Electrode material, electrode slurry, production method for electrode material, electrode, and production method for electrode
A non-aqueous binder coating the electrode active material in a shell shape addresses the oxidation issues of conventional aqueous binders, enhancing the performance and longevity of secondary battery electrodes by maintaining uniform distribution and binding properties.
Patent Information
- Application Number
- PCT/JP2024/011955
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2024-03-22
- Filing Date
- 2024-03-26
- Publication Date
- 2024-10-03
AI Technical Summary
Conventional aqueous binders for secondary battery electrodes, such as those containing carboxymethylcellulose and styrene-butadiene rubber, deteriorate in positive electrode environments due to oxidation, leading to uneven distribution and weakened binding properties, which results in decreased electrode capacity and cycle characteristics.
The use of a non-aqueous binder, like fluororesin, which coats the entire surface of the electrode active material in a shell shape, preventing lithium dissolution and ensuring uniform distribution, thereby enhancing binding properties and cycle characteristics.
This approach effectively suppresses the decrease in electrode capacity and improves cycle characteristics by maintaining the non-aqueous binder's integrity and uniform dispersion, even when using lithium-containing active materials, while reducing the amount of organic solvent required.
Smart Images

Figure JP2024011955_03102024_PF_FP_ABST
Abstract
Description
Electrode material, electrode slurry, electrode material manufacturing method, electrode, and electrode manufacturing method
[0001] The present invention relates to an electrode material for a secondary battery, an electrode slurry, a method for manufacturing an electrode material, an electrode, and a method for manufacturing an electrode.
[0002] Electrodes constituting secondary batteries such as lithium ion secondary batteries are generally produced by applying a slurry in which an electrode active material, a binder, and a conductive additive are dispersed onto a current collector and then drying the slurry.
[0003] Conventionally, polyvinylidene fluoride (PVDF), which has excellent properties such as mechanical strength, adhesiveness, and oxidation resistance, has been widely used as a binder for electrodes.
[0004] However, since PVDF is insoluble in water, it is necessary to prepare a slurry by dissolving PVDF in an organic solvent such as N-methyl-pyrrolidone (NMP), which poses a problem of increased environmental impact due to the use of organic solvents. Therefore, in recent years, there has been a demand for the development of an aqueous binder that can be dispersed in an aqueous solvent with a low environmental impact.
[0005] Carboxymethyl cellulose (CMC) and styrene-butadiene rubber (SBR) have been developed as aqueous binders for use in negative electrodes. However, when these aqueous binders are used directly in positive electrodes, there is a problem that they are subject to oxidative degradation in the positive electrode environment.
[0006] Patent Document 1 discloses a binder composed of an acrylic polymer as an aqueous binder used in a positive electrode. This aqueous binder does not dissolve in water, and is dispersed as suspended particles in an aqueous solvent to prepare a positive electrode slurry. When this positive electrode slurry is applied to a current collector and dried to prepare a positive electrode, the aqueous binder is unevenly distributed in the recesses between the positive electrode active material particles while maintaining its particle shape.
[0007] JP 2017-91789 A
[0008] The aqueous binder disclosed in Patent Document 1 is effective in terms of oxidation resistance, but because the positive electrode active material contains lithium, when this aqueous binder is dispersed in an aqueous solvent together with the positive electrode active material and a conductive additive to prepare a positive electrode slurry, the transition metals such as lithium in the positive electrode active material dissolve into the aqueous solvent, resulting in a decrease in positive electrode capacity. Note that this problem can also occur in negative electrodes using a material containing lithium as the negative electrode active material.
[0009] Furthermore, because the aqueous binder is only unevenly distributed in the recesses between the positive electrode active materials, it is difficult to uniformly disperse the aqueous binder within the positive electrode. This weakens the binding between the positive electrode active materials and between the positive electrode active material and the current collector, resulting in a problem of reduced cycle performance of the secondary battery. Note that this problem can also occur when the aqueous binder is used in the negative electrode.
[0010] The present invention has been made in view of the above points, and aims to provide an electrode material for a secondary battery, an electrode slurry, a method for manufacturing an electrode material, an electrode, and a method for manufacturing an electrode, which suppress a decrease in electrode capacity and have excellent cycle characteristics.
[0011] The electrode material according to the present invention is an electrode material for a secondary battery, and contains an active material, the entire surface of which is coated with a non-aqueous binder in the form of a shell.
[0012] In a preferred embodiment, a portion of the surface of the electrode active material is coated with a metal oxide, and the non-aqueous binder coats the entire surface of the electrode active material in a shell-like manner so as to cover the metal oxide.
[0013] The electrode slurry according to the present invention is an electrode slurry containing an electrode mixture, the electrode mixture containing an active material whose entire surface is coated with a shell-like coating of a non-aqueous binder, and a conductive assistant, and the electrode mixture is dispersed in an aqueous solvent.
[0014] The method for producing an electrode material according to the present invention is a method for producing an electrode material for a secondary battery, and includes the steps of dissolving a powder of a non-aqueous binder in a non-aqueous solvent and dispersing a powder of an electrode active material in the non-aqueous solvent, and evaporating the non-aqueous solvent to coat the entire surface of the electrode active material with the non-aqueous binder in a shell-like form.
[0015] The electrode according to the present invention is an electrode for a secondary battery having an electrode mixture formed on a current collector, the electrode mixture including an electrode material in which the entire surface of an electrode active material is coated with a non-aqueous binder in a shell-like manner, and a conductive assistant, the electrode active material included in the electrode material is dispersed in a state in which the entire surface is coated with the non-aqueous binder in a shell-like manner, and the total volume of the non-aqueous binder that coats the entire surface of the electrode active material is defined as V 1 The total volume of the non-aqueous binder present in the region surrounded by the electrode active material coated with the non-aqueous binder is V 2 When V 1 >V 2 is.
[0016] The electrode according to the present invention is an electrode for a secondary battery having an electrode mixture formed on a current collector, the electrode mixture including an electrode material in which the entire surface of an electrode active material is coated with a non-aqueous binder in a shell-like shape, and a conductive assistant, the electrode active material included in the electrode material is dispersed in a state in which the entire surface is coated with a non-aqueous binder in a shell-like shape, and the sum of the volumes of the regions surrounded by the electrode active material coated with the non-aqueous binder is defined as V 3 The total volume of the non-aqueous binder present in the region surrounded by the electrode active material coated with the non-aqueous binder is V 2 When V 3 >V 2 is.
[0017] The method for manufacturing an electrode for a secondary battery according to the present invention includes the steps of: forming an electrode material in which the entire surface of an electrode active material is coated with a non-aqueous binder in a shell-like manner; dispersing an electrode mixture containing the electrode material and a conductive additive in an aqueous solvent to form an electrode slurry; and applying the electrode slurry onto a current collector and then drying the applied film.
