Resin particles, method for producing resin particles, hot melt material, coating material, and resin composition
By producing resin particles with a high polybutylene succinate content and controlling hollow portions, the challenges of particle size and environmental impact are addressed, resulting in improved uniformity and performance across various applications.
Patent Information
- Application Number
- PCT/JP2024/013042
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-30
- Filing Date
- 2024-03-29
- Publication Date
- 2024-10-03
AI Technical Summary
Existing methods for producing resin particles face challenges such as difficulty in achieving desired particle size, high organic solvent usage, and adverse effects on optical properties, color tone, and adhesion due to hollow portions within the particles, particularly large-diameter hollow parts.
Resin particles with a high content of polybutylene succinate, a biodegradable material, are produced with controlled hollow portions by emulsifying polybutylene succinate in water using polyvinyl alcohol and an electrolyte, reducing the formation of large-diameter hollow parts to enhance uniformity and performance across various applications.
The approach results in resin particles with improved uniformity in strength and specific gravity, reduced environmental impact, and enhanced suitability for diverse applications by minimizing the negative effects of hollow portions, thereby improving optical properties and adhesion.
Smart Images

Figure JPOXMLDOC01-APPB-T000001
Abstract
Description
Resin particles, method for producing resin particles, hot melt material, paint, and resin composition
[0001] The present invention relates to resin particles, a method for producing resin particles, a hot melt material, a coating material, and a resin composition.
[0002] Resin particles are used in various fields such as paints, optical components, resin modifiers, antiblocking agents, etc. Resin particles are required to have various properties depending on their applications, and in consideration of industrial productivity, it is also important that they can be easily produced.
[0003] On the other hand, in recent years, with the growing interest in environmental issues, in order to reduce the environmental load, it is required to use materials derived from non-petroleum raw materials and biodegradable materials in all fields where resins are used. Also, in terms of the environmental load, it is preferable to reduce or not use organic solvents in the production process of resin particles.
[0004] As methods for producing resin particles using biodegradable materials, there have been proposed a method for producing resin particles using a freeze-pulverization method (Patent Document 1), a solvent solution precipitation method in which resin particles are produced by dissolving a resin in a solvent and then precipitating it by adding a poor solvent (Patent Documents 2 to 4), and a method for producing resin particles by emulsifying a resin at high temperature using a solvent that does not dissolve the resin and an emulsifier (Patent Documents 5 to 7).
[0005] JP 2018-002291 A, WO 2012 / 105140 A, JP 2005-002302 A, JP 2018-193500 A, WO 2017 / 195642 A, JP 2004-099883 A, JP 2022-161001 A
[0006] However, the methods for producing resin particles described in Patent Documents 1 and 6 have a problem in that it is difficult to obtain resin particles having a desired particle size. In addition, the methods for producing resin particles described in Patent Documents 2 to 6 have a problem in that they require the use of a large amount of organic solvent, which is undesirable from the viewpoint of environmental load.
[0007] Furthermore, as described above, resin particles are used in a variety of applications, but problems may arise when resin particles are used for each application. For example, when used in paint applications, problems such as changes or impairment of the color tone of the coating film may occur. When used in optical applications, problems such as changes in refractive index may occur. When used in hot melt materials, problems such as reduced adhesiveness may occur. The resin particles of Patent Document 7 also cause a problem in that the polyhydric alcohol fatty acid ester causes discoloration when used in hot melt materials.
[0008] In order to solve the above problems, it has been proposed to solve the above problems by improving the average particle size or particle size distribution of resin particles, but none of the resin particles can solve the above problems, and there is a demand for resin particles that reduce the environmental load and can be suitably used in various applications.
[0009] In view of the above-mentioned problems, and as a result of various studies, the present invention has found that hollow portions formed inside particles within a specific particle diameter range are one cause of the above-mentioned problems. The present invention provides resin particles that can be suitably used for various applications by reducing the number of hollow portions having a predetermined size formed inside particles within a specific particle diameter range, and a method for producing the same.
[0010] [Resin Particles] The resin particles are resin particles containing polybutylene succinate. Polybutylene succinate is a biodegradable plastic that can be naturally decomposed by microorganisms in soil in nature. Polybutylene succinate can use raw material monomers derived from non-petroleum sources (preferably plant sources), which can reduce the environmental impact.
[0011] The content of polybutylene succinate in the resin constituting the resin particles is preferably 50% by mass or more, more preferably 60% by mass or more, more preferably 70% by mass or more, more preferably 80% by mass or more, more preferably 90% by mass or more, more preferably 95% by mass or more, and more preferably 99% by mass or more.
[0012] The resin particles may contain a plasticizer. Known plasticizers can be used as the plasticizer. Examples of the plasticizer include alkylsulfonamides, arylsulfonaryls, alkylene glycol benzoates, and dialkylene glycol benzoates. The plasticizers may be used alone or in combination. The plasticizer is preferably contained in the resin particles in an amount of 1 to 40% by mass, and more preferably 5 to 30% by mass.
[0013] The resin particles may contain an antistatic agent. The antistatic agent is not particularly limited, and examples thereof include polyoxyethylene alkylphenol ether and stearic acid monoglyceride. The antistatic agent may be used alone or in combination of two or more types. The content of the antistatic agent in the resin particles is preferably 1 to 40% by mass, and more preferably 3 to 30% by mass.
[0014] Resin particles are used in a variety of applications, such as paints, optical components, resin modifiers, and antiblocking agents. After extensive investigations into the problems that arise when resin particles are used in these applications, it was discovered that hollow portions of a specific size formed within a specific range within the resin particles are one of the causes of the problems.
[0015] Specifically, in large-diameter particles having a particle diameter 1.6 to 4.0 times the volume average particle diameter of the resin particles, the number of large-diameter hollow portions formed within these large-diameter particles is reduced, thereby preventing or reducing problems that occur when the resin particles are used.
[0016] Large-diameter particles refer to particles with a particle diameter 1.6 to 4.0 times the volume average particle diameter of the resin particles. Because of their large particle diameter, large-diameter particles with a particle diameter 1.6 to 4.0 times the volume average particle diameter have a high probability of being incident on the large-diameter particles when light is incident on the resin particles in the usage environment, resulting in a significant impact on the optical properties and color tone of the large-diameter particles. Furthermore, when the resin particles dissolve during use, the large volume of the large-diameter particles increases the amount of emulsifier and air that the large-diameter particles can retain in their hollow spaces, resulting in a significant adverse impact on the intended use of the resin particles. For this reason, the present invention focuses particularly on large-diameter particles among the resin particles.
