Epoxy resin composition, prepreg, and fiber-reinforced composite material
The epoxy resin composition balances heat resistance and recyclability by using specific components, allowing for high heat resistance and efficient fiber recovery, addressing the trade-off in existing technologies.
Patent Information
- Application Number
- PCT/JP2024/012229
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-28
- Filing Date
- 2024-03-27
- Publication Date
- 2024-10-03
AI Technical Summary
Existing epoxy resin compositions for fiber-reinforced composite materials face a trade-off between heat resistance and recyclability, where high crosslinking density improves heat resistance but complicates decomposition, making it difficult to recover reinforcing fibers.
An epoxy resin composition comprising specific components such as bifunctional epoxy resins, aromatic diamines, and trifunctional or tetrafunctional epoxy resins, which balance depolymerizability and heat resistance by controlling the glass transition temperature and crosslinking density, allowing for both high heat resistance and recyclability.
The composition achieves sufficient heat resistance while maintaining excellent recyclability, enabling the recovery of reinforcing fibers and reducing environmental impact through efficient depolymerization processes.
Smart Images

Figure JP2024012229_03102024_PF_FP_ABST
Abstract
Description
Epoxy resin composition, prepreg and fiber-reinforced composite material
[0001] The present invention relates to an epoxy resin composition having excellent recyclability, and to a prepreg and a fiber-reinforced composite material using the same as a matrix resin.
[0002] Epoxy resins are suitable for use as matrix resins in fiber-reinforced composite materials that are combined with reinforcing fibers such as carbon fibers, glass fibers, and aramid fibers, taking advantage of their high strength, rigidity, heat resistance, and adhesiveness.
[0003] Fiber-reinforced composite materials are generally manufactured using sheet-like intermediate substrates (prepregs) made of reinforcing fibers impregnated with epoxy resin. After laminating the prepregs, molded products are obtained by heating the laminate to harden the epoxy resin. Because a wide range of properties can be achieved by varying the laminate design of the prepregs, they are used in a variety of fields, including aircraft, automobiles, sports, and medicine.
[0004] In recent years, the applications of fiber-reinforced composite materials have been rapidly expanding, and there is a demand for epoxy resin compositions and fiber-reinforced composite materials that are carbon-neutral and have excellent recyclability in addition to heat resistance and rigidity. As a matrix resin for such thermomechanically re-deformable fiber-reinforced composite materials, an epoxy resin composition using 4,4'-diaminodiphenyl disulfide as a curing agent is known (Patent Document 1).
[0005] International Publication No. 2015 / 181054
[0006] The epoxy resin composition described in Patent Document 1 cannot depolymerize the cured product of the epoxy resin composition with an organic solvent after curing the fiber-reinforced composite material, and therefore the reinforcing fibers cannot be recovered from the fiber-reinforced composite material, resulting in poor recyclability.
[0007] To improve heat resistance, it is necessary to increase the crosslink density. However, a high crosslink density leads to a complex network, which makes the resin difficult to decompose and makes depolymerization by chemical treatment impossible. Therefore, the present invention aims to overcome the trade-off between depolymerization and heat resistance in the prior art and to provide an epoxy resin composition that has sufficient heat resistance while also having excellent recyclability. Furthermore, the present invention aims to provide prepregs and fiber-reinforced composite materials with excellent recyclability by using the epoxy resin composition as a matrix resin.
[0008] The epoxy resin composition according to the present invention has the following configuration: 1. An epoxy resin composition comprising the following components [A], [B], and [C], wherein the epoxy resin of component [B] is contained in an amount of 10 to 30 parts by mass per 100 parts by mass of the total epoxy resin.
[0009] [A]: a bifunctional epoxy resin that is liquid at 23°C; [B]: an epoxy resin having an average epoxy equivalent of 400 to 1200 and a structure of formula (I) described below, or an epoxy resin having an average epoxy equivalent of 150 to 500 and a structure of formula (II) described below; [C]: an aromatic diamine having a structure of formula (III) described below. 2. The epoxy resin composition according to above 1, wherein component [A] is a bisphenol-type epoxy resin having an average epoxy equivalent of 160 to 200. 3. The epoxy resin composition according to above 1 or 2, wherein component [B] has the structure of formula (I), and the epoxy resin composition is a bisphenol F-type epoxy resin having an average epoxy equivalent of 800 to 1200. 4. The epoxy resin composition according to any of above 1 to 3, wherein component [C] is an aromatic diamine having a structure of formula (IV) described below, or an aromatic diamine having the structure of formula (IV) or a structural isomer thereof. 5. 5. The epoxy resin composition according to any one of the above 1 to 4, wherein the glass transition temperature of the cured product after curing at 150°C to 220°C for 120 minutes is 110°C or higher. 6. The epoxy resin composition according to any one of the above 1 to 5, further comprising, as component [D], a trifunctional or tetrafunctional epoxy resin in an amount of 5 to 30 parts by mass per 100 parts by mass of the total epoxy resin. 7. The epoxy resin composition according to any one of the above 1 to 6, further comprising, as component [E], a difunctional naphthalene-type epoxy resin.
[0010] The prepreg according to the present invention comprises the above epoxy resin composition and reinforcing fibers. The fiber-reinforced composite material according to the present invention is obtained by curing the above prepreg.
[0011] According to the present invention, an epoxy resin composition having excellent recyclability and sufficient heat resistance can be obtained.
[0012] The epoxy resin composition of the present invention contains the following components [A], [B], and [C] in specific ratios as described below: Component [A]: a bifunctional epoxy resin that is liquid at 23°C, Component [B]: an epoxy resin having an average epoxy equivalent of 400 to 1200 and a structure represented by formula (I) as described below, or an epoxy resin having an average epoxy equivalent of 150 to 500 and a structure represented by formula (II), and Component [C]: an aromatic diamine having a structure represented by formula (III). Each of the components is described below.
