Adhesive laminate sheet
The double-sided adhesive laminate sheet, featuring a nonwoven fluororesin fiber base layer and integrated fluororesin adhesive layers with an air layer, addresses the lack of heat insulation and resistance in existing sheets by achieving low thermal conductivity and maintaining strength at high temperatures.
Patent Information
- Application Number
- PCT/JP2024/012124
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-03-26
- Publication Date
- 2024-10-03
AI Technical Summary
Existing adhesive laminate sheets lack both heat insulation properties and heat resistance, despite being designed for thermal environments.
A double-sided adhesive laminate sheet with a specific structure, comprising a base layer of nonwoven fabric made from fluororesin fibers, two adhesive layers made from fluororesin adhesive components, and an air layer, where the adhesive layers are integrated with the base layer to enhance adhesive strength and heat resistance, and the air layer improves thermal conductivity.
The laminate sheet achieves excellent heat insulation properties with thermal conductivity of 0.20 W/(K·m) or less and maintains adhesive strength after exposure to high temperatures, demonstrating both heat resistance and insulation.
Smart Images

Figure JP2024012124_03102024_PF_FP_ABST
Abstract
Description
Adhesive laminated sheet
[0001] The present invention relates to an adhesive laminate sheet.
[0002] Adhesive sheets have been developed that are intended to be exposed to a hot environment.
[0003] For example, Patent Document 1 discloses a heat-resistant tape that includes a substrate layer and a pressure-sensitive adhesive layer, in which the substrate layer is a glass fiber fabric impregnated with a fluorine-containing resin, and in which a silicon-containing agent is present between the glass fiber fabric and the fluorine-containing resin.
[0004] Patent No. 7132919
[0005] The adhesive tape disclosed in Patent Document 1 is said to provide a heat-resistant tape with high productivity, but does not take into consideration heat insulation properties.
[0006] Therefore, an object of the present invention is to provide an adhesive laminated sheet having excellent heat insulation and heat resistance.
[0007] As a result of extensive research, the present inventors have found that the above-mentioned problems can be solved by an adhesive laminated sheet having a predetermined structure.
[0008] a first mixed layer impregnated with the first adhesive component and a second adhesive layer laminated in this order, the first adhesive layer comprising a first adhesive component, the second adhesive layer comprising a second adhesive component, the base layer comprising a nonwoven fabric sheet made of fluororesin fibers, the base layer comprising: a first mixed layer impregnated with the first adhesive component and provided in a range of 2% to 30% of the thickness of the base layer from the first adhesive layer side main surface of the base layer toward the second adhesive layer side main surface, a second mixed layer impregnated with the second adhesive component and provided in a range of 2% to 30% of the thickness of the base layer from the second adhesive layer side main surface of the base layer toward the first adhesive layer side main surface, and an air layer containing air and provided in a range of 40% to 96% of the thickness of the base layer from the first mixed layer toward the second mixed layer, the double-sided adhesive laminate sheet having a porosity of 20% or more, the first adhesive component of the first adhesive layer and the first adhesive component of the first mixed layer are integrated, and the second adhesive component of the second adhesive layer and the second adhesive component of the second mixed layer are integrated, and the adhesive strength A of the first adhesive layer at 23°C and humidity 50% 11 Adhesion strength A of the first adhesive layer after heating at 200°C for 300 hours 12 The rate of change of (A 12 / A 11 ) is 0.40 or more, and the adhesive strength A of the second adhesive layer at 23°C and humidity of 50% 21 Adhesion strength A of the second adhesive layer after heating at 200°C for 300 hours 22 The rate of change of (A 22 / A 21 ) is 0.40 or more.
[0009] The first adhesive component and the second adhesive component are preferably fluororesin adhesive components.
[0010] a second adhesive layer formed on the first adhesive layer and a second adhesive layer in this order, the first adhesive layer comprising a first adhesive component which is a fluororesin-based adhesive component; the second adhesive layer comprising a second adhesive component which is a fluororesin-based adhesive component; the base layer comprising a nonwoven fabric sheet made of fluororesin fibers; the base layer comprising: a first mixed layer impregnated with the first adhesive component, the first mixed layer being provided in a range of 2% to 30% of the thickness of the base layer from the first adhesive layer side main surface of the base layer toward the second adhesive layer side main surface; a second mixed layer impregnated with the second adhesive component, the second mixed layer being provided in a range of 2% to 30% of the thickness of the base layer from the second adhesive layer side main surface of the base layer toward the first adhesive layer side main surface; and an air layer containing air, the first mixed layer being provided in a range of 40% to 96% of the thickness of the base layer from the first mixed layer toward the second mixed layer. The double-sided adhesive laminate sheet is characterized in that the porosity of the double-sided adhesive laminate sheet is 20% or more, the first adhesive component of the first adhesive layer and the first adhesive component of the first mixed layer are integrated, and the second adhesive component of the second adhesive layer and the second adhesive component of the second mixed layer are integrated.
[0011] The double-sided pressure-sensitive adhesive laminate sheet of the first embodiment and the double-sided pressure-sensitive adhesive laminate sheet of the second embodiment preferably have the following configurations. The thermal conductivity is preferably 0.20 W / (K·m) or less. The fluororesin fiber is preferably at least PTFE, PFA, or FEP. The thickness of the first pressure-sensitive adhesive layer or the thickness of the second pressure-sensitive adhesive layer is preferably equal to or less than the thickness of the base layer. The thickness of the base layer is preferably 20 μm to 1000 μm. The thickness of the first pressure-sensitive adhesive layer and the thickness of the second pressure-sensitive adhesive layer are preferably 5 μm to 500 μm.
[0012] According to the present invention, there is provided an adhesive laminated sheet having excellent heat insulation and heat resistance.
[0013] Fig. 1 is a schematic diagram of a double-sided pressure-sensitive adhesive laminate sheet, and Fig. 2 is a diagram summarizing the relationship between porosity and thermal conductivity in each example and each comparative example.
[0014] Hereinafter, when an upper limit value and a lower limit value are separately described, it is considered that a numerical range combining any upper limit value and any lower limit value is substantially disclosed.
[0015] In the following, unless otherwise specified, various measurements are carried out at room temperature (23° C.).
[0016] Hereinafter, a double-sided pressure-sensitive adhesive laminate sheet 10 according to the present invention will be described mainly with reference to FIG. 1, but the present invention is not limited thereto in any way.
[0017] <<<Structure of Double-Sided Adhesive Laminate Sheet 10>>> The double-sided adhesive laminate sheet 10 according to the present invention is a double-sided adhesive laminate sheet in which a first adhesive layer 1, a base layer A, and a second adhesive layer 2 are laminated in this order.
[0018] On the surface of the double-sided pressure-sensitive adhesive laminate sheet 10, another layer (for example, a protective film) may be laminated.