[0017] When large-diameter hollows are formed in large-diameter particles, the large-diameter hollows contain a large amount of air that has replaced the emulsifier and / or water used in the resin particle manufacturing process. If a large amount of emulsifier or air is contained in the large-diameter hollows, for example, when light passes through the resin particles, the light is likely to be diffused by the inner wall of the large-diameter hollows or the surface of the emulsifier. This can adversely affect the optical properties and color tone of the resin particles during use due to changes in the refractive index at the interface between the emulsifier in the large-diameter hollows and the air or the inner wall of the large-diameter hollows. Furthermore, if the resin particles melt during use, the emulsifier contained in the large-diameter hollows can leak out, causing changes in color tone and adversely affecting the environment in which the resin particles are used.
[0018] Therefore, by focusing on the large-diameter hollow portions of large-diameter particles and setting the average number of these large-diameter hollow portions to 10 or less, problems that arise when using resin particles can be prevented or reduced, allowing the resin particles to be used suitably in various applications.
[0019] The resin particles of the present invention are large-diameter particles (hereinafter sometimes simply referred to as "large-diameter particles") having a particle diameter 1.6 to 4.0 times the volume-average particle diameter of all resin particles. In any 10 large-diameter particles having internal hollow portions, the average number of large-diameter hollow portions (hereinafter sometimes simply referred to as "large-diameter hollow portions") having a major axis 0.05 times or more the particle diameter of the large-diameter particles is 10 or less. The average number of large-diameter hollow portions in the resin particles is preferably 8 or less, more preferably 7 or less, and even more preferably 6 or less. The "hollow portions of the resin particles" refers to voids formed within the resin particles.
[0020] By setting the average number of large-diameter hollow portions among any 10 large-diameter particles having hollow portions to 10 or less, adverse effects on optical properties, color tone, adhesiveness, etc., during use of the resin particles can be prevented or reduced, allowing the resin particles to be suitably used for various purposes. Furthermore, the strength and specific gravity of the resin particles can be made approximately uniform, and the homogenization of other components containing the resin particles and materials using the resin particles can be achieved.
[0021] The content of large-diameter particles in the resin particles is preferably 5% by volume or more, more preferably 6% by volume or more, more preferably 7% by volume or more, more preferably 8% by volume or more, and more preferably 9% by volume or more. The content of large-diameter particles in the resin particles is preferably 20% by volume or less, more preferably 19% by volume or less, more preferably 18% by volume or less, more preferably 17% by volume or less, and more preferably 16% by volume or less.
[0022] Furthermore, in the resin particles of the present invention, among medium-sized particles (hereinafter sometimes simply referred to as "medium-sized particles") having a particle diameter that is 1.0 times or more and less than 1.6 times the volume average particle diameter of all the resin particles, in any 10 medium-sized particles having hollow portions therein, the average number of medium-sized hollow portions (hereinafter sometimes simply referred to as "medium-sized hollow portions") having a major axis that is 0.05 times or more the particle diameter of the medium-sized particles is preferably 5 or less, more preferably 4 or less, and even more preferably 3 or less.
[0023] By setting the average number of medium-sized hollow portions among any 10 medium-sized particles having hollow portions to 5 or less, adverse effects on optical properties, color tone, adhesiveness, etc., during use of the resin particles can be prevented or reduced, making the resin particles more suitable for various purposes. Furthermore, the strength and specific gravity of the resin particles can be made approximately uniform, and the homogenization of other components into which the resin particles are mixed can also be improved.
[0024] The content of medium-sized particles in the resin particles is preferably 15% by volume or more, more preferably 17% by volume or more, more preferably 19% by volume or more, more preferably 21% by volume or more, and more preferably 23% by volume or more. The content of medium-sized particles in the resin particles is preferably 50% by volume or less, more preferably 45% by volume or less, more preferably 40% by volume or less, more preferably 35% by volume or less, and more preferably 30% by volume or less.
[0025] Here, the volume average particle size of the resin particles refers to a value measured as follows. The volume average particle size and coefficient of variation (CV value) of the resin particles are measured using a measuring device commercially available from Beckman Coulter, Inc. under the trade name "Coulter Multisizer III." The measurement is performed using an aperture calibrated in accordance with the Multisizer™ 3 user's manual published by Beckman Coulter, Inc.
[0026] The aperture used for measurement is selected appropriately by selecting an aperture having a size of 50 μm when the assumed volume average particle diameter of the resin particles to be measured is 1 μm or more and 10 μm or less, selecting an aperture having a size of 100 μm when the assumed volume average particle diameter of the resin particles to be measured is more than 10 μm and 30 μm or less, or selecting an aperture having a size of 280 μm when the assumed volume average particle diameter of the resin particles is more than 30 μm and 90 μm or less. If the volume average particle diameter after measurement differs from the assumed volume average particle diameter, change to an aperture having an appropriate size and perform the measurement again.
[0027] Furthermore, when an aperture having a size of 50 μm is selected, Current (aperture current) is set to −800 and Gain is set to 4; when an aperture having a size of 100 μm is selected, Current (aperture current) is set to −1600 and Gain is set to 2; and when apertures having sizes of 280 μm and 400 μm are selected, Current (aperture current) is set to −3200 and Gain is set to 1.
[0028] The measurement sample is prepared by dispersing 0.1 g of resin particles in 10 mL of a 0.1% by mass aqueous solution of a nonionic surfactant (manufactured by Kao Corporation, trade name "Pelex SS-H") using a touch mixer (manufactured by Yamato Scientific Co., Ltd., "TOUCHMIXER MT-31") and an ultrasonic cleaner (manufactured by Velvoclear, "ULTRASONIC CLEANER VS-150") to prepare a dispersion.
