Positive electrode active material for non-aqueous electrolyte secondary batteries, and non-aqueous electrolyte secondary battery
The use of lithium-containing composite oxide with specific void structure in the positive electrode active material enhances battery capacity and retention in non-aqueous electrolyte secondary batteries, addressing existing limitations in lithium-ion batteries.
Patent Information
- Application Number
- PCT/JP2024/012367
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-29
- Filing Date
- 2024-03-27
- Publication Date
- 2024-10-03
Smart Images

Figure JP2024012367_03102024_PF_FP_ABST
Abstract
Description
Positive electrode active material for non-aqueous electrolyte secondary battery and non-aqueous electrolyte secondary battery
[0001] The present disclosure relates to a positive electrode active material for a non-aqueous electrolyte secondary battery and a non-aqueous electrolyte secondary battery using the positive electrode active material.
[0002] In recent years, non-aqueous electrolyte secondary batteries such as lithium-ion batteries have been widely used in applications requiring high capacity, such as automotive applications and power storage applications. The positive electrode active material, which is a main component of the positive electrode, has a significant impact on battery performance, such as capacity, durability (capacity retention rate), and charge / discharge efficiency. Therefore, much research has been conducted on the positive electrode active material.
[0003] For example, Patent Document 1 discloses a secondary particle having voids inside the secondary particle and a cross section of 1 μm in order to improve the capacity retention rate of the battery. 2 It is disclosed that a lithium composite metal oxide having 0.3 to 15 voids per pore is used as a positive electrode active material. 2 Only voids with an area of 1% or more are counted, and a void ratio of 1% or more and 50% or less is considered preferable.
[0004] JP 2016-169817 A
[0005] However, in non-aqueous electrolyte secondary batteries such as lithium ion batteries, there is still room for improvement in terms of improving battery capacity.
[0006] Therefore, an object of the present disclosure is to provide a positive electrode active material for a non-aqueous electrolyte secondary battery that can improve battery capacity, and a non-aqueous electrolyte secondary battery including the positive electrode active material for a non-aqueous electrolyte secondary battery.
[0007] The positive electrode active material for a non-aqueous electrolyte secondary battery according to the present disclosure has a lithium-containing composite oxide containing secondary particles formed by aggregation of primary particles, and the lithium-containing composite oxide has a field of view of 76.46 μm when a cross section of the secondary particle is observed. 2 The number of voids observed per field of view is 300 or more, and the field of view is 76.46 μm. 2 The median value of the nearest gap distance between voids observed per unit area is 170 nm or less.
[0008] The nonaqueous electrolyte secondary battery according to the present disclosure is characterized by including a positive electrode containing the above-described positive electrode active material for a nonaqueous electrolyte secondary battery, a negative electrode, and a nonaqueous electrolyte secondary battery.
[0009] According to the present disclosure, it is possible to improve battery capacity.
[0010] 1 is a cross-sectional view of a non-aqueous electrolyte secondary battery according to an embodiment of the present invention; 2 is a scanning electron microscope image of a cross section of a secondary particle of a lithium-containing composite oxide according to an embodiment of the present invention; 3 is a schematic diagram of a cross section of a secondary particle;
[0011] Hereinafter, with reference to the drawings, an example of an embodiment of a positive electrode active material for a nonaqueous electrolyte secondary battery according to the present disclosure and a nonaqueous electrolyte secondary battery including the positive electrode active material will be described. Note that selective combinations of the components of the multiple embodiments and modifications described below are within the scope of the present disclosure.
[0012] FIG. 1 is a cross-sectional view of a nonaqueous electrolyte secondary battery according to an embodiment. The nonaqueous electrolyte secondary battery 10 shown in FIG. 1 includes a wound electrode assembly 14 formed by winding a positive electrode 11 and a negative electrode 12 with a separator 13 interposed therebetween, a nonaqueous electrolyte, insulating plates 18 and 19 disposed above and below the electrode assembly 14, respectively, and a battery case 15 for accommodating the above components. The battery case 15 is composed of a cylindrical case body 16 with a bottom and a sealing body 17 that closes the opening of the case body 16. Note that, instead of the wound electrode assembly 14, other electrode bodies may be used, such as a laminated electrode body formed by alternately stacking positive and negative electrodes with separators interposed therebetween. Examples of the battery case 15 include a cylindrical, prismatic, coin-shaped, or button-shaped metal case, and a resin case formed by laminating a resin sheet (a so-called laminate type).
[0013] The non-aqueous electrolyte has, for example, ion conductivity (for example, lithium ion conductivity). The non-aqueous electrolyte may be a liquid electrolyte (electrolytic solution) or a solid electrolyte.
