Polypropylene-based foamed particles, polypropylene-based foamed article, and methods for producing these
The method of combining polypropylene and polyethylene resins, followed by specific processing steps, addresses the challenge of filling thin-walled molds, resulting in foamed particles with superior filling properties and surface quality.
Patent Information
- Application Number
- PCT/JP2024/011571
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-27
- Filing Date
- 2024-03-25
- Publication Date
- 2024-10-03
AI Technical Summary
Conventional polypropylene foam particles face challenges in filling molds with thin-walled portions effectively, leading to unevenness and poor aesthetics in the resulting foam molded products.
A method involving a first melt-kneading step of combining polypropylene and polyethylene resins, followed by a second melt-kneading step to create resin particles with a specific aspect ratio, and a foaming process to produce expanded polypropylene particles with a sea-island structure, enhancing filling properties into molds with thin-walled portions.
The method produces foamed polypropylene particles with excellent thin-walled filling properties and surface beauty, ensuring uniformity and quality in foam molded products without grain gaps.
Smart Images

Figure JP2024011571_03102024_PF_FP_ABST
Abstract
Description
Polypropylene-based expanded beads, polypropylene-based expanded molded article, and their manufacturing method
[0001] The present invention relates to expanded polypropylene beads, expanded polypropylene molded articles, and methods for producing the same.
[0002] Polypropylene foam molded articles obtained by molding expanded polypropylene beads made of a polypropylene resin are used in a variety of applications, including automotive interior components, core materials for automotive bumpers, heat insulating materials, cushioning packaging materials, and returnable containers.
[0003] As techniques relating to such polypropylene-based expanded beads and polypropylene-based expanded molded articles, for example, the techniques described in Patent Documents 1 and 2 are known.
[0004] In recent years, the applications of foam molded articles have tended to expand, and in addition, there is an increasing demand for foam molded articles having more complex shapes (for example, thin-walled portions) according to desired applications.
[0005] International Publication No. 2017 / 030124 International Publication No. 2013 / 099550
[0006] However, the above-mentioned conventional technology has room for improvement in terms of the filling ability of polypropylene-based expanded beads into a molding die (hereinafter sometimes simply referred to as a "mold") for molding (particularly in-mold foam molding) the polypropylene-based expanded beads, particularly in terms of the filling ability into a mold having a thin-walled portion forming portion, which is the portion for forming the thin-walled portion of the resulting polypropylene-based expanded molded article.
[0007] In view of the above circumstances, an object of one embodiment of the present invention is to provide expanded polypropylene beads that have excellent filling properties into a mold having a thin-walled portion-forming portion.
[0008] The present inventors have conducted extensive research to solve the above problems and have completed the present invention.
[0009] That is, one embodiment of the present invention is a method for producing expanded polypropylene-based beads, which includes a first melt-kneading step of melt-kneading a polypropylene-based resin (a) and a polyethylene-based resin (b) to obtain a mixed resin, a second melt-kneading step of melt-kneading the mixed resin to obtain polypropylene-based resin particles, and an expansion step of expanding the polypropylene-based resin particles, wherein the L / D of the polypropylene-based resin particles is 2.0 or more.
[0010] Another embodiment of the present invention is a polypropylene-based expanded particle having a sea-island structure in which a continuous phase containing a polypropylene-based resin (a) and a dispersed phase containing a polyethylene-based resin (b) are phase-separated, and the aspect ratio of the dispersed phase is 7.5 to 20.0.
[0011] According to one embodiment of the present invention, it is possible to provide expanded polypropylene beads that are excellent in fillability into a mold having a thin-walled portion-forming portion.
[0012] 1 is an example of a DSC curve obtained by heating an expanded bead according to one embodiment of the present invention from 40°C to 220°C at a heating rate of 10°C / min using a differential scanning calorimeter. The horizontal axis represents temperature, and the vertical axis represents heat quantity.
[0033] FIG. 1 is a schematic diagram of an expanded molded article according to an example of the present invention.
[0034] FIG. 2 is a diagram showing an example of a transmission electron microscope image of an expanded bead according to one embodiment of the present invention. The lightly stained phase represents a continuous phase containing a polypropylene-based resin (a), and the darkly stained phase represents a dispersed phase containing a polyethylene-based resin (b).
[0013] An embodiment of the present invention will be described below, but the present invention is not limited thereto. The present invention is not limited to the respective configurations described below, and various modifications are possible within the scope of the claims. Furthermore, embodiments or examples obtained by combining the technical means disclosed in different embodiments or examples are also included in the technical scope of the present invention. Furthermore, new technical features can be formed by combining the technical means disclosed in each embodiment. All academic literature and patent documents described in this specification are incorporated herein by reference. Furthermore, unless otherwise specified in this specification, the term "A to B" representing a numerical range means "greater than or equal to A (including and greater than A) and less than or equal to B (including and less than B)."
[0014] In this specification, a "structural unit derived from an X monomer" contained in a polymer, copolymer, or resin may be referred to as an "X unit."
[0015] [Method for producing expanded polypropylene-based beads] A method for producing expanded polypropylene-based beads according to one embodiment of the present invention comprises a first melt-kneading step of melt-kneading a polypropylene-based resin (a) and a polyethylene-based resin (b) to obtain a mixed resin, a second melt-kneading step of melt-kneading and granulating the mixed resin to obtain polypropylene-based resin particles, and an expansion step of expanding the polypropylene-based resin particles, wherein the L / D of the polypropylene-based resin particles is 2.0 or more.
[0016] The method for producing expanded polypropylene beads according to one embodiment of the present invention has the above-mentioned configuration, and therefore can provide expanded polypropylene beads that have excellent fillability into a mold having a thin-walled portion (hereinafter, sometimes referred to as "thin-walled portion fillability"). The thin-walled portion fillability of the expanded beads can be evaluated by the method described in the examples.
[0017] The polypropylene-based expanded beads obtained by the method for producing polypropylene-based expanded beads according to one embodiment of the present invention are foam-molded in a mold, preferably a mold having a thin-wall portion-forming portion, by a known method, to provide a polypropylene-based expanded molded article having a thin-wall portion without irregularities.
[0018] In this specification, "polypropylene-based resin particles" may be referred to as "resin particles," "polypropylene-based resin particles according to one embodiment of the present invention" may be referred to as "the present resin particles," "polypropylene-based expanded particles" may be referred to as "expanded particles," "polypropylene-based expanded particles according to one embodiment of the present invention" may be referred to as "the present expanded particles," "method for producing polypropylene-based expanded particles" may be referred to as "production method," "method for producing polypropylene-based expanded particles according to one embodiment of the present invention" may be referred to as "the present production method," and "polypropylene-based resin expanded molded body" may be referred to as "expanded molded body."
[0019] <First Melt-Kneading Step> This production method includes a first melt-kneading step of melt-kneading a polypropylene-based resin (a) and a polyethylene-based resin (b) to obtain a mixed resin. In the first melt-kneading step, it is preferable to prepare a mixed resin consisting only of the polypropylene-based resin (a) and the polyethylene-based resin (b), because this allows the polyethylene-based resin to be efficiently dispersed. The first melt-kneading step may also be a step of obtaining mixed resin particles containing the polypropylene-based resin (a) and the polyethylene-based resin (b).
[0020] The embodiment of the first melt-kneading step is not particularly limited, as long as it is possible to melt-knead the polypropylene resin (a) and the polyethylene resin (b) to obtain a mixed resin. Specific examples of the first melt-kneading step include the following methods (A1) and (A2): (A1) First, the polypropylene resin (a) and the polyethylene resin (b) are mixed or blended in a mixer or the like to prepare a mixture. Then, the mixture is supplied to the melt-kneading device and melt-kneaded to obtain a mixed resin; (A2) A method in which the polypropylene resin (a) and the polyethylene resin (b) are supplied to the melt-kneading device, a mixture is obtained in the melt-kneading device, and the mixture is melt-kneaded to obtain a mixed resin.
[0021] The mixing device in the method (A1) is not particularly limited, and examples thereof include a blender (for example, a ribbon blender or a flash blender) and a mixer (for example, a tumbler mixer or a super mixer).
[0022] The melt-kneading device in the methods (A1) and (A2) is not particularly limited, and examples thereof include an extruder, a kneader, a Banbury mixer, a roll, etc. Because of their excellent productivity and convenience, the melt-kneading device is preferably an extruder, and more preferably a multi-screw extruder (for example, a twin-screw extruder).
[0023] In the first melt-kneading step, the temperature at which the polypropylene resin (a) and the polyethylene resin (b) are melt-kneaded is not particularly limited as long as it is a temperature at which the polypropylene resin (a) and the polyethylene resin (b) melt, but for example, the melt-kneading is preferably carried out so that the temperature of the melt-kneaded resins (resin temperature) is 200° C. to 240° C., more preferably 210° C. to 230° C., and even more preferably 215° C. to 225° C. If the resin temperature in the first melt-kneading step is within the above range, there is an advantage that the polypropylene resin (a) and the polyethylene resin (b) can be melt-kneaded efficiently without thermal decomposition.
[0024] In the methods (A1) and (A2), the melt-kneaded mixture can be further cooled and solidified, and cut into a desired shape. For example, the mixture melt-kneaded in an extruder can be extruded through a die attached to the extruder, cooled and solidified in a water bath, and then cut into pellets or granules.
