Ophthalmic medical instrument and manufacturing method therefor
A dual-layer ophthalmic medical device with controlled cationic and hydroxyl group content in its resin layers addresses the issue of poor sustained release and stability in hydrogel contact lenses, achieving effective drug delivery and wearability through precise structural unit ratios and photopolymerization.
Patent Information
- Application Number
- PCT/JP2024/011360
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2024-02-05
- Filing Date
- 2024-03-22
- Publication Date
- 2024-10-03
AI Technical Summary
Hydrogels made of ionic monomers with cationic and/or anionic monomers often exhibit poor sustained drug release properties and shape stability issues, particularly when used in ophthalmic medical devices like contact lenses, due to changes in shape when saturated with water, affecting wearability.
An ophthalmic medical device comprising two resin layers (A and B) with specific structural units, where layer A has a cationic group and layer B contains a hydroxyl group, with controlled ratios of these units to enhance sustained drug release and shape stability, and a method involving photopolymerization to form these layers.
The device achieves excellent sustained release properties and high shape stability, improving wearability and drug delivery over time, as demonstrated by ToF-SIMS ion images and sustained release tests.
Smart Images

Figure JP2024011360_03102024_PF_FP_ABST
Abstract
Description
Ophthalmic medical device and manufacturing method thereof
[0001] The present invention relates to an ophthalmic medical device and a method for manufacturing the same. This application claims priority to Japanese Patent Application No. 2023-052635 filed on March 29, 2023, and Japanese Patent Application No. 2024-015699 filed on February 5, 2024, the contents of which are incorporated herein by reference.
[0002] Ophthalmic medical devices with sustained drug release have been investigated for the purpose of delivering drugs to affected areas of the eye over a long period of time by wearing a drug-containing ophthalmic medical device. One such ophthalmic medical device is a drug-loaded hydrogel contact lens (Patent Document 1). To control the drug release rate, surface modification of the hydrogel, such as plasma irradiation, ultraviolet irradiation, or graft polymerization of a surface-modifying monomer, has been proposed (Patent Document 2). Dimethylacrylamide or methacrylic acid is used as the surface-modifying monomer. Furthermore, to control the initial release of an anionic drug, sustained-release hydrogel contact lenses have been proposed (Patent Document 3). The hydrogel is composed of ionic monomers, including at least a cationic monomer and an anionic monomer, and the content of the anionic monomer is within a predetermined range relative to the cationic monomer.
[0003] Japanese Patent Publication No. 2008-539837 Japanese Patent Publication No. 2005-218780 International Publication No. 2010 / 095478
[0004] However, hydrogels made of ionic monomers, such as cationic monomers and / or anionic monomers, may exhibit reduced sustained drug release. In particular, when a hydrogel is molded into an ophthalmic medical device such as a contact lens, and then the hydrogel is impregnated with ionic monomer units and polymerized to modify the hydrogel with ionic groups in order to produce a sustained-release ophthalmic medical device more efficiently, the shape of the contact lens when saturated with water changes from the shape of the unmodified contact lens when saturated with water, resulting in poor wearability.
[0005] An object of the present invention is to provide an ophthalmic medical device that has excellent sustained release properties, high shape stability, and excellent wearability, and a method for producing the same.
[0006] As a result of extensive research, the present inventors have found that an ophthalmic medical device having at least two resin layers, each having a specific configuration, has excellent sustained drug release properties and shape stability. The present invention is based on this finding and includes the following aspects.
[0007] [1] An ophthalmic medical device comprising a resin layer (A) and a resin layer (B), wherein at least a portion of the surface of the ophthalmic medical device is formed by the resin layer (A), the resin layer (A) has a thickness of 1 μm or more at its thickest part, the resin layer (A) comprises at least one structural unit selected from the group consisting of a structural unit (a1) derived from a monomer having a cationic group (excluding monomers having a zwitterionic group) and a structural unit (a2) derived from a monomer having an anionic group (excluding monomers having a zwitterionic group), and the resin layer (A) and the resin layer (B) satisfy either or both of the following relationships (1) and (2): (1) The ratio of the content of the structural unit (a1) in the resin layer (A) to the content of the structural unit (a1) in the resin layer (B) is ≥ 2.0. (2) The content of the structural unit (a2) in the resin layer (A) to the content of the structural unit (a2) in the resin layer (B) is ≥ 2.0. [2] The ophthalmic medical device of [1], wherein the resin layer (B) contains a structural unit (b1) derived from a monomer having a hydroxyl group. [3] The ophthalmic medical device of [1] or [2], wherein the resin layer (A) contains a structural unit (a3) derived from a monomer having a zwitterionic group. [4] The ophthalmic medical device of any of [1] to [3], wherein a portion of the surface of the ophthalmic medical device that comes into contact with the eyeball is formed by the resin layer (A). [5] The ophthalmic medical device of any of [1] to [4], which is a medical contact lens. [6] The ophthalmic medical device of any of [1] to [5], wherein the ophthalmic medical device contains a drug. [7] The ophthalmic medical device according to [6], wherein the drug is released when immersed in phosphate buffered saline containing 2% by mass of sodium chloride. [8] A method for producing a monomer having a cationic group (excluding monomers having a zwitterionic group) and a monomer having an anionic group (excluding monomers having a zwitterionic group) by irradiation with active energy rays in the presence of a photopolymerization initiator.and forming the resin layer (B) on the resin layer (A) by polymerizing a monomer mixture containing at least one monomer selected from the group consisting of a monomer having a hydroxyl group, the monomer mixture being in contact with the resin layer (A) or via another resin layer. [9] A method for producing the ophthalmic medical device according to any of [1] to [7], comprising forming the resin layer (A) on the resin layer (B) containing a structural unit (b1) derived from a monomer having a hydroxyl group by irradiating the resin layer (B) with active energy rays in the presence of a photopolymerization initiator, the polymerizing monomer mixture being in contact with the resin layer (B) or via another resin layer.
[0008] According to the present invention, an ophthalmic medical device having excellent sustained release properties, high shape stability, and excellent wearability, and a method for producing the same can be provided.
[0009] 1 is a ToF-SIMS ion image of a cross section of the contact lens of Example 1. FIG. 2 is a ToF-SIMS ion image of a cross section of the contact lens of Example 2.
[0010] In this specification, "acrylic resin" refers to a resin having an acrylic monomer unit. The acrylic resin may further have a monomer unit other than the acrylic monomer (such as a styrene unit). The content of the acrylic monomer unit in the acrylic resin is preferably 50 mol% or more, more preferably 70 mol% or more, and even more preferably 90 mol% or more. "Acrylic monomer" refers to a compound having a (meth)acryloyl group. "(meth)acryloyl group" is a general term for acryloyl groups and methacryloyl groups. The same applies to "(meth)acrylate," "(meth)acrylic acid," "(meth)acrylonitrile," and "(meth)acrylamide." The "to" symbol indicating a numerical range means that the numerical values before and after it are included as the lower and upper limits.
[0011] [Ophthalmic Medical Device] The ophthalmic medical device of the present invention includes a resin layer (A) and a resin layer (B), with the resin layer (A) forming at least a portion of the surface of the ophthalmic medical device. The resin layer (A) includes at least one structural unit selected from the group consisting of a structural unit (a1) derived from a monomer having a cationic group (excluding monomers having a zwitterionic group) and a structural unit (a2) derived from a monomer having an anionic group (excluding monomers having a zwitterionic group). The resin layer (A) has a thickness of 1 μm or greater at its thickest point. The resin layer (B) may or may not include the structural unit (a1) or the structural unit (a2).
[0012] In the ophthalmic medical device of the present invention, the resin layer (A) and the resin layer (B) satisfy one or both of the following relationships (1) and (2): (1) the content of the structural unit (a1) in the resin layer (A) / the content of the structural unit (a1) in the resin layer (B) ≥ 2.0 (2) the content of the structural unit (a2) in the resin layer (A) / the content of the structural unit (a2) in the resin layer (B) ≥ 2.0
[0013] In other words, the ratio of the content of the structural unit (a1) in the resin layer (A) to the content of the structural unit (a1) in the resin layer (B) is at least 2 times, and / or the ratio of the content of the structural unit (a2) in the resin layer (A) to the content of the structural unit (a2) in the resin layer (B) is at least 2 times. In other words, the ophthalmic medical device of the present invention has a resin layer (A) having at least one structural unit selected from the group consisting of the structural unit (a1) and the structural unit (a2), and a resin layer (B) in which the content of the structural unit (a1) is no more than half the content of the structural unit (a1) in the resin layer (A), or the content of the structural unit (a2) is no more than half the content of the structural unit (a2) in the resin layer (A). When the resin layer (A) contains both the structural unit (a1) and the structural unit (a2), it is preferable that the structural unit (a1) or the structural unit (a2) that is contained in the greater amount satisfies either the relationship (1) or (2) above.
