Electrode and all-solid-state battery

By incorporating lithium and Group 3 to 15 elements with sulfur in the solid electrolyte of all-solid-state batteries, optimized through time-of-flight secondary ion mass spectrometry, the ionic conductivity is enhanced, addressing the conductivity gap with conventional electrolytes and improving battery performance and safety.

WO2024204182A1PCT designated stage expired Publication Date: 2024-10-03TDK CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/011923
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-26
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

All-solid-state batteries face challenges in achieving high ionic conductivity in their solid electrolytes, which is essential for improved performance and safety, as conventional solid electrolytes often have lower conductivity compared to organic electrolytes.

Method used

The development of an electrode and all-solid-state battery design that incorporates a solid electrolyte containing lithium, elements from Group 3 to 15, and sulfur, optimized through negative ion analysis using time-of-flight secondary ion mass spectrometry, to enhance ionic conductivity, with specific peak intensity ratios and compound formulations that improve ion mobility.

Benefits of technology

This approach results in a solid electrolyte with increased ionic conductivity, reducing internal resistance and enhancing the performance of all-solid-state batteries, achieving conductivity levels of 0.1 mS/cm or more, depending on the peak intensity ratio, thereby improving safety and output.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024011923_03102024_PF_FP_ABST
    Figure JP2024011923_03102024_PF_FP_ABST
Patent Text Reader

Abstract

This electrode comprises a compound that includes Li, one or more elements selected from Group 3–15 elements, and S. The peak intensity Ra of SO3 - and the peak intensity Rb of SO4 -, which are obtained through negative ion analysis by a time-of-flight secondary ion mass spectrometry, satisfy the relationship Ra > Rb.
Need to check novelty before this filing date? Find Prior Art

Description

Electrodes and all-solid-state batteries

[0001] The present invention relates to an electrode and an all-solid-state battery. This application claims priority to Japanese Patent Application No. 2023-058719, filed on March 31, 2023, the contents of which are incorporated herein by reference.

[0002] In recent years, all-solid-state batteries have been attracting attention from the perspective of improving safety and increasing power output. One of the features of all-solid-state batteries is the use of a solid electrolyte. The properties required of a solid electrolyte include ionic conductivity, redox resistance, and formability. One of the challenges is to improve ionic conductivity compared to conventional organic electrolytes. In general, many solid electrolytes have lower conductivity than organic electrolytes.

[0003] Patent Document 1 discloses a solid electrolyte represented by the following composition formula (1) (where 0<z<2 is satisfied and X is Cl or Br): Li 6-3z Y z X 6 ...Formula (1)

[0004] Patent Document 2 discloses a solid electrolyte made of a compound represented by the following formula (2): AaEbGcXd (where A is at least one element selected from the group consisting of Li, Cs, and Ca, and X is at least one element selected from the group consisting of F, Cl, Br, and I).

[0005] International Publication No. 2018 / 025582 International Publication No. 2021 / 261558

[0006] Such a solid electrolyte is used in a solid electrolyte layer and may also be used together with an active material in an electrode. The solid electrolyte contained in the electrode desirably has high ionic conductivity, similar to the solid electrolyte used in the solid electrolyte layer.

[0007] The present invention has been made in view of the problems of the prior art described above, and provides an electrode and an all-solid-state battery including a solid electrolyte having high ionic conductivity.

[0008] In order to solve the above problems, the present invention provides the following means.

[0009] Aspect 1 of the present invention is a method for producing a zeolite containing Li, one or more elements selected from the group consisting of elements of Groups 3 to 15, and S, and wherein SO 2 is obtained by negative ion analysis using time-of-flight secondary ion mass spectrometry. 3 - Peak intensity Ra and SO 4 - and a peak intensity Rb of Ra satisfying Ra>Rb.

[0010] Aspect 2 of the present invention is directed to the electrode of aspect 1, wherein the compound is SO 3 - Peak intensity Ra and SO 4 - The peak intensity ratio R1 (Ra / Rb) of the peak intensity Rb to the peak intensity Rb satisfies 6.0>R1>1.0.

[0011] Aspect 3 of the present invention is directed to the electrode of aspect 1, wherein the compound is SO 3 - Peak intensity Ra and SO 4 - The peak intensity ratio R1 (Ra / Rb) of the peak intensity Rb to the peak intensity Rb satisfies 1.8>R1>1.2.

[0012] Aspect 4 of the present invention is directed to the electrode of aspect 1, wherein the compound is SO 3 - Peak intensity Ra and SO 4 - The peak intensity ratio R1 (Ra / Rb) of the peak intensity Rb to the peak intensity Rb satisfies 1.7>R1>1.4.

[0013] Aspect 5 of the present invention is an electrode according to any one of Aspects 1 to 4, wherein the compound is a compound that ... - Peak, SO 2 - Peak, SO 3 - Peak, SO 4 - The peaks of SO 3 - The peak of has the strongest peak intensity.

[0014] A sixth aspect of the present invention is the electrode of any one of the first to fifth aspects, wherein the compound is represented by the following formula (1): LiaEbGcXd (1) (in formula (1), E is at least one element selected from the group consisting of Al, Sc, Y, Zr, Hf, and lanthanoids, and G is SO 3 , S.O. 4 , S.O. 5 , S 2 O 3 , S 2 O 4 , S 2 O 5 , S 2 O 6 , S 2 O 7 , S 2 O 8 X is at least one element selected from the group consisting of F, Cl, Br, and I. 0.5≦a<6, 0<b<2, 0.1<c≦6, and 0<d≦6.1.

[0015] A seventh aspect of the present invention is an all-solid-state battery in which a positive electrode and a negative electrode face each other via a solid electrolyte layer, and at least one of the solid electrolyte layer, the positive electrode, and the negative electrode includes an electrode according to any one of Aspects 1 to 6.

[0016] Aspect 8 of the present invention is the all-solid-state battery of aspect 7, wherein the solid electrolyte layer contains a compound represented by the following formula (2): LiaEbGcXd (2) (in formula (2), E is at least one element selected from the group consisting of Al, Sc, Y, Zr, Hf, and lanthanoids, and G is SO 3 , S.O. 4 , S.O. 5 , S 2 O 3 , S 2 O 4 , S 2 O 5 , S 2 O 6 , S 2 O 7 , S 2 O 8X is at least one element selected from the group consisting of F, Cl, Br, and I. 0.5≦a<6, 0<b<2, 0.1<c≦6, and 0<d≦6.1.

[0017] According to the electrode of the present invention, it is possible to provide an electrode containing a solid electrolyte having high ionic conductivity.

[0018] 1 is a cross-sectional view of an all-solid-state battery according to an embodiment of the present invention;

[0019] The present embodiment will be described in detail below with reference to the accompanying drawings. The drawings used in the following description may show characteristic portions enlarged for the sake of clarity, and the dimensional proportions of each component may differ from the actual proportions. The materials, dimensions, etc. exemplified in the following description are merely examples, and the present invention is not limited thereto. Appropriate modifications may be made within the scope of the present invention.

[0020] [All-Solid-State Battery] FIG. 1 is a cross-sectional schematic diagram of an all-solid-state battery 100 according to this embodiment. The all-solid-state battery 100 shown in FIG. 1 includes a power generating element 40 and an exterior body 50. The exterior body 50 covers the periphery of the power generating element 40. The power generating element 40 is connected to the outside via a pair of connected terminals 60, 62. Although a stacked-type battery is shown in FIG. 1, a wound-type battery may also be used. The all-solid-state battery 100 is used, for example, in laminated batteries, prismatic batteries, cylindrical batteries, coin batteries, button batteries, etc.

[0021] <Power generating element> The power generating element 40 includes a solid electrolyte layer 10, a positive electrode 20, and a negative electrode 30. The power generating element 40 is charged or discharged by the exchange of ions between the positive electrode 20 and the negative electrode 30 via the solid electrolyte layer 10 and the exchange of electrons via an external circuit.

[0022] In the all-solid-state battery 100 according to this embodiment, at least one of the positive electrode 20 and the negative electrode 30 contains Li, one or more elements selected from the group consisting of elements of Groups 3 to 15, and S in the electrode mixture layer, and SO 3 - Peak intensity Ra and SO4 - The following description will be given taking as an example a case where the compound is contained in both the positive electrode 20 and the negative electrode 30.

[0023] 1, the positive electrode 20 has a plate-shaped (foil-shaped) positive electrode current collector 22 and a positive electrode mixture layer 24. The positive electrode mixture layer 24 is in contact with at least one surface of the positive electrode current collector 22.

[0024] (Positive Electrode Current Collector) The positive electrode current collector 22 may be made of any electronically conductive material that is resistant to oxidation during charging and corrosion. The positive electrode current collector 22 may be made of, for example, a metal such as aluminum, stainless steel, nickel, or titanium, or a conductive resin. The positive electrode current collector 22 may be in the form of a powder, foil, punched, or expanded.

[0025] (Positive Electrode Mixture Layer) The positive electrode mixture layer 24 contains a positive electrode active material and a solid electrolyte, and may contain a binder and a conductive additive. Known binders and conductive additives can be used. The conductive additive is, for example, carbon black. The conductive additive may also be vapor-grown carbon fiber, carbon nanotubes, metals, etc.

[0026] (Positive Electrode Active Material) The positive electrode active material is not particularly limited as long as it can reversibly absorb and release lithium ions, and insert and extract (intercalate and deintercalate) lithium ions, and any positive electrode active material used in known lithium ion secondary batteries can be used. Examples of the positive electrode active material include lithium-containing metal oxides and lithium-containing metal phosphates.