[0025] <Mixed Resin> The mixed resin obtained in the first melt-kneading step will be described. The mixed resin is a resin obtained by melt-kneading a polypropylene-based resin (a) and a polyethylene-based resin (b). The mixed resin is preferably a resin consisting only of a polypropylene-based resin (a) and a polyethylene-based resin (b).
[0026] The mixed resin preferably contains 60 to 99% by weight of polypropylene resin (a) and 1 to 40% by weight of polyethylene resin (b) based on 100% by weight of the mixed resin, more preferably 65 to 95% by weight of polypropylene resin (a) and 5 to 35% by weight of polyethylene resin (b), and even more preferably 70 to 90% by weight of polypropylene resin (a) and 10 to 30% by weight of polyethylene resin (b). This configuration has the advantage of being able to provide a polypropylene foam molded product that has sufficient strength, excellent surface beauty, and is free of unevenness in its thin-walled portions.
[0027] In other words, the first melt-kneading step is preferably a step of preparing a mixed resin containing the above-mentioned amounts of polypropylene-based resin (a) and polyethylene-based resin (b). Here, the content of each resin component in the mixed resin is proportional to the amount of each resin component melted and kneaded in the first melt-kneading step. Therefore, in the first melt-kneading step, it is preferable to melt-knead 60 to 99 parts by weight of polypropylene-based resin (a) and 1 to 40 parts by weight of polyethylene-based resin (b) so that the total is 100 parts by weight. It is more preferable to melt-knead 65 to 95 parts by weight of polypropylene-based resin (a) and 5 to 35 parts by weight of polyethylene-based resin (b) so that the total is 100 parts by weight. It is even more preferable to melt-knead 70 to 90 parts by weight of polypropylene-based resin (a) and 10 to 30 parts by weight of polyethylene-based resin (b) so that the total is 100 parts by weight.
[0028] (Polypropylene-based resin (a)) The polypropylene-based resin (a) that is a raw material for the mixed resin will be described below. The polypropylene-based resin (a) is a polypropylene-based resin.
[0029] In this specification, the term "polypropylene resin" refers to a resin containing 50 mol % or more of propylene units out of 100 mol % of all structural units constituting the resin.
[0030] The polypropylene-based resin (a) may be (i) a homopolymer of propylene, (ii) a block copolymer, impact copolymer, alternating copolymer, random copolymer, or graft copolymer of propylene and a monomer other than propylene, or (iii) a mixture of two or more of these.
[0031] Among these, it is preferable that the polypropylene-based resin (a) is a random copolymer of propylene and a monomer other than propylene, since this has the advantage that the resin particles and expanded particles can be processed at a low heating temperature in the expansion step and in-mold foam molding step described below.
[0032] The polypropylene-based resin (a) may have, in addition to the propylene unit, one or more structural units derived from a monomer other than a propylene monomer, and may have one or more types. The "monomer other than a propylene monomer" from which the polypropylene-based resin is derived (raw material) may also be referred to as a "comonomer." The "structural unit derived from a monomer other than a propylene monomer" contained in the polypropylene-based resin may also be referred to as a "comonomer unit."
[0033] Examples of comonomers from which comonomer units that can constitute the polypropylene-based resin (a) are derived include α-olefins having 2 or 4 to 12 carbon atoms, such as ethylene, 1-butene, isobutene, 1-pentene, 3-methyl-1-butene, 1-hexene, 4-methyl-1-pentene, 3,4-dimethyl-1-butene, 1-heptene, 3-methyl-1-hexene, 1-octene, and 1-decene.
[0034] Specific examples of the polypropylene-based resin (a) include polypropylene homopolymer, ethylene / propylene random copolymer, 1-butene / propylene random copolymer, 1-butene / ethylene / propylene random copolymer, ethylene / propylene block copolymer, 1-butene / propylene block copolymer, propylene / chlorinated vinyl copolymer, propylene / maleic anhydride copolymer, and styrene-modified polypropylene-based resin.
[0035] As the polypropylene-based resin (a), one of the above-mentioned specific examples may be used alone, or two or more may be used in combination. Among the above-mentioned specific examples, ethylene / propylene random copolymers and 1-butene / ethylene / propylene random copolymers are preferred because the resulting resin particles have good expandability and the resulting expanded beads have good moldability.
[0036] Consider a case where an ethylene / propylene random copolymer is used as the polypropylene-based resin (Case A). In Case A, the ethylene content of the ethylene / propylene random copolymer is preferably 0.2 wt% to 15.0 wt%, more preferably 0.5 wt% to 10.0 wt%, and even more preferably 0.5 wt% to 4.0 wt%, based on 100 wt% of each copolymer. The ethylene content can also be referred to as the content of structural units derived from ethylene (ethylene units). When the ethylene unit content in the ethylene / propylene random copolymer is (i) 0.2 wt% or more, the expandability of the resin beads and / or the moldability of the resulting expanded beads tend to be good, and (ii) when it is 15.0 wt% or less, there is no risk of a decrease in the mechanical properties of the expanded molded article obtained by molding the expanded beads.
[0037] The melting point of the polypropylene resin (a) is not particularly limited, but is preferably 135°C to 160°C, more preferably 136°C to 155°C, more preferably 137°C to 153°C, and more preferably 138°C to 152°C. When the melting point of the polypropylene resin (a) is (i) 135°C or higher, a foamed molded article with excellent dimensional stability at high temperatures tends to be obtained, and (ii) when it is 155°C or lower, a foamed molded article can be foam-molded in a mold at low steam pressure. The melting point of the polypropylene resin can be measured by the method described in the examples.
[0038] The melt flow rate (MFR) of the polypropylene resin (a) at 230° C. is not particularly limited, but is preferably 1.00 g / 10 min to 20.00 g / 10 min, more preferably 2.00 g / 10 min to 15.00 g / 10 min, and even more preferably 2.50 g / 10 min to 11.0 g / 10 min. When the MFR of the polypropylene resin (a) is within the above range, expanded beads having a high closed cell content can be provided, and as a result, (i) the compressive strength of the resulting expanded molded article tends to be good, and (ii) the surface properties of the resulting expanded molded article tend to be good. The MFR of the polypropylene resin (a) at 230°C is a value determined by measurement using a melt mass-flow rate (hereinafter, referred to as MFR) measuring device according to JIS-K7210 under the following conditions: orifice diameter: 2.0959±0.005 mm, orifice length: 8.000±0.025 mm, load: 2160 g, and temperature: 230±0.2°C. MFR is also sometimes referred to as "melt index (MI)."
[0039] (Polyethylene Resin (b)) The polyethylene resin (b) that is the raw material of the mixed resin will be described below. The polyethylene resin (b) is a polyethylene resin.
[0040] In this specification, the term "polyethylene resin" refers to a resin containing 50 mol % or more of ethylene units out of 100 mol % of all structural units constituting the resin.
[0041] In this specification, a resin containing 50 mol % of propylene units and 50 mol % of ethylene units out of 100 mol % of all structural units constituting the resin is considered to be a "polypropylene-based resin."
[0042] The polyethylene resin (b) may be (i) a homopolymer of ethylene, (ii) a block copolymer, alternating copolymer, random copolymer, or graft copolymer of ethylene and a monomer other than ethylene, or (iii) a mixture of two or more of these.
[0043] The polyethylene resin (b) may have, in addition to the ethylene unit, one or more structural units derived from a monomer other than an ethylene monomer, or may have one or more types of structural units.
[0044] Examples of the comonomer from which the comonomer unit that can constitute the polyethylene resin (b) is derived include α-olefins having 3 to 12 carbon atoms, such as propylene, 1-butene, isobutene, 1-pentene, 3-methyl-1-butene, 1-hexene, 4-methyl-1-pentene, 3,4-dimethyl-1-butene, 1-heptene, 3-methyl-1-hexene, 1-octene, and 1-decene; or vinyl monomers, such as vinyl acetate and (meth)acrylic acid.
[0045] Specific examples of the polyethylene resin (b) include high-density polyethylene, medium-density polyethylene, low-density polyethylene, linear low-density polyethylene, linear very low-density polyethylene, ethylene / vinyl acetate copolymer, ethylene / acrylic acid copolymer, and ethylene / methacrylic acid copolymer.
[0046] As the polyethylene resin (b), one of the above-mentioned specific examples may be used alone, or two or more of them may be used in combination. Among the above-mentioned specific examples, high-density polyethylene is preferred because of its high crystallinity and easy availability.
[0047] The melting point of the polyethylene resin (b) is not particularly limited, but is preferably 100°C to 140°C, more preferably 105°C to 130°C, and even more preferably 110°C to 128°C. When the melting point of the polyethylene resin (b) is (i) 100°C or higher, the resulting foamed molded article tends to have excellent mechanical properties such as compressive strength, and (ii) when it is 130°C or lower, there is an advantage that the foamed beads have excellent expandability. The melting point of the polyethylene resin can be measured by the method described in the examples.
