Method for producing polypropylene resin foam molded body

The method of heating polypropylene resin foam particles without internal pressure, followed by water spraying and cooling, addresses the deformation issue while enhancing sound absorption in polypropylene resin foam products, making them suitable for diverse applications.

WO2024204495A1PCT designated stage expired Publication Date: 2024-10-03KANEKA CORP

Patent Information

Application Number
PCT/JP2024/012567
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2024-03-28
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Polypropylene resin foam molded products often deform significantly after manufacturing, and existing methods that apply internal pressure during molding do not adequately address the need for both sound absorption performance and minimal deformation.

Method used

A method involving heating polypropylene resin foam particles without internal pressure, followed by water spraying and water cooling, to produce a product with a porosity of 25% or more, which results in a polypropylene resin foam molded product with excellent sound absorption performance and reduced deformation.

Benefits of technology

The method effectively achieves both excellent sound absorption performance and a small amount of deformation in the polypropylene resin foam molded product, making it suitable for various applications such as packaging, insulation, and automotive components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024012567_03102024_PF_FP_ABST
    Figure JP2024012567_03102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention addresses the problem of providing a polypropylene resin foam molded body which has excellent sound absorption performance, and in which the amount of deformation is reduced. The present invention provides a method for producing a polypropylene resin foam molded body, the method comprising: a step in which polypropylene resin foam particles, to which no internal pressure is applied, are heated within a mold; and a water cooling step in which a pre-polypropylene resin foam molded body, or both of the pre-polypropylene resin foam molded body and the mold are water-cooled by spraying water thereon for a specific period of time. The porosity of the polypropylene resin foam molded body is 25% or more.
Need to check novelty before this filing date? Find Prior Art

Description

Method for producing polypropylene resin foam molded body

[0001] The present invention relates to a method for producing a polypropylene resin foam molded article.

[0002] Polypropylene-based resin foam molded articles are widely used in applications such as cushioning packaging materials, logistics materials (e.g., returnable boxes, cushioning materials for truck transport, etc.), heat insulating materials, civil engineering and construction materials, and automotive components (e.g., tool boxes, floor core materials, etc.) (e.g., Patent Document 1).

[0003] Foamed materials having sound-absorbing properties are required for automobile interior materials. For example, the technology of Patent Document 2 is known as a polypropylene resin foam molded article having sound-absorbing properties.

[0004] JP 2001-198940 A JP 2007-45979 A

[0005] However, polypropylene-based resin foam molded articles may be deformed (for example, shrunk) after production, and there is a demand for polypropylene-based resin foam molded articles that are less likely to deform after production.

[0006] An object of one embodiment of the present invention is to provide a polypropylene resin foam molded article that has excellent sound absorbing properties and a small amount of deformation.

[0007] The present inventors have conducted extensive research to solve the above problems and have completed the present invention.

[0008] That is, a method for producing a polypropylene-based resin foam molded product according to one embodiment of the present invention includes a heating step of heating polypropylene-based resin foam beads to which no internal pressure has been applied in a mold, and a water-cooling step of water-cooling the pre-polypropylene-based resin foam molded product obtained in the heating step, or both the pre-polypropylene-based resin foam molded product and the mold, by spraying water for one second or more, and the polypropylene-based resin foam molded product has a porosity of 25% or more.

[0009] According to one embodiment of the present invention, it is possible to provide a polypropylene resin foam molded article that has excellent sound absorbing properties and a small amount of deformation.

[0010] Fig. 1 is a schematic diagram of a polypropylene-based resin foam molded article 100 used to evaluate the amount of deformation. Fig. 2 is a front view of an outlet hole having a star-shaped cross section. Fig. 3 is a view of a star-shaped polypropylene-based resin particle viewed from one direction. Fig. 4 is a view of a star-shaped polypropylene-based resin foam particle viewed from one direction. Fig. 5 is a front view of an outlet hole having an anchor cross-shaped cross section different from that of Fig. 2. Fig. 6 is a front view of an outlet hole having a cross section different from that of Figs. 2 and 5.

[0011] An embodiment of the present invention will be described below, but the present invention is not limited thereto. The present invention is not limited to the respective configurations described below, and various modifications are possible within the scope of the claims. Furthermore, embodiments or examples obtained by combining the technical means disclosed in different embodiments or examples are also included in the technical scope of the present invention. Furthermore, new technical features can be formed by combining the technical means disclosed in each embodiment. All academic literature and patent documents described in this specification are incorporated herein by reference. Furthermore, unless otherwise specified in this specification, the term "A to B" representing a numerical range means "greater than or equal to A (including and greater than A) and less than or equal to B (including and less than B)."

[0012] In this specification, a "structural unit derived from an X monomer" contained in a polymer, copolymer, or resin may be referred to as an "X unit."

[0013] Unless otherwise specified in this specification, the structural unit is X 1 Units and X 2 Units, ... and X n A copolymer containing units (n is an integer of 2 or more) is referred to as "X 1 / X 2 / ・・・ / X n Also referred to as "copolymer". X 1 / X 2 / ・・・ / X nUnless otherwise specified, the polymerization mode of the copolymer is not particularly limited, and the copolymer may be a random copolymer, an alternating copolymer, a block copolymer, or a graft copolymer.

[0014] Unless otherwise specified herein, the term "C" refers to functional groups and compounds. n-m " means that the number of carbon atoms contained in the functional group or compound is n to m.

[0015] [1. Technical Concept of One Embodiment of the Invention] The present inventors have conducted extensive research with the aim of providing a polypropylene resin foam molded article that has excellent sound absorbing properties and a small amount of deformation. In the process, the present inventors have newly discovered that a foam molded article with excellent sound absorbing properties can be obtained by molding foamed beads to which no internal pressure has been applied.

[0016] On the other hand, as described in Patent Documents 1 and 2, conventionally, when producing a polypropylene resin foam molded article, a technique of molding polypropylene resin foam beads to which internal pressure has been applied has been commonly used.

[0017] However, the present inventors have newly discovered a problem that when expanded beads to which no internal pressure is applied are molded, the amount of deformation of the expanded molded article may become large.

[0018] Therefore, the present inventors have conducted further intensive research in order to provide a foamed molded article with little deformation even when foamed beads to which no internal pressure has been applied are molded. As a result, the present inventors have made the surprising new discovery that, in producing a foamed molded article having a porosity of a certain level or more using foamed beads to which no internal pressure has been applied, a polypropylene resin foamed molded article with little deformation can be obtained by including a step of spraying water for one second or more onto the foamed molded article or onto both the foamed molded article and the mold.

[0019] That is, the present inventors have made the surprising new discovery that a polypropylene resin foam molded product having excellent sound absorption performance and little deformation can be provided by using a manufacturing method for a polypropylene resin foam molded product having the following configuration, and have thus completed the present invention: a manufacturing method for a polypropylene resin foam molded product, comprising: a heating step of heating polypropylene resin foam beads to which no internal pressure has been applied in a mold; and a water-cooling step of water-cooling the pre-polypropylene resin foam molded product obtained in the heating step, or both the pre-polypropylene resin foam molded product and the mold, by spraying water for one second or more, wherein the polypropylene resin foam molded product has a porosity of 25% or more.

[0020] Before describing in detail the method for producing a polypropylene-based resin foam molded article in one embodiment of the present invention (hereinafter, sometimes referred to as "this production method"), we will first provide a detailed description of the polypropylene-based resin foam beads used in this production method and the polypropylene-based resin particles that serve as the raw material (material) for the polypropylene-based resin foam beads.

[0021] In this specification, "polypropylene resin particles" may be referred to as "resin particles," "expanded polypropylene beads" may be referred to as "expanded beads," and "polypropylene foam molded body" may be referred to as "expanded molded body." In this specification, "resin particles according to one embodiment of the present invention" may be referred to as "the present resin particles," and "expanded beads according to one embodiment of the present invention" may be referred to as "the present expanded beads." Furthermore, "polypropylene foam molded body according to one embodiment of the present invention" may be referred to as "the present foam molded body," and "method for producing a polypropylene resin foam molded body according to one embodiment of the present invention" may be referred to as "the present production method."

[0022] 2. Polypropylene-Based Resin Particles In this specification, the term "polypropylene-based resin particles" refers to resin particles containing a polypropylene-based resin. In other words, the polypropylene-based resin particles contain a polypropylene-based resin as a resin component.

[0023] The raw materials (materials) contained in the polypropylene-based resin particles will be described in detail below.

[0024] <Polypropylene Resin> In this specification, the term "polypropylene resin" refers to a resin containing 50 mol % or more of propylene units in 100 mol % of all structural units constituting the resin.

[0025] The polypropylene-based resin may be (i) a homopolymer of propylene, (ii) a block copolymer, impact copolymer, alternating copolymer, random copolymer, or graft copolymer of propylene and a monomer other than propylene, or (iii) a mixture of two or more of these.

