Binder composition for non-aqueous secondary battery negative electrode, slurry composition for non-aqueous secondary battery negative electrode, negative electrode for non-aqueous secondary battery, and non-aqueous secondary battery
A binder composition with a particulate binder of specific monomer units and particle size distribution addresses the issue of negative electrode swelling in non-aqueous secondary batteries, enhancing cycle performance by forming a strong network within the electrode composite layer.
Patent Information
- Application Number
- PCT/JP2024/011128
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-29
- Filing Date
- 2024-03-21
- Publication Date
- 2024-10-03
AI Technical Summary
Existing binder compositions for non-aqueous secondary battery negative electrodes do not adequately suppress swelling during repeated charging and discharging, leading to suboptimal cycle characteristics.
A binder composition containing a particulate binder with a specific ratio of ethylenically unsaturated carboxylic acid, aromatic vinyl, and aliphatic conjugated diene monomer units, with controlled average particle diameters and insoluble content in tetrahydrofuran, forming a strong network to prevent swelling and enhance cycle performance.
The binder composition effectively suppresses negative electrode swelling and improves cycle characteristics of non-aqueous secondary batteries by forming a robust network, even with silicon-based active materials that expand significantly during charging and discharging.
Smart Images

Figure JP2024011128_03102024_PF_FP_ABST
Abstract
Description
Binder composition for non-aqueous secondary battery negative electrode, slurry composition for non-aqueous secondary battery negative electrode, non-aqueous secondary battery negative electrode, and non-aqueous secondary battery
[0001] The present invention relates to a binder composition for a non-aqueous secondary battery negative electrode, a slurry composition for a non-aqueous secondary battery negative electrode, a non-aqueous secondary battery negative electrode, and a non-aqueous secondary battery.
[0002] Non-aqueous secondary batteries such as lithium ion secondary batteries (hereinafter sometimes simply referred to as "secondary batteries") are small, lightweight, have high energy density, and are capable of repeated charge and discharge, and are therefore used in a wide range of applications. Therefore, in recent years, improvements to battery components such as electrodes have been investigated with the aim of further improving the performance of non-aqueous secondary batteries.
[0003] An electrode used in a secondary battery typically includes a current collector and an electrode mixture layer (positive electrode mixture layer or negative electrode mixture layer) formed on the current collector. The electrode mixture layer is formed, for example, by applying a slurry composition containing an electrode active material and a binder composition containing a binding agent onto the current collector and then drying the applied slurry composition.
[0004] In recent years, efforts have been made to improve the binder compositions used in forming electrode mixture layers in order to further improve the performance of secondary batteries. For example, Patent Document 1 discloses a binder composition for an electric storage device electrode capable of producing an electric storage device (secondary battery) electrode that exhibits excellent adhesion and good charge / discharge durability. The binder composition includes a polymer A containing 20 to 70 parts by mass of repeating units derived from an unsaturated carboxylic acid and 0 to 30 parts by mass of repeating units derived from an unsaturated carboxylic acid ester, where the total of all repeating units contained is taken as 100 parts by mass, and having a swelling ratio in an electrolytic solution of 130% or less, and a liquid solvent (B). In the examples of Patent Document 1, the polymer A is obtained by two-stage polymerization, in which a predetermined monomer mixture is polymerized in the first stage, followed by further polymerization of an unsaturated carboxylic acid such as methacrylic acid in the second stage. The polymer A obtained by such two-stage polymerization may have a so-called core-shell structure.
[0005] JP 2016-58184 A
[0006] However, when the binder composition of Patent Document 1 is used to prepare a negative electrode of a secondary battery, there is room for improvement in terms of sufficiently suppressing swelling of the negative electrode due to repeated charge and discharge, and in terms of enabling the secondary battery to exhibit excellent cycle characteristics.
[0007] Therefore, an object of the present invention is to provide a binder composition for a non-aqueous secondary battery negative electrode that effectively suppresses swelling of the negative electrode due to repeated charge / discharge and enables the secondary battery to exhibit excellent cycle characteristics. Another object of the present invention is to provide a slurry composition for a non-aqueous secondary battery negative electrode that effectively suppresses swelling of the negative electrode due to repeated charge / discharge and enables the secondary battery to exhibit excellent cycle characteristics. Another object of the present invention is to provide a non-aqueous secondary battery negative electrode that is less likely to swell even with repeated charge / discharge and enables the secondary battery to exhibit excellent cycle characteristics. Another object of the present invention is to provide a non-aqueous secondary battery that is less likely to swell the negative electrode due to charge / discharge and has excellent cycle characteristics.
[0008] The present inventors have conducted extensive research with the aim of solving the above-mentioned problems, and have newly discovered that the above-mentioned problems can be solved by using a binder composition for a non-aqueous secondary battery negative electrode containing a particulate binder and water, the particulate binder containing a polymer containing predetermined monomer units in a predetermined ratio, and having particle diameters measured by different predetermined methods that satisfy a predetermined relationship, and have completed the present invention.
[0009] That is, an object of the present invention is to advantageously solve the above-mentioned problems, and [1] the present invention provides a binder composition for a non-aqueous secondary battery negative electrode, comprising a particulate binder and water, wherein the particulate binder comprises a polymer containing an ethylenically unsaturated carboxylic acid monomer unit, an aromatic vinyl monomer unit, and an aliphatic conjugated diene monomer unit, and the content of the ethylenically unsaturated carboxylic acid monomer unit is 5.0 mass% or more and 1.0 mass% or less when the total repeating units of the polymer are taken as 100 mass%. The particulate binder has an average particle diameter Da when a binder composition for a non-aqueous secondary battery negative electrode adjusted to have a solids concentration of 0.5% by mass is measured by dynamic light scattering, an average particle diameter Db when a binder composition for a non-aqueous secondary battery negative electrode adjusted to have a solids concentration of 0.005% by mass is measured by dynamic light scattering, and an average particle diameter Dc when the binder composition for a non-aqueous secondary battery negative electrode is measured by laser diffraction scattering, which satisfy the following formulas (1) and (2): Da - Db ≦ 60.0 nm (1) 1.40 ≦ Da / Dc ≦ 2.00 (2) This is a binder composition for a non-aqueous secondary battery negative electrode. The binder composition for a non-aqueous secondary battery negative electrode as described above can effectively suppress swelling of the negative electrode due to repeated charge and discharge, and can enable the secondary battery to exhibit excellent cycle characteristics. In this specification, the average particle diameter Da, average particle diameter Db, and average particle diameter Dc can be measured according to the method described in the Examples. In this specification, the phrase "containing a monomer unit" means that "a polymer obtained using the monomer contains a structural unit derived from the monomer." The content ratio of the monomer unit in the polymer is expressed as follows: 1 It can be measured using a nuclear magnetic resonance (NMR) method such as H-NMR.
[0010] [2] In the binder composition for a non-aqueous secondary battery negative electrode according to [1] above, the particulate binder preferably has an insoluble content in tetrahydrofuran of more than 90% by mass and less than 100% by mass. When the insoluble content in tetrahydrofuran of the particulate binder is within the above range, the battery characteristics of the resulting secondary battery can be improved. In this specification, the "insoluble content in tetrahydrofuran" of the particulate binder can be measured according to the method described in the Examples.
[0011] [3] In the binder composition for a non-aqueous secondary battery negative electrode according to [1] or [2] above, the content of the aliphatic conjugated diene monomer unit is preferably 30.0% by mass or more and 60.0% by mass or less, where the total repeating units of the polymer are taken as 100% by mass. When the content of the aliphatic conjugated diene monomer unit is equal to or more than the lower limit, swelling of the resulting negative electrode can be effectively suppressed. On the other hand, when the content of the aliphatic conjugated diene monomer unit is equal to or less than the upper limit, the cycle characteristics of the resulting secondary battery can be improved.
[0012] [4] In the binder composition for a non-aqueous secondary battery negative electrode according to any one of [1] to [3] above, the polymer preferably further contains an ethylenically unsaturated amide monomer unit. If the polymer further contains an ethylenically unsaturated amide monomer unit, the cycle characteristics of the resulting secondary battery can be improved.
[0013] [5] In the binder composition for a non-aqueous secondary battery negative electrode according to the above item [4], the content of the ethylenically unsaturated amide monomer unit is preferably 3.5% by mass or more, based on the total mass of all repeating units of the polymer being 100% by mass. When the content of the ethylenically unsaturated amide monomer unit is equal to or more than the lower limit, the cycle characteristics of the resulting secondary battery can be further improved.
[0014] Another object of the present invention is to advantageously solve the above-mentioned problems, and [6] the present invention provides a slurry composition for a non-aqueous secondary battery negative electrode, comprising a negative electrode active material and the binder composition for a non-aqueous secondary battery negative electrode according to any one of [1] to [5] above. The above-mentioned slurry composition for a non-aqueous secondary battery negative electrode effectively suppresses swelling of the negative electrode due to repeated charge and discharge, and enables the secondary battery to exhibit excellent cycle characteristics.
[0015] [7] In the slurry composition for a non-aqueous secondary battery negative electrode according to [6] above, the negative electrode active material preferably contains a silicon-based negative electrode active material. When the negative electrode active material contains a silicon-based negative electrode active material, the capacity of the resulting secondary battery can be improved. Furthermore, since silicon-based negative electrode active materials undergo particularly large expansion and contraction during charge and discharge, the use of a slurry composition for a non-aqueous secondary battery negative electrode containing the binder composition for a non-aqueous secondary battery negative electrode of the present invention effectively prevents the disconnection of the conductive paths in the negative electrode mixture layer due to the large expansion and contraction during charge and discharge, thereby effectively preventing a decrease in the cycle characteristics of the secondary battery.
