Top plate for cooking device, production method therefor, and method for assessing charring
The use of an organopolysiloxane-coated glass substrate on cooker top plates addresses the challenges of burnt-on material removal and surface durability, enabling efficient burn removal and objective evaluation by enhancing the cooking surface's hardness and heat resistance.
Patent Information
- Application Number
- PCT/JP2024/011978
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-11-29
- Filing Date
- 2024-03-26
- Publication Date
- 2024-10-03
AI Technical Summary
Existing cooker top plates face difficulties in easily removing burnt-on material from the cooking surface and suffer from scratches or peeling of the coating film when a fluorine-based coating is used, leading to subjective evaluation of burn removal ease and variability among evaluators.
A top plate with a glass substrate coated with an organopolysiloxane film having a trifunctional siloxane unit, providing a three-dimensional crosslinked structure with a thickness of 100 nm or less, and a hydrolyzed condensate of a trifunctional alkoxide, which enhances the cooking surface's hardness and facilitates easy removal of burnt material while maintaining heat resistance and reducing the risk of scratches.
The solution allows for easy removal of burnt material from the cooking surface, maintains excellent hardness to prevent scratches, and provides a reliable method for evaluating burn removal ease with minimal variability among evaluators, ensuring effective performance under heat resistance tests.
Smart Images

Figure JP2024011978_03102024_PF_FP_ABST
Abstract
Description
Cooking appliance top plate, manufacturing method thereof, and method for evaluating burn-on
[0001] The present invention relates to a top plate for a cooker, a method for manufacturing the top plate for a cooker, and a method for evaluating scorching.
[0002] A cooking appliance top plate is provided on the top of an induction cooker, a radiant heater cooker, a gas cooker, etc. The cooking appliance top plate is made of a glass substrate having a front surface on which a cooking utensil is placed and a back surface opposite the cooking surface.
[0003] In the following Patent Document 1, Li 2 O-Al 2 O 3 -SiO 2 The top plate for a cooker disclosed in Patent Document 1 uses a crystallized glass substrate containing a transition element and having a main component of 1,000 to 1,000 ppm or more. In the top plate for a cooker disclosed in Patent Document 1, a brightness improving layer and a substrate color improving layer are provided on the lower surface (rear surface) of the crystallized glass substrate, but no film is provided on the cooking surface side.
[0004] Furthermore, Patent Document 2 listed below discloses a top plate for a cookware having a base made of crystallized glass and a cooking surface on which an object to be heated is placed. The cooking surface of the top plate for a cookware in Patent Document 2 has a surface structure containing fluorine.
[0005] Furthermore, Patent Document 3 listed below discloses a top plate for a cooker, which includes a substrate and a coating layer having a columnar structure formed on one surface of the substrate and composed of a plurality of columnar structures made of zirconium oxide. In Patent Document 3, a burnt-on removal test was conducted on each sample of the cooker top plate produced in the examples and comparative examples. In the burnt-on removal test, a commercially available barbecue sauce was dripped onto each sample of the cooker top plate, and the sample was baked at 150°C for 30 minutes to prepare a sample for evaluation. Half of the sample was then immersed in water for 5 minutes, and then a wooden stick was placed on the sample at a pressure of 10 kg / cm. 2The burnt-on removal test is conducted by pressing the sample against the plate with a force of 1000 and rubbing it 50 times. In Patent Document 3, the burnt-on removal test is used to determine which top plates for cookware can be easily removed even if burnt-on food occurs.
[0006] JP 2021-178774 A JP 09-132428 A JP 2011-196667 A
[0007] However, when the surface of a glass substrate serves as a cooking surface, as in the case of the cooker top plate of Patent Document 1, food may be spilled on the cooking surface during heating, for example, when food boils over inside the cookware. In this case, the burnt-on food adhering to the cooking surface can be difficult to remove. Furthermore, the burnt-on food removal test of Patent Document 3, which involves scraping off the burnt food and observing how it is removed, makes it difficult to objectively evaluate the ease of removing the burnt-on food.
[0008] Furthermore, even if burnt food is scraped off under certain conditions, there is a problem that the degree of removal varies depending on the evaluator. On the other hand, when a coating film containing fluorine is provided on a glass substrate and the surface of the coating film serves as a cooking surface, as in the case of the top plate for a cooker in Patent Document 2, the coating film provided on the cooking surface may rub against a cooking utensil such as a pot, causing scratches on the coating film or peeling off. Therefore, there is a need for a top plate for a cooker that makes it easy to remove burnt food attached to the cooking surface and that has excellent hardness on the cooking surface side.
[0009] An object of the present invention is to provide a top plate for a cooker that is easy to remove when burnt food is spilled on the cooking surface and that has excellent hardness on the cooking surface side, and a method for manufacturing the top plate for the cooker. Another object of the present invention is to provide a method for evaluating burnt-on surfaces, which can reliably evaluate the ease of removing burnt-on materials from plate-like members such as a top plate for a cooker with little variability between evaluators.
[0010] A top plate for a cooker that solves the above-mentioned problems and various aspects of a method for manufacturing the top plate for a cooker will be described below.
[0011] A top plate for a cooker according to a first aspect of the present invention comprises a glass substrate and a coating film provided on a main surface of the glass substrate, the coating film containing an organopolysiloxane having a trifunctional siloxane unit represented by the following formula (1), wherein the coating film has a three-dimensional crosslinked structure including siloxane bonds, and the coating film has a thickness of 100 nm or less.
[0012]
[0013] (In formula (1), R 1 is an alkyl group having 1 to 6 carbon atoms, a phenyl group, or a vinyl group.
[0014] A top plate for a cooker according to Aspect 2 is preferably the same as Aspect 1, wherein the surface of the coating film has an arithmetic mean height Sa of 0.4 nm or more and 10 nm or less, measured with a measurement field size of 316.77 μm × 237.72 μm and a resolution of 640 pixels × 480 pixels.
[0015] A top plate for a cooker according to Aspect 3 is the top plate for a cooker according to Aspect 1 or Aspect 2, wherein the contact angle of water with the surface of the coating film is preferably 80 degrees or more.
[0016] A top plate for a cooker according to Aspect 4 is the top plate of any one of Aspects 1 to 3, wherein the glass substrate is preferably made of borosilicate glass or low-expansion glass-ceramics.
[0017] A top plate for a cooker according to Aspect 5 is the top plate for a cooker according to any one of Aspects 1 to 4, wherein the average linear thermal expansion coefficient of the glass substrate at 30°C to 380°C is 40 x 10 -7 / °C or less is preferred.
[0018] A top plate for a cooker according to Aspect 6 is any one of Aspects 1 to 5, wherein the coating film preferably contains a hydrolysis condensate of a trifunctional alkoxide represented by the following formula (2):
[0019]
[0020] (In formula (2), R 1 is an alkyl group having 1 to 6 carbon atoms, a phenyl group, or a vinyl group, and R is an alkoxy group.
[0021] A top plate for a cooker according to Aspect 7 is the top plate for a cooker according to Aspect 6, wherein the R 1 is preferably a methyl group.
[0022] A top plate for a cooker according to Aspect 8 is any one of Aspects 1 to 7, and preferably has a pencil hardness of 9H or more as measured from the coating film side of the top plate for a cooker.
[0023] The top plate for a cooker according to Aspect 9 is preferably any one of Aspects 1 to 8, in which a scorching evaluation sample is prepared by dropping an evaluation liquid onto the surface of the coating film and heating it, and when the scorching evaluation sample is photographed from the opposite side of the glass substrate from the coating film, the area ratio of the scorched portion determined from the obtained image is 70% or less.
[0024] The top plate for a cooker according to Aspect 10 is preferably any one of Aspects 1 to 9, in which, when subjected to a heat resistance test at a temperature of 350°C for 24 hours, the change in the contact angle of water on the surface of the coating film before and after the heat resistance test is less than 3 degrees.
[0025] A top plate for a cooker according to an eleventh aspect is any one of the first to tenth aspects, wherein the surface of the top plate for a cooker on the side of the coating film is preferably a cooking surface on which a cookware is placed.
[0026] The top plate for a cooker according to aspect 12 is any one of aspects 1 to 11, and may have a printed layer having a pattern on the main surface of the glass substrate, and the coating film may be provided on the main surface of the glass substrate so as to cover the printed layer.
[0027] A top plate for a cooker according to Aspect 13 is the same as Aspect 12, wherein the pattern is preferably a dot-like, lattice-like, line-like, or ring-like pattern.
[0028] A manufacturing method of a top plate for a cooker according to Aspect 14 of the present invention is a manufacturing method of a top plate for a cooker comprising a glass substrate and a coating film provided on a main surface of the glass substrate, characterized by comprising the steps of: applying, onto the main surface of the glass substrate, a coating liquid containing a compound represented by the following formula (2) or a hydrolysis-condensation product obtained by hydrolyzing and condensing at least a portion of the compound; and baking the glass substrate coated with the coating liquid at a temperature of 200°C or higher to form a coating film on the main surface of the glass substrate.
[0029]
[0030] (In formula (2), R 1 is an alkyl group having 1 to 6 carbon atoms, a phenyl group, or a vinyl group, and R is an alkoxy group.
[0031] A method for producing a top plate for a cooker according to Aspect 15 comprises the steps of: 1 is preferably a methyl group.
[0032] The burn-on evaluation method according to aspect 16 of the present invention is a burn-on evaluation method for evaluating the ease of removal of burn-on matter on a plate-shaped member, and is characterized by comprising a preparation step of preparing a plate-shaped member having opposing first and second main surfaces and preparing a burn-on evaluation sample on the first main surface of the plate-shaped member, and an evaluation step of evaluating the ease of removal of burn-on matter in the burn-on evaluation sample from the second main surface side of the plate-shaped member.
[0033] The method for evaluating burn-in according to aspect 17 is preferably the same as in aspect 16, wherein the evaluation step includes an imaging step of imaging the burn-in evaluation sample from the second main surface side of the plate-shaped member, and a measurement step of measuring the area of at least one of the burnt portion and the non-burnt portion in the burn-in evaluation sample from the image captured in the imaging step.
[0034] In the method for evaluating scorching according to aspect 18, in the manufacturing process of aspect 16 or aspect 17, an evaluation liquid may be dripped onto the first main surface of the plate-shaped member, and the plate-shaped member onto which the evaluation liquid has been dripped may be heated to produce a scorching evaluation sample on the first main surface of the plate-shaped member.
[0035] In the method for evaluating scorching according to Aspect 19, in the imaging step of Aspect 17 or Aspect 18, the scorching evaluation sample may be imaged from the second main surface side of the plate-like member using bright field illumination.
[0036] In the burn-on evaluation method according to aspect 20, in the measurement step of any one of aspects 17 to 19, the area of the entire region in which the burn-on evaluation sample is provided may be measured from the image captured in the imaging step.
[0037] In the method for evaluating scorching according to aspect 21, in the manufacturing process of any one of aspects 18 to 20, after dripping the evaluation liquid, the area of the drop of the evaluation liquid may be measured before heating the plate-shaped member, thereby measuring the area of the entire region in which the scorching evaluation sample is provided.
[0038] In the burn-on evaluation method of aspect 22, in the measurement process of any one of aspects 17 to 21, a burn-on area ratio, which is the ratio of the area of the burnt portion to the area of the entire region in which the burn-on evaluation sample is provided, may be calculated.
[0039] In the method for evaluating scorching according to Aspect 23, in the measuring step of Aspect 22, whether the plate-like member is a good product or a bad product may be determined from the scorched area ratio.
[0040] A top plate for a cooker according to aspect 24 of the present invention is characterized in that the burnt area ratio determined by the burnt-on evaluation method according to any one of aspects 16 to 23 is 70% or less.
[0041] According to the present invention, it is possible to provide a top plate for a cooker that is easy to remove when burnt food is spilled on the cooking surface and that has excellent hardness on the cooking surface side, and a method for manufacturing the top plate for the cooker. Furthermore, according to the present invention, it is possible to provide a method for evaluating burnt-on properties that can reliably evaluate the ease of removing burnt-on materials from a plate-like member such as a top plate for a cooker with little variability between evaluators.
