Soft magnetic resin composition and molded body using same

The integration of hydrotalcite powder into soft magnetic resin compositions with PPS resin and metal powders addresses the issue of corrosive gas generation and rusting, maintaining high electromagnetic and mechanical properties, suitable for automotive components.

WO2024204360A1PCT designated stage expired Publication Date: 2024-10-03TODA KOGYO CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/012269
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-27
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Soft magnetic resin compositions using PPS resin suffer from corrosive gas generation, leading to mold maintenance issues and deterioration of electromagnetic properties due to rusting of soft magnetic metal powder, which current technologies fail to adequately address.

Method used

Incorporating hydrotalcite powder, specifically Mg-Al hydrotalcite, into the soft magnetic resin composition with PPS resin and soft magnetic metal powder to reduce corrosive gas generation while maintaining high electromagnetic properties, mechanical strength, and impact resistance.

Benefits of technology

The addition of hydrotalcite effectively suppresses corrosive gas generation and rusting, enhancing the physical and electromagnetic properties of molded articles, making them suitable for automotive parts with improved heat resistance and mechanical strength.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
  • Figure JPOXMLDOC01-APPB-T000003
    Figure JPOXMLDOC01-APPB-T000003
Patent Text Reader

Abstract

One embodiment of the present invention provides a soft magnetic resin composition from which it is possible to form a molded body which, without showing a reduction in magnetic properties, has excellent physical properties such as IZOD impact strength, bending strength, and heat resistance, and in which generation of corrosive gas is reduced. This soft magnetic resin composition contains a soft magnetic metal powder, a PPS resin, and a hydrotalcite powder. The contained amount of the hydrotalcite powder is 0.1-15.0 wt% with respect to the PPS resin. This molded body is obtained from said soft magnetic resin composition.
Need to check novelty before this filing date? Find Prior Art

Description

Soft magnetic resin composition and molded body using the same

[0001] The present disclosure relates to a soft magnetic resin composition that has excellent physical properties such as heat resistance, flexural strength, and IZOD impact strength without deteriorating electromagnetic properties, and that can reduce the generation of corrosive gases. The present disclosure also relates to a molded article using the soft magnetic resin composition.

[0002] In recent years, with the trend toward electric vehicles, there has been a demand for automotive parts that are high-frequency, small, lightweight, and fuel-efficient. Currently, soft magnetic materials such as electromagnetic steel sheets and dust cores are primarily used for automotive parts (motor parts such as rotors and stators, choke coils such as inductors, transformers, and reactors, and current sensors). From the perspectives of further miniaturization and high frequency, as well as molding flexibility, it is expected that these soft magnetic materials will be replaced by molded articles made of soft magnetic resin compositions.

[0003] In general, the soft magnetic resin composition is prepared by kneading a rubber or plastic material with a soft magnetic powder, and then molding the mixture into a desired shape using a molding machine such as an injection molding machine.

[0004] Automotive parts are strongly required to have high heat resistance and mechanical strength, and for this reason, PPS resin, which is said to have high heat resistance and little deterioration in mechanical properties at high temperatures, is used as a binder resin in resin compositions.

[0005] However, in the injection molding of a resin composition using PPS resin, a corrosive gas (Cl 2 ) derived from the PPS resin is generated. - Or SO 4 2- ) may increase the frequency of mold maintenance in the production process, shorten the mold life, and cause deterioration of molded articles of soft magnetic resin compositions due to rusting of the soft magnetic metal powder. Therefore, there is a strong demand for reducing corrosive gases.

[0006] Furthermore, when used in an AC magnetic field, soft magnetic materials are required to have high magnetic permeability, high saturation magnetization, and low iron loss. However, there is a concern that the soft magnetic metal powder contained in the soft magnetic resin composition may deteriorate due to oxidation from its surface.

[0007] For example, Patent Documents 1 and 2 describe that deterioration of electromagnetic properties and rusting are suppressed by using a resin composition that uses surface-treated soft magnetic metal powder.