[0029] A beaker filled with ISOTON (registered trademark) II (measurement electrolyte manufactured by Beckman Coulter) is placed in the measuring section of a Coulter Multisizer III, and while gently stirring the contents of the beaker, the dispersion liquid is dropped into the beaker. After the reading of the densitometer on the Coulter Multisizer III main unit screen is adjusted to 5-10%, measurement is initiated. During measurement, the contents of the beaker are gently stirred to prevent air bubbles from being introduced, and measurement is terminated when 100,000 resin particles have been measured. The volume-average particle diameter of the resin particles is the arithmetic mean value in the particle size distribution based on the volume of 100,000 particles. The coefficient of variation (CV value) is a value calculated from formula (1) and represents the distribution width of the data. Coefficient of variation (CV value) (%) = standard deviation × 100 / (volume-average particle diameter of primary particles) (1)
[0030] The average number of large hollow portions among any 10 large hollow particles is a value measured in the following manner. Large particles are randomly selected from large particles having a particle diameter 1.6 to 4.0 times the volume average particle diameter of all resin particles. The large particles are cut in half from the center. The procedure for cutting large particles in half from the center is as follows. When a large particle is projected, the cutting line is formed by connecting points on the surface of the large particle that form the outline of the projection in the direction in which the area of the projection of the large particle is maximized. The large particles can be cut along this cutting line.
[0031] After processing the large diameter particles using a sample cross-section preparation device (manufactured by JEOL Ltd., product name "IB-19500CP"), the cross-section of the large diameter particle is observed using a scanning electron microscope (SEM) (manufactured by Hitachi High-Tech Corporation, product name "SU-3800") at a magnification of 500 to 1000 times. If a hollow portion is observed, the large diameter particle is extracted as the particle to be measured. The shape of the hollow portion is not particularly limited, and may be, for example, spherical, spindle-shaped, needle-shaped, or irregularly shaped.
[0032] The particle size of the large-diameter particles is measured based on the cross section of the large-diameter particles using a measurement system (trade name "SEM Data Manager" manufactured by Hitachi High-Technologies Corporation). The diameter of the large-diameter particles is the smallest diameter of a perfect circle that can enclose the cross section of the obtained large-diameter particles.
[0033] The major axis of the hollow portion is measured using a measurement system (manufactured by Hitachi High-Tech Corporation under the trade name "SEM Data Manager"). The major axis of the hollow portion is the diameter of the smallest circle that can enclose the hollow portion. When multiple hollow portions exist in a large-diameter particle, the major axis of each hollow portion is measured.
[0034] Based on the major axis of the obtained hollow portion and the particle diameter of the large-diameter particle containing this hollow portion, it is determined whether the hollow portion is 0.05 times or more the particle diameter of the large-diameter particle, and if it is 0.05 times or more, the hollow portion is determined to be a large-diameter hollow portion.
[0035] The above procedure is repeated until the total number of measured particles reaches 10. When the total number of measured particles reaches 10, the procedure is stopped and the total number of large diameter hollow portions among the 10 measured particles is calculated. If multiple large diameter hollow portions are formed in one large diameter particle, each large diameter hollow portion is counted as one large diameter hollow portion. The above procedure is considered as one measurement routine, and the measurement routine is repeated 10 times, and the average number of large diameter hollow portions per measured particle is calculated for each measurement routine. The average number of large diameter hollow portions per measured particle for each measurement routine is arithmetically averaged, and the obtained value is the average number of large diameter hollow portions.
[0036] The procedure for measuring the average number of medium-diameter hollow portions among any 10 medium-diameter particles having hollow portions is carried out by replacing, in the procedure for measuring the average number of large-diameter hollow portions described above, "large-diameter particles are arbitrarily extracted from large-diameter particles having a particle diameter of 1.6 to 4.0 times the volume average particle diameter of all the resin particles" with "medium-diameter particles are arbitrarily extracted from medium-diameter particles having a particle diameter of 1.0 times or more and less than 1.6 times the volume average particle diameter of all the resin particles," and by replacing "large-diameter particles" and "large-diameter hollow portions" with "medium-diameter particles" and "medium-diameter hollow portions," respectively.
[0037] The contents of large and medium-sized particles in the resin particles are determined by calculating the content V1 (volume %) of particles having a particle diameter of 4.0 times or less the volume average particle diameter, the content V2 (volume %) of particles having a particle diameter of less than 1.6 times the volume average particle diameter, and the content V3 (volume %) of particles having a particle diameter of less than 1.0 times the volume average particle diameter in the volume-based cumulative distribution measured as described above. The contents of large and medium-sized particles in the resin particles are calculated based on the following formulas: Content (volume %) of large particles = V1 - V2 Content (volume %) of medium-sized particles = V2 - V3
[0038] The volume average particle diameter of the resin particles is preferably 5 μm or more, more preferably 8 μm or more, and more preferably 10 μm or more. The volume average particle diameter of the resin particles is preferably 300 μm or less, more preferably 250 μm or less, and more preferably 200 μm or less. When the volume average particle diameter of the resin particles is within the above range, the effects of the resin particles can be more effectively exhibited.
[0039] When resin particles are used in a hot melt material, the volume average particle diameter of the resin particles is preferably 5 μm or more, more preferably 8 μm or more, and more preferably 10 μm or more. The volume average particle diameter of the resin particles is preferably 300 μm or less, more preferably 250 μm or less, and more preferably 200 μm or less. When the volume average particle diameter of the resin particles is 5 μm or more, the adhesiveness of the hot melt material is improved. When the volume average particle diameter of the resin particles is 300 μm or less, the resin particles can be sufficiently melted when the hot melt material is melted, thereby improving the adhesiveness to the adherend.
[0040] When resin particles are contained in a paint, the volume average particle diameter of the resin particles is preferably 5 μm or more, more preferably 8 μm or more. The volume average particle diameter of the resin particles is preferably 100 μm or less, more preferably 75 μm or less, and more preferably 50 μm or less. When the volume average particle diameter of the resin particles is 5 μm or more, the effect of the resin particles (for example, a matte effect) can be effectively exhibited in the coating film formed from the paint. When the volume average particle diameter of the resin particles is 100 μm or less, the effect of the resin particles (for example, a matte effect) can be effectively exhibited in the coating film formed from the paint.
[0041] When the resin particles are contained in a synthetic resin to form a resin composition, the volume average particle diameter of the resin particles is preferably 5 μm or more, more preferably 8 μm or more, and more preferably 10 μm or more, and is preferably 100 μm or less, more preferably 75 μm or less, and more preferably 50 μm or less.
[0042] The coefficient of variation (CV value) of the resin particles may be adjusted appropriately depending on the application of the resin particles, and is preferably 80% or less, and more preferably 70% or less.
