Steel wire and machine component
The steel wire with a specific composition and microstructure addresses the low yield strength and high permanent elongation issues in non-thermal bolts by achieving high yield strength and improved formability without bluing treatment, enhancing the manufacturing efficiency and performance of high-strength bolts.
Patent Information
- Application Number
- PCT/JP2024/013328
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-03-29
- Publication Date
- 2024-10-03
AI Technical Summary
Conventional non-thermal bolts face challenges with high dislocation density leading to low bolt yield strength and large permanent elongation, making them unsuitable for high-strength applications, and require bluing heat treatment to enhance strength, which complicates the manufacturing process.
A steel wire with a specific chemical composition and microstructure, including a balanced ratio of ferrite and martensite, is developed to achieve high yield strength and suppressed permanent elongation without the need for post-forming aging heat treatment, ensuring excellent formability and strength in mechanical parts.
The steel wire composition and microstructure enable high yield strength and reduced permanent elongation in mechanical parts, improving formability and processing without the need for bluing treatment, thus enhancing the manufacturing efficiency and performance of high-strength bolts.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002 
Figure JPOXMLDOC01-APPB-T000003
Abstract
Description
Steel wire and machine parts
[0001] The present disclosure relates to steel wire and machine parts.
[0002] High-strength materials are required for machine parts such as steel bolts and screws in order to reduce their weight and size. Conventionally, these machine parts have been manufactured by softening a steel wire rod for machine structures containing C, Mn, Cr, Mo, etc. through spheroidizing annealing, then forming it into a predetermined shape through cold heading or rolling, and then quenching and tempering it to impart strength.
[0003] Heat treatments such as spheroidizing annealing and quenching / tempering reduce manufacturing costs and CO 2 In order to increase the amount of waste, non-heat treated bolts are known, which are made by omitting these heat treatments and by increasing the strength of wire rod by adjusting the composition or by rapid cooling, and then by wiredrawing the wire rod to impart strength to the wire. Various wire rods and steel wires for manufacturing machine parts such as non-heat treated bolts have been proposed (see, for example, Patent Documents 1 to 5).
[0004] Patent Document 1: JP 2-166229 A Patent Document 2: WO 2016 / 121820 Patent Document 3: WO 2017 / 122830 Patent Document 4: WO 2018 / 008698 Patent Document 5: JP 2021-183710 A
[0005] Non-heat treated bolts are made by forming steel wire that has been strengthened by wire drawing. As the strength of the steel wire increases, the mold becomes more susceptible to damage and wear during forming, and the product is more susceptible to processing cracks, making it difficult to apply to high-strength bolts. Furthermore, conventional non-heat treated bolts have a high dislocation density, which results in low bolt yield strength, resulting in a problem of large permanent elongation. To address this issue, a bluing process is required after forming into bolts and other mechanical parts, in which the bolts are held at 300-400°C.
[0006] An object of the present disclosure is to provide a steel wire suitable for manufacturing mechanical parts, which has high strength and excellent formability in cold forging, and which can provide high yield strength and suppressed permanent elongation even when bluing heat treatment after forming is omitted, and a mechanical part.
[0007] The above-mentioned problems are solved by the following means. <1> In mass%, C: 0.08 to 0.80%, Si: 0.03 to 1.50%, Mn: 0.50 to 2.00%, P: 0.050% or less, S: 0.050% or less, Al: 0.005 to 0.080%, N: 0.0010 to 0.0150%, O: 0.003% or less, Ti: 0 to 0.050%, B: 0 to 0.0050%, Cr: 0 to 1.50%, Mo: 0 to 0.50%, Nb: 0 to 0.050%, V: 0 to 0.20%, Cu: 0 to 0.50%, Ni: 0 to 0.70%, Sn: 0 to 0.30%, (I) A steel sheet having a chemical composition consisting of Sb: 0 to 0.005%, and Ca: 0 to 0.0050%, with the balance consisting of Fe and impurity elements, wherein the contents of C, Si, Mn, Cr, Ni, Mo, and Cu in mass% are (C%), (Si%), (Mn%), (Cr%), (Ni%), (Mo%), and (Cu%), respectively; and (I) the chemical composition is, in mass%, C: 0.08 to 0.80%, Si: 0.03 to 1.50%, Mn: 0.50 to 2.00%, P: 0.050% or less, S: 0.050% or less, Al: 0.005 to 0.080%, N: 0.0010 to 0.0150%, and O : When the content is 0.003% or less and the balance is Fe and impurity elements, DI = 0.311 × (C%) 0.5 × (1 + 0.64 × (Si%)) × (1 + 4.10 × (Mn%)), and (II) when the chemical composition contains, in mass%, one or more elements selected from the group consisting of Ti: 0 to 0.050%, B: 0 to 0.0050%, Cr: 0 to 1.50%, Mo: 0 to 0.50%, Nb: 0 to 0.050%, V: 0 to 0.20%, Cu: 0 to 0.50%, Ni: 0 to 0.70%, Sn: 0 to 0.30%, Sb: 0 to 0.005%, and Ca: 0 to 0.0050%, and the B content is less than 0.0003%, then DI = 0.311 × (C%). 0.5× (1 + 0.64 × (Si %)) × (1 + 4.10 × (Mn %)) × (1 + 2.33 × (Cr %)) × (1 + 0.25 × (Ni %)) × (1 + 3.14 × (Mo %)) × (1 + 0.27 × (Cu %)), (III) the chemical composition is, in mass %, Ti: 0 to 0.050%, B: 0 to 0.0050%, Cr: 0 to 1.50%, Mo: 0 to 0.50%, Nb: 0 to 0.050%, V: 0 to 0.20%, Cu: 0 to 0.50%, Ni: 0 to 0.70%, Sn: 0 to 0.30%, Sb: 0 to 0.005%, and Ca: 0 to 0.0050%, and the B content is 0.0003 to 0.0050%, DI = 0.311 × (C%) 0.5x (1 + 0.64 x (Si %)) x (1 + 4.10 x (Mn %)) x (1 + 2.33 x (Cr %)) x (1 + 0.25 x (Ni %)) x (1 + 3.14 x (Mo %)) x (1 + 0.27 x (Cu %)) x (1 + 1.5 x (0.90 - (C %))), DI is 1.40 or more and 4.50 or less, and when the diameter of the steel wire is D, a total area ratio of ferrite and martensite in the metal structure at a ¼D part that is ¼D deep from the surface of the steel wire in a cross section perpendicular to the longitudinal direction of the steel wire is 30.0% or less, <2> A steel wire according to <1>, wherein, when F1 = (C%) + 0.10 × (Si%) + 0.18 × (Mn%) + 0.20 × (Cr%), the tensile strength is 860 × F1 + 450 MPa or more and 920 × F1 + 670 MPa or less, the value of (tensile strength - 0.2% proof stress) / uniform elongation is 20 + 25 × (C%) or less, and the reduction of area is 66 - 48 × (C%) or more.<3> A mechanical part having a cylindrical shaft portion, comprising, in mass%, C: 0.08 to 0.80%, Si: 0.03 to 1.50%, Mn: 0.50 to 2.00%, P: 0.050% or less, S: 0.050% or less, Al: 0.005 to 0.080%, N: 0.0010 to 0.0150%, O: 0.003% or less, Ti: 0 to 0.050%, B: 0 to 0.0050%, Cr: 0 to 1.50%, Mo: 0 to 0.50%, Nb: 0 to 0.050%, V: 0 to 0.20%, Cu: 0 to 0.50%, Ni: 0 to 0.70%, (I) A steel sheet having a chemical composition consisting of Sn: 0 to 0.30%, Sb: 0 to 0.005%, and Ca: 0 to 0.0050%, with the balance being Fe and impurity elements, wherein the contents of C, Si, Mn, Cr, Ni, Mo, and Cu in mass% are (C%), (Si%), (Mn%), (Cr%), (Ni%), (Mo%), and (Cu%), respectively; and (I) the chemical composition is, in mass%, C: 0.08 to 0.80%, Si: 0.03 to 1.50%, Mn: 0.50 to 2.00%, P: 0.050% or less, S: 0.050% or less, Al: 0.005 to 0.080%, N: 0.0010 to 0.0150%, and O When the content is 0.003% or less and the balance is Fe and impurity elements, DI = 0.311 × (C%). 0.5 × (1 + 0.64 × (Si%)) × (1 + 4.10 × (Mn%)), and (II) when the chemical composition contains, in mass%, one or more elements selected from the group consisting of Ti: 0 to 0.050%, B: 0 to 0.0050%, Cr: 0 to 1.50%, Mo: 0 to 0.50%, Nb: 0 to 0.050%, V: 0 to 0.20%, Cu: 0 to 0.50%, Ni: 0 to 0.70%, Sn: 0 to 0.30%, Sb: 0 to 0.005%, and Ca: 0 to 0.0050%, and the B content is less than 0.0003%, then DI = 0.311 × (C%). 