon, or polytetrafluoroethylene; a fabric material woven from polyolefin resin fibers or a nonwoven fabric of the fibers; and an aggregate of insulating material particles. Among these, a microporous membrane formed from a polyolefin resin is preferred from the viewpoint of reducing the overall separator thickness and increasing the active material ratio in the nonaqueous secondary battery to improve the capacity per volume.

[0104] The thickness of the separator is preferably 1.0 μm or more, more preferably 3 μm or more, and is preferably 40 μm or less, more preferably 30 μm or less, and even more preferably 25 μm or less, from the viewpoint of reducing the internal resistance of the separator in the nonaqueous secondary battery and from the viewpoint of excellent workability when producing the nonaqueous secondary battery.

[0105] Examples of methods for producing nonaqueous secondary batteries include stacking a positive electrode and a negative electrode with a separator interposed therebetween, rolling or folding the resulting stack according to the battery shape, placing the stack in a battery container, injecting an electrolyte into the battery container, and sealing the container. Furthermore, if necessary, expandable metals; overcurrent protection elements such as fuses and PTC elements; lead plates, etc. may be inserted to prevent pressure buildup within the battery and overcharging and discharging. The shape of the nonaqueous secondary battery may be, for example, a coin type, button type, sheet type, cylindrical type, prismatic type, flat type, etc. The battery container is preferably made of a material that prevents moisture from penetrating into the battery, such as a metal or a laminate of aluminum.

[0106] The nonaqueous secondary battery does not require a large amount of solvent-containing slurry in the process of producing the composite powder composition and the electrode, which reduces the energy required for production. Furthermore, continuous operation is easy, and the yield can be increased.

[0107] The present invention will be specifically described below with reference to examples. However, the present invention is not limited to the examples shown below, and may be modified as desired within the scope of the claims and their equivalents. In the following description, "%" and "parts" representing amounts are by weight unless otherwise specified. Furthermore, the operations described below were carried out in air at room temperature and normal pressure (25°C, 1 atm) unless otherwise specified.

[0108] <Method for measuring the sieve residue rate of binder powder> The following sieve test was performed using a sieve with a mesh size of 250 μm (60 mesh) and a sieve with a mesh size of 74 μm (200 mesh), and the sieve residue rate of the binder powder in the sieve test using each sieve was measured. W(0) g of binder powder was sieved using the sieves. The weight W(1) g of the binder powder (residual component) remaining on the sieve was measured. The sieve residue rate was calculated using the following formula (M1). Sieve residue rate (%) = W(1) / W(0) × 100 (M1)

[0109] <Method for measuring the average primary particle size of the particulate polymer contained in the binder powder> The binder powder was added to a 1% aqueous solution of linear alkylbenzenesulfonate sodium, and the mixture was dispersed by ultrasonic waves to obtain a dispersion in which the particulate polymer contained in the binder powder was dispersed. The cumulative particle size distribution of this dispersion was measured using a Coulter counter (a particle size measuring instrument "Coulter Counter LS230" manufactured by Coulter). The particle size at which the integrated value accumulated from the small diameter side of this cumulative particle size distribution reached 50% was obtained as the volume-based average primary particle size of the particulate polymer contained in the binder powder.

[0110] <Method for measuring glass transition temperature> The glass transition temperature Tg of the particulate polymer contained in the binder powder was measured using a differential scanning calorimeter (manufactured by Nano Technology Co., Ltd., "DSC6220SII") at a temperature rise rate of 20°C / min in accordance with JIS K 7121:1987.

[0111] <Method for measuring volume average particle size of electrode active material> The electrode active material was subjected to dry cumulative particle size distribution measurement using a laser diffraction / scattering particle size distribution analyzer (Microtrac MT3200II manufactured by Nikkiso Co., Ltd.) The particle size at which the integrated value, calculated from the small diameter side of this cumulative particle size distribution, reached 50% was obtained as the volume average particle size of the electrode active material.