[0043] The circularity of the resin particles is preferably 0.80 or more, more preferably 0.85 or more, and even more preferably 0.90 or more, from the viewpoint of light diffusibility or flowability.
[0044] The circularity of the resin particles refers to a value measured as follows: The circularity of the resin particles is measured using a flow particle image analyzer (manufactured by Sysmex Corporation, product name "FPIA (registered trademark)-3000S").
[0045] Specifically, 0.2 g of resin particles to be measured was added to 20 mL of a 0.25% by mass aqueous solution of sodium dodecylbenzenesulfonate, and ultrasonic waves were applied for 5 minutes using a BRANSON ultrasonic disperser, "BRANSON SONIFIER 450" (output: 400 W, frequency: 20 kHz), manufactured by BRANSON, to disperse the resin particles in the aqueous solution of sodium dodecylbenzenesulfonate, preparing a dispersion for measurement. For measurement, the flow particle image analyzer equipped with a standard objective lens (10x magnification) was used, and Particle Sheath (manufactured by Sysmex Corporation, trade name "PSE-900A") was used as the sheath liquid for the flow particle image analyzer. The dispersion for measurement prepared according to the above procedure was introduced into the flow particle image analyzer, and measurement was performed under the following measurement conditions. Before starting the measurement, the flow particle image analyzer is automatically focused using a suspension of standard polymer particles [for example, ThermoFisher Scientific's "5200A" (standard polystyrene particles diluted with ion-exchange water)]. The circularity is calculated by dividing the perimeter calculated from the diameter of a perfect circle having the same projected area as the image of the resin particle by the perimeter of the image of the resin particle. Measurement mode: HPF mode; Particle diameter measurement range: 0.996 to 200 μm; Particle circularity measurement range: 0.5 to 1.0; Number of particles measured: 1,000
[0046] The content of coarse particles having a particle diameter 20 times or more the volume average particle diameter of the resin particles is preferably 20% by mass or less, more preferably 15% by mass or less, and even more preferably 10% by mass or less. When the content of coarse particles is 20% by mass or less, the content of coarse particles, which tend to have large hollow spaces inside, is reduced, thereby reducing the total volume of hollow spaces formed within the entire resin particles and also reducing the amount of emulsifier and air remaining in the hollow spaces formed in the resin particles. Therefore, when the resin particles are used, adverse effects on optical properties, color tone, adhesiveness, etc. are more effectively prevented or reduced, and the resin particles can be used more suitably for various purposes.
[0047] The content of coarse particles having a particle diameter of 20 times or more the volume average particle diameter of the resin particles refers to the weight value after passing the obtained resin particle-containing dispersion through a metal mesh having mesh openings closest to 20 times the volume average particle diameter, washing and removing the emulsifier from the coarse particles remaining on the metal mesh, and drying.
[0048] [Method for Producing Resin Particles] A method for producing resin particles will be described. The method for producing resin particles is not particularly limited. As a method for producing resin particles, for example, a production method including a step of supplying and mixing polybutylene succinate, polyvinyl alcohol having a saponification degree of 60 to 85 mol %, and an electrolyte into water to prepare a raw material solution, stirring the raw material solution at a heating temperature of 120°C or higher to emulsify and disperse the polybutylene succinate in water to prepare a dispersion (dispersion step), and a step of cooling the obtained dispersion to produce resin particles containing polybutylene succinate (cooling step) is preferably used.
[0049] In the dispersion step, when dispersing polybutylene succinate in water, the polybutylene succinate is emulsified and dispersed in water using polyvinyl alcohol having a saponification degree of 60 to 85 mol % at a heating temperature of 120° C. or higher. The "heating temperature" refers to the temperature of a raw material solution containing polybutylene succinate, polyvinyl alcohol, an electrolyte, and water.
[0050] In the dispersion step, polybutylene succinate is emulsified and dispersed in water at a heating temperature of 120°C or higher. The polybutylene succinate is heated in water to melt or soften and become fluid droplets. Polyvinyl alcohol is adsorbed onto the surface of these droplet-like polybutylene succinate. Note that the term "droplet-like" includes not only a liquid state but also a softened state with fluidity.
[0051] By using polyvinyl alcohol having a degree of saponification of 60 to 85 mol %, good dispersibility of polyvinyl alcohol in water is ensured, while the excellent adsorptive power of polyvinyl alcohol on the surface of polybutylene succinate droplets stabilizes the polybutylene succinate droplets, and the size of the polybutylene succinate droplets is controlled to an appropriate size.
[0052] The saponification degree of polyvinyl alcohol is preferably 60 mol% or more, more preferably 62 mol% or more, more preferably 65 mol% or more, and more preferably 67 mol% or more. The saponification degree of polyvinyl alcohol is preferably 85 mol% or less, more preferably 83 mol% or less, more preferably 80 mol% or less, and more preferably 78 mol% or less. When the saponification degree of polyvinyl alcohol is 60 mol% or more, it can be more uniformly adsorbed onto the surface of polybutylene succinate droplets, the droplet size of polybutylene succinate can be controlled to an appropriate size, and resin particles with fewer coarse particles can be produced. When the saponification degree of polyvinyl alcohol is 85 mol% or less, the adsorption property of polybutylene succinate to the droplet surface can be improved, the droplet size of polybutylene succinate can be controlled to an appropriate size, and resin particles with fewer coarse particles can be produced. The degree of saponification of polyvinyl alcohol refers to the mol % of --OAc (--OCOCH3) in polyvinyl acetate that has been converted to --OH.
[0053] The degree of polymerization of polyvinyl alcohol is preferably 300 or more, more preferably 500 or more, and more preferably 600 or more. The degree of polymerization of polyvinyl alcohol is preferably 3000 or less, more preferably 2700 or less, and more preferably 2500 or less. When the degree of polymerization of polyvinyl alcohol is 300 or more, the adsorption of polybutylene succinate to the droplet surface is improved, the coalescence of polybutylene succinate droplets is reduced, and resin particles with fewer coarse particles can be produced. When the degree of polymerization of polyvinyl alcohol is 3000 or less, the absorption of water containing polyvinyl alcohol into the interior of polybutylene succinate droplets can be reduced, making it difficult for hollow portions to be formed within the resin particles.