[0008] Japanese Patent Application Laid-Open No. 7-235410 Japanese Patent Application Laid-Open No. 2021-121004

[0009] However, no measures have been taken to prevent rusting of the molding die or soft magnetic metal powder caused by corrosive gases derived from the PPS resin.

[0010] Therefore, the technical object of the present disclosure is to obtain a soft magnetic resin composition that has excellent physical properties such as heat resistance, bending strength, and IZOD impact strength, without deteriorating electromagnetic properties, and that reduces the generation of corrosive gases, and a molded article using the same.

[0011] The above technical object can be achieved by the present embodiment as follows.

[0012] That is, the soft magnetic resin composition according to the first embodiment contains soft magnetic metal powder, PPS resin, and hydrotalcite powder, and contains 0.1 to 15.0% by weight of hydrotalcite relative to the PPS resin.

[0013] The soft magnetic resin composition according to the second embodiment is the soft magnetic resin composition according to the first embodiment, containing 1.0 to 15.0% by weight of PPS resin.

[0014] The soft magnetic resin composition according to the third embodiment is the soft magnetic resin composition according to the first or second embodiment, containing 0.001 to 4.0% by weight of hydrotalcite.

[0015] The soft magnetic resin composition according to the fourth embodiment is the soft magnetic resin composition according to any one of the first to third embodiments, except that the hydrotalcite powder is Mg—Al-based hydrotalcite.

[0016] The molded article according to the fifth embodiment is a molded article made by using the soft magnetic resin composition according to any one of the first to fourth embodiments.

[0017] According to this embodiment, J sThe generation of corrosive gases can be reduced without reducing the saturation magnetization. Furthermore, molded articles obtained using the soft magnetic resin composition according to this embodiment have physical properties such as high bending strength and high IZOD impact strength. Therefore, this resin composition is suitable for use in injection molding of automotive parts.

[0018] 1 is a graph showing the effect of suppressing weight increase due to rusting of a metal rod caused by a corrosive gas, and a graph showing the effect of suppressing weight increase due to rusting of a soft magnetic resin composition molded body (core) caused by a corrosive gas.

[0019] This embodiment will be described in detail below.

[0020] The soft magnetic resin composition according to this embodiment contains at least a soft magnetic metal powder, a PPS resin, and a hydrotalcite powder.

[0021] The soft magnetic metal powder used in this embodiment is not particularly limited, and may be any soft magnetic metal powder typically used in resin compositions, such as FeSi, FeSiCr, FeSiAl, or carbonyl iron powder.

[0022] The soft magnetic metal powder preferably has an average particle size of 1.0 to 100.0 μm, more preferably 10.0 to 90.0 μm. From the viewpoint of packing properties and flowability, it is desirable that the powder be spherical.

[0023] It is desirable to subject the soft magnetic metal powder to various surface treatments in order to prevent deterioration of magnetic properties due to oxidation, improve compatibility with resins, and improve the strength of molded products.

[0024] Examples of materials that can be surface-treated include silane-based coupling agents, titanium-based coupling agents, aluminum-based coupling agents, siloxane polymers, organic phosphoric acid-based surface treatment agents, inorganic phosphoric acid-based surface treatment agents, etc. In particular, by treating the surface of the soft magnetic metal powder in advance with a silane-based coupling agent, the strength of the molded product can be further improved.

[0025] The hydrotalcite powder used in this embodiment is represented by the general formula: [M 2+ 1-x M 3+ x (OH)2 ][A n- x/n ・mH 2 O] (in the formula, M 2+ is Mg 2+ , Co 2+ , Ni 2+ , Zn 2+ It represents a divalent metal ion such as M 3+ is Al 3+ , Fe 3+ , Cr 3+ It indicates a trivalent metal ion such as n- Ha, OH - , Cl - , CO 3 2- , S.O. 4 2- The compound is a layered compound represented by the formula (I) above. x satisfies 0<x<1. n is the valence of A. m satisfies 0≦m<1.

[0026] The hydrotalcite powder used in this embodiment preferably contains Mg as the divalent metal ion. 2+ Al as a trivalent metal ion 3+ A part or all of these metal ions may be substituted with other metal ions.