[0048] The density of the polyethylene resin (b) is not particularly limited, but is preferably 0.900 g / cm 3 ~0.970g / cm 3 and preferably 0.910 g / cm 3~0.965g / cm 3 It is more preferable that the density of the polyethylene resin (b) is 0.900 g / cm 3 ~0.970g / cm 3 In this case, shrinkage of the resulting foamed molded article tends to be suppressed. The density of the polyethylene resin can be measured by the method described in JIS K7112:1999.
[0049] The melt flow rate (MFR) of the polyethylene resin (b) at 190°C is not particularly limited, but is preferably 0.01 g / 10 min to 20.00 g / 10 min, more preferably 0.00 g / 10 min to 5.00 g / 10 min, and even more preferably 0.01 g / 10 min to 2.50 g / 10 min. When the MFR of the polyethylene resin (b) is within the above range, expanded beads having a high closed cell content can be provided, and as a result, (i) the compressive strength of the obtained expanded molded article tends to be good, and (ii) the surface properties of the obtained expanded molded article tend to be good. The MFR of the polyethylene resin (b) at 190°C is a value determined by measurement using a melt mass-flow rate (hereinafter, referred to as MFR) measuring device according to JIS-K7210 under the following conditions: orifice diameter: 2.0959±0.005 mm, orifice length: 8.000±0.025 mm, load: 2160 g, and temperature: 190±0.2°C. MFR is also sometimes referred to as "melt index (MI)."
[0050] In recent years, in order to reduce the environmental load, there has been a demand for the use of recycled resins when producing resin products. For this reason, it is preferable that the polypropylene-based resin (a) and the polyethylene-based resin (b), as well as other resins added in the second melt-kneading step described below, contain recycled materials (recycled resins), and more preferably recycled resins. The recycled resin refers to a polypropylene-based resin or polyethylene-based resin that has been in the form of a polypropylene-based resin or polyethylene-based resin product (e.g., foamed beads, foamed molded articles, films, packaging containers such as food trays, bags, and bottles, miscellaneous goods such as clothing cases and clear files) at least once, and then re-formed into a polypropylene-based resin (or polypropylene-based resin particles) or a polyethylene-based resin (or polyethylene-based resin particles) by any means (e.g., melting).
[0051] The method for producing recycled resins, in other words, the method for recycling polypropylene-based resin products and polyethylene-based resin products, is not particularly limited, and known methods can be used. Examples include a method of crushing and melting polypropylene-based resin products and polyethylene-based resin products, and a method of shredding these resin products. In one embodiment of the present invention, pulverized or cut polypropylene-based resin products and / or polyethylene-based resin products can be used as the polypropylene-based resin (a) and / or polyethylene-based resin (b). That is, the first melt-kneading step may be a step of melt-kneading pulverized or cut polypropylene-based resin products and / or polyethylene-based resin products as described above.
[0052] When recycled polypropylene-based resins and polyethylene-based resins are used as the polypropylene-based resin (a) and / or the polyethylene-based resin (b), or as other resins added in the second melt-kneading step described below, the preferred aspects (e.g., composition, melting point, MFR, etc.) of the recycled polypropylene-based resin and polyethylene-based resin are as described above.
[0053] <Second Melt-Kneading Step> The present production method includes a second melt-kneading step of melt-kneading the mixed resin prepared in the first melt-kneading step to obtain resin particles. In other words, in addition to the first melt-kneading step, the present production method further includes a second melt-kneading step of melt-kneading the mixed resin to obtain resin particles.
[0054] The L / D of the resin particles obtained in the second melt-kneading step is 2.0 or more. By expanding resin particles having an L / D of 2.0 or more in the expansion step described below, a foamed molded article having excellent surface beauty and expanded particles having excellent thin-walled section filling ability can be provided. Therefore, the second melt-kneading step can also be said to be a step of obtaining resin particles containing a mixed resin and having an L / D of 2.0 or more (i.e., the present resin particles).
[0055] The L / D of the present resin particles is more preferably 2.2 or more, and even more preferably 2.4 or more. Furthermore, the L / D of the present resin particles is preferably 2.7 or less. When the L / D of the present resin particles is within the above range, (i) expanded beads with excellent thin-wall filling ability and expanded molded articles with excellent surface beauty can be provided, and (ii) the L / D of the expanded beads obtained by shrinking the resin particles upon heating in the expansion step described below tends to approach 1, i.e., the anisotropy of the expanded beads tends to be reduced, resulting in even better surface beauty of the expanded molded articles. The L / D of the resin particles can be measured by the method described in the Examples.
[0056] The average weight per particle of the present resin particles is preferably 1.0 mg to 3.6 mg, and more preferably 1.0 mg to 2.0 mg. When the average weight per particle of the present resin particles is within the above range, it tends to be easier to obtain resin particles having an L / D ratio of 2.0 or more.
[0057] The mode of the second melt-kneading step is not particularly limited as long as it is possible to melt-knead the mixed resin and, if necessary, other resins and / or additives to obtain resin particles. Specific examples of the second melt-kneading step include the following methods (B1) and (B2): (B1) First, the mixed resin and, if necessary, other resins and / or additives are mixed or blended using a mixer or the like to prepare a resin composition. Then, the resin composition is supplied to a melt-kneading device and melt-kneaded to obtain resin particles; (B2) A method in which the mixed resin and, if necessary, other resins and / or additives are supplied to a melt-kneading device to obtain a resin composition in the melt-kneading device, and the resin composition is melt-kneaded to obtain resin particles.
[0058] The mixing device in the method (B1) is not particularly limited, and examples thereof include a blender (for example, a ribbon blender or a flash blender) and a mixer (for example, a tumbler mixer or a super mixer).
[0059] The melt-kneading device in the methods (B1) and (B2) is not particularly limited, and examples thereof include an extruder, a kneader, a Banbury mixer, a roll, etc. Because of their excellent productivity and convenience, the melt-kneading device is preferably an extruder, and more preferably a multi-screw extruder (for example, a twin-screw extruder).
[0060] In the second melt-kneading step, the temperature at which the mixed resin and, as necessary, other resins and / or additives are melt-kneaded is not particularly limited as long as it is a temperature at which the mixed resin and any other resins used melt, but for example, it is preferable to melt-knead so that the temperature of the resin to be melt-kneaded (resin temperature) is 200° C. to 240° C., more preferably 210° C. to 230° C., and even more preferably 215° C. to 225° C. If the resin temperature in the second melt-kneading step is within the above range, there is an advantage that the mixed resin and / or other resins can be melt-kneaded efficiently without thermal decomposition.
[0061] The second melt-kneading step preferably includes a particle forming step in which the melt-kneaded resin composition is stretched and molded (granulated) into particles having an L / D ratio of 2.0 or more.
[0062] The form of the particle molding step is not particularly limited as long as the melt-kneaded resin composition can be molded into a particle shape with an L / D of 2.0 or more. For example, by using a melt-kneading device equipped with a die and connected to a cutting device, the melt-kneaded resin composition can be easily molded into a desired shape in the particle molding step. Specifically, the melt-kneaded resin composition is discharged from the nozzle of the die equipped in the melt-kneading device, and after discharge, the resin composition is stretched and cut with a cutting device, thereby molding into a particle shape with an L / D of 2.0 or more. The shape of the obtained resin particles is not particularly limited as long as the L / D is 2.0 or more, but cylindrical, elliptical cylindrical, etc. are preferred because they are easy to use for foaming.
[0063] (Other Resins) In the second melt-kneading step, other resins may be melt-kneaded in addition to the mixed resin. In other words, the resin particles (and resin composition) may contain other resins. Examples of other resins to be melt-kneaded in the second melt-kneading step (in other words, contained in the resulting resin particles) include polyolefin resins such as polypropylene resins and polyethylene resins; styrene resins such as polystyrene, styrene / maleic anhydride copolymer, and styrene / ethylene copolymer; and the like. In addition, the other resins may be recycled (recycled resins), and from the viewpoint of reducing environmental load, recycled resins are preferred. When a polyolefin resin is used as the other resin, the polyolefin resin may be the same type of resin as the polypropylene resin (a) or the polyethylene resin (b), or a different type of resin may be used. In other words, in this specification, "other resins" means resins not used in the first melt-kneading step, and does not mean resins other than the polypropylene resin (a) and the polyethylene resin (b).
[0064] The content of the other resin in the resin particles (and resin composition) obtained by the second melt-kneading step is preferably 20% by weight to 80% by weight, and more preferably 25% by weight to 75% by weight, based on 100% by weight of the total amount of the mixed resin and other resins. According to this configuration, the presence of multiple types of resin in the resin particles broadens the resin composition distribution, making the DSC ratio (described below) less dependent on the foaming temperature. As a result, even if the foaming temperature is not precisely reproducible, expanded beads having roughly the same DSC ratio can be produced. In other words, this has the advantage of improving the quality stability of the expanded beads. The content of the other resin in the resin particles may be 0% by weight.
[0065] The content of each resin component in the resin particles is proportional to the amount of each resin component melted and kneaded in the second melt-kneading step. Therefore, in the second melt-kneading step, it is preferable to melt-knead 20 to 80 parts by weight of the mixed resin and 20 to 80 parts by weight of the other resin so that the total amount is 100 parts by weight, and it is more preferable to melt-knead 25 to 75 parts by weight of the mixed resin and 25 to 75 parts by weight of the other resin so that the total amount is 100 parts by weight.