[0026] The polypropylene resin preferably contains 75 mol % or more of propylene units out of 100 mol % of all structural units constituting the polypropylene resin.

[0027] The polypropylene-based resin preferably contains one or more selected from the group consisting of (i) a homopolymer of propylene, (ii) a block copolymer of propylene and a monomer other than propylene, and (iii) a random copolymer of propylene and a monomer other than propylene, and more preferably consists of only one or more selected from the group.

[0028] The polypropylene-based resin is preferably a random copolymer of propylene and a monomer other than propylene, since this has the advantage that the resin particles and the expanded particles can be processed at a low heating temperature during expansion of the resin particles and molding of the expanded particles.

[0029] A polypropylene-based resin may have, in addition to a propylene unit, one or more units, or may have one or more types, of structural units derived from a monomer other than a propylene monomer. A "monomer other than a propylene monomer" used in the production of a polypropylene-based resin may also be referred to as a "comonomer." A "structural unit derived from a monomer other than a propylene monomer" contained in a polypropylene-based resin may also be referred to as a "comonomer unit."

[0030] Comonomers include α-olefins having 2 or 4 to 12 carbon atoms, such as ethylene, 1-butene, isobutene, 1-pentene, 3-methyl-1-butene, 1-hexene, 4-methyl-1-pentene, 3,4-dimethyl-1-butene, 1-heptene, 3-methyl-1-hexene, 1-octene, and 1-decene.

[0031] Specific examples of polypropylene-based resins include polypropylene homopolymers, ethylene / propylene random copolymers, 1-butene / propylene random copolymers, 1-butene / ethylene / propylene random copolymers, ethylene / propylene block copolymers, 1-butene / propylene block copolymers, propylene / chlorinated vinyl copolymers, propylene / maleic anhydride copolymers, and styrene-modified polypropylene-based resins.

[0032] As the polypropylene-based resin, one of the above-mentioned specific examples may be used alone, or two or more may be used in combination. Among the above-mentioned specific examples, ethylene / propylene random copolymers and / or 1-butene / ethylene / propylene random copolymers are preferred as the polypropylene-based resin, in terms of the resin particles having good expandability and the expanded particles having good moldability.

[0033] Consider a case where an ethylene / propylene random copolymer or a 1-butene / ethylene / propylene random copolymer is used as the polypropylene-based resin (Case A). In Case A, the ethylene content of the ethylene / propylene random copolymer or the 1-butene / ethylene / propylene random copolymer is not particularly limited, but is preferably 0.2 wt% to 10.0 wt%, more preferably 0.3 wt% to 5.0 wt%, and even more preferably 0.4 wt% to 2.5 wt% based on 100 wt% of each copolymer. The ethylene content in the copolymer refers to the content (wt%) of ethylene units contained in 100 wt% of all structural units constituting the copolymer. When the ethylene content in the ethylene / propylene random copolymer or the 1-butene / ethylene / propylene random copolymer is (i) 0.2 wt% or more, the expandability of the resin particles and / or the moldability of the expanded particles tend to be good, and (ii) when it is 10.0 wt% or less, there is no risk of a decrease in the mechanical properties of the expanded molded article.

[0034] In case A, the 1-butene content in the 1-butene / ethylene / propylene random copolymer is not particularly limited, but is preferably 0.2 to 10.0% by weight, more preferably 1.0 to 8.0% by weight, even more preferably 2.0 to 6.0% by weight, and particularly preferably 3.0 to 5.0% by weight, based on 100% by weight of the copolymer. The 1-butene content in the copolymer refers to the content (% by weight) of 1-butene units contained in 100% by weight of all structural units constituting the copolymer. When the 1-butene content in the 1-butene / ethylene / propylene random copolymer is (i) 0.2% by weight or more, the expandability of the resin particles and / or the moldability of the expanded particles tend to be improved, and (ii) when it is 10.0% by weight or less, there is no risk of a decrease in the mechanical properties of the expanded molded article.

[0035] In case A, the total content of ethylene units and 1-butene units in the 1-butene / ethylene / propylene random copolymer is not particularly limited, but is preferably 0.5 to 10.0% by weight, more preferably 1.0 to 8.0% by weight, even more preferably 2.0 to 6.0% by weight, and particularly preferably 3.0 to 5.0% by weight, based on 100% by weight of the 1-butene / ethylene / propylene random copolymer. When the total content of ethylene units and 1-butene units in the 1-butene / ethylene / propylene random copolymer is (i) 0.5% by weight or more, the expandability of the resin particles and / or the moldability of the expanded particles tend to be good, and (ii) when it is 10.0% by weight or less, there is no risk of a decrease in the mechanical properties of the expanded molded article.

[0036] The melting point of the polypropylene resin is not particularly limited, but is preferably 135°C to 160°C, more preferably 138°C to 158°C, more preferably 140°C to 156°C, more preferably 143°C to 154°C, even more preferably 145°C to 152°C, and particularly preferably 148°C to 150°C. When the melting point of the polypropylene resin is (i) 135°C or higher, a foamed molded article having excellent heat resistance can be obtained. When the melting point is (ii) 160°C or lower, it becomes easy to increase the expansion ratio of the foamed beads during the production of the foamed beads. Furthermore, when the melting point of the polypropylene resin is within the aforementioned range, it has the advantage that a polypropylene resin foamed molded article having excellent sound absorption performance and little deformation can be obtained. The method for measuring the melting point of the polypropylene resin will be described in detail in the Examples below.

[0037] The melt index (MI) of the polypropylene resin at 230°C (230±0.2°C) is preferably 3.0 g / 10 min to 30.0 g / 10 min, more preferably 4.0 g / 10 min to 20.0 g / 10 min, more preferably 5.0 g / 10 min to 15.0 g / 10 min, even more preferably 7.0 g / 10 min to 13.0 g / 10 min, and particularly preferably 8.5 g / 10 min to 12.0 g / 10 min. The MI is sometimes referred to as "melt flow rate (MFR)." This configuration has the advantage of being able to produce a polypropylene resin foam molded product with excellent sound absorption performance and minimal deformation. The method for measuring the MI of the polypropylene resin will be described in detail in the Examples below.

[0038] The polypropylene resin can be obtained by a known method. The polymerization catalyst used for synthesizing the polypropylene resin is not particularly limited, and for example, a Ziegler catalyst or a metallocene catalyst can be used.

[0039] The resin component of the polypropylene-based resin particles preferably contains 50% by weight or more of polypropylene-based resin, more preferably 60% by weight or more, more preferably 70% by weight or more, more preferably 80% by weight or more, even more preferably 90% by weight or more, and even more preferably 95% by weight or more, based on 100% by weight of the resin component. The resin component of the polypropylene-based resin particles may contain 100% by weight of polypropylene-based resin, based on 100% by weight of the resin component. In other words, the resin component of the polypropylene-based resin particles may be composed only of polypropylene-based resin.

[0040] The resin component of the polypropylene-based resin particles preferably contains, in 100% by weight of the resin component, a total of 50% by weight or more of one or more selected from the group consisting of ethylene / propylene random copolymers and 1-butene / ethylene / propylene random copolymers, more preferably 60% by weight or more, more preferably 70% by weight or more, more preferably 80% by weight or more, even more preferably 90% by weight or more, and even more preferably 95% by weight or more. The resin component of the polypropylene-based resin particles may contain, in 100% by weight of the resin component, a total of 100% by weight of one or more selected from the group consisting of ethylene / propylene random copolymers and 1-butene / ethylene / propylene random copolymers. In other words, the resin component of the polypropylene-based resin particles may be composed solely of one or more selected from the group consisting of ethylene / propylene random copolymers and 1-butene / ethylene / propylene random copolymers.

[0041] <Other Resins, etc.> The resin particles may further contain resins other than polypropylene-based resins (sometimes referred to as "other resins, etc.") as resin components, provided that the effects of the present invention are not impaired. Examples of the other resins include: (a) ethylene-based resins such as high-density polyethylene, medium-density polyethylene, low-density polyethylene, linear low-density polyethylene, linear very low-density polyethylene, ethylene / vinyl acetate copolymer, ethylene / acrylic acid copolymer, and ethylene / methacrylic acid copolymer; (b) polyphenylene ether-based resins such as polyphenylene ether and modified polyphenylene ether; (c) polyolefin-based waxes such as propylene / α-olefin-based wax; (d) olefin-based rubbers such as ethylene / propylene rubber, ethylene / butene rubber, ethylene / hexene rubber, and ethylene / octene rubber; and (e) polystyrene-based resins and hydrogenated styrene-based copolymers. Note that polyphenylene ether-based resins are amorphous resins.

[0042] When the resin particles contain other resins, the content of the other resins in the resin particles is, for example, 0.1 to 20.0 parts by weight, more preferably 0.5 to 15.0 parts by weight, even more preferably 1.0 to 10.0 parts by weight, and even more preferably 3.0 to 8.0 parts by weight, relative to 100 parts by weight of the polypropylene resin. When the content of the other resins is within the above range, there is an advantage that the expandability of the resin particles and / or the moldability of the expanded particles tend to be good.