[0027] The hydrotalcite powder used in this embodiment contains plate-like particles. The average plate surface diameter is 0.01 to 1.0 μm, preferably 0.02 to 0.8 μm, and more preferably 0.03 to 0.7 μm. If the average plate surface diameter is less than 0.01 μm, dispersibility in the resin is insufficient. If the average plate surface diameter exceeds 1.0 μm, it is difficult to industrially produce the plate-like particles.

[0028] The BET specific surface area of ​​the hydrotalcite powder used in this embodiment is preferably 1 to 150 m 2 / g, more preferably 5 to 100 m 2 / g, and even more preferably 8 to 50 m 2 / g. 2 It is difficult to industrially obtain hydrotalcite particles having a BET specific surface area of ​​less than 150 m / g. 2If the particle size exceeds 1 / g, the particles will aggregate severely, making it difficult to uniformly disperse the particles in the resin.

[0029] The hydrotalcite powder used in this embodiment may have its particle surfaces coated with at least one surface treatment agent selected from the group consisting of higher fatty acids, anionic surfactants, higher fatty acid phosphate esters, coupling agents, and polyhydric alcohol esters, as necessary. By coating with a surface coating, the dispersibility of the hydrotalcite powder in the resin is improved.

[0030] The hydrotalcite powder used in this embodiment can be produced by a conventional method. For example, a method can be used in which a mixture prepared by mixing a magnesium compound and an aluminum compound is first calcined, and then the Mg—Al composite oxide thus obtained is hydrated with an aqueous solution containing an anion. In another example, a calcium salt aqueous solution is added to a mixed aqueous solution prepared by mixing an alkaline aqueous solution containing an anion, an aqueous magnesium salt solution, and an aqueous aluminum salt solution, and then the resulting aqueous solution containing the calcium salt is heated and aged to obtain hydrotalcite powder.

[0031] The PPS resin used in this embodiment is not particularly limited, but preferably has an average molecular weight of 10,000 to 100,000. When a low-molecular-weight PPS resin is used, the injection molding composition has excellent moldability due to its low melt viscosity, but physical properties such as strength may be inferior. When a high-molecular-weight PPS resin is used, the injection molding composition has excellent physical properties due to its high melt viscosity, but moldability may be inferior if the filling amount of soft magnetic metal powder is high.

[0032] Furthermore, the melt viscosity of the PPS resin can be appropriately set depending on the soft magnetic metal powder. A preferred melt viscosity is within the range of 5 to 200 Pa·s at 310°C. If the melt viscosity at 310°C is less than 5 Pa·s, the mechanical strength of the resulting soft magnetic resin composition may decrease. On the other hand, if the melt viscosity at 310°C exceeds 200 Pa·s, the fluidity of the soft magnetic resin composition may decrease significantly. This may make injection molding difficult.

[0033] There are no particular limitations on the molecular structure of the PPS resin. That is, the molecular structure may be, for example, either a crosslinked type or a linear type. Furthermore, various elastomers such as rubber or elastic resins may be blended into the PPS resin as needed.

[0034] The content of the hydrotalcite powder in the soft magnetic resin composition according to this embodiment is 0.1 to 15.0% by weight relative to the PPS resin. If the content of the hydrotalcite powder relative to the PPS resin is less than 0.1% by weight, the effect of reducing corrosive gases is insufficient. If the content of the hydrotalcite powder relative to the PPS resin exceeds 15.0% by weight, the mechanical properties, magnetic properties, and fluidity are reduced. The content of the hydrotalcite powder relative to the PPS resin is more preferably 0.5 to 13.0% by weight, and even more preferably 1.0 to 10.0% by weight.

[0035] The soft magnetic resin composition according to this embodiment preferably contains 0.001 to 4.0% by weight of hydrotalcite powder. If the content of hydrotalcite powder is less than 0.001% by weight, the effect of reducing corrosive gases is insufficient. If the content of hydrotalcite powder exceeds 4.0% by weight, the amount of non-magnetic components increases. This may result in deterioration of mechanical properties, magnetic properties, and fluidity. The content of hydrotalcite powder is preferably 0.005 to 3.5% by weight, and more preferably 0.01 to 3.0% by weight.

