Slurry for forming positive electrode of nonaqueous electrolyte secondary battery, nonaqueous electrolyte secondary battery, and method for producing nonaqueous electrolyte secondary battery
The slurry formulation with a specific conductive additive ratio and electrolyte in non-aqueous electrolyte secondary batteries enhances the electronic conductivity and adhesion of the positive electrode, addressing the challenges of liquid absorption and cycle performance.
Patent Information
- Application Number
- PCT/JP2024/012309
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-28
- Filing Date
- 2024-03-27
- Publication Date
- 2024-10-03
AI Technical Summary
Non-aqueous electrolyte secondary batteries face challenges in improving the electronic conductivity of positive electrode active materials, which affects the output characteristics, and using conductive additives with high specific surface areas can lead to poor adhesion and cycle characteristics due to liquid absorption issues.
A slurry for forming a positive electrode with a specific range of conductive additive specific surface area and content, combined with an electrolyte, ensuring electronic conductivity of 1.0 mS/cm or more and controlled carbon content, to enhance adhesion and cycle performance.
The solution results in a positive electrode active material layer with improved electronic conductivity and adhesion to the current collector, leading to excellent cycle characteristics and battery performance.
Smart Images

Figure JP2024012309_03102024_PF_FP_ABST
Abstract
Description
Slurry for forming positive electrode of non-aqueous electrolyte secondary battery, non-aqueous electrolyte secondary battery, and method for manufacturing non-aqueous electrolyte secondary battery
[0001] The present invention relates to a slurry for forming a positive electrode of a nonaqueous electrolyte secondary battery, a nonaqueous electrolyte secondary battery, and a method for manufacturing a nonaqueous electrolyte secondary battery.
[0002] Non-aqueous electrolyte secondary batteries, typified by lithium-ion secondary batteries, have high energy density and excellent storage performance, low-temperature operation, etc., and are widely used in portable electronic devices such as mobile phones and laptop computers. Furthermore, larger batteries are being used in transportation equipment such as automobiles, and their use as storage devices for nighttime electricity and electricity generated by natural energy sources is also progressing.
[0003] Techniques for increasing the capacity of non-aqueous electrolyte secondary batteries have been studied. For example, Patent Document 1 discloses a technique for making an electrode active material layer function as a secondary battery in the form of a slurry containing a high amount of active material. Specifically, the document describes an electrochemical cell including: a positive electrode made of a non-binding material containing a first active material and an electrolyte solution in a first non-aqueous liquid electrolyte; a negative electrode made of a non-binding material containing a second active material and an electrolyte solution in a second non-aqueous liquid electrolyte; and an ion-permeable membrane disposed between the positive electrode and the negative electrode, wherein the positive electrode and the negative electrode each have a thickness of about 200 μm to about 3000 μm. According to the technology described in Patent Document 1, as in the above-mentioned positive and negative electrodes, the electrode active material layers (positive electrode active material layer and negative electrode active material layer) contain an electrolyte and are in a slurry state and unbound, so that the electrode active material layer can be made into a thick film while maintaining its flexibility, and no binder is required to bind the solid particles together, making it possible to significantly increase the overall charge capacity and energy density while maintaining the flexibility of the battery. A nonaqueous electrolyte secondary battery in which the electrode active material layer is formed in a slurry state containing an electrolytic solution (electrolyte), as described in Patent Document 1, may be referred to as a quasi-solid secondary battery in the following description.
[0004] Among electrode active materials, carbon-based materials are widely used as negative electrode active materials and have relatively high electronic conductivity. On the other hand, the electronic conductivity of positive electrode active materials is generally inferior to that of carbon-based materials. Therefore, improving the electronic conductivity of positive electrode active materials in nonaqueous electrolyte secondary batteries is considered to be an important technological element for improving the battery's output characteristics.
[0005] Japanese Patent Application Laid-Open No. 2017-147222
[0006] To increase the capacity (energy density) of quasi-solid secondary batteries, attempts have been made to increase the content of ion-storing positive electrode active material in the slurry-like positive electrode active material layer. Furthermore, attempts have been made to reduce the content of conductive additives in the positive electrode active material layer in order to increase the content of positive electrode active material. However, reducing the content of conductive additives in the positive electrode active material layer reduces the conductivity of the positive electrode active material layer, resulting in disadvantages in output characteristics. Attempts have been made to maintain high output characteristics by using small amounts of conductive additives that have a large specific surface area and are easy to form an electronic conductive network. However, the inventors have found that conductive additives with a large specific surface area have high liquid absorption properties, which can limit the improvement of battery performance. That is, even when used in small amounts, the slurry becomes powder-like, a tendency that is more pronounced in slurries with a high content of positive electrode active material. As a result, it has been found that positive electrode active material layers made from such slurries are prone to losing adhesion to the positive electrode current collector, and the resulting batteries tend to have poor cycle characteristics.
[0007] The present invention aims to provide a positive electrode-forming slurry for a nonaqueous electrolyte secondary battery (quasi-solid secondary battery), which contains a positive electrode active material, a conductive additive, and an electrolyte, and which can provide a nonaqueous electrolyte secondary battery with excellent adhesion to a positive electrode current collector and excellent cycle characteristics, even when a conductive additive with a large specific surface area is used. Another object of the present invention is to provide a nonaqueous electrolyte secondary battery using this positive electrode-forming slurry, and a method for producing the same.
[0008] The above-mentioned problems of the present invention have been solved by the following means: [1] A slurry for forming a positive electrode of a non-aqueous electrolyte secondary battery containing a positive electrode active material, a conductive additive, and an electrolyte, wherein the conductive additive has a specific surface area x (m 2 / g) and a content y (mass %) of the conductive additive in the solid content of the positive electrode-forming slurry satisfy 5≦x×y≦420 and 100≦x, and the positive electrode active material has an electronic conductivity z (mS / cm) of 1.0 or more. [2] The positive electrode-forming slurry according to [1], wherein x, y, and z satisfy z≦(−0.0175×x×y)+10. [3] The positive electrode-forming slurry according to [1], wherein x, y, and z satisfy z≦(−0.0175×x×y)+10. [4] The positive electrode-forming slurry according to [1], wherein the electrical resistance of the surface of the positive electrode active material is 1.0×10 8 The positive electrode-forming slurry according to [1] or [2], wherein the surface of a positive electrode active material layer formed using the positive electrode-forming slurry has a carbon content of 5.0 mass % or less. [4] The positive electrode-forming slurry according to any one of [1] to [3], wherein the surface of the positive electrode active material layer formed using the positive electrode-forming slurry has a carbon content of 5.0 mass % or less. [5] The positive electrode-forming slurry according to any one of [1] to [4], wherein, in Raman spectroscopic analysis of the surface of the positive electrode active material, the ratio of the G band peak intensity to the D band peak intensity (G / D) is 0.5 to 4.0. [6] A non-aqueous electrolyte secondary battery having a positive electrode, a separator, and a negative electrode in this order, wherein the positive electrode-forming slurry according to any one of [1] to [5] is used as the positive electrode active material layer of the positive electrode. [7] A method for producing a non-aqueous electrolyte secondary battery, comprising applying the positive electrode-forming slurry according to any one of [1] to [5] onto a positive electrode current collector to form a slurry positive electrode active material layer.