[0016] Another object of the present invention is to advantageously solve the above-mentioned problems, and [8] the present invention provides a negative electrode for a non-aqueous secondary battery, comprising a current collector and a negative electrode composite layer located on the current collector, wherein the negative electrode composite layer is a layer formed from the slurry composition for a non-aqueous secondary battery negative electrode according to [6] or [7] above. Such a non-aqueous secondary battery negative electrode is less likely to swell even with repeated charge and discharge, and can enable the secondary battery to exhibit excellent cycle characteristics.
[0017] Another object of the present invention is to advantageously solve the above-mentioned problems, and [9] the present invention is a nonaqueous secondary battery comprising a positive electrode, a negative electrode, a separator, and an electrolyte solution, wherein the negative electrode is the nonaqueous secondary battery negative electrode of [8]. Such a nonaqueous secondary battery is less likely to swell in the negative electrode due to charge and discharge, and has excellent cycle characteristics.
[0018] Therefore, according to the present invention, a binder composition for a non-aqueous secondary battery negative electrode can be provided that effectively suppresses swelling of the negative electrode due to repeated charge and discharge and allows the secondary battery to exhibit excellent cycle characteristics. Furthermore, according to the present invention, a slurry composition for a non-aqueous secondary battery negative electrode can be provided that effectively suppresses swelling of the negative electrode due to repeated charge and discharge and allows the secondary battery to exhibit excellent cycle characteristics. Furthermore, according to the present invention, a non-aqueous secondary battery negative electrode that is less likely to swell even with repeated charge and discharge and allows the secondary battery to exhibit excellent cycle characteristics can be provided. Furthermore, according to the present invention, a non-aqueous secondary battery that is less likely to swell of the negative electrode due to charge and discharge and has excellent cycle characteristics can be provided.
[0019] 1 is a schematic diagram showing a possible structure of a particulate binder used in a binder composition of the present invention. FIG.
[0020] Hereinafter, embodiments of the present invention will be described in detail. Hereinafter, the binder composition for a non-aqueous secondary battery negative electrode of the present invention (hereinafter sometimes simply abbreviated as "binder composition") can be used to prepare a slurry composition for a non-aqueous secondary battery negative electrode (hereinafter sometimes simply abbreviated as "slurry composition"). Furthermore, the slurry composition for a non-aqueous secondary battery negative electrode of the present invention can be used when producing a negative electrode for a non-aqueous secondary battery such as a lithium ion secondary battery (hereinafter sometimes simply abbreviated as "negative electrode"). Furthermore, the non-aqueous secondary battery negative electrode of the present invention can be used in a non-aqueous secondary battery.
[0021] (Binder Composition for Non-Aqueous Secondary Battery Negative Electrode) The binder composition for non-aqueous secondary battery negative electrode of the present invention contains a particulate binder and water, and may optionally further contain other components in addition to the particulate binder and water.
[0022] <Particulate Binder> The particulate binder serves to hold components such as the negative electrode active material so that they do not detach from the negative electrode mixture layer formed using a slurry composition containing a binder composition.
[0023] Here, the particulate binder contained in the binder composition of the present invention includes a polymer containing ethylenically unsaturated carboxylic acid monomer units, aromatic vinyl monomer units, and aliphatic conjugated diene monomer units, and the content of the ethylenically unsaturated carboxylic acid monomer units is 5.0 mass% or more and 15.0 mass% or less when the total repeating units of the polymer are taken as 100 mass%. Further, the particulate binder has an average particle diameter Da (hereinafter sometimes simply referred to as "average particle diameter Da") when a binder composition adjusted to have a solid content of 0.5% by mass is measured by a dynamic light scattering method, an average particle diameter Db (hereinafter sometimes simply referred to as "average particle diameter Db") when a binder composition adjusted to have a solid content of 0.005% by mass is measured by a dynamic light scattering method, and an average particle diameter Dc (hereinafter sometimes simply referred to as "average particle diameter Dc") when the binder composition is measured by a laser diffraction scattering method. These satisfy the following formulas (1) and (2): Da - Db ≦ 60.0 nm (1) 1.40 ≦ Da / Dc ≦ 2.00 (2) The use of the above-mentioned particulate binder in the binder composition effectively suppresses swelling of the negative electrode due to repeated charge and discharge, and allows the secondary battery to exhibit excellent cycle characteristics. The reasons for these are presumed to be as follows.
[0024] It is presumed that a particulate binder in which the above-mentioned average particle diameters satisfy a predetermined relationship can have a structure capable of forming a good network. While not particularly limited, a specific explanation will be given using FIG. 1 as an example. A particulate binder 10 in which the above-mentioned average particle diameters satisfy a predetermined relationship can include a main body portion 11 and a string-like portion 12 covering the main body portion 11. The fact that the average particle diameters Da and Db satisfy the relationship of formula (1) means that the string-like portions 12 of the particulate binder 10 are firmly bonded to the main body portion 11, and the fact that the average particle diameters Da and Dc satisfy the relationship of formula (2) means that the string-like portions 12 of the particulate binder 10 are well spread. Therefore, such a particulate binder 10 can form a good network in the negative electrode composite layer by the string-like portions 12 of the particulate binders 10. Furthermore, it is believed that the polymer contained in the particulate binder 10 has a predetermined composition, particularly a predetermined proportion of ethylenically unsaturated carboxylic acid monomer units, which strengthens the network in the negative electrode mixture layer. As a result, swelling of the negative electrode due to repeated charge and discharge is effectively suppressed, and the secondary battery exhibits excellent cycle characteristics. While using a silicon-based negative electrode active material as the negative electrode active material increases the capacity of the resulting secondary battery, the silicon-based negative electrode active material typically exhibits poor cycle characteristics due to its particularly large expansion and contraction during charge and discharge. However, as described above, the use of the binder composition of the present invention strengthens the network in the negative electrode mixture layer, effectively suppressing disconnection of the conductive paths in the negative electrode mixture layer due to large expansion and contraction during charge and discharge, thereby effectively suppressing deterioration in the cycle characteristics of the resulting secondary battery. Therefore, the binder composition of the present invention is particularly suitable for use in preparing a slurry composition using a silicon-based negative electrode active material.
[0025] <<Properties of Particulate Binder>> The particulate binder must have a difference (Da - Db) between the average particle diameter Da and the average particle diameter Db of 60.0 nm or less, preferably 50.0 nm or less, and more preferably 40.0 nm or less. If the difference (Da - Db) between the average particle diameter Da and the average particle diameter Db is equal to or less than the upper limit, the network in the negative electrode mixture layer becomes stronger, and swelling of the negative electrode can be effectively suppressed. Furthermore, the cycle life of the resulting secondary battery can be improved. On the other hand, the difference (Da - Db) between the average particle diameter Da and the average particle diameter Db is, for example, 5.0 nm or more, or may be 10.0 nm or more, or may be 20.0 nm or more.
[0026] The particulate binder must have a ratio (Da / Dc) of the average particle diameter Da to the average particle diameter Dc of 1.40 or more, preferably 1.50 or more, more preferably 1.55 or more, even more preferably 1.60 or more, even more preferably 1.70 or more, and must be 2.00 or less, preferably 1.90 or less, and more preferably 1.80 or less. If the ratio (Da / Dc) of the average particle diameter Da to the average particle diameter Dc is within the above range, the network in the negative electrode mixture layer becomes stronger, and swelling of the negative electrode can be effectively suppressed. Furthermore, the cycle life of the resulting secondary battery can be improved.
[0027] The average particle diameter Da is not particularly limited as long as the values of "Da-Db" and "Da / Dc" are within a predetermined range, but is preferably 180 nm or more, more preferably 200 nm or more, even more preferably 220 nm or more, even more preferably 240 nm or more, and preferably 340 nm or less, more preferably 300 nm or less, and even more preferably 260 nm or less. If the average particle diameter Da is equal to or greater than the above lower limit, the strength of the resulting negative electrode can be further improved. On the other hand, if the average particle diameter Da is equal to or less than the above upper limit, the viscosity of the binder composition can be effectively prevented from increasing excessively, thereby maintaining good viscosity of the binder composition.
[0028] The average particle diameter Db is preferably 130 nm or more, more preferably 150 nm or more, even more preferably 180 nm or more, even more preferably 200 nm or more, and preferably 300 nm or less, more preferably 280 nm or less, and even more preferably 250 nm or less. If the average particle diameter Db is equal to or greater than the lower limit, the network in the negative electrode mixture layer becomes stronger. On the other hand, if the average particle diameter Db is equal to or less than the upper limit, an excessive increase in the viscosity of the binder composition can be effectively suppressed, thereby maintaining good viscosity of the binder composition.
[0029] Here, when the particulate binder has a structure such as that shown in Fig. 1, the average particle diameter Da and the average particle diameter Db depend on the particle diameter of the entire particulate binder, and are presumed to be particularly significantly affected by the string-like portions 12 that cover the main body portion 11 of the particulate binder 10. Therefore, the values of the average particle diameter Da and the average particle diameter Db can be adjusted, for example, by the type and amount of the monomer used to form the particulate binder (particularly the type and amount of the monomer that can form the string-like portions 12), the amount of the molecular weight adjuster, and the polymerization conditions.