[0014] The liquid electrolyte (electrolytic solution) contains, for example, a non-aqueous solvent and an electrolyte salt dissolved in the non-aqueous solvent. Examples of the non-aqueous solvent include esters, ethers, nitriles, amides, and mixed solvents of two or more of these. Examples of the non-aqueous solvent include ethylene carbonate (EC), ethyl methyl carbonate (EMC), dimethyl carbonate (DMC), diethyl carbonate (DEC), and mixed solvents of these. The non-aqueous solvent may contain a halogen-substituted compound (e.g., fluoroethylene carbonate) in which at least a portion of the hydrogen atoms of these solvents are substituted with halogen atoms such as fluorine. Examples of the electrolyte salt include LiPF 6 Lithium salts such as
[0015] Furthermore, examples of the solid electrolyte that can be used include solid or gel polymer electrolytes, inorganic solid electrolytes, and the like. The polymer electrolyte includes, for example, a lithium salt and a matrix polymer, or a non-aqueous solvent, a lithium salt, and a matrix polymer. The matrix polymer is, for example, a polymer material that absorbs the non-aqueous solvent and gels. Examples of the polymer material include fluororesin, acrylic resin, and polyether resin. Examples of the inorganic solid electrolyte include materials known in all-solid-state lithium ion secondary batteries (e.g., oxide-based solid electrolytes, sulfide-based solid electrolytes, halogen-based solid electrolytes, and the like).
[0016] The case body 16 is, for example, a cylindrical metal container with a bottom. A gasket 28 is provided between the case body 16 and the sealing body 17 to ensure airtightness inside the battery. The case body 16 has, for example, a protruding portion 22, which is a portion of the side surface that protrudes inward and supports the sealing body 17. The protruding portion 22 is preferably formed in an annular shape along the circumferential direction of the case body 16, and supports the sealing body 17 on its upper surface.
[0017] The sealing body 17 has a structure in which a filter 23, a lower valve body 24, an insulating member 25, an upper valve body 26, and a cap 27 are stacked in this order from the electrode body 14 side. Each component constituting the sealing body 17 has, for example, a disk or ring shape, and all components except for the insulating member 25 are electrically connected to each other. The lower valve body 24 and the upper valve body 26 are connected to each other at their respective centers, and the insulating member 25 is interposed between their respective peripheral edges. When the internal pressure of the nonaqueous electrolyte secondary battery 10 increases due to heat generation caused by an internal short circuit or the like, for example, the lower valve body 24 deforms and ruptures, pushing the upper valve body 26 toward the cap 27, thereby interrupting the current path between the lower valve body 24 and the upper valve body 26. When the internal pressure further increases, the upper valve body 26 ruptures, and gas is discharged from the opening of the cap 27.
[0018] 1 , a positive electrode lead 20 attached to the positive electrode 11 passes through a through-hole in the insulating plate 18 and extends toward the sealing body 17, and a negative electrode lead 21 attached to the negative electrode 12 passes outside the insulating plate 19 and extends toward the bottom of the case body 16. The positive electrode lead 20 is connected by welding or the like to the underside of a filter 23, which is the bottom plate of the sealing body 17, and a cap 27, which is the top plate of the sealing body 17 and is electrically connected to the filter 23, serves as the positive electrode terminal. The negative electrode lead 21 is connected by welding or the like to the inner bottom surface of the case body 16, and the case body 16 serves as the negative electrode terminal.
[0019] The positive electrode 11, the negative electrode 12, and the separator 13 will be described in detail below.
[0020] [Positive Electrode] The positive electrode 11 has a positive electrode core and a positive electrode mixture layer formed on the positive electrode core. The positive electrode core can be a foil of a metal, such as aluminum or an aluminum alloy, that is stable within the potential range of the positive electrode 11, or a film with such a metal disposed on the surface. The positive electrode mixture layer contains a positive electrode active material, a binder, and a conductive agent, and is preferably provided on both sides of the positive electrode core. The positive electrode active material contains a lithium-containing composite oxide containing secondary particles formed by aggregation of primary particles. The positive electrode 11 can be produced, for example, by applying a slurry of the positive electrode mixture to the positive electrode core, drying the coating, and then compressing it to form a positive electrode mixture layer on both sides of the positive electrode core.
[0021] Examples of binders contained in the positive electrode mixture layer include fluorine-based resins such as polytetrafluoroethylene (PTFE) and polyvinylidene fluoride (PVDF), polyacrylonitrile (PAN), polyimide resins, acrylic resins, polyolefin resins, styrene-butadiene rubber (SBR), carboxymethyl cellulose (CMC) or a salt thereof, polyacrylic acid (PAA) or a salt thereof (PAA-Na, PAA-K, etc., or a partially neutralized salt), polyvinyl alcohol (PVA), and the like. These may be used alone or in combination of two or more. The content of the binder is, for example, 0.5 to 5% by mass relative to the mass of the positive electrode mixture layer.
[0022] Examples of the conductive agent contained in the positive electrode mixture layer include carbon materials such as carbon black (CB), acetylene black (AB), ketjen black, carbon nanotubes (CNT), and graphite. These may be used alone or in combination of two or more. The content of the conductive agent is, for example, 0.1 to 10 mass% relative to the mass of the positive electrode mixture layer.
[0023] 2 is a scanning electron microscope (SEM) image of a cross section of a secondary particle of a lithium-containing composite oxide according to an embodiment. As shown in FIG. 2, a secondary particle 30 of the lithium-containing composite oxide is an aggregate of a large number of primary particles 32, and has a plurality of voids 34 formed between the primary particles 32. In addition, in the cross section observation of the lithium-containing composite oxide, a field of view of 76.46 μm 2 The number of voids observed per field of view is 300 or more, and the field of view is 76.46 μm. 2 The median value of the nearest void distance of the voids observed per unit area is 170 nm or less. When the voids formed in the secondary particles of the lithium-containing composite oxide have the above-mentioned characteristics, the battery capacity can be improved.