0.5× (1 + 0.64 × (Si %)) × (1 + 4.10 × (Mn %)) × (1 + 2.33 × (Cr %)) × (1 + 0.25 × (Ni %)) × (1 + 3.14 × (Mo %)) × (1 + 0.27 × (Cu %)), (III) the chemical composition is, in mass %, Ti: 0 to 0.050%, B: 0 to 0.0050%, Cr: 0 to 1.50%, Mo: 0 to 0.50%, Nb: 0 to 0.050%, V: 0 to 0.20%, Cu: 0 to 0.50%, Ni: 0 to 0.70%, Sn: 0 to 0.30%, Sb: 0 to 0.005%, and Ca: 0 to 0.0050%, and the B content is 0.0003 to 0.0050%, DI = 0.311 × (C%) 0.5 x (1 + 0.64 x (Si %)) x (1 + 4.10 x (Mn %)) x (1 + 2.33 x (Cr %)) x (1 + 0.25 x (Ni %)) x (1 + 3.14 x (Mo %)) x (1 + 0.27 x (Cu %)) x (1 + 1.5 x (0.90 - (C %))), DI is 1.40 or more and 4.50 or less, and when the diameter of the shaft portion is d, a total area ratio of ferrite and martensite in the metal structure at a ¼ d portion that is ¼ d deep from the surface of the shaft portion in a cross section perpendicular to the longitudinal direction of the shaft portion is 30.0% or less, and the shaft portion <4> A mechanical component according to <3>, wherein, when F1 = (C%) + 0.10 × (Si%) + 0.18 × (Mn%) + 0.20 × (Cr%), the tensile strength is 860 × F1 + 430 MPa or more and 920 × F1 + 660 MPa or less, the value of (tensile strength - 0.2% proof stress) / uniform elongation is 38 + 25 × (C%) or less, 0.2% proof stress / tensile strength is 0.97 - 0.10 × (C%) or more, and reduction of area is 65 - 48 × (C%) or more.
[0008] According to the present disclosure, there are provided a steel wire and a mechanical component suitable for manufacturing mechanical components, which have high strength and excellent formability in cold forging, and which can achieve high yield strength and suppressed permanent elongation even when aging heat treatment after forming is omitted.
[0009] The wire rod according to the present disclosure will be described. In this disclosure, a numerical range expressed using "to" means a range that includes the numerical values before and after "to" as the lower and upper limits. However, when the numerical values before and after "to" are followed by "greater than" or "less than," the numerical range does not include the numerical values as the lower or upper limit. The content of an element in a chemical composition may be expressed by adding "amount" to the element symbol (e.g., C content, Si content, etc.). Regarding the content of an element in a chemical composition, "%" means "mass %." When the content of an element in a chemical composition is described as "0 to," it means that the element may not be included. The term "process" includes not only an independent process, but also a process that cannot be clearly distinguished from other processes, as long as the intended purpose of the process is achieved. The "surface" of a steel wire means the "outer surface." The "center axis" of a steel wire means an imaginary line that passes through the center point of a cross section perpendicular to the longitudinal direction of the steel wire and extends in the longitudinal direction (axial direction). "1 / 4D" is synonymous with "D / 4".
[0010] [Steel Wire] The steel wire according to the present disclosure has a chemical composition, in mass%, of C: 0.08 to 0.80%, Si: 0.03 to 1.50%, Mn: 0.50 to 2.00%, P: 0.050% or less, S: 0.050% or less, Al: 0.005 to 0.080%, N: 0.0010 to 0.0150%, and O: 0.003% or less, with the balance being Fe and impurity elements, wherein the contents of C, Si, Mn, and Cr, in mass%, are (C%), (Si%), (Mn%), and (Cr%), respectively, and DI=0.311×(C%). 0.5× (1 + 0.64 × (Si%)) × (1 + 4.10 × (Mn%)), DI is 1.40 or more and 4.50 or less; when the diameter of the steel wire is D, the total area ratio of ferrite and martensite in the metal structure at a ¼D portion that is ¼D deep from the surface of the steel wire in a cross section perpendicular to the longitudinal direction of the steel wire is 30.0% or less; when F1 = (C%) + 0.10 × (Si%) + 0.18 × (Mn%) + 0.20 × (Cr%), the tensile strength is 860 × F1 + 450 MPa or more and 920 × F1 + 670 MPa or less; the value of (tensile strength - 0.2% yield strength) / uniform elongation is 20 + 25 × (C%) or less; and the reduction of area is 66 - 48 × (C%) or more.
[0011] The inventors of the present disclosure studied the effects of steel wire and its mechanical properties on formability during processing into machine parts and the characteristics of the machine parts, and discovered that by setting the composition of the steel wire within a specific range, controlling the area ratio of ferrite and martensite in the steel wire structure, and further reducing the (tensile strength - 0.25% proof stress) / uniform elongation of the steel wire and increasing the reduction of area, it is possible to achieve excellent formability and a high bolt proof stress ratio and reduced permanent elongation after processing into a non-heat treated bolt. As mentioned above, since non-heat treated parts are strengthened before forming, their application to high-strength parts has been problematic due to reduced die life and processing cracks in the product. When the steel wire structure has a high area ratio of martensite, during processing that results in high strain, such as bolt head processing, the strength of the part increases due to work hardening, and the deformation resistance during processing increases. The inventors of the present disclosure have found that reducing the (tensile strength - 0.25% proof stress) / uniform elongation of a steel wire reduces work hardening, suppressing work hardening in high strain processing such as bolt head processing, and reducing the load on the die. Furthermore, they have found that increasing the reduction in drawing of the steel wire can suppress processing cracks in non-thermal refined parts.
[0012] If the area ratio of the ferrite structure in the steel wire is high, the yield strength ratio of the mechanical part will be low. Untempered bolts have a high dislocation density because their strength is imparted by wire drawing. If they contain a large number of mobile dislocations, they will undergo plastic deformation with small strains, lowering the elastic limit and resulting in low yield strength. In order to increase the yield strength of steel with a high dislocation density, it is effective to lock the solute carbon and nitrogen contained in the steel to the dislocations and suppress their movement. If the area ratio of the martensite structure in the steel wire is high, processing cracks will occur when the steel is formed into a mechanical part, and the yield strength ratio of the mechanical part will be low.
[0013] Conventional non-heat treated bolts use a heat treatment called bluing, which involves maintaining the temperature at 300 to 400°C to fix carbon to dislocations, thereby suppressing dislocation movement and increasing the bolt's yield strength. The inventors of the present disclosure have discovered that by reducing the area ratio of ferrite and martensite in the steel wire structure and setting the steel wire's (tensile strength - 0.25% yield strength) / uniform elongation within a specific range, the yield strength ratio of non-heat treated machine parts can be increased and permanent elongation can be suppressed without bluing. This is presumably because the solute carbon concentration is high after wire drawing, so carbon fixes mobile dislocations without heating to the bluing temperature of 300 to 400°C, suppressing dislocation movement and reducing work hardening, resulting in a high yield strength ratio.
[0014] <Chemical Composition> The chemical composition of the steel wire according to the present disclosure contains, as essential elements, in mass%, C: 0.08 to 0.80%, Si: 0.03 to 1.50%, Mn: 0.50 to 2.00%, P: 0.050% or less, S: 0.050% or less, Al: 0.005 to 0.080%, N: 0.0010 to 0.0150%, and O: 0.003% or less, with the balance being Fe and impurity elements, where the contents of C, Si, Mn, and Cr in mass% are (C%), (Si%), (Mn%), and (Cr%), respectively, and DI = 0.311 × (C%). 0.5 When DI is calculated as follows: × (1 + 0.64 × (Si%)) × (1 + 4.10 × (Mn%)), the DI is 1.40 or more and 4.50 or less.