[0066] The resin particles are preferably polypropylene-based resin particles. In other words, the resin particles preferably contain 50% by weight or more of polypropylene-based resin in a total of 100% by weight of the mixed resin and other resins contained in the resin particles. The content of polypropylene-based resin in a total of 100% by weight of the mixed resin and other resins contained in the resin particles is more preferably 60% by weight or more, even more preferably 70% by weight or more, even more preferably 80% by weight or more, and particularly preferably 90% by weight or more. The content of polypropylene-based resin in the resin particles can be calculated as the total amount of polypropylene-based resin (a) contained in the mixed resin and the polypropylene-based resin contained in the other resins.
[0067] (Additives) In the second melt-kneading step, additives may be melt-kneaded in addition to the mixed resin and other resins. In other words, the resin particles (and the resin composition) obtained by the second melt-kneading step may contain additives. Examples of additives to be melt-kneaded in the second melt-kneading step (in other words, contained in the obtained resin particles) include colorants, water-absorbing substances (for example, (i) polyols such as glycerin and diglycerin, (ii) polyethers such as polyethylene glycol and polyethylene oxide, and (iii) metal borates such as borax and zinc borate), foam nucleating agents (for example, inorganic substances such as talc, calcium carbonate, silica, kaolin, barium sulfate, calcium hydroxide, aluminum hydroxide, aluminum oxide, titanium oxide, and zinc borate), antistatic agents (for example, glycerin monostearate, glycerin mono-distearate, etc.), and the like. Examples of additives that can be used include: flame retardants (e.g., hindered amine flame retardants, bromine flame retardants, phosphate ester flame retardants, melamine flame retardants, etc.), antioxidants (e.g., hindered phenol antioxidants, etc.), heat stabilizers (e.g., phosphorus-based heat stabilizers and sulfur-based heat stabilizers, etc.), light stabilizers (benzotriazole UV absorbers, triazine UV absorbers, HALS and / or hindered amine light stabilizers, etc.), crystal nucleating agents, conductive agents (carbon, carbon nanotubes, metal fillers, etc.), lubricants, acid scavengers (calcium oxide and fatty acid calcium, etc.), antiblocking agents, metal chelating agents (IRGANOX MD1024, ADK STAB CDA-1, etc.), lubricants, and antibacterial agents. In particular, additives that contribute to stabilizing the resin, such as antioxidants, are preferably added in the first melt-kneading step. By using a stabilizer in the first melt-kneading step, deterioration of the recycled resin is suppressed, even when recycled resin is used, and the physical properties tend to be less likely to decrease.
[0068] The amount of additive used in the second melt-kneading step is preferably 0.1 to 5.0 parts by weight, more preferably 0.2 to 4.0 parts by weight, and even more preferably 0.3 to 3.5 parts by weight, relative to 100 parts by weight of the total amount of the mixed resin and other resins used in the second melt-kneading step. When multiple types of additives are used in the second melt-kneading step, the amount of additive used in the second melt-kneading step refers to the total amount of the multiple types of additives used. The amount of additive used in the second melt-kneading step (in other words, the content of additive in the resin particles) may be 0 part by weight.
[0069] The above-mentioned other resins and / or additives can also be used in the first melt-kneading step. When the other resins and / or additives are used in the first melt-kneading step, it is preferable that the total amount of the other resins and / or additives used in the first melt-kneading step and the amount of the other resins and / or additives used in the second melt-kneading step be within the above-mentioned range. In particular, it is preferable that additives that contribute to stabilizing the resin, such as antioxidants, be added in the first melt-kneading step. By using additives that contribute to stabilizing the resin in the first melt-kneading step, when recycled resin is used as a raw material, deterioration of the recycled resin can be suppressed, and the physical properties of the resulting expanded beads tend to be improved.
[0070] The present resin particles are produced through a first melt-kneading step and a second melt-kneading step, and thereby become resin particles having a sea-island structure in which a continuous phase made of a polypropylene-based resin containing a polypropylene-based resin (a) and a dispersed phase made of a polyethylene-based resin containing a polyethylene-based resin (b) are phase-separated. The average dispersion area per particle of the polyethylene-based resin phase as the dispersed phase in the present resin particles is 0.01 μm, since this allows the provision of expanded beads and foamed molded articles having sufficient strength. 2 ~3.00μm 2 It is preferable that the thickness is 0.02 μm. 2 ~1.60μm 2The average dispersion area of the polyethylene resin phase, which is the dispersed phase in the resin particles, can be measured by the method described in the Examples.
[0071] <Expansion Step> The present production method includes an expansion step of expanding the resin particles obtained in the second melt-kneading step. The expansion step can also be said to be a step of obtaining expanded beads by expanding the present resin particles.
[0072] The form of the expansion step is not particularly limited as long as it is possible to expand the present resin particles and obtain expanded particles. However, a method including a depressurization expansion step in which the present resin particles are expanded in an aqueous dispersion medium is preferred, as it has the advantage of enabling stable production of expanded particles.
[0073] An example of a specific embodiment of the depressurization foaming step is a method including a dispersing step, a temperature-pressure increasing step, a holding step, and a releasing step. Hereinafter, each step that can be included in the foaming step according to one embodiment of the present invention (hereinafter, sometimes referred to as "this foaming step") will be described in detail using such an embodiment as an example.
[0074] (Dispersion Step) The foaming step preferably includes a dispersion step, which is a step of preparing a dispersion in which the resin particles, a foaming agent, and, if necessary, a dispersant and / or a dispersion aid are dispersed in an aqueous dispersion medium.
[0075] The container used in the dispersion step is not particularly limited, but is preferably a container that can withstand the foaming temperature and foaming pressure described below. The container is preferably, for example, a pressure-resistant container, more preferably an autoclave-type pressure-resistant container. The container may be equipped with a stirrer inside.
[0076] The aqueous dispersion medium is not particularly limited as long as it can uniformly disperse the resin particles, the foaming agent, etc.
[0077] In terms of enabling stable production of expanded beads, it is preferable to use, as the aqueous dispersion medium, pure water such as RO water (water purified by a reverse osmosis membrane method), distilled water, deionized water (water purified by an ion exchange resin), or ultrapure water.
[0078] Examples of the blowing agent include (a) (a-1) inorganic blowing agents such as nitrogen, carbon dioxide, air (a mixture of oxygen, nitrogen, and carbon dioxide), and (a-2) water; and (b) organic blowing agents such as (b-1) saturated hydrocarbons having 3 to 5 carbon atoms such as propane, normal butane, isobutane, normal pentane, isopentane, and neopentane, (b-2) ethers such as dimethyl ether, diethyl ether, and methyl ethyl ether, and (b-3) halogenated hydrocarbons such as monochloromethane, chloroethane, and hydrofluoroolefins.
[0079] In the present method for producing expanded beads, it is preferable to use a dispersant (e.g., an inorganic substance such as tricalcium phosphate or kaolin) and a dispersing aid (e.g., an anionic surfactant such as sodium dodecylbenzenesulfonate or sodium alkanesulfonate). This configuration can reduce adhesion of resin particles (sometimes called blocking) and improve the stability of the dispersion in the container. As a result, it has the advantage of enabling stable production of expanded beads.
[0080] The aqueous dispersion medium and the blowing agent may each be used alone or in combination of two or more.
[0081] (Temperature-Pressure Increase Step and Holding Step) The foaming step preferably further includes, after the dispersion step and before the release step, (i) a temperature-pressure increase step in which the temperature inside the container is increased to a constant temperature and the pressure inside the container is increased to a constant pressure, and (ii) a holding step in which the temperature and pressure inside the container are held at a constant temperature and a constant pressure. The holding step is preferably carried out after the temperature-pressure increase step. In this specification, the (a) constant temperature in the temperature-pressure increase step and the holding step may be referred to as the foaming temperature, and the (b) constant pressure in the foaming step may be referred to as the foaming pressure.
[0082] The foaming temperature cannot be generally defined because it varies depending on the types and amounts of base resin and additives contained in the resin particles, the type and amount of foaming agent added, etc. The foaming temperature is preferably the melting point of the resin particles used in the foaming step −20.0° C. to the melting point +20.0° C., more preferably the melting point of the resin particles −10.0° C. to the melting point +15.0° C., and even more preferably the melting point of the resin particles −5.0° C. to the melting point +13.0° C.
[0083] The expansion pressure is preferably 0.5 MPa (gauge pressure) to 10.0 MPa (gauge pressure), more preferably 1.0 MPa (gauge pressure) to 5.0 MPa (gauge pressure), and even more preferably 1.5 MPa (gauge pressure) to 3.0 MPa (gauge pressure). When the expansion pressure is 0.5 MPa (gauge pressure) or more, expanded beads with a suitable density can be obtained.
[0084] In the holding step, the time (holding time) for which the dispersion in the container is held at temperatures near the foaming temperature and foaming pressure is not particularly limited. The holding time is preferably 10 to 60 minutes, more preferably 12 to 50 minutes, and even more preferably 15 to 40 minutes.
[0085] (Discharging Step) The resin particles can be expanded by the discharging step, resulting in expanded particles. The discharging step can also be described as a step of opening one end of the container and discharging the dispersion liquid in the container into a region (space) with a pressure lower than the expansion pressure (i.e., the pressure inside the container).