[0018] According to the present invention, it is possible to provide an electrode material for a secondary battery, an electrode slurry, a method for manufacturing an electrode material, an electrode, and a method for manufacturing an electrode, which suppress a decrease in electrode capacity and have excellent cycle characteristics.
[0019] FIG. 1 is a diagram schematically showing the structure of a cathode material in an embodiment of the present invention. FIG. 2 is a diagram schematically showing the structure of a cathode plate produced using a cathode slurry containing the cathode material in this embodiment. FIG. 3 is a diagram schematically showing the structure of a cathode plate produced using a cathode slurry containing the cathode material in another embodiment of the present invention. FIG. 4 is a diagram schematically showing a modified example 1 of the cathode material. FIG. 5 is a diagram schematically showing a modified example 2 of the cathode material. FIG. 6 is a diagram schematically showing a modified example 3 of the cathode material. FIG. 7 is a photograph taken with an SEM of the cross section of the positive electrode plate produced in Example 1. FIG. 8 is a photograph taken with an SEM of the cross section of the positive electrode plate after dyeing the fluorine component in the positive electrode plate. FIG. 9 is a photograph taken with an SEM of the cross section of the positive electrode plate produced in Comparative Example 1. FIG. 10 is a photograph taken with an SEM of the cross section of the positive electrode plate after dyeing the fluorine component in the positive electrode plate. 1 is a photograph taken with an SEM of a cross section of a positive electrode plate produced in Example 2. FIG. 1 is a photograph taken with an SEM of a cross section of a positive electrode plate after dyeing the fluorine component in the positive electrode plate. FIG. 2 is a photograph taken with an SEM of a cross section of a positive electrode plate produced in Comparative Example 2. FIG. 3 is a photograph taken with an SEM of a cross section of a positive electrode plate after dyeing the fluorine component in the positive electrode plate. FIG. 4 is a photograph taken with an SEM of a cross section of a resin-embedded positive electrode plate produced in Example 1. FIG. 5 is a photograph showing a line diagram of a portion in contact with the positive electrode active material in a region where the fluorine component in the positive electrode plate has been dyed. FIG. 6 is a photograph taken with an SEM of a cross section of a resin-embedded positive electrode plate produced in Comparative Example 1. FIG. 7 is a photograph showing a line diagram of a portion in contact with the positive electrode active material in a region where the fluorine component in the positive electrode plate has been dyed. FIG. 8 is a graph showing measurement results of the cycle characteristics of a lithium ion battery produced using the positive electrode material produced in Example 1. 1 is a graph showing the measurement results of the cycle characteristics of a lithium ion battery produced using the positive electrode material produced in Example 3.
[0020] Hereinafter, embodiments of the present invention will be described in detail with reference to the drawings. In the following embodiments, a positive electrode will be described as an example of an electrode of a secondary battery, but the present invention is not limited thereto and can also be applied to a negative electrode. That is, in this specification, the term "electrode" includes a positive electrode and a negative electrode. For example, "electrode material" includes a positive electrode material and a negative electrode material, "electrode active material" includes a positive electrode active material and a negative electrode active material, "electrode mixture" includes a positive electrode mixture and a negative electrode mixture, and "electrode slurry" includes a positive electrode slurry and a negative electrode slurry.
[0021] The cathode material in this embodiment is a cathode material for a secondary battery, and as shown in the schematic diagram of Fig. 1, the cathode material 1 includes a cathode active material 10, and the entire surface of the cathode active material 10 is covered in a shell-like shape with a non-aqueous binder 20. Here, the non-aqueous binder 20 is made of a fluorine-based resin that is insoluble in aqueous solvents such as water but soluble in non-aqueous solvents such as organic solvents, and typically includes polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), fluorine-based rubber, etc.
[0022] The secondary batteries to which the positive electrode material of this embodiment is applied include lithium ion secondary batteries, lithium sulfur secondary batteries, etc. In addition, the positive electrode active material is, for example, LiCoO 2 , LiNiO 2 , LiNi 0.8 Co 0.2 O 2 , LiMn 2 O 4 , LiFePO 4 , LiNiCoMnO 2 The positive electrode active material preferably includes two or more types of positive electrode active materials having different particle sizes. A positive electrode active material having a small particle size can be formed, for example, by using a flux method.
[0023] The cathode material 1 in this embodiment can be produced by a process of dissolving powder of the non-aqueous binder 20 in a non-aqueous solvent, dispersing powder of the cathode active material 10 in the non-aqueous solvent, and heating and evaporating the non-aqueous solvent to coat the entire surface of the cathode active material 10 in a shell shape with the non-aqueous binder 20. The non-aqueous solvent may be dried in a vacuum at room temperature without heating.
[0024] The non-aqueous solvent is made of a material in which the powder of the non-aqueous binder 20 can be dissolved, and includes an organic solvent such as N-methyl-2-pyrrolidone (NMP).
[0025] The amount of non-aqueous binder 20 used in the process of producing the cathode material 1 may be determined appropriately depending on the amount of cathode active material 10 within a range that can coat the entire surface of the cathode active material 10 in a shell-like shape.
[0026] The positive electrode slurry in this embodiment includes a positive electrode mixture containing the positive electrode material 1 and a conductive additive, and the positive electrode mixture is dispersed in an aqueous solvent. Note that the non-aqueous binder 20 that coats the surface of the positive electrode active material 10 is not dissolved in the aqueous solvent.
[0027] The aqueous solvent is made of a material in which the powder of the non-aqueous binder 20 is insoluble, and includes water or a dispersant such as polyvinylpyrrolidone (PVP). The conductive additive is not particularly limited, but preferably includes cellulose nanofibers. Because aqueous solvents have low viscosity, a positive electrode slurry with an appropriate viscosity can be obtained by using cellulose nanofibers, which have high viscosity, as a conductive additive.
[0028] The positive electrode plate of this embodiment can be produced by applying the positive electrode slurry to a current collector and then drying the coating film. The drying of the coating film may be performed by thermocompressing the positive electrode slurry and the current collector together using a roll press or the like.
[0029] In the cathode material 1 of this embodiment, the entire surface of the cathode active material 10 is coated in a shell shape with the nonaqueous binder 20, so that even when a cathode mixture containing the cathode material 1 and a conductive additive is dispersed in an aqueous solvent to prepare a cathode slurry, lithium in the cathode active material 10 does not dissolve into the aqueous solvent. As a result, it is possible to suppress a decrease in the cathode capacity caused by lithium dissolving into the aqueous solvent.
