Coil structure and method for manufacturing same, multilayer substrate circuit using coil structure, magnetic device, and copper foil with resin for coil structure

The use of a resin-based insulating material without glass cloth in coil structures addresses the limitations of conventional magnetic devices, enabling high-capacity and high-frequency applications with improved insulation and reduced capacitance.

WO2024204737A1PCT designated stage expired Publication Date: 2024-10-03TAMURA KK

Patent Information

Application Number
PCT/JP2024/013098
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-29
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Conventional magnetic devices using glass cloth substrates face limitations in high voltage, high frequency, and large capacity applications due to insufficient insulation and increased parasitic capacitance.

Method used

A coil structure with a flat conductor and insulating material, where the insulating material is a cured product of an insulating resin composition without glass cloth, featuring high withstand voltage and low dielectric constant, and including epoxy resin, polyamide, polyimide, and phenoxy resins, is used, along with a method of laminating resin-coated copper foil and forming a multilayer circuit board.

Benefits of technology

This configuration enables magnetic devices with excellent withstand voltage characteristics and low capacitance, allowing for thin, high-capacity, and high-frequency applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024013098_03102024_PF_FP_ABST
    Figure JP2024013098_03102024_PF_FP_ABST
Patent Text Reader

Abstract

Provide are a coil structure, a multilayer circuit board, and a magnetic device with which it is possible to achieve excellent withstand voltage characteristics and low capacitance between coils without using a glass cloth. A coil structure C comprises: coil patterns 21, 22, 23 which are planar conductors each wound on a plane; and an insulating material 1 for providing insulation between the coil patterns 21, 22, 23. The coil patterns 21, 22, 23 and the insulating material 1 are alternately laminated. The insulating material 1 is a cured product of an insulating resin composition that does not contain glass cloth. A multilayer circuit board P includes the coil structure C. A magnetic device D is constituted by laminating a plurality of the coil structures C and the multilayer circuit boards P, and mounting a core 4 thereon.
Need to check novelty before this filing date? Find Prior Art

Description

Coil structure and manufacturing method thereof, multilayer substrate circuit using coil structure, magnetic device, and resin-coated copper foil for coil structure

[0001] The present invention relates to a coil structure used in a magnetic device such as a transformer configured by stacking coils, a manufacturing method thereof, and a multilayer substrate circuit using the coil structure. The present invention also relates to a magnetic device employing the coil structure or the multilayer substrate circuit, and a resin-coated copper foil for the coil structure.

[0002] For example, as shown in Patent Document 1, a laminated printed coil has been known as a thin transformer used in switching power supplies, etc. This printed coil (1) uses a cloth made of glass fiber (called glass cloth) as a base material, (2) the base material is impregnated with and solidified by epoxy resin to form a substrate, (3) a spiral planar coil is formed on the front and back surfaces of the substrate by printing or pasting, and (4) a heat-resistant resin is applied to the surface of the planar coil to ensure its insulation.

[0003] Japanese Patent Application Publication No. 9-326316

[0004] However, because the above-mentioned conventional technology uses a substrate (commonly called prepreg) formed by impregnating and solidifying epoxy resin into glass cloth, simply making conventional magnetic devices thinner poses the problem of being unable to use them for large capacity, high voltage, or high frequency applications due to insufficient insulation between laminations and increased parasitic capacitance.

[0005] The present invention has been proposed to solve the problems of the prior art as described above. An object of the present invention is to provide a coil structure, a multilayer circuit board, and a magnetic device that achieve excellent voltage resistance characteristics and low capacitance between coils without using glass cloth.

[0006] The coil structure of the present invention is characterized by having a flat conductor wound on a plane and an insulating material that provides insulation between the conductors, the conductors and the insulating material being alternately laminated, and the insulating material being a cured product of an insulating resin composition that does not contain glass cloth.

[0007] In the present invention, the following configurations can be adopted. (1) The insulating resin composition has a withstand voltage of 100 kV / mm or more and a dielectric constant of 4.0 or less. (2) The insulating resin composition has adhesive properties. (3) The insulating resin composition contains an epoxy resin. (4) The insulating resin composition contains at least one of a polyamide resin, a polyimide resin, and a polyamideimide resin. (5) The insulating resin composition comprises (a1) a liquid epoxy resin, (a2) a solid epoxy resin having a softening point of 125°C or less, (b) an aromatic diamine compound having a benzoate group and a polymethylene group in the main chain, (c) a solvent-soluble polyimide resin having a Tg of 200°C or more and a weight-average molecular weight Mw of 50,000 or less, and (d) a phenoxy resin having a Tg of 130°C or more, and when the total amount of (a1) the liquid epoxy resin, (a2) the solid epoxy resin, and (b) the aromatic diamine compound is 100 parts by weight, the total amount of (c) the solvent-soluble polyimide resin and (d) the phenoxy resin is 15 parts by weight or more and 150 parts by weight or less. (6) The insulating resin composition is a polyimide derived from (A) an acid dianhydride and (B) a diamine, wherein the (A) acid anhydride includes (A1) an acid anhydride having an ester bond, and the (B) diamine includes (B1) a dimer diamine in an amount of 0.3 or more moles, where the total mole number of diamines is 1.0. (7) The insulating resin composition is a polyimide derived from (A) an acid dianhydride and (B) a diamine, wherein the (B) diamine includes (B1) a diamine having a fluorene skeleton and (B2) a dimer diamine.

[0008] The following configurations are also encompassed by the present invention. (1) A coil structure formed by multi-layering resin-coated copper foils in which the insulating resin composition is formed on one side of the copper foil. (2) A multi-layer circuit board including the coil structure. (3) The multi-layer circuit board in which a shielding layer is provided on the outermost layer or an intermediate layer. (4) A magnetic device in which a core is attached to the multi-layer circuit board. (5) A magnetic device in which a plurality of the multi-layer circuit boards are stacked and a core is attached. (6) A magnetic device in which a plurality of the coil structure and the multi-layer circuit boards are stacked and a core is attached. (7) A magnetic device having an operating frequency of 500 kHz to 1 MHz. (8) A resin-coated copper foil for a coil structure in which an insulating resin composition is formed on one side of copper foil, wherein a resin layer made of the insulating resin composition or an insulating resin composition different from the insulating resin composition in a semi-cured state is formed on the surface of the insulating resin composition of the resin-coated copper foil, and a protective film is laminated on the surface of the semi-cured resin layer. (9) A resin-coated copper foil for a coil structure, characterized in that a resin layer made of the insulating resin composition in a semi-cured state is formed on one side of a copper foil, and a protective film is laminated on the surface of the semi-cured resin layer. (10) A method for manufacturing a coil structure, characterized in that the resin-coated copper foil is laminated so that the semi-cured resin layer and the copper foil are in contact with each other with the protective film peeled off.