[0013] (Component [A]) Component [A] used in the present invention is a difunctional epoxy resin that is liquid at 23°C. Here, n-functional epoxy refers to a resin having n epoxy groups per molecule of the main component (structural isomers, such as optical isomers and 2,2'- and 2,4'-isomers, which differ only in the substitution position of the epoxy group on the benzene ring or naphthalene ring, are considered to be the same species), and difunctional epoxy resin refers to an epoxy resin having two epoxy groups per molecule. Liquid means that the viscosity is 25,000 mPa·s or less at 23°C. Being liquid, it can be melt-mixed with component [B] and kneaded with component [C] to obtain a resin composition with so-called latent curability, in which the curing reaction does not proceed between 23°C and 80°C, but proceeds above 80°C. Component [A] preferably has a viscosity of 15,000 mPa·s or less at 23°C, and more preferably 7,000 mPa·s or less. By setting the viscosity to 15,000 mPa·s or less, it is possible to impregnate reinforcing fibers with the resin composition to produce a sheet-like prepreg, and by setting the viscosity to 7,000 mPa·s or less, it is possible to mold a fiber-reinforced composite material using the filament winding method or resin transfer molding method. Component [A] is preferably contained in an amount of 5 to 80 parts by mass, and more preferably 50 to 70 parts by mass, per 100 parts by mass of the total epoxy resin. By setting the amount of component [A] to 50 to 70 parts by mass per 100 parts by mass of the total epoxy resin, an epoxy resin composition can be obtained that exhibits an excellent balance between the depolymerization property and heat resistance of the cured product. (Hereinafter, the depolymerizability of the cured product may be simply referred to as depolymerizability.) Examples of the epoxy resin of component [A] include bisphenol-type epoxy resins such as bisphenol A-type epoxy resins, bisphenol F-type epoxy resins, and bisphenol S-type epoxy resins, biphenyl-type epoxy resins, naphthalene-type epoxy resins, epoxy resins having a fluorene skeleton, polypropylene glycol-type epoxy resins, polyethylene glycol-type epoxy resins, and long-chain aliphatic epoxy resins, which fall within the above definition of a liquid.
[0014] Component [A] of the present invention is preferably a bisphenol-type epoxy resin, and in particular, one having an average epoxy equivalent of 160 to 200 is preferred. By adjusting the average epoxy equivalent to 160 to 200, an epoxy resin composition having excellent heat resistance and a glass transition temperature of the cured product of 110°C or higher can be obtained. This is also preferred because it has excellent compatibility with component [B].
[0015] In the present invention, the average epoxy equivalent can be evaluated by potentiometric titration in accordance with JIS-K7236 (2001). For example, approximately 300 mg of epoxy resin is weighed and placed in a glass beaker, and 10 mL of chloroform is added. The solution is stirred using a magnetic stirrer until the weighed components are dissolved in the chloroform. 20 mL of acetic acid is added to the solution, followed by 10 mL of tetraethylammonium bromide acetate solution (0.4 g / mL acetic acid) and stirring. An electrode is immersed in the solution, and potentiometric titration is performed using a perchloric acid-acetic acid standard solution (0.1 mol / L), allowing the average epoxy equivalent to be calculated.
[0016] (Component [B]) Component [B] used in the present invention has a structure of formula (I) or formula (II). The epoxy resin having the structure of formula (I) has an average epoxy equivalent of 400 to 1,200, and the epoxy resin having the structure of formula (II) has an average epoxy equivalent of 150 to 500.
[0017]
[0018] (In formula (I), R 1 , R 2 is a hydrogen atom or an alkyl group having 1 to 10 carbon atoms, and R 1 and R 2 may be the same or different. 1 represents an integer from 1 to 30.)
[0019]
[0020] (In formula (II), R 3 represents a bisphenol structure, and n 2represents an integer of 1 to 30.) Hereinafter, in this specification, for example, "an epoxy resin having the structure of formula (I)" will be simply referred to as "an epoxy resin of formula (I)".
[0021] The epoxy resin of formula (I) has an average epoxy equivalent of 400 to 1200. By adjusting the average epoxy equivalent of the epoxy resin of formula (I) to 400 to 1200, an epoxy resin composition having an excellent balance between depolymerization property and heat resistance can be obtained.
[0022] In the epoxy resin of formula (I), R 1 , R 2 is a hydrogen atom or an alkyl group having 1 to 10 carbon atoms, an epoxy resin composition having excellent heat resistance can be obtained. The epoxy resin of formula (I) is bifunctional and has a long chain structure, and when the disulfide bond in formula (III) described below is cleaved, it decomposes in large domain units, improving depolymerization properties. In addition, 1 When is an integer of 1 to 30, an epoxy resin composition having an excellent balance between depolymerization property and heat resistance can be obtained.
[0023] When component [B] of the present invention has the structure of formula (I), it is preferably a bisphenol F epoxy resin having an average epoxy equivalent of 800 to 1200. By using a bisphenol F epoxy resin having an average epoxy equivalent of 800 to 1200, an epoxy resin composition having even better depolymerization properties and heat resistance can be obtained. Furthermore, since the viscosity of the plasticized resin composition after depolymerization of the cured product is reduced, the regeneration properties are favorable, which is preferable.
[0024] The epoxy resin of formula (II) has an average epoxy equivalent of 150 to 500. By adjusting the average epoxy equivalent of the epoxy resin of formula (II) to 150 to 500, an epoxy resin composition having an excellent balance between depolymerization property and heat resistance can be obtained. The epoxy resin of formula (II) preferably has an average epoxy equivalent of 200 to 350. By adjusting the average epoxy equivalent of the epoxy resin of formula (II) to 200 to 350, an epoxy resin composition having an even better balance between depolymerization property and heat resistance can be obtained. The epoxy resin of formula (II) preferably has a molecular weight of 450 or more.
[0025] In the epoxy resin of formula (II), R 3 When the epoxy resin of formula (II) has a bisphenol structure, an epoxy resin composition having excellent heat resistance can be obtained. The bisphenol structure is a compound having two hydroxyphenyl groups, and examples thereof include bisphenol A, bisphenol E, bisphenol F, and bisphenol S. Among these, bisphenol A or bisphenol F is preferred because the epoxy resin of formula (II) has a low viscosity.
[0026] In addition, n of the epoxy resin of formula (II) 2 When is an integer of 1 to 30, an epoxy resin composition having an excellent balance between depolymerization property and heat resistance can be obtained.
[0027] The epoxy resin of formula (II) has disulfide bonds, and therefore, even after the epoxy resin composition has cured, the disulfide bonds can be cleaved by a solution or hydrolysis treatment, resulting in depolymerization. Furthermore, the epoxy resin of formula (II), like the epoxy resin of formula (I), is bifunctional and has a long chain structure, and further has disulfide bonds itself. Therefore, not only when the disulfide bonds in formula (III) are cleaved, but also when the disulfide bonds themselves are cleaved, the epoxy resin of formula (II) decomposes in large domain units, thereby further improving depolymerization properties.
[0028] The epoxy resin of component [B] used in the present invention is contained in an amount of 10 to 30 parts by mass per 100 parts by mass of the total epoxy resin. That is, when an epoxy resin of formula (I) is selected as component [B], the epoxy resin of formula (I) is contained in an amount of 10 to 30 parts by mass per 100 parts by mass of the total epoxy resin. When an epoxy resin of formula (II) is selected as component [B], the epoxy resin of formula (II) is contained in an amount of 10 to 30 parts by mass per 100 parts by mass of the total epoxy resin. When an epoxy resin of formula (I) and an epoxy resin of formula (II) are used in combination, the total amount of both epoxy resins is preferably 10 to 30 parts by mass per 100 parts by mass of the total epoxy resin. By containing the epoxy resin of component [B] in such a predetermined amount, an epoxy resin composition having an excellent balance between depolymerization property and heat resistance can be obtained.
