Semiconductor encapsulation release film

The semiconductor encapsulation release film with a lubricant or surfactant in its surface layer and specific diiodomethane contact angle addresses the issue of flow marks, ensuring high productivity and low-cost production with enhanced surface uniformity and mold releasability.

WO2024203992A1PCT designated stage expired Publication Date: 2024-10-03MITSUI CHEM ICT MATERIA INC
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/011559
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-29
Filing Date
2024-03-25
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Conventional semiconductor encapsulation release films are insufficient in suppressing flow marks during the molding process, particularly in compression and transfer molding, and increasing surface roughness or elastic modulus can lead to deterioration in laser mark visibility and mold release performance.

Method used

A semiconductor encapsulation release film with a surface layer containing 0.1% to 10% by mass of a lubricant or surfactant, preferably a fatty acid amide-based lubricant or fluorine-based surfactant, and a diiodomethane contact angle of 60° to 70°, which effectively impedes resin flow and prevents flow marks without compromising mold releasability.

Benefits of technology

The film effectively suppresses flow marks on molded products while maintaining high mold releasability, enabling easy release and cost-effective production with improved surface uniformity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024011559_03102024_PF_FP_ABST
    Figure JP2024011559_03102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention addresses the problem of providing a semiconductor encapsulation release film capable of not only easily releasing a molded article after resin encapsulation regardless of mold structure, etc., but also effectively suppressing the occurrence of flow marks. This problem is solved by a semiconductor encapsulation release film wherein the semiconductor encapsulation release film has a surface layer that contains 0.1-10 mass% of a lubricant or a surfactant relative to the weight of the surface layer of the semiconductor encapsulation release film. The problem is also solved by a semiconductor encapsulation release film that has a surface layer having a diiodomethane contact angle of 60-70° as measured after heating at 175°C for 10 seconds.
Need to check novelty before this filing date? Find Prior Art

Description

Semiconductor encapsulation release film

[0001] The present invention relates to a process release film, preferably a semiconductor encapsulation release film used in a semiconductor encapsulation process, and in particular to a semiconductor encapsulation release film that is placed between a semiconductor chip or the like and the inner surface of a mold when a semiconductor chip or the like is placed in the mold and resin is injected and molded.

[0002] In recent years, efforts to reduce the size and weight of semiconductor packages and the like have led to the development of a method for reducing the amount of encapsulating resin used. Therefore, in order to ensure strong adhesion at the interface between the semiconductor chip and the resin even when the amount of encapsulating resin used is reduced, it is desirable to reduce the amount of release agent contained in the encapsulating resin. Therefore, a method for ensuring releasability between the encapsulating resin and the mold after curing and molding has been adopted, in which a release film (semiconductor encapsulation release film) is disposed between the inner surface of the mold and the semiconductor chip.

[0003] In semiconductor encapsulation processes using such semiconductor encapsulation release films, it is possible to easily release the encapsulant of the semiconductor package from the mold when molding the semiconductor package with resin. However, traces of the flow of the encapsulating resin, so-called flow marks, may appear on the surface of the molded package. Flow marks are particularly likely to appear when using liquid resin in compression molding or in transfer molding. Furthermore, as the molding method in BGA and WL-CSP systems has shifted from the conventional transfer molding method to the compression molding method, the size of each shot has become larger, and the requirements for uniformity in the surface appearance of the molded package, flow marks of the encapsulant, etc. have become higher.

[0004] In response to this, it has been proposed to improve the flow marks by increasing the surface roughness of the semiconductor encapsulation release film (Patent Documents 1 and 2), and it has also been proposed to improve the flow marks by increasing the elastic modulus of the surface of the semiconductor encapsulation release film (Patent Document 3).

[0005] JP 2016-92272 A International Publication No. 2016 / 093178 A1 International Publication No. 2019 / 131163 A1

[0006] However, when the surface roughness of a semiconductor-encapsulating release film increases, laser mark visibility may deteriorate. Furthermore, when the elastic modulus of the surface of a semiconductor-encapsulating release film increases, the surface portion with a high elastic modulus may crack when the film is made to conform to a mold, or the release layer on the surface may be easily torn. Furthermore, conventional semiconductor-encapsulating release films have been insufficient in suppressing the occurrence of flow marks.

[0007] The present invention has been made in consideration of the above circumstances, and aims to provide a semiconductor encapsulation release film that not only allows molded products after resin encapsulation to be easily released without relying on mold structure, etc., but also effectively suppresses the occurrence of flow marks.

[0008] As a result of intensive research to solve the above problems, the present inventors have found that the generation of flow marks can be suppressed by adding a specific amount of lubricant or surfactant to the surface layer of a semiconductor-encapsulating release film, and further found that the generation of flow marks can be suppressed by having a diiodomethane contact angle within a specific range, thereby completing the present invention. That is, the present invention and its respective aspects are as described in the following [1] to [6].

[0009] [1] A semiconductor-encapsulating release film having a surface layer containing 0.1% by mass to 10% by mass of a lubricant or a surfactant, based on the weight of the surface layer of the semiconductor-encapsulating release film. [2] The semiconductor-encapsulating release film according to [1], wherein the lubricant contains a fatty acid amide-based lubricant. [3] The semiconductor-encapsulating release film according to [1], wherein the surfactant contains a fluorine-based surfactant. [4] A semiconductor-encapsulating release film having a surface layer having a diiodomethane contact angle of 60° to 70° measured after heating at 175°C for 10 seconds. [5] The semiconductor-encapsulating release film according to [1] or [4], wherein the surface layer contains a 4-methyl-1-pentene (co)polymer. [6] The semiconductor-encapsulating release film according to [5], which is used in a semiconductor encapsulation process using an encapsulating resin containing an epoxy resin.

[0010] The semiconductor encapsulation release film of the present invention can effectively suppress the occurrence of flow marks without impairing the releasability of conventional semiconductor encapsulation release films. Therefore, by using this film, molded products obtained by resin-encapsulating semiconductor chips and the like can be easily released from the mold, and molded products without flow marks can be produced with high productivity and low cost.

[0011] Fig. 1 is a schematic diagram showing an example of a semiconductor encapsulation process using the semiconductor encapsulation release film of the present invention. Fig. 2 is a schematic diagram showing an example of a semiconductor encapsulation process using the semiconductor encapsulation release film of the present invention. Fig. 3 is a schematic diagram showing an example of a semiconductor encapsulation process using the semiconductor encapsulation release film of the present invention. Fig. 4 is a schematic diagram showing an example of a semiconductor encapsulation process using the semiconductor encapsulation release film of the present invention. Fig. 5 is a schematic diagram showing methods for evaluating flow marks and releasability in the examples. Fig. 6 is a schematic diagram showing methods for evaluating flow marks and releasability in the examples.

[0012] Semiconductor-Encapsulating Release Film The semiconductor-encapsulating release film of the present invention has a surface layer containing 0.1% by mass to 10% by mass of a lubricant or surfactant, based on the weight of the surface layer of the semiconductor-encapsulating release film.

