Method for manufacturing conductive pigment paste and method for manufacturing mixture paste

The method of pulverizing high-concentration conductive pigments and mixing with specific components addresses the challenges of dispersibility and stability in conductive pigment pastes, leading to improved battery electrode performance.

WO2024204162A1PCT designated stage expired Publication Date: 2024-10-03KANSAI PAINT CO LTD

Patent Information

Application Number
PCT/JP2024/011891
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-27
Filing Date
2024-03-26
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Conductive pigment pastes with high pigment concentrations and high viscosity often suffer from poor pigment dispersibility and storage stability, which affects the conductivity and finishability of battery electrode layers.

Method used

A method involving the pulverization of conductive pigments with a concentration of 50% or more, followed by mixing with a pigment dispersion resin, solvent, and fluororesin, using specific conditions such as temperature and dispersion treatments, to create a conductive pigment paste with improved dispersibility and stability.

Benefits of technology

The method results in a conductive pigment paste with excellent pigment dispersibility, storage stability, and enhanced battery electrode performance, including improved conductivity and finishability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
  • Figure JPOXMLDOC01-APPB-T000003
    Figure JPOXMLDOC01-APPB-T000003
Patent Text Reader

Abstract

The present invention addresses the problem of providing: a conductive pigment paste and a mixture paste having excellent pigment dispersibility and storage stability even in a high pigment concentration; and an electrode layer for a lithium ion secondary battery, the electrode layer having excellent performance in various aspects (such as conductivity and battery performance). Provided as a solution for the problem is a method for manufacturing a conductive pigment paste containing a pigment dispersion resin (A), a conductive pigment (B), a solvent (C), and an optional fluorine resin (D), the method being characterized by sequentially carrying out step 1 for pulverizing a conductive pigment composition having a pigment concentration of 50% by mass or more of the conductive pigment (B) in a pulverizer and step 2 for mixing and dispersing a component containing the pigment dispersion resin (A), the solvent (C) and the optional fluorine resin (D) in the conductive pigment composition obtained in the step 1.
Need to check novelty before this filing date? Find Prior Art

Description

Method for producing conductive pigment paste and method for producing composite paste

[0001] The present invention relates to a method for producing a conductive pigment paste and a composite paste that are excellent in conductivity, pigment dispersibility, and storage stability even at a high pigment concentration, and to a method for producing a battery electrode layer that has excellent battery performance.

[0002] Paste-like pigment dispersions in which a pigment is dispersed in a mixture of a pigment dispersing resin, a solvent, and the like have conventionally been widely used in fields such as paints, battery electrodes, coating materials, coating materials, electromagnetic wave shields, display panels, touch screen panels, colored films, colored sheets, decorative materials, protective materials, magnet modifiers, printing inks, device members, electronic device members, printed wiring boards, solar cells, functional rubber members, and resin molded films. Furthermore, conductive pigments, conductive polymers, and the like are incorporated into these materials to impart functions such as electrostatic coating properties, conductivity, electromagnetic wave shielding properties, and antistatic properties.

[0003] In these fields, there is an increasing demand for improvements in performance such as pigment dispersibility, storage stability, conductivity, coatability, and finish. To this end, pigment dispersing resins and pigment pastes are being developed that have excellent pigment dispersing ability and excellent pigment dispersion stability that prevents reagglomeration of pigment particles in the formed pigment dispersion.

[0004] When designing a pigment paste, it is important to prepare a highly concentrated and uniformly dispersed pigment paste using a small amount of pigment dispersing resin, in order to prevent the pigment dispersing resin from adversely affecting the conductive properties of the final product itself, such as the coating film, and from the perspective of reducing the amounts of solvent and pigment dispersing resin used and reducing the energy used during drying.

[0005] For example, Patent Document 1 discloses a method for manufacturing an electrode for a non-aqueous electrolyte battery, which comprises the steps of: kneading a carbon-based conductive agent and a dispersion solvent, and then dispersing the carbon-based conductive agent using a medium-type disperser; adding an active material and a binder to the paste obtained in the above step and kneading them to form an active material paste; and applying the active material paste to an electrode substrate. However, these inventions sometimes fail to achieve uniform dispersion when using pastes with high pigment concentrations and / or high viscosity, resulting in poor storage stability.

[0006] Japanese Patent Application Publication No. 10-144302

[0007] An object of the present invention is to provide a method for producing a conductive pigment paste and a method for producing a composite paste that are excellent in pigment dispersibility and storage stability even in pastes with high pigment concentrations and / or high viscosity, and further to provide a method for producing a coating film (battery electrode layer) that is excellent in finish quality, conductivity, etc.

[0008] As a result of intensive research into solving the above-mentioned problems, the present inventors have found that the above-mentioned problems can be solved by a method for producing a conductive pigment paste containing a pigment dispersing resin (A), a conductive pigment (B), a solvent (C), and a fluororesin (D) that can be included as needed, the method comprising the steps of sequentially carrying out the following: Step 1: pulverizing a conductive pigment composition having a pigment concentration of the conductive pigment (B) of 50 mass % or more using a pulverizer; and Step 2: mixing and dispersing components including the pigment dispersing resin (A), the solvent (C), and the fluororesin (D) that can be included as needed with the conductive pigment composition obtained in Step 1, and have thereby completed the present invention.

[0009] That is, the present invention provides the following methods for producing a conductive pigment paste, a composite paste, and a battery electrode layer. Item 1. A method for producing a conductive pigment paste containing a pigment dispersing resin (A), a conductive pigment (B), a solvent (C), and a fluororesin (D) that can be included as needed, comprising the steps of: Step 1: pulverizing a conductive pigment composition having a pigment concentration of the conductive pigment (B) of 50 mass % or more using a pulverizer; and Step 2: mixing and dispersing components including the pigment dispersing resin (A), the solvent (C), and the fluororesin (D) that can be included as needed with the conductive pigment composition obtained in Step 1. Item 2. A method for producing a conductive pigment paste according to Item 1, wherein the conductive pigment (B) contains carbon nanotubes (B1). Item 3. The carbon nanotubes (B1) before and after the pulverization in Step 1 satisfy the following (1) and (2): (1) 1560 cm -1 More than 1600cm -1 The maximum peak intensity within the following range is G, 1310 cm -1 1350cm or more -1Item 2. A method for producing a conductive pigment paste according to Item 2, wherein the following conditions are satisfied: (1) the G / D ratio of the carbon nanotubes (B1) before pulverization is 0.1 or more and 5.0 or less, when D is the maximum peak intensity within the following range; and (2) where α is the G / D ratio of the carbon nanotubes (B1) before pulverization and β is the G / D ratio of the carbon nanotubes (B1) after pulverization, β / α<1.00. Item 4. A method for producing a conductive pigment paste according to any one of Items 1 to 3, wherein the pigment dispersion resin (A) has at least one alkyl group having 12 or more carbon atoms. Item 5. A method for producing a conductive pigment paste according to any one of Items 1 to 4, wherein the pigment dispersion resin (A) has at least one polar functional group selected from the group consisting of an amide group, an imide group, a hydroxyl group, a carboxyl group, a sulfonic acid group, a phosphate group, a silanol group, a cyano group, a pyrrolidone group, and an amino group, and wherein the concentration of the polar functional group in the pigment dispersion resin (A) is 0.3 mmol / g to 23 mmol / g. Item 6. Item 7. A method for producing a conductive pigment paste according to any one of Items 1 to 5, wherein the conductive pigment paste contains a fluororesin (D), and the step of mixing the fluororesin (D) includes a step of previously mixing and dissolving the fluororesin with a solvent at a liquid temperature of 40°C or higher, or a step of mixing the fluororesin (D) with a solvent and then heating the resulting mixture to a temperature of 40°C or higher. Item 8. A method for producing a conductive pigment paste according to any one of Items 1 to 6, wherein the solvent (C) is N-methyl-2-pyrrolidone. Item 8. A method for producing a conductive pigment paste according to any one of Items 1 to 7, wherein Step 2 includes the sequential steps of: Step 2-1: adding components containing a conductive pigment composition in an amount of 70 mass% or less, based on 100 mass% of the total amount of the conductive pigment composition contained in the conductive pigment paste obtained after dispersion, into a disperser, and performing a dispersion treatment; and Step 2-2: adding the conductive pigment composition into the disperser until the desired concentration is reached, and performing a dispersion treatment. Item 9. Item 9. A method for producing a composite paste for a lithium ion secondary battery, comprising: step 3: mixing at least one electrode active material (F) with the conductive pigment paste obtained by the method for producing a conductive pigment paste according to any one of items 1 to 8.Item 10. A method for producing an electrode layer for a lithium ion secondary battery, comprising a step of coating a current collector with the lithium ion secondary battery composite paste obtained by the production method of Item 9. Item 11. A method for producing an electrode for a lithium ion secondary battery, comprising a step of coating an electrode insulating portion on an end or an upper layer of the electrode layer obtained by the production method of an electrode layer for a lithium ion secondary battery of Item 10.

[0010] The method for producing a conductive pigment paste and the method for producing a composite paste of the present invention are excellent in pigment dispersibility and storage stability even at high pigment concentrations and / or high viscosities, and can sufficiently reduce the viscosity of the paste with a relatively small amount of dispersing resin. Furthermore, the resulting coating film (battery electrode layer) is excellent in finish, conductivity, battery performance, etc.

[0011] Hereinafter, embodiments of the present invention will be described in detail.

[0012] The present invention is not limited to the following embodiments and should be understood to include various modifications within the scope of the present invention. In the present invention, a composition containing a conductive pigment (B) at a pigment concentration of 50% by mass or more and obtained by pulverizing the conductive pigment (B) with a pulverizer is referred to as a "conductive pigment composition." A paste prepared by further blending the conductive pigment composition with at least one pigment dispersion resin (A), a solvent (C), an optional fluororesin (D), and optionally other various components is referred to as a "conductive pigment paste." The term "conductive pigment paste" refers to a paste containing a conductive pigment, but does not mean that the paste itself is conductive. The conductive pigment paste can be considered to be a paste that does not substantially contain an electrode active material. A paste prepared by further blending at least one electrode active material and optionally other various components for coating the conductive pigment paste is referred to as a "composite paste." The composite paste applied to a substrate and dried is referred to as a "coating film" or "composite layer." When the coating film is used for a battery electrode, it can also be referred to as an "electrode layer." Carbon nanotubes can also be abbreviated as "CNT."

