Lithium primary battery

The lithium primary battery design with a specific magnesium content in the lithium alloy and optimized electrode configuration addresses uneven lithium consumption, ensuring uniformity and maintaining battery performance by ensuring the lithium primary battery maintains conductivity and energy density.

WO2024204693A1PCT designated stage expired Publication Date: 2024-10-03PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/013008
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-29
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Lithium primary batteries experience performance deterioration due to uneven lithium consumption at the negative electrode, leading to isolation and breakage, which disrupts electrical connectivity and reduces battery performance.

Method used

A lithium primary battery design featuring a wound electrode group with a band-shaped positive electrode and negative electrode, where the negative electrode contains a lithium alloy with 0.02% to 11% magnesium by mass, and the electrodes are configured such that the ratio of opposing surface areas to the total negative electrode surface area is 90% or more, ensuring uniform lithium consumption and maintaining electrode integrity.

Benefits of technology

This configuration ensures uniform lithium consumption, prevents isolation of the negative electrode, maintains conductivity, and enhances pulse discharge characteristics and energy density, while avoiding negative electrode breakage and performance degradation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024013008_03102024_PF_FP_ABST
    Figure JP2024013008_03102024_PF_FP_ABST
Patent Text Reader

Abstract

This lithium primary battery is provided with an electrode group and a nonaqueous electrolyte solution. The electrode group is configured by spirally winding a belt-like positive electrode and a belt-like negative electrode, with a separator being interposed therebetween. The positive electrode contains at least one material that is selected from the group consisting of manganese dioxide and graphite fluoride, and the negative electrode contains a lithium alloy. The lithium alloy contains 0.02% by mass to 11% by mass (inclusive) of Mg. The negative electrode has a first negative electrode main surface that is on the outer peripheral side of the electrode group and a second negative electrode main surface that is on the inner peripheral side of the electrode group. The positive electrode has a first positive electrode main surface that is on the inner peripheral side of the electrode group and a second positive electrode main surface that is on the outer peripheral side of the electrode group. The first negative electrode main surface has a first facing region that faces the first positive electrode main surface, and the second negative electrode main surface has a second facing region that faces the second positive electrode main surface. The ratio of the total area S1 of the first facing region and the second facing region to the total area S0 of the first negative electrode main surface and the second negative electrode main surface is 90% or more.
Need to check novelty before this filing date? Find Prior Art

Description

Lithium primary battery

[0001] The present disclosure relates to lithium primary batteries.

[0002] Lithium primary batteries have a high energy density and low self-discharge, and are therefore used as power sources for many electronic devices. The wound electrode group of a lithium primary battery is composed of a strip-shaped positive electrode, a strip-shaped negative electrode, and a separator disposed between the positive and negative electrodes, wound together in a spiral shape. Manganese dioxide or the like is used for the positive electrode. For the negative electrode, for example, a sheet-shaped (foil-shaped) lithium metal or lithium alloy is used.

[0003] Patent Document 1 proposes a "non-aqueous electrolyte battery comprising a spiral electrode body in which a strip-shaped negative electrode and a strip-shaped positive electrode, each having a light metal as an active material, are wound with a separator interposed therebetween, the width of the negative electrode being configured to be equal to or less than the width of the positive electrode, and a negative electrode current collector tab being crimped to the negative electrode so as not to cover the front surface of the negative electrode in the longitudinal direction, wherein the negative electrode current collector tab is disposed within a semicircle at 180° in the winding direction from the end of the positive electrode in the electrode body."

[0004] Patent Document 2 proposes "a cylindrical nonaqueous electrolyte primary battery having an electrode group with a wound structure in which a positive electrode containing manganese dioxide or graphite fluoride and a negative electrode are spirally wound with a separator interposed therebetween, the negative electrode having a metallic lithium-containing layer and a current collector, and a lithium-aluminum alloy is formed on the surface of the metallic lithium-containing layer opposite the current collector in a portion occupying 20 to 75% of the width thereof."

[0005] Patent Document 3 proposes an electrochemical cell having "a spiral electrode stack including an anode, a cathode, and a separator, the separator being disposed between the anode and the cathode and spirally wound together with the anode and the cathode, an outer segment of the anode along the outer periphery of the electrode stack, the remainder of the periphery constituting the outer segment of the cathode, the length of the outer segment of the anode being 10% or less of the total length of the anode, an anode tab attached to the inner surface of the outer segment of the anode, an electrolyte, a member in mechanical and electrical contact with the outer segment of the cathode, the conductive member extending on the outer segment of the anode beyond the outer edge of the segment, and insulating means disposed along the inner surface of the outer segment of the anode and serving as a barrier against ion migration, wherein during voltage reversal, the anode metal is preferentially plated from the outer segment of the anode onto the opposing conductive member."

[0006] Patent Document 4 proposes "a lithium primary battery comprising a positive electrode using iron disulfide as a positive electrode active material, a negative electrode using a lithium alloy as a negative electrode active material, an electrode group in which the positive electrode and the negative electrode are wound with a separator interposed therebetween, and a non-aqueous electrolyte solution, wherein the lithium alloy contains 0.02 to 0.2 mol % of at least one of magnesium and tin."

[0007] Japanese Utility Model Application Publication No. 2-70365 Japanese Patent Application Publication No. 2009-266715 Japanese Patent Application Publication No. 2-257573 International Publication No. 2012 / 066709 Pamphlet

[0008] During discharge, lithium is consumed unevenly in the negative electrode, resulting in locally increased lithium consumption. At the end of discharge, part of the negative electrode is damaged or broken, isolating the lithium. The isolated lithium no longer contributes to discharge because it is no longer electrically connected to the negative electrode current collector, which can result in a decrease in battery performance.

[0009] One aspect of the present disclosure provides a wound electrode group and a nonaqueous electrolyte, wherein the electrode group is configured by spirally winding a strip-shaped positive electrode, a strip-shaped negative electrode, and a separator disposed between the positive electrode and the negative electrode, wherein the positive electrode includes at least one selected from the group consisting of manganese dioxide and graphite fluoride, wherein the negative electrode includes a lithium alloy, and the lithium alloy includes 0.02 mass % or more and 11 mass % or less of magnesium, wherein the negative electrode has a first negative electrode main surface on an outer periphery of the electrode group and a second negative electrode main surface on an inner periphery of the electrode group, wherein the positive electrode has a first positive electrode main surface on the inner periphery of the electrode group and a second positive electrode main surface on the outer periphery of the electrode group, wherein the first negative electrode main surface has a first opposing region facing the first positive electrode main surface, and the second negative electrode main surface has a second opposing region facing the second positive electrode main surface, The lithium primary battery relates to a lithium primary battery in which a ratio of a total area S1 of the first opposing region and the second opposing region to a total area S0 of the first negative electrode principal surface and the second negative electrode principal surface is 90% or more.

[0010] According to the present disclosure, it is possible to suppress the deterioration of performance of a lithium primary battery.

[0011] The novel features of the present invention are set forth in the appended claims, but the present invention, both in terms of structure and content, together with other objects and features of the present invention, will be better understood from the following detailed description taken in conjunction with the drawings.

[0012] Fig. 1 is a schematic cross-sectional view showing an example of a wound electrode group of a lithium primary battery according to an embodiment of the present disclosure; Fig. 2 is a schematic top view showing an example of the vicinity of a connection part of a negative electrode with a negative electrode lead member; Fig. 3 is a schematic cross-sectional view showing an example of the vicinity of a connection part of a negative electrode with a negative electrode lead member; Fig. 4 is a schematic cross-sectional view showing another example of the vicinity of a connection part of a negative electrode with a negative electrode lead member; Fig. 5 is a schematic cross-sectional view showing yet another example of the vicinity of a connection part of a negative electrode with a negative electrode lead member; Fig. 6 is a front view of a part of a lithium primary battery according to an embodiment of the present disclosure, in cross section.