[0013] The semiconductor encapsulating release film of the present invention is a film consisting of a single layer or multiple layers, and the surface layer refers to the single layer film itself when the semiconductor encapsulating release film consists of a single layer, or to the outermost layer of the layers constituting the film when the semiconductor encapsulating release film consists of multiple layers, which is the layer that comes into direct contact with the encapsulating resin in the semiconductor encapsulation process.

[0014] By including a lubricant or a surfactant, when the molten encapsulating resin flows during molding in the semiconductor encapsulation process, the semiconductor encapsulation release film, which comes into direct contact with the encapsulating resin, does not hinder the flow of the encapsulating resin. As a result, the encapsulating resin spreads evenly to cover the semiconductor chip, which is thought to prevent the generation of flow marks.

[0015] The content of the lubricant or surfactant contained in the surface layer of the semiconductor-encapsulating release film of the present invention is 0.1% by mass to 10% by mass, based on the weight of the surface layer of the semiconductor-encapsulating release film. This content may be preferably 0.2% by mass to 7% by mass, and more preferably 0.5% to 5% by mass. A content of 0.1% by mass or more can effectively suppress the occurrence of flow marks. A content of 10% by mass or less can allow the semiconductor-encapsulating release film itself to have an appropriate composition, thereby preventing impairment of releasability.

[0016] The temperature of the molding die in the semiconductor encapsulation process is about 110° C. to 190° C., and the lubricant or surfactant that can be used in the semiconductor encapsulation release film of the present invention is preferably stable at the above temperature.

[0017] Lubricant The lubricant in the present invention includes paraffin and hydrocarbon resins, fatty acids, fatty acid amides, fatty acid esters, fatty alcohols, partial esters of fatty acids and polyhydric alcohols, and composite lubricants.

[0018] Examples of the paraffin and hydrocarbon resins include paraffin wax, microcrystalline wax, liquid paraffin, paraffin-based synthetic wax, polyethylene wax, polypropylene wax, montan wax, hydrocarbon-based wax, and silicone oil.

[0019] Examples of the fatty acids include stearic acid, hydroxystearic acid, complex stearic acid, and hardened oil.

[0020] Examples of the fatty acid amides include stearamide, oxystearamide, oleylamide, erucylamide, laurylamide, palmitylamide, behenamide, methylolamide, monoamides of higher fatty acids, methylene bisstearamide, ethylene bisstearamide, ethylene bisoleylamide, ethylene bilaurylamide, bisamides of higher fatty acids, stearyl oleylamide, N-stearyl erucamide, N-oleyl palmitamide, and special fatty acid amides. Furthermore, examples of the fatty acid amide-based lubricants that may be used include ethylenediamine-stearic acid-sebacic acid polycondensates.

[0021] Examples of the fatty acid ester include n-butyl stearate, polyhydric alcohol fatty acid ester, saturated fatty acid ester, special fatty acid ester, and aromatic alcohol fatty acid ester.

[0022] Examples of the fatty alcohol include higher alcohols.

[0023] Examples of the partial esters of fatty acids and polyhydric alcohols include glycerin fatty acid esters and hydroxystearic acid triglycerides.

[0024] Examples of the composite lubricant include distearyl epoxy hexahydrophthalate, sodium alkyl sulfate, long-chain aliphatic compounds, nonionic ester surfactants, block copolymers of ethylene oxide and propylene oxide, and fine powder of tetrafluoroethylene resin.

[0025] The lubricant is preferably a fatty acid amide-based lubricant. Examples of fatty acid amide-based lubricants include EBS, and commercially available products such as Kaowax (registered trademark) series (manufactured by Kao Corporation), Light Amide (registered trademark) series (manufactured by Kyoeisha Chemical Co., Ltd.), and BA (manufactured by Dai-Nippon Chemical Co., Ltd.) may also be used.

[0026] Surfactant Examples of the surfactant in the present invention include silicone surfactants, fluorine surfactants, amphoteric surfactants, nonionic surfactants, and anionic surfactants.

[0027] Examples of the silicone surfactant include side-chain modified polydimethylsiloxane, both-end modified polydimethylsiloxane, one-end modified polydimethylsiloxane, and both-end modified polydimethylsiloxane of side chain, and those having a polyoxyethylene group or a polyoxyethylene polyoxypropylene group as a modifying group are particularly preferred because they exhibit good properties as an aqueous surfactant. Furthermore, polyether-modified silicone surfactants can also be used as the silicone surfactant, and examples thereof include compounds in which a polyalkylene oxide structure is introduced into the Si part side chain of dimethylsiloxane.

[0028] Examples of the fluorosurfactants include perfluoroalkyl sulfonic acid compounds, perfluoroalkyl carboxylic acid compounds, perfluoroalkyl phosphate ester compounds, perfluoroalkyl ethylene oxide adducts, and polyoxyalkylene ether polymer compounds having a perfluoroalkyl ether group on the side chain. Examples of the perfluoroalkyl sulfonic acid compounds include perfluoroalkyl sulfonic acid and perfluoroalkyl sulfonate salts. Examples of the perfluoroalkyl carboxylic acid compounds include perfluoroalkyl carboxylic acids and perfluoroalkyl carboxylate salts. Examples of the polyoxyalkylene ether polymer compounds having a perfluoroalkyl ether group on the side chain include sulfate ester salts of polyoxyalkylene ether polymers having a perfluoroalkyl ether group on the side chain, and salts of polyoxyalkylene ether polymers having a perfluoroalkyl ether group on the side chain. Counterions of the salts in these fluorosurfactants include Li, Na, K, NH 4 , N.H. 3 CH 2 CH 2 OH, NH 2 (CH 2 CH 2 OH) 2 , NH(CH 2 CH 2 OH) 3The fluorosurfactant may be a polymerizable fluorosurfactant, and in particular may be a polymerizable fluorosurfactant containing a polyfluoroalkyl group having 6 or less carbon atoms.

[0029] Examples of the amphoteric surfactant include lauryl aminopropionate, lauryl dimethyl betaine, stearyl dimethyl betaine, and lauryl dihydroxyethyl betaine.

[0030] Examples of the nonionic surfactants include polyoxyethylene alkylphenyl ethers, polyoxyethylene alkyl esters, polyoxyethylene alkylamines, polyoxyethylene alkylamides, polyoxyethylene propylene block polymers, sorbitan fatty acid esters, polyoxyethylene sorbitan fatty acid esters, and ethylene oxide adducts of acetylene alcohol.

[0031] Examples of the anionic surfactant include polyoxyethylene alkyl ether acetates, dodecylbenzenesulfonates, laurates, and salts of polyoxyethylene alkyl ether sulfates.

[0032] The surfactant is preferably a fluorine-based surfactant. Examples of the fluorine-based surfactant that can be used include commercially available products such as the Megafac (registered trademark) series (manufactured by DIC Corporation), the Fluorad series (manufactured by Sumitomo 3M Limited), the Surflon (registered trademark) series (manufactured by AGC Seimi Chemical Co., Ltd.), the Asahi Guard (registered trademark) series (manufactured by AGC Corporation), the EF series (manufactured by Shin-Akita Chemical Co., Ltd.), and the Polyfox series (manufactured by Omnova Solutions).