[0030] Furthermore, when a positive electrode plate is produced using the positive electrode slurry containing the positive electrode material 1 of this embodiment, the non-aqueous binder 20 does not dissolve in an aqueous solvent, and therefore the positive electrode active material 10 is uniformly dispersed in a state in which the entire surface is covered with a shell-like coating of the non-aqueous binder 20, as shown in the schematic diagram of Fig. 2. Therefore, the non-aqueous binder 20 is also uniformly dispersed, and the positive electrode active material 10 can be uniformly bound to each other and to the current collector throughout the positive electrode, thereby realizing a secondary battery with excellent cycle characteristics.
[0031] In particular, when the positive electrode active material 10 contains two or more types of positive electrode active material 10 with different particle sizes, the positive electrode active material 10 is dispersed more uniformly, and the binding strength between the positive electrode active material 10 and between the positive electrode active material 10 and the current collector is enhanced via the non-aqueous binder 20, resulting in further improvement in cycle characteristics.
[0032] The cathode material 1 in this embodiment has a structure in which the entire surface of the cathode active material 10 is coated with the non-aqueous binder 20 in a shell-like shape, but also includes a structure in which only a part of the surface is coated with the non-aqueous binder 20.
[0033] When a positive electrode mixture containing a conventional non-aqueous binder 20 such as PVDF is dispersed in an organic solvent to prepare a positive electrode slurry, the conductive additive such as carbon black contained in the positive electrode mixture does not dissolve in the organic solvent, and further, the small holes on the nanometer level absorb the organic solvent, so that a large amount of organic solvent is used.
[0034] On the other hand, an organic solvent (nonaqueous solvent) is also used to prepare the cathode material 1 in this embodiment, but the organic solvent only contains the cathode active material 10 and the nonaqueous binder 20 that dissolves in the organic solvent, so the amount of nonaqueous solvent used can be significantly reduced compared to when a cathode mixture containing a conventional nonaqueous binder 20 such as PVDF is dispersed in an organic solvent to prepare a cathode slurry. As a result, the cathode in this embodiment is manufactured using a cathode slurry in which a cathode mixture containing the cathode material 1 and a conductive additive is dispersed in an aqueous solvent, so the amount of nonaqueous solvent used when manufacturing a secondary battery can be significantly reduced.
[0035] Furthermore, in the cathode material 1 of this embodiment, the entire surface of the cathode active material 10 is coated in a shell-like manner with the nonaqueous binder 20, thereby achieving the effects of suppressing a decrease in cathode capacity and improving cycle characteristics. Therefore, in order to achieve such effects, the amount of nonaqueous binder 20 used in the process of producing the cathode material 1 may be within a range that allows the entire surface of the cathode active material 10 to be coated in a shell-like manner, depending on the amount of the cathode active material 10. Typically, a minimum amount of nonaqueous binder 20, including an excess amount, may be used, taking into consideration variations in the size of the cathode active material 10, variations in the process of producing the cathode material 1, and the like.
[0036] As described above, when a positive electrode plate is produced using the positive electrode slurry containing the positive electrode material 1 of this embodiment, the positive electrode active material 10 is uniformly dispersed in a state in which the entire surface is coated with a shell-like coating of the nonaqueous binder 20, as shown in the schematic diagram of Fig. 3. In this case, since only a minimum amount of the nonaqueous binder 20 is used, only an excess amount of the nonaqueous binder 40 is present in the region 50 surrounded by the positive electrode active material 10 coated with the nonaqueous binder 20, and most of the region 50 is in a void state.
[0037] Therefore, the total volume of the non-aqueous binder 20 covering the entire surface of the positive electrode active material 10 is V 1 The total volume of the non-aqueous binder 40 present in the region 50 surrounded by the positive electrode active material 10 coated with the non-aqueous binder 20 is V 2 When V 1 >V2 Furthermore, the total volume of the region 50 surrounded by the positive electrode active material 10 coated with the non-aqueous binder 20 is V 3 When V 3 >V 2 This is the relationship.
[0038] The above relationship is established by defining the total area of the non-aqueous binder 20 covering the entire surface of the positive electrode active material 10 as A when the positive electrode mixture formed on the current collector is viewed in a cross section perpendicular to the film thickness direction. 1 The total area of the non-aqueous binder 40 present in the region 50 surrounded by the positive electrode active material 10 coated with the non-aqueous binder 20 is A 2 When this is done, A 1 >A 2 The total area of the region 50 surrounded by the positive electrode active material 10 coated with the non-aqueous binder 20 is A 3 When this is done, A 3 >A 2 This becomes:
[0039] Incidentally, in the cathode material 1 of this embodiment, the entire surface of the cathode active material 10 is coated with the non-aqueous binder 20 in a shell shape. Therefore, even if a cathode mixture containing the cathode material 1 and a conductive additive is dispersed in an aqueous solvent to prepare a cathode slurry, lithium of the cathode active material 10 does not dissolve into the aqueous solvent, and therefore a decrease in the cathode capacity can be suppressed.
[0040] Furthermore, when a positive electrode plate is produced using the positive electrode slurry containing the positive electrode material 1 of this embodiment, the non-aqueous binder 20 does not dissolve in an aqueous solvent, and therefore the positive electrode active material 10 is uniformly dispersed in a state in which the entire surface is covered with a shell-like coating of the non-aqueous binder 20. Therefore, the non-aqueous binder 20 is also uniformly dispersed, and the positive electrode active material 10 can be uniformly bound to each other and to the current collector throughout the positive electrode, thereby realizing a secondary battery with excellent cycle characteristics.
[0041] Such an effect is obtained by coating the surface of the positive electrode active material 10 with the non-aqueous binder 20 in a shell-like manner, and therefore the entire surface of the positive electrode active material 10 does not necessarily have to be completely coated with the non-aqueous binder 20 in a shell-like manner, and such an effect can be obtained even when only a portion of the surface of the positive electrode active material 10 is coated with the non-aqueous binder 20 in a shell-like manner.
[0042] For example, when a positive electrode plate is produced using a positive electrode slurry in this embodiment, in which a positive electrode mixture containing a positive electrode material 1 in which a portion of the surface of the positive electrode active material 10 is coated in a shell-like manner with the nonaqueous binder 20 is dispersed in an aqueous solvent, and when a positive electrode plate is produced using a positive electrode slurry in which a positive electrode mixture containing the nonaqueous binder 20 is dispersed in an organic solvent using a conventional method, using the same amount of nonaqueous binder 20, it has been confirmed that the secondary battery produced according to this embodiment has superior characteristics in terms of positive electrode capacity and cycle characteristics compared to the secondary battery produced according to the conventional method.