[0030] The average particle diameter Dc is not particularly limited as long as the value of "Da / Dc" is within a predetermined range, but is preferably 30 nm or more, more preferably 50 nm or more, even more preferably 100 nm or more, even more preferably 130 nm or more, preferably 250 nm or less, more preferably 200 nm or less, and even more preferably 150 nm or less. If the average particle diameter Dc is equal to or greater than the above lower limit, the strength of the resulting negative electrode can be further improved. On the other hand, if the average particle diameter Dc is equal to or greater than the above lower limit, the dispersibility of the particulate binder in the binder composition can be improved. The value of the average particle diameter Dc can be adjusted, for example, by the type and amount of monomer used to form the particulate binder, the polymerization conditions, etc.
[0031] The particulate binder preferably has an insoluble content in tetrahydrofuran (THF) of more than 90% by mass, more preferably 95% by mass or more, and even more preferably 97% by mass or more, and preferably less than 100% by mass, and more preferably 99% by mass or less. If the insoluble content in tetrahydrofuran of the particulate binder is within the above range, the battery characteristics of the resulting secondary battery can be improved.
[0032] The particulate binder preferably has an electrolyte swelling degree of 110% by mass or more, more preferably 120% by mass or more, and preferably 150% by mass or less, and more preferably 140% by mass or less. If the insoluble content in tetrahydrofuran of the particulate binder is within the above range, the battery characteristics of the obtained secondary battery can be improved. In this specification, the "electrolyte swelling degree" of the particulate binder can be measured according to the method described in the Examples.
[0033] The particulate binder preferably has a tensile strength of 1.5 MPa or more, more preferably 2.0 MPa or more, even more preferably 3.0 MPa or more, and even more preferably 3.8 MPa or more, in a repeated tensile test measured according to the method described in the Examples. The tensile strength in the repeated tensile test is, for example, 20.0 MPa or less, or may be 15.0 MPa or less, or may be 10.0 MPa or less.
[0034] <<Composition of polymer contained in particulate binder>> The polymer contained in the particulate binder (hereinafter may be simply referred to as "polymer") contains ethylenically unsaturated carboxylic acid monomer units, aromatic vinyl monomer units, and aliphatic conjugated diene monomer units, and may optionally contain ethylenically unsaturated amide monomer units and other monomer units.
[0035] [Ethylenically unsaturated carboxylic acid monomer unit] An ethylenically unsaturated carboxylic acid monomer capable of forming an ethylenically unsaturated carboxylic acid monomer unit usually does not have any hydroxyl groups (—OH) other than the hydroxyl group in the carboxyl group. Examples of the ethylenically unsaturated carboxylic acid monomer include ethylenically unsaturated monocarboxylic acids and derivatives thereof, ethylenically unsaturated dicarboxylic acids and acid anhydrides thereof, and derivatives thereof. The ethylenically unsaturated carboxylic acid monomer may be used alone or in combination of two or more types in any ratio.
[0036] Examples of ethylenically unsaturated monocarboxylic acids include acrylic acid, methacrylic acid, and crotonic acid. Examples of derivatives of ethylenically unsaturated monocarboxylic acids include 2-ethylacrylic acid, isocrotonic acid, α-acetoxyacrylic acid, β-trans-aryloxyacrylic acid, α-chloro-β-E-methoxyacrylic acid, and β-diaminoacrylic acid. Examples of ethylenically unsaturated dicarboxylic acids include maleic acid, fumaric acid, and itaconic acid. Examples of acid anhydrides of ethylenically unsaturated dicarboxylic acids include maleic anhydride, diacrylic anhydride, methylmaleic anhydride, and dimethylmaleic anhydride. Examples of derivatives of ethylenically unsaturated dicarboxylic acids include methylmaleic acid, phenylmaleic acid, chloromaleic acid, dichloromaleic acid, and fluoromaleic acid.
[0037] The ethylenically unsaturated carboxylic acid monomer is preferably a monofunctional ethylenically unsaturated carboxylic acid monomer having one ethylenically unsaturated bond (C=C) in the molecule. Furthermore, from the viewpoint of polymerizability, the ethylenically unsaturated carboxylic acid monomer is preferably an ethylenically unsaturated monocarboxylic acid or an ethylenically unsaturated dicarboxylic acid, more preferably acrylic acid, methacrylic acid, or itaconic acid, and even more preferably acrylic acid or methacrylic acid. That is, the polymer preferably contains at least one monomer unit selected from the group consisting of an ethylenically unsaturated monocarboxylic acid unit and an ethylenically unsaturated dicarboxylic acid unit, more preferably at least one monomer unit selected from the group consisting of an acrylic acid unit, a methacrylic acid unit, and an itaconic acid unit, and even more preferably at least one of an acrylic acid unit and a methacrylic acid unit. Furthermore, it is particularly preferable that the polymer contains both an acrylic acid unit and a methacrylic acid unit.
[0038] The content of the ethylenically unsaturated carboxylic acid monomer units in the polymer must be 5.0% by mass or more, preferably 10.0% by mass or more, more preferably 13.0% by mass or more, and must be 15.0% by mass or less, preferably 14.5% by mass or less, when the total repeating units (total monomer units) in the polymer is 100% by mass. If the content of the ethylenically unsaturated carboxylic acid monomer units in the polymer is equal to or greater than the above-mentioned lower limit, swelling of the resulting negative electrode can be effectively suppressed. Furthermore, the cycle characteristics of the resulting secondary battery can be improved. On the other hand, if the content of the ethylenically unsaturated carboxylic acid monomer units in the polymer is equal to or less than the above-mentioned upper limit, the strength retention rate of the particulate binder under repeated tension can be improved. As a result, even if the negative electrode mixture layer repeatedly expands and contracts due to charge and discharge of the secondary battery, the particulate binder can be effectively prevented from breaking or collapsing.
[0039] [Aromatic vinyl monomer unit] Examples of aromatic vinyl monomers that can form aromatic vinyl monomer units include aromatic monovinyl compounds such as styrene, styrene sulfonic acid and its salts, α-methylstyrene, p-t-butylstyrene, butoxystyrene, vinyltoluene, chlorostyrene, and vinylnaphthalene. Among these, styrene and its derivatives are preferred. These can be used alone or in combination of two or more, but it is preferable to use one type alone.
[0040] The content of the aromatic vinyl monomer units in the polymer is preferably 10.0% by mass or more, more preferably 20.0% by mass or more, and even more preferably 30.0% by mass or more, and preferably 60.0% by mass or less, more preferably 40.0% by mass or less, and even more preferably 34.0% by mass or less, when the total repeating units in the polymer is 100% by mass. If the content of the aromatic vinyl monomer units is equal to or greater than the lower limit, the cycle characteristics of the resulting secondary battery can be improved. On the other hand, if the content of the aromatic vinyl monomer units is equal to or less than the upper limit, the flexibility of the resulting negative electrode can be improved.
[0041] [Aliphatic Conjugated Diene Monomer Unit] Examples of aliphatic conjugated diene monomers capable of forming aliphatic conjugated diene monomer units include aliphatic conjugated diene compounds having 4 or more carbon atoms, such as 1,3-butadiene, isoprene, 2,3-dimethyl-1,3-butadiene, and 1,3-pentadiene. Among these, 1,3-butadiene and isoprene are preferred, and 1,3-butadiene is more preferred. These can be used alone or in combination of two or more, but it is preferable to use one type alone. By using 1,3-butadiene to form aliphatic conjugated diene monomer units of a polymer, the dispersion stability and thermal stability of the resulting polymer can be improved.
[0042] The content of the aliphatic conjugated diene monomer units in the polymer is preferably 30.0% by mass or more, more preferably 40.0% by mass or more, and even more preferably 45.0% by mass or more, and is preferably 70.0% by mass or less, more preferably 60.0% by mass or less, even more preferably 50.0% by mass or less, and even more preferably 48.0% by mass or less, based on 100% by mass of all repeating units in the polymer. If the content of the aliphatic conjugated diene monomer units is equal to or greater than the lower limit, a negative electrode with superior flexibility can be obtained. On the other hand, if the content of the aliphatic conjugated diene monomer units is equal to or less than the upper limit, the cycle life of the resulting secondary battery can be improved.
[0043] [Ethylenically Unsaturated Amide Monomer Unit] It is preferable that the polymer further contains an ethylenically unsaturated amide monomer unit, since this can improve the cycle characteristics of the resulting secondary battery.
[0044] Examples of the ethylenically unsaturated amide monomer that can form the ethylenically unsaturated amide monomer unit include those obtained by amidating the above-mentioned ethylenically unsaturated carboxylic acid monomer (ethylenically unsaturated amide monomer). For example, examples of those obtained by amidating an ethylenically unsaturated monocarboxylic acid (ethylenically unsaturated monoamide monomer) include acrylamide, methacrylamide, crotonamide, etc. Among these, acrylamide and methacrylamide are preferred, and acrylamide is particularly preferred.
[0045] The content of the ethylenically unsaturated amide monomer units in the polymer is preferably 1.0% by mass or more, more preferably 3.0% by mass or more, even more preferably 3.5% by mass or more, even more preferably 4.0% by mass or more, and preferably 15.0% by mass or less, more preferably 10.0% by mass or less, and even more preferably 5.0% by mass or less, based on 100% by mass of all repeating units in the polymer. If the content of the ethylenically unsaturated amide monomer units is equal to or greater than the lower limit, the cycle characteristics of the resulting secondary battery can be further improved. On the other hand, if the content of the ethylenically unsaturated amide monomer units is equal to or less than the upper limit, the flexibility of the resulting negative electrode can be improved.