[0015] The steel wire according to the present disclosure may contain other optional elements as necessary. When the steel wire according to the present disclosure contains optional elements, when the content of B is less than 0.0003%, DI=0.311×(C%). 0.5 × (1 + 0.64 × (Si%)) × (1 + 4.10 × (Mn%)) × (1 + 2.33 × (Cr%)) × (1 + 0.25 × (Ni%)) × (1 + 3.14 × (Mo%)) × (1 + 0.27 × (Cu%)), and when the B content is 0.0003 to 0.0050%, DI = 0.311 × (C%) 0.5 × (1 + 0.64 × (Si %)) × (1 + 4.10 × (Mn %)) × (1 + 2.33 × (Cr %)) × (1 + 0.25 × (Ni %)) × (1 + 3.14 × (Mo %)) × (1 + 0.27 × (Cu %)) × (1 + 1.5 × (0.90 - (C %))). In any case of the B content, the DI is 1.40 or more and 4.50 or less. If the DI is less than 1.40, the strength and yield strength ratio of the mechanical part will be low. A preferred DI is 1.60 or more. If the DI exceeds 4.50, the workability will be deteriorated. A preferred DI is 4.00 or less, and more preferably 3.00 or less.
[0016] C: 0.08 to 0.80% C is added to ensure the strength required for mechanical parts. If the C content is less than 0.08%, it is difficult to ensure the strength required for mechanical parts. On the other hand, if the C content exceeds 0.80%, ductility, toughness, and cold forgeability deteriorate. Therefore, the C content is set to 0.08 to 0.80%. The lower limit of the C content is 0.08%, preferably 0.15%, and more preferably 0.20%, and the upper limit of the C content is 0.80%, preferably 0.75%, and more preferably 0.70%. A preferred C content that achieves high strength, ductility, toughness, and cold workability is 0.15 to 0.75%, and more preferably 0.20 to 0.70%.
[0017] Si: 0.03 to 1.50% Si functions as a deoxidizing element and is effective in imparting the necessary strength to mechanical components. If the Si content is less than 0.03%, these effects are insufficient. If the Si content exceeds 1.50%, the ductility and toughness of the mechanical component deteriorate, and the deformation resistance of the steel wire increases, deteriorating cold forgeability. Therefore, the Si content is set to 0.03 to 1.50%. The Si content is preferably 0.05 to 1.00%, and more preferably 0.10 to 0.60%.
[0018] Mn: 0.50 to 2.00% Mn is an element necessary for imparting the necessary strength to mechanical components. If the Mn content is less than 0.50%, the effect is insufficient. If the Mn content exceeds 2.00%, the toughness of the mechanical components deteriorates, and the deformation resistance of the steel wire increases, deteriorating cold forgeability. Therefore, the Mn content is set to 0.50 to 2.00%. The preferred Mn content is 0.70 to 1.50%, and more preferably 0.90 to 1.20%.
[0019] P: 0.050% or less P is contained in steel wire as an impurity. P segregates at grain boundaries of mechanical components and deteriorates toughness, so it is desirable to reduce the P content. Therefore, the upper limit of the P content is set to 0.050%. A preferred upper limit of the P content is 0.020%, and a more preferred upper limit is 0.015% or less. Note that the lower limit of the P content is preferably 0% (i.e., no P is contained), but from the viewpoint of reducing the dephosphorization cost, it may be more than 0% (or 0.0001% or more).
[0020] S: 0.050% or less S is contained in the steel wire as sulfides such as MnS. These sulfides improve the machinability of the wire rod or the drawn steel wire. If the S content exceeds 0.050%, the cold heading property of the steel wire deteriorates and the toughness of the mechanical parts deteriorates. Therefore, the upper limit of the S content is set to 0.050%. A preferred upper limit of the S content is 0.030%. A more preferred upper limit is 0.015%. Note that the lower limit of the S content may be more than 0% (or 0.001% or more) from the viewpoint of reducing the desulfurization cost.
[0021] Al: 0.005 to 0.080% Al functions as a deoxidizing element, and also forms AlN to refine crystal grains and improve the toughness of mechanical components. It also has the effect of fixing solute N, suppressing dynamic strain aging, and reducing deformation resistance. If the Al content is less than 0.005%, these effects are insufficient. If the Al content exceeds 0.080%, the effects saturate and manufacturability may decrease. Therefore, the Al content is set to 0.005 to 0.080%. The preferred Al content is 0.010 to 0.065%, and more preferably 0.020 to 0.055%.
[0022] N: 0.0010 to 0.0150% N forms nitrides with Al, Ti, Nb, V, etc., which refines crystal grains and improves the toughness of machine parts. If the N content is less than 0.0010%, the amount of nitride precipitation is insufficient, and the effect cannot be obtained. If the N content exceeds 0.0150%, dynamic strain aging due to solute N increases the deformation resistance of the steel wire, degrading workability. Therefore, the N content is set to 0.0010 to 0.0150%. The N content is preferably 0.0020 to 0.0100%, and more preferably 0.0025 to 0.0060%.
[0023] O: 0.003% or less O is an impurity and is inevitably contained in steel. If the O content exceeds 0.003%, coarse oxides may form, which may reduce fatigue strength, so the O content is limited to 0.003% or less. The preferred upper limit of the O content is 0.002%.
[0024] Balance: Fe and impurity elements In the chemical composition of the steel wire according to the present disclosure, the balance is Fe and impurity elements (sometimes referred to as "impurities" in the present disclosure as appropriate). Here, impurities refer to components contained in raw materials or components mixed in during the manufacturing process, but not intentionally added. Furthermore, impurities also include components that are intentionally added but contained in amounts that do not affect the performance of the steel wire according to the present disclosure after wire drawing.
[0025] Furthermore, the steel wire according to the present disclosure may contain, in mass %, one or more elements selected from the group consisting of the following Groups A to D, in place of a portion of Fe:
[0026] [Group A] One or two selected from the group consisting of Ti: 0.050% or less, and B: 0.0050% or less
[0027] Ti: 0.050% or less Ti functions as a deoxidizing element and has the effect of refining crystal grains to improve workability. If the Ti content exceeds 0.050%, these effects saturate and coarse oxides or nitrides are generated, which may deteriorate the fatigue strength of mechanical parts. Therefore, if Ti is contained, the Ti content should be more than 0% but not more than 0.050%. The preferred Ti content is 0.003 to 0.050%, and more preferably 0.007 to 0.040%.
[0028] B: 0.0050% or less B has the effect of suppressing ferrite. If the B content exceeds 0.0050%, carbides may be generated at grain boundaries, which may deteriorate wiredrawability. Therefore, when B is contained, the B content should be more than 0 to 0.0050%. The B content is preferably 0.0003 to 0.0050%, and more preferably 0.0008 to 0.0030%.
[0029] [Group B] One or more selected from the group consisting of Cr: 0 to 1.50%, Mo: 0 to 0.50%, Nb: 0 to 0.050%, and V: 0 to 0.20%.
[0030] Cr: 1.50% or less Cr is an element necessary for imparting the necessary strength to mechanical components. If the Cr content exceeds 1.50%, the martensite fraction increases, degrading workability and increasing the deformation resistance of the steel wire, degrading cold forgeability. Therefore, the Cr content is set to 1.50% or less. The preferred Cr content is 0.05 to 0.80%, and more preferably 0.10 to 0.50%.
[0031] Mo: 0.50% or less Mo has the effect of imparting the necessary strength to mechanical parts. If the Mo content exceeds 0.50%, the alloy cost increases, and the deformation resistance of the steel wire increases, deteriorating cold forgeability. Therefore, when Mo is contained, the Mo content should be more than 0 to 0.50%. The Mo content is preferably 0.03 to 0.35%, and more preferably 0.05 to 0.25%. The Mo content may be 0.15% or less.
