Optical laminate, polarizing lens, and eyewear
The optical laminate with a gray polarizing element and hue-adjusting dyes in the adhesive layer addresses the issue of uneven visibility in high-transmittance polarized lenses by ensuring uniform transmittance and hue adjustment, enhancing comfort and visibility while simplifying manufacturing.
Patent Information
- Application Number
- PCT/JP2024/012001
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-28
- Filing Date
- 2024-03-26
- Publication Date
- 2024-10-03
AI Technical Summary
Polarized lenses with higher transmittance than ordinary lenses suffer from uneven visibility due to non-uniform polarization characteristics across the visible light range, leading to unnatural and uncomfortable viewing experiences, especially when reflecting light is blocked, and existing methods complicate manufacturing and increase costs.
An optical laminate with a gray-colored polarizing element and an adhesive layer containing hue-adjusting dyes is used, ensuring a saturation difference of 10 or less, which adjusts the hue and transmittance uniformly across the visible light range, integrated into polarized lenses for eyewear.
The solution provides polarized lenses that maintain natural visibility and comfort while effectively blocking reflected light, reducing the difference in color between transmitted and blocked light, and simplifies manufacturing by eliminating the need for complex dye adjustments in the lens resin.
Smart Images

Figure JP2024012001_03102024_PF_FP_ABST
Abstract
Description
Optical laminate, polarized lens and eyewear
[0001] The present invention relates to an optical laminate including a polarizing element, and to a polarized lens and eyewear (sunglasses, goggles, etc.) using the same.
[0002] BACKGROUND ART Eyewear such as sunglasses and goggles use tinted lenses (also called colored lenses) to add fashion and anti-glare properties, and colored polarized lenses with polarization properties are also used to provide even higher anti-glare properties.
[0003] Polarized lenses are lenses that utilize the polarization phenomenon to transmit only polarized light compared to non-polarized light. Eyewear using polarized lenses, particularly when used outdoors, not only attenuates direct light from external sources, but also blocks the transmission of light reflected by diffuse reflection (horizontally polarized, also known as S-polarized light) and transmits only vertically polarized light (also known as P-polarized light), thereby reducing glare from light sources and providing clear vision even in reflected light or backlit conditions. Eyewear with such polarization functionality can be used not only for sports and leisure activities, but also to ensure sufficient visibility and increase safety when driving a car, etc.
[0004] In particular, for fashionable eyewear, which is expected to be worn indoors as well as outdoors, higher transmittance than ordinary lenses is required, and there is a tendency for them to be designed to satisfy "lens category 1" (visible transmittance (τv): 43% < τv ≦ 80%) as specified in the European standard for lens transmittance (EN ISO12312-1:2013 / Al:2015).
[0005] As an example of a colored polarized lens, Patent Document 1 discloses sunglasses that use a colored polarizing element that uses a plurality of azo dyes, which are adsorbed and oriented on a polyvinyl alcohol (PVA) film and adjusted to a brown color.
[0006] Another known method for obtaining colored polarized lenses is to produce colored polarized sunglasses by using a grayish polarizing film and lenses containing a colored resin material in order to suppress changes in the characteristics of the polarizing element, as described in Patent Document 2.
[0007] Furthermore, Patent Document 3 describes eyeglasses with a polarizing plate that are provided with an adhesive layer that compensates for color changes caused by the polarizing section. It is disclosed that such eyeglasses can compensate for color changes caused by the polarizing element because they include a polarizing section that transmits polarized light and an adhesive layer that compensates for color changes.
[0008] JP 2021-71546 A International Publication No. 2014 / 030611 JP 2015-021995 A
[0009] However, the polarizing element disclosed in Patent Document 1 mainly has a wavelength range with λmax in a specific wavelength range of the visible light range, and therefore does not have uniform polarization characteristics throughout the visible light range. Therefore, when wearing eyewear, a difference in visibility occurs between the portion of the scenery that is perceived as reduced light and the portion of the scenery that appears as reflected light is blocked. Particularly in fields that require higher transmittance than general polarized lenses (designed primarily for outdoor use with a transmittance of 10-30%), such as "Lens Category 1" as specified in the European standard for lens transmittance, the difference in visibility between the portion of the scenery that is perceived as reduced light and the portion of the scenery that appears as reflected light is blocked becomes larger than when using a conventional polarizing element with low transmittance designed for outdoor use, potentially resulting in a more unnatural and uncomfortable view.
[0010] Furthermore, the method described in Patent Document 2 uses a gray-colored polarizing element to make the polarization characteristics more uniform across the entire visible light range, but this is cumbersome because it requires adjusting the dyeing of the lens resin. Furthermore, the total thickness of the lens resin is reduced by cutting during lens molding, which changes the color density of the lens. As a result, to ensure quality, it is necessary to adjust the dyeing and manage the processing time for each lens product, which raises concerns about increased manufacturing costs. Furthermore, Patent Document 3 only mentions the transmission characteristics of natural light and does not mention the impact on visibility of fields including polarized light, making it unclear how visible the portions of the scenery are when reflected light is blocked.
[0011] Therefore, the present invention aims to provide an optical laminate that provides a natural, comfortable feeling when worn with eyewear and exhibits excellent visibility in fields where higher transmittance than that of ordinary polarized lenses is required, as well as polarized lenses and eyewear that use the same.
[0012] As a result of extensive research to solve the above-mentioned problems, the inventors discovered that the above-mentioned problems can be solved by using a grayish polarizing element with a high transmittance of incident natural light in an optical laminate for colored eyewear, and by incorporating a hue-adjusting dye capable of adjusting the hue into the adhesive layer in the optical laminate, and thus completed the present invention.
[0013] An optical laminate according to an embodiment of the present invention comprises a support, a polarizing element, and at least one adhesive layer between the support and the polarizing element, wherein the polarizing element contains at least one dye-based dichroic pigment and exhibits a grayish color, and at least one adhesive layer contains one or more hue-adjusting pigments that adjust the hue and transmittance in the visible light range of the optical laminate, and wherein the saturation difference |Δc| represented by the following formula (1) is 10 or less. (In formula (1), a * s and b * s is the L when natural light is incident on the optical laminate * a * b * is the hue value in the color space, and a * kz and b *kz is the L when polarized light is incident in a direction perpendicular to the absorption axis of the optical laminate. * a * b * hue value in the color space (CIE 1976)
[0014] In one embodiment of the present invention, the hue-adjusting dye comprises at least one of the following dyes (A) to (D): (A) a dye that exhibits a reddish color (having λmax in a wavelength range of about 400 to 500 nm), (B) a dye that exhibits a greenish color (having λmax in a wavelength range of about 500 to 600 nm), (C) a dye that exhibits a bluish color (having λmax in a wavelength range of about 600 to 700 nm), or (D) a dye that exhibits a yellowish color (having λmax in a wavelength range of about 380 to 500 nm).
[0015] In one embodiment of the present invention, the adhesive layer contains an amorphous polyester resin.
[0016] In one embodiment of the present invention, in the polarizing element, L * a * b * Hue value a in color space (CIE 1976) * s and b * Each s is in the range of -5 to 5.
[0017] In one embodiment of the present invention, the polarizing element has optical characteristics in which the luminosity-corrected transmittance (Ys) for incident natural light is 43% or more and 80% or less.
[0018] A polarized lens according to an embodiment of the present invention comprises a lens substrate and the above-described optical laminate.
[0019] Eyewear according to an embodiment of the present invention includes the above-described polarized lens.
[0020] According to the present invention, it is possible to provide an optical laminate that provides a natural, comfortable feeling when worn with eyewear and exhibits excellent visibility in fields where higher transmittance than that of ordinary polarized lenses is required, as well as polarized lenses and eyewear that use the same.
[0021] FIG. 1 is a schematic diagram showing an example of an embodiment of an optical laminate according to the present invention. FIG. 2 is a schematic diagram showing an example of another embodiment of an optical laminate according to the present invention. FIG. 3 is a schematic diagram showing an example of shaping (bending) processing of an optical laminate according to the present invention. FIG. 4 is a diagram comparing the waveforms of the natural light incident transmittance of the optical laminates of Example 1 and Comparative Example 1. FIG. 5 is a diagram comparing the waveforms of the natural light incident transmittance of the optical laminates of Example 2 and Comparative Example 2. FIG. 6 is a diagram comparing the waveforms of the natural light incident transmittance of the optical laminates of Example 3 and Comparative Example 3. FIG. 7 is a diagram comparing the waveforms of the natural light incident transmittance of the optical laminates of Example 4 and Comparative Example 4. FIG. 8 is a diagram comparing the waveforms of the natural light incident transmittance of the optical laminates of Example 5 and Comparative Example 5. FIG. 9 is a diagram comparing the waveforms of the natural light incident transmittance of the optical laminates of Example 6 and Comparative Example 6. FIG. 10 is a diagram comparing the waveforms of the polarized incident orthogonal transmittance of the optical laminates of Example 1 and Comparative Example 1. FIG. 11 is a diagram comparing the waveforms of the polarized incident orthogonal transmittance of the optical laminates of Example 2 and Comparative Example 2. FIG. 12 is a diagram comparing the waveforms of the polarized incident orthogonal transmittance of the optical laminates of Example 3 and Comparative Example 3. 1 is a diagram comparing the waveforms of polarized incident orthogonal transmittance of the optical laminates of Example 4 and Comparative Example 4. FIG. 2 is a diagram comparing the waveforms of polarized incident orthogonal transmittance of the optical laminates of Example 5 and Comparative Example 5. FIG. 3 is a diagram comparing the waveforms of polarized incident orthogonal transmittance of the optical laminates of Example 6 and Comparative Example 6.