[0054] The viscosity of a 4% by mass aqueous solution of polyvinyl alcohol at 20°C is preferably 3.0 mPa·s or more, more preferably 3.5 mPa·s or more, and more preferably 4.0 mPa·s or more. The viscosity of a 4% by mass aqueous solution of polyvinyl alcohol at 20°C is preferably 20.0 mPa·s or less, more preferably 18.0 mPa·s or less, and more preferably 16.0 mPa·s or less. A viscosity of 3.0 mPa·s or more reduces the coalescence of polybutylene succinate droplets, making it possible to produce resin particles with fewer coarse particles. A viscosity of 20.0 mPa·s or less improves dispersibility in water, allowing for more uniform adsorption on the surface of polybutylene succinate droplets, making the polybutylene succinate droplet size appropriate, and making it possible to produce resin particles with fewer coarse particles. The viscosity of a 4% by mass aqueous solution of polyvinyl alcohol at 20°C refers to a value measured in accordance with JIS K9550:2020.
[0055] In the dispersion step, the amount of polyvinyl alcohol used is preferably 5 parts by mass or more, more preferably 10 parts by mass or more, and more preferably 15 parts by mass or more, per 100 parts by mass of polybutylene succinate. In the dispersion step, the amount of polyvinyl alcohol used is preferably 50 parts by mass or less, more preferably 40 parts by mass or less, and more preferably 30 parts by mass or less, per 100 parts by mass of polybutylene succinate. When the amount of polyvinyl alcohol used is 5 parts by mass or more, the droplet size of polybutylene succinate can be controlled to an appropriate size, resin particles with fewer coarse particles can be produced, and resin particles can be produced without using an organic solvent, thereby reducing the environmental burden. When the amount of polyvinyl alcohol used is 50 parts by mass or less, polyvinyl alcohol is incorporated into the droplets, reducing the amount of polyvinyl alcohol remaining inside the resin particles.
[0056] In the dispersion process, a raw material solution in which polybutylene succinate is dispersed in water is stirred in a stirring vessel, and polybutylene succinate droplets collide with each other, coalesce, and grow. During this growth process, polybutylene succinate droplets may coalesce while incorporating water containing polyvinyl alcohol. The polybutylene succinate droplets are then cooled and dried to form resin particles. At this time, if polyvinyl alcohol and water are incorporated into the droplets, hollow portions are formed in the resin particles due to evaporation of the incorporated water, and the polyvinyl alcohol incorporated together with the water remains in these hollow portions.
[0057] Therefore, in the above-mentioned method for producing resin particles, polybutylene succinate is emulsified and dispersed in water in the presence of an electrolyte. When the droplets absorb water containing polyvinyl alcohol, the difference in osmotic pressure caused by the electrolyte attracts more water into the droplets, increasing the amount of water inside the droplets. As a result, the droplets burst due to the water absorbed inside them, expelling the water and eliminating the pool of water inside the droplets. The action of the electrolyte reduces the amount of water and polyvinyl alcohol absorbed into the droplets, making it difficult for hollows to form in the resin particles. Even if hollows do form, they can be kept small.
[0058] Furthermore, in the above-described resin particle manufacturing method, polyvinyl alcohol is used to control the size of polybutylene succinate droplets to an appropriate size, thereby reducing the generation of coarse droplets. While larger droplets tend to absorb water more easily, controlling the droplet size to an appropriate size makes it difficult for the droplets to absorb water, and the action of the electrolyte also causes the droplets to expel any water they may have absorbed. Therefore, the synergistic effect of polyvinyl alcohol and the electrolyte allows for the easy production of resin particles with fewer coarse particles and reduced hollow spaces within.
[0059] The electrolyte is not particularly limited, and examples thereof include metal halides [for example, alkali metal halide salts such as sodium halides (e.g., sodium chloride, sodium fluoride, sodium bromide) and potassium halides (e.g., potassium chloride, potassium fluoride, potassium bromide); alkaline earth metal halide salts such as magnesium halides (e.g., magnesium chloride, magnesium fluoride, magnesium bromide), calcium halides (e.g., calcium chloride, calcium fluoride, calcium bromide), and barium halides (e.g., barium chloride, barium fluoride, barium bromide)], metal salts of organic acids (e.g., sodium phthalate, potassium phthalate), Examples of suitable electrolytes include ammonium salts of organic acids (e.g., ammonium phthalate, ammonium succinate, ammonium adipate, ammonium citrate, ammonium tartrate), sulfates (e.g., sodium sulfate, potassium sulfate), and nitrates (e.g., sodium nitrate, potassium nitrate). Metal halides, metal salts of organic acids, sulfates, and nitrates are preferred, and alkali metal halide salts, metal salts of polycarboxylic acids, alkali metal sulfates, and alkali metal nitrates are more preferred. The electrolytes may be used alone or in combination of two or more. Regarding the metal salts of organic acids, when the organic acid is a polycarboxylic acid, it is sufficient that at least one carboxy group of the carboxy groups (—COOH) forms a salt, and it is not necessary that all carboxy groups form salts.
[0060] In the dispersion step, the amount of electrolyte used is preferably 0.05 parts by mass or more, more preferably 0.10 parts by mass or more, and more preferably 0.15 parts by mass or more, per 100 parts by mass of polybutylene succinate. In the dispersion step, the amount of electrolyte used is preferably 5.0 parts by mass or less, more preferably 3.0 parts by mass or less, and more preferably 1.0 parts by mass or less, per 100 parts by mass of polybutylene succinate. When the amount of electrolyte used is within the above range, the formation of hollow spaces within the resin particles can be reduced, or even if hollow spaces are formed, the size of the hollow spaces can be reduced. Furthermore, when the amount of electrolyte used is 5.0 parts by mass or less, the droplet size of polybutylene succinate can be controlled to an appropriate size without inhibiting the above-mentioned effect of polyvinyl alcohol, and resin particles with few coarse particles can be produced.
[0061] In the present invention, when the electrolyte is present in a hydrated state, the amount of the electrolyte used refers to the mass of the electrolyte calculated as an anhydrous form. The "mass of the electrolyte calculated as an anhydrous form" refers to the mass of the electrolyte in a dry state that does not contain any water (crystal water).