[0019] <<First Adhesive Layer 1>> The first adhesive layer 1 is made of a first adhesive component. In other words, the first adhesive layer 1 is composed of a first adhesive component.
[0020] The first adhesive component is preferably a heat-resistant adhesive component, in other words, the first adhesive layer 1 is preferably made of a first heat-resistant adhesive component.
[0021] In the present invention, the first adhesive component constituting the double-sided pressure-sensitive adhesive laminate sheet 10 "has heat resistance" means that in the double-sided pressure-sensitive adhesive laminate sheet 10, the adhesive strength A of the first adhesive layer 1 at 23°C and humidity of 50% is 11 Adhesion strength A of the first adhesive layer 1 after heating at 200°C for 300 hours 12 The rate of change of (A 12 / A 11 ) is 0.40 or more.
[0022] The resin that is the main component of the first adhesive component is not particularly limited. Examples of the first adhesive component include a fluororesin-based adhesive component or a silicone resin-based adhesive component. The first adhesive component is preferably a fluororesin-based adhesive component because it is compatible with the nonwoven fabric sheet made of fluororesin fibers. Examples of fluororesins that constitute the fluororesin-based adhesive component include copolymers containing fluoromonomers such as vinylidene fluoride, hexafluoropropylene, and tetrafluoroethylene.
[0023] Furthermore, if the adhesive component according to the present invention is a fluororesin-based adhesive component, it can be an adhesive component that does not contain a silicone resin-based adhesive component (silicone-free), which is preferable because it can reduce environmental pollution and product defects due to decomposition products.
[0024] The first adhesive component may contain other additives to the extent that the effects of the present invention are not impaired. Examples of other additives include fillers, antioxidants, heat stabilizers, light stabilizers, antistatic agents, flame retardants, plasticizers, tackifiers, pigments, etc. The content of the other additives in the first adhesive component is, for example, 10% by mass or less, 5% by mass or less, 1% by mass or less, etc., when the entire first adhesive component is taken as 100% by mass.
[0025] Thickness T of the first adhesive layer 1 1 is not particularly limited, and is preferably 5 μm to 500 μm, 7 μm to 250 μm, or 10 μm to 100 μm.
[0026] Overall thickness T of the double-sided adhesive laminated sheet 10 10 The thickness T of the first adhesive layer 1 1 The ratio (T 1 / T 10 ) is preferably 0.01 or more, 0.02 or more, or 0.05 or more, and is preferably 0.40 or less, 0.30 or less, or 0.25 or less.
[0027] <<Second Adhesive Layer 2>> The second adhesive layer 2 is made of a second adhesive component. In other words, the second adhesive layer 2 is composed of a second adhesive component.
[0028] The second adhesive component is preferably a heat-resistant adhesive component, in other words, the second adhesive layer 2 is preferably made of a second heat-resistant adhesive component.
[0029] In the present invention, the second adhesive component constituting the double-sided pressure-sensitive adhesive laminate sheet 10 "has heat resistance" means that in the double-sided pressure-sensitive adhesive laminate sheet 10, the adhesive strength A of the second adhesive layer 2 at 23°C and humidity of 50% is 21 Adhesion strength A of the second adhesive layer 2 after heating at 200°C for 300 hours 22 The rate of change of (A 22 / A 21 ) is 0.40 or more.
[0030] The second adhesive component can be the same as that described as the first adhesive component, and therefore a description thereof will be omitted.
[0031] Here, the second adhesive component constituting the second adhesive layer 2 and the first adhesive component constituting the first adhesive layer 1 may be the same component or different components, but it is preferable that both have adhesiveness and heat resistance.
[0032] The second adhesive component is preferably a fluororesin adhesive component because it is compatible with the nonwoven fabric sheet made of fluororesin fibers. It is more preferable that both the first adhesive component and the second adhesive component are fluororesin adhesive components.
[0033] Thickness T of the second adhesive layer 2 2 is not particularly limited, and is preferably 5 μm to 500 μm, 7 μm to 250 μm, or 10 μm to 100 μm.
[0034] Overall thickness T of the double-sided adhesive laminated sheet 10 10 The thickness T of the second adhesive layer 2 2 The ratio (T 2 / T 10 ) is preferably 0.01 or more, 0.02 or more, or 0.05 or more, and is preferably 0.40 or less, 0.30 or less, or 0.25 or less.
[0035] <<Base Material Layer A>> The base material layer A includes a nonwoven fabric sheet (not shown) made of fluororesin fibers, and has an area where the nonwoven fabric sheet is impregnated with an adhesive component and an area where the nonwoven fabric sheet is not impregnated with an adhesive component.
[0036] More specifically, in the thickness direction, the base material layer A has a first adhesive layer 1 side main surface S A1 (the main surface in contact with the first adhesive layer 1) to the main surface S A2 a first mixed layer A1 formed toward the second adhesive layer 2 side (the main surface in contact with the second adhesive layer 2) and impregnated with the first adhesive component; and a second adhesive layer 2 side main surface S A2 to the first adhesive layer 1 side main surface S A1 and a second mixed layer A2 which is a region impregnated with a second adhesive component and is formed toward the first mixed layer A1 and the second mixed layer A2, and an air layer A0 which contains air and is formed between the first mixed layer A1 and the second mixed layer A2 and from the first mixed layer A1 toward the second mixed layer A2.
[0037] In other words, the air layer A0 is a layer formed between the first mixed layer A1 and the second mixed layer A2 and made of a nonwoven fabric sheet containing air.
[0038] Here, the nonwoven fabric sheet constituting the substrate layer A is porous. When the porous nonwoven fabric sheet comes into contact with the paint or coating film, the adhesive component penetrates into the pores of the nonwoven fabric sheet, forming a mixed layer containing fibers and the adhesive component. Furthermore, the areas of the nonwoven fabric sheet that have not been penetrated by the adhesive component maintain the porous state inherent to the nonwoven fabric sheet, forming an air layer containing air. In this way, the substrate layer A includes a mixed layer and an air layer.
[0039] In the base layer A of the present invention, the first adhesive component constituting the first adhesive layer 1 and the first adhesive component constituting the first mixed layer A1 are integrated (continuous). Similarly, the second adhesive component constituting the second adhesive layer 2 and the second adhesive component constituting the second mixed layer A2 are integrated (continuous). In this way, by adopting a structure in which the first adhesive component of the first adhesive layer 1 and the first adhesive component of the first mixed layer A1 are integrated, and the second adhesive component of the second adhesive layer 2 and the second adhesive component of the second mixed layer A2 are integrated, it is possible to increase the adhesive strength between the adhesive layer and the base layer.
[0040] As the nonwoven fabric sheet constituting the base material layer A, a conventionally known one can be used.