[0086] In the releasing step, the "region under a pressure lower than the foaming pressure" refers to a "region under a pressure lower than the foaming pressure" or a "space under a pressure lower than the foaming pressure", and can also be referred to as "an atmosphere under a pressure lower than the foaming pressure". The region under a pressure lower than the foaming pressure is not particularly limited as long as it is lower than the foaming pressure, and may be, for example, a region under atmospheric pressure.
[0087] This process of producing expanded beads from resin beads through one expansion step is called the "first-stage expansion step," and the resulting expanded beads are called "first-stage expanded beads."
[0088] (Second-stage expansion step) In order to obtain expanded beads with a high expansion ratio, this expansion step preferably includes a step of re-expanding the first-stage expanded beads obtained in the first-stage expansion step. This step of re-expanding the first-stage expanded beads is called the "second-stage expansion step," and the expanded beads obtained by the second-stage expansion step are called "second-stage expanded beads." The specific method for the second-stage expansion step is not particularly limited, and any known method can be used.
[0089] <Physical Properties of Expanded Beads> The physical properties that the expanded beads obtained by the present production method (the present expanded beads) may have will be described in detail below.
[0090] (DSC Ratio of Expanded Beads) The DSC ratio of the expanded beads is not particularly limited, but is preferably 10.0% to 40.0%, more preferably 15.0% to 30.0%, and even more preferably 18.0% to 25.0%. When the DSC ratio of the expanded beads is 10.0% or more, there is an advantage that there is no risk of wrinkles forming on the surface of the expanded beads and that a foamed molded article having excellent mechanical properties such as compressive strength can be obtained. On the other hand, when the DSC ratio of the expanded beads is 40.0% or less, there is an advantage that the expanded beads can exhibit excellent expandability and expansion properties and that a foamed molded article having excellent internal fusion can be obtained at a low molding pressure. The DSC ratio of the expanded beads can be measured by the method described in the Examples.
[0091] The present expanded beads preferably have three or more melting peaks in a DSC curve obtained by heating the present expanded beads from 40°C to 220°C at a heating rate of 10°C / min using a differential scanning calorimeter, as shown in Figure 1.
[0092] Fig. 1 will be explained in more detail. Fig. 1 shows an example of a DSC curve obtained by heating expanded polypropylene resin beads from 40°C to 220°C at a heating rate of 10°C / min. In Fig. 1, line a is a line connecting the maximum point between the highest melting peak and the melting peak adjacent to that (lower temperature side) to the point at 100°C, and line b is a line connecting the maximum point to the point representing the temperature after completion of melting. Ql is the low-temperature side region surrounded by the DSC curve and line a, and the heat quantity calculated from this region Ql is the low-temperature side heat of fusion. Qh is the high-temperature side region surrounded by the DSC curve and line b, and the heat quantity calculated from this region Qh is the high-temperature side heat of fusion.
[0093] Since the present expanded beads contain a polypropylene-based resin (a) and a polyethylene-based resin (b), the expanded beads have three melting peaks as shown in Figure 1, i.e., two melting peaks derived from the polypropylene-based resin and one melting peak derived from the polyethylene-based resin.
[0094] (Expansion Ratio of Expanded Beads) The expansion ratio of the expanded beads is not particularly limited, but is preferably 3.0 to 50.0 times, more preferably 10.0 to 30.0 times, and even more preferably 15.0 to 27.0 times. When the expansion ratio of the expanded beads is within the above range, it is possible to obtain a lightweight expanded molded article with high production efficiency, and it is advantageous in that it is possible to provide an expanded molded article with sufficient strength. The expansion ratio of the expanded beads can be measured by the method described in the Examples. Furthermore, when two-stage expansion is performed in the expansion process, the expansion ratio of the expanded beads refers to the expansion ratio of the second-stage expanded beads.
[0095] (L / D of expanded beads) The L / D of the expanded beads is more preferably 0.8 to 1.2, even more preferably 0.9 to 1.1, and particularly preferably 1.0. When the L / D of the expanded beads is within the above range, a foamed molded article with excellent surface beauty can be provided. The L / D of the expanded beads can be measured by the method described in the examples.
[0096] (Average Dispersion Area and Aspect Ratio of Polyethylene Resin Phase in Expanded Beads) The expanded beads are formed by expanding the resin beads having the above-described islands-in-a-sea structure. Therefore, the expanded beads also have a sea-island structure in which a continuous phase made of a polypropylene resin containing the polypropylene resin (a) and a dispersed phase made of a polyethylene resin containing the polyethylene resin (b) are phase-separated.
[0097] An example of a transmission electron microscope image of the expanded beads is shown in Figure 3. In Figure 3, the lightly stained phase represents the continuous phase containing the polypropylene-based resin (a), and the darkly stained phase represents the dispersed phase containing the polyethylene-based resin (b).
[0098] The average dispersion area per particle of the polyethylene resin phase as the dispersed phase in the present expanded beads is 0.01 μm, which can provide expanded beads and foamed molded articles having sufficient strength. 2 ~3.00μm 2 It is preferable that the thickness is 0.02 μm. 2 ~1.60μm 2 The average dispersion area of the polyethylene resin phase, which is the dispersed phase in the expanded beads, can be measured by the method described in the Examples.
[0099] Furthermore, since the present expanded particles have a sea-island structure and are formed by expanding the present resin particles having a predetermined L / D, the polyethylene resin phase, which is the dispersed phase, becomes an expanded particle having a sea-island structure with a relatively large aspect ratio.
[0100] Specifically, the aspect ratio per particle of the polyethylene resin phase serving as the dispersed phase in the expanded beads is preferably 7.5 to 20.0, more preferably 8.0 to 18.0, even more preferably 9.0 to 16.0, and particularly preferably 9.5 to 15.5, because expanded beads having excellent filling properties in thin-walled sections can be provided, and polypropylene-based expanded molded articles having excellent surface beauty and no irregularities in thin-walled sections can be provided. The aspect ratio of the polyethylene resin phase serving as the dispersed phase in the expanded beads can be measured by the method described in the Examples.
[0101] The present inventors have surprisingly found that expanded polypropylene-based particles having the above-mentioned islands-in-a-sea structure and in which the aspect ratio of the dispersed polyethylene-based resin phase is within the above-mentioned range are excellent in fillability into a mold having a thin-walled portion. Therefore, the expanded polypropylene-based particles can also be described as follows: expanded polypropylene-based particles having an islands-in-a-sea structure in which a continuous phase containing a polypropylene-based resin (a) and a dispersed phase containing a polyethylene-based resin (b) are phase-separated, and the aspect ratio of the dispersed phase is 7.5 to 20.0.
[0102] The present expanded beads having the above-described configuration can be suitably produced by the present production method, but it goes without saying that the present expanded beads are not limited to those produced by this method as long as they have the above-described configuration.
[0103] The present expanded beads may contain other resins and / or additives in addition to the polypropylene-based resin (a) and the polyethylene-based resin (b). Note that the specific aspects of each component that may be contained in the present expanded beads (e.g., the polypropylene-based resin (a), the polyethylene-based resin (b), the other resins and / or additives) are the same as those described in the section on resin particles, and therefore, the description therein is incorporated by reference and will not be repeated here.
[0104] <Other Methods for Producing Expanded Beads> In the above, the method for producing the expanded beads has been described by taking as an example a method including a first melt-kneading step and a second melt-kneading step. However, the method for producing the expanded beads is not limited to such a method as long as it can produce expanded polypropylene-based beads having a sea-island structure in which a continuous phase containing a polypropylene-based resin (a) and a dispersed phase containing a polyethylene-based resin (b) are phase-separated, and the dispersed phase has an aspect ratio of 7.5 to 20.0.
[0105] Examples of the method for producing the expanded beads (other production methods) other than the method including the first melt-kneading step and the second melt-kneading step include a method in which the raw materials for the expanded beads, i.e., the polypropylene-based resin (a), the polyethylene-based resin (b), and other resins and / or additives, are mixed (melt-kneaded) using a multi-screw extruder having two or more screws, each having a ratio (L / D) of the effective length L of the screw to the screw diameter D of 30 to 40. Such an embodiment is also included in one embodiment of the present invention.
[0106] Therefore, another embodiment of the method for producing expanded polypropylene beads according to the present invention can also be expressed as follows: a method for producing expanded polypropylene beads, comprising: a melt-kneading step of melt-kneading a polypropylene resin (a), a polyethylene resin (b), and other resins and / or additives using a multi-screw extruder having two or more screws, each having a ratio (L / D) of the effective screw length L to the screw diameter D of 30 or more, to obtain polypropylene resin beads; and an expansion step of expanding the polypropylene resin beads, wherein the L / D of the polypropylene resin beads is 2.0 or more.
[0107] [Polypropylene-based foam molded article] The foam molded article of the present invention is a foam molded article obtained by molding the foam beads of the present invention (for example, in-mold foam molding). The foam molded article of the present invention can also be said to be a foam molded article made from the foam beads of the present invention as a raw material.