[0022] Hereinafter, embodiments according to the present invention will be described in detail. Note that the following embodiments are examples of some typical embodiments of the present invention, and various modifications can be made within the scope of the present invention. Furthermore, the term "adjustment" means that the hue value, transmittance value, and waveform structure of the polarizing element used in the optical laminate are used as a reference, and these values are adjusted using a separate dye so that the desired hue value, transmittance value, and waveform structure are obtained when the optical laminate is produced. Furthermore, the term "near" means that there is a tolerance of 1 to 10 nm before and after each wavelength band.
[0023] The optical laminate of the present invention comprises a support, a polarizing element, and at least one adhesive layer between the support and the polarizing element, the polarizing element containing at least one dye-based dichroic dye and exhibiting a grayish color, and at least one adhesive layer containing one or more hue-adjusting dyes that adjust the hue and visible light transmittance of the optical laminate, and the optical laminate has a saturation difference |Δc| expressed by the following formula (1) of 10 or less:
[0024] (In formula (1), a * s and b * s is the L when natural light is incident on the optical laminate * a * b * is the hue value in the color space, and a * kz and b * kz is the L when polarized light is incident perpendicular to the absorption axis of the optical laminate. * a * b * hue value in the color space (CIE 1976)
[0025] By using an optical laminate having such a configuration in the polarized lenses of eyewear, it is possible to reduce the difference in color between the part of the scenery that is perceived as being dimmed and the part of the scenery that is perceived as having reflected light blocked when the eyewear is worn, thereby realizing eyewear that looks natural and comfortable when worn and has excellent visibility. In particular, the optical laminate of the present invention can be applied to colored eyewear products for lens category 1 specified in European standards, which can provide a more natural wearing experience without a significant change in the color of the scenery that is transmitted (the "natural light incident transmission hue" described below) and the color of the blocked reflected light (the "polarized light incident orthogonal transmission hue" described below).
[0026] Furthermore, when the optical laminate of the present invention is applied to a polarized lens, the optical design is performed solely within the optical laminate, thereby providing a polarized lens that is less susceptible to changes in optical properties that occur during lens polishing and other processes, compared to when the dye is dyed or incorporated into the resin that forms the lens substrate. Furthermore, since the dye is contained only in the adhesive layer, a wide range of support materials can be used without being limited by the type of support. Since these dyes are poorly soluble in water, they are not susceptible to bleaching or discoloration even when exposed to water or high humidity, providing a highly reliable colored polarized lens. Furthermore, the hue of the optical laminate can be designed by combining several gray-based polarizing elements with different transmittances and toning the adhesive layer of the optical laminate. This eliminates the need to manufacture individually toned polarizing elements as in the past, and allows for the simple production of optical laminates with a wide variety of colors.
[0027] <Optical laminate> Fig. 1 shows one embodiment of an optical laminate according to the present invention. As shown in Fig. 1, the optical laminate 100 of the present invention includes two supports 10, a polarizing element 20, and two adhesive layers 30 between each of the supports 10 and the polarizing element 20, which are arranged in the following order from the external light incident side: first support / adhesive layer / polarizing element / adhesive layer / second support. That is, the polarizing element 20 is arranged so as to be interposed between the two supports (first support and second support) 10 via the respective adhesive layers 30.
[0028] 2, an optical laminate 110 optionally further includes a support 10, which is arranged in the following order from the external light incident side: first support / adhesive layer / polarizing element / adhesive layer / second support / adhesive layer / third support. That is, the optical laminate 110 includes three supports 10, a polarizing element 20, and three adhesive layers 30, with the polarizing element 20 interposed between the two supports (first support and second support) 10 via the respective adhesive layers 30. A further support (third support) 10 is provided on the opposite side (viewing side) from the external light incident side via an adhesive layer 30. In either embodiment, the first support is arranged on the external light incident side when the eyewear is worn, and the second support (or third support) is arranged on the side that will be integrally molded with the resin material (lens substrate 40) during the processing of the polarized lens, as described below.
[0029] (Support) The support is an optically transparent resin material used to protect the polarizing element and to impart rigidity and integral molding to the polarized lens. In addition to the first support and the second support, a third support may be provided as the support depending on the design of the optical laminate. The first support, the second support, and even the third support may be made of the same material, or may be made of different materials depending on the design of the optical laminate. Furthermore, each member of the optical laminate can be laminated via an adhesive layer. The film thickness of each support is usually 10 μm or more and 200 μm or less, preferably 40 μm or more and 100 μm or less, and a film or sheet-shaped material can be used as the support.
[0030] The material of the support may be, for example, a material containing a polycarbonate (PC)-based resin, a triacetyl cellulose (TAC)-based resin, a polyamide (PA)-based resin, or the like, and may be appropriately changed depending on the type of injection-molded resin. In this case, to ensure adhesion, it is desirable that the injection-molded resin of the lens substrate and the support of the optical laminate be made of the same material, but this is not limited thereto. In addition, the first support, the second support, and even the third support may be the same support, or may be different types of support.
[0031] At least one support or at least one adhesive layer in the optical laminate may contain an ultraviolet absorber. In this case, it is preferably the first support or an adhesive layer disposed between the first support and the polarizing element, which not only protects the wearer's eyes from ultraviolet light but also suppresses photodegradation of the support, polarizing element, and color-adjusting pigment. However, the arrangement of the component having ultraviolet absorbing function is not limited to the above method and may be disposed at any position in the optical laminate or lens substrate.
[0032] (Polarizing Element) The polarizing element used in the present invention is an absorption-type polarizing element containing at least one dye-based dichroic dye. Examples of polarizing elements include polyvinyl alcohol (PVA)-based polarizing films and coated polarizing elements, with PVA-based polarizing films being more preferred. PVA-based polarizing films can be produced by known stretching methods, such as adsorbing a dye-based dichroic dye onto a polymer film containing PVA or a derivative thereof and then uniaxially stretching the film to approximately 2 to 5 times its original size. The thickness of the polarizing element is typically 5 μm to 30 μm. In particular, from the standpoint of hue design, azo compounds are preferred as dichroic dyes, and from the standpoint of heat resistance, direct dyes having sulfonic acid groups are preferred. A polarizing element made of a PVA-based polarizing film is also referred to as a bare polarizing film.
[0033] The azo compound-based dichroic dyes can be used alone or in combination of two or more depending on the hue design of the polarizing element. Examples of such dichroic dyes include C.I. Direct Yellow 12, C.I. Direct Yellow 28, C.I. Direct Yellow 44, C.I. Direct Yellow 142, C.I. Direct Orange 26, C.I. Direct Orange 39, C.I. Direct Orange 71, C.I. Direct Orange 107, C.I. Direct Red 2, C.I. Direct Red 31, C.I. I. Direct Red 79, C. I. Direct Red 81, C. I. Direct Red 117, C. I. Direct Red 247, C. I. Direct Green 80, C. I. Direct Green 59, C. I. Direct Blue 71, C. I. Direct Blue 78, C. I. Direct Blue 168, C. I. Direct Blue 202, C. I. Direct Violet 9, C. I. Direct Violet 51, C. I. Examples of suitable acrylic acid esters include C.I. Direct Brown 106 and C.I. Direct Brown 223.
[0034] As other dichroic dyes, dyes produced by known methods may be used. Examples of known methods include the method described in JP-A-3-12606 and the method described in JP-A-59-145255. Examples of commercially available dyes include Kayafect Violet P Liquid, Kayafect Yellow Y, Kayafect Orange G, Kayafect Blue KW, and Kayafect Blue Liquid 400, all manufactured by Nippon Kayaku Co., Ltd.
[0035] When designing a mixed color hue, a gray hue can generally be designed by using, as a dye-based polarizing element, at least three types of dyes having λmax in the wavelength bands of approximately 380 to 430 nm, approximately 430 to 580 nm, and approximately 580 to 680 nm, based on the principle of the three primary colors.
[0036] The polarizing element used in the present invention preferably has a uniform transmittance over the visible light range, and exhibits a grayish hue. The grayish hue includes a color intermediate between black and white (generally called gray or achromatic color) as well as a hue with a slight color tint. Specifically, the L obtained from the transmittance of the polarizing element alone is * a * b * Hue value a in color space (CIE 1976) * s and b * Each of the hue values a is preferably in the range of -5 or more and 5 or less (including 0), and more preferably in the range of -3 or more and 3 or less (including 0). * s and b * By having s, color design using a hue-adjusting dye, which will be described later, becomes easier.
[0037] The polarizing element used in the present invention preferably has optical properties such that the luminosity-corrected transmittance (Ys) for incident natural light is 43% or more and 80% or less, and more preferably the luminosity-corrected transmittance (Ys) is 50% or more. Such optical properties are more suitable for satisfying the European Standard Lens Category 1 standard when the optical laminate is applied to eyewear products. Furthermore, when designing a polarizing element with such high transmittance, the use of a dye-based polarizing element is more preferable than an iodine-based polarizing element, taking into account the ease of hue adjustment and heat resistance during lens processing.
[0038] As described above, polarizing elements with high transmittance, specifically polarizing elements with Ys exceeding 50%, have, in principle, a degree of polarization (luminosity-corrected polarization, Py) of less than 90%. Eyewear with polarizing elements with a degree of polarization of less than 90% is classified as "sunglasses with polarization function," but here, lenses and sunglasses with polarization function will be referred to as "polarized lenses" and "polarized sunglasses," regardless of the value of the degree of polarization.