[0046] [Other Monomer Units] Monomers that can form other monomer units are not particularly limited, and examples thereof include nitrile group-containing monomers such as acrylonitrile and methacrylonitrile; and ethylenically unsaturated carboxylic acid ester monomers obtained by esterifying the above-mentioned ethylenically unsaturated carboxylic acid monomers. Here, the above-mentioned ethylenically unsaturated carboxylic acid ester monomers also include ethylenically unsaturated carboxylic acid ester monomers containing a hydroxyalkyl group, such as hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, and hydroxybutyl (meth)acrylate. In this specification, "(meth)acrylate" means acrylate and / or methacrylate.
[0047] The content of other monomer units in the polymer is preferably 10.0% by mass or less, more preferably 5.0% by mass or less, even more preferably 1.0% by mass or less, and particularly preferably 0% by mass or less, when all repeating units in the polymer are taken as 100% by mass. That is, it is particularly preferable that the polymer does not contain other monomer units.
[0048] [Method for preparing polymer contained in particulate binder] The polymer contained in the particulate binder can be polymerized according to a known polymerization method such as solution polymerization, suspension polymerization, bulk polymerization, emulsion polymerization, etc. Among these, emulsion polymerization is preferred because it is easy to adjust the average particle size of each particulate binder. As the polymerization reaction, addition polymerization such as ionic polymerization, radical polymerization, and living radical polymerization can be used.
[0049] During the polymerization reaction, it is preferable that the polymerization system contains a molecular weight modifier (chain transfer agent) because this allows the properties of the particulate binder to be appropriately adjusted. Examples of molecular weight modifiers include alkyl mercaptans such as n-hexyl mercaptan, n-octyl mercaptan, t-octyl mercaptan, n-dodecyl mercaptan, t-dodecyl mercaptan, and n-stearyl mercaptan; xanthogen compounds such as dimethyl xanthogen disulfide and diisopropyl xanthogen disulfide; terpinolene; thiuram compounds such as tetramethylthiuram disulfide, tetraethylthiuram disulfide, and tetramethylthiuram monosulfide; phenolic compounds such as 2,6-di-t-butyl-4-methylphenol and styrenated phenol; allyl compounds such as allyl alcohol; halogenated hydrocarbon compounds such as dichloromethane, dibromomethane, and carbon tetrabromide; thio compounds such as thioglycolic acid, thiomalic acid, and 2-ethylhexyl thioglycolate; diphenylethylene; and α-methylstyrene dimer. Among these, t-dodecyl mercaptan is preferred. The molecular weight modifiers described above may be used singly or in combination of two or more kinds in any ratio.
[0050] The amount of the molecular weight modifier used is preferably 0.05 parts by mass or more, more preferably 0.10 parts by mass or more, and even more preferably 0.15 parts by mass or more, relative to 100 parts by mass of the total amount of the monomers used, and is preferably 2.00 parts by mass or less, more preferably 1.00 parts by mass or less, even more preferably 0.50 parts by mass or less, and even more preferably 0.30 parts by mass or less. If the amount of the molecular weight modifier used is within the above range, the properties and the like of the particulate binder can be appropriately adjusted.
[0051] In the polymerization reaction, in addition to the molecular weight modifier, commonly used additives such as an emulsifier, a dispersant, a polymerization initiator, a polymerization aid, etc. The amounts of these additives used may be the amounts commonly used.
[0052] The maximum temperature during the polymerization reaction is preferably above 80° C., more preferably at least 85° C., and is preferably below 100° C., more preferably at most 95° C. If the maximum temperature is within the above range, the properties of the particulate binder can be appropriately adjusted.
[0053] In the polymerization reaction, the duration of the temperature exceeding 80°C is preferably 1 hour or more, more preferably 2 hours or more, and even more preferably 3 hours or more, and is preferably 7 hours or less, more preferably 6 hours or less, and even more preferably 5 hours or less. If the duration of the temperature is within the above range, the properties of the particulate binder can be appropriately adjusted.
[0054] <<Content of Particulate Binder>> The content of the particulate binder in the binder composition (including the solvent described below) used to prepare the slurry composition is preferably 20% by mass or more, more preferably 30% by mass or more, and is preferably 60% by mass or less, more preferably 50% by mass or less.
[0055] <Solvent> The binder composition of the present invention must contain water as a solvent, but may contain a small amount of organic solvent other than water, as long as the object of the present invention is not impaired.
[0056] <Other Components> The binder composition of the present invention may contain other components as long as the object of the present invention is not impaired. Examples of other components include antioxidants, antifoaming agents, dispersants, etc. One type of other component may be used alone, or two or more types may be used in combination at any ratio.
[0057] <Method for preparing binder composition for non-aqueous secondary battery negative electrode> The binder composition of the present invention is not particularly limited, and can be prepared by mixing a particulate binder and other components that can be used optionally in the presence of water. When the binder composition is prepared using a dispersion of a particulate binder, the liquid contained in the dispersion may be used as a solvent for the binder composition as it is.
[0058] (Slurry Composition for Non-Aqueous Secondary Battery Negative Electrode) The slurry composition for non-aqueous secondary battery negative electrode of the present invention is a composition used for forming a negative electrode composite layer of a negative electrode, and contains the above-mentioned binder composition for non-aqueous secondary battery negative electrode and a negative electrode active material. That is, the slurry composition of the present invention contains at least a particulate binder, a negative electrode active material, and water. Furthermore, since the slurry composition of the present invention contains the binder composition of the present invention, it is possible to effectively suppress swelling of the negative electrode due to repeated charge and discharge, and to enable the secondary battery to exhibit excellent cycle characteristics. Note that the slurry composition of the present invention may further contain other components in addition to the particulate binder, the negative electrode active material, and water.
[0059] <Binder Composition> The binder composition of the present invention containing a predetermined particulate binder and water is used as the binder composition. Here, the content of the particulate binder in the slurry composition is preferably 0.5 parts by mass or more, more preferably 1.0 part by mass or more, and preferably 5.0 parts by mass or less, and more preferably 3.0 parts by mass or less, relative to 100 parts by mass of the negative electrode active material.
[0060] <Negative electrode active material> The negative electrode active material is not particularly limited, and known negative electrode active materials used in secondary batteries can be used. For example, negative electrode active materials that can be used in the negative electrode composite layer of a lithium ion secondary battery, which is an example of a secondary battery, are not particularly limited, and include carbon-based negative electrode active materials, metal-based negative electrode active materials, and negative electrode active materials that are combinations of these.
[0061] Carbon-based negative electrode active materials refer to active materials with a carbon backbone that can insert (also referred to as "doping") lithium. Specific examples of carbon-based negative electrode active materials include carbonaceous materials such as coke, mesocarbon microbeads (MCMB), mesophase pitch-based carbon fibers, pyrolytic vapor-grown carbon fibers, phenolic resin baked bodies, polyacrylonitrile-based carbon fibers, pseudoisotropic carbon, furfuryl alcohol resin baked bodies (PFA), and hard carbon, as well as graphitic materials such as natural graphite and artificial graphite. Metal-based negative electrode active materials refer to active materials that contain metals, and typically contain an element capable of inserting lithium in their structure, and have a theoretical electrical capacity per unit mass of 500 mAh / g or more when lithium is inserted. Examples of metal-based negative electrode active materials include lithium metal, elemental metals capable of forming lithium alloys (e.g., Ag, Al, Ba, Bi, Cu, Ga, Ge, In, Ni, P, Pb, Sb, Si, Sn, Sr, Zn, Ti, etc.), and oxides, sulfides, nitrides, silicides, carbides, phosphides, etc. of these. Further examples include oxides such as lithium titanate. Note that the above-mentioned negative electrode active materials may be used alone or in combination of two or more.
[0062] From the viewpoint of improving the capacity of the secondary battery, the negative electrode active material preferably contains at least a metal-based negative electrode active material, and particularly preferably contains a silicon-containing negative electrode active material (silicon-based negative electrode active material). Here, since silicon-based negative electrode active materials undergo particularly large expansion and contraction during charge and discharge, use of a slurry composition containing the binder composition of the present invention effectively suppresses disconnection of the conductive paths in the negative electrode mixture layer due to the large expansion and contraction during charge and discharge, and as a result, can effectively suppress deterioration of the cycle characteristics of the secondary battery.
[0063] When the negative electrode active material contains a silicon-based negative electrode active material, the proportion of the silicon-based negative electrode active material per 100 parts by mass of the negative electrode active material is preferably 1.0 part by mass or more, more preferably 3.0 parts by mass or more, and even more preferably 5.0 parts by mass or more, and is preferably 20.0 parts by mass or less, more preferably 15.0 parts by mass or less, and even more preferably 10.0 parts by mass or less.
[0064] <Other Components> Other components that can be incorporated into the slurry composition are not particularly limited, and include thickeners, conductive materials, and the same components as those that can be incorporated into the binder composition of the present invention. Examples of thickeners include carboxymethyl cellulose and lithium salts of acrylic acid / acrylamide / hydroxyethylacrylamide copolymers. Note that, one type of other component may be used alone, or two or more types may be used in combination at any ratio.
[0065] <Preparation of Slurry Composition for Non-Aqueous Secondary Battery Negative Electrode> The method for preparing the slurry composition is not particularly limited. For example, the binder composition, the negative electrode active material, and other components used as needed can be mixed in the presence of water to prepare the slurry composition. The solvent used in preparing the slurry composition also includes the solvent contained in the binder composition. The mixing method is not particularly limited, and mixing can be performed using a commonly used stirrer, disperser, or the like.
