Method for improving releasability of regenerated pellets, and coated regenerated pellets

Coating recycled polyarylene sulfide resin pellets with an olefin resin and silicone compounds addresses the poor mold releasability and mold deposit issues, enhancing the efficiency and applicability of recycled materials in molding processes.

WO2024204841A1PCT designated stage expired Publication Date: 2024-10-03POLYPLASTICS CO LTD

Patent Information

Application Number
PCT/JP2024/013423
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-04-01
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Recycled polyarylene sulfide resin pellets exhibit poor mold releasability due to decomposition of matrix polymers, deterioration of additives, and micronization of fillers during the recycling process, leading to reduced fluidity and crystallinity, and the use of mold release agents can result in uneven distribution and increased application frequency, which affects work efficiency and mold deposits.

Method used

Coating recycled polyarylene sulfide resin pellets with a compound comprising an olefin resin, fatty acid derivatives, and silicone compounds, with a total coating amount of 0.04 to 3.0 parts by mass, to improve mold releasability and prevent mold deposits.

Benefits of technology

The coated recycled pellets demonstrate enhanced mold releasability, reducing the frequency of mold release agent application and preventing mold deposits, thereby improving work efficiency and expanding the application range of recycled materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
  • Figure 00000045_0000
    Figure 00000045_0000
Patent Text Reader

Abstract

Provided are: a method for improving the releasability of regenerated pellets from a mold; and coated regenerated resin pellets excellent in releasability from a mold. The method is for improving the releasability of regenerated pellets containing a polyarylene sulfide resin, the method including: coating at least a portion of the surfaces of pellets containing a polyarylene sulfide resin with a compound (A) that includes at least one selected from: (A-1) an olefin resin having a melt viscosity of 0.1 to 8.0 Pa·s at 140°C; (A-2) a fatty acid derivative; and (A-3) a silicone-based compound. The total amount of compound (A) coating is 0.04 to 3.0 parts by mass relative to 100 parts by mass of the pellets (Q).
Need to check novelty before this filing date? Find Prior Art

Description

Method for improving releasability of recycled pellets, and coated recycled pellets

[0001] The present invention relates to a method for improving the releasability of recycled pellets, and to coated recycled pellets.

[0002] Toward the creation of a sustainable recycling-based society, technologies for recycling and utilizing plastic waste have been investigated (for example, Patent Document 1). Polyarylene sulfide resins have excellent heat resistance, mechanical properties, chemical resistance, dimensional stability, and flame retardancy, and are therefore widely used as materials for electrical and electronic equipment components, automobile components, chemical equipment components, etc. Therefore, recycling and utilizing materials containing polyarylene sulfide resins can help create a sustainable recycling-based society.

[0003] Japanese Patent Application Laid-Open No. 2022-103152

[0004] Incidentally, when molding a resin material containing polyarylene sulfide resin, a method of injection molding or extrusion molding a pellet-shaped resin material (hereinafter simply referred to as "pellets") can be generally employed. Furthermore, as a method of obtaining pellets, for example, a method of mixing a polyarylene sulfide resin with other components, such as inorganic fillers as necessary, and melt-kneading and extruding the mixture using a single-screw or twin-screw extruder to obtain pellets can be employed. When recycling materials containing polyarylene sulfide resin, molded products or items discharged after a long period of residence in a cylinder during molding (hereinafter collectively referred to as "recycled products") are crushed and re-pelletized to form recycled pellets (hereinafter also referred to as "repellet"). However, recycled pellets may have decomposed matrix polymers, deteriorated additives, and refined fillers due to shear stress during crushing of the recycled products and thermal history resulting from undergoing one or more molding processes. In such cases, changes in fluidity, crystallinity, polarity, etc. may occur compared to virgin materials that have not undergone a molding process. When such recycled pellets are used alone or as a mixture with virgin material in molding, mold release may be worse than when virgin material is used alone. Reducing the amount of recycled pellets used to prevent poor mold release may result in only small amounts of recycled material being used effectively. While one method of improving mold release is to apply a release agent to the mold used during molding, this can be problematic when the recycled pellet mix ratio is high or when injection molding molded products with a large contact area with the mold. Another method of improving mold release is to supply recycled pellets mixed with a release agent to the raw material supply section during molding. However, segregation between the recycled pellets and the release agent during the raw material supply process can lead to uneven distribution of the release agent in the mixture, resulting in uneven mold release. Furthermore, adding additional components to the recycled material can easily cause mold deposits (MD) during molding, depending on the type and amount of the component, which can lead to mold contamination.

[0005] The present disclosure aims to provide a method for improving the mold releasability of recycled pellets, and to provide coated recycled pellets that have excellent mold releasability. Specifically, the present disclosure aims to provide a recycled polyarylene sulfide resin composition that has excellent mold releasability while suppressing the generation of mold deposits during molding, and a method for producing the same.