[0014] The ophthalmic medical device has a structure having two or more layers with different proportions of the structural unit (a1) or (a2), thereby achieving good sustained release of the drug. The content of the structural unit (a1) or (a2) in the resin layer (A) forming the entirety of at least one surface of the ophthalmic medical device may be at least twice the content of the structural unit (a1) or (a2) in the other resin layers (including the resin layer (B)), or the content of the structural unit (a1) or (a2) in the resin layer (A) forming a portion of at least one surface of the ophthalmic medical device may be at least twice the content of the structural unit (a1) or (a2) in the other resin layers (including the resin layer (B)).
[0015] The content of the structural unit (a1) or (a2) in the resin layer (A) is preferably at least 3 times, more preferably at least 4 times, and even more preferably at least 5 times the content of the structural unit (a1) or (a2) in the resin layer (B). If the structural unit (a1) or (a2) is not contained in the resin layer (B), the upper limit of this ratio becomes infinite, so there is no upper limit, but it is usually 100 times or less.
[0016] The content ratio of the structural unit (a1) or (a2) can be determined by regarding the ion intensity ratio in a time-of-flight secondary ion mass spectrometer (ToF-SIMS) as a parameter corresponding to the amount of the substance present. Specifically, it can be determined by the following method. Mass spectra are obtained using ToF-SIMS at the surface and at the center of the cross section of the ophthalmic medical device, and the intensity ratio of ions derived from the structural unit (a1) or (a2) to common ions derived from all structural units of the resin component at each measurement position is calculated. The quotient of these values (ion intensity ratio at the surface / ion intensity ratio at the center) is used as the content ratio of the structural unit (a1) or (a2). The ions derived from the structural unit (a1) or (a2) may be any ions that can characterize the structural unit (a1) or (a2), and can be selected appropriately depending on the type of structural unit (a1). The common ions derived from all structural units of the resin component may be any ions that are common to all structural units, and can be selected appropriately depending on the type of structural unit that constitutes the resin component.
[0017] Whether the ophthalmic medical device has layers with different contents of the structural unit (a1) or (a2) can be confirmed by optical microscopic observation of the cross section of the ophthalmic medical device, ToF-SIMS ion images, or the like.
[0018] The resin layer (A) is typically provided on at least a portion of the surface of the ophthalmic medical device that comes into contact with the eyeball when in use, but may also be provided on at least a portion of the surface that does not come into contact with the eyeball, or on at least a portion of each of both surfaces. Furthermore, the resin layer (A) may be provided on the entire surface of the ophthalmic medical device that comes into contact with the eyeball when in use, or on the entire surface of the side that does not come into contact with the eyeball, or on the entire surface of each of both surfaces. The resin layer (A) may be provided so as to cover the entire surface of the ophthalmic medical device, or the entire surface and side surfaces. It is preferable that the resin layer (A) be provided on the surface that comes into contact with the eyeball when in use, as this will result in good sustained release properties.
[0019] The resin layer (A) and the resin layer (B) may be provided in contact with each other, or may be provided with another resin layer interposed therebetween.
[0020] Furthermore, in a structure having at least two resin layers, the interface between the layers does not have to be clear. That is, the at least two resin layers are not limited to those obtained by, for example, sequentially laminating resin layers (A) and (B) in stages, but may also be in a form in which the content of the structural unit (a1) or (a2) has a gradient structure in the thickness direction (this form is also considered to be two or more layers). More specifically, a resin component containing the structural unit (a1) or (a2) and a resin component not containing the structural unit (a1) or (a2) are diluted in a solvent to form a coating solution, which is then applied, dried, and molded into the shape of an ophthalmic medical device. This allows the resin component containing the structural unit (a1) or (a2) to concentrate on the surface of the layer, resulting in a layer with a gradient structure in the thickness direction. The form in which the content ratio of the structural unit (a1) or (a2) has a gradient structure in the thickness direction can be confirmed using a time-of-flight secondary ion mass spectrometer (ToF-SIMS).
[0021] Examples of ophthalmic medical devices include medical contact lenses, implantable drug-releasing devices, punctal plugs, and conjunctival rings. Among these, medical contact lenses are preferred in terms of convenience for patients, non-invasiveness, and the need for physician training.
[0022] The thickness of the ophthalmic medical device is not particularly limited, but is, for example, 50 to 1000 μm.
[0023] <Resin Layer (A)> The resin layer (A) contains at least one structural unit selected from the group consisting of the structural unit (a1) and the structural unit (a2). The resin layer (A) preferably contains only one of the structural units (a1) and (a2). In one embodiment, the resin layer (A) contains the structural unit (a1) but does not contain the structural unit (a2). In another embodiment, the resin layer (A) contains the structural unit (a2) but does not contain the structural unit (a1). Examples of the cationic group of the monomer having a cationic group in the structural unit (a1) include a tertiary amino group and a quaternary ammonium group. The monomer having a cationic group may be an acrylic monomer or a monomer other than an acrylic monomer, and these may be used in combination. It is preferred that at least a portion of the monomer having a cationic group is an acrylic monomer. Examples of monomers having a cationic group include ethyl methacrylates (particularly ammonium chlorides) such as dimethylaminoethyl (meth)acrylate, diethylaminoethyl (meth)acrylate, trimethyl(3-(meth)acryloylaminopropyl)ammonium salt, 2-(meth)acryloxyethyltrimethylammonium salt, 2-(meth)acryloxyethyldimethylethylammonium salt, and 2-(meth)acryloxyethyldimethyl n-pentylammonium salt, (meth)acryloyloxyethyldimethylbenzylammonium chloride, and 2-((meth)acryloyloxy)ethyltrimethylammonium chloride. These monomers may be used alone or in combination of two or more.
[0024] Examples of the anionic group of the monomer having an anionic group in the structural unit (a2) include a carboxylic acid group, a sulfonic acid group, and a phosphate group. The monomer having an anionic group may be an acrylic monomer, or a monomer other than an acrylic monomer, and these may be used in combination. It is preferable that at least a portion of the monomer having an anionic group is an acrylic monomer. Examples of monomers having an anionic group include monocarboxylic acids such as (meth)acrylic acid, 2-methacryloyloxyethyl succinic acid, 2-methacryloyloxyethyl hexahydrophthalic acid, vinylbenzoic acid, and allylacetic acid; unsaturated carboxylic acid monomers such as dicarboxylic acids such as (anhydrous) maleic acid, fumaric acid, and itaconic acid; unsaturated hydrocarbons having a sulfonic acid group such as vinylsulfonic acid and styrenesulfonic acid; 2-(meth)acryloyloxyethanesulfonic acid, 2-(meth)acryloyloxypropanesulfonic acid, and 3-(meth)acryloyloxypropanesulfone. Examples of such monomers include (meth)acrylates having a sulfonic acid group, such as 2-(meth)acryloyloxybutanesulfonic acid, 4-(meth)acryloyloxybutanesulfonic acid, 2-(meth)acryloyloxy-2,2-dimethylethanesulfonic acid, and p-(meth)acryloyloxymethylbenzenesulfonic acid; unsaturated sulfonic acid monomers, such as (meth)allylsulfosuccinate esters having 5 to 20 carbon atoms; and unsaturated phosphoric acid monomers, such as 2-(meth)acryloyloxyethyl acid phosphate and bis(2-(meth)acryloyloxyethyl) acid phosphate. These monomers may be used alone or in combination of two or more.
[0025] The resin layer (A) may contain a structural unit (b1) derived from a monomer having a hydroxyl group. Examples of the monomer having a hydroxyl group in the structural unit (b1) include (meth)acrylic acid hydroxyalkyl esters such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 5-hydroxypentyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, and 8-hydroxyoctyl (meth)acrylate; caprolactone-modified monomers such as caprolactone-modified 2-hydroxyethyl (meth)acrylate; and diethylene glycol. Examples of the monomer include oxyalkylene-modified monomers such as (meth)acrylate and polyethylene glycol (meth)acrylate; primary hydroxyl group-containing monomers such as 2-acryloyloxyethyl-2-hydroxyethyl phthalate; secondary hydroxyl group-containing monomers such as 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-chloro-2-hydroxypropyl (meth)acrylate and 2-hydroxy-3-acryloyloxypropyl (meth)acrylate; and tertiary hydroxyl group-containing monomers such as 2,2-dimethyl-2-hydroxyethyl (meth)acrylate. These monomers may be used alone or in combination of two or more. The structural unit (b1) may be an alcoholysis product or hydrolyzate of a structural unit derived from vinyl acetate, or a hydrolyzate of a structural unit derived from an alkoxysilane.