[0036] The soft magnetic resin composition according to this embodiment preferably contains 1.0 to 15.0% by weight of PPS resin. If the PPS resin content is less than 1% by weight, the soft magnetic resin composition may not have sufficient fluidity. In such cases, it may be difficult to obtain a good molded product. If the PPS resin content exceeds 15% by weight, the electromagnetic properties may be reduced. The PPS resin content is more preferably 2.0 to 12.0% by weight, and even more preferably 3.0 to 10.0% by weight.

[0037] The soft magnetic metal powder content of the soft magnetic resin composition according to this embodiment is preferably 82.0 to 98.5% by weight. If the soft magnetic metal powder content is less than 82.0% by weight, the required magnetic properties may not be obtained. If the soft magnetic metal powder content exceeds 98.5% by weight, the mechanical strength of the resulting molded body may decrease, and moldability such as fluidity and recyclability may be significantly reduced. The soft magnetic metal powder content is more preferably 85.0 to 97.0% by weight, and even more preferably 90.0 to 95.0% by weight.

[0038] Next, a method for producing the soft magnetic resin composition according to this embodiment will be described.

[0039] The soft magnetic resin composition according to this embodiment can be obtained by a known method for producing soft magnetic resin compositions. For example, first, a soft magnetic metal powder, a PPS resin component, and a hydrotalcite powder are uniformly mixed, and then melt-kneaded using a kneading extruder or the like. The resulting kneaded product is then crushed or cut into granules or pellets to obtain the soft magnetic resin composition.

[0040] The soft magnetic resin composition according to this embodiment may contain a plastic molding lubricant and various stabilizers as appropriate in order to obtain effects such as improved moldability, improved heat resistance, prevention of oxidative degradation, and rust prevention.

[0041] Examples of lubricants include saturated and unsaturated fatty acids such as propionic acid, stearic acid, linoleic acid, oleic acid, malonic acid, glutaric acid, adipic acid, maleic acid, and fumaric acid, and derivatives thereof. Examples of derivatives include metal soaps such as calcium stearate, magnesium stearate, and lithium stearate, and fatty acid amides such as hydroxystearic acid amide, ethylene bislauric acid amide, and ethylene bisoleic acid amide. Other examples include waxes such as paraffin wax, polysiloxanes such as dimethylpolysiloxane and silicone oil, and fluorine compounds such as fluorine-containing oil.

[0042] As a stabilizer, an antioxidant is preferably added to suppress deterioration due to heat. Examples of antioxidants include hindered amine stabilizers. Other examples include hindered / lesshindered phenolic antioxidants such as pentaerythrityl-tetrakis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate], metal deactivators such as N,N'-bis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionylhydrazine, phosphite antioxidants, and thioether antioxidants. The combined use of a hindered / lesshindered phenolic antioxidant with a phosphite antioxidant or a metal deactivator is particularly effective.

[0043] The antioxidant is preferably contained in the range of 0.1 to 1.0 wt %, more preferably 0.2 to 0.8 wt %, based on the total amount of the resin composition.

[0044] If necessary, a known mold release agent such as zinc stearate or calcium stearate may be added to the resin.

[0045] Furthermore, in order to modify properties such as impact resistance, known resin modifiers such as silicone rubber, acrylic rubber, and butadiene rubber can be added to the resin as needed.

[0046] The molding method for obtaining a molded article using the soft magnetic resin composition according to this embodiment is not particularly limited. Any of known methods such as the transfer method, injection method, extrusion method, inflation method, calendaring method, T-die method, blowing method, vacuum method, lamination method, spray-up method, foaming method, matched die method, and SMC method can be used depending on the material properties of the soft magnetic resin composition, the molding purpose, and the application. Furthermore, a combination of multiple methods among these methods can also be used. In particular, the preferred molding method for a soft magnetic resin composition using PPS resin, which is a thermoplastic resin, is the injection method or the extrusion method. These molding methods are applied to many industrial parts. Furthermore, these molding methods enable continuous, high-speed, and mass production.