[0043] <Additives> The resin particles may contain any additives in addition to the polypropylene-based resin. Examples of additives include colorants, hydrophilic compounds, crystal nucleating agents, antistatic agents, flame retardants, antioxidants, light stabilizers, conductive agents, and lubricants. Such additives may be contained in the resin particles, or may be added directly to the dispersion when the resin particles are foamed.

[0044] The hydrophilic compound is a substance used for the purpose of increasing the amount of water impregnated in the resin particles. The hydrophilic compound can impart foamability to the resin particles. The foamability imparting effect of the hydrophilic compound to the resin particles is particularly remarkable when water is used as the foaming agent.

[0045] <Physical Properties of Polypropylene-Based Resin Particles> (Particle Weight of Resin Particles) The weight per particle of the resin particles (particle weight) is not particularly limited, but is preferably 0.50 mg / particle to 6.0 mg / particle, more preferably 1.0 mg / particle to 5.0 mg / particle, even more preferably 1.5 mg / particle to 4.0 mg / particle, and particularly preferably 1.8 mg / particle to 3.0 mg / particle. This configuration has the advantage of improving the productivity of the polypropylene-based resin particles and the mechanical properties of polypropylene-based resin foam molded articles.

[0046] (Shape of Resin Particles) The resin particles are preferably, but not limited to, irregularly shaped resin particles. In other words, the shape of the resin particles is preferably, but not limited to, shapes generally used in producing expanded beads (spherical and cylindrical). For example, the shape is preferably one selected from the group consisting of star, anchor cross, macaroni, cross, L-shape, Y-shape, T-shape, U-shape, and polygonal shapes, and more preferably star-shape. This configuration has the advantage of being able to produce a polypropylene resin foam molded product with excellent sound absorption performance and little deformation.

[0047] In this specification, the "shape of polypropylene-based resin particles" refers to the "shape of a cross section perpendicular to the thickness direction of the polypropylene-based resin particles." When the polypropylene-based resin particles are obtained using an extruder, the thickness direction of the polypropylene-based resin particles can also be referred to as the extrusion direction of the extruder.

[0048] In other words, the shape of the resin particles is preferably such that the degree of irregularity of the resulting expanded beads satisfies the preferred numerical range of the degree of irregularity of the expanded beads described below, for example, a star shape.

[0049] Here, Fig. 2 is a front view of a discharge hole having a star-shaped cross section, which can also be considered an image obtained by imaging the discharge hole from the front. Specifically, Fig. 2 is a front view of a discharge hole provided in a die for obtaining star-shaped resin particles, which are the raw material for star-shaped expanded beads, and shows the cross-sectional shape of the discharge hole. In this specification, the "shape of the cross section of the discharge hole perpendicular to the extrusion direction of the extruder" is also referred to as the "cross-sectional shape of the discharge hole." Star-shaped resin particles are resin particles obtained by extrusion through the die shown in Fig. 2. Fig. 3 is a view of star-shaped polypropylene-based resin particles from one direction, which can also be considered an image obtained by imaging the star-shaped polypropylene-based resin particles from one direction. Star-shaped resin particles are resin particles having the shape shown in Fig. 3.

[0050] Fig. 5 is a front view of a discharge hole having an anchor-cross-shaped cross section, different from that shown in Fig. 2, and can also be considered an image obtained by photographing the discharge hole having an anchor-cross-shaped cross section from the front of the discharge hole. Specifically, Fig. 5 is a front view of a discharge hole provided in a die for obtaining anchor-cross-shaped resin particles, which are the raw material for anchor-cross-shaped expanded beads, and shows the cross-sectional shape of the discharge hole. The anchor-cross-shaped resin particles are resin particles obtained by extrusion through the die shown in Fig. 5.

[0051] In this specification, the term "macaroni-shaped" refers to a cylindrical shape having a hollow hole. Figure 6 is a front view of an outlet hole having a cross-sectional shape different from those in Figures 2 and 5, and can also be considered an image obtained by photographing an outlet hole having a cross-sectional shape different from those in Figures 2 and 5 from the front of the outlet hole. Specifically, Figure 6 is a front view of an outlet hole provided in a die for obtaining macaroni-shaped resin particles, which are the raw material for macaroni-shaped expanded beads, and shows the cross-sectional shape of the outlet hole. Macaroni-shaped resin particles are resin particles obtained by extrusion through the die shown in Figure 6.

[0052] The polypropylene-based resin particles according to one embodiment of the present invention may or may not have hollow holes.

[0053] [3. Expanded Polypropylene Resin Particles] Expanded polypropylene resin particles according to one embodiment of the present invention are expanded particles obtained by expanding the polypropylene resin particles described in [2. Polypropylene Resin Particles]. That is, the expanded polypropylene resin particles according to one embodiment of the present invention contain components contained in polypropylene resin particles (for example, polypropylene resin).

[0054] <Physical Properties of Expanded Polypropylene Resin Beads> (Bulk Density of Expanded Beads) The bulk density of the expanded beads is preferably 10.0 g / L to 300.0 g / L, more preferably 12.0 g / L to 100.0 g / L, even more preferably 14.0 g / L to 60.0 g / L, even more preferably 15.0 g / L to 50.0 g / L, and particularly preferably 16.0 g / L to 40.0 g / L. This configuration has the advantage of providing expanded beads with little variation in expansion ratio and good moldability. The method for measuring the bulk density of expanded beads will be described in detail in the Examples below.

[0055] (Degree of irregularity of expanded beads) The degree of irregularity of the expanded polypropylene resin beads, as expressed by the following formula, is preferably 2.20 or more: Degree of irregularity = true density of expanded polypropylene resin beads / bulk density of expanded polypropylene resin beads.

[0056] In this specification, the irregularity is an index showing the bulkiness of the expanded beads. The present inventors have surprisingly found that a foamed molded article obtained from expanded beads having an irregularity of 2.20 or more has the advantages of excellent sound absorption performance and reduced deformation.

[0057] The degree of deformation of the expanded beads is preferably 2.20 or more, more preferably 2.40 or more, and even more preferably 2.50 or more. This configuration has the advantage that a polypropylene resin foam molded article having excellent sound absorption performance and a small amount of deformation can be obtained.

[0058] Furthermore, the upper limit of the degree of irregularity of the expanded beads is not particularly limited, but is preferably 3.00 or less, more preferably 2.90 or less, even more preferably 2.80 or less, and particularly preferably 2.70 or less. This configuration has the advantage of producing a foamed molded article with high mechanical properties. Details of the method for measuring the degree of irregularity of the expanded beads will be explained in detail in the Examples below.

[0059] The shape of the present expanded beads satisfying the above-mentioned preferred range of the degree of irregularity can be a shape other than the shapes (spherical and cylindrical) generally used in the production of expanded beads. A "shape other than spherical and cylindrical" is sometimes referred to as an "irregular shape." In other words, the present expanded beads are preferably irregularly shaped expanded beads. The shape of the present expanded beads is preferably one selected from the group consisting of star-shaped, anchor-cross-shaped, macaroni-shaped, cross-shaped, L-shaped, Y-shaped, T-shaped, U-shaped, and polygonal shapes, and a star-shaped shape is more preferred. This configuration has the advantage of being able to produce a polypropylene resin foam molded article with excellent sound absorption performance and little deformation.

[0060] The shape of the expanded beads is the same or substantially the same as the shape of the resin beads. When the resin beads are irregularly shaped resin beads, the expanded beads obtained by expanding the resin beads are irregularly shaped expanded beads. Specifically, for example, when the resin beads are star-shaped, the expanded beads obtained by expanding the resin beads are also star-shaped. Here, Figure 4 is an image of star-shaped expanded polypropylene resin beads.

[0061] The expanded polypropylene beads according to one embodiment of the present invention may or may not have hollow holes.

[0062] <Method of manufacturing expanded polypropylene resin beads> The method of manufacturing the expanded beads is not particularly limited, and known manufacturing methods can be used as appropriate. One embodiment of the method of manufacturing the expanded beads will be described in detail below, but the above description (for example, the description in the section <Additives>) will be used as appropriate for matters other than those described in detail below. Note that the method of manufacturing the expanded beads is not limited to the following manufacturing method.

[0063] (Granulation Step) In producing the present expanded beads, first, a step of producing polypropylene-based resin beads (granulation step) can be carried out.

[0064] The granulation step is not particularly limited as long as resin particles can be obtained, and known methods can be used. An example of the granulation step is a method in which the following steps (S1) to (S3) are carried out in order: (S1) a predetermined amount of polypropylene resin and, if necessary, additives are melt-kneaded using an extruder to prepare a melt-kneaded product; (S2) the melt-kneaded product is extruded through a die provided in the extruder; and (S3) the extruded melt-kneaded product is chopped to a desired length to obtain polypropylene resin particles.