[0112] <Method for measuring the ratio of the average particle size of the particulate polymer in the electrode active material layer to the average particle size of the electrode active material> A cross section for observation was formed on the positive electrode using a cross section polisher (manufactured by JEOL Ltd., "IB-09020CP"). Next, the cross section was observed using an FE-SEM (field emission scanning electron microscope, manufactured by JEOL Ltd., "JSM-7800F"). The cross section was observed at a magnification of 1000x, an irradiation voltage of 1 kV, and an irradiation current of 5.0 × 10 -8 The experiment was carried out under the conditions of A.

[0113] In the cross-sectional image of the positive electrode active material layer obtained by cross-sectional observation, the diameter of each of the particulate polymer particles (primary particles) in the positive electrode active material layer was measured by performing circumscribing circle fitting on the particles. The average value of the diameters of 50 randomly selected particulate polymer particles was taken as the average particle diameter D of the particulate polymer in the positive electrode active material layer. B Specifically, the cross-sectional images were analyzed using image analysis software (Mitani Shoji Co., Ltd., "WinROOF"), with the emphasis conditions set to "brightness: 40" and "contrast: +30," a filter set to 7x7, and two threshold values ​​set to binarize (threshold values ​​119 and 165). The surface of each of the 50 obtained SEM images was then viewed in plan view to determine the area of ​​the particulate polymer. Assuming that the particulate polymers were perfect spheres, the diameter of the particulate polymer was calculated from the area of ​​the obtained particulate polymer. The volume was calculated from the diameters of the 50 particulate polymers, assuming that the particulate polymers were perfect spheres. The total volume of all the particulate polymers was set to 100%, and the volume of the particulate polymers present in each particle size range was expressed as a percentage. The particle diameter at which the integrated volume of the particulate polymers, calculated from the small diameter side, reached 50% was defined as the average particle diameter (D B )

[0114] In addition, in the cross-sectional image of the positive electrode active material layer obtained by cross-sectional observation, the diameter of each particle of the positive electrode active material in the positive electrode active material layer was measured by performing circumscribing circle fitting on the particles of the positive electrode active material in the positive electrode active material layer. The average value of the diameters of 50 randomly selected positive electrode active material particles was defined as the average particle diameter D of the positive electrode active material in the positive electrode active material layer. A Specifically, the cross-sectional images were analyzed using image analysis software (Mitani Shoji Co., Ltd., "WinROOF") with the emphasis conditions set to "brightness: 40" and "contrast: +30," a filter set to 7x7, and two threshold values ​​(threshold values ​​195 and 255) for binarization. The surface of each of the 50 SEM images obtained was then viewed in plan view to determine the area of ​​the positive electrode active material particles. The positive electrode active material particles were assumed to be perfect spheres, and the diameters of the positive electrode active material particles were calculated from the areas of the obtained positive electrode active material particles. The volumes of the 50 positive electrode active material particles were calculated from the diameters of the positive electrode active material particles, assuming that the positive electrode active material particles were perfect spheres. The total volume of all the positive electrode active material particles was set to 100%, and the volume of the positive electrode active material particles present in each particle size range was expressed as a percentage. The particle diameter at which the cumulative volume of the positive electrode active material particles, calculated from the smallest diameter side, reached 50% was defined as the average particle diameter (D A )

[0115] Average particle size D of the particulate polymer in the positive electrode active material layer B and the average particle size D of the positive electrode active material A The ratio (D B / D A ) was calculated.

[0116] <Method for Evaluating Adhesion Strength Between Current Collector and Electrode Active Material Layer> A rectangular test piece measuring 40 mm in length and 10 mm in width was cut from a positive electrode. Cellophane tape (compliant with JIS Z1522) was fixed to a stable test table, and the test piece was attached to the cellophane tape. The attachment was performed so that the positive electrode active material layer of the test piece was in contact with the cellophane tape. One end of the current collector was pulled vertically at a pulling rate of 100 mm / min to measure the stress when the current collector was peeled off. This stress measurement was performed three times, and the average value of the stresses was calculated as the peel strength. A higher peel strength indicates better adhesion strength between the positive electrode active material layer and the current collector. Therefore, based on the measured peel strength, the adhesive strength was evaluated according to the following criteria: A: Peel strength of 30 N / m or more; B: Peel strength of 25 N / m or more but less than 30 N / m. C: Peel strength is 20 N / m or more and less than 25 N / m. D: Peel strength is less than 20 N / m.