[0027] The lithium-containing metal oxide is, for example, lithium cobalt oxide (LiCoO 2 ), lithium nickel oxide (LiNiO 2 ), lithium manganese spinel (LiMn 2 O 4 ), and the general formula: LiNi x Co y Mn z O 2 A composite metal oxide represented by (x + y + z = 1), a lithium vanadium compound (LiVOPO 4 , Li3 V 2 (P.O. 4 ) 3 ), olivine-type LiMPO 4 (wherein M represents at least one selected from Co, Ni, Mn, and Fe), lithium titanate (Li 4 Ti 5 O 12 ) etc.

[0028] The positive electrode active material may not contain lithium. Examples of such a positive electrode active material include lithium-free metal oxides (MnO 2 , V 2 O 5 etc.), lithium-free metal sulfides (MoS 2 etc.), lithium-free fluorides (FeF 3 , V.F. 3 When using a positive electrode active material that does not contain lithium, the negative electrode is doped with lithium ions in advance, or a negative electrode containing lithium ions is used.

[0029] The content of the positive electrode active material in the positive electrode mixture layer 24 is not particularly limited, but is preferably 50% by mass to 98% by mass, and more preferably 55% by mass to 95% by mass, based on the total mass of the positive electrode active material, the solid electrolyte, the conductive additive, and the binder.

[0030] (Solid Electrolyte) The solid electrolyte contained in the positive electrode mixture layer 24 contains Li, one or more elements selected from the group consisting of elements of Groups 3 to 15, and S, and is determined to be SO 2 by negative ion analysis using time-of-flight secondary ion mass spectrometry. 3 - Peak intensity Ra and SO 4 -The positive electrode mixture layer 24 includes a compound in which the peak intensity Rb of Ra satisfies Ra > Rb. The configuration in which the solid electrolyte contained in the positive electrode mixture layer 24 includes the compound includes a configuration in which the solid electrolyte contained in the positive electrode mixture layer 24 is made of the compound. The compound itself is a solid electrolyte (solid electrolyte material). Note that a solid electrolyte is a substance that can move ions by applying an external electric field. When the ionic conductivity of the solid electrolyte is high, ions are exchanged smoothly in the all-solid-state battery, and the internal resistance is reduced.

[0031] SO in the compound 3 - Peak intensity Ra and SO 4 - It is preferable that the peak intensity ratio R1 (Ra / Rb) of the peak intensity Rb of the compound satisfies 6.0>R1>1.0. When R1 satisfies this inequality, the ionic conductivity of the compound is 0.1 mS / cm or more. 3 - Peak intensity Ra and SO 4 - It is more preferable that the peak intensity ratio R1 (Ra / Rb) of the peak intensity Rb of the compound satisfies 1.8>R1>1.2. When R1 satisfies this inequality, the ionic conductivity of the compound is 0.5 mS / cm or more. 3 - Peak intensity Ra and SO 4 - It is more preferable that the peak intensity ratio R1 (Ra / Rb) of the peak intensity Rb to the peak intensity Rb of the compound satisfies 1.7 > R1 > 1.4. When R1 satisfies this inequality, the ionic conductivity of the compound is 1 mS / cm or more.

[0032] In addition, the compound was found to be SO - Peak, SO 2 - Peak, SO 3 - Peak, SO 4 - The peaks of SO were detected. 3 -The peak intensity of the peak having the strongest peak can be satisfied.

[0033] (Negative ion analysis by time-of-flight secondary ion mass spectrometry) Time-of-flight secondary ion mass spectrometry (TOF-SIMS) is a technique in which an ion beam (primary ions) is irradiated onto the surface of a solid sample, and the ions (secondary ions) emitted from the surface are mass-separated by utilizing the difference in their time of flight (the time of flight is proportional to the square root of the ion's weight). When measured, TOF-SIMS spectrum data has the horizontal axis as time and the vertical axis as ion counts (intensity), but by converting the time axis to mass number, the horizontal axis becomes mass number, and the mass distribution of the secondary ions, i.e., a mass spectrum, can be obtained.

[0034] "SO 3 - The "peak intensity of SO 3 - The number of detected negative ions is also referred to as "SO 4 - The "peak intensity of SO 4 - (negative ions) detected. 3 - Peak intensity Ra and SO 4 - The peak intensity Rb of the SO 3 - The detected count of negative ions is SO 4 - This means that the number of detected counts is greater than the number of detected counts of negative ions.

[0035] The compound contained in the solid electrolyte contained in the positive electrode mixture layer 24 contains Li, one or more elements selected from the group consisting of elements of Groups 3 to 15, and S, and is found to be SO 4 - The peak intensity of Rb is higher than that of SO 3 - The ionic conductivity can be improved by increasing the peak intensity Ra of SO 4The tetrahedral structure of the SiO2 exhibits high ionic conductivity, and the O (oxygen) bonds to different atoms. 4 - In addition to SO 3 - It is believed that SO 4 It is thought that the difference in structure causes lattice distortion, resulting in high ionic conductivity.

[0036] In the present invention, in a solid electrolyte containing Li, one or more elements selected from the group 3 to 15 elements, and S, 3 - Peak intensity Ra and SO 4 - It was revealed that the peak intensity ratio R1 (Ra / Rb) of the peak intensity Rb to the peak intensity R1 can be used as an index of ionic conductivity.

[0037] The compound can be represented by the following formula (1): LiaEbGcXd (1) (In formula (1), E is at least one element selected from the group consisting of Al, Sc, Y, Zr, Hf, and lanthanoids. G is SO 3 , S.O. 4 , S.O. 5 , S 2 O 3 , S 2 O 4 , S 2 O 5 , S 2 O 6 , S 2 O 7 , S 2 O 8 X is at least one element selected from the group consisting of F, Cl, Br, and I. 0.5≦a<6, 0<b<2, 0.1<c≦6, and 0<d≦6.1.

[0038] In formula (1), a satisfies 0.5≦a<6, and when E is Al, Sc, Y, or a lanthanide, it preferably satisfies 2.0≦a≦4.0, more preferably 2.5≦a≦3.5. When E is Zr or Hf, it is preferable that a satisfies 1.0≦a≦3.0, and more preferably 1.5≦a≦2.5. In the compound represented by formula (1), when a is 0.5≦a<6, the Li content in the compound becomes appropriate, and the ionic conductivity of the solid electrolyte layer 10 becomes high.

[0039] In formula (1), E is an essential component and is at least one element selected from the group consisting of Al, Sc, Y, Zr, Hf, and lanthanoids. E improves the ionic conductivity of the solid electrolyte. b is 0<b<2. Since the effect of including E can be more effectively obtained, b is preferably 0.6≦b. Furthermore, E is an element that forms the skeleton of the solid electrolyte. When b≦b≦1, the solid electrolyte has a low density, which is preferable.

[0040] In the halide-based solid electrolyte represented by formula (1), 0.1<c≦6 is satisfied. c is more preferably 0.5≦c because the effect of widening the potential window on the reduction side due to the inclusion of G is more pronounced. c is preferably c≦3 so that a decrease in the ionic conductivity of the solid electrolyte caused by an excessively high G content does not occur.

[0041] In the halide-based solid electrolyte represented by formula (1), X is an essential component. X is at least one element selected from the group consisting of F, Cl, Br, and I. X has a large ionic radius per valence. Therefore, when the halide-based solid electrolyte represented by formula (1) contains X, lithium ions flow more easily, resulting in an effect of increasing ionic conductivity. X preferably contains Cl, since this results in a solid electrolyte with high ionic conductivity. Furthermore, when X contains F, X preferably contains F and two or more elements selected from the group consisting of Cl, Br, and I, since this results in a solid electrolyte with high ionic conductivity.

[0042] When X is F, the resulting solid electrolyte has sufficiently high ionic conductivity and excellent oxidation resistance. When X is Cl, the resulting solid electrolyte has high ionic conductivity and a good balance of oxidation resistance and reduction resistance. When X is Br, the resulting solid electrolyte has sufficiently high ionic conductivity and a good balance of oxidation resistance and reduction resistance. When X is I, the resulting solid electrolyte has high ionic conductivity.

[0043] In the halide-based solid electrolyte represented by formula (1), d satisfies 0<d≦6.1. d is preferably 1≦d. When d is 1≦d, the strength of the pellet increases when the solid electrolyte is pressure-molded into a pellet. Furthermore, when d is 1≦d, the ionic conductivity of the solid electrolyte increases. Furthermore, d is preferably d≦5 so that an excessively high content of X does not result in a shortage of G, thereby narrowing the potential window of the solid electrolyte.

[0044] The halide-based solid electrolyte represented by formula (1) is, for example, Li 2 Zr(SO 4 ) Cl 4 , Li 2 Zr(SO 3 ) Cl 4 , Li 2 Zr(SO 4 ) 0.3 (SO 3 ) 0.7 Cl 4 , Li 2 Zr(SO 4 ) 0.5 (SO 3 ) 0.5 Cl 4 , Li 2 Zr(SO 4 ) 0.7 (SO 3 ) 0.3 Cl 4 , Li 2 Zr(S 2 O 3 ) Cl 4 , Li 2 Zr(SO 4 ) 0.3 (S 2 O 3 ) 0.7 Cl 4 , Li2 Zr(SO 4 ) 0.5 (S 2 O 3 ) 0.5 Cl 4 , Li 2 Zr(SO 4 ) 0.7 (S 2 O 3 ) 0.3 Cl 4 , is.

[0045] (Binder) The binder bonds the positive electrode active material, the solid electrolyte, and the conductive additive to one another in the positive electrode mixture layer 24, and also firmly bonds the positive electrode mixture layer 24 to the positive electrode current collector 22. The positive electrode mixture layer 24 preferably contains a binder. The binder preferably has oxidation resistance and good adhesiveness.