[0042] FIG. 1 is a schematic cross-sectional view showing a top plate for a cooker according to a first embodiment of the present invention. FIG. 2 is a schematic view illustrating the surface condition of the cooking surface of the top plate for a cooker according to the first embodiment of the present invention. FIG. 3 is a view illustrating a method for evaluating the burnt area ratio. FIG. 4 is a schematic cross-sectional view showing a top plate for a cooker according to a second embodiment of the present invention. FIG. 5 is a schematic view illustrating the surface condition of the cooking surface of a top plate for a cooker according to a comparative example. FIG. 6 is a schematic cross-sectional view showing a top plate for a cooker according to a third embodiment of the present invention. FIG. 7 is a schematic cross-sectional view illustrating an example of a plate-like member used in the method for evaluating burnt food according to a fourth embodiment of the present invention. FIGS. 8(a) to 8(c) are schematic cross-sectional views illustrating a manufacturing process in the method for evaluating burnt food according to the fourth embodiment of the present invention. FIG. 9 is a schematic cross-sectional view illustrating an imaging process in the method for evaluating burnt food according to the fourth embodiment of the present invention. FIG. 10 is a view illustrating an example of a photograph captured in the imaging process in the method for evaluating burnt food according to the fourth embodiment of the present invention. Fig. 11 is a diagram for explaining a method for measuring the areas of the burnt and non-burnt portions in the photograph of Fig. 10. Figs. 12(a) and (b) are photographs for confirming the anti-burn effect in Example 22. Figs. 13(a) and (b) are photographs for confirming the anti-burn effect in Comparative Example 9.
[0043] Preferred embodiments will be described below, but the following embodiments are merely examples and the present invention is not limited to the following embodiments.
[0044] [First embodiment] (Top plate for cooking appliance) Fig. 1 is a schematic cross-sectional view showing a top plate for a cooking appliance according to a first embodiment of the present invention. As shown in Fig. 1, a top plate for a cooking appliance 1 (hereinafter, "top plate for a cooking appliance" may be simply referred to as "top plate") includes a glass substrate 2. The glass substrate 2 has a front surface 2a and a back surface 2b that face each other. The front surface 2a is the main surface that faces the cooking surface 1a on which cooking utensils such as pots and frying pans are placed. The back surface 2b is the main surface that faces a light source or a heating device inside the cooking appliance. Therefore, the front surface 2a and the back surface 2b are in a front-back relationship.
[0045] The glass substrate 2 preferably has an average transmittance of 20% or more in the wavelength range of 700 nm to 3000 nm. This makes it easier to improve heating performance when the top plate 1 is used in an induction cooking heater, a radiant heater, or the like. The average transmittance of the glass substrate 2 in the wavelength range of 700 nm to 3000 nm is more preferably 30% or more, even more preferably 40% or more, and particularly preferably 50% or more. The upper limit of the average transmittance of the glass substrate 2 in the wavelength range of 700 nm to 3000 nm is not particularly limited, but may be, for example, 90% or less or 80% or less.
[0046] The glass substrate 2 may also transmit at least a portion of light in the wavelength range of 400 nm to 700 nm. The glass substrate 2 may be colored and transparent in the visible range, but is preferably colorless and transparent in the visible range from the viewpoint of further enhancing the aesthetic appeal of the top plate 1. In this specification, "transparent in the visible range" means that the light transmittance in the visible wavelength range of 400 nm to 700 nm is 70% or more.
[0047] The top plate 1 is repeatedly heated and cooled. Therefore, it is preferable that the glass substrate 2 has high heat resistance and a low thermal expansion coefficient. Specifically, the softening temperature of the glass substrate 2 is preferably 700°C or higher, more preferably 750°C or higher, even more preferably 800°C or higher, and particularly preferably 850°C or higher. In addition, the average linear thermal expansion coefficient of the glass substrate 2 at 30°C to 380°C is preferably -10 x 10 -7 / °C or more, more preferably -8 × 10 -7 / °C or more, more preferably -5 × 10 -7 / °C or more, preferably 50 x 10 -7 / °C or less, more preferably 45 x 10 -7 / °C or less, more preferably 40 x 10 -7 / °C or less, and even more preferably 35 x 10 -7 / °C or less, and even more preferably 30 x 10 -7 / °C or less, and even more preferably 25 x 10 -7 / °C or less, and even more preferably 20 x 10 -7 / °C or less, and even more preferably 15 x 10 -7 / °C or less, particularly preferably 10 x 10 -7 / °C or less. Therefore, it is preferable that the glass substrate 2 is made of glass with a high glass transition temperature and low expansion, or low-expansion crystallized glass (low-expansion crystallized glass). A specific example of low-expansion crystallized glass is "N-0" manufactured by Nippon Electric Glass Co., Ltd. In this case, it is possible to easily improve the heat resistance and thermal shock resistance of the top plate 1. Furthermore, borosilicate glass or the like may be used for the glass substrate 2, or alkali-free glass, aluminosilicate glass, or the like. In this case, it is possible to reduce costs. In addition, in this case, it is possible to easily obtain transparent glass.
[0048] There is no particular limitation on the thickness of the glass substrate 2. The thickness of the glass substrate 2 can be appropriately set depending on the light transmittance, etc. The thickness of the glass substrate 2 can be, for example, about 2 mm to 6 mm.
[0049] The surface 2a of the glass substrate 2 is preferably smooth, and more preferably an unpolished surface (fire-polished surface). The arithmetic mean height Sa on the surface 2a of the glass substrate 2 is preferably 0.5 nm or less, more preferably 0.4 nm or less, and even more preferably 0.3 nm or less. The lower limit of the arithmetic mean height Sa on the surface 2a of the glass substrate 2 is not limited, but may be 0.1 nm or more. When the arithmetic mean height Sa on the surface 2a of the glass substrate 2 is equal to or less than the above upper limit, it becomes easier to adjust the film thickness of the coating film 3 and the arithmetic mean height Sa on the surface 3a of the coating film 3. Furthermore, a high-quality appearance with little haze can be obtained.
[0050] The arithmetic mean height Sa is a parameter defined by ISO 25178. In this embodiment, the arithmetic mean height Sa can be measured with a measurement field size of 316.77 μm×237.72 μm and a resolution of 640 pixels×480 pixels.
[0051] A coating film 3 is provided on the surface 2a of the glass substrate 2. The coating film 3 contains an organopolysiloxane having a trifunctional siloxane unit represented by the following formula (1). The coating film 3 also has a three-dimensional crosslinked structure including siloxane bonds. The thickness of the coating film 3 is 100 nm or less.
[0052]
[0053] In formula (1), R 1 is an alkyl group having 1 to 6 carbon atoms, a phenyl group, or a vinyl group. 1 is preferably an alkyl group having 1 to 6 carbon atoms or a phenyl group. In this case, when food is burnt on the cooking surface 1a, the burnt food can be more easily removed. Furthermore, in formula (1), R 1 is more preferably a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, a pentyl group, a hexyl group, or a phenyl group, and even more preferably a methyl group or a phenyl group. In particular, a methyl group or a phenyl group is preferred because of its excellent heat resistance.
[0054] The organopolysiloxane is preferably a hydrolysis condensation product of a trifunctional alkoxide represented by the following formula (2).
[0055]
[0056] In formula (2), R 1 is an alkyl group having 1 to 6 carbon atoms, a phenyl group, or a vinyl group, and R is an alkoxy group. 1 is preferably an alkyl group having 1 to 6 carbon atoms or a phenyl group. In this case, when food is burnt on the cooking surface 1a, the burnt food can be more easily removed. Furthermore, in formula (2), R 1 is more preferably a methyl group, ethyl group, n-propyl group, isopropyl group, n-butyl group, isobutyl group, sec-butyl group, tert-butyl group, pentyl group, hexyl group, or phenyl group, and even more preferably a methyl group or a phenyl group. In particular, a methyl group or a phenyl group is preferable because of its excellent heat resistance. R is preferably a methoxy group, ethoxy group, propoxyl group, butoxy group, pentoxy group, or hexoxy group, and more preferably a methoxy group or an ethoxy group.
[0057] Examples of trifunctional alkoxides include methyltrimethoxysilane, methyltriethoxysilane, methyltri(n-propoxy)silane, methyltri(i-propoxy)silane, methyltri(n-butoxy)silane, methyl(n-pentoxy)silane, methyl(n-hexoxy)silane, methyltri(phenoxy)silane, ethyltrimethoxysilane, ethyltriethoxysilane, ethyltri(n-propoxy)silane, ethyltri(i-propoxy)silane, ethyltri(n-butoxy)silane, ethyltri(n-pentoxy)silane, ethyltri(n-hexoxy)silane, and ethyltri(phenoxy)silane. Si)silane, ethyltriphenoxysilane, n-propyltrimethoxysilane, n-propyltriethoxysilane, n-propyltri(n-propoxy)silane, n-propyltri(i-propoxy)silane, i-propyltrimethoxysilane, i-propyltriethoxysilane, i-propyltri(n-propoxy)silane, i-propyltri(i-propoxy)silane, n-butyltrimethoxysilane, n-butyltriethoxysilane, n-butyltri(n-propoxy)silane, n-butyltri(i-propoxy)silane, n-butyltri(n-butyl cyclopentyltrimethoxysilane, n-pentyltriethoxysilane, n-pentyltri(n-propoxy)silane, n-pentyltri(i-propoxy)silane, n-pentyltri(n-butoxy)silane, n-pentyltri(n-pentoxy)silane, cyclopentyltrimethoxysilane, cyclopentyltriethoxysilane, cyclopentyl(n-propoxy)silane, cyclopentyl(i-propoxy)silane, cyclopentyltri(n-butoxy)silane, cyclopentyltri(n-pentoxy)silane, cyclopentyltri (cyclopentoxy)silane, n-hexyltrimethoxysilane, n-hexyltriethoxysilane, n-hexyltri(n-propoxy)silane, n-hexyltri(i-propoxy)silane, n-hexyltri(n-butoxy)silane, n-hexyltri(n-pentoxy)silane, n-hexyltri(n-hexoxy)silane, cyclohexyltrimethoxysilane, cyclohexyltriethoxysilane, cyclohexyltri(n-propoxy)silane, cyclohexyltri(n-butoxy)silane, cyclohexyltri(n-pentoxy)silane,Examples of such silanes include cyclohexyltri(n-hexoxyl)silane, cyclohexyltri(cyclohexoxy)silane, phenyltrimethoxysilane, phenyltriethoxysilane, phenyltri(n-propoxy)silane, phenyltri(n-butoxy)silane, phenyltri(n-pentoxy)silane, phenyltri(n-hexoxy)silane, phenyltri(phenoxy)silane, vinyltrimethoxysilane, vinyltriethoxysilane, vinyltri(n-propoxy)silane, vinyltri(i-propoxy)silane, vinyltri(n-butoxy)silane, vinyl(n-pentoxy)silane, vinyl(n-hexoxy)silane, and vinyltri(phenoxy)silane. The trifunctional alkoxide is preferably methyltrimethoxysilane, methyltriethoxysilane, phenyltrimethoxysilane, phenyltriethoxysilane, vinyltrimethoxysilane, or vinyltriethoxysilane, more preferably methyltrimethoxysilane, methyltriethoxysilane, phenyltrimethoxysilane, or phenyltriethoxysilane, and even more preferably methyltriethoxysilane.
[0058] The top plate 1 of this embodiment has the above-mentioned configuration, so when food spills or the like and burns to the cooking surface 1a, the burnt food is easy to remove, and the cooking surface 1a side has excellent hardness.
[0059] In conventional top plates, when the surface of a glass substrate serves as a cooking surface, food can be burned onto the cooking surface when spilled during heating, such as when food boils over inside the cookware. In this case, there is a problem that the burned food attached to the cooking surface is difficult to remove. Furthermore, when a coating film is provided on the glass substrate and the surface of the coating film serves as the cooking surface, the coating film on the cooking surface can rub against a cookware such as a pot, causing scratches or peeling of the coating film.
[0060] In response to this, the present inventors focused on the coating film 3 provided on the surface 2a of the glass substrate 2, and discovered that by using a film having the above-mentioned specific structure and film thickness as the coating film 3, even if food spills or the like and burns to the cooking surface 1a, the burnt-on food can be easily removed, and the hardness of the cooking surface 1a can be increased.