[0033] The fluorosurfactant preferably has a hexane solubility of 5 wt % or more. The higher the hexane solubility, the better the compatibility with the resin constituting the surface layer. When other additives are added, the additives are more easily dispersed, and the additives are more likely to exhibit their effects. Furthermore, the fluorosurfactant is required to have heat resistance sufficient to prevent decomposition by heat applied in the manufacturing process of the semiconductor encapsulation release film. The fluorosurfactant preferably has a 10% weight loss temperature of 220°C or higher as measured by TG. The 10% weight loss temperature as measured by TG is more preferably 250°C or higher, and even more preferably 270°C or higher. From the viewpoint of adequate bleeding to the surface, the melting point of the fluorosurfactant is preferably 30°C or higher, and more preferably 40°C or higher.

[0034] Surface Layer The surface layer is not particularly limited as long as it is a layer that is commonly used in semiconductor encapsulation release films, but it preferably contains a resin selected from the group consisting of 4-methyl-1-pentene (co)polymers, fluororesins, and polystyrene-based resins.

[0035] The 4-methyl-1-pentene (co)polymer that can be used in the surface layer may be a homopolymer of 4-methyl-1-pentene, or may be a copolymer of 4-methyl-1-pentene and another olefin having 2 to 20 carbon atoms (hereinafter referred to as "olefin having 2 to 20 carbon atoms").

[0036] In the case of a copolymer of 4-methyl-1-pentene and an olefin having 2 to 20 carbon atoms, the olefin having 2 to 20 carbon atoms copolymerized with the 4-methyl-1-pentene can impart flexibility to the 4-methyl-1-pentene. Examples of the olefin having 2 to 20 carbon atoms include ethylene, propylene, 1-butene, 1-hexene, 1-heptene, 1-octene, 1-decene, 1-tetradecene, 1-hexadecene, 1-heptadecene, 1-octadecene, 1-eicosene, etc. These olefins may be used alone or in combination of two or more.

[0037] In the case of a copolymer of 4-methyl-1-pentene and an olefin having 2 to 20 carbon atoms, it is preferable that the proportion of structural units derived from 4-methyl-1-pentene is 96% by weight to 99% by weight, and the proportion of other structural units derived from olefins having 2 to 20 carbon atoms is 1% by weight to 4% by weight. Reducing the content of structural units derived from olefins having 2 to 20 carbon atoms makes it possible to harden the copolymer, which is advantageous for suppressing the occurrence of wrinkles during sealing processes, etc. On the other hand, increasing the content of structural units derived from olefins having 2 to 20 carbon atoms makes it possible to soften the copolymer, which is advantageous for improving mold conformability.

[0038] The 4-methyl-1-pentene (co)polymer can be produced by methods known to those skilled in the art. For example, it can be produced by a method using a known catalyst such as a Ziegler-Natta catalyst or a metallocene catalyst. The 4-methyl-1-pentene (co)polymer is preferably a (co)polymer with high crystallinity. The crystalline copolymer may be either a copolymer having an isotactic structure or a copolymer having a syndiotactic structure, but a copolymer having an isotactic structure is particularly preferred in terms of physical properties and is also easily available. Furthermore, the stereoregularity and molecular weight of the 4-methyl-1-pentene (co)polymer are not particularly limited as long as it can be molded into a film and has the strength to withstand the temperature, pressure, etc., during mold molding. The 4-methyl-1-pentene copolymer may be a commercially available copolymer such as TPX (registered trademark) (manufactured by Mitsui Chemicals, Inc.).

[0039] The fluororesin that can be used for the surface layer may be a resin containing structural units derived from tetrafluoroethylene. It may be a homopolymer of tetrafluoroethylene, but it may also be a copolymer with other olefins. Examples of other olefins include ethylene. A copolymer containing tetrafluoroethylene and ethylene as monomer structural units is a preferred example, and in such a copolymer, the proportion of structural units derived from tetrafluoroethylene is preferably 55% by weight to 100% by weight, and the proportion of structural units derived from ethylene is preferably 0% by weight to 45% by weight.

[0040] The polystyrene-based resins that can be used for the surface layer include styrene homopolymers and copolymers, and the styrene-derived structural units contained in the polymer preferably account for at least 60% by weight, more preferably 80% by weight or more.

[0041] The polystyrene resin may be either isotactic polystyrene or syndiotactic polystyrene, but isotactic polystyrene is preferred from the viewpoint of ease of availability, etc., and syndiotactic polystyrene is preferred from the viewpoint of mold releasability, heat resistance, etc. One type of polystyrene may be used alone, or two or more types may be used in combination.

[0042] The surface layer may further contain other resins in addition to the fluororesin, 4-methyl-1-pentene copolymer, and / or polystyrene-based resin. In this case, it is preferable that the other resins have a relatively high hardness. Examples of the other resins include polyamide-6, polyamide-66, polybutylene terephthalate, and polyethylene terephthalate. In this way, even when the release layer A contains a large amount of soft resin (for example, when the 4-methyl-1-pentene copolymer contains a large amount of olefin having 2 to 20 carbon atoms), the surface layer can be made hard by further containing a resin with a relatively high hardness.

[0043] The content of these other resins is preferably, for example, 3% by weight to 30% by weight of the resin components constituting the surface layer. By making the content of the other resins 3% by weight or more, the effect of adding them can be substantial, and by making the content 30% by weight or less, the releasability from the mold and the molded product can be maintained.

[0044] Furthermore, in addition to the 4-methyl-1-pentene (co)polymer, fluororesin, and / or polystyrene-based resin, the surface layer may contain known additives that are generally blended into resins for films, such as a heat stabilizer, a weather stabilizer, a rust inhibitor, a copper-resistant stabilizer, an antistatic agent, etc., within a range that does not impair the object of the present invention. The content of these additives can be, for example, 0.0001 to 10 parts by weight per 100 parts by weight of the fluororesin, 4-methyl-1-pentene copolymer, and / or polystyrene-based resin.

[0045] The surface layer preferably has a contact angle with water (water contact angle) of 90° to 130°, more preferably 95° to 120°, even more preferably 98° to 115°, and particularly preferably 100° to 110°.

[0046] In one embodiment, the surface layer has a contact angle with diiodomethane (diiodomethane contact angle) of 60° to 70°, preferably 61.5° to 69.5°, and more preferably 62.0° to 69.0°.

[0047] In measuring the diiodomethane contact angle, it is preferable to take into consideration the conditions under which the semiconductor encapsulation release film is heated in a typical semiconductor encapsulation process. In the semiconductor encapsulation process, compression molding is performed at a temperature of about 110°C to 190°C, and the semiconductor encapsulation release film and mold are heated before compression. The diiodomethane contact angle of the surface layer can be measured after heating at a temperature of 175°C or higher for 10 seconds or longer. The heating temperature and heating time under these measurement conditions may be higher or longer as long as they are within the ranges typically used in semiconductor encapsulation processes.