[0041] The fluororesin fibers constituting the nonwoven fabric sheet are not particularly limited, and examples include fibers made from polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF), tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer (PFA), tetrafluoroethylene-hexafluoropropylene copolymer (FEP), etc. From the viewpoint of improving heat resistance, the fluororesin constituting the fluororesin fibers is preferably PTFE, PFA or FEP.
[0042] The fiber diameter and fiber length of the fluororesin fibers and the density of the nonwoven fabric sheet may be appropriately adjusted taking into consideration the porosity of the base layer A (or the porosity of the air layer A0), strength, ease of impregnation with the adhesive component, etc.
[0043] Thickness T of base material layer A A is not particularly limited, and is preferably 20 μm to 1000 μm, 50 μm to 800 μm, or 100 μm to 500 μm.
[0044] Here, the thickness T of the first adhesive layer 1 1 is the thickness T of the base layer A A Specifically, the thickness T of the base material layer A is preferably A The thickness T of the first adhesive layer 1 1 The thickness ratio (T 1 / T A) is preferably 1.00 or less, 0.90 or less, or 0.80 or less. 1 / T A The lower limit of the thickness T 2 is the thickness T of the base layer A A Specifically, the thickness T of the base material layer A is preferably A The thickness T of the second adhesive layer 2 2 The thickness ratio (T 2 / T A ) is preferably 1.00 or less, 0.90 or less, or 0.80 or less. 1 / T A The lower limit of ) is not particularly limited, but is, for example, 0.05, 0.08, or 0.10.
[0045] <Air Layer A0> The air layer A0 is a layer formed by a nonwoven fabric sheet, and air is held by the nonwoven fabric sheet. In other words, the air layer A0 usually contains air and a nonwoven fabric fiber sheet.
[0046] The air layer A0 is provided in a range of 40% to 96% of the thickness of the base material layer A. In other words, the thickness T A The thickness T of the air layer A0 A0 The proportion of ([T A0 / T A ] × 100) is 40% to 96%. A0 / T A ]×100 is preferably 50% or more, 60% or more, 70% or more, or 80% or more, and is preferably 95% or less, or 94% or less.
[0047] Thickness T of air layer A0 A0 is not particularly limited, but is preferably 10 μm to 500 μm, 50 μm to 500 μm, or 100 μm to 500 μm.
[0048] <First Mixed Layer A1> The nonwoven fabric sheet constituting the first mixed layer A1 is the same as the nonwoven fabric sheet constituting the air layer A0, and therefore a description thereof will be omitted.
[0049] Furthermore, the first adhesive component constituting the first mixed layer A1 is the same as the first adhesive component constituting the first adhesive layer 1, and therefore a description thereof will be omitted.
[0050] The first mixed layer A1 is provided in a range of 2% to 30% of the thickness of the base layer A. The upper limit is preferably 25% or less, 20% or less, 15% or less, or 10% or less. By setting the impregnation ratio of the first mixed layer A1 in such a range, it is easy to obtain an adhesive laminate sheet with an excellent balance of adhesive strength, heat insulation, etc.
[0051] Thickness T of the first mixed layer A1 A1 is not particularly limited, but is preferably 1 μm to 100 μm, 2 μm to 50 μm, or 5 μm to 20 μm.
[0052] <Second Mixed Layer A2> The nonwoven fabric sheet constituting the second mixed layer A2 is the same as the nonwoven fabric sheet constituting the air layer A0, and therefore a description thereof will be omitted.
[0053] Furthermore, the second adhesive component constituting the second mixed layer A2 is the same as the second adhesive component constituting the second adhesive layer 2, and therefore a description thereof will be omitted.
[0054] The second mixed layer A2 is provided in a range of 2% to 30% of the thickness of the base layer A. The upper limit is preferably 25% or less, 20% or less, 15% or less, or 10% or less. By setting the impregnation ratio of the second mixed layer A2 in such a range, it is easy to obtain an adhesive laminate sheet with an excellent balance of adhesive strength, heat insulation, etc.
[0055] Thickness T of the second mixed layer A2 A2 is not particularly limited, but is preferably 1 μm to 100 μm, 2 μm to 50 μm, or 5 μm to 20 μm.
[0056] <<<Physical Properties / Characteristics of Double-Sided Pressure-Sensitive Adhesive Laminate Sheet 10>>> <<Porosity>> The porosity of the double-sided pressure-sensitive adhesive laminate sheet 10 is 20% or more, and preferably 25% or more, or 30% or more. There are no particular limitations on the upper limit of the porosity of the double-sided pressure-sensitive adhesive laminate sheet 10, and it is preferably, for example, 60%, 70%, or 80%. Setting the porosity of the double-sided pressure-sensitive adhesive laminate sheet 10 within this range makes it easier to obtain a double-sided pressure-sensitive adhesive laminate sheet with excellent heat insulation properties.
[0057] The porosity of the double-sided adhesive laminate sheet 10 is calculated as ([volume of air layer A0] / [volume of double-sided adhesive laminate sheet 10]) × [volume % of air in air layer A0], or ([volume of air layer A0] × [volume % of air in air layer A0]) / [volume of adhesive laminate sheet 10].
[0058] The porosity of the double-sided pressure-sensitive adhesive laminated sheet 10 can be adjusted by the thickness of each layer, etc.
[0059] <<Thermal Conductivity>> The double-sided pressure-sensitive adhesive laminate sheet 10 preferably has a thermal conductivity of 0.20 W / (K·m) or less, 0.18 W / (K·m) or less, or 0.15 W / (K·m) or less. When the double-sided pressure-sensitive adhesive laminate sheet 10 satisfies this thermal conductivity, it is likely to exhibit sufficient functionality as a pressure-sensitive adhesive sheet having heat insulation properties.
[0060] The thermal conductivity (k) of the double-sided pressure-sensitive adhesive laminate sheet 10 is calculated by the transient method from the "thermal diffusivity," "density," and "specific heat" using the following formula. The thermal diffusivity is measured on a double-sided pressure-sensitive adhesive laminate sheet 10 cut into a 5 cm square using an ultra-high sensitivity thermal diffusivity analyzer for thin films (ai-Phase Mobile M3 Type 1, manufactured by Ai-Phase Corporation) in accordance with ISO 22007-3. The specific heat is measured on a double-sided pressure-sensitive adhesive laminate sheet 10 cut into a 5 cm square using a differential scanning calorimeter (DSC) (DSC6200, manufactured by Hitachi, Ltd.) in accordance with JIS K 7123. The density is calculated from the weight of the double-sided pressure-sensitive adhesive laminate sheet 10 cut into a 5 cm square measured using a balance and the volume value of the double-sided pressure-sensitive adhesive laminate sheet 10 calculated in the "porosity calculation" section above. k = αρC P (k: thermal conductivity [W / (m・K)], α: thermal diffusivity [m2 / s], ρ: density [kg / m 3 ], C P : specific heat (constant pressure specific heat) [J / (Kg K)])
[0061] <<Adhesive Strength>> The double-sided pressure-sensitive adhesive laminate sheet 10 preferably satisfies at least one of the following (1) or (2), and preferably satisfies both of the following (1) and (2): (1) Adhesive strength A of the first pressure-sensitive adhesive layer 1 at 23°C and a humidity (relative humidity) of 50% 11 Adhesion strength A of the first adhesive layer 1 after heating at 200°C for 300 hours 12 The rate of change of (A 12 / A 11 (2) The adhesive strength A of the second adhesive layer 2 at 23°C and a humidity (relative humidity) of 50% is 0.40 or more (more preferably, 0.60 or more, or 1.00 or more). 21 Adhesion strength A of the second adhesive layer 2 after heating at 200°C for 300 hours 22 The rate of change of (A 22 / A 21 ) is 0.40 or more (more preferably 0.60 or more, or 1.00 or more).