[0006] The present disclosure includes the following aspects: [1] A method for improving the mold releasability of recycled pellets containing a polyarylene sulfide resin, comprising coating at least a portion of the surface of pellets (Q) containing a polyarylene sulfide resin with a compound (A) containing one or more selected from (A-1) an olefin resin having a melt viscosity of 0.1 to 8.0 Pa s at 140°C, (A-2) a fatty acid derivative, and (A-3) a silicone-based compound, wherein the total amount of coating with compound (A) is 0.04 to 3.0 parts by mass per 100 parts by mass of pellets (Q) containing a polyarylene sulfide resin. [2] The method according to [1], wherein pellets (Q) containing a polyarylene sulfide resin are recycled pellets (Q2) of an article containing a polyarylene sulfide resin and / or a polyarylene sulfide resin composition. [3] Use of compound (A) for improving the mold releasability of recycled pellets containing a polyarylene sulfide resin, comprising coating at least a portion of the surface of pellets (Q) containing a polyarylene sulfide resin with compound (A) containing one or more selected from (A-1) an olefin resin having a melt viscosity of 0.1 to 8.0 Pa s at 140°C, (A-2) a fatty acid derivative, and (A-3) a silicone compound, wherein the total coating amount of compound (A) is 0.04 to 3.0 parts by mass per 100 parts by mass of pellets (Q) containing the polyarylene sulfide resin. [4] The use according to [3], wherein pellets (Q) containing a polyarylene sulfide resin are recycled pellets (Q2) of an article containing a polyarylene sulfide resin and / or a polyarylene sulfide resin composition. [5] Coated recycled pellets (Y) in which at least a portion of the surface of recycled pellets (X) containing a polyarylene sulfide resin is coated with a compound (A) containing one or more selected from (A-1) an olefin resin having a melt viscosity of 0.1 to 8.0 Pa·s at 140°C, (A-2) a fatty acid derivative, and (A-3) a silicone-based compound, and the total coating amount of compound (A) is 0.04 to 3.0 parts by mass per 100 parts by mass of recycled pellets (X). [6] The release resistance value (R Y) of the recycled pellet (X) containing the uncoated polyarylene sulfide resin not coated with the compound (A) (R X ) to the ratio value [R Y / R X[7] The coated recycled pellet (Y) according to [5], wherein the polyarylene sulfide resin-containing recycled pellet (X) contains an elastomer having a reactive functional group in an amount of 1% by mass or more, based on the total amount of the polyarylene sulfide resin-containing recycled pellet (X). [8] The coated recycled pellet (Y) according to any one of [5] to [7], wherein the polyarylene sulfide resin-containing recycled pellet (X) contains an elastomer containing an α-olefin-derived structural unit and a structural unit derived from a glycidyl ester of an α,β-unsaturated acid. [9] The coated recycled pellet (Y) according to any one of [5] to [7], wherein the polyarylene sulfide resin-containing recycled pellet (X) contains an elastomer having a reactive functional group, and the compound (A) contains (A-1) an olefin resin having a melt viscosity of 0.1 to 8.0 Pa s at 140°C in an amount of 95% by mass or more, based on the total amount of the compound (A).

[10] The coated recycled pellets (Y) according to [5] or [6], wherein the recycled pellets (X) containing a polyarylene sulfide resin do not contain an elastomer having a reactive functional group, or the content of the elastomer having a reactive functional group is less than 1 mass% relative to the total amount of the recycled pellets (X) containing the polyarylene sulfide resin.

[11] A method for producing coated recycled pellets (Y), comprising coating at least a portion of the surface of the recycled pellets (X) containing a polyarylene sulfide resin with a compound (A) containing one or more selected from (A-1) an olefin resin having a melt viscosity of 0.1 to 8.0 Pa s at 140°C, (A-2) a fatty acid derivative, and (A-3) a silicone-based compound, wherein the total amount of the compound (A) is 0.04 to 3.0 parts by mass relative to 100 parts by mass of the recycled pellets (X).

[12] The method for producing the coated recycled pellets (Y) according to

[11] , wherein the compound (A) is in a powder, flake, or granular form, and the coating comprises contacting the recycled pellets (X) containing a polyarylene sulfide resin with the compound (A) at a temperature equal to or higher than the melting point of the compound (A).

[13] The method for producing coated recycled pellets (Y) according to

[11] , wherein the coating step includes contacting recycled pellets (X) containing a polyarylene sulfide resin with a liquid compound (A).