[0039] The reflected light blocking effect of a polarized lens produced using the optical laminate of the present invention depends on the degree of polarization of the polarizing element, but when Py is below 90%, it is not easy to quantitatively demonstrate this effect. Therefore, since a polarizing element with a high Ys cannot achieve both high transmittance and high polarization, it is necessary to verify the blocking effect by sensory evaluation of the actual reflected light blocking effect or by performing measurements using polarized light incidence (B: polarized light incidence measurement) as described below. The Py required for such a polarizing element is preferably 15% or more, more preferably 30% or more, and even more preferably 45% or more.
[0040] (Adhesive Layer) The adhesive layer is a layer for adhering the support and the polarizing element. A resin material containing at least a base polymer (hereinafter also referred to as the main agent) and a curing aid such as a crosslinking agent can be used as the adhesive layer. Depending on the dilution component of the adhesive, the adhesive may be water-based, solvent-based, or solventless, and the type may be appropriately selected according to the surface properties of the adherend and the curing method. In consideration of compatibility with the hue-adjusting dye described below, the adhesive layer included in the optical laminate of the present invention is preferably a solvent-based or solventless adhesive layer, and a solvent-based adhesive layer is particularly preferred because of the ease of preparing the dye solution and adjusting the dye concentration and transmittance in the system. Hereinafter, a solvent-based or solventless adhesive layer will be referred to as a "solvent-based or solventless adhesive layer," and a water-based adhesive layer will be referred to as an "aqueous adhesive layer."
[0041] The adhesive layer is provided to bring the support and the polarizing element or the support and another support into close contact, and at least one layer may be included in the optical laminate, or multiple layers may be provided depending on the design of the optical laminate. Furthermore, when a TAC-based resin film is used as the support of the optical laminate, the polarizing element or the TAC-based resin films may be laminated together with an aqueous adhesive layer, and the aqueous adhesive layer may be used in combination with a solvent-based or solventless adhesive layer.
[0042] In a solvent-based or solventless adhesive layer, a transparent photocurable resin or thermosetting resin can be preferably used as the main component, examples of which include acrylic resins, urethane resins, epoxy resins, silicone resins, rubber resins, polyvinyl ether resins, and polyester resins. In particular, when processing a polarized lens using the optical laminate of the present invention and a lens substrate, as described below, a shaping process involving heat and a step of integral molding with a resin are required, and therefore, from the viewpoint of these moldability, it is preferable that the adhesive layer contain a thermosetting resin, and among these, it is particularly preferable that it contain an amorphous polyester resin.
[0043] The amorphous polyester resin is preferably soluble in organic solvents, has a mass average molecular weight of 15,000 or more and 30,000 or less, and has a glass transition temperature of -20°C or more and 20°C or less. These properties enable the formation of an adhesive layer that is excellent in lens processability and interlayer adhesion, and further allows for easy layer formation by the coating method described below. Examples of amorphous polyester resins include the commercially available "Vylon" series (product numbers: 200, 240, 245, 500, etc.) manufactured by Toyobo Co., Ltd.
[0044] A curing agent may be added to the amorphous polyester resin together with the dilution solvent. The type of curing agent is not particularly limited, but isocyanate compounds are preferred. Furthermore, a curing aid (also called a curing catalyst) or the like may be further added to accelerate curing and control physical properties. The dilution solvent is not particularly limited as long as it dissolves the resin and various additives, but examples thereof include methyl ethyl ketone (MEK), cyclopentanone (CPN), and cyclohexanone (CHN).
[0045] (Hue-Adjusting Dye) At least one adhesive layer used in the present invention contains one or more hue-adjusting dyes that adjust the hue and visible light transmittance of the optical laminate. The hue-adjusting dye has a maximum absorption wavelength (also referred to as λmax) in the visible light range and is used to adjust the hue and visible light transmittance of the optical laminate, and preferably does not contribute to polarization. The hue-adjusting dye may be contained in at least one adhesive layer, and one or more types may be blended into other adhesive layers depending on the optical design. When hue-adjusting dyes are contained in multiple adhesive layers, various hue-adjusting dyes may be separately contained in each adhesive layer, or the amount of hue-adjusting dye may be adjusted to incorporate the hue-adjusting dye into the adhesive layer so that the optical laminate has the desired optical properties. Materials commonly referred to as "dyes for resin coloring" or the like can be used as the hue-adjusting dye.
[0046] Examples of dyes for resin coloring include Solvent Yellow 33, Disperse Yellow 54, Disperse Yellow 160, Disperse Yellow 201, Solvent Orange 60, Solvent Red 111, Solvent Red 135, Solvent Red 168, Solvent Red 207, Disperse Red 22, Solvent Red 52, Solvent Red 179, Disperse Red 60, Disperse Violet 31, Solvent Blue 36, and Solvent Violet Solvent Blue 13, Disperse Blue 14, Solvent Blue 94, Solvent Blue 63, Solvent Blue 104, Solvent Blue 97, Solvent Green 20, Solvent Violet 13, Disperse Violet 28, Solvent Violet 36, and the like.
[0047] The hue-adjusting dye preferably has heat resistance. The required heat resistance means that the hue-adjusting dye does not decompose or discolor due to heat caused by the thermal history during bending of the optical laminate or lens molding, which will be described later.
[0048] The hue and transmittance of the optical laminate are adjusted using a hue-adjusting dye by incorporating into the adhesive layer, for example, one or two to four dyes corresponding to each wavelength range in the visible light range selected from (A) to (D) below, based on the transmittance waveform exhibited by the polarizing element. This reduces the transmittance in the wavelength range corresponding to λmax of each dye, thereby enabling the transmittance waveform to be adjusted in a balanced manner across the visible light range, and enabling any color tone to be designed.
[0049] (A) Dyes that exhibit red (having λmax in a wavelength range of about 400 to 500 nm); for example, Solvent Red 111, Solvent Red 135, Solvent Red 168, Solvent Red 207, Disperse Red 22, Solvent Red 52, Solvent Red 179, and Disperse Red 60. (B) Dyes that exhibit green (having λmax in a wavelength range of about 500 to 600 nm); for example, Solvent Green 3, Solvent Green 20, and Solvent Green 28. (C) Dyes that exhibit a blue color (having λmax in a wavelength region of about 600 to 700 nm); for example, Disperse Blue 14, Solvent Blue 94, Solvent Blue 63, Solvent Blue 104, and Solvent Blue 97. (D) Dyes that exhibit a yellow color (having λmax in a wavelength region of about 380 to 500 nm); for example, Solvent Yellow 33, Disperse Yellow 54, Disperse Yellow 160, Disperse Yellow 201, and Solvent Orange 60.
[0050] The hue-adjusting dye is not limited to the dyes (A) to (D) above, and dyes exhibiting other colors of the same kind or dyes having multiple light absorption wavelength ranges may be used as long as they satisfy the objectives of the present invention. Examples of other resin coloring dyes include Disperse Violet 13, Disperse Violet 28, and Solvent Violet 36.
[0051] As the hue-adjusting dye for use in the present invention, for example, in the case of the dye (A) above, Solvent Red 168 represented by the following chemical formula (1), in the case of the dye (B) above, Solvent Green 20 represented by the following chemical formula (2), in the case of the dye (C) above, Solvent Blue 97 represented by the following chemical formula (3), and in the case of the dye (D) above, Disperse Yellow 201 represented by the following chemical formula (4) can be particularly preferably used. Commercially available examples of these dyes (A) to (D) include the Plast series manufactured by Arimoto Chemical Industry Co., Ltd.
[0052]
[0053]
[0054]
[0055]
[0056] The amount of each of the dyes (A) to (D) alone is, for example, 0.001 to 0.5 parts by weight, preferably 0.002 to 0.4 parts by weight, per 100 parts by weight of the base material of the adhesive layer. Furthermore, when all of the dyes (A) to (D) are used in combination, the total amount is 0.004 to 2.0 parts by weight, preferably 0.008 to 1.6 parts by weight, per 100 parts by weight of the base material. By including the dyes (A) to (D) in such amounts, when the polarizing element and the adhesive layer are laminated, the transmittance is reduced by 10% to 15% compared to the gray polarizing element before lamination, thereby allowing the optical laminate to exhibit the desired hue. Furthermore, by having the total amount of the dyes (A) to (D) within the above range, leaching of the dyes can be suppressed during lens processing of the optical laminate and during use of the lens.
[0057] As commercially available hue-adjusting dyes, for example, Plast Red 8320 from the Plast series manufactured by Arimoto Chemical Industry Co., Ltd. can be used for Solvent Red 168, Plast Green 8645 from the same manufacturer can be used for Solvent Green 20, Plast Blue 8590 from the same manufacturer can be used for Solvent Blue 97, and Plast Yellow 8070 from the same manufacturer can be used for Disperse Yellow 201.
[0058] In addition to the above-mentioned hue-adjusting dye, at least one adhesive layer used in the present invention may contain a function-imparting material such as a specific wavelength absorbing dye. The use of a function-imparting material is desirable because it does not interact with the hue-adjusting dye, such as aggregation, and is also preferable in that it can impart functionality while adjusting the hue of the optical laminate during the manufacturing process of the adhesive layer. In eyewear, the specific wavelength absorbing dye can be used to absorb light within a specific wavelength range in the visible light region from incident light (external light) in order to enhance the contrast of the field of view or to impart effects such as anti-glare properties. The specific wavelength absorbing dye preferably has heat resistance. The required heat resistance means that the specific wavelength absorbing dye does not decompose or discolor due to heating caused by the thermal history that occurs during bending of the optical laminate or lens molding, as described below.