[0065] In the step (S1), a blend may be prepared in advance by blending a predetermined amount of polypropylene resin and, if necessary, additives, and the blend may be fed to an extruder and melt-kneaded to prepare a melt-kneaded product.

[0066] In the step (S2), the shape of the die may be selected according to the desired shape of the expanded beads. Here, the shape of the die is the same as or approximately the same as the desired shape of the expanded beads. For example, when resin beads obtained by extruding a resin composition using the die shown in FIG. 6 are used, macaroni-shaped expanded beads can be obtained.

[0067] In the step (S3), before the molten kneaded material is chopped, the extruded molten kneaded material may be cooled and solidified using a cooling medium such as water.

[0068] (Dispersion Step) In the production of the present expanded beads, a step (dispersion step) of dispersing the polypropylene resin particles and the blowing agent in an aqueous dispersion medium in a vessel may next be carried out.

[0069] Examples of the vessel include a pressure vessel and an autoclave-type pressure vessel. The vessel may be equipped with a stirrer therein.

[0070] Examples of aqueous dispersion media include (a) dispersion media obtained by adding methanol, ethanol, ethylene glycol, glycerin, or the like to water, (b) water such as ultrapure water, pure water, tap water, and industrial water, and (c) solutions containing salts such as sodium chloride or sodium sulfate (aqueous solutions).

[0071] Examples of the blowing agent include (a) (a-1) inorganic blowing agents such as nitrogen, carbon dioxide, air (a mixture of oxygen, nitrogen, and carbon dioxide), and (a-2) water; and (b) organic blowing agents such as (b-1) saturated hydrocarbons having 3 to 5 carbon atoms such as propane, normal butane, isobutane, normal pentane, isopentane, and neopentane, (b-2) ethers such as dimethyl ether, diethyl ether, and methyl ethyl ether, and (b-3) halogenated hydrocarbons such as monochloromethane, chloroethane, and hydrofluoroolefins.

[0072] In the present method for producing expanded beads, it is preferable to use a dispersant (e.g., an inorganic substance such as tricalcium phosphate, kaolin, or talc) and a dispersing aid (e.g., an anionic surfactant such as sodium dodecylbenzenesulfonate). This configuration can reduce adhesion of resin particles (sometimes called blocking) and improve the stability of the dispersion in the container. As a result, it has the advantage of enabling stable production of expanded beads.

[0073] The aqueous dispersion medium and the blowing agent may each be used alone or in combination of two or more.

[0074] The amounts of the aqueous dispersion medium, blowing agent, dispersant, and dispersion aid used are not particularly limited, and can be appropriately set taking into consideration (i) the stability of the dispersion (dispersibility of resin particles), (ii) the density of the resulting expanded beads, (iii) the fusion properties of the expanded molded article obtained by molding the resulting expanded beads, (iv) productivity, and (v) economic efficiency.

[0075] In the method for producing expanded beads of the present invention, it is preferable to use a pH adjuster (e.g., citric acid, malic acid, succinic acid, tartaric acid, oxalic acid, etc.), which has the advantage of being able to suppress corrosion of equipment.

[0076] The amount of the pH adjuster used is not particularly limited, but is preferably 0.001 to 1.00 parts by weight, more preferably 0.003 to 0.50 parts by weight, and even more preferably 0.005 to 0.30 parts by weight, relative to 100 parts by weight of the polypropylene-based resin particles. This configuration has the advantages of high productivity of the expanded beads and suppressing corrosion of equipment.

[0077] The method for dispersing the polypropylene-based resin particles and the blowing agent in the aqueous dispersion medium in the container, i.e., the specific method for the dispersion step, is not particularly limited, and examples thereof include a method in which the aqueous dispersion medium, the polypropylene-based resin particles, and the blowing agent are supplied to the container, and the mixture in the container is stirred with a stirrer provided in the container.

[0078] (Temperature-Pressure Increase Step and Maintaining Step) The present method for producing expanded beads preferably further includes, after the dispersing step and before the releasing step, (1) a temperature-pressure increase step of increasing the temperature inside the container to a constant temperature and increasing the pressure inside the container to a constant pressure, and (2) a maintaining step of maintaining the temperature and pressure inside the container at a constant temperature and a constant pressure, in this order. In this specification, in the temperature-pressure increase step and the maintaining step, (a) the constant temperature may be referred to as the foaming temperature, and (b) the constant pressure may be referred to as the foaming pressure.

[0079] The foaming temperature is preferably (i) the melting point of (a) a mixture containing a polypropylene-based resin and, if necessary, additives, (b) the melt-kneaded product, or (c) the resin particles −20.0°C to the melting point +20.0°C; more preferably (ii) the melting point of (a) a mixture containing a polypropylene-based resin and, if necessary, additives, (b) the melt-kneaded product, or (c) the resin particles −10.0°C to the melting point +15.0°C; and even more preferably (iii) the melting point of (a) a mixture containing a polypropylene-based resin and, if necessary, additives, (b) the melt-kneaded product, or (c) the resin particles −5.0°C to the melting point +13.0°C.

[0080] Specifically, the expansion temperature is preferably 130.0° C. to 170.0° C., more preferably 135.0° C. to 165.0° C., further preferably 138.0° C. to 162.0° C., and particularly preferably 140.0° C. to 160.0° C. This configuration has the advantage of making it easy to obtain expanded beads with good expandability and moldability.

[0081] The expansion pressure is preferably 0.5 MPa (gauge pressure) to 10.0 MPa (gauge pressure), more preferably 0.6 MPa (gauge pressure) to 5.0 MPa (gauge pressure), and even more preferably 0.6 MPa (gauge pressure) to 3.5 MPa (gauge pressure). When the expansion pressure is 0.5 MPa (gauge pressure) or more, expanded beads with a suitable density can be obtained.

[0082] In the holding step, the time (holding time) for holding the dispersion in the container at temperatures near the foaming temperature and foaming pressure is not particularly limited, but is, for example, preferably 10 minutes to 60 minutes, more preferably 12 minutes to 50 minutes, and even more preferably 15 minutes to 40 minutes.

[0083] (Releasing Step) When producing the present expanded beads, a step (releasing step) of releasing the dispersion obtained in the dispersing step into a region having a pressure lower than the pressure inside the container may be carried out.

[0084] The discharging step can expand the resin particles, resulting in expanded particles. The discharging step can also be described as a step of opening one end of the container and discharging the dispersion liquid in the container into a region (space) with a pressure lower than the expansion pressure (i.e., the pressure inside the container).

[0085] In the releasing step, the term "region under a pressure lower than the foaming pressure" refers to a "region under a pressure lower than the foaming pressure" or a "space under a pressure lower than the foaming pressure", and can also be referred to as "an atmosphere under a pressure lower than the foaming pressure". The region under a pressure lower than the foaming pressure may be, for example, a region under atmospheric pressure.

[0086] (Expansion Process) The process from the dispersion process to the release process may be referred to as the expansion process. The process of producing expanded beads from resin beads in this manner is referred to as the "first-stage expansion process," and the obtained expanded beads are referred to as "first-stage expanded beads."

[0087] (Second-stage expansion process) In order to obtain expanded beads with a high expansion ratio, the first-stage expanded beads obtained in the first-stage expansion process may be expanded again. The process of increasing the expansion ratio of the first-stage expanded beads is called the "second-stage expansion process", and the polypropylene resin expanded beads obtained by the second-stage expansion process are called "second-stage expanded beads". The specific method for the second-stage expansion process is not particularly limited, and known methods can be used.

[0088] [4. Polypropylene-based resin foam molded article] The polypropylene-based resin foam molded article according to one embodiment of the present invention is preferably a foam molded article obtained by the manufacturing method described in the section below, [5. Manufacturing method for polypropylene-based resin foam molded article]. This method has the advantage of being able to obtain a polypropylene-based resin foam molded article that has excellent sound absorption performance and little deformation.

[0089] The polypropylene-based resin foam molded article according to one embodiment of the present invention is not particularly limited, but is preferably a polypropylene-based resin foam molded article having a moisture content of 140% to 300%, calculated from the following formula (1) using the weight (wet weight) of the polypropylene-based resin foam molded article measured after leaving it at room temperature for 1 hour and the weight (dry weight) of the polypropylene-based resin foam molded article measured after further drying at 75°C for 12 hours and leaving it at room temperature for 4 hours: Moisture content (%) = {(wet weight - dry weight) / dry weight} × 100 ... (1).

[0090] This configuration has the advantage that a polypropylene resin foam molded article having excellent sound absorbing properties and a small amount of deformation can be obtained.

[0091] <Physical Properties of Polypropylene-Based Resin Foam Molded Article> (Moisture Content of Foam Molded Article) The moisture content of the foam molded article is 140% to 300%, preferably 150% to 295%, more preferably 180% to 290%, more preferably 200% to 285%, even more preferably 250% to 280%, and particularly preferably 270% to 280%. This configuration has the advantage of enabling the production of a polypropylene-based resin foam molded article with little deformation.