[0024] A method for observing the cross section of a secondary particle to measure the number of voids, the nearest void distance, etc., is described below. (1) Exposing the cross section of the secondary particle. For example, a method of processing a lithium-containing composite oxide with a focused ion beam (FIB) processing device to expose the cross section may be used. Alternatively, a positive electrode containing a lithium-containing composite oxide may be cut and processed with an ion milling device to obtain a cross section of the lithium-containing composite oxide contained in the positive electrode mixture layer. The sample to be cross-sectionally processed may be not only a lithium-containing composite oxide powder or electrode, but also a lithium-containing composite oxide powder solidified with a resin. (2) Using a scanning electron microscope, a backscattered electron image of the cross section of the exposed secondary particle is taken to obtain a cross-sectional image of the secondary particle. The backscattered electron image is taken at a magnification of, for example, 20,000 times. (3) The cross-sectional image of the secondary particle obtained above is imported into a computer and binarized using image analysis software to obtain a binarized image in which the particle cross section in the cross-sectional image is converted into white and the voids present in the particle cross section are converted into black. Image analysis software such as Image J or Avizo-Materials Science can be appropriately selected. To extract particle cross sections and voids within the cross-sectional image, it is preferable to perform noise removal on the cross-sectional image using a non-local means filter or BM3D, and then apply edge detection and the Marker-Based-Watershed method with a brightness threshold superimposed thereon. (4) For the binarized image, image analysis software is used to calculate the number of voids observed per field of view in the secondary particle cross section and the center of gravity of each void observed per field of view in the secondary particle cross section. The secondary particle cross section refers to the entire cross-sectional area of the secondary particle, including both black and white portions. The center of gravity of a void is defined as the center of gravity of the pixels contained in the area surrounded by the periphery of the void, assuming that the weights of the pixels constituting the image are uniform. Furthermore, for the binarized image, image analysis software is used to calculate the area of each void present in the secondary particle cross section. The field of view of the secondary particle cross section when calculating the number of voids present in the secondary particle cross section, the position of the center of gravity of each void, and the area of each void is, for example, 76.46 μm 2 It is desirable to do so.
[0025] In terms of improving the capacity of the battery, the lithium-containing composite oxide has a secondary particle cross-sectional field of view of 76.46 μm 2 The number of voids observed per unit area is 300 or more, preferably 400 or more, and more preferably 500 or more. The upper limit of the number of voids is not particularly limited, but is, for example, 1,200.
[0026] The closest gap distance of voids will be explained using the schematic diagram of a secondary particle cross section shown in Fig. 3. In the cross section of a secondary particle 30, the shortest distance among the distances from the centroid position A of a void 34a formed between primary particles 32 to the centroid positions (B, C, D) of other nearby voids (e.g., 34b, 34c, 34d) is defined as the closest gap distance of void A. In Fig. 3, the closest gap distance of void A is the distance from the centroid position A of void 34a to the centroid position B of void 34b. In this embodiment, the closest gap distance of void A is calculated from the centroid positions of each void calculated in the cross section observation of the secondary particle described above, within a field of view of 76.46 µm 2 The nearest void distances for all voids observed per unit area are calculated, and the median value of the calculated nearest void distances is calculated. In this embodiment, the calculated median value is used as the distance between the voids in the field of view of 76.46 μm in the secondary particle cross section. 2 The distance is the median of the nearest void distances observed per unit area.
[0027] In terms of improving the capacity of the battery, the lithium-containing composite oxide has a field of view of 76.46 μm in the cross section of the secondary particle. 2 The nearest gap distance of voids observed per unit area is 170 nm or less, preferably 160 nm or less, and more preferably 150 nm or less. The lower limit of the nearest gap distance is not particularly limited, but is, for example, 80 nm.
[0028] The lithium-containing composite oxide is, for example, a composite oxide having an average void area of 3000 nm2 determined by cross-sectional observation of secondary particles, which can further improve the capacity of a battery. 2 Preferably, the wavelength is 1500 nm or less. 2 The upper limit of the average area of the voids is, for example, 200 nm 2 That's all.
[0029] The lithium-containing composite oxide preferably has a porosity of 2.0% or less, more preferably 1.5% or less, determined by cross-sectional observation of secondary particles, in order to further improve the capacity of the battery. The porosity is the ratio of the total area of voids to the cross-section of the secondary particles, and is calculated by the formula (total area of voids / cross-sectional area of secondary particles) × 100. For example, when the field of view for observing the cross-section of the secondary particles is 76.46 μm 2 In this case, the porosity is the cross-sectional area of the secondary particle of 76.46 μm 2 It is calculated from the total area of voids observed per unit area.
[0030] The volume-based median diameter (D50) of the secondary particles of the lithium-containing composite oxide is, for example, 3 to 30 μm, preferably 5 to 25 μm. D50 refers to the particle size at which the cumulative frequency in the volume-based particle size distribution is 50% from the smallest particle size, and is also called the median diameter. The particle size distribution of the composite oxide can be measured using a laser diffraction particle size distribution measuring device (for example, MT3000II manufactured by Microtrac-Bell Co., Ltd.) using water as the dispersion medium. The lithium-containing composite oxide also has, for example, a layered crystal structure. Specific examples include a layered structure belonging to the space group R-3m or a layered structure belonging to the space group C2 / m.