[0061] The reason for this can be explained as follows.
[0062] 5, when the cooking surface 101a is formed by the surface 102a of the glass substrate 102, hydroxyl groups are unevenly distributed on the surface 102a (cooking surface 101a) of the glass substrate 102. The hydroxyl groups unevenly distributed on the cooking surface 101a have a high affinity for burnt-on food 110, and therefore, it is thought that the burnt-on food 110 adheres firmly to the cooking surface 101a, making it difficult to remove.
[0063] In contrast, in the top plate 1 of this embodiment, the cooking surface 1a is formed by the coating film 3 having the above-mentioned specific structure, and therefore, as shown in Figure 2, organic substituents such as methyl groups, vinyl groups, and phenyl groups are unevenly distributed on the surface 3a (cooking surface 1a) of the coating film 3. Such organic substituents unevenly distributed on the cooking surface 1a have a low affinity for burnt-on food 10, and are therefore thought to make it easier to remove burnt-on food 10 adhering to the cooking surface 1a. Thus, when the coating film 3 having the above-mentioned specific structure is provided on the glass substrate 2 of the top plate 1, a remarkable effect is exhibited.
[0064] Furthermore, because the top plate 1 facilitates the removal of burnt-on food 10 adhering to the cooking surface 1a due to the above-described mechanism, this effect is exhibited even when the coating film 3 is thin, allowing the coating film 3 to be thinned. In particular, by making the coating film 3 thicker than 100 nm, the high hardness of the glass substrate can be easily utilized, and the hardness of the cooking surface 1a side of the top plate 1 can be further increased. As such, the top plate 1 has excellent hardness on the cooking surface 1a side, making it less likely for the coating film 3 to be scratched by rubbing against cooking utensils such as pots, and also making it less likely for the coating film 3 to peel off from the cooking surface 1a.
[0065] In this embodiment, the thickness of the coating film 3 is preferably 0.5 nm or more, more preferably 1 nm or more, even more preferably 1.7 nm or more, even more preferably 2 nm or more, even more preferably 2.5 nm or more, even more preferably 3 nm or more, even more preferably 3.5 nm or more, even more preferably 4 nm or more, even more preferably 4.5 nm or more, even more preferably 5 nm or more, even more preferably 6 nm or more, even more preferably 7 nm or more, even more preferably 8 nm or more, particularly preferably 9 nm or more, and is preferably 90 nm or less, more preferably 80 nm or less, even more preferably 70 nm or less, even more preferably 60 nm or less, and even more preferably is 55 nm or less, even more preferably 50 nm or less, even more preferably less than 50 nm, even more preferably 45 nm or less, even more preferably 40 nm or less, even more preferably 35 nm or less, even more preferably 30 nm or less, even more preferably 25 nm or less, even more preferably 20 nm or less, even more preferably 19 nm or less, even more preferably 18 nm or less, even more preferably 17 nm or less, even more preferably 16 nm or less, even more preferably 15 nm or less, even more preferably 14 nm or less, even more preferably 13 nm or less, even more preferably 12 nm or less, even more preferably 11 nm or less, and particularly preferably 10 nm or less. When the thickness of the coating film 3 is equal to or greater than the above-mentioned lower limit, burnt-on food 10 adhering to the cooking surface 1a can be more easily removed. Furthermore, the arithmetic mean height Sa of the coating film 3 on the surface 3a can be more easily adjusted. Furthermore, when the thickness of the coating film 3 is equal to or less than the above-mentioned upper limit, the hardness of the cooking surface 1a side of the top plate 1 can be further increased.
[0066] The thickness of the coating film 3 can be measured, for example, by measuring and calculating the spectral reflectance or spectral transmittance, or by calculating by spectroscopic ellipsometry. If these methods are difficult to use, the thickness of the coating film 3 can also be measured by observing the cross section with a transmission electron microscope, or by partially peeling the film and measuring the height of the resulting step with a stylus profilometer or a laser microscope.
[0067] In this embodiment, the arithmetic mean height Sa of the surface 3a of the coating film 3 is preferably 0.3 nm or more, more preferably 0.4 nm or more, even more preferably 0.5 nm or more, even more preferably 1 nm or more, even more preferably 1.5 nm or more, even more preferably 2 nm or more, even more preferably 3 nm or more, even more preferably 4 nm or more, even more preferably 5 nm or more, even more preferably 6 nm or more, even more preferably 7 nm or more, for example, 8 nm or more, 9 nm or more, or 10 nm or more, and is preferably 30 nm or less, more preferably 28 nm or less, even more preferably 25 nm or less, even more preferably 20 nm or less, even more preferably 15 nm or less, even more preferably 12 nm or less, even more preferably 10 nm or less, and particularly preferably 8 nm or less. When the arithmetic mean height Sa of the surface 3a of the coating film 3 is equal to or greater than the above lower limit, burnt-on food 10 adhering to the cooking surface 1a can be more easily removed. Furthermore, when the arithmetic mean height Sa of the surface 3a of the coating film 3 is equal to or less than the above upper limit, a luxurious appearance with little cloudiness can be easily obtained, and the luxurious feel of glass can also be easily maintained to the touch.
[0068] In this embodiment, the contact angle of water with the surface 3a of the coating film 3 is preferably 75 degrees or more, more preferably 80 degrees or more, even more preferably 85 degrees or more, particularly preferably 90 degrees or more, and is preferably 150 degrees or less, more preferably 140 degrees or less, even more preferably 130 degrees or less, and particularly preferably 120 degrees or less. When the contact angle of water with the surface 3a of the coating film 3 is equal to or greater than the above-mentioned lower limit, burnt-on food 10 adhering to the cooking surface 1a can be removed more easily. When the contact angle of water with the surface 3a of the coating film 3 is equal to or less than the above-mentioned upper limit, the surface becomes moderately wettable, making cleaning with a damp cloth easier.
[0069] The contact angle (θ) of water with respect to the surface 3 a of the coating film 3 can be measured based on the sessile drop method (θ / 2 approximation method) of JIS R 3257: 1999. For example, in this embodiment, the coating film 3 is placed horizontally with the surface 3 a facing upward, and 3 μL of pure water is dropped onto it, and then the contact angle can be measured using a contact angle meter (DropMaster DMe-200, manufactured by Kyowa Interface Science Co., Ltd.).
[0070] In this embodiment, the pencil hardness measured from the coating film 3 side of the top plate 1 is preferably 7H or higher, more preferably 8H or higher, and even more preferably 9H or higher. The upper limit of the pencil hardness measured from the coating film 3 side of the top plate 1 is not particularly limited, but may be 13H or lower. In this case, scratches on the coating film 3 due to friction with cooking utensils such as pots and pans are less likely to occur, and the coating film 3 is less likely to peel off from the cooking surface 1a. In particular, when the top plate 1 is used as a top plate for an induction cooker, higher scratch resistance is required because the cooking utensils rub directly against the top plate. The use of the top plate 1 is not particularly limited, but if the top plate 1 has high scratch resistance, it can be suitably used as a top plate for an induction cooker.
[0071] The pencil hardness measured from the coating film 3 side of the top plate 1 can be measured in accordance with JIS K5600-5-4:1999.
[0072] In this embodiment, when a sample for evaluating burnt-on properties of the top plate 1 is prepared, the area ratio of burnt portions (burnt area ratio) on the surface 3a (cooking surface 1a) of the coating film 3 is preferably 70% or less, more preferably 50% or less, even more preferably 10% or less, and particularly preferably 5% or less. When the burnt area ratio is equal to or less than the above upper limit, burnt-on material 10 adhering to the cooking surface 1a can be more easily removed. The lower limit of the burnt area ratio is not particularly limited, but can be, for example, 0.1%.
[0073] The burnt-on evaluation sample can be prepared, for example, by dropping 1 mL of grilled meat sauce (manufactured by Ebara Foods Industries Co., Ltd., product name "Extremely Delicious Grilled Meat Sauce, Sweet") as the evaluation liquid onto the surface 3a of the coating film 3 and heating at 250°C for 30 minutes. In addition to commercially available grilled meat sauce, other liquids that can be used for evaluation include sugar soy sauce, jam, wheat flour or potato starch dissolved in water, sugar water, mirin, etc. The amount of the evaluation liquid dropped can be, for example, 1 mL or more and 3 mL or less. The heating temperature can be, for example, 100°C or more and 300°C or less.
[0074] 3, the scorching evaluation sample 11 is imaged by a camera 12 from the side opposite to the coating film 3 of the glass substrate 2 (the rear surface 2b side). At this time, it is desirable to image the sample by bright field illumination, for example, while illuminating the rear surface 2b side of the glass substrate 2 with light from an illumination 13. Note that the image can be captured by the camera 12 at an angle θ of 0 to 20 degrees with respect to a direction perpendicular to the rear surface 2b of the glass substrate 2, for example.
[0075] In the obtained image, the burnt area ratio can be calculated from the area ratio of the burnt portion to the entire area where the burnt evaluation sample 11 is provided.
[0076] In this embodiment, when the top plate 1 is subjected to a heat resistance test at a temperature of 350° C. for 24 hours, the change in the contact angle of water on the surface 3 a of the coating film 3 before and after the heat resistance test is preferably less than 3 degrees, more preferably 2.5 degrees or less, even more preferably 2 degrees or less, and even more preferably 1 degree or less. In this case, even when the top plate 1 is used for a long period of time or exposed to harsh conditions, the properties of the surface 3 a of the coating film 3 are unlikely to change, so that burnt-on food 10 adhering to the cooking surface 1 a can be easily removed while maintaining the hardness of the cooking surface 1 a.
[0077] In this embodiment, from the viewpoint of further improving the heat resistance of the top plate 1 and further improving the adhesion of the glass substrate 2 to the coating film 3, it is preferable that the coating film 3 contains substantially no phosphate ester compounds, and it is particularly preferable that it contains substantially no phosphorus. Furthermore, from the viewpoint of further improving the heat resistance of the top plate 1 and further reducing the environmental load, it is preferable that the coating film 3 contains substantially no fluorine. Furthermore, from the viewpoint of further reducing the environmental load, it is preferable that the coating film 3 contains substantially no chlorine.
[0078] In this specification, "the coating film 3 is substantially free of phosphate ester compounds and / or phosphorus" means that the content of phosphate ester compounds and / or phosphorus is less than 1 mass% relative to 100 mass% of the entire coating film 3. Of course, the content of phosphate ester compounds and / or phosphorus in the coating film 3 may be less than 0.1 mass%, or the coating film 3 may contain no phosphate ester compounds and / or phosphorus at all. Furthermore, "the coating film 3 is substantially free of fluorine" means that the content of fluorine is less than 1 mass% relative to 100 mass% of the entire coating film 3. Of course, the content of fluorine in the coating film 3 may be less than 0.1 mass%, or the coating film 3 may contain no fluorine at all. Furthermore, "the coating film 3 is substantially free of chlorine" means that the content of chlorine is less than 1 mass% relative to 100 mass% of the entire coating film 3. Of course, the content of chlorine in the coating film 3 may be less than 0.1 mass%, or the coating film 3 may contain no chlorine at all.
[0079] In the top plate 1, it is preferable that the coating film 3 is substantially free of organopolysiloxane and oxide microparticles other than its raw materials. In this case, the coating liquid can be applied more uniformly during manufacturing, further improving the adhesion and hardness between the glass substrate 2 and the coating film 3. Furthermore, the occurrence of poor appearance due to aggregates of oxide microparticles can be suppressed. Furthermore, since the surface of the coating film 3 can be prevented from becoming excessively uneven, burnt-on food 10 is less likely to bite into the cooking surface 1a, making it even easier to remove the burnt-on food 10.
[0080] The oxide fine particles refer to fine particles having an average primary particle diameter of 1000 nm or less as measured by observation with a transmission electron microscope. The average particle diameter of the oxide fine particles is preferably 1 nm or more, more preferably 5 nm or more, and is preferably 100 nm or less, more preferably 15 nm or less.
