Polyvinyl alcohol-based resin composition, film or sheet, and multilayer structure

The resin composition with formic acid and acetic acid radicals in polyvinyl alcohol resin addresses the stability issues during melt molding, ensuring thermal stability and gas barrier properties, improving the quality of molded products.

WO2024204482A1PCT designated stage expired Publication Date: 2024-10-03MITSUBISHI CHEM CORP
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/012537
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-27
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Polyvinyl alcohol (PVA) resins exhibit poor thermal and molding stability during melt molding due to their close melting point and decomposition temperature, leading to viscosity changes and deterioration of gas barrier properties when modified with plasticizers or copolymerized with other monomers.

Method used

A resin composition containing a polyvinyl alcohol resin with appropriate amounts of formic acid and acetic acid radicals, specifically within the range of 4 to 500 ppm for formic acid and 10,000 ppm or less for acetic acid, improves thermal and molding stability by maintaining crystallinity and gas barrier properties.

Benefits of technology

The resin composition achieves excellent thermal stability and molding stability during melt molding, maintaining gas barrier properties and preventing viscosity changes, thus enhancing the quality of molded products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-C000001
    Figure JPOXMLDOC01-APPB-C000001
  • Figure JPOXMLDOC01-APPB-C000002
    Figure JPOXMLDOC01-APPB-C000002
  • Figure JPOXMLDOC01-APPB-C000003
    Figure JPOXMLDOC01-APPB-C000003
Patent Text Reader

Abstract

The present invention pertains to a resin composition containing a PVA-based resin, formic acid root, and acetic acid root, wherein the content of the formic acid root in the resin composition is 4-500 ppm, and the content ratio of the formic acid root to the acetic acid root (formic acid root / acetic acid root) is 0.001-0.200.
Need to check novelty before this filing date? Find Prior Art

Description

Polyvinyl alcohol-based resin composition, film or sheet, and multilayer structure

[0001] The present invention relates to a resin composition that contains a polyvinyl alcohol-based resin and has excellent thermal stability and molding stability during melt molding, a film or sheet made of the resin composition, and a multilayer structure that includes a layer made of the resin composition.

[0002] Gas barrier properties are required for containers and packaging films used in a wide range of fields, including agriculture, civil engineering, industry, medicine, packaging, leisure, toys, miscellaneous goods, daily necessities, containers, and parts, in order to prevent deterioration of the quality of the contents. Polyvinyl alcohol (PVA) has high crystallinity due to hydrogen bonding between hydroxyl groups, and due to this high crystallinity, it has excellent gas barrier properties. Therefore, PVA-based resins or resin compositions thereof are used as gas barrier layers for the above-mentioned containers and packaging films.

[0003] Generally, molded articles such as containers and films are produced by melt molding from the viewpoint of productivity. It is known that it is difficult to produce molded articles from polyvinyl alcohol (PVA) by hot melt molding because the melting point and decomposition temperature are close to each other. However, modified PVA-based resins that can be melt molded have also been proposed. (For example, PVA-based resins having a 1,2-diol structure in the side chain are described in Patent Documents 1, 2, and 3.) Furthermore, because molded articles of PVA-based resins are hard, it is known that a plasticizer is added to PVA-based resin compositions for melt molding, such as packaging films and containers (for example, Patent Document 4).

[0004] Japanese Patent Publication No. 2002-284818 Japanese Patent Publication No. 2004-285143 Japanese Patent Publication No. 2006-95825 Japanese Patent Publication No. 2001-288321

[0005] However, since the excellent gas barrier properties of PVA-based resins are based on the high crystallinity of the PVA molecular chains, modified PVA-based resins containing plasticizers or copolymerized with other monomers have the problem of disrupting the crystallinity and degrading the gas barrier properties. Furthermore, when PVA-based resins are melt-molded for a long period of time, the viscosity of the PVA-based resin changes significantly and increases, resulting in poor molding stability. Furthermore, the thermal stability is also poor, resulting in the generation of thermally degraded products. Therefore, improvements to the above problems have been desired.

[0006] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a resin composition which contains a PVA-based resin and has excellent thermal stability and molding stability during melt molding.

[0007] The present inventors have found that a resin composition containing a PVA-based resin and an appropriate amount of formic acid groups and acetate groups improves the thermal stability and molding stability during melt molding compared to a PVA-based resin alone, and have completed the present invention.

[0008] That is, the gist of the present invention is as follows.

[0009] A first aspect of the present invention is a resin composition comprising a polyvinyl alcohol-based resin, a formate group, and an acetate group, wherein the content of the formate group in the resin composition is 4 to 500 ppm, and the content ratio of the formate group to the acetate group (formate group / acetate group) is 0.001 to 0.200.

[0010] A resin composition according to a second aspect of the present invention is characterized in that, in the first aspect, the content of the acetate group in the resin composition is 10,000 ppm or less.