[0048] The surface layer preferably has heat resistance capable of withstanding the temperature of the mold during molding (typically 110°C to 190°C). From this perspective, the surface layer preferably contains a crystalline resin having a crystalline component. The melting point of the crystalline resin does not necessarily have to be equal to or higher than the maximum temperature of the mold during molding, but is preferably 200°C or higher, and more preferably 200°C to 300°C. The melting point can be measured by thermal analysis (DSC method), but if multiple melting peaks are detected, the melting point is determined from the melting peak with the highest temperature.

[0049] In order to impart crystallinity to the surface layer, for example, a 4-methyl-1-pentene (co)polymer preferably contains at least a structural unit derived from 4-methyl-1-pentene, a fluororesin preferably contains at least a structural unit derived from tetrafluoroethylene, and a polystyrene resin preferably contains at least syndiotactic polystyrene.

[0050] When the semiconductor encapsulating release film is composed of a single layer, the thickness of the surface layer, which is the single-layer film itself, is 10 μm to 300 μm, preferably 30 μm to 150 μm. A semiconductor encapsulating release film having a thickness within the above range is preferable because it provides good handleability when used as a roll and reduces the amount of film waste. When the semiconductor encapsulating release film is composed of multiple layers, the thickness of the surface layer is not particularly limited as long as it provides sufficient releasability for molded products, but is usually 1 μm to 50 μm, preferably 5 μm to 30 μm.

[0051] The surface layer may have an uneven shape as needed, thereby improving the mold releasability. The method for imparting unevenness to the surface layer is not particularly limited, but a general method such as embossing can be used.

[0052] When the semiconductor-encapsulating release film of the present invention is a film consisting of multiple layers, the semiconductor-encapsulating release film may have any layer in addition to the surface layer, such as a substrate layer, a mold-side release layer, a gas barrier layer, a protective resin layer, an adhesive layer, etc.

[0053] The substrate layer has a function of supporting the surface layer. The substrate layer is not particularly limited as long as it is a layer that is commonly used in semiconductor encapsulation release films, but is preferably a layer containing one or more resins selected from polyethylene terephthalate, polyethersulfone, polyphenylsulfone, polyarylate, polyetheramide, thermoplastic polyimide, etc.

[0054] The substrate layer may be any resin layer including a non-stretched film, but is particularly preferably a stretched film.

[0055] The stretched film is preferably a stretched film selected from the group consisting of a stretched polyester film, a stretched polyamide film, a stretched polypropylene film, and a stretched polyethylene film.

[0056] As the stretched polyester film, stretched polyethylene terephthalate (PET) film and stretched polybutylene terephthalate (PBT) film are preferred, and biaxially stretched polyethylene terephthalate (PET) film is particularly preferred. There are no particular limitations on the polyamide constituting the stretched polyamide film, but polyamide-6, polyamide-66, etc. can be preferably used. As the stretched polypropylene film, uniaxially stretched polypropylene film, biaxially stretched polypropylene film, etc. can be preferably used. As the stretched polyethylene film, uniaxially stretched polyethylene film, biaxially stretched polyethylene film, etc. can be preferably used.

[0057] From the viewpoint of controlling the strength of the film and its thermal dimensional change rate within an appropriate range, the substrate layer preferably has heat resistance capable of withstanding the temperature of the mold during molding (typically 110°C to 190°C). From this viewpoint, the substrate layer preferably contains a crystalline resin having a crystalline component, and the melting point of the crystalline resin is preferably 100°C or higher, more preferably 140°C to 300°C, even more preferably 150°C to 270°C, and particularly preferably 170°C to 240°C. The melting point does not necessarily have to be higher than the maximum temperature of the mold during molding. Furthermore, the melting point can be measured by thermal analysis (DSC method), but if multiple melting peaks are detected, the melting point is determined from the melting peak with the highest temperature.

[0058] The substrate layer can be made of either an amorphous resin or a crystalline resin, but preferably contains a crystalline resin having a crystalline component as described above. The crystalline resin contained in the substrate layer can be, for example, a polyester resin, a polyamide resin, a polypropylene resin, a polyethylene resin, or other crystalline resin, and can be used in part or in whole. Specifically, it is preferable to use polyethylene terephthalate or polybutylene terephthalate for polyester resins, polyamide-6 or polyamide-66 for polyamide resins, isotactic polypropylene for polypropylene resins, and high-density polyethylene, low-density polyethylene, or linear low-density polyethylene for polyethylene resins.

[0059] The thickness of the substrate layer is not particularly limited as long as the film strength can be ensured, but is usually 1 μm to 100 μm, and preferably 5 μm to 50 μm.

[0060]

[0033] The semiconductor encapsulating release film of the present invention may have a mold-side release layer in addition to the surface layer and the substrate layer. That is, the mold-side release layer is a layer laminated on the opposite side of the surface layer via the substrate layer, and is a layer in contact with the mold.

[0061] The mold-side release layer may be a layer having the same configuration as the surface layer, or may be a layer having a different configuration. From the viewpoints of preventing warping and ease of handling due to the fact that both surfaces have similar release properties, it is preferable that the mold-side release layer has the same or substantially the same configuration as the surface layer. From the viewpoint of optimally designing the surface layer and the mold-side release layer in relation to the process in which they are used, for example, from the viewpoint of making the mold-side release layer excellent in releasability from the mold and the surface layer excellent in peelability from the molded product, it is preferable that the surface layer and the mold-side release layer have different configurations.

[0062] When the surface layer and the mold-side release layer have different configurations, the surface layer and the mold-side release layer may be made of the same material but have different configurations such as thickness, or they may be made of different materials and have different configurations in other respects.

[0063] Gas Barrier Layer The gas barrier layer may be laminated in the semiconductor-encapsulating release film of the present invention to improve the gas barrier properties of the film. The gas barrier layer may be an inorganic layer or an organic layer. From the viewpoints of cost, transparency, heat resistance, etc., an inorganic layer is preferred, and from the viewpoints of adhesion to the substrate and resistance to cracking, etc., an organic layer is preferred. Furthermore, by laminating an inorganic layer and an organic layer, a configuration can be achieved that makes use of the advantages of both.

[0064] There are no particular restrictions on the inorganic material that forms a suitable inorganic layer, as long as it does not react with other layers, does not decompose, and can maintain its layer when heated during molding or the like. However, a material that does not react with other layers, does not decompose, and can maintain its layer even when heated up to 165°C is preferred, and more preferably a material that does not react with other layers, does not decompose, and can maintain its layer even when heated up to 185°C.

[0065] The inorganic layer is preferably a thin film of a metal or an oxide thereof that has been made amorphous (non-crystalline).For example, a thin film of a metal or an oxide thereof that has been made amorphous (non-crystalline) can be used, such as silicon (Si), aluminum (Al), magnesium (Mg), calcium (Ca), potassium (K), tin (Sn), sodium (Na), boron (B), titanium (Ti), lead (Pb), zirconium (Zr), or yttrium (Y).Among the above, aluminum, silicon, their oxides, and combinations thereof are preferred from the viewpoints of gas barrier properties and ease of forming the inorganic layer, and aluminum and its oxides are more preferred from the viewpoints of mold releasability, gas permeability, ease of production, and ductility (ease of stretching).