[0009] In the description of the present invention, a numerical range expressed using "to" means a range including the numerical values written before and after "to" as the lower and upper limits. In the present invention, "nonaqueous electrolyte" means an electrolyte that does not substantially contain water. In other words, the "nonaqueous electrolyte" may contain a small amount of water within a range that does not impair the effects of the present invention. In the present invention, the "nonaqueous electrolyte" has a water concentration of 200 ppm (by mass) or less, preferably 100 ppm or less, and more preferably 20 ppm or less. Note that it is practically difficult to make a nonaqueous electrolyte completely anhydrous, and it usually contains 1 ppm or more of water. In the present invention, "nonaqueous solvent" also means a solvent that does not substantially contain water. In other words, the "nonaqueous solvent" may contain a small amount of water within a range that does not impair the effects of the present invention. In the present invention, the "nonaqueous solvent" has a water concentration of 200 ppm (by mass) or less, preferably 100 ppm or less, and more preferably 20 ppm or less. In reality, it is difficult to make a non-aqueous solvent completely free of water, and it usually contains 1 ppm or more of water.
[0010] The positive electrode-forming slurry for a nonaqueous electrolyte secondary battery of the present invention uses a conductive additive with a large specific surface area, yet in a slurry state, it is possible to obtain a nonaqueous electrolyte secondary battery (quasi-solid secondary battery) with excellent adhesion to the positive electrode current collector and excellent cycle characteristics. The nonaqueous electrolyte secondary battery of the present invention uses a conductive additive with a large specific surface area in the slurry-like positive electrode active material layer, yet it is possible to obtain a nonaqueous electrolyte secondary battery (quasi-solid secondary battery) with excellent adhesion to the positive electrode active material layer and excellent cycle characteristics. According to the manufacturing method of a nonaqueous electrolyte secondary battery of the present invention, it is possible to obtain the above-mentioned nonaqueous electrolyte secondary battery (quasi-solid secondary battery).
[0011] FIG. 1 is a longitudinal sectional view showing a schematic diagram of a basic layer structure of an embodiment of a secondary battery according to the present invention.
[0012] Although preferred embodiments of the present invention will be described, the present invention is not limited to these embodiments except as defined in the present invention.
[0013] [Slurry for forming a positive electrode] The slurry for forming a positive electrode of the present invention (also referred to as "positive electrode slurry of the present invention") is a slurry (suspension, dispersion) containing a positive electrode active material, a conductive additive, and an electrolyte, and is a slurry suitable for forming a positive electrode active material layer of a non-aqueous electrolyte secondary battery. In the positive electrode slurry of the present invention, the specific surface area x (m 2 / g) and the content y (mass%) of the conductive additive in the positive electrode slurry solid content satisfy 5≦x×y≦420 and 100≦x, and the electronic conductivity z (mS / cm) of the positive electrode active material is 1.0 or more. In the present invention, the "solid content" in the positive electrode slurry means the positive electrode active material and the conductive additive, and does not include the electrolyte. In this way, a positive electrode active material whose electronic conductivity has been increased to a specific level and a specific surface area of 100 m 2 By using a conductive additive having a specific surface area of 1 / g or more and controlling the relationship between the specific surface area and the content of the conductive additive, it is possible to improve the adhesion of the resulting slurry-like positive electrode active material layer to a current collector, even when a conductive additive with a high specific surface area is used, and the resulting electrode has excellent electronic conductivity. As a result, a nonaqueous electrolyte secondary battery having this slurry-like positive electrode active material layer has excellent cycle characteristics.
[0014] The positive electrode slurry of the present invention contains an electrolyte (that is, contains an electrolytic solution in which an electrolyte is added to a dispersion medium).
[0015] Specific surface area x (m 2 / g) and the content y (mass%) of this conductive additive in the positive electrode slurry solid content satisfy 5≦x×y≦420, preferably 7≦x×y≦401, more preferably 9≦x×y≦300, and even more preferably 9≦x×y≦280. The smaller the value of x×y (the value obtained by multiplying x by y), the more excellent the adhesion, electronic conductivity, and cycle characteristics tend to be.
[0016] The "specific surface area x" can be measured by the BET method as follows. -BET specific surface area measurement method- 0.2 g of the conductive additive is dried at 120°C for 6 hours, and then measured using a BELSORP mini (product name) manufactured by Microtrac under the following measurement conditions: Adsorption temperature: 77K Adsorption gas: N 2 Equilibration time: 100 seconds Purge gas: He
[0017] Furthermore, the above-mentioned "content y of the conductive additive in the solid content of the positive electrode slurry" refers to, for example, the proportion of the conductive additive in the total content of the positive electrode active material and the conductive additive when the solid content of the positive electrode slurry is composed of the positive electrode active material and the conductive additive.
[0018] Specific surface area x (m 2 / g) is not particularly limited as long as the relationship between x and y is satisfied, and 2 / g or more is preferable, and 180m 2 The upper limit is not particularly limited. For example, when the specific surface area x is 1500 m 2 The specific surface area x of the conductive additive is 100 to 1500 m 2 / g, and 100 to 1200m 2 / g, and more preferably in the range of 150 to 1000m 2 / g, and more preferably in the range of 150 to 900m 2 It is more preferable that the range is / g.
[0019] The content y (mass%) of the conductive additive in the positive electrode slurry solid content is not particularly limited as long as the relationship between x and y is satisfied, and is preferably 0.03 to 4.00 mass%, more preferably 0.03 to 2.00 mass%, even more preferably 0.05 to 1.00 mass%, still more preferably 0.05 to 0.80 mass%, still more preferably 0.05 to 0.50 mass%, still more preferably 0.05 to 0.45 mass%, still more preferably 0.05 to 0.30 mass%, still more preferably 0.05 to 0.20 mass%, and particularly preferably 0.05 to 0.10 mass%.
[0020] The electron conductivity z (mS / cm) of the positive electrode active material is 1.0 or more, preferably 1.2 or more. There is no particular upper limit, and a practical upper limit is 8.0 or less. The range of electron conductivity z is preferably 1.0 to 8.0, more preferably 1.0 to 7.0, even more preferably 1.2 to 6.0, still more preferably 1.2 to 5.0, even more preferably 1.2 to 4.0, still more preferably 1.2 to 3.0, and particularly preferably 1.2 to 2.5. When the electron conductivity z of the positive electrode active material is within the above range, the specific surface area of 100 m2 By using the cathode active material in combination with a conductive additive of 1 / g or more and satisfying the relationship between the specific surface area and the content of the conductive additive, the adhesion and the battery performance of the resulting battery can be improved while sufficiently increasing the electronic conductivity in the resulting cathode active material layer. The electronic conductivity of the cathode active material can be controlled by selecting the constituent materials of the cathode active material, applying a surface coating layer to the cathode active material, or the like. The electronic conductivity of the cathode active material can be measured by the method described in the Examples.
[0021] Preferably, the specific surface area x of the conductive additive, the content y of the conductive additive, and the electronic conductivity z of the positive electrode active material further satisfy z≦(−0.0175×x×y) + 10. When this relationship is satisfied, the adhesion, electronic conductivity, and cycle characteristics of the positive electrode active material layer tend to be further improved.