[0011] The resin composition of Aspect 3 of the present invention is characterized in that in Aspect 1 or 2, the polyvinyl alcohol-based resin contains a structural unit having a modifying group other than ethylene.

[0012] The resin composition of Aspect 4 of the present invention is characterized in that, in any one of Aspects 1 to 3, the polyvinyl alcohol resin contains a structural unit having a hydrophilic modifying group.

[0013] The resin composition of Aspect 5 of the present invention is characterized in that, in any one of Aspects 1 to 4, the polyvinyl alcohol-based resin contains a structural unit having a primary hydroxyl group in the side chain.

[0014] A resin composition according to a sixth aspect of the present invention is characterized in that, in any one of the first to fifth aspects, the content of formic acid groups is 5 to 100 ppm.

[0015] A seventh aspect of the present invention is a molded article containing the resin composition of any one of the first to sixth aspects.

[0016] Aspect 8 of the present invention is a film containing the resin composition according to any one of Aspects 1 to 6.

[0017] A ninth aspect of the present invention is a sheet containing the resin composition according to any one of the first to sixth aspects.

[0018] A tenth aspect of the present invention is a multilayer structure containing at least one layer made of the resin composition according to any one of the first to sixth aspects.

[0019] The resin composition of the present invention contains a PVA-based resin and has excellent thermal stability and molding stability when subjected to melt molding.

[0020] [Resin Composition] The resin composition of the present invention is a resin composition containing a polyvinyl alcohol-based resin (PVA-based resin), a formate group, and an acetate group, wherein the content of the formate group in the resin composition is 4 to 500 ppm, and the content ratio of the formate group to the acetate group (formate group / acetate group) is 0.001 to 0.200.

[0021] <PVA-Based Resin> The PVA-based resin used in the resin composition of the present invention is a PVA-based resin that is formed, including film formation, by a solution casting method. It includes not only unmodified PVA, but also copolymer-modified PVA-based resins obtained by saponifying a copolymer obtained by copolymerizing a modifying monomer to impart desired properties (e.g., water resistance), and post-modified PVA-based resins obtained by post-modifying a PVA-based resin. In this specification, unless otherwise specified, "PVA-based resin" is a general term for unmodified PVA, copolymer-modified PVA, and post-modified PVA. When copolymer-modified PVA and post-modified PVA are collectively referred to, they are called "modified PVA-based resins."

[0022] 1. Unmodified PVA-based resin Unmodified PVA-based resin is a polyvinyl alcohol obtained by saponifying polyvinyl ester obtained by polymerizing vinyl ester-based monomers, and contains vinyl alcohol units represented by the following formula (1) and vinyl ester units (the following formula (2)) which are unsaponified portions. Vinyl ester units are included when the saponification degree is less than 100%.

[0023]

[0024]

[0025] Examples of the vinyl ester monomer include vinyl formate, vinyl acetate, vinyl propionate, vinyl valerate, vinyl butyrate, vinyl isobutyrate, vinyl pivalate, vinyl caprate, vinyl laurate, vinyl stearate, vinyl benzoate, and vinyl versatate, with vinyl acetate being economically preferred.

[0026] In formula (2), R a depends on the type of vinyl ester monomer used, and when vinyl acetate monomer is used, it becomes a methyl group.

[0027] The number average degree of polymerization of the unmodified PVA-based resin (measured in accordance with JIS K6726:1994) is usually 150 to 4000, preferably 200 to 2000, more preferably 250 to 800, and even more preferably 300 to 600. If the average degree of polymerization is too low, it tends to be difficult to form a stable shape during melt molding, whereas if it is too high, the viscosity of the resin composition tends to become too high, making molding difficult.

[0028] The viscosity of an aqueous solution of an unmodified PVA resin may be used as an index of the average degree of polymerization. The viscosity of a 4 wt % aqueous solution at 20°C, measured in accordance with JIS K6726:1994, is usually 1.5 to 20 mPa·s, preferably 2 to 12 mPa·s, and particularly preferably 2.5 to 8 mPa·s. If the viscosity is too low, it tends to be difficult to form a stable shape during melt molding, while if the viscosity is too high, molding tends to be difficult.

[0029] The saponification degree of the unmodified PVA-based resin is usually 70 to 99.9 mol%, preferably 75 to 99.7 mol%, and particularly preferably 78 to 99.5 mol%. If the saponification degree is too low, the flexibility tends to be too high, and shape stability during lamination tends to decrease. The saponification degree is measured in accordance with JIS K6726:1994.

[0030] The melting point of the unmodified PVA resin is preferably about 200 to 250°C, and the decomposition temperature is preferably about 250 to 300°C, although this may vary depending on the degree of polymerization and the degree of saponification.

[0031] In the case of a typical PVA-based resin, the main chain bond is mainly 1,3-diol bond, and the content of 1,2-diol bond is about 1.5 to 1.7 mol %. However, the content of 1,2-diol bond can be increased by increasing the polymerization temperature when polymerizing the vinyl ester-based monomer.