[0062] When the double-sided pressure-sensitive adhesive laminate sheet 10 satisfies such adhesive strength, it is likely to exhibit sufficient functionality as a heat-resistant pressure-sensitive adhesive sheet.
[0063] The adhesive strength of the double-sided pressure-sensitive adhesive laminate sheet 10 was evaluated by polishing the surface of an aluminum alloy (A5052) plate with sandpaper, and then laminating the adhesive layer of a double-sided pressure-sensitive adhesive laminate sheet 10 cut to a size of 5 cm x 5 mm to the polished surface with a hand roller. Measurements were performed on the evaluation objects, divided into two conditions: (1) immediately after lamination, and (2) after lamination, heated in an oven at 200°C for 300 hours, and then cooled at room temperature for 1 hour. The measurements were performed using a Tensilon universal testing machine (RTC-1210, manufactured by A&D Manufacturing) at a peel angle of 90° and a peel speed of 50 mm / min. Measurements were performed five times under each of the above conditions (1) and (2), and the average value was used to determine the adhesive strength.
[0064] Adhesion strength A of first adhesive layer 1 11 and adhesive strength A of the second adhesive layer 221 is not particularly limited, and is preferably 0.05 [N / 5 mm] or more, 0.1 [N / 5 mm] or more, or 0.2 [N / 5 mm] or more. 12 and adhesive strength A of the second adhesive layer 2 22 is not particularly limited, and is preferably 0.05 [N / 5mm] or more, 0.1 [N / 5mm] or more, 0.2 [N / 5mm] or more, 0.3 [N / 5mm] or more, or 0.5 [N / 5mm] or more.
[0065] <<<<Method for Manufacturing Double-Sided Pressure-Sensitive Adhesive Laminate Sheet 10 >>> The double-sided pressure-sensitive adhesive laminate sheet 10 can be manufactured according to a conventionally known method as long as the method is capable of maintaining the air layer A0 within the layer.
[0066] A double-sided adhesive laminate sheet 10 including a substrate layer A can be obtained by applying a predetermined adhesive paint (a composition containing an adhesive and a solvent) to a predetermined nonwoven fabric sheet, drying it, or by placing a previously prepared adhesive paint film adjacent to it and pressing it, and controlling the air layer derived from the nonwoven fabric sheet and the mixed layer, which is the area impregnated with the adhesive component, to form an appropriate shape. The double-sided adhesive laminate sheet 10 can be produced, for example, by the following method. An adhesive paint containing an adhesive that will be the first adhesive component and an appropriate solvent is applied to a release film (such as a PET film), and then the adhesive paint is dried to form a film provided with an adhesive layer made of the first adhesive component. The adhesive layer made of the first adhesive component provided on the release film and one main surface of the nonwoven fabric sheet (main surface S on the side of the first adhesive layer 1) are then applied to the release film. A1 ) are brought into contact with the nonwoven fabric sheet, and while applying pressure (and heat as needed), a pressure-sensitive adhesive layer made of the first pressure-sensitive adhesive component is pressed into the nonwoven fabric sheet, thereby impregnating a portion of the pressure-sensitive adhesive component into the nonwoven fabric sheet, thereby forming a first mixed layer A1. The portion of the pressure-sensitive adhesive layer that has not been impregnated into the nonwoven fabric sheet becomes the first pressure-sensitive adhesive layer 1. Similarly, the other main surface of the nonwoven fabric sheet (the main surface S on the side of the second pressure-sensitive adhesive layer 2) is pressed against the nonwoven fabric sheet. A2) and a pressure-sensitive adhesive layer made of a second pressure-sensitive adhesive component provided on a release film is brought into contact with the base layer A, and pressure (and heating as needed) is applied to partially impregnate the nonwoven fabric sheet with the pressure-sensitive adhesive component, thereby forming a second mixed layer A2 and a second pressure-sensitive adhesive layer 2. At this time, the pressing depth of each pressure-sensitive adhesive layer is adjusted to form an air layer A0, which is a region in the nonwoven fabric sheet between the first mixed layer A1 and the second mixed layer A2 where no pressure-sensitive adhesive component is present. The release film is removed as needed to obtain the double-sided pressure-sensitive adhesive laminate sheet 10. In this manufacturing method, because the nonwoven fabric sheet is pressurized, the thickness of the nonwoven fabric sheet at the raw material stage may differ from that of the nonwoven fabric sheet at the double-sided pressure-sensitive adhesive laminate sheet 10 stage. To achieve the desired thickness of the base layer A, the nonwoven fabric sheet may be compressed in advance, or a nonwoven fabric sheet with a thickness that takes into account deformation of the nonwoven fabric sheet may be used.
[0067] However, the method for manufacturing the double-sided pressure-sensitive adhesive laminate sheet 10 is not limited to this. For example, the method for manufacturing the double-sided pressure-sensitive adhesive laminate sheet 10 may be a method in which an undried pressure-sensitive adhesive coating is directly applied to a nonwoven fabric sheet, the pressure-sensitive adhesive coating is dried while adjusting the impregnation of the pressure-sensitive adhesive coating into the nonwoven fabric sheet so that an air layer remains within the layer of the double-sided pressure-sensitive adhesive laminate sheet 10, and the mixed layer and pressure-sensitive adhesive layer are formed.
[0068] <<<<Uses of Double-Sided Pressure-Sensitive Adhesive Laminate Sheet 10 >>> The double-sided pressure-sensitive adhesive laminate sheet 10 according to the present invention has a predetermined air layer, and therefore has excellent heat insulating properties and conformability, and can therefore be suitably used for various heat insulating or heat-resistant applications.
[0069] Next, the present invention will be explained in more detail with reference to examples and comparative examples, but the present invention is not limited to these examples in any way.