[0013] [Method for producing conductive pigment paste] The present invention is a method for producing a conductive pigment paste containing a pigment dispersing resin (A), a conductive pigment (B), a solvent (C), and a fluororesin (D) that can be included as needed, and includes: a step of first grinding the conductive pigment (B) in a grinder at a pigment concentration of 50 mass% or more to obtain a conductive pigment composition (step 1: grinding step); and a step of mixing and dispersing components including the pigment dispersing resin (A), the solvent (C), and the fluororesin (D) that can be included as needed with the conductive pigment composition obtained in step 1 (step 2: dispersing step). The present invention may also include another step between, before, or after steps 1 and 2.

[0014] Step 1 (Crushing Step) Step 1 is a step of pulverizing (including disintegration) the conductive pigment (B) using a pulverizer to obtain a conductive pigment composition. The pigment concentration of the conductive pigment (B) is usually 50% by mass or more, preferably 80% by mass or more, more preferably 90% by mass or more, even more preferably 95% by mass or more, particularly preferably 99% by mass or more, and even particularly preferably 100% by mass, based on 100% by mass of the conductive pigment composition. Note that the "pigment concentration of the conductive pigment (B)" refers to the pigment concentration of the conductive pigment (B) contained in the conductive pigment composition, and does not include pigments or solids other than the conductive pigment (B). As components other than the conductive pigment (B) in the conductive pigment composition, solvents, resins, and pigments other than the conductive pigment (B), as described below, can be suitably used. The solid content concentration of the conductive pigment composition is usually 50% by mass or more, preferably 80% by mass or more, more preferably 90% by mass or more, even more preferably 95% by mass or more, particularly preferably 99% by mass or more, and even more particularly preferably 100% by mass, based on 100% by mass of the conductive pigment composition. The "solid content concentration" mentioned above is the proportion (% by mass) of solids when 1 g of a sample is dried by heating at 130°C for 3 hours.

[0015] Furthermore, the conductive pigment composition obtained in step 1 may contain components other than the conductive pigment (B) as long as the pigment concentration and solids concentration are as described above, and may contain, for example, a pigment dispersion resin (A) described below, a pigment other than the conductive pigment (B), a solvent (C), and a fluororesin (D) that can be contained as needed, but the conductive pigment composition preferably contains substantially only the conductive pigment (B), and particularly preferably contains substantially only the carbon nanotubes (B1). Furthermore, when the conductive pigment paste is used for an electrode layer, it is preferable that it does not substantially contain the electrode active material described below, because it will be mixed in in a later step (step 3).

[0016] Conductive pigment (B) The conductive pigment (B) is a conductive pigment, and any known conductive pigment can be used, but it is preferable that the conductive pigment (B) contains carbon nanotubes (B1). The conductive pigment (B) may further contain a conductive pigment (B2) other than the carbon nanotubes (B1).

[0017] The content of the carbon nanotubes (B1) in the conductive pigment (B) is, for example, 50% by mass or more, preferably 75% by mass or more, more preferably 95% by mass or more, particularly preferably 99% by mass or more, and even more particularly preferably 100% by mass, based on 100% by mass of the conductive pigment (B).

[0018] Carbon nanotubes (B1) As the carbon nanotubes (B1), single-walled carbon nanotubes or multi-walled carbon nanotubes can be used alone or in combination. In particular, from the viewpoints of viscosity, conductivity, and cost, it is preferable to use multi-walled carbon nanotubes.

[0019] When carbon nanotubes (B1) are used, the content thereof is, based on 100 mass% of the total amount of the conductive pigment paste, for example, 0.5 mass% or more, preferably 1 mass% or more, more preferably 2 mass% or more, and for example, 10 mass% or less, preferably 7 mass% or less, more preferably 6 mass% or less. Also, based on 100 mass% of the total amount of solids in the conductive pigment paste, the content thereof is, for example, 5 mass% or more, preferably 10 mass% or more, more preferably 20 mass% or more, and for example, 90 mass% or less, preferably 70 mass% or less, more preferably 50 mass% or less.

[0020] The average outer diameter of the carbon nanotubes (B1) is, for example, 1 nm or more, preferably 3 nm or more, more preferably 5 nm or more, and for example, 30 nm or less, preferably 28 nm or less, more preferably 25 nm or less.

[0021] The average length of the carbon nanotubes (B1) is, for example, 0.1 μm or more, preferably 1 μm or more, more preferably 5 μm or more, and for example, 100 μm or less, preferably 80 μm or less, more preferably 60 μm or less.

[0022] The BET specific surface area of ​​the carbon nanotubes (B1) is usually 100 m due to the relationship between viscosity and conductivity. 2 / g or more, preferably 130m 2 / g or more, more preferably 160m 2 / g or more, and is usually 800m 2 / g or less, preferably 600m 2 / g or less, more preferably 400m 2 The BET specific surface area of ​​the present invention can be calculated by the BET method using nitrogen adsorption measurement. Specifically, for example, the BET specific surface area (m 2 / g) can be measured.

[0023] The amount of acidic groups in the carbon nanotubes (B1) is, from the viewpoint of dispersibility and storage stability, usually 0.01 mmol / g or more, preferably 0.01 mmol / g or more, and usually 1.0 mmol / g or less, preferably 0.5 mmol / g or less, more preferably 0.2 mmol / g or less, and even more preferably 0.1 mmol / g or less. If the amount of acidic groups is 0.01 mmol / g or more, dispersibility will be good, and if it is 1.0 mmol / g or less, storage stability will be good.

[0024] The acidic groups can be imparted to the carbon nanotubes by the acid treatment described below.

[0025] (Acid Treatment Method) The acid treatment method is not particularly limited as long as it can bring the carbon nanotubes into contact with an acid, but a method of immersing the carbon nanotubes in an acid treatment solution (aqueous acid solution) is preferred. The acid contained in the acid treatment solution is not particularly limited, but examples include nitric acid, sulfuric acid, and hydrochloric acid. These can be used alone or in combination of two or more. Among these, nitric acid and sulfuric acid are preferred. The amount of acidic groups in the carbon nanotubes can be adjusted by the concentration, temperature, treatment time, etc. of the acid treatment solution.

[0026] After the acid treatment, excess acid components adhering to the surface can be removed by a washing method described below, thereby obtaining acid-treated carbon nanotubes. The method for washing the acid-treated carbon nanotubes is not particularly limited, but washing with water is preferred. For example, carbon nanotubes are recovered from the acid-treated carbon nanotubes by a known method such as filtration, and then the carbon nanotubes are washed with water. After the washing, if necessary, water adhering to the surface can be removed by drying, thereby obtaining acid-treated carbon nanotubes.

[0027] Furthermore, the volume-equivalent median diameter (D50) of the carbon nanotubes (B1), as measured by the method described in the Examples below, is usually 10 μm or more, preferably 15 μm or more, more preferably 20 μm or more, and usually 250 μm or less, preferably 200 μm or less, more preferably 150 μm or less. Here, the median diameter (D50) can be determined by irradiating carbon nanotube particles with laser light and converting the diameter of the carbon nanotubes from the scattered light into a spherical equivalent. The larger the median diameter (D50), the more carbon nanotube aggregates there are, indicating poor dispersibility. If the median diameter (D50) is greater than 250 μm, the more likely carbon nanotube aggregates are present in the electrode, resulting in non-uniform conductivity throughout the electrode. On the other hand, if the median diameter (D50) is less than 10 μm, the fiber length is short, resulting in insufficient conductive paths and reduced conductivity. When the median diameter (D50) is within the range of 10 μm or more and 250 μm or less, the carbon nanotubes can be uniformly dispersed in the electrode while maintaining their electrical conductivity.

[0028] In addition, in the Raman spectrum of the carbon nanotube (B1), -1 More than 1600cm -1 The maximum peak intensity within the following range is G, 1310 cm -1 1350cm or more -1 When the maximum peak intensity within the following range is defined as D, the G / D ratio is usually 0.1 or more, preferably 0.4 or more, more preferably 0.6 or more, and is usually 5.0 or less, preferably 3.0 or less, more preferably 1.0 or less.

[0029] Here, it is preferable that the G / D ratio is in the range of 0.1 to 5.0, since there are fewer defects and crystal interfaces on the carbon surface and the conductivity is likely to be high.

[0030] When carbon nanotubes (B1) are used as the conductive pigment (B), the carbon nanotubes (B1) before and after the pulverization in step 1 preferably satisfy the following (1) and (2): (1) 1560 cm -1 More than 1600cm-1 The maximum peak intensity within the following range is G, 1310 cm -1 1350cm or more -1 The G / D ratio of the carbon nanotubes (B1) before pulverization is 0.1 or more and 5.0 or less, where D is the maximum peak intensity within the following range. (2) When the G / D ratio of the carbon nanotubes (B1) before pulverization is α and the G / D ratio of the carbon nanotubes (B1) after pulverization is β, β / α<1.00. Furthermore, the value of β / α decreases as pulverization progresses, and is usually β / α<1.00, preferably 0.50<β / α<1.00, more preferably 0.70<β / α<0.98, and even more preferably 0.90<β / α<0.96. When β / α is within the above range, the pulverized surface is moderately activated in a relatively short pulverization time, and good dispersibility and storage stability are obtained in the dispersion step of Step 2 described below, and the coating film can have excellent conductivity and finish.

[0031] Other conductive pigments (B2) Examples of other conductive pigments (B2) other than the carbon nanotubes (B1) include at least one conductive carbon selected from the group consisting of acetylene black, ketjen black, furnace black, thermal black, graphene, and graphite. Preferably, it is at least one selected from the group consisting of acetylene black, ketjen black, furnace black, and thermal black, more preferably at least one selected from the group consisting of acetylene black and ketjen black, and even more preferably acetylene black.

[0032] The average primary particle diameter of the other conductive pigment (B2) is, for example, 10 nm or more, preferably 20 nm or more, and more preferably, for example, 80 nm or less, preferably 70 nm or less. Here, the average primary particle diameter refers to the average particle diameter of primary particles obtained by observing the conductive pigment (B2) with an electron microscope, determining the projected area of ​​each of 100 particles, calculating the diameter of a circle equivalent to that area, and then simply averaging the diameters of the 100 particles. Note that if the pigment is in an aggregated state, the calculation is performed using the primary particles that make up the aggregated particles.

[0033] The BET specific surface area of ​​the other conductive pigment (B2) is not particularly limited. 2 / g or more, preferably 10m 2 / g or more, more preferably 20m 2 / g or more, for example, 500m 2 / g or less, preferably 250m 2 / g or less, more preferably 200m 2 / g or less.

[0034] The dibutyl phthalate (DBP) oil absorption of the other conductive pigment (B2) is not particularly limited and is, in view of the relationship between pigment dispersibility and conductivity, for example, 60 ml / 100 g or more, preferably 150 ml / 100 g or more, and for example, 1,000 ml / 100 g or less, preferably 800 ml / 100 g or less.