[0009] According to the present invention, since the insulating material between the coils is composed of a cured product of an insulating resin composition that does not contain glass cloth, it is possible to provide a coil structure, a multilayer circuit board and a magnetic device that enable large capacity, high frequency and thin thickness due to the high withstand voltage and low dielectric constant of the insulating resin composition, as well as a resin-coated copper foil for the coil structure.

[0010] 1A and 1B are diagrams showing the basic configuration of a magnetic device of the present invention, where (a) is a top view of a coil structure, (b) is a perspective view of a state in which a core is attached to the coil structure, and (c) is a cross-sectional view taken along line A-A' in (b). Cross-sectional views showing each step of a manufacturing method for the magnetic device of FIG. 1 are diagrams showing a first embodiment of a magnetic device of the present invention, where (a) is a perspective view and (b) is a cross-sectional view taken along line B-B' in (a). A second embodiment of a magnetic device of the present invention, where (a) is a perspective view and (b) is a cross-sectional view taken along line C-C' in (a). A third embodiment of a magnetic device of the present invention, where (a) is a perspective view and (b) is a cross-sectional view taken along line D-D' in (a). A fourth embodiment of a magnetic device of the present invention, where (a) is a perspective view and (b) is a cross-sectional view taken along line E-E' in (a). A fifth embodiment of a magnetic device of the present invention, where (a) is a perspective view and (b) is a cross-sectional view taken along line B-B' in (a). 10A and 10B are diagrams showing a sixth embodiment of the magnetic device of the present invention, in which (a) is a perspective view and (b) is a cross-sectional view taken along the line BB' in (a). 11A are cross-sectional views schematically showing a method for manufacturing a resin-coated copper foil according to a seventh embodiment. 12A are cross-sectional views schematically showing a method for manufacturing a resin-coated copper foil according to an eighth embodiment. 13A are cross-sectional views schematically showing a method for manufacturing a resin-coated copper foil according to a ninth embodiment.

[0011] 1 shows a basic embodiment of a magnetic device D of the present invention, where (a) is a top view of a coil structure, (b) is a perspective view of the coil structure with a core attached, and (c) is a cross-sectional view taken along line A-A' in (b). The magnetic device D of this embodiment is intended to be a multilayer transformer, and therefore has conductors made of primary coil patterns 21 and 22 and a secondary coil pattern 23 embedded at predetermined intervals within an insulating material 1 made of a cured product of an insulating resin composition, and the coil patterns 21, 22, and 23 are insulated from each other by the insulating material 1.

[0012] In this embodiment, the insulating material 1 is a rectangular parallelepiped with an opening 10 formed in its center. The primary coil patterns 21, 22 and the secondary coil pattern 23 are embedded in a rectangular spiral shape surrounding the opening 10. The ends of each coil pattern 21, 22, 23 are connected to external terminals via lead wires (not shown). A core 4 of a magnetic device D is attached around the insulating material 1. The core 4 in this embodiment is generally called an E-core and has left and right legs 41, 42 and upper and lower yoke portions 43, 44 arranged around the insulating material 1, and a central leg 45 that passes through the opening 10 and connects the upper and lower yoke portions 43, 44. The core 4 is made of a magnetic material and serves as a magnetic path through which magnetic flux generated by each coil pattern 21, 22, 23 flows. The core 4 can be a powder magnetic core, a ferrite core, a laminated steel plate, a metal composite core, or the like. The metal composite core is a magnetic body made by kneading magnetic powder and resin and then hardening the resin.

[0013] (2) Manufacturing Method As shown in FIG. 2, the magnetic device D is constructed by laminating multiple coil structures C, each of which has a coil pattern 2a formed on the surface of an insulating material 1a having a predetermined thickness. (2-1) Formation of an Insulating Material Layer on a Copper Foil Surface To manufacture each coil structure C, as shown in FIG. 2(a), an insulating material (called varnish) 1a dispersed or dissolved in a solvent is first applied to the surface of a copper foil 3a having a predetermined thickness (e.g., 18 μm, 25 μm, or 35 μm). In this case, the thickness of the applied insulating material 1a is adjusted so that the thickness of the insulating material 1a after evaporation of the solvent is the desired value (e.g., 25 μm). The solvent is then evaporated by pre-drying at approximately 100 to 120°C. In this state, the insulating resin composition is not completely cured and the resin surface remains sticky. Therefore, when storing or transporting the insulating material 1a, the surface of the insulating material 1a is covered with a polypropylene protective film.

[0014] (2-2) Thermal Curing of Insulating Material After the insulating material 1a is laminated on one side of the copper foil 3a, a new copper foil 3b is laminated on the side of the insulating material 1a opposite the copper foil 3a (the side on which the insulating material 1a is exposed), as shown in FIG. 2(b). In this case, the new copper foil 3b is adhered and fixed to the surface of the insulating material 1a due to the adhesiveness of the insulating material 1a. In this state, the insulating material 1a with the copper foils 3a and 3b laminated on both sides is placed in a vacuum press and thermally cured by heating and pressurizing at 180°C for 120 minutes, 1 MPa, and a vacuum of 5 torr.

[0015] In the case of a coil structure C that uses only one layer of coil pattern, such as a coil for contactless power supply or an antenna for an RF tag, an insulating material 1a is applied to one side of the copper foil 3a, and after pre-drying, it is heated and hardened as is.

[0016] (2-3) Formation of Coil Pattern After the insulating material 1a is removed from the vacuum press and the laminate of the hardened insulating material 1a and the copper foils 3a, 3b is etched to form the coil patterns 2a, 2b on both sides of the insulating material 1a. Any known technique can be used for the etching, such as a method used to create a conventional coil structure using glass cloth as a base material. By performing the etching, unnecessary portions of the copper foils 3a, 3b are removed, as shown in FIG. 2(c), to obtain a coil structure C in which the coil patterns 2a, 2b are formed on both sides of the hardened insulating material 1a.