[0032] 2. Modified PVA-based Resin Copolymerized modified PVA-based resins are obtained by saponifying a copolymer obtained by copolymerizing a modifying monomer. Examples of copolymerizable monomers (modifying monomers) used in the copolymerized modified PVA-based resins include olefins such as ethylene, propylene, isobutylene, α-octene, α-dodecene, and α-octadecene; unsaturated acids such as acrylic acid, methacrylic acid, crotonic acid, maleic acid, maleic anhydride, and itaconic acid, or their salts or mono- or dialkyl esters; nitriles such as acrylonitrile and methacrylonitrile; amides such as acrylamide and methacrylamide; olefin sulfonic acids such as ethylene sulfonic acid, allyl sulfonic acid, and methallylsulfonic acid, or their salts; alkyl vinyl ethers, N-acrylamidomethyltrimethylammonium chloride, allyltrimethylammonium chloride, dimethylallyl vinyl ketone, N-vinylpyrrolidone, vinyl chloride, vinylidene chloride, polyoxyethylene (meth)allyl ether ... Examples of the polyoxyalkylene (meth)allyl ether include polyoxyalkylene (meth)acrylates such as polyoxyethylene (meth)acrylate and polyoxypropylene (meth)acrylate; polyoxyalkylene (meth)acrylamides such as polyoxyethylene (meth)acrylamide and polyoxypropylene (meth)acrylamide; hydroxy group-containing α-olefins such as polyoxyethylene (1-(meth)acrylamide-1,1-dimethylpropyl) ester, polyoxyethylene vinyl ether, polyoxypropylene vinyl ether, polyoxyethylene allylamine, polyoxypropylene allylamine, polyoxyethylene vinylamine, polyoxypropylene vinylamine, 3-butene-1-ol, 4-pentene-1-ol, and 5-hexene-1-ol, and derivatives thereof, such as acylated products.

[0033] The post-modified PVA-based resin can be obtained by post-modifying a PVA-based resin, such as a PVA-based resin having an acetoacetyl group formed by reaction with diketene, a PVA-based resin having a polyalkylene oxide group formed by reaction with ethylene oxide, a PVA-based resin having a hydroxyalkyl group formed by reaction with an epoxy compound, or a PVA-based resin obtained by reaction with an aldehyde compound having various functional groups.

[0034] The modification amount in the modified PVA-based resin, i.e., the content of structural units derived from various monomers in the copolymer or functional groups introduced by post-reaction, cannot be generally determined because the properties vary greatly depending on the type of modification, but is usually 0.1 to 20 mol %, and particularly preferably in the range of 0.5 to 15 mol %.

[0035] Among these various modified PVA-based resins, in this embodiment, it is preferable to use a PVA resin containing a structural unit having a modifying group other than ethylene, from the viewpoint of barrier properties at low humidity.

[0036] Among these various modified PVA-based resins, in this embodiment, from the viewpoint of water solubility, a PVA-based resin containing a structural unit having a hydrophilic modified group (hydrophilic modified group) is preferably used. Examples of the hydrophilic modified group include a hydroxyl group, a carboxyl group, and an amino group. From the viewpoint of melt processing, a PVA-based resin containing a structural unit having a primary hydroxyl group in a side chain is preferred. In particular, from the viewpoint of thermal stability, a PVA-based resin containing a structural unit having a 1,2-diol modified group is preferred.

[0037] The modified PVA-based resin containing a structural unit having a 1,2-diol modifying group contains a structural unit having a 1,2-diol modifying group in a side chain in addition to a vinyl alcohol unit represented by the following formula (1) constituting polyvinyl alcohol and a vinyl ester unit (the following formula (2)) which is an unsaponified portion. The vinyl ester unit is included when the saponification degree is less than 100%.

[0038]

[0039]

[0040] In formula (2), R a depends on the type of vinyl ester monomer used, and for example, when vinyl acetate monomer is used, it becomes a methyl group.

[0041] As a structural unit having a 1,2-diol modified group in a side chain, a side chain 1,2-diol-containing unit represented by the following formula (3) is preferred.

[0042]

[0043] In formula (3), R 1 ~R 6 each independently represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, and X represents a single bond or a bonding chain.

[0044] In general formula (3), R 1 ~R 6 are each independently a hydrogen atom or an alkyl group having 1 to 4 carbon atoms (such as a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, or a tert-butyl group, which may have a substituent such as a halogen group, a hydroxyl group, an ester group, a carboxylic acid group, or a sulfonic acid group). A hydrogen atom is more preferred. 1 ~R 6 may be all the same or different, but are preferably all hydrogen atoms. When all are hydrogen atoms, the terminals of the side chains become primary hydroxyl groups, which is preferable in that the reactivity with adhesive resins such as acid-modified polyolefin resins is improved and the formation of a laminate is facilitated.