[0035] Pulverization Method and Pulverizer The conductive pigment (B) is pulverized (including disintegration) using a pulverizer. In the present invention, it is particularly preferable that the conductive pigment (B) contains carbon nanotubes. In the pulverization step of step 1, pulverization is carried out using a pulverizer equipped with pulverizing media such as glass beads, zirconia beads, steel balls, etc. The pulverization is carried out by utilizing the crushing or destructive force generated by collisions between the pulverizing media and / or between the pulverizer and the pulverizer. Known pulverizers such as high-speed impact mills, jet mills, roll mills, attritors, ball mills, vibration mills, and bead mills can be used.

[0036] Furthermore, various types of steam or gas can be blown into the mill during pulverization to further activate the surface of the conductive pigment (B) or adjust the activity. As the steam, an acidic or basic compound is suitable, and as the gas, oxygen, nitrogen, etc. are suitable.

[0037] The above-mentioned pulverization is preferably carried out by so-called dry dispersion. Here, "dry dispersion" refers to pulverizing a pigment without substantially containing any liquid components, and since energy can be applied directly to the pigment, highly efficient and powerful pulverization (disintegration) is possible. In addition, since the pulverized surface is activated and interacts with surrounding substances, good dispersibility and storage stability can be obtained in the dispersion step (Step 2) described below, and the resulting coating film can have excellent conductivity and finish.

[0038] The outer diameter of the grinding media is preferably 0.1 to 5 mm, more preferably 0.5 to 3 mm. Within this range, a desired grinding force can be obtained, and when the conductive pigment (B) is carbon nanotubes, the pigment can be efficiently ground and disintegrated without excessively destroying the fiber shape.

[0039] Step 2 (Dispersion Step) Step 2 is a step of mixing and dispersing components containing the pigment dispersing resin (A), the solvent (C), and the fluororesin (D) which may be included as needed into the conductive pigment composition obtained in Step 1, and a liquid conductive pigment paste can be obtained by Step 2.

[0040] The upper limit of the solid content of the conductive pigment paste is usually less than 80% by mass, preferably less than 50% by mass, more preferably less than 20% by mass, and even more preferably less than 10% by mass. The lower limit is usually 0.1% by mass or more, preferably 0.5% by mass or more, more preferably 1% by mass or more, and even more preferably 2% by mass or more.

[0041] The conductive pigment paste is a conductive pigment paste containing a pigment dispersion resin (A), a conductive pigment (B), a solvent (C), and optionally a fluororesin (D), wherein the pigment dispersion resin (A) preferably has at least one polar functional group selected from the group consisting of an amide group, an imide group, a hydroxyl group, a carboxyl group, a sulfonic acid group, a phosphate group, a silanol group, a cyano group, a pyrrolidone group, and an amino group, and the concentration of the polar functional group in the pigment dispersion resin (A) is preferably 0.3 mmol / g or more and 23 mmol / g or less. Furthermore, the conductive pigment paste preferably further contains a highly polar, low-molecular-weight component (E) as needed.

[0042] In the dispersing step of step 2, the above-mentioned components can be uniformly mixed and dispersed using a conventionally known dispersing machine, such as a paint shaker, sand mill, ball mill, pebble mill, LMZ mill, DCP pearl mill, planetary ball mill, homogenizer, twin-screw kneader, thin film rotary high-speed mixer (manufactured by Filmix, trade name "Clearmix", etc.), etc. The order in which the components are mixed is not particularly limited.

[0043] Pigment Dispersion Resin (A) The pigment dispersion resin (A) preferably has at least one alkyl group having 12 or more carbon atoms. The alkyl group having 12 or more carbon atoms can be any known alkyl group (hydrocarbon group) without any particular limitation. A linear or branched alkyl group is preferred, and a linear alkyl group is more preferred. The alkyl group having 12 or more carbon atoms is preferably an alkyl group having 12 or more but less than 30 carbon atoms, more preferably an alkyl group having 15 or more but less than 26 carbon atoms, and even more preferably an alkyl group having 19 or more but less than 24 carbon atoms. The alkyl group having 12 or more carbon atoms can be introduced into the resin by (co)polymerizing a polymerizable monomer containing an alkyl group having 12 or more carbon atoms. Examples of polymerizable monomers containing an alkyl group having 12 or more carbon atoms include lauryl (meth)acrylate, stearyl (meth)acrylate, isostearyl (meth)acrylate, behenyl (meth)acrylate, lauryl (meth)acrylamide, stearyl (meth)acrylamide, and behenyl (meth)acrylamide. These can be used alone or in combination of two or more. It is believed that when the pigment dispersing resin (A) has a relatively bulky side chain of an alkyl group having 12 or more carbon atoms, the pigment dispersibility and storage stability are improved due to steric repulsion.

[0044] Furthermore, the pigment dispersion resin (A) preferably has at least one polar functional group selected from the group consisting of an amide group, an imide group, a hydroxyl group, a carboxyl group, a sulfonic acid group, a phosphate group, a silanol group, a cyano group, a pyrrolidone group, and an amino group. When the pigment dispersion resin (A) has a polar functional group, the polar functional group concentration is preferably 0.3 mmol / g or more and 23 mmol / g or less. Furthermore, the acid group may be in the form of a salt. Among these, it is preferable to use at least an amide group, a hydroxyl group, a carboxyl group, a sulfonic acid group, a phosphate group, and an amino group as the polar functional group, and it is more preferable to use at least a hydroxyl group, a carboxyl group, and an amino group.

[0045] The type of resin is not particularly limited as long as it is a resin other than the fluororesin (D) described below. Examples include acrylic resins, polyester resins, epoxy resins, polyether resins, alkyd resins, urethane resins, polyvinyl alcohol, polyvinyl acetal, polyvinylpyrrolidone, polyvinyl acetate, silicone resins, polycarbonate resins, chlorine-based resins, and composite resins thereof. These resins can be used alone or in combination of two or more.

[0046] Among these, from the viewpoints of pigment dispersibility, storage stability, finish quality, etc., the pigment dispersing resin (A) preferably contains a vinyl (co)polymer (A1) obtained by polymerizing or copolymerizing a monomer containing a polymerizable unsaturated group-containing monomer of the following formula (1), and in particular, an acrylic resin (co)polymerized with at least one polymerizable unsaturated group-containing monomer containing a (meth)acryloyl group is preferred. Note that the "(co)polymer" in the present invention includes both a polymer obtained by polymerizing one type of monomer and a copolymer obtained by copolymerizing two or more types of monomers.

[0047] C(-R) 2 = C(-R) 2... Formula (1) [In the above formula, R may be the same or different and is a hydrogen atom or an organic group.] Examples of the vinyl (co)polymer (A1) include hydroxyl group-containing vinyl (co)polymers, carboxyl group-containing vinyl (co)polymers, amide group-containing vinyl (co)polymers, sulfonic acid group-containing vinyl (co)polymers, phosphate group-containing vinyl (co)polymers, pyrrolidone group-containing vinyl (co)polymers, and amino group-containing (co)polymers. These (co)polymers may be used alone or in combination of two or more.

[0048] Examples of hydroxyl group-containing vinyl (co)polymers include polyhydroxyethyl (meth)acrylate, polyvinyl alcohol, vinyl alcohol-fatty acid vinyl copolymer, vinyl alcohol-ethylene copolymer, vinyl alcohol-(N-vinylformamide) copolymer, copolymers of hydroxyethyl (meth)acrylate with other polymerizable unsaturated monomers, etc. The vinyl alcohol units in the (co)polymer may be those obtained by (co)polymerizing fatty acid vinyl units and then hydrolyzing them.

[0049] Examples of the carboxyl group-containing vinyl (co)polymer include a polymer of (meth)acrylic acid, and a copolymer of poly(meth)acrylic acid and other polymerizable unsaturated monomers.

[0050] Examples of the amide group-containing vinyl (co)polymer include a polymer of (meth)acrylamide, and a copolymer of (meth)acrylamide and other polymerizable unsaturated monomers.

[0051] Examples of sulfonic acid group-containing vinyl (co)polymers include polymers of allylsulfonic acid or styrenesulfonic acid, and copolymers of allylsulfonic acid and / or styrenesulfonic acid with other polymerizable unsaturated monomers.

[0052] Examples of the phosphoric acid group-containing vinyl (co)polymer include a polymer of (meth)acryloyloxyalkyl acid phosphate, and a copolymer of (meth)acryloyloxyalkyl acid phosphate with other polymerizable unsaturated monomers.

[0053] Examples of the amino group-containing vinyl (co)polymer include copolymers of N,N-dimethylaminoethyl (meth)acrylate, N,N-diethylaminoethyl (meth)acrylate and other polymerizable unsaturated monomers.

[0054] Examples of other copolymerizable unsaturated monomers include vinyl carboxylate ester monomers such as vinyl formate, vinyl acetate, vinyl propionate, isopropenyl acetate, vinyl valerate, vinyl caprylate, vinyl caprate, vinyl laurate, vinyl stearate, vinyl benzoate, vinyl versatate, and vinyl pivalate; olefins such as ethylene, propylene, and butylene; aromatic vinyls such as styrene and α-methylstyrene; methyl (meth)acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate; Examples of the monomer include ethylenically unsaturated carboxylic acid alkyl ester monomers such as dimethyl fumarate, dimethyl maleate, diethyl maleate, and diisopropyl itaconate; vinyl ether monomers such as methyl vinyl ether, n-propyl vinyl ether, isobutyl vinyl ether, and dodecyl vinyl ether; halogenated vinyl monomers or vinylidene monomers such as vinyl chloride, vinylidene chloride, vinyl fluoride, and vinylidene fluoride; allyl compounds such as allyl acetate and allyl chloride; and quaternary ammonium group-containing monomers such as 3-(meth)acrylamidopropyltrimethylammonium chloride. These monomers can be used singly or in combination of two or more.

[0055] From the viewpoints of pigment dispersibility, storage stability, and compatibility with the solvent, the polar functional group concentration of the pigment dispersing resin (A) is usually 0.3 mmol / g to 23 mmol / g, preferably 0.3 mmol / g to 12 mmol / g, more preferably 0.4 mmol / g to 8.0 mmol / g, even more preferably 0.4 mmol / g to 6.0 mmol / g, and even more preferably 0.4 mmol / g to 2.0 mmol / g.

[0056] The vinyl (co)polymer (A1) can be produced by a polymerization method known per se, and for example, solution polymerization is preferably used, but is not limited thereto, and bulk polymerization, emulsion polymerization, suspension polymerization, etc. When solution polymerization is carried out, it may be continuous polymerization or batch polymerization, and the monomers may be charged all at once or in portions, or may be added continuously or intermittently.