[14] The method includes selecting a compound (A) prior to the coating step, wherein the selection of the compound (A) includes selecting (A-1) a compound (A) containing an olefin resin having a melt viscosity of 0.1 to 8.0 Pa s at 140°C in a total amount of 95% by mass or more relative to the total amount of the compound (A), when the recycled pellets (X) containing a polyarylene sulfide resin contain an elastomer having a reactive functional group in an amount of 1% by mass or more relative to the total amount of the recycled pellets (X) containing a polyarylene sulfide resin, When the recycled pellets (X) containing a polyarylene sulfide resin do not contain an elastomer having a reactive functional group, or the content of the elastomer having a reactive functional group is less than 1 mass% relative to the total amount of the recycled pellets (X) containing a polyarylene sulfide resin, the compound (A) contains one or more selected from (A-1) an olefin resin having a melt viscosity of 0.1 to 8.0 Pa s at 140°C, (A-2) a fatty acid derivative, and (A-3) a silicone-based compound in a total amount of 95 mass% or more relative to the total amount of the compound (A).

[15] A method for producing coated recycled pellets (Y) according to any one of [5] to

[10] , comprising: a polyarylene sulfide resin composition (Z) comprising the coated recycled pellets (Y) according to any one of [5] to

[10] ; and virgin pellets (V) containing a polyarylene sulfide resin.

[16] The polyarylene sulfide resin composition (Z) according to

[15] , wherein the content of the coated recycled pellets (Y) is 50% by mass or more based on the total amount of the coated recycled pellets (Y) and the virgin pellets (V) containing a polyarylene sulfide resin.

[0007] The present invention provides a method for improving the mold releasability of recycled pellets, and a coated recycled pellet having excellent mold releasability. Specifically, the present invention provides a recycled polyarylene sulfide resin composition having excellent mold releasability while suppressing mold deposit generation during molding, and a method for producing the same.

[0008] Fig. 1 is a diagram illustrating a double cylindrical test piece for measuring mold release resistance during molding, (a) is a top view, (b) is a bottom view, (c) is a perspective view, and (d) is a dimensional drawing. Fig. 2 is a schematic diagram of a molded body used for evaluating mold deposits, with the upper side being a top view and the lower side being a cross-sectional view.

[0009] An embodiment of the present disclosure will be described in detail below, but the scope of the present disclosure is not limited to the embodiment described herein, and various modifications can be made without departing from the spirit of the present disclosure. Each aspect disclosed in this specification can be combined with any other feature disclosed in this specification. Furthermore, when multiple upper and lower limit values ​​are described for a specific parameter, any of these upper and lower limit values ​​can be combined to form a suitable numerical range. The expression "X to Y" indicating a numerical range means "X or more and Y or less." If a specific description described for one embodiment also applies to other embodiments, that description may be omitted in other embodiments.

[0010] [First embodiment: method for improving releasability] A method for improving the releasability of recycled pellets according to the present disclosure is a method for improving the releasability of recycled pellets containing a polyarylene sulfide resin, and comprises coating at least a portion of the surface of pellets (Q) containing a polyarylene sulfide resin with compound (A) containing one or more selected from (A-1) an olefin resin having a melt viscosity of 0.1 to 8.0 Pa s at 140°C, (A-2) a fatty acid derivative, and (A-3) a silicone-based compound, wherein the total amount of coating with compound (A) is 0.04 to 3.0 parts by mass per 100 parts by mass of pellets (Q) containing a polyarylene sulfide resin.

[0011] "Improving mold releasability" means that the mold releasability of recycled pellets during molding is improved compared to pellets not coated with compound (A). In one embodiment, the method for improving mold releasability is preferably a method for improving mold releasability while suppressing mold deposit generation during molding. In this specification, "recycling" refers to pulverizing an article (recycled product) such as a molded body and regenerating it as a raw material for use in manufacturing a molded body, and "recycled pellets" refer to the resulting pulverized material melted and then pelletized. In contrast, raw materials not used in manufacturing a molded body (raw materials that have not undergone the molding process) are referred to as "virgin material," and pelletized materials are referred to as "virgin pellets." The recycled article (recycled product) may be a molded product or may be one that has been retained in a cylinder for a long period of time during molding and then ejected. Examples include defective products generated during the manufacturing process of molded products, parts other than the product obtained during injection molding (e.g., runners, sprues, etc.), unused products, and chunks of polyethylene sulfide resin material used for purging during molding. In this specification, "coating" means that at least a portion of the surface of the pellet is covered with compound (A), and may include compound (A) adhering or adhering to a portion of the surface of the pellet, and compound (A) spreading in a layer to cover a portion of the surface. "Adhering or adhering" may include a state in which solid (e.g., powdery) compound (A) is adhered by electrostatic force or the like, or a state in which part of the solid compound (A) is melted, with the remaining part remaining solid, and the melted part adhering to the surface of the pellet.

[0012] In the present disclosure, "recycled pellets containing a polyarylene sulfide resin" (hereinafter also simply referred to as "recycled pellets") refers to pellets obtained by pulverizing an article (a recycled product) containing a polyarylene sulfide resin or a polyarylene sulfide resin composition and regenerating the pellets as a raw material for use in producing a molded article. The shape of the recycled pellets is not particularly limited, and they can be any shape, such as cylindrical (approximately cylindrical), spherical, or the like.