[0031] Furthermore, from the viewpoint of suppressing a decrease in the capacity retention rate during charge-discharge cycles, the lithium-containing composite oxide preferably contains at least one element M selected from the group consisting of Al, Ba, Bi, Ca, Ce, Er, Eu, Hf, Mg, Nb, La, Sb, Sr, Ta, Ti, V, and Zr. The content of the element M is preferably 0.01 mol % or more and 5 mol % or less with respect to the total molar amount of elements excluding Li and O constituting the lithium-containing composite oxide.
[0032] The lithium-containing composite oxide preferably contains at least one element selected from the group consisting of Ni, Co, and Mn, for example, in order to suppress a decrease in the capacity retention rate during charge-discharge cycles.
[0033] From the viewpoint of, for example, improving the capacity of the battery and suppressing a decrease in the capacity retention rate during charge / discharge cycles, the lithium-containing composite oxide preferably contains 50 mol % or more of Ni relative to the total number of moles of elements excluding Li and O, and more preferably contains 60 mol % or more and 90 mol % or less of Ni.
[0034] Specific examples of suitable lithium-containing composite oxides include those represented by the general formula Li a Ni b Mn c Co d M f O 2 (wherein 1.05≦a≦1.15, 0.50≦b≦0.95, 0≦c≦0.50, 0≦d≦0.1, 0≦f≦0.05, b+c+d+f=1, and M is, for example, at least one element selected from the above-mentioned M elements).
[0035] The positive electrode mixture layer may contain a lithium-containing composite oxide in which the number of voids in the cross section of the secondary particle and the median value of the nearest neighbor gap distance of the voids do not satisfy the above ranges. The content of the lithium-containing composite oxide in which the number of voids in the cross section of the secondary particle and the median value of the nearest neighbor gap distance of the voids satisfy the above ranges is, for example, preferably 50 mass% or more, more preferably 80 mass% or more, and may be substantially 100 mass% of the total mass of the positive electrode active material.
[0036] Hereinafter, an example of the method for producing the lithium-containing composite oxide according to the present disclosure will be described.
[0037] The manufacturing process of a lithium-containing composite oxide includes, for example, a first step of obtaining a composite hydroxide or composite oxide containing a metal element such as Ni, Co, or Mn, a second step of mixing the composite hydroxide or composite oxide with a lithium compound and firing the mixture, and a third step of washing and drying the fired product. In the first step, the mixture may be pre-fired at a temperature lower than that of the main firing in the second step. As a result of studies by the present inventors, it has been found that, for example, the firing temperature and washing conditions during the manufacturing process affect the number of voids in the cross section of the secondary particles of the lithium-containing composite oxide and the length of the nearest neighbor gap distance of the voids.
[0038] In the first step, for example, an alkaline solution such as sodium hydroxide is added dropwise to a stirred solution of a metal salt containing at least one element selected from the group consisting of Ni, Co, and Mn, or the element M, to adjust the pH to the alkaline side (e.g., 8.5 to 12.5), thereby precipitating (co-precipitating) a composite hydroxide. The composite hydroxide is then calcined in the air or under an oxygen stream to obtain a composite oxide. The calcination temperature is preferably 600°C or lower, and may be 300 to 500°C.
[0039] The pre-firing may be a multi-stage firing process, for example, including at least a first firing step in which firing is performed in the atmosphere at 100 to 300°C, and a second firing step in which the fired product obtained in the first firing step is fired in the atmosphere at 300 to 600°C. In the first firing step, the temperature is raised to a first set temperature of 300°C or less at a first heating rate of 0.2 to 5.5°C / min. In the second firing step, the temperature is raised to a second set temperature of 600°C or less at a second heating rate of 0.1 to 3.5°C / min, which is slower than the first heating rate. Note that multiple first and second heating rates may be set for each predetermined temperature range within the above range.
[0040] The holding time of the first set temperature in the first firing step is preferably 5 hours or less, more preferably 3 hours or less. The holding time of the first set temperature is the time for which the first set temperature is maintained after reaching the first set temperature (the same applies to the second firing step), and the holding time may be zero. The holding time of the second set temperature in the second firing step is preferably 1 to 10 hours, more preferably 1 to 5 hours. Although it varies depending on the main firing temperature, etc., the lower the pre-firing temperature, the smaller the median value of the nearest gap distance of voids tends to be.
[0041] In the second step, for example, the composite hydroxide or composite oxide obtained in the first step is mixed with a lithium compound. An example of the lithium compound is Li 2 CO 3 , LiOH, Li 2 O 2 , Li 2 O, LiNO 3 , LiNO 2 , Li 2 SO 4, LiOH·H 2 Examples of the metal element include O, LiH, and LiF. The composite hydroxide or composite oxide and the lithium compound are mixed in such a manner that the molar ratio of the metal elements Me and Li is, for example, 1:0.95 to 1:1.15, and preferably 1:1.05 to 1:1.15.
[0042] The firing step of the mixture in the third step is a multi-stage firing step, for example, including a first firing step in which firing is performed at 500°C to 700°C under an oxygen stream, and a second firing step in which the fired product obtained in the first firing step is fired under an oxygen stream at a temperature exceeding 700°C. In the first firing step, the temperature is raised to a first set temperature of 700°C or less at a first heating rate of, for example, 0.2 to 5.5°C / min. In the second firing step, the temperature is raised to a second set temperature of 1000°C or less at a second heating rate of, for example, 0.1 to 3.5°C / min, which is slower than the first heating rate. Note that a plurality of first and second heating rates may be set for each predetermined temperature range within the above range.