[0057] The polymerization initiator used in the solution polymerization is not particularly limited, but specific examples thereof include azo compounds such as azobisisobutyronitrile, 2,2'-azobis(2-methylbutyronitrile), azobis-2,4-dimethylpaleronitrile, and azobis(4-methoxy-2,4-dimethylpaleronitrile); acetyl peroxide, benzoyl peroxide, lauroyl peroxide, acetylcyclohexylsulfonyl peroxide, and 2,4,4-trimethylpentyl- ... peroxides such as diisopropyl peroxydicarbonate, di-2-ethylhexyl peroxydicarbonate, and diethoxyethyl peroxydicarbonate; perester compounds such as t-butyl peroxyneodecanate, α-cumyl peroxyneodecanate, and t-butyl peroxyneodecanate; and known radical polymerization initiators such as azobisdimethylvaleronitrile and azobismethoxyvaleronitrile can be used.

[0058] The polymerization reaction temperature is not particularly limited, but can usually be set in the range of about 30°C or higher and 200°C or lower.

[0059] The vinyl (co)polymer (A1) obtainable as described above has a degree of polymerization of, for example, 100 or more, preferably 150 or more, and for example, 4,000 or less, preferably 3,000 or less, more preferably 700 or less.

[0060] The weight average molecular weight is, for example, 1,000 or more, preferably 2,000 or more, more preferably 7,000 or more, and for example, 2,000,000 or less, preferably 1,000,000 or less, more preferably 500,000 or less.

[0061] Unless otherwise specified, the weight average molecular weight in this specification is a value obtained by converting the retention time (retention volume) measured using a gel permeation chromatograph (GPC) into the molecular weight of polystyrene using the retention time (retention volume) of a standard polystyrene of known molecular weight measured under the same conditions. Specifically, the gel permeation chromatograph is "HLC8120GPC" (manufactured by Tosoh Corporation, trade name) and four columns, "TSKgel G-4000HXL", "TSKgel G-3000HXL", "TSKgel G-2500HXL" and "TSKgel G-2000HXL" (all manufactured by Tosoh Corporation, trade name), can be measured under the conditions of a mobile phase of tetrahydrofuran, a measurement temperature of 40 ° C, a flow rate of 1 mL / min, and a detector RI.

[0062] After completion of the synthesis, the vinyl (co)polymer (A1) can be converted into a solid or a resin solution in which any solvent has been substituted by removing the solvent and / or replacing the solvent.

[0063] The solvent may be removed by heating at normal pressure or under reduced pressure. The solvent replacement method may involve adding a replacement solvent at any stage before, during, or after the solvent removal.

[0064] In the case of the vinyl (co)polymer (A1), the content of the alkyl group having 12 or more carbon atoms in the dispersion resin (A) is preferably 1 to 100% by mass, more preferably 10 to 90% by mass, even more preferably 20 to 80% by mass, and particularly preferably 30 to 60% by mass, when the total mass of all monomers is taken as 100% by mass. When a compound having a reactive alkyl group having 12 or more carbon atoms is subsequently added to the resin, the content of the alkyl group having 12 or more carbon atoms is calculated based on the mass proportion of the compound.

[0065] When the pigment dispersion resin (A) is converted from a solid state into a resin solution, it is preferable to first mix and dissolve it in a solvent at a liquid temperature of 60°C or higher (preferably 80°C or higher) (the upper limit is 200°C or lower, preferably 100°C or lower) to form a resin solution, and then mix it with other components [components (B), (C), (D), etc.], from the viewpoint of solubility in the solvent. The "liquid temperature" refers to the temperature of the solvent or resin solution at the time of dissolution. The solid pigment dispersion resin (A) may be mixed and dissolved in a solvent at 60°C or higher in advance, or the solid pigment dispersion resin (A) and solvent may be mixed and then heated to a temperature of 60°C or higher. The pigment dispersion resin (A) may also contain components other than the pigment dispersion resin (A) and the solvent. The solvents used may be used alone or in combination of two or more. Suitable solvents include those listed as solvents (C) described below.

[0066] The solid content of the pigment dispersion resin (A) is, based on 100% by mass of the total solid content of the conductive pigment paste, for example, 0.1% by mass or more, preferably 1% by mass or more, and more preferably 3% by mass or more, and for example, 40% by mass or less, preferably 30% by mass or less, and more preferably 20% by mass or less.

[0067] The solid content of the pigment dispersion resin (A), based on 100% by mass of the total amount of the conductive pigment paste, is, for example, 0.1% by mass or more, preferably 0.4% by mass or more, and more preferably 0.7% by mass or more, and for example, 10% by mass or less, preferably 5% by mass or less, and more preferably 2% by mass or less.

[0068] The solid content of the pigment dispersion resin (A) is, based on 100% by mass of the content of the conductive pigment (B), for example, 0.1% by mass or more, preferably 1% by mass or more, and more preferably 5% by mass or more, and for example, 150% by mass or less, preferably 120% by mass or less, and more preferably 80% by mass or less.

[0069] Solvent (C) Suitable solvents for the solvent (C) include water and various organic solvents. Specific examples include hydrocarbon solvents such as n-butane, n-hexane, n-heptane, n-octane, cyclopentane, cyclohexane, and cyclobutane; aromatic solvents such as toluene and xylene; ketone solvents such as methyl isobutyl ketone; ether solvents such as n-butyl ether, dioxane, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, and diethylene glycol; ethyl acetate, n-butyl acetate, isobutyl acetate, ethylene glycol monomethyl ether, and diethylene glycol; Examples of suitable solvents include ester-based solvents such as ethyl ether acetate and butyl carbitol acetate; ketone-based solvents such as methyl ethyl ketone, methyl isobutyl ketone and diisobutyl ketone; alcohol-based solvents such as ethanol, isopropanol, n-butanol, sec-butanol and isobutanol; and amide-based solvents such as Equamide (an amide-based solvent, trade name, manufactured by Idemitsu Kosan Co., Ltd.), N,N-dimethylformamide, N,N-dimethylacetamide, N-methylformamide, N-methylacetamide, N-methylpropioamide and N-methyl-2-pyrrolidone.

[0070] Among these, amide solvents are preferred, and N-methyl-2-pyrrolidone is more preferred. These solvents can be used alone or in combination of two or more.

[0071] Furthermore, from the viewpoint of pigment dispersibility in the conductive pigment paste and preventing deterioration or hydrolysis of the resin component, it is preferable that the conductive pigment paste be substantially free of water. Here, "substantially free of water" means that the water content is typically 1% by mass or less, preferably 0.5% by mass or less, and particularly preferably 0.1% by mass or less, based on 100% by mass of the total amount of the conductive pigment paste. In the present invention, the water content of the conductive pigment paste can be measured by Karl Fischer coulometric titration. Specifically, the measurement can be performed using a Karl Fischer moisture meter (manufactured by Kyoto Electronics Manufacturing Co., Ltd., product name "MKC-610"), with the temperature of the moisture vaporizer (manufactured by Kyoto Electronics Manufacturing Co., Ltd., product name "ADP-611") attached to the device set to 130°C.

[0072] When an amide compound (solvent) such as N-methyl-2-pyrrolidone is used, an amine component may be contained as an impurity, and in the conductive pigment paste of the present invention, the viscosity or tendency to thicken may vary from lot to lot depending on the amine component as an impurity.

[0073] Furthermore, when the conductive pigment paste of the present invention is used to form an electrode layer by the method described below, the solvent and other components volatilize and do not remain. However, it is preferable to recover and reuse the volatilized solvent in order to reduce waste, be environmentally friendly, and / or reduce raw material costs. That is, it is preferable to use a recycled product as the solvent (C). This recycled solvent (recycled product) will also contain the amine compound (E1) originally contained in the conductive pigment paste of the present invention, which will also result in differences in the viscosity or thickening tendency of the conductive pigment paste from lot to lot. Furthermore, amine compounds often have a strong odor.

[0074] Therefore, it is preferable to control and adjust the content of the amine compound in the recycled solvent (C) to a certain amount or less, and the content of the amine compound is usually 1% by mass or less, preferably 0.5% by mass or less, and particularly preferably 0.1% by mass or less.

[0075] The content of the amine compound can be quantified by a general analysis such as ion chromatography-mass spectrometry (IC-MS). The content can be quantified by preparing a calibration curve in advance for the peaks of amine species that are expected to be present.

[0076] The above phrase "a recycled product is used as the solvent (C)" means that the solvent (C) used in the conductive pigment paste of the present invention contains 10 mass % or more (preferably 20 mass % or more) of a recycled product.

[0077] The content of the solvent (C) in the conductive pigment paste is, based on 100% by mass of the total amount of the conductive pigment paste, for example, 40% by mass or more, preferably 60% by mass or more, and more preferably 80% by mass or more, and for example, 99% by mass or less, preferably 98% by mass or less, and more preferably 97% by mass or less. Furthermore, the solid content of the conductive pigment paste is, based on 100% by mass of the total amount of the conductive pigment paste, for example, 1% by mass or more, preferably 2% by mass or more, and more preferably 3% by mass or more, and for example, 60% by mass or less, preferably 40% by mass or less, and more preferably 20% by mass or less.

[0078] Fluororesin (D) The fluororesin (D) is a resin intended for forming a film of an electrode layer, and can be contained in the conductive pigment paste as necessary, and preferably contains the fluororesin (D). In addition, the fluororesin (D) is an essential component of the composite paste described below.

[0079] As the fluororesin (D), polyvinylidene fluoride (PVDF) is particularly preferred, and one type may be used alone or two or more types may be used in combination. The polyvinylidene fluoride may be variously modified, and from the viewpoint of adhesion to the substrate, it is preferred that the polyvinylidene fluoride has a polar functional group.

[0080] The fluororesin (D) may be contained during pigment dispersion, or may be added after pigment dispersion. Alternatively, it may be contained during the production of a composite paste, which will be described later. The weight-average molecular weight of the fluororesin (D) is, from the viewpoints of adhesion to the substrate, reinforcement of film properties, and solvent resistance, for example, 100,000 or more, preferably 500,000 or more, more preferably 650,000 or more, and for example, 3,000,000 or less, preferably 2,000,000 or less.