[0022] The electrical resistance of the surface of the positive electrode active material (particles) is not particularly limited. For example, 8 Ω or less, and may be 1.2×10 8 Ω or less, more preferably 1.0×10 8 It is more preferable that the electrical resistance is 3.0×10 Ω or less. 7 ~2.0 x 10 8 Ω, and preferably 3.0×10 7 ~1.2 × 10 8 Ω, and preferably 3.0×10 7 ~6.0 x 10 7 Ω, more preferably 3.0×10 7 ~5.0 x 10 7 Ω, more preferably 3.5×10 7 ~5.0 x 10 7 It is more preferable that the electrical resistance is Ω. The lower the electrical resistance, the higher the electronic conductivity. In the present invention, it is preferable to use a positive electrode active material whose electronic conductivity is increased to a specific range. The electrical resistance of the surface of the positive electrode active material can be controlled by selecting the constituent materials of the positive electrode active material, surface coating treatment, etc. The electrical resistance of the surface of the positive electrode active material can be measured by the method described in the Examples.
[0023] The carbon content of the surface of the positive electrode active material layer formed using the positive electrode slurry of the present invention is not particularly limited, but is preferably 6.5% by mass or less, more preferably 5.6% by mass or less, even more preferably 5.3% by mass or less, even more preferably 5.0% by mass or less, even more preferably 4.5% by mass or less, even more preferably 4.2% by mass or less, even more preferably 3.5% by mass or less, and even more preferably 3.3% by mass or less. Here, the carbon content of the surface of the positive electrode active material layer corresponds to the carbon content derived from carbon-containing components contained in the positive electrode active material layer (e.g., a surface coating of the positive electrode active material, a conductive additive, etc.). When the carbon content is 4.5% by mass or less, adhesion to the current collector, electronic conductivity, and output characteristics tend to be further improved. The carbon content of the positive electrode active material layer surface is preferably 2.5 to 6.5% by mass, more preferably 2.5 to 5.6% by mass, even more preferably 2.5 to 5.3% by mass, even more preferably 2.5 to 5.0% by mass, even more preferably 2.5 to 4.5% by mass, even more preferably 2.5 to 4.2% by mass, even more preferably 2.5 to 4.0% by mass, even more preferably 2.5 to 3.5% by mass, even more preferably 2.5 to 3.4% by mass, even more preferably 2.5 to 3.3% by mass. The carbon content of the positive electrode active material layer surface can be measured using energy dispersive X-ray spectroscopy (SEM-EDX) by the method described in the examples.
[0024] In Raman spectroscopic analysis of the surface of a positive electrode active material (particle), the ratio of the G band peak intensity to the D band peak intensity (G / D, also referred to as the G-D ratio) is preferably 0.5 to 4.0. The G-D ratio is considered to indicate the crystalline state of the surface coating of the positive electrode active material surface. A higher G-D ratio indicates higher crystallinity (fewer defects). A G-D ratio within the above range is preferable in that the electronic conductivity z of the positive electrode active material can be controlled within an appropriate range. The G-D ratio is preferably 0.5 to 3.5, preferably 0.5 to 3.0, preferably 0.5 to 2.0, more preferably 0.7 to 1.3, even more preferably 0.8 to 1.2, even more preferably 0.9 to 1.2, and even more preferably 1.0 to 1.2. The G-D ratio can be measured by Raman spectroscopic analysis using the method described in the Examples.
[0025] Each component constituting the positive electrode slurry of the present invention will be described in more detail below.
[0026] <Positive electrode active material> The positive electrode active material is preferably one that can reversibly insert and release lithium ions. There are no particular limitations on the material as long as it exhibits the above-mentioned electronic conductivity, and it may be a transition metal oxide, an organic substance, an element that can be composited with Li, such as sulfur, or a composite of sulfur and a metal. Among them, it is preferable to use a lithium-containing transition metal oxide as the positive electrode active material, and a transition metal element M a A transition metal oxide containing at least one element selected from Co, Ni, Fe, Mn, Cu, and V is more preferred. b (Elements of Group 1 (Ia) of the periodic table other than lithium, elements of Group 2 (IIa), Al, Ga, In, Ge, Sn, Pb, Sb, Bi, Si, P, B, etc.) may be mixed. The amount of the mixed element may be determined by the following formula: a The amount of Li / M is preferably 0 to 30 mol % relative to the amount of Li / M (100 mol %). aMore preferably, the lithium-containing transition metal oxide is synthesized by mixing the above-mentioned components so that the molar ratio of the above-mentioned components is 0.3 to 2.2. Specific examples of the lithium-containing transition metal oxide include (MA) a transition metal oxide having a layered rock salt structure, (MB) a transition metal oxide having a spinel structure, (MC) a lithium-containing transition metal phosphate compound, (MD) a lithium-containing transition metal halide phosphate compound, and (ME) a lithium-containing transition metal silicate compound.
[0027] (MA) Specific examples of transition metal oxides having a layered rock salt structure include LiCoO 2 (Lithium cobalt oxide [LCO]), LiNi 2 O 2 (lithium nickel oxide), LiNi 0.85 Co 0.10 Al 0.05 O 2 (nickel cobalt lithium aluminum oxide [NCA]), LiNi 1/3 Co 1/3 Mn 1/3 O 2 (Lithium nickel manganese cobalt oxide [NMC]) and LiNi 0.5 Mn 0.5 O 2 (Lithium manganese nickel oxide). (MB) Specific examples of transition metal oxides having a spinel structure include LiMn 2 O 4 (LMO), LiCoMnO 4 , Li 2 FeMn 3 O 8 , Li 2 CuMn 3 O 8 , Li 2 CrMn 3 O 8 and Li 2 NiMn 3 O 8 Examples of the (MC) lithium-containing transition metal phosphate compound include LiFePO 4 and Li 3 Fe 2 (P.O. 4 ) 3 Olivine-type iron phosphate salts such as LiFeP 2 O7 Iron pyrophosphates such as LiCoPO 4 Cobalt phosphates such as Li 3 V 2 (P.O. 4 ) 3 (MD) Examples of lithium-containing transition metal halide phosphate compounds include, for example, Li 2 FePO 4 Fluorophosphate iron salts such as F, Li 2 MnPO 4 Fluorophosphate manganese salts such as F and Li 2 CoPO 4 Examples of the (ME) lithium-containing transition metal silicate compound include cobalt fluoride phosphates such as Li 2 FeSiO 4 , Li 2 MnSiO 4 and Li 2 CoSiO 4 In the present invention, the positive electrode active material is preferably a lithium-containing transition metal phosphate compound (MC), such as LiFePO 4 is more preferred.
[0028] The shape of the positive electrode active material is not particularly limited, but particulate form is preferred. The average particle size (average particle size in equivalent spheres) of the positive electrode active material is not particularly limited. For example, it can be 0.1 to 50 μm, preferably 0.2 to 30 μm, more preferably 0.5 to 20 μm, and even more preferably 0.8 to 10 μm. A conventional grinder or classifier can be used to adjust the positive electrode active material to a predetermined particle size. The positive electrode active material obtained by the calcination method may be used after washing with water, an acidic aqueous solution, an alkaline aqueous solution, or an organic solvent.
[0029] When a commercially available positive electrode active material is used, the average particle size of the positive electrode active material is the value listed in the manufacturer's catalog. When the manufacturer's average particle size information is unavailable or when a synthesized positive electrode active material is used, the positive electrode active material is dispersed in water and the average particle size (volume-based median diameter D50 in water) obtained by measurement using a laser diffraction / scattering particle size distribution measurement device (e.g., HORIBA Particle LA-960V2) is used. This also applies to the average particle size of solid particles other than the positive electrode active material.