[0043] The holding time of the first set temperature in the first firing step is preferably 5 hours or less, more preferably 3 hours or less. The holding time of the first set temperature is the time for which the first set temperature is maintained after reaching the first set temperature (the same applies to the second firing step), and the holding time may be zero. The holding time of the second set temperature in the second firing step is preferably 1 to 10 hours, more preferably 1 to 5 hours. The firing of the mixture is carried out, for example, in an oxygen stream with an oxygen concentration of 60% or more, and the flow rate of the oxygen stream is set to 10 cm / min. 3 The flow rate should be 0.2 to 4 mL / min per kg of the mixture and 0.3 L / min or more per kg of the mixture.
[0044] In the fourth step, the fired product obtained in the third step is washed with water to remove impurities such as excess Li, and the washed fired product is dried. If necessary, the fired product is pulverized, classified, etc., to adjust the D50 of the positive electrode active material to a desired range. The washed fired product may be dried in a vacuum or in the air. An example of the drying temperature is 150 to 250°C, and an example of the drying treatment time is 1 to 5 hours. The water washing may be performed by either adding the active material to water and stirring it, or by passing water through the active material to wet it. The electrical conductivity of the water used for washing is 1 x 10 at 25°C.-4 It is preferable that the surface roughness is S / m or less. The degree of water washing can be adjusted by the solid-liquid ratio of the calcined product to water, the water washing time, the stirring speed, etc. For example, the solid-liquid ratio of the calcined product to water is preferably 1:0.1 to 1:10, and more preferably 1:0.5 to 1:5. Although it varies depending on the main calcination temperature, water washing conditions, etc., the median value of the nearest neighbor gap distance of the pores in the lithium-containing composite oxide tends to be smaller by performing water washing.
[0045] In the manufacturing process of the lithium-containing composite oxide, the addition of element M, the pre-baking conditions, the main baking conditions, the water-washing conditions, and the like are appropriately changed so that the number of voids in the cross section of the secondary particle of the composite oxide, the median value of the nearest gap distance between the voids, and the like satisfy the above-specified ranges.
[0046] [Negative Electrode] The negative electrode 12 has a negative electrode core and a negative electrode mixture layer formed on the negative electrode core. The negative electrode core can be a foil of a metal, such as copper or a copper alloy, that is stable within the potential range of the negative electrode 12, or a film with such a metal disposed on the surface. The negative electrode mixture layer preferably contains a negative electrode active material, a binder, and, if necessary, a conductive agent such as carbon nanotubes, and is provided on both sides of the negative electrode core. The binder may be the same as that of the positive electrode 11. The negative electrode 12 can be produced, for example, by applying a negative electrode mixture slurry containing a negative electrode active material and a binder to the surface of the negative electrode core, drying the coating, and then compressing it to form a negative electrode mixture layer on both sides of the negative electrode core.
[0047] The negative electrode mixture layer generally contains, as the negative electrode active material, a carbon material that reversibly absorbs and releases lithium ions. Suitable examples of the carbon material include natural graphite such as flake graphite, lump graphite, and amorphous graphite, and artificial graphite such as lump artificial graphite (MAG) and graphitized mesophase carbon microbeads (MCMB). Furthermore, as the negative electrode active material, an active material containing at least one of an element that alloys with Li, such as Si or Sn, and a material containing such an element may be used. A suitable example of the active material is SiO 2 The negative electrode active material is a Si-containing material in which Si fine particles are dispersed in a silicate phase such as lithium silicate or a silicon dioxide phase. A carbon material and a Si-containing material may be used in combination as the negative electrode active material.
[0048] [Separator] The separator 13 may be, for example, a porous sheet having ion permeability and insulating properties. Specific examples of the porous sheet include a microporous thin film, a woven fabric, and a nonwoven fabric. Suitable materials for the separator 13 include polyolefins such as polyethylene and polypropylene, and cellulose. The separator 13 may have a single-layer structure or a multi-layer structure. Furthermore, a highly heat-resistant resin layer such as an aramid resin may be formed on the surface of the separator 13.
[0049] A filler layer containing an inorganic filler may be formed at the interface between the separator 13 and at least one of the positive electrode 11 and the negative electrode 12. Examples of inorganic fillers include oxides and phosphate compounds containing metal elements such as Ti, Al, Si, and Mg. The filler layer can be formed by applying a slurry containing the filler to the surface of the positive electrode 11, the negative electrode 12, or the separator 13.
[0050] The present disclosure will be further described below with reference to examples, but the present disclosure is not limited to these examples.