[0017] (2-4) Multilayering of Coil Patterns and Insulating Materials To obtain a multilayer circuit board P by stacking the coil structures C configured as described above, the following procedure is followed. After the coil patterns 2a and 2b are formed on both sides in step (2-3), two new copper foils 3a with insulating material 1a (see FIG. 2(a)) are prepared, and the surfaces from which the protective films have been removed are overlapped with the surfaces of the copper foils 3a with the coil patterns 2a and 2b (see FIG. 2(c)). After three layers of insulating material 1a are thus obtained, as in step (2-2), these three layers of insulating material 1a are placed in a vacuum press and heated and pressurized to thermally harden the newly laminated insulating material 1a. Note that FIG. 2 shows a schematic representation of the insulating material 1a and the copper foils 3a and 3b, revealing gaps between the etched coil patterns 2a and 2b. However, because the pre-dried insulating material 1a is flexible, these gaps are filled with the insulating material 1a during pressurization in the vacuum press.

[0018] The copper foil 3a with insulating material 1a in FIG. 2(a) is a copper foil with an insulating resin composition formed on one side, known as a resin-coated copper foil. In this embodiment, a semi-cured insulating resin composition layer (resin layer) is formed on the copper foil, and the thicknesses of the copper foil and resin layer are not particularly limited. For example, when the copper foil is 35 μm thick, the resin layer thickness is preferably 5 μm to 200 μm, and more preferably 10 μm to 150 μm. A thickness below the upper limit allows for a thinner layer structure. A thickness above the lower limit improves voltage resistance. Multiple resin layers can be stacked here. For example, a resin layer can be formed on the copper foil in advance, cured, and then another resin layer formed on the cured surface, thereby improving voltage resistance. Note that the multiple resin layers may be made of different insulating resin compositions. Laminating a protective film on the semi-cured resin surface of the resin-coated copper foil prevents dust and other particles from adhering to the resin layer surface and improves handling. Examples of materials used for the protective film include polyolefins such as polyethylene, polypropylene, and polyvinyl chloride, polyesters such as PET and PEN, polycarbonate, and polyimide.

[0019] (2-5) Formation of Coil Pattern After the newly laminated insulating material 1a has hardened, the copper foil 3a exposed on both sides thereof is etched to form coil patterns 2c and 2d as shown in FIG. 2(e).

[0020] (2-6) Creation of Multilayer Circuit Board By repeating the above steps, the primary coil patterns 21, 22 and secondary coil pattern 23, each made up of the coil patterns 2a-2d that make up the individual coil structures, are embedded at a predetermined interval within the block-shaped insulating material 1, in which the insulating materials 1a that make up the individual coil structures are stacked and integrated. As a result, a multilayer circuit board P is formed as a whole in the shape of a single block, as shown in FIG. 2(f). By attaching a core 4 to this multilayer circuit board P, the magnetic device D of this embodiment can be obtained. Note that if the outermost coil pattern of the multilayer circuit board P is to be covered with an insulating material, after forming the outermost coil pattern in step (2-5), the insulating material 1a is applied to its surface, followed by pre-drying and thermal curing.

[0021] (3) Insulating Material In the above embodiment, an insulating resin composition that does not contain glass cloth is used as the insulating material. That is, since the prepreg is made by impregnating glass cloth with resin, a decrease in voltage resistance characteristics and an increase in electrostatic capacitance between coil patterns due to the physical properties of the glass cloth are unavoidable. Therefore, in this embodiment, a cured product of an insulating resin composition that does not contain glass cloth is used as the insulating material. In particular, an insulating resin composition that does not contain glass cloth preferably has a voltage resistance of 100 kV / mm or more and a dielectric constant of 4.0 or less. Furthermore, it is preferable that the insulating resin composition has adhesive properties before it is thermally cured.

[0022] (3-1) Specific Examples of Insulating Resin Compositions The insulating resin composition constituting the insulating material preferably has high withstand voltage characteristics and low capacitance when a magnetic device is constructed by forming coil patterns on both sides of the insulating material, and contains, for example, at least one thermosetting resin selected from the group consisting of epoxy resins, phenolic resins, cyanate resins, melamine resins, amino resins, imide resins, and amide-imide resins. When the thermosetting resin contains an epoxy resin, the epoxy resin contains, for example, at least one resin selected from the group consisting of multifunctional epoxy resins, bisphenol-type epoxy resins, novolac-type epoxy resins, and biphenyl-type epoxy resins.

[0023] The insulating resin composition may further contain at least one component selected from the group consisting of a filler, a curing agent, and a curing accelerator. The filler may contain, for example, at least one selected from the group consisting of silica, aluminum hydroxide, magnesium hydroxide, calcium carbonate, talc, and alumina. The curing agent may contain, for example, at least one of a phenolic curing agent and a dicyandiamide curing agent. The curing accelerator may contain, for example, at least one selected from the group consisting of imidazoles, phenolic compounds, amines, and organic phosphines. For example, polyimide resins, epoxy resins, etc. can be used.

[0024] The insulating resin composition may further contain inorganic fillers, flame retardants, and additives as necessary. Various inorganic fillers, including known ones, can be used for the purpose of improving the heat resistance, flame retardancy, low expansion coefficient, thermal conductivity, etc., of the cured product of the insulating resin composition. Specific examples of inorganic fillers include silica, alumina, talc, aluminum hydroxide, magnesium hydroxide, titanium oxide, mica, aluminum borate, barium sulfate, and calcium carbonate. Only one of these inorganic fillers may be used, or two or more may be used in combination. Furthermore, the inorganic filler may be used as is, or may be surface-treated with an epoxy silane-type or amino silane-type silane coupling agent depending on the purpose.

[0025] Examples of the flame retardant include phosphorus-based flame retardants and halogen-based flame retardants. Specific examples of the phosphorus-based flame retardant include phosphate esters such as condensed phosphate esters and cyclic phosphate esters, phosphazene compounds such as cyclic phosphazene compounds, and phosphinate-based flame retardants such as metal phosphinates such as aluminum dialkylphosphinates. Examples of the halogen-based flame retardant include bromine-based flame retardants. From the viewpoint of halogen-free, phosphorus-based flame retardants are preferably used. The flame retardants exemplified above may be used alone or in combination of two or more.

[0026] Examples of additives include antifoaming agents such as silicone-based antifoaming agents and acrylate-based antifoaming agents, heat stabilizers, antistatic agents, ultraviolet absorbers, dyes and pigments, lubricants, dispersants such as wetting dispersants, etc. Of these additives, only one type may be used, or two or more types may be used in combination.

[0027] (3-2) Preferable Insulating Resin Composition In the present embodiment, the following resin compositions represented by materials A to D are preferred as the insulating material: (a) Material A, Material D An insulating resin composition comprising: (a1) a liquid epoxy resin, (a2) a solid epoxy resin having a softening point of 125°C or less, (b) an aromatic diamine compound having a benzoate group and a polymethylene group in the main chain, (c) a solvent-soluble polyimide resin having a Tg of 200°C or more and a weight-average molecular weight Mw of 50,000 or less, and (d) a phenoxy resin having a Tg of 130°C or more, wherein when the total amount of (a1) the liquid epoxy resin, (a2) the solid epoxy resin, and (b) the aromatic diamine compound is 100 parts by weight, the total amount of (c) the solvent-soluble polyimide resin and (d) the phenoxy resin is 15 parts by weight or more and 150 parts by weight or less.