[0066] (Negative electrode for non-aqueous secondary battery) The negative electrode for a non-aqueous secondary battery of the present invention comprises a current collector and a negative electrode mixture layer located on the current collector, the negative electrode mixture layer being a layer formed using the above-mentioned slurry composition for a non-aqueous secondary battery negative electrode. Since the negative electrode of the present invention has a negative electrode mixture layer formed using the slurry composition of the present invention, it is less likely to swell even with repeated charge and discharge, and the secondary battery can exhibit excellent cycle characteristics.
[0067] <Negative electrode mixture layer> The negative electrode mixture layer is made of a dried product of the slurry composition of the present invention, and typically contains a negative electrode active material and a component derived from a particulate binder, and may optionally further contain other components. Note that the components contained in the negative electrode mixture layer are those contained in the slurry composition of the present invention, and the preferred abundance ratio of each component is the same as the preferred abundance ratio of each component in the slurry composition. Furthermore, the particulate binder is present in particulate form in the binder composition and the slurry composition, but may be in particulate form or any other shape in the negative electrode mixture layer formed using the slurry composition.
[0068] <Current Collector> A material that is electrically conductive and electrochemically durable is used as the current collector of the negative electrode. Specifically, the current collector may be made of, for example, iron, copper, aluminum, nickel, stainless steel, titanium, tantalum, gold, platinum, or the like. Copper foil is particularly preferred as the current collector of the negative electrode. Note that these materials may be used alone or in combination of two or more in any ratio.
[0069] <Method for Manufacturing Negative Electrode> Here, the negative electrode composite layer of the negative electrode of the present invention can be formed using, for example, the following methods. 1) A method in which the slurry composition of the present invention is applied to the surface of a current collector and then dried; 2) A method in which the current collector is immersed in the slurry composition of the present invention and then dried; and 3) A method in which the slurry composition of the present invention is applied to a release substrate and dried to produce a negative electrode composite layer, and the obtained negative electrode composite layer is transferred to the surface of the current collector. Among these, method 1) is particularly preferred because it makes it easy to control the layer thickness of the negative electrode composite layer. Method 1) specifically includes a step of applying the slurry composition to the current collector (application step) and a step of drying the slurry composition applied to the current collector to form a negative electrode composite layer on the current collector (drying step).
[0070] <<Coating Step>> The method for applying the slurry composition onto the current collector is not particularly limited, and known methods can be used. Specifically, examples of the application method include a doctor blade method, a dipping method, a reverse roll method, a direct roll method, a gravure method, an extrusion method, and a brush coating method. In this case, the slurry composition may be applied to only one side or both sides of the current collector. The thickness of the slurry film on the current collector after application and before drying can be appropriately set depending on the thickness of the negative electrode composite layer obtained by drying.
[0071] <<Drying Step>> The method for drying the slurry composition on the current collector is not particularly limited and any known method can be used, for example, a drying method using warm air, hot air, or low-humidity air, a vacuum drying method, or a drying method using irradiation with infrared rays, electron beams, etc. By drying the slurry composition on the current collector in this manner, a negative electrode composite layer is formed on the current collector, and a negative electrode including the current collector and the negative electrode composite layer located on the current collector can be obtained.
[0072] After the drying step, the negative electrode mixture layer may be subjected to a pressure treatment using a mold press, a roll press, or the like. The pressure treatment improves the adhesion between the negative electrode mixture layer and the current collector and further increases the density of the resulting negative electrode mixture layer. In addition, when the negative electrode mixture layer contains a curable polymer, it is preferable to cure the polymer after the formation of the negative electrode mixture layer.
[0073] (Nonaqueous secondary battery) The nonaqueous secondary battery of the present invention comprises a positive electrode, a negative electrode, an electrolyte, and a separator, the negative electrode being the above-described negative electrode for a nonaqueous secondary battery. Because the secondary battery of the present invention comprises the negative electrode of the present invention, swelling of the negative electrode due to charge and discharge is unlikely to occur, and the secondary battery has excellent cycle characteristics. Note that, as an example, the following description will be given of a case where the secondary battery is a lithium ion secondary battery, but the present invention is not limited to the following example. As the negative electrode has been described above, a description thereof will be omitted below.
[0074] <Positive Electrode> The positive electrode included in the secondary battery of the present invention is not particularly limited, and a known positive electrode used in secondary batteries can be used. Specifically, the positive electrode can be a positive electrode obtained by forming a positive electrode mixture layer on a current collector using a known manufacturing method.
[0075] The positive electrode active material to be blended into the positive electrode composite layer is not particularly limited, and known positive electrode active materials used in secondary batteries can be used. Examples of the positive electrode active material to be blended into the positive electrode composite layer include compounds containing transition metals, such as transition metal oxides, transition metal sulfides, and composite metal oxides of lithium and transition metals. Examples of transition metals include Ti, V, Cr, Mn, Fe, Co, Ni, Cu, and Mo. Specifically, the positive electrode active material is not particularly limited, and examples thereof include lithium-containing cobalt oxide (LiCoO 2 ), lithium manganese oxide (LiMn 2 O 4 ), lithium-containing nickel oxide (LiNiO 2 ), LiNi 5 / 10 Co 2 / 10 Mn 3 / 10 Lithium-containing composite oxides of Co-Ni-Mn, such as O2 (NMC532), lithium-containing composite oxides of Ni-Mn-Al, lithium-containing composite oxides of Ni-Co-Al, olivine-type lithium iron phosphate (LiFePO 4 ), olivine-type lithium manganese phosphate (LiMnPO 4 ), Li 1+x Mn 2-x O 4 (0<X<2) Lithium-excess spinel compound represented by Li[Ni 0.17 Li 0.2 Co 0.07 Mn 0.56 ]O 2 , LiNi 0.5 Mn 1.5 O 4 The above-mentioned positive electrode active materials may be used singly or in combination of two or more.
[0076] The positive electrode current collector may be made of the material described for the negative electrode current collector. Aluminum foil is particularly preferred as the positive electrode current collector. The material used for the positive electrode current collector may be one type alone or two or more types in any combination.
[0077] <Electrolyte> As the electrolyte, an organic electrolyte solution in which a supporting electrolyte is dissolved in an organic solvent is usually used. As the supporting electrolyte of a lithium ion secondary battery, for example, a lithium salt is used. As the lithium salt, for example, LiPF 6 , LiAsF 6 , LiBF 4 , LiSbF 6 , LiAlCl 4 , LiClO 4 , C.F. 3 SO 3 Li, C 4 F 9 SO 3 Li, CF 3 COOLi, (CF 3 CO) 2 NLi, (CF 3 SO 2 ) 2 NLi, (C 2 F 5 SO 2 Among them, LiPF is preferred because it is easily soluble in solvents and shows a high degree of dissociation. 6 , LiClO 4 , C.F. 3 SO 3 Li is preferred. Note that one type of electrolyte may be used alone, or two or more types may be used in combination at any ratio. Generally, the use of a supporting electrolyte with a higher degree of dissociation tends to result in higher lithium ion conductivity, so the lithium ion conductivity can be adjusted by the type of supporting electrolyte.
[0078] The organic solvent used in the electrolyte is not particularly limited as long as it can dissolve the supporting electrolyte. Suitable examples include carbonates such as dimethyl carbonate (DMC), ethylene carbonate (EC), diethyl carbonate (DEC), propylene carbonate (PC), butylene carbonate (BC), ethyl methyl carbonate (EMC), and vinylene carbonate (VC); esters such as γ-butyrolactone and methyl formate; ethers such as 1,2-dimethoxyethane and tetrahydrofuran; and sulfur-containing compounds such as sulfolane and dimethyl sulfoxide. Mixtures of these solvents may also be used. Among these, carbonates are preferred due to their high dielectric constant and wide stable potential range. Generally, the lower the viscosity of the solvent used, the higher the lithium ion conductivity, so the lithium ion conductivity can be adjusted by the type of solvent. The concentration of the electrolyte in the electrolyte can be adjusted as appropriate. Known additives can also be added to the electrolyte.
[0079] <Separator> The separator is not particularly limited, and for example, those described in JP 2012-204303 A can be used. Among these, a microporous film made of a polyolefin resin (polyethylene, polypropylene, polybutene, polyvinyl chloride) is preferred because it allows the thickness of the entire separator to be thin, thereby increasing the proportion of electrode active material in the secondary battery and increasing the capacity per volume.
[0080] <Method for Manufacturing Secondary Battery> The secondary battery of the present invention can be manufactured, for example, by stacking a positive electrode and a negative electrode with a separator interposed therebetween, rolling or folding the resulting assembly as needed according to the battery shape, placing it in a battery container, injecting an electrolyte into the battery container, and sealing it. The secondary battery of the present invention uses the negative electrode of the present invention. The secondary battery of the present invention may be provided with an overcurrent protection element such as a fuse or a PTC element, an expanded metal, a lead plate, or the like, as needed, to prevent internal pressure buildup, overcharging and overdischarging, and the like. The shape of the secondary battery may be, for example, a coin type, a button type, a sheet type, a cylindrical type, a rectangular type, a flat type, or the like.
[0081] The present invention will be described in detail below based on examples, but the present invention is not limited to these examples. In the following description, "%" and "parts" representing amounts are based on mass unless otherwise specified. Furthermore, in a polymer produced by copolymerizing multiple types of monomers, the proportion of a repeating unit (monomer unit) formed by polymerizing a certain monomer in the polymer usually coincides with the ratio (feed ratio) of the certain monomer to all monomers used in the polymerization of the polymer, unless otherwise specified.