[0066] Examples of methods for forming the inorganic layer include physical vapor deposition (PVD) methods such as vacuum deposition, sputtering, and ion plating, and chemical vapor deposition (CVD) methods such as plasma chemical vapor deposition, thermal chemical vapor deposition, and photochemical vapor deposition.

[0067] The thickness of the inorganic layer varies depending on the material used, etc., but is typically 5 nm to 200 nm. A thickness of 5 nm or more reduces outgassing permeability, effectively preventing mold contamination and clogging of the vacuum line used for film adsorption. Furthermore, a thickness of 200 nm or less makes it easy to prevent a decrease in mold followability. The thickness of the inorganic layer is preferably 5 nm to 200 nm, more preferably 8 nm to 180 nm, and even more preferably 10 nm to 150 nm. When an aluminum layer is used as the inorganic layer, the thickness is also preferably 5 nm to 200 nm, more preferably 8 nm to 180 nm, and even more preferably 10 nm to 150 nm.

[0068] The organic material forming the organic layer is not particularly limited, but at least one polymer selected from the group consisting of a polymer having a vinyl alcohol unit and a polymer having a vinylidene chloride unit is particularly suitable. The "vinyl alcohol unit" refers to a unit in which the acetoxy group of a vinyl acetate unit is converted to a hydroxyl group by chemically converting a polymer obtained by polymerizing vinyl acetate. The polymer may or may not have a crosslinked structure.

[0069] Alternatively, the organic layer may be formed by heating and curing a mixture of a polycarboxylic acid such as polyacrylic acid or polymethacrylic acid and a polyamine compound such as polyethyleneimine or polyallylimine, etc. In this case, the degree of neutralization is preferably set to 50 to 100 equivalent % in order to prevent gelation of the mixture.

[0070] Protective Resin Layer The protective resin layer is a layer formed to protect the gas barrier layer from external impacts, etc., when the gas barrier layer is made of a metal or a metal oxide. The material of the protective resin layer is not particularly limited as long as it can be formed on the gas barrier layer by a coating method such as application, printing, or dipping, and preferred examples include resins such as urethane resins, melamine resins, acrylic resins, polyvinylidene chloride, ethylene-vinyl alcohol resins, polyvinyl alcohol resins, metal acrylate resins, and crosslinked polyamide resins. Of these, urethane resins, metal acrylate resins, and crosslinked polyamide resins are more preferred, and metal acrylate resins and crosslinked polyamide resins are most preferred.

[0071] Adhesive Layer The adhesive layer is a layer that bonds the surface layer or the mold-side release layer to the base layer, as needed. The material used for the adhesive layer is not particularly limited as long as it can firmly bond the surface layer (or the mold-side release layer) to the base layer and does not peel off during the resin sealing step or the mold release step.

[0072] When the surface layer or the mold-side release layer is bonded to the base layer by the adhesive layer, from the viewpoint of improving the adhesiveness of the surface layer or the mold-side release layer, the surface of the surface layer or the mold-side release layer that comes into contact with the base layer can be subjected to corona treatment. It is preferable that the surface of the surface layer or the mold-side release layer that comes into contact with the base layer be subjected to corona treatment so that the water contact angle based on JIS R3257 of the surface of the surface layer or the mold-side release layer that comes into contact with the base layer is 30° or less.

[0073] When the semiconductor-encapsulating release film is composed of multiple layers, the total thickness of the semiconductor-encapsulating release film is, for example, 10 μm to 300 μm, preferably 15 μm to 150 μm. A total thickness of the semiconductor-encapsulating release film within the above range is preferable because it provides good handling when used as a roll and reduces the amount of film waste. The thickness of each layer constituting the semiconductor-encapsulating release film can be appropriately adjusted within the above total thickness range, as long as the function of each layer is not impaired.

[0074] According to another aspect of the present invention, there is provided a semiconductor-encapsulating release film having a surface layer having a diiodomethane contact angle of 60° to 70° measured after heating at 175° C. for 10 seconds.

[0075] In the semiconductor encapsulation process, the semiconductor encapsulation release film and mold are usually heated to a temperature of about 110°C to 190°C before the semiconductor encapsulation release film and the encapsulating resin come into contact with each other. However, by having the diiodomethane contact angle of the surface layer after heating at 175°C for 10 seconds be 60° to 70°, the fluidity of the semiconductor encapsulation resin is not impaired, and the occurrence of flow marks on the molded product can be effectively suppressed.

[0076] Therefore, the heating temperature and heating time in the measurement conditions may be higher or longer as long as they are within the ranges typically used in semiconductor encapsulation processes.

[0077] The value of the diiodomethane contact angle can be adjusted by adding a lubricant or surfactant to the surface layer. By adding a lubricant or surfactant, the value of the diiodomethane contact angle can be increased. From the viewpoint of making the diiodomethane contact angle 60° or more, the amount of lubricant or surfactant added is preferably 0.1 mass% or more with respect to the weight of the surface layer.

[0078] The surface layer of the semiconductor-encapsulating release film of the present invention can be made of the above-mentioned resin, and preferably a resin containing a 4-methyl-1-pentene (co)polymer. When the semiconductor-encapsulating release film of the present invention is a film consisting of multiple layers, the semiconductor-encapsulating release film may have any of the above-mentioned layers, such as the substrate layer, mold-side release layer, gas barrier layer, protective resin layer, and adhesive layer, in addition to the surface layer.

[0079] The semiconductor encapsulation release film of the present invention can be placed between a semiconductor chip or the like and the inner surface of a mold when a resin is injected into the mold after the semiconductor chip or the like is placed therein. Use of the semiconductor encapsulation release film of the present invention can effectively prevent flow marks from appearing on the surface of the molded product produced.

[0080] 1, 2A, 2B, and 2C are schematic diagrams showing an example of a semiconductor encapsulation process using the semiconductor encapsulation release film of the present invention.

[0081] As shown in FIG. 1a, the semiconductor encapsulating release film 1 of the present invention is supplied from a rolled wound wound by rolls 1-2 and 1-3 into the upper mold 2. Next, the semiconductor encapsulating release film 1 is placed on the inner surface of the upper mold 2. If necessary, the inner surface of the upper mold 2 may be evacuated to allow the semiconductor encapsulating release film 1 to adhere to the inner surface of the upper mold 2. A semiconductor chip 6 placed on a substrate is placed in the lower mold 5 of a molding machine. By placing an encapsulating resin on the semiconductor chip 6 or by injecting a liquid encapsulating resin so as to cover the semiconductor chip 6, the encapsulating resin 4 is accommodated between the upper mold 2 and the lower mold 5 to which the semiconductor encapsulating release film 1 is adhered by exhaust suction. Next, as shown in FIG. 1b, the upper mold 2 and the lower mold 5 are closed with the semiconductor encapsulating release film 1 of the present invention interposed therebetween, and the encapsulating resin 4 is cured.