[0108] When molding a foamed molded article having a thin-walled portion, it is necessary to use a mold having a thin-walled portion-forming region. The thin-walled portion-forming region is a very narrow space (e.g., approximately 5 mm wide) corresponding to the dimensions of the thin-walled portion of the resulting foamed molded article. When ordinary foamed beads are filled into a mold having a thin-walled portion-forming region to mold a foamed molded article having a thin-walled portion, the foamed beads are not sufficiently filled into the thin-walled portion-forming region, resulting in a problem of poor aesthetics, with obvious gaps between the particles. On the other hand, the foamed molded article of the present invention is made from the foamed beads, which have excellent fillability into a mold having a thin-walled portion-forming region, and therefore has a beautiful thin-walled portion without gaps between the particles. The foamed molded article of the present invention may have a thin-walled portion. Furthermore, the foamed beads of the present invention can be suitably used to produce a foamed molded article having a thin-walled portion.
[0109] <Method for producing foamed molded article> The method for producing the foamed molded article is not particularly limited as long as it is possible to produce a foamed molded article by molding the foamed beads (preferably in-mold foam molding), and any known method can be used. As a method for producing the foamed molded article, for example, the method described in the section <Method for producing foamed molded article> of International Publication WO2022 / 149538 can be suitably used.
[0110] [Others] An embodiment of the present invention may include the following configuration.
[0111] [1] A method for producing expanded polypropylene-based beads, comprising: a first melt-kneading step of melt-kneading a polypropylene-based resin (a) and a polyethylene-based resin (b) to obtain a mixed resin; a second melt-kneading step of melt-kneading the mixed resin to obtain polypropylene-based resin particles; and an expansion step of expanding the polypropylene-based resin particles, wherein the L / D of the polypropylene-based resin particles is 2.0 or more.
[0112] [2] The method for producing expanded polypropylene beads according to [1], wherein in the first melt-kneading step, 60 to 99 parts by weight of the polypropylene resin (a) and 1 to 40 parts by weight of the polyethylene resin (b) are melt-kneaded to a total of 100 parts by weight.
[0113] [3] The method for producing expanded polypropylene-based beads according to [1] or [2], wherein the expansion step includes a depressurization expansion step of expanding the polypropylene-based resin particles in an aqueous dispersion medium.
[0114] [4] The method for producing expanded polypropylene beads according to any one of [1] to [3], wherein the polypropylene resin (a) and / or the polyethylene resin (b) contain recycled resins.
[0115] [5] The polypropylene-based resin particles have a sea-island structure in which a continuous phase containing the polypropylene-based resin (a) and a dispersed phase containing the polyethylene-based resin (b) are phase-separated, and the average dispersed area per dispersed phase is 0.01 μm 2 ~3.00μm 2 [1] to [4], the method for producing expanded polypropylene beads.
[0116] [6] The method for producing expanded polypropylene beads according to any one of [1] to [5], wherein the melting point of the polypropylene resin (a) is 135°C to 160°C.
[0117] [7] The method for producing expanded polypropylene beads according to any one of [1] to [6], wherein the melting point of the polyethylene resin (b) is 100°C to 140°C.
[0118] [8] The density of the polyethylene resin (b) is 0.900 g / cm 3 ~0.970g / cm 3 [8] The method for producing expanded polypropylene beads according to any one of [1] to [7],
[0119] [9] Expanded polypropylene-based particles having a sea-island structure in which a continuous phase containing a polypropylene-based resin (a) and a dispersed phase containing a polyethylene-based resin (b) are phase-separated, and the aspect ratio of the dispersed phase is 7.5 to 20.0.
[0120]
[10] The expanded polypropylene beads according to [9], wherein the polypropylene resin (a) and / or the polyethylene resin (b) contain recycled resins.
[0121]
[11] The expanded polypropylene beads according to [9] or
[10] , which have three or more melting peaks in a DSC curve obtained by heating from 40°C to 220°C at a heating rate of 10°C / min using a differential scanning calorimeter.
[0122]
[12] The average dispersion area per dispersed phase is 0.01 μm 2 ~3.00μm 2 The expanded polypropylene beads according to any one of [9] to
[11] ,
[0123]
[13] The expanded polypropylene beads according to any one of [9] to
[12] , having a DSC ratio of 10.0% to 40.0%.
[0124]
[14] The expanded polypropylene beads according to any one of [9] to
[13] , wherein L / D is 0.8 to 1.2.
[0125]
[15] A method for producing a polypropylene-based expanded molded article, comprising a step of molding the expanded polypropylene beads obtained by the method for producing expanded polypropylene beads described in any one of [1] to [8], or the expanded polypropylene beads described in any one of [9] to
[14] .
[0126]
[16] A polypropylene-based expanded molded article obtained by molding expanded polypropylene beads obtained by the method for producing expanded polypropylene beads described in any one of [1] to [8], or the expanded polypropylene beads described in any one of [9] to
[14] .
[0127]
[17] The method for producing expanded polypropylene beads according to any one of [1] to [8], wherein the polypropylene resin (a) is at least one selected from the group consisting of a propylene homopolymer, and a block copolymer and a random copolymer of propylene and a monomer other than propylene.
[0128]
[18] The expanded polypropylene beads according to any one of [9] to
[14] , wherein the polypropylene resin (a) is at least one selected from the group consisting of a propylene homopolymer, and a block copolymer or random copolymer of propylene and a monomer other than propylene.
[0129]
[19] The method for producing expanded polypropylene beads according to any one of [1] to [8] and
[17] , wherein the polypropylene resin particles contain a mixed resin containing a polypropylene resin (a) and a polyethylene resin (b) and other resins, and the polypropylene resin (a) accounts for 50% by weight or more of the total amount of the mixed resin and other resins contained in the resin particles, 100% by weight.
[0130]
[20] The method for producing expanded polypropylene beads according to any one of [1] to [8] and
[17] , wherein the polypropylene resin particles contain a mixed resin containing a polypropylene resin (a) and a polyethylene resin (b) and other resins, and the other resins account for 20 to 80% by weight of 100% by weight of the total amount of the mixed resin and other resins contained in the resin particles.
[0131]
[21] The expanded polypropylene beads according to any one of [9] to
[14] and
[18] , having an expansion ratio of 3.0 to 50.0 times.
[0132] The present invention will be specifically explained below with reference to examples, but the technical scope of the present invention is not limited to these examples.
[0133] [Materials] The materials used in the examples and comparative examples are shown below.
[0134] <Mixed Resins> Polypropylene-based resin (a): ethylene / propylene random copolymer [ethylene content 9%, melting point 151°C, MFR 7g / 10min] Polyethylene-based resin (b): high-density polyethylene (HDPE) [melting point 126°C, MFR 0.15g / 10min] Note that recycled resins were used as the polypropylene-based resin (a) and the polyethylene-based resin (b).
[0135] <Other Resins> (Recycled Resins) Recycled Polypropylene Resin: Ethylene / Propylene Random Copolymer [Ethylene Content 9%, Melting Point 151°C, MFR 7g / 10min] Recycled Polyethylene Resin: High Density Polyethylene (HDPE) [Melting Point 126°C, MFR 0.15g / 10min] (Non-Recycled Resin) Non-Recycled Polypropylene Resin: 1-Butene / Ethylene / Propylene Random Copolymer [Ethylene Content 1%, 1-Butene Content 3%, Melting Point 148°C, MFR 10g / 10min] <Additives> Carbon Black [Primary Particle Size 20nm to 100nm] Talc [Talc Powder PK-S, manufactured by Hayashi Kasei Co., Ltd.] Glycerin [Purified Glycerin D, manufactured by Lion Corporation] Hindered Amine Flame Retardant [NOR116, manufactured by BASF].
[0136] [Measurement Methods] The evaluation methods used in the examples and comparative examples are described below.
[0137] (Measurement of Melting Point of Polypropylene Resin and Polyethylene Resin) The melting points of polypropylene resin and polyethylene resin were measured using a differential scanning calorimeter [DSC7020, manufactured by Hitachi High-Tech Science Corporation]. The specific measurement procedure was as follows: (1) 5 mg to 6 mg of the resin to be measured was weighed out and melted by heating from 40 ° C. to 220 ° C. at a heating rate of 10 ° C. / min; (2) The melted resin was crystallized by cooling from 220 ° C. to 40 ° C. at a heating rate of 10 ° C. / min; (3) The temperature was further increased from 40 ° C. to 220 ° C. at a heating rate of 10 ° C. / min; (4) The temperature of the peak (melting peak) of the DSC curve obtained during the second heating (i.e., during (3)) was taken as the melting point Tm of the polypropylene resin or polyethylene resin.
[0138] (Measurement of MFR of polypropylene-based resin and polyethylene-based resin) For polypropylene-based resin, MFR was measured using a melt mass-flow rate measuring device according to JIS K7210 under the following conditions: orifice 2.0959±0.005 mmφ, orifice length 8.000±0.025 mm, load 2160 g, and temperature 230±0.2° C. For polyethylene-based resin, MFR was measured using a melt mass-flow rate measuring device according to JIS K7210 under the following conditions: orifice 2.0959±0.005 mmφ, orifice length 8.000±0.025 mm, load 2160 g, and temperature 190±0.2° C.