[0081] Furthermore, "substantially free of oxide fine particles" means that the content of oxide fine particles is less than 3% by mass relative to 100% by mass of the entire coating film 3.
[0082] When oxide fine particles are contained, the content of the oxide fine particles is preferably 50% by mass or less, and more preferably 10% by mass or less, relative to 100% by mass of the entire coating film 3 .
[0083] The oxide fine particles are not particularly limited, and for example, silica, titania, zirconia, antimony oxide, alumina, indium oxide, and mixtures thereof can be used.
[0084] An example of a method for manufacturing the top plate 1 will now be described.
[0085] (Method for Manufacturing Top Plate 1) In the method for manufacturing the top plate 1 of this embodiment, first, a glass substrate 2 is prepared. As the glass substrate 2, the above-mentioned materials can be used.
[0086] Next, a coating liquid is applied to the surface 2a of the prepared glass substrate 2. The method for applying the coating liquid is not particularly limited, and examples include spray coating, dip coating, spin coating, dispenser coating, roll coating, blade coating, and screen printing. The coating liquid is preferably applied by spray coating. When the coating liquid is applied by spray coating, the arithmetic mean height Sa of the resulting coating film 3 on the surface 3a can be easily controlled by the composition of the coating liquid, the application pressure, or the nozzle shape, and the arithmetic mean height Sa can be increased, making it even easier to remove burnt-on food 10 adhering to the cooking surface 1a.
[0087] As the coating liquid, a liquid containing a compound represented by the following formula (2) or a hydrolysis condensation product obtained by hydrolyzing and condensing at least a portion of the compound (hereinafter, sometimes referred to as a siloxane polymer) can be used.
[0088]
[0089] In formula (2), R1 is an alkyl group having 1 to 6 carbon atoms, a phenyl group, or a vinyl group, and R is an alkoxy group. 1 is preferably an alkyl group having 1 to 6 carbon atoms or a phenyl group, more preferably a methyl group, ethyl group, n-propyl group, isopropyl group, n-butyl group, isobutyl group, sec-butyl group, tert-butyl group, pentyl group, hexyl group, or phenyl group, and even more preferably a methyl group or a phenyl group. In particular, a methyl group or a phenyl group is preferred because of its excellent heat resistance. R is preferably a methoxy group, ethoxy group, propoxyl group, butoxy group, pentoxy group, or hexoxy group, and more preferably a methoxy group or an ethoxy group.
[0090] The size of the siloxane polymer can be increased by proceeding with a hydrolysis and condensation reaction, and the volume average size of the siloxane polymer can be, for example, 0.5 nm to 10 nm.
[0091] The content of the siloxane polymer, in terms of solid content by mass percentage in the liquid, is preferably 0.5% or more, more preferably 0.8% or more, and is preferably 25% or less, more preferably 20% or less, even more preferably 14% or less, even more preferably 12% or less, even more preferably 10% or less, even more preferably 8% or less, even more preferably 6% or less, even more preferably 4% or less, and particularly preferably 3% or less. In this case, the coating film 3 can be more easily formed.
[0092] The coating liquid preferably contains a trifunctional alkoxide and its hydrolysis condensate as the siloxane polymer. The siloxane polymer may contain, in addition to the trifunctional siloxane unit, a tetrafunctional siloxane unit, a difunctional siloxane unit, or a monofunctional siloxane unit. The trifunctional siloxane unit preferably accounts for 60% or more, more preferably 70% or more, even more preferably 80% or more, and particularly preferably 90% or more, of the molar ratio of Si. The more trifunctional siloxane units contained in the siloxane polymer, the higher the durability and anti-sticking performance of the coating film 3 can be achieved.
[0093] Examples of trifunctional alkoxides include methyltrimethoxysilane, methyltriethoxysilane, methyltri(n-propoxy)silane, methyltri(i-propoxy)silane, methyltri(n-butoxy)silane, methyl(n-pentoxy)silane, methyl(n-hexoxy)silane, methyltri(phenoxy)silane, ethyltrimethoxysilane, ethyltriethoxysilane, ethyltri(n-propoxy)silane, ethyltri(i-propoxy)silane, ethyltri(n-butoxy)silane, ethyltri(n-pentoxy)silane, ethyltri(n-hexoxy)silane, and ethyltri(phenoxy)silane. Si)silane, ethyltriphenoxysilane, n-propyltrimethoxysilane, n-propyltriethoxysilane, n-propyltri(n-propoxy)silane, n-propyltri(i-propoxy)silane, i-propyltrimethoxysilane, i-propyltriethoxysilane, i-propyltri(n-propoxy)silane, i-propyltri(i-propoxy)silane, n-butyltrimethoxysilane, n-butyltriethoxysilane, n-butyltri(n-propoxy)silane, n-butyltri(i-propoxy)silane, n-butyltri(n-butyl cyclopentyltrimethoxysilane, n-pentyltriethoxysilane, n-pentyltri(n-propoxy)silane, n-pentyltri(i-propoxy)silane, n-pentyltri(n-butoxy)silane, n-pentyltri(n-pentoxy)silane, cyclopentyltrimethoxysilane, cyclopentyltriethoxysilane, cyclopentyl(n-propoxy)silane, cyclopentyl(i-propoxy)silane, cyclopentyltri(n-butoxy)silane, cyclopentyltri(n-pentoxy)silane, cyclopentyltri (cyclopentoxy)silane, n-hexyltrimethoxysilane, n-hexyltriethoxysilane, n-hexyltri(n-propoxy)silane, n-hexyltri(i-propoxy)silane, n-hexyltri(n-butoxy)silane, n-hexyltri(n-pentoxy)silane, n-hexyltri(n-hexoxy)silane, cyclohexyltrimethoxysilane, cyclohexyltriethoxysilane, cyclohexyltri(n-propoxy)silane, cyclohexyltri(n-butoxy)silane, cyclohexyltri(n-pentoxy)silane,Examples of such silanes include cyclohexyltri(n-hexoxyl)silane, cyclohexyltri(cyclohexoxy)silane, phenyltrimethoxysilane, phenyltriethoxysilane, phenyltri(n-propoxy)silane, phenyltri(n-butoxy)silane, phenyltri(n-pentoxy)silane, phenyltri(n-pentoxy)silane, phenyltri(n-hexoxy)silane, phenyltri(phenoxy)silane, vinyltrimethoxysilane, vinyltriethoxysilane, vinyltri(n-propoxy)silane, vinyltri(i-propoxy)silane, vinyltri(n-butoxy)silane, vinyl(n-pentoxy)silane, vinyl(n-hexoxy)silane, and vinyltri(phenoxy)silane. The trifunctional alkoxide is preferably methyltrimethoxysilane, methyltriethoxysilane, phenyltrimethoxysilane, phenyltriethoxysilane, vinyltrimethoxysilane, or vinyltriethoxysilane, and more preferably methyltriethoxysilane.
[0094] The coating liquid may contain an alumina precursor, a zirconia precursor, a titania precursor, or an yttria precursor. These may be used alone or in combination. When the coating liquid contains an alumina precursor, a zirconia precursor, a titania precursor, or an yttria precursor, the durability of the coating film 3 can be further improved.
[0095] The content of the alumina precursor, zirconia precursor, titania precursor, or yttria precursor (total amount when a plurality of types are included) can be, for example, 0% to 30% in terms of mass percentage of alumina, zirconia, titania, or yttria in the solid content.
[0096] Examples of alumina precursors include aluminum alkoxides, hydrolysis condensates of aluminum alkoxides, water-soluble aluminum salts, aluminum chelates, etc. Examples of water-soluble aluminum salts include aluminum nitrate, aluminum chloride, aluminum sulfate, aluminum acetate, aluminum formoacetate, aluminum acetylacetate, etc.
[0097] Examples of the zirconia precursor include zirconium alkoxides, hydrolysis condensates of zirconium alkoxides, etc. Examples of the titania precursor include titanium alkoxides, hydrolysis condensates of titanium alkoxides, etc.
[0098] The coating liquid contains a solvent. The solvent is not particularly limited, and examples thereof include water, alcohols, ketones, ethers, cellosolves, esters, glycol ethers, etc. One of these solvents may be used alone, or two or more of them may be used in combination.
[0099] Water can be used in the hydrolysis reaction of trifunctional alkoxides, etc. However, if the water content is too high, the surface tension is high, which makes it more likely that cracks will occur in the resulting coating film 3. Therefore, the water content can be set to, for example, a molar ratio of 0.5 to 10 with respect to Si atoms.
[0100] Furthermore, from the viewpoint of making the coating liquid easier to dry, the coating liquid preferably contains a solvent having a boiling point of less than 90° C. Examples of solvents having a boiling point of less than 90° C. include methanol, ethanol, isopropyl alcohol, tetrahydrofuran, and hexane. The content of the solvents having a boiling point of less than 90° C. (the total amount when multiple types are included) can be, for example, 10% or more and 90% or less by mass percentage of the entire coating liquid.
[0101] The higher the content of isopropyl alcohol in the coating liquid, the larger the arithmetic mean height Sa of the resulting coating film 3. The content of isopropyl alcohol, in terms of mass percentage of the entire coating liquid, is preferably 20% or more, more preferably 30% or more, and is preferably 90% or less, more preferably 80% or less.
[0102] It is preferable that the coating liquid does not substantially contain oxide microparticles other than the raw materials for the siloxane polymer. In this case, the coating liquid can be more easily prepared, and a uniform coating film can be more easily formed. As a result, the hardness of the cooking surface 1a can be further increased. Furthermore, when a coating film 3 is formed on a glass substrate 2 by spray coating, the adhesion and hardness between the glass substrate 2 and the coating film 3 can be further improved, and further, poor appearance due to agglomerates of oxide microparticles can be prevented. It is preferable that the oxide microparticles are a component different from the matrix-forming component.
[0103] The oxide fine particles refer to fine particles having an average primary particle diameter of 1000 nm or less as measured by observation with a transmission electron microscope. The average particle diameter of the oxide fine particles is preferably 1 nm or more, more preferably 5 nm or more, and preferably 100 nm or less, more preferably 15 nm or less.
[0104] Furthermore, "substantially free of oxide microparticles" means that the content of oxide microparticles is less than 0.1 mass% relative to the total amount of the coating liquid (the state before the raw materials of the siloxane polymer are hydrolyzed and condensed).
[0105] When oxide fine particles are contained, the content of the oxide fine particles is preferably 0.5 mass % or less, more preferably 0.2 mass % or less, relative to the total amount of the coating liquid (the state before the raw material of the siloxane polymer is hydrolyzed and condensed).
[0106] The oxide fine particles are not particularly limited, and for example, silica, titania, zirconia, antimony oxide, alumina, indium oxide, and mixtures thereof can be used.
[0107] The solid content (heat residue) of the coating liquid can be, for example, 0.5 to 5% by mass.
[0108] When applying the coating liquid by the spray coating method, the coating liquid is sprayed onto the surface 2a of the glass substrate 2. Nozzles used in the spray coating method include two-fluid nozzles and one-fluid nozzles, but a two-fluid spray gun using a two-fluid nozzle is preferred. In this case, the adhesion between the glass substrate 2 and the coating film 3 can be further improved.
[0109] In the spray coating method, the amount of coating liquid applied per unit area (spray application amount) is preferably 3 g / m 2 More preferably, 5 g / m 2 More preferably, 10 g / m 2 or more, and preferably 150 g / m 2 or less, more preferably 100 g / m 2 More preferably 50 g / m or less 2 The following is the results. Although it depends on the solid content concentration of the coating liquid, when the spray application amount is large, the arithmetic mean height Sa of the surface 3a of the resulting coating film 3 tends to be large. Also, the film thickness of the resulting coating film 3 tends to be large. On the other hand, when the spray application amount is small, the arithmetic mean height Sa of the surface of the resulting coating film 3 tends to be small. Also, the film thickness of the resulting coating film 3 tends to be small.
[0110] The air flow rate in the spray coating method can be, for example, 10 L / min to 200 L / min. The air pressure can be, for example, 0.05 MPa to 0.5 MPa. The gun distance can be, for example, 60 mm or more and 300 mm or less. The gun distance refers to the distance from the gun to the surface 2a of the glass substrate 2 on which the film is to be formed.