[0117] Example 1 (1-1. Production of binder powder) - Preparation of monomer composition - A monomer composition was prepared by mixing 67.0 parts of styrene as an aromatic monovinyl monomer, 32.5 parts of n-butyl acrylate as a (meth)acrylic acid alkyl ester monomer, and 0.5 parts of ethylene glycol dimethacrylate as a crosslinkable monomer.

[0118] - Preparation of Metal Hydroxide - An aqueous magnesium chloride solution prepared by dissolving 10.0 parts of magnesium chloride in 200 parts of ion-exchanged water and an aqueous sodium hydroxide solution prepared by dissolving 7.0 parts of sodium hydroxide in 50 parts of ion-exchanged water were prepared. The aqueous sodium hydroxide solution was gradually added to the aqueous magnesium chloride solution with stirring to prepare a colloidal dispersion containing magnesium hydroxide as the metal hydroxide.

[0119] - Suspension polymerization - A particulate polymer was prepared by suspension polymerization. Specifically, the monomer composition obtained as described above was added to the colloidal dispersion containing the magnesium hydroxide, followed by further stirring. Thereafter, 3.0 parts of t-butylperoxy-2-ethylhexanoate (manufactured by NOF Corporation, "Perbutyl O") as a polymerization initiator was further added to the colloidal dispersion to obtain a mixed solution. The obtained mixed solution was subjected to high-shear stirring at 12,000 rpm for 1 minute using an in-line emulsifying disperser (manufactured by Pacific Machinery Works, "Cavitron") to form droplets of the monomer composition in the colloidal dispersion containing magnesium hydroxide.

[0120] The colloidal dispersion in which droplets of the monomer composition were formed as described above was placed in a reactor, heated to 90°C, and subjected to a polymerization reaction for 5 hours to obtain a dispersion. This dispersion was purified by subjecting it to a reduced pressure treatment at 90°C for 2 hours using an evaporator to obtain an aqueous dispersion containing a particulate polymer.

[0121] Washing, Drying, and Classification While stirring the aqueous dispersion containing the particulate polymer, sulfuric acid was added dropwise at room temperature (25°C) and acid washing was performed until the pH reached 6.5 or less. Subsequently, a water washing treatment, which included, in this order, filtering out the solid content, dehydrating the obtained solid content, and adding 500 parts of ion-exchanged water to the solid content to form a reslurry, was repeated 10 times. After that, filtration was performed, and the obtained solid content was placed in a dryer and dried at 40°C for 48 hours. The dried solid content was classified using an ultrasonic sieve (mesh opening: 75 μm) to obtain a binder powder having a powdery form. The particulate polymer contained in the obtained binder powder was solid particles without internal voids. The obtained binder powder was evaluated by the method described above.

[0122] (1-2. Production of composite powder composition) NMC811 (LiNi) as a positive electrode active material was mixed in a high-speed mixer (FS2 type, manufactured by Earth Technica Co., Ltd.). 0.8 Mn 0.1 Co 0.1 O 296.0 parts of carbon black (volume average particle size: 30.0 μm) and 2.0 parts of carbon black (Super C65, manufactured by Imerys) as a conductive material (solids equivalent) were added and mixed for 30 minutes at 10°C, an agitator rotation speed of 2000 rpm, and a chopper rotation speed of 3500 rpm. Thereafter, 2.0 parts of the binder powder prepared above was added and mixed for 30 minutes at 10°C, an agitator rotation speed of 500 rpm, and a chopper rotation speed of 800 rpm, to obtain a powdered composite powder composition.