[0029] Commercially available epoxy resins of formula (I) of component [B] include bisphenol A epoxy resins such as jER (registered trademark) 1001, jER (registered trademark) 1004, and jER (registered trademark) 1007 (all manufactured by Mitsubishi Chemical Corporation), and EPICLON (registered trademark) 1050, EPICLON (registered trademark) 3050, and EPICLON (registered trademark) 4050 (all manufactured by DIC Corporation). Bisphenol F epoxy resins include jER (registered trademark) 4004P and jER (registered trademark) 4005P (all manufactured by Mitsubishi Chemical Corporation), and YDF-2001 and YDF-2004 (all manufactured by KOKDO Co., Ltd.).
[0030] Commercially available epoxy resins of formula (II) of component [B] include "FLEP (registered trademark)" 50 and "FLEP (registered trademark)" 60 (both manufactured by Toray Fine Chemicals Co., Ltd.).
[0031] The epoxy resin composition of the present invention may further contain a trifunctional or tetrafunctional epoxy resin as component [D], which is preferably contained in an amount of 5 to 30 parts by mass, more preferably 5 to 20 parts by mass, per 100 parts by mass of the total epoxy resin.
[0032] Typically, when a trifunctional or tetrafunctional epoxy resin is blended, the crosslink density increases, improving heat resistance but decreasing depolymerization resistance. However, by adjusting the content of component [D] to 5 to 30 parts by mass per 100 parts by mass of the total epoxy resin, an epoxy resin composition with an excellent balance between depolymerization resistance and heat resistance can be obtained. Furthermore, by adjusting the content of component [D] to 5 to 20 parts by mass per 100 parts by mass of the total epoxy resin, an epoxy resin composition with an even better balance between depolymerization resistance and heat resistance can be obtained.
[0033] Examples of the trifunctional or tetrafunctional epoxy resin of component [D] include naphthalene-type epoxy resins, epoxy resins having a fluorene skeleton, and glycidylamine-type epoxy resins such as tetraglycidyldiaminodiphenylmethane, tetraglycidylxylenediamine, triglycidylaminophenol, and triglycidylaminocresol. These may be used alone or in combination. In particular, N,N,N',N'-tetraglycidyldiaminodiphenylmethane, triglycidylaminophenol, and triglycidylaminocresol are preferred because they are liquid at 23°C and can yield epoxy resin compositions with excellent heat resistance.
[0034] The epoxy resin composition of the present invention may further contain a difunctional naphthalene-type epoxy resin as component [E], preferably one having an average epoxy equivalent of 110 to 280, and more preferably one having an average epoxy equivalent of 150 to 280. By adjusting the average epoxy equivalent to 110 to 280, an epoxy resin composition having excellent heat resistance and a cured product with a glass transition temperature of 110°C or higher can be obtained, and by adjusting the average epoxy equivalent to 150 to 280, an epoxy resin composition having excellent heat resistance and a cured product with a glass transition temperature of 130°C or higher can be obtained. This is also preferred because it has excellent compatibility with component [A].
[0035] Component [E] is preferably contained in an amount of 5 to 80 parts by mass, more preferably 50 to 70 parts by mass, per 100 parts by mass of the total epoxy resin. By containing 50 to 70 parts by mass of component [E] per 100 parts by mass of the total epoxy resin, heat resistance is improved while maintaining depolymerization properties. Furthermore, even when miscible with component [A], the component remains liquid, and excellent processability into prepregs is achieved.
[0036] By including component [E], the naphthalene structure is rigid, and the crosslinking density is reduced due to the presence of a bifunctional epoxy resin, so that an epoxy resin composition having even more excellent heat resistance while maintaining depolymerization properties can be obtained.
[0037] Commercially available bifunctional naphthalene epoxy resins of component [E] include EPICLON (registered trademark) HP-4032SS, EPICLON (registered trademark) HP-4032D, and EPICLON (registered trademark) HP-4770 (all manufactured by DIC Corporation), and diglycidyl 1,4'-dihydroxynaphthalene (manufactured by Air Water Performance Chemicals Inc.).
[0038] Among these, "EPICLON (registered trademark)" HP-4770 is preferred because it gives an epoxy resin composition having excellent heat resistance and a glass transition temperature of the cured product of 130°C or higher. (Component [C]) Component [C] in the present invention is an aromatic diamine having the structure of formula (III).
[0039]
[0040] (In formula (III), R 4 , R 5 represents a hydrogen atom, a halogen atom, or an alkyl group having 1 to 8 carbon atoms; R 4 and R 5 may be the same or different.) In the aromatic diamine of formula (III), R 4 , R 5 are each a substituent selected from a hydrogen atom, a halogen atom, and an alkyl group having 1 to 8 carbon atoms, an epoxy resin composition having an excellent balance between depolymerization ability and heat resistance can be obtained. The aromatic diamine of formula (III) has a disulfide bond in its structure, and therefore, even after the epoxy resin composition has cured, the cured product can be depolymerized by utilizing the phenomenon that the disulfide bond is cleaved by a solution or hydrolysis treatment.
[0041] Commercially available aromatic diamines of the formula (III) include 4,4'-diaminodiphenyl disulfide and 2,2'-diaminodiphenyl disulfide (both manufactured by Tokyo Chemical Industry Co., Ltd.).
[0042] Of the aromatic diamines represented by formula (III), component [C] of the present invention is preferably an aromatic diamine having a structure represented by formula (IV), or an aromatic diamine having a structure represented by formula (IV) or a structural isomer thereof.
[0043]
[0044] (In formula (IV), R 4 , R 5 represents a hydrogen atom, a halogen atom, or an alkyl group having 1 to 8 carbon atoms; R 4 and R 5 may be the same or different.) In the structure of formula (IV), the amino groups are located at the 2,2'-positions, which creates steric hindrance and results in a low crosslink density, thereby obtaining an epoxy resin composition with an excellent balance between depolymerization property and heat resistance. In addition, using a mixture of an aromatic diamine having the structure of formula (IV) and its structural isomer is preferred because it allows the viscosity of the epoxy resin composition to be reduced by a eutectic that lowers the melting point.
[0045] The epoxy resin composition of the present invention preferably has a glass transition temperature of 110°C or higher, more preferably 130°C or higher, and even more preferably 150°C or higher, after curing for 120 minutes at 150°C to 220°C. The glass transition temperature can be measured using a differential scanning calorimeter in accordance with JIS-K7121 (1999). Here, the term "cured product after curing for 120 minutes at 150°C to 220°C" refers to a cured product that has been cured by maintaining the temperature at any temperature in the range of 150°C to 220°C for 120 minutes or longer.