[0028] Material A has a certain degree of flexibility and can be formed into a thin insulating layer, and has durability and excellent processing properties as well as high insulating properties, so it has excellent reduced capacitance between coil patterns and voltage resistance properties.

[0029] (b) Material B: A polyimide derived from (A) an acid dianhydride and (B) a diamine, wherein the (A) acid dianhydride includes (A1) an acid anhydride having an ester bond, and the (B) diamine contains (B1) dimer diamine in a molar amount of 0.3 or more, where the molar amount of all diamines is 1.0.

[0030] Although general polyimides have excellent heat resistance and mechanical properties, they have a high dielectric constant, which results in a large capacitance. A high dielectric constant results in a large capacitance, which generates heat when used in high-speed (high-frequency) communications, causing malfunctions and other problems. Another issue with polyimides is their high water absorption. Material B has a dimer skeleton and an ester skeleton, and therefore has the properties of low dielectric constant and water absorption.

[0031] (c) Material C: A polyimide derived from (A) an acid dianhydride and (B) a diamine, wherein the (B) diamine has (B1) a diamine having a fluorene skeleton and (B2) a dimer diamine.

[0032] According to Material C, by introducing a fluorene skeleton and a dimer skeleton into the diamine component, the imide group concentration is reduced, the polarity of the entire molecule is reduced, and the dielectric constant can be reduced. In addition, the mechanical strength is excellent and high values ​​of the relative dielectric constant and dielectric loss tangent can be obtained.

[0033] (4) Coil Structure The magnetic device of this embodiment has multiple coil patterns 21, 22, and 23 formed inside an insulating material 1, and a core 4 attached thereto, as shown in FIG. 1 . However, the present invention is not limited to magnetic devices with cores. For example, the present invention also encompasses a coil structure having a flat conductor wound on a plane and an insulating material insulating between the conductors, in which the conductors and the insulating material are alternately stacked, but does not have a core. It also encompasses a multilayer circuit board in which multiple coil structures of this type are stacked without using a core. The operating frequency of the magnetic device is preferably in the range of 500 kHz to 1 MHz, which is suitable for power transformers, for example. However, this embodiment can also be applied to coil structures used in circuits with higher frequency bands.

[0034] As the material for the coil, in addition to a coil pattern obtained by etching copper foil, it is also possible to use a copper plate having a certain thickness or a rod-shaped or wire-shaped conductor used as a bus bar. In the case of such a rigid conductor, it is also possible to form a coil structure by applying an insulating material made of an insulating resin composition around the conductor or by covering it with an insulating tape or sheet, and then heating and curing the applied material.

[0035] (5) Multilayer Circuit Board A multilayer circuit board is formed by stacking a plurality of the above-described coil structures or by combining the above-described coil structure with another circuit board. The multilayer circuit board also includes a structure in which a plurality of substrates on which the coil pattern of the coil structure is formed as part of a circuit board including a wiring pattern are stacked. Furthermore, the multilayer circuit board can be formed by stacking not only the same coil structure but also a plurality of different types of coil structures described in the embodiments of this specification, or by combining and stacking a coil structure using a conventional glass cloth with a coil structure not including the glass cloth according to this embodiment.

[0036] 3, a magnetic device according to a first embodiment uses a multilayer circuit board formed by stacking coil structures, and has the same basic configuration as that shown in FIG. 1. In this embodiment, primary coil patterns 21 and 22 and a secondary coil pattern 23 are embedded in an insulating material 1 at a predetermined interval while maintaining insulation therebetween. Connectors 5 are provided on both ends of the insulating material 1 for connecting the primary coil patterns 21 and 22 and the secondary coil pattern 23 to external devices.

[0037] The magnetic device of this embodiment has multiple coil patterns built into a single multilayer circuit board, and therefore has a configuration specialized for miniaturization and thinness, and is suitable for applications such as: power semiconductor drive power supplies, white goods and air conditioner controls, power adapters, etc., with a power capacity of approximately 30 W or less. In addition, the use of a multilayer board also has the effect of enabling integration with peripheral circuit components.

[0038] 4, the magnetic device of the second embodiment is formed by stacking multilayer circuit boards P1, P2, and P3, each including a coil structure. That is, in this embodiment, the primary coil patterns 21 and 22 and the secondary coil pattern 23 are formed by separate multilayer circuit boards P1, P2, and P3, respectively, and these multilayer circuit boards P1, P2, and P3 are stacked to form a single magnetic device D as a whole.

[0039] The magnetic device of this embodiment has the effect of improving power by stacking multiple multilayer circuit boards P1, P2, and P3 to reduce current density. Furthermore, when the number of coil patterns is increased, the central insulating material 1 is repeatedly subjected to a heat curing process each time the coil structure is stacked. In this embodiment, if there is a risk of thermal degradation due to separate heating, the individual multilayer circuit boards P1, P2, and P3 are manufactured separately, thereby reducing the number of heat curing processes applied to the insulating material 1 and eliminating the effects of thermal degradation. Another advantage is that if the number of coil turns needs to be changed depending on the rating, capacity, etc. of the magnetic device D, this can be achieved simply by changing the stacked multilayer circuit boards P1, P2, and P3.

[0040] The magnetic device of this embodiment is suitable for applications with a power supply capacity of about 300 W or less, such as: power supplies for industrial equipment; power supplies for actuators; power supplies for servo amplifiers; battery chargers; and power supplies for LED lighting.

[0041] 5, the magnetic device of the third embodiment is formed by laminating a multilayer circuit board P including a secondary coil pattern 23 and primary coil structures C1 and C2, which are formed by overlapping copper plates 6 punched into a square and connected in a coil shape. Around the copper plates 6 of the primary coil structures C1 and C2, an insulating material 1 made of a thermosetting composition similar to the insulating material 1 of the multilayer circuit board P is formed. Methods for forming the insulating material 1 on the surface of the copper plates 6 include coating and covering with tape or sheet. Alternatively, the copper plate 6 formed into a coil shape can be placed in a mold, and the insulating material 1 can be injected and pre-dried, followed by heating and curing using a vacuum press or the like.