[0123] (1-3. Production of Positive Electrode: Dry Method (Electrostatic Coating)) Using an electrostatic screen printing device (manufactured by Berg Kogyo Co., Ltd., "T-1"), the above composite powder composition was dry coated onto an aluminum foil (thickness 15 μm) as a current collector to obtain a positive electrode blank. The coating was carried out so that the amount of the coated composite powder composition per unit area of ​​the current collector (coating weight) was 18 mg / cm. 2 This positive electrode blank was subjected to a hot roll press (temperature 130°C, load 30 t) to obtain a positive electrode including a current collector and a positive electrode active material layer (density of the positive electrode active material layer: 3.3 g / cm 3 The resulting positive electrode was evaluated by the method described above.

[0124] Example 2 A binder powder, a composite powder composition, and a positive electrode were produced and evaluated in the same manner as in Example 1, except that an ultrasonic sieve with a mesh size of 100 μm was used in the classification of step (1-1).

[0125] Example 3 A binder powder, a composite powder composition, and a positive electrode were produced and evaluated in the same manner as in Example 1, except that an ultrasonic sieve with a mesh size of 297 μm was used in the classification of step (1-1).

[0126] Example 4 - Emulsion Polymerization Method - A monomer composition containing 63 parts of styrene as an aromatic monovinyl monomer, 24.5 parts of n-butyl acrylate as a (meth)acrylic acid alkyl ester monomer, 2 parts of methacrylic acid as an ethylenically unsaturated carboxylic acid monomer, and 10 parts of glycidyl methacrylate and 0.5 parts of ethylene glycol dimethacrylate as crosslinkable monomers, 1 part of sodium dodecylbenzenesulfonate as an emulsifier, 150 parts of ion-exchanged water, and 0.5 parts of potassium persulfate as a polymerization initiator was placed in a 5 MPa pressure vessel equipped with a stirrer, and after thorough stirring, the mixture was heated to 60°C to initiate polymerization. When the polymerization conversion rate reached 96%, the reaction was stopped by cooling, and an aqueous dispersion containing a particulate polymer was obtained. The particulate polymer obtained in this manner was solid particles.

[0127] - Drying and Classification - The aqueous dispersion obtained above was dried using a spray dryer ("ADL311-A" manufactured by Yamato Scientific Co., Ltd.) to obtain a powdery solid. Specifically, the aqueous dispersion was diluted with ion-exchanged water to 10% by weight, and the dispersion was prepared under conditions of an inlet temperature of 110°C and a flow rate of 3.0 g / min. The dried powdery solid was classified using an ultrasonic sieve (mesh opening 75 μm) to obtain a binder powder having a powdery form. The particulate polymer contained in the obtained binder powder was solid particles without internal voids. The obtained binder powder was evaluated by the method described above.

[0128] In step (1-2), the binder powder produced in Example 4 was used instead of the binder powder produced in Example 1. In addition, in step (1-2), the type of the positive electrode active material was changed to NMC811 (LiNi 0.8 Mn 0.1 Co 0.1 O 2 The powder composite composition and the positive electrode were produced and evaluated in the same manner as in Example 1, except for the above-mentioned points.

[0129] Example 5 The amount of sodium dodecylbenzenesulfonate used as an emulsifier was changed to 0.5 parts. The type of positive electrode active material was changed to NMC811 (LiNi 0.8 Mn 0.1 Co0.1 O 2 The binder powder, composite powder composition, and positive electrode were produced and evaluated in the same manner as in Example 4, except for the above-mentioned points.

[0130] Example 6 In the suspension polymerization in step (1-1), the amount of magnesium chloride was changed from 10.0 parts to 15.0 parts, and the amount of sodium hydroxide was changed from 7.0 parts to 10.5 parts. In step (1-2), the type of the positive electrode active material was changed to NMC811 (LiNi 0.8 Mn 0.1 Co 0.1 O 2 The binder powder, composite powder composition, and positive electrode were produced and evaluated in the same manner as in Example 1, except for the above points.

[0131] Example 7 A binder powder, a composite powder composition, and a positive electrode were produced and evaluated in the same manner as in Example 1, except that in the suspension polymerization in step (1-1), the amount of magnesium chloride was changed from 10.0 parts to 5.0 parts, and the amount of sodium hydroxide was changed from 7.0 parts to 3.5 parts.