[0043] The cathode material 1 in which a portion of the surface of the cathode active material 10 is coated in a shell-like shape with the non-aqueous binder 20 may be produced by setting the amount of the non-aqueous binder 20 used in the production process of the cathode material 1 to a range that allows a portion of the surface of the cathode active material 10 to be coated in a shell-like shape.
[0044] In addition, when a portion of the surface of the positive electrode active material 10 is coated in a shell-like manner with the non-aqueous binder 20, in order to achieve the effects of the present invention, it is preferable that 50% or more of the surface of the positive electrode active material 10 is coated with the non-aqueous binder 20, and it is more preferable that 70% or more of the surface of the positive electrode active material 10 is coated with the non-aqueous binder 20.
[0045] When a positive electrode plate is produced using a positive electrode slurry containing such a positive electrode material 1, the positive electrode active material 10 is uniformly dispersed with a part of its surface coated with a shell-like coating of the non-aqueous binder 20, as shown in the schematic diagram of Fig. 4. In this case, a smaller amount of the non-aqueous binder 20 is used than when the non-aqueous binder 20 is coated in a shell-like manner on the entire surface of the positive electrode active material 10. Therefore, in the region 50 surrounded by the positive electrode active material 10 coated with the non-aqueous binder 20, almost no non-aqueous binder 40 is present, resulting in a void state.
[0046] Therefore, similarly to the case where the non-aqueous binder 20 is coated in a shell-like manner on the entire surface of the positive electrode active material 10, the total volume of the non-aqueous binder 20 that coats a part of the surface of the positive electrode active material 10 is V 1 The total volume of the non-aqueous binder 40 present in the region 50 surrounded by the positive electrode active material 10 coated with the non-aqueous binder 20 is V 2 When V 1 >V 2 Furthermore, the total volume of the region 50 surrounded by the positive electrode active material 10 coated with the non-aqueous binder 20 is V 3 When V 3 >V 2 This is the relationship.
[0047] The above relationship is established when the total area of the non-aqueous binder 20 covering a part of the surface of the positive electrode active material 10 is defined as A when the positive electrode mixture formed on the current collector is viewed in a cross section perpendicular to the film thickness direction. 1 The total area of the non-aqueous binder 40 present in the region 50 surrounded by the positive electrode active material 10 coated with the non-aqueous binder 20 is A 2 When this is done, A 1 >A 2 The total area of the region 50 surrounded by the positive electrode active material 10 coated with the non-aqueous binder 20 is A 3 When this is done, A 3 >A 2 This becomes:
[0048] <Modification> In the above embodiment, the cathode material 1 has a structure in which the entire surface or a portion of the surface of the cathode active material 10 is coated in a shell shape with the non-aqueous binder 20. However, if the thickness of the coating non-aqueous binder 20 is too thick, the electrical resistance at the surface of the cathode active material 10 increases, which may result in a decrease in battery capacity. In this modification, a structure of the cathode material 1 is shown that can suppress a decrease in battery capacity due to an increase in the thickness of the non-aqueous binder 20.
[0049] 5 is a diagram schematically illustrating a modified example 1 of the cathode material 1, in which a portion of the surface of the cathode active material 10 is coated with a metal oxide 30, and the non-aqueous binder 20 forms a shell-like coating over the entire surface of the cathode active material 10 so as to cover the metal oxide 30. This structure can suppress an increase in electrical resistance on the surface of the cathode active material 10, thereby suppressing a decrease in battery capacity while maintaining the effect of improving binding properties (improved cycle characteristics) provided by the non-aqueous binder 20.
[0050] The cathode material 1 in this modified example 1 can be produced by carrying out a step of adhering a metal oxide 30 to a part of the surface of the cathode active material 10 before a step of coating the entire surface of the cathode active material 10 with a non-aqueous binder 20 in a shell-like shape. This allows the entire surface of the cathode active material 10 to be coated with the non-aqueous binder 20 in a shell-like shape so as to cover the metal oxide 30.
[0051] The metal oxide 30 that coats the surface of the positive electrode active material 10 is not particularly limited as long as it is a material with low electrical resistance, and examples of usable materials include titanium oxide, niobium oxide, and titanium-containing oxides. Coating the surface of the positive electrode active material 10 with the metal oxide 30 can be performed, for example, by mixing the positive electrode active material 10 and the metal oxide 30 and sintering or firing the mixture.
[0052] FIG. 6 is a diagram showing a modified example 2 of the cathode material 1, in which the entire surface of the cathode active material 10 is covered with either a non-aqueous binder 20 or a metal oxide 30 in a shell-like structure.
[0053] FIG. 7 is a diagram schematically illustrating a modified example 3 of the cathode material 1, in which the entire surface of the cathode active material 10 is covered with a shell-like metal oxide 30, and a portion of the surface of the metal oxide 30 is covered with a non-aqueous binder 20.
[0054] In the cathode material 1 having the structure shown in FIGS. 6 and 7 , although the entire surface of the cathode active material 10 is not coated with the non-aqueous binder 20, a part of the surface of the cathode active material 10 or the entire surface is coated with the metal oxide 30. Therefore, it is possible to suppress a decrease in battery capacity while maintaining the effect of improving the binding property by the non-aqueous binder 20.
[0055] The cathode material 1 having the structure shown in FIGS. 6 and 7 can be produced by the steps of: adhering a metal oxide 30 to a part of the surface or the entire surface of a cathode active material 10; dissolving a powder of a non-aqueous binder 20 in a non-aqueous solvent; dispersing the powder of the cathode active material 10 having the metal oxide 30 adhered to its surface in the non-aqueous solvent; and evaporating the non-aqueous solvent.
[0056] The amount of metal oxide 30 used in the process of producing the cathode material 1 may be determined appropriately depending on the amount of cathode active material 10 within a range that can cover a part or the entire surface of the cathode active material 10 .
[0057] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples.
[0058] [Example 1] <Preparation of Cathode Material> 0.05 g of powder of a non-aqueous binder (PVDF) was dissolved in 0.45 g of a non-aqueous solvent (NMP solvent), and 0.95 g of a cathode active material (lithium iron phosphate (LiFePO 4 ) powder was dispersed in the non-aqueous solvent. The non-aqueous solvent was then evaporated by heating at 100°C for 2 minutes. This produced a positive electrode material 1 in which the entire surface of the positive electrode active material 10 was coated with the non-aqueous binder in a shell shape.
[0059] <Preparation of Positive Electrode Plate> The positive electrode material 1 prepared by the above method, a conductive additive (including cellulose nanofibers), and a dispersant were mixed in a mass ratio of 95:4:1 in an aqueous solvent (pure water) to prepare a positive electrode slurry.