[0045] In formula (3), X is a single bond or a bonding chain. Examples of the bonding chain (X) include hydrocarbon groups such as alkylene groups, alkenylene groups, alkynylene groups, phenylene groups, and naphthylene groups (these hydrocarbon groups may be substituted with halogen atoms such as fluorine atoms, chlorine atoms, and bromine atoms), -O-, -(CH 2 O) m -, -(OCH 2 ) m -, -(CH 2 O) m CH 2 -, -CO-, -COCO-, -CO(CH 2 )m CO-, -CO(C 6 H 4 )CO-, -S-, -CS-, -SO-, -SO 2 -, -NR-, -CONR-, -NRCO-, -CSNR-, -NRCS-, -NRNR-, -HPO 4 -, -Si(OR) 2 -, -OSi(OR) 2 -, -OSi(OR) 2 O-, -Ti (OR) 2 -, -OTi(OR) 2 -, -OTi(OR) 2 Examples include O-, -Al(OR)-, -OAl(OR)-, -OAl(OR)O-, etc. (each R is independently an arbitrary substituent, preferably a hydrogen atom or an alkyl group, and m is an integer of 1 to 5). From the viewpoint of stability during production or use, X is preferably a single bond, an alkylene group having 6 or less carbon atoms (particularly a methylene group), or -CH 2 OCH 2 Among them, a single bond is most preferable in terms of thermal stability and stability under high temperature and acidic conditions.

[0046] The structural unit represented by the above formula (3) includes R 5 and R 6 is a hydrogen atom, and a structural unit having a primary hydroxyl group on the side chain is particularly preferred, and the most preferred structural unit is 1 ~R 6 are all hydrogen atoms and X is a single bond, and is a structural unit represented by the following formula (3a):

[0047]

[0048] The degree of modification (content) of the modified PVA-based resin is preferably 0.1 to 20 mol%, more preferably 0.5 to 15 mol%, even more preferably 1 to 10 mol%, and particularly preferably 2 to 8 mol%. If the modification rate is too low, the reactivity with adhesive resins such as acid-modified polyolefin-based resins tends to decrease, while if it is too high, the crystallization rate becomes too slow, and when a laminate is formed with another resin, the laminate tends to deform, resulting in a poor appearance.

[0049] The number-average degree of polymerization of the modified PVA-based resin (measured in accordance with JIS K6726:1994) is preferably 150 to 4000, more preferably 200 to 2000, even more preferably 250 to 800, and particularly preferably 300 to 600. If the average degree of polymerization is too low, it tends to be difficult to form a stable shape during melt molding, whereas if it is too high, the viscosity of the resin composition tends to become too high, making molding difficult.

[0050] The viscosity of a 4% by mass aqueous solution of the modified PVA-based resin at 20°C, measured in accordance with JIS K6726: 1994, is preferably 1.5 to 20 mPa s, more preferably 2 to 12 mPa s, and particularly preferably 2.5 to 8 mPa s. If the viscosity is too low, it tends to be difficult to form a stable shape during melt molding, while if the viscosity is too high, molding tends to be difficult.

[0051] The saponification degree of the modified PVA-based resin (average saponification degree measured in accordance with JIS K6726:1994) is preferably 70 to 100 mol%, more preferably 80 to 99.9 mol%, and particularly preferably 85 to 99.7 mol%. If the saponification degree is too low, the gas barrier property tends to decrease.

[0052] The melting point of the modified PVA resin is preferably 160 to 230°C, and the decomposition temperature is preferably 250 to 350°C, although this depends on the degree of polymerization and the degree of saponification.

[0053] The PVA-based resin that can be used in the resin composition of the present invention may be a single type or a mixture of two or more types. When a mixture of two or more types is used, examples of the mixture include a combination of the above-mentioned unmodified PVA-based resins, an unmodified PVA-based resin and various modified PVA-based resins, and different types of modified PVA-based resins. Examples of the mixture include a combination of modified PVA-based resins of the same type but different in saponification degree, polymerization degree, modification rate, etc.

[0054] The PVA-based resin content in the resin composition is preferably 80% by mass or more, more preferably 90% by mass or more, and even more preferably 95% by mass or more.

[0055] <Formic Acid, Formate Ion> Formic acid is a carboxylic acid that has a formyl group in addition to a carboxy group.

[0056] The thermal stability and molding stability of PVA-based resins can be improved by adjusting the ratio of acid to base they contain. Generally, acetic acid and / or acetate salts are used as the acid. However, the present inventors have discovered that the thermal stability and molding stability of PVA-based resins during melt molding can be improved by using formic acid and / or formate salts as the acid in addition to acetic acid and / or acetate salts. While the reason for this is unclear, it is presumed that because formic acid and formate salts have reducing properties, oxidative decomposition of the PVA-based resin is suppressed compared to when acetic acid or acetate salts alone are used. Here, acetic acid and acetate ions are collectively referred to as "acetate radicals," and formic acid and formate ions are collectively referred to as "formate radicals."