[0082] As the mold is closed and hardened, the encapsulating resin 4 flows into the mold, and flows into the cavity, filling it so as to surround the side surfaces of the semiconductor chip 6, thereby encapsulating the semiconductor chip 6. As shown in Figure 1c, the upper mold 2 and the lower mold 5 are opened and the encapsulated semiconductor chip 6 is removed. After the mold is opened and the molded product is removed, the semiconductor encapsulating release film 1 can be reused multiple times, or a new semiconductor encapsulating release film can be supplied and the product can be subjected to the next resin molding process.

[0083] The semiconductor encapsulation release film of the present invention is adhered to an upper mold, interposed between the mold and the encapsulating resin, and resin molding is performed, thereby preventing the resin from adhering to the mold, preventing the resin from contaminating the resin molding surface of the mold, and enabling the molded product to be easily released. Note that the release film can be supplied anew for each resin molding operation, or can be supplied anew for each multiple resin molding operations.

[0084] The order of the process of placing the semiconductor encapsulating release film 1 on the inner surface of the molding die 8 and the process of placing the semiconductor chip 6 inside the molding die 8 is not particularly limited, and they may be performed simultaneously, or the semiconductor encapsulating release film may be placed after the semiconductor chip 6 is placed, or the semiconductor encapsulating release film 1 may be placed after the semiconductor chip 6 is placed.

[0085] Furthermore, the method is not limited to the compression molding method shown in FIG. 1 in which a solid sealing resin material 4 is pressurized and heated, but a transfer molding method in which a fluid sealing resin material is injected as will be described later may also be employed.

[0086] 2A, 2B, and 2C are schematic diagrams showing a transfer molding method, which is an example of a method for producing a resin-encapsulated semiconductor using the release film of the present invention.

[0087] 2A , the semiconductor encapsulating release film 22 of the present invention is supplied from a rolled wound material into a molding die 28 by rolls 24 and 26 (step a). Next, the semiconductor encapsulating release film 22 is placed on the inner surface 30A of the upper die 30 (step b). If necessary, the inner surface 30A of the upper die may be evacuated to allow the semiconductor encapsulating release film 22 to adhere tightly to the inner surface 30A of the upper die. Next, a semiconductor chip 34 to be resin-encapsulated (semiconductor chip 34 fixed to a substrate 34A) is placed in the molding die 28, and an encapsulating resin material 36 is set therein (step c), and the die is then clamped (step d).

[0088] 2B , the encapsulating resin material 36 is injected into the molding die 28 under predetermined heating and pressure conditions (step e). The temperature (molding temperature) of the molding die 28 at this time is, for example, 165°C to 185°C, the molding pressure is, for example, 7 MPa to 12 MPa, and the molding time is, for example, about 90 seconds. After maintaining this for a certain period of time, the upper mold 30 and the lower mold 32 are opened, and the resin-encapsulated semiconductor package 40 and the semiconductor encapsulation release film 22 are simultaneously or sequentially released from the molds (step f).

[0089] 2C , by removing excess resin portion 42 from the obtained semiconductor package 40, a desired semiconductor package 44 can be obtained. Although the semiconductor encapsulation release film 22 may be used as is for resin encapsulation of other semiconductor chips, it is preferable to operate the roll to advance the film each time a molding cycle is completed, and to supply new semiconductor encapsulation release film 22 to the molding die 28.

[0090] The order of the process of placing the semiconductor encapsulating release film 22 on the inner surface of the mold 28 and the process of placing the semiconductor chip 34 inside the molding mold 28 is not particularly limited, and they may be performed simultaneously, or the semiconductor encapsulating release film 22 may be placed after the semiconductor chip 34 is placed, or the semiconductor chip 34 may be placed after the semiconductor encapsulating release film 22 is placed.

[0091] The encapsulating resin preferably used in the manufacturing process using the semiconductor encapsulating release film of the present invention is not particularly limited, and may be either a thermoplastic resin or a thermosetting resin, although thermosetting resins are widely used in the technical field. The resin material is also not particularly limited, but epoxy-based resins, polyimide-based resins, silicone encapsulating resins, etc. can be preferably used, and epoxy-based encapsulating resins are particularly preferred.

[0092] An example of an epoxy-based encapsulating resin that is preferably used in a production process using the release film for process of this embodiment is an epoxy resin composition that contains an epoxy resin, a phenolic resin, a curing accelerator, and an inorganic filler.

[0093] The epoxy resin used in the epoxy resin composition generally refers to a monomer, oligomer, or polymer having two or more epoxy groups per molecule. Examples include, but are not limited to, orthocresol novolac epoxy resins, phenol novolac epoxy resins, biphenyl epoxy resins, bisphenol epoxy resins, stilbene epoxy resins, triphenolmethane epoxy resins, phenol aralkyl epoxy resins (including phenylene skeletons, biphenyl skeletons, etc.), naphthol epoxy resins, alkyl-modified triphenolmethane epoxy resins, triazine nucleus-containing epoxy resins, and dicyclopentadiene-modified phenolic epoxy resins. These may be used alone or in combination of two or more. Among these, crystalline epoxy resins are particularly preferred because they have low melt viscosity, can be highly loaded with inorganic fillers, and thus can reduce the moisture absorption of the epoxy resin composition and improve solder crack resistance.

[0094] The phenolic resin used in the epoxy resin composition generally refers to a monomer, oligomer, or polymer having two or more phenolic hydroxyl groups per molecule. Examples include, but are not limited to, phenol novolac resin, cresol novolac resin, phenol aralkyl resin (including a phenylene skeleton, a biphenyl skeleton, or the like), naphthol aralkyl resin (including a phenylene skeleton, a biphenyl skeleton, or the like), triphenolmethane resin, terpene-modified phenolic resin, and dicyclopentadiene-modified phenolic resin. These may be used alone or in combination of two or more.

[0095] The curing accelerator used in the epoxy resin composition refers to a compound that can act as a catalyst for the crosslinking reaction between the epoxy resin and the phenolic resin, and examples thereof include diazabicycloalkenes such as 1,8-diazabicyclo(5,4,0)undecene-7 and derivatives thereof, amine compounds such as tributylamine and benzyldimethylamine, organic phosphorus compounds such as triphenylphosphine and tetraphenylphosphonium tetraphenylborate salts, imidazole compounds such as 2-methylimidazole, etc. These may be used alone or in combination of two or more.

[0096] The type of inorganic filler used in the epoxy resin composition is not particularly limited, and those generally used in sealing materials can be used. Examples include fused silica, crystalline silica, secondary agglomerated silica, alumina, titanium white, aluminum hydroxide, talc, clay, glass fiber, etc., and these may be used alone or in combination of two or more. Fused silica is particularly preferred. Fused silica can be used in either crushed or spherical form, but it is more preferred to mainly use spherical silica in order to increase the blending amount and suppress an increase in the melt viscosity of the epoxy resin composition.