[0081] When the fluororesin (D) is contained, the content thereof is, based on 100 mass% of the solid content of the conductive pigment paste, for example, 10.0 mass% or more, preferably 30.0 mass% or more, more preferably 40.0 mass% or more, and for example, 99.0 mass% or less, preferably 80.0 mass% or less, more preferably 60.0 mass% or less. Also, based on 100 mass% of the total amount of the conductive pigment paste, the content thereof is, for example, 0.1 mass% or more, preferably 0.5 mass% or more, more preferably 1 mass% or more, and for example, 10 mass% or less, preferably 7 mass% or less, more preferably 5 mass% or less.

[0082] When converting the fluororesin (D) from a solid state into a resin solution, from the viewpoint of solubility in the solvent, it is preferable to first mix and dissolve the fluororesin with a solvent at a liquid temperature of 40°C or higher (preferably 60°C or higher, more preferably 80°C or higher) (the upper limit is 200°C or lower, preferably 100°C or lower) to form a resin solution, and then mix and disperse the fluororesin with the conductive pigment composition. The "liquid temperature" refers to the temperature of the solvent or resin solution at the time of dissolution. The solid fluororesin (D) may be mixed and dissolved in a solvent at 40°C or higher in advance, or the solid fluororesin (D) and solvent may be mixed and heated to 40°C or higher. The mixture may also contain components other than the fluororesin (D) and the solvent. When the above-mentioned hot dissolution is performed, the fluororesin (D) is preferably polyvinylidene fluoride (or a modified product thereof). The solvents used may be one type alone or two or more types in combination, and the types listed above for the solvent (C) can be suitably used. Furthermore, it is preferable to cool the hot-dissolved resin solution as described above to a predetermined temperature of 10°C or higher but lower than 40°C, and from the viewpoint of preventing precipitation, it is preferable that the cooling step be performed at a cooling rate of 0.5°C / min or higher (preferably 1°C / min or higher) defined by the following formula: cooling rate = (solution temperature at start of cooling - solution temperature at end of cooling) / cooling time.

[0083] Highly Polar, Low-Molecular-Weight Component (E) The highly polar, low-molecular-weight component (E) is a component that increases the wettability and / or storage stability of the conductive pigment, and examples thereof include known basic components and acidic components. Among these, it is preferable that the highly polar, low-molecular-weight component (E) contains an amine compound (E1).

[0084] The content of the amine compound (E1) in the highly polar, low-molecular-weight component (E) is, for example, 50% by mass or more, preferably 75% by mass or more, and more preferably 95% by mass or more, based on 100% by mass of the highly polar, low-molecular-weight component (E).

[0085] Examples of the amine compound (E1) include ammonia, primary amines, secondary amines, and tertiary amines.

[0086] Examples of primary amines include ethylamine, n-propylamine, sec-propylamine, n-butylamine, sec-butylamine, i-butylamine, tert-butylamine, pentylamine, hexylamine, heptylamine, octylamine, decylamine, laurylamine, myristyrylamine, 1,2-dimethylhexylamine, 3-pentylamine, 2-ethylhexylamine, allylamine, aminoethanol, 1-aminopropanol, 2-aminopropanol, aminobutanol, aminopentanol, aminohexanol, 3-ethoxypropylamine, 3-propoxypropylamine, 3-isopropoxypropylamine, 3-butoxypropylamine, 3-isobutoxypropylamine, 3-(2-ethylhexyloxy)propylamine, aminocyclopentane, aminocyclohexane, aminonorbornene, aminomethylcyclohexane, aminobenzene, benzylamine, phenethylamine, α-phenylethylamine, naphthylamine, Primary monoamines such as furfurylamine; ethylenediamine, 1,2-diaminopropane, 1,3-diaminopropane, 1,2-diaminobutane, 1,3-diaminobutane, 1,4-diaminobutane, 1,5-diaminopentane, 1,6-diaminohexane, 1,7-diaminoheptane, 1,8-diaminooctane, dimethylaminopropylamine, diethylaminopropylamine, bis-(3-aminopropyl)ether, 1,2-bis-(3-aminopropoxy)ethane, 1,3-bis -(3-aminopropoxy)-2,2'-dimethylpropane, aminoethylethanolamine, 1,2-bisaminocyclohexane, 1,3-bisaminocyclohexane, 1,4-bisaminocyclohexane, 1,3-bisaminomethylcyclohexane, 1,4-bisaminomethylcyclohexane, 1,3-bisaminoethylcyclohexane, 1,4-bisaminoethylcyclohexane, 1,3-bisaminopropylcyclohexane, 1,4-bisaminopropylcyclohexane, hydrogenated 4,4'-Diaminodiphenylmethane, 2-aminopiperidine, 4-aminopiperidine, 2-aminomethylpiperidine, 4-aminomethylpiperidine, 2-aminoethylpiperidine, 4-aminoethylpiperidine, N-aminoethylpiperidine, N-aminopropylpiperidine, N-aminoethylmorpholine, N-aminopropylmorpholine, isophoronediamine, menthanediamine, 1,4-bisaminopropylpiperazine, o-phenylenediamine, m-phenylenediamine, p-phenylenediamine, 2,4-tolylenediamine, 2,6-tolylenediamine, 2,4-toluenediamine, m-aminobenzylamine, 4-chloro-o-phenylenediamine, tetrachloro-p-xylylenediamine, 4-methoxy-6-methyl-m-phenylenediamine, m-xylylenediamine, p-xylylenediamine, 1,5-naphthalenediamine, 2,6-naphthalenediamine, benzidine, 4,4'-bis( o-toluidine), dianisidine, 4,4'-diaminodiphenylmethane, 2,2-(4,4'-diaminodiphenyl)propane, 4,4'-diaminodiphenyl ether, 4,4'-thiodianiline, 4,4'-diaminodiphenyl sulfone, 4,4'-diaminoditolyl sulfone, methylenebis(o-chloroaniline), 3,9-bis(3-aminopropyl)2,4,8,10-tetraoxaspiro[5,5]undecane, diethylenetriamine, Examples of the primary polyamines include iminobispropylamine, methyliminobispropylamine, bis(hexamethylene)triamine, triethylenetetramine, tetraethylenepentamine, pentaethylenehexamine, N-aminoethylpiperazine, N-aminopropylpiperazine, 1,4-bis(aminoethylpiperazine), 1,4-bis(aminopropylpiperazine), 2,6-diaminopyridine, and bis(3,4-diaminophenyl)sulfone.

[0087] Examples of secondary amines include diethylamine, dipropylamine, di-n-butylamine, di-sec-butylamine, diisobutylamine, di-n-pentylamine, di-3-pentylamine, dihexylamine, dioctylamine, di(2-ethylhexyl)amine, methylhexylamine, diallylamine, pyrrolidine, piperidine, 2,4-lupethidine, 2,6-lupethidine, 3,5-lupethidine, diphenylamine, Secondary monoamines such as N-methylaniline, N-ethylaniline, dibenzylamine, methylbenzylamine, dinaphthylamine, pyrrole, indoline, indole, and morpholine; N,N'-dimethylethylenediamine, N,N'-dimethyl-1,2-diaminopropane, N,N'-dimethyl-1,3-diaminopropane, N,N'-dimethyl-1,2-diaminobutane, N,N'-dimethyl-1,3-diaminobutane, N,N' -dimethyl-1,4-diaminobutane, N,N'-dimethyl-1,5-diaminopentane, N,N'-dimethyl-1,6-diaminohexane, N,N'-dimethyl-1,7-diaminoheptane, N,N'-diethylethylenediamine, N,N'-diethyl-1,2-diaminopropane, N,N'-diethyl-1,3-diaminopropane, N,N'-diethyl-1,2-diaminobutane, N,N'-diethyl-1,3-diaminobutane and secondary polyamines such as hexane, N,N'-diethyl-1,4-diaminobutane, N,N'-diethyl-1,6-diaminohexane, piperazine, 2-methylpiperazine, 2,5-dimethylpiperazine, 2,6-dimethylpiperazine, homopiperazine, 1,1-di-(4-piperidyl)methane, 1,2-di-(4-piperidyl)ethane, 1,3-di-(4-piperidyl)propane, and 1,4-di-(4-piperidyl)butane.

[0088] Examples of tertiary amines include trimethylamine, triethylamine, tri-n-propylamine, tri-iso-propylamine, tri-1,2-dimethylpropylamine, tri-3-methoxypropylamine, tri-n-butylamine, tri-iso-butylamine, tri-sec-butylamine, tri-pentylamine, tri-3-pentylamine, tri-n-hexylamine, tri-n-octylamine, tri-2-ethylhexylamine, tri-dodecylamine, tri-laurylamine, dicyclohexylethylamine, cyclohexyldiethylamine, tri-cyclohexylamine, N,N-dimethylhexylamine, N-methyldihexylamine, N,N-dimethylcyclohexylamine, N-methyldicyclohexylamine, N,N-diethylethanolamine, N,N-dimethylethanolamine, N-ethyldiethanolamine, triethanolamine, tribenzylamine, N,N-dimethylbenzylamine, diethylbenzylamine, tertiary monoamines such as diphenylamine, triphenylamine, N,N-dimethylamino-p-cresol, N,N-dimethylaminomethylphenol, 2-(N,N-dimethylaminomethyl)phenol, N,N-dimethylaniline, N,N-diethylaniline, pyridine, quinoline, N-methylmorpholine, N-methylpiperidine, 2-(2-dimethylaminoethoxy)-4-methyl-1,3,2-dioxabornane, and 2-, 3-, and 4-picoline; tetramethylethylenediamine , pyrazine, N,N'-dimethylpiperazine, N,N'-bis((2-hydroxy)propyl)piperazine, hexamethylenetetramine, N,N,N',N'-tetramethyl-1,3-butanamine, 2-dimethylamino-2-hydroxypropane, diethylaminoethanol, N,N,N-tris(3-dimethylaminopropyl)amine, 2,4,6-tris(N,N-dimethylaminomethyl)phenol, heptamethylisobiguanide, and other tertiary polyamines.

[0089] These may be used alone or in combination of two or more.

[0090] Of these, primary amine compounds are preferred, and monoamine compounds (monoamines) are more preferred.

[0091] Examples of the amine compound (E1) include alkanolamines, aliphatic amines, alicyclic amines, and aromatic amines, and any of these can be suitably used, with aromatic amines being preferred.

[0092] Since it is preferable that no amine compound remains in the electrode layer after drying, the weight-average molecular weight of the amine compound (E1) is preferably less than 1,000, more preferably 800 or less, even more preferably 500 or less, particularly preferably 350 or less, and even more preferably 250 or less. For the same reason, the boiling point of the amine compound is preferably 400°C or less, more preferably 300°C or less, and even more preferably 200°C or less. Furthermore, if the boiling point is low, there is a possibility of volatilization during production or storage, and furthermore, from the viewpoint of odor, the lower limit is preferably 50°C or more, more preferably 100°C or more. Furthermore, the amine value of the amine compound (E1) is usually 5 mgKOH / g or more, preferably 50 mgKOH / g or more, more preferably 105 mgKOH / g or more, and is usually within the range of 1,000 mgKOH / g or less.