[0060] This positive electrode slurry was applied to a positive electrode current collector (aluminum foil), heated at 100° C. for 6 minutes to dry, and then pressed together with the aluminum foil to prepare a positive electrode plate.
[0061] [Example 2] The positive electrode active material was a ternary system (LiNiCoMnO 2 A positive electrode plate was produced in the same manner as in Example 1, except that the material of Example 1 was used.
[0062] Comparative Example 1 A positive electrode active material (lithium iron phosphate), a conductive additive (acetylene black), and a binder (PVDF) were mixed in a mass ratio of 90:5:5 in an organic solvent (NMP) using a conventional method to form a positive electrode slurry. A positive electrode plate was then produced using the same method as in Example 1.
[0063] Comparative Example 2 The positive electrode active material was a ternary material (LiNiCoMnO 2 A positive electrode plate was produced in the same manner as in Comparative Example 1, except that the material of
[0064] <Evaluation of Dispersion State of Non-Aqueous Binder in Positive Electrode Plate> FIG. 8A is a photograph of the cross section of the positive electrode plate produced in Example 1 taken with a scanning electron microscope (SEM), and FIG. 8B is a photograph of the fluorine component (PVDF) in the positive electrode plate taken with an energy dispersive X-ray spectroscopy (EDS) of the cross section of the positive electrode plate at the same position, in which the area where the fluorine component was detected by the EDS was dyed and highlighted.
[0065] The SEM cross-sectional photographs were obtained by preparing a cross-section of the prepared positive electrode plate sample using a focused ion beam (FIB), and then photographing the conductively treated cross-section under conditions of an acceleration voltage of 15 kV and a magnification of 2000 times.
[0066] 8B , it was confirmed that many areas on the surface of the positive electrode active material 10 were covered in a shell shape with the non-aqueous binder (PVDF) 20. It was also confirmed that the amount of binder (PVDF) 20 present in the gaps formed between the positive electrode active materials 10 was small.
[0067] That is, the total volume of the binder (PVDF) 20 covering the surface of the positive electrode active material 10 is V 1, the total volume of the binder (PVDF) 20 present in the region surrounded by the positive electrode active material 10 coated with the binder (PVDF) 20 is V 2 When V 1 >V 2 It was confirmed that the relationship between the total volume of the area surrounded by the positive electrode active material 10 coated with the binder (PVDF) 20 was V 3 When V 3 >V 2 It was confirmed that there is a relationship between
[0068] In addition, the total area of the binder (PVDF) 20 covering the surface of the positive electrode active material 10 in the cross section of the positive electrode mixture is A 1 The total area of the binder (PVDF) 20 present in the region surrounded by the positive electrode active material 10 coated with the binder (PVDF) 20 is A 2 When this is done, A 1 >A 2 It was confirmed that the relationship between the above and the binder (PVDF) 20 was satisfied. 3 When this is done, A 3 >A 2 It was confirmed that there is a relationship between
[0069] 9A is a SEM photograph of the cross section of the positive electrode plate produced in Comparative Example 1, and FIG. 9B is a photograph of the fluorine component (PVDF) in the positive electrode plate at the same position on the cross section, photographed by EDS (energy dispersive X-ray spectroscopy), with the area where the fluorine component was detected by EDS dyed and highlighted. The SEM cross-sectional photograph was taken under the same conditions as in Example 1.
[0070] 9B , in the positive electrode plate produced in Comparative Example 1, it was confirmed that the binder (PVDF) 20 was dispersed among the positive electrode active material 10, but the area on the surface of the positive electrode active material 10 that was covered with the binder (PVDF) in a shell-like shape was hardly confirmed. That is, in the positive electrode plate produced in Comparative Example 1, it was confirmed that the binder (PVDF) was present in a state of being pressed into the gaps formed between the positive electrode active material 10. That is, it was confirmed that the binder (PVDF) was not present around the positive electrode active material 10 in a state that covered the positive electrode active material 10 with a thin film in a shell-like shape, as in Example 1, but that the binder (PVDF) was present so as to fill the gaps formed between the positive electrode active material 10.
[0071] FIG. 10A is a photograph of the cross section of the positive electrode plate fabricated in Example 2 taken by SEM, showing the positive electrode active material (LiNiCoMnO 2 The particle size of the positive electrode active material (LiFePO 4 ) particle size. Also, FIG. 10B is a photograph of the fluorine component (PVDF) in the positive electrode plate, taken by EDS (energy dispersive X-ray spectroscopy) of the cross section of the positive electrode plate at the same position, in which the area where the fluorine component was detected by EDS was dyed and highlighted. The SEM cross-sectional photograph was taken under the same conditions as in Example 1.
[0072] 10B , in the positive electrode plate produced in Example 2, similarly to Example 1, it was confirmed that many regions on the surface of the positive electrode active material 10 were covered in a shell-like shape with the non-aqueous binder (PVDF) 20. It was also confirmed that the amount of binder (PVDF) 20 present in the gaps formed between the positive electrode active materials 10 was small.
[0073] That is, the total volume of the binder (PVDF) 20 covering the surface of the positive electrode active material 10 is V 1 , the total volume of the binder (PVDF) present in the region surrounded by the positive electrode active material 10 coated with the binder (PVDF) 20 is V 2 When V 1 >V 2It was confirmed that the relationship between the total volume of the area surrounded by the positive electrode active material 10 coated with the binder (PVDF) was V 3 When V 3 >V 2 It was confirmed that there is a relationship between
[0074] In addition, the total area of the binder (PVDF) 20 covering the surface of the positive electrode active material 10 in the cross section of the positive electrode mixture is A 1 The total area of the binder (PVDF) 20 present in the region surrounded by the positive electrode active material 10 coated with the binder (PVDF) 20 is A 2 When this is done, A 1 >A 2 It was confirmed that the relationship between the above and the binder (PVDF) 20 was satisfied. 3 When this is done, A 3 >A 2 It was confirmed that there is a relationship between
[0075] 11A is a SEM photograph of the cross section of the positive electrode plate produced in Comparative Example 2, and FIG. 11B is a photograph of the fluorine component (PVDF) in the positive electrode plate taken at the same position on the cross section of the positive electrode plate by EDS (energy dispersive X-ray spectroscopy), in which the area where the fluorine component was detected by EDS was dyed and highlighted. The SEM cross-sectional photograph was taken under the same conditions as in Example 1.
[0076] 11B , in the positive electrode plate produced in Comparative Example 2, it was confirmed that the binder (PVDF) 20 was dispersed among the positive electrode active material 10, as in Comparative Example 1. However, on the surface of the positive electrode active material 10, there was hardly any region coated with the binder (PVDF) in a shell-like manner. That is, in the positive electrode plate produced in Comparative Example 1, it was confirmed that the binder (PVDF) was present in a state of being pressed into the gaps formed between the positive electrode active material 10. That is, it was confirmed that the binder (PVDF) was not present around the positive electrode active material 10 in a state of covering the positive electrode active material 10 with a thin film in a shell-like manner, as in Example 1, but that the binder (PVDF) was present so as to fill the gaps formed between the positive electrode active material 10.