[0070] <<Preparation of Double-Sided Pressure-Sensitive Adhesive Laminate Sheet>> A double-sided pressure-sensitive adhesive laminate sheet was prepared as follows: The measurement methods used in this preparation are as follows.
[0071] <Measurement of Adhesive Layer Thickness> The thickness of the adhesive layer was measured using a micrometer (MDH-25MC, manufactured by Mitutoyo Corporation) and the average value was calculated by measuring five points at each of the four corners of the main surface of a 5 cm square cut adhesive layer.
[0072] <Adhesive Strength Measurement of Adhesive Layer> The adhesive strength of the adhesive layer was measured by polishing the surface of an aluminum alloy (A5052) aluminum plate with sandpaper in advance, and then peeling off one PET film from a double-sided PET film-attached adhesive layer cut to a size of 5 cm x 5 mm, and laminating the exposed adhesive layer surface to the polished surface with a hand roller. Measurements were performed using a Tensilon universal testing machine (RTC-1210, manufactured by A&D Manufacturing) at a peel angle of 90° and a peel speed of 50 mm / min. The measurement was performed a total of five times, and the average value was taken as the adhesive strength.
[0073] Example 1 Coating 1 was prepared by dispersing a copolymer resin composed of TFE and propylene in tetrahydrofuran (THF) to a concentration of 20 wt %. Subsequently, Coating 1 was applied to the treated surface of a 38 μm-thick release PET film 1 using an applicator, and then dried at 90°C for 3 minutes to obtain a single-sided PET film-attached composition 1. Furthermore, the treated surface of a release PET film 2, which has a lighter release property than release PET film 1, was laminated to the composition 1 side of single-sided PET film-attached composition 1 using a laminator at room temperature and 0.1 MPa to obtain a double-sided PET film-attached adhesive layer 1. The adhesive layer 1 had a thickness of 25 μm and an adhesive strength of 0.1 N / 5 mm. The double-sided PET film-attached adhesive layer 1 was cut into a total of two sheets (hereinafter, the first double-sided PET film-attached adhesive layer 1 is referred to as double-sided PET film-attached adhesive layer 1a, and its adhesive layer 1 is referred to as adhesive layer 1a, and the second double-sided PET film-attached adhesive layer 1 is referred to as double-sided PET film-attached adhesive layer 1b, and its adhesive layer 1 is referred to as adhesive layer 1b). Then, the release PET film 2 from the first double-sided PET film-attached adhesive layer 1a was peeled off to expose the adhesive layer 1a surface, and then one side of a nonwoven fabric sheet (Tomyfirec F, manufactured by Tomoegawa Paper Co., Ltd.) composed of fluororesin fiber as a substrate was thermally laminated to the exposed adhesive layer 1a surface using a laminator under conditions of 120°C and 0.3 MPa, thereby obtaining a single-sided adhesive laminate sheet 1 with a single PET film attached on one side, in which the adhesive of adhesive layer 1a was partially impregnated from one side into the nonwoven fabric sheet. Next, the release PET film 2 of the second double-sided PET film-attached adhesive layer 1b was peeled off to expose the adhesive layer 1b surface, and then the other surface of the nonwoven fabric sheet of the single-sided adhesive laminate sheet 1 with a PET film on one side was thermally laminated to the exposed adhesive layer 1b surface using a laminator at 120°C and 0.3 MPa, thereby obtaining a double-sided adhesive laminate sheet 1 with a PET film on both sides, in which some of the adhesive of the adhesive layer 1b had impregnated into the interior from the other surface of the nonwoven fabric sheet of the single-sided adhesive laminate sheet 1 with a PET film on one side.
[0074] Example 2 Two double-sided PET film-attached adhesive layers 1 were prepared as in Example 1. Subsequently, the release PET films 2 were peeled off from each of the two double-sided PET film-attached adhesive layers 1 to expose the adhesive layer 1 surface. The two exposed adhesive layer 1 surfaces were then laminated together using a laminator at room temperature and 0.1 MPa to obtain a double-sided PET film-attached adhesive layer 2. The adhesive layer 2 had a thickness of 50 μm. The double-sided PET film-attached adhesive layer 2 was cut into a total of two sheets (hereinafter, the first double-sided PET film-attached adhesive layer 2 will be referred to as double-sided PET film-attached adhesive layer 2a, and the adhesive layer 2 will be referred to as adhesive layer 2a; the second double-sided PET film-attached adhesive layer 2 will be referred to as double-sided PET film-attached adhesive layer 2b, and the adhesive layer 2 will be referred to as adhesive layer 2b). Then, one of the release PET films 1 of the first double-sided PET film-attached adhesive layer 2a was peeled off to expose the adhesive layer 2a surface, and then one side of a nonwoven fabric sheet (Tommy Firec F, manufactured by Tomoegawa Paper Co., Ltd.) made of fluororesin fiber as a substrate was thermally laminated to the exposed adhesive layer 2a surface using a laminator at 120°C and 0.3 MPa, thereby obtaining a single-sided adhesive laminate sheet 2 with a PET film on one side, in which part of the adhesive of the adhesive layer 2a has impregnated into the interior from one side of the nonwoven fabric sheet. Next, one of the release PET films 1 of the second double-sided PET film-attached adhesive layer 2b was peeled off to expose the adhesive layer 2b surface, and then the other surface of the nonwoven fabric sheet of the single-sided adhesive laminate sheet 2 with a PET film on one side was thermally laminated to the exposed adhesive layer 2b surface using a laminator at 120°C and 0.3 MPa, thereby obtaining a double-sided adhesive laminate sheet 2 with a PET film on both sides, in which some of the adhesive of the adhesive layer 2b had impregnated into the interior from the other surface of the nonwoven fabric sheet of the single-sided adhesive laminate sheet 2 with a PET film on one side.