[0026] The resin layer (A) may contain a structural unit (a3) derived from a zwitterionic monomer. The zwitterionic group of the zwitterionic monomer in the structural unit (a3) is a group having a cationic moiety and an anionic moiety. Examples of the cationic moiety include groups similar to the cationic group of the monomer having a cationic group. Examples of the anionic moiety include groups similar to the anionic group of the monomer having an anionic group. The monomer having a zwitterionic group may be an acrylic monomer or a monomer other than an acrylic monomer, and these may be used in combination. It is preferable that at least a portion of the monomer having a zwitterionic group is an acrylic monomer. Examples of monomers having an amphoteric ionic group include [2-((meth)acryloyloxy)ethyl]dimethyl-(3-sulfopropyl)ammonium hydroxide, [3-((meth)acryloylamino)propyl]dimethyl(3-sulfopropyl)ammonium hydroxide, 2-((meth)acryloyloxy)ethyl-2-(triethylammonio)ethyl phosphate, and [[2-((meth)acryloyloxy)ethyl](dimethyl)ammonio]acetate. These monomers may be used alone or in combination of two or more.
[0027] The resin layer (A) may contain a structural unit derived from a monomer other than the structural unit (a1), the structural unit (a2), the structural unit (b1), and the structural unit (a3) (the structural unit is also referred to as the "other structural unit," and the monomer from which the other structural unit is derived is also referred to as the "other monomer"). Examples of the other monomer include (meth)acrylates such as glycidyl (meth)acrylate; di(meth)acrylates such as ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, and polyethylene glycol di(meth)acrylate; and acrylamides such as (meth)acrylamide, hydroxyethyl (meth)acrylamide, hydroxymethyl (meth)acrylamide, dimethyl (meth)acrylamide, diethyl (meth)acrylamide, N-methyl (meth)acrylamide, dimethylaminopropyl (meth)acrylamide, and isopropyl (meth)acrylamide. These monomers may be used alone or in combination of two or more.
[0028] The resin layer (A) preferably further contains the structural unit (b1), and more preferably further contains the structural unit (a3) and other structural units. When the resin layer (A) contains the structural unit (a2) but does not contain the structural unit (a1), the resin layer (A) preferably further contains the structural unit (b1), and more preferably further contains other structural units.
[0029] The content of the structural unit (a1) or (a2) in the resin layer (A) (when the resin layer (A) contains both the structural units (a1) and (a2), this refers to the structural unit with the largest content; the same applies hereinafter) is preferably 1 mol % or more, more preferably 3 mol % or more, and even more preferably 5 mol % or more, relative to all structural units in the resin layer (A). The upper limit is usually 90 mol % or less, preferably 70 mol % or less, more preferably 50 mol % or less, and even more preferably 30 mol % or less. The above upper and lower limits can be combined arbitrarily. For example, it may be 1 to 90 mol %, 1 to 70 mol %, 3 to 50 mol %, or 5 to 30 mol %. If the content is 1 mol % or more, the anionic drug or cationic drug will be loaded in large amounts, and if it is 90 mol % or less, the release effect tends to be better.
[0030] When the resin layer (A) contains the structural unit (b1), the molar ratio of the structural unit (a1) or (a2) to the structural unit (b1) in the resin layer (A) is preferably 1 / 99 to 50 / 50, more preferably 3 / 97 to 30 / 70, and even more preferably 5 / 95 to 20 / 80. When this molar ratio is 1 / 99 to 50 / 50, the balance between the sustained release of the anionic or cationic drug and shape stability tends to be better.
[0031] When the resin layer (A) contains the structural unit (a3), the molar ratio of the structural unit (a1) or (a2) to the structural unit (a3) in the resin layer (A) is preferably 10 / 90 to 90 / 10, more preferably 30 / 70 to 70 / 30, and even more preferably 40 / 60 to 60 / 40. When this molar ratio is 10 / 90 or higher, the effect of supporting and releasing anionic or cationic drugs tends to be better, while when it is 90 / 10 or lower, the effect of inhibiting protein adhesion tends to be better.
[0032] The thickness of the thickest part of the resin layer (A) is 1 μm or more. When the thickness of the thickest part is 1 μm or more, excellent sustained release of the drug is achieved. The thickness of the thickest part of the resin layer (A) is preferably 5 μm or more, more preferably 20 μm or more, even more preferably 50 μm or more, and particularly preferably 100 μm or more. The thickness of the thickest part of the resin layer (A) is usually 1000 μm or less, preferably 500 μm or less. The above upper and lower limits can be arbitrarily combined. For example, it may be 1 to 1000 μm, 5 to 1000 μm, 20 to 1000 μm, 50 to 500 μm, or 100 to 500 μm.
[0033] <Resin Layer (B)> The resin layer (B) may contain the structural unit (a1) or (a2). When the resin layer (B) contains the structural unit (a1) or (a2), the content of at least one of them is 1 / 2 or less of the content of the structural unit (a1) or (a2) in the resin layer (A). It is preferable that the content of both the structural units (a1) and (a2) is 1 / 2 or less of the respective contents in the resin layer (A). The resin layer (B) may not contain the structural unit (a1) or (a2). In that case, the ratio of the content of the structural unit (a1) in the resin layer (A) to the content of the structural unit (a1) or (a2) in the resin layer (B) becomes infinite, that is, 2 or more.
[0034] The content of the structural unit (a1) or (a2) in the resin layer (B) is preferably 10 mol% or less, more preferably 5 mol% or less, and even more preferably 1 mol% or less, relative to all structural units in the resin layer (B). The resin layer (B) may not contain any structural unit (a1) or (a2), but the lower limit is usually 0.001 mol% or more, preferably 0.01 mol% or more, and more preferably 0.1 mol% or more. A content of 10 mol% or less tends to provide excellent shape stability. The above upper and lower limits can be arbitrarily combined. For example, it may be 0.001 to 10 mol%, 0.01 to 5 mol%, or 0.1 to 1 mol%.
[0035] The resin layer (B) may further contain one or more of a structural unit (b1) derived from a monomer having a hydroxyl group, a structural unit (a3) derived from a monomer having an amphoteric ionic group, and other structural units. The resin layer (B) preferably contains the structural unit (b1).
[0036] When the resin layer (A) contains the structural unit (a1) but does not contain the structural unit (a2), the resin layer (B) preferably contains the structural unit (b1) and the structural unit (a2), and more preferably further contains other structural units. When the resin layer (A) contains the structural unit (a2) but does not contain the structural unit (a1), the resin layer (B) preferably contains the structural unit (b1) and other structural units.
[0037] The content of the structural unit (b1) relative to all structural units in the resin layer (B) is preferably 30 mol% or more, more preferably 50 mol% or more, and even more preferably 70 mol% or more. The upper limit of the content of the structural unit (b1) is usually 99 mol% or less, and preferably 98 mol% or less. If the content of the structural unit (b1) is 30 mol% or more, the wearability of the ophthalmic medical device tends to be excellent. The above upper and lower limits can be combined in any way. For example, it may be 30 to 99 mol%, 50 to 99 mol%, or 70 to 98 mol%.
[0038] The resin layer (B) may be a resin known to be used in ophthalmic medical devices. The resin layer (B) may be an acrylic resin. The resin layer (B) may be a hydrogel. A "hydrogel" is a structure having a network structure formed by physical or chemical crosslinking of polymer molecular chains, which swells by absorbing water into the network structure. When the resin having hydroxyl groups is a hydrogel, it is easy to carry a drug. The resin layer (B) may be molded into the shape of the ophthalmic medical device. The thickness of the resin layer (B) is not particularly limited, but is, for example, 50 to 500 μm.
[0039] The resin layer (B) may be a commercially available product or may be manufactured by a known method. A commercially available contact lens may be used as the resin layer (B) preformed into the shape of the ophthalmic medical device. Examples of commercially available contact lenses include polyvinyl alcohol-based, silicone methacrylate-based, fluorine methacrylate-based, silicone hydrogel-based, glycerol methacrylate-based, N,N-dimethylacrylamide-based, and hydroxyethyl methacrylate (hereinafter also referred to as "HEMA")-based lenses.