[0093] As the other highly polar, low-molecular-weight component, for example, an acidic highly polar, low-molecular-weight component selected from organic acids and inorganic acids can be used alone or in combination with two or more thereof in combination with the amine compound (E1). Also, a basic highly polar, low-molecular-weight component selected from organic bases and inorganic bases can be used alone or in combination with two or more thereof. Examples of organic acids include organic carboxylic acids (formic acid, acetic acid, propionic acid, benzoic acid, phthalic acid, etc.) and organic sulfonic acids (benzenesulfonic acid, etc.). Examples of inorganic acids include hydrochloric acid, sulfuric acid, nitric acid, phosphoric acid, etc., and their acid anhydrides can also be used.

[0094] Examples of the organic base include basic components other than amine compounds, and examples of the inorganic base include metal hydroxides (sodium hydroxide, potassium hydroxide, etc.).

[0095] The content of the highly polar, low-molecular-weight component (E) is, for example, 1% by mass or more, preferably 1.5% by mass or more, and more preferably 2% by mass or more, based on 100% by mass of the solid content of the conductive pigment paste, and is, for example, 600% by mass or less, preferably 300% by mass or less, and more preferably 50% by mass or less.

[0096] Furthermore, based on 100% by mass of the solid content of the conductive pigment (B), the lower limit is, for example, 1% by mass or more, preferably 2% by mass or more, and more preferably 5% by mass or more. The upper limit is, for example, 1,000% by mass or less, preferably 500% by mass or less, and more preferably 50% by mass or less. Based on 100% by mass of the total amount of the conductive pigment paste, the lower limit is, for example, 0.01% by mass or more, preferably 0.05% by mass or more, and more preferably 0.1% by mass or more. The upper limit is, for example, 10% by mass or less, preferably 5% by mass or less, and more preferably 1% by mass or less.

[0097] The highly polar, low-molecular-weight component (E) [especially the amine compound (E1)] often has a strong odor, which can worsen the working environment during blending or the drying process. Furthermore, it is generally expensive, which can increase costs. Therefore, it is necessary to limit the content to the minimum necessary.

[0098] The content ratio of the solvent (C) to the highly polar, low-molecular-weight component (E) is preferably within a range of 100 / 0.01 to 100 / 10, more preferably 100 / 0.02 to 100 / 7, even more preferably 100 / 0.05 to 100 / 5, and even more preferably 100 / 0.1 to 100 / 4, in terms of the mass ratio of the solvent (C) to the highly polar, low-molecular-weight component (E).

[0099] Other Components The conductive pigment paste may further contain other components in addition to the above-described components (A), (B), and (C), and the components (D) and (E) that may be contained as necessary.

[0100] Examples of other components include resins other than the pigment dispersing resin (A) and the fluororesin (D), neutralizing agents, antifoaming agents, preservatives, rust inhibitors, plasticizers, and pigments other than the conductive pigment (B).

[0101] Examples of pigments other than the conductive pigment (B) include white pigments such as titanium white and zinc oxide; blue pigments such as cyanine blue and indanthrene blue; green pigments such as cyanine green and verdigris; organic red pigments such as azo-based and quinacridone-based pigments, red pigments such as red iron oxide; organic yellow pigments such as benzimidazolone-based, isoindolinone-based, isoindoline-based, and quinophthalone-based pigments; and yellow pigments such as titanium yellow and yellow lead. These pigments can be used alone or in combination of two or more. These pigments other than the conductive pigment (B) can be used for purposes such as color adjustment and film property reinforcement, as long as they do not significantly impair conductivity. They may be dispersed simultaneously with the pigment dispersion resin (A) and the conductive pigment (B), or they may be dispersed in the pigment dispersion resin (A) and the conductive pigment (B) to form a paste and then mixed as a pigment or pigment paste.

[0102] The content of pigments other than the conductive pigment (B) is preferably 10 mass% or less, more preferably 5 mass% or less, and even more preferably 1 mass% or less, based on 100 mass% of all pigments in the conductive pigment paste, and it is particularly preferable that no pigments are substantially contained.

[0103] The viscosity of the conductive pigment paste is determined from the viewpoint of pigment dispersibility and storage stability, and is set to a value of 2 s -1 The viscosity at 1000 kJ / min is, for example, less than 5,000 mPa·s, preferably less than 2,500 mPa·s, more preferably less than 1,000 mPa·s, and is, for example, 10 mPa·s or more, preferably 50 mPa·s or more, more preferably 100 mPa·s or more.

[0104] The viscosity can be measured using, for example, a cone and plate viscometer (manufactured by HAAKE, trade name "Mars2", diameter 35 mm, cone and plate tilted at 2°).

[0105] [Method for producing a composite paste (for lithium ion secondary batteries)] Step 3 (electrode active material mixing step) In the production method of the present invention, first, a conductive pigment paste containing a conductive pigment is prepared by the steps 1 and 2. Furthermore, in step 3 (electrode active material mixing step), the conductive pigment paste and at least one electrode active material (F) are mixed to produce a composite paste for a lithium ion secondary battery.

[0106] The solids content of the electrode active material (F), based on 100% by mass of the total amount of the composite paste, is preferably typically 10% by mass or more, and preferably 20% by mass or more, and is preferably typically 99% by mass or less, and preferably 95% by mass or less, which is suitable from the standpoint of battery performance. The fluororesin (D), which was an optional component in the conductive pigment paste, is an essential component in the composite paste and is always contained therein. The solids content of the fluororesin (D), based on 100% by mass of the total amount of the composite paste, is preferably typically 0.05% by mass or more, and preferably 0.1% by mass or more, and is preferably typically 10% by mass or less, and preferably 2% by mass or less, which is suitable from the standpoint of battery performance, paste viscosity, and the like.

[0107] In the mixing step of step 3, the composite paste can be mixed uniformly using a conventionally known mixer and disperser.

[0108] The solid content of the pigment dispersion resin (A) in the solid content of the composite paste is usually 0.01% by mass or more, preferably 0.05% by mass or more, based on 100% by mass of the total amount of the composite paste, and is usually 10% by mass or less, preferably 1% by mass or less, which is suitable from the viewpoints of battery performance, paste viscosity, etc.

[0109] In the composite paste of the present invention, from the viewpoint of storage stability (suppression of thickening) of the composite paste, a high-polarity, low-molecular-weight component (E) is contained, and it is preferable that the high-polarity, low-molecular-weight component (E) contains at least one amine compound (E1). From the viewpoint of alleviating aggregation between the conductive pigment (B) and the electrode active material (F) by bringing the high-polarity, low-molecular-weight component (E) into contact with (wetting) the conductive pigment (B), and then mixing the electrode active material (F), it is preferable to include a sequence of first mixing the conductive pigment (B) and the high-polarity, low-molecular-weight component (E).

[0110] The solid content of the conductive pigment (B) in the composite paste solid content of the present invention is usually 0.01% by mass or more, preferably 0.05% by mass or more, more preferably 0.1% by mass or more, based on 100% by mass of the total amount of the composite paste. It is usually 30% by mass or less, preferably 10% by mass or less, more preferably 5% by mass or less, which is suitable from the viewpoint of battery performance. Furthermore, the content of the solvent (C) in the composite paste of the present invention is usually 1% by mass or more, preferably 4% by mass or more, more preferably 7% by mass or more, based on 100% by mass of the total amount of the composite paste. It is usually 90% by mass or less, preferably 70% by mass or less, more preferably 50% by mass or less, which is suitable from the viewpoint of electrode drying efficiency and paste viscosity.

[0111] The composite paste is suitable for use as a positive or negative electrode for a lithium ion secondary battery, and is preferably used as a positive electrode.

[0112] Electrode active material (F) Examples of the electrode active material (F) include lithium nickel oxide (LiNiO 2 ), lithium manganese oxide (LiMn 2 O 4 ), lithium cobalt oxide (LiCoO 2 ), LiNi 1/3 Co 1/3 Mn 1/3 O 2 lithium composite oxides such as lithium iron phosphate (LiFePO 4), sodium composite oxide, potassium composite oxide, etc. These electrode active materials (F) can be used singly or in combination of two or more. The electrode active material containing lithium iron phosphate is inexpensive and has relatively good cycle characteristics and energy density, and therefore can be suitably used.

[0113] The particle size of the electrode active material is usually 0.5 μm or more, preferably 10.5 μm or more, and usually 30 μm or less, preferably 20 μm or less.

[0114] The solid content of the electrode active material (F) in 100% by mass of the solid content of the lithium ion secondary battery electrode composite paste of the present invention is usually 50% by mass or more, preferably 60% by mass or more, and is preferably less than 100% by mass from the viewpoints of battery capacity, battery resistance, etc.

[0115] When the electrode active material (F) is contained in the composite paste, the paste may thicken during storage. The reason for this is that the electrode active material (F) has alkali metal hydroxides (e.g., LiOH, KOH, NaOH, etc.) derived from the raw materials on the particle surface, which is thought to cause aggregation (thickening) due to the conductive pigment (B) having an acidic surface. Therefore, by containing a certain amount or more of the highly polar, low-molecular-weight component (E) [particularly the amine compound (E1)], the thickening of the composite paste during storage can be suppressed.

[0116] Furthermore, the electrode active material (F) of the present invention can be suitably used as an electrode active material composite (F-1) in which at least a portion of its surface is covered with carbon nanotubes. The composite (F-1) can be obtained by previously mixing the electrode active material (F), carbon nanotubes, and, if necessary, other components (e.g., a solvent or a dispersion resin). If necessary, a drying step can be performed after mixing, thereby enabling the carbon nanotubes to be more uniformly adsorbed and / or fixed to the electrode active material (F). Furthermore, the electrode active material composite (F-1) produced as described above can form a uniform conductive network around the electrode active material by adsorbing and / or fixing the carbon nanotubes to the surface of the electrode active material. As the carbon nanotubes that can be used in the electrode active material composite (F-1), any known carbon nanotubes can be used without particular limitation, but the carbon nanotubes listed for the carbon nanotubes (B1) can be suitably used.

[0117] [Lithium-ion secondary battery electrode] Method for producing electrode layer for lithium-ion secondary battery As described above, an electrode layer for a lithium-ion secondary battery (also referred to as an electrode mixture layer or a mixture layer) can be produced by applying a mixture paste for a lithium-ion secondary battery to the surface of a core material (current collector) of a positive electrode or a negative electrode and drying the applied paste, and is particularly preferably used for a positive electrode.