[0046] Examples of binders used in the positive electrode mixture layer 24 include polyvinylidene fluoride (PVDF) or copolymers thereof, polytetrafluoroethylene (PTFE), polyamide (PA), polyimide (PI), polyamideimide (PAI), polybenzimidazole (PBI), polyethersulfone (PES), polyacrylic acid (PA) and copolymers thereof, metal ion crosslinked polyacrylic acid (PA) and copolymers thereof, maleic anhydride-grafted polypropylene (PP), maleic anhydride-grafted polyethylene (PE), and mixtures thereof. Among these, it is particularly preferable to use PVDF as the binder.

[0047] The content of the solid electrolyte in the positive electrode mixture layer 24 is not particularly limited, but is preferably 1% by mass to 50% by mass, and more preferably 5% by mass to 30% by mass, based on the total mass of the positive electrode active material, the solid electrolyte, the conductive additive, and the binder.

[0048] The binder content in the positive electrode mixture layer 24 is not particularly limited, but is preferably 0.1% by mass to 10% by mass, and more preferably 0.1% by mass to 5% by mass, based on the total mass of the positive electrode active material, solid electrolyte, conductive additive, and binder. If the binder content is too small, it tends to be difficult to form a positive electrode 20 with sufficient adhesive strength. Conversely, if the binder content is too large, general binders are electrochemically inactive and do not contribute to discharge capacity, making it difficult to obtain sufficient volume or mass energy density.

[0049] (Conductive additive) The conductive additive improves the electronic conductivity of the positive electrode mixture layer 24. Known conductive additives can be used. Examples of the conductive additive include carbon materials such as carbon black, graphite, carbon nanotubes, and graphene; metals such as aluminum, copper, nickel, stainless steel, iron, and amorphous metals; conductive oxides such as ITO; and mixtures thereof. The conductive additive may be in the form of powder or fiber.

[0050] There are no particular limitations on the content of the conductive additive in the positive electrode mixture layer 24. When a conductive additive is added, the mass ratio of the conductive additive is usually preferably 0.5% by mass to 20% by mass, and more preferably 1% by mass to 5% by mass, based on the total mass of the positive electrode active material, solid electrolyte, conductive additive, and binder.

[0051] 1, the negative electrode 30 has a negative electrode current collector 32 and a negative electrode mixture layer 34. The negative electrode mixture layer 34 is in contact with the negative electrode current collector 32. In the following description of the "negative electrode," description of components common to the "positive electrode" may be omitted.

[0052] (Negative Electrode Current Collector) The negative electrode current collector 32 may be any material as long as it has electronic conductivity. The negative electrode current collector 32 may be made of, for example, a metal such as copper, aluminum, nickel, stainless steel, or iron, or a conductive resin. The negative electrode current collector 32 may be in the form of a powder, a foil, a punched piece, or an expanded piece.

[0053] (Negative electrode mixture layer) The negative electrode mixture layer 34 includes a negative electrode active material and a solid electrolyte. The negative electrode mixture layer 34 may include a binder and a conductive additive. Known binders and conductive additives can be used. The conductive additive is, for example, carbon black. The conductive additive may be vapor-grown carbon fiber, carbon nanotubes, metals, or the like. The binder and conductive additive may be the same as those described for the positive electrode mixture layer 24 and contained in the same proportions.

[0054] The negative electrode active material is not particularly limited as long as it can reversibly absorb and release lithium ions and insert and extract lithium ions. As the negative electrode active material, any negative electrode active material used in known lithium ion secondary batteries can be used.

[0055] Examples of the negative electrode active material include carbon materials such as natural graphite, artificial graphite, mesocarbon microbeads, mesocarbon fiber (MCF), cokes, glassy carbon, and organic compound sintered bodies; metals that can be combined with lithium, such as Si, SiOx, Sn, and aluminum; alloys of these; composite materials of these metals and carbon materials; and lithium titanate (Li 4 Ti 5 O 12 ), SnO 2 The negative electrode active material is natural graphite or lithium titanate (Li 4 Ti 5 O 12 ) is preferred.

[0056] The content of the negative electrode active material in the negative electrode mixture layer 34 is not particularly limited, but is preferably 50% by mass to 98% by mass, and more preferably 55% by mass to 95% by mass, based on the total mass of the negative electrode active material, the solid electrolyte, the conductive additive, and the binder.

[0057] (Solid Electrolyte) The solid electrolyte contained in the negative electrode mixture layer 34, like the positive electrode mixture layer 24, contains Li, one or more elements selected from the group 3 to group 15 elements, and S, and is determined to be SO by negative ion analysis using time-of-flight secondary ion mass spectrometry. 3 - Peak intensity Ra and SO4 - The negative electrode mixture layer 34 includes a compound in which the peak intensity Rb of the positive electrode mixture layer 24 satisfies Ra>Rb. The configuration in which the solid electrolyte contained in the negative electrode mixture layer 34 includes the compound includes a configuration in which the solid electrolyte contained in the negative electrode mixture layer 34 is made of the compound. The compound may have the same configuration as that described for the positive electrode mixture layer 24. A description thereof will be omitted below.

[0058] The content of the solid electrolyte in the negative electrode mixture layer 34 is not particularly limited, but is preferably 1% by mass to 60% by mass, and more preferably 10% by mass to 55% by mass, based on the total mass of the negative electrode active material, the solid electrolyte, the conductive additive, and the binder.

[0059] The binder content in the negative electrode mixture layer 34 is not particularly limited, but is preferably 0.1% by mass to 10% by mass, and more preferably 0.1% by mass to 5% by mass, based on the total mass of the negative electrode active material, solid electrolyte, conductive additive, and binder. If the binder content is too small, it tends to be difficult to form a negative electrode 30 with sufficient adhesive strength. Conversely, if the binder content is too large, it tends to be difficult to obtain a sufficient volume or mass energy density because general binders are electrochemically inactive and do not contribute to discharge capacity.

[0060] There are no particular limitations on the content of the conductive additive in the negative electrode mixture layer 34. When the conductive additive is added, the mass ratio of the conductive additive is usually preferably 0.5% by mass to 20% by mass, and more preferably 1% by mass to 5% by mass, based on the total mass of the negative electrode active material, solid electrolyte, conductive additive, and binder.

[0061] "Solid Electrolyte Layer" The solid electrolyte layer 10 is sandwiched between the positive electrode 20 and the negative electrode 30. The solid electrolyte layer 10 includes a solid electrolyte that can transfer ions when an external voltage is applied. For example, the solid electrolyte conducts lithium ions and inhibits the transfer of electrons.

[0062] The solid electrolyte may contain, for example, lithium. The solid electrolyte may be, for example, an oxide-based material, a sulfide-based material, or a halide-based material. Furthermore, the compound (solid electrolyte) contained in the electrode according to this embodiment described above may be used or may be contained in part.

[0063] The solid electrolyte may be in the form of a powder (particles) or a sintered body obtained by sintering a powder. The solid electrolyte may also be a compact obtained by compressing a powder, a compact obtained by molding a mixture of a powder and a binder, or a coating formed by applying a coating containing a powder, a binder, and a solvent and then heating to remove the solvent.

[0064] The solid electrolyte may be, for example, a halide-based solid electrolyte represented by the following formula (2): LiaEbGcXd (2)

[0065] In formula (2), a satisfies 0.5≦a<6, and when E is Al, Sc, Y, or a lanthanide, it preferably satisfies 2.0≦a≦4.0, more preferably 2.5≦a≦3.5. When E is Zr or Hf, it is preferable that a satisfies 1.0≦a≦3.0, and more preferably 1.5≦a≦2.5. In the compound represented by formula (2), when a is 0.5≦a<6, the Li content in the compound becomes appropriate, and the ionic conductivity of the solid electrolyte layer 10 becomes high.

[0066] In formula (2), E is an essential component and is at least one element selected from the group consisting of Al, Sc, Y, Zr, Hf, and lanthanoids. E improves the ionic conductivity of the solid electrolyte. b is 0<c<2. Since the effect of including E can be more effectively obtained, b is preferably 0.6≦b. Furthermore, E is an element that forms the skeleton of the solid electrolyte. When b≦b≦1, it is preferable because the solid electrolyte has a low density.

[0067] In the halide-based solid electrolyte represented by formula (2), 0.1<c≦6 is satisfied. c is more preferably 0.5≦c because the effect of widening the potential window on the reduction side due to the inclusion of G is more pronounced. c is preferably c≦3 so as to prevent a decrease in the ionic conductivity of the solid electrolyte caused by an excessively high G content.

[0068] In the halide-based solid electrolyte represented by formula (2), X is an essential component. X is at least one element selected from the group consisting of F, Cl, Br, and I. X has a large ionic radius per valence. Therefore, when the halide-based solid electrolyte represented by formula (2) contains X, lithium ions flow more easily, resulting in an effect of increasing ionic conductivity. X preferably contains Cl, since this results in a solid electrolyte with high ionic conductivity. Furthermore, when X contains F, X preferably contains F and two or more elements selected from the group consisting of Cl, Br, and I, since this results in a solid electrolyte with high ionic conductivity.

[0069] When X is F, the resulting solid electrolyte has sufficiently high ionic conductivity and excellent oxidation resistance. When X is Cl, the resulting solid electrolyte has high ionic conductivity and a good balance of oxidation resistance and reduction resistance. When X is Br, the resulting solid electrolyte has sufficiently high ionic conductivity and a good balance of oxidation resistance and reduction resistance. When X is I, the resulting solid electrolyte has high ionic conductivity.