[0139] (Measurement of L / D of resin particles and expanded beads) For 10 randomly selected resin particles or expanded beads, the L / D per resin particle or expanded bead was calculated using the following method, and the arithmetic mean of the L / D per particle of the 10 resin particles or expanded beads was taken as the L / D of the resin particle or expanded bead. The specific method for measuring L / D per resin particle or expanded bead was as follows: the length of the longest part of a single resin particle or expanded bead in question was taken as L, and the maximum diameter of the resin particle or expanded bead in a cross section perpendicular to the L direction was taken as Dmax and the minimum diameter was taken as Dmin; the L / D per resin particle or expanded bead was calculated using the following formula: L / D per resin particle or expanded bead = L / ((Dmax + Dmin) / 2).
[0140] (Measurement of DSC Ratio of Expanded Beads) The DSC ratio of expanded beads was measured using a differential scanning calorimeter [DSC7020, manufactured by Hitachi High-Tech Science Corp.]. The specific measurement procedure was as follows: (1) 5 mg to 6 mg of expanded beads were weighed; (2) The expanded beads were heated from 40°C to 220°C at a heating rate of 10°C / min to melt the expanded beads; (3) In the DSC curve of the expanded beads obtained in the process (2), (3a) a line a was drawn connecting the maximum point between the highest melting peak and the melting peak adjacent thereto (on the lower temperature side) and the point representing a temperature of 100°C, and (3b) a line a was drawn connecting the maximum point and the point representing the temperature after melting was completed. (4) (4a) The heat quantity calculated from the high-temperature region surrounded by the line segment b connecting the maximum point and the point representing the temperature after completion of melting, the DSC curve, and (4b) the heat quantity calculated from the low-temperature region surrounded by the line segment a connecting the maximum point and the point representing the temperature of 100°C, the DSC curve, and (4c) the sum of Qh and Ql was defined as the total heat of fusion (= Qh + Ql); (5) The DSC ratio of the expanded beads was calculated based on the following formula: DSC ratio of expanded beads (%) = [Qh / (Qh + Ql)] × 100.
[0141] (Measurement of Expansion Ratio of Expanded Beads) The expansion ratio of expanded beads was measured by the following procedure: (1) 3 g to 10 g of expanded beads were weighed out and dried at 60°C for 6 hours; (2) The dried expanded beads were conditioned (left in the room) at 23°C and 50% humidity, and then the weight w (g) of the expanded beads was measured; (3) The expanded beads were submerged in a measuring cylinder containing ethanol, and the volume v (cm) of the expanded beads was determined from the rise in the water level in the measuring cylinder. 3 (4) The true specific gravity of the expanded beads was calculated based on the following formula: True specific gravity ρb (g / cm 3 )=w(g) / v(cm 3 ); (5) Density ρr of resin particles before foaming (g / cm 3The expansion ratio of the expanded beads was calculated from the ratio of the density of the expanded beads (K) to the true specific gravity ρb of the expanded beads according to the following formula: Expansion ratio of expanded beads K = ρr / ρb. The volume measurement method as described in (3) above is sometimes called the "submersion method." In addition, in the examples and comparative examples shown below, the density ρr of the resin particles before expansion was 0.9 g / cm3. 3 It was decided.
[0142] (Measurement of the average dispersion area of the polyethylene-based resin phase in the resin particles) The average dispersion area of the polyethylene-based resin phase in the resin particles was measured by the following procedure: (1) the resin particles were cut at an arbitrary position; (2) the cross section of the cut resin particles was measured using RuO 4 (3) A photograph of the cross section of the resin particle was taken at a magnification of 40,000 times using a transmission electron microscope [device: H-7650 manufactured by Hitachi High-Technologies Corporation, acceleration voltage: 100 kV]; (4) In the obtained transmission electron microscope photograph, 10 polyethylene-based resin phases (RuO 4 The area of the polyethylene resin phase was measured and the arithmetic mean value was taken as the average dispersion area of the polyethylene resin phase in the resin particles.
[0143] (Measurement of the average dispersion area of the polyethylene resin phase in the expanded beads) The average dispersion area of the polyethylene resin phase in the expanded beads was measured by the following procedure: (1) the expanded beads were cut at an arbitrary position; (2) the cross section of the cut expanded beads was measured using RuO 4 (3) A photograph of the cross section of the expanded beads was taken at a magnification of 40,000 times using a transmission electron microscope [device: H-7650 manufactured by Hitachi High-Technologies Corporation, acceleration voltage: 100 kV]; (4) In the obtained transmission electron microscope photograph, 10 polyethylene resin phases (RuO 4 The area of the phase was measured, and the arithmetic mean value was taken as the average dispersed area of the polyethylene resin phase in the expanded beads.
[0144] (Aspect Ratio of Polyethylene Resin Phase in Expanded Beads) The aspect ratio of the polyethylene resin phase in expanded beads was measured by the following procedure: (1) In a transmission electron micrograph obtained in the above-mentioned process (measuring the average dispersed area of the polyethylene resin phase in expanded beads), 10 polyethylene resin phases were randomly selected, and for each of the phases, the length Y of its longest part and the length X of its maximum diameter in the direction perpendicular to the Y direction were measured; (2) The aspect ratio A per polyethylene resin phase was calculated based on the following formula, and the arithmetic mean value was used as the aspect ratio of the polyethylene resin phase in expanded beads: Aspect ratio A per polyethylene resin phase = Y / X.
[0145] (Measurement of density of foam molded article) The density of a foam molded article (foam molded article density) was measured by the following methods (1) to (3): (1) The volume V (L) of the foam molded article was calculated based on the dimensions of the foam molded article including the thin-walled portion; (2) Furthermore, the weight W (g) of the foam molded article was measured; (3) The density of the foam molded article was calculated based on the following formula: Density (g / L) of foam molded article = W / V.
[0146] (Evaluation of Thin-Walled Portion Filling Ability) The thin-walled portions of the obtained foamed molded article were visually observed, and the thin-walled portion filling ability of the expanded beads was evaluated according to the following criteria: 1 (Good): Almost no gaps (gaps between the expanded beads) at the corners of the thin-walled portion. 0 (Poor): Clear gaps at the corners of the thin-walled portion. Note that almost no gaps at the corners of the thin-walled portion mean that the expanded beads have filled up to the corners of the thin-walled portion, and clear gaps at the corners of the thin-walled portion mean that the expanded beads have not filled up to the corners of the thin-walled portion.
[0147] (Evaluation of Surface Beauty of Foam Molded Articles) The side surfaces of the obtained foam molded articles were visually observed, and the surface beauty of the foam molded articles was evaluated according to the following criteria. The larger the number, the fewer intergranular gaps, surface irregularities, wrinkles, and shrinkage there are, and the surface is more beautiful. 1 (Good): Almost no intergranular gaps, inconspicuous surface irregularities, no wrinkles or shrinkage, and beautiful. 0 (Poor): Intergranular gaps, surface irregularities, shrinkage, or wrinkles are observed.
[0148] [Example 1] (Preparation of mixed resin) 95 parts by weight of polypropylene-based resin (a) and 5 parts by weight of polyethylene-based resin (b) were blended using a tumbler mixer. The blended mixture was melt-kneaded at a resin temperature of 220 ° C using a twin-screw extruder, and the extruded strand was water-cooled in a 2 m long water tank and then cut to produce mixed resin particles (5.0 mg / particle) (first melt-kneading step). This was designated mixed resin 1.
[0149] (Preparation of Resin Particles) Mixed resin 1 and the other resins and additives listed in Table 1 were blended using a tumbler mixer to obtain a mixture. The resulting mixture was melt-kneaded at a resin temperature of 220 ° C. using a twin-screw extruder having a screw with a ratio (L / D) of the effective length L to the screw diameter D of 28 (second melt-kneading step). The melt-kneaded product was then extruded from the twin-screw extruder into strands through a die with a hole having a diameter of 1.2 mm. After water cooling, the resulting strands were cut to an L / D ratio of 2.5 while stretching the resin composition by adjusting the pelletizer take-up speed and cutter rotation speed. This resulted in resin particles with a maximum length L = 2.15 mm, an average maximum diameter Dmax and minimum diameter Dmin ((Dmax + Dmin) / 2) = 0.86 mm, L / D = 2.5, and an average weight of 1.2 mg / particle. The average dispersion area of the polyethylene resin phase was measured for the resulting resin particles. The results are shown in Table 1.
[0150] (Preparation of Expanded Beads) 100 parts by weight (2.4 kg) of the obtained resin particles, 200 parts by weight of pure water, 0.22 parts by weight of kaolin (ASP170, manufactured by BASF) as a dispersant, and 0.38 parts by weight of an aqueous solution of sodium dodecylbenzenesulfonate (Neopelex G-15, manufactured by Kao Corporation) as a dispersing aid were placed in a pressure-resistant autoclave. Thereafter, while stirring the raw materials in the pressure-resistant autoclave, 4 parts by weight of carbon dioxide as a blowing agent was introduced into the pressure-resistant autoclave to prepare a dispersion (dispersion step). The temperature inside the pressure-resistant autoclave was then heated to the foaming temperature listed in Table 1. After maintaining the foaming temperature for 10 minutes, additional carbon dioxide was injected into the pressure-resistant autoclave, and the pressure inside the pressure-resistant autoclave was increased to a foaming pressure of 2.2 MPa (gauge pressure) (heating-pressure increase step). Next, the pressure autoclave was maintained at the foaming temperature and foaming pressure for 20 minutes (maintenance step), and then the valve at the bottom of the pressure autoclave was opened to release the dispersion through a 3.6 mm orifice into a foaming tube under atmospheric pressure, thereby obtaining expanded beads (release step). During this release, carbon dioxide was additionally injected into the pressure-resistant sealed vessel to maintain the pressure inside the pressure-resistant sealed vessel at 2.2 MPa (gauge pressure) so that the pressure inside the pressure-resistant sealed vessel would not drop below the foaming pressure. The resulting expanded beads had a sea-island structure consisting of a continuous phase containing the polypropylene-based resin (a) and a dispersed phase containing the polyethylene-based resin (b). The resulting expanded beads were measured for DSC ratio, expansion ratio, average dispersed area of the polyethylene-based resin phase, and aspect ratio of the polyethylene-based resin phase. The results are shown in Table 1.