[0030] The chemical formula of the compound obtained by the above calcination method can be measured by inductively coupled plasma (ICP) emission spectroscopy, or simply calculated from the difference in mass of the powder before and after calcination.
[0031] The surface of the positive electrode active material may be coated with an oxide such as another metal oxide, a carbon-based material, or the like. These surface coating layers can function as an interface resistance stabilizing layer. Examples of surface coating materials include metal oxides containing Ti, Nb, Ta, W, Zr, Al, Si, or Li. Specific examples include titanate spinel, tantalum-based oxides, niobium-based oxides, and lithium niobate-based compounds, such as Li 4 Ti 5 O 12 , Li 2 Ti 2 O 5 , LiTaO 3 , LiNbO 3 , LiAlO 2 , Li 2 ZrO 3 , Li 2 WO 4 , Li 2 TiO 3 , Li 2 B 4 O 7 , Li 3 P.O. 4 , Li 2 MoO 4 , Li 3 BO 3 , LiBO 2 , Li 2 CO 3 , Li 2 SiO 3, SiO 2 , TiO 2 , ZrO 2 , Al 2 O 3 , B 2 O 3 , and Li 3 AlF 6 Carbon-based materials such as C, SiC, and SiOC (carbon-doped silicon oxide) can also be used as the surface coating material.
[0032] The positive electrode active material is preferably surface-coated with a carbonaceous material from the viewpoint of increasing the electronic conductivity to a desired level. The positive electrode active material is preferably surface-coated with carbon (C). The carbon surface coating can be formed by baking the positive electrode active material in the presence of an additive (organic substance) that serves as a carbon source. Examples of the additive that can be used include styrene-maleic anhydride copolymer, polystyrene, and polycarbonate.
[0033] The surface of the positive electrode active material may be treated with sulfur or phosphorus. Furthermore, the particle surfaces of the positive electrode active material may be treated with actinic rays or an active gas (plasma, etc.) before or after the surface coating.
[0034] The positive electrode active materials may be used alone or in combination of two or more.
[0035] The content of the positive electrode active material in the positive electrode slurry solids varies depending on the content y of the conductive additive, but is preferably 96.00 to 99.97 mass%, more preferably 98.00 to 99.97 mass%, even more preferably 99.00 to 99.95 mass%, still more preferably 99.20 to 99.95 mass%, still more preferably 99.50 to 99.95 mass%, still more preferably 99.55 to 99.95 mass%, still more preferably 99.70 to 99.95 mass%, and still more preferably 99.90 to 99.95 mass%.
[0036] <Conductive additive> The conductive additive is a material having a specific surface area of 100 m 2 / g or more, there are no particular limitations, and those known as common conductive additives can be used. For example, the conductive additive may be an electron-conductive material such as graphites such as natural graphite and artificial graphite, carbon blacks such as acetylene black, ketjen black, and furnace black, amorphous carbon such as needle coke, carbon fibers such as vapor-grown carbon fibers or carbon nanotubes, or carbonaceous materials such as graphene or fullerene. Metal powders or metal fibers such as copper and nickel may also be used. Conductive polymers such as polyaniline, polypyrrole, polythiophene, polyacetylene, and polyphenylene derivatives may also be used. In the present invention, the conductive additive is preferably a carbonaceous material, more preferably carbon blacks, and more preferably ketjen black. When a positive electrode active material and a conductive additive are used in combination, those conductive additives that do not intercalate or deintercalate Li during charging and discharging the battery and do not function as an active material are considered to be conductive additives. Therefore, among conductive additives, those that can function as an active material in the active material layer during charging and discharging the battery are classified as active materials rather than conductive additives. Whether or not a material functions as an active material when the battery is charged and discharged is not uniquely determined, but is determined by the combination with the active material.
[0037] Examples of commercially available conductive additives include the following: Ketjen black: carbon ECP (specific surface area = 890 m 2 / g), carbon ECP600JD (specific surface area = 1480 m 2 / g), carbon ECP200L (specific surface area = 430 m 2 / g) (both manufactured by Lion Corporation), carbon black: LITX300 (specific surface area = 180 m 2 / g), LITX-HP (specific surface area = 100 m 2 / g) (both manufactured by CABOT Corporation) Carbon nanotubes (CNT): BT1001M (specific surface area = 272 m 2 / g), BT1003M (specific surface area = 230 m 2 / g) (both manufactured by LG), JENOTUBE6A (specific surface area = 680 m 2 / g), JENOTUBE10B (specific surface area = 230m 2 / g) (both from JEIO)
[0038] The conductive additive may be used alone or in combination of two or more.
[0039] The shape of the conductive additive is not particularly limited, but is preferably particulate. The average particle size (average particle size in equivalent sphere form) of the conductive additive is not particularly limited. For example, it is preferably 0.01 to 50 μm, more preferably 0.1 to 10 μm, and even more preferably 0.2 to 2.0 μm.
[0040] The conductive additive may be surface-treated. The surface treatment method is not particularly limited, and preferred are surface treatment using a chemical treatment agent and atomic layer deposition (ALD) treatment. Preferred examples of the chemical treatment agent include organosilicon compounds (more preferably, silane coupling agents) and organic phosphonic acid compounds, such as methyltrimethoxysilane (MTMS), octadecyltrimethoxysilane, hexamethyldisilazane, tetraethoxysilane, trifluoropropyltrimethoxysilane, vinyltrimethoxysilane, phenyltrimethoxysilane, 3-aminopropyltriethoxysilane, 1H,1H,2H,2H-perfluorooctyltriethoxysilane, trimethoxy(octyl)silane, 1H,1H,2H,2H-perfluorooctanephosphonic acid, 1-octylphosphonic acid, and perfluoropolyethertriethoxysilane (KY1903 (trade name)). In the ALD process, the layer to be deposited is HfO 2 , SiO 2 , ZrO 2 , Ta 2 O 5 , TiO 2 The following can be mentioned:
[0041] <Electrolyte> The electrolyte may be any electrolyte used in electrolytic solutions for quasi-solid secondary batteries. Metal salts are preferred, including lithium salts, potassium salts, sodium salts, calcium salts, and magnesium salts. The lithium salt is preferably a lithium salt commonly used in electrolytes for lithium ion secondary batteries, including, for example, the following lithium salts:
[0042] (L-1) Inorganic lithium salt: LiPF6 , LiBF 4 , LiAsF 6 , LiSbF 6 Inorganic fluoride salts such as LiClO 4 , LiBrO 4 , LiIO 4 perhalogenates such as LiAlCl 4 Inorganic chloride salts, etc.