[0047] Representative examples of this embodiment are shown below, but this embodiment is not limited to these examples.

[0048] The average platelet diameter of the hydrotalcite powder was measured from a transmission electron microscope photograph of the observation sample. The average of the measured values ​​was defined as the average platelet diameter of the hydrotalcite powder. The transmission electron microscope used was a "JEM-1200EX II (manufactured by JEOL)." A solution containing hydrotalcite powder dispersed in water or alcohol was poured onto the mesh. The particles adhering to the mesh were dried to create an observation sample. Particles (200 points) whose platelets were attached horizontally to the mesh were selected from the observation sample. The platelet diameter of the selected particles was measured.

[0049] The BET specific surface area of ​​the hydrotalcite powder was measured using a Monosorb MS-21 (manufactured by QUANTA CHROME).

[0050] The molding density of the soft magnetic resin composition was determined using an "electronic pycnometer EW-120SG" (manufactured by Yasuda Seiki Seisakusho, Ltd.) Specifically, the molding density of a core obtained by molding a molten soft magnetic resin composition in a mold having a diameter of 25 mm and a height of 10.5 mm was measured with the electronic pycnometer.

[0051] Magnetic properties of soft magnetic resin composition (saturation magnetization J s ) was determined by the following method. First, a molten soft magnetic resin composition was molded in a mold having a diameter of 25 mm and a height of 10.5 mm to obtain a core. The magnetic properties of the obtained core were measured in a magnetic field of 1114.1 kA / m (14 kOe) using a "DC Magnetization Characteristic Automatic Recorder 3257" (manufactured by Yokogawa Hokushin Electric Co., Ltd.).

[0052] amplitude permeability μ a and iron loss P cv The soft magnetic resin composition was injection molded using an injection molding machine J55AD manufactured by The Japan Steel Works, Ltd., to obtain a ring core having an outer diameter of Φ32 mm, an inner diameter of Φ19 mm, and a height of 7 mm. a and iron loss P cvThe measurement was carried out using a BH analyzer SY-8218 manufactured by Iwasaki Electric Co., Ltd. under the conditions of Bm=50 mT and 10 kHz.

[0053] A molded article for strength testing having a total length of 80 mm, a total width of 12.7 mm, and a thickness of 3.2 mm was obtained by injection molding the soft magnetic resin composition using an injection molding machine J55AD manufactured by The Japan Steel Works, Ltd. The injectability of the soft magnetic resin composition was determined based on the injection pressure recorded during injection molding of the test piece.

[0054] The bending strength and IZOD impact strength of a strength test molded article using a soft magnetic resin composition were measured in accordance with ASTM D790 and D256 standards. More specifically, a strength test molded article was obtained using an injection molding machine, Model J55AD, manufactured by The Japan Steel Works, Ltd. Then, the bending strength and IZOD impact strength of the strength test molded article were measured using a computer-measured precision universal testing machine, Model AG-1, manufactured by Shimadzu Corporation and Model No. 158, manufactured by Yasuda Seiki Seisakusho Co., Ltd.

[0055] Example 1 0.28 parts by weight of an aminoalkyl silane coupling agent was added to 92.7 parts by weight of Fe6.5Si powder (average particle size D50 = 75 μm). The resulting mixture was heated and mixed at 120°C until homogeneous. In this way, a surface-treated powder was obtained. This surface-treated powder was mixed with 6.4 parts by weight of PPS resin (average molecular weight: 41,000, melt viscosity: 60 Pa s at 310°C) and Mg-Al hydrotalcite powder (average plate surface diameter: 0.24 μm, BET value: 11 m 2 0.1 parts by weight of cellulose acetate / g was added. The resulting mixture was thoroughly mixed in a Henschel mixer to obtain a soft magnetic resin composition mixture.

[0056] The obtained soft magnetic resin composition mixture was fed in a fixed amount to a twin-screw kneader and kneaded at a temperature at which the PPS resin melted. The kneaded product was cut into pellets. In this way, a soft magnetic resin composition was obtained.