[0059] The specific wavelength absorbing dye may be blended in one type or two or more types in the adhesive layer depending on the optical design. The specific wavelength absorbing dye preferably has optical characteristics of λmax in the wavelength range of 570 nm to 600 nm, with a half-width of approximately 10 nm to 60 nm. Examples of such specific wavelength absorbing dyes include cyanine-based, squarylium-based, xanthene-based, oxonol-based, azo-based, and tetraazaporphyrin-based dyes, with tetraazaporphyrin-based dyes that exhibit a blue to purple color being particularly preferred.
[0060] Furthermore, as other function-imparting materials, in addition to the above-mentioned hue-adjusting dye, at least one of the adhesive layers used in the present invention may contain infrared-absorbing materials, ultraviolet-absorbing materials, photochromic materials, etc. that are compatible with or dispersible in the adhesive layer.
[0061] (Adjusting the hue of the optical laminate) Adjusting the hue of the optical laminate of the present invention includes using a polarizing element having a grayish color, which is a general-purpose color tone, as a reference and simply adjusting the transmittance of the grayish color of the polarizing element to a transmittance suitable for sunglasses without changing the hue much, and adjusting the transmittance of the polarizing element to a transmittance suitable for sunglasses while changing the grayish color of the polarizing element to the desired hue.
[0062] The polarizing element used in the optical laminate of the present invention preferably has a transmittance higher than the transmittance finally exhibited by the optical laminate. For example, when the desired optical laminate exhibits a Ys of 45% or more and 50% or less, the polarizing element preferably has a Ys of 58% or more and 62% or less, and when the desired optical laminate exhibits a Ys of 60% or more and 70% or less, the polarizing element preferably has a Ys of 75% or more and 80% or less. By combining an adhesive layer containing the above-mentioned hue-adjusting dye based on a polarizing element having such a predetermined Ys, it becomes possible to easily design a variety of hues from several types of polarizing elements without manufacturing polarizing elements with hue adjustments for each type.
[0063] (Method of Forming Adhesive Layer) The adhesive layer can be formed by a known coating method such as flow coating, spraying, bar coating, gravure coating, roll coating, blade coating, air knife coating, lip coating, comma coater method, die coater method, etc. In the present invention, in view of the physical properties of the components that form the adhesive layer, which will be described later, the comma coater method and die coater method can be particularly preferably used.
[0064] The adhesive layer is formed by applying an adhesive composition containing the above-mentioned main agent and hue-adjusting pigment to a base substrate so that the thickness after solvent removal is typically 5 μm to 50 μm, preferably 10 μm to 30 μm. If the thickness is less than 5 μm, sufficient interlayer adhesion strength may not be obtained. Furthermore, if the thickness exceeds 50 μm, fluctuations or undulations may occur on the coated surface, which may affect visibility when the resulting optical laminate is applied to eyewear. The base substrate refers to a substrate onto which the adhesive composition is directly applied to form the adhesive layer. In the present invention, the adhesive composition may be applied directly to a support, or may be applied to a polyethylene terephthalate (PET) resin film (also called a release film) coated with a release agent, and then the adhesive layer may be transferred to the polarizing element surface or the support surface by transfer.
[0065] The adhesive composition applied to the base substrate is dried at a temperature of 40 to 140°C, preferably 80 to 130°C, for 1 to 3 minutes to remove the solvent, thereby obtaining the adhesive layer used in the present invention. In addition, in the drying method using the above temperature conditions, it is desirable to provide multiple drying ovens and gradually increase the temperature from low to high in order to form an adhesive layer with a good surface appearance. Furthermore, the air surface is laminated with the surface of the support or polarizing element that will be the adherend surface of the optical laminate described below. At this time, one or both surfaces of the support or polarizing element that will be the adherend surface may be subjected to a surface modification treatment such as corona treatment or plasma treatment to improve adhesion.
[0066] After the above-described lamination, an aging treatment may be carried out to promote the crosslinking reaction of the curing agent in the adhesive layer. The conditions for the aging treatment vary depending on the type of resin and crosslinking agent used, but the adhesive layer used in the present invention is preferably kept in a thermostatic chamber at 25 to 50°C, preferably 35 to 40°C, for about one day to one week. From the viewpoint of improving the adhesion between the layers, the aging treatment is preferably carried out after laminating one surface of the support, which will be the adherend surface, and the surface of the polarizing element via the adhesive layer.
[0067] (Method for manufacturing optical laminate) The method for manufacturing the optical laminate of the present invention includes step a) of forming a polarizing element, step b) of forming an adhesive layer, and step c) of laminating the support and the polarizing element using the adhesive layer, and may be performed continuously in order starting from the step of forming the polarizing element, or each step may be performed sequentially.
[0068] From the viewpoint of ease of manufacturing and quality stability, step b) of forming the adhesive layer preferably includes a step of dissolving various dyes in a solvent and then mixing the resulting solution with the main component of the adhesive layer. Specifically, the various dyes are dissolved in the same solvent as the dilution solvent used for the main component, and the resulting dye solution is blended into the main component or a solution of the main component. This allows the various dyes to be uniformly mixed in the main component. The term "dissolved" also includes the meaning of a uniformly dispersed state.
[0069] Furthermore, when preparing various dyes, each dye solution may be prepared using the same dilution solvent, and each dye solution may be mixed simultaneously or sequentially into the main agent or the main agent solution, or all dyes may be mixed together using the same dilution solvent to prepare a dye solution, which may then be mixed into the main agent or the main agent solution.
[0070] Hereinafter, examples of producing the optical laminate according to the present invention will be described, but the types and blending amounts of the various materials are not limited to those described below.
[0071] In step a) of forming a polarizing element, a grayish PVA-based polarizing film that uses a dichroic dye to exhibit predetermined optical properties is used as the polarizing element, and a TAC-based resin film is used as the first support. Based on a known method for producing a polarizing plate, a polarizing element is produced that has a support (first support) on only one side via an aqueous adhesive layer made of a PVA-based resin material.
[0072] In step b) of forming the adhesive layer, a base solution containing an amorphous polyester resin as a base, cyclohexanone as a diluting solvent, isocyanate as a curing agent, and dibutyltin dilaurate (DBSn) as a curing catalyst is prepared. At this time, the various materials are mixed in a ratio of 20 to 40 parts by mass of cyclohexanone, preferably 25 to 35 parts by mass, 1 to 3 parts by mass of a polyisocyanate compound solution (manufactured by Soken Chemical & Engineering Co., Ltd., "590E"), and 0.005 to 0.02 parts by mass, preferably 0.008 to 0.015 parts by mass, based on 100 parts by mass of the amorphous polyester resin.
[0073] Next, a dye solution containing at least one of Disperse Yellow 201, Solvent Blue 97, Solvent Red 168, and Solvent Green 20 as a hue-adjusting dye is prepared. At this time, based on 100 parts by mass of the amorphous polyester resin contained in the adhesive composition, cyclohexanone as a diluting solvent is 1 part by mass to 25 parts by mass, preferably 5 parts by mass to 18 parts by mass, Disperse Yellow 201 is 0.001 parts by mass to 0.03 parts by mass, preferably 0.008 parts by mass to 0.025 parts by mass, and Solvent Blue 97, Solvent Red 168, and Solvent Green 20 are each 0.001 parts by mass to 0.8 parts by mass, preferably 0.01 parts by mass to 0.5 parts by mass, and the diluting solvent and the hue-adjusting dye are mixed so that the ratio is 0.001 parts by mass to 0.8 parts by mass, preferably 0.01 parts by mass to 0.5 parts by mass. By uniformly mixing the base solution and the dye solution, an adhesive composition containing the base and the hue-adjusting dye can be prepared.
[0074] In step c) of laminating the support and the polarizing element using the adhesive layer, the obtained adhesive composition is applied to a PA-based resin film serving as a second support. Next, in the drying step, the solvent is evaporated from the coating film on the PA-based resin film coated with the adhesive composition using multiple drying ovens, each set at a temperature range of 40°C to 100°C. The amount of coating is adjusted so that the thickness of the adhesive layer after drying is 20 μm to 30 μm. The adhesive layer side is then bonded to the polarizing element, thereby producing an optical laminate having a laminate structure of first support / water-based adhesive layer / polarizing element / adhesive layer / second support.
[0075] Further, other examples of producing the optical laminate of the present invention will be described, but the types and blending amounts of the various materials are not limited to those described below.
[0076] In step a) of forming a polarizing element, a grayish PVA-based polarizing film that uses a dichroic dye to exhibit predetermined optical properties is used as the polarizing element, a TAC-based resin film is used as the first support, and the same TAC-based resin film is used as the second support, and a polarizing element is produced in which both sides are sandwiched between supports (the first support and the second support) via an aqueous adhesive layer made of a PVA-based resin material, based on a known method for producing a polarizing plate.
[0077] In step b) of forming the adhesive layer, a base solution containing an amorphous polyester resin as a base, cyclohexanone as a diluting solvent, isocyanate as a curing agent, and dibutyltin dilaurate (DBSn) as a curing catalyst is prepared. At this time, the various materials are mixed in a ratio of 20 to 40 parts by mass of cyclohexanone, preferably 25 to 35 parts by mass, 1 to 3 parts by mass of a polyisocyanate compound solution (manufactured by Soken Chemical & Engineering Co., Ltd., "590E"), and 0.005 to 0.02 parts by mass, preferably 0.008 to 0.015 parts by mass of DBSn, based on 100 parts by mass of the amorphous polyester resin.