[0046] Specifically, the cured resin obtained under the above conditions is heated from 25° C. to 300° C. at a temperature increase rate of 10° C. / min, held at 300° C. for 3 minutes, and then rapidly cooled to 25° C. at a temperature decrease rate of 30° C. / min. In a differential scanning calorimetry chart (with thermal energy on the vertical axis and temperature on the horizontal axis) during the temperature increase from 25° C. to 300° C., the glass transition temperature is determined by the point where a line equidistant in the vertical direction from an extended line of each baseline intersects with the curve of the stepwise change in the glass transition.
[0047] Generally, glass transition temperature and depolymerization property are correlated, and the higher the glass transition temperature, the higher the durability and the longer the material life. By achieving a glass transition temperature of 110°C or higher for the cured product obtained under the above conditions, it can be used in aerospace applications such as secondary structural materials like interior materials, and in general industrial applications such as high-heat-resistant applications like bicycles, wind turbines, ships, railway vehicles, and laptop computer housings. Furthermore, by achieving a glass transition temperature of 130°C or higher for the cured product, it can be used in general industrial applications such as automotive structural components. Furthermore, by achieving a glass transition temperature of 150°C or higher for aerospace applications such as primary aircraft structural materials like main wings, tails, and floor beams. Furthermore, it is preferable that the glass transition temperature of the cured product obtained under the above conditions be 250°C or lower. By achieving a glass transition temperature of 250°C or lower, the crosslink density of the cured product can be within a depolymerizable range.
[0048] As described above, by combining the components [A] to [C], the trade-off between heat resistance and ease of depolymerization can be overcome, and excellent heat resistance can be obtained, thereby maintaining durability in an actual usage environment while maintaining susceptibility to depolymerization treatment, which is advantageous in that it allows for recyclability.
[0049] The epoxy resin composition of the present invention may contain thermoplastic resins, rubber particles, inorganic particles such as silica, nanoparticles such as carbon nanotubes (CNTs) and graphene, etc., for the purpose of adjusting the viscoelasticity, improving the tack and drape properties of the prepreg, or enhancing the mechanical properties and toughness of the resin composition, as long as the effects of the present invention are not lost. Examples of thermoplastic resins soluble in epoxy resins include polyvinyl acetal resins such as polyvinyl formal and polyvinyl butyral, polyvinyl alcohol, phenoxy resin, polyamide, polyimide, polyvinylpyrrolidone, polysulfone, and polyethersulfone. Examples of rubber particles include crosslinked rubber particles and core-shell rubber particles in which a different polymer is graft-polymerized onto the surface of crosslinked rubber particles.
[0050] The epoxy resin composition of the present invention may be prepared by kneading using a machine such as a kneader, a planetary mixer, a three-roll mill, or a twin-screw extruder, or by mixing by hand using a beaker and a spatula, etc., provided that uniform kneading is possible.
[0051] The prepreg of the present invention includes the epoxy resin composition and at least one reinforcing fiber selected from the group consisting of carbon fiber, glass fiber, and aramid fiber. The reinforcing fiber may be surface-treated. Examples of surface treatments include metal coating as a conductor, treatment with a coupling agent, treatment with a sizing agent, treatment with a binder, and treatment with an additive. These reinforcing fibers may be used alone or in combination. Among these, polyacrylonitrile (PAN), pitch, rayon, and other carbon fibers, which have excellent specific strength and specific rigidity, are preferred from the perspective of weight reduction. Glass fiber is preferred from the perspective of improving the economic viability of the resulting fiber-reinforced composite material, and a combination of carbon fiber and glass fiber is particularly preferred from the perspective of balancing mechanical properties and economic efficiency. Furthermore, aramid fiber is preferred from the perspective of improving the impact resistance and formability of the resulting fiber-reinforced composite material, and a combination of carbon fiber and aramid fiber is particularly preferred from the perspective of balancing mechanical properties and impact resistance. Furthermore, from the viewpoint of increasing the electrical conductivity of the resulting fiber-reinforced composite material, reinforcing fibers coated with a metal such as nickel, copper, ytterbium, etc. Among these, PAN-based carbon fibers, which are excellent in mechanical properties such as strength and elastic modulus, can be more preferably used.
[0052] The prepreg can be produced by impregnating a reinforcing fiber substrate with the epoxy resin composition of the present invention. Examples of the impregnation method include the hot melt method (dry method). The fiber weight content of the prepreg can be adjusted by changing the amount of resin applied to the release paper.
[0053] As a method for molding the prepreg, for example, press molding, autoclave molding, bagging molding, wrapping tape method, internal pressure molding, etc. can be used appropriately.
[0054] The reinforcing fibers contained in the prepreg of the present invention may be in the form of a woven fabric. In the case of a woven fabric, the weave is preferably a plain weave, a twill weave, a satin weave, or the like. Plain weave, twill weave, satin weave, or the like provides excellent handleability as a sheet-like prepreg and excellent shape conformability during lamination, facilitating the molding of complex-shaped components. Here, excellent shape conformability refers to the ability to conform to the shape without fiber orientation collapse during the process of laminating a reinforcing fiber woven fabric or the like onto a three-dimensional mold, thereby producing a molded product with satisfactory quality and performance. Furthermore, during the process of laminating a preform onto a three-dimensional mold, a preform is created using the reinforcing fiber woven fabric or the like. This requires a trimming process in which portions of the substrate that do not conform to the mold shape are cut with scissors or a cutter, or portions that do not end up in the final product are fixed with tape. This trimming process requires a lot of time and effort and causes material waste.
[0055] The reinforcing fibers contained in the prepreg of the present invention may be in the form of discontinuous fibers. By using discontinuous fibers as the reinforcing fibers, it becomes easier to form a complex shape when molding a sheet-like prepreg by applying an external force.
[0056] Furthermore, when the reinforcing fibers are discontinuous, they are preferably randomly dispersed in bundles in the prepreg, which makes it easier to mold the prepreg into a complex shape when an external force is applied to the prepreg to form it.
[0057] Furthermore, when the reinforcing fibers are discontinuous, they are preferably dispersed randomly in a substantially monofilament shape in the prepreg. When the reinforcing fibers are discontinuous, randomly dispersing the discontinuous reinforcing fibers in a substantially monofilament shape reduces the amount of reinforcing fibers present as fiber bundles in the prepreg, thereby minimizing weak portions at the fiber bundle ends and providing excellent reinforcement efficiency and isotropy. Here, "substantially monofilament" refers to the presence of fine strands of less than 500 reinforcing fiber single yarns. It is more preferable that the reinforcing fibers are dispersed in a monofilament shape, i.e., as single yarns, and it is even more preferable that the monofilament-like single fibers are dispersed randomly. When the reinforcing fibers are discontinuous, the reinforcing fibers may be in the form of a nonwoven fabric.
[0058] Next, the fiber-reinforced composite material of the present invention will be described.