[0075] Example 3: Double-sided PET film-attached adhesive layer 1 prepared in Example 1 and double-sided PET film-attached adhesive layer 2 prepared in Example 2 were prepared. Subsequently, release PET film 2 of the prepared double-sided PET film-attached adhesive layer 1 and release PET film 1 of the double-sided PET film-attached adhesive layer 2 were peeled off to expose the adhesive layer 1 and adhesive layer 2 surfaces. The two exposed adhesive layer surfaces were then laminated together using a laminator at room temperature and 0.1 MPa to obtain double-sided PET film-attached adhesive layer 3. The thickness of adhesive layer 3 was 75 μm. The double-sided PET film-attached adhesive layer 3 was cut into a total of two sheets (hereinafter, the first double-sided PET film-attached adhesive layer 3 will be referred to as double-sided PET film-attached adhesive layer 3a, and the second double-sided PET film-attached adhesive layer 3 will be referred to as double-sided PET film-attached adhesive layer 3b, and the second double-sided PET film-attached adhesive layer 3 will be referred to as double-sided PET film-attached adhesive layer 3b). Then, one of the release PET films 1 of the first double-sided PET film-attached adhesive layer 3a was peeled off to expose the adhesive layer 3a surface, and then one side of a nonwoven fabric sheet (Tommy Firec F, manufactured by Tomoegawa Paper Co., Ltd.) made of fluororesin fiber as a substrate was thermally laminated to the exposed adhesive layer 3a surface using a laminator at 120°C and 0.3 MPa, thereby obtaining a single-sided adhesive laminate sheet 3 with a PET film on one side, in which part of the adhesive of the adhesive layer 3a has impregnated into the interior from one side of the nonwoven fabric sheet. Next, one of the release PET films 1 of the second double-sided PET film-attached adhesive layer 3b was peeled off to expose the adhesive layer 3b surface, and then the other surface of the nonwoven fabric sheet of the single-sided adhesive laminate sheet 3 with a PET film on one side was thermally laminated to the exposed adhesive layer 3b surface using a laminator at 120°C and 0.3 MPa, thereby obtaining a double-sided adhesive laminate sheet 3 with a PET film on both sides in which some of the adhesive of the adhesive layer 3b had impregnated into the interior from the other surface of the nonwoven fabric sheet of the single-sided adhesive laminate sheet 3 with a PET film on one side.
[0076] Example 4 Two double-sided PET film-attached adhesive layers 2 were prepared as in Example 2. Subsequently, the release PET films 1 were peeled off from each of the two double-sided PET film-attached adhesive layers 2 to expose the adhesive layer 2 surfaces. The two exposed adhesive layer 2 surfaces were then laminated together using a laminator at room temperature and 0.1 MPa to obtain a double-sided PET film-attached adhesive layer 4. The adhesive layer 4 had a thickness of 100 μm. A total of two double-sided PET film-attached adhesive layers 4 were cut (hereinafter, the first double-sided PET film-attached adhesive layer 4 will be referred to as double-sided PET film-attached adhesive layer 4a, and its adhesive layer 4 will be referred to as adhesive layer 4a; the second double-sided PET film-attached adhesive layer 4 will be referred to as double-sided PET film-attached adhesive layer 4b, and its adhesive layer 4 will be referred to as adhesive layer 4b). Then, one of the release PET films 1 of the first double-sided PET film-attached adhesive layer 4a was peeled off to expose the adhesive layer 4a surface, and then one side of a nonwoven fabric sheet (Tommy Firec F, manufactured by Tomoegawa Paper Co., Ltd.) made of fluororesin fiber as a substrate was thermally laminated to the exposed adhesive layer 4a surface using a laminator at 120°C and 0.3 MPa, thereby obtaining a single-sided adhesive laminate sheet 4 with a PET film on one side, in which part of the adhesive of the adhesive layer 4a has impregnated into the interior from one side of the nonwoven fabric sheet. Next, one of the release PET films 1 of the second double-sided PET film-attached adhesive layer 4b was peeled off to expose the adhesive layer 4b surface, and then the other surface of the nonwoven fabric sheet of the single-sided adhesive laminate sheet 4 with a PET film on one side was thermally laminated to the exposed adhesive layer 4b surface using a laminator at 120°C and 0.3 MPa, thereby obtaining a double-sided adhesive laminate sheet 4 with a PET film on both sides in which some of the adhesive of the adhesive layer 4b had impregnated into the interior from the other surface of the nonwoven fabric sheet of the single-sided adhesive laminate sheet 4 with a PET film on one side.
[0077] Comparative Example 1: The double-sided PET film-attached adhesive layer 2 prepared in Example 2 and the double-sided PET film-attached adhesive layer 4 prepared in Example 4 were prepared. Subsequently, the release PET film 1 was peeled off from each of the prepared double-sided PET film-attached adhesive layer 2 and double-sided PET film-attached adhesive layer 4 to expose the adhesive layer 2 and adhesive layer 4 surfaces. The two exposed adhesive layer surfaces were then laminated together using a laminator at room temperature and 0.1 MPa to obtain a double-sided PET film-attached adhesive layer 5. The adhesive layer 5 had a thickness of 150 μm. The double-sided PET film-attached adhesive layer 5 was cut into a total of two sheets (hereinafter, the first double-sided PET film-attached adhesive layer 5 will be referred to as double-sided PET film-attached adhesive layer 5a, and its adhesive layer 5 will be referred to as adhesive layer 5a; the second double-sided PET film-attached adhesive layer 5 will be referred to as double-sided PET film-attached adhesive layer 5b, and its adhesive layer 5 will be referred to as adhesive layer 5b). Then, one of the release PET films 1 of the first double-sided PET film-attached adhesive layer 5a was peeled off to expose the adhesive layer 5a surface, and then one side of a nonwoven fabric sheet (Tommy Firec F, manufactured by Tomoegawa Paper Co., Ltd.) made of fluororesin fiber as a substrate was thermally laminated to the exposed adhesive layer 5a surface using a laminator at 120°C and 0.3 MPa, thereby obtaining a single-sided adhesive laminate sheet 5 with a PET film on one side, in which part of the adhesive of the adhesive layer 5a has impregnated into the interior from one side of the nonwoven fabric sheet. Next, one of the release PET films 1 of the second double-sided PET film-attached adhesive layer 5b was peeled off to expose the adhesive layer 5b surface, and then the other surface of the nonwoven fabric sheet of the single-sided adhesive laminate sheet 5 with a PET film on one side was thermally laminated to the exposed adhesive layer 5b surface using a laminator at 120°C and 0.3 MPa, thereby obtaining a double-sided adhesive laminate sheet 5 with a double-sided PET film in which part of the adhesive of the adhesive layer 5b had impregnated into the interior from the other surface of the nonwoven fabric sheet of the single-sided adhesive laminate sheet 5 with a PET film on one side.