[0092] As described above, the moisture content of a polypropylene resin foam molded article is calculated according to the following formula (1): the weight (moisture weight; Ww) of the polypropylene resin foam molded article measured after being left at room temperature for 1 hour after molding, and the weight (dry weight; Wd) of the polypropylene resin foam molded article measured after being dried at 75°C for 24 hours and then left at room temperature for 4 hours: moisture content (%) = {(Ww - Wd) / Wd} × 100 (1) "After molding" refers to the time after the foam molded article is removed from the mold. "After being left for 1 hour" refers to the time from 1 hour to 1.5 hours. "After being left for 4 hours" refers to the time from 4 hours to 4.5 hours.

[0093] (Porosity of foam molded article) The porosity of the foam molded article is 25% or more, preferably 27% or more, more preferably 28% or more, and even more preferably 30% or more. This configuration has the advantage that a polypropylene-based resin foam molded article with excellent sound absorption performance can be obtained.

[0094] The porosity of the foam molded article is preferably 60% or less, more preferably 55% or less, even more preferably 50% or less, and particularly preferably 45% or less. This configuration has the advantage of being able to obtain a polypropylene-based resin foam molded article with excellent mechanical strength. The method for measuring the porosity of a polypropylene-based resin foam molded article will be described in detail in the Examples below. The porosity is the value measured after the foam molded article is left at room temperature for 1 hour after molding, then cured and dried in a constant temperature chamber at 75°C for 24 hours, and then left at room temperature for another 4 hours.

[0095] (Maximum sound absorption coefficient of foam molded article) The maximum sound absorption coefficient of the foam molded article is preferably 0.85 or more, more preferably 0.90 or more, even more preferably 0.96 or more, and particularly preferably 0.97 or more. According to this configuration, the foam molded article can be said to have excellent sound absorption performance. The upper limit of the maximum sound absorption coefficient of the foam molded article is not particularly limited, but is, for example, 1.00 or less. The method for measuring the maximum sound absorption coefficient of a polypropylene resin foam molded article will be explained in detail in the Examples below.

[0096] (Deformation amount of foam molded article) The deformation amount of the foam molded article is preferably 2.5 mm or less, more preferably 2.0 mm or less, more preferably 1.5 mm or less, even more preferably 1.0 mm or less, and particularly preferably 0.5 mm or less. According to this configuration, the deformation amount of the foam molded article can be said to be small. The lower limit of the deformation amount of the foam molded article is not particularly limited, but can be, for example, 0.0 mm, in other words, there can be no deformation. The method for measuring the deformation amount of a polypropylene resin foam molded article will be explained in detail in the Examples below.

[0097] 5. Method for producing polypropylene-based resin foam molded article A method for producing a polypropylene-based resin foam molded article according to one embodiment of the present invention is a method for producing a polypropylene-based resin foam molded article, comprising: a heating step of heating polypropylene-based resin foam beads to which no internal pressure has been applied in a mold; and a water-cooling step of water-cooling the pre-polypropylene-based resin foam molded article obtained in the heating step, or both the pre-polypropylene-based resin foam molded article and the mold, by spraying water for one second or more, and the polypropylene-based resin foam molded article has a porosity of 25% or more.

[0098] The present manufacturing method has the above-mentioned configuration, and therefore has the advantage of being able to produce a polypropylene resin foam molded article that has excellent sound absorbing properties and a small amount of deformation.

[0099] In this specification, the sound absorption performance of a polypropylene-based resin foam molded body is evaluated based on the maximum sound absorption coefficient of the polypropylene-based resin foam molded body. That is, in this specification, a polypropylene-based resin foam molded body having "excellent sound absorption performance" means that the polypropylene-based resin foam molded body has a high maximum sound absorption coefficient.

[0100] The manufacturing method described in Section [5. Manufacturing method for polypropylene-based resin foam molded article] is a method for manufacturing the foam molded article described in Section [4. Polypropylene-based resin foam molded article], and as described above, the foam molded article described in Section [4. Polypropylene-based resin foam molded article] is preferably a foam molded article obtained by the manufacturing method described in Section [5. Manufacturing method for polypropylene-based resin foam molded article].

[0101] The present production method preferably includes a step of in-mold foaming of the expanded polypropylene resin beads described in the section [3. Expanded Polypropylene Resin Beads].

[0102] In the present production method, the expanded polypropylene resin particles are preferably irregularly shaped expanded particles, which has the advantage of producing a polypropylene resin foam molded article that has excellent sound absorption properties and little deformation.

[0103] In this manufacturing method, a mold is used. In this manufacturing method, it is preferable to use, for example, a mold composed of a fixed mold that cannot be driven and a movable mold that can be driven. Here, the fixed mold and the movable mold can be configured so that a molding space can be formed inside the fixed mold and the movable mold by driving the movable mold toward the fixed mold (this operation may be referred to as "mold closing").

[0104] This manufacturing method may include a filling step, prior to the heating step, of filling the molding space of the mold with expanded polypropylene resin beads to which no internal pressure has been applied. Examples of the filling step include, but are not limited to, the following steps (b1) to (b4) in order: (b1) mounting a mold composed of a fixed mold that cannot be driven and a movable mold that can be driven on an in-mold foam molding machine; (b2) driving the movable mold toward the fixed mold so that a small gap (also called cracking) is formed so that the fixed mold and the movable mold are not completely closed; (b3) filling the molding space formed inside the fixed mold and the movable mold with expanded beads to which no internal pressure has been applied, for example, through a filling machine; (b4) driving the movable mold so that the fixed mold and the movable mold are completely closed (i.e., completely closed).

[0105] The expanded polypropylene resin beads to which no internal pressure is applied can also be said to be expanded polypropylene resin beads having an internal pressure of 0.1 MPa (absolute pressure). That is, in the filling step, the expanded beads having an internal pressure of 0.1 MPa (absolute pressure) are filled into the molding space.

[0106] (Heating step) A method for producing a polypropylene-based foam molded article according to one embodiment of the present invention includes a heating step of heating polypropylene-based resin foam beads in a mold to which no internal pressure has been applied. The heating step can also be said to be a step of heating the foam beads filled in the molding space of the mold to which no internal pressure has been applied in the filling step. In the heating step, by heating the foam beads in the mold (in the molding space of the mold), the foam beads in the mold can be fused together, resulting in a foam molded article.

[0107] In this specification, the foam molded article present in the mold obtained after the heating step, which has not been water-cooled or is in the process of being water-cooled, may be referred to as a "pre-polypropylene resin foam molded article" for convenience in order to distinguish it from the polypropylene resin foam molded article finally obtained.

[0108] In the heating step, the expanded polypropylene resin particles obtained in the releasing step are heated without applying internal pressure. In other words, in the heating step, the expanded polypropylene resin particles having an internal pressure of 0.1 MPa (absolute pressure) are heated. This configuration has the advantage of being able to produce a polypropylene resin foam molded article with excellent sound absorption performance.

[0109] In the heating step, the temperature of the steam is not particularly limited, but is preferably 143° C. to 170° C., more preferably 145° C. to 168° C., even more preferably 147° C. to 165° C., and particularly preferably 148° C. to 162° C. This configuration has the advantage of producing a polypropylene resin foam molded article with good fusion.

[0110] In the heating step, the pressure of the steam is not particularly limited, but is preferably 0.30 MPa (gauge pressure) to 0.70 MPa (gauge pressure), more preferably 0.32 MPa (gauge pressure) to 0.65 MPa (gauge pressure), even more preferably 0.34 MPa (gauge pressure) to 0.60 MPa (gauge pressure), and particularly preferably 0.35 MPa (gauge pressure) to 0.55 MPa (gauge pressure). This configuration has the advantage of producing a polypropylene resin foam molded article with good fusion.

[0111] (Water-cooling step) The present production method includes a water-cooling step in which the pre-polypropylene resin foam molded article obtained in the heating step, or both the pre-polypropylene resin foam molded article and the mold, are water-cooled by spraying water for at least one second. A polypropylene resin foam molded article can be obtained by the water-cooling step. Furthermore, by carrying out the water-cooling step having the above-described configuration, there is an advantage in that a polypropylene resin foam molded article with a small amount of deformation can be obtained.

[0112] The temperature of the water is preferably 10° C. to 70° C., more preferably 12° C. to 65° C., even more preferably 14° C. to 60° C., and particularly preferably 15° C. to 55° C. This configuration has the advantages of improving the productivity of polypropylene resin foam molded articles and reducing the cost of steam used in molding.