[0040] <Drug> The ophthalmic medical device may contain a drug. When the ophthalmic medical device contains a drug, all of the resin layers constituting the ophthalmic medical device may contain the drug, or only some of the resin layers constituting the ophthalmic medical device may contain the drug.
[0041] The drug is not particularly limited and can be appropriately selected from known drugs depending on the disease to be treated. The drug may be, for example, a nucleic acid, a protein, a carbohydrate (such as a polysaccharide), another organic compound, an inorganic compound, or a combination of two or more of these.
[0042] Examples of drugs used for ophthalmic diseases include anti-infective agents (antibacterial agents, antiviral agents, antifungal agents, antiprotozoal agents, etc.), angiogenesis inhibitors (anti-vascular endothelial growth factor (VEGF) agents, etc.), anti-inflammatory agents, ocular hypotensive agents, anti-cancer agents, anesthetics, autonomic nervous system agents, steroids (corticosteroids, etc.), antihistamines, mast cell stabilizers, immunosuppressants, and mitotic inhibitors.
[0043] Examples of antibacterial agents include bacitracin, chloramphenicol, ciprofloxacin, erythromycin, moxifloxacin, gatifloxacin, gentamicin, levofloxacin, sulfacetamide, polymyxin B, vancomycin, tobramycin, or a combination thereof. Examples of antiviral agents include trifluridine, vidarabine, acyclovir, valacyclovir, famciclovir, foscarnet, ganciclovir, formivirsen, cidofovir, or a combination thereof. Examples of antifungal agents include amphotericin B, natamycin, fluconazole, itraconazole, ketoconazole, miconazole, or a combination thereof. Antiprotozoal agents include, for example, polymyxin B, neomycin, clotrimazole, miconazole, ketoconazole, propamidine, polyhexamethylene biguanide, chlorhexidine, itraconazole, or a combination thereof. Anti-inflammatory agents include, for example, any known steroidal anti-inflammatory drug (SAID), any known non-steroidal anti-inflammatory drug (NSAID), or a combination thereof. SAIDs include, for example, glucocorticoids such as dexamethasone, prednisolone, fluorometholone, loteprednol, medrysone, and rimexolone. NSAIDs include, for example, diclofenac, flurbiprofen, ketorolac, bromofenac, nepafenac, or a combination thereof. Antineoplastic agents include chemotherapeutic agents well known in the art. Anesthetic agents include, for example, aminoamides, aminoesters, or a combination thereof. Aminoamides include, for example, lidocaine, prilocaine, mepivacaine, ropivacaine, or a combination thereof. Aminoesters include, for example, benzocaine, procaine, proparacaine, tetracaine, or a combination thereof.Examples of autonomic nervous system drugs include acetylcholine, carbachol, pilocarpine, physostigmine, echothiophate, atropine, scopolamine, homotrapine, cyclopentolate, tropicamide, dipivefrin, epinephrine, phenylephrine, apraclonidine, brimonidine, cocaine, hydroxyamphetamine, naphazoline, tetrahydrozoline, dapiprazole, betaxolol, carteolol, levobunolol, metipranolol, timolol, bepotastine besilate, or a combination thereof. Examples of antihistamine drugs include pheniramine, antazoline, naphazoline, emedastine, levocarbastine, cromolyn, or a combination thereof. Mast cell stabilizers include, for example, lodoxamide, pemirolast, nedocromil, olopatadine, ketotifen, azelastine, epinastine, or combinations thereof.
[0044] As the drug, an anionic drug, an amphoteric drug or a cationic drug is preferred because it is easily adsorbed to the acrylic resin and the release thereof is easily controlled.
[0045] Anionic drugs are drugs that have an anionic group and exhibit a negative charge in water, such as nucleic acids, tranilast, azazolast hydrate, sodium cromoglycate, glutathione, pranoprofen, bromfenac sodium, diclofenac sodium, bevotastine besilate, or a combination thereof.
[0046] As the nucleic acid of drug, for example, antisense oligonucleotide can be mentioned.Antisense oligonucleotide is also called antisense nucleic acid, and refers to the single-stranded oligonucleotide that comprises the transcription product of target gene or at least a part of the target transcription product that can hybridize (i.e., complementary) base sequence, and can suppress the expression of the transcription product of target gene or the level of the target transcription product mainly by antisense effect.
[0047] The target gene or target transcript whose expression is suppressed, altered, or modified by the antisense effect is not particularly limited, but examples include genes derived from the organism into which the nucleic acid complex is introduced, such as genes whose expression is increased in various diseases. Furthermore, the transcript of the target gene is mRNA transcribed from genomic DNA encoding the target gene, and also includes mRNA that has not undergone base modification and unprocessed mRNA precursors. The target transcript may include not only mRNA but also non-coding RNA (ncRNA) such as miRNA. More generally, the transcript may be any RNA synthesized by a DNA-dependent RNA polymerase. In one embodiment, the target transcript may be, for example, metastasis associated lung adenocarcinoma transcript 1 (malat1) non-coding RNA, scavenger receptor B1 (SR-B1) mRNA, or dystrophia myotonica-protein kinase (DMPK) mRNA. The nucleotide sequences of genes and transcripts can be obtained from publicly known databases, such as the NCBI (National Center for Biotechnology Information) database. Anionic drugs may be used in combination with other drugs.
[0048] Amphoteric drugs are drugs that have anionic and cationic groups and have zero charge in water.The ophthalmic drug olopatadine has a single positively charged tertiary amine group and a single negatively charged carboxylic acid group, so it is considered to have a net charge of zero.Examples of amphoteric drugs include levocabastine hydrochloride, amlexanox, olopatadine, lomefloxacin hydrochloride, ofloxacin, norfloxacin, levofloxacin, tosufloxacin, pirenoxine, rapamycin, or combinations thereof.Amphoteric drugs can also be used in combination with other drugs.
[0049] A cationic drug is a drug that has a cationic group and exhibits a positive charge in water. The cationic drug may be a cationic polymer. Examples of cationic polymers include epsilon polylysine (εPLL) and polyquat, which are antibacterial peptides containing multiple arginine and / or lysine groups. The cationic drug may be a drug containing a guanidinium group. Drugs containing at least one guanidinium group include antihistamines such as epinastine and emedastine; glaucoma drugs such as apraclonidine and brimonidine; guanine derivative antivirals such as ganciclovir and valganciclovir; arginine-containing antibacterial peptides such as defensin and indolicidin; and biguanide antibacterial agents such as chlorhexidine, alexidine, and polyhexamethylene biguanide (PHMB). Other cationic drugs include ketotifen, cationic steroids, neostigmine methylsulfate, oxybuprocaine hydrochloride, naphazoline nitrate, naphazoline hydrochloride, sodium chondroitin sulfate, pilocarpine hydrochloride, distigmine bromide, echothiopate iodide, epinepherine, epinepherine bitartrate, carteolol hydrochloride, befunolol hydrochloride, and ripasudil. Cationic drugs may be used in combination with other drugs.
[0050] When the ophthalmic medical device contains a drug, the drug is preferably released when the device is immersed in phosphate buffered saline containing 2% by mass of sodium chloride (NaCl). If the drug is released in the phosphate buffered saline, the drug can be released under in vivo conditions, making the device useful as an ophthalmic medical device.
[0051] Furthermore, the total amount of drug released when the ophthalmic medical device is immersed in the phosphate buffered saline for 24 hours (hereinafter also referred to as "24-hour release amount") is preferably at least twice, more preferably at least six times, even more preferably at least 10 times, and preferably not more than 1000 times, more preferably not more than 500 times, and even more preferably not more than 100 times. If the 24-hour release amount is at least twice the amount released after 15 minutes, the sustained release of the drug when worn for 24 hours is excellent. If the 24-hour release amount is not more than 1000 times the amount released after 15 minutes, the early drug release is excellent. The above upper and lower limits can be combined arbitrarily. For example, it may be 2 to 1000 times, 6 to 500 times, or 10 to 100 times.