[0078] Comparative Example 2 A copolymer resin composed of EA, 2EHA, and 2HEA was dispersed in ethyl acetate to a concentration of 30 wt %, to prepare Coating 2. Subsequently, Coating 2 was applied to the treated surface of a 38 μm-thick release PET film 1 using an applicator, and then dried at 90°C for 3 minutes to obtain Single-sided PET film-attached Composition 2. Furthermore, the treated surface of Release PET film 2, which has a lighter release property than Release PET film 1, was laminated to the Composition 2 side of Single-sided PET film-attached Composition 2 using a laminator at room temperature and 0.1 MPa to obtain Double-sided PET film-attached Adhesive Layer 6. The Adhesive Layer 6 had a thickness of 25 μm and an adhesive strength of 2.0 N / 5 mm. The double-sided PET film-attached adhesive layer 6 was cut into two sheets in total (hereinafter, the first double-sided PET film-attached adhesive layer 6 is referred to as double-sided PET film-attached adhesive layer 6a, and its adhesive layer 6 is referred to as adhesive layer 6a, and the second double-sided PET film-attached adhesive layer 6 is referred to as double-sided PET film-attached adhesive layer 6b, and its adhesive layer 6 is referred to as adhesive layer 6b). Then, the release PET film 2 of the first double-sided PET film-attached adhesive layer 6a was peeled off to expose the adhesive layer 6a surface, and then one side of a nonwoven fabric sheet (Tomyfirec F, manufactured by Tomoegawa Paper Co., Ltd.) composed of fluororesin fiber as a substrate was thermally laminated to the exposed adhesive layer 6a surface using a laminator under conditions of 120°C and 0.3 MPa, thereby obtaining a single-sided adhesive laminate sheet 6 with a PET film on one side, in which the adhesive of the adhesive layer 6a was partially impregnated from one side of the nonwoven fabric sheet to the interior. Next, the release PET film 2 of the second double-sided PET film-attached adhesive layer 6b was peeled off to expose the adhesive layer 6b surface, and then the other surface of the nonwoven fabric sheet of the single-sided adhesive laminate sheet 6 with a PET film on one side was thermally laminated to the exposed adhesive layer 6b surface using a laminator at 120°C and 0.3 MPa, thereby obtaining a double-sided adhesive laminate sheet 6 with a PET film on both sides, in which some of the adhesive of the adhesive layer 6b had impregnated into the interior from the other surface of the nonwoven fabric sheet of the single-sided adhesive laminate sheet 6 with a PET film on one side.
[0079] Comparative Example 3 A resin composed of a styrene copolymer, an aromatic hydrocarbon resin, and a polyolefin resin was dispersed in toluene to a concentration of 30 wt %, to prepare Coating 3. Subsequently, Coating 3 was applied to the treated surface of a 38 μm-thick release PET film 1 using an applicator, and then dried at 90°C for 3 minutes to obtain Single-Sided PET Film Composition 3. Furthermore, the treated surface of Release PET Film 2, which has a lighter release property than Release PET Film 1, was laminated to the Composition 3 surface of Single-Sided PET Film Composition 3 using a laminator at room temperature and 0.1 MPa to obtain Double-Sided PET Film-Attached Adhesive Layer 7. The thickness of Adhesive Layer 7 was 27 μm, and the adhesive strength was 0.9 N / 5 mm. The double-sided PET film-attached adhesive layer 7 was cut into two sheets in total (hereinafter, the first double-sided PET film-attached adhesive layer 7 is referred to as double-sided PET film-attached adhesive layer 7a, and its adhesive layer 7 is referred to as adhesive layer 7a, and the second double-sided PET film-attached adhesive layer 7 is referred to as double-sided PET film-attached adhesive layer 7b, and its adhesive layer 7 is referred to as adhesive layer 7b). Then, the release PET film 2 from the first double-sided PET film-attached adhesive layer 7a was peeled off to expose the adhesive layer 7a surface, and then one side of a nonwoven fabric sheet (Tomyfirec F, manufactured by Tomoegawa Paper Co., Ltd.) composed of fluororesin fiber as a substrate was thermally laminated to the exposed adhesive layer 7a surface using a laminator under conditions of 120°C and 0.3 MPa, thereby obtaining a single-sided adhesive laminate sheet 7 with a PET film on one side, in which the adhesive of adhesive layer 7a was partially impregnated from one side of the nonwoven fabric sheet to the interior. Next, the release PET film 2 of the second double-sided PET film-attached adhesive layer 7b was peeled off to expose the adhesive layer 7b surface, and then the other side of the nonwoven fabric sheet of the single-sided adhesive laminate sheet 7 with a PET film on one side was thermally laminated to the exposed adhesive layer 7b surface using a laminator at 120°C and 0.3 MPa, thereby obtaining a double-sided adhesive laminate sheet 7 with a PET film on both sides, in which some of the adhesive of the adhesive layer 7b had impregnated into the interior from the other side of the nonwoven fabric sheet of the single-sided adhesive laminate sheet 7 with a PET film on one side.
[0080] <Examples 5 and 6, Comparative Examples 4 to 7> Double-sided PET film-attached double-sided adhesive laminate sheets 4 according to Examples 5 and 6 and Comparative Examples 4 to 7 were obtained in the same manner as in Example 1, except that the thickness of the air layer, the thickness of the adhesive layer, the volume ratio of the mixed layer, the total thickness, and the porosity were changed as shown in Table 1.
[0081] <<Measurements and Calculations of Double-Sided PSA Laminate Sheets>> The following measurements and calculations were carried out on each of the double-sided PSA laminate sheets with PET films on both sides obtained above in Examples 1 to 4 and Comparative Examples 1 to 3. The results obtained are shown in Table 1. A graph of thermal conductivity versus porosity is shown in Figure 2.
[0082] <Thickness Measurement> Each double-sided adhesive laminate sheet with a double-sided PET film cut into a 5 cm square was cut perpendicular to the main surface to expose the cross section of each double-sided adhesive laminate sheet with a double-sided PET film. A microscope (VHX-8000, manufactured by Keyence Corporation) was used to measure the overall thickness of each double-sided adhesive laminate sheet and the thicknesses of the "two adhesive layers (hereinafter referred to as adhesive layer A and adhesive layer B)," "air layer," and "two mixed layers (hereinafter referred to as mixed layer A and mixed layer B)" therein by image analysis. Each thickness was measured at 20 random locations in the width direction (direction perpendicular to the perpendicular direction) of the exposed cross section of the double-sided adhesive laminate sheet with a double-sided PET film, and the average value was calculated.
[0083] <Calculation of Void Ratio> The void ratio was calculated as the proportion of air in the volume of the air layer relative to the volume of the double-sided pressure-sensitive adhesive laminate sheet. To calculate the volume of the air layer, first, the void ratio of the substrate (nonwoven fabric sheet) was calculated using the following formula. The apparent density of the substrate was measured using a geometric measurement method in accordance with JIS Z 8807. Substrate void ratio (%) = (1 - (apparent density of substrate / true density of substrate fiber material)) x 100. The substrate void ratio was calculated using the above formula, and the volume of air in the air layer was calculated by multiplying this substrate void ratio by the apparent volume of the air layer calculated using the thickness of the air layer in the above "thickness measurement." Next, the volume of the double-sided pressure-sensitive adhesive laminate sheet was calculated using the thickness of the double-sided pressure-sensitive adhesive laminate sheet in the above "thickness measurement." The proportion of the volume of air in the air layer relative to the volume of the double-sided pressure-sensitive adhesive laminate sheet obtained from the above was calculated as the void ratio.