[0082] In the examples and comparative examples, the average particle diameter Da of the particulate binder measured by dynamic light scattering (solid content concentration 0.5 mass %), the average particle diameter Db of the particulate binder measured by dynamic light scattering (solid content concentration 0.005 mass %), the average particle diameter Dc of the particulate binder measured by laser diffraction scattering, the THF-insoluble content, the degree of electrolyte swelling, the repeated tensile test, the tensile strength in the repeated tensile test, the electrode swelling, and the cycle characteristics were measured and evaluated as follows.
[0083] <Average particle diameter Da of particulate binder measured by dynamic light scattering (solid content concentration 0.5% by mass)> First, ion-exchanged water was added to the binder composition (aqueous dispersion of particulate binder) obtained in the examples and comparative examples to adjust the solid content concentration to 0.5% by mass. Next, using a particle size distribution measuring device (manufactured by Otsuka Electronics Co., Ltd., model "FPAR-1000") that uses dynamic light scattering as its measurement principle, the particle size distribution of the binder composition with the adjusted solid content concentration was measured, and the particle diameter (D50) at which the cumulative frequency of light scattering intensity calculated from the small diameter side reached 50% in the measured particle size distribution was taken as the average particle diameter Da. The measurement conditions for the dynamic light scattering method were as follows. Dispersion medium: water Measurement temperature: 25°C Measurement concentration (solid content concentration): 0.5% by mass Scattering angle: 160° Light source laser wavelength: 632.8 nm
[0084] <Average particle diameter Db (solid content concentration 0.005 mass%) of particulate binder measured by dynamic light scattering> The average particle diameter Db was calculated in the same manner as the above average particle diameter Da, except that ion-exchanged water was further added to the binder composition to change the measured concentration (solid content concentration) from 0.5 mass% to 0.005 mass%.
[0085] <Average particle diameter of particulate binder measured by laser diffraction scattering method> Using a particle size distribution measuring device (manufactured by Shimadzu Corporation, product name "SALD-2300") that uses laser diffraction scattering as its measurement principle, the particle size distribution of the binder compositions (aqueous dispersions of particulate binder, solid content concentration adjusted to 0.1% by mass) obtained in the examples and comparative examples was measured in accordance with JIS Z8825, and the particle diameter (D50) at which the cumulative volume calculated from the smallest diameter side became 50% in the measured particle size distribution was defined as the average particle diameter Dc.
[0086] <THF-insoluble content> The THF-insoluble content of the particulate binder was measured using the binder compositions obtained in the Examples and Comparative Examples. Specifically, the binder composition was first dropped into a petri dish so that the solid content was 1.5 g. Next, the binder composition was dried for 24 hours in an environment of 22 to 25°C, and further dried for 1 hour at 110°C to obtain a film of the particulate binder. Next, this film was cut into 2.5 mm square pieces, and approximately 0.3 g was precisely weighed. The mass of the film piece obtained by cutting was designated as W0. Next, the film piece was immersed in 80 mL of THF at 25°C for 24 hours. Next, the film piece was removed from the THF and vacuum-dried at 105°C for 3 hours, and the mass W1 of the film piece was measured. Then, the THF-insoluble content (mass%) was calculated according to the following formula (3): Insoluble content (mass%) = (W1 / W0) × 100 (3)
[0087] <Electrolyte Swelling Degree> The electrolyte swelling degree of the particulate binder was measured using the binder compositions obtained in the Examples and Comparative Examples. Specifically, the binder composition was first dried in an environment with a humidity of 50% and a temperature of 23 to 25°C to form a film with a thickness of 1±0.3 mm. The formed film was dried in a vacuum dryer at a temperature of 60°C for 10 hours to obtain a particulate binder film. Next, this film was cut and approximately 1 g was precisely weighed. The mass of the obtained film piece was designated W0. This film piece was immersed in an electrolyte solution (composition: 1.0 M LiPF6 solution (solvent: a mixed solvent of EC / EMC = 3 / 7 (mass ratio), with 2 mass% vinylene carbonate (solvent ratio) added as an additive)) in an environment with a temperature of 60°C for 3 days to allow swelling. Thereafter, the film piece was pulled out, the electrolyte solution on the surface was wiped with a Kimwipe, and the mass was measured. The mass of the film piece after swelling was designated as W1. The electrolyte swelling degree was calculated using the following formula (4): electrolyte swelling degree (mass%)=W1 / W0×100 (4)
[0088] <Repeated Tensile Test> A repeated tensile test was performed using the binder compositions obtained in the Examples and Comparative Examples. Specifically, the binder composition was first dropped into a 10 cm diameter Petri dish so that the solid content was 3.9 g. The binder composition was then dried for 24 hours in an environment of 22 to 25°C, and then further dried for 10 hours in an environment of -0.09 kPa (gauge pressure) or less and 100°C to obtain a film of particulate binder. The obtained film was cut into a dumbbell shape and immersed in a solvent of ethylene carbonate (EC) / ethyl methyl carbonate (EMC) = 3 / 7 (mass ratio) at 60°C for 72 hours. Then, a repeated tensile test was performed in a separately prepared solvent of EC / EMC = 3 / 7 (mass ratio), and the presence or absence of breakage of the dumbbell-shaped film was confirmed. The test conditions for the repeated tensile test were as follows. Tensile speed: 100 mm / min Tensile elongation: 30% Number of repetitions: 500 Test temperature: 20°C Test humidity: dew point -40°C or less Equipment manufacturer: Toyo Seiki Seisakusho Co., Ltd. Model: Strograph E3-L
[0089] <Tensile strength in repeated tensile test> The tensile strength of the dumbbell-shaped film subjected to the repeated tensile test was measured. Specifically, the tensile test was performed 500 times, and the tensile strength at a tensile elongation of 30% at the 500th time was defined as the tensile strength in the repeated tensile test. Note that the film produced using the binder composition obtained in Comparative Example 4 was not subjected to tensile strength measurement in the repeated tensile test because the film broke during the repeated tensile test.
[0090] <Electrode swelling> The thickness (d0) of the negative electrode produced in the negative electrode production process was measured. A secondary battery was produced using this negative electrode. The produced secondary battery was left standing for 5 hours in an environment at 25°C with the electrode immersed in the electrolyte. Next, the left-standing secondary battery was charged to a cell voltage of 3.65V using a constant current method at a rate of 0.2C in an environment at 25°C. The charged secondary battery was then subjected to an aging treatment for 12 hours in an environment at 60°C. Subsequently, the aging-treated secondary battery was discharged to a cell voltage of 3.00V using a constant current method at a rate of 0.2C in an environment at 25°C. Next, the secondary battery was reassembled, and the assembled secondary battery was subjected to 100 cycles of charge / discharge operation under conditions of a cell voltage of 4.20V to 3.00V and a charge / discharge rate of 1C in an environment at 25°C. The discharged secondary battery was then disassembled to remove the negative electrode, and the thickness of the negative electrode after cycling (d1) was measured as the total thickness of the negative electrode minus the thickness of the current collector. The rate of change in the negative electrode thickness (d1) after cycling relative to the negative electrode thickness (d0) at the time of secondary battery manufacture was calculated as follows: Swelling of negative electrode after cycling = {(d1 - d0) / d0} x 100 (%), and the result was evaluated according to the following criteria. The smaller the swelling of the negative electrode after cycling, the better the suppression of swelling of the negative electrode due to repeated charge and discharge. A: Swelling of negative electrode after cycling is less than 25% B: Swelling of negative electrode after cycling is 25% or more but less than 27% C: Swelling of negative electrode after cycling is 27% or more but less than 30% D: Swelling of negative electrode after cycling is 30% or more
[0091] <Cycle Characteristics> The cycle characteristics were evaluated using the secondary batteries fabricated in the examples and comparative examples. Specifically, first, the laminate cell type secondary batteries were subjected to electrolyte injection, aging, and conditioning. Next, a charge-discharge cycle was performed in an environment of 25°C, in which the battery was charged to a cell voltage of 4.20 V using a constant current method of 0.5 C and then discharged to a cell voltage of 2.75 V, and the initial capacity C0 was measured. This charge-discharge cycle was further repeated, and the capacity C1 after 100 cycles was measured. The capacity retention C2 was then calculated according to the following formula: C2 (%) = (C1 / C0) x 100. A larger value of the capacity retention C2 indicates better cycle characteristics. A: Capacity retention C2 is 93% or more. B: Capacity retention C2 is 88% or more but less than 93%. C: Capacity retention C2 is 83% or more but less than 88%. D: Capacity retention C2 is less than 83%.