[0059] A fiber-reinforced composite material according to one aspect of the present invention is a fiber-reinforced composite material containing a cured product of the epoxy resin composition of the present invention (hereinafter referred to as the "cured epoxy resin product of the present invention") as a matrix resin, and is typically obtained by curing the prepreg of the present invention described above. More specifically, a fiber-reinforced composite material containing a cured product of the epoxy resin composition of the present invention as a matrix resin can be obtained by laminating prepregs having the epoxy resin composition of the present invention as a matrix resin, as required, and then heating and curing the laminate.
[0060] In the present invention, depolymerization refers to the overall process by which polymerized substances are decomposed by external stimuli or other factors, ultimately resulting in the conversion to monomers. In the early stages of depolymerization of a cured epoxy resin, only the surface is swollen or slightly dissolved. This state facilitates separation and disassembly when the cured epoxy resin is bonded to a different material, such as metal, making it recyclable. As depolymerization progresses, the entire thickness becomes plasticized and a rubbery state is achieved. In this state, the cured epoxy resin can be treated as a plastic resin and recycled, for example, in a regenerated form. In the final stage of depolymerization, the cured epoxy resin is significantly dissolved and loses its original shape. Even if the cured epoxy resin appears to retain its original shape when depolymerized under static conditions, it is considered to have lost its original shape if it loses its shape and collapses when moved. In the case of a fiber-reinforced composite material, this state allows the reinforcing fibers contained within it to be recovered as recycled fibers (resources).
[0061] Methods for depolymerizing and plasticizing the cured epoxy resin composition of the fiber-reinforced composite material of the present invention using a solution or hydrolysis treatment include thermal decomposition, supercritical water decomposition, subcritical water decomposition, superheated steam decomposition, liquid-phase decomposition, dissolution, and glycol decomposition. The dissolution method using a solution is preferred because depolymerization by disulfide cleavage is easy, and the superheated steam method is preferred because it does not require neutralization of the solution or washing of the recovered fibers. The solution of the present invention is not particularly limited as long as it can dissolve the cured epoxy resin of the present invention, but includes, for example, at least one liquid selected from acidic solutions, organic solvents, hydrogen peroxide solutions, and ionic liquids. These liquids are capable of dissolving or plasticizing the cured epoxy resin of the present invention, allowing for efficient depolymerization. The solution may be used alone or in combination of two or more.
[0062] Examples of the acidic solution used as a dissolving solution for the epoxy resin composition include phosphoric acid, sulfuric acid, hydrochloric acid, nitric acid, etc. The acidic component may be used alone or in combination of two or more.
[0063] Examples of organic solvents used as the dissolving solution include aliphatic hydrocarbon solvents, aromatic hydrocarbon solvents, alcohol solvents, ketone solvents, ether solvents, amide solvents, ester solvents, and N-methyl-2-pyrrolidone having a lactam structure. Among these, N-methyl-2-pyrrolidone is preferred because it is highly water-soluble and allows for the recovered fibers to be washed with water. One organic solvent may be used alone, or two or more organic solvents may be used in combination. Examples of aliphatic hydrocarbon solvents include pentane, hexane, heptane, octane, and glycol. Examples of aromatic hydrocarbon solvents include benzene, toluene, xylene, and tetralin. Examples of alcohol solvents include benzyl alcohol. Examples of ketone solvents include acetone, methyl ethyl ketone, methyl isobutyl ketone, diisobutyl ketone, cyclohexanone, and diacetone alcohol. Among these, acetone and methyl ethyl ketone are preferred because they are highly volatile and allow for easy drying of the recovered fibers. The organic solvent may contain a decomposition catalyst. The decomposition catalyst includes iron oxide and alkali metal compounds.
[0064] Examples of the ionic liquid used as the dissolving solution include ionic liquids containing at least one cation selected from imidazolium-based, pyridinium-based, pyrrolidinium-based, quaternary ammonium-based, and quaternary phosphonium-based cations. One type of ionic liquid may be used alone, or two or more types may be used in combination.
[0065] The fiber-reinforced composite material of the present invention is preferable because it can provide a cascade recycled composite by undergoing the steps (i) to (iii).
[0066] (i) The fiber length of the reinforcing fibers in the fiber-reinforced composite material is set to 2 to 100 mm.
[0067] (ii) Depolymerizing and plasticizing the cured epoxy resin composition by dissolving or hydrolyzing the composition.
[0068] (iii) The plasticized fiber reinforced composite material is randomly dispersed and hot pressed under conditions of 100 to 200° C. and 0.7 to 15 MPa.
[0069] By obtaining a cascade recycled composite through steps (i) to (iii), it becomes possible to recycle the cured product of the epoxy resin composition, which is the matrix resin in the fiber-reinforced composite material, without depolymerizing it until it is separated from the reinforcing fibers, which is preferable because it significantly reduces greenhouse gas emissions when recycling the fiber-reinforced composite material. In other words, the cascade recycled composite of the present invention is preferable because it has a low environmental impact during production.
[0070] The processing (i) for making the reinforcing fibers in the fiber-reinforced composite material of the present invention have a fiber length of 2 to 100 mm can be performed using a hammer mill crusher, a sand grind mill type wet crusher, a pelletizer, a high-speed rotor crusher, a rotary shear crusher, a ball mill crusher, etc. If all the fibers originally have a length of 2 to 100 mm, they may be used as they are.
[0071] The fiber length of the reinforcing fibers in the cascade recycled composite is preferably 3 to 20 mm, and by setting the fiber length in the range of 3 to 20 mm, fiber dispersion is improved and a highly rigid composite can be obtained. Furthermore, the fiber length is also preferably 60 to 100 mm, and setting the fiber length in the range of 60 to 100 mm is preferable because it simplifies the processing step and reduces greenhouse gas emissions. After use, the composite can be further processed to a fiber length of 50 mm or less and recycled, thereby significantly reducing greenhouse gas emissions.
[0072] The fiber-reinforced composite material according to one aspect of the present invention is preferably used in sports applications, general industrial applications, and aerospace applications. More specifically, as sports application components, it is preferably used for golf shafts, fishing rods, tennis and badminton rackets, hockey sticks, and ski poles. As general industrial application components, it is preferably used for structural materials for automobiles, bicycles, wind turbines, ships, and railway vehicles, and electronic device components such as IC trays and housings for information devices such as laptop computers. As aerospace application components, it is preferably used for aircraft primary structural materials such as main wings, tails, and floor beams, and secondary structural materials such as interior materials.
[0073] The present invention will be explained in more detail below by showing examples, but the present invention is not limited to the descriptions of these examples.
[0074] 1. Materials Used <Epoxy Resin> The epoxy resins used in the present examples and comparative examples are listed below. In Tables 1 to 4, epoxy equivalent weight is abbreviated as "EEW."