[0042] In this embodiment, by using a conductor made of copper plate 6, which has a larger cross-sectional area than an etched coil pattern, for the secondary coil structures C1 and C2, it is possible to further reduce the current density, which has the effect of improving power. Also, by combining a multilayer circuit board P using copper foil 3 with coil structures C1 and C2 using copper plate 6, for example, when using the magnetic device D as a power transformer, the conductor cross-sectional area and insulating material thickness of the combined coil structures C1 and C2 can be easily changed depending on the required power capacity, input / output voltage, etc., providing excellent versatility.

[0043] The magnetic device of this embodiment is suitable for applications with a power supply capacity of about 1 kW or less, such as: power supplies for industrial equipment; power supplies for actuators; power supplies for servo amplifiers; battery chargers; and power supplies for servers.

[0044] 6 , in the fourth embodiment, a conductor coil structure C3 made of a copper plate 6 is used as the primary coil instead of the multilayer circuit board P of the third embodiment. That is, for the secondary coil structures C1 and C2, a square copper plate 6 punched into a coil shape is used as in the third embodiment, and for the primary coil structure C3, a rectangular winding is used as the copper plate 6. The insulating material 1 formed around the copper plate 6 can be the same as the insulating material formed around the copper plate 6 of the third embodiment. In this case, the cross-sectional shape, cross-sectional area, and number of turns of the conductor copper plate 6 for the secondary coil structures C1 and C2 and the primary coil structure C3 can be changed to suit the characteristics of the required magnetic device.

[0045] In this embodiment, by using a conductor made of copper plate 6 for all of the coil structures C1, C2, and C3, the current density can be further reduced, thereby improving power. Therefore, the present invention is suitable for applications with a power supply capacity of approximately 1 kW or less, such as: power supplies for industrial equipment; battery chargers; and power supplies for servers.

[0046] 7, a magnetic device according to a fifth embodiment has a shield layer S provided on the outermost layer of a multilayer circuit board P. The shield layer S can be made of any of the following: A sheet material in which soft magnetic powder is dispersed in resin A sheet material in which carbon powder is dispersed in resin A sheet material in which a metal layer is coated with resin According to the fifth embodiment, leakage flux generated from the coil can be prevented from leaking out from the outermost layer.

[0047] 8, in a magnetic device according to a sixth embodiment, a shield layer S is provided in an intermediate layer of a multilayer circuit board P. The shield layer S may be that described in the fifth embodiment. According to the sixth embodiment, the degree of coupling between the primary coil and the secondary coil can be adjusted.

[0048] The effects of Examples 1 to 6 of the present invention in terms of capacitance (1 MHz), withstand voltage, low leakage, and total thickness were confirmed in comparison with Comparative Examples 1 and 2, which used prepreg as the insulating material.

[0049] (1) Comparative Example 1 A coil structure was prepared by laminating three layers of 100 μm thick prepreg (glass cloth-based epoxy resin substrate R-1766 / R-1661 sold by Panasonic Industries Co., Ltd.) as an insulating material, and providing a 25 μm thick coil pattern on both sides of the laminate. Dielectric constant of insulating material (1 MHz): 4.7 Withstand voltage: 64 kV / mm Insulating material thickness: 100 μm × 3 = 300 μm Coil pattern thickness: 25 μm × 2 = 50 μm Total thickness: 350 μm Distance between patterns: 300 μm

[0050] (2) Comparative Example 2 A coil structure was produced using one layer of the same 100 μm thick prepreg as in Comparative Example 1 (glass cloth-based epoxy resin substrate R-1766 / R-1661 sold by Panasonic Industries Co., Ltd.) as the insulating material, with a 25 μm thick coil pattern provided on both sides. Dielectric constant of insulating material (1 MHz): 4.7 Withstand voltage: 64 kV / mm Insulating material thickness: 100 μm x 1 = 100 μm Coil pattern thickness: 25 μm x 2 = 50 μm Total thickness: 150 μm Distance between patterns: 100 μm

[0051] (3) Example 1 Polyimide + Material A A single-layer coil structure in which a coil pattern was formed on a 25 μm thick polyimide film-based flexible substrate material (single-sided copper-clad laminate R-F770 sold by Panasonic Industries Co., Ltd.) as an insulating material, and a single-layer coil structure in which a coil pattern was formed on one side of the following Material A were laminated so that the coil patterns were on the outside. (3-1) Polyimide (R-F770) Dielectric constant of insulating material (1 MHz) 3.2 Withstand voltage 276 kV / mm Insulating material thickness 25 μm Coil pattern thickness 25 μm (3-2) Specific example of material A 98 parts by weight of bisphenol A type epoxy resin Epiclon 850-S (manufactured by DIC Corporation, epoxy equivalent 188), 147 parts by weight of dicyclopentadiene type epoxy resin HP-7200H (manufactured by DIC Corporation, epoxy equivalent 283, softening point 83°C), 126 parts by weight of Elastomer 250P (polytetramethylene oxide-di-p-aminobenzoate) manufactured by Ihara Chemical Co., Ltd., melting point 60°C), 100 parts by weight of soluble polyimide resin Q-VR-X0163 (manufactured by PI Technical Research Institute Co., Ltd., Tg A mixture of 246°C, 20% resin solids by weight, 303 parts by weight of phenoxy resin ERF-001M30 (manufactured by Nippon Steel Chemical Co., Ltd., Tg 146°C, 30% resin solids by weight), and 18 parts by weight of HCA was prepared to prepare a resin varnish with a resin solids content of 40% by weight. The resin varnish prepared in this manner was applied to the copper foil on which the coil pattern was to be formed, pre-baked at 120°C for 10 minutes, and then thermally cured at 180°C for 120 minutes to obtain Material A1, a cured epoxy resin. Dielectric constant of insulating material (1 MHz): 3.1; Withstand voltage: 229 kV / mm; Insulating material thickness: 25 μm; Coil pattern thickness: 25 μm. (3-3) (Polyimide + Material A) Total thickness and pattern spacing values: Total thickness: 100 μm; Pattern spacing: 50 μm