[0013] The following describes embodiments of the present disclosure using examples, but the present disclosure is not limited to the examples described below. In the following description, specific numerical values ​​and materials may be exemplified, but other numerical values ​​and materials may be applied as long as the effects of the present disclosure are obtained. In this specification, the term "numerical value A to numerical value B" includes numerical value A and numerical value B and can be read as "numerical value A or more and numerical value B or less." In the following description, when lower and upper limits are exemplified for numerical values ​​of specific physical properties or conditions, any of the exemplified lower limits and any of the exemplified upper limits can be arbitrarily combined, as long as the lower limit is not equal to or greater than the upper limit. When multiple materials are exemplified, one of the materials may be selected and used alone, or two or more materials may be used in combination.

[0014] A lithium primary battery according to an embodiment of the present disclosure includes a wound electrode assembly and a nonaqueous electrolyte. The electrode assembly is configured by spirally winding a strip-shaped positive electrode, a strip-shaped negative electrode, and a separator disposed between the positive electrode and the negative electrode. The positive electrode includes at least one material selected from the group consisting of manganese dioxide and graphite fluoride as a positive electrode active material. The negative electrode includes a lithium alloy as a negative electrode active material. The lithium alloy includes 0.02% by mass or more and 11% by mass or less of magnesium (Mg).

[0015] The negative electrode has a first negative electrode main surface on the outer periphery of the electrode group and a second negative electrode main surface on the inner periphery of the electrode group. The positive electrode has a first positive electrode main surface on the inner periphery of the electrode group and a second positive electrode main surface on the outer periphery of the electrode group. The first negative electrode main surface has a first opposing region facing the first positive electrode main surface. The second negative electrode main surface has a second opposing region facing the second positive electrode main surface. The ratio of the total area S1 of the first opposing region and the second opposing region to the total area S0 of the first negative electrode main surface and the second negative electrode main surface (hereinafter also referred to as the "S1 / S0 ratio") is 90% or more. The S1 / S0 ratio means (S1 / S0) x 100.

[0016] In some cases, a negative electrode lead member is connected to a predetermined location on the negative electrode main surface (first main surface or second main surface) and insulating tape is attached to cover the negative electrode lead member. In this case, the area of ​​the portion of the negative electrode main surface that is covered with insulating tape directly or via the negative electrode lead member is not included in the area of ​​the negative electrode main surface (the total area S0 of the negative electrode main surfaces).

[0017] In the opposing region between the positive electrode principal surface and the negative electrode principal surface, a negative electrode lead member may be connected to a predetermined location on the negative electrode principal surface (first principal surface or second principal surface), and insulating tape covering the negative electrode lead member may be affixed. In this case, the area of ​​the portion of the negative electrode principal surface that is covered with insulating tape directly or via the negative electrode lead member is not included in the area of ​​the opposing region between the positive electrode principal surface and the negative electrode principal surface (the total area S1 of the opposing regions).

[0018] In addition, in the opposing region between the positive electrode principal surface and the negative electrode principal surface, a positive electrode lead member may be connected to a predetermined location on the positive electrode principal surface, and insulating tape covering the positive electrode lead member may be attached. In this case, the area of ​​the portion of the positive electrode principal surface that is covered with insulating tape directly or via the positive electrode lead member is included in the area of ​​the opposing region between the positive electrode principal surface and the negative electrode principal surface (the total area S1 of the opposing regions).

[0019] By having the Mg content in the lithium alloy be 0.02% by mass or more, the strength of the negative electrode is improved. By having an S1 / S0 ratio of 90% or more, lithium is consumed uniformly in the negative electrode during discharge. These factors combine to suppress lithium isolation due to partial loss or fracture of the negative electrode at the end of discharge, and significantly suppress deterioration of battery performance (e.g., pulse discharge characteristics) due to lithium isolation. In the lithium primary battery according to the present disclosure, negative electrode isolation at the end of discharge is suppressed, the shape of the negative electrode is maintained, conductivity is ensured throughout the negative electrode, lithium in the negative electrode is effectively utilized, and high output characteristics are obtained even at the end of discharge. However, if the Mg content in the lithium alloy exceeds 11% by mass, the proportion of Li in the negative electrode decreases, and the absolute amount of Li decreases, which may result in deterioration of battery performance.

[0020] The S1 / S0 ratio is preferably 95% or more, and more preferably 98% or more.

[0021] If the Mg content in the lithium alloy is less than 0.02% by mass, even if the S1 / S0 ratio is 90% or more, the strength of the negative electrode decreases, which can cause the negative electrode to break at the end of discharge. If the S1 / S0 ratio is less than 90%, the region where the first negative electrode main surface does not face the first positive electrode main surface at the end of the winding of the negative electrode becomes large, and lithium is consumed less in this region, while lithium is consumed more in the other regions. In this case, even if the Mg content in the lithium alloy is 0.02% by mass or more, the negative electrode can break at the end of discharge due to uneven lithium consumption.

[0022] Since it is easy to adjust the S1 / S0 ratio to 90% or more, it is preferable that the positive and negative electrodes are wound so that the positive electrode is disposed at the outermost periphery of the electrode group. That is, it is preferable that the positive electrode has an outermost peripheral portion disposed at the outermost periphery of the electrode group. Also, typically, the positive and negative electrodes are wound so that the positive electrode is disposed at the innermost periphery of the electrode group. If the negative electrode is disposed at the innermost periphery of the electrode group, there is a possibility that burrs on the positive electrode current collector at the end of the positive electrode winding start side will break through the separator and come into contact with the negative electrode.

[0023] A negative electrode lead member may be connected to the negative electrode. The negative electrode lead member may be attached to the first negative electrode main surface or the second negative electrode main surface. The shape of the negative electrode lead member is, for example, a thin flake. The negative electrode lead member may be made of a material that can be electrically connected to a lithium alloy and is durable against a non-aqueous electrolyte. Examples of materials for the negative electrode lead member include Ni, Fe, Cu, Sn, Au, Pt, stainless steel, conductive resin, etc. The negative electrode lead member may contain one or more of these materials. The negative electrode lead member is connected, for example, by crimping to a lithium alloy foil or a negative electrode current collector. For example, one end of the negative electrode lead member is connected to the negative electrode, and the other end of the negative electrode lead member is connected to a negative electrode terminal disposed on the battery lid (sealing body). When the battery case also serves as the negative electrode terminal, the other end of the negative electrode lead member may be connected to the inner bottom surface of the battery case.

[0024] From the viewpoint of preventing and protecting against internal short circuits, it is preferable that insulating tape be attached to the negative electrode so as to cover the connection portion of the negative electrode lead member with the negative electrode and the vicinity of this connection portion.

[0025] FIG. 1 is a schematic cross-sectional view showing an example of a wound electrode group of a lithium primary battery according to an embodiment of the present disclosure. FIG. 1 shows a cross section perpendicular to the winding axis of the electrode group. A separator is interposed between the positive electrode and the negative electrode, but the separator is not shown in FIG. 1 for convenience. Note that FIG. 1 is a schematic view and does not necessarily reflect actual dimensions, thickness, and the like. FIG. 1 shows an example of an electrode group, and the electrode group included in the lithium primary battery according to the present disclosure is not limited to this example. The positional relationship between the winding start end and winding end end of the positive and negative electrodes, the number of windings, and the like are not limited to those shown in the example.

[0026] The lithium primary battery includes an electrode group 200 housed in an electrode case. As shown in FIG. 1 , the electrode group 200 is configured by spirally winding a strip-shaped positive electrode 201 and a strip-shaped negative electrode 202. A separator (not shown) is interposed between the positive electrode 201 and the negative electrode 202. The positive electrode 201 contains at least one material selected from the group consisting of manganese dioxide and graphite fluoride. The negative electrode 202 contains a lithium alloy, and the lithium alloy contains 0.02 mass % or more and 11 mass % or less of Mg. Although not shown, a positive electrode lead member may be connected to the positive electrode 201.