[0097] In addition to the above components, the epoxy resin composition preferably used in the production process using the semiconductor encapsulation release film of this embodiment can also contain various additives, such as inorganic ion exchangers, coupling agents, colorants typified by carbon black, natural waxes, synthetic waxes, higher fatty acids and their metal salts, paraffin, and other mold release agents, brominated epoxy resins, antimony oxide, phosphorus compounds, and other flame retardants, silicone oils, rubber, and other low-stress components, and antioxidants, as needed.

[0098] Manufacturing Method of Semiconductor-Encapsulating Release Film The semiconductor-encapsulating release film of the present invention contains a lubricant or surfactant in its surface layer, and the resin constituting the surface layer can be mixed with the lubricant or surfactant by any method to form a resin for the surface layer.

[0099] As a method for mixing the resin for the surface layer, for example, the resin such as a 4-methyl-1-pentene copolymer, the lubricant or surfactant, and other components can be mixed using a Henschel mixer, a V-type blender, a tumbler blender, a ribbon blender, etc. Alternatively, the blend mixed as described above can be melt-mixed using a single-screw extruder, a multi-screw extruder, a kneader, a Banbury mixer, etc. to obtain a resin composition in which the components are uniformly dispersed and mixed, which can be used as the resin for the surface layer.

[0100] The semiconductor-encapsulating release film of the present invention can be produced by any method. When the semiconductor-encapsulating release film of the present invention is a single layer, the surface layer resin may be mixed and melt-extruded to form a film of a predetermined thickness.

[0101] When the semiconductor-encapsulating release film of the present invention is composed of multiple layers, examples of the method include: 1) a method of manufacturing a semiconductor-encapsulating release film by co-extrusion molding and laminating a surface layer and a base layer (co-extrusion forming method); 2) a method of manufacturing a semiconductor-encapsulating release film by applying and drying a molten resin of a resin that will become the surface layer or adhesive layer onto a film that will become the base layer, or by applying and drying a resin solution in which a resin that will become the surface layer or adhesive layer is dissolved in a solvent, onto the film that will become the base layer (coating method); and 3) a method of manufacturing a semiconductor-encapsulating release film by manufacturing a film that will become the surface layer and a film that will become the base layer in advance and laminating these films (lamination method).

[0102] In the method 3), various known lamination methods can be used to laminate the resin films, such as extrusion lamination, dry lamination, and thermal lamination.

[0103] In the dry lamination method, each resin film is laminated using an adhesive. Any adhesive known for dry lamination can be used. Examples of such adhesives include polyvinyl acetate adhesives; polyacrylic ester adhesives made of homopolymers or copolymers of acrylic esters (ethyl acrylate, butyl acrylate, 2-ethylhexyl acrylate, etc.), or copolymers of acrylic esters and other monomers (methyl methacrylate, acrylonitrile, styrene, etc.); cyanoacrylate adhesives; ethylene copolymer adhesives made of copolymers of ethylene and other monomers (vinyl acetate, ethyl acrylate, acrylic acid, methacrylic acid, etc.); cellulose adhesives; polyester adhesives; Adhesives that can be used include polyamide-based adhesives; polyimide-based adhesives; amino resin-based adhesives made from urea resins or melamine resins; phenolic resin-based adhesives; epoxy-based adhesives; polyurethane-based adhesives crosslinked with polyols (such as polyether polyols and polyester polyols) and isocyanates and / or isocyanurates; reactive (meth)acrylic adhesives; rubber-based adhesives made from chloroprene rubber, nitrile rubber, styrene-butadiene rubber, etc.; silicone-based adhesives; inorganic adhesives made from alkali metal silicates, low-melting-point glass, etc.; and others. The resin film to be laminated in method 3) may be commercially available or may be manufactured by a known manufacturing method. The resin film may be subjected to surface treatments such as corona treatment, atmospheric pressure plasma treatment, vacuum plasma treatment, and primer coating treatment. The method for manufacturing the resin film is not particularly limited, and known manufacturing methods can be used.

[0104] 1) The co-extrusion molding method is preferable because it is less likely to cause defects due to foreign matter getting caught between the resin layer that serves as the surface layer and the resin layer that serves as the base layer, and less likely to cause warping of the semiconductor encapsulation release film. 3) The lamination method is a suitable manufacturing method when a stretched film is used as the base layer. In this case, it is preferable to form an appropriate adhesive layer at the interface between the films as needed. To improve the adhesion between the films, the interface between the films may be subjected to a surface treatment such as corona discharge treatment as needed.

[0105] The coating means in the coating method 2) is not particularly limited, and various coaters such as a roll coater, a die coater, a spray coater, etc. The melt extrusion means is not particularly limited, and an extruder having a T-die or an inflation die, etc., is used.

[0106] The semiconductor encapsulation release film of the present invention can be preferably used not only in processes for resin-encapsulating semiconductor elements, but also in processes for molding and releasing various molded products using a molding die, such as fiber-reinforced plastic molding and release processes, plastic lens molding and release processes, etc.

[0107] As described above, the semiconductor-encapsulating release film of the present invention can effectively suppress the occurrence of flow marks without impairing the releasability of conventional semiconductor-encapsulating release films. Therefore, by using the semiconductor-encapsulating release film of the present invention, molded products obtained by resin-encapsulating semiconductor chips or the like can be easily released from the mold, and molded products free from flow marks can be produced with high productivity and low cost.

[0108] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0109] The sample films of the Examples and Comparative Examples were evaluated by the following methods.

[0110] Measurement of Contact Angle with Diiodomethane (Diiodomethane Contact Angle) A sample film was heated in an oven at 175°C for 10 seconds. After the heat treatment, the sample film was allowed to cool to room temperature, and the diiodomethane contact angle of the surface was measured using a contact angle measuring device (FACECA-W, manufactured by Kyowa Interface Science Co., Ltd.) in accordance with JIS R3257.

[0111] Mold Release and Flow Trace Evaluation Test As shown in Figures 3A and 3B, a lower SUS plate 71, a brass frame 73 with a central 6 x 6 cm cutout, and a mold protection film 61 (a film to prevent the resin from adhering to the evaluation mold) were stacked. Liquid encapsulating resin 50 (product name: R4212-2C, manufactured by Nagase ChemteX Corporation) was placed in the center of the lower SUS plate 71 so that the resin measured approximately 2 x 2 cm when viewed from above (see Figure 3B). After heat treatment at 175°C for 10 seconds, the sample film 60 was placed on an upper SUS plate 72. The sample film 60 and the upper SUS plate 72 were stacked from above so that the sample film 60 (or the surface layer film in the case of a multilayer film) was in contact with the liquid encapsulating resin 50, thereby preparing a laminate 80 for evaluation. The evaluation laminate 80 was placed in a press heated to 175° C. and pressed at a pressure of 0.8 MPa for 90 seconds to compression-mold the liquid sealing resin 50. Thereafter, the upper SUS plate 72, the brass frame 73, and the sample film 60 were peeled off from the evaluation laminate 80.