[0111] The application temperature of the coating liquid can be, for example, 10° C. or higher and 30° C. or lower. The surface temperature of the surface 2 a of the glass substrate 2 when applying the coating liquid can be, for example, 10° C. or higher and 80° C. or lower. The humidity when applying the coating liquid can be, for example, 20% or higher and 60% or lower.
[0112] The drying temperature of the coating liquid is not particularly limited, but can be, for example, 100° C. or higher and 150° C. or lower. The drying time can be, for example, 5 minutes or higher and 120 minutes or lower.
[0113] Next, the glass substrate with the coating liquid applied thereto is baked at a temperature of 200° C. or higher, thereby forming a coating film 3 on the surface 2 a of the glass substrate 2 and obtaining the top plate 1 .
[0114] The firing temperature of the film-coated glass substrate is preferably 200° C. or higher, more preferably 250° C. or higher, even more preferably 300° C. or higher, and preferably 500° C. or lower, more preferably 400° C. or lower, and even more preferably 380° C. or lower. A higher firing temperature is preferable to make the resulting coating film 3 dense and obtain high hardness. When the firing temperature of the film-coated glass substrate is equal to or higher than the above lower limit, the hardness of the resulting coating film 3 can be further increased.
[0115] On the other hand, the upper limit of the baking temperature of the film-coated glass substrate is R 1 It is preferable that the temperature is equal to or lower than the temperature at which the
[0116] The baking time for the film-coated glass substrate is not particularly limited, but is preferably 5 minutes or more, more preferably 20 minutes or more, and is preferably 120 minutes or less, more preferably 60 minutes or less.
[0117] The film-coated glass substrate can be fired using, for example, a hot air heating device, a contact heating device, or a far-infrared heating device.
[0118] In this way, a coating film 3 containing an organopolysiloxane having a trifunctional siloxane unit represented by the above formula (1) can be formed on the surface 2a of the glass substrate 2. The obtained coating film 3 has a three-dimensional crosslinked structure containing siloxane bonds.
[0119] The coating film 3 may contain other components to the extent that the effects of the present invention are not impaired. Examples of other components include color pigments such as copper phthalocyanine. The content of the other components may be, for example, 10 mass % or less with respect to the entire coating film 3. However, the coating film 3 may not substantially contain other components.
[0120] [Second embodiment] Fig. 4 is a schematic cross-sectional view showing a top plate for a cooking appliance according to a second embodiment of the present invention. As shown in Fig. 4, a top plate for a cooking appliance 21 has a light-shielding layer 22 and a heat-resistant resin layer 23 provided on the rear surface 2b of a glass substrate 2.
[0121] The light-shielding layer 22 may be, for example, a layer containing glass and a color pigment, or a layer containing a heat-resistant resin and a color pigment. Examples of the heat-resistant resin layer include a layer containing a heat-resistant resin and a color pigment, or a layer containing a heat-resistant resin, a color pigment, and an extender pigment. Examples of the heat-resistant resin include a silicone resin. Other aspects are the same as those of the first embodiment.
[0122] The top plate 21 of the second embodiment also has the above-mentioned coating film 3, so when food spills or the like and burns on the cooking surface 21a, the burnt food is easy to remove, and the hardness of the cooking surface 21a side is excellent.
[0123] As in the second embodiment, a light-shielding layer 22 and a heat-resistant resin layer 23 may be provided on the rear surface 2b of the glass substrate 2. Both the light-shielding layer 22 and the heat-resistant resin layer 23 may be provided, or only one of them may be provided. Furthermore, the light-shielding layer 22 and the heat-resistant resin layer 23 may each be provided as a single layer or as a plurality of layers. Alternatively, layers other than the light-shielding layer 22 and the heat-resistant resin layer 23 may be provided on the rear surface 2b of the glass substrate 2.
[0124] As long as the effects of the present invention are not impaired, a layer such as a decorative layer or a hard coat layer may be provided on a portion of the surface 3 a of the coating film 3. In a plan view, the area where these layers are provided can be, for example, 0% or more and 80% or less of the entire area of the coating film 3. It is preferable that the decorative layer, the hard coat layer, or the like be provided between the glass substrate 2 and the coating film 3.
[0125] [Third embodiment] Fig. 6 is a schematic cross-sectional view showing a top plate for a cooking appliance according to a third embodiment of the present invention. As shown in Fig. 6, a top plate for a cooking appliance 31 has a printed layer 32 having a pattern provided on the surface 2a of a glass substrate 2. In addition, a coating film 3 is provided on the surface 2a of the glass substrate 2 so as to cover the printed layer 32.
[0126] Examples of the pattern include dots, grids, lines, and rings.
[0127] When the printed layer 32 is dot-shaped and each dot has a substantially circular shape, the diameter of the dot may be, for example, 0.1 mm to 3 mm. When the printed layer 32 is lattice-shaped, line-shaped, or ring-shaped, the width of each line may be, for example, 0.1 mm to 3 mm.
[0128] In addition, in a plan view, the ratio of the area of the entire region where the printed layer 32 is provided to the area of the entire surface 2 a of the glass substrate 2 can be, for example, 0.1% or more and 20% or less. In addition, the thickness of the printed layer 32 can be, for example, 0.1 μm or more and 10 μm or less.
[0129] The print layer 32 may be made of glass or may be made of resin. The print layer 32 may contain glass and an inorganic pigment, or may contain a resin and an inorganic pigment. As the inorganic pigment, a color pigment or an extender pigment may be used. As the inorganic pigment, both a color pigment and an extender pigment may be used.
[0130] The same glass substrate 2 and coating film 3 as those in the first embodiment can be used. In this embodiment, the film thickness and surface roughness of the coating film 3 are measured on the glass substrate 2 in a portion where the printing layer 32 is not provided.
[0131] The top plate 31 of the third embodiment also includes the coating film 3 described above. Therefore, when food is burned onto the cooking surface 31a due to spillage or the like, the burnt-on food is easily removed, and the hardness of the cooking surface 31a side is excellent. Incidentally, by providing the coating film 3 also on the patterned printing layer 32 as in this embodiment, the burnt-on food can be easily removed even when it is burnt onto the printing layer 32. However, in the present invention, the coating film 3 does not necessarily have to be provided on the printing layer 32. In this case, it is sufficient that the coating film 3 is provided on the surface 2a of the glass substrate 2 in the areas where the printing layer 32 is not provided.
[0132] Fourth Embodiment (Method for Evaluating Burn-In) FIG. 7 is a schematic cross-sectional view for explaining a plate-like member as an example used in a method for evaluating burn-in according to a fourth embodiment of the present invention.
[0133] The method for evaluating burnt-on food of this embodiment is a method for evaluating the ease of removing burnt-on food from a plate-like member 41 shown in Fig. 7. In this embodiment, the plate-like member 41 is a top plate for a cooking appliance.
[0134] The plate-shaped member 41 has a first main surface 41a and a second main surface 41b facing each other. In this embodiment, the first main surface 41a is a cooking surface on which cooking utensils such as pots and frying pans are placed in the top plate of the cooker. The second main surface 41b is a main surface facing a light source and a heating device inside the cooker. Therefore, the first main surface 41a and the second main surface 41b are opposite each other.
[0135] When plate-shaped member 41 is a top plate for a cooker as in this embodiment, food may be spilled on the cooking surface during heating, for example, when food boils over inside the cookware. According to the method for evaluating scorching in this embodiment, when scorching occurs on first main surface 41 a, which is the cooking surface, the ease of removal of the scorched material adhering to first main surface 41 a can be evaluated.
[0136] Specifically, the scorching evaluation method of this embodiment includes a preparation process for preparing a scorching evaluation sample on the first main surface 41a of the plate-shaped member 41, an imaging process for imaging the scorching evaluation sample from the second main surface 41b side of the plate-shaped member 41, and a measurement process for measuring the area of at least one of the scorched portion and the non-scorched portion in the scorching evaluation sample from the image captured in the imaging process.
[0137] (Fabrication Process) FIGS. 8A to 8C are schematic cross-sectional views illustrating fabrication processes in a method for evaluating scorching according to a fourth embodiment of the present invention.
[0138] In the preparation process, first, a plate-shaped member 41 shown in FIG. 8( a) is prepared. At this time, to facilitate imaging in the subsequent imaging process, the second main surface 41b of the plate-shaped member 41 may be smoothed by polishing or the like, or a coating film, if any, may be removed from the second main surface 41b of the plate-shaped member 41, as long as it does not affect the ease of removing burnt material from the first main surface 41a of the plate-shaped member 41. Next, as shown in FIG. 8( b), an evaluation liquid 42 is dripped onto the first main surface 41a of the plate-shaped member 41. The evaluation liquid 42 is not particularly limited, and examples thereof include commercially available yakiniku sauce, jam, sugar, soy sauce, sugar-soy sauce, mirin, milk, and the like. The amount of the evaluation liquid 42 dripped can be, for example, 1 mL or more and 3 mL or less. It is preferable to thoroughly stir the evaluation liquid 42 immediately before dripping.
[0139] Next, the plate-shaped member 41 onto which the evaluation liquid 42 has been dropped is heated. As a result, a scorching evaluation sample 51 is produced on the first main surface 41a of the plate-shaped member 41, as shown in Fig. 8(c) . When heating the plate-shaped member 41, the entire plate-shaped member 41 may be heated, or the area onto which the evaluation liquid 42 has been dropped may be heated partially. The heating means is not particularly limited, and may be a hot air type, infrared type, electromagnetic wave type, gas type, or the like, and for example, a heating furnace, heater, burner, or the like may be used.
[0140] The heating temperature of the plate-shaped member 41 is not particularly limited, but can be, for example, 100° C. to 300° C. The heating time of the plate-shaped member 41 is not particularly limited, but can be, for example, 1 minute to 60 minutes.
[0141] (Imaging Step) FIG. 9 is a schematic cross-sectional view for explaining the imaging step in the method for evaluating scorching according to the fourth embodiment of the present invention.
[0142] As shown in FIG. 9 , in the imaging process, the scorching evaluation sample 51 is imaged by a camera 52 from the second main surface 41b of the plate-like member 41. Furthermore, in the imaging process, bright-field illumination is used to image the second main surface 41b of the plate-like member 41 while illuminating it with light from an illumination device 53. Note that imaging by the camera 52 can be performed, for example, by tilting the camera 52 at an angle θ of 0 to 20 degrees relative to a direction perpendicular to the second main surface 41b of the plate-like member 41. When an area sensor camera is used as the camera 52, it is preferable to use a surface illumination device as the illumination device 53, and to illuminate and image the entire scorched portion at once. When a line sensor camera is used as the camera 52, it is preferable to use a linear illumination device as the illumination device 53, and to image the plate-like member 41 while it is being transported in one direction. Optical elements such as a mirror, a half mirror, a prism, or an optical filter may also be used as appropriate. The method for imaging the burnt-on evaluation sample 51 in the imaging step is not particularly limited as long as it allows the area of at least one of the burnt and non-burnt portions to be measured in the measurement described below. The resolution of the image obtained by imaging is preferably sufficient to calculate the burnt area, and the resolution of the image obtained by imaging is preferably, for example, 100 ppi to 500 ppi.
[0143] (Measurement step) Fig. 10 is a diagram showing an example of a photograph taken in the imaging step in the method for evaluating burnt-on food according to the fourth embodiment of the present invention. Fig. 11 is a diagram for explaining a method for measuring the areas of the burnt and non-burnt portions in the photograph of Fig. 10.
[0144] As shown in an example in Fig. 11 , in the measurement step, a burnt portion 54 and a non-burnt portion 55 are distinguished from the image captured in the imaging step (Fig. 10). In the image shown in Fig. 11 , the burnt portion 54 is displayed in black, and the non-burnt portion 55 is displayed in white. The burnt portion 54 is a portion where the burnt evaluation sample 51 is in close contact with the plate-like member 41, and the non-burnt portion 55 is a portion where the burnt evaluation sample 51 is floating (where the burnt evaluation sample 51 is not in close contact with the plate-like member 41).