[0057] Formic acid can generally be produced by a method such as (i) reacting methanol with carbon monoxide under strongly basic conditions to produce methyl formate, followed by hydrolysis; (ii) reacting methyl formate with ammonia to produce formaldehyde, followed by hydrolysis with sulfuric acid; or (iii) reacting sodium hydroxide with carbon monoxide to produce sodium formate, followed by neutralization with hydrochloric acid.

[0058] Commercially available formic acid may be used, and examples of commercially available formic acid include formic acid manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.

[0059] Formate ions can be added using a formate salt, such as sodium formate, potassium formate, lithium formate, magnesium formate, calcium formate, barium formate, zinc formate, copper formate, iron formate, nickel formate, manganese formate, lead formate, tin formate, chromium formate, or ammonium formate, with sodium formate being preferred.

[0060] Commercially available sodium formate may be used, and examples of commercially available sodium formate include sodium formate manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.

[0061] The content of formic acid groups in the resin composition of the present invention (per mass of the total resin composition) is 4 to 500 ppm, preferably 4 to 450 ppm, and more preferably 5 to 100 ppm. The content of formic acid groups is preferably 4.3 ppm or more, more preferably 4.5 ppm or more, even more preferably 4.8 ppm or more, still more preferably 5 ppm or more, particularly preferably 10 ppm or more, and particularly preferably 15 ppm or more. The content of formic acid groups is preferably 450 ppm or less, more preferably 400 ppm or less, even more preferably 300 ppm or less, still more preferably 200 ppm or less, particularly preferably 150 ppm or less, and particularly preferably 100 ppm or less. The numerical range of the formic acid group content can be set by arbitrarily combining the above-mentioned lower and upper limits and the numerical values ​​described in the Examples section. The same applies to numerical ranges other than the content of formic acid groups.

[0062] In order to obtain the effect of improving thermal stability and molding stability due to the formic acid group, the above-mentioned content (4 to 500 ppm) is necessary. When the formic acid group content is 4 ppm or more, thermal stability is improved. Furthermore, when the formic acid group content is 500 ppm or less, molding stability during melt molding is improved. The content of formic acid groups in the resin composition can be measured by the measurement method described in the Examples section.

[0063] The resin composition of the present invention may contain, as the formate radical, only formic acid, only formate ions, or both formic acid and formate ions.

[0064] <Acetic acid, acetate ion> The resin composition of the present invention further contains acetate radicals (acetic acid, acetate ion). Acetic acid is a type of carboxylic acid and has a linear saturated hydrocarbon chain. Acetic acid can be synthesized by carbonylation of methanol, and an example of a commercially available product is acetic acid manufactured by Fujifilm Wako Pure Chemical Industries, Ltd. Acetate ions can be added using acetate salts. The acetate salt is not limited to any particular salt, and sodium acetate is preferably used. An example of a commercially available sodium acetate product is sodium acetate manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.

[0065] The content of acetate groups in the resin composition of the present invention (per mass of the total resin composition) is preferably 1,000 ppm or more, more preferably 1,500 ppm or more, even more preferably 1,800 ppm or more, and particularly preferably 2,000 ppm or more, from the viewpoint of molding stability during melt molding. The content of acetate groups is preferably 10,000 ppm or less, more preferably 9,500 ppm or less, even more preferably 9,000 ppm or less, and particularly preferably 8,500 ppm or less, from the viewpoint of thermal stability. The content of acetate groups is, for example, 10,000 ppm or less, preferably 1,000 to 10,000 ppm.

[0066] The acetate group may be contained as an impurity generated during the production process of the PVA-based resin, or may be added separately. The acetate group content in the resin composition can be measured by the method described in the Examples section.

[0067] Furthermore, the content ratio of formate groups to acetate groups (formate groups / acetate groups) is 0.001 or more, preferably 0.0015 or more, more preferably 0.0018 or more, and particularly preferably 0.002 or more, from the viewpoint of thermal stability and molding stability. Furthermore, the content ratio of formate groups to acetate groups (formate groups / acetate groups) is 0.200 or less, more preferably 0.100 or less, and particularly preferably 0.050 or less, from the viewpoint of thermal stability. That is, the content ratio of formate groups to acetate groups (formate groups / acetate groups) is 0.001 to 0.200. Note that the content ratio of formate groups to acetate groups (formate groups / acetate groups) is based on mass.

[0068] The resin composition of the present invention may contain only acetic acid, only acetate ions, or both acetic acid and acetate ions as the acetate radical.

[0069] <Other Components> 1. Other Plasticizers The resin composition of the present invention may contain other plasticizers within a range that does not impair the effects of the present invention (water solubility, gas barrier properties).