[0051] Example 1 Synthesis of Positive Electrode Active Material [Ni 0.8 Mn 0.2 ](OH) 2 The composite hydroxide represented by the formula (1) was calcined in air by increasing the temperature from room temperature to 150°C at a rate of 5.0°C / min, and then calcined again by increasing the temperature to 400°C at a rate of 1.0°C / min, to obtain a Ni, Mn-containing composite oxide. The Ni, Mn-containing composite oxide, lithium hydroxide, tungsten oxide, and antimony oxide were mixed so that the molar ratio of the total amount of Ni and Mn to Li, W, and Sb was 1:1.11:0.003:0.003. The mixture was stirred under an oxygen stream (10 cm) with an oxygen concentration of 95%. 3 The mixture was heated from room temperature to 650°C at a rate of 2.0°C / min (flow rate of 2.5 mL / min per kg of mixture and 5 L / min per kg of mixture), and then fired at a rate of 1.0°C / min to 820°C. The fired product was then heated to a solid-liquid ratio of the fired product to water of 1:0.8, and the electrical conductivity was measured to be 1 × 10 -5The mixture was poured into water having a viscosity of 0.15 S / m or less, washed with water for 5 minutes while stirring at 400 rpm, and then vacuum dried at 180° C. for 2 hours to obtain a positive electrode active material (lithium-containing composite oxide).
[0052] The cross section of the secondary particles of the positive electrode active material was exposed by the above-mentioned method, and the cross section of the secondary particles was observed using an SEM (20,000x magnification). It was confirmed that the positive electrode active material was a secondary particle formed by agglomeration of many primary particles, and that the secondary particles contained many voids. Furthermore, from the SEM image of the particle cross section, the above-mentioned image analysis method was used to determine the field of view of the secondary particle cross section at 76.46 μm 2 The number of voids observed per unit area, the median of the nearest void distance, the average void area, and the porosity were determined and are summarized in Table 1 (the same applies to the following Examples and Comparative Examples).
[0053] [Preparation of Positive Electrode] The positive electrode active material, acetylene black, and polyvinylidene fluoride were mixed in a solid content mass ratio of 92:5:3, and N-methyl-2-pyrrolidone (NMP) was used as a dispersion medium to prepare a positive electrode mixture slurry. Next, the positive electrode mixture slurry was applied to a positive electrode core made of aluminum foil, the coating was dried and compressed, and then the positive electrode core was cut to a predetermined electrode size to obtain a positive electrode having a positive electrode mixture layer formed on both sides of the positive electrode core.
[0054] [Preparation of Negative Electrode] Graphite was used as the negative electrode active material. The negative electrode active material, a sodium salt of CMC, and a dispersion of SBR were mixed in a solid content mass ratio of 98:1:1, and water was used as a dispersion medium to prepare a negative electrode mixture slurry. Next, the negative electrode mixture slurry was applied to a negative electrode core made of copper foil, the coating was dried and rolled, and then the negative electrode core was cut to a predetermined electrode size to obtain a negative electrode having a negative electrode mixture layer formed on both sides of the negative electrode core.
[0055] [Preparation of non-aqueous electrolyte] Ethylene carbonate (EC), dimethyl carbonate (DMC), and ethyl methyl carbonate (EMC) were mixed in a volume ratio of 20:75:5. 6 was dissolved in the above solution to a concentration of 1.3 mol / L to prepare a non-aqueous electrolyte.
[0056] [Preparation of Test Cell] The positive electrode and negative electrode with leads attached were wound with a separator interposed therebetween to prepare a wound electrode assembly. The electrode assembly was inserted into an exterior case made of aluminum laminate film, and vacuum dried at 105°C for 2 hours. After that, a non-aqueous electrolyte solution was poured into the exterior case, and the opening of the exterior case was sealed to obtain a test cell (non-aqueous electrolyte secondary battery).
[0057] Example 2 A test cell was produced in the same manner as in Example 1, except that in synthesizing the positive electrode active material, a Ni-Mn-containing composite oxide, lithium hydroxide, tungsten oxide, niobium oxide, and antimony oxide were mixed so that the molar ratio of the total amount of Ni and Mn to Li, W, Nb, and Sb was 1:1.11:0.003:0.003:0.0025.
[0058] Example 3 A test cell was produced in the same manner as in Example 1, except that in synthesizing the positive electrode active material, a Ni-Mn-containing composite oxide, lithium hydroxide, tungsten oxide, and niobium oxide were mixed so that the molar ratio of the total amount of Ni and Mn to Li, W, and Nb was 1:1.11:0.005:0.0025, and the upper limit temperature during firing was set to 800°C.
[0059] Example 4 A test cell was produced in the same manner as in Example 1, except that in synthesizing the positive electrode active material, a Ni-Mn-containing composite oxide, lithium hydroxide, tungsten oxide, niobium oxide, and calcium hydroxide were mixed so that the molar ratio of the total amount of Ni and Mn to Li, W, Nb, and Ca was 1:1.11:0.003:0.003:0.0075.
[0060] Example 5 A test cell was produced in the same manner as in Example 1, except that in synthesizing the positive electrode active material, a Ni- and Mn-containing composite oxide, lithium hydroxide, tungsten oxide, niobium oxide, calcium hydroxide, and strontium hydroxide were mixed so that the molar ratio of the total amount of Ni and Mn to Li, W, Nb, Ca, and Sr was 1:1.11:0.003:0.003:0.0015:0.0015.
[0061] Example 6 A test cell was produced in the same manner as in Example 1, except that in synthesizing the positive electrode active material, a Ni-Mn-containing composite oxide, lithium hydroxide, tungsten oxide, niobium oxide, aluminum hydroxide, and calcium hydroxide were mixed so that the molar ratio of the total amount of Ni and Mn to Li, W, Nb, Al, and Ca was 1:1.05:0.003:0.0025:0.005:0.0075, and the upper limit temperature during firing was set to 810°C.