[0052] <Method for Manufacturing Ophthalmic Medical Device> One example of a method for manufacturing the ophthalmic medical device of the present invention includes a method comprising: polymerizing a monomer mixture containing at least one monomer selected from the group consisting of monomers having a cationic group (excluding monomers having a zwitterionic group) and monomers having an anionic group (excluding monomers having a zwitterionic group) by irradiation with active energy rays in the presence of a photopolymerization initiator to form a resin layer (A); and polymerizing a monomer mixture containing a monomer having a hydroxyl group on the resin layer (A), in contact with the resin layer (A), or via another resin layer, to form a resin layer (B). By polymerizing in two stages in this manner, an ophthalmic medical device can be obtained having resin layers (A) and (B) with different contents of the structural unit (a1) or (a2).
[0053] The monomer mixture for forming the resin layer (A) may further contain one or more of a monomer having a hydroxyl group, a monomer having a zwitterionic group, and other monomers. The monomer mixture for forming the resin layer (B) may further contain one or more of a monomer having a cationic group, a monomer having an anionic group, a monomer having a zwitterionic group, and other monomers.
[0054] The content of the monomer having a cationic group or the monomer having an anionic group in the monomer mixture for forming the resin layer (A), and the content of the monomer having a cationic group or the monomer having an anionic group in the monomer mixture for forming the resin layer (B) are each adjusted in accordance with the content ratio of the structural unit (a1) or (a2) described above.
[0055] As the polymerization method, known methods can be used, such as thermal polymerization by heating, photopolymerization by irradiating with active energy rays such as ultraviolet rays, and a combination of these.
[0056] The first-stage polymerization to form the resin layer (A) is preferably carried out by irradiating the monomer mixture with active energy rays in the presence of a photopolymerization initiator. When thermal polymerization is employed, the temperature is gradually raised from near room temperature and heat is applied to a temperature range of 30 to 120°C for several minutes to several hours. In typical thermal polymerization, unreacted monomers having cationic groups or monomers having anionic groups during the first-stage polymerization are mixed in during the second-stage polymerization to form the resin layer (B), which tends to increase the content of the structural unit (a1) or (a2) in the resin layer (B) and reduce the difference in the ratio with the content in the resin layer (A). On the other hand, carrying out the first-stage polymerization by irradiating active energy rays in the presence of a photopolymerization initiator is preferred because it can suppress the generation of unreacted monomers.
[0057] The second-stage polymerization for forming the resin layer (B) is also preferably carried out by irradiating active energy rays in the presence of a photopolymerization initiator. By irradiating active energy rays in the presence of a photopolymerization initiator, the polymerization time can be shortened, and migration of unreacted monomers having cationic groups or monomers having anionic groups in the resin layer (A) to the resin layer (B) can be suppressed. Examples of active energy rays include ultraviolet rays and electron beams. Examples of photopolymerization initiators include alkylphenone initiators and acylphosphine oxide initiators.
[0058] During polymerization, the monomer mixture and, if necessary, a photopolymerization initiator are poured into a mold and polymerization is carried out, whereby the resin layer (A) or the resin layer (B) having the desired shape can be formed.
[0059] When the ophthalmic medical device is a contact lens, a monomer mixture is injected between the male mold and the female mold, and polymerized by applying heat or irradiating with active energy rays. The same mold may be used for the first and second polymerization stages, or different molds may be used for both the male mold and the female mold. By using the same mold only for the male mold, specifically, without removing the polymerized resin layer (A) attached to the male mold after the first polymerization stage from the male mold, a female mold with a larger gap between the male mold and the female mold than the first stage is used to inject the mixed monomers that form the substrate, and polymerize them between the male mold with the resin layer (A), contact lenses in which the resin layer (A) and the resin layer (B) have different contents of the structural unit (a1) or (a2) can be efficiently produced.
[0060] Another method for producing the ophthalmic medical device of the present invention includes a method in which a monomer mixture containing at least one monomer selected from the group consisting of monomers having a cationic group (excluding monomers having a zwitterionic group) and monomers having an anionic group (excluding monomers having a zwitterionic group) is polymerized by irradiating active energy rays in the presence of a photopolymerization initiator on or in contact with resin layer (B) containing structural unit (b1) derived from a monomer having a hydroxyl group, or via another resin layer, to form resin layer (A).
[0061] In the case where the resin layer (B) is formed first and then the monomer mixture for forming the resin layer (A) is polymerized to form the resin layer (A), if the polymerization of the monomer mixture is carried out by thermal polymerization, it takes a long time to form the resin layer (A), and the produced ophthalmic medical device tends to swell significantly in phosphate buffered saline, resulting in poor shape stability, possibly because a monomer having a cationic group or a monomer having an anionic group is impregnated into the resin layer (B) to form a polymer having a cationic group or an anionic group in the resin layer (B). Therefore, it is preferable to polymerize the monomer mixture for forming the resin layer (A) by irradiation with active energy rays in the presence of a photopolymerization initiator.
[0062] If necessary, the resulting ophthalmic medical device is impregnated with a drug, for example, by immersing the ophthalmic medical device in an aqueous solution of the drug.
[0063] The present invention will be explained in more detail below with reference to examples and comparative examples, but the present invention is not limited to these examples in any way.
[0064] Example 1 Preparation of a Two-Layer Contact Lens As monomers for forming the resin layer (A), 9 parts by mass of trimethyl(3-methacryloylaminopropyl)ammonium chloride, a monomer having a cationic group, 82% by mass of 2-hydroxyethyl methacrylate, a monomer having a hydroxyl group, 9 parts by mass of [[2-(methacryloyloxy)ethyl](dimethyl)ammonio]acetate, a monomer having a zwitterionic group, 0.4 parts by mass of polyethylene glycol dimethacrylate (n=4), another monomer, and 0.2 parts by mass of 2-hydroxy-2-methyl-1-phenylpropan-1-one as a photopolymerization initiator were added and mixed. In polyethylene glycol dimethacrylate (n=4), n represents the number of repeating units of the ethylene glycol chain (the same applies hereinafter). 0.1 mL of this mixture was added between a polypropylene male mold A and a female mold B (DIA 11 mm, B.C. (base curve) 8.2 mm, center thickness 0.2 mm), and the mixture was irradiated with ultraviolet light (365 nm, 140 mW) for 2 minutes to form a resin layer (A) located on the surface of the contact lens. When the molds were separated, the resin layer (A) was found to be attached to the male mold A. As monomers for forming the resin layer (B), 97.6 parts by mass of 2-hydroxyethyl methacrylate, a hydroxyl group-containing monomer, 2.4 parts by mass of methacrylic acid, a monomer having an anionic group, 0.4 parts by mass of polyethylene glycol dimethacrylate (n=4), another monomer, and 0.2 parts by mass of 2-hydroxy-2-methyl-1-phenylpropan-1-one, a photopolymerization initiator, were added and mixed. 0.1 mL of this mixture was added to a polypropylene female mold C, and the mixture was mated with the male mold A to which the resin layer (A) was attached. The distance between the male mold A and the female mold C was 11 mm in diameter, 8.2 mm in base curve (BC), and 0.3 mm in center thickness. The lens was irradiated with ultraviolet light (365 nm, 140 mW) for 2 minutes to form a resin layer (B). This resulted in a contact lens having a resin layer (A) with a maximum thickness of 200 μm and a resin layer (B) with a maximum thickness of 100 μm.
[0065] Comparative Example 1 The contact lens of Comparative Example 1 was a contact lens (a commercially available HEMA-based hydrogel contact lens) made of a uniform resin component that did not contain the structural unit (a1) or the structural unit (a2), but contained a structural unit (b1) derived from a monomer having a hydroxyl group.
[0066] (Comparative Example 2) <Preparation of a Single-Layer Contact Lens> A contact lens (commercially available HEMA-based hydrogel contact lens) that did not contain the structural unit (a1) or the structural unit (a2) but contained a structural unit (b1) derived from a monomer having a hydroxyl group was placed in a centrifuge tube and washed twice with pure water, then washed five times in ethanol, and further immersed in ethanol for 20 minutes to replace the water content in the contact lens with ethanol. The ethanol-treated contact lens was added to a mixed solution of 15 mL of dehydrated ethanol and 144 μL of 3-methacryloyloxypropyltrimethoxysilane and allowed to react at room temperature for 24 hours to obtain an acrylate-modified contact lens. After the reaction, the contact lens was thoroughly washed with ethanol. A monomer having a cationic group and a monomer having a zwitterionic group were dissolved in dehydrated ethanol in a molar ratio of 50:50 to a total monomer concentration of 0.5 mol / L to obtain a monomer solution. Trimethyl(3-methacryloylaminopropylammonium chloride was used as the monomer having a cationic group, and [[2-(methacryloyloxy)ethyl](dimethyl)ammonio]acetate was used as the monomer having a zwitterionic group. An acrylate-modified contact lens was immersed in 100 mL of the monomer solution, and 0.5 mol % azobisisobutyronitrile relative to the total monomers was added. The temperature was raised to 75°C while bubbling with nitrogen, and polymerization was carried out for 24 hours. The contact lens was then removed and washed thoroughly with ethanol, and then washed with pure water to remove the ethanol. A contact lens made of a resin component in which cationic groups were uniformly distributed was obtained.