[0132] Example 8 A binder powder, a composite powder composition, and a positive electrode were produced and evaluated in the same manner as in Example 1, except that in the suspension polymerization of step (1-1), the amount of magnesium chloride was changed from 10.0 parts to 3.0 parts, and the amount of sodium hydroxide was changed from 7.0 parts to 2.1 parts.

[0133] Example 9 The amount of sodium dodecylbenzenesulfonate used as an emulsifier was changed to 1.5 parts. The type of positive electrode active material was changed to NMC811 (LiNi 0.8 Mn 0.1 Co 0.1 O 2 The binder powder, composite powder composition, and positive electrode were produced and evaluated in the same manner as in Example 4, except for the above-mentioned points.

[0134] Example 10 A binder powder, a composite powder composition, and a positive electrode were produced and evaluated in the same manner as in Example 1, except that in the suspension polymerization of step (1-1), the amount of magnesium chloride was changed from 10.0 parts to 2.0 parts, and the amount of sodium hydroxide was changed from 7.0 parts to 1.4 parts.

[0135] Example 11 A binder powder, a composite powder composition, and a positive electrode were produced and evaluated in the same manner as in Example 1, except that in step (1-2), the binder powder produced in Example 4 was used instead of the binder powder produced in Example 1.

[0136] Example 12 In the suspension polymerization in step (1-1), the amount of magnesium chloride was changed from 10.0 parts to 3.0 parts, and the amount of sodium hydroxide was changed from 7.0 parts to 2.1 parts. In step (1-2), the type of the positive electrode active material was changed to NMC811 (LiNi 0.8 Mn 0.1 Co 0.1 O 2 The binder powder, composite powder composition, and positive electrode were produced and evaluated in the same manner as in Example 1, except for the above points.

[0137] Example 13 A binder powder, a composite powder composition, and a positive electrode were produced and evaluated in the same manner as in Example 1, except that in the preparation of the monomer composition in step (1-1), the amount of styrene as the aromatic monovinyl monomer was changed to 50.0 parts, and the amount of n-butyl acrylate as the (meth)acrylic acid alkyl ester monomer was changed to 49.5 parts.

[0138] Example 14 A binder powder, a composite powder composition, and a positive electrode were produced and evaluated in the same manner as in Example 1, except that in the preparation of the monomer composition in step (1-1), the amount of styrene as the aromatic monovinyl monomer was changed to 87.3 parts, and the amount of n-butyl acrylate as the (meth)acrylic acid alkyl ester monomer was changed to 2.2 parts.

[0139] Example 15 A binder powder, a composite powder composition, and a positive electrode were produced and evaluated in the same manner as in Example 1, except that in the preparation of the monomer composition in step (1-1), the amount of styrene as the aromatic monovinyl monomer was changed to 99.5 parts, and the amount of n-butyl acrylate as the (meth)acrylic acid alkyl ester monomer was changed to 0 parts.

[0140] Example 16 A binder powder, a composite powder composition, and a positive electrode were produced and evaluated in the same manner as in Example 1, except that in the preparation of the monomer composition in step (1-1), the amount of styrene as the aromatic monovinyl monomer was changed to 47.0 parts, and the amount of n-butyl acrylate as the (meth)acrylic acid alkyl ester monomer was changed to 52.5 parts.

[0141] Example 17 Polyvinylidene fluoride (PVDF, manufactured by Arkema, "KYNAR HSV900") was used as a raw material for the binder powder, and was classified using an ultrasonic sieve (mesh opening: 75 μm) to obtain a binder powder. The obtained binder powder was evaluated by the method described above.

[0142] In step (1-2), the binder powder produced in Example 17 was used instead of the binder powder produced in Example 1. In addition, in step (1-2), the type of the positive electrode active material was changed to NMC811 (LiNi 0.8 Mn 0.1 Co 0.1 O 2 The volume average particle size was changed to 3.0 μm. Except for the above, the composite powder composition and the positive electrode were produced and evaluated in the same manner as in Example 1.