[0027] The negative electrode 202 has a first negative electrode main surface NS1 on the outer periphery side of the electrode group 200 and a second negative electrode main surface NS2 on the inner periphery side of the electrode group 200. The positive electrode 201 has a first positive electrode main surface PS1 on the inner periphery side of the electrode group 200 and a second positive electrode main surface PS2 on the outer periphery side of the electrode group 200. The first negative electrode main surface NS1 has a first opposing region NP1 facing the first positive electrode main surface PS1. The second negative electrode main surface NS2 has a second opposing region NP2 facing the second positive electrode main surface PS2.

[0028] The positive electrode 201 and the negative electrode 202 are wound such that the positive electrode 201 is disposed on the outermost and innermost peripheries of the electrode assembly 200. The positive electrode 201 has an innermost periphery portion PI disposed on the innermost periphery of the electrode assembly 200. The innermost periphery portion PI is a portion where at least the inner periphery side of the positive electrode (first positive electrode main surface PS1) does not face the negative electrode 202. The innermost periphery portion PI occupies at least one periphery of the innermost periphery of the electrode assembly 200. The innermost periphery portion PI occupies, for example, 1 to 1.9 peripheries of the innermost periphery of the electrode assembly 200.

[0029] The positive electrode 201 has an outermost peripheral portion PO1 disposed at the outermost periphery of the electrode assembly 200. The outermost peripheral portion PO1 is a portion where at least the outer peripheral side of the positive electrode (second positive electrode main surface PS2) does not face the negative electrode 202. In FIG. 1 , the outermost peripheral portion PO1 corresponds to one full turn of the outermost periphery of the electrode assembly 200. In the electrode assembly 200, the positive electrode 201 and the negative electrode 202 are wound such that the end PE on the winding end side of the positive electrode 201 and the end NE on the winding end side of the negative electrode 202 are positioned at approximately the same position.

[0030] 1 , the entire first negative electrode main surface NS1 faces the first positive electrode main surface PS1, and the entire second negative electrode main surface NS2 faces the second positive electrode main surface PS2. The ratio of the total area S1 of the first opposing region NP1 and the second opposing region NP2 to the total area S0 of the first negative electrode main surface NS1 and the second negative electrode main surface NS2 (S1 / S0 ratio) is 100%.

[0031] In FIG. 1 , the outermost portion PO1 is one circumference of the outermost circumference of the electrode group, but it may be more than one circumference of the outermost circumference of the electrode group, for example, 1 to 1.4 circumferences of the outermost circumference of the electrode group. In this case, the S1 / S0 ratio is 100%. In FIG. 1 , the S1 / S0 ratio is 100%, but the S1 / S0 ratio may be 90% or more. The outermost portion PO1 may be smaller than one circumference of the outermost circumference of the electrode group, as long as the S1 / S0 ratio is within the range of 90% or more.

[0032] The positive electrode 201 has an nth periphery portion PO(n+1) located n turns inward from the outermost periphery portion PO1, which is disposed at the outermost periphery of the electrode assembly 200. n is an integer equal to or greater than 1. The positive electrode 201 in FIG. 1 has first to fourth peripheries. In FIG. 1, PO2 indicates the first periphery portion (n=1) located at the first turn inward from the outermost periphery portion PO1, and PO3 indicates the second periphery portion (n=2) located at the second turn inward from the outermost periphery portion PO1. In the wound positive electrode 201, position B1 indicates the end of the outermost periphery portion PO1 on the first periphery portion PO2 side, and position B2 indicates the end of the first periphery portion PO2 opposite the outermost periphery portion PO1. The outermost periphery portion PO1 is the region from the end PE on the winding end side of the wound positive electrode 201 to position B1. The first winding portion PO2 is the region from position B1 to position B2 of the wound positive electrode.

[0033] The negative electrode 202 has a region X1 where the first negative electrode main surface NS1 faces the first positive electrode main surface PS1 of the outermost peripheral portion PO1. In Fig. 1 , the negative electrode lead member 210 is connected to the second negative electrode main surface NS2 in the region X1. Because the region X1 has a small curvature, a good connection state between the negative electrode 202 and the negative electrode lead member 210 is easily ensured.

[0034] The negative electrode 202 has a region X(n+1) in which the first negative electrode main surface NS1 faces the first positive electrode main surface PS1 of the nth periphery PO(n+1). n is an integer equal to or greater than 1. A negative electrode lead member 210 may be connected to the second negative electrode main surface NS2 of the region X(n+1). In the case of FIG. 1 , the negative electrode 202 has a region X1 and regions X2 to X5 (n = 1 to 4) located more inward than the region X1. In FIG. 1 , the negative electrode lead member 210 is connected to the region X1, but it may also be connected to any of the regions X2 to X5. For example, the negative electrode lead member 210 may be connected to the region X2 facing the first positive electrode main surface PS1 of the first periphery PO2.

[0035] The location where the negative electrode lead member 210 in FIG. 1 is connected is preferably regions X2 to X4, with region X3 located near the radial center of the electrode assembly 200 being more preferred. In this case, breakage of the negative electrode at the end of discharge is more suppressed, a good connection state between the negative electrode 202 and the negative electrode lead member 210 is more likely to be maintained, and pulse discharge characteristics are more likely to be improved. The reasons for this are thought to be that when the negative electrode lead member is located at or near the radial center of the electrode assembly, the influence of the winding of the negative electrode is reduced compared to when the negative electrode lead member is located at the radial end of the electrode assembly, and the negative electrode capacity relative to the positive electrode capacity is relatively large. For example, in region X1, lithium is consumed in the outermost peripheral portion PO1 and the half of the first periphery portion PO2 on the region X1 side. On the other hand, in region X2, lithium is consumed in the half of the first periphery portion PO2 on the region X2 side and the half of the second periphery portion PO3 on the region X2 side. In region X2, the ratio of (positive electrode capacity / negative electrode capacity) per area is smaller than in region X1.

[0036] The negative electrode lead member 210 may be connected to the first negative electrode main surface NS1, but is preferably connected to the second negative electrode main surface NS2 as shown in Fig. 1. When the negative electrode lead member 210 is connected to the second negative electrode main surface NS2, the second negative electrode main surface NS2 side (inner peripheral side) of the negative electrode 202 is curved into a concave shape as the negative electrode 202 is wound, thereby ensuring a stable electrical connection. In addition, the end face of the negative electrode lead member 210 in the width direction (winding direction) is likely to be covered by the negative electrode 202, which can suppress short circuits caused by the presence of burrs on the end face.

[0037] As shown in FIG. 1 , the line segment connecting the end PE at the winding end side of the positive electrode 201 (outermost peripheral portion PO1) to the axis C (winding axis) is designated L1, and the line segment connecting the axis C to the negative electrode lead member 210 connected to region X1 is designated L2. In this case, the angle θ in FIG. 1 formed by L1 and L2 may be, for example, 270° or less, 180° or less, 90° or less, or 45° or less. Since lithium isolation at the end of discharge is suppressed and the overall shape of the negative electrode is maintained until the end of discharge, the position to connect the negative electrode lead member can be appropriately determined depending on the battery structure. The same applies when connecting the negative electrode lead member to regions X2 to X5.

[0038] When the negative electrode lead member 210 is connected to region X1, it is preferable that the negative electrode lead member 210 be connected to a location in region X1 where the angle θ in FIG. 1 is 0 to 50°. In this case, pulse discharge characteristics are likely to be improved. As the positive electrode expands during discharge, the electrode group expands radially, causing the outer peripheral surface of the electrode group to contact the inner surface of the battery case, resulting in uneven surface pressure on the electrode group on the outer peripheral side of the electrode group including region X1, which can lead to uneven discharge reactions. Since the unevenness of the discharge reaction is suppressed in region X1 (θ = 0 to 50°) compared to region X1 (θ = over 50°), it is presumed that a good connection state between the negative electrode and the negative electrode lead member is more easily maintained during discharge, resulting in improved pulse discharge characteristics.