[0078] Next, a dye solution containing at least one of Disperse Yellow 201, Solvent Blue 97, Solvent Red 168, and Solvent Green 20 as a hue-adjusting dye is prepared. At this time, based on 100 parts by mass of the amorphous polyester resin contained in the adhesive composition, cyclohexanone as a diluting solvent is 1 part by mass to 25 parts by mass, preferably 5 parts by mass to 18 parts by mass, Disperse Yellow 201 is 0.001 parts by mass to 0.03 parts by mass, preferably 0.008 parts by mass to 0.025 parts by mass, and Solvent Blue 97, Solvent Red 168, and Solvent Green 20 are each 0.001 parts by mass to 0.8 parts by mass, preferably 0.01 parts by mass to 0.5 parts by mass, and the diluting solvent and the hue-adjusting dye are mixed so that the ratio is 0.001 parts by mass to 0.8 parts by mass, preferably 0.01 parts by mass to 0.5 parts by mass. By uniformly mixing the base solution and the dye solution, an adhesive composition containing the base and the hue-adjusting dye can be prepared.
[0079] In step c) of laminating the support and the polarizing element using the adhesive layer, the obtained adhesive composition is applied to a release film. Next, in the drying step, the solvent is evaporated from the coating film of the release film coated with the adhesive composition using multiple drying ovens, each set at a temperature range of 40°C to 100°C. The coating amount is adjusted so that the thickness of the adhesive layer after drying is 23 μm to 30 μm. The adhesive layer is then bonded to the second support surface, and the release film is removed. A PA-based resin film is then bonded to the exposed surface of the adhesive layer as a third support, thereby producing an optical laminate having a laminate structure of first support / aqueous adhesive layer / polarizing element / aqueous adhesive layer / second support / adhesive layer / third support.
[0080] (Evaluation of Optical Laminate) A method for evaluating the optical properties of the optical laminate of the present invention will be described. The optical properties (natural light incident transmittance and polarized light incident transmittance) of the optical laminate can be measured using, for example, a spectrophotometer "UH-4150" manufactured by Hitachi High-Tech Science Corporation. The evaluation of the optical properties may be carried out in the form of a polarized lens, as long as it does not interfere with the measurement.
[0081] (A: Measurement of Natural Light Incident Transmittance) The natural light incident transmittance, which is one of the optical properties of the optical laminate, is measured using natural light (not polarized light) as a light source. Hereinafter, this measurement will be simply referred to as "A" or "Measurement A." The natural light incident transmittance corresponds to the brightness of eyewear and the visibility of the color of scenery that is visible through the eyewear when wearing eyewear containing the optical laminate.
[0082] Specifically, in Measurement A, one test piece is placed so that the transmission axis or absorption axis is oriented at 0 degrees and 90 degrees, and the transmittance of each is measured in the wavelength range of visible light (380 to 780 nm) under detection conditions usually with a pitch of 10 nm or less, preferably with a pitch of 5 nm or less. The average value of these transmittances is obtained as the transmittance waveform of the optical laminate. From the obtained transmittance waveform, the luminosity-corrected transmittance (Ys, unit: %) is calculated based on JIS Z8781-2. At this time, the value of light source correction can preferably be a C light source or a D65 light source. Furthermore, from this transmittance waveform, L * a * b * Based on the color space (CIE1976, JIS Z8781-4), the values (L * s, a * s and b * s) is calculated.
[0083] Similarly, two test pieces are placed one on top of the other so that their transmission axes or absorption axes are parallel, and the luminous efficacy-corrected parallel transmittance (Yp, unit: %) is calculated from the obtained transmittance.Furthermore, two test pieces are placed one on top of the other so that their transmission axes or absorption axes are perpendicular, and the luminous efficacy-corrected orthogonal transmittance (Yc, unit: %) is calculated from the obtained transmittance.From these transmittances, the luminous efficacy-corrected polarization degree (Py, unit: %) can be calculated using the following formula (2).
[0084]
[0085] (B: Measurement of Polarized Incident Transmittance) Polarized incident transmittance, which is another optical property of the optical laminate, is optically measured using polarized light as a light source. This is a measurement method generally referred to as the absolute polarization method (Ky-Kz method), and the light source is polarized light emitted through a polarizing element having a luminosity-corrected polarization degree of 99.99% or more obtained in accordance with ISO Z8781-2. Hereinafter, this measurement will be simply referred to as "B" or "Measurement B." Polarized incident transmittance corresponds to the visibility of the colors of a scene when eyewear including the optical laminate is worn, including when reflected light is blocked by the polarizing element of the eyewear.
[0086] Specifically, in Measurement B, one test piece is placed so that the polarized light from the light source is perpendicular to the absorption axis of the test piece, and the transmittance of each wavelength is measured in the wavelength range of the visible light region (wavelengths of 380 to 780 nm) under detection conditions of 10 nm pitch or less, preferably 5 nm pitch or less. The transmittance of each wavelength is taken as the polarized incident orthogonal transmittance (Kz, unit: %). From the obtained transmittance waveform, the luminosity-corrected polarized incident orthogonal transmittance (Ykz, unit: %) is calculated based on JIS Z8781-2, as in Measurement A. In this case, the value of light source correction can preferably be a C light source or a D65 light source. Measurements A and B are performed under the same conditions. Furthermore, from this transmittance waveform, L * a * b * Based on the color space (CIE1976, JIS Z8781-4), the values (L * kz, a * kz and b * kz) is calculated.
[0087] (Calculation of saturation difference) The saturation difference is the value (a * s and b * s) and the value (a * kz and b * kz), and the absolute value of the magnitude of the difference between these hue values is represented as |Δc|.
[0088]
[0089] The saturation difference |Δc| is the absolute value of the difference between the color of a scene viewed through transmission when wearing eyewear containing an optical laminate (natural light incident transmission hue) and the color of a scene including when reflected light is blocked by the polarizing element of the eyewear (polarized light incident orthogonal transmission hue). If the saturation difference |Δc| is too large, when viewing a scene containing a lot of reflected light, there is a high possibility that the scene will be perceived as unnaturally colored, different from the color normally perceived. Therefore, by reducing the saturation difference |Δc|, even when viewing a scene containing a lot of reflected light, the coloring due to blocking by the polarizing element will be reduced, and the scene will be perceived as less strange.
[0090] The saturation difference |Δc| exhibited by the optical laminate of the present invention is 10 or less. This makes it possible to provide an optical laminate with excellent visibility and eyewear using the same. Furthermore, the saturation difference |Δc| is preferably 8 or less, more preferably 5 or less, even more preferably 4 or less, even more preferably 3 or less, and particularly preferably 2 or less. On the other hand, if the saturation difference |Δc| exceeds 10, there is a high possibility that, although it depends on the hue of the eyewear, when a scene containing a lot of reflected light is viewed, the scene will be perceived as unnaturally colored, different from the color normally perceived.
[0091] <Polarized Lens> The polarized lens of the present invention comprises a lens substrate and an optical laminate, and is suitable for use in eyewear. A polarized lens for eyewear can be obtained by molding the optical laminate into a desired shape so that the first support is on the outside (the side opposite the lens substrate). Furthermore, eyewear such as sunglasses or goggles can be obtained by fixing the polarized lens for eyewear to a frame. An example of the process for forming a polarized lens is described below, but the process is not limited to this.
[0092] A polarized lens can be formed by sequentially carrying out the steps of forming a sheet- (or film-) shaped optical laminate containing polarizing elements, shaping (bending) the optical laminate, insert-molding the shaped optical laminate and a resin, and applying a hard coat to the resulting insert-molded product.
[0093] The shaping (bending) of the optical laminate is performed using a heat press or the like to facilitate combining the lens substrate and the optical laminate, which will be described later, and processing them into a lens shape. A mold designed to a predetermined size is used for the shaping, and the shape of the mold is appropriately designed according to the design of the eyewear product, etc. FIG. 3 is a schematic diagram showing an example of the shaping (bending) of the optical laminate according to the present invention. As shown in FIG. 3 , the optical laminate 100 is placed in a bending mold 50 (concave mold), and then the optical laminate 100 is pressed with a hemispherical mold 51 (convex mold, also called a hot iron ball) heated to a predetermined temperature, thereby obtaining a bent optical laminate 101. That is, the second support 12, which is the support on the viewing side of the optical laminate 100, is injection molded using the spherical mold 51, thereby producing the bent optical laminate 101.
[0094] The bending conditions are determined in consideration of the bendability and heat resistance (discoloration of the polarizing element, etc.) of the optical laminate, and the temperature is usually 70 to 120° C., preferably 80 to 100° C., and the time is in the range of 1 to 3 minutes. At this time, only a portion of the optical laminate to be used in the subsequent insert molding step may be simultaneously or sequentially trimmed from the sheet-like optical laminate.
[0095] (Lens substrate) The lens substrate is a resin material used for integrating with the optical laminate of the present invention and processing it into a lens shape. In the bending process described above, a resin (also referred to as a lens substrate) may be further injected. In this case, there is an advantage that the thickness unevenness of the optical laminate of the present invention becomes invisible, and even for lenses without focal refractive power, resin injection is performed to produce products that are particularly excellent in impact resistance, appearance, and eye fatigue. In order to prevent deterioration of appearance due to refractive index differences, it is preferable that the injected resin be the same material as the layer with which the injected resin is in contact. For such integration processing, an insert molding method can generally be used.