[0013] The pellets (Q) containing a polyarylene sulfide resin (hereinafter also simply referred to as "pellets (Q)") may be virgin pellets or recycled pellets. When the pellets (Q) are virgin pellets (Q1), at least a portion of the surface of the virgin pellets (Q1) containing a polyarylene sulfide resin is coated with the compound (A) described below to form coated virgin pellets (Q1a). Even in this case, the total amount of coating with the compound (A) is 0.04 to 3.0 parts by mass per 100 parts by mass of the virgin pellets (Q1). The obtained coated virgin pellets (Q1a) are once molded into a molded body (or after being discharged after a long residence in the cylinder during molding), and then crushed and repelletized to form recycled pellets. The coated virgin pellets (Q1a) have excellent mold releasability when initially molded, and even when subsequently formed into recycled pellets, they have excellent mold releasability when molded.

[0014] When the pellet (Q) is a recycled pellet (Q2), at least a portion of the surface of the recycled pellet (Q2) containing a polyarylene sulfide resin is coated with the compound (A) described below to produce a coated recycled pellet (Q2a). Even in this case, the total amount of coating with the compound (A) is 0.04 to 3.0 parts by mass per 100 parts by mass of the recycled pellet (Q2). The recycled pellet (Q2) is obtained by pulverizing an article containing a polyarylene sulfide resin (i.e., an article using a polyarylene sulfide resin or a resin composition containing a polyarylene sulfide resin) into pellet form. The coated recycled pellet (Q2a) has excellent releasability from a mold, even when remolded as a recycled pellet. The shape of the pellet (Q) is not particularly limited and can be any shape, such as a cylindrical (approximately cylindrical) or spherical shape. The coated recycled pellets (Q2a) in this embodiment correspond to the coated recycled pellets (Y) in the third embodiment described later, and the recycled pellets (Q2) correspond to the recycled pellets (X) that constitute the coated recycled pellets (Y). In one embodiment, the pellets (Q) containing a polyarylene sulfide resin are preferably recycled pellets (Q2) of an article containing a polyarylene sulfide resin (i.e., an article containing a polyarylene sulfide resin and / or a polyarylene sulfide resin composition).

[0015] Details of the types and amounts of the "polyarylene sulfide resin" and "compound (A)", as well as the coating method, are the same as those described in the section on the coated recycled pellets (Y) and their manufacturing method in the third embodiment described later.

[0016] [Second Embodiment: Use of Compound (A)] The use of compound (A) according to the present disclosure is a use of compound (A) for improving the demolding properties of recycled pellets containing a polyarylene sulfide resin during injection molding, comprising coating at least a portion of the surface of pellets (Q) containing a polyarylene sulfide resin with compound (A) comprising one or more selected from (A-1) an olefin resin having a melt viscosity of 0.1 to 8.0 Pa s at 140°C, (A-2) a fatty acid derivative, and (A-3) a silicone-based compound, wherein the total coating amount of compound (A) is 0.04 to 3.0 parts by mass per 100 parts by mass of pellets (Q). In one embodiment, the pellets containing a polyarylene sulfide resin are preferably recycled pellets of an article containing a polyarylene sulfide resin (i.e., an article containing a polyarylene sulfide resin and / or a polyarylene sulfide resin composition). Details of the types and amounts of the "polyarylene sulfide resin" and "compound (A)", as well as the coating method, are the same as those described in the section on coated recycled pellets (Y) and their production method described below.

[0017] [Third Embodiment: Coated Recycled Pellets (Y)] The coated recycled pellets (Y) according to the present disclosure comprise recycled pellets (X) (hereinafter simply referred to as "pellets (X)") containing a polyarylene sulfide resin, at least a portion of whose surface is coated with compound (A), and the total amount of coating compound (A) is 0.04 to 3.0 parts by mass per 100 parts by mass of the recycled pellets (X). This configuration allows for the production of coated recycled pellets with excellent mold releasability. The coated recycled pellets can be used alone or as a mixture with virgin material. This reduces the number of times a mold release agent needs to be applied to the mold during molding, even when the content of coated recycled pellets (Y) is high (the proportion of coated recycled pellets is 50% or more). This increases the amount of recycled material used and improves work efficiency. Furthermore, excellent mold releasability, even when producing molded products with a large contact area with the mold, broadens the range of part shapes to which the recycled material can be applied. The recycled pellet (X) in this embodiment can also be used as the pellet (Q) described in the section on the method for improving releasability according to the first embodiment and the use of compound (A) according to the second embodiment, and the coated recycled pellet (Y) has the same configuration as the coated recycled pellet (Q2a) in the first embodiment.