[0075] [Component [A]] jER (registered trademark) 825 (bisphenol A type epoxy resin, average epoxy equivalent: 175, viscosity of 7000 mPa·s at 23°C, manufactured by Mitsubishi Chemical Corporation) EPALLOY (registered trademark) 5000 (hydrogenated bisphenol A type epoxy resin, viscosity of 2000 mPa·s at 23°C, average epoxy equivalent: 220, manufactured by Huntsman Corporation).
[0076] [Component [B]] jER (registered trademark) 1001 (bisphenol A type epoxy resin, compound having the structure of formula (I), average epoxy equivalent: 475, solid at 23°C, manufactured by Mitsubishi Chemical Corporation) jER (registered trademark) 1004 (bisphenol A type epoxy resin, compound having the structure of formula (I), average epoxy equivalent: 925, solid at 23°C, manufactured by Mitsubishi Chemical Corporation) jER (registered trademark) 4004P (bisphenol F type epoxy resin, compound having the structure of formula (I), average epoxy equivalent: 908, solid at 23°C, manufactured by Mitsubishi Chemical Corporation) jER (registered trademark) 4005P (bisphenol F type epoxy resin, compound having the structure of formula (I), average epoxy equivalent: 1075, solid at 23°C, manufactured by Mitsubishi Chemical Corporation) "FLEP (registered trademark)" 60 (epoxy resin, compound having the structure of formula (II), average epoxy equivalent: 279, semi-solid at 23°C, manufactured by Toray Fine Chemicals Co., Ltd.) "FLEP (registered trademark)" 50 (epoxy resin, compound having the structure of formula (II), average epoxy equivalent: 327, semi-solid at 23°C, manufactured by Toray Fine Chemicals Co., Ltd.).
[0077] [Component [D]] - "Sumiepoxy (registered trademark)" ELM434 (N,N,N',N'-tetraglycidyldiaminodiphenylmethane, average epoxy equivalent: 120, manufactured by Sumitomo Chemical Co., Ltd.).
[0078] [Component [E]] "EPICLON (registered trademark)" HP-4032D (naphthalene-type epoxy resin, average epoxy equivalent: 142, viscosity of 39,000 mPa·s at 23°C, manufactured by DIC Corporation) "EPICLON (registered trademark)" HP-4770 (difunctional naphthalene-type epoxy resin that is solid at 23°C, average epoxy equivalent: 204, manufactured by DIC Corporation).
[0079] [Epoxy resins other than components [A], [B], [D], and [E]] jER (registered trademark) 1007 (bisphenol A-type epoxy resin, having the structure of formula (I) but with an average epoxy equivalent of 1975, manufactured by Mitsubishi Chemical Corporation) jER (registered trademark) 4007P (bisphenol F-type epoxy resin, having the structure of formula (I) but with an average epoxy equivalent of 2250, manufactured by Mitsubishi Chemical Corporation) FLEP (registered trademark) 125X (epoxy resin having a disulfide bond, having the structure of formula (II) but with an average epoxy equivalent of 850, manufactured by Toray Fine Chemicals Co., Ltd.) In Table 4, "epoxy resins other than components [A], [B], [D], and [E]" are abbreviated as "other epoxies."
[0080] <Curing Agent> [Component [C]] 4,4'-Diaminodiphenyl disulfide (aromatic diamine, a compound having the structure of formula (III) but not the structure of formula (IV), manufactured by Tokyo Chemical Industry Co., Ltd.) 2,2'-Diaminodiphenyl disulfide (aromatic diamine, a compound having the structure of formula (IV), manufactured by Tokyo Chemical Industry Co., Ltd.).
[0081] [Aromatic diamines other than component [C]] 4,4'-diaminodiphenyl sulfone (Tokyo Chemical Industry Co., Ltd.) In Tables 1, 2 and 4, "aromatic diamines other than component [C]" is abbreviated as "other aromatic diamines."
[0082] 2. Sample Preparation Method [Method for Preparing Epoxy Resin Composition] Predetermined amounts of the epoxy resin components, component [A], component [B], component [D], and component [E], were placed in a stainless steel beaker, heated to 40 to 150°C, and appropriately kneaded until the components were compatible with each other.
[0083] The prepared mixture of epoxy resin components was cooled to 60°C or below, and component [C] and other aromatic diamines were added thereto, followed by kneading at 60°C for 30 minutes to obtain an epoxy resin composition.
[0084] [Method for producing cured resin product] The epoxy resin composition obtained by the above [Method for preparing epoxy resin composition] was degassed in a vacuum and then poured into a mold set to a thickness of 1 mm using a Teflon (registered trademark) spacer. Next, the temperature was raised from 30°C to 180°C at a rate of 1.0°C per minute in a hot air oven, and then the epoxy resin composition was cured by holding at 180°C for 120 minutes. Subsequently, the temperature was lowered to 30°C and the composition was removed from the mold to produce a cured resin product with a thickness of 1 mm.
[0085] [Method for producing a fiber-reinforced composite material] The epoxy resin composition prepared according to the above [Method for preparing an epoxy resin composition] was applied to a sheet of unidirectionally aligned carbon fiber "TORAYCA (registered trademark)" T700S-12K-60E (manufactured by Toray Industries, Inc., basis weight 150 g / m 2 ) to obtain a prepreg. The obtained prepreg was cut into a length of 200 mm and a width of 200 mm, and five sheets were stacked so that the fiber directions were perpendicular to each other. The prepreg was then sandwiched between molds and pressed at 3.5 MPa using a press heated to 150 to 200°C, and heat-cured for 90 minutes. The mold was then removed from the press and cooled to 30°C using a metal plate, obtaining a fiber-reinforced composite material.
[0086] Vf (unit: %) refers to the volume ratio of reinforcing fibers in a fiber-reinforced composite material, and can be calculated using the following formula: Vf = (W × 100) / (ρ × T), where W is 1 cm of reinforcing fiber substrate. 2 Mass of reinforcing fibers per unit (g / cm 2 ) ρ: Density of reinforcing fiber (g / cm 3 ) T: thickness of the fiber reinforced composite material (cm).
[0087] 3. Evaluation Methods [Method for Measuring Glass Transition Temperature] 5 mg of a sample was weighed out from the 1 mm thick cured resin product obtained by the above [Method for Producing Cured Resin Product] into a sample pan, and measurement of glass transition temperature was carried out using a differential scanning calorimeter Q-2500 (manufactured by TA Instruments) in accordance with JIS-K7121 (1999).
[0088] The sample was heated from 25°C to 300°C at a heating rate of 10°C / min, held at 300°C for 3 minutes, and then rapidly cooled to 25°C at a heating rate of 30°C / min. In a differential scanning calorimetry chart (vertical axis represents thermal energy, horizontal axis represents temperature) during the heating process from 25°C to 300°C, the glass transition temperature was determined from the point where a line equidistant from an extended line of each baseline in the vertical direction intersected with the curve of the stepwise change in the glass transition. The above measurement was repeated three times, and the resulting number average value was taken as the glass transition temperature.