[0145] Next, the area of at least one of the identified burnt portion 54 and non-burnt portion 55 is measured from the image shown in Figure 11. Note that the distinction between the burnt portion 54 and the non-burnt portion 55 and the measurement of their areas can be performed using, for example, image analysis software. Also, for convenience of explanation in this specification, the burnt portion 54 and the non-burnt portion 55 are distinguished by black and white, but of course, in actual analysis, the burnt portion 54 and the non-burnt portion 55 may also be distinguished by color.
[0146] In this embodiment, the ease of removal of burnt-on material can be evaluated using the area of at least one of the burnt portion 54 and the non-burnt portion 55. For example, when the area of the burnt portion 54 is used to evaluate the ease of removal of burnt-on material, it can be evaluated that the smaller the area of the burnt portion 54, the easier it is to remove the burnt-on material from the plate-shaped member 41. Furthermore, when the area of the non-burnt portion 55 is used to evaluate the ease of removal of burnt-on material, it can be evaluated that the larger the area of the non-burnt portion 55, the easier it is to remove the burnt-on material from the plate-shaped member 41.
[0147] 11 , the area of region 56 where burnt-on evaluation sample 51 is provided may be measured, and the ease of removing the burnt-on material may be evaluated using the burnt-on area ratio, which is the ratio of the area of burnt portion 54 to the area of region 56. In this case, it can be evaluated that the smaller the burnt-on area ratio, the easier it is to remove the burnt-on material from plate-like member 41.
[0148] Alternatively, the area of the region 56 where the burnt-on evaluation sample 51 is provided may be measured, and the ease of removing the burnt-on material may be evaluated using the non-burnt area ratio, which is the ratio of the area of the non-burnt portion 55 to the area of the region 56. In this case, it can be evaluated that the greater the non-burnt area ratio, the easier it is to remove the burnt-on material from the plate-like member 41.
[0149] The area of region 56 is the area of the entire region where burnt-on evaluation sample 51 is provided. The area of region 56 corresponds to the sum of the area of burnt portion 54 and the area of non-burnt portion 55.
[0150] The area of the entire region where the scorching evaluation sample 51 is provided may be determined by imaging the region where the scorching evaluation sample 51 is provided from the first main surface 41a side of the plate-shaped member 41. Alternatively, the area of the entire region where the scorching evaluation sample 51 is provided may be determined by measuring the drop area of the evaluation liquid 42 after dripping the evaluation liquid 42 and before heating the plate-shaped member 41 in the production process. In this case, the drop area of the evaluation liquid 42 may be determined by imaging the region where the evaluation liquid 42 is provided from the first main surface 41a side of the plate-shaped member 41, or by imaging the region where the evaluation liquid 42 is provided from the second main surface 41b side of the plate-shaped member 41. The scorched area ratio and the non-scorched area ratio may be determined using the area of the entire region where the scorching evaluation sample 51 is provided measured in this manner.
[0151] The method for evaluating burnt-on matter of this embodiment has the above-described configuration, and therefore can reliably evaluate the ease of removal of burnt-on matter on the plate-shaped member 41 with little variation depending on the evaluator.
[0152] Conventionally, the method of scraping off burnt material from a plate-like member and observing how the burnt material is removed has had the problem that it is difficult to objectively evaluate the ease of removing the burnt material. Also, even if the burnt material is scraped off under consistent conditions, there is a problem that the degree of removal varies depending on the evaluator.
[0153] In contrast, the burnt-on evaluation method of the present embodiment evaluates the ease of removing the burnt-on material using the area of at least one of the burnt portion 54 and the non-burnt portion 55, so that the ease of removing the burnt-on material can be evaluated objectively, and the evaluation can be made reliably with little variation depending on the evaluator.
[0154] In the above embodiment, the evaluation process includes an imaging process and a measurement process. However, in the present invention, the evaluation method is not particularly limited as long as the ease of removal of burnt-on material can be evaluated in the evaluation process. For example, the burnt portion 54 and the non-burnt portion 55 may be visually observed to evaluate the ease of removal of burnt material. The burnt portion 54 and the non-burnt portion 55 can be distinguished by visually observing the side of the plate-like member 41 where the burnt material is present and the opposite side. Specifically, the portion where the burnt-on evaluation sample 51 is in close contact with the plate-like member 41 is designated as the burnt portion 54, and the portion where the burnt-on evaluation sample 51 is floating is designated as the non-burnt portion 55.
[0155] In this way, when the ease of removing burnt material is evaluated by visually observing the burnt portion 54, it can be evaluated that the smaller the area of the burnt portion 54, the easier it is to remove the burnt material from the plate-shaped member 41. Furthermore, when the ease of removing burnt material is evaluated by visually observing the non-burnt portion 55, it can be evaluated that the larger the area of the non-burnt portion 55, the easier it is to remove the burnt material from the plate-shaped member 41. Furthermore, it is also possible to evaluate the ease of removing burnt material by visually confirming the burnt portion 54 and the non-burnt portion 55. In this case, it can be evaluated that the smaller the ratio of the area of the burnt portion 54 to the total area of the burnt portion 54 and the non-burnt portion 55, the easier it is to remove the burnt material from the plate-shaped member 41. Furthermore, it can be evaluated that the larger the ratio of the area of the non-burnt portion 55 to the total area of the burnt portion 54 and the non-burnt portion 55, the easier it is to remove the burnt material from the plate-shaped member 41.
[0156] The method for evaluating scorching according to the present embodiment can be used, for example, to distinguish between good and bad products of the plate-shaped member 41. For example, in the inspection process of the plate-shaped member 41, the scorched area ratio calculated by the above-described method may be used to distinguish between good and bad products.
[0157] In this embodiment, a top plate for a cooking appliance is used as the plate-shaped member 41, but the plate-shaped member 41 may also be, for example, a worktop such as a kitchen top, a small item, a turntable for a microwave oven, or a window for a stove or fireplace, and its use is not particularly limited.
[0158] The plate-shaped member 41 desirably transmits at least a portion of light in the wavelength range of 400 nm to 700 nm. The plate-shaped member 41 may be transparent in the visible range or may be colorless and transparent. In this specification, "transparent in the visible range" refers to a light transmittance of 70% or more in the visible wavelength range of 400 nm to 700 nm. However, the plate-shaped member 41 may be colored or have low transparency as long as the type of camera 52, the type of lighting 53, and the like allow the scorching evaluation sample 51 to be imaged. Furthermore, for example, the plate-shaped member 41 may have an average transmittance of 30% or more in the wavelength range of 700 nm to 3000 nm. The scorching evaluation sample 51 can be imaged by changing the type of camera 52 and the type of lighting 53 according to the target wavelength.
[0159] The shape of the plate-like member 41 is not particularly limited and can be determined appropriately depending on the application. The shape of the plate-like member 41 can be, for example, a rectangular plate, a circular plate, an elliptical plate, a polygonal plate, etc. The thickness of the plate-like member 41 is not particularly limited and can be, for example, 2 mm or more and 6 mm or less.
[0160] [Cooking Appliance Top Plate] The cooking appliance top plate according to the fourth embodiment of the present invention has a burnt area ratio of 70% or less as determined by the above-described burnt-on evaluation method. Therefore, when food spills or the like causes burnt food to burn on the cooking surface, the burning-on food can be easily removed from the cooking appliance top plate according to the fourth embodiment of the present invention.
[0161] In the case of a top plate for a cooker, the burnt area ratio determined by the above-mentioned burnt-on evaluation method is preferably 65% or less, more preferably 50% or less, even more preferably 40% or less, even more preferably 30% or less, even more preferably 20% or less, even more preferably 10% or less, even more preferably 8% or less, and particularly preferably 5% or less. When the burnt area ratio is equal to or less than the upper limit, burnt-on material adhering to the cooking surface can be more easily removed. The lower limit of the burnt area ratio is not particularly limited, but can be, for example, 0.1%.
[0162] The top plate for a cooker may have any of the configurations of the top plates for a cooker described in the first to third embodiments.
[0163] The top plate of this embodiment has the above-described configuration, which allows the burnt area ratio determined by the above-described burnt-on evaluation method to be reduced. In particular, by providing the surface 2a with a coating film 3 containing an organopolysiloxane having a trifunctional siloxane unit represented by the above formula (1), the burnt area ratio determined by the above-described burnt-on evaluation method can be reduced. Therefore, when burnt food is spilled on the cooking surface 1a, the burnt-on food can be easily removed.
[0164] [Top plate for cooking appliance and manufacturing method thereof] The present invention will be described in more detail below based on specific examples. The present invention is not limited to the following examples, and can be implemented with appropriate modifications within the scope of the present invention.
[0165] Preparation of glass substrate A: As the glass substrate A, a transparent crystallized glass plate (manufactured by Nippon Electric Glass Co., Ltd., "N-0", average linear thermal expansion coefficient at 30°C to 380°C: 1 × 10 -7 / °C, thickness: 4 mm, arithmetic mean height Sa: 0.30 nm) was prepared.
[0166] Preparation of glass substrate B: As the glass substrate B, an aluminoborosilicate glass (manufactured by Nippon Electric Glass Co., Ltd., "OA-11", average linear thermal expansion coefficient at 30°C to 380°C: 37 × 10-7 / °C, thickness: 0.5 mm, arithmetic mean height Sa: 0.26 nm) was prepared.
[0167] Preparation of coating liquid A: 1 part by mass of methyltriethoxysilane was mixed with 0.51 parts by mass of water, 36.1 parts by mass of isopropyl alcohol, and nitric acid, followed by stirring, to obtain coating liquid A. At this time, the hydrolysis and condensation reaction of methyltriethoxysilane was allowed to proceed, causing the size of the hydrolysis condensate to grow, so that the volume average size of the hydrolysis condensate measured by dynamic light scattering measurement was 1.0 nm. The nitric acid was adjusted to pH = 4 and mixed. The solid content (heating residue) concentration of the obtained coating liquid A was 1.0 mass%.
[0168] Preparation of coating liquid B: 1 part by mass of methyltriethoxysilane was mixed with 0.51 parts by mass of water, 36.1 parts by mass of denatured ethanol (containing 82.2% by mass of ethanol as the main component, and also containing methanol, isopropyl alcohol, etc.), and nitric acid, and stirred to obtain coating liquid B. At this time, the hydrolysis and condensation reaction of methyltriethoxysilane was allowed to proceed, causing the size of the hydrolysis condensate to grow, so that the volume average size of the hydrolysis condensate measured by dynamic light scattering measurement was 1.0 nm. Note that the nitric acid was adjusted to pH = 4 and mixed. The solid content (heating residue) concentration of the obtained coating liquid B was 1.0 mass%.
[0169] Preparation of Coating Liquid C: 1 part by mass of methyltrimethoxysilane was mixed with 0.66 parts by mass of water, 30.9 parts by mass of isopropyl alcohol, 16.3 parts by mass of 1-methoxy-2-propanol, and nitric acid, followed by stirring, to obtain Coating Liquid C. During this process, the hydrolysis and condensation reactions of methyltrimethoxysilane were allowed to proceed, causing the size of the hydrolysis condensate to grow until the volume average size of the hydrolysis condensate measured by dynamic light scattering measurement was 0.7 nm. The nitric acid was mixed after adjusting the pH to 4. The solids (heating residue) concentration of the obtained Coating Liquid C was 1.0% by mass.
[0170] Preparation of coating liquid D: 0.73 parts by mass of methyltrimethoxysilane and 0.27 parts by mass of phenyltrimethoxysilane were mixed with 2.42 parts by mass of water, 44.2 parts by mass of isopropyl alcohol, and nitric acid and stirred to obtain coating liquid D. At this time, the hydrolysis and condensation reaction of methyltrimethoxysilane and phenyltrimethoxysilane was allowed to proceed, and the size of the hydrolysis condensate was grown, so that the volume average size of the hydrolysis condensate measured by dynamic light scattering measurement was 1.0 nm. Note that the nitric acid was adjusted to pH = 4 and mixed. The solid content (heating residue) concentration of the obtained coating liquid D was 1.1% by mass.