[0067] Example 2 Preparation of a Two-Layer Contact Lens As monomers for forming the resin layer (A), 5 parts by mass of methacryloyloxyethyl acid phosphate, a monomer having an anionic group, 95 parts by mass of 2-hydroxyethyl methacrylate, a monomer having a hydroxyl group, 0.4 parts by mass of polyethylene glycol dimethacrylate (n=4), another monomer, and 0.2 parts by mass of 2-hydroxy-2-methyl-1-phenylpropan-1-one, a photopolymerization initiator, were mixed together. 0.1 mL of this mixture was added between a polypropylene male mold A and a female mold B (DIA 11 mm, B.C. (base curve) 8.2 mm, center thickness 0.2 mm), and ultraviolet light (365 nm, 140 mW) was applied for 2 minutes to form the resin layer (A) located on the surface of the contact lens. When the molds were separated, the resin layer (A) was found to be attached to the male mold A. As the monomer for forming the resin layer (B), 100 parts by mass of the hydroxyl group-containing monomer 2-hydroxyethyl methacrylate, 0.4 parts by mass of another monomer, polyethylene glycol dimethacrylate (n = 4), and 0.2 parts by mass of 2-hydroxy-2-methyl-1-phenylpropan-1-one as a photopolymerization initiator were mixed together. 0.1 mL of this mixture was added to a polypropylene female mold C, and the male mold A with the resin layer (A) attached was mated with it. The distance between the male mold A and the female mold C was 11 mm, B.C. (base curve) 8.2 mm, and center thickness 0.3 mm. The resin layer (B) was formed by irradiating with ultraviolet light (365 nm, 140 mW) for 2 minutes. This resulted in a contact lens having a resin layer (A) with a thickness of 200 μm at its thickest portion and a resin layer (B) with a thickness of 100 μm at its thickest portion.
[0068] (Comparative Example 3) As monomers for forming a contact lens, 99 parts by mass of 2-hydroxyethyl methacrylate, a monomer having a hydroxyl group, 1 part by mass of methacrylic acid, a monomer having an anionic group, 0.4 parts by mass of polyethylene glycol dimethacrylate (n=4), another monomer, and 0.2 parts by mass of 2-hydroxy-2-methyl-1-phenylpropan-1-one, a photopolymerization initiator, were mixed together. 0.1 mL of this mixture was placed between a polypropylene male mold A and a female mold B (DIA 11 mm, B.C. (base curve) 8.2 mm, center thickness 0.2 mm), and the mixture was irradiated with ultraviolet light (365 nm, 140 mW) for 2 minutes. This resulted in a contact lens made of a resin component in which anionic groups were uniformly distributed.
[0069] Example 3 Preparation of a Two-Layer Contact Lens As monomers for forming the resin layer (A), 15 parts by mass of a 75% aqueous solution of N-(2-acryloyloxyethyl)-N-benzyl-N,N-dimethylammonium chloride, which is a monomer having a cationic group, 70 parts by mass of 2-hydroxyethyl methacrylate, which is a monomer having a hydroxyl group, 15 parts by mass of [[2-(methacryloyloxy)ethyl](dimethyl)ammonio]acetate, which is a monomer having a zwitterionic group, 0.96 parts by mass of polyethylene glycol dimethacrylate (n=14), which is another monomer, and 0.2 parts by mass of 2-hydroxy-2-methyl-1-phenylpropan-1-one, which is a photopolymerization initiator, were added and mixed. 0.1 mL of this reaction solution was added between a polypropylene male mold A and a female mold B (DIA 11 mm, B.C. (base curve) 8.2 mm, center thickness 0.2 mm), and ultraviolet light (365 nm, 140 mW) was applied for 2 minutes to form a resin layer (A) located on the surface of the contact lens. When the molds were separated, the resin layer (A) was found to be attached to the male mold A. As monomers for forming the resin layer (B), 97.6 parts by mass of 2-hydroxyethyl methacrylate, a monomer having a hydroxyl group, 2.4 parts by mass of methacrylic acid, a monomer having an anionic group, 0.4 parts by mass of ethylene glycol dimethacrylate, another monomer, and 0.2 parts by mass of 2-hydroxy-2-methyl-1-phenylpropan-1-one, a photopolymerization initiator, were added and mixed. 0.1 mL of this mixture was added to a polypropylene female mold C, and this was mated with the male mold A to which the resin layer (A) was attached. The space between the male mold A and the female mold C had a DIA of 11 mm, B.C. The lens had a base curve of 8.2 mm and a center thickness of 0.3 mm. The lens was irradiated with ultraviolet light (365 nm, 140 mW) for 2 minutes to form a resin layer (B). This resulted in a contact lens having a resin layer (A) with a maximum thickness of 200 μm and a resin layer (B) with a maximum thickness of 100 μm.
[0070] Example 4 To 100 parts by mass of a mixture of 9 parts by mass of trimethyl(3-methacryloylaminopropyl)ammonium chloride, a monomer having a cationic group, 82 parts by mass of 2-hydroxyethyl methacrylate, a monomer having a hydroxyl group, and 9 parts by mass of [[2-(methacryloyloxy)ethyl](dimethyl)ammonio]acetate, a monomer having a zwitterionic group, as monomers for forming the resin layer (A), 10 parts by mass of water and 10 parts by mass of ethanol were added, and 0.4 parts by mass of polyethylene glycol dimethacrylate (n=4), as another monomer, and 0.2 parts by mass of 2-hydroxy-2-methyl-1-phenylpropan-1-one, as a photopolymerization initiator, were added and mixed. 0.1 mL of this reaction solution was added between a polypropylene male mold A and a female mold B (DIA 11 mm, B.C. (base curve) 8.2 mm, center thickness 0.2 mm), and ultraviolet light (365 nm, 140 mW) was applied for 2 minutes to form a resin layer (A) located on the surface of the contact lens. When the molds were separated, the resin layer (A) was found to be attached to the male mold A. As monomers for forming the resin layer (B), 97.6 parts by mass of 2-hydroxyethyl methacrylate, a monomer having a hydroxyl group, 2.4 parts by mass of methacrylic acid, a monomer having an anionic group, 0.4 parts by mass of ethylene glycol dimethacrylate, another monomer, and 0.2 parts by mass of 2-hydroxy-2-methyl-1-phenylpropan-1-one, a photopolymerization initiator, were added and mixed. 0.1 mL of this mixture was added to a polypropylene female mold C, and this was mated with the male mold A to which the resin layer (A) was attached. The space between the male mold A and the female mold C had a DIA of 11 mm, B.C. The lens had a base curve of 8.2 mm and a center thickness of 0.3 mm. The lens was irradiated with ultraviolet light (365 nm, 140 mW) for 2 minutes to form a resin layer (B). This resulted in a contact lens having a resin layer (A) with a maximum thickness of 200 μm and a resin layer (B) with a maximum thickness of 100 μm.
[0071] (Measurement and Evaluation) The contact lenses of each example were subjected to the following measurements and evaluations.