[0032] Nb: 0.050% or less Nb has the effect of increasing the strength of machine parts by precipitating carbides and nitrides, the effect of improving toughness by refining crystal grains, and the effect of reducing solute N and reducing deformation resistance. If the Nb content exceeds 0.050%, the effect saturates and cold forgeability may deteriorate. Therefore, when Nb is contained, the Nb content should be more than 0 to 0.050%. A preferable Nb content is 0.001 to 0.040%. A more preferable Nb content is 0.005 to 0.030%.
[0033] V: 0.20% or less V has the effect of precipitating carbides and nitrides to increase the strength of mechanical parts. If the V content exceeds 0.20%, the alloy cost increases. Therefore, when V is contained, the V content should be more than 0 to 0.20%. The preferred V content range is 0.01 to 0.15%. The V content may be 0.10% or less.
[0034] [Group C] One or more selected from the group consisting of Cu: 0 to 0.50%, Ni: 0 to 0.70%, Sn: 0 to 0.30%, and Sb: 0 to 0.005%.
[0035] Cu: 0.50% or less Cu precipitates finely, imparting the necessary strength to mechanical components and improving corrosion resistance. If the Cu content exceeds 0.50%, hot ductility deteriorates and surface defects become more likely to occur. Therefore, if Cu is contained, the Cu content should be greater than 0 and 0.50%. The preferred Cu content is 0.02 to 0.30%. The Cu content may be 0.20% or less.
[0036] Ni: 0.70% or less Ni has the effect of improving corrosion resistance. If the Ni content exceeds 0.70%, the alloy cost increases. Therefore, when Ni is contained, the Ni content should be more than 0 to 0.70%. The Ni content is preferably 0.02 to 0.50%, and more preferably 0.05 to 0.30%. The Ni content may be 0.25% or less.
[0037] Sn: 0.30% or less Sn has the effect of improving corrosion resistance. If the Sn content exceeds 0.30%, ductility decreases and cold workability deteriorates, so the Sn content is limited to 0.30% or less. The preferred upper limit of the Sn content is 0.20%.
[0038] Sb: 0.005% or less Sb has the effect of improving corrosion resistance. If the Sb content exceeds 0.005%, ductility decreases and cold workability deteriorates, so the Sb content is limited to 0.005% or less. The preferred upper limit of the Sb content is 0.004%, and the more preferred upper limit is 0.003%. The Sb content may be 0.002% or less.
[0039] [Group D] Ca: 0.0050% or less Ca is added as a deoxidizing element. Ca has the effect of refining oxides and improving fatigue strength. If the Ca content exceeds 0.0050%, ductility decreases and cold workability deteriorates, so the Ca content is limited to 0.0050% or less. The preferred upper limit of the Ca content is 0.0040%, and the more preferred upper limit is 0.0030%.
[0040] <Metal Structure> Next, the metal structure of the steel wire according to the present disclosure will be described. In the metal structure of the steel wire according to the present disclosure, in a cross section (C cross section) perpendicular to the longitudinal direction of the steel wire, the total area ratio of ferrite and martensite at a depth of 1 / 4D from the surface (outer peripheral surface) of the steel wire is 30.0% or less. If the total area ratio of ferrite and martensite exceeds 30.0%, workability deteriorates and the yield strength ratio of mechanical components decreases. The total area ratio of ferrite and martensite is preferably 20.0% or less, more preferably 10.0% or less. Furthermore, the remainder of the metal structure at the 1 / 4D portion is preferably bainite and / or pearlite. If the total area ratio of bainite and pearlite is 70.0% or more, workability improves and the yield strength ratio of mechanical components increases. The total area ratio of bainite and pearlite is preferably 80.0% or more, more preferably 90.0% or more.
[0041] (Method for Measuring Metallic Structure) For structural observation, two samples were taken from positions 50 mm apart in the axial direction of the steel wire, and the cross section (C section) perpendicular to the central axis of each steel wire sample was mirror-polished, corroded with picral, and the 1 / 4D section was observed. First, the C section of the steel wire to be measured was mirror-polished and then etched with picral (a 5% picric acid + 95% ethanol solution) to reveal the structure. Next, a structural photograph of a 20 μm × 20 μm or larger area at each of four locations circumferentially spaced 90° apart in the 1 / 4D section was taken at a magnification of 5000 times using a field emission scanning electron microscope (FE-SEM). A structure that does not contain carbides within the grains was determined to be ferrite or martensite.
[0042] The metal structure may include bainite, pearlite, martensite, and ferrite. A structure that does not contain intragranular carbides is considered ferrite or martensite. A structure other than ferrite or martensite is considered bainite or pearlite. Therefore, structures other than ferrite or martensite (structures that do not contain intragranular carbides) in the photographed structure are visually marked, and the area of the ferrite or martensite structure region is determined by image analysis (software name: Nireco's small general-purpose image processing analysis system LUZEX_AP). This operation is performed by measuring and calculating two samples, and the area percentage of ferrite or martensite in this disclosure is determined by averaging these values. The total area percentage of bainite and pearlite is determined by subtracting the area percentage of ferrite or martensite from 100.
[0043] Areas that do not contain carbides within the grains in the photographed structure are visually marked, and the area of the total area of the ferrite and martensite regions is determined by image analysis (software name: Nireco's small general-purpose image processing analysis system LUZEX_AP). This operation is performed for at least two samples, and the average value is calculated and used as the total area percentage of the ferrite and martensite structures in the present disclosure.
[0044] <Mechanical Properties> Tensile strength: 860 × F1 + 450 MPa or more, 920 × F1 + 670 MPa or less When the contents of C, Si, Mn, and Cr in mass% are (C%), (Si%), (Mn%), and (Cr%), respectively, and F1 = (C%) + 0.10 × (Si%) + 0.18 × (Mn%) + 0.20 × (Cr%), the steel wire according to the present disclosure has a tensile strength of 860 × F1 + 450 MPa or more and 920 × F1 + 670 MPa or less. By having a tensile strength of 860 × F1 + 450 MPa or more and 920 × F1 + 670 MPa or less, the strength required after processing into mechanical parts can be obtained. The tensile strength is preferably 860 × F1 + 480 MPa or more and 920 × F1 + 640 MPa or less. Tensile tests of steel wires were performed using JIS Z2241:2011 No. 14A test pieces according to the test method of JIS Z2241:2011 to measure tensile strength (TS), 0.2% proof stress, uniform elongation, and reduction of area. The 0.2% proof stress was defined as the stress at which the plastic elongation reached 0.2% of the extensometer gauge length using the offset method defined in JIS Z2241:2011. Tensile test pieces were machined immediately after bending the steel wire. The tensile test was performed on three samples, and the average value was used.
[0045] (Tensile strength - 0.2% yield strength) / uniform elongation: 20 + 25 × (C%) or less The steel wire according to the present disclosure has (Tensile strength - 0.2% yield strength) / uniform elongation of 20 + 25 × (C%) or less. By having (Tensile strength - 0.2% yield strength) / uniform elongation of 20 + 25 × (C%) or less, workability is improved. (Tensile strength - 0.2% yield strength) / uniform elongation is preferably 15 + 20 × (C%) or less. Uniform elongation is the elongation up to the maximum load in a tensile test, and the maximum load displacement is expressed as L M , the initial inter-rating distance is L 0 When M -L 0 ) / L 0 x 100 (%).
[0046] If the martensite fraction of the steel wire is high, cracks will occur during bolt forming and the bolt's yield strength ratio will decrease. Furthermore, even if the total area ratio of ferrite and martensite is reduced, if the steel wire's (tensile strength - 0.25% yield strength) / uniform elongation is large, the workability when formed into parts will decrease. The reason for this is that, to improve workability, it is necessary to reduce work hardening, but if the (tensile strength - 0.25% yield strength) / uniform elongation of the steel wire is large, the work hardening will increase and the workability of the steel wire will decrease.
[0047] Reduction of area: 66-48×(C%) or more The steel wire according to the present disclosure has a reduction of area of 66-48×(C%) or more. A reduction of area of 66-48×(C%) or more improves workability. The reduction of area is preferably 74-48×(C%) or more.
[0048] (Diameter) The wire diameter D of the steel wire according to the present disclosure is not particularly limited, but is preferably 2.0 to 22.0 mm, and more preferably 4.0 to 16.0 mm.