[0070] 2. Other Resins The resin composition of the present invention may contain other polymers (resins) within a range that does not impair the effects of the present invention (for example, less than 30% by mass of the resin composition). Examples of polymers (resins) that can be contained include various thermoplastic resins such as polyamide, polyester, polyethylene, polypropylene, and polystyrene.

[0071] 3. Other Additives The resin composition of the present invention may further contain, as necessary, a reinforcing agent, a filler, a pigment, a dye, a lubricant, an antioxidant, an antistatic agent, an ultraviolet absorber, a heat stabilizer, a light stabilizer, a surfactant, an antibacterial agent, an antistatic agent, a drying agent, an antiblocking agent, a flame retardant, a crosslinking agent, a curing agent, a foaming agent, a crystal nucleating agent, and the like, within a range that does not impair the effects of the present invention (for example, 10% by mass or less of the resin composition).

[0072] The resin composition of the present invention having the above-described composition has good thermal stability and molding stability due to the coexistence of formic acid groups and acetate groups, without impairing the properties of the PVA-based resin.

[0073] <Method for Producing Resin Composition> The resin composition having the above-described composition can be produced by (i) dry-blending a PVA-based resin with formic acid and / or a formate, acetic acid and / or an acetate, and other components, followed by melt-kneading, or (ii) mixing an aqueous solution of a PVA-based resin with formic acid and / or a formate, acetic acid and / or an acetate, and other components. Method (i) is preferred, as it allows for the production of a pellet-shaped resin composition. Acetate radicals may be present as impurities generated during the production process of the PVA-based resin. In this case, it is not necessary to add acetic acid and / or an acetate in methods (i) and (ii).

[0074] When acetic acid and / or an acetate salt is added, the order of addition of formic acid and / or a formate salt and acetic acid and / or an acetate salt does not matter. They may be pre-mixed and added to the PVA-based resin as a mixture. Furthermore, formic acid and / or a formate salt may be added to a pre-mixed mixture of the PVA-based resin and acetic acid and / or an acetate salt.

[0075] [Melt-molded article of resin composition and manufacturing method thereof] The resin composition of the present invention is melt-moldable, and a melt extrusion molding method commonly used for thermoplastic resins can be employed. Therefore, the resin composition of the present invention can be suitably used for manufacturing various molded articles. For example, the resin composition of the present invention can be used for melt-molded articles requiring gas barrier properties, particularly for bags made from melt-molded films, stretched films, and sheets, and containers and lids made from cups, trays, tubes, bottles, and the like. The film, sheet, or container may be made from the resin composition of the present invention alone (single layer), or may be used as a multilayer structure in which two or more layers of other thermoplastic resins, papers, etc. are laminated. In such a multilayer structure, at least one layer made from the resin composition of the present invention (resin composition layer) is sufficient.

[0076] Examples of uses of the multilayer structure containing a resin composition layer of the present invention include food packaging materials such as coffee capsules and shrink films, medicine packaging materials, cosmetic packaging materials such as cases for lotion and foundation, packaging materials for metal parts, packaging materials for electronic parts, packaging materials for items in which deterioration of properties due to oxidation or moisture absorption should be suppressed, packaging materials for substances in which odor transfer or odor leakage is a concern, and multilayer structures used in various agricultural sheets and agricultural materials such as mulch sheets, fumigation sheets, seedling trays, and covering sheets.

[0077] Applicable melt molding methods include injection molding and extrusion molding. Extrusion molding is particularly suitable as a molding method for films or sheets, and examples thereof include T-die molding and inflation molding (tubular film method). Not only single-layer extrusion but also multi-layer extrusion may be used. Multi-layer extrusion (co-extrusion molding) is suitable for producing a multi-layer structure in which films are laminated.

[0078] The obtained film or sheet may be subjected to secondary processing such as uniaxial or biaxial stretching. Since the resin composition of the present invention has excellent stretchability, it is preferable to subject the film or sheet to a stretching treatment in order to improve the strength of the film and further improve the gas barrier properties.

[0079] The present invention will be further explained below with reference to examples and comparative examples, but the present invention is not limited to the following examples.

[0080] [Measurement and Evaluation Methods] 1. Saponification Degree (mol %) Measured in accordance with JIS K6726:1994.

[0081] 2. Number average degree of polymerization: Measured in accordance with JIS K6726:1994.

[0082] 3. Degree of modification (mol %): Calculated from the amount of copolymerizable monomer charged during synthesis of the PVA-based resin.