[0057] The composition, molding density, and electromagnetic properties of the obtained soft magnetic resin composition are shown in Table 1.

[0058] The injection pressure during injection molding of the soft magnetic resin composition and the bending strength and IZOD impact strength of the molded article for strength test obtained by injection molding were measured. The results are shown in Table 2.

[0059] Examples 2 to 4, Comparative Examples 1 and 2 Soft magnetic resin compositions were prepared in the same manner as in Example 1, except that the blending ratio of the soft magnetic powder, PPS resin, and hydrotalcite powder was changed as shown in Table 1.

[0060]

[0061]

[0062] Rust formation of the metal rod due to corrosive gas was evaluated as follows. 20 g of soft magnetic resin composition pellets were pre-dried (140°C x 3 hours) and placed in a test tube. The metal rod was passed through a rubber stopper with a hole, and the test tube was sealed with the rubber stopper. The test tube was heated at 350°C x 3 hours in a solder pot (POT-28C) manufactured by Taiyo Electric Industrial Co., Ltd. At this time, corrosive gas generated from the pellets in the test tube adhered to the metal rod. The metal rod was then removed from the test tube and exposed for 16 days under conditions of 23°C x 95% RH in an Espec Corporation thermo-hygrostat LH-114. The weight increase of the metal rod due to rust was calculated by subtracting the weight before exposure from the weight after exposure. The results are shown in Table 3 and Figure 1.

[0063]

[0064] It was confirmed that the weight gain of the metal rod decreased as the amount of hydrotalcite added increased. Furthermore, the appearance of the metal rod also indicated that the addition of hydrotalcite suppressed rust. That is, the soft magnetic resin composition according to this embodiment was confirmed to be more effective in suppressing corrosion of the surrounding metal than the soft magnetic resin composition of Comparative Example 1, which did not contain hydrotalcite powder. The soft magnetic resin composition of Comparative Example 2 exhibited a decrease in the bending strength and IZOD impact strength of the molded body.

[0065] Rust formation of the soft magnetic metal powder in the molded body due to corrosive gas was evaluated as follows. A soft magnetic resin composition was melted and molded in a mold with a diameter of 25 mm and a height of 10.5 mm to form a core, which was then exposed for 1000 hours at a temperature of 85°C and a humidity of 90% RH using an LH-114 thermo-hygrostat manufactured by Espec Corporation. The weight before exposure was subtracted from the weight after exposure to calculate the weight increase of the core. The results are shown in Table 4 and FIG. 2.

[0066]

[0067] It was confirmed that the weight increase of the core decreased as the amount of hydrotalcite added increased. Furthermore, the appearance of the core also indicated that rusting was suppressed by the addition of hydrotalcite. In other words, the molded body using the soft magnetic resin composition according to this embodiment contains hydrotalcite, and therefore, it is possible to suppress deterioration of the soft magnetic metal powder in the molded body due to rusting.

[0068] Therefore, by using the soft magnetic resin composition according to this embodiment, a molded article can be obtained in which the generation of corrosive gases is reduced while maintaining high electromagnetic properties and mechanical properties, and therefore the soft magnetic resin composition is suitable as a soft magnetic resin composition for automobile parts, for example.

Claims

1. A soft magnetic resin composition comprising a soft magnetic metal powder, a PPS resin, and a hydrotalcite powder, the hydrotalcite being contained in an amount of 0.1 to 15.0% by weight relative to the PPS resin.

2. The soft magnetic resin composition according to claim 1, containing 1.0 to 15.0% by weight of PPS resin.

3. The soft magnetic resin composition according to claim 1 or 2, containing 0.001 to 4.0% by weight of hydrotalcite.

4. The soft magnetic resin composition according to claim 1 or 2, wherein the hydrotalcite powder is an Mg-Al based hydrotalcite.

5. A molded article made using the soft magnetic resin composition according to claim 1 or 2.

Citation Information

Patent Citations

  • Electromagnetic wave shield material and manufacturing method thereof

    JP2001237591A

  • Electromagnetic wave absorption sheet

    JP2013172049A

  • Resin composition

    JP2019156987A