[0072] <Measurement of the magnification of the content of structural units (a1) and (a2) in resin layer (A) and resin layer (B)> The contact lenses of Examples 1 and 2 and Comparative Examples 1 to 3 were each dried, and ion mass spectrometry was performed on the cross section of the contact lens. The contact lens was sandwiched between two sheets of ultraviolet-curable resin (Chemiseal U-2904D), embedded using UV light, and subjected to ion mass spectrometry using a microtome to expose the surface and cross section passing through the center, and ion mass spectrometry was performed on the resin layer (A) and the resin layer (B). The ion mass spectrometry was performed using a time-of-flight secondary ion mass spectrometer (ToF-SIMS M6 manufactured by ION-TOF). For Example 1 and Comparative Examples 1 and 2, primary ions Bi 3 2+ Acceleration voltage: 30 kV, probe current: approximately 0.07 pA, positive and negative secondary ion collection, measurement range: 500, 200 μm square scanning (beam scanning), 30 scans integration, C 7 H 12 NO + and C 2 H 3 + The intensity of the primary ions Bi was measured, and the content ratio of the structural unit (a1) was calculated using the following formula (1). 3 2+ Acceleration voltage: 30 kV, probe current: approximately 0.07 pA, positive and negative secondary ion collection, measurement range: 500, 200 μm square scanning (beam scanning), 30 scans integration, PO 4 H 2 - and C 2 H - The strength of the resin layer (A) was measured, and the ratio of the content of the structural unit (a1) was calculated using the following formula (2). 7 H 12 NO + Strength of resin layer (A) / (C 2 H 3 + Strength of resin layer (B) / (C 7 H 12 NO + Strength of resin layer (B) / (C 2 H 3 +Ratio of the content of the structural unit (a2) = ((PO of the resin layer (A)) 4 H 2 - Strength of resin layer (A) / (C 2 H - Strength of resin layer (B) / (PO 4 H 2 - Strength of resin layer (B) / (C 2 H - (Intensity of) ... (2) The results are shown in Table 1. Figures 1 and 2 show ToF-SIMS ion images of the cross sections of the contact lenses of Examples 1 and 2, respectively. In Figure 1, the higher the concentration of cationic groups derived from trimethyl(3-methacryloylaminopropyl)ammonium chloride, the brighter the color tone. In Figure 2, the higher the concentration of anionic groups derived from methacryloyloxyethyl acid phosphate, the brighter the color tone.
[0073] <Preparation of Drug-Loaded Contact Lens 1> Each of the contact lenses of Example 1 and Comparative Examples 1 and 2 was immersed for 24 hours in 2 mL of a 1 mg / mL aqueous solution of a nucleic acid as a model drug to obtain drug-loaded contact lens 1. The nucleic acid used was a Malat1 antisense oligonucleotide represented by CdsTdsAdsGdsTdsTdsCdsAdsCdsTdsGdsAdsTdsGdsCd (wherein the nucleic acid bases are represented by A = adenine, T = thymine, G = guanine, and C = cytosine, the sugar moieties are represented by d = 2'-deoxyribose, and the internucleoside bond is represented by s = phosphorothioate).
[0074] <Sustained Release Test 1> The drug-containing contact lens 1 was placed in a 24-well cell culture plate, and 1000 μL of phosphate-buffered saline (PBS) containing NaCl to adjust the NaCl concentration to 2% by mass was added. After standing at 37°C for 15 minutes, the entire amount of PBS was collected. Next, 1000 μL of PBS containing NaCl was added, and after standing at 37°C for 15 minutes (30 minutes in total), the entire amount of PBS was collected. Next, 1000 μL of PBS containing NaCl was added, and after standing at 37°C for 30 minutes (1 hour in total), the entire amount of PBS was collected. Thereafter, the addition of PBS containing NaCl, standing at 37°C for 1 hour, 4 hours, 8 hours, and 24 hours in total, and the entire amount of PBS was collected were repeated.
[0075] <Measurement 1 of cumulative release amount> In the sustained release test 1, the PBS samples collected 15 minutes, 30 minutes, 1 hour, 4 hours, 8 hours, and 24 hours after the initial addition of PBS are used as measurement samples, and a gradient is applied using 0.1M triethyleneamine aqueous solution and 0.1M triethylamine 50% acetonitrile / aqueous solution by HPLC [Agilent Technologies], and the absorbance at a wavelength of 260 nm is measured, and the drug concentration is determined using a calibration curve prepared in advance, and the cumulative release amount (μg) up to each time is calculated. The results are shown in Table 1.
[0076] <Preparation of Drug-Loaded Contact Lens 2> The contact lens of Example 1 was immersed for 24 hours in 2 mL of a 1 mg / mL aqueous solution of bepotastine besilate, a low molecular weight anionic drug, as a model drug, to obtain drug-loaded contact lens 2.
[0077] <Sustained Release Test 2> The drug-containing contact lens 2 was subjected to a sustained release test similar to the sustained release test 1 above.
[0078] <Measurement of cumulative release amount 2> In the sustained release test 2, PBS samples were collected 15 minutes, 30 minutes, 1 hour, 4 hours, 8 hours, and 24 hours after the initial addition of PBS, and used as measurement samples. The absorbance at a wavelength of 262 nm was measured using a spectrophotometer [JASCO V-750 spectrophotometer, manufactured by Jusco Engineering Co., Ltd.], the drug concentration was determined using a calibration curve prepared in advance, and the cumulative amount of elution (μg) up to each time point was calculated.
[0079] <Preparation of Drug-Loaded Contact Lens 3> Each of the contact lenses of Example 2 and Comparative Example 3 was immersed for 24 hours in 1 mL of a 1 mg / mL aqueous solution of ripasudil hydrochloride hydrate (4-Fluoro-5-{[(2S)-2-methyl-1,4-diazepan-1-yl]sulfonyl}isoquinoline monohydrochloride dihydrate), a low molecular weight cationic drug, to obtain drug-loaded contact lens 3.
[0080] <Sustained Release Test 3> The drug-containing contact lens 3 was subjected to a sustained release test similar to the sustained release test 1 above.
[0081] <Measurement of cumulative release amount 3> In the sustained release test 3, PBS samples were collected 15 minutes, 30 minutes, 1 hour, 4 hours, 8 hours, and 24 hours after the initial addition of PBS. These samples were used as measurement samples, and their absorbance at a wavelength of 279 nm was measured using a spectrophotometer [JASCO V-750 spectrophotometer manufactured by Jusco Engineering Co., Ltd.]. The drug concentration was determined using a calibration curve prepared in advance, and the cumulative release amount (μg) up to each time point was calculated. The results are shown in Table 1.
[0082] <Evaluation of Shape Stability of Contact Lenses> Each of the contact lenses of Examples 1 and 2 and Comparative Examples 1 to 3 was immersed in phosphate-buffered saline for 24 hours to fully hydrate them, after which the liquid on the surface was removed with filter paper and their masses (mass before drying) were measured. The contact lenses were then placed in a dryer at 105°C for 3 hours to dry them, and their masses (mass after drying) were measured. The water content at saturation was calculated from the measurement results using the following formula: Water content = {(mass before drying) - (mass after drying)} / (mass before drying) x 100 Furthermore, the ratio of the water content of the contact lens of each example to the water content of the contact lens of Comparative Example 1 (a commercially available HEMA-based hydrogel contact lens) was calculated as the swelling degree using the following formula. The results are shown in Table 1. Swelling degree = (water content of contact lens of each example) / (water content of contact lens of Comparative Example 1)
[0083] <Animal Experiments> (1) Animal Experiment Protocol A test was conducted to evaluate the sustained release of nucleic acid drugs from contact lenses using 15- to 16-week-old rabbits (Japanese White (Kbl: JW)). The contact lenses used were those of Examples 1, 3, and 4, each having a resin layer (A) and a resin layer (B), and were sterilized in an autoclave (120°C, 2 atmospheres, 20 minutes). A control group was also included. The nucleic acid drug used was antisense oligonucleotide (ASO sequence 1) (G(s)^T(s)^5(s)^a^t^a^a^c^c^t^g^g^t^T(s)^5(s)^A(s), lowercase: DNA, uppercase: ALNA[Ms], ^: PS bond). Drug-containing contact lenses were obtained by immersion in 2 mL of a 1 mg / mL aqueous solution of the nucleic acid drug for 24 hours. In the contact lens group, on the day of contact lens wear (Day 1), the upper and lower eyelids of each rabbit's left and right eyes were gently pinched up, and a contact lens containing the test substance was placed in the space between the eyelid and the eyeball using tweezers or the like, bringing it into contact with the eyeball. The wearing condition was continuously observed for 8 hours from the start of wear, and the condition was recorded every hour. After 8 hours of wear, the test substance was removed from all animals. In the eye drop group, 50 μL of eye drop solution (PBS) was administered twice daily to each eye for 5 days (days 1 to 5). After administration, the upper and lower eyelids were gently brought together and held for approximately 1 second to prevent leakage of the test substance. For tear collection, tear samples were collected from the left eye of all animals in the contact lens wear group using Schirmer test paper 3 minutes, 15 minutes, 1 hour, 3 hours, 8 hours, and 24 hours after wear. In the instillation group, tear fluid was collected from the left eye of all animals using Schirmer test strips 3 minutes, 15 minutes, 1 hour, and 3 hours after the first instillation. The collected tear fluid was transferred to a sample cup and stored in a -80°C freezer. For eyeball sampling, after the final observation for eye irritation (day 4 or 8), the animals were deeply anesthetized with 2% propofol administered intravenously through the auricular vein (1.5 mL / kg) and the abdominal aorta and vein were cut to exsanguinate the animals. The left eye was then enucleated and frozen on dry ice. After freezing, the cornea was sampled. The sampled ocular tissue (cornea) was transferred to a container and stored in a -80°C freezer.