[0049] [Machine Component] A machine component according to the present disclosure includes a cylindrical shaft portion and has a chemical composition, in mass%, of C: 0.08 to 0.80%, Si: 0.03 to 1.50%, Mn: 0.50 to 2.00%, P: 0.050% or less, S: 0.050% or less, Al: 0.005 to 0.080%, N: 0.0010 to 0.0150%, and O: 0.003% or less, with the balance being Fe and impurity elements, wherein the mass% contents of C, Si, Mn, Cr, Ni, Mo, and Cu are (C%), (Si%), (Mn%), (Cr%), (Ni%), (Mo%), and (Cu%), respectively, and DI = 0.311 × (C%). 0.5× (1 + 0.64 × (Si%)) × (1 + 4.10 × (Mn%)), DI is 1.40 or more and 4.50 or less, where d is the diameter of the shaft portion, a total area fraction of ferrite and martensite in the metal structure at a ¼d portion that is ¼d deep from the surface of the shaft portion in a cross section perpendicular to the longitudinal direction of the shaft portion is 30.0% or less, where F1 = (C%) + 0.10 × (Si%) + 0.18 × (Mn%) + 0.20 × (Cr%), the shaft portion has a tensile strength of 860 × F1 + 450 MPa or more and 920 × F1 + 670 MPa or less, a value of (tensile strength - 0.2% proof stress) / uniform elongation is 38 + 25 × (C%) or less, and 0.2% proof stress / tensile strength is 0.97 - 0.10 × (C%) or more, The aperture is 65-48×(C%) or more.
[0050] The mechanical component according to the present disclosure is obtained by cold forging the steel wire according to the present disclosure. Since the chemical composition of the steel wire does not change before and after cold forging, the chemical composition of the mechanical component is the same as that of the steel wire. The optional elements are also the same as those described for the steel wire. The reasons for limiting the content of each element and the preferred range are also the same as those for the steel wire.
[0051] When the mechanical component according to the present disclosure contains an optional element, DI is calculated as follows according to the content of B: When the content of B is less than 0.0003%, DI = 0.311 × (C%) 0.5 × (1 + 0.64 × (Si%)) × (1 + 4.10 × (Mn%)) × (1 + 2.33 × (Cr%)) × (1 + 0.25 × (Ni%)) × (1 + 3.14 × (Mo%)) × (1 + 0.27 × (Cu%)). On the other hand, when the B content is 0.0003 to 0.0050%, DI = 0.311 × (C%). 0.5 × (1 + 0.64 × (Si %)) × (1 + 4.10 × (Mn %)) × (1 + 2.33 × (Cr %)) × (1 + 0.25 × (Ni %)) × (1 + 3.14 × (Mo %)) × (1 + 0.27 × (Cu %)) × (1 + 1.5 × (0.90 - (C %))). Regardless of the B content, the DI value is 1.40 or more and 4.50 or less. The preferred range of DI in mechanical parts is the same as that of the steel wire described above.
[0052] <Metal structure> In the mechanical component according to the present disclosure, when the diameter of the shaft portion is d, the total area ratio of ferrite and martensite in the metal structure at a ¼ d portion that is a depth of ¼ d from the surface of the shaft portion in a cross section perpendicular to the longitudinal direction of the shaft portion is 30.0% or less, and the preferable range is also the same as that of the steel wire described above.
[0053] <Mechanical Properties> In the mechanical component according to the present disclosure, when the contents of C, Si, Mn, Cr, Ni, Mo, and Cu in mass % are (C%), (Si%), (Mn%), (Cr%), (Ni%), (Mo%), and (Cu%), respectively, the shaft portion has the following mechanical properties.
[0054] Tensile strength: 860×F1+430 MPa or more and 920×F1+660 MPa or less When F1=(C%)+0.10×(Si%)+0.18×(Mn%)+0.20×(Cr%), the mechanical component according to the present disclosure has a tensile strength of 860×F1+430 MPa or more and 920×F1+660 MPa or less. When the tensile strength of the shaft is within this range, the strength required for the mechanical component is obtained.
[0055] (Tensile strength - 0.2% yield strength) / uniform elongation: 38 + 25 × (C%) or less The shaft portion of the mechanical component according to the present disclosure has (tensile strength - 0.2% yield strength) / uniform elongation of 38 + 25 × (C%) or less. By having (tensile strength - 0.2% yield strength) / uniform elongation of 38 + 25 × (C%) or less, permanent elongation of the mechanical component is suppressed. (Tensile strength - 0.2% yield strength) / uniform elongation is preferably 30 + 20 × (C%) or less. More preferably, it is 23 + 23 × (C%) or less.
[0056] 0.2% Yield Strength / Tensile Strength: 0.97-0.10×(C%) or More The shaft portion of the mechanical component according to the present disclosure has a 0.2% yield strength / tensile strength of 0.97-0.10×(C%) or more. When the 0.2% yield strength / tensile strength is 0.97-0.10×(C%) or more, permanent elongation of the mechanical component is suppressed.
[0057] Reduction of Area: 65-48×(C%) or More The shaft portion of the mechanical component according to the present disclosure has a reduction of area of 65-48×(C%) or more. A reduction of area of 65-48×(C%) or more improves toughness. The reduction of area is preferably 73-48×(C%) or more.
[0058] (Diameter) The diameter d of the shaft portion of the mechanical component according to the present disclosure is not particularly limited, but is preferably 2.0 to 22.0 mm, and more preferably 4.0 to 16.0 mm.
[0059] The use of the mechanical component according to the present disclosure is not particularly limited as long as it is a mechanical component that includes a cylindrical shaft portion. Examples of applications include automotive components having a shaft shape, such as bolts, torsion bars, and stabilizers, and various industrial machines, and the mechanical component according to the present disclosure is particularly suitable for bolts for automobiles and construction.
[0060] [Method for manufacturing steel wire and mechanical component] Next, a preferred method for manufacturing the steel wire and mechanical component according to the present disclosure will be described. Note that the method for manufacturing the steel wire and mechanical component described below is one example for obtaining the steel wire and mechanical component according to the present disclosure, and is not limited to the following procedure and method, and any method may be adopted as long as it can realize the steel wire and mechanical component according to the present disclosure.
[0061] <Method for manufacturing steel wire> A steel billet made of predetermined components satisfying the above-described chemical composition is heated to 1050 to 1250°C (surface temperature, the same applies hereinafter), held in the furnace for 90 minutes or more, then hot rolled at an entry temperature of 750 to 850°C for finish rolling, and wound into a ring shape at 780 to 880°C. If the heating temperature is less than 1050°C or the furnace residence time during heating is less than 90 minutes, the solid solution of carbides becomes insufficient, resulting in a decrease in the yield strength ratio of the mechanical part. If the heating temperature exceeds 1250°C, the surface hardness of the mechanical part decreases. If the entry temperature for finish rolling exceeds 850°C, the crystal grains become coarse, degrading the workability of the steel wire. If the entry temperature is less than 750°C, the crystal grain size becomes non-uniform, degrading the yield strength ratio of the mechanical part. If the winding temperature exceeds 880°C, the crystal grains become coarse, degrading the workability of the steel wire. If the coiling temperature is less than 780°C, the area ratio of ferrite increases and the yield strength ratio of the mechanical part decreases.
[0062] After coiling, primary cooling is performed to 750°C at an average cooling rate of 2 to 15°C / s. If the primary cooling rate to 750°C after coiling is less than 2°C / s, the crystal grains become coarse and the workability of the steel wire deteriorates. If the rate exceeds 15°C / s, the recovery and recrystallization of γ grains is delayed, resulting in mixed grains. As a result, the γ grain size becomes non-uniform, and the yield strength ratio and permanent elongation of mechanical parts deteriorate.
[0063] Thereafter, secondary cooling is performed at an average cooling rate of 25° C. / s or more from 750° C. to 520° C. If the cooling rate from 750° C. to 520° C. is less than 25° C. / s, the area ratio of ferrite increases, and the yield strength ratio of the mechanical part decreases.
[0064] Next, the steel wire is tertiarily cooled at an average cooling rate of 20°C / s or less from 520°C to 450°C. If the average cooling rate from 520°C to 450°C exceeds 20°C / s, the workability of the steel wire deteriorates, and the yield strength ratio and permanent elongation of the mechanical part deteriorate.