[0112] In the above test, the releasability of the sample film 60 when the upper SUS plate 72, the brass frame 73, and the sample film 60 were peeled off from the evaluation laminate 80 was evaluated according to the following criteria: ◯: The sample film peeled off easily when pulled by hand (applied tension). ×: The sample film adhered to the sealing resin and could not be peeled off by hand.

[0113] In the above test, the presence or absence of flow marks on the sealing resin after peeling off the upper SUS plate 72, the brass frame 73, and the sample film 60 from the evaluation laminate 80 was evaluated according to the following criteria: ◯: No flow marks are observed visually. ×: Flow marks are observed visually.

[0114] (Kneading) A resin composition was prepared using a 4-methyl-1-pentene copolymer resin (product name: TPX, brand name: MX022, melting point: 229°C) manufactured by Mitsui Chemicals, Inc. and the lubricant or surfactant in the amount shown in Table 1-1 and Table 1-2.

[0115] (Film Formation) The obtained resin composition was melt-extruded at a temperature of 270°C, and the slit width of the T-die was adjusted to obtain a 50 μm-thick surface layer of the sample films of Examples 1 to 11 and Comparative Examples 1 and 2. Similarly, a 15 μm-thick film was molded, and one surface of the film was subjected to corona treatment so that the water contact angle based on JIS R3257 was 30° or less, thereby obtaining a surface layer film to be used for the sample films of Example 12 and Comparative Example 3.

[0116] Example 12 A urethane adhesive was applied by gravure coating to one side of a biaxially stretched PET (polyethylene terephthalate) film (manufactured by Toray Industries, Inc., product name: Lumirror S10) having a thickness of 12 μm at a rate of 1.5 g / m. 2 The corona-treated surface of the surface layer film for Example 12 was then attached by dry lamination, and then 1.5 g / m of a urethane adhesive was applied to the biaxially stretched PET (polyethylene terephthalate) film side of this laminate film. 2 The corona-treated surface of the surface layer film for Comparative Example 3 was then dry laminated to form a mold-side release layer, resulting in a sample film of Example 12 with a five-layer structure (surface layer / adhesive layer / substrate layer / adhesive layer / mold-side release layer). The urethane adhesive used was Takelac A-616 (manufactured by Mitsui Chemicals, Inc.) as the base agent and Takenate A-65 (manufactured by Mitsui Chemicals, Inc.) as the curing agent. The base agent and curing agent were mixed in a mass ratio (base agent:curing agent) of 16:1 and diluted with ethyl acetate. The dry lamination conditions were a substrate width of 900 mm, a conveying speed of 30 m / min, a drying temperature of 50°C to 60°C, a laminating roll temperature of 50°C, and a roll pressure of 3.0 MPa.

[0117] Comparative Example 3: One side of a biaxially stretched PET (polyethylene terephthalate) film (manufactured by Toray Industries, Inc., product name: Lumirror S10) having a thickness of 12 μm was gravure coated with a urethane adhesive at 1.5 g / m 2 The corona-treated surface of the surface layer film for Comparative Example 3 was then attached by dry lamination, and then 1.5 g / m of a urethane adhesive was applied to the biaxially stretched PET (polyethylene terephthalate) film side of this laminate film. 2The corona-treated surface of the surface layer film for Comparative Example 3 was then dry laminated to form a mold-side release layer, resulting in a sample film of Comparative Example 3 with a five-layer structure (surface layer / adhesive layer / substrate layer / adhesive layer / mold-side release layer). The urethane adhesive used was Takelac A-616 (manufactured by Mitsui Chemicals, Inc.) as the base agent and Takenate A-65 (manufactured by Mitsui Chemicals, Inc.) as the curing agent. The base agent and curing agent were mixed in a mass ratio (base agent:curing agent) of 16:1 and diluted with ethyl acetate. The dry lamination conditions were a substrate width of 900 mm, a conveying speed of 30 m / min, a drying temperature of 50°C to 60°C, a laminating roll temperature of 50°C, and a roll pressure of 3.0 MPa.

[0118] The above-mentioned diiodomethane contact angle, releasability, and flow marks evaluation tests were carried out using the sample films of Examples 1 to 12 and Comparative Examples 1 to 3. The evaluation results are shown in Tables 1-1 and 1-2.

[0119]

[0120] Tables 1-1 and 1-2 show that the generation of flow marks can be suppressed while maintaining releasability in sample films containing a predetermined amount of lubricant or surfactant. It is also clear that the generation of flow marks can be suppressed while maintaining releasability in sample films having a predetermined diiodomethane contact angle.

[0121] The semiconductor encapsulation release film of the present invention combines high levels of mold releasability and flow mark suppression, and therefore, by using this film, molded articles obtained by resin-encapsulating semiconductor chips or the like can be easily released from the mold, and molded articles free of appearance defects such as flow marks can be produced with high productivity and at relatively low cost, thereby providing technical effects of great practical value, and is highly applicable in various fields of industry, including the semiconductor process industry. Furthermore, the semiconductor encapsulation release film of the present invention can be used not only for semiconductor packages, but also for various mold molding processes in fiber-reinforced plastic molding processes, plastic lens molding processes, and the like, and is therefore highly applicable in various fields of industries other than the semiconductor industry that perform mold molding.

[0122] 1, 1-2, 1-3: Semiconductor encapsulation release film 2: Upper mold 3: Suction port 4: Sealing resin 4-2: Semiconductor package 5: Lower mold 6: Semiconductor chip 7: Substrate 8: Molding mold 22: Semiconductor encapsulation release film 24, 26: Roll 28: Molding mold 30: Upper mold 32: Lower mold 34: Semiconductor chip 34A: Substrate 36: Sealing resin 40, 44: Semiconductor package 50: Liquid sealing resin 60: Sample film 61: Mold protection film 71: Lower SUS plate 72: Upper SUS plate 73: Brass frame 80: Evaluation laminate

Claims

1. A semiconductor encapsulation release film having a surface layer containing 0.1% by mass to 10% by mass of a lubricant or surfactant, based on the weight of the surface layer of the semiconductor encapsulation release film.

2. The semiconductor encapsulation release film according to claim 1, wherein the lubricant comprises a fatty acid amide-based lubricant.

3. The semiconductor encapsulation release film according to claim 1, wherein the surfactant comprises a fluorine-based surfactant.

4. A semiconductor encapsulation release film having a surface layer with a diiodomethane contact angle of 60° to 70° measured after heating at 175° C. for 10 seconds.

5. The semiconductor encapsulation release film according to claim 1 or 4, wherein the surface layer contains a 4-methyl-1-pentene (co)polymer.

6. The semiconductor encapsulation release film according to claim 5, which is used in a semiconductor encapsulation process using an encapsulation resin containing an epoxy resin.

Citation Information

Patent Citations

  • Method of manufacturing semiconductor sealing device, and semiconductor sealing device

    JP2010129897A

  • Releasing film for process, application thereof, and method of producing resin-sealed semiconductor using same

    JP2018176695A

  • Release film

    JP2018178106A

  • Multi-layer release film

    JP2020142474A

  • Release film

    WO2019131163A1