[0018] (Recycled Pellets (X)) Recycled pellets (X) are recycled pellets containing a polyarylene sulfide resin, and are pellets obtained by pulverizing an article containing a polyarylene sulfide resin (i.e., an article containing a polyarylene sulfide resin or a polyarylene sulfide resin composition (recycled product)) and recycling it as a raw material for use in producing a molded article. As with the above, the recycled article may be a molded article, or may be an article that has been discharged after being retained in a cylinder for a long period of time during molding. Examples of recycled articles include defective articles generated during the manufacturing process of molded articles, parts other than the product obtained during injection molding (e.g., runners, sprues, etc.), unused products, and chunks of polyarylene sulfide resin material used for purging during molding. The shape of the pellets is not particularly limited, and they may be any shape, such as cylindrical (approximately cylindrical), spherical, etc.

[0019] In one embodiment, the recycled pellets (X) may be pellets of a resin-containing material recycled from molded products of virgin pellets containing a polyarylene sulfide resin, or may be pellets recycled from molded products of recycled material (recycled pellets) containing a polyarylene sulfide resin. Virgin pellets have never undergone a molding process and therefore do not have a thermal history during molding. In contrast, recycled pellets have a thermal history of being heated at high temperatures during the manufacturing stage of the recycled product.

[0020] The polyarylene sulfide resin is a resin having a repeating unit represented by the following general formula (I): -(Ar-S)- (I) (where Ar represents an arylene group).

[0021] The arylene group is not particularly limited, but examples thereof include a p-phenylene group, an m-phenylene group, an o-phenylene group, a substituted phenylene group, a p,p'-diphenylene sulfone group, a p,p'-biphenylene group, a p,p'-diphenylene ether group, a p,p'-diphenylene carbonyl group, and a naphthalene group.

[0022] The polyarylene sulfide resin can be a homopolymer using the same repeating unit represented by the general formula (I) above, or a copolymer containing different repeating units. A preferred homopolymer has a p-phenylene group as the arylene group, that is, a p-phenylene sulfide group as the repeating unit. This is because homopolymers having a p-phenylene sulfide group as the repeating unit have extremely high heat resistance and exhibit high strength, high rigidity, and high dimensional stability over a wide temperature range. By using such homopolymers, molded articles with excellent physical properties can be obtained.

[0023] As the copolymer, a combination of two or more different arylene sulfide groups among the above-mentioned arylene group-containing arylene sulfide groups can be used. Among these, a combination containing a p-phenylene sulfide group and an m-phenylene sulfide group is preferred from the viewpoint of obtaining a molded product with high physical properties such as heat resistance, moldability, and mechanical properties. A polymer containing 70 mol% or more of p-phenylene sulfide groups is more preferred, and a polymer containing 80 mol% or more is even more preferred. The polyarylene sulfide resin containing phenylene sulfide groups is a polyphenylene sulfide resin (PPS resin).

[0024] Polyarylene sulfide resins are generally known to have a substantially linear molecular structure without branching or crosslinking, or a structure with branching or crosslinking, depending on the production method thereof. In one embodiment, from the viewpoint of improving the toughness of a molded article, it is more preferable that the polyarylene sulfide resin does not contain a structure with a crosslinking structure.

[0025] The melt viscosity of the recycled pellets (X) is not limited as long as it does not impair the effects of the present disclosure, and is preferably 310°C and a shear rate of 1200 sec. -1 The melt viscosity measured by the method may be 5 to 300 Pa·s, or may be 8 to 250 Pa·s.

[0026] The recycled pellets (X) may contain other components contained in the recycled product. In one embodiment, the content of the polyarylene sulfide resin in the recycled pellets (X) is preferably 30 to 99% by mass, more preferably 50 to 95% by mass, based on the total amount of the recycled pellets (X). In one embodiment, the content of the polyarylene sulfide resin in the thermoplastic resin (excluding elastomers) contained in the recycled pellets (X) is preferably 80 to 100% by mass, more preferably 90 to 100% by mass, based on the total amount of the thermoplastic resin (excluding elastomers).

[0027] Examples of other components that may be contained in the recycled pellets (X) include elastomers, organic or inorganic fillers, mold release agents, and other additives that are generally added to thermoplastic resins (for example, flame retardants, colorants such as dyes and pigments, stabilizers such as antioxidants and ultraviolet absorbers, lubricants, crystallization accelerators, crystal nucleating agents, etc.).

[0028] Examples of the elastomer include an olefin-based elastomer, a styrene-based elastomer, a polyester-based elastomer, and the like, which may be grafted. It is preferable that the composition contains one or more selected from these, and it is more preferable that the composition contains an olefin-based elastomer.

[0029] The elastomer may be an elastomer having a reactive functional group, such as an acid-modified elastomer modified with an acid or acid anhydride, such as (meth)acrylic acid or maleic anhydride; an elastomer using a copolymerizable monomer having a glycidyl group or an epoxy group (such as glycidyl (meth)acrylate); or an epoxy-modified elastomer obtained by epoxidizing the unsaturated bond of an elastomer.