[0062] Example 7 A test cell was produced in the same manner as in Example 1, except that in synthesizing the positive electrode active material, a Ni-Mn-containing composite oxide, lithium hydroxide, tungsten oxide, niobium oxide, and erbium nitrate were mixed so that the molar ratio of the total amount of Ni and Mn to Li, W, Nb, and Er was 1:1.11:0.003:0.003:0.0005.
[0063] Example 8 A test cell was produced in the same manner as in Example 1, except that in synthesizing the positive electrode active material, a Ni-Mn-containing composite oxide, lithium hydroxide, tungsten oxide, niobium oxide, and titanium oxide were mixed so that the molar ratio of the total amount of Ni and Mn to Li, W, Nb, and Ti was 1:1.11:0.003:0.003:0.003, and the upper limit temperature during firing was set to 830°C.
[0064] Example 9 A test cell was produced in the same manner as in Example 1, except that in synthesizing the positive electrode active material, a Ni-Mn-containing composite oxide, lithium hydroxide, tungsten oxide, niobium oxide, antimony oxide, and bismuth oxide were mixed so that the molar ratio of the total amount of Ni and Mn to Li, W, Nb, Sb, and Bi was 1:1.09:0.003:0.003:0.0025:0.0001, and the upper limit temperature during firing was set to 840°C.
[0065] Example 10 A test cell was produced in the same manner as in Example 1, except that in synthesizing the positive electrode active material, a Ni- and Mn-containing composite oxide, lithium hydroxide, tungsten oxide, niobium oxide, calcium hydroxide, and zirconium oxide were mixed so that the molar ratio of the total amount of Ni and Mn to Li, W, Nb, Ca, and Zr was 1:1.11:0.003:0.003:0.002:0.001, and the upper limit temperature during firing was set to 830°C.
[0066] Comparative Example 1 A test cell was produced in the same manner as in Example 1, except that in synthesizing the positive electrode active material, a Ni- and Mn-containing composite oxide, lithium hydroxide, tungsten oxide, niobium oxide, and antimony oxide were mixed so that the molar ratio of the total amount of Ni and Mn to Li, W, Nb, and Sb was 1:1.11:0.003:0.003:0.001.
[0067] Comparative Example 2 A test cell was produced in the same manner as in Example 1, except that in synthesizing the positive electrode active material, a Ni- and Mn-containing composite oxide, lithium hydroxide, tungsten oxide, iron oxide, and antimony oxide were mixed so that the molar ratio of the total amount of Ni and Mn to Li, W, Fe, and Sb was 1:1.11:0.0025:0.02:0.0025, and the upper limit temperature during firing was set to 800°C.
[0068] Comparative Example 3 A test cell was produced in the same manner as in Example 1, except that in synthesizing the positive electrode active material, a Ni-Mn-containing composite oxide, lithium hydroxide, tungsten oxide, niobium oxide, aluminum hydroxide, and calcium hydroxide were mixed so that the molar ratio of the total amount of Ni and Mn to Li, W, Nb, Al, and Ca was 1:1.15:0.001:0.001:0.01:0.01, and the upper limit temperature during firing was set to 790°C.
[0069] Comparative Example 4 A test cell was produced in the same manner as in Example 1, except that in synthesizing the positive electrode active material, a Ni-Mn-containing composite oxide, lithium hydroxide, tungsten oxide, niobium oxide, and aluminum hydroxide were mixed so that the molar ratio of the total amount of Ni and Mn to Li, W, Nb, and Al was 1:1.09:0.001:0.003:0.01, and the upper limit temperature during firing was set to 810°C.
[0070] Comparative Example 5 A test cell was produced in the same manner as in Example 1, except that in the synthesis of the positive electrode active material, a Ni-Mn-containing composite oxide, lithium hydroxide, niobium oxide, and strontium hydroxide were mixed so that the molar ratio of the total amount of Ni and Mn to Li, Nb, and Sr was 1:1.11:0.0025:0.0025, and the upper limit temperature during firing was set to 800°C.
[0071] [Charge / Discharge Test] Each test cell to be evaluated was charged at a constant current of 0.2 C in a temperature environment of 25°C until the cell voltage reached 4.5 V, and then charged at a constant voltage of 4.5 V until the current reached 0.02 C. After resting each test cell for 10 minutes, each test cell was discharged at a constant current of 0.2 C in a temperature environment of 25°C until the voltage reached 2.5 V. The discharge capacity at this time was recorded as the battery capacity. The results are summarized in Table 1.
[0072] Furthermore, for each test cell, the above charge / discharge cycle was repeated 25 times, and the capacity retention rate was calculated using the following formula. The results are shown in Table 1. Capacity retention rate (%) = (discharge capacity at 3rd cycle / discharge capacity at 25th cycle) x 100
[0073]
[0074] As shown in Table 1, the battery capacity of all the test cells of the examples was improved compared to the test cells of the comparative examples. 2 The number of voids observed per unit area is 300 or more, and the field of view is 76.46 μm. 2By using a lithium-containing composite oxide in which the median value of the nearest void distance of voids observed per unit area is 170 nm or less as a positive electrode active material, it is possible to improve the battery capacity. Furthermore, the test cells of the examples used lithium composite oxides containing specific elements, and all of them showed a capacity retention rate of 95% or more. On the other hand, the test cells of the comparative examples also used lithium composite oxides containing specific elements, but some of the comparative examples showed a capacity retention rate of less than 95%. From this, it can be seen that, as in the examples, in the cross section of the secondary particles, 2 The number of voids observed per unit area is 300 or more, and the field of view is 76.46 μm. 2 It can be said that by using a lithium-containing composite oxide in which the median value of the nearest neighbor gap distance of the voids observed per unit area is 170 nm or less and further containing a specific element, it is possible to achieve both of the two effects of improving the battery capacity and suppressing the decrease in the capacity retention rate during charge-discharge cycles.