[0043] (L-2) Fluorine-containing organic lithium salt: LiCF 3 SO 3 perfluoroalkanesulfonates such as LiN(CF 3 SO 2 ) 2 , LiN(CF 3 CF 2 SO 2 ) 2 , LiN(FSO 2 ) 2 , LiN(CF 3 SO 2 ) (C 4 F 9 SO 2 perfluoroalkanesulfonylimide salts such as LiC(CF 3 SO 2 ) 3 perfluoroalkanesulfonylmethide salts such as Li[PF 5 (CF 2 CF 2 CF 3 ) )], Li[PF 4 (CF 2 CF 2 CF 3 ) 2 ], Li[PF 3 (CF 2 CF 2 CF 3 ) 3 ], Li[PF 5 (CF 2 CF 2 CF 2 CF 3 ) )], Li[PF 4 (CF 2 CF 2 CF 2 CF 3 ) 2 ], Li[PF3 (CF 2 CF 2 CF 2 CF 3 ) 3 perfluoroalkyl fluorophosphates such as
[0044] (L-3) Oxalatoborate salts: lithium bis(oxalato)borate, lithium difluorooxalatoborate, etc.
[0045] Among these, LiPF 6 , LiBF 4 , LiAsF 6 , LiSbF 6 , LiClO 4 , Li(R f1 SO 3 ), LiN(R f1 SO 2 ) 2 , LiN(FSO 2 ) 2 , or LiN(R f1 SO 2 ) (R f2 SO 2 ) is preferred, and LiPF 6 , LiBF 4 , LiN(R f1 SO 2 ) 2 , LiN(FSO 2 ) 2 , or LiN(R f1 SO 2 ) (R f2 SO 2 ) is more preferred, and LiPF 6 is particularly preferred. f1 and R f2 Each of the groups represents a perfluoroalkyl group, and the number of carbon atoms is preferably 1 to 6. The lithium salts used in the electrolytic solution of the present invention may be used alone or in any combination of two or more.
[0046] In the present invention, it is preferable to add the above-mentioned electrolyte to a dispersion medium and use it as an electrolytic solution. The concentration of the lithium salt in the electrolytic solution is usually 10.0 to 50.0 mass %, preferably 15.0 to 30.0 mass %, and the molar concentration is preferably 0.5 to 1.5 M.
[0047] <Dispersion medium> A non-aqueous solvent is used as the dispersion medium. As the non-aqueous solvent, an aprotic organic solvent is preferred, and among these, an aprotic organic solvent having 2 to 10 carbon atoms is more preferred. Examples of such non-aqueous solvents include linear or cyclic carbonate compounds, lactone compounds, linear or cyclic ether compounds, ester compounds, nitrile compounds, amide compounds, oxazolidinone compounds, nitro compounds, linear or cyclic sulfone or sulfoxide compounds, and phosphate ester compounds. Compounds having an ether bond, carbonyl bond, ester bond, or carbonate bond are preferred. These compounds may have a substituent.
[0048] Examples of non-aqueous solvents include ethylene carbonate, fluorinated ethylene carbonate, vinylene carbonate, propylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, methyl propyl carbonate, γ-butyrolactone, γ-valerolactone, 1,2-dimethoxyethane, tetrahydrofuran, 2-methyltetrahydrofuran, tetrahydropyran, 1,3-dioxolane, 4-methyl-1,3-dioxolane, 1,3-dioxane, 1,4-dioxane, and methyl acetate. , ethyl acetate, methyl propionate, ethyl propionate, methyl butyrate, methyl isobutyrate, methyl trimethylacetate, ethyl trimethylacetate, acetonitrile, glutaronitrile, adiponitrile, methoxyacetonitrile, 3-methoxypropionitrile, N,N-dimethylformamide, N-methylpyrrolidone (NMP), N-methyloxazolidinone, N,N'-dimethylimidazolidinone, nitromethane, nitroethane, sulfolane, trimethyl phosphate, dimethyl sulfoxide, dimethyl sulfoxide phosphate, etc. These may be used alone or in combination of two or more. Among these, at least one selected from the group consisting of ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, and γ-butyrolactone is preferred, and a combination of a high-viscosity (high-dielectric constant) solvent (e.g., relative dielectric constant ε≧30) such as ethylene carbonate or propylene carbonate with a low-viscosity solvent (e.g., viscosity≦1 mPa·s) such as dimethyl carbonate, ethyl methyl carbonate, or diethyl carbonate is more preferred. Using a mixed solvent of such a combination improves the dissociation of the electrolyte salt and the mobility of ions. A combination of ethylene carbonate, dimethyl carbonate, and ethyl methyl carbonate is particularly preferred as the nonaqueous solvent. However, the nonaqueous solvent used in the present invention is not limited to these. The dispersion medium is preferably a mixed solvent of ethylene carbonate (EC), dimethyl carbonate (DMC), and ethyl methyl carbonate (EMC).
[0049] The positive electrode slurry of the present invention does not contain a binder. The binder here refers to a binder used in general nonaqueous electrolyte secondary batteries, and includes, for example, thermoplastic resins such as fluororesins (polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF), etc.), polyethylene, polypropylene, polyacrylic, and polyimide; elastomers such as ethylene-propylene-diene rubber (EPDM), sulfonated EPDM, styrene-butadiene rubber (SBR), and fluororubber; and polysaccharide polymers.
[0050] The positive electrode slurry of the present invention preferably has a solids content of more than 60% by mass, more preferably 65% by mass or more, and even more preferably 70% by mass or more, and the solids content is preferably 60 to 95% by mass, more preferably 65 to 92% by mass, even more preferably 70 to 90% by mass, still more preferably 72 to 88% by mass, and particularly preferably 75 to 85% by mass.
[0051] <Other Components> The positive electrode slurry of the present invention may optionally contain an ionic liquid, a thickener, an antifoaming agent, a leveling agent, a dehydrating agent, an antioxidant, etc. These may be those typically used in nonaqueous electrolyte secondary batteries. When the positive electrode slurry of the present invention contains other components, the amount of the other components is preferably 0.05 to 1.5 parts by mass, more preferably 0.1 to 1.0 parts by mass, per 100 parts by mass of the total content of the positive electrode active material and the conductive additive.
[0052] [Non-aqueous electrolyte secondary battery] The non-aqueous electrolyte secondary battery of the present invention (hereinafter also referred to as "secondary battery of the present invention") has a positive electrode, a separator, and a negative electrode in this order, and uses the above-mentioned positive electrode slurry of the present invention as the positive electrode active material layer.
[0053] Prior to describing the secondary battery of the present invention, the structure of a general nonaqueous electrolyte secondary battery will be described. FIG. 1 is a cross-sectional view showing a schematic representation of the laminated structure of a general nonaqueous electrolyte secondary battery 10, including the working electrode when the battery is operated. The nonaqueous electrolyte secondary battery 10 has a laminated structure (hereinafter also referred to as an electrode laminate) including, as viewed from the negative electrode side, a negative electrode current collector 1, a negative electrode active material layer 2, a separator 3, a positive electrode active material layer 4, and a positive electrode current collector 5, in this order. The negative electrode active material layer 2 and the positive electrode active material layer 4 are filled with a nonaqueous electrolyte (not shown) and separated by the separator 3. The separator 3 has pores, and during normal battery use, functions as a separator between the positive and negative electrodes, insulating them by allowing the electrolyte and ions to pass through the pores. With this structure, for example, in the case of a lithium-ion secondary battery, electrons (e - ) is supplied, and at the same time, lithium ions (Li + ) moves and accumulates in the negative electrode. On the other hand, during discharge, the lithium ions (Li + ) is returned to the positive electrode side through the electrolyte, and electrons are supplied to the operating part 6. In the illustrated example, a light bulb is used as the operating part 6, and it is lit by discharge.