[0151] (Preparation of second-stage expanded beads) The obtained expanded beads were dried at 80°C and then placed in a pressure-resistant vessel. In the pressure-resistant vessel, the expanded beads were impregnated with pressurized air to adjust the internal pressure of the expanded beads to 0.3 MPa (absolute pressure). The pressurized expanded beads were contacted with water vapor at 0.07 MPa (gauge pressure) to obtain second-stage expanded beads. The obtained second-stage expanded beads had an expansion ratio of 26.1 times and an L / D ratio of 1.0.
[0152] (Preparation of Foam Molded Article) The resulting two-stage foamed beads were placed in a pressure-resistant sealed container, and air was introduced into the pressure-resistant sealed container. The foamed beads in the pressure-resistant sealed container were impregnated with the pressurized air, thereby applying an internal pressure of 0.20 MPa (absolute pressure) to the foamed beads. The foamed beads to which internal pressure had been applied were filled into the molding space of a mold installed in a molding machine (Toyo Machinery Metal Co., Ltd. P-150N molding machine). The mold used here had a movable mold and a fixed mold, and the movable mold and fixed mold could form a molding space capable of molding the foam molded article 100 shown in FIG. 2. The foam molded article 100 was a box-shaped foam molded article having six thin-walled portions 3. The external dimensions of the foam molded article 100 were 350 mm long x 320 mm wide x 175 mm high, with the vertical wall portion 1 having a thickness of 20 mm, the horizontal wall portion 1 having a thickness of 20 mm, and the bottom portion 2 having a thickness of 10 mm. The thin-walled portion 3 had a plate shape with a thickness gradient from top to bottom, measuring 80 mm in length, 10 mm in maximum thickness, 5 mm in minimum thickness, and 100 mm in height. The foamed beads filled in the mold were heated with steam at 0.32 MPa (gauge pressure) to fuse the foamed beads, and the mold and the surface of the molded body were cooled with cooling water to obtain a foamed molded body. The density, thin-walled portion filling property, and surface aesthetics of the obtained foamed molded body were measured and evaluated. The results are shown in Table 1.
[0153] [Examples 2 to 9] Mixed resins, resin particles, expanded particles, and foamed molded articles were obtained in the same manner as in Example 1, except that the blending amounts of each component, the L / D ratio of the resin particles, and / or the foaming conditions were changed as shown in Table 1. The physical properties were measured and evaluated. The results are shown in Table 1.
[0154] In Examples 4 to 9, mixed resin 2 was used as the raw material for resin particles. The mixed resin 2 was prepared in the same manner as mixed resin 1, except that 70 parts by weight of polypropylene-based resin (a) and 30 parts by weight of polyethylene-based resin (b) were mixed in the first melt-kneading step.
[0155] Comparative Examples 1 and 2: Polypropylene resin (a) and polyethylene resin (b) in the amounts shown in Table 1 were melt-kneaded with additives by the method described in the section (Preparation of Resin Particles) of Example 1 to obtain resin particles. As described above, Comparative Examples 1 and 2 did not use mixed resins, so the first and second melt-kneading steps were not performed. Using the obtained resin particles, expanded beads and foamed molded articles were obtained by the same method as in Example 1, except that the foaming conditions were changed as shown in Table 1, and the physical properties were measured and evaluated. The results are shown in Table 1.
[0156] Comparative Example 3: The blended amounts of mixed resin 1 and additives listed in Table 1 were melt-kneaded using the method described in (Preparation of Resin Particles), extruded into strands through a die with holes 1.2 mm in diameter, and the resulting strands were water-cooled. The pelletizer's take-up speed and cutter rotation speed were adjusted to stretch the resin composition while cutting it so that the L / D ratio was 1.5, yielding resin particles with an average weight of 1.2 mg per particle. Using these resin particles, expanded beads and foamed molded articles were obtained in the same manner as in Example 1, except that the foaming conditions were changed as listed in Table 1. The physical properties were measured and evaluated. The results are shown in Table 1.
[0157] The expanded beads of Examples 1 to 9 and Comparative Examples 1 to 3 had three melting peaks in the DSC curves obtained by heating from 40°C to 220°C at a heating rate of 10°C / min using a differential scanning calorimeter.
[0158] According to one embodiment of the present invention, it is possible to provide polypropylene-based expanded beads that have excellent fillability into a mold having a thin-walled portion. The polypropylene-based expanded molded article obtained by expanding the polypropylene-based expanded beads according to one embodiment of the present invention has excellent fillability into a thin-walled portion, and therefore can be used for various purposes such as cushioning packaging materials, logistics materials, heat insulating materials, civil engineering and construction materials, and automotive parts, and is particularly suitable for use in expanded molded articles having complex shapes.
Claims
1. A method for producing polypropylene-based expanded particles, comprising: a first melt-kneading step of melt-kneading a polypropylene-based resin (a) and a polyethylene-based resin (b) to obtain a mixed resin; a second melt-kneading step of melt-kneading the mixed resin to obtain polypropylene-based resin particles; and an expansion step of expanding the polypropylene-based resin particles, wherein the L / D of the polypropylene-based resin particles is 2.0 or more.
2. A method for producing polypropylene-based expanded beads according to claim 1, wherein in the first melt-kneading step, 60 to 99 parts by weight of the polypropylene-based resin (a) and 1 to 40 parts by weight of the polyethylene-based resin (b) are melt-kneaded to a total of 100 parts by weight.
3. The method for producing expanded polypropylene-based beads according to claim 1, wherein the expansion step includes a depressurization expansion step of expanding the polypropylene-based resin beads in an aqueous dispersion medium.
4. The method for producing polypropylene-based expanded beads according to claim 1, wherein the polypropylene-based resin (a) and / or the polyethylene-based resin (b) contain recycled resins.
5. The polypropylene-based resin particles have a sea-island structure in which a continuous phase containing the polypropylene-based resin (a) and a dispersed phase containing the polyethylene-based resin (b) are phase-separated, and the average dispersion area per dispersed phase is 0.01 μm 2 ~3.00μm 2 The method for producing expanded polypropylene beads according to claim 1, 6. The method for producing polypropylene-based expanded beads according to claim 1, wherein the polypropylene-based resin (a) has a melting point of 135°C to 160°C.
7. The method for producing polypropylene-based expanded beads according to claim 1, wherein the melting point of the polyethylene-based resin (b) is 100°C to 140°C.
8. Polypropylene-based expanded particles having a sea-island structure in which a continuous phase containing a polypropylene-based resin (a) and a dispersed phase containing a polyethylene-based resin (b) are phase-separated, and the aspect ratio of the dispersed phase is 7.5 to 20.
0.
9. The polypropylene-based expanded particles according to claim 8, wherein the polypropylene-based resin (a) and / or the polyethylene-based resin (b) contain recycled resins.
10. The polypropylene-based expanded beads according to claim 8, which have three or more melting peaks in a DSC curve obtained by heating from 40°C to 220°C at a heating rate of 10°C / min using a differential scanning calorimeter.
11. The average dispersion area per one of the dispersed phases is 0.01 μm 2 ~3.00μm 2 The polypropylene-based expanded particles according to claim 8, 12. The polypropylene-based expanded beads according to claim 8, having a DSC ratio of 10.0% to 40.0%.
13. The polypropylene-based expanded beads according to claim 8, wherein L / D is 0.8 to 1.
2.
14. A method for producing a polypropylene-based expanded molded article, comprising a step of molding polypropylene-based expanded beads obtained by the method for producing polypropylene-based expanded beads according to any one of claims 1 to 7, or the polypropylene-based expanded beads according to any one of claims 8 to 13.
15. A polypropylene-based expanded molded article obtained by molding expanded polypropylene beads obtained by the method for producing expanded polypropylene beads described in any one of claims 1 to 7, or the expanded polypropylene beads described in any one of claims 8 to 13.
Citation Information
Patent Citations
Polypropylene resin foam particles and polypropylene resin foam molded article
WO2022149538A1
Method for producing polypropylene-based resin-foamed particle
JP2005023302A
Method for producing preliminary expanded particle of polypropylene-based resin
JP2010121020A
Expandable, storage-stable polymer beads
JP2022511523A
Pre-expanded polypropylene resin particle, and method for production thereof
WO2009047998A1
Cited By
Polyolefin-based resin foam particles, method for producing same, and polyolefin-based resin foam molded body
WO2026182162A1