[0070] In the halide-based solid electrolyte represented by formula (2), d satisfies 0<d≦6.1. d is preferably 1≦d. When d is 1≦d, the strength of the pellet increases when the solid electrolyte is pressure-molded into a pellet. Furthermore, when d is 1≦d, the ionic conductivity of the solid electrolyte increases. Furthermore, d is preferably d≦5 so that an excessively high content of X does not result in a shortage of G, thereby narrowing the potential window of the solid electrolyte.

[0071] The halide-based solid electrolyte represented by formula (2) is, for example, Li 2 Zr(SO 4 ) Cl 4 , Li 2 Zr(SO3 ) Cl 4 , Li 2 Zr(SO 4 ) 0.3 (SO 3 ) 0.7 Cl 4 , Li 2 Zr(SO 4 ) 0.5 (SO 3 ) 0.5 Cl 4 , Li 2 Zr(SO 4 ) 0.7 (SO 3 ) 0.3 Cl 4 , Li 2 Zr(S 2 O 3 ) Cl 4 , Li 2 Zr(SO 4 ) 0.3 (S 2 O 3 ) 0.7 Cl 4 , Li 2 Zr(SO 4 ) 0.5 (S 2 O 3 ) 0.5 Cl 4 , Li 2 Zr(SO 4 ) 0.7 (S 2 O 3 ) 0.3 Cl 4 is.

[0072] The solid electrolyte may be a sulfide-based solid electrolyte, and a compound containing Li, S, Si and / or P may be used as the sulfide-based solid electrolyte. The sulfide-based solid electrolyte may further contain Ge, Cl, Br, or I. The sulfide-based solid electrolyte may be amorphous, crystalline, or of an argyrodite type. Examples of sulfide-based solid electrolytes include Li, 2 S-P 2 S 5 solid electrolyte (Li7P 3 S 11 , Li 3 P.S.4 , Li 8 P 2 S 9 etc.), Li 2 S-SiS 2 , LiI-Li 2 S-SiS 2 , LiI-Li 2 S-P 2 S 5 , LiI-LiBr-Li 2 S-P 2 S 5 , Li 2 S-P 2 S 5 -GeS 2 solid electrolyte (Li 13 GeP 3 S 16 , Li 10 GeP 2 S 12 etc.), LiI-Li 2 S-P 2 O 5 , LiI-Li 3 P.O. 4 -P 2 S 5 , Li 7-x P.S. 6-x Cl x (x is 1.0 to 1.9).

[0073] The sulfide-based solid electrolyte may be a compound represented by the following formula (3): LiqMrPsOtXuSv (3) In formula (3), Li is lithium, M is a tetravalent metal, P is phosphorus, O is oxygen, S is sulfur, X is at least one selected from the group consisting of F, Cl, Br, and I, and q, r, s, t, u, and v are numbers satisfying 1≦q≦20, 0≦r≦2, 1≦s≦5, 0≦t≦5, 0≦u≦5, and v=q / 2+2×r+2.5×s−t−u / 2. M is preferably Si or Ge.

[0074] <Exterior Body> The exterior body 50 houses the power generating element 40 inside. The exterior body 50 prevents moisture and the like from entering from the outside to the inside. As shown in Fig. 1 , the exterior body 50 has a metal foil 52 and a resin layer 54 laminated on each side of the metal foil 52. The exterior body 50 is a metal laminate film in which the metal foil 52 is coated with the resin layer 54 from both sides.

[0075] The metal foil 52 is, for example, aluminum foil or stainless steel foil. The resin layer 54 can be, for example, a resin film such as polypropylene. The materials constituting the inner and outer resin layers 54 may be different. For example, the outer material can be a polymer with a high melting point, such as polyethylene terephthalate (PET) or polyamide (PA), and the inner material can be polyethylene (PE) or polypropylene (PP).

[0076] <Terminals> The terminals 60 and 62 are connected to the positive electrode 20 and the negative electrode 30, respectively. The terminal 62 connected to the positive electrode 20 is a positive electrode terminal, and the terminal 60 connected to the negative electrode 30 is a negative electrode terminal. The terminals 60 and 62 are responsible for electrical connection to the outside. The terminals 60 and 62 are made of a conductive material such as aluminum, nickel, or copper. The connection method may be welding or screw fastening. It is preferable to protect the terminals 60 and 62 with insulating tape to prevent short circuits.

[0077] [Manufacturing Method of All-Solid-State Battery] Next, a manufacturing method of the all-solid-state battery according to this embodiment will be described. The all-solid-state battery according to this embodiment contains the above-mentioned compound (solid electrolyte) in at least one of the positive electrode and the negative electrode. That is, at least one of the positive electrode and the negative electrode contains Li, one or more elements selected from the elements of Groups 3 to 15, and S, and the SO 3 - Peak intensity Ra and SO 4 - The compound includes a compound in which the peak intensity Rb of Ra satisfies Ra>Rb.

[0078] First, a solid electrolyte is prepared. This solid electrolyte includes both the solid electrolyte constituting the solid electrolyte layer and the above-mentioned compound (solid electrolyte) contained in the electrode. The solid electrolyte can be produced, for example, by mixing raw material powders containing predetermined elements in a predetermined molar ratio and causing a mechanochemical reaction. When performing the mechanochemical reaction, the state of SxOy after synthesis is adjusted to be different. Specifically, unreacted components of the raw materials can be left by changing the rotation speed, revolution speed, synthesis time, state of the raw material powder at the time of introduction, and atmosphere inside the pot of the planetary ball mill.

[0079] When a halide raw material is contained in the raw powder, the halide raw material is likely to evaporate when the temperature is increased. Therefore, halogen gas may be present in the sintering atmosphere to compensate for the halogen. Furthermore, when a halide raw material is contained in the raw powder, sintering may be performed by hot pressing using a mold with high airtightness. In this case, the mold has high airtightness, so evaporation of the halide raw material due to sintering can be suppressed. By sintering in this manner, a solid electrolyte in the form of a sintered body made of a compound having a predetermined composition is obtained.

[0080] Next, the positive electrode 20 is prepared. The positive electrode is manufactured by applying a paste containing a positive electrode active material onto a positive electrode current collector 22 and drying it to form a positive electrode mixture layer 24. The above-described solid electrolyte may be added to the paste containing the positive electrode active material.

[0081] Next, the negative electrode 30 is prepared. The negative electrode is manufactured by applying a paste containing a negative electrode active material onto a negative electrode current collector 32 and drying it to form a negative electrode mixture layer 34. The above-described solid electrolyte may be added to the paste containing the negative electrode active material.

[0082] The power generating element 40 can be produced, for example, by powder molding. A guide with a hole is placed on the positive electrode 20, and the guide is filled with a solid electrolyte. The surface of the solid electrolyte is then smoothed, and the negative electrode 30 is placed on top of the solid electrolyte. This sandwiches the solid electrolyte between the positive electrode 20 and the negative electrode 30. Pressure is then applied to the positive electrode 20 and the negative electrode 30 to pressure-molde the solid electrolyte. This pressure molding produces a laminate in which the positive electrode 20, solid electrolyte layer 10, and negative electrode 30 are stacked in this order.

[0083] Next, external terminals are welded to the positive electrode current collector 22 of the positive electrode 20 and the negative electrode current collector 32 of the negative electrode 30, which form the laminate, by a known method, to electrically connect the positive electrode current collector 22 or the negative electrode current collector 32 to the external terminals. Thereafter, the laminate connected to the external terminals is housed in an exterior body 50, and the opening of the exterior body 50 is hermetically sealed by heat sealing. Through the above steps, the all-solid-state battery 100 of this embodiment is obtained.

[0084] The all-solid-state battery 100 according to this embodiment contains the above-described solid electrolyte, and therefore conducts Li ions smoothly and has low internal resistance.

[0085] The above describes the embodiments of the present invention in detail with reference to the drawings. However, each configuration and combination thereof in each embodiment is an example, and additions, omissions, substitutions, and other modifications of the configurations are possible within the scope that does not deviate from the spirit of the present invention.

[0086] <Positive Electrode Examples> [Positive Electrode Example 1] (Preparation of Compound (Solid Electrolyte)) The compound (solid electrolyte) according to this embodiment was prepared as follows. In a glove box filled with an Ar gas atmosphere, lithium sulfate (Li 2 SO 4 ) and zirconium chloride (ZrCl 4) and the raw material powder were weighed so that the molar ratio was 1:1. The raw material powder was charged into a zirconia sealed container for a planetary ball mill, which had zirconia balls already placed therein. Next, a lid was placed on the sealed container, and the lid was screwed onto the container body, and the space between the lid and the container was sealed with polyimide tape. The polyimide tape has the effect of blocking moisture. Next, the zirconia sealed container was set in the planetary ball mill. A mechanochemical reaction was carried out for 24 hours at a rotation speed of 500 rpm and a revolution speed of 500 rpm (the rotation direction and the revolution direction were opposite to each other), and the Li of the positive electrode Example 1 was obtained. 2 Zr(SO 4 ) Cl 4 A powder of 1000 ppm was obtained.

[0087] The planetary ball mill was placed in an Ar gas atmosphere. The zirconia sealed container for the planetary ball mill was screwed and sealed with polyimide tape, and when the zirconia sealed container was set in the planetary ball mill, it was firmly pressed and fixed in place. This structure meant that there was little moisture entering the zirconia sealed container from the atmosphere.