[0092] Example 1 Preparation of Binder Composition 2.1 parts of styrene as an aromatic vinyl monomer, 3.3 parts of 1,3-butadiene as an aliphatic conjugated diene monomer, 0.1 parts of methacrylic acid as an ethylenically unsaturated carboxylic acid monomer, 0.23 parts of dodecyl diphenyl ether disulfonic acid sodium salt as an emulsifier, 15 parts of ion-exchanged water, and 0.02 parts of potassium persulfate as a polymerization initiator were placed in a 5 MPa pressure vessel A equipped with a stirrer to obtain a mixture A. The obtained mixture A was thoroughly stirred and then heated to 57°C to initiate polymerization and react for 5 hours, and then heated to 70°C and reacted for an additional 4 hours to obtain seed particles. Separately, into a 5 MPa pressure vessel B equipped with a stirrer, 31.6 parts of styrene as an aromatic vinyl monomer, 44 parts of 1,3-butadiene as an aliphatic conjugated diene monomer, 14.2 parts of acrylic acid as an ethylenically unsaturated carboxylic acid group monomer, 4.7 parts of acrylamide as an ethylenically unsaturated amide group monomer, 0.5 parts of tert-dodecyl mercaptan as a molecular weight modifier, 0.20 parts of sodium lauryl sulfate as an emulsifier, and 44 parts of ion-exchanged water were added to obtain a mixture B. After obtaining the seed particles, the temperature of the contents of the pressure vessel A was heated to 75°C, and mixture B was added to the pressure vessel A over 5 hours. At the same time, polymerization was initiated by starting the addition of 0.5 parts of potassium persulfate as a polymerization initiator to the heat-resistant vessel A. That is, the total monomer composition was 33.7 parts of styrene, 47.3 parts of 1,3-butadiene, 14.2 parts of acrylic acid, 4.7 parts of acrylamide, and 0.1 parts of methacrylic acid. Five hours after the start of polymerization, the addition of the entire mixture containing these monomer compositions was completed, after which 0.5 parts of potassium persulfate was added. The mixture was then heated to 90°C and reacted for 4 hours. When the polymerization conversion rate reached 97%, the mixture was cooled to stop the reaction. A 5% aqueous solution of sodium hydroxide was added to the mixture containing this polymer, and the pH was adjusted to 8. Thereafter, unreacted monomers were removed by heating and distillation under reduced pressure. The mixture was then further cooled, and a binder composition containing the desired particulate binder was obtained.Using the obtained binder composition, the average particle diameter Da of the particulate binder measured by dynamic light scattering (solid content concentration 0.5 mass%), the average particle diameter Db of the particulate binder measured by dynamic light scattering (solid content concentration 0.005 mass%), the average particle diameter Dc of the particulate binder measured by laser diffraction scattering, the THF insoluble content, the electrolyte swelling degree, the repeated tensile test, and the tensile strength of the repeated tensile test were measured. The results are shown in Table 1.
[0093] <Preparation of Slurry Composition for Negative Electrode> 87.3 parts of artificial graphite as a carbon-based negative electrode active material and SiO as a silicon-based negative electrode active material were placed in a planetary mixer equipped with a disperser. x 9.7 parts of carboxymethylcellulose sodium aqueous solution as a thickener (solid content equivalent) was added, and the solid content concentration was adjusted to 61.5% with ion-exchanged water, and mixed at room temperature for 40 minutes. After mixing, the solid content concentration was gradually adjusted to 56% and 51% with ion-exchanged water, and 1.0 part (solid content equivalent) of the binder composition obtained as described above was added to obtain a mixed solution. The obtained mixed solution was degassed under reduced pressure to obtain a negative electrode slurry composition with good fluidity.
[0094] <Production of Negative Electrode> The above-described negative electrode slurry composition was applied to a copper foil (current collector) having a thickness of 16 μm using a comma coater in an amount of 10 mg / cm. 2 The copper foil coated with the negative electrode slurry composition was transported at a speed of 0.5 m / min through an oven at 75°C for 2 minutes and then through an oven at 120°C for 2 minutes to dry the negative electrode slurry composition on the copper foil, thereby obtaining a negative electrode blank. The negative electrode blank was rolled using a roll press to obtain a negative electrode having a negative electrode composite layer thickness of 80 μm.
[0095] <Production of Positive Electrode> 96 parts of lithium nickel manganese cobalt oxide as a positive electrode active material, 2 parts of PVDF (polyvinylidene fluoride) as a binder for a positive electrode composite layer in terms of solid content, 2 parts of acetylene black as a conductive material, and 20 parts of N-methylpyrrolidone as a solvent were added to a planetary mixer and mixed to obtain a positive electrode slurry composition. The obtained positive electrode slurry composition was applied to a 16 μm-thick aluminum foil (current collector) using a comma coater so that the coating amount after drying was 24.5 mg / cm. 2 The aluminum foil coated with the positive electrode slurry composition was transported at a speed of 0.5 m / min through an oven at 60°C for 2 minutes and then through an oven at 120°C for 2 minutes to dry the positive electrode slurry composition on the aluminum foil, thereby obtaining a positive electrode blank. The positive electrode blank was rolled using a roll press to obtain a positive electrode having a positive electrode composite layer thickness of 70 μm.
[0096] <Preparation of Separator> A single-layer polypropylene separator (width 65 mm, length 500 mm, thickness 25 μm; manufactured by a dry method; porosity 55%) was prepared. This separator was cut into a 5 cm × 5 cm square and used in the following secondary battery.
[0097] <Preparation of Secondary Battery> An aluminum packaging material was prepared as the battery packaging. The positive electrode was cut into a 4 cm x 4 cm square and placed so that the surface on the current collector side was in contact with the aluminum packaging material. Next, the square separator was placed on the surface of the positive electrode composite layer of the positive electrode. Furthermore, the negative electrode was cut into a 4.2 cm x 4.2 cm square and placed on the separator so that the surface on the negative electrode composite layer side faced the separator. Then, LiPF 5 with a concentration of 1.0 M was used as an electrolyte. 6A solution (the solvent was a mixed solvent of ethylene carbonate (EC) / ethyl methyl carbonate (EMC) = 3 / 7 (mass ratio), containing 2 mass% vinylene carbonate and 2 mass% fluoroethylene carbonate as additives) was filled into the battery. Furthermore, in order to seal the opening of the aluminum packaging, the aluminum packaging exterior was closed by heat sealing at 150°C, and a laminate cell type secondary battery was produced. The resulting secondary battery was evaluated for electrode swelling and cycle characteristics. The results are shown in Table 1.
[0098] (Example 2) In preparing the binder composition, the amount of the molecular weight modifier in mixture B was changed from 0.5 parts to 0.25 parts, and the same procedures, measurements, and evaluations were carried out as in Example 1. The results are shown in Table 1.
[0099] Example 3 In the preparation of the binder composition, the acrylic acid of mixture B was changed from 14.2 parts to 11.8 parts, the 1,3-butadiene from 44 parts to 46.7 parts, the styrene from 31.6 parts to 32.2 parts, and the acrylamide from 4.7 parts to 3.8 parts, i.e., the monomer composition as a whole was changed to 34.3 parts of styrene, 50.0 parts of 1,3-butadiene, 11.8 parts of acrylic acid, 3.8 parts of acrylamide, and 0.1 part of methacrylic acid. Except for this, various operations, measurements, and evaluations were carried out in the same manner as in Example 1. The results are shown in Table 1.
[0100] (Example 4) In preparing the binder composition, the amount of the molecular weight modifier in mixture B was changed from 0.5 parts to 0.25 parts, and the same procedures, measurements, and evaluations were carried out as in Example 3. The results are shown in Table 1.
[0101] Example 5 In the preparation of the binder composition, the 1,3-butadiene in mixture B was changed from 44 parts to 44.9 parts, the styrene from 31.6 parts to 32.4 parts, and the acrylamide from 4.7 parts to 3.0 parts, i.e., the monomer composition as a whole was changed to 34.5 parts of styrene, 48.2 parts of 1,3-butadiene, 14.2 parts of acrylic acid, 3.0 parts of acrylamide, and 0.1 part of methacrylic acid. Except for this, various operations, measurements, and evaluations were carried out in the same manner as in Example 2. The results are shown in Table 1.
[0102] Example 6 In the preparation of the binder composition, the acrylic acid of mixture B was changed from 14.2 parts to 10.0 parts, the 1,3-butadiene was changed from 44 parts to 44.9 parts, the styrene was changed from 31.6 parts to 32.4 parts, the acrylamide was changed from 4.7 parts to 3.0 parts, and 4.2 parts of methacrylic acid was added, i.e., the overall monomer composition was changed to 34.5 parts of styrene, 48.2 parts of 1,3-butadiene, 10.0 parts of acrylic acid, 3.0 parts of acrylamide, and 4.3 parts of methacrylic acid. Except for this, various operations, measurements, and evaluations were carried out in the same manner as in Example 2. The results are shown in Table 1.
[0103] Comparative Example 1 Various operations, measurements, and evaluations were carried out in the same manner as in Example 1, except that the binder composition used was a particulate binder formed by two-stage polymerization and obtained by the following preparation method. The results are shown in Table 1.
[0104] <Preparation of Binder Composition> First, in the first-stage polymerization, 24 parts of styrene as an aromatic vinyl monomer, 69 parts of 1,3-butadiene as an aliphatic conjugated diene monomer, 100 parts of ion-exchanged water, 0.7 parts of dodecylbenzenesulfonic acid as an emulsifier, 0.1 parts of α-methylstyrene dimer as a chain transfer agent, and 0.3 parts of potassium persulfate as a polymerization initiator were placed in a 5 MPa pressure vessel equipped with a stirrer and thoroughly stirred. The mixture was then heated to 60°C to initiate polymerization. The polymerization was continued until the polymerization conversion rate reached 96%. Next, in the second-stage polymerization, 7 parts of methacrylic acid as an ethylenically unsaturated carboxylic acid monomer and 37 parts of ion-exchanged water were continuously added to the same pressure vessel under stirring to continue the polymerization. This aqueous dispersion was heated to 70 ° C., and when the polymerization conversion rate reached 97%, the reaction was stopped by cooling. A polymer was formed as a shell on the outer surface of the core, obtaining a mixture containing a particulate binder having a core-shell structure. Subsequently, unreacted monomers were removed by heated vacuum distillation. A 5% aqueous sodium hydroxide solution was added to the mixture containing the particulate binder, and the pH was adjusted to 7 to obtain a binder composition (aqueous dispersion). Using the obtained binder composition, the average particle diameter Da of the particulate binder (solid content concentration 0.5% by mass) measured by dynamic light scattering, the average particle diameter Db of the particulate binder (solid content concentration 0.005% by mass) measured by dynamic light scattering, the average particle diameter Dc of the particulate binder measured by laser diffraction scattering, the THF insoluble content, the electrolyte swelling degree, the repeated tensile test, and the tensile strength of the repeated tensile test were measured. The results are shown in Table 1.