[0062] In the dispersion step, the amount of water used is preferably 100 parts by mass or more, more preferably 150 parts by mass or more, and more preferably 200 parts by mass or more, per 100 parts by mass of polybutylene succinate. The amount of water used is preferably 2200 parts by mass or less, more preferably 1000 parts by mass or less, and more preferably 800 parts by mass or less, per 100 parts by mass of polybutylene succinate. When the amount of water used is 100 parts by mass or more, the polybutylene succinate can be thoroughly stirred to fully utilize the effects of the polyvinyl alcohol and the electrolyte, reducing the generation of hollow spaces and producing resin particles with fewer coarse particles. When the amount of water used is 2200 parts by mass or less, production efficiency can be improved.
[0063] In the dispersion step, a water-soluble polymer other than polyvinyl alcohol may be added to the raw material solution. By adding a water-soluble polymer to the water, the water-soluble polymer is adsorbed onto the surface of the polybutylene succinate droplets, thereby stabilizing the polybutylene succinate droplets and controlling the polybutylene succinate droplets to an appropriate size.
[0064] The water-soluble polymer is not particularly limited, and examples thereof include hydroxypropyl cellulose, hydroxypropylmethyl cellulose, methyl cellulose, ethyl cellulose, ethylmethyl cellulose, hydroxyethyl cellulose, carboxymethyl cellulose, carboxyethyl cellulose, polyvinylpyrrolidone, etc. The water-soluble polymers may be used alone or in combination of two or more.
[0065] In the dispersion step, a surfactant may be added to the water used to prepare the dispersion. The addition of a surfactant to the water is preferred because it serves as an auxiliary agent for adjusting the particle size of the resin particles. The surfactant may be any of anionic surfactants, cationic surfactants, nonionic surfactants, and zwitterionic surfactants. The surfactants may be used alone or in combination of two or more.
[0066] Examples of anionic surfactants include sodium oleate; fatty acid soaps such as castor oil potassium soap; alkyl sulfate ester salts such as sodium lauryl sulfate and ammonium lauryl sulfate; alkyl benzene sulfonates such as sodium dodecylbenzene sulfonate; alkyl naphthalene sulfonates; alkanesulfonates; dialkyl sulfosuccinates; alkyl phosphate ester salts; naphthalene sulfonate formalin condensates; polyoxyethylene alkyl phenyl ether sulfate ester salts; polyoxyethylene sulfonated phenyl ether phosphate; and polyoxyethylene alkyl sulfate ester salts.
[0067] Examples of cationic surfactants include alkylamine salts such as laurylamine acetate and stearylamine acetate; and quaternary ammonium salts such as lauryltrimethylammonium chloride.
[0068] Examples of nonionic surfactants include (meth)acrylate sulfate ester surfactants (commercially available products include RMA-564, RMA-568, and RMA-1114 manufactured by Nippon Nyukazai Co., Ltd.), polyoxyalkylene branched decyl ethers, polyoxyethylene tridecyl ethers, polyoxyalkylene alkyl ethers, polyoxyalkylene tridecyl ethers, polyoxyethylene isodecyl ethers, polyoxyalkylene lauryl ethers, polyoxyalkylene alkyl ethers, polyether polyols, polyoxyethylene styrenated phenyl ethers, polyoxyethylene naphthyl ethers, polyoxyethylene phenyl ethers, polyoxyethylene polyoxypropylene glycols, polyoxyethylene lauryl ethers, polyoxyethylene oleyl cetyl ethers, polyoxyethylene glyceryl isostearate, polyoxyethylene alkyl ethers, polyoxyethylene alkylphenyl ethers, polyoxyethylene fatty acid esters, sorbitan fatty acid esters, polyoxysorbitan fatty acid esters, polyoxyethylene alkylamines, glycerin fatty acid esters, and oxyethylene-oxypropylene block polymers.
[0069] Commercially available nonionic reactive surfactants can be used. Examples of the nonionic reactive surfactant include alkyl ether surfactants (commercially available products include ADEKA REASOAP ER-10, ER-20, ER-30, and ER-40, and Kao LATEMURU PD-420, PD-430, and PD-450); and alkyl phenyl ether or alkyl phenyl ester surfactants (commercially available products include Aqualon RN-10, RN-20, RN-30, RN-50, AN-10, AN-20, AN-30, and AN-5065, and Adeka REASOAP NE-10, NE-20, NE-30, and NE-40, both of which are manufactured by Dai-ichi Kogyo Seiyaku Co., Ltd.).
[0070] In the dispersing step, the heating temperature at which polybutylene succinate is emulsified and dispersed in water to prepare a dispersion is preferably 120° C. or higher. In the dispersing step, the heating temperature at which polybutylene succinate is emulsified and dispersed in water to prepare a dispersion is preferably 180° C. or lower. When the heating temperature at which the dispersion is prepared is 120° C. or higher, the polybutylene succinate is sufficiently melted or softened, and droplets of polybutylene succinate are smoothly formed, allowing the effects of polyvinyl alcohol and the electrolyte to be fully exerted, thereby reducing the formation of hollow portions and enabling the production of resin particles with few coarse particles.
[0071] In the dispersion step, the time for stirring the raw material liquid containing polybutylene succinate, polyvinyl alcohol, an electrolyte, and water to emulsify and disperse is preferably 30 minutes or more, more preferably 45 minutes or more, and even more preferably 60 minutes or more. In the dispersion step, the upper limit of the time for stirring the raw material liquid containing polybutylene succinate, polyvinyl alcohol, an electrolyte, and water to emulsify and disperse is not particularly limited, but is preferably 3 hours or less from the viewpoint of production efficiency.
[0072] The dispersion produced in the dispersion step is cooled, and the polybutylene succinate droplets in the dispersion are cooled to produce resin particles, thereby obtaining a suspension containing the resin particles. The dispersion may be cooled to a temperature at which the polybutylene succinate solidifies, and is preferably cooled until the temperature of the dispersion reaches 20°C. The dispersion is preferably cooled while being stirred.
[0073] The dispersion is preferably cooled slowly because this allows for gradual crystallization and reduces aggregation of the resin particles. Specifically, the cooling rate of the dispersion is preferably 0.5 to 2.0°C / min, and more preferably 0.6 to 1.0°C / min.
[0074] The resin particles produced by cooling the dispersion are extracted through a known process of filtration, washing, dehydration, and drying. Specifically, polyvinyl alcohol, electrolyte, water, and other additives are separated or reduced from the suspension containing the resin particles to produce a cake containing the resin particles. The method for separating or reducing the polyvinyl alcohol and electrolyte from the suspension is not particularly limited, and examples thereof include suction filtration, centrifugation, and pressure separation.