[0084] <Calculation of Thermal Conductivity> The thermal conductivity (k) was calculated by the transient method from "thermal diffusivity," "density," and "specific heat" using the following formula. The "thermal diffusivity" and "specific heat" were values measured by the methods described below. The "density" was calculated from the weight of a double-sided pressure-sensitive adhesive laminate sheet cut into a 5 cm square measured on a balance and the volume value of the double-sided pressure-sensitive adhesive laminate sheet calculated in the "void ratio calculation" above. k = αρC P (k: thermal conductivity [W / (m・K)], α: thermal diffusivity [m 2 / s], ρ: density [kg / m 3 ], C P : specific heat (constant pressure specific heat) [J / (Kg K)])
[0085] <Thermal Diffusivity Measurement> The thermal diffusivity measurement was carried out on a double-sided pressure-sensitive adhesive laminated sheet cut into a 5 cm square using an ultra-high sensitivity thermal diffusivity measuring device for thin films (ai-Phase Mobile M3 Type 1, manufactured by ai-Phase Corporation) in accordance with ISO 22007-3.
[0086] <Specific Heat Measurement> Specific heat measurement was carried out on a double-sided pressure-sensitive adhesive laminate sheet cut into a 5 cm square using a differential scanning calorimeter (DSC) (DSC6200, manufactured by Hitachi, Ltd.) in accordance with JIS K 7123.
[0087] <Adhesive Strength Measurement> The adhesive strength of the double-sided PSA laminate sheet was measured using an aluminum alloy (A5052) plate whose surface was previously polished with sandpaper. A 5 cm x 5 mm double-sided PSA laminate sheet with a double-sided PET film was cut into pieces and the exposed adhesive layer was then bonded to the polished surface with a hand roller. The test specimens were divided into two conditions: (1) immediately after lamination, and (2) after lamination, heated in an oven at 200°C for 300 hours, and then cooled at room temperature for 1 hour. Measurements were performed using a Tensilon universal testing machine (RTC-1210, manufactured by A&D Manufacturing) at a peel angle of 90° and a peel speed of 50 mm / min. Measurements were performed five times under each of the above conditions (1) and (2), and the average value was used as the adhesive strength.
[0088] Table 1 shows the evaluation results of adhesive strength (at room temperature, after test) for only one side of each double-sided pressure-sensitive adhesive laminate sheet, but the same values are obtained for the other side.
[0089]
[0090] As described above, from this example, an adhesive laminated sheet having excellent heat insulation properties (for example, thermal conductivity of 0.20 W / (K·m) or less) and heat resistance could be obtained.
[0091] 10 adhesive laminated sheet 1, 2 adhesive layer A substrate layer A0 air layer A1, A2 mixed layer
Claims
1. A double-sided adhesive laminate sheet having a first adhesive layer, a base layer, and a second adhesive layer laminated in this order, wherein the first adhesive layer is made of a first adhesive component, the second adhesive layer is made of a second adhesive component, the base layer includes a nonwoven fabric sheet made of fluororesin fibers, the base layer includes: a first mixed layer impregnated with the first adhesive component, the first mixed layer being provided in a range of 2% to 30% of the thickness of the base layer from the first adhesive layer side main surface of the base layer toward the second adhesive layer side main surface, a second mixed layer impregnated with the second adhesive component, the second mixed layer being provided in a range of 2% to 30% of the thickness of the base layer from the second adhesive layer side main surface of the base layer toward the first adhesive layer side main surface, and an air layer including air being provided in a range of 40% to 96% of the thickness of the base layer from the first mixed layer toward the second mixed layer, the double-sided adhesive laminate sheet having a porosity of 20% or more, the first adhesive component of the first adhesive layer and the first adhesive component of the first mixed layer are integrated, and the second adhesive component of the second adhesive layer and the second adhesive component of the second mixed layer are integrated, and the adhesive strength A of the first adhesive layer at 23° C. and humidity 50% 11 Adhesive strength A of the first adhesive layer after heating at 200° C. for 300 hours 12 The rate of change of (A 12 / A 11 ) is 0.40 or more, and the adhesive strength A of the second adhesive layer at 23° C. and a humidity of 50% is 21 Adhesive strength A of the second adhesive layer after heating at 200° C. for 300 hours 22 The rate of change of (A 22 / A 21 ) is 0.40 or more.
2. The double-sided adhesive laminate sheet according to claim 1, wherein the first adhesive component and the second adhesive component are fluororesin-based adhesive components.
3. A double-sided adhesive laminated sheet having a first adhesive layer, a base layer, and a second adhesive layer laminated in this order, wherein the first adhesive layer is made of a first adhesive component which is a fluororesin-based adhesive component, the second adhesive layer is made of a second adhesive component which is a fluororesin-based adhesive component, and the base layer includes a nonwoven fabric sheet made of fluororesin fibers, the base layer including: a first mixed layer impregnated with the first adhesive component, the first mixed layer being provided in a range of 2% to 30% of the thickness of the base layer from the first adhesive layer side main surface of the base layer toward the second adhesive layer side main surface, a second mixed layer impregnated with the second adhesive component, the second mixed layer being provided in a range of 2% to 30% of the thickness of the base layer from the second adhesive layer side main surface of the base layer toward the first adhesive layer side main surface, and an air layer including air, the first mixed layer being provided in a range of 40% to 96% of the thickness of the base layer from the first mixed layer toward the second mixed layer, A double-sided adhesive laminate sheet, characterized in that the double-sided adhesive laminate sheet has a porosity of 20% or more, the first adhesive component of the first adhesive layer and the first adhesive component of the first mixed layer are integrated, and the second adhesive component of the second adhesive layer and the second adhesive component of the second mixed layer are integrated.
4. The double-sided pressure-sensitive adhesive laminate sheet according to any one of claims 1 to 3, characterized in that it has a thermal conductivity of 0.20 W / (K·m) or less.
5. The double-sided adhesive laminate sheet according to any one of claims 1 to 3, characterized in that the fluororesin fiber is at least PTFE, PFA or FEP.
6. A double-sided adhesive laminate sheet described in any one of claims 1 to 3, characterized in that the thickness of the first adhesive layer or the thickness of the second adhesive layer is less than the thickness of the base layer.
7. The double-sided adhesive laminate sheet according to any one of claims 1 to 3, characterized in that the thickness of the base layer is 20 µm to 1000 µm.
8. A double-sided adhesive laminate sheet according to any one of claims 1 to 3, characterized in that the thickness of the first adhesive layer and the thickness of the second adhesive layer are each 5 μm to 500 μm.
Citation Information
Patent Citations
Double-coated self-adhesive tape for fixing building interior material
JP1995138539A
Double-sided pressure-sensitive adhesive tape
JP2005187539A
Method for producing fluorine-based hollow fiber
JP2010047859A
Polyimide resin composition and adhesive sheet
JP2016132736A
Sheet-like heater
WO2020170888A1