[0105] Comparative Example 2 In the preparation of the binder composition, the acrylic acid in mixture B was changed from 14.2 parts to 9.5 parts, the 1,3-butadiene from 44 parts to 49.1 parts, the styrene from 31.6 parts to 32.6 parts, and the acrylamide from 4.7 parts to 3.3 parts, i.e., the monomer composition as a whole was changed to 34.7 parts of styrene, 52.4 parts of 1,3-butadiene, 9.5 parts of acrylic acid, 3.3 parts of acrylamide, and 0.1 part of methacrylic acid. Except for this, various operations, measurements, and evaluations were carried out in the same manner as in Example 1. The results are shown in Table 1.
[0106] Comparative Example 3 Except for using a binder composition prepared by the following method, various operations, measurements, and evaluations were carried out in the same manner as in Example 1. The results are shown in Table 1.
[0107] <Preparation of Binder Composition> 65.0 parts of styrene as an aromatic vinyl monomer, 30.0 parts of 1,3-butadiene as an aliphatic conjugated diene monomer, 1.5 parts of acrylic acid and 3.5 parts of itaconic acid as ethylenically unsaturated carboxylic acid monomers, 4 parts of sodium dodecylbenzenesulfonate as an emulsifier, 150 parts of ion-exchanged water, and 0.5 parts of potassium persulfate as a polymerization initiator were placed in a 5 MPa pressure vessel equipped with a stirrer, and after thorough stirring, the mixture was heated to 50°C to initiate polymerization. The reaction was stopped by cooling when the polymerization conversion rate reached 96%. A 5% aqueous sodium hydroxide solution was then added to the mixture containing this polymer to adjust the pH to 8. After that, unreacted monomers were removed by heating and vacuum distillation, and the mixture was cooled to 30°C or below to obtain a binder composition (aqueous dispersion) containing a particulate binder.
[0108] Comparative Example 4 In the preparation of the binder composition, the acrylic acid of mixture B was changed from 14.2 parts to 18.9 parts, the 1,3-butadiene from 44 parts to 40.3 parts, the styrene from 31.6 parts to 29 parts, and the acrylamide from 4.7 parts to 6.3 parts, that is, the monomer composition as a whole was changed to 31.1 parts of styrene, 43.6 parts of 1,3-butadiene, 18.9 parts of acrylic acid, 6.3 parts of acrylamide, and 0.1 part of methacrylic acid. Except for this, various operations, measurements, and evaluations were carried out in the same manner as in Example 1. The results are shown in Table 1.
[0109] Comparative Example 5 Except for using a binder composition prepared by the following method, various operations, measurements, and evaluations were carried out in the same manner as in Example 1. The results are shown in Table 1.
[0110] <Preparation of Binder Composition> 62.5 parts of styrene as an aromatic vinyl monomer, 34 parts of 1,3-butadiene as an aliphatic conjugated diene monomer, 3.5 parts of itaconic acid as an ethylenically unsaturated carboxylic acid monomer, 4 parts of sodium dodecylbenzenesulfonate as an emulsifier, 150 parts of ion-exchanged water, and 0.5 parts of potassium persulfate as a polymerization initiator were placed in a 5 MPa pressure vessel equipped with a stirrer, and after thorough stirring, the mixture was heated to 50°C to initiate polymerization. When the polymerization conversion rate reached 96%, the mixture was cooled to terminate the reaction. A 5% aqueous solution of sodium hydroxide was then added to the mixture containing the polymer to adjust the pH to 8. After that, unreacted monomers were removed by heating and vacuum distillation, and the mixture was cooled to 30°C or below to obtain a binder composition (aqueous dispersion) containing a particulate binder.
[0111] In Table 1, "AA" represents acrylic acid, "IA" represents itaconic acid, "MAA" represents methacrylic acid, "BD" represents 1,3-butadiene, "ST" represents styrene, and "AAm" represents acrylamide.
[0112]
[0113] As is clear from Table 1, by using the binder compositions for nonaqueous secondary battery negative electrodes of Examples 1 to 6, it is possible to effectively suppress swelling of the negative electrode due to repeated charge and discharge, and to enable the secondary battery to exhibit excellent cycle characteristics.
[0114] Therefore, according to the present invention, a binder composition for a non-aqueous secondary battery negative electrode can be provided that effectively suppresses swelling of the negative electrode due to repeated charge and discharge and allows the secondary battery to exhibit excellent cycle characteristics. Furthermore, according to the present invention, a slurry composition for a non-aqueous secondary battery negative electrode can be provided that effectively suppresses swelling of the negative electrode due to repeated charge and discharge and allows the secondary battery to exhibit excellent cycle characteristics. Furthermore, according to the present invention, a non-aqueous secondary battery negative electrode that is less likely to swell even with repeated charge and discharge and allows the secondary battery to exhibit excellent cycle characteristics can be provided. Furthermore, according to the present invention, a non-aqueous secondary battery that is less likely to swell of the negative electrode due to charge and discharge and has excellent cycle characteristics can be provided.
[0115] 10 Particulate binder 11 Main body 12 String-like portion
Claims
1. A binder composition for a non-aqueous secondary battery negative electrode, comprising a particulate binder and water, wherein the particulate binder comprises a polymer containing an ethylenically unsaturated carboxylic acid monomer unit, an aromatic vinyl monomer unit, and an aliphatic conjugated diene monomer unit, and the content ratio of the ethylenically unsaturated carboxylic acid monomer unit is 5.0% by mass or more and 15.0% by mass or less, when the total repeating units of the polymer are taken as 100% by mass, and the particulate binder has an average particle diameter Da, as measured by a dynamic light scattering method on a binder composition for a non-aqueous secondary battery negative electrode adjusted to have a solid content concentration of 0.5% by mass, an average particle diameter Db, as measured by a dynamic light scattering method on a binder composition for a non-aqueous secondary battery negative electrode adjusted to have a solid content concentration of 0.005% by mass, and an average particle diameter Dc, as measured by a laser diffraction scattering method, which satisfy the following formulas (1) and (2): A binder composition for a non-aqueous secondary battery negative electrode, which satisfies the relationships: Da-Db≦60.0 nm (1) and 1.40≦Da / Dc≦2.00 (2).
2. The binder composition for a negative electrode of a non-aqueous secondary battery according to claim 1, wherein the particulate binder has an insoluble content in tetrahydrofuran of more than 90% by mass and less than 100% by mass.
3. The binder composition for a non-aqueous secondary battery negative electrode according to claim 1 or 2, wherein the content of the aliphatic conjugated diene monomer unit is 30.0 mass% or more and 60.0 mass% or less, when the total repeating units of the polymer are taken as 100 mass%.
4. The binder composition for a non-aqueous secondary battery negative electrode according to any one of claims 1 to 3, wherein the polymer further contains an ethylenically unsaturated amide monomer unit.
5. The binder composition for a non-aqueous secondary battery negative electrode according to claim 4, wherein the content of the ethylenically unsaturated amide monomer unit is 3.5 mass% or more, when the total amount of all repeating units of the polymer is taken as 100 mass%.
6. A slurry composition for a non-aqueous secondary battery negative electrode, comprising a negative electrode active material and the binder composition for a non-aqueous secondary battery negative electrode according to any one of claims 1 to 5.
7. The slurry composition for a non-aqueous secondary battery negative electrode according to claim 6, wherein the negative electrode active material comprises a silicon-based negative electrode active material.
8. A negative electrode for a non-aqueous secondary battery comprising a current collector and a negative electrode mixture layer located on the current collector, wherein the negative electrode mixture layer is a layer formed from the slurry composition for a non-aqueous secondary battery negative electrode according to claim 6 or 7.
9. A nonaqueous secondary battery comprising a positive electrode, a negative electrode, a separator, and an electrolyte, wherein the negative electrode is the negative electrode for a nonaqueous secondary battery according to claim 8.
Citation Information
Patent Citations
Electrode for secondary battery, binder for secondary battery electrode, manufacturing method and secondary battery
JP2012204303A
Binder composition for power storage device electrode, slurry for power storage device electrode, power storage device electrode, and power storage device
JP2016058184A
Slurry composition for lithium ion secondary battery negative electrode, negative electrode for lithium ion secondary battery, and lithium ion secondary battery
JP2016048633A
Production method of binder composition for nonaqueous secondary battery electrode, production method of slurry composition for nonaqueous secondary battery electrode, production method of electrode for nonaqueous secondary battery, and production method of nonaqueous secondary battery
JP2017117597A
Binder composition for lithium ion secondary battery, slurry composition for lithium ion secondary battery, method for manufacturing electrode for secondary battery, and lithium ion secondary battery
WO2015098507A1
Cited By
Binder, binder composition, electrode slurry, electrode, and nonaqueous secondary battery
WO2026168490A1