[0075] [Additional Note] Configuration 1: A positive electrode active material for a secondary battery having a lithium-containing composite oxide containing secondary particles formed by aggregation of primary particles, wherein the lithium-containing composite oxide has a field of view of 76.46 μm in cross-sectional observation of the secondary particles. 2 The number of voids observed per field of view is 300 or more, and the field of view is 76.46 μm. 2 A positive electrode active material for a non-aqueous electrolyte secondary battery, wherein the median value of the nearest neighbor gap distance of voids observed per cross section of the lithium-containing composite oxide is 170 nm or less. 2The positive electrode active material for a non-aqueous electrolyte secondary battery according to Configuration 1, wherein the positive electrode active material for a non-aqueous electrolyte secondary battery is as follows: Configuration 3: The positive electrode active material for a non-aqueous electrolyte secondary battery according to Configuration 1 or 2, wherein the lithium-containing composite oxide has a porosity of 2.0% or less as determined by cross-sectional observation of the secondary particles; Configuration 4: The positive electrode active material for a non-aqueous electrolyte secondary battery according to any one of Configurations 1 to 3, wherein the lithium-containing composite oxide contains at least one element selected from the group consisting of Al, Ba, Bi, Ca, Ce, Er, Eu, Hf, Mg, Nb, La, Sb, Sr, Ta, Ti, V, and Zr; Configuration 5: The positive electrode active material for a non-aqueous electrolyte secondary battery according to any one of Configurations 1 to 4, wherein the lithium-containing composite oxide contains at least one element selected from the group consisting of Ni, Co, and Mn; Configuration 6: A non-aqueous electrolyte secondary battery comprising a positive electrode containing the positive electrode active material for a non-aqueous electrolyte secondary battery according to any one of Configurations 1 to 5, a negative electrode, and a non-aqueous electrolyte.
[0076] REFERENCE SIGNS LIST 10 Non-aqueous electrolyte secondary battery, 11 Positive electrode, 12 Negative electrode, 13 Separator, 14 Electrode body, 15 Battery case, 16 Case body, 17 Sealing body, 18, 19 Insulating plate, 20 Positive electrode lead, 21 Negative electrode lead, 22 Protruding portion, 23 Filter, 24 Lower valve body, 25 Insulating member, 26 Upper valve body, 27 Cap, 28 Gasket, 30 Secondary particles, 32 Primary particles, 34 Voids.
Claims
1. A positive electrode active material for a non-aqueous electrolyte secondary battery having a lithium-containing composite oxide including secondary particles formed by agglomeration of primary particles, wherein the lithium-containing composite oxide has a field of view of 76.46 μm in cross-sectional observation of the secondary particles. 2 The number of voids observed per field of view is 300 or more, and the field of view is 76.46 μm 2 The positive electrode active material for a non-aqueous electrolyte secondary battery has a median closest gap distance of 170 nm or less when observed per unit area.
2. The lithium-containing composite oxide has an average void area of 3000 nm2 as determined by cross-sectional observation of the secondary particles. 2 2. The positive electrode active material for a non-aqueous electrolyte secondary battery according to claim 1, wherein:
3. The positive electrode active material for a non-aqueous electrolyte secondary battery according to claim 1 or 2, wherein the lithium-containing composite oxide has a porosity of 2.0% or less as determined by cross-sectional observation of the secondary particles.
4. The positive electrode active material for a nonaqueous electrolyte secondary battery according to claim 1 or 2, wherein the lithium-containing composite oxide contains at least one element selected from the group consisting of Al, Ba, Bi, Ca, Ce, Er, Eu, Hf, Mg, Nb, La, Sb, Sr, Ta, Ti, V, and Zr.
5. The positive electrode active material for a non-aqueous electrolyte secondary battery according to claim 1 or 2, wherein the lithium-containing composite oxide contains at least one element selected from the group consisting of Ni, Co, and Mn.
6. A non-aqueous electrolyte secondary battery comprising a positive electrode containing the positive electrode active material for non-aqueous electrolyte secondary batteries according to claim 1 or 2, a negative electrode, and a non-aqueous electrolyte.
Citation Information
Patent Citations
Toroidal-type continuously variable transmission
JP2016169817A
Composite cathode active material, cathode and lithium battery including the same, and method of preparing the composite cathode active material
CN110556520A
Positive electrode active material for lithium ion secondary battery, positive electrode for lithium ion secondary battery, and lithium ion secondary battery
WO2014024571A1
Positive electrode active material, positive electrode material, positive electrode, and nonaqueous electrolyte secondary battery
WO2014142279A1
Nonaqueous electrolyte secondary battery positive electrode active material and nonaqueous electrolyte secondary battery