[0077] <Measurement of Coverage Ratio> Based on the SEM photograph of FIG. 8B (Example 1) and the SEM photograph of FIG. 9B (Comparative Example 1), the coverage ratio C (%) defined by the following formula (1) was measured for a cross section of the positive electrode mixture formed on the positive electrode current collector.
[0078] C = (C 2 ÷C 1 ) × 100 (1) In formula (1), C 1 represents the perimeter of the positive electrode active material 10, and C 2 represents the total length of the contact portion of the binder (PVDF) in contact with the periphery of the positive electrode active material 10.
[0079] As a result, the coverage rate of the positive electrode plate prepared in Example 1 was 60%, whereas the coverage rate of the positive electrode plate prepared in Comparative Example 1 was 23%.
[0080] When observing the cross section of a positive electrode plate with an SEM, the binder (PVDF) present at the back of the cross section may be imaged as if it were present on the same plane as the cross section. To avoid this effect, the positive electrode plates prepared in Example 1 and Comparative Example 1 were embedded in resin, and then cross sections of the resin-embedded positive electrode plates were prepared using a broad ion beam (BIB) method. The conductive cross section was then photographed under conditions of an accelerating voltage of 15 kV and a magnification of 3000 times to obtain an SEM cross-sectional photograph.
[0081] FIG. 12A is a photograph of a cross section of a resin-embedded positive electrode plate prepared in Example 1, taken with an SEM. FIG. 12B is a photograph of the fluorine component (PVDF) in the positive electrode plate, taken with an EDS (energy dispersive X-ray spectroscopy) image of the cross section of the positive electrode plate at the same position, in which the region where the fluorine component was detected by the EDS was stained, and in which a portion 20 in the stained region that is in contact with the positive electrode active material 10 is shown in a line diagram.
[0082] Similarly, FIG. 13A is a photograph of a cross section of a resin-embedded positive electrode plate prepared in Comparative Example 1, taken with an SEM. FIG. 13B is a photograph of the fluorine component (PVDF) in the positive electrode plate, taken with an EDS (energy dispersive X-ray spectroscopy) image of the cross section of the positive electrode plate at the same position, in which the region where the fluorine component was detected by the EDS was stained, and in which a portion 20 in the stained region that is in contact with the positive electrode active material 10 is shown in a line diagram.
[0083] 12B (Example 1) and the SEM photograph of Fig. 13B (Comparative Example 1), the coverage C (%) defined by the above formula (1) was measured for the cross section of the positive electrode mixture formed on the positive electrode current collector. As a result, the coverage was 37% for the positive electrode plate prepared in Example 1, whereas the coverage was 10% for the positive electrode plate prepared in Comparative Example 1.
[0084] The reason why the coverage rate C of the resin-embedded positive electrode plate is smaller than the coverage rate C of the non-resin-embedded positive electrode plate is thought to be that when the positive electrode plate is embedded in resin, after which the resin is hardened by heating, a particularly thinly coated portion of the binder (PVDF) peels off from the surface of the positive electrode active material 10 due to the influence of factors such as the difference in expansion coefficient between the positive electrode active material and the resin.
[0085] From the above results, it is preferable that the coverage C of the resin-embedded positive electrode plate in the cross section of the positive electrode mixture formed on the positive electrode current collector is 30% or more.
[0086] <Evaluation of Cycle Characteristics of Lithium-Ion Secondary Battery> The positive electrode plate prepared in Example 1 and a negative electrode plate (lithium metal foil) were wound with a separator interposed therebetween to prepare an electrode body, and this electrode body was housed in a battery case together with a non-aqueous electrolyte to prepare a lithium-ion secondary battery.
[0087] The produced lithium ion secondary battery was repeatedly charged and discharged at a charge and discharge rate of 1 C to measure the change in discharge capacity [mAh / g] and to measure the cycle characteristics.
[0088] FIG. 14 is a graph showing the measurement results of cycle characteristics, in which the graph indicated by arrow A shows the cycle characteristics of the lithium ion secondary battery produced using the positive electrode material of Example 1, and the graph indicated by arrow B shows the cycle characteristics of the lithium ion secondary battery produced using the positive electrode material of Comparative Example 1.
[0089] 14 , the cycle characteristics of the lithium ion secondary battery produced using the positive electrode material of Example 1 show that the number of cycles until the discharge capacity decreases to one-third of the initial capacity is improved by about twice as much as the cycle characteristics of the lithium ion secondary battery produced using the positive electrode material of Comparative Example 1. This is thought to be because the positive electrode active material 10 is uniformly dispersed in a state where the entire surface is covered with the non-aqueous binder 20 in a shell-like shape, and the non-aqueous binder 20 also uniformly disperses, and the positive electrode active material 10 and the positive electrode active material 10 and the current collector are uniformly bound by the non-aqueous binder 20 throughout the positive electrode.
[0090] 14 , the initial capacity of the lithium ion secondary battery produced using the cathode material of Example 1 is slightly lower than the initial capacity of the lithium ion secondary battery produced using the cathode material of Comparative Example 1. This is thought to be because the entire surface of the cathode active material 10 is covered with the nonaqueous binder 20 in a shell-like shape, which increases the electrical resistance on the surface of the cathode active material 10.
[0091] [Example 3] <Preparation of Cathode Material> A powder of a cathode active material (lithium iron phosphate) and a powder of metal oxides (titanium oxide and niobium oxide) were mixed in a mass ratio of 99.8:0.2, and the mixture was sintered at a temperature of 800°C for 180 minutes to adhere metal oxide 30 to the surface of cathode active material 10.
[0092] Thereafter, in the same manner as in Example 1, the entire surface of the positive electrode active material 10 was coated with a non-aqueous binder (PVDF) to form a shell-like coating so as to cover the metal oxide, thereby producing a positive electrode material 1 having the structure shown in FIG. 5 .
[0093] <Evaluation of Cycle Characteristics of Lithium Ion Secondary Battery> A lithium ion secondary battery was produced using the cathode material 1 produced in Example 3 in the same manner as in Example 1, and the cycle characteristics were measured.
[0094] FIG. 15 is a graph showing the measurement results of cycle characteristics, in which the graph indicated by arrow A shows the cycle characteristics of the lithium ion secondary battery produced using the cathode material of Example 1, the graph indicated by arrow B shows the cycle characteristics of the lithium ion secondary battery produced using the cathode material of Comparative Example 1, and the graph indicated by arrow C shows the cycle characteristics of the lithium ion secondary battery produced using the cathode material of Example 3.