[0030] Examples of olefin-based elastomers include copolymers of α-olefins and copolymers of α-olefins and copolymerizable monomers. The α-olefin is preferably one or more selected from α-olefins having 2 to 13 carbon atoms (e.g., ethylene, propylene, 1-butene, 1-pentene, 4-methyl-1-pentene, 1-hexene, 1-octene, etc.). Examples of copolymers of α-olefins and copolymerizable monomers include, but are not limited to, α-olefin-unsaturated carboxylic acid alkyl ester copolymers and olefin-based copolymers containing structural units derived from α-olefins and structural units derived from glycidyl esters of α,β-unsaturated acids. Examples of glycidyl esters of α,β-unsaturated acids include, but are not limited to, acrylic acid glycidyl ester, methacrylic acid glycidyl ester, and ethacrylic acid glycidyl ester. Specific preferred examples of the olefin-based elastomer include ethylene propylene rubber (EPR), ethylene-glycidyl methacrylate copolymer (E-GMA), ethylene-glycidyl methacrylate-methyl acrylate copolymer (E-GMA-MA), etc. The olefin-based elastomer may be contained alone or in combination of two or more kinds.

[0031] Examples of styrene-based elastomers include block copolymers composed of a polymer block mainly composed of a vinyl aromatic compound such as styrene and a polymer block mainly composed of an unhydrogenated and / or hydrogenated conjugated diene compound. Specific preferred examples of styrene-based elastomers include styrene-butadiene rubber (SBR) and styrene-ethylene-butylene-styrene block copolymer (SEBS). Furthermore, the styrene-based elastomer may be a modified copolymer into which a functional group (such as an epoxy group, a carboxyl group, or an acid anhydride group) has been introduced. Examples of modified copolymers include epoxidized styrene-diene copolymers in which the unsaturated bond of the diene has been epoxidized (e.g., epoxidized styrene-diene-styrene block copolymers or hydrogenated polymers thereof). The styrene-based elastomers may be used alone or in combination of two or more.

[0032] Examples of polyester-based elastomers include block copolymers having an aromatic polyester such as polyethylene terephthalate or polybutylene terephthalate as a hard segment and a polyether such as polyethylene glycol or polytetramethylene glycol, or an aliphatic polyester such as polyethylene adipate, polybutylene adipate or polycaprolactone as a soft segment. One type of polyester-based elastomer may be contained alone, or two or more types may be contained in combination.

[0033] Elastomers are sometimes blended with virgin materials to improve impact resistance, etc., but in recycled pellets, at least a portion of their chemical structure may change due to shear during crushing of the recycled product or thermal history resulting from undergoing one or more molding processes, which can lead to poor mold releasability. In particular, if the elastomer has reactive functional groups, mold releasability may be further impaired when molding a recycled material containing a polyarylene sulfide resin. However, the coated recycled pellets (Y) according to the present disclosure can improve mold releasability during molding, even when the recycled pellets (X) contain an elastomer (particularly an elastomer having reactive functional groups). In one embodiment, the recycled pellets (X) may contain an elastomer having reactive functional groups. In another embodiment, the recycled pellets (X) may not contain an elastomer having reactive functional groups, or the content of the elastomer may be less than 5% by mass, less than 1% by mass, or less than 0.01% by mass relative to the total amount of the recycled pellets (X).

[0034] The term "reactive functional group" as used herein refers to a functional group that has a high affinity (reactivity) with a metal material at the melting temperature of the resin. Examples of reactive functional groups include glycidyl groups, epoxy groups, carboxyl groups, hydroxyl groups, acid anhydride groups, salts of carboxyl groups, carboxylic acid ester groups, amide groups, amino groups, isocyanate groups, isothiocyanate groups, acetoxy groups, silanol groups, alkoxysilane groups, alkynyl groups, oxazoline groups, thiol groups, and sulfonic acid groups. In one embodiment, the elastomer may include an olefin-based elastomer, a styrene-based elastomer, or a polyester-based elastomer containing one or more groups selected from the group consisting of glycidyl groups, epoxy groups, carboxyl groups, hydroxyl groups, acid anhydride groups, salts of carboxyl groups, carboxylic acid ester groups, amide groups, and amino groups, isocyanate groups, isothiocyanate groups, acetoxy groups, silanol groups, alkoxysilane groups, alkynyl groups, oxazoline groups, thiol groups, and sulfonic acid groups.

[0035] In one embodiment, the recycled pellets (X) may contain, as the elastomer having a reactive functional group, one or more selected from an olefin-based elastomer containing a structural unit derived from an α-olefin and a structural unit derived from a glycidyl ester of an α,β-unsaturated acid, and a styrene-based elastomer containing an epoxidized styrene-diene copolymer in which the unsaturated bond of the diene has been epoxidized.

[0036] In one embodiment, the recycled pellets (X) may include an elastomer including structural units derived from an α-olefin and structural units derived from a glycidyl ester of an α,β-unsaturated acid. In one embodiment, the recycled pellets (X) may include an elastomer including a glycidyl ester of methacrylic acid.