[0096] The resin used for the lens substrate is not particularly limited, and examples thereof include thermoplastic resins that can be molded by injection molding, and thermosetting resins that can be molded by distillation polymerization or the like and are commonly used for eyewear lenses, etc. Examples of such resins include (meth)acrylic resins such as methyl methacrylate homopolymers and copolymers of methyl methacrylate and one or more other monomers, diethylene glycol bisallyl carbonate resins such as diethylene glycol bisallyl carbonate homopolymers and copolymers of diethylene glycol bisallyl carbonate and one or more other monomers, acrylonitrile-styrene copolymers, halogen-containing copolymers, polysulfide resins such as homopolymers of monomers having sulfide bonds and copolymers of monomers having sulfide bonds and one or more other monomers, polyurea resins, PA resins, PC resins, polystyrene resins, polyolefin resins, polyvinyl chloride resins, polyester resins, PET resins, polyurethane resins, and sulfur-containing urethane resins such as polythiourethane resins, and epoxy resins. From the viewpoint of adhesion to the optical laminate, it is preferable that the material of the lens substrate is the same as that of the layer that it contacts. As a specific example of such a resin combination, the support of the optical laminate on the integrated processing side can be made of a PA-based resin, and the lens substrate can also be made of a PA-based resin, so that the support and the lens substrate can be fused together.
[0097] <Eyewear> The eyewear of the present invention comprises the above-described polarized lens. The polarized lens may have a hard coating, an anti-reflection film, or the like formed on its surface as appropriate, and the eyewear of the present invention can be produced by fixing the polarized lens to a frame by edging, drilling, screwing, or the like.
[0098] Furthermore, the eyewear of the present invention may contain the above-mentioned ultraviolet absorber in any layer of the optical laminate or lens substrate to provide ultraviolet absorption ability, and may also contain a dye or metal oxide or the like in any layer or laminate it between layers to provide infrared absorption function, or may contain a photochromic material in any layer or laminate it between layers to provide dimming function.
[0099] The eyewear of the present invention can be worn both indoors and outdoors as highly fashionable eyewear. In this case, a higher transmittance than that of ordinary lenses is required, and the eyewear is designed to meet "Lens Category 1" (luminous transmittance (τv): 43% < τv ≦ 80%) as specified in the European standard for lens transmittance (EN ISO 12312-1:2013 / Al:2015). The European standard (EN ISO 12312-1:2013 / Al:2015) is a standard for personal protective equipment such as sunglasses, and corresponds to the personal protective equipment regulations established in the European region. In this standard, the explanatory label for general-use sunglasses lenses and an overview of the luminous transmittance (τv) and lens classification requirements are as follows. Here, τv corresponds to the above-mentioned Ys.
[0100] Explanation label: Light-tinted sunglasses Lens category 0: τv > 80% Lens category 1: 43% < τv ≦ 80% Explanation label: General-purpose sunglasses Lens category 2: 18% < τv ≦ 43% Lens category 3: 8% < τv ≦ 18% Explanation label: Special-purpose sunglasses Lens category 4: 3% < τv ≦ 8%
[0101] Based on the above embodiments, the present invention relates to the following [1] to [7]: [1] An optical laminate comprising a support, a polarizing element, and at least one adhesive layer between the support and the polarizing element, wherein the polarizing element contains at least one dye-based dichroic dye and exhibits a grayish color, and at least one adhesive layer contains one or more hue-adjusting dyes that adjust the hue and transmittance of the optical laminate in the visible light region, and the saturation difference |Δc| represented by the following formula (1) is 10 or less. (In formula (1), a * s and b * s is the L when natural light is incident on the optical laminate * a * b * is the hue value in the color space, and a * kz and b * kz is the L when polarized light is incident in a direction perpendicular to the absorption axis of the optical laminate. * a* b * (These are hue values in the color space (CIE 1976)). [2] The optical laminate according to the above [1], wherein the hue-adjusting dye comprises at least one of the dyes (A) to (D) below. (A) Dye that exhibits a reddish color (having λmax in a wavelength range of about 400 to 500 nm) (B) Dye that exhibits a greenish color (having λmax in a wavelength range of about 500 to 600 nm) (C) Dye that exhibits a bluish color (having λmax in a wavelength range of about 600 to 700 nm) (D) Dye that exhibits a yellowish color (having λmax in a wavelength range of about 380 to 500 nm). [3] The optical laminate according to the above [1] or [2], wherein the adhesive layer comprises an amorphous polyester resin. [4] In the polarizing element, * a * b * Hue value a in color space (CIE 1976) * s and b * The optical laminate according to any one of [1] to [3] above, wherein s is in the range of -5 or more and 5 or less. [5] The optical laminate according to any one of [1] to [4] above, wherein the polarizing element has the optical property of a luminosity-corrected transmittance (Ys) for incident natural light of 43% or more and 80% or less. [6] A polarized lens comprising a lens substrate and the optical laminate according to any one of [1] to [5] above. [7] Eyewear comprising the polarized lens according to [6] above.
[0102] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. In Examples 1 to 6, in order to compare the effects of the present invention, the compositions, layer structures, etc. were designed to be as similar as possible so that the optical properties in Measurement A could be compared with the optical properties in Measurement A of Comparative Examples 1 to 6.
[0103] [Example 1] (Preparation of Polarizing Element) A dyeing solution was prepared by dissolving the following dyes 1 to 4 and sodium sulfate in water, based on the description in Example 1 of JP-A No. 11-218611. That is, as the dyeing solution, an aqueous solution was prepared at 45°C containing 0.04 mass % of dye 1, 0.02 mass % of dye 2, 0.06 mass % of dye 3, 0.04 mass % of dye 4, and 0.3 mass % of sodium sulfate.
[0104] <Dye 1> C.I. Direct Orange 39 (Kayafect Orange G, manufactured by Nippon Kayaku Co., Ltd.) was used. <Dye 2> C.I. Direct Red 81 (Red 4BL, manufactured by Nippon Chemical Industry Co., Ltd.) was used. <Dye 3> A dye represented by the following chemical formula (5) described in JP-A-11-218611 was synthesized according to the same publication. <Dye 4> A dye represented by the following chemical formula (6), which is disclosed in Example 38 of JP-A-60-156759, was synthesized according to the same publication.
[0105] Next, a PVA-based resin film ("VF-PS#7500" manufactured by Kuraray Co., Ltd.) was immersed in water while being uniaxially stretched to swell, and then immersed in the prepared dyeing solution and further stretched with an aqueous boric acid solution, thereby orienting each coloring matter (each dye) in the resin film. The total magnification of uniaxial stretching from swelling to boric acid treatment was 4 to 5 times. After stretching, the resin film was dried for 3 minutes in a dryer at 70°C while maintaining tension, thereby producing a polarizing element. The obtained polarizing element exhibited a grayish color, and its optical properties were measured using a spectrophotometer "UH-4150" manufactured by Hitachi High-Tech Science Corporation, whereby the optical properties were Ys = 60.5% and Py = 47.7%. In addition, L * a * b * The hues in the color space are L * s = 82.1, a * s = 0.4, and b * s=-0.2.
[0106] (Preparation of Adhesive Composition) An adhesive composition was obtained containing an organic solvent-soluble polyester resin (Vylon 500, manufactured by Toyobo Co., Ltd., resin solids content 44.9%) as the main component of the adhesive composition, 2% by mass of an isocyanate-based curing agent (590E, manufactured by Soken Chemical & Engineering Co., Ltd.), 0.01% by mass of dibutyltin dilaurate (DBSn), the following hue-adjusting dyes, and 0.21% by mass of cyclohexanone as a dilution solvent. Here, each hue-adjusting dye was dissolved in a dilution solvent in advance, and then this dye solution was uniformly mixed with a main component solution containing the main component, curing agent, DBSn, and dilution solvent. <Hue-adjusting dyes> Disperse Yellow 201 (manufactured by Arimoto Chemical Industry Co., Ltd.): 0.016% by mass Solvent Red 168 (manufactured by Arimoto Chemical Industry Co., Ltd.): 0.160% by mass
[0107] (Preparation of optical laminate) The obtained polarizing element and a TAC film (manufactured by Island Polymer Industries GmbH, "13SG80S-LH", film thickness 80 μm) that had been saponified (immersed in a 2 N sodium hydroxide aqueous solution at 40° C. for 10 minutes) as a first support were bonded together using an aqueous adhesive layer containing a PVA resin (solid content of the PVA resin was 2.0% by mass), and this was dried at 80° C. for 3 minutes to remove moisture, thereby adhering the polarizing element and the first support, thereby producing a polarizing element having a first support on one side of the polarizing element.
[0108] Next, the obtained adhesive composition was applied by a die coater method to one side of a PA resin film (manufactured by EMS, "TRF-800," film thickness 80 μm) used as a second support. The coating film was dried at 100°C for 3 minutes to remove the solvent, thereby producing an adhesive layer (film thickness 24 μm). The prepared polarizing element surface was then bonded to the air side of the adhesive layer (the surface on which the second support was not placed), thereby obtaining an optical laminate exhibiting a reddish color. Furthermore, the obtained optical laminate was subjected to an aging treatment at 35°C for one week to promote the curing reaction of the adhesive layer and to enhance adhesion between the polarizing element and the second support. The optical properties of the obtained optical laminate were measured by Measurement A and Measurement B, respectively, using a spectrophotometer "UH-4150" manufactured by Hitachi High-Tech Science Corporation. Furthermore, the saturation difference |Δc| and the luminosity-corrected polarization degree (Py) were calculated based on the above-mentioned formulas (1) and (2). The results are shown in Table 1.