[0075] Next, if necessary, the cake can be washed with an aqueous medium (e.g., water) and then dried to obtain resin particles. The method for washing the resin particles is not particularly limited, and examples include a method in which the cake is supplied to a centrifugal separator, an aqueous medium is supplied to the cake to wash the resin particles, and the aqueous medium after washing is removed by centrifugation.
[0076] After washing, the resin particles are dried, and in this drying process, the aqueous medium attached to the outer surface of the resin particles as well as the water incorporated therein are evaporated and removed. Hollow portions are formed by the evaporation of the water incorporated into the resin particles. However, as described above, the amount of water and polyvinyl alcohol incorporated into the polybutylene succinate droplets is reduced in the dispersion process. Therefore, after the resin particles are dried, the number of hollow portions formed within the resin particles is small, and in particular, the generation of large-diameter hollow portions is suppressed to a low level. Furthermore, the amount of polyvinyl alcohol incorporated into the polybutylene succinate droplets is also suppressed to a low level, so the amount of polyvinyl alcohol remaining in the resulting resin particles is also suppressed to a low level.
[0077] The obtained resin particles may be classified as necessary. The classification method of the resin particles is not particularly limited, and examples thereof include air classification, screen classification, and the like. Air classification refers to a method of classifying resin particles by utilizing an air flow. Screen classification refers to a method of supplying resin particles onto a screen and vibrating the screen to classify the resin particles on the screen into particles that pass through the meshes of the screen and particles that do not pass through.
[0078] The resin particles thus obtained are preferably stored as a packaged product sealed in a moisture-resistant packaging material so as not to absorb moisture in the air. The moisture-resistant packaging material is preferably a material having a water vapor permeability of 50 g / m 2 Packaging materials with a shelf life of 24 hours or less are preferred. Examples of such packaging materials include bags made of low-density polyethylene with a thickness of 50 to 150 μm, bags made of a vapor-deposited film in which a metal film is vapor-deposited on one side of a synthetic resin film, and bags made of a laminated film in which a metal film is laminated on one side of a synthetic resin film. The water vapor permeability refers to a value measured under conditions of a temperature of 40°C and a relative humidity of 90% using a water vapor transmission rate measuring device (manufactured by MOCON, USA, under the trade name "Permatran (registered trademark) W3 / 31") based on Method B (infrared sensor method) described in JIS K7129 (2000 edition).
[0079] [Uses of Resin Particles] As described above, the resin particles have a predetermined number of large-diameter hollow portions formed therein or less, so that the physical properties of the resin particles, such as strength and specific gravity, are substantially uniform, and even when the resin particles are contained in other materials for various uses, the materials containing the resin particles can be maintained substantially homogeneous. Furthermore, the materials using the resin particles can be maintained substantially homogeneous.
[0080] Furthermore, since the number of large-diameter hollow sections in the resin particles is set to a predetermined number or less, even when light passes through the resin particles, as described above, the proportion of large-diameter hollow sections formed within the resin particles is low, and there is almost no adverse effect from these large-diameter hollow sections and the emulsifier remaining in the large-diameter hollow sections, so the optical properties of other materials containing the resin particles are not impaired.
[0081] Furthermore, even in applications where the resin particles do not retain their particle shape due to dissolution during use, the amount of emulsifier remaining inside the resin particles is reduced, so there is almost no adverse effect from the emulsifier leaking out from the resin particles, and the properties of the material using the resin particles are not impaired.
[0082] Therefore, the resin particles can be used by being contained in, for example, external preparations such as quasi-drugs, hot melt materials, cosmetics, matting agents for paints, paints such as powder paints, rheology modifiers, antiblocking agents, slip imparting agents, light diffusing agents, additives for sintering and molding fine ceramics, fillers for adhesives, medical diagnostic testing agents, automotive materials, and building materials. The resin particles may also be contained in a synthetic resin to form a resin composition, and this resin composition may be used to mold a molded article. The resin particles may also be used as a hot melt material.
[0083] The resin particles are preferably used by being contained in external preparations such as quasi-drugs, hot melt materials, cosmetics, matting agents for paints, paints, and anti-blocking agents for packaging materials for food and drink.
[0084] The resin particles of the present invention have a predetermined number of large-diameter hollow portions or less, and the physical properties such as strength and specific gravity of each resin particle are formed to be approximately uniform.By uniformly mixing the resin particles with other components that contain the resin particles, a homogeneous component containing the resin particles can be obtained.
[0085] Since the resin particles of the present invention have a predetermined number of large-diameter hollow portions or less, the optical properties of light incident on the resin particles are not substantially changed even when the light is transmitted through or reflected by the resin particles, and therefore the resin particles of the present invention can be suitably used for optical applications.
[0086] Since the resin particles of the present invention have a reduced number of large hollow spaces formed therein, the amount of emulsifier remaining in the large hollow spaces can also be reduced. Even if the shape of the resin particles is lost during use, the amount of emulsifier leaking out from the resin particles is also reduced. This reduces the effect of the remaining emulsifier in applications using the resin particles, allowing the resin particles to be used suitably in their intended applications.
[0087] The present invention will be described in more detail below using examples, but the present invention is not limited thereto. Specific numerical values of the blending ratios (content ratios), physical property values, parameters, etc. used in the following description can be replaced with the upper limit values (numeric values defined as "equal to or less than") or lower limit values (numeric values defined as "equal to or more than" or "exceeding") of the corresponding blending ratios (content ratios), physical property values, parameters, etc. described in the "Summary of the Invention."