[0095] 15 , it can be seen that the initial capacity of the lithium ion secondary battery fabricated using the cathode material of Example 3 is improved compared to the initial capacity of the lithium ion secondary battery fabricated using the cathode material of Example 1. This is thought to be because the metal oxide 30 with low electrical resistance was attached to the surface of the cathode active material 10, thereby suppressing an increase in electrical resistance on the surface of the cathode active material 10. Note that the improvement in cycle characteristics achieved by coating the entire surface of the cathode active material 10 with the nonaqueous binder 20 in a shell-like form was maintained.
[0096] Although the present invention has been described above with reference to preferred embodiments, such description is not intended to be limiting and various modifications are possible.
[0097] For example, in the above embodiment, the cathode material 1 is manufactured by dissolving a powder of the non-aqueous binder 20 in a non-aqueous solvent, dispersing a powder of the cathode active material 10 in the non-aqueous solvent, and then evaporating the non-aqueous solvent to coat the entire surface of the cathode active material 10 in a shell-like manner with the non-aqueous binder 20. However, the present invention is not limited to this. For example, if the average particle size of the non-aqueous binder 20 is about half or less of the average particle size of the cathode active material 10, the cathode active material 10 may be manufactured by mixing and heating a powder of the cathode active material 10 and a powder of the finely divided non-aqueous binder 20 without using an aqueous solvent such as water or a non-aqueous solvent such as an organic solvent. In this case, the average particle size of the cathode active material 10 is preferably in the range of 1 μm to 10 μm.
[0098] In the above embodiment, the positive electrode is used as an example of the electrode of the secondary battery. However, the negative electrode may be made of lithium titanate (Li 4 Ti 5 O 12 Even when a negative electrode active material containing lithium, such as graphite or silicon, is used, the lithium of the negative electrode active material does not dissolve in the aqueous solvent, thereby suppressing a decrease in the negative electrode capacity. Furthermore, even when a negative electrode active material, such as graphite or silicon, is used in the negative electrode, the negative electrode active materials are bound together and between the negative electrode active material and the current collector by the uniformly dispersed non-aqueous binder, thereby realizing a secondary battery with excellent cycle characteristics.
[0099] REFERENCE SIGNS LIST 1 Positive electrode material (electrode material) 10 Positive electrode active material (electrode active material) 20, 40 Non-aqueous binder 30 Metal oxide 50 Region surrounded by positive electrode active material coated with non-aqueous binder
Claims
1. An electrode material for a secondary battery, comprising an electrode active material, the entire surface of the electrode active material being coated in a shell shape with a non-aqueous binder.
2. The electrode material according to claim 1, wherein a portion of the surface of the electrode active material is covered with a metal oxide, and the non-aqueous binder forms a shell-like coating over the entire surface of the electrode active material so as to cover the metal oxide.
3. An electrode material for a secondary battery, comprising an electrode active material, the entire surface of the electrode active material being covered in a shell shape with either a non-aqueous binder or a metal oxide.
4. An electrode material for a secondary battery, comprising: an electrode active material; an entire surface of the electrode active material is covered in a shell shape with a metal oxide; and a portion of the surface of the metal oxide is covered with a non-aqueous binder.
5. The electrode material according to any one of claims 1 to 4, wherein the non-aqueous binder contains a fluorine-based resin.
6. The electrode material according to any one of claims 1 to 4, wherein the electrode active material is a positive electrode active material.
7. The electrode material according to any one of claims 1 to 4, wherein the electrode active material comprises a lithium-containing composite oxide.
8. An electrode slurry comprising an electrode mixture, the electrode mixture comprising the electrode material according to any one of claims 1 to 4 and a conductive assistant, the electrode mixture being dispersed in an aqueous solvent.
9. The electrode slurry according to claim 8, wherein the non-aqueous binder coating the surface of the electrode active material is not dissolved in the aqueous solvent.
10. The electrode slurry according to claim 8, wherein the conductive assistant comprises cellulose nanofibers.
11. A method for producing an electrode material for a secondary battery, comprising: a step of dissolving a powder of a non-aqueous binder in a non-aqueous solvent and dispersing a powder of an electrode active material in the non-aqueous solvent; and a step of evaporating the non-aqueous solvent to coat the entire surface of the electrode active material with the non-aqueous binder in a shell-like shape.
12. The method for producing an electrode material according to claim 11, further comprising a step of adhering a metal oxide to a portion of the surface of the electrode active material prior to the two steps, and the entire surface of the electrode active material is coated with the non-aqueous binder in a shell shape so as to cover the metal oxide.
13. A method for producing an electrode material for a secondary battery, comprising: a step of adhering a metal oxide to a portion of the surface of an electrode active material; a step of dissolving a non-aqueous binder powder in a non-aqueous solvent and dispersing the powder of the electrode active material having the metal oxide adhered to its surface in the non-aqueous solvent; and a step of evaporating the non-aqueous solvent, wherein in the step of evaporating the non-aqueous solvent, the entire surface of the electrode active material is covered in a shell-like shape with either the non-aqueous binder or the metal oxide.
14. A method for producing an electrode material for a secondary battery, comprising the steps of: attaching a metal oxide to the entire surface of an electrode active material; dissolving a powder of a non-aqueous binder in a non-aqueous solvent and dispersing the powder of the electrode active material having the metal oxide attached to its entire surface in the non-aqueous solvent; and evaporating the non-aqueous solvent, wherein in the step of evaporating the non-aqueous solvent, a portion of the surface of the metal oxide is covered with the non-aqueous binder.
15. An electrode for a secondary battery comprising an electrode mixture formed on a current collector, the electrode mixture comprising the electrode material according to any one of claims 1 to 4 and a conductive assistant, the electrode active material contained in the electrode material is dispersed in a state in which the entire surface is covered with a shell-like non-aqueous binder, and the total volume of the non-aqueous binder covering the entire surface of the electrode active material is V 1 The total volume of the non-aqueous binder present in the region surrounded by the electrode active material coated with the non-aqueous binder is V 2 Then, V 1 >V 2 That is, the electrode.
16. An electrode for a secondary battery comprising an electrode mixture formed on a current collector, the electrode mixture comprising the electrode material according to any one of claims 1 to 4 and a conductive assistant, the electrode active material contained in the electrode material is dispersed in a state in which the entire surface is covered with a non-aqueous binder in a shell shape, and the total area of the non-aqueous binder covering the entire surface of the electrode active material in a cross section of the electrode mixture is A 1 The total area of the non-aqueous binder present in the region surrounded by the electrode active material coated with the non-aqueous binder is A 2 Then, A 1 >A 2 That is, the electrode.