[0065] The wire is then held at 420-460°C for 30-100 seconds (primary holding), heated from 490°C to 550°C at an average heating rate of 10°C / s or more, held at 550-620°C for 60-200 seconds (secondary holding), and then water-cooled to obtain a wire rod. If the primary holding time at 420-460°C is less than 30 seconds, the yield strength ratio and permanent elongation of the mechanical parts deteriorate. If the primary holding time exceeds 100 seconds, the value of (tensile strength - 0.2% yield strength) / uniform elongation of the steel wire increases, and the yield strength ratio and permanent elongation of the mechanical parts deteriorate. If the average heating rate from 490°C to 550°C is less than 10°C / s, the yield strength ratio and permanent elongation of the mechanical parts deteriorate. If the secondary holding temperature is less than 550°C, the yield strength ratio and permanent elongation of the mechanical parts deteriorate, and if it exceeds 620°C, the strength decreases. If the secondary holding time is less than 60 seconds, the yield strength ratio and permanent elongation of the mechanical part will deteriorate, and if it exceeds 200 seconds, the reduction in area of the steel wire will decrease.
[0066] The obtained wire rod was subjected to a surface treatment with zinc phosphate and then subjected to one-pass wire drawing at room temperature using a die with an approach total angle of 5° to 14°, with a wire drawing reduction of 12% to 35% and a steel wire surface temperature of 80°C to 200°C immediately after wire drawing. If the approach total angle is less than 5°, the reduction of area of the steel wire will decrease due to heat generation caused by friction, and if it exceeds 14°, the deformation will be non-uniform and the reduction of area of the steel wire will decrease. If the wire drawing reduction is less than 12%, the strength of the steel wire will decrease, and if it exceeds 35%, the wire may break during drawing. The surface temperature of the steel wire immediately after wire drawing was measured using a radiation thermometer at the steel wire exit side of the die. If the surface temperature of the steel wire immediately after wire drawing is less than 80°C, wire breakage may occur due to seizure caused by insufficient lubrication, and if it exceeds 200°C, the reduction of area of the steel wire will decrease. After wire drawing, the wire is aged by holding at 150°C to 250°C for 30 to 180 minutes. If the aging temperature is less than 150° C., the reduction in area of the steel wire may decrease, and if it exceeds 250° C., the yield strength ratio of the mechanical part may decrease. If the aging time is less than 30 minutes or exceeds 180 minutes, the yield strength ratio and permanent set of the mechanical part may deteriorate.
[0067] The steel wire obtained as described above is subjected to cold heading and rolling to be processed into the shape of a machine part such as a bolt, etc. If necessary, zinc plating and baking treatment are performed.
[0068] The steel wire according to the present disclosure is obtained by wiredrawing the wire rod produced as described above, and plastic flow is observed in the surface layer of the longitudinal cross section of the steel wire. The steel wire produced using the wire rod has high strength and drawing ability, and is excellent in high strength and formability of mechanical parts. Mechanical parts produced using such steel wire have a high yield strength ratio and suppressed permanent elongation even if a bluing treatment after forming is omitted.
[0069] The steel wire and mechanical component according to the present disclosure will be described in more detail below with reference to examples. However, these examples do not limit the steel wire and mechanical component according to the present disclosure.
[0070] <Production and Evaluation of Steel Wire> Steels A to X having the chemical compositions shown in Table 1 were heated, hot-rolled, cooled, and held under the conditions shown in Table 2 to produce wire rods. Thereafter, wire drawing and aging treatment were performed under the conditions shown in Table 3 to produce steel wires. In Table 1, blank spaces indicate that the element is not included, and the remainder is Fe and impurities. Note that the blank space for B is "B<0.0003". In addition, underlines in each table indicate that the element is outside the scope of the present disclosure.
[0071]
[0072]
[0073]
[0074] The obtained steel wires were subjected to microstructural observation, tensile tests, and compression tests. Table 4 shows the microstructure and mechanical properties of the steel wires for each test number. For microstructural observation, a cross section (C cross section) perpendicular to the central axis of the steel wire was mirror-polished, corroded with picral, and the 1 / 4D section was observed. Tensile tests were performed using JIS Z2241:2011 No. 14A test pieces according to the test method of JIS Z2241:2011, and the tensile strength (TS), 0.2% proof stress, uniform elongation, and reduction of area were measured. Tensile test pieces were obtained by machining the steel wires immediately after drawing. The tensile test was performed on three samples, and the average value was used. Note that the steel wire with test number 24 broke during wiredrawing, so tensile tests and compression tests were not performed.
[0075] For the compression test, a cylindrical test piece with a diameter D and a height of 1.5 × D was cut from the steel wire, and a notch parallel to the axial direction of the steel wire was made on the side of the cylinder. The notch depth was 0.8 mm, the notch angle was 30°, and the R at the notch tip was 0.15. The specimen was compressed in the axial direction using a smooth pressure plate, and the presence or absence of cracks was confirmed. If no cracks were found, the compression rate was increased by approximately 1% and compression processing was performed again. The maximum compression rate at which cracks did not occur was defined as the critical compression rate. When a crack of 1.0 mm or more occurred in the notch, it was judged that cracks had occurred. Steel wires with a critical compression rate (%) of 94-0.048 × TS (MPa) or more were judged to have good strength and formability.
[0076]
[0077] <Production and Evaluation of Mechanical Components> The steel wires shown in Table 4 were processed into bolt shapes by cold heading and rolling. Test numbers 1, 4, 8, 9, 11, 13, 14, 15, 19, 21, 23, 24, and 25 were processed into bolt shapes with threads of M6 and shank lengths of 100 mm, while test numbers 2, 3, 5, 6, 7, 10, 12, 16, 17, 18, 20, 22, 26, and 27 were processed into bolt shapes with threads of M8 and shank lengths of 100 mm. These bolts were then electrogalvanized and baked at 200°C for 120 minutes after plating to obtain mechanical components (bolts). Microstructure observation samples and tensile test pieces were taken from the shanks of the obtained mechanical components (bolts), and microstructure observation and tensile testing were performed. The tensile test specimens were JIS Z2241:2011 No. 14A test specimens, and measurements were performed according to the test method of JIS Z2241:2011. The diameter of the parallel portion of the tensile test specimen was 5 mm for the bolt with thread M6 and 7 mm for the bolt with thread M8. A proof load test was also performed using the obtained machine parts (bolts). Table 5 shows the structure and mechanical properties of the bolt shank for each test number. The machine part with test number 26 was not subjected to a tensile test or proof load test because cracks occurred during bolt processing.
[0078] For microstructural observation, a cross section (C section) perpendicular to the central axis of the bolt shank was mirror-polished, corroded with picral, and the 1 / 4d section was observed. Tensile tests were performed on bolts to test specimens with a threaded section of M5, a parallel section of 4 mm, and a length of 70 mm. The tests were performed in air at room temperature with a gauge length of 20 mm and a crosshead speed of 10 mm / min to measure the tensile strength (TS), 0.2% proof stress, and uniform elongation. Tensile tests were performed on one part (bolt) of each test number. A proof stress ratio (0.2% proof stress / tensile strength) of 0.90 or more and a permanent elongation of 1 μm or less was judged to be good.
[0079] The proof load test was performed as follows: The shaft of the machine part was machined into a coarse thread shape by rolling or machining. After threading, the machine part was fitted with an adapter as specified in JIS B1051:2014 so that the length of the play thread was equal to the outer diameter of the thread. When the tensile strength of the mechanical part is 600 MPa or more but less than 700 MPa, the stress is 440 MPa, when it is 700 MPa or more but less than 800 MPa, the stress is 515 MPa, when it is 800 MPa or more but less than 900 MPa, the stress is 580 MPa, when it is 900 MPa or more but less than 1000 MPa, the stress is 650 MPa, when it is 1000 MPa or more but less than 1100 MPa, the stress is 830 MPa, when it is 1100 MPa or more but less than 1200 MPa, the stress is 910 MPa, when it is 1200 MPa or more but less than 1300 MPa, the stress is 970 MPa, and when it is 1300 MPa or more but less than 1400 MPa, the stress is 1050 MPa. A tensile stress of 1050 MPa is applied in the axial direction for 15 seconds. The difference (L1 - L0) between the total length L1 of the mechanical part after unloading and the total length L0 of the mechanical part before the test is defined as the permanent elongation. The total length L1 of the mechanical part after unloading and the total length L0 of the mechanical part before the test were measured with a micrometer.