[0083] 4. Measurement of Formic Acid Radical Content Formic acid radical content was determined with reference to Journal of Pharmaceutical and Biomedical Analysis 41 (2006) 738-743. 5.0 g of p-toluenesulfonic acid was dissolved in ethanol to prepare a 500 ml solution (1% p-toluenesulfonic acid-ethanol solution). 0.5 g of sample (pellets were freeze-pulverized) was precisely weighed into a 20 ml vial, and 5 ml of 1% p-toluenesulfonic acid-ethanol solution was added using a volumetric pipette. The vial was then sealed with hand clippers (the blank contained only 5 ml of 1% p-toluenesulfonic acid-ethanol solution). The vial was placed in an ultrasonic cleaner set at 60°C and operated for 2 hours to convert the formic acid to ethyl ester. The vial was then removed from the ultrasonic cleaner and allowed to stand at room temperature for at least 3 hours. 0.5 g of formic acid was precisely weighed into a volumetric flask and the volume was adjusted to 50 ml with ethanol (10,000 mg / L solution). The solution was diluted stepwise to prepare standard solutions, and 0.5 g of the standard solution was precisely weighed into a 20 ml vial. 5 ml of a 1% p-toluenesulfonic acid-ethanol solution was added using a volumetric pipette, and the vial was sealed with a hand clipper. Headspace analysis was performed under the conditions shown in Table 1 below.

[0084]

[0085] In Table 1, GC means gas chromatography, and MS means mass spectrometry.

[0086] 5. Measurement of Acetate Radical Content The acetate radical content was measured by the pH measurement and neutralization titration methods described below. (1) pH Measurement: 6.00 g of resin composition pellets and 138 g of water were weighed into a medium bottle, the bottle's lid was closed, and the bottle was placed in a thermostatic water bath at 30±1°C and stirred for 2 hours to dissolve. After 2 hours, the lid of the medium bottle was opened, and stirring and dissolution continued for 10 minutes, after which stirring was stopped. The electrodes of the pH meter "F-54 (HORIBA)" were removed from the immersion solution and washed with pure water. The pH meter was then calibrated with buffer solutions of pH = 4.01 and pH = 6.86. After calibration, the sample was immersed in the electrode and the pH was measured. (2) Neutralization Titration: 3.00 g of resin composition pellets and 100 g of water were weighed into an Erlenmeyer flask. The mixture was heated and stirred to dissolve. After dissolution, the mixture was cooled to room temperature, and 5 drops of indicator (methyl orange) were added. The solution was titrated with a 0.1 mol / L aqueous HCl solution until it turned yellow-red.

[0087] 6. Thermal Stability Thermal stability was evaluated by the following TGA constant temperature method. 5 mg of resin composition pellets were heated under conditions of 20 mL / min in a nitrogen atmosphere, 230°C temperature, and 1 hour using a thermogravimetric analyzer (Perkin Elmer, Pyris 1 TGA), and the weight was measured to determine the residual rate. When the residual rate was 90% or more, the thermal stability was evaluated as good. When the residual rate was less than 90%, the thermal stability was evaluated as poor.

[0088] 7. Molding Stability Dynamic viscosity behavior was evaluated by the following method. 55 g of resin composition pellets were kneaded for 30 minutes under conditions of 230°C and 50 rpm in a Plastograph (manufactured by Brabender). The torque values ​​were measured after 5 minutes and after 20 minutes, and the torque ratio (Torque (20 minutes) / Torque (5 minutes)) was used for evaluation. A larger value indicates a greater increase in the viscosity of the PVA-based resin composition. In melt molding, it is preferable for the PVA-based resin composition to exhibit dynamic viscosity behavior with minimal viscosity change.

[0089] [PVA-based resin] A PVA-based resin having a 1,2-diol-containing side chain structural unit represented by formula (3a) was used as the side-chain primary hydroxyl group-containing PVA-based resin. The PVA-based resin having a 1,2-diol-containing side chain structural unit in a side chain had a degree of modification (content of the 1,2-diol-containing side chain structural unit) of 6 mol%, a degree of saponification measured in accordance with JIS K6726 of 99.2 mol%, and a number-average degree of polymerization measured in accordance with JIS K6726 of 450.

[0090]

[0091] (1) Formic acid: Formic acid manufactured by Fujifilm Wako Pure Chemical Industries, Ltd. was used. (2) Sodium formate: Sodium formate manufactured by Fujifilm Wako Pure Chemical Industries, Ltd. was used. (3) Acetic acid: Acetic acid manufactured by Fujifilm Wako Pure Chemical Industries, Ltd. was used. (4) Sodium acetate: Sodium acetate manufactured by Fujifilm Wako Pure Chemical Industries, Ltd. was used.

[0092] [Preparation and Evaluation of Resin Compositions] (Examples 1 to 6, Comparative Examples 1 to 4) A side chain 1,2-diol-modified PVA-based resin, formic acid, sodium formate, acetic acid, and sodium acetate were blended in the proportions shown in Table 2, and melt-kneaded under the following conditions using a twin-screw extruder TEM-18DS (Shibaura Machine Co., Ltd.) to prepare pellets of each resin composition according to Examples 1 to 6 and Comparative Examples 1 to 4.