17. An electrode for a secondary battery comprising an electrode mixture formed on a current collector, the electrode mixture comprising the electrode material according to any one of claims 1 to 4 and a conductive assistant, the electrode active material contained in the electrode material is uniformly dispersed in a state in which the entire surface is covered with a non-aqueous binder in a shell shape, and the sum of the volumes of the regions surrounded by the electrode active material covered with the non-aqueous binder is V 3 The total volume of the non-aqueous binder present in the region surrounded by the electrode active material coated with the non-aqueous binder is V 2 Then, V 3 >V 2 That is, the electrode.
18. An electrode for a secondary battery comprising an electrode mixture formed on a current collector, the electrode mixture comprising the electrode material according to any one of claims 1 to 4 and a conductive assistant, the electrode active material contained in the electrode material is uniformly dispersed in a state in which the entire surface is covered with a non-aqueous binder in a shell shape, and the sum of the areas of the regions surrounded by the electrode active material covered with the non-aqueous binder in a cross section of the electrode mixture is A 3 The total area of the non-aqueous binder present in the region surrounded by the electrode active material coated with the non-aqueous binder is A 2 Then, A 3 >A 2 That is, the electrode.
19. A method for manufacturing an electrode for a secondary battery, comprising the steps of: forming an electrode material in which the entire surface of an electrode active material is covered in a shell shape with a non-aqueous binder by the method described in any one of claims 11 to 14; dispersing an electrode mixture containing the electrode material and a conductive assistant in an aqueous solvent to form an electrode slurry; and coating the electrode slurry on a current collector and then drying the coating film.
20. An electrode material for a secondary battery, comprising an electrode active material, a portion of a surface of the electrode active material being coated in a shell shape with a non-aqueous binder.
21. The electrode material according to claim 20, wherein 50% or more of the surface of the electrode active material is covered with the non-aqueous binder.
22. The electrode material according to claim 20, wherein the non-aqueous binder contains a fluorine-based resin.
23. The electrode material according to claim 20, wherein the electrode active material comprises a positive electrode active material.
24. The electrode material according to claim 20, wherein the electrode active material comprises a lithium-containing composite oxide.
25. An electrode slurry comprising an electrode mixture, the electrode mixture comprising the electrode material according to any one of claims 20 to 24 and a conductive assistant, the electrode mixture being dispersed in an aqueous solvent.
26. The electrode slurry according to claim 25, wherein the non-aqueous binder coating the surface of the electrode active material is not dissolved in the aqueous solvent.
27. The electrode slurry according to claim 25, wherein the conductive assistant comprises cellulose nanofibers.
28. A method for producing an electrode material for a secondary battery, comprising: a step of dissolving a powder of a non-aqueous binder in a non-aqueous solvent and dispersing a powder of an electrode active material in the non-aqueous solvent; and a step of evaporating the non-aqueous solvent to coat a part of the surface of the electrode active material with the non-aqueous binder in a shell-like shape.
29. An electrode for a secondary battery comprising an electrode mixture formed on a current collector, the electrode mixture comprising the electrode material according to any one of claims 20 to 24 and a conductive assistant, the electrode active material contained in the electrode material is dispersed in a state in which a part of the surface is covered with a shell-like non-aqueous binder, and the total volume of the non-aqueous binder covering the entire surface of the electrode active material is V 1 The total volume of the non-aqueous binder present in the region surrounded by the electrode active material coated with the non-aqueous binder is V 2 Then, V 1 >V 2 That is, the electrode.
30. An electrode for a secondary battery comprising an electrode mixture formed on a current collector, the electrode mixture comprising the electrode material according to any one of claims 20 to 24 and a conductive assistant, the electrode active material contained in the electrode material is dispersed in a state in which a part of the surface is covered with a non-aqueous binder in a shell shape, and the total area of the non-aqueous binder covering the entire surface of the electrode active material in a cross section of the electrode mixture is A 1 The total area of the non-aqueous binder present in the region surrounded by the electrode active material coated with the non-aqueous binder is A 2 Then, A 1 >A 2 That is, the electrode.
31. An electrode for a secondary battery comprising an electrode mixture formed on a current collector, the electrode mixture comprising the electrode material according to any one of claims 20 to 24 and a conductive assistant, the electrode active material contained in the electrode material is dispersed in a state in which a part of the surface is covered with a non-aqueous binder in a shell shape, and the sum of the volumes of the regions surrounded by the electrode active material covered with the non-aqueous binder is defined as V. 3 The total volume of the non-aqueous binder present in the region surrounded by the electrode active material coated with the non-aqueous binder is V 2 Then, V 3 >V 2 That is, the electrode.
32. An electrode for a secondary battery comprising an electrode mixture formed on a current collector, the electrode mixture comprising the electrode material according to any one of claims 20 to 24 and a conductive assistant, the electrode active material contained in the electrode material is dispersed in a state in which a part of the surface is coated with a non-aqueous binder in a shell shape, and the sum of the areas of the regions surrounded by the electrode active material coated with the non-aqueous binder in a cross section of the electrode mixture is A 3 The total area of the non-aqueous binder present in the region surrounded by the electrode active material coated with the non-aqueous binder is A 2 Then, A 3 >A 2 That is, the electrode.
33. An electrode for a secondary battery comprising an electrode mixture formed on a current collector, the electrode mixture comprising the electrode material according to any one of claims 20 to 24 and a conductive assistant, the electrode active material contained in the electrode material is dispersed in a state in which a part of the surface is covered in a shell shape with a non-aqueous binder, and the coverage C defined by the following formula (1) is 30% or more in the cross section of the electrode mixture. C=(C 2 ÷C 1 ) × 100 (1) (In formula (1), C 1 represents the perimeter of the electrode active material, and C 2 represents the total length of the contact portion of the non-aqueous binder that is in contact with the periphery of the electrode active material.) 34. A method for manufacturing an electrode for a secondary battery, comprising the steps of: forming an electrode material in which a portion of the surface of an electrode active material is covered in a shell shape with a non-aqueous binder by the method described in claim 28; dispersing an electrode mixture containing the electrode material and a conductive assistant in an aqueous solvent to form an electrode slurry; and applying the electrode slurry onto a current collector and then drying the applied film.
Citation Information
Patent Citations
Positive electrode, secondary battery, and method of manufacturing the same
JP2017091789A
Lithium secondary battery
JP2008159385A
Nonaqueous electrolyte secondary battery
JP2011181386A
Method for producing positive electrode for secondary battery, secondary battery, and method for producing stack for secondary battery
WO2014057993A1