[0080]
[0081] From the above results, the steel wires of test numbers 1 to 21 that satisfy the requirements of the present disclosure have excellent formability during bolting, and have achieved high yield strength ratios and suppressed permanent set even without bluing treatment after bolting. On the other hand, the steel wires of test numbers 23, 25, and 27 have good strength and formability, but have insufficient yield strength ratios after bolting and large permanent set.
[0082] (Additional Notes) The present disclosure includes the following aspects. <1> A chemical composition containing, in mass%, C: 0.08 to 0.80%, Si: 0.03 to 1.50%, Mn: 0.50 to 2.00%, P: 0.050% or less, S: 0.050% or less, Al: 0.005 to 0.080%, N: 0.0010 to 0.0150%, and O: 0.003% or less, with the balance consisting of Fe and impurity elements, wherein the mass% contents of C, Si, Mn, and Cr are (C%), (Si%), (Mn%), and (Cr%), respectively, and DI = 0.311 × (C%). 0.5a steel wire in which, when F1=(C%)+0.10×(Si%)+0.18×(Mn%)+0.20×(Cr%), the tensile strength is 860×F1+450 MPa or more and 920×F1+670 MPa or less, a value of (tensile strength−0.2% yield strength) / uniform elongation is 20+25×(C%) or less, and a reduction of area is 66−48×(C%) or more. <2> The chemical composition contains, in mass%, C: 0.08 to 0.80%, Si: 0.03 to 1.50%, Mn: 0.50 to 2.00%, P: 0.050% or less, S: 0.050% or less, Al: 0.005 to 0.080%, N: 0.0010 to 0.0150%, and O: 0.003% or less, and further contains one or more elements selected from the group consisting of the following A to D groups, with the balance consisting of Fe and impurity elements: [Group A] One or two elements selected from the group consisting of Ti: 0.050% or less, and B: 0.005% or less [Group B] Cr: 1.50% or less, Mo: 0.50% or less, Nb: 0.050% or less, and V [Group C] One or more selected from the group consisting of Cu: 0.50% or less, Ni: 0.70% or less, Sn: 0.30% or less, and Sb: 0.005% or less [Group D] Ca: 0.0050% or less The contents of C, Si, Mn, Cr, Ni, Mo, and Cu in mass% are (C%), (Si%), (Mn%), (Cr%), (Ni%), (Mo%), and (Cu%), respectively, and when the content of B is less than 0.0003%, DI = 0.311 × (C%). 0.5 × (1 + 0.64 × (Si%)) × (1 + 4.10 × (Mn%)) × (1 + 2.33 × (Cr%)) × (1 + 0.25 × (Ni%)) × (1 + 3.14 × (Mo%)) × (1 + 0.27 × (Cu%)), and when the B content is 0.0003 to 0.005%, DI = 0.311 × (C%) 0.5x (1 + 0.64 x (Si %)) x (1 + 4.10 x (Mn %)) x (1 + 2.33 x (Cr %)) x (1 + 0.25 x (Ni %)) x (1 + 3.14 x (Mo %)) x (1 + 0.27 x (Cu %)) x (1 + 1.5 x (0.90 - (C %))), DI is 1.4 or more and 4.5 or less, and when the diameter of the steel wire is D, a total area ratio of ferrite and martensite in the metal structure at a ¼D part that is ¼D deep from the surface of the steel wire in a cross section perpendicular to the longitudinal direction of the steel wire is 30.0% or less, A steel wire having a tensile strength of 860×F1+450 MPa or more and 920×F1+670 MPa or less, where F1=(C%)+0.10×(Si%)+0.18×(Mn%)+0.20×(Cr%), a value of (tensile strength−0.2% proof stress) / uniform elongation of 20+25×(C%) or less, and an area reduction of 66−48×(C%) or more. <3> The steel wire according to <2>, having a chemical composition including, by mass%, the Group A. <4> The steel wire according to <2> or <3>, having a chemical composition including, by mass%, the Group B. <5> The steel wire according to any one of <2> to <4>, having a chemical composition including, by mass%, the Group C. <6> The steel wire according to any one of <2> to <5>, having a chemical composition including, by mass%, the Group D.
[0083] <7> A mechanical part having a cylindrical shaft portion, the chemical composition of which is, in mass%, C: 0.08 to 0.80%, Si: 0.03 to 1.50%, Mn: 0.50 to 2.00%, P: 0.050% or less, S: 0.050% or less, Al: 0.005 to 0.080%, N: 0.0010 to 0.0150%, and O: 0.003% or less, with the balance being Fe and impurity elements, wherein the contents of C, Si, Mn, and Cr, in mass%, are (C%), (Si%), (Mn%), and (Cr%), respectively, and DI = 0.311 × (C%). 0.5× (1 + 0.64 × (Si%)) × (1 + 4.10 × (Mn%)), DI is 1.4 or more and 4.5 or less, where d is the diameter of the shaft portion, a total area fraction of ferrite and martensite in the metal structure at a ¼ d portion that is ¼ d deep from the surface of the shaft portion in a cross section perpendicular to the longitudinal direction of the shaft portion is 30.0%, the shaft portion has a tensile strength of 860 × F1 + 430 MPa or more and 920 × F1 + 660 MPa or less, where F1 = (C%) + 0.10 × (Si%) + 0.18 × (Mn%) + 0.20 × (Cr%), a value of (tensile strength - 0.2% yield strength) / uniform elongation is 38 + 25 × (C%) or less, and 0.2% yield strength / tensile strength is 0.97 - 0.10 × (C%) or more, A mechanical part having a drawing ratio of 65-48×(C%) or more. <8> A mechanical part having a cylindrical shaft portion, the chemical composition of which is, in mass%, C: 0.08 to 0.80%, Si: 0.03 to 1.50%, Mn: 0.50 to 2.00%, P: 0.050% or less, S: 0.050% or less, Al: 0.005 to 0.080%, N: 0.0010 to 0.0150%, O: 0.003% or less, and further containing one or more elements selected from the group consisting of the following A to D groups, with the balance consisting of Fe and impurity elements: [Group A] one or two elements selected from the group consisting of Ti: 0.050% or less, and B: 0.005% or less [Group B] Cr: 1.50% or less, Mo: 0.50% or less, Nb: 0.050% or less, and V: 0.20% or less [Group C] One or more selected from the group consisting of Cu: 0.50% or less, Ni: 0.70% or less, Sn: 0.30% or less, and Sb: 0.005% or less [Group D] Ca: 0.0050% or less The contents of C, Si, Mn, Cr, Ni, Mo, and Cu in mass% are (C%), (Si%), (Mn%), (Cr%), (Ni%), (Mo%), and (Cu%), respectively, and when the content of B is less than 0.0003%, DI = 0.311 × (C%) 0.5× (1 + 0.64 × (Si%)) × (1 + 4.10 × (Mn%)) × (1 + 2.33 × (Cr%)) × (1 + 0.25 × (Ni%)) × (1 + 3.14 × (Mo%)) × (1 + 0.27 × (Cu%)), and when the B content is 0.0003 to 0.005%, DI = 0.311 × (C%) 0.5 x (1 + 0.64 x (Si %)) x (1 + 4.10 x (Mn %)) x (1 + 2.33 x (Cr %)) x (1 + 0.25 x (Ni %)) x (1 + 3.14 x (Mo %)) x (1 + 0.27 x (Cu %)) x (1 + 1.5 x (0.90 - (C %))), DI is 1.4 or more and 4.5 or less, and when the diameter of the shaft portion is d, the total area ratio of ferrite and martensite in the metal structure at a ¼ d portion that is ¼ d deep from the surface of the shaft portion in a cross section perpendicular to the longitudinal direction of the shaft portion is 30.0% or less, and the shaft portion A mechanical component having a tensile strength of 860×F1+430 MPa or more and 920×F1+660 MPa or less, where F1=(C%)+0.10×(Si%)+0.18×(Mn%)+0.20×(Cr%), a value of (tensile strength−0.2% proof stress) / uniform elongation of 38+25×(C%) or less, a 0.2% proof stress / tensile strength of 0.97−0.10×(C%) or more, and a reduction of area of 65−48×(C%) or more. <9> The mechanical component according to <8>, having a chemical composition including Group A by mass%. <10> The mechanical component according to <8> or <9>, having a chemical composition including Group B by mass%. <11> The mechanical component according to any one of <8> to <10>, having a chemical composition including Group C by mass%. <12> The mechanical component according to any one of <8> to <11>, having a chemical composition including, by mass%, the D group.