[0039] On the other hand, when the negative electrode lead member 210 is connected to the region X(n+1) which is located more inward than the region X1, the effect of non-uniform surface pressure on the outer periphery of the electrode group is smaller in the region X(n+1) than in the region X1, and therefore the effect of improving the pulse discharge characteristics can be stably obtained at any position within the region X(n+1).

[0040] Fig. 2 is a schematic top view showing an example of the vicinity of the connection part of the negative electrode with the negative electrode lead member. Fig. 3 is a schematic cross-sectional view showing an example of the vicinity of the connection part of the negative electrode with the negative electrode lead member. Fig. 3 is a cross-sectional view taken along III-III in Fig. 2. Fig. 4 is a schematic cross-sectional view showing another example of the vicinity of the connection part of the negative electrode with the negative electrode lead member. Figs. 3 and 4 show cross sections in the width direction of the negative electrode.

[0041] 2 to 4, the negative electrode lead member 210 has a first main surface S1 on the negative electrode 202 side and a second main surface S2 opposite to the first main surface S1. The negative electrode lead member 210 has a first region 210a overlapping with the negative electrode 202 and a second region 210b near the first region 210a. In the first region 210a, the first main surface S1 is in close contact with the second negative electrode main surface NS2.

[0042] An insulating tape 240 covering the negative electrode lead member 210 is attached to the negative electrode 202. Specifically, a first insulating tape 240a is attached to the negative electrode 202 so as to cover the first main surface S1 of the first region 210a and the second region 210b. A second insulating tape 240b is attached to the negative electrode 202 so as to cover the second main surface S2 of the first region 210a and the second region 210b. A portion of the second negative electrode main surface NS2 is covered by the second insulating tape 240b. A portion of the first negative electrode main surface NS1 is covered by the first insulating tape 240a. The first insulating tape 240a in FIG. 4 is smaller in size and covers a smaller area of ​​the first negative electrode main surface NS1 than the first insulating tape 240a in FIG. 3 .

[0043] 5 is a schematic cross-sectional view showing yet another example of the vicinity of the connection part of the negative electrode with the negative electrode lead member. FIG. 5 shows a cross section in the width direction of the negative electrode.

[0044] 5, the negative electrode lead member 210 has a first main surface S1 on the negative electrode 202 side and a second main surface S2 opposite the first main surface S1. The negative electrode lead member 210 has a first region 210a overlapping with the negative electrode 202 and a second region 210b near the first region 210a. The first region 210a includes a connection region 210c where the first main surface S1 is in close contact with the second negative electrode main surface NS2. The region of the first region 210a other than the connection region 210c overlaps with the negative electrode 202 via a first insulating tape 240a.

[0045] An insulating tape 240 covering the negative electrode lead member 210 is attached to the negative electrode 202. Specifically, a first insulating tape 240a is attached to the second negative electrode main surface NS2 so as to cover the first region 210a (excluding the connection region 210c) and the first main surface S1 of the second region 210b. A second insulating tape 240b is attached to the second negative electrode main surface NS2 so as to cover the second main surface S2 of the first region 210a and the second region 210b. A portion of the second negative electrode main surface NS2 is covered by the first insulating tape 240a and the second insulating tape 240b. The region of the first region 210a other than the connection region 210c and the first main surface S1 of the second region 210b are covered by the first insulating tape 240a without the negative electrode 202 in between. The first negative electrode main surface NS1 is not covered with the first insulating tape 240 a or the second insulating tape 240 b. Compared to the cases of Figures 4 and 5 in which part of the first negative electrode main surface NS1 is covered with the second insulating tape, a larger area of ​​the first negative electrode main surface NS1 that contributes to the discharge reaction (lithium consumption) can be ensured, which is advantageous in terms of improving output characteristics and increasing energy density.

[0046] The first negative electrode main surface NS1 and the second negative electrode main surface NS2 in FIGS. 3 to 5 may be the second negative electrode main surface NS2 and the first negative electrode main surface NS1, respectively.

[0047] The S1 / S0 ratio can be determined as follows. A wound electrode group is removed from a battery before use (undischarged), and one end face of the electrode group (for example, in the case of FIG. 6 , the end face of the electrode group 200 on the bottom side of the electrode case 100) is observed to confirm that the positive electrode is disposed at the outermost periphery of the electrode group (outermost periphery). If the electrode group is covered with a separator, the separator may be removed before confirmation. If the outermost periphery is equal to or greater than one outermost periphery of the electrode group, the S1 / S0 ratio is 100%. If the outermost periphery is less than one outermost periphery of the electrode group, a check mark is placed where the first negative electrode principal surface faces the end of the winding of the positive electrode (outermost periphery). Thereafter, the negative electrode is removed from the electrode group, unfolded, and the length and width dimensions of the negative electrode are measured to determine the total area S0 of the first negative electrode principal surface and the second negative electrode principal surface. The length from the end of the first negative electrode main surface on the winding start side to the checked point P is measured, and the area of ​​the first opposing region is calculated from this length and width. The area of ​​the second opposing region is the same as the area of ​​the second negative electrode main surface. The total area S1 of the first opposing region and the second opposing region is calculated, and the S1 / S0 ratio is calculated.

[0048] When insulating tape is applied to the first negative electrode main surface to cover the negative electrode lead member, the portion of the first negative electrode main surface covered with the insulating tape is not included in the first negative electrode main surface. When insulating tape is applied to the second negative electrode main surface to cover the negative electrode lead member, the portion of the second negative electrode main surface covered with the insulating tape is not included in the second negative electrode main surface.

[0049] The ratio of the positive electrode capacity to the negative electrode capacity (positive electrode capacity / negative electrode capacity) is preferably smaller than 1. In this case, lithium isolation due to partial loss or breakage of the negative electrode at the end of discharge is likely to be suppressed. (positive electrode capacity / negative electrode capacity) may be, for example, 0.91 to 0.96 or 0.92 to 0.95.

[0050] The lithium primary battery of the present disclosure will be described in more detail below.

[0051] (Negative Electrode) The negative electrode contains a lithium alloy, and the lithium alloy contains 0.02 to 11 mass % of Mg. From the viewpoint of ensuring capacity, the Li content in the lithium alloy may be 89 mass % or more, or may be 95 mass % or more.

[0052] The negative electrode may include a foil (sheet) of a lithium alloy, which may be formed into any shape and thickness depending on the shape, dimensions, performance specifications, etc. of the lithium primary battery.

[0053] The negative electrode may include a negative electrode current collector (e.g., copper foil) supporting the lithium alloy, or may be a foil-shaped lithium alloy without a negative electrode current collector. In the battery of the present disclosure, the shape of the negative electrode (lithium alloy) is maintained even at the end of discharge, ensuring the conductivity of the entire negative electrode even without a negative electrode current collector. The battery can have a higher energy density (higher capacity) by the volume of the negative electrode current collector. Because the lithium alloy contains Mg, and the relatively high strength Mg remains at the end of discharge, the negative electrode can be constructed using only a foil-shaped (sheet-shaped) lithium alloy without using a negative electrode current collector.

[0054] The lithium alloy contains at least Mg and may be substantially free of Al, although it is preferable for it to contain Al from the viewpoint of improving output voltage. Hereinafter, a lithium alloy containing Mg and substantially free of Al will also be referred to as a "Li-Mg alloy." A lithium alloy containing Mg and Al will also be referred to as a "Li-Mg-Al alloy." Note that "substantially free of Al" means that the amount of Al is below the detection limit in composition analysis of the lithium alloy (e.g., ICP atomic emission spectroscopy, atomic absorption spectroscopy, etc.).