[0037] In one embodiment, when the elastomer has a reactive functional group, the content of the reactive functional group may be 0.1 to 10 mass %, or may be 0.5 to 8 mass %, of the total amount of the elastomer. The content of the reactive functional group can be calculated from the manufacturer's catalog value of the copolymer composition and the molecular weight of the functional group.

[0038] In one embodiment, the content of the elastomer is preferably 1% by mass or more, more preferably 1 to 20% by mass, and even more preferably 2 to 15% by mass, based on the total amount of the recycled pellets (X). In one embodiment, the recycled pellets (X) may contain the elastomer having a reactive functional group in an amount of 1% by mass or more, 2% by mass or more, or 3 to 10% by mass, based on the total amount of the recycled pellets (X).

[0039] In another embodiment, the content of the elastomer may be less than 1% by mass, less than 0.8% by mass, or even 0% by mass, based on the total amount of the recycled pellets (X).

[0040] Examples of organic or inorganic fillers include fibrous fillers such as glass fibers, carbon fibers, zinc oxide fibers, titanium oxide fibers, wollastonite, silica fibers, silica-alumina fibers, alumina fibers, zirconia fibers, boron nitride fibers, silicon nitride fibers, boron fibers, potassium titanate fibers, stainless steel fibers, aluminum fibers, titanium fibers, copper fibers, brass fibers, polyamides, high molecular weight polyethylene, aramids, fluororesins, polyester resins, and acrylic resins, and other high-melting point organic fibrous substances; carbon black, graphite, silica, quartz powder, glass beads, Examples of fillers include milled glass fiber, glass balloons, glass powder, talc (granular), silicates such as calcium silicate, aluminum silicate, and diatomaceous earth, metal oxides such as iron oxide, titanium oxide, zinc oxide, and granular alumina, metal carbonates such as calcium carbonate and magnesium carbonate, metal sulfates such as calcium sulfate and barium sulfate, and powdery and granular fillers such as silicon carbide, silicon nitride, boron nitride, and various metal powders; and plate-like fillers such as mica, glass flakes, talc (plate-like), mica, kaolin, clay, alumina (plate-like), and various metal foils. In terms of mechanical strength, heat resistance, etc., it is preferable to contain an inorganic filler.

[0041] The content of the organic or inorganic filler in the recycled pellets (X) is preferably 10 to 70% by mass, more preferably 15 to 65% by mass, and even more preferably 20 to 60% by mass.

[0042] The recycled pellets (X) may contain a release agent. The release agent contained in the recycled pellets (X) is not particularly limited as long as it is a commonly available agent. Examples include fatty acid esters, fatty acid metal salts, fatty acid amides, and low-molecular-weight polyolefins. For example, a fatty acid ester of pentaerythritol (e.g., pentaerythritol tetrastearate) may be used. When the recycled pellets (X) contain a release agent, the content of the release agent is preferably 0.04 to 3.0 mass% of the total amount of the recycled pellets (X), more preferably 0.07 to 2.5 mass%, and even more preferably 0.1 to 2.0 mass%. The release agent in the recycled pellets (X) can be distinguished from the specific compound (A) described below in that it is present in a state kneaded into the pellets. For example, compound (A) can be extracted by washing the recycled pellets (X) with an organic solvent such as acetone or chloroform and dissolving the compound (A) on the surface in the solvent, as described below. However, the release agent kneaded into the pellets cannot be extracted by this method.

[0043] The method for producing the recycled pellets (X) is not limited, and examples include a method in which a molded product of a polyarylene sulfide resin (preferably a molded product of a virgin polyarylene sulfide resin) is crushed using a known crusher, and the crushed product is melt-kneaded and extruded using a conventionally known single-screw or twin-screw extruder, and then cut into pellets. The melt-kneading temperature is a temperature above the melting point of the polyarylene sulfide resin contained in the recycled pellets (X), and is typically 280 to 360°C, preferably 290 to 350°C. The average particle size of the crushed product is not limited, and for example, the volume-based cumulative 50% diameter (D50) measured by a laser diffraction scattering method is preferably 0.3 to 20 mm, more preferably 0.4 to 15 mm, even more preferably 1 to 10 mm, and more preferably 1 to 3 mm.

[0044] Examples of recycled products that are used as raw materials for the recycled pellets (X) include defective products generated during the manufacturing process of molded products, parts other than the product obtained during injection molding (e.g., runners, sprues, etc.), unused products, and chunks of polyethylene sulfide resin material used for purging during molding, and it is preferable that the recycled product contains one or more selected from these. In one embodiment, the recycled product may be an injection-molded product.