[0118] The conductive pigment paste obtained by the manufacturing method of the present invention can be used not only as a paste for a composite layer (electrode layer) but also as a primer layer (also referred to as a functional layer or adhesive layer) between an electrode core material and a composite layer (electrode layer). The lithium-ion secondary battery composite paste can be applied by a known method using a die coater or the like. The amount of the lithium-ion secondary battery composite paste applied is not particularly limited, but can be set so that the thickness of the composite layer after drying is, for example, 0.04 mm or more, preferably 0.06 mm or more, and, for example, 0.30 mm or less, preferably 0.24 mm or less. The temperature of the drying step can be appropriately set within a range of, for example, 80°C or more, preferably 100°C or more, and, for example, 250°C or less, preferably 200°C or less. The drying time can be appropriately set within a range of, for example, 5 seconds or more, and, for example, 120 minutes or less, preferably 60 minutes or less.

[0119] In the drying step, all or part of the solvent (C) and the highly polar, low-molecular-weight component (E) that may be contained as needed volatilize. As described above, in order to reduce waste, be environmentally friendly, and / or reduce costs, it is preferable to recover and reuse the volatilized components (C) and (E).

[0120] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these specific embodiments. In each example, "parts" means parts by mass and "%" means % by mass.

[0121] [Preparation of Dispersion Resin] Preparation Example 1: A reaction vessel equipped with a thermometer, thermostat, stirrer, reflux condenser, and water separator was charged with 75 parts of N-methyl-2-pyrrolidone (Note 1) and heated to 120°C in a nitrogen stream. Once the temperature reached 120°C, a mixture of the monomer species shown in Table 1 below (100 parts in total) and 2 parts of 2,2'-azobis(2-methylbutyronitrile) was added dropwise over 3 hours. After the addition was completed, the mixture was aged at 120°C for 30 minutes, and then a mixture of 1 part of 2,2'-azobis(2-methylbutyronitrile) and 20 parts of N-methyl-2-pyrrolidone (Note 1) was added dropwise over 1 hour. After further aging at 120°C for 1 hour, the mixture was cooled, and N-methyl-2-pyrrolidone (Note 1) was added to obtain an acrylic resin (A1) with a solids content of 50%. The polar functional group concentration was 1.3 mmol / g.

[0122] (Note 1) N-methyl-2-pyrrolidone: Water content 500 ppm (Note 2), amine content 500 ppm (Note 2), recycled product (Note 2) Water content and amine content were measured using a Karl Fischer moisture meter (Kyoto Electronics Manufacturing Co., Ltd., product name "MKC-610") and ion chromatography (Shimadzu Corporation, product name "Prominence HIC-NS").

[0123] Production Example 2 Acrylic resin (A2) with a solids content of 50% was obtained in the same manner as in Production Example 1, except that the monomer species shown in Table 1 below were used. The weight-average molecular weight of the obtained resin is shown in Table 1 below. In the table, "resin A1" means acrylic resin (A1), and "resin A2" means acrylic resin (A2).

[0124]

[0125] The abbreviations for the monomer species in Table 1 above are as follows: SLMA: lauryl methacrylate (having a hydrocarbon group with 12 carbon atoms) BEMA: behenyl methacrylate (having a hydrocarbon group with 22 carbon atoms) St: styrene DMAEMA: N,N-dimethylaminoethyl methacrylate.

[0126] [Pulverization of Carbon Nanotubes (CNT)] Production Example 3 Using a continuous dry bead mill "Drystar SDA1" (manufactured by Ashizawa Finetech Co., Ltd.), carbon nanotubes (CNT1 (Table 2 below)) were pulverized for 1 hour at a feed rate of 0.5 kg / hr using zirconia beads (diameter 3.0 mm), a filling rate of 70%, and a mill peripheral speed of 5.0 m / s, to obtain a pulverized carbon nanotube product (C1-1). When the G / D ratio of the carbon nanotubes before pulverization is α and the G / D ratio after pulverization is β, β / α was 0.97. The G / D ratio was measured by the method described below.

[0127] Production Example 4 Using a continuous dry bead mill "Drystar SDA1" (manufactured by Ashizawa Finetech Co., Ltd.), carbon nanotubes (CNT1 (Table 2 below)) were pulverized for 2 hours at a feed rate of 0.5 kg / hr using zirconia beads (diameter 3.0 mm), a filling rate of 70%, and a mill peripheral speed of 5.0 m / s, to obtain a pulverized carbon nanotube product (C1-2). When the G / D ratio of the carbon nanotubes before pulverization is α and the G / D ratio after pulverization is β, β / α was 0.95. The G / D ratio was measured by the method described below.

[0128] Production Example 5 Using a continuous dry bead mill "Drystar SDA1" (manufactured by Ashizawa Finetech Co., Ltd.), carbon nanotubes (CNT2 (Table 2 below)) were pulverized for 2 hours at a feed rate of 0.5 kg / hr using zirconia beads (diameter 3.0 mm), a filling rate of 70%, and a mill peripheral speed of 5.0 m / s, to obtain a pulverized carbon nanotube product (C2-2). When the G / D ratio of the carbon nanotubes before pulverization is α and the G / D ratio after pulverization is β, β / α was 0.95. The G / D ratio was measured by the method described below.

[0129] Production Example 6 Using a continuous dry bead mill "Drystar SDA1" (manufactured by Ashizawa Finetech Co., Ltd.), carbon nanotubes (CNT3 (Table 2 below)) were pulverized for 1 hour at a feed rate of 0.5 kg / hr using zirconia beads (diameter 3.0 mm), a filling rate of 70%, and a mill peripheral speed of 5.0 m / s, to obtain a pulverized carbon nanotube product (C3-1). When the G / D ratio of the carbon nanotubes before pulverization is α and the G / D ratio after pulverization is β, β / α was 0.97. The G / D ratio was measured by the method described below.

[0130]

[0131] The carbon nanotubes are all multi-walled carbon nanotubes. The median diameter (D50), G / D ratio, specific surface area (BET specific surface area), and amount of acidic groups in Table 2 were measured by the methods described below.

[0132] [Production of Conductive Pigment Paste and Composite Paste] Example 1A 5,000 parts of N-methyl-2-pyrrolidone (Note 1), 200 parts of crushed carbon nanotubes (C1-2), 80 parts of polyvinylpyrrolidone (solids content: 40 parts) (Note 3) as a dispersing resin, 1,800 parts of a resin solution of KF Polymer W#7300 (manufactured by Kureha Corporation, trade name, polyvinylidene fluoride, weight average molecular weight: 1,000,000) (solids content: 180 parts) (Note 4), and 25 parts of benzylamine as an amine were mixed in a container with stirring, and finally, N-methyl-2-pyrrolidone (Note 1) was added to adjust the total mass to 10,000 parts. Subsequently, the mixture was dispersed in a ball mill for 4 hours to produce a conductive pigment paste (A-1). (Note 3) Polyvinylpyrrolidone: Weight average molecular weight (Mw) 12,000, polar functional group concentration 9.0 (mmol / g) (Note 4) The polyvinylidene fluoride resin solution was prepared by mixing and dissolving polyvinylidene fluoride and N-methyl-2-pyrrolidone (Note 1) at a temperature of 80°C in advance, and then cooling the mixture to 30°C over 40 minutes to obtain a resin solution.

[0133] Examples 2A to 10A, Comparative Examples 1A to 2A Conductive pigment pastes (A-2) to (A-12) were obtained in the same manner as in Example 1A, except that the dispersion resin, carbon nanotubes (CNT), and amine were used in the formulations shown in Table 3 below. Note that in the comparative examples, carbon nanotubes [CNT1 (C1-0)] that had not been pulverized (dry dispersed) were used. The results of the evaluation tests of the conductive pigment pastes described below are also shown in Table 3 below.

[0134]

[0135] The blending amount of the dispersing resin in Table 3 above is the value of the solid content. The composition of the dispersing resin in Table 3 above is as follows: Polyvinyl butyral: average degree of polymerization 600, hydroxyl group content 12 mol%, butyral group content 87 mol%, acetyl group content 1 mol%, polar functional group concentration 1.0 (mmol / g) Polymethyl methacrylate: weight average molecular weight 20,000, methyl methacrylate homopolymer, polar functional group concentration 0 (mmol / g). The boiling points and molecular weights of the amines in Table 3 above are as follows: Benzylamine: boiling point 185°C, molecular weight 107 Aminomethylpropanol: boiling point 166°C, molecular weight 89.

[0136] Example 1B 100 parts of the conductive pigment paste (A-1) were mixed with electrode active material particles (composition formula LiNi 0.5 Mn 1.5 O 4 Lithium nickel manganese oxide particles with a spinel structure represented by the formula (I), an average particle diameter of 6 μm, and a BET specific surface area of ​​0.7 m 2 900 parts of the mixture (1000 parts / g) was mixed in a disperser to prepare a composite paste (B-1).

[0137] Examples 2B to 10B, Comparative Examples 1B to 2B Composite pastes (B-2) to (B-12) were obtained in the same manner as in Example 1B except for the formulations shown in Table 4 below. The results of the evaluation tests of the composite pastes described below are also shown in Table 3 above.

[0138]

[0139] <Median diameter (D50)> The median diameter (D50) was measured using a laser diffraction / scattering particle size distribution analyzer "LA-960" (trade name, manufactured by HORIBA) according to the following procedure.

[0140] [Preparation of Aqueous Dispersion Medium] 0.10 g of F10MC (trade name, manufactured by Nippon Paper Industries Co., Ltd., carboxymethylcellulose sodium (hereinafter also referred to as CMCNa)) was added to 100 mL of distilled water, and the mixture was stirred at room temperature for 24 hours or more to dissolve, thereby preparing an aqueous dispersion medium containing 0.1 mass % CMCNa.

[0141] [Preparation of CMCNa Aqueous Solution] 2.0 g of F10MC (trade name, carboxymethylcellulose sodium, manufactured by Nippon Paper Industries Co., Ltd.) was added to 100 mL of distilled water and dissolved by stirring at room temperature for 24 hours or more to prepare a 2.0 mass % aqueous solution of CMCNa.

[0142] [Pretreatment before measurement] 6.0 mg of carbon nanotubes were weighed into a vial, and 6.0 g of the aqueous dispersion medium was added. An ultrasonic homogenizer (Microtec Nichion Corporation, "SmurtNR-50") was used for pretreatment before measurement. The tip was confirmed to be free of deterioration, and the tip was adjusted so that it was immersed 10 mm or more below the surface of the sample being treated. A carbon nanotube aqueous dispersion was prepared by homogenizing the solution through ultrasonic irradiation using auto-power operation with a constant output power, with a time set (irradiation time) of 40 seconds, a power set of 50%, and a start power of 50% (output of 50%).