[0084] (2) Measurement of Nucleic Acid Drug Content in Tears and Corneas. A guanidine hydrochloride-containing buffer was added to Schirmer test paper containing tear samples, followed by the addition of zirconia beads and disruption using a mixer mill. The disrupted solution was centrifuged at room temperature and shaken for 30 minutes at room temperature to prepare a homogenate. The resulting homogenate was centrifuged at 4°C, and the supernatant was collected in a sample tube and mixed with a 25:24:1 (mass ratio) mixture of phenol, chloroform, and isoamyl alcohol. A 5% aqueous ammonia solution was then added and mixed, and the mixture was allowed to stand at room temperature (23°C) before being centrifuged at 4°C. The supernatant was evaporated to dryness using nitrogen and then redissolved in DEPC (diethylpyrocarbonate)-treated water. The resulting solution was stored in a -80°C freezer until use. The corneal sample was transferred to a dedicated disruption tube, refrozen at -80°C for a certain period, and disrupted using a multi-beads shocker. After disruption, a proteinase K-containing buffer was added depending on the corneal mass for protein cleavage. The resulting homogenate was stored in a -80°C freezer until use. The content of nucleic acid drugs (ASO sequence 1 concentration) in tears and corneas was measured using hybridization-ELISA. The samples prepared as described above (lysate obtained from tear samples or homogenate obtained from corneal samples) were mixed with a solution of a DNA sequence (template DNA) complementary to digoxigenin-biotin-labeled ASO sequence 1 and stirred at 37°C for 1 hour for hybridization. S1 nuclease solution was added to the mixture and stirred at 37°C for 2 hours to cleave unhybridized nucleic acids. The reaction solution was added to a streptavidin plate and washed, followed by the addition of an alkaline phosphatase-modified anti-digoxigenin antibody solution and the reaction was allowed to proceed for 30 minutes at 37°C. After washing, AttoPhos AP Fluorescent Substrate (Promega) was added, and the fluorescence intensity was measured using a plate reader (excitation: 440 nm, emission: 535 nm).The fluorescence intensity of the blank sample (a sample obtained from a group not administered with a drug (untreated or eye drop group)) was subtracted from the obtained fluorescence intensity, and the calibration curve samples were subjected to nonlinear regression with a 4-parameter logistic curve using analysis software (Fusion (registered trademark) Data Analysis Software / PerkinElmer). The concentration of ASO sequence 1 contained in the sample was back-calculated from the regression equation of the calibration curve. Furthermore, the content of the nucleic acid drug in the tears and cornea was calculated by multiplying the back-calculated ASO sequence 1 concentration by the dilution rate of the homogenate. The results are shown in Table 2.
[0085]
[0086] In Table 1, the "ratio of the content of the structural unit (a1) or (a2)" indicates the ratio of the content of the structural unit (a1) for Example 1, and the ratio of the content of the structural unit (a2) for Example 2. In Table 1, the ToF-SIMS intensity ratios for Example 1 and Comparative Examples 1 and 2 are 7 H 12 NO + and C 2 H 3 + The ratio of (C 7 H 12 NO + / C 2 H 3 + The ToF-SIMS intensity ratios in Example 2 and Comparative Example 3 are 4 H 2 - and C 2 H - Ratio to (PO 4 H 2 - / C 2 H - )
[0087] As shown in Table 1, the contact lenses of Examples 1 and 2 gradually eluted the drug in the sustained-release test, demonstrating excellent sustained-release properties, a water content equivalent to that of the contact lens of Comparative Example 1 at saturation, and excellent shape stability. In contrast, the commercially available hydrogel contact lens of Comparative Example 1 did not adsorb the drug because it did not contain cationic groups, and no drug elution was observed. The contact lens of Comparative Example 2, which was made of a resin component with uniformly distributed cationic groups, demonstrated sustained drug release, but it was confirmed that its water content at saturation was higher and its degree of swelling was greater than that of the contact lens of Comparative Example 1. This suggests that the shape change due to water absorption was significant, causing shape change during wear and resulting in poor wearability. The contact lens of Comparative Example 3, made of a resin component with uniformly distributed anionic groups, was confirmed to have inferior sustained-release properties, possibly due to the low content of anionic groups near the surface and the low overall anionic group content.
[0088]
[0089] As shown in Table 2, the results of the animal experiments showed that the contact lens wear groups of Examples 1, 3, and 4 all showed a reduced drug release rate into tears (sustained release) compared to the eye drop group. It was also revealed that the amount of drug delivered to the cornea was increased in the contact lens wear group compared to the eye drop group. From the above, it was demonstrated that sustained drug release using contact lenses increases and sustains drug exposure, making it a useful technology for enhancing the effectiveness of ophthalmic pharmaceuticals.
[0090] According to the present invention, an ophthalmic medical device having excellent sustained release properties, high shape stability, and excellent wearability, and a method for producing the same can be provided.
Claims
1. An ophthalmic medical device comprising a resin layer (A) and a resin layer (B), wherein at least a portion of the surface of the ophthalmic medical device is formed by the resin layer (A), the resin layer (A) has a thickness of 1 μm or more at its thickest part, the resin layer (A) comprises at least one structural unit selected from the group consisting of a structural unit (a1) derived from a monomer having a cationic group (excluding monomers having a zwitterionic group) and a structural unit (a2) derived from a monomer having an anionic group (excluding monomers having a zwitterionic group), and the resin layer (A) and the resin layer (B) satisfy either one or both of the following relationships (1) and (2). (1) The content of the structural unit (a1) in the resin layer (A) / The content of the structural unit (a1) in the resin layer (B) ≧2.0 (2) The content of the structural unit (a2) in the resin layer (A) / The content of the structural unit (a2) in the resin layer (B) ≧2.0 2. The ophthalmic medical device according to claim 1, wherein the resin layer (B) contains a structural unit (b1) derived from a monomer having a hydroxyl group.
3. The ophthalmic medical device according to claim 1 or 2, wherein the resin layer (A) contains a structural unit (a3) derived from a monomer having a zwitterionic group.
4. An ophthalmic medical instrument according to claim 1 or 2, wherein a part of the surface of the ophthalmic medical instrument that comes into contact with the eyeball is formed by said resin layer (A).
5. The ophthalmic medical device according to claim 1 or 2, which is a medical contact lens.
6. An ophthalmic medical device according to claim 1 or 2, which contains a drug.
7. The ophthalmic medical device according to claim 6, wherein the drug is released when immersed in phosphate buffered saline containing 2% by weight sodium chloride.
8. A method for producing an ophthalmic medical device according to claim 1 or 2, comprising: forming the resin layer (A) by polymerization of a monomer mixture containing at least one monomer selected from the group consisting of a monomer having a cationic group (excluding monomers having a zwitterionic group) and a monomer having an anionic group (excluding monomers having a zwitterionic group) by irradiation with active energy rays in the presence of a photopolymerization initiator; and forming the resin layer (B) on the resin layer (A) by polymerization of a monomer mixture containing a monomer having a hydroxyl group, in contact with the resin layer (A) or via another resin layer.
9. A method for producing an ophthalmic medical device according to claim 1 or 2, comprising forming the resin layer (A) by polymerization of a monomer mixture containing at least one monomer selected from the group consisting of monomers having a cationic group (excluding monomers having a zwitterionic group) and monomers having an anionic group (excluding monomers having a zwitterionic group) on the resin layer (B) containing a structural unit (b1) derived from a monomer having a hydroxyl group, by irradiating the resin layer (B) with active energy rays in the presence of a photopolymerization initiator, either in contact with the resin layer (B) or via another resin layer.
Citation Information
Patent Citations
Hydrogel soft contact lens material containing betaine zwitter-ion and preparation method of hydrogel soft contact lens material
CN107118300A
Drug-loaded anti-adhesion contact lens hydrogel material and preparation method thereof
CN112795030A
Method of manufacturing contact lens for extended releasing medicine visual acuity correction and extended releasing medicine agent
JP1999024010A
Medicine sustained release ocular lens
JP2004305313A
Diffusion-controlled coatings in medical devices
JP2004535227A