[0109] [Example 2] (Preparation of Optical Laminate) An optical laminate exhibiting a bluish color was prepared in the same manner as in Example 1, except that a hue-adjusting dye was used in the formulation described below instead of the adhesive composition used in Example 1, and cyclohexanone was used as the dilution solvent at 0.348 mass%. The optical properties of the obtained optical laminate were measured by Measurement A and Measurement B. In addition, the saturation difference |Δc| and the luminosity-corrected polarization index (Py) were calculated based on the above-mentioned formulas (1) and (2). The results are shown in Table 1. <Hue-adjusting dye> Solvent Blue 97 (manufactured by Arimoto Chemical Industry Co., Ltd.): 0.060 mass% Solvent Red 168 (manufactured by Arimoto Chemical Industry Co., Ltd.): 0.020 mass%
[0110] Example 3 (Preparation of Optical Laminate) An optical laminate exhibiting a greenish color was prepared in the same manner as in Example 1, except that a hue-adjusting dye was used in the formulation described below instead of the adhesive composition used in Example 1, and cyclohexanone was used as the dilution solvent at 0.304 mass %. The optical properties of the obtained optical laminate were measured by Measurement A and Measurement B, respectively. In addition, the saturation difference |Δc| and the luminosity-corrected polarization degree (Py) were calculated based on the above-mentioned formulas (1) and (2), respectively. The results are shown in Table 1. <Hue adjustment dye> Disperse Yellow 201 (manufactured by Arimoto Chemical Industry Co., Ltd.): 0.012 mass% Solvent Blue 97 (manufactured by Arimoto Chemical Industry Co., Ltd.): 0.028 mass% Solvent Green 20 (manufactured by Arimoto Chemical Industry Co., Ltd.): 0.0520 mass% Solvent Red 168 (manufactured by Arimoto Chemical Industry Co., Ltd.): 0.016% by mass
[0111] Example 4 (Preparation of Optical Laminate) An optical laminate exhibiting a brownish color was prepared in the same manner as in Example 1, except that the adhesive composition used in Example 1 was replaced with a hue-adjusting dye in the formulation shown below, and 0.348% by mass of cyclohexanone was used as the dilution solvent. The optical properties of the obtained optical laminate were measured by Measurement A and Measurement B. The saturation difference |Δc| and the luminosity-corrected polarization index (Py) were calculated based on the above-mentioned formulas (1) and (2). The results are shown in Table 1. <Hue-adjusting dye> Disperse Yellow 201 (manufactured by Arimoto Chemical Industry Co., Ltd.): 0.080% by mass Solvent Green 20 (manufactured by Arimoto Chemical Industry Co., Ltd.): 0.004% by mass Solvent Red 168 (manufactured by Arimoto Chemical Industry Co., Ltd.): 0.128% by mass
[0112] [Example 5] (Preparation of Polarizing Element) A polarizing element was prepared in the same manner as in Example 1, except that the blending amounts of dyes 1 to 4 used in Example 1 were changed so that dye 1 was 0.02% by mass, dye 2 was 0.01% by mass, dye 3 was 0.03% by mass, and dye 4 was 0.02% by mass. The obtained polarizing element exhibited a grayish color, and when its optical properties were measured using a spectrophotometer "UH-4150" manufactured by Hitachi High-Tech Science Corporation, the optical properties were: Ys = 77.1%, Py = 19.6%, L* a * b * The hues in the color space are L * s = 90.4, a * s = 3.5, and b * s=-2.8.
[0113] (Preparation of Optical Laminate) An optical laminate exhibiting a reddish color was prepared in the same manner as in Example 1, except that the polarizing element obtained above was used instead of the polarizing element used in Example 1. The optical properties of the obtained optical laminate were measured by Measurement A and Measurement B. In addition, the saturation difference |Δc| and the luminosity-corrected polarization degree (Py) were calculated based on the above-mentioned formulas (1) and (2). The results are shown in Table 1.
[0114] [Example 6] (Preparation of Optical Laminate) An optical laminate exhibiting a bluish color was prepared in the same manner as in Example 1, except that the polarizing element used in Example 5 and the adhesive composition used in Example 2 were used. The optical properties of the obtained optical laminate were measured by Measurement A and Measurement B. In addition, the saturation difference |Δc| and the luminosity-corrected polarization degree (Py) were calculated based on the above-mentioned formulas (1) and (2). The results are shown in Table 1.
[0115] Comparative Example 1 (Preparation of Polarizing Element) A polarizing element exhibiting a reddish color was prepared in the same manner as in Example 1, except that only Dye 2 described in Example 1 was used. The optical properties of the obtained polarizing element were measured, and the results were Ys=45.9%, L * a * b * The hues in the color space are a * s = 16.3, and b * On the other hand, Ykz was 12.5%, L * a * b * The hues in the color space are a * kz = 47.5, and b * The kz was 34.1.
[0116] (Preparation of Adhesive Composition) An adhesive composition was prepared in the same manner as in Example 1, except that no hue-adjusting dye was used.
[0117] (Preparation of Optical Laminate) A comparative optical laminate was prepared in the same manner as in Example 1, except that the polarizing element and adhesive composition obtained above were used. The optical properties of the obtained optical laminate were measured by Measurement A and Measurement B. In addition, the saturation difference |Δc| and the luminosity-corrected polarization degree (Py) were calculated based on the above-mentioned formulas (1) and (2). The results are shown in Table 1.
[0118] Comparative Example 2 (Preparation of Polarizing Element) A polarizing element exhibiting a bluish color was prepared in the same manner as in Example 1, except that only dye 3 described in Example 1 was used. The optical properties of the obtained polarizing element were measured, and the results were Ys=49.7%, L * a * b * The hue in the color space is a * s = 0.7, and b * On the other hand, Ykz was 14.7%, L * a * b * The hue in the color space is a * kz = 6.9, and b * kz = -28.4.
[0119] (Preparation of Optical Laminate) A comparative optical laminate was prepared in the same manner as in Comparative Example 1, except that the polarizing element obtained as described above was used. The optical properties of the obtained optical laminate were measured by Measurement A and Measurement B. In addition, the saturation difference |Δc| and the luminosity-corrected polarization degree (Py) were calculated based on the above-mentioned formulas (1) and (2). The results are shown in Table 1.
[0120] Comparative Example 3 (Preparation of Polarizing Element) A polarizing element exhibiting a greenish color was prepared in the same manner as in Example 1, except that only dye 4 described in Example 1 was used. The optical properties of the obtained polarizing element were measured, and the results were Ys=50.2%, L * a * b * The hue in the color space is a * s = -9.0, and b * On the other hand, Ykz was 14.1%, L * a * b *The hue in the color space is a * kz = -30.5, and b * kz=1.2.
[0121] (Preparation of Optical Laminate) A comparative optical laminate was prepared in the same manner as in Comparative Example 1, except that the polarizing element obtained above was used. The optical properties of the obtained optical laminate were measured by Measurement A and Measurement B. In addition, the saturation difference |Δc| and the luminosity-corrected polarization degree (Py) were calculated based on the above-mentioned formulas (1) and (2). The results are shown in Table 1.
[0122] Comparative Example 4 (Preparation of Polarizing Element) A comparative polarizing element exhibiting a brownish color was prepared in the same manner as in Example 1, except that dyes 1 and 4 described in Example 1 were used. The optical properties of the obtained polarizing element were measured, and the results were: Ys = 47.0%, a * s = 1.1, and b * s = 38.4. Ykz = 16.3%, L * a * b * The hue in the color space is a * kz = 17.7, and b * The kz was 93.3.
[0123] (Preparation of Optical Laminate) A comparative optical laminate was prepared in the same manner as in Comparative Example 1, except that the polarizing element obtained above was used. The optical properties of the obtained optical laminate were measured by Measurement A and Measurement B. In addition, the saturation difference |Δc| and the luminosity-corrected polarization degree (Py) were calculated based on the above-mentioned formulas (1) and (2). The results are shown in Table 1.
[0124] Comparative Example 5 (Preparation of Polarizing Element) A polarizing element exhibiting a reddish color was prepared in the same manner as in Example 1, except that only Dye 2 described in Example 1 was used and the concentration of the dyeing solution and the dyeing time were adjusted so that the Ys of the polarizing element was 55 to 60%. When the optical properties of the obtained polarizing element were measured, Ys was 58.4%, L * a * b * The hue in the color space is a * s = 18.6, and b *s = 4.0. Ykz = 26.9%, L * a * b * The hue in the color space is a * kz = 45.7, and b * The kz was 12.5.
[0125] (Preparation of Optical Laminate) A comparative optical laminate was prepared in the same manner as in Comparative Example 1, except that the polarizing element obtained above was used. The optical properties of the obtained optical laminate were measured by Measurement A and Measurement B. In addition, the saturation difference |Δc| and the luminosity-corrected polarization degree (Py) were calculated based on the above-mentioned formulas (1) and (2). The results are shown in Table 1.
[0126] Comparative Example 6 (Preparation of Polarizing Element) A polarizing element exhibiting a blue-based color was prepared in the same manner as in Example 1, except that only dye 3 described in Example 1 was used and the concentration of the dyeing solution and the dyeing time were adjusted so that the Ys of the polarizing element was 65 to 70%. When the optical properties of the obtained polarizing element were measured, Ys was 69.8%, L * a * b * The hue in the color space is a * s = -0.3, and b * s = -7.8. Ykz = 45.3%, L * a * b * The hue in the color space is a * kz = -0.1, and b * kz=-18.8.
[0127] (Preparation of Optical Laminate) A comparative optical laminate was prepared in the same manner as in Comparative Example 1, except that the polarizing element obtained above was used. The optical properties of the obtained optical laminate were measured by Measurement A and Measurement B. In addition, the saturation difference |Δc| and the luminosity-corrected polarization degree (Py) were calculated based on the above-mentioned formulas (1) and (2). The results are shown in Table 1.