[0054] Next, the basic structure characteristic of quasi-solid secondary batteries will be described. As described above, in quasi-solid secondary batteries, the electrode active material layer is formed in a slurry state containing an electrode active material and an electrolyte. Therefore, the electrode active material layer is a layer using a slurry (suspension, dispersion) in which the electrode active material is dispersed in a non-aqueous electrolyte, which distinguishes the structure from a typical non-aqueous electrolyte secondary battery. That is, in a typical non-aqueous electrolyte secondary battery, a coating solution is prepared by dispersing the electrode active material in a medium that does not contain an electrolyte, and the coating solution is applied to a current collector to form a coating film. The coating film is then dried to form a thin-film electrode active material layer. This coating solution usually contains a binder, which firmly binds the electrode active material particles together to form a hard electrode active material layer. Since the non-aqueous electrolyte is present on the electrode active material layer thus formed (between the negative electrode active material layer and the positive electrode active material layer), even if there are portions in the electrode active material layer that can be penetrated by the non-aqueous electrolyte, the electrode active material layer is in the form of a hard solid particle layer overall, not a slurry layer. In contrast, in a quasi-solid secondary battery, the electrode active material layer is an electrode slurry layer formed by dispersing solid particles containing an electrode active material and a conductive additive in a non-aqueous electrolyte solution obtained by dissolving a lithium salt (electrolyte) in a non-aqueous solvent. For this electrode slurry layer to function as an electrode active material layer, strong binding between the electrode active material particles is not required, and therefore the electrode slurry layer usually does not contain a binder. Except for the fact that the electrode active material layer is an electrode slurry layer and that the electrode slurry layer is in contact with the separator, the basic layer configuration of a quasi-solid secondary battery is the same as the layer configuration shown in FIG. 1 .
[0055] In the secondary battery of the present invention, the positive electrode active material layer is a slurry layer formed from the positive electrode slurry of the present invention, and the negative electrode active material layer can be a negative electrode active material layer formed from a conventional negative electrode slurry.
[0056] In the secondary battery of the present invention, the materials and components such as the positive electrode current collector, negative electrode active material, negative electrode current collector, and separator are not particularly limited, except that the positive electrode slurry of the present invention is used to form the positive electrode active material layer. These materials and components can be appropriately applied to those used in ordinary secondary batteries. For components and manufacturing methods typically used in these secondary batteries, reference can be made to, for example, JP 2016-201308 A, JP 2005-108835 A, JP 2012-185938 A, WO 2018 / 135395, and the like.
[0057] In the secondary battery of the present invention, the thickness of the positive electrode active material layer (slurry layer) is not particularly limited and may be, for example, 5 to 500 μm, preferably 20 to 300 μm. In the secondary battery of the present invention, the thickness of the negative electrode active material layer is not particularly limited and may be, for example, 5 to 500 μm, preferably 20 to 300 μm.
[0058] [Method for Manufacturing Nonaqueous Electrolyte Secondary Battery] The method for manufacturing a nonaqueous electrolyte secondary battery of the present invention includes applying the positive electrode slurry of the present invention to a positive electrode current collector to form a slurry-like positive electrode active material layer. The method for applying the slurry is not particularly limited, and can be, for example, application using a roll coater, drop coating, applying the slurry evenly to the current collector and then pressing (roll press or flat press), or applying the slurry by placing it within a frame of a specified thickness and spreading it. Regarding the method for manufacturing the nonaqueous electrolyte secondary battery of the present invention, any conventional method can be appropriately adopted, except that the positive electrode active material layer is formed using a specific positive electrode slurry. For example, JP 2016-201308 A, JP 2005-108835 A, JP 2012-185938 A, JP 2017-147222 A, etc. can be appropriately referenced.
[0059] The nonaqueous electrolyte secondary battery of the present invention can be installed in electronic devices such as notebook computers, pen-input personal computers, mobile personal computers, electronic book players, mobile phones, cordless phone handsets, pagers, handheld terminals, portable fax machines, portable copiers, portable printers, headphone stereos, video camcorders, LCD televisions, handheld vacuum cleaners, portable CD players, mini-discs, electric shavers, transceivers, electronic organizers, calculators, memory cards, portable tape recorders, radios, backup power supplies, and memory cards. It can also be installed in consumer electronic devices such as automobiles, electric vehicles, motors, lighting fixtures, toys, game devices, road conditioners, clocks, flash devices, cameras, and medical devices (pacemakers, hearing aids, shoulder massagers, etc.). It can also be used for various military and space applications. It can also be combined with solar cells.
[0060] The present invention will be described in more detail below with reference to examples, but the present invention should not be construed as being limited thereto.
[0061] <Preparation of Positive Electrode Active Material> LFP (LiFePO 4 10 parts by mass of powder raw material (Gelon, particle size 2.5 μm) was mixed with 90 parts by mass of water, and a styrene-maleic anhydride copolymer was added as an additive in the amount shown in Table 1, followed by stirring and mixing for 3 hours. This was then baked at 700°C for 10 hours in a nitrogen atmosphere to obtain positive electrode active materials LFP1, LFP1-2, LFP2, LFP3, LFP4, and LFP5, each surface-coated with a carbon-based material.
[0062] NCM (LiNi 1/3 Co 1/3 Mn 1/3 O 2 10 parts by mass of a powder raw material (NCM111 (trade name), particle size 8 μm, manufactured by Toshima Manufacturing Co., Ltd.) was mixed with 90 parts by mass of water, and a styrene-maleic anhydride copolymer was added as an additive in the amount shown in Table 1, followed by stirring and mixing for 3 hours. This was then baked at 700°C for 10 hours in a nitrogen atmosphere, yielding positive electrode active materials NCM1 and NCM2 whose surfaces were coated with a carbon-based material.
[0063] <Measurement of Electronic Conductivity of Positive Electrode Active Material> The electronic conductivity of each positive electrode active material obtained above was measured by the following method. 30 mg of the positive electrode active material was placed in a cylindrical tube with an inner diameter of 10 mm and pressed at 10 MPa to obtain a pressed product of the positive electrode active material (thickness: approximately 0.15 mm). Then, stainless steel rods with a diameter of 10 mm were inserted through the upper and lower openings of the tube, and the ends of the rods were placed so as to contact the surface of the pressed product. A constant voltage of 10 mV was applied to measure the resistance. The measurement was performed three times (N3), and the average of the obtained resistance values was calculated to obtain the powder resistance (mΩ). The electronic conductivity (mS / cm) of the positive electrode active material was calculated using the obtained powder resistance according to the following formula. In the formula below, the film thickness refers to the thickness (cm) of the pressed product, and the area refers to the area (cm) of the circular surface (one side) of the pressed product. 2 ) For the resistance measurement, an electrochemical measurement device (VMP-300 (trade name), manufactured by BIOLOGIC) was used. The measurement results are shown in Table 1. Electronic conductivity = 1 ÷ powder resistance × film thickness ÷ area
[0064]
[0065] <Preparation of Conductive Aid> The following conductive aids were prepared: AB: Li-100 (trade name), acetylene black, specific surface area = 69 m 2 / g, Denka ECP600JD: Carbon ECP600JD (trade name), Ketjen Black, specific surface area = 1480 m 2 / g, LITX300 (trade name), carbon black, specific surface area = 180 m 2 / g, CABOT Carbon ECP: Carbon ECP (trade name), Ketjen Black, specific surface area = 890 m 2 / g, manufactured by Lion
[0066] <Preparation of non-aqueous electrolyte solution A> A mixed solvent of ethylene carbonate (EC), dimethyl carbonate (DMC), and ethyl methyl carbonate (EMC) in a mass ratio of EC:DMC:EMC=3:4:3 was added to the non-aqueous electrolyte solution A. 6 These were mixed to a concentration of 1M to prepare a non-aqueous electrolyte solution (non-aqueous electrolyte solution A).