[0143] <Comparative Example 1> A binder powder, a composite powder composition, and a positive electrode were produced and evaluated in the same manner as in Example 1, except that in step (1-1), classification was performed using an ultrasonic sieve with a mesh size of 354 μm.

[0144] Comparative Example 2: The amount of sodium dodecylbenzenesulfonate used as an emulsifier was changed to 2.0 parts. The type of the positive electrode active material was changed to NMC811 (LiNi 0.8 Mn 0.1 Co 0.1 O2 The binder powder, composite powder composition, and positive electrode were produced and evaluated in the same manner as in Example 4, except for the above-mentioned points.

[0145] <Comparative Example 3> Polyvinylidene fluoride (PVDF, manufactured by Arkema, "KYNAR HSV900") was used as a raw material for the binder powder, and was classified using an ultrasonic sieve (mesh opening: 354 μm) to obtain a binder powder. The obtained binder powder was evaluated by the method described above.

[0146] In step (1-2), the binder powder produced in Comparative Example 3 was used instead of the binder powder produced in Example 1. In addition, in step (1-2), the type of the positive electrode active material was changed to NMC811 (LiNi 0.8 Mn 0.1 Co 0.1 O 2 The volume average particle size was changed to 3.0 μm. Except for the above, the composite powder composition and the positive electrode were produced and evaluated in the same manner as in Example 1.

[0147] <Results> The results of the above-mentioned Examples and Comparative Examples are shown in the table below. In the table below, the meanings of the abbreviations are as follows: Tg: glass transition temperature PVDF: polyvinylidene fluoride Sieve residue (250 μm): sieve residue in a sieve test using a sieve with a mesh size of 250 μm Sieve residue (74 μm): sieve residue in a sieve test using a sieve with a mesh size of 250 μm

[0148]

[0149]

[0150]

Claims

1. A binder powder for non-aqueous secondary battery electrodes, comprising a particulate polymer having an average primary particle size of 0.3 μm or more, wherein the proportion of particles having a particle size exceeding 250 μm is 10% by weight or less.

2. The binder powder for a non-aqueous secondary battery electrode according to claim 1, wherein the proportion of particles having a particle size exceeding 74 μm in the binder powder is 10% by weight or less.

3. The binder powder for a non-aqueous secondary battery electrode according to claim 1, wherein the particulate polymer has an average primary particle size of 0.5 μm or more and 15 μm or less.

4. The binder powder for a non-aqueous secondary battery electrode according to claim 1, wherein the particulate polymer has a glass transition temperature of 35° C. or more and 100° C. or less.

5. A composite powder composition comprising the binder powder for a non-aqueous secondary battery electrode according to any one of claims 1 to 4 and an electrode active material.

6. An electrode for a non-aqueous secondary battery comprising a current collector and an electrode active material layer formed on the current collector from the composite powder composition according to claim 5.

7. The average particle diameter D of the particulate polymer contained in the electrode active material layer B and the average particle size D of the electrode active material A Compared to D B / D A The electrode for a non-aqueous secondary battery according to claim 6 , wherein is 0.01 or more and 1.0 or less.

8. A non-aqueous secondary battery comprising the electrode for a non-aqueous secondary battery according to claim 6.

9. A method for producing an electrode for a non-aqueous secondary battery, comprising the step of forming an electrode active material layer from the composite powder composition according to claim 5 by a dry process.

Citation Information

Patent Citations

  • Electric double-layer capacitor

    JP2001176757A

  • Binder for electrochemical element electrode, particle composite for electrochemical element electrode, electrochemical element electrode, electrochemical element, and method for producing electrochemical element electrode

    JP6327249B2

  • Nonaqueous secondary battery functional layer composition, nonaqueous secondary battery functional layer, and nonaqueous secondary battery

    US20200052270A1

  • Adhesive interlayer for battery electrode through dry manufacturing

    US20200144591A1

  • Nonaqueous secondary battery functional layer composition, nonaqueous secondary battery functional layer, and nonaqueous secondary battery

    WO2018034093A1