[0088] <Measurement of mass spectrum by TOF-SIMS> The solid electrolyte of positive electrode Example 1 (Li 2 Zr(SO 4 ) Cl 4 ) was measured for mass spectrum by time-of-flight secondary ion mass spectrometry, and SO 3 - Peak intensities Ra and SO 4 - A peak intensity Rb of

[0089] Measurement was performed using the following TOF-SIMS equipment and conditions: (1) Equipment: TOF-SIMS5 manufactured by ION-TOF (2) Measurement conditions Measurement mode: Spectrometry Primary ion: Bi 3 ++ Acceleration voltage: 25 kV Measurement area: 40,000 μm 2 (200μm×200μm) Measuring ion species: Negative Electron neutralization: Yes

[0090] <Measurement of ionic conductivity> The solid electrolyte of positive electrode Example 1 (Li 2 ZrSO 4 Cl 4 The ionic conductivity of the obtained solid electrolyte (Li 2 Zr(SO 4 ) Cl 4 The powder of ) was filled into a die for pressure molding and pressure molded under a load of about 30 KN to prepare a cell for measuring ionic conductivity.

[0091] The pressure molding die is composed of a cylinder made of PEEK (polyether ether ketone) with a diameter of 10 mm, and upper and lower punches made of SKD11 material with a diameter of 9.99 mm.

[0092] Next, a 50 mm diameter, 5 mm thick stainless steel disk and a Teflon (registered trademark) disk with four screw holes were prepared, and the pressure molding die was set up as follows: stainless steel disk / Teflon (registered trademark) disk / pressure molding die / Teflon (registered trademark) disk / stainless steel disk. The four screws were tightened with a torque of approximately 3 N m. Screws were inserted into the screw holes on the sides of the upper and lower punches to form external connection terminals.

[0093] The external connection terminal was connected to a potentiostat (VersaSTAT3 manufactured by Princeton Applied Research) equipped with a frequency response analyzer, and the ionic conductivity was measured using an impedance measurement method. Measurement was performed at a measurement frequency range of 1 MHz to 0.1 Hz, an amplitude of 10 mV, and a temperature of 25°C. The compound (solid electrolyte) (Li 2 Zr(SO 4 ) Cl 4 ) has an ionic conductivity of 2.4 × 10 -3 The viscosity was S / cm.

[0094] (Preparation of Positive Electrode Mixture) To prepare a positive electrode mixture, lithium cobalt oxide (LiCoO 2 ) and Li of positive electrode example 1 2 Zr(SO 4 ) Cl 4 The positive electrode active material and the Li of the positive electrode example 1 were prepared.2 Zr(SO 4 ) Cl 4 The positive electrode active material and the positive electrode active material of Example 1 were weighed out so as to have a concentration of 65 wt % and 35 wt %, respectively. 2 Zr(SO 4 ) Cl 4 The mixture was mixed in an agate mortar for 15 minutes to obtain a positive electrode mixture.

[0095] (Fabrication of charge / discharge half-cells) Fabrication of charge / discharge half-cells was carried out in a glove box with a dew point of approximately -70°C. A pellet fabrication jig was used to prepare the half-cells. The pellet fabrication jig had a PEEK (polyether ether ketone) cylinder with an outer diameter of 30 mm, an inner diameter of 10 mm, and a height of 20 mm, and upper and lower punches with diameters of 9.99 mm. The upper and lower punches were made of die steel (SKD11 material).

[0096] A lower punch is inserted into the PEEK cylinder, and solid electrolyte Li is placed on the lower punch. 2 Zr(SO 4 ) Cl 4 Next, the PEEK cylinder was vibrated to level the surface of the solid electrolyte, and then an upper punch was inserted onto the solid electrolyte, and the solid electrolyte was pressed with a press under a load of 373 MPa to form a solid electrolyte layer.

[0097] Next, the upper punch was removed, and 15 mg of the above-mentioned positive electrode mixture was placed on the solid electrolyte layer. Next, the PEEK cylinder was vibrated to level the surface of the positive electrode mixture, and then the upper punch was inserted onto the positive electrode mixture and pressed with a press under a load of 373 MPa. Next, the lower punch was removed, and a lithium foil with a diameter of 10 mm and a thickness of 100 μm was placed on the solid electrolyte layer, and the lower punch was inserted. The half cell was configured as follows: (LiCoO 2 +Li 2 Zr(SO 4 ) Cl 4 ) / Li 2 Zr(SO 4 ) Cl 4 / Li.

[0098] Two stainless steel plates with a diameter of 50 mm and a thickness of 5 mm and two Bakelite® plates with a diameter of 50 mm and a thickness of 2 mm were also prepared. Four screw holes were then formed in each of the two stainless steel plates and the two Bakelite® plates. The screw holes were positioned so that when the half-cell, the two stainless steel plates, and the two Bakelite® plates were stacked, the two stainless steel plates and the two Bakelite® plates would overlap in plan view, but would not overlap with the half-cell in plan view.

[0099] Next, a stainless steel plate, a Bakelite® plate, a half cell, a Bakelite® plate, and a stainless steel plate were stacked in this order, and screws were inserted into the screw holes and tightened with a torque of 1 N m. In this way, a half cell was obtained in which the upper and lower punches of the electrochemical cell were insulated by the Bakelite® plate. Next, the half cell was left to stand in a thermostatic bath at 25°C for 48 hours to stabilize the open circuit voltage.

[0100] <Measurement of rate characteristics> The fabricated half-cells were charged and discharged under the following conditions. The voltage range was 2.8 V to 4.2 V. Charging was performed at a constant current of 0.1 C, and after the constant voltage, charging was terminated when the current reached a value equivalent to 0.05 C. Discharging was performed at 0.1 C and 1.0 C, and the ratio of the discharge capacity at 1 C to the discharge capacity at 0.1 C, taken as 100%, was determined (rate characteristics (unit: %)). The results are shown in Table 1.

[0101] The combination of raw materials, synthesis time, and characteristics of the synthesis process for the solid electrolyte (compound) of positive electrode example 1 are summarized in Table 1 below. Measurement results of the properties of the solid electrolyte are summarized in Table 2 below. Measurement results of the rate characteristics of the half cell are summarized in Table 3 below. The contents of Tables 1 and 2 are common to the positive electrode example and the negative electrode example; for example, Example 1 refers to the solid electrolyte of positive electrode example 1 and the solid electrolyte of negative electrode example 1.

[0102] [Positive Electrode Example 2] The solid electrolyte of positive electrode example 2 (Li 2 Zr(SO 4 ) Cl 4) was synthesized in the same manner as in Positive Electrode Example 1, except that the raw materials were weighed in a glove box filled with a mixed atmosphere of dry air with a dew point of about -40°C and argon gas at a volume ratio of 20%:80%, and the planetary ball mill was installed in the mixed atmosphere of dry air with a dew point of about -40°C and argon gas at a volume ratio of 20%:80%. 2 Zr(SO 4 ) Cl 4 ) powder was obtained.

[0103] The combination of raw materials, synthesis time, and characteristics of the synthesis process for the solid electrolyte (compound) of Positive Electrode Example 2 are summarized in Table 1 below. The measurement results of the properties of the solid electrolyte are summarized in Table 2 below. The measurement results of the rate characteristics of the half cell are summarized in Table 3 below.

[0104] [Positive Electrode Example 3] The solid electrolyte of positive electrode example 3 (Li 2 Zr(SO 4 ) Cl 4 ) was synthesized in the same manner as in Positive Electrode Example 1, except that the raw materials were weighed in a glove box filled with a mixed atmosphere of dry air with a dew point of about -40°C and argon gas at a volume ratio of 40%:60%, and the synthesis was performed by placing a planetary ball mill in the mixed atmosphere of dry air with a dew point of about -40°C and argon gas at a volume ratio of 40%:60%. 2 Zr(SO 4 ) Cl 4 ) powder was obtained.

[0105] The combination of raw materials, synthesis time, and characteristics of the synthesis process for the solid electrolyte (compound) of Positive Electrode Example 3 are summarized in Table 1 below. The measurement results of the properties of the solid electrolyte are summarized in Table 2 below. The measurement results of the rate characteristics of the half cell are summarized in Table 3 below.

[0106] [Positive Electrode Example 4] The solid electrolyte of positive electrode example 4 (Li 2 Zr(SO 3 ) Cl 4 ) is made from lithium sulfite (Li 2 SO 3 ) and zirconium chloride (ZrCl4 The solid electrolyte (Li) of Positive Electrode Example 4 was synthesized in the same manner as in Positive Electrode Example 1, except that 2 Zr(SO 3 ) Cl 4 ) powder was obtained.

[0107] The combination of raw materials, synthesis time, and characteristics of the synthesis process for the solid electrolyte (compound) of Positive Electrode Example 4 are summarized in Table 1 below. The measurement results of the properties of the solid electrolyte are summarized in Table 2 below. The measurement results of the rate characteristics of the half cell are summarized in Table 3 below.

[0108] [Positive Electrode Example 5] The solid electrolyte of positive electrode example 5 (Li 2 Zr(SO 3 ) Cl 4 ) was synthesized in the same manner as in Example 4, except that the raw materials were weighed in a glove box containing a mixed atmosphere of dry air with a dew point of about -40°C and argon gas at a volume ratio of 40%:60%, and a planetary ball mill was installed in the mixed atmosphere of dry air with a dew point of about -40°C and argon gas at a volume ratio of 40%:60%. 2 Zr(SO 3 ) Cl 4 ) powder was obtained.

[0109] The combination of raw materials, synthesis time, and characteristics of the synthesis process for the solid electrolyte (compound) of Positive Electrode Example 5 are summarized in Table 1 below. The measurement results of the properties of the solid electrolyte are summarized in Table 2 below. The measurement results of the rate characteristics of the half cell are summarized in Table 3 below.