[0067] <Preparation of Positive Electrode Slurry> The positive electrode active material and conductive additive, and nonaqueous electrolyte A listed in Table 2 were mixed for 90 seconds at 1250 rpm in a centrifugal planetary mixer (Thinky Corporation: Awatori Rentaro (product name)) to obtain a positive electrode slurry. The contents of each component in this positive electrode slurry were as follows. The positive electrode active material and conductive additive were used in amounts such that the respective contents of the positive electrode active material and conductive additive relative to the total of the positive electrode active material and conductive additive were the proportions (mass %) listed in Table 2. The amount of nonaqueous electrolyte A in the positive electrode slurry was 15 ml, so that the solids content of the positive electrode slurry was 75 mass %. In this way, a positive electrode slurry containing the positive electrode active material, conductive additive, and electrolyte was obtained.
[0068] <Electrical Resistance of Positive Electrode Active Material Particle Surface> As an index of the conductivity of the positive electrode active material particle surface, the electrical resistance of the positive electrode active material particle surface was measured using an atomic force microscope (AFM) as follows. 10 mg of positive electrode active material particles were adhered to carbon tape and placed on the sample stage of a scanning probe microscope (PeakForce TUNA (trade name), manufactured by Bruker). The cantilever of the microscope was brought close to the positive electrode active material particles, and the current value I (unit: nA) flowing when a voltage was applied was measured in ultra-low current measurement mode. A voltage was applied from -1.5 V to +1.5 V in 0.1 V increments. In this way, 31 data points of the current value I versus the voltage value V were obtained. The obtained voltage value V and current value I were fitted with a straight line (the following formula) to obtain the electrical resistance value R (Ω) as the slope. V = RI (formula)
[0069] <Carbon Amount on Positive Electrode Active Material Layer Surface> Each positive electrode obtained in the same manner as in <Preparation of Nonaqueous Electrolyte Secondary Battery> below was punched out to a diameter of 10 mm, and the positive electrode active material layer surface (the surface opposite to the positive electrode current collector) was observed using a field emission scanning electron microscope (FE-SEM) (manufactured by JEOL Ltd., JSM 7100F (trade name)) at an acceleration voltage of 1.5 kV, and elemental analysis was performed by automatic detection using an energy dispersive X-ray spectroscope (EDX) (manufactured by Thermo Fisher Scientific, Noran System 7 (trade name)). The mass ratio of the carbon amount to the total element amount detected by the automatic detection was defined as the C amount (mass %) on the surface of the positive electrode active material layer.
[0070] <G-D ratio of the surface of the positive electrode active material particles> 10 mg of each of the positive electrode active material particles obtained above was adhered to a carbon tape, and a Raman spectrum was obtained by irradiating a 532 nm laser using a confocal Raman microscope (manufactured by Renishaw, inVia Qontor (trade name)). -1 ) peak intensity of the G band (wavenumber 1600 cm -1 The G / D ratio of each of the positive electrode active materials LFP1-2, LFP2 to LFP5, and NCM2 used in the examples was between 0.7 and 1.4.
[0071] <Method for Evaluating Adhesion (Adhesion Force) of Positive Electrode Active Material Layer to Current Collector> The positive electrode slurry was applied to a horizontally placed aluminum current collector (length: 4.5 cm, width: 6.5 cm) to a thickness of 300 μm and a coating area of 4 cm square, to prepare a positive electrode consisting of the current collector and a slurry positive electrode active material layer. While maintaining the horizontal position, the area (S1) of the positive electrode active material layer was measured. The area was measured by taking an image of the positive electrode active material layer using a digital microscope imaging device (Keyence Corporation VHX-7000) and calculating the area of the positive electrode active material layer using the same device. Next, the positive electrode was placed on an adsorption plate so that the current collector was in contact with the adsorption plate and adsorbed to the adsorption plate. In this adsorption state, the adsorption plate was rotated 90° so that the surface of the positive electrode active material layer was perpendicular to the horizontal direction, fixed, and held for 1 minute. Thereafter, the adsorption plate was returned to a horizontal position so that the positive electrode active material layer was facing up, and within 15 seconds of returning it to a horizontal position, the area (S2) of the positive electrode active material layer was measured again. From S1 and S2, the area change rate before and after the fixation was calculated according to the following formula, and the obtained area change rate was applied to the following evaluation criteria and evaluated. If the positive electrode active material layer is in a powder state and collapses while being fixed vertically, S2 will be smaller than S1. If the fluidity in the positive electrode active material layer is high and the positive electrode active material layer sags while being fixed vertically, S2 will be larger than S1. (Area change rate) = |(S2) - (S1) | / (S1) × 100 (%) - Evaluation criteria - A: Less than 0.5% B: 0.5% or more and less than 1% C: 1% or more and less than 2% D: 2% or more and less than 3% E: 3% or more and less than 4% F: 4% or more and less than 5% G: 5% or more
[0072] <Method for evaluating the electronic conductivity of an electrode> The positive electrode slurry was applied to an aluminum current collector to a thickness of 300 μm and an area of 16 cm. 2After forming a positive electrode active material layer by coating so that the thickness was such ... 2 ) For the resistance measurement, an electrochemical measurement device (VMP-300 (trade name), manufactured by Biologic) was used. Electronic conductivity = 1 ÷ electrode resistance × film thickness ÷ area Evaluation criteria A: 20 mS / cm or more B: 16 mS / cm or more and less than 20 mS / cm C: 12 mS / cm or more and less than 16 mS / cm D: 8 mS / cm or more and less than 12 mS / cm E: 4 mS / cm or more and less than 8 mS / cm F: 2 mS / cm or more and less than 4 mS / cm G: Less than 2 mS / cm
[0073] <Preparation of Nonaqueous Electrolyte Secondary Battery> 1) Preparation of Positive Electrode: Each of the positive electrode slurries obtained above was applied to an aluminum current collector to a thickness of 300 μm to prepare a positive electrode consisting of a positive electrode current collector and a positive electrode active material layer (slurry). 2) Preparation of Negative Electrode: 64% by mass of artificial graphite (Showa Denko Kogyo, UF-G30 (product name)) as the negative electrode active material, 1% by mass of acetylene black (Denka Co., Ltd., Denka Black (product name)) as a conductive additive, and 35% by mass of nonaqueous electrolyte A were mixed in a centrifugal planetary mixer (Thinky Corporation: Awatori Rentaro (product name)) at 1250 rpm for 90 seconds to prepare a negative electrode-forming slurry. The negative electrode-forming slurry obtained above was applied to a copper current collector to a thickness of 300 μm to prepare a negative electrode consisting of a negative electrode current collector and a negative electrode active material layer (slurry). 3) Battery Fabrication Then, a separator was placed on the negative electrode, followed by a positive electrode, to form a laminate of negative electrode current collector-negative electrode active material layer (slurry)-separator-positive electrode active material layer (slurry)-positive electrode current collector. An aluminum tab was attached to the end of the aluminum current collector, and a nickel tab was attached to the end of the copper current collector by ultrasonic welding, to form an electrode assembly. This electrode assembly was sandwiched between two aluminum laminate films, and three sides were heat-sealed, with the remaining side vacuum-sealed to form a laminated battery (quasi-solid secondary battery).