[0055] That is, the lithium alloy may be a Li-Mg alloy, and a Li-Mg-Al alloy is preferable. When the lithium alloy contains Mg, the relatively high-strength Mg remains in a thin foil (sheet) shape at the end of discharge, and can play the role of a core material, suppressing breakage of the negative electrode at the end of discharge. When the lithium alloy contains Al, a low-resistance negative electrode coating is formed. When the lithium alloy contains Mg together with Al, non-uniform Li consumption due to Al segregation is suppressed. In this case, the effects of Mg and Al are stably obtained throughout the negative electrode, and Li is uniformly consumed on the negative electrode surface, resulting in a larger proportion of Li that can contribute to the discharge reaction at the end of discharge.

[0056] In the case of the Li-Mg-Al alloy, a low-resistance coating is formed, and the output voltage can be increased compared to the case of lithium metal or a lithium alloy containing only one of Mg and Al.

[0057] The Mg content in the Li—Mg alloy is preferably 0.05 mass % or more and 3 mass % or less, and more preferably 0.2 mass % or more and 1 mass % or less.

[0058] The Mg content in the Li—Mg—Al alloy is preferably 0.05% by mass or more and 3% by mass or less, more preferably 0.2% by mass or more and 1% by mass or less. The Al content in the Li—Mg—Al alloy is preferably 0.01% by mass or more (or 0.1% by mass or more) and 0.5% by mass or less. The total content of Mg and Al in the Li—Mg—Al alloy may be 0.03% by mass or more and 11% by mass or less, or 0.1% by mass or more and 5% by mass or less. In the case of the Li—Mg—Al alloy, the mass ratio of Mg to Al: Mg / Al may be, for example, 0.2 or more and 50 or less.

[0059] The lithium alloy may contain metal elements other than Li, Mg, and Al. Examples of the other metal elements include Sn, Ni, Pb, In, and K. From the viewpoint of ensuring discharge capacity and stabilizing internal resistance, the total content of metal elements other than lithium contained in the lithium alloy is preferably 11 mass% or less.

[0060] The composition of the lithium alloy can be determined by inductively coupled plasma (ICP) emission spectroscopy or atomic absorption spectroscopy (AAS).

[0061] (Positive Electrode) The positive electrode contains at least one material selected from the group consisting of manganese dioxide and graphite fluoride as a positive electrode active material. When this positive electrode is used, it is advantageous in terms of output voltage compared to a positive electrode made of iron disulfide. As the manganese dioxide, calcined electrolytic manganese dioxide is preferably used. A positive electrode containing manganese dioxide exhibits a relatively high voltage and is advantageous in terms of improving discharge characteristics (pulse discharge characteristics). It may also contain chemical manganese dioxide. The manganese dioxide may be in a mixed crystal state containing multiple types of crystalline states. The positive electrode may also contain manganese oxides other than manganese dioxide. Examples of manganese oxides other than manganese dioxide include MnO, Mn 3 O 4 , Mn 2 O 3 , Mn 2 O 7 The main component of the manganese oxide contained in the positive electrode is preferably manganese dioxide. Here, "main component" means that the proportion of manganese dioxide in the manganese oxide is 50% by mass or more. The proportion of manganese dioxide in the manganese oxide may be 70% by mass or more, or may be 90% by mass or more.

[0062] If iron disulfide is used as the positive electrode active material, the output voltage will be significantly reduced. This is because a positive electrode containing iron disulfide has a more base standard electrode potential than a positive electrode containing manganese dioxide or graphite fluoride. The nominal voltage of a lithium primary battery whose positive electrode active material is manganese dioxide or graphite fluoride is 3.0 V, while the nominal voltage of a lithium primary battery whose positive electrode active material is iron disulfide is 1.5 V. Because the nominal voltage difference is approximately 1.5 V, the use of iron disulfide as the positive electrode active material significantly reduces the output voltage, especially during pulse discharge at low temperatures. Furthermore, in the case of a positive electrode containing iron disulfide, the voltage at the end of discharge may be reduced due to the influence of Fe and S eluted from the positive electrode.

[0063] The positive electrode includes, for example, a strip-shaped positive electrode current collector and a positive electrode mixture layer held on the positive electrode current collector. The positive electrode mixture layer is formed, for example, by applying a wet positive electrode mixture to the surface of the sheet-shaped positive electrode current collector or by filling the positive electrode current collector with the wet positive electrode mixture, pressing the positive electrode mixture in the thickness direction, and drying the sheet-shaped positive electrode current collector.

[0064] The positive electrode mixture may contain a positive electrode active material, a binder, a conductive agent, etc. Examples of the binder include fluororesins such as polytetrafluoroethylene, rubber particles, and acrylic resins. Examples of the conductive agent include conductive carbon materials. Examples of the conductive carbon materials include natural graphite, artificial graphite, carbon black, and carbon fiber.

[0065] Examples of materials for the positive electrode current collector include stainless steel, aluminum, and titanium. The positive electrode current collector is preferably a perforated current collector. Examples of perforated current collectors include expanded metal, net, and punched metal.

[0066] (Non-aqueous electrolyte) The non-aqueous electrolyte contains, for example, a non-aqueous solvent and a lithium salt. The concentration of lithium ions contained in the non-aqueous electrolyte (total concentration of the lithium salt) is, for example, 0.2 mol / L or more and 2.0 mol / L or less, and may be 0.3 mol / L or more and 1.5 mol / L or less.

[0067] Examples of non-aqueous solvents include organic solvents that are commonly used in non-aqueous electrolytes for lithium primary batteries. Examples of non-aqueous solvents include ethers, esters, and carbonate esters. Examples of non-aqueous solvents that can be used include dimethyl ether, γ-butyl lactone, propylene carbonate (PC), ethylene carbonate (EC), dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, 1,2-dimethoxyethane (DME), 1,2-diethoxyethane, methyl acetate, ethyl acetate, and propyl acetate. The non-aqueous electrolyte may contain one non-aqueous solvent or two or more non-aqueous solvents.

[0068] From the viewpoint of improving the discharge characteristics of a lithium primary battery, the nonaqueous solvent preferably contains a cyclic carbonate having a high boiling point and a chain ether having low viscosity even at low temperatures. The cyclic carbonate preferably contains at least one selected from the group consisting of PC and EC, with PC being particularly preferred. The chain ether preferably contains DME.

[0069] Examples of the lithium salt include lithium salts used as solutes in lithium primary batteries. Examples of such lithium salts include LiCF 3 SO 3 , LiClO 4 , LiBF 4 , LiPF 6 , LiRaSO 3 (Ra is a fluorinated alkyl group having 1 to 4 carbon atoms), LiFSO 3 , LiN(SO 2 Rb)(SO 2 Rc) (Rb and Rc each independently represent a fluorinated alkyl group having 1 to 4 carbon atoms), LiN(FSO 2 ) 2 , LiN(SO 2 CF 3 ) 2 , LiN(SO 2 F) (POF 2 ), LiPO 2 F 2 , LiB(C 2 O 4 ) 2 , LiBF 2 (C 2 O 4 Among them, LiCF is preferred from the viewpoint of stability against lithium alloys containing Al and Mg. 3 SO 3 , LiBF 4 , and LiN(FSO 2 ) 2 The non-aqueous electrolyte may contain one or more of these lithium salts.

[0070] The nonaqueous electrolyte may further contain other components such as the additives described above. Examples of other components besides the additives include propane sultone, propene sultone, ethylene sulfite, 3,2-dioxathiolane-2,2-dioxide, vinylene carbonate, vinylethylene carbonate, fluoroethylene carbonate, adiponitrile, succinonitrile, and succinic anhydride. The other components may be lithium salts or may be capable of generating lithium ions.

[0071] (Separator) A lithium primary battery usually includes a separator interposed between the positive electrode and the negative electrode. As the separator, a porous sheet formed of an insulating material that is resistant to the internal environment of a lithium primary battery may be used. Specific examples include a synthetic resin nonwoven fabric, a synthetic resin microporous membrane, or a laminate thereof.