[0110] [Positive Electrode Example 6] The solid electrolyte of positive electrode example 6 (Li 2 Zr(SO 4 ) 0.3 (SO 3 ) 0.7 Cl 4 ) is made from lithium sulfate (Li 2 SO 4 ) and lithium sulfite (Li 2 SO 3 ) and zirconium chloride (ZrCl 4) were weighed out to a molar ratio of 3:7:10 to prepare raw material powders, and the solid electrolyte (Li 2 Zr(SO 4 ) 0.3 (SO 3 ) 0.7 Cl 4 ) powder was obtained.

[0111] The combination of raw materials, synthesis time, and characteristics of the synthesis process for the solid electrolyte (compound) of Positive Electrode Example 6 are summarized in Table 1 below. The measurement results of the properties of the solid electrolyte are summarized in Table 2 below. The measurement results of the rate characteristics of the half cell are summarized in Table 3 below.

[0112] [Positive Electrode Example 7] The solid electrolyte of positive electrode example 7 (Li 2 Zr(SO 4 ) 0.5 (SO 3 ) 0.5 Cl 4 ) is made from lithium sulfate (Li 2 SO 4 ) and lithium sulfite (Li 2 SO 3 ) and zirconium chloride (ZrCl 4 ) were weighed out in a molar ratio of 1:1:2 to prepare raw material powders, and the raw materials were weighed out in a glove box filled with a mixed atmosphere of dry air with a dew point of approximately -40°C and argon gas in a volume ratio of 20%:80%, and the synthesis was performed by placing a planetary ball mill in the same mixed atmosphere of dry air with a dew point of approximately -40°C and argon gas in a volume ratio of 20%:80%. The solid electrolyte (Li 2 Zr(SO 4 ) 0.5 (SO 3 ) 0.5 Cl 4 ) powder was obtained.

[0113] The combination of raw materials, synthesis time, and characteristics of the synthesis process for the solid electrolyte (compound) of Positive Electrode Example 7 are summarized in Table 1 below. The measurement results of the properties of the solid electrolyte are summarized in Table 2 below. The measurement results of the rate characteristics of the half cell are summarized in Table 3 below.

[0114] [Positive Electrode Example 8] The solid electrolyte of positive electrode example 8 (Li 2 Zr(SO 4 ) 0.7 (SO 3 ) 0.3 Cl 4 ) is made from lithium sulfate (Li 2 SO 4 ) and lithium sulfite (Li 2 SO 3 ) and zirconium chloride (ZrCl 4 ) were weighed out in a molar ratio of 7:3:10 to prepare raw material powders, and the raw materials were weighed out in a glove box filled with a mixed atmosphere of dry air with a dew point of approximately -40°C and argon gas in a volume ratio of 40%:60%, and the synthesis was performed by placing a planetary ball mill in the same mixed atmosphere of dry air with a dew point of approximately -40°C and argon gas in a volume ratio of 40%:60%. The solid electrolyte (Li 2 Zr(SO 4 ) 0.7 (SO 3 ) 0.3 Cl 4 ) powder was obtained.

[0115] The combination of raw materials, synthesis time, and characteristics of the synthesis process for the solid electrolyte (compound) of positive electrode example 8 are summarized in Table 1 below. The measurement results of the properties of the solid electrolyte are summarized in Table 2 below. The measurement results of the rate characteristics of the half cell are summarized in Table 3 below.

[0116] [Positive Electrode Example 9] The solid electrolyte of positive electrode example 9 (Li 2 Zr(S 2 O 3 ) Cl 4 ) is made by using Li as a raw material. 2 S 2 O 3 and zirconium chloride (ZrCl4 ) was used in the same manner as in Positive Electrode Example 1, and the solid electrolyte (Li 2 Zr(S 2 O 3 ) Cl 4 ) powder was obtained.

[0117] The combination of raw materials, synthesis time, and characteristics of the synthesis process for the solid electrolyte (compound) of Positive Electrode Example 9 are summarized in Table 1 below. The measurement results of the properties of the solid electrolyte are summarized in Table 2 below. The measurement results of the rate characteristics of the half cell are summarized in Table 3 below.

[0118] [Positive Electrode Example 10] The solid electrolyte of positive electrode example 10 (Li 2 Zr(S 2 O 3 ) Cl 4 ) was synthesized in the same manner as in Positive Electrode Example 9, except that the raw materials were weighed in a glove box filled with a mixed atmosphere of dry air with a dew point of about -40°C and argon gas at a volume ratio of 40%:60%, and the planetary ball mill was installed in the mixed atmosphere of dry air with a dew point of about -40°C and argon gas at a volume ratio of 40%:60%, and the Li 2 Zr(S 2 O 3 ) Cl 4 The powder obtained was:

[0119] The combination of raw materials, synthesis time, and characteristics of the synthesis process for the solid electrolyte (compound) of Positive Electrode Example 10 are summarized in Table 1 below. The measurement results of the properties of the solid electrolyte are summarized in Table 2 below. The measurement results of the rate characteristics of the half cell are summarized in Table 3 below.

[0120] [Positive Electrode Example 11] The solid electrolyte of positive electrode example 11 (Li 2 Zr(SO 4 ) 0.3 (S 2 O 3 ) 0.7 Cl 4 ) is made from lithium sulfate (Li 2 SO 4 ) and Li 2 S 2 O 3and zirconium chloride (ZrCl 4 ) were weighed out to a molar ratio of 3:7:10 to prepare raw material powders, respectively. The solid electrolyte (Li 2 Zr(SO 4 ) 0.3 (S 2 O 3 ) 0.7 Cl 4 The powder obtained was:

[0121] The combination of raw materials, synthesis time, and characteristics of the synthesis process for the solid electrolyte (compound) of Positive Electrode Example 11 are summarized in Table 1 below. The measurement results of the properties of the solid electrolyte are summarized in Table 2 below. The measurement results of the rate characteristics of the half cell are summarized in Table 3 below.

[0122] [Positive Electrode Example 12] The solid electrolyte of positive electrode example 12 (Li 2 Zr(SO 4 ) 0.5 (S 2 O 3 ) 0.5 Cl 4 ) is made from lithium sulfate (Li 2 SO 4 ) and Li 2 S 2 O 3 and zirconium chloride (ZrCl 4 ) were weighed out in a molar ratio of 1:1:2 to prepare raw material powders, and the raw materials were weighed out in a glove box filled with a mixed atmosphere of dry air with a dew point of approximately -40°C and argon gas in a volume ratio of 20%:80%, and the synthesis was performed by placing a planetary ball mill in the same mixed atmosphere of dry air with a dew point of approximately -40°C and argon gas in a volume ratio of 20%:80%. The solid electrolyte (Li 2 Zr(SO 4 ) 0.5 (S 2 O 3 ) 0.5 Cl 4 ) powder was obtained.

[0123] The combination of raw materials, synthesis time, and characteristics of the synthesis process for the solid electrolyte (compound) of Positive Electrode Example 12 are summarized in Table 1 below. The measurement results of the properties of the solid electrolyte are summarized in Table 2 below. The measurement results of the rate characteristics of the half cell are summarized in Table 3 below.

[0124] [Positive Electrode Example 13] The solid electrolyte of positive electrode example 13 (Li 2 Zr(SO 4 ) 0.7 (S 2 O 3 ) 0.3 Cl 4 ) is made from lithium sulfate (Li 2 SO 4 ) and Li 2 S 2 O 3 and zirconium chloride (ZrCl 4 ) were weighed out in a molar ratio of 7:3:10 to prepare raw material powders, and the raw materials were weighed out in a glove box filled with a mixed atmosphere of dry air with a dew point of approximately -40°C and argon gas in a volume ratio of 40%:60%, and the synthesis was performed by placing a planetary ball mill in the same mixed atmosphere of dry air with a dew point of approximately -40°C and argon gas in a volume ratio of 40%:60%. The solid electrolyte (Li 2 Zr(SO 4 ) 0.7 (S 2 O 3 ) 0.3 Cl 4 ) powder was obtained.

[0125] The combination of raw materials, synthesis time, and characteristics of the synthesis process for the solid electrolyte (compound) of Positive Electrode Example 13 are summarized in Table 1 below. The measurement results of the properties of the solid electrolyte are summarized in Table 2 below. The measurement results of the rate characteristics of the half cell are summarized in Table 3 below.

[0126] [Positive Electrode Example 14] The solid electrolyte of positive electrode example 14 (Li 6 P.S. 5 Cl) is lithium sulfide (Li 2 S) and phosphorus sulfide (P 2 S 5The solid electrolyte (LiCl) of cathode example 14 was synthesized in the same manner as cathode example 1, except that raw material powders were prepared by weighing out lithium chloride (LiCl) and lithium fluoride (LiCl) in a molar ratio of 5:1:2, and all of the raw material powders were added at the same time. 6 P.S. 5 Cl) powder was obtained.

[0127] The combination of raw materials, synthesis time, and characteristics of the synthesis process for the solid electrolyte (compound) of positive electrode Example 14 are summarized in Table 1 below. The measurement results of the properties of the solid electrolyte are summarized in Table 2 below. The measurement results of the rate characteristics of the half cell are summarized in Table 3 below.

[0128] [Positive Electrode Example 15] The solid electrolyte of positive electrode example 15 (Li 9.54 Si 1.74 P 1.44 S 11.7 Cl 0.3 ) is lithium sulfide (Li 2 S) and silicon sulfide (SiS 2 ) and phosphorus sulfide (P 2 S 5 The solid electrolyte (LiCl) was synthesized in the same manner as in Example 1 except that raw material powders were prepared by weighing out the raw material powders in a molar ratio of 4.62:1.74:0.72:0.3, and the raw material powders were all added at the same time. 9.54 Si 1.74 P 1.44 S 11.7 Cl 0.3 ) was synthesized.