[0171] Preparation of coating liquid E: 1 part by mass of methyltrimethoxysilane, 0.145 parts by mass of aluminum nitrate nonahydrate, 1.12 parts by mass of water, 50.6 parts by mass of isopropyl alcohol, and nitric acid were mixed and stirred to obtain coating liquid E. At this time, the hydrolysis and condensation reaction of methyltrimethoxysilane was allowed to proceed, causing the size of the hydrolysis condensate to grow, and the emulsified liquid was passed through a filter with a pore size of 0.45 μm to obtain a transparent liquid E. In addition, the volume average size of the hydrolysis condensate measured by dynamic light scattering measurement was set to 3.8 nm. Note that the nitric acid was adjusted to pH = 4 and mixed.
[0172] Preparation of Coating Liquid F: 1 part by mass of methyltrimethoxysilane, 0.145 parts by mass of aluminum nitrate nonahydrate, 1.12 parts by mass of water, 33.0 parts by mass of isopropyl alcohol, 17.6 parts by mass of 1-methoxy-2-propanol, and nitric acid were mixed and stirred to obtain Coating Liquid F. At this time, the hydrolysis and condensation reaction of methyltrimethoxysilane was allowed to proceed, causing the size of the hydrolysis condensate to grow, and the emulsified liquid was passed through a filter with a pore size of 0.45 μm to obtain a transparent liquid F. In addition, the volume average size of the hydrolysis condensate measured by dynamic light scattering measurement was adjusted to 3.8 nm. The nitric acid was adjusted to pH = 4 and mixed.
[0173] Preparation of Coating Solution G: 1 part by mass of tetraethoxysilane, 0.342 parts by mass of n-octyltriethoxysilane, 0.413 parts by mass of water, 39.2 parts by mass of isopropyl alcohol, and nitric acid were mixed and stirred to obtain Coating Solution G. At this time, the hydrolysis and condensation reactions of tetraethoxysilane and n-octyltriethoxysilane were allowed to proceed, causing the size of the hydrolysis condensate to grow, and the volume average size of the hydrolysis condensate measured by dynamic light scattering measurement was 1.8 nm. The nitric acid was mixed after adjusting the pH to 4. The solids (heating residue) concentration of the obtained Coating Solution G was 1.2% by mass.
[0174] Example 1 A film-coated glass substrate was formed by spray-coating the coating liquid A onto the main surface of a glass substrate A. The amount of coating (spray coating amount) during spray coating was 123.3 g / m per unit area. 2 A two-fluid spray gun was used, the gun distance was 65 mm, the air pressure was 0.2 MPa, and the liquid discharge rate was 0.2 kg / hour.
[0175] Next, the obtained film-coated glass substrate was placed in a hot air heating furnace, and the temperature was raised from room temperature to 350°C over 0.5 hours, and then maintained at 350°C for 30 minutes. Thereafter, the temperature was lowered. As a result, a top plate for a cooker was obtained in which a coating film was formed on the main surface of the glass substrate.
[0176] (Examples 2 to 21 and Comparative Examples 1 to 8) Top plates for cookers were obtained in the same manner as in Example 1, except that the types of glass substrate and coating liquid, and the application method and conditions were changed as shown in Table 1 below. In Examples 9 and 14, the film-coated glass substrates were prepared by dip coating instead of spray coating, and the dip pull-up speed was set to 0.5 mm / sec. In Comparative Examples 1 and 2, the glass substrates were used as they were as top plates for cookers.
[0177] [Evaluation] (Film Thickness) For the top plates for cookers obtained in Examples 1 to 21 and Comparative Examples 1 to 8, the spectral reflectance was measured using a microspectrophotometer (manufactured by Olympus Corporation, product number "USPM-RU"), and the film thickness of the coating film was determined assuming the refractive index of the coating film to be 1.4.
[0178] (Arithmetic Mean Height Sa) The top plates for cookers obtained in Examples 1 to 21 and Comparative Examples 1 to 8 were evaluated for arithmetic mean height Sa in accordance with ISO 25178.
[0179] Specifically, a white light interference microscope (manufactured by Ryoka Systems Co., Ltd., "VertScan (Model: R5300GL-A150-AC)"), objective lens: 20x, lens barrel: 1x Body, zoom lens: No Relay, measurement field size: 316.77 μm x 237.72 μm, resolution: 640 pixels x 480 pixels, measurement mode: phase mode, wavelength filter: 520 nm, CCD camera: SONY HR-57 1 / 2 was used, and after measurement, bad pixels were interpolated, primary surface correction was performed, and the arithmetic mean height Sa of the surface of the coating film was measured.
[0180] (Pencil Hardness) The top plates for cookware obtained in Examples 1 to 21 and Comparative Examples 1 to 8 were evaluated for pencil hardness in accordance with JIS K5600-5-4:1999.
[0181] (Contact Angle) The contact angle θ of the cooker top plates obtained in Examples 1 to 21 and Comparative Examples 1 to 8 was evaluated based on the sessile drop method (θ / 2 approximation method) of JIS R 3257: 1999. Specifically, a contact angle meter ("DropMaster DMe-200" manufactured by Kyowa Interface Science Co., Ltd.) was used to drop 3 μL of pure water onto each cooker top plate placed horizontally, and measurement was performed.
[0182] (Appearance) The appearance (degree of cloudiness) of the top plates for cookware obtained in Examples 1 to 21 and Comparative Examples 1 to 8 was evaluated for differences in appearance compared to the corresponding uncoated glass substrates. Specifically, under an environment with a specified illuminance, the appearance was visually evaluated using the following three evaluation criteria: no noticeable cloudiness at all, no noticeable cloudiness, and slightly noticeable cloudiness.
[0183] <Evaluation criteria> Slightly noticeable cloudiness: When comparing in a 100 lux environment, the difference is visible. Not noticeable cloudiness: When comparing in a 100 lux environment, the difference is barely noticeable. Not noticeable cloudiness at all: When comparing in a 100 lux environment, the difference is barely noticeable, and even when comparing in a 300 lux environment, the difference is barely noticeable.
[0184] (Burnt Area Ratio) Samples for evaluating burnt areas were prepared for the top plates for cookers obtained in Examples 1 to 15, 17 to 21 and Comparative Examples 1 to 8, and the area ratio of burnt areas on the surface of the coating film (burnt area ratio) was determined.
[0185] The sample for evaluating scorching was prepared by dropping 1 mL of yakiniku sauce (manufactured by Ebara Foods Industry Co., Ltd., product name "Goku-Uma Yakiniku Sauce, Sweet") as a liquid for evaluation onto the surface of the coating film, and then heating it at 250°C for 30 minutes.
[0186] The burnt area ratio was determined by photographing the burnt evaluation sample from the opposite side of the glass substrate from the coating film using a camera (Basler, monochrome camera acA2440-35um), and calculating the area ratio of the burnt portion to the entire area where the burnt evaluation sample was provided in the resulting image. The camera images were taken under conditions of a lens focal length of 16 mm, FNO = 2.8, and WD = 350 mm, while illuminating with white LED surface lighting. The camera images were also taken at an angle θ = 4 degrees with respect to the direction perpendicular to the back surface of the glass substrate.
[0187] The results are shown in Tables 1 and 2 below.
[0188]
[0189]
[0190] As is clear from Tables 1 and 2, the cooker top plates of Examples 1 to 15 and 17 to 21, which had a specific coating film formed on a glass substrate with a film thickness of 100 nm or less, had a small burnt area ratio, allowed burnt material to be easily removed, and had excellent hardness on the coating film side. Furthermore, when the cooker top plates of Examples 1 to 21 were subjected to a heat resistance test at 350°C for 24 hours, the change in the water contact angle on the coating film surface before and after the test was less than 1 degree, confirming enhanced heat resistance.
[0191] In Comparative Example 7, the pencil hardness was insufficient, which is believed to be due to the presence of octyl groups (alkyl groups with 8 carbon atoms) in the organopolysiloxane contained in the coating film. Furthermore, in Comparative Example 8, sufficient anti-sticking performance was not obtained, which is believed to be due to the decomposition of the octyl groups during baking at 350°C. In fact, in Comparative Example 8, the contact angle of pure water was small.
[0192] (Example 22 and Comparative Example 9) A glass substrate A was prepared with a dot pattern printed by screen printing. Next, a coating film was formed on the glass substrate A with the printed dot pattern under the same conditions as in Examples 3, 15, 19, and 20. The film thickness, arithmetic mean height, pure water contact angle, and pencil hardness of the coating film were measured in the gaps between the printed dots, and no significant difference was found compared to when the coating was applied to a glass substrate A without dot printing. In all cases, the burnt material on the burnt-on evaluation samples prepared on the surface could be removed simply by pinching it with the fingers.
[0193] [Method for evaluating burn-on defects] Fig. 12(b) is a photograph for confirming the anti-burn effect and ease of removal of burn-on materials in Example 22, in which a coating film was formed on a glass substrate A printed with a dot pattern under the same conditions as in Example 19. Fig. 13(b) is a photograph for confirming the anti-burn effect and ease of removal of burn-on materials in Comparative Example 9, in which the glass substrate A itself (without a coating film) printed with a dot pattern was used. Figs. 12(a) and 13(a) each show photographs of the burn-on materials in the burn-on defect evaluation sample immediately after their formation (photographs before the burn-on material removal process was performed).
[0194] Next, an evaluation of burnt-on portions was carried out for Example 22 and Comparative Example 9. Specifically, the side of the glass substrate A on which the dot pattern was printed opposite to the side on which the burnt-on matter was present was visually observed, and the areas where the burnt-on matter was in close contact with the glass substrate A on which the dot pattern was printed (burnt areas) were confirmed. As a result, the area of the burnt areas in Example 22 was smaller than that in Comparative Example 9.
[0195] Next, the ease of removal of burnt-on material was confirmed. As shown in Figure 12(b), in Example 22, in which a coating film was formed under the same conditions as in Example 19 on glass substrate A printed with a dot pattern, burnt-on material could be removed by pinching it with fingers. On the other hand, as shown in Figure 13(b), in Comparative Example 9, in which glass substrate A printed with a dot pattern was used as is, burnt-on material remained firmly attached to glass substrate A even after being rubbed hard with a stainless steel scale.
[0196] [Method for Evaluating Burn-In (Including Imaging Step)] The method for evaluating burn-in of the present invention will be described in more detail below based on specific experimental examples. The present invention is not limited to the following experimental examples, and can be practiced with appropriate modifications within the scope of the present invention.
[0197] Preparation of glass substrate A: A transparent crystallized glass plate (manufactured by Nippon Electric Glass Co., Ltd., "N-0", average linear thermal expansion coefficient at 30°C to 380°C: 1 × 10 -7 / °C, thickness: 4 mm) was prepared.
[0198] Preparation of glass substrate B: As the glass substrate B, an aluminoborosilicate glass (manufactured by Nippon Electric Glass Co., Ltd., "OA-11", average linear thermal expansion coefficient at 30°C to 380°C: 37 × 10 -7 / °C, thickness: 0.5 mm) was prepared.
[0199] Preparation of coating liquid A: 1 part by mass of methyltriethoxysilane was mixed with 0.51 parts by mass of water, 36.1 parts by mass of isopropyl alcohol, and nitric acid, followed by stirring, to obtain coating liquid A. At this time, the hydrolysis and condensation reaction of methyltriethoxysilane was allowed to proceed, causing the size of the hydrolysis condensate to grow, so that the volume average size of the hydrolysis condensate measured by dynamic light scattering measurement was 1.0 nm. The nitric acid was adjusted to pH = 4 and mixed. The solid content (heating residue) concentration of the obtained coating liquid A was 1.0 mass%.
[0200] Preparation of coating liquid B: 1 part by mass of methyltriethoxysilane was mixed with 0.51 parts by mass of water, 36.1 parts by mass of denatured ethanol (containing 82.2% by mass of ethanol as the main component, and also containing methanol, isopropyl alcohol, etc.), and nitric acid, and stirred to obtain coating liquid B. At this time, the hydrolysis and condensation reaction of methyltriethoxysilane was allowed to proceed, causing the size of the hydrolysis condensate to grow, so that the volume average size of the hydrolysis condensate measured by dynamic light scattering measurement was 1.0 nm. Note that the nitric acid was adjusted to pH = 4 and mixed. The solid content (heating residue) concentration of the obtained coating liquid B was 1.0 mass%.