[0072] Examples of synthetic resins used for nonwoven fabrics include polypropylene, polyphenylene sulfide, and polybutylene terephthalate. Examples of synthetic resins used for microporous membranes include polyolefin resins such as polyethylene, polypropylene, and ethylene-propylene copolymers. The microporous membrane may contain inorganic particles as needed.

[0073] The thickness of the separator is, for example, 5 μm or more and 100 μm or less.

[0074] FIG. 6 shows a partial cross-sectional front view of a lithium primary battery according to one embodiment of the present invention. The lithium primary battery 10 includes a cylindrical electrode case 100 with a bottom, a wound electrode assembly 200 housed in the electrode case 100, and a sealing plate 300 that closes the opening of the electrode case 100. The sealing plate 300 is fixed to the electrode case 100 near the opening by welding. An opening is formed in the center of the sealing plate 300, and an external terminal 330 is disposed in this opening. An insulating gasket 310 is disposed between the external terminal 330 and the sealing plate 300. The electrode assembly 200 is housed inside the electrode case 100 together with a nonaqueous electrolyte (not shown). To prevent internal short circuits, an upper insulating plate 230A and a lower insulating plate 230B are disposed on the upper and lower parts of the electrode assembly 200, respectively.

[0075] The electrode group 200 is constructed by spirally winding a strip-shaped positive electrode 201 and a strip-shaped negative electrode 202 with a separator 203 interposed therebetween. A negative electrode lead member 210 is connected to the negative electrode 202. The negative electrode lead member 210 is connected to an external terminal 330 (negative electrode terminal) by welding or the like. A positive electrode lead member 220 is connected to the positive electrode 201. The positive electrode lead member 220 is connected to the inner bottom surface of the electrode case 100 by welding or the like.

[0076] The negative electrode 202 includes at least a foil-shaped (or sheet-shaped) lithium alloy. The lithium alloy contains 0.02 to 11 mass % or less of Mg. The S1 / S0 ratio of the negative electrode 202 is 90% or more. The positive electrodes 201 are disposed on the outermost and innermost peripheries of the electrode assembly 200.

[0077] The structure and shape of the lithium primary battery are not particularly limited. The wound electrode group may be cylindrical or flat. The shape of the lithium primary battery may be cylindrical or prismatic.

[0078] Examples of materials for the electrode case include stainless steel, nickel-plated steel, iron, titanium, and aluminum. However, when the positive electrode and the electrode case are electrically connected as shown in FIG. 6, austenitic stainless steel (e.g., SUS316) is preferred from the viewpoint of corrosion resistance.

[0079] 6 is used as a negative electrode terminal, it may also be used as a positive electrode terminal, i.e., the positive electrode lead member may be connected to the external terminal, and the negative electrode lead member may be connected to the inner bottom surface of the battery case.

[0080] <<Notes>> The above description of the embodiment discloses the following techniques. (Technology 1) A battery comprising a wound electrode group and a non-aqueous electrolyte, wherein the electrode group is configured by spirally winding a strip-shaped positive electrode, a strip-shaped negative electrode, and a separator disposed between the positive electrode and the negative electrode, wherein the positive electrode contains at least one material selected from the group consisting of manganese dioxide and graphite fluoride, wherein the negative electrode contains a lithium alloy, and wherein the lithium alloy contains 0.02 mass % or more and 11 mass % or less of magnesium, wherein the negative electrode has a first negative electrode main surface on an outer periphery of the electrode group and a second negative electrode main surface on an inner periphery of the electrode group, wherein the positive electrode has a first positive electrode main surface on an inner periphery of the electrode group and a second positive electrode main surface on an outer periphery of the electrode group, wherein the first negative electrode main surface has a first opposing region facing the first positive electrode main surface, and the second negative electrode main surface has a second opposing region facing the second positive electrode main surface, A lithium primary battery, in which a ratio of a total area S1 of the first opposing region and the second opposing region to a total area S0 of the first negative electrode main surface and the second negative electrode main surface is 90% or more. (Technology 2) The lithium primary battery according to Technology 1, in which the lithium alloy contains aluminum, The magnesium content in the lithium alloy is 0.05% by mass or more and 3% by mass or less, and The aluminum content in the lithium alloy is 0.01% by mass or more and 0.5% by mass or less. (Technology 3) The lithium primary battery according to Technology 2, in which the magnesium content in the lithium alloy is 0.2% by mass or more and 1% by mass or less. (Technology 4) The lithium primary battery according to any one of Technology 1 to 3, in which a negative electrode lead member is connected to the negative electrode. (Technology 5) The lithium primary battery according to Technology 4, wherein the positive electrode has an outermost peripheral portion disposed on the outermost periphery of the electrode group, the negative electrode includes a region X1 in which the first negative electrode main surface faces the first positive electrode main surface of the outermost peripheral portion, and the negative electrode lead member is connected to the second negative electrode main surface of the region X1.(Technology 6) The lithium primary battery according to Technology 4, wherein the positive electrode has an outermost portion disposed at the outermost periphery of the electrode group and an nth periphery portion located n th periphery more inward than the outermost portion, the negative electrode includes a region X(n+1) where the first negative electrode main surface faces the first positive electrode main surface of the nth periphery portion, and the negative electrode lead member is connected to the second negative electrode main surface of the region X(n+1). (Technology 7) The lithium primary battery according to Technology 4, wherein the negative electrode lead member is connected near the center in the radial direction of the electrode group. (Technology 8) The lithium primary battery according to any one of Technologies 4 to 7, wherein the negative electrode lead member has a first main surface on the negative electrode side and a second main surface opposite to the first main surface, the negative electrode lead member has a first region overlapping the negative electrode and a second region near the first region, the first region includes a connection region in close contact with the second negative electrode main surface, a first insulating tape is attached to the second negative electrode main surface so as to cover an area other than the connection region of the first region and the first main surface of the second region, and a second insulating tape is attached to the second negative electrode main surface so as to cover the first region and the second main surface of the second region. (Technology 9) The lithium primary battery according to any one of Technologies 1 to 8, wherein the negative electrode does not include a negative electrode current collector and is the lithium alloy in a foil form.

[0081] [Examples] Hereinafter, the present disclosure will be specifically described based on examples and comparative examples, but the present disclosure is not limited to the following examples.

[0082] Example 1 (Preparation of Negative Electrode) A lithium alloy foil was cut to obtain a strip-shaped negative electrode. The lithium alloy foil used was a Li-Mg alloy foil with an Mg content of 0.5 mass %.

[0083] (Preparation of Positive Electrode) 100 parts by mass of the positive electrode active material were mixed with 5 parts by mass of Ketjen Black as a conductive agent, 5 parts by mass of polytetrafluoroethylene as a binder, and an appropriate amount of pure water to prepare a wet positive electrode mixture. Electrolytic manganese dioxide (MnO) that had been baked at 400°C for 5 hours was used as the positive electrode active material. 2 ) was used.

[0084] Next, the positive electrode mixture was filled into a positive electrode current collector made of stainless steel expanded metal (height 0.2 mm) to prepare a positive electrode precursor. The positive electrode precursor was then dried, rolled by a roll press, and cut to obtain a strip-shaped positive electrode. Subsequently, a portion of the filled positive electrode mixture was peeled off, and one end of a stainless steel positive electrode lead member was resistance-welded to the exposed portion of the positive electrode current collector.

[0085] A positive electrode was prepared using electrolytic manganese dioxide so that the ratio (positive electrode capacity / negative electrode capacity) was 0.93. The positive electrode capacity was calculated by multiplying the theoretical capacity per gram of manganese dioxide by the mass of manganese dioxide contained in the positive electrode. The mass of manganese dioxide was calculated by multiplying the mass of electrolytic manganese dioxide filled in the positive electrode by the purity of the electrolytic manganese dioxide, 0.9. The theoretical capacity per gram of manganese dioxide was 308 mAh. The negative electrode capacity was calculated by multiplying the theoretical capacity per gram of lithium (3861 mAh) by the mass of lithium contained in the negative electrode.