[0113] The water spray pressure is preferably 0.3 MPa (gauge pressure) to 0.7 MPa (gauge pressure), more preferably 0.4 MPa (gauge pressure) to 0.65 MPa (gauge pressure), even more preferably 0.4 MPa (gauge pressure) to 0.6 MPa (gauge pressure), and particularly preferably 0.4 MPa (gauge pressure) to 0.55 MPa (gauge pressure). This configuration has the advantage of allowing water (cooling water) to be effectively sprayed onto both the pre-polypropylene resin foam molded article and the mold, or onto the pre-polypropylene resin foam molded article.

[0114] The time for spraying water (sometimes referred to herein as the "water cooling time") is 1 second or more, preferably 1 to 90 seconds, more preferably 3 to 60 seconds, even more preferably 5 to 50 seconds, and particularly preferably 10 to 45 seconds. This configuration has the advantage that a polypropylene resin foam molded article with a small amount of deformation can be obtained.

[0115] When spraying water onto the pre-polypropylene resin foam molded article, a method of directly spraying water onto the foam molded article can be used.

[0116] When spraying water onto both the pre-polypropylene resin foam molded article and the mold, the method of spraying water is not particularly limited, but examples include a method of directly spraying water onto a mold having holes formed therein. If water is directly sprayed onto a mold having holes formed therein, the water will eventually be sprayed onto the pre-polypropylene resin foam molded article inside the mold through the holes. In this way, when the water sprayed onto the mold is also eventually sprayed onto the pre-polypropylene resin foam molded article inside the mold, this is considered to be "spraying water onto both the pre-polypropylene resin foam molded article and the mold."

[0117] As described above, in the water cooling step, spraying water directly onto the pre-polypropylene resin foam molded article, or onto both the pre-polypropylene resin foam molded article and the mold, has the advantage of allowing the pre-polypropylene resin foam molded article to be cooled efficiently.

[0118] (Mold Release and Drying Step) The present production method may include a mold release and drying step in which the in-mold foam molded article is removed from the mold and dried to obtain a foam molded article.

[0119] The method for releasing the in-mold foam molded article from the mold is not particularly limited, but examples thereof include a method using air and a method using a demolding tool.

[0120] The drying temperature is not particularly limited, but is preferably 70° C. to 85° C., more preferably 75° C. to 83° C., even more preferably 75° C. to 81° C., and particularly preferably 75° C. to 80° C. This configuration has the advantage that a polypropylene resin foam molded article with a low moisture content can be obtained with little energy consumption.

[0121] The drying time is not particularly limited, but is preferably 10 to 24 hours, more preferably 12 to 24 hours, even more preferably 14 to 24 hours, and particularly preferably 16 to 24 hours. This configuration has the advantage that a polypropylene resin foam molded article with a low moisture content can be obtained with little energy consumption.

[0122] Alternatively, the drying may be performed by cooling at room temperature for 1 hour, followed by drying at 75°C for 24 hours, and then cooling at room temperature for 4 hours. In this specification, room temperature refers to 20°C to 25°C.

[0123] An embodiment of the present invention may have the following configuration.

[0124] [1] A method for producing a polypropylene-based resin foam molded article, comprising: a heating step of heating polypropylene-based resin foam beads to which no internal pressure has been applied in a mold; and a water-cooling step of water-cooling the pre-polypropylene-based resin foam molded article obtained in the heating step, or both the pre-polypropylene-based resin foam molded article and the mold, by spraying water for one second or more, wherein the polypropylene-based resin foam molded article has a porosity of 25% or more.

[0125] [2] The method for producing a polypropylene-based resin foam molded article according to [1], wherein the expanded polypropylene-based resin beads have a degree of irregularity of 2.20 or more, as expressed by the following formula: degree of irregularity = true density of the expanded polypropylene-based resin beads / bulk density of the expanded polypropylene-based resin beads.

[0126] [3] The method for producing a polypropylene resin foam molded article according to [1] or [2], wherein the polypropylene resin foam particles are irregularly shaped foam particles.

[0127] [4] The method for producing a polypropylene-based resin foam molded article according to any one of [1] to [3], wherein the expanded polypropylene-based resin particles have a bulk density of 10.0 g / L to 300.0 g / L.

[0128] [5] The method for producing a polypropylene resin foam molded article according to any one of [1] to [4], wherein the water spray pressure is 0.3 MPa (gauge pressure) to 0.7 MPa (gauge pressure).

[0129] [6] The method for producing a polypropylene resin foam molded article according to any one of [1] to [5], wherein the temperature of the water is 10°C to 70°C.

[0130] [7] The method for producing a polypropylene-based resin foam molded article according to [2], wherein the polypropylene-based resin foam beads have a degree of irregularity of 3.00 or less: degree of irregularity = true density of the polypropylene-based resin foam beads / bulk density of the polypropylene-based resin foam beads.

[0131] [8] The method for producing a polypropylene-based resin foam molded article according to any one of [1] to [7], wherein the expanded polypropylene-based resin particles are obtained by expanding polypropylene-based resin particles containing a polypropylene-based resin.

[0132] [9] The method for producing a polypropylene-based resin foam molded article according to any one of [1] to [8], wherein the polypropylene-based resin has a melt index at 230°C of 3.0 g / 10 min to 30.0 g / 10 min.

[0133]

[10] The method for producing a polypropylene-based resin foam molded article according to any one of [1] to [9], wherein the melting point of the polypropylene-based resin is 135°C to 160°C.

[0134]

[11] The method for producing a polypropylene-based resin foam molded article according to any one of [1] to

[10] , wherein the polypropylene-based resin comprises at least one selected from the group consisting of a propylene homopolymer, a block copolymer of propylene and a monomer other than propylene, and a random copolymer of propylene and a monomer other than propylene.

[0135]

[12] The method for producing a polypropylene resin foam molded article according to any one of [1] to

[11] , wherein the resin component in the polypropylene resin particles contains, based on 100% by weight of the resin component, 50% by weight or more in total of one or more selected from the group consisting of an ethylene / propylene random copolymer and a 1-butene / ethylene / propylene random copolymer.

[0136]

[13] The method for producing a polypropylene resin foam molded article according to any one of [1] to

[12] , wherein the weight of each of the polypropylene resin particles is 0.50 mg / particle to 6.0 mg / particle.

[0137]

[14] The method for producing a polypropylene resin foam molded article according to any one of [1] to

[13] , wherein the shape of the polypropylene resin particles is one selected from the group consisting of star-shaped, anchor cross-shaped, macaroni-shaped, cross-shaped, L-shaped, Y-shaped, T-shaped, U-shaped, and polygonal shapes.

[0138]

[15] The method for producing a polypropylene-based resin foam molded article according to any one of [1] to

[14] , wherein the polypropylene-based resin foam molded article has a moisture content of 140% to 300%. Here, the moisture content is calculated from the weight (Ww) of the polypropylene-based resin foam molded article measured after leaving it at room temperature for 1 hour after molding, and the weight (Wd) of the polypropylene-based resin foam molded article measured after further drying at 75°C for 12 hours and leaving it at room temperature for 4 hours, using the following formula (1): moisture content (%)={(Ww-Wd) / Wd}×100... (1).

[0139]

[16] The method for producing a polypropylene-based resin foam molded article according to any one of [1] to

[15] , wherein the polypropylene-based resin foam molded article has a porosity of 60% or less.

[0140]

[17] The method for producing a polypropylene-based resin foam molded body according to any one of [1] to

[16] , wherein the polypropylene-based resin foam molded body has a maximum sound absorption coefficient of 0.85 or more and 1.00 or less.

[0141]

[18] The method for producing a polypropylene resin foam molded article according to any one of [1] to

[17] , wherein the deformation amount of the polypropylene resin foam molded article is 0.0 mm or more and 2.5 mm or less.

[0142]

[19] The method for producing a polypropylene resin foam molded article according to any one of [1] to

[18] , wherein the water is sprayed for 90 seconds or less.

[0143]

[20] The method for producing a polypropylene-based resin foam molded article according to any one of [1] to [7], wherein the expanded polypropylene-based resin particles contain a polypropylene-based resin having a melt index at 230°C of 3.0 g / 10 min to 30.0 g / 10 min.

[0144] The present invention will be specifically explained below with reference to examples, but the technical scope of the present invention is not limited to these examples.

[0145] [Materials] The materials used in the examples and comparative examples are shown below.

[0146] (Polypropylene Resins) Polypropylene Resin A: 1-butene / ethylene / propylene random copolymer (propylene units 96 mol%, melting point 149°C, 1-butene content 3.8 wt%, ethylene content 0.5 wt%, MI = 10.1 g / 10 min) Polypropylene Resin B: ethylene / propylene random copolymer (propylene units 96 mol%, melting point 144°C, ethylene content 2.8 wt%, MI = 8.4 g / 10 min) Polypropylene Resin C: ethylene / propylene random copolymer (propylene units 96 mol%, melting point 142°C, ethylene content 3.0 wt%, MI = 6.9 g / 10 min) (Additives) Glycerin: purified glycerin D (manufactured by Lion Corporation) Melamine: melamine (manufactured by Nissan Chemical Industries, Ltd.) Talc: talcan powder (registered trademark) PK-S (manufactured by Hayashi Kasei Co., Ltd.).