[0084] The disclosure of Japanese Patent Application No. 2023-059431, filed on March 31, 2023, is incorporated herein by reference in its entirety. All documents, patent applications, and technical standards mentioned herein are incorporated herein by reference to the same extent as if each individual document, patent application, and technical standard was specifically and individually indicated to be incorporated herein by reference.
Claims
1. In mass%, C: 0.08-0.80%, Si: 0.03-1.50%, Mn: 0.50-2.00%, P: 0.050% or less, S: 0.050% or less, Al: 0.005-0.080%, N: 0.0010-0.0150%, O: 0.003% or less, Ti: 0-0.050%, B: 0-0.0050%, Cr: 0-1.50%, Mo: 0-0.50%, Nb: 0-0.050%, V: 0-0.20%, Cu: 0-0.50%, Ni: 0-0.70%, Sn: 0-0.30%, A steel sheet having a chemical composition consisting of Sb: 0-0.005%, and Ca: 0-0.0050%, with the balance consisting of Fe and impurity elements, the contents of C, Si, Mn, Cr, Ni, Mo, and Cu in mass% are (C%), (Si%), (Mn%), (Cr%), (Ni%), (Mo%), and (Cu%), respectively, (I) the chemical composition is, in mass%, C: 0.08-0.80%, Si: 0.03-1.50%, Mn: 0.50-2.00%, P: 0.050% or less, S: 0.050% or less, Al: 0.005-0.080%, N: 0.0010-0.0150%, and O When the content is 0.003% or less and the balance is Fe and impurity elements, DI = 0.311 × (C%) 0.5 (II) when the chemical composition contains, in mass%, one or more elements selected from the group consisting of Ti: 0-0.050%, B: 0-0.0050%, Cr: 0-1.50%, Mo: 0-0.50%, Nb: 0-0.050%, V: 0-0.20%, Cu: 0-0.50%, Ni: 0-0.70%, Sn: 0-0.30%, Sb: 0-0.005%, and Ca: 0-0.0050%, and the B content is less than 0.0003%, DI=0.311×(C%). 0.5 (III) the chemical composition is, in mass %, Ti: 0-0.050%, B: 0-0.0050%, Cr: 0-1.50%, Mo: 0-0.50%, Nb: 0-0.050%, V: 0-0.20%, Cu: 0-0.50%, Ni: 0-0.70%, Sn: 0-0.30%, Sb: 0-0.005%, and Ca: 0-0.0050%, and the content of B is 0.0003 to 0.0050%, DI=0.311×(C%) 0.5 x (1+0.64×(Si%)) x (1+4.10×(Mn%)) x (1+2.33×(Cr%)) x (1+0.25×(Ni%)) x (1+3.14×(Mo%)) x (1+0.27×(Cu%)) x (1+1.5×(0.90-(C%))), DI is 1.40 or more and 4.50 or less, when the diameter of the steel wire is D, a total area ratio of ferrite and martensite in the metal structure at a ¼D part that is ¼D deep from the surface of the steel wire in a cross section perpendicular to the longitudinal direction of the steel wire is 30.0% or less, A steel wire having a tensile strength of 860×F1+450 MPa or more and 920×F1+670 MPa or less, where F1=(C%)+0.10×(Si%)+0.18×(Mn%)+0.20×(Cr%), a value of (tensile strength−0.2% yield strength) / uniform elongation of 20+25×(C%) or less, and a reduction in area of 66−48×(C%) or more.
2. The steel wire according to claim 1, wherein the total area ratio of bainite and pearlite in the metal structure at the 1 / 4D portion is 70.0% or more.
3. A machine part having a cylindrical shaft portion, comprising, in mass%, C: 0.08-0.80%, Si: 0.03-1.50%, Mn: 0.50-2.00%, P: 0.050% or less, S: 0.050% or less, Al: 0.005-0.080%, N: 0.0010-0.0150%, O: 0.003% or less, Ti: 0-0.050%, B: 0-0.0050%, Cr: 0-1.50%, Mo: 0-0.50%, Nb: 0-0.050%, V: 0-0.20%, Cu: 0-0.50%, Ni: 0-0.70%, A steel sheet having a chemical composition of Sn: 0-0.30%, Sb: 0-0.005%, and Ca: 0-0.0050%, with the balance being Fe and impurity elements, and the contents of C, Si, Mn, Cr, Ni, Mo, and Cu in mass % are (C%), (Si%), (Mn%), (Cr%), (Ni%), (Mo%), and (Cu%), respectively, (I) the chemical composition is, in mass %, C: 0.08-0.80%, Si: 0.03-1.50%, Mn: 0.50-2.00%, P: 0.050% or less, S: 0.050% or less, Al: 0.005-0.080%, N: 0.0010-0.0150%, and O: 0.0010-0.0150%. When the content is 0.003% or less and the balance is Fe and impurity elements, DI = 0.311 × (C%) 0.5 (II) when the chemical composition contains, in mass%, one or more elements selected from the group consisting of Ti: 0-0.050%, B: 0-0.0050%, Cr: 0-1.50%, Mo: 0-0.50%, Nb: 0-0.050%, V: 0-0.20%, Cu: 0-0.50%, Ni: 0-0.70%, Sn: 0-0.30%, Sb: 0-0.005%, and Ca: 0-0.0050%, and the B content is less than 0.0003%, DI=0.311×(C%). 0.5 (III) the chemical composition is, in mass %, Ti: 0-0.050%, B: 0-0.0050%, Cr: 0-1.50%, Mo: 0-0.50%, Nb: 0-0.050%, V: 0-0.20%, Cu: 0-0.50%, Ni: 0-0.70%, Sn: 0-0.30%, Sb: 0-0.005%, and Ca: 0-0.0050%, and the content of B is 0.0003 to 0.0050%, DI=0.311×(C%) 0.5 x (1+0.64 x (Si%)) x (1+4.10 x (Mn%)) x (1+2.33 x (Cr%)) x (1+0.25 x (Ni%)) x (1+3.14 x (Mo%)) x (1+0.27 x (Cu%)) x (1+1.5 x (0.90-(C%))), DI is 1.40 or more and 4.50 or less, and when a diameter of the shaft portion is d, a total area ratio of ferrite and martensite in the metal structure at a 1 / 4d portion that is 1 / 4d deep from the surface of the shaft portion in a cross section perpendicular to the longitudinal direction of the shaft portion is 30.0% or less, and the shaft portion is A mechanical part having a tensile strength of 860×F1+430 MPa or more and 920×F1+660 MPa or less, where F1=(C%)+0.10×(Si%)+0.18×(Mn%)+0.20×(Cr%), a value of (tensile strength-0.2% yield strength) / uniform elongation of 38+25×(C%) or less, a 0.2% yield strength / tensile strength of 0.97-0.10×(C%) or more, and a reduction in area of 65-48×(C%) or more.
4. The mechanical component according to claim 3, wherein the total area ratio of bainite and pearlite in the metal structure at the 1 / 4d portion is 70.0% or more.
Citation Information
Patent Citations
Manufacture of steel wire rod for non-heat treated bolt
JP1990166229A
Non-refined steel material for weld bolt and method for producing the same
JP2015190002A
Steel wire, wire for non-heat-treated mechanical components, and non-heat-treated mechanical component
JP2021183710A
Wire material for non-refined machine component; steel wire for non-refined machine component; non-refined machine component; and method for manufacturing wire material for non-refined machine component, steel wire for non-refined machine component, and non-refined machine component
WO2013031640A1
Rod material for non-tempered machine component, steel rod for non-tempered machine component, and non-tempered machine component
WO2016121820A1
Cited By
Wire rod and manufacturing method therefor
WO2026127437A1