[0089] [Method for Evaluating Depolymerization of Epoxy Resin Composition] Three square test pieces, each 15 mm wide and 15 mm long, were cut from the 1 mm thick cured resin obtained by the above [Method for Producing Cured Resin] and placed in a stainless steel beaker containing 65 g of a solution of either benzyl alcohol, methyl ethyl ketone (MEK), or N-methyl-2-pyrrolidone (NMP). The test pieces were evaluated according to the following criteria. Each stainless steel beaker was covered and stored at 23°C. No change in the cured epoxy resin: N Only the surface is swollen or slightly dissolved: A Plasticized throughout the entire thickness and in a rubbery state: B The cured epoxy resin is significantly dissolved and has lost its original shape: C
[0090] Example 1 An epoxy resin composition was prepared according to the above-mentioned [Method for preparing an epoxy resin composition] using 70 parts by mass of "jER (registered trademark)" 825, which corresponds to component [A], as the epoxy resin, 30 parts by mass of "jER (registered trademark)" 1001, which corresponds to component [B] and has an average epoxy equivalent of 400 to 1200 and a structure of formula (I), and 26.5 parts by mass of 4,4'-diaminodiphenyl disulfide, which corresponds to component [C], as the curing agent.
[0091] This epoxy resin composition was used to prepare a cured epoxy resin product according to the [Method for preparing cured epoxy resin product], and the glass transition temperature was measured according to the [Method for measuring glass transition temperature]. The glass transition temperature was 136°C, demonstrating good heat resistance.
[0092] The depolymerization property in MEK after 30 days evaluated according to the [Method for evaluating depolymerization property of epoxy resin composition] was rated A, meaning that only the surface was slightly dissolved, indicating good depolymerization property.
[0093] (Examples 2 to 21) Epoxy resin compositions and cured epoxy resin materials were prepared in the same manner as in Example 1, except that the resin compositions were changed as shown in Table 1. The evaluation results are shown in Tables 1, 2, and 3.
[0094]
[0095]
[0096]
[0097] (Example 22) The epoxy resin composition obtained in Example 1 was impregnated into a sheet of unidirectionally aligned carbon fiber "TORAYCA (registered trademark)" T700S-12K-60E, to form a carbon fiber sheet having a basis weight of 190 g / m 2 The prepreg obtained had good tack and was easy to handle. The fiber reinforced composite material obtained according to the [Method for producing a fiber reinforced composite material] had a fiber volume fraction Vf of 65% and was of good quality.
[0098] (Example 23) The epoxy resin composition obtained in Example 2 was impregnated into unidirectionally aligned carbon fiber sheets "TORAYCA (registered trademark)" T700S-12K-60E, to form a sheet having a basis weight of 190 g / m 2 The prepreg obtained was difficult to handle because the viscosity of the resin composition was low and the tackiness was too strong. The fiber volume fraction Vf of the fiber reinforced composite material obtained according to the [Method for producing a fiber reinforced composite material] was 64%, and the quality was good.
[0099] Example 24 The prepreg obtained in Example 22 was shaped into a mold for the roof of an automobile, but the shape conformability was poor, and complicated trimming was required.
[0100] Example 25 The epoxy resin composition obtained in Example 1 was mixed with carbon fiber "TORAYCA (registered trademark)" T700S-12K-60E to a basis weight of 192 g / m 2The resulting woven fabric prepreg was molded into a mold for the roof of an automobile, and showed excellent conformability, eliminating the need for trimming.
[0101] (Example 26) Carbon fiber "TORAYCA (registered trademark)" T700S-12K-60E was cut into a length of 12 mm and randomly dispersed in bundles or approximately monofilaments, resulting in a basis weight of 150 g / m 2 A nonwoven fabric having the following characteristics was obtained. The obtained nonwoven fabric was impregnated with the epoxy resin composition obtained in Example 1 to obtain a nonwoven fabric prepreg. When the obtained nonwoven fabric prepreg was molded into a mold shaped like an automobile roof, it exhibited excellent shape conformability and no trimming was required.
[0102] Example 27: The fiber-reinforced composite material obtained in Example 22 was pulverized using a biaxial pulverizer to obtain chips containing reinforcing fibers with fiber lengths of 5 mm to 100 mm. The obtained chips were treated with superheated steam at 300°C for 30 minutes, which depolymerized and plasticized the cured epoxy resin of the fiber-reinforced composite material. The plasticized chips were randomly dispersed and hot-pressed at 180°C and 10 MPa, yielding a regenerated template.
[0103] Comparative Example 1 An epoxy resin composition was prepared and a cured epoxy resin material was produced in the same manner as in Example 1, except that only 100 parts by mass of "jER (registered trademark)" 825, which corresponds to component [A], was used as the epoxy resin. The resin composition and evaluation results are shown in Table 4. The heat resistance of the obtained resin composition was good, but the depolymerization property was insufficient.
[0104] Comparative Example 2 An epoxy resin composition was prepared and a cured epoxy resin material was produced in the same manner as in Example 1, except that the epoxy resins used were 95 parts by mass of jER (registered trademark) 825, which corresponds to component [A], and 5 parts by mass of jER (registered trademark) 1001, which corresponds to component [B] and has an average epoxy equivalent of 400 to 1200 and a structure represented by formula (I). The resin composition and evaluation results are shown in Table 4. The heat resistance of the resulting resin composition was good, but the depolymerization property was insufficient.
[0105] Comparative Example 3 An epoxy resin composition was prepared and a cured epoxy resin material was produced in the same manner as in Example 1, except that the epoxy resins used were 60 parts by mass of jER (registered trademark) 825, which corresponds to component [A], and 40 parts by mass of jER (registered trademark) 1001, which corresponds to component [B] and has an average epoxy equivalent of 400 to 1200 and a structure represented by formula (I). The resin composition and evaluation results are shown in Table 4. The resulting resin composition had good depolymerization properties, but insufficient heat resistance.
[0106] Comparative Example 4 An epoxy resin composition was prepared and a cured epoxy resin material was produced in the same manner as in Example 1, except that the epoxy resins used were 90 parts by mass of jER (registered trademark) 825, which corresponds to component [A], and 10 parts by mass of jER (registered trademark) 1007, which has the structure of formula (I) but an average epoxy equivalent of 1975 and does not correspond to any of components [A], [B], [D], or [E]. The resin composition and evaluation results are shown in Table 4. The resulting resin composition had good depolymerization properties, but insufficient heat resistance.