[0147] [Measurement Methods] The measurement methods used in the examples and comparative examples are described below.

[0148] (Melting Point of Polypropylene Resin) The melting point of the polypropylene resin was determined by measurement using a differential scanning calorimeter (DSC6200, manufactured by Seiko Instruments Inc.) according to a DSC method. The specific operating procedures were as follows (1) to (4): (1) The temperature of 5 mg to 6 mg of polypropylene-based resin was raised from 40.0°C to 220.0°C at a heating rate of 10.0°C / min to melt the polypropylene-based resin; (2) The temperature of the molten polypropylene-based resin was then lowered from 220.0°C to 40.0°C at a heating rate of 10.0°C / min to crystallize the polypropylene-based resin; (3) The temperature of the crystallized polypropylene-based resin was then further raised from 40.0°C to 220.0°C at a heating rate of 10.0°C / min; (4) The temperature of the peak (melting peak) of the DSC curve of the polypropylene-based resin obtained during the second heating (i.e., during (3)) was determined as the melting point of the polypropylene-based resin. In addition, when there are multiple peaks (melting peaks) in the DSC curve of the polypropylene-based resin obtained during the second heating by the above-mentioned method, the temperature of the peak (melting peak) with the maximum heat of fusion was taken as the melting point of the polypropylene-based resin.

[0149] (MI of Polypropylene Resin) The MI of the polypropylene resin was measured using an MI measuring device described in JIS K7210:1999 under the following conditions: orifice diameter: 2.0959±0.005 mmφ, orifice length: 8.000±0.025 mm, load: 2.16 kgf, and temperature: 230°C (230±0.2°C).

[0150] (Degree of irregularity of expanded beads) The degree of irregularity of expanded beads was calculated by dividing the "true density" measured by the method described below by the "bulk density" measured by the method described below. Specifically, it was measured using the following formula: Degree of irregularity = true density of expanded polypropylene resin beads / bulk density of expanded polypropylene resin beads.

[0151] (Bulk Density of Expanded Beads) The bulk density of expanded beads was measured by the following methods (1) to (3): (1) The expanded beads were divided into a volume V1 (cm 3(2) The powder surface (top end) of the container was scraped off, and the weight W1 (g) of the expanded beads in the container was measured. (3) The bulk density of the expanded beads was calculated using the following formula: Bulk density of expanded beads (g / L) = Weight W1 (g) of expanded beads / {Volume of container V1 (cm 3 ) / 1000}.

[0152] (True Density of Expanded Beads) The weight W2 (g) of the expanded polypropylene resin beads was accurately measured to the nearest 0.001 g (rounded off to the fourth decimal point). The weighed expanded polypropylene resin beads were immersed in a measuring cylinder containing 100 mL of water at 23°C, and the volume V2 (cm) of the expanded polypropylene resin beads was determined from the rising scale. 3 The true density of the expanded beads was calculated using the following formula: True density of expanded beads (g / L) = Weight of expanded beads W2 (g) / {Volume of expanded beads V2 (cm 3 ) / 1000}.

[0153] (Maximum Sound Absorption Coefficient of Foam Molded Article) A sample measuring 29 mm in diameter and 60.0 mm in thickness was cut out from a polypropylene resin foam molded article (370 mm long x 320 mm wide x 60 mm thick). Both skin surfaces of this sample were cut to a thickness of 40.0 mm to prepare a sample for measuring normal incident sound absorption coefficient. Using this sample, the normal incident sound absorption coefficient was measured at frequencies from 500 Hz to 6400 Hz in accordance with JIS A1405. The normal incident sound absorption coefficient was measured in a state where the sample was in close contact with a rigid wall that reflected sound waves, i.e., in a state where there was no air behind it. The normal incident sound absorption coefficient was measured using an SR-4100 normal incident sound absorption coefficient measuring device manufactured by Ono Sokki Co., Ltd. From the obtained frequency-normal incident sound absorption coefficient curve, the normal incident sound absorption coefficient (maximum sound absorption coefficient) at the frequency at which the normal incident sound absorption coefficient was maximized was read.

[0154] In this specification, the phrase "excellent sound absorption performance" of a foam molded article means that the foam molded article has a maximum sound absorption coefficient of 0.85 or more.

[0155] (Deformation Amount of Foam Molded Article) Hereinafter, a method for evaluating the deformation amount of the present foam molded article will be described with reference to FIG. 1 . FIG. 1 is a schematic diagram of a polypropylene resin foam molded article 100 used to evaluate the deformation amount. The foam molded article 100 was produced by in-mold foam molding of foamed beads using a mold for a shock-absorbing box for storing goods as the mold for deformation amount evaluation. The mold used was a box-shaped shock-absorbing box with dimensions of 400 mm in the longitudinal direction (Y direction) × 300 mm in the lateral direction (Z direction) × 145 mm in the thickness direction (X direction), with a side thickness of 21 mm.

[0156] In this specification, the phrase "small deformation amount" of the foam molded article means that the deformation amount of the foam molded article is 2.5 mm or less.

[0157] In FIG. 1 , the X direction can be considered the thickness direction of the foam molded body 100. The Y direction can be considered the longitudinal direction of the foam molded body 100, and is a direction perpendicular to the X direction. The Z direction can be considered the lateral direction of the foam molded body 100, and is a direction perpendicular to both the X direction and the Y direction. As shown in FIG. 1 , the dimensions (lengths) of the lateral direction (Z direction) of the two end portions in the longitudinal direction (Y direction) of the foam molded body 100 were defined as L1 (mm) and L2 (mm), respectively, and the lateral direction (Z direction) dimension of the central portion in the longitudinal direction (Y direction) was defined as L3 (mm). The thickness dimension of the side (lateral direction (Z direction) and longitudinal direction (Y direction)) was defined as L4 (mm).

[0158] The deformation amount of the foam molded article was measured by the following methods (1) to (3): (1) using a mold having dimensions (lengths) of 400 mm in the longitudinal direction (Y direction), 300 mm in the lateral direction (Z direction), and 145 mm in the thickness direction (X direction), with a side thickness of 21 mm, the foam beads were foam-molded in-mold; (2) the Z-direction dimensions (mm) (L1, L2) of the two longitudinal end portions of the obtained foam molded article (foam molded article 100) and the Z-direction dimension (mm) (L3) of the longitudinal center portion were measured; (3) the deformation amount was calculated according to the following formula: deformation amount (mm) = {(L1 + L2) / 2} - L3.

[0159] (Moisture Content of Foam Molded Article) The moisture content was measured using a polypropylene resin foam molded article having the dimensions obtained by molding using the mold shown in the section (Deformation of Foam Molded Article). After molding, the foam molded article was left at room temperature for 1 hour, and then the moisture weight Ww (g) of the foam molded article was measured. The foam molded article was then cured and dried for 24 hours in a constant temperature chamber at 75°C, and then left at room temperature for another 4 hours. The dry weight Wd (g) of the foam molded article was then measured, and the moisture content (%) of the foam molded article was calculated using the following formula (1): Moisture Content (%) = {(Ww - Wd) / Wd} × 100 (1).

[0160] (Filling Ability of Foam Molded Articles) Five polypropylene resin foam molded articles having the dimensions obtained by molding using the mold shown in the section (Deformation Amount of Foam Molded Articles) were produced. The outer periphery of the opening (not the outer periphery of the tip of the side wall or the outer periphery of the bottom) of each of the five box-shaped foam molded articles obtained was observed to check for the presence or absence of defects of foam beads extending over 10 mm or more, and the number of foam molded articles with such defects was counted. The filling ability was evaluated according to the following criteria: 1 (Acceptable): 0 foam molded articles with defects of 10 mm or more 0 (Unacceptable): 1 or more foam molded articles with defects of 10 mm or more

[0161] (Porosity of foam molded article) A test piece of Φ29 × 40 mm was cut out from a polypropylene resin foam molded article (length 370 mm × width 320 mm × thickness 50 mm) prepared for porosity measurement, for measuring normal incident sound absorption coefficient. For the test piece, Vc was measured according to the method described in Procedure C of ASTM D2856-87, and the porosity (%) was calculated according to the following formula: Porosity (%) = {(Va - Vc) × 100} / Va.

[0162] Here, the volume Vc (cm 3 ) is the volume of the test piece (Φ29 × 40 mm) obtained by measurement using an air comparison type hydrometer Model 1000 manufactured by Tokyo Science Co., Ltd. Also, the volume Va (cm 3 ) is the apparent volume calculated by measuring the diameter D (cm) and height H (cm) of the test piece (Φ29 × 40 mm) with a vernier caliper after measuring Vc with the air comparison type hydrometer, using the following formula: Volume Va (cm 3 ) = πD2 H / 4.