[0201] Plate-like member A: The prepared glass substrate A was used as it was as the plate-like member.
[0202] Plate-shaped member B: A film-coated glass substrate was formed by spray-coating the coating liquid B onto the main surface of the glass substrate A. The amount of coating (spray coating amount) during spray coating was 24.6 g / m per unit area. 2 A two-fluid spray gun was used, the gun distance was 65 mm, the air pressure was 0.2 MPa, and the liquid discharge rate was 0.2 kg / hour.
[0203] Next, the obtained film-coated glass substrate was placed in a hot air heating furnace, and the temperature was raised from room temperature to 350°C over 0.5 hours, and then maintained at 350°C for 30 minutes. The temperature was then lowered, and a plate-shaped member B serving as a top plate for a cooker was obtained, in which a coating film was formed on the main surface of the glass substrate.
[0204] Plate-shaped members C to F: Plate-shaped members C to F were obtained as top plates for cookers in the same manner as plate-shaped member B, except that the coating conditions were changed as shown in Table 3 below. For plate-shaped member C, the film-coated glass substrate was prepared by dip coating instead of spray coating, and the dip pull-up speed was set to 0.5 mm / sec.
[0205]
[0206] (Experimental Examples 1 to 6) Plate-shaped members A to F were evaluated for scorching. Specifically, 1 mL of yakiniku sauce (manufactured by Ebara Foods Industry Co., Ltd.) was dropped onto the first main surface of each plate-shaped member as a liquid for evaluation, and the plate-shaped member was heated at 250°C for 30 minutes to prepare a sample for evaluating scorching on the first main surface of each plate-shaped member. In plate-shaped member A, one main surface of the glass substrate was used as the first main surface. In plate-shaped members B to F, the main surface on the side where the coating film was provided was used as the first main surface.
[0207] Next, the burn-on evaluation samples were imaged from the second main surface side of each plate-shaped member using a camera (Basler, monochrome camera acA2440-35um) to obtain 8-bit grayscale images. The camera images were taken using bright-field illumination with a lens focal length of 16 mm, FNO = 2.8, and WD = 350 mm, while being illuminated by white LED surface lighting. The camera images were also taken at an angle θ = 4 degrees with respect to the direction perpendicular to the second main surface of the plate-shaped member.
[0208] Next, the areas of the burnt and non-burnt portions of the captured image of the burnt evaluation sample were measured using image analysis software (manufactured by MVTEC, product number "HALCON18"), and the burnt area ratio was calculated from the ratio of the area of the burnt portion to the total area of the region where the burnt evaluation sample was provided.
[0209] The analysis using the image analysis software was carried out as follows.
[0210] First, the contrast in the image at the time of capture was corrected. Specifically, a primary gray value plane was generated by fitting it to the entire area surrounding the region in the captured image where the burn-in evaluation sample was provided, and a corrected image was created by correcting the gray values of the original image so that the gray value g became g = 128 g / g, where g is the gray value of each pixel in the original image and g is the gray value of the generated gray value plane.
[0211] Next, threshold processing was performed on the corrected image, and a region R1 where the gray value was 100 or less or 160 or more was extracted, and this was defined as the entire region where the evaluation sample was located. At this time, opening and closing processing was performed as appropriate to ensure that the surrounding shape was a smooth region. Furthermore, the analysis range was narrowed to the extracted region R1, and threshold processing was performed again on the corrected image, and a region R2 of the burnt portion where the gray value was 100 or less was extracted. By calculating the ratio of the areas (number of pixels) of region R1 and region R2, the ratio of the area of the burnt portion (region R2) to the area of the entire region where the burnt evaluation sample was located (region R1) was calculated, and this was defined as the burnt area ratio.
[0212] The samples for evaluating burnt deposits prepared in each experiment were also tested for ease of peeling. The test for ease of peeling was performed by poking the sample for evaluating burnt deposits with a pen, and the test was evaluated according to the following criteria. Note that, in the following criteria, the larger the number, the more difficult it is to peel off the burnt deposits.
[0213] <Evaluation criteria> 1: When the burnt lump is lightly touched with a pen, the entire burnt lump peels off. 2: When the burnt lump is lightly pressed with a pen, the entire burnt lump peels off. 3: When the burnt lump is pressed firmly with a pen, the entire burnt lump peels off. 4: When the burnt lump is pressed firmly with a pen, the burnt lump breaks up and peels off in parts. When the remaining part is pressed firmly with the pen repeatedly, the entire burnt lump peels off. 5: When the burnt lump is pressed firmly with a pen, the burnt lump only breaks up in parts. The entire burnt lump cannot be peeled off.
[0214] The results are shown in Table 4 below.
[0215]
[0216] As is clear from Table 4, it was confirmed that the smaller the burnt area ratio obtained by the burnt evaluation test in Experimental Examples 1 to 6, the easier it was to peel off the burnt parts.
[0217] (Experimental Examples 7 and 8) Next, a plate-like member G having a glass substrate A as a base material and a coating film containing an organopolysiloxane, and a plate-like member H having a glass substrate B as a base material and a coating film containing an organopolysiloxane were prepared, and the same scorching evaluation test as in Experimental Examples 1 to 6 was performed six times to determine the scorching area ratio for each. The standard deviation and standard error of the scorching area ratios for the six times were also determined.
[0218] The results are shown in Table 5 below.
[0219]
[0220] As is clear from Table 5, the burnt area ratio measured in the burnt evaluation tests of Experimental Examples 7 and 8 had sufficiently small values of 2 × standard error, which corresponds to the 95% confidence interval. Thus, it was confirmed that the burnt evaluation method of Experimental Examples 7 and 8 can reliably evaluate the ease of removal of burnt material from a plate-shaped member with little variability between evaluators.
[0221] REFERENCE SIGNS LIST 1, 21, 31... Cooking appliance top plate 1a, 21a, 31a... Cooking surface 2... Glass substrate 2a, 3a... Front surface 2b... Back surface 3... Coating film 10... Burnt-on object 11... Burnt-on evaluation sample 12... Camera 13... Lighting 22... Light-shielding layer 23... Heat-resistant resin layer 32... Printed layer 41... Plate-shaped member 41a... First main surface 41b... Second main surface 42... Evaluation liquid 51... Burnt-on evaluation sample 52... Camera 53... Lighting 54... Burnt area 55... Non-burnt area 56... Area
Claims
1. A top plate for a cooker comprising: a glass substrate; and a coating film provided on a main surface of the glass substrate, the coating film containing an organopolysiloxane having a trifunctional siloxane unit represented by the following formula (1), wherein the coating film has a three-dimensional crosslinked structure including siloxane bonds, and the coating film has a thickness of 100 nm or less. (In formula (1), R 1 is an alkyl group having 1 to 6 carbon atoms, a phenyl group, or a vinyl group.
2. The top plate for a cooker according to claim 1, wherein the surface of the coating film has an arithmetic mean height Sa of 0.4 nm or more and 10 nm or less, measured with a measurement field size of 316.77 μm × 237.72 μm and a resolution of 640 pixels × 480 pixels.
3. A top plate for a cooker according to claim 1 or 2, wherein the contact angle of water with the surface of said coating film is 80 degrees or more.
4. The top plate for a cooker according to claim 1 or 2, wherein the glass substrate is made of borosilicate glass or low expansion glass ceramics.
5. The average linear thermal expansion coefficient of the glass substrate at 30°C to 380°C is 40 x 10 -7 3. The top plate for a cooker according to claim 1, wherein the temperature is 0.15 to 1.5°C.
6. A top plate for a cooker according to claim 1 or 2, wherein the coating film contains a hydrolysis condensation product of a trifunctional alkoxide represented by the following formula (2): (In formula (2), R 1 is an alkyl group having 1 to 6 carbon atoms, a phenyl group, or a vinyl group, and R is an alkoxy group.
7. The R of the compound represented by formula (2) 1 The top plate for a cooker according to claim 6, wherein is a methyl group.
8. A top plate for a cooker according to claim 1 or 2, wherein the pencil hardness of the top plate for a cooker measured from the coating film side is 9H or more.
9. A top plate for a cooker as described in claim 1 or 2, wherein a scorching evaluation sample is prepared by dropping an evaluation liquid onto the surface of the coating film and heating it, and when the scorching evaluation sample is imaged from the opposite side of the glass substrate to the coating film, the area ratio of the scorched portion determined from the image obtained is 70% or less.
10. A top plate for a cooker as described in claim 1 or 2, wherein, when a heat resistance test is conducted at a temperature of 350°C for 24 hours, the change in the contact angle of water on the surface of the coating film before and after the heat resistance test is less than 3 degrees.
11. The top plate for a cooker according to claim 1 or 2, wherein the surface of the top plate for a cooker on the side of the coating film is a cooking surface on which a cookware is placed.
12. A top plate for a cooker as described in claim 1 or 2, wherein a printed layer having a pattern is provided on a main surface of the glass substrate, and the coating film is provided on the main surface of the glass substrate so as to cover the printed layer.
13. The top plate for a cooker according to claim 12, wherein the pattern is a dot, a lattice, a line, or a ring pattern.
14. A method for manufacturing a top plate for a cooker, comprising a glass substrate and a coating film provided on a main surface of the glass substrate, the method comprising the steps of: applying, onto the main surface of the glass substrate, a coating liquid containing a compound represented by the following formula (2) or a hydrolysis condensate obtained by hydrolyzing and condensing at least a portion of the compound; and baking the glass substrate with the coating liquid applied thereto at a temperature of 200°C or higher to form a coating film on the main surface of the glass substrate. (In formula (2), R 1 is an alkyl group having 1 to 6 carbon atoms, a phenyl group, or a vinyl group, and R is an alkoxy group.
15. The R of the compound represented by formula (2) 1 The method for producing a top plate for a cooker according to claim 14, wherein is a methyl group.
16. A method for evaluating the ease of removal of burnt-on matter on a plate-shaped member, comprising: a production process for preparing a plate-shaped member having opposing first and second main surfaces, and producing a burnt-on evaluation sample on the first main surface of the plate-shaped member; and an evaluation process for evaluating the ease of removal of burnt-on matter in the burnt-on evaluation sample from the second main surface side of the plate-shaped member.
17. The scorching evaluation method according to claim 16, wherein the evaluation process includes: an imaging process for imaging the scorching evaluation sample from the second main surface side of the plate-shaped member; and a measurement process for measuring the area of at least one of the scorched portion and the non-scorched portion of the scorching evaluation sample from the image captured in the imaging process.
18. A scorching evaluation method as described in claim 16, wherein in the preparation process, an evaluation liquid is dripped onto the first main surface of the plate-like member, and the plate-like member onto which the evaluation liquid has been dripped is heated, thereby preparing a scorching evaluation sample on the first main surface of the plate-like member.
19. The method for evaluating scorching according to claim 17, wherein in the imaging step, the sample for evaluating scorching is imaged from the second main surface side of the plate-like member by bright field illumination.
20. The method for evaluating scorching according to claim 17, wherein in the measuring step, the area of the entire region in which the sample for evaluating scorching is provided is measured from the image captured in the imaging step.
21. A method for evaluating scorching as described in claim 18, wherein in the preparation process, after the evaluation liquid is dripped and before the plate-shaped member is heated, the drip area of the evaluation liquid is measured to measure the entire area of the region in which the scorching evaluation sample is provided.
22. The method for evaluating scorching according to claim 17, wherein in the measuring step, a scorched area ratio is calculated, which is the ratio of the area of the scorched portion to the area of the entire region in which the scorched evaluation sample is provided.
23. The method for evaluating scorching according to claim 22, wherein in the measuring step, the plate-like member is judged to be a good product or a defective product based on the scorched area ratio.
24. A top plate for a cooker, in which the burnt area rate determined by the burnt area evaluation method described in any one of claims 16 to 23 is 70% or less.
Citation Information
Patent Citations
Top plate for cooking tool
JP1997132428A
Top plate for cooker, coating film of the top plate for cooker, and method for manufacturing the top plate for cooker
JP2011196667A
Top plate for heating cooker
JP2021178774A
Stain-proof glass
JP2002326841A
Top plate for cooking utensils
JP2003146700A