[0088] The following compounds were used in the examples and comparative examples: [Polybutylene succinate] Polybutylene succinate (manufactured by Mitsubishi Chemical Corporation, trade name "BioPBS FZ71PM", raw material monomers containing monomers derived from non-petroleum raw materials)
[0089] [Polyvinyl alcohol] Polyvinyl alcohol 1 (manufactured by Denka Company, trade name "Denka Poval MP-10R", degree of saponification: 70.5 to 74.5 mol%, viscosity of a 4 mass% aqueous solution at 20°C: 6.0 to 9.0 mPa·s, degree of polymerization: 900) Polyvinyl alcohol 2 (manufactured by Mitsubishi Chemical Corporation, trade name "Gohsenol GM-14L", degree of saponification: 86.5 to 89.0 mol%, viscosity of a 4 mass% aqueous solution at 20°C: 20.5 to 24.5 mPa·s, degree of polymerization: 1500) Polyvinyl alcohol 3 (manufactured by Mitsubishi Chemical Corporation, trade name "Gohsenol GL-05", degree of saponification: 86.5 to 89.0 mol%, viscosity of a 4 mass% aqueous solution at 20°C: 4.8 to 5.8 mPa·s, degree of polymerization: 600)
[0090] [Electrolytes] Sodium chloride Sodium sulfate Disodium succinate hexahydrate
[0091] (Examples 1 to 4, Comparative Examples 1 to 3) A predetermined amount of ion-exchanged water and polyvinyl alcohol as an emulsifier shown in Table 1 were charged into a stirrer equipped with a stirrer, a thermometer, and a cooling mechanism to prepare an aqueous polyvinyl alcohol solution.
[0092] Next, the polybutylene succinate and electrolyte in the predetermined amounts shown in Table 1 were charged into a stirrer to prepare a raw material solution. The raw material solution was stirred at a heating temperature of 120°C for 60 minutes to emulsify and disperse the polybutylene succinate in water to prepare a dispersion. In Table 1, the amount of disodium succinate hexahydrate charged into the stirrer is shown as the mass of disodium succinate converted into anhydrous form.
[0093] The dispersion was then cooled at a rate of 0.75°C / min until its temperature reached 30°C, producing resin particles containing polybutylene succinate, and a suspension containing the resin particles was prepared. The resin particles were separated from the resulting suspension using a centrifuge (manufactured by Tanabe Willtec Co., Ltd.). The resin particles were washed with ion-exchanged water.
[0094] The resulting resin particles were then dried for 20 hours at 60°C under a vacuum of 0.05 MPa, and then classified using a classifier equipped with a screen having a mesh size of 100 µm (manufactured by Toyo Hightec Co., Ltd., product name "Hibolter NR300") in an air atmosphere at a relative humidity of 20% to obtain resin particles.
[0095] The volume average particle size and coefficient of variation (CV value) of the resulting resin particles were measured in the same manner as above, and the results are shown in Table 1.
[0096] The average number of large-diameter hollow portions in 10 randomly selected large-diameter particles having hollow portions therein was measured in the same manner as described above. The results are shown in Table 1.
[0097] Of the resulting resin particles, the average number of hollow portions in any 10 medium-sized particles having hollow portions therein was measured in the same manner as described above. The results are shown in Table 1.
[0098] The content of coarse particles having a particle size 20 times or more the volume average particle size of the resin particles was measured for the obtained resin particles in the same manner as described above. The results are shown in Table 1.
[0099] The contents of large and medium diameter particles in the obtained resin particles were measured in the same manner as described above, and the results are shown in Table 1.
[0100]
[0101] (Cross-reference to related applications) This application claims priority based on Japanese Patent Application No. 2023-55854, filed on March 30, 2023, the disclosure of which is incorporated herein by reference in its entirety.
[0102] The resin particles of the present invention can be uniformly mixed with another component containing the resin particles to obtain a homogeneous component containing the resin particles.
[0103] The resin particles of the present invention do not substantially change the optical properties of light incident on the resin particles, and therefore can be suitably used in optical applications.
[0104] The resin particles of the present invention can reduce the amount of emulsifier that flows out from the resin particles even if the shape of the resin particles disappears during use.
[0105] Therefore, the resin particles of the present invention can be suitably used for applications such as topical agents, hot melt materials, cosmetics, matting agents for paints, paints such as powder paints, rheology modifiers, antiblocking agents, slip imparting agents, light diffusing agents, additives for sintering and molding fine ceramics, fillers for adhesives, medical diagnostic testing agents, automotive materials, building materials, and molding materials.
Claims
1. Resin particles containing polybutylene succinate, characterized in that, among large-diameter particles having a particle diameter 1.6 to 4.0 times the volume average particle diameter of the resin particles, any 10 large-diameter particles having hollow portions therein have an average number of large-diameter hollow portions having a major axis of 0.05 times or more the particle diameter of each large-diameter particle of 10 or less.
2. The resin particles described in claim 1, characterized in that, among medium-sized particles having a particle diameter that is 1.0 times or more and less than 1.6 times the volume average particle diameter of the resin particles, in any 10 medium-sized particles having hollow portions therein, the average number of medium-sized hollow portions having a major axis that is 0.05 times or more the particle diameter of each medium-sized particle is 5 or less.
3. The resin particles according to claim 1 or 2, characterized in that the volume average particle diameter of the resin particles is 5 to 300 μm.
4. Resin particles according to claim 1 or 2, characterized in that the content of coarse particles having a particle diameter 20 times or more the volume average particle diameter of the resin particles is 20 mass % or less.
5. A method for producing resin particles, comprising: a dispersing step of mixing polybutylene succinate, polyvinyl alcohol having a degree of saponification of 60 to 85 mol%, an electrolyte and water, and emulsifying and dispersing the polybutylene succinate in water at a heating temperature of 120°C or higher to produce a dispersion; and a cooling step of cooling the dispersion to produce resin particles containing polybutylene succinate.
6. The method for producing resin particles described in claim 5, characterized in that the polyvinyl alcohol has a viscosity of 3.0 to 20.0 mPa·s in a 4% by weight aqueous solution at 20°C.
7. The method for producing resin particles according to claim 5 or 6, characterized in that in the dispersion step, 100 parts by weight of water and 15 to 50 parts by weight of polyvinyl alcohol are mixed.
8. A method for producing resin particles as described in claim 5 or 6, characterized in that the electrolyte contains at least one electrolyte selected from the group consisting of metal halides, metal salts of organic acids, ammonium salts of organic acids, sulfates, and nitrates.
9. A hot melt material comprising the resin particles according to claim 1 or 2.
10. A paint comprising the resin particles according to claim 1 or 2.
11. A resin composition comprising the resin particles according to claim 1 or 2.
Citation Information
Patent Citations
Powder coating
JP1997302306A
Sunglasses
JP1999183854A
Aliphatic polyester resin powder suitable for selective laser sintering and method for preparing the same
JP2018532853A
Resin particles and method for producing the same
JP2022161001A
Three-dimensional molding material excellent in biodegradability and molded product thereof
JP2023037365A