[0129] The combination of raw materials, synthesis time, and characteristics of the synthesis process for the solid electrolyte (compound) of Positive Electrode Example 15 are summarized in Table 1 below. The measurement results of the properties of the solid electrolyte are summarized in Table 2 below. The measurement results of the rate characteristics of the half cell are summarized in Table 3 below.

[0130] [Positive Electrode Example 16] The solid electrolyte of positive electrode example 16 (Li 2 Zr(SO 3 ) Cl 4 ) was synthesized in the same manner as in Positive Electrode Example 4, except that the mechanochemical reaction was carried out for 48 hours, and a solid electrolyte (Li2 Zr(SO 3 ) Cl 4 ) powder was obtained.

[0131] The combination of raw materials, synthesis time, and characteristics of the synthesis process for the solid electrolyte (compound) of Positive Electrode Example 16 are summarized in Table 1 below. The measurement results of the properties of the solid electrolyte are summarized in Table 2 below. The measurement results of the rate characteristics of the half cell are summarized in Table 3 below.

[0132] [Positive Electrode Example 17] The solid electrolyte of positive electrode example 17 (Li 2 Zr(SO 3 ) Cl 4 ) was synthesized in the same manner as in Positive Electrode Example 4, except that the mechanochemical reaction was carried out for 72 hours, and a solid electrolyte (Li 2 Zr(SO 3 ) Cl 4 ) powder was obtained.

[0133] The combination of raw materials, synthesis time, and characteristics of the synthesis process for the solid electrolyte (compound) of positive electrode Example 17 are summarized in Table 1 below. The measurement results of the properties of the solid electrolyte are summarized in Table 2 below. The measurement results of the rate characteristics of the half cell are summarized in Table 3 below.

[0134] <Comparative Positive Electrode Examples> [Comparative Positive Electrode Example 1] The solid electrolyte (Li 2 ZrCl 6 ) is made from lithium chloride (LiCl) and zirconium chloride (ZrCl 4 ) were weighed in a molar ratio of 2:1 to prepare raw material powders, and the solid electrolyte (Li 2 ZrCl 6 ) powder was obtained.

[0135] The combination of raw materials, synthesis time, and characteristics of the synthesis process for the solid electrolyte (compound) of Comparative Positive Electrode Example 1 are summarized in Table 1 below. The measurement results of the properties of the solid electrolyte are summarized in Table 2 below. The measurement results of the rate characteristics of the half cell are summarized in Table 3 below.

[0136] [Comparative Positive Electrode Example 2] The solid electrolyte of Comparative Positive Electrode Example 2 (LiYCl 6 ) is made from the raw materials lithium chloride (LiCl) and yttrium chloride (YCl 3 ) were weighed out in a molar ratio of 3:1 to prepare raw material powders, and the solid electrolyte (LiYCl) of Comparative Example 2 was synthesized in the same manner as in Example 1. 6 ) powder was obtained.

[0137] The combination of raw materials, synthesis time, and characteristics of the synthesis process for the solid electrolyte (compound) of Comparative Positive Electrode Example 2 are summarized in Table 1 below. The measurement results of the properties of the solid electrolyte are summarized in Table 2 below. The measurement results of the rate characteristics of the half cell are summarized in Table 3 below.

[0138] [Comparative Positive Electrode Example 3] The solid electrolyte (Li 3 ZrPO 4 Cl 4 ) is made from lithium phosphate (Li 3 P.O. 4 ) and zirconium chloride (ZrCl 4 ) were weighed to a molar ratio of 1:1 to prepare raw material powders, and the solid electrolyte (Li 3 ZrPO 4 Cl 4 ) powder was obtained.

[0139] The combination of raw materials, synthesis time, and characteristics of the synthesis process for the solid electrolyte (compound) of Comparative Positive Electrode 3 are summarized in Table 1 below. The measurement results of the properties of the solid electrolyte are summarized in Table 2 below. The measurement results of the rate characteristics of the half cell are summarized in Table 3 below.

[0140] [Comparative Positive Electrode Example 4] The solid electrolyte (Li 2 Zr(SO 4 ) Cl 4) was synthesized in the same manner as in Positive Electrode Example 1, except that the raw materials were weighed in a glove box filled with a mixed atmosphere of dry air with a dew point of about -40°C and argon gas at a volume ratio of 60%:40%, and the synthesis was performed by placing a planetary ball mill in the mixed atmosphere of dry air with a dew point of about -40°C and argon gas at a volume ratio of 60%:40%. 2 Zr(SO 4 ) Cl 4 ) powder was obtained.

[0141] The combination of raw materials, synthesis time, and characteristics of the synthesis process for the solid electrolyte (compound) of Comparative Positive Electrode 4 are summarized in Table 1 below. The measurement results of the properties of the solid electrolyte are summarized in Table 2 below. The measurement results of the rate characteristics of the half cell are summarized in Table 3 below.

[0142] [Comparative Positive Electrode Example 5] The solid electrolyte (Li 2 Zr(SO 3 ) Cl 4 ) was synthesized in the same manner as in Positive Electrode Example 1, except that the raw materials were weighed in a glove box filled with a mixed atmosphere of dry air with a dew point of about -40°C and argon gas at a volume ratio of 60%:40%, and the planetary ball mill was installed in the mixed atmosphere of dry air with a dew point of about -40°C and argon gas at a volume ratio of 60%:40%, and the solid electrolyte (Li 2 Zr(SO 3 ) Cl 4 ) powder was obtained.

[0143] The combination of raw materials, synthesis time, and characteristics of the synthesis process for the solid electrolyte (compound) of Comparative Positive Electrode 5 are summarized in Table 1 below. The measurement results of the properties of the solid electrolyte are summarized in Table 2 below. The measurement results of the rate characteristics of the half cell are summarized in Table 3 below.

[0144] [Comparative Positive Electrode Example 6] The solid electrolyte of Comparative Positive Electrode Example 6 (Li 2 Zr(S 2 O 3 ) Cl 4) was synthesized in the same manner as in Positive Electrode Example 1, except that the raw materials were weighed in a glove box filled with a mixed atmosphere of dry air with a dew point of about -40°C and argon gas at a volume ratio of 60%:40%, and the planetary ball mill was installed in the mixed atmosphere of dry air with a dew point of about -40°C and argon gas at a volume ratio of 60%:40%, and the Li 2 Zr(S 2 O 3 ) Cl 4 The powder obtained was:

[0145] The combination of raw materials, synthesis time, and characteristics of the synthesis process for the solid electrolyte (compound) of Comparative Positive Electrode Example 6 are summarized in Table 1 below. The measurement results of the properties of the solid electrolyte are summarized in Table 2 below. The measurement results of the rate characteristics of the half cell are summarized in Table 3 below.

[0146] <Negative Electrode Examples> The solid electrolytes (compounds) of negative electrode Examples 1 to 17 were the same as the solid electrolytes (compounds) of positive electrode Examples 1 to 17, respectively, and correspond to the compounds of Examples 1 to 17 listed in Table 1. The characteristics of negative electrode Examples 1 to 17 correspond to the characteristics of Examples 1 to 17 listed in Table 2.

[0147]

[0148]

[0149]

[0150] (Preparation of negative electrode mixture) To prepare a negative electrode mixture, lithium titanate (Li 4 Ti 5 O 12 ) and Li of negative electrode example 1 2 Zr(SO 4 ) Cl 4 The negative electrode active material and the Li of negative electrode example 1 were prepared. 2 Zr(SO 4 ) Cl 4 The negative electrode active material and the negative electrode active material of Example 1 were weighed out so as to have a concentration of 60 wt % and 40 wt %, respectively. 2 Zr(SO 4 ) Cl 4The mixture was mixed in an agate mortar for 15 minutes to obtain a negative electrode mixture.

[0151] (Fabrication of charge / discharge half-cells) Fabrication of charge / discharge half-cells was carried out in a glove box with a dew point of approximately -70°C. A pellet fabrication jig was used to prepare the half-cells. The pellet fabrication jig had a PEEK (polyether ether ketone) cylinder with an outer diameter of 30 mm, an inner diameter of 10 mm, and a height of 20 mm, and upper and lower punches with diameters of 9.99 mm. The upper and lower punches were made of die steel (SKD11 material).

[0152] A lower punch is inserted into the PEEK cylinder, and solid electrolyte Li is placed on the lower punch. 2 Zr(SO 4 ) Cl 4 Next, the PEEK cylinder was vibrated to level the surface of the solid electrolyte, and then an upper punch was inserted onto the solid electrolyte, and the solid electrolyte was pressed with a press under a load of 373 MPa to form a solid electrolyte layer.

[0153] Next, the upper punch was removed, and 15 mg of the above-mentioned negative electrode mixture was placed on the solid electrolyte layer. Next, the PEEK cylinder was vibrated to level the surface of the negative electrode mixture, and then the upper punch was inserted onto the negative electrode mixture and pressed with a press under a load of 373 MPa. Next, the lower punch was removed, and a lithium foil with a diameter of 10 mm and a thickness of 100 μm was placed on the solid electrolyte layer, and the lower punch was inserted. The half cell was configured as follows: (Li 4 Ti 5 O 12 +Li 2 Zr(SO 4 ) Cl 4 ) / Li 2 Zr(SO 4 ) Cl 4 / Li.

[0154] Two stainless steel plates with a diameter of 50 mm and a thickness of 5 mm and two Bakelite® plates with a diameter of 50 mm and a thickness of 2 mm were also prepared. Four screw holes were then formed in each of the two stainless steel plates and the two Bakelite® plates. The screw holes were positioned so that when the half-cell, the two stainless steel plates, and the two Bakelite® plates were stacked, the two stainless steel plates and the two Bakelite® plates would overlap in plan view, but would not overlap with the half-cell in plan view.