[0163] Example 1 (Preparation of Polypropylene-Based Resin Particles) 100 parts by weight of polypropylene-based resin, 0.15 parts by weight of glycerin, and 0.05 parts by weight of talc were weighed out and dry-blended using a small tumbler manufactured by O-N Machine Co., Ltd. to obtain a mixture. The mixture was melt-kneaded at a resin temperature of 200°C using a twin-screw extruder (TEM26-SX manufactured by Toshiba Machine Co., Ltd.) and extruded into strands (products) from a five-line die attached to the tip of the extruder. The extruded product (strands) were water-cooled in a 2-m-long water tank. The water-cooled product was then taken up and chopped into pieces (chopping process) using a chopping device (manufactured by Ishinaka Iron Works). This procedure yielded polypropylene-based resin particles (weight per particle: 2.5 mg) having the shape (star-shaped) shown in Table 1.

[0164] (Preparation of Expanded Polypropylene Resin Beads) A 10 L pressure vessel was charged with 100 parts by weight of the resulting polypropylene resin particles, 442 parts by weight of water as an aqueous dispersion medium, 0.33 parts by weight of kaolin as a dispersant, 0.05 parts by weight of sodium dodecylbenzenesulfonate as a dispersing aid, 0.03 parts by weight of citric acid as a pH adjuster, and 3.5 to 4.5 parts by weight of carbon dioxide as a blowing agent, according to the foaming pressure, to prepare a dispersion containing a foaming agent. The resulting dispersion was heated to a foaming temperature (temperature inside the pressure vessel) of 151.0°C while stirring. After the temperature and pressure inside the pressure vessel reached the predetermined foaming temperature and foaming pressure (heating-pressure increasing step), the temperature and pressure inside the pressure vessel were maintained at the predetermined foaming temperature and foaming pressure for an additional 30 minutes (maintenance step). Carbon dioxide was then introduced, and the pressure inside the pressure vessel was maintained at the foaming pressure of 2.5 MPa (gauge pressure). The valve at the bottom of the pressure vessel was opened, and the dispersion liquid in the pressure vessel was released through a 4.0 mm diameter orifice to atmospheric pressure, yielding expanded polypropylene resin beads (release step). The expanded polypropylene resin beads were dried at 75°C for 24 hours. The resulting first-stage expanded beads exhibited two peaks derived from the polypropylene resin in the DSC curve measured by the DSC method. The bulk density of the expanded polypropylene resin beads was evaluated. The results are shown in Table 1.

[0165] (Preparation of Polypropylene-Based Resin Foam Molded Article) The obtained polypropylene-based resin foam particles were filled into a mold for a box-shaped molded article using a polyolefin in-mold foam molding machine (manufactured by Dabo Corporation) (filling step). The polypropylene-based resin foam particles were heat-fused with steam at 0.28 MPa (gauge pressure) (heating step). Then, water (cooling water) at 30°C was sprayed into the mold at a spray pressure of 0.4 MPa (gauge pressure) for 5 seconds to cool the pre-polypropylene-based resin foam molded article (water-cooling step). Specifically, water was sprayed directly onto the mold from a copper pipe through a cooling water nozzle. Since the mold had holes through which steam could pass, spraying water directly onto the mold allowed the water to be sprayed not only onto the mold but also onto the pre-polypropylene-based resin foam molded article. That is, in the water-cooling step, water was sprayed onto both the pre-polypropylene-based resin foam molded article and the mold for 5 seconds. Thereafter, the mold was opened, and the polypropylene-based resin in-mold foam molded article was removed from the mold using air or a demolding tool (demolding step). The obtained in-mold foamed article was left at room temperature for 1 hour, then cured and dried in a thermostatic chamber at 75°C for 24 hours (drying step), and then left at room temperature for another 4 hours, after which the maximum sound absorption coefficient, deformation amount, moisture content, packing property, and porosity were measured. The results are shown in Table 1.

[0166] [Examples 2 to 8, Comparative Examples 1 to 3] Expanded beads and foamed molded articles were obtained in the same manner as in Example 1, except that the type and amount of each material and each production condition were changed as shown in Table 1. The physical properties of the obtained expanded beads and foamed molded articles were measured and evaluated. The results are shown in Table 1.

[0167] The "air pressure (absolute pressure)" shown in Table 1 refers to the internal pressure of the expanded beads during molding.

[0168] According to the method for producing a polypropylene-based resin foam molded article according to one embodiment of the present invention, a polypropylene-based resin foam molded article having excellent sound-absorbing properties and a small amount of deformation can be provided. The polypropylene-based resin foam molded article can be suitably used for various applications such as cushioning packaging materials, logistics materials, heat insulation materials, civil engineering and construction materials, and automotive components.

[0169] 100 Polypropylene resin foam molded body X Thickness direction Y Longitudinal direction Z Shortitudinal direction

Claims

1. A method for producing a polypropylene resin foam molded product, comprising: a heating step of heating polypropylene resin foam particles to which no internal pressure has been applied in a mold; and a water-cooling step of water-cooling the pre-polypropylene resin foam molded product obtained in the heating step, or both the pre-polypropylene resin foam molded product and the mold, by spraying water for one second or more onto the pre-polypropylene resin foam molded product, wherein the polypropylene resin foam molded product has a porosity of 25% or more.

2. The method for producing a polypropylene-based resin foamed molded article according to claim 1, wherein the polypropylene-based resin foamed beads have a degree of irregularity of 2.20 or more, as represented by the following formula: degree of irregularity = true density of the polypropylene-based resin foamed beads / bulk density of the polypropylene-based resin foamed beads.

3. The method for producing a polypropylene resin foamed molded article according to claim 1, wherein the polypropylene resin foamed particles are irregularly shaped foamed particles.

4. The method for producing a polypropylene resin foamed molded article according to claim 1, wherein the polypropylene resin foamed particles have a bulk density of 10.0 g / L to 300.0 g / L.

5. The method for producing a polypropylene resin foam molded article according to claim 1, wherein the water spray pressure is 0.3 MPa (gauge pressure) to 0.7 MPa (gauge pressure).

6. The method for producing a polypropylene resin foam molded article according to claim 1, wherein the temperature of the water is 10°C to 70°C.

7. The method for producing a polypropylene resin foamed molded article according to claim 1, wherein the polypropylene resin foam particles are produced by foaming polypropylene resin particles containing a polypropylene resin.

8. The method for producing a polypropylene resin foam molded article according to claim 7, wherein the polypropylene resin has a melt index at 230° C. of 3.0 g / 10 min to 30.0 g / 10 min.

9. The method for producing a polypropylene resin foam molded article according to claim 7, wherein the melting point of the polypropylene resin is 135°C to 160°C.

10. A method for producing a polypropylene resin foam molded product as described in claim 7, wherein the resin component in the polypropylene resin particles contains a total of 50% by weight or more of one or more types selected from the group consisting of ethylene / propylene random copolymers and 1-butene / ethylene / propylene random copolymers, based on 100% by weight of the resin component.

11. The method for producing a polypropylene resin foam molded article according to claim 7, wherein the weight of each of the polypropylene resin particles is 0.50 mg / particle to 6.0 mg / particle.

12. The method for producing a polypropylene resin foam molded product according to claim 1, wherein the polypropylene resin foam molded product has a moisture content of 140% to 300%. Here, the moisture content is calculated from the weight (Ww) of the polypropylene resin foam molded product measured after leaving it at room temperature for 1 hour following molding, and the weight (Wd) of the polypropylene resin foam molded product measured after further drying at 75°C for 12 hours and leaving it at room temperature for 4 hours, using the weight (Wd) of the polypropylene resin foam molded product measured according to the following formula (1): moisture content (%) = {(Ww - Wd) / Wd} x 100 ... (1).

13. The method for producing a polypropylene resin foam molded article according to claim 1, wherein the polypropylene resin foam molded article has a maximum sound absorption coefficient of 0.85 or more and 1.00 or less.

14. A method for producing a polypropylene resin foam molded article according to any one of claims 7 to 13, wherein the deformation amount of the polypropylene resin foam molded article is 0.0 mm or more and 2.5 mm or less.

15. A method for producing a polypropylene-based resin foamed molded article according to any one of claims 1 to 6, wherein the polypropylene-based resin foamed particles contain a polypropylene-based resin having a melt index at 230°C of 3.0 g / 10 min to 30.0 g / 10 min.

Citation Information

Patent Citations

  • Method for manufacturing thermoplastic resin in-mold foamed molded object

    JP2001198940A

  • Interior material for automobile

    JP2007045979A

  • Polypropylene resin foam particle

    JP1997249763A

  • Thermoplastic resin foamed and molded product

    JP2006240286A

  • Polyolefin resin foam particle and foam molded body in polyolefin resin mold

    JP2015108030A

Cited By

  • Polyolefin resin foam particles and method for producing the same

    JP2026147675A

  • Polyolefin resin foam molded product

    JP2026161223A