[0128]
[0129] As shown in Table 1, the optical laminates of Examples 1 to 6 and Comparative Examples 1 to 6 had Ys in the range of 45 to 70%, satisfying the European Standard Lens Category 1. Regarding the optical characteristics (natural light incident transmittance) measured by Measurement A, as shown in Figures 4 to 9, the transmittance waveforms of Examples 1 to 6 and Comparative Examples 1 to 6 were nearly identical, and as shown in Table 1, the Ys and hue values were also nearly equivalent. This demonstrates that the optical laminates of Examples 1 to 6, which were toned using a gray polarizing element and an adhesive layer containing a hue-adjusting dye, can be optically designed comparable to Comparative Examples 1 to 6, which were toned using only a polarizing element. Furthermore, the Py of the optical laminates of Examples 1 to 6 was in the range of 18 to 49%, confirming their polarizing function. These Py values were generally lower than the Py of Comparative Examples 1 to 6. This is because when dyes are used in a mixed color, it is more difficult to achieve high polarization performance due to the influence of the sub-absorption wavelength range of each dye than when dyes are used in a single color.
[0130] On the other hand, in the optical characteristics (polarized light incident transmittance) by Measurement B, as shown in Figures 10 to 15, the transmittance waveforms of Examples 1 to 6 and Comparative Examples 1 to 6 did not match, and the waveform structure of Comparative Examples 1 to 6 was generally sunken. Accordingly, as shown in Table 1, the Ykz values of Examples 1 to 6 were higher than those of Comparative Examples 1 to 6. Furthermore, as shown in Figures 4 to 15, the waveform structure of Examples 1 to 6 was almost the same between Measurement A and Measurement B, indicating that the difference in hue value between Measurement A and Measurement B was small. As a result, the saturation difference |Δc| of Examples 1 to 6 was within the range of 1 to 4, which was more than 10 times lower than the |Δc| of Comparative Example 1. Therefore, it can be said that eyewear using the optical laminate of the present invention, while having a polarization function, reduces unnatural coloring caused by the polarizing element and has better visibility, even when blocking reflected light including polarized light, compared to Comparative Examples 1 to 6, which were toned using only a polarizing element.
[0131] (Sensory evaluation of visibility) The optical laminates produced in Examples 1 to 6 and Comparative Examples 1 to 6 were placed to cover both eyes of a test subject, likening them to eyewear, and the presence or absence of a difference in the color of the entire scenery and the color of the blocked reflected light was sensorily verified based on the visibility of the scenery actually seen through the optical laminates. The optical laminates for both eyes of the test subject were placed so that the absorption axis was horizontal to the ground.
[0132] The visibility evaluation was performed under the following conditions 1 to 3. The evaluation results are shown in Table 3. <Condition 1> As a scene with almost no reflected light, the color perceived through the optical laminate was confirmed in an indoor room with fluorescent lights on. <Condition 2> As a condition with a strong influence of reflected light, the evaluation was performed outdoors on a sunny day in the presence of sunlight reflected from automobile windshields, building windows, etc., based on the following evaluation criteria. The evaluation criteria were determined by 10 testers observing the same scene and assigning a four-point scale as shown in Table 2. <Condition 3> As a condition with an even stronger influence of reflected light than Condition 2, the evaluation was performed outdoors on a sunny day in the same scene as Condition 2, but after it had rained. This assumes a situation with more reflected light, such as puddles and wet roads. The evaluation criteria were the same as Condition 2.
[0133]
[0134] Reference Example 1 An optical laminate of the Reference Example was produced in the same manner as in Example 1, except that the polarizing element of Example 1 was replaced with a dye-based polarizing element used in conventional colored polarized lenses. The polarizing element used was "Brown-30" manufactured by Nippon Kayaku Co., Ltd., which exhibits a brownish color. The optical properties of the obtained optical laminate were measured by Measurement A and Measurement B. Furthermore, the saturation difference |Δc| and the luminosity-corrected polarization degree (Py) were calculated based on the above-mentioned formulas (1) and (2). As shown in Table 1, the results were: Ys = 29.0%, Ykz = 0.0%, |Δc| = 8.5, Py = 99.8%, and L * a * b * The hue in the color space is L * s = 60.8, a * s = 1.8, and b * s=17.0, L* kz=-10.1, a * kz = 5.1, and b * The kz value was 6.9. The sensory evaluation was carried out on the obtained optical laminate. The results are shown in Table 3.
[0135] Reference Example 2 An optical laminate was produced in the same manner as in Example 1, except that the polarizing element in Example 1 was replaced with a dye-based polarizing element used in conventional colored polarized lenses. Ruby-15, manufactured by Nippon Kayaku Co., Ltd., which exhibits a reddish-brown color, was used as the polarizing element. The optical properties of the obtained optical laminate were measured by Measurement A and Measurement B. Furthermore, the saturation difference |Δc| and the luminosity-corrected polarization degree (Py) were calculated based on the above-mentioned formulas (1) and (2). As shown in Table 1, the results were: Ys = 15.7%, Ykz = 0.0%, |Δc| = 21.5, Py = 99.0%, and L * a * b * The hue in the color space is L * s = 46.6, a * s = 17.5, b * s=14.0, L * kz=-12.9, a * kz = 0.5, and b * The optical coefficient of curvature was -0.8. The optical laminate was subjected to the sensory evaluation described above. The results are shown in Table 3.
[0136]
[0137] From the results of condition 1, it was confirmed that when the optical laminates of Examples 1 to 6 were used in a situation where there was almost no reflected light, the color of the scenery perceived was the same as in Comparative Examples 1 to 6. Furthermore, in the results of conditions 2 and 3, the sensory evaluation of visibility for all of the optical laminates of Examples 1 to 6 was "good" or "double circle," confirming that visibility was good under the conditions verified.
[0138] On the other hand, the sensory evaluation of visibility was "×" or "Δ" for all of the optical laminates of Comparative Examples 1 to 6. This is presumably because the reflected light is blocked by the polarizing elements of the optical laminate, causing the portion accompanied by reflected light to appear darker in color, similar to when the axes of the two polarizing elements overlap at right angles.
[0139] In the optical laminates of Reference Examples 1 and 2, the field of view appears to be tinged with a dark color due to the polarizing element, as shown in the results for Condition 1, but the sensory evaluation of visibility under Conditions 2 and 3 was "◎", confirming that there is no difference in visibility with conventional polarizing elements for outdoor use. This is presumably because the entire field of view appears to be tinged with a dark color, the degree of polarization is high, and Ykz is in the 0% range, making it impossible to perceive differences in hue.
[0140] From the results of the sensory evaluation, it was found that in Examples 1 to 6, the difference between the color of the entire scenery and the color of the blocked reflected light was smaller than in Comparative Examples 1 to 6, and the scenery looked more natural.
[0141] The optical laminate of the present invention can provide a more natural wearing sensation without causing a significant change in the color of the scenery that is transmitted (natural light incident transmission hue) and the color of the blocked reflected light (polarized light incident orthogonal transmission hue), and therefore can be used in eyewear products, and is particularly suitable for application to colored eyewear products for European Standard Lens Category 1.
[0142] REFERENCE SIGNS LIST 10 Support 11 First support 12 Second support 20 Polarizing element 30 Adhesive layer 40 Lens substrate 50 Bending mold (concave mold) 51 Hemispherical mold (convex mold) 100, 110 Optical laminate 101 Bent optical laminate
Claims
1. An optical laminate comprising a support, a polarizing element, and at least one adhesive layer between the support and the polarizing element, wherein the polarizing element contains at least one dye-based dichroic dye and exhibits a grayish color, and at least one of the adhesive layers contains one or more hue-adjusting dyes that adjust the hue and transmittance in the visible light range of the optical laminate, and the saturation difference |Δc| represented by the following formula (1) is 10 or less. (In formula (1), a * s and b * s is the L when natural light is incident on the optical laminate * a * b * is the hue value in the color space, * kz and b * kz is the L when polarized light is incident perpendicular to the absorption axis of the optical laminate. * a * b * hue value in the color space (CIE 1976) 2. The optical laminate according to claim 1, wherein the hue-adjusting dye comprises at least one of the following dyes (A) to (D): (A) a dye that exhibits a reddish color (having λmax in a wavelength range of about 400 to 500 nm), (B) a dye that exhibits a greenish color (having λmax in a wavelength range of about 500 to 600 nm), (C) a dye that exhibits a blueish color (having λmax in a wavelength range of about 600 to 700 nm), and (D) a dye that exhibits a yellowish color (having λmax in a wavelength range of about 380 to 500 nm).
3. The optical laminate according to claim 1 or 2, wherein the adhesive layer contains an amorphous polyester resin.
4. In the polarizing element, L * a * b * Hue value a in color space (CIE 1976) * s and b * The optical laminate according to claim 1 or 2, wherein s is in the range of -5 or more and 5 or less.
5. The optical laminate according to claim 1 or 2, wherein the polarizing element has optical characteristics such that the luminosity-corrected transmittance (Ys) for natural light incidence is 43% or more and 80% or less.
6. A polarized lens comprising a lens substrate and the optical laminate according to claim 1 or 2.
7. Eyewear comprising the polarized lens according to claim 6.
Citation Information
Patent Citations
Polarizing optical article
JP2001311918A
Laminated plastic film for optical filter
JP2010115818A
Polarizing plate
KR1020160114394A
Optical film and eyewear
WO2020196449A1