[0093] Diameter (D) 20 mm L / D = 48 Screw rotation speed: 300 rpm Set temperatures: C1 / C2 / C3 / C4 / C5 / C6 / D = 160 / 200 / 200 / 210 / 210 / 200 / 200°C Screw pattern: 2-position mixing screw Screen mesh: 90 / 120 / 90 mesh Discharge rate: 5 kg / hr

[0094] The resin composition pellets prepared according to the above measurement and evaluation methods were evaluated for thermal stability by a constant temperature TGA method and molding stability by dynamic viscosity behavior. The results are shown in Table 2.

[0095]

[0096] As shown in Table 2 above, the resin composition of Comparative Example 1, which contains a large amount of formate groups and has a high formate group / acetate group ratio, and the resin compositions of Comparative Examples 2 and 3, which have a low formate group / acetate group ratio, have low residual rates in the TGA constant temperature evaluation, indicating poor thermal stability. Furthermore, the resin composition of Comparative Example 4, which contains a small amount of formate groups, has poor molding stability, indicating a large viscosity change in the dynamic viscosity behavior evaluation. On the other hand, the resin compositions of Examples 1 to 6 had high residual rates in the TGA constant temperature evaluation and small viscosity changes in the dynamic viscosity behavior evaluation. These results demonstrate that the resin compositions of the present invention have good thermal stability and molding stability.

[0097] (Examples 7-8, Comparative Examples 5-6) An unmodified PVA-based resin was used as the PVA-based resin. The PVA-based resin used had a degree of saponification of 87.6 mol% as measured in accordance with JIS K6726 and a number-average degree of polymerization of 500 as measured in accordance with JIS K6726. Resin composition pellets according to Examples 7-8 and Comparative Examples 5-6 were prepared in the same manner as Examples 1-6 and Comparative Examples 1-4, except that the unmodified PVA-based resin, formic acid, sodium formate, acetic acid, and sodium acetate were blended in the proportions shown in Table 3. The resin composition pellets prepared according to the above measurement and evaluation methods were evaluated for thermal stability using a constant temperature TGA method and molding stability based on dynamic viscosity behavior. The results are also shown in Table 3.

[0098]

[0099] As shown in Table 3 above, the resin composition of Comparative Example 6, which contains a small amount of formic acid groups, exhibited poor molding stability due to the large viscosity change in the dynamic viscosity behavior evaluation. On the other hand, the resin compositions of Examples 7 and 8 had a high residual rate in the TGA constant temperature evaluation, and the viscosity change in the dynamic viscosity behavior evaluation was smaller than that of the resin compositions of Comparative Examples 5 and 6. These results demonstrate that the resin compositions of the present invention have good thermal stability and molding stability.

[0100] Although the above examples show specific embodiments of the present invention, the examples are merely illustrative and should not be construed as limiting. Various modifications that are obvious to those skilled in the art are intended to fall within the scope of the present invention.

[0101] This application is based on a Japanese patent application (Patent Application No. 2023-58957) filed on March 31, 2023, the contents of which are incorporated herein by reference.

[0102] The resin composition of the present invention contains a PVA-based resin and has sufficient thermal stability and molding stability during melt molding, and therefore can be suitably used for various packaging materials, particularly food packaging materials such as coffee capsules.

Claims

1. A resin composition comprising a polyvinyl alcohol resin, a formic acid group, and an acetate group, wherein the content of the formic acid group in the resin composition is 4 to 500 ppm, and the content ratio of the formic acid group to the acetate group (formic acid group / acetate group) is 0.001 to 0.

200.

2. The resin composition according to claim 1, wherein the content of the acetate group in the resin composition is 10,000 ppm or less.

3. The resin composition according to claim 1, wherein the polyvinyl alcohol resin contains a structural unit having a modifying group other than ethylene.

4. The resin composition according to claim 1, wherein the polyvinyl alcohol resin contains a structural unit having a hydrophilic modifying group.

5. The resin composition according to claim 1, wherein the polyvinyl alcohol resin contains a structural unit having a primary hydroxyl group in a side chain.

6. The resin composition according to claim 1, wherein the content of the formic acid group is 5 to 100 ppm.

7. A molded article comprising the resin composition according to any one of claims 1 to 6.

8. A film containing the resin composition according to any one of claims 1 to 6.

9. A sheet containing the resin composition according to any one of claims 1 to 6.

10. A multilayer structure comprising at least one layer made of the resin composition according to any one of claims 1 to 6.

Citation Information

Patent Citations

  • Polyvinyl alcohol-based resin composition

    JP2001288321A

  • Novel vinyl alcohol resin and its use

    JP2002284818A

  • Polyvinyl alcohol-based resin having 1,2-glycol bonds in side chains and method for producing the same

    JP2004285143A

  • Recording medium

    JP2006095825A

  • Shipment and delivery assisting system and program

    JP2023058957A