[0052] (4) Example 2 Polyimide + Material B A single-layer coil structure in which a coil pattern was formed on a single-sided copper-clad laminate (R-F770) using the polyimide of Example 1, and a single-layer coil structure in which a coil pattern was formed on one side of the following Material B, were laminated so that the coil patterns were on the outside. (4-1) Polyimide: Same as in Example 1. (4-2) Example of Material B: A 1-L four-neck separable flask equipped with a stirrer, reflux condenser, and thermometer was charged with 0.5 g of 4,4-oxydianiline, 4 g of dimer diamine (PRIAMINE 1075, Croda Japan), 6.2 g of 2,2',3,3',5,5'-hexamethyl[1,1'-biphenyl]-4,4'-diyl bis(1,3-dioxo-1,3-dihydro-2-benzofuran-5-carboxylate), and 32 g of n-methyl-2-pyrrolidone. While blowing nitrogen into the reaction vessel at 0.1 mL / sec, the mixture was heated and stirred at 50°C for approximately 3.5 hours. After confirming that the salt had dissolved, the mixture was stirred at room temperature for an additional 24 hours to synthesize polyamic acid, a precursor to polyimide. This polyamic acid itself is a solution and can be used as a varnish for coating copper foil as is. The polyamic acid synthesized in this way was applied to the copper foil on which the coil pattern was to be formed, and then pre-baked at 120°C for 10 minutes, heat-cured at 150°C for 60 minutes, and then further heat-cured at 180°C for 30 minutes, thereby causing ring-closing polymerization of the polyamic acid and obtaining a polyimide resin, Material B. Dielectric constant of insulating material (1 MHz): 2.65 Withstand voltage: 308 kV / mm Thickness of insulating material: 25 μm Thickness of coil pattern: 25 μm (4-3) (Polyimide + Material B) Total thickness and distance between patterns: Same as Example 1

[0053] (5) Example 3 Polyimide + Material C A single-layer coil structure in which a coil pattern was formed on a single-sided copper-clad laminate (R-F770) using the polyimide of Example 1, and a single-layer coil structure in which a coil pattern was formed on one side of the following Material C, were laminated so that the coil patterns were on the outside. (5-1) Polyimide (R-F770) Same as in Example 1. (5-2) Material C: A 1 L four-neck separable flask equipped with a stirrer, reflux condenser, and thermometer was charged with 8.7 g of 9,9-bis(4-aminophenyl)fluorene, 13.35 g of dimer diamine (Croda Japan, PRIAMINE 1075), 10.9 g of pyromellitic dianhydride, and 76.9 g of n-methyl-2-pyrrolidone. While blowing nitrogen into the reaction vessel at 0.1 mL / sec, the mixture was heated and stirred at 50°C for approximately 3.5 hours. After confirming the salt had dissolved, the mixture was stirred at room temperature for an additional 24 hours to synthesize polyamic acid, a precursor to polyimide. Like Material B, this polyamic acid itself is a solution and can be used as a varnish for application to copper foil. The polyamic acid synthesized in this way was applied to the copper foil on which the coil pattern was to be formed, and then pre-baked at 120°C for 10 minutes, heat-cured at 150°C for 60 minutes, and then further heat-cured at 180°C for 30 minutes, thereby causing ring-closing polymerization of the polyamic acid and obtaining a polyimide resin, Material C. - Dielectric constant of insulating material (1 MHz): 2.7 - Withstand voltage: 333 kV / mm - Insulating material thickness: 25 μm - Coil pattern thickness: 25 μm (5-3) (Polyimide + Material C) Total thickness and pattern distance: Same as Example 1

[0054] (6) Example 4 Material A alone A coil structure was prepared using material A alone as the insulating material, with coil patterns formed on both sides. The insulating thickness of material A was set to 50 μm, which was equal to the total thickness of polyimide and material A in Example 1.

[0055] (7) Example 5 Material B Alone A coil structure was prepared using Material B alone as the insulating material, with coil patterns formed on both sides. The insulating thickness of Material B was set to 50 μm, which was equal to the total thickness of the polyimide and Material A in Example 1.

[0056] (8) Example 6 Material C Alone A coil structure was prepared using Material C alone as the insulating material, with coil patterns formed on both sides. The insulating thickness of Material C was set to 50 μm, which was equal to the total thickness of the polyimide and Material A in Example 1.

[0057] (9) Example 7 Figure 9 shows a schematic diagram of an example of the manufacturing method for the resin-coated copper foil of this example. (1) The resin varnish of Material D was applied to an 18 μm copper foil (Cu) using a die coater and dried at 190°C to produce a resin-coated copper foil (A1) having a fully cured resin layer with a resin thickness of 51 μm. (2) Subsequently, the resin varnish of Material A was applied to the cured resin film of the resin-coated copper foil film and dried at 120°C to produce a resin-coated copper foil (A2) by further laminating a semi-cured resin layer with a thickness of 51 μm. The volatile content was adjusted to 0.5 wt%. (3) A PEN (polyethylene naphthalate) film was then laminated on the semi-cured resin layer as a protective film to produce a resin-coated copper foil (A3) for multilayering. (4) For the evaluation, the protective film PEN was removed from the resin-coated copper foil (A3), and a copper foil Cu for conducting electricity was laminated on the surface of the semi-cured resin material A to create an evaluation sample S. This evaluation sample corresponds to a single layer portion of the coil structure of this embodiment in which conductors and insulating materials are alternately laminated, and the electrical characteristics obtained from this sample correspond to the electrical characteristics of the coil structure. (5) Specific example of material D: 98 parts by weight of bisphenol A type epoxy resin Epiclon 850-S (manufactured by DIC Corporation, epoxy equivalent 188), 147 parts by weight of dicyclopentadiene type epoxy resin HP-7200H (manufactured by DIC Corporation, epoxy equivalent 283, softening point 83°C), 126 parts by weight of Elastomer 250P (polytetramethylene oxide-di-p-aminobenzoate) manufactured by Ihara Chemical Co., Ltd., melting point 60°C), 100 parts by weight of soluble polyimide resin Q-VR-X0163 (manufactured by PI Technical Research Institute Co., Ltd., Tg 246°C, resin solid content 20% by weight), 303 parts by weight of phenoxy resin ERF-001M30 (manufactured by Nippon Steel Chemical Co., Ltd., Tg 146°C) A mixture of 18 parts by weight of PEG (resin solids content 30% by weight), 18 parts by weight of HCA, and 10 parts by weight of 2E4MZ (manufactured by Shikoku Chemical Industry Co., Ltd.) was prepared to prepare a resin varnish with a resin solids content of 40% by weight. The dielectric constant of the insulating material (1 MHz) was 3.1. The withstand voltage was 229 kV / mm. The insulating material thickness was 25 μm.