[0086] (Attachment of negative electrode lead member) One end of a nickel negative electrode lead member was connected to a predetermined location on the negative electrode by pressure welding. The negative electrode lead was attached to a predetermined location on the negative electrode (second negative electrode main surface) so that it would be located in region X1 (FIG. 1, θ=45°) of the negative electrode when the electrode group was constructed. Insulating tape (first insulating tape and second insulating tape) was attached to the negative electrode so as to cover the negative electrode lead member. The insulating tape was attached as shown in FIG. 3.

[0087] (Preparation of Electrode Assembly) An electrode assembly was prepared by winding a positive electrode and a negative electrode with a separator interposed therebetween. A 25 μm thick polypropylene microporous film was used as the separator. The electrode assembly was constructed so that the positive electrode had a first outermost peripheral portion and the S1 / S0 ratio was 100%.

[0088] (Preparation of non-aqueous electrolyte) LiCF was dissolved in a mixed solvent of PC, EC, and DME (volume ratio 25:25:50). 3 SO 3 was dissolved in the solution at a concentration of 0.6 mol / L to prepare a non-aqueous electrolyte solution.

[0089] (Assembly of Lithium Primary Battery) The electrode group was housed in a stainless steel, bottomed, cylindrical electrode case (outer diameter 17.5 mm, height 50.5 mm) that also served as a positive electrode terminal. An upper insulating plate and a lower insulating plate were placed on the upper and lower end surfaces of the electrode group, respectively. The other end of the positive electrode lead member was connected to the inner surface of the bottom of the electrode case by resistance welding. A sealing plate equipped with an external terminal (negative electrode terminal) was prepared. A gasket was interposed between the sealing plate and the external terminal. The other end of the negative electrode lead member was connected to the external terminal by resistance welding. A nonaqueous electrolyte was injected into the electrode case, and then the open end of the electrode case and the periphery of the sealing plate were laser welded, and the opening of the electrode case was sealed with the sealing plate. In this manner, a lithium primary battery (Battery A1) having the structure shown in FIG. 6 was fabricated.

[0090] Battery B1 of Comparative Example 1 was produced in the same manner as Battery A1 of Example 1, except that a Li—Al alloy foil with an Al content of 0.2 mass % was used as the lithium alloy foil. The Li—Al alloy was a lithium alloy containing Al and substantially no Mg.

[0091] Battery B2 of Comparative Example 2 was fabricated in the same manner as Battery A1 of Example 1, except that the S1 / S0 ratio was set to 89%. The S1 / S0 ratio was adjusted by changing the position of the end of the negative electrode on the winding start side.

[0092] Comparative Example 3: A Li-Al alloy foil with an Al content of 0.2% by mass was used as the lithium alloy foil. The S1 / S0 ratio was set to 89%. The S1 / S0 ratio was adjusted by changing the position of the end of the negative electrode on the winding start side. Other than the above, Battery B3 of Comparative Example 3 was fabricated in the same manner as Battery A1 of Example 1.

[0093] Comparative Example 4 Battery B4 of Comparative Example 4 was produced in the same manner as in Comparative Example B1, except that the negative electrode lead was attached to a predetermined location on the negative electrode (second negative electrode type surface) so that the negative electrode lead was arranged in region X1 (θ=270° in FIG. 1 ) of the negative electrode when the electrode group was constructed.

[0094] Examples 2 and 3, Comparative Examples 5 and 6 Batteries A2 and A3 of Examples 2 and 3 and batteries B5 and B6 of Comparative Examples 5 and 6 were produced in the same manner as battery A1 of Example 1, except that Li—Mg alloy foils having Mg contents shown in Table 1 were used as the lithium alloy foils.

[0095] Examples 4 to 5 Batteries A4 to A5 of Examples 4 to 5 were fabricated in the same manner as Battery A1 of Example 1, except that the S1 / S0 ratio was set to 95% or 90%. The S1 / S0 ratio was adjusted by changing the position of the end of the negative electrode on the winding start side.

[0096] Example 6 and Comparative Example 7: Graphite fluoride (CF) was used as the positive electrode active material. n ) or iron disulfide (FeS 2 Battery A6 of Example 6 and battery B7 of Comparative Example 7 were fabricated in the same manner as battery A1 of Example 1, except that 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 2

[0097] Comparative Example 8 Battery B8 of Comparative Example 8 was produced in the same manner as Battery A6 of Example 6, except that lithium metal foil was used instead of the lithium alloy foil.

[0098] Examples 7 to 9 Batteries A7 to A9 of Examples 7 to 9 were produced in the same manner as Battery A1 of Example 1, except that the negative electrode lead was attached to a predetermined location on the negative electrode (second negative electrode main surface) so that the negative electrode lead was arranged in region X1 of the negative electrode (θ = 90°, 180°, or 270° in FIG. 1 ) when the electrode group was constructed.

[0099] Examples 10 to 13 Batteries A10 to A13 of Examples 10 to 13 were produced in the same manner as Battery A1 of Example 1, except that the negative electrode lead was attached to a predetermined location on the negative electrode (second negative electrode main surface) so that it was arranged in region X2 of the negative electrode (θ = 45°, 90°, 180°, or 270° in FIG. 1 ) when the electrode group was constructed.

[0100] Examples 14 to 16 Batteries A14 to A16 of Examples 14 to 16 were produced in the same manner as battery A1 of Example 1, except that the negative electrode lead was attached to a predetermined location on the negative electrode (second negative electrode main surface) so that the negative electrode lead was arranged in region X3, X4, or X5 (θ=45° in FIG. 1 ) of the negative electrode when the electrode group was constructed.

[0101] Examples 17 to 30 Batteries A17 to A30 of Examples 17 to 30 were produced in the same manner as Battery A1 of Example 1, except that Li-Mg-Al alloy foils having Mg contents and Al contents shown in Table 7 were used as the lithium alloy foils.

[0102] Examples 31-32 Batteries A31-A32 of Examples 31-32 were produced in the same manner as battery A27 of Example 27, except that the insulating tapes (first insulating tape and second insulating tape) were attached as shown in FIG. 4 or 5 .

[0103] After assembly, the resulting batteries of the Examples and Comparative Examples were aged for 7 days in an atmosphere at 45° C., and then evaluated as follows.

[0104] [Evaluation] The aged batteries were discharged at a constant current of 20 mA until the depth of discharge (DOD) reached 90% (until the discharged quantity of electricity reached 90% of the positive electrode capacity) in an environment of 23±2° C. The batteries with a DOD of 90% were left in an environment of 0° C. for 4 hours or more, and then pulse-discharged at 500 mA for 5 seconds in an environment of 0° C., and the minimum voltage at this time was determined.

[0105] The evaluation results are shown in Tables 1 to 8. Tables 1 to 8 also show the positive electrode capacity.

[0106]

[0107]

[0108]

[0109]

[0110]

[0111]

[0112]

[0113]

[0114] As shown in Tables 1 and 2, Batteries A1 to A5, which had an S1 / S0 ratio of 90% or more, a Mg content in the Li-Mg alloy of the negative electrode in the range of 0.02 to 11% by mass, and a positive electrode containing manganese dioxide, exhibited superior pulse discharge characteristics compared to Batteries B1 to B6.

[0115] Battery A1, which had a 100% S1 / S0 ratio and a 0.5% Mg content in the Li-Mg alloy anode, showed significantly improved pulse discharge characteristics compared to battery B7, which had a 89% S1 / S0 ratio and a Li-Al alloy anode (B3 → A1). Battery B1, which had a 100% S1 / S0 ratio but a Li-Al alloy anode, exhibited reduced anode strength and fractured the anode at the end of discharge, resulting in no improvement in pulse discharge characteristics compared to battery B3 (B3 → B1). Battery B2, which had a 0.5% or higher Mg content in the Li-Mg alloy but a 89% S1 / S0 ratio, exhibited uneven lithium consumption at the anode, resulting in fracture of the anode at the end of discharge, resulting in a smaller improvement in pulse discharge characteristics compared to battery B3 (B3 → B2).