[0143] [Measurement] Using the carbon nanotube aqueous dispersion, the proportion of dispersed carbon nanotube particles of 1 μm or less and the median diameter (D50) were measured according to the following method. The optical model of the LS 13 320 Universal Liquid Module was set to a refractive index of 1.520 for carbon nanotubes and 1.333 for water. After module cleaning, approximately 1.0 mL of CMCNa aqueous solution was filled. After performing offset measurement, optical axis adjustment, and background measurement at a pump speed of 50%, the prepared carbon nanotube aqueous dispersion was added to a particle size distribution analyzer so that the relative concentration (relative concentration), which indicates the percentage of light scattered outside the beam by particles, was 8-12% or the PIDS was 40-55%. The dispersion was then subjected to ultrasonic irradiation at 78 W for 2 minutes (measurement pretreatment) using the particle size distribution analyzer accessory. After circulating for 30 seconds to remove air bubbles, the particle size distribution was measured. A graph of particle size (particle diameter) versus volume % was obtained, and the proportion of dispersed particles of 1 μm or less and the median diameter (D50) were determined. For each carbon nanotube sample, three measurement samples were collected from different locations and particle size distribution was measured, and the proportion of dispersed particles of 1 μm or less and the median diameter (D50) were calculated as the average value.

[0144] <G / D ratio of carbon nanotubes> The Raman spectrum of the carbon nanotubes was measured by placing the carbon nanotubes in a Raman microscope (manufactured by Horiba, Ltd., product name "XploRA") and using a laser wavelength of 532 nm. -1 More than 1600cm -1 The maximum peak intensity within the following range is G, 1310 cm -1 More than 1350cm -1 The G / D ratio of the carbon nanotube was determined by setting the maximum peak intensity within the following range as D.

[0145] <Specific surface area (BET specific surface area)> The BET specific surface area of ​​the carbon nanotubes was measured in accordance with JIS Z8830:2013 using a specific surface area measuring device (BERSORP-MAX (Microtrac Bell Co., Ltd.)). 2 / g) was measured.

[0146] <Amount of Acidic Groups in Carbon Nanotubes (CNT)> 2 g of CNT was weighed out, immersed in 50 ml of a 0.01 M benzylamine / n-methylpyrrolidone solution, and dispersed for 1 hour using an ultrasonic irradiator. The solution was then centrifuged, and the supernatant was filtered. The benzylamine remaining in the resulting filtrate was quantitatively analyzed by potentiometric titration with 0.1 M hydrochloric acid, and the amount of acidic groups (mmol / g) per 1 g of the resulting CNT was determined.

[0147] Evaluation Tests Evaluation tests were carried out on the conductive pigment pastes and composite pastes obtained in the above Examples and Comparative Examples. If there was even one unacceptable evaluation result, the evaluation was deemed unacceptable.

[0148] <Dispersibility> The dispersibility of the obtained conductive pigment paste was evaluated using a particle gauge according to the dispersion test of JIS K-5600-2-5, based on the following criteria. C and D are failures. A: The pigment is dispersed at less than 10 μm. Dispersibility is very good. B: The pigment is dispersed at 10 μm or more and less than 20 μm. Dispersibility is somewhat good. C: The pigment is dispersed at 20 μm or more, but no agglomerates are visible to the naked eye. Dispersibility is somewhat poor. D: Agglomerates are visible to the naked eye. Dispersibility is very poor.

[0149] <Volume Resistivity (Conductivity)> The volume resistivity of the obtained conductive pigment paste was further measured. For the volume resistivity measurement, a 5 mass% solution of polyvinylidene fluoride (manufactured by Kureha Corporation, product name "KF Polymer W#7300", solvent: N-methyl-2-pyrrolidone) was used as the binder. The conductive pigment paste and KF Polymer W#7300 solution were weighed out so that the ratio of the mass of the conductive pigment (B) in the obtained conductive pigment paste to the total mass of the solid content of the pigment dispersion resin (A) and the solid content of the KF Polymer W#7300 in the conductive pigment paste was 5:100, and mixed for 2 minutes using an ultrasonic homogenizer to obtain a measurement sample. The measurement sample was applied to a glass plate (2 mm × 100 mm × 150 mm) using a doctor blade method and dried by heating at 80°C for 60 minutes to form a coating film on the glass plate. After measuring the film thickness of the obtained coating film, the resistance value was measured with a resistivity meter (manufactured by Mitsubishi Chemical Analytech Co., Ltd., trade name "MCP-TP03P") using an ASP probe (manufactured by Mitsubishi Chemical Analytech Co., Ltd., trade name "Loresta-GP MCP-T610"), and the volume resistivity was calculated by multiplying the obtained resistance value by a resistivity correction factor (RCF) of 4.532 and the film thickness of the coating film. The volume resistivity was evaluated according to the following criteria. D is unacceptable. A: The volume resistivity is less than 7 Ω cm and the conductivity is good. B: The volume resistivity is 7 Ω cm or more and less than 15 Ω cm and the conductivity is normal. D: The volume resistivity is 15 Ω cm or more and the conductivity is poor.

[0150] <Initial Viscosity> The obtained composite paste was measured at a shear rate of 2.0 sec using a cone and plate viscometer (manufactured by HAAKE, product name "Mars2", diameter 35 mm, cone and plate tilted at 2°). -1 The viscosity was measured and evaluated according to the following criteria. D is unacceptable. A: The viscosity is less than 10 Pa·s. B: The viscosity is 10 Pa·s or more and less than 20 Pa·s. C: The viscosity is 20 Pa·s or more and less than 50 Pa·s. D: The viscosity is 50 Pa·s or more.

[0151] [Production of Battery Electrode Layer] Application Examples 1C to 10C The composite pastes obtained in Examples 1B to 10B were applied to both sides of a long aluminum foil (positive electrode current collector) having an average thickness of 15 μm in a weight per side of 10 mg / cm 2 The positive electrode layer was formed by applying the mixture in a strip shape by a roller coating method so that the solid content was 100% (based on the solid content) and drying (drying temperature 180°C, 10 minutes). The positive electrode active material layer (positive electrode layer) supported on the positive electrode current collector was rolled using a roll press to adjust the properties. The resulting electrode layer had a residual solvent content of less than 1% and was an electrode layer with good finish.

Claims

1. A method for producing a conductive pigment paste containing a pigment dispersing resin (A), a conductive pigment (B), a solvent (C), and a fluororesin (D) that can be included as necessary, the method comprising the steps of sequentially carrying out the following steps: step 1: pulverizing a conductive pigment composition having a pigment concentration of the conductive pigment (B) of 50 mass% or more using a pulverizer; and step 2: mixing and dispersing components containing the pigment dispersing resin (A), the solvent (C), and the fluororesin (D) that can be included as necessary into the conductive pigment composition obtained in step 1.

2. A method for producing a conductive pigment paste according to claim 1, characterized in that the conductive pigment (B) contains carbon nanotubes (B1).

3. In the carbon nanotubes (B1) before and after the crushing in step 1, the following (1) and (2) are -1 More than 1600cm -1 The maximum peak intensity within the following range is G, 1310 cm -1 More than 1350cm -1 The method for producing a conductive pigment paste according to claim 2, wherein the G / D ratio of the carbon nanotubes (B1) before pulverization is 0.1 or more and 5.0 or less, when the maximum peak intensity within the following range is D: (2) When the G / D ratio of the carbon nanotubes (B1) before pulverization is α and the G / D ratio of the carbon nanotubes (B1) after pulverization is β, β / α<1.

00.

4. The method for producing a conductive pigment paste according to claim 1, characterized in that the pigment dispersing resin (A) has at least one alkyl group having 12 or more carbon atoms.

5. A method for producing a conductive pigment paste according to claim 1, characterized in that the pigment dispersion resin (A) has at least one polar functional group selected from the group consisting of an amide group, an imide group, a hydroxyl group, a carboxyl group, a sulfonic acid group, a phosphate group, a silanol group, a cyano group, a pyrrolidone group, and an amino group, and the concentration of the polar functional group in the pigment dispersion resin (A) is 0.3 mmol / g to 23 mmol / g.

6. The method for producing a conductive pigment paste according to claim 1, characterized in that the conductive pigment paste contains a fluororesin (D), and the step of mixing the fluororesin (D) includes a step of mixing and dissolving the fluororesin with a solvent having a liquid temperature of 40°C or higher in advance, or a step of mixing the fluororesin (D) with a solvent and then heating the mixture to a temperature of 40°C or higher.

7. The method for producing a conductive pigment paste according to claim 1, wherein the solvent (C) is N-methyl-2-pyrrolidone.

8. The method according to claim 1, characterized in that step 2 includes the steps of: step 2-1: adding components containing the conductive pigment composition in an amount of 70 mass% or less, based on 100 mass% of the total amount of the conductive pigment composition contained in the conductive pigment paste obtained after dispersion, into a disperser, and performing a dispersion treatment; and step 2-2: adding the conductive pigment composition into the disperser until the desired concentration is reached, and performing a dispersion treatment.

9. A method for producing a composite paste for lithium ion secondary batteries, comprising: step 3: mixing at least one type of electrode active material (F) with the conductive pigment paste obtained by the method for producing a conductive pigment paste according to any one of claims 1 to 8.

10. A method for producing an electrode layer for a lithium ion secondary battery, comprising the step of coating a current collector with the composite paste for a lithium ion secondary battery obtained by the method according to claim 9.

11. A method for producing an electrode for a lithium ion secondary battery, comprising the step of applying an electrode insulating part to the end or upper layer of the electrode layer obtained by the method for producing an electrode layer for a lithium ion secondary battery according to claim 10.

Citation Information

Patent Citations

  • Manufacturing method of lithium ion battery, manufacturing device of lithium ion battery and lithium ion battery

    JP2016115576A

  • Method for manufacturing electroconductive paste, and electroconductive paste

    WO2016084697A1

Cited By

  • Carbon nanotube dispersion paste for non-aqueous electrolyte secondary battery, composite paste, and electrode layer for non-aqueous electrolyte secondary battery

    WO2025205322A1

  • Carbon nanotube-dispersed paste, method for producing carbon nanotube-dispersed paste, mixture paste for lithium ion secondary battery, electrode layer for non-aqueous electrolyte lithium ion secondary battery, electrode for non-aqueous electrolyte lithium ion secondary battery, and non-aqueous electrolyte lithium ion secondary battery

    WO2026071079A1