[0074] <Cycle Characteristics> The laminated battery obtained above was charged and discharged under the following condition 1 to measure the initial discharge capacity, and then charged and discharged 200 times under the condition 2 to measure the discharge capacity at the 200th cycle (output evaluation discharge capacity). From the obtained initial discharge capacity and output evaluation discharge capacity, the discharge capacity retention rate was calculated using the following formula and evaluated according to the following evaluation criteria. The initial discharge capacity of all laminated batteries was 150 mAh / g. (Discharge capacity retention rate) = [(output evaluation discharge capacity) / (initial discharge capacity)] × 100 (%) - Condition 1 - Charge and discharge conditions for Experiments No. 1 to 25 and 29 to 35 (Experiments using LFP as the active material) Constant current (CC)-constant voltage (CV) charge: current value 10 mA, upper limit voltage 3.6 V, end current value 0.5 mA CC discharge: current value 10 mA, end voltage value 2.0 V Experiment No. Charge-discharge conditions for Experiments No. 26 to 28 (experiments using NMC as the active material) CC-CV charge: current value 10 mA, upper limit voltage 4.2 V, end current value 0.5 mA CC discharge: current value 10 mA, upper limit voltage 3.0 V - Condition 2 - Charge-discharge conditions for Experiments No. 1 to 25 and 29 to 35 (experiments using LFP as the active material) CC-CV charge: current value 10 mA, upper limit voltage 3.6 V, end current value 0.5 mA CC discharge: current value 10 mA, upper limit voltage 2.0 V Experiment No. Charge / discharge conditions 26 to 28 (experiments using NMC as the active material) CC-CV charge: current value 10 mA, upper limit voltage 4.2 V, final current value 0.5 mA CC discharge: current value 10 mA, upper limit voltage 3.0 V - Evaluation criteria - A: 95% or more B: 93% or more and less than 95% C: 91% or more and less than 93% D: 89% or more and less than 91% E: 87% or more and less than 89% F: 85% or more and less than 87% G: Less than 85%
[0075]
[0076] (Note for Table 2) The column "Satisfies formula A" indicates whether x, y, and z satisfy z≦(−0.0175×x×y)+10. If they do, it is marked as "TRUE," and if they do not, it is marked as "FALSE."
[0077]
[0078] The positive electrode slurries of Experiments 1 to 9, 18, 21, 25, and 26 did not satisfy either of the following conditions: the specific surface area x of the conductive additive and the content y of the conductive additive in the positive electrode slurry solids satisfy 5≦x×y≦420 and 100≦x, and the electronic conductivity z of the positive electrode active material does not satisfy 1.0 or more. The positive electrode active material layers formed using these positive electrode slurries had an area change rate of 5% or more (except for No. 26) in the above adhesion evaluation, and the electrode electronic conductivity was low at less than 2 mS / cm, resulting in poor adhesion to the current collector and poor electronic conductivity. The secondary batteries fabricated using these positive electrode slurries had a discharge capacity retention rate of less than 85%, resulting in poor cycle characteristics. Experiment No. The positive electrode slurries of Nos. 10 to 17, 19, 20, 22 to 24, and 27 to 35 satisfy the following: the specific surface area x of the conductive additive and the content y of the conductive additive in the positive electrode slurry solids satisfy 5≦x×y≦420 and 100≦x; and the electronic conductivity z of the positive electrode active material satisfies 1.0 or more. The positive electrode active material layers formed using these positive electrode slurries were excellent in adhesion to the current collector and electronic conductivity. The secondary batteries fabricated using these positive electrode slurries also had excellent cycle characteristics. The slurries of the present invention contain positive electrode active materials whose electronic conductivity is increased within a specific range and whose specific surface area is 100 m 2 / g or more of conductive additive and controlling the relationship between the specific surface area and content of the conductive additive, it is believed that the degree of absorption of the dispersion medium is controlled, making it less likely to become powdery, and ensuring adhesion to the current collector. In addition to adhesion, the positive electrode active material layer also has excellent electronic conductivity. As a result, it is believed that a secondary battery with excellent cycle characteristics was obtained. In particular, when formula A is satisfied, adhesion, electronic conductivity, and battery performance tended to be further improved. A reduced carbon content in the positive electrode active material layer tended to be preferable in terms of improving adhesion, electronic conductivity, and battery performance. This is believed to be because the amount of electrolyte absorbed by the carbonaceous component is reduced.
[0079] While the present invention has been described in connection with embodiments thereof, we do not intend to limit our invention to any of the details of the description unless otherwise specified, and believe that the claims should be construed broadly without departing from the spirit and scope of the invention as set forth in the appended claims.
[0080] This application claims priority based on Japanese Patent Application No. 2023-051784, filed on March 28, 2023, the contents of which are incorporated herein by reference as part of the present specification.
[0081] REFERENCE SIGNS LIST 10 Non-aqueous electrolyte secondary battery 1 Negative electrode current collector 2 Negative electrode active material layer 3 Separator 4 Positive electrode active material layer 5 Positive electrode current collector 6 Operating part (light bulb)
Claims
1. A slurry for forming a positive electrode of a non-aqueous electrolyte secondary battery containing a positive electrode active material, a conductive assistant, and an electrolyte, 2 / g) and a content y (mass %) of the conductive assistant in a solid content of the slurry for forming a positive electrode satisfy 5≦x×y≦420 and 100≦x, and an electronic conductivity z (mS / cm) of the positive electrode active material is 1.0 or more.
2. The positive electrode forming slurry according to claim 1, wherein x, y and z satisfy z≦(−0.0175×x×y)+10.
3. The electrical resistance of the surface of the positive electrode active material is 1.0×10 8 The positive electrode forming slurry according to claim 2 , having a resistance of Ω or less.
4. The slurry for forming a positive electrode according to claim 3, wherein the amount of carbon on the surface of the positive electrode active material layer formed using the slurry for forming a positive electrode is 5.0 mass % or less.
5. The positive electrode forming slurry according to claim 4, wherein in a Raman spectroscopic analysis of the surface of the positive electrode active material, the ratio of the peak intensity of G band to the peak intensity of D band (G / D) is 0.5 to 4.
0.
6. A non-aqueous electrolyte secondary battery having a positive electrode, a separator, and a negative electrode in this order, the positive electrode active material layer of which uses the positive electrode forming slurry according to any one of claims 1 to 5.
7. A method for producing a non-aqueous electrolyte secondary battery, comprising applying the positive electrode forming slurry according to any one of claims 1 to 5 onto a positive electrode current collector to form a positive electrode active material layer in a slurry form.
Citation Information
Patent Citations
Rechargeable lithium-ion secondary battery
JP2005108835A
Nonaqueous secondary battery
JP2012185938A
Nonaqueous electrolyte and nonaqueous secondary battery
JP2016201308A
Lithium-ion battery
JP2017147222A
Copper member
JP2023051784A