[0107] Comparative Example 5 An epoxy resin composition was prepared and a cured epoxy resin material was produced in the same manner as in Example 1, except that the epoxy resins used were 90 parts by mass of jER (registered trademark) 825, which corresponds to component [A], and 10 parts by mass of jER (registered trademark) 4007P, which has the structure of formula (I) but has an average epoxy equivalent of 2250 and does not correspond to any of components [A], [B], [D], or [E]. The resin composition and evaluation results are shown in Table 4. The resulting resin composition had good depolymerization properties, but insufficient heat resistance.
[0108] Comparative Example 6 An epoxy resin composition was prepared and a cured epoxy resin product was produced in the same manner as in Example 1, except that the epoxy resins used were 95 parts by mass of jER (registered trademark) 825, which corresponds to component [A], and 5 parts by mass of FLEP (registered trademark) 50, which corresponds to component [B] and has an average epoxy equivalent of 150 to 500 and a structure represented by formula (II). The resin composition and evaluation results are shown in Table 4. The heat resistance of the resulting resin composition was good, but the depolymerization property was insufficient.
[0109] Comparative Example 7 An epoxy resin composition was prepared and a cured epoxy resin product was produced in the same manner as in Example 1, except that the epoxy resins used were 60 parts by mass of jER (registered trademark) 825, which corresponds to component [A], and 40 parts by mass of FLEP (registered trademark) 50, which corresponds to component [B] and has an average epoxy equivalent of 150 to 500 and a structure represented by formula (II). The resin composition and evaluation results are shown in Table 4. The resulting resin composition had good depolymerization properties, but insufficient heat resistance.
[0110] Comparative Example 8 An epoxy resin composition was prepared and a cured epoxy resin material was produced in the same manner as in Example 1, except that the epoxy resins used were 90 parts by mass of jER (registered trademark) 825, which corresponds to component [A], and 10 parts by mass of FLEP (registered trademark) 125X, which has the structure of formula (II) but an average epoxy equivalent of 850 and does not correspond to any of components [A], [B], [D], or [E]. The resin composition and evaluation results are shown in Table 4. The resulting resin composition had good depolymerization properties, but insufficient heat resistance.
[0111] Comparative Example 9 An epoxy resin composition was prepared and a cured epoxy resin material was produced in the same manner as in Example 1, except that 70 parts by mass of jER (registered trademark) 825, which corresponds to component [A], and 30 parts by mass of jER (registered trademark) 1001, which corresponds to component [B] and has an average epoxy equivalent of 400 to 1200 and a compound epoxy resin having the structure of formula (I), were used as the epoxy resin, and component [C] was not included and an aromatic diamine other than component [C] was used as the curing agent. The resin composition and evaluation results are shown in Table 4. The heat resistance of the resulting resin composition was good, but depolymerization property was insufficient.
[0112]
[0113] The numerical values of each component in the table are in parts by mass, with the total amount of all epoxy resin components contained in the epoxy resin composition being 100 parts by mass.
Claims
1. An epoxy resin composition comprising the following components [A], [B], and [C], with the epoxy resin of component [B] being contained in an amount of 10 to 30 parts by mass per 100 parts by mass of the total epoxy resin: [A]: a bifunctional epoxy resin that is liquid at 23°C; [B]: an epoxy resin having an average epoxy equivalent of 400 to 1200 and a structure represented by formula (I), or an epoxy resin having an average epoxy equivalent of 150 to 500 and a structure represented by formula (II). (In formula (I), R 1 , R 2 is a hydrogen atom or an alkyl group having 1 to 10 carbon atoms; R 1 and R 2 may be the same or different. 1 represents an integer from 1 to 30.) (In formula (II), R 3 represents a bisphenol structure, n 2 represents an integer of 1 to 30. [C]: an aromatic diamine having a structure of formula (III) (In formula (III), R 4 , R 5 is a hydrogen atom, a halogen atom, or an alkyl group having 1 to 8 carbon atoms; R 4 and R 5 may be the same or different.) 2. The epoxy resin composition according to claim 1, wherein component [A] is a bisphenol type epoxy resin having an average epoxy equivalent of 160 to 200.
3. The epoxy resin composition according to claim 1, wherein when component [B] has the structure of formula (I), it is a bisphenol F type epoxy resin and has an average epoxy equivalent of 800 to 1,200.
4. The epoxy resin composition according to claim 1, wherein component [C] is an aromatic diamine having a structure of formula (IV), or an aromatic diamine having a structure of formula (IV) or a structural isomer thereof. (In formula (IV), R 4 , R 5 is a hydrogen atom, a halogen atom, or an alkyl group having 1 to 8 carbon atoms; R 4 and R 5 may be the same or different.) 5. The epoxy resin composition according to claim 1, which has a glass transition temperature of 110°C or higher after curing at 150°C to 220°C for 120 minutes.
6. The epoxy resin composition according to claim 1, further comprising, as component [D], a trifunctional or tetrafunctional epoxy resin in an amount of 5 to 30 parts by mass per 100 parts by mass of the total epoxy resin.
7. The epoxy resin composition according to claim 1, further comprising a difunctional naphthalene-type epoxy resin as component [E].
8. A prepreg comprising the epoxy resin composition according to any one of claims 1 to 7 and at least one reinforcing fiber selected from the group consisting of carbon fiber, glass fiber and aramid fiber.
9. The prepreg according to claim 8, wherein the reinforcing fibers are in the form of a woven fabric.
10. The prepreg according to claim 8, wherein the reinforcing fibers are in the form of discontinuous fibers.
11. The prepreg according to claim 8, wherein the reinforcing fibers are randomly dispersed in bundles or approximately monofilament form.
12. A fiber-reinforced composite material obtained by curing the prepreg according to claim 8.
13. A cascade recycled composite obtained from the fiber reinforced composite material of claim 12 through steps (i) to (iii). (i) The fiber length of the reinforcing fibers in the fiber reinforced composite material is set to 2 to 100 mm. (ii) The cured epoxy resin composition is depolymerized and plasticized by a dissolving solution or hydrolysis treatment. (iii) The plasticized fiber reinforced composite material is randomly dispersed and hot-pressed under conditions of 100 to 200°C and 0.7 to 15 MPa.
14. Aerospace components using the fiber-reinforced composite material according to claim 12.
15. An automobile component using the fiber-reinforced composite material according to claim 12.
Citation Information
Patent Citations
Thermomechanically reprocessable epoxy composites and processes for their manufacturing
WO2015181054A1
Resin composition for sealing liquid crystal cell made of film
JP1995070286A
Particle dispersed resin sheet, substrate for image display apparatus and image display apparatus
JP2005140863A
Resin composition for semiconductor encapsulation and semiconductor encapsulation device
JP2014141573A
Thermosetting epoxy resin composition having high strength and high cycle moldability
JP2015160938A
Cited By
Amine-based curing agent, curable resin composition, cured product, decomposition method for cured product, and recovery method for filler
WO2025100425A1
Conductive resin composition and cured product thereof
WO2026225311A1