[0116] In Battery B4, where the connection point of the negative electrode lead member was in region X1 (θ = 270° in Figure 1), the pulse discharge characteristics were even worse than in Battery B1, where the connection point of the negative electrode lead member was in region X1 (θ = 45° in Figure 1). In Battery B5, the Mg content in the Li-Mg alloy was less than 0.02% by mass, which reduced the strength of the negative electrode, caused the negative electrode to fracture at the end of discharge, and reduced the pulse discharge characteristics. In Battery B6, the Mg content in the Li-Mg alloy was more than 11% by mass, which reduced the amount of Li contained in the negative electrode, resulting in reduced pulse discharge characteristics.

[0117] As shown in Table 3, battery A6, which had a 100% S1 / S0 ratio, a 0.5% Mg content in the Li-Mg alloy anode, and a positive electrode containing graphite fluoride, exhibited excellent pulse discharge characteristics. Battery B8, which had a 100% S1 / S0 ratio but used lithium metal foil for the negative electrode, exhibited reduced negative electrode strength, resulting in the negative electrode breaking at the end of discharge and reduced pulse discharge characteristics. Battery B7, which had a 0.5% Mg content in the Li-Mg alloy and a 100% S1 / S0 ratio, exhibited a significant reduction in the minimum voltage during pulse discharge due to the use of iron disulfide as the positive electrode active material.

[0118] As shown in Table 4, all of the batteries A1, A7 to A9, in which the negative electrode lead was connected to a predetermined position in region X1 (θ = 45°, 90°, 180°, or 270° in Figure 1), exhibited excellent pulse discharge characteristics. When the negative electrode lead was connected to region X1, the pulse discharge characteristics were further improved when θ = 45° (Battery A1).

[0119] As shown in Table 5, all of the batteries A10 to A13 in which the negative electrode lead was connected to a predetermined position in region X2 (θ = 45°, 90°, 180°, or 270° in FIG. 1) exhibited excellent pulse discharge characteristics.

[0120] As shown in Table 6, when the negative electrode lead was connected to any of the regions X1 to X5 (θ = 45° in FIG. 1) in FIG. 1, the pulse discharge characteristics improved as the location where the negative electrode lead member was connected became closer to the center in the radial direction of the electrode group.

[0121] As shown in Table 7, the pulse discharge characteristics were improved in batteries A17 to A30, which used a Li—Mg—Al alloy for the negative electrode and had a Mg content of 0.05 to 3 mass% and an Al content of 0.01 to 0.5 mass%. In particular, the pulse discharge characteristics were significantly improved in batteries A23 to A30, which used a Li—Mg—Al alloy for the negative electrode and had a Mg content of 0.2 to 1 mass% and an Al content of 0.01 to 0.5 mass%.

[0122] As shown in Table 8, excellent pulse discharge characteristics were obtained for all of batteries A27, A31, and A32, in which insulating tape covering the negative electrode lead member was attached to the negative electrode as shown in Figure 3, Figure 4, or Figure 5. The smaller the area of ​​the negative electrode covered with insulating tape, the higher the minimum voltage during pulse discharge, and battery A32 obtained the highest minimum voltage during pulse discharge.

[0123] The lithium primary battery of the present disclosure is suitable for use, for example, as a main power source or memory backup power source for various meters (for example, smart meters for electricity, water, gas, etc.).

[0124] While the present invention has been described in terms of presently preferred embodiments, such disclosure is not to be interpreted as limiting. Various changes and modifications will no doubt become apparent to those skilled in the art to which the present invention pertains upon reading the above disclosure. It is therefore intended that the appended claims be interpreted to cover all changes and modifications that do not depart from the true spirit and scope of the invention.

[0125] 10: Lithium primary battery, 100: Electrode case, 200: Electrode group, 201: Positive electrode, 202: Negative electrode, 203: Separator, 210: Negative electrode lead member, 210a: First region, 210b: Second region, 210c: Connection region, 220: Positive electrode lead member, 230A: Upper insulating plate, 230B: Lower insulating plate, 240: Insulating tape, 240a: First insulating tape, 240b: Second insulating tape, 300: Sealing plate, 310: Gasket, 330: External terminal

Claims

1. A battery comprising a wound electrode group and a non-aqueous electrolyte, wherein the electrode group is configured by spirally winding a strip-shaped positive electrode, a strip-shaped negative electrode, and a separator disposed between the positive electrode and the negative electrode, wherein the positive electrode contains at least one material selected from the group consisting of manganese dioxide and graphite fluoride, wherein the negative electrode contains a lithium alloy, and wherein the lithium alloy contains 0.02 mass % or more and 11 mass % or less of magnesium, wherein the negative electrode has a first negative electrode main surface on the outer periphery side of the electrode group and a second negative electrode main surface on the inner periphery side of the electrode group, wherein the positive electrode has a first positive electrode main surface on the inner periphery side of the electrode group and a second positive electrode main surface on the outer periphery side of the electrode group, wherein the first negative electrode main surface has a first opposing region facing the first positive electrode main surface, and the second negative electrode main surface has a second opposing region facing the second positive electrode main surface, a ratio of a total area S1 of the first opposing region and the second opposing region to a total area S0 of the first negative electrode principal surface and the second negative electrode principal surface is 90% or more.

2. The lithium primary battery according to claim 1, wherein the lithium alloy contains aluminum, the magnesium content in the lithium alloy is 0.05% by mass or more and 3% by mass or less, and the aluminum content in the lithium alloy is 0.01% by mass or more and 0.5% by mass or less.

3. The lithium primary battery according to claim 2, wherein the magnesium content in the lithium alloy is 0.2% by mass or more and 1% by mass or less.

4. The lithium primary battery according to claim 1, wherein a negative electrode lead member is connected to the negative electrode.

5. The lithium primary battery according to claim 4, wherein the positive electrode has an outermost portion arranged on the outermost periphery of the electrode group, the negative electrode includes a region X1 where the first negative electrode main surface faces the first positive electrode main surface of the outermost portion, and the negative electrode lead member is connected to the second negative electrode main surface of the region X1.

6. The lithium primary battery according to claim 4, wherein the positive electrode has an outermost portion disposed on the outermost periphery of the electrode group and an nth peripheral portion located nth circumference further inward than the outermost portion, the negative electrode includes a region X(n+1) where the first negative electrode main surface faces the first positive electrode main surface of the nth peripheral portion, and the negative electrode lead member is connected to the second negative electrode main surface of the region X(n+1).

7. The lithium primary battery according to claim 4, wherein the negative electrode lead member is connected near the center in the radial direction of the electrode group.

8. The lithium primary battery according to claim 4, wherein the negative electrode lead member has a first main surface on the negative electrode side and a second main surface opposite to the first main surface, the negative electrode lead member has a first region overlapping with the negative electrode and a second region adjacent to the first region, the first region includes a connection region in close contact with the second negative electrode main surface, a first insulating tape is affixed to the second negative electrode main surface so as to cover an area other than the connection region of the first region and the first main surface of the second region, and a second insulating tape is affixed to the second negative electrode main surface so as to cover the first region and the second main surface of the second region.

9. The lithium primary battery according to claim 1, wherein the negative electrode is a foil of the lithium alloy without a negative electrode current collector.

Citation Information

Patent Citations

  • Non-aqueous electrolyte battery

    JP1990070365U

  • Electrochemical cell

    JP1990257573A

  • Cylindrical nonaqueous electrolyte primary battery and its manufacturing method

    JP2009266715A

  • Lithium cell

    JP1986074264A

  • Organic electrolyte battery

    JP1993290826A