[0155] Next, a stainless steel plate, a Bakelite® plate, a half cell, a Bakelite® plate, and a stainless steel plate were stacked in this order, and screws were inserted into the screw holes and tightened with a torque of 1 N m. In this way, a half cell was obtained in which the upper and lower punches of the electrochemical cell were insulated by the Bakelite® plate. Next, the half cell was left to stand in a thermostatic bath at 25°C for 48 hours to stabilize the open circuit voltage.

[0156] <Measurement of rate characteristics> The fabricated half-cells were charged and discharged under the following conditions. The voltage range was 1.0 V to 2.5 V. Charging was performed at a constant current of 0.1 C, and after the constant voltage, charging was terminated when the current reached a value equivalent to 0.05 C. Discharging was performed at 0.1 C and 1.0 C, and the ratio of the discharge capacity at 1 C to the discharge capacity at 0.1 C, taken as 100%, was determined (rate characteristics (unit: %)). The results are shown in Table 1.

[0157] The results of measuring the rate characteristics of the half cells of the solid electrolytes of Negative Electrode Examples 1 to 17 are summarized in Table 4 below.

[0158] <Negative Electrode Comparative Examples> The solid electrolytes (compounds) of negative electrode comparative examples 1 to 6 were the same as the solid electrolytes (compounds) of positive electrode comparative examples 1 to 6, respectively, and correspond to the compounds of comparative examples 1 to 6 listed in Table 1. The properties of negative electrode comparative examples 1 to 6 correspond to the properties of comparative examples 1 to 6 listed in Table 2. Half cells of the solid electrolytes (compounds) of negative electrode comparative examples 1 to 6 were also prepared in the same manner as the half cells of the solid electrolytes (compounds) of negative electrode examples 1 to 17, and their rate characteristics were measured. The measurement results are summarized in Table 4 below.

[0159]

[0160] In Examples 1 to 17 and Comparative Examples 4 to 6, SO 3 - Peak intensity Ra and SO 4 - When comparing the peak intensity Rb of the sample with the peak intensity ratio R1 (Ra / Rb), it can be seen that the ionic conductivities of Examples 1 to 17, in which the peak intensity ratio R1 is greater than 1, are greater than the ionic conductivities of Comparative Examples 4 to 6, in which the peak intensity ratio R1 is less than 1. Specifically, of Examples 1 to 17, Example 17 has the smallest ionic conductivity, with an ionic conductivity of 2.8 × 10 -4 [S / cm], whereas Comparative Example 5, which has the highest ionic conductivity among Comparative Examples 4 to 6, has an ionic conductivity of 1.0 × 10 -4 [S / cm]. In this way, the peak intensity ratio R1 (Ra / Rb) can be used as an index relating to ionic conductivity.

[0161] The peak intensity ratio R1 (Ra / Rb) for Examples 1 to 17 satisfies 6.0>R1>1.0, 5.71 (Example 17) ≧ R1 ≧ 1.18 (Example 10). The ionic conductivity for Examples 1 to 15 is 3.1×10 -4 [S / cm] (Example 3) or more, 5.4 × 10 -3 [S / cm] (Example 15) or less.

[0162] The peak intensity ratio R1 (Ra / Rb) for Examples 1, 2, 4, 6, 7, 8, 9, 11 to 15 satisfied the relationship 1.8>R1>1.2. The ionic conductivity for Examples 1, 2, 4, 6, 7, 8, 9, 11 to 15 was 9.4×10 ‐4 (Example 8) 5.4 × 10 -3 [S / cm] (Example 15) or less. When 1.8 > R1 > 1.2, the ionic conductivity is 9.4 × 10 ‐4 [S / cm] or more. In this way, the peak intensity ratio R1 (Ra / Rb) can be used as an index relating to ionic conductivity.

[0163] Furthermore, the peak intensity ratio R1 (Ra / Rb) of Examples 1, 2, 4, 6, 7, 9, 11, 12, 14, and 15 satisfies 1.7>R1>1.4.

[0164] Furthermore, Examples 1 to 3 are compounds of the same composition, but have different ionic conductivities. This is due to the different atmospheres in which the synthesis was performed (synthesis atmospheres). In this way, the ionic conductivity can be adjusted by adjusting the synthesis atmosphere. Similarly, Examples 4 and 5 are compounds of the same composition, but have different ionic conductivities due to the different synthesis atmospheres. Similarly, Examples 9 and 10 are compounds of the same composition, but have different ionic conductivities due to the different synthesis atmospheres.

[0165] Examples 6 to 8 are compounds with the same constituent elements, but SO 4 and SO 3 The ratio of SO 2 is different, and the ionic conductivity is also different. This is due to the different ratios of the raw materials used for synthesis and the different synthesis atmospheres. In this way, by adjusting the synthesis atmosphere, 4 and SO 3 Similarly, Examples 11 to 13 are compounds in which the constituent elements are the same, but the SO 4 and SO 3 The ratio of SO 2 to SO 3 is different, and the ionic conductivity is also different. This is due to the difference in the synthesis atmosphere. 4 and SO 3 The ratio can be adjusted to adjust the ionic conductivity.

[0166] Although the compounds in Examples 4, 16, and 17 have the same composition, their ionic conductivities are different. This is due to the different synthesis times. In this way, the ionic conductivities can also be adjusted by adjusting the synthesis time. The synthesis times in Examples 4, 16, and 17 were 24 hours, 48 ​​hours, and 72 hours, respectively, and the ionic conductivities were 3.1 × 10 -3 [S / cm], 3.0×10 -4 [S / cm], 2.8×10 -4[S / cm]. Example 4, in which the synthesis time was 24 hours, had the highest ionic conductivity. The ionic conductivity of Example 4 is one order of magnitude higher than the ionic conductivity of Examples 16 and 17. In this way, by adjusting the synthesis time, it is possible to improve the ionic conductivity by one order of magnitude or more even for compounds with the same composition.

[0167] When comparing compounds of the same composition, the Ar gas atmosphere had the highest ionic conductivity of the three synthetic atmospheres: an Ar gas atmosphere, a mixed atmosphere of dry air with a dew point of approximately -40°C and argon gas in a volume ratio of 20%:80%, and a mixed atmosphere of dry air with a dew point of approximately -40°C and argon gas in a volume ratio of 40%:60%.

[0168] DESCRIPTION OF SYMBOLS 10...Solid electrolyte layer, 20...Positive electrode, 22...Positive electrode current collector, 24...Positive electrode mixture layer, 30...Anode, 32...Anode current collector, 34...Anode mixture layer, 40...Power generating element, 50...Exterior body, 52...Metal foil, 54...Resin layer, 60, 62...Terminal, 100...All-solid-state battery

Claims

1. SO containing Li, one or more elements selected from Groups 3 to 15, and S, and obtained by negative ion analysis using time-of-flight secondary ion mass spectrometry. 3 - Peak intensity Ra and SO 4 - and a peak intensity Rb of Ra > Rb.

2. SO in the above compound 3 - Peak intensity Ra and SO 4 - 2. The electrode according to claim 1, wherein a peak intensity ratio R1 (Ra / Rb) of a peak intensity Rb of the first peak to a peak intensity Rb of the second peak satisfies 6.0>R1>1.

0.

3. SO in the above compound 3 - Peak intensity Ra and SO 4 - 2. The electrode according to claim 1, wherein a peak intensity ratio R1 (Ra / Rb) of a peak intensity Rb of a peak intensity R1 satisfies 1.8>R1>1.

2.

4. SO in the above compound 3 - Peak intensity Ra and SO 4 - 2. The electrode according to claim 1, wherein a peak intensity ratio R1 (Ra / Rb) of a peak intensity Rb of a peak intensity R1 satisfies 1.7>R1>1.

4.

5. The compound is found to be SO - Peak, SO 2 - Peak, SO 3 - Peak, SO 4 - The peaks of SO were detected. 3 - The electrode of claim 1 , wherein the peak of 6. The electrode according to claim 1, wherein the compound is represented by the following formula (1): LiaEbGcXd (1) (In formula (1), E is at least one element selected from the group consisting of Al, Sc, Y, Zr, Hf, and lanthanoids. G is SO 3 , S.O. 4 , S.O.5 , S 2 O 3 , S 2 O 4 , S 2 O 5 , S 2 O 6 , S 2 O 7 , S 2 O 8 X is at least one element selected from the group consisting of F, Cl, Br, and I. 0.5≦a<6, 0<b<2, 0.1<c≦6, and 0<d≦6.

1.

7. An all-solid-state battery comprising a positive electrode and a negative electrode facing each other via a solid electrolyte layer, and at least one of the positive electrode and the negative electrode comprising the electrode according to any one of claims 1 to 6.

8. The all-solid-state battery according to claim 7, wherein the solid electrolyte layer contains a compound represented by the following formula (2): LiaEbGcXd (2) (In formula (2), E is at least one element selected from the group consisting of Al, Sc, Y, Zr, Hf, and lanthanoids. G is SO 3 , S.O. 4 , S.O. 5 , S 2 O 3 , S 2 O 4 , S 2 O 5 , S 2 O 6 , S 2 O 7 , S 2 O 8 X is at least one element selected from the group consisting of F, Cl, Br, and I. 0.5≦a<6, 0<b<2, 0.1<c≦6, and 0<d≦6.1.

Citation Information

Patent Citations

  • gaming machines

    JP2023058719A

  • Solid electrolyte material, and cell

    WO2018025582A1

  • Solid electrolyte and solid electrolyte battery

    WO2021261558A1

  • Solid electrolyte material, manufacturing method therefor and battery

    JP2022176803A

  • Battery and method for producing same

    WO2022154112A1