[0058] (10) Example 8 Figure 10 shows a schematic diagram of an example of the manufacturing method for the resin-coated copper foil of this example. (1) Resin varnish of material B was applied to an 18 μm copper foil using a die coater and dried at 190°C to produce a resin-coated copper foil (B1) having a fully cured resin layer with a resin thickness of 51 μm. (2) Subsequently, resin varnish of material A was applied to the cured resin film of the resin-coated copper foil film and dried at 120°C to produce a resin-coated copper foil (B2) by further laminating a semi-cured resin layer with a thickness of 51 μm. The volatile content was adjusted to 0.5 wt%. (3) A PEN (polyethylene naphthalate) film was then laminated on the semi-cured resin layer as a protective film to produce a resin-coated copper foil (B3) for multilayering. (4) For evaluation, the PEN protective film was removed from the resin-coated copper foil (B3), and a copper foil (Cu) for conducting electricity was laminated on the surface of the semi-cured resin material A to prepare an evaluation sample S. (11) Example 9 (1) The resin varnish of material B was applied to an 18 μm copper foil using a die coater and dried at 190°C to produce a resin-coated copper foil (C1) having a fully cured resin layer with a resin thickness of 51 μm. (2) Subsequently, the resin varnish of material B was applied to the cured resin film of the resin-coated copper foil film and dried at 120°C to produce a resin-coated copper foil (C2) by further laminating a semi-cured resin layer with a thickness of 51 μm. The volatile content was adjusted to 0.5 wt%. (3) A PEN (polyethylene naphthalate) film was then laminated on the semi-cured resin layer as a protective film to prepare a resin-coated copper foil (C3) for multilayer construction. (4) For the evaluation, the protective film PEN was removed from the resin-coated copper foil (C3), and copper foil Cu for conducting electricity was laminated on the surface of the semi-cured resin material B to create an evaluation sample S.

[0059] (12) Evaluation Method Evaluation of the comparative examples and examples was carried out by the following method. (12-1) Capacitance The capacitance was calculated using the following formula: Capacitance C = (dielectric constant of insulating material × dielectric constant of vacuum × pattern area) / distance between patterns For Examples 1 to 3, the capacitance was calculated using the above formula for two capacitors having two types of dielectric, and the final capacitance was calculated using the following formula to find the combined capacitance when the two capacitors are connected in series: 1 / C = 1 / C1 + 1 / C2

[0060] (12-2) Withstand Voltage Based on the value of withstand voltage per thickness of the insulating material, it was calculated by converting it into the distance between patterns.

[0061] (12-3) Low Leakage (Leakage Magnetic Flux) Evaluation Since the leakage magnetic flux from between patterns decreases in inverse proportion to the distance between patterns, an evaluation was made based on the distance between patterns. ・Over 100 μm: × ・100 to 50 μm: ○ ・50 μm or less: ◎

[0062] (12-4) Total Thickness The total thickness was calculated by adding the thickness of the insulating material between patterns and the thickness of the patterns sandwiching the insulating material.

[0063] (12-5) Measurement method (1) Dielectric constant (1MHz) Shape of evaluation sample 20mm x 20mm x 200μm thick Manufacturer KEYSIGHT Name and model number of evaluation equipment RF Impedance / Material Analyzer, 1.8 GHz 4291B Measurement conditions Measured at 1MHz (2) Withstand voltage (kV / mm) Shape of evaluation sample 100mm x 100mm, 100μm thick for the prepreg of the comparative example, and 25μm thick for other materials Manufacturer Keisoku Giken Co., Ltd. Name and model number of evaluation equipment Ultra-high voltage withstand voltage tester 7472 type Measurement conditions Measured in accordance with IPC-TM-650 TM 2.5.7

[0064] The evaluation results for Examples 1 to 6 are shown in Table 1 below.

[0065] The evaluation results for Examples 7 to 9 are shown in Table 2 below.

[0066] [13. Discussion of Examples] (1) Capacitance As can be seen from Comparative Examples 1 and 2, when the insulating material is the same material, the capacitance is inversely proportional to the thickness of the insulating material (the distance between the coil patterns formed on both sides of the insulating material). Therefore, to reduce the capacitance, it is necessary to increase the insulating material thickness, but doing so makes it difficult to thin the magnetic device. In Examples 1 to 9, which do not use prepreg, the total thickness is reduced to 100 μm, but the capacitance is significantly reduced to about two-thirds of that of Comparative Example 2, which has an insulating material thickness of 100 μm and a total thickness of 150 μm.

[0067] Even when comparing Examples 1 to 3, in which polyimide and materials A to C are laminated together, Examples 4 to 6, in which materials A to C, which have a lower dielectric constant than polyimide, are used alone, exhibit reduced capacitance despite the same insulating thickness. From this, it is believed that magnetic devices in which polyimide and any of materials A to C are laminated together, as in Examples 1 to 3, exhibit reduced capacitance compared to magnetic devices using polyimide alone of the same thickness. According to Examples 4 to 6, of the three materials, materials B and C are superior in terms of capacitance, with the effect of material B being particularly notable. Materials B and C, even when combined with polyimide, are superior in terms of capacitance to material A. This point is also confirmed by the significant reduction in capacitance observed in Examples 7 to 9, in which two layers of materials A and B are combined and laminated together, compared to Examples 8 and 9, which include material B, and especially in Example 8, in which only material B is laminated in two layers.

[0068] (2) Withstand Voltage Compared to prepreg, polyimide and materials A to C have significantly superior withstand voltage characteristics as materials. Therefore, Examples 1 to 9 have far superior withstand voltage characteristics compared to Comparative Examples 1 and 2. Although polyimide alone exhibits excellent withstand voltage characteristics, combining it with material B or material C, which has even higher withstand voltage characteristics, can produce magnetic devices with excellent withstand voltage characteristics, as shown in Examples 2 and 3. In particular, material C exhibited the best withstand voltage characteristics, even compared to materials A and B. As shown in Examples 1 and 4, material A exhibits lower withstand voltage characteristics than polyimide alone. However, its withstand voltage is superior to that of the prepregs of Comparative Examples 1 and 2, and its capacitance is lower than that of polyimide. Therefore, material A is more suitable than polyimide alone for applications that meet the required withstand voltage and capacitance. Considering the low capacitance and excellent withstand voltage characteristics, it is clear that coil structures and multilayer circuit boards using material B, and magnetic devices incorporating such coil structures or multilayer circuit boards, exhibit extremely superior characteristics in practical use.

[0069] (3) Low Leakage All of Examples 1 to 9 exhibit excellent low leakage characteristics compared to Comparative Examples 1 and 2. In particular, despite the fact that the distance between the coil patterns is significantly reduced to 50 μm and the thickness of the insulating material is reduced, the reduction in leakage flux is advantageous for use in various magnetic devices.

[0070] (4) Total Thickness In all of Examples 1 to 9, the total thickness is significantly reduced compared to Comparative Examples 1 and 2. In particular, even if the insulating material is thinned to the same thickness as the coil pattern, it is possible to achieve the desired capacitance, withstand voltage, and low leakage, thereby realizing a smaller and thinner magnetic device.

[0071] [14. Other Embodiments] The present invention is not limited to the above-described embodiments, and in the implementation stage, the components can be modified and embodied without departing from the spirit of the invention. Furthermore, various inventions can be formed by appropriately combining multiple components disclosed in the above-described embodiments. For example, some components may be deleted from all of the components shown in the embodiments. Specifically, the following other embodiments are also included.

[0072] (1) When constructing a coil structure, a multilayer circuit board, and a magnetic device, the insulating material for insulating between conductors is not limited to a single type, but may be a laminate of different types of insulating materials as shown in Examples 1 to 3. Also, by using a different type of insulating material for each coil structure and laminating multiple coil structures with different insulating materials, it is possible to construct a thicker coil structure or a multilayer circuit board and a magnetic device.

[0073] (2) Although the present invention is characterized by not using glass cloth, it is not preferable to use any other substrate for resin impregnation, not limited to glass cloth, which is impregnated with an insulating resin composition. That is, many of the conventionally known substrates for resin impregnation are inferior in capacitance and withstand voltage characteristics compared to the homogeneous layer of the insulating resin composition shown in this embodiment, and if such a substrate is present in the insulating material, it becomes impossible to obtain the desired electrical and magnetic characteristics.

[0074] (3) Examples of conductors that can be used include coil patterns made by etching copper foil, copper plate coils, bus bars, and rectangular windings. When using copper foil, a coil pattern can be punched out in advance and then superimposed on the surface of a pre-dried or heat-cured insulating material, or uncured insulating material can be applied or sprayed onto the punched coil pattern. In the case of rigid conductors, they can be immersed (dipped) in a liquid insulating material, and then pre-dried and heat-cured after being removed.

[0075] (4) Materials A to C are not limited to the compositions described in the examples, and as long as they fall within the range of each material shown in [1. Basic structure of magnetic device], superior effects can be expected compared to the polyimide described in the examples.

[0076] D...Magnetic device C, C1, C2, C3...Coil structure P, P1, P2, P3...Multilayer circuit board S...Shield layer 1, 1a...Insulating material 10...Opening 21, 22, 23, 2a, 2b...Coil pattern 3, 3a, 3b...Copper foil 4...Core 41, 42...Leg portion 43, 44...Yoke portion 45...Central leg portion 5...Connector 6...Copper plate

Claims

1. A coil structure comprising a flat conductor wound on a plane and insulating material that provides insulation between the conductors, the conductors and the insulating material being alternately laminated, and the insulating material being a cured product of an insulating resin composition that does not contain glass cloth.

2. The coil structure according to claim 1, characterized in that the insulating resin composition has a withstand voltage of 100 kV / mm or more and a dielectric constant of 4.0 or less.

3. The coil structure according to claim 1 or 2, characterized in that the insulating resin composition has adhesive properties.

4. The coil structure according to claim 3, wherein the insulating resin composition contains an epoxy resin.

5. The coil structure according to claim 3 or 4, characterized in that the insulating resin composition contains at least one of a polyamide resin, a polyimide resin, and a polyamideimide resin.

6. The coil structure according to claim 4 or 5, characterized in that the insulating resin composition contains: (a1) a liquid epoxy resin; (a2) a solid epoxy resin having a softening point of 125°C or less; (b) an aromatic diamine compound having a benzoate group and a polymethylene group in its main chain; (c) a solvent-soluble polyimide resin having a Tg of 200°C or more and a weight-average molecular weight Mw of 50,000 or less; and (d) a phenoxy resin having a Tg of 130°C or more; and when the total amount of (a1) the liquid epoxy resin, (a2) the solid epoxy resin, and (b) the aromatic diamine compound is 100 parts by weight, the total amount of (c) the solvent-soluble polyimide resin and (d) the phenoxy resin is 15 parts by weight or more and 150 parts by weight or less.

7. A coil structure according to any one of claims 3 to 6, characterized in that the insulating resin composition is a polyimide derived from (A) an acid dianhydride and (B) a diamine, wherein the (A) acid anhydride includes (A1) an acid anhydride having an ester bond, and the (B) diamine is (B1) a dimer diamine in an amount of 0.3 or more moles per mole of the total diamine taken as 1.

0.

8. A coil structure according to any one of claims 3 to 6, characterized in that the insulating resin composition is a polyimide derived from (A) an acid dianhydride and (B) a diamine, and the (B) diamine has (B1) a diamine having a fluorene skeleton and (B2) a dimer diamine.

9. The coil structure according to claim 1, which is formed by forming said insulating resin composition on one side of a copper foil and forming a multi-layered resin-coated copper foil.

10. A multilayer circuit board comprising a coil structure according to any one of claims 1 to 9.

11. The multilayer circuit board according to claim 10, further comprising a shielding layer on the outermost layer or an intermediate layer.

12. A magnetic device comprising a core attached to the multilayer circuit board according to claim 10 or 11.

13. A magnetic device comprising a plurality of multilayer circuit boards according to claim 10 or 11 stacked together and fitted with a core.

14. A magnetic device comprising a coil structure according to claim 1 and a multilayer circuit board according to claim 10 or 11 stacked together, and a core attached.

15. A magnetic device according to any one of claims 12 to 14, wherein the operating frequency is 500 kHz to 1 MHz.

16. A resin-coated copper foil for coil structures, comprising an insulating resin composition formed on one side of the copper foil, a resin layer made of the insulating resin composition in a semi-cured state or an insulating resin composition different from the insulating resin composition formed on the surface of the insulating resin composition of the resin-coated copper foil, and a protective film laminated on the surface of the semi-cured resin layer.

17. A resin-coated copper foil for coil structures, characterized in that a resin layer made of the insulating resin composition in a semi-cured state is formed on one side of a copper foil, and a protective film is laminated on the surface of the semi-cured resin layer.

18. A method for manufacturing a coil structure, comprising laminating the resin-coated copper foil according to claim 16 or 17 so that the copper foil is in contact with the semi-cured resin layer with the protective film removed.

Citation Information

Patent Citations

  • Thin transformer

    JP1997326316A

  • Inductor and method for manufacturing the same

    JP2004200468A

  • Polyimide, adhesive, film-like adhesive, adhesion layer, adhesive sheet, copper foil with resin, copper-clad laminate, printed wiring board, and multilayer wiring board and method for producing the same

    JP2018168370A

  • Resin material and multilayer printed wiring board

    JP2020094213A

Cited By

  • Resin film, resin-equipped copper foil, multilayer wiring board, coil structure, and magnetic device