[0045] (Compound (A)) Recycled pellets (X) containing polyarylene sulfide resin have at least a portion of their surface coated with compound (A). By coating at least a portion of the surface of recycled pellets (X) with compound (A), coated recycled pellets (Y) with excellent mold releasability can be obtained. As described above, "coating" means that at least a portion of the pellet's surface is covered with compound (A), and may include compound (A) adhering or adhering to a portion of the pellet's surface, and compound (A) spreading in a layer to cover a portion of the surface. "Adhesion or adhering" may include a state in which solid (e.g., powdery) compound (A) is adhered by electrostatic force or the like, or a state in which part of the solid compound (A) is melted, and the remaining part remains solid, with the melted part adhering to the pellet's surface. From the viewpoint of preventing uneven distribution of compound (A) during the raw material supply process during molding and thus reducing the likelihood of uneven release properties, it is preferable that at least a portion (more preferably the entirety) of the surface of pellets (X) containing a polyarylene sulfide resin is coated with compound (A) in the form of a layer. That at least a portion of the surface of recycled pellets (X) is coated with compound (A) can be confirmed by directly measuring the pellets using an ATR method or the like, or by washing the pellets with an organic solvent such as acetone or chloroform, dissolving the compound (A) on the surface in the solvent, extracting the compound (A) adhering to the surface, and subjecting it to FT-IR measurement, for example.

[0046] In one embodiment, the recycled pellet (X) is preferably continuously covered on at least a portion of its surface with the compound (A), from the viewpoint of preventing uneven distribution of the compound (A) during the raw material supply process during molding and thus reducing the occurrence of uneven release properties. In one embodiment, the recycled pellet (X) is preferably provided with a layer or thin film (hereinafter collectively referred to as a "layer") of the compound (A) on at least a portion of its surface, from the viewpoint of preventing uneven distribution of the compound (A) during the raw material supply process during molding and thus reducing the occurrence of uneven release properties. In one embodiment, the layer of the compound (A) is preferably formed with a spread over at least a portion of the surface of the recycled pellet (X), from the viewpoint of preventing uneven distribution of the compound (A) during the raw material supply process during molding and thus reducing the occurrence of uneven release properties. In one embodiment, the compound (A) is preferably adhered to at least a portion of the surface of the recycled pellet (X), from the viewpoint of preventing uneven distribution of the compound (A) during the raw material supply process during molding and thus reducing the occurrence of uneven release properties. As described above, "adhered" means that the pellet and at least a portion of the compound (A) are fused together.

[0047] In one embodiment, compound (A) may be an organic substance that is solid or liquid at room temperature (20 to 25°C). In another embodiment, compound (A) may be an organic substance that is solid at room temperature (20 to 25°C) and has a melting point of 50 to 135°C (preferably 55 to 130°C, more preferably 70 to 125°C, 90 to 120°C). The melting point is a value measured according to the DSC method (method described in JIS K7121). In this specification, room temperature (20 to 25°C) preferably means 25°C.

[0048] Examples of the compound (A) include (A-1) an olefin resin having a melt viscosity of 0.1 to 8.0 Pa s at 140°C (hereinafter also referred to as "(A-1) olefin resin"), (A-2) a fatty acid derivative, and (A-3) a silicone-based compound, and it is preferable to include at least one selected from these.

[0049] In one embodiment, the content of one or more compounds selected from (A-1) an olefin resin having a melt viscosity of 0.1 to 8.0 Pa·s at 140°C, (A-2) a fatty acid derivative, and (A-3) a silicone-based compound is preferably 95% by mass or more, more preferably 98% by mass or more, in total, relative to the total amount of compound (A). It is even more preferable that compound (A) consists of one or more compounds selected from these. Examples of (A-1) an olefin resin having a melt viscosity of 0.1 to 8.0 Pa·s at 140°C include polyolefin resins having a degree of polymerization of about 500 to 1000 and 1 to 10 (preferably 1 to 4) carbon atoms. Specific examples include polyethylene resins, polypropylene resins, and ethylene-olefin copolymers having a degree of polymerization of 500 to 1000. These (A-1) olefin resins may be used alone or in combination of two or more. Among these, it is preferable to include a polyethylene resin and / or a polypropylene resin, and it is more preferable to include a polyethylene resin.

[0050] The melt viscosity of the (A-1) olefin resin at 140°C is 0.1 to 8.0 Pa·s, preferably 0.5 to 7.0 Pa·s, more preferably 1.0 to 6.5 Pa·s, and particularly preferably 2.0 to 6.0 Pa·s. (A-1) olefin resins having a melt viscosity of 0.1 to 8.0 Pa·s at 140°C have good dispersibility when coating pellets, and are easily coated uniformly over the entire pellet. As a result, good mold release properties can be easily achieved. Furthermore, since the (A-1) olefin resin is less likely to decompose during molding, volatile components derived from the (A-1) olefin resin are easily reduced, and mold deposits (MD) can be reduced. The melt viscosity at 140°C can be measured using a B-type viscometer (e.g., the "RB-80H" manufactured by Toki Sangyo Co., Ltd.) in accordance with JIS K7117.

[0051] The (A-2) fatty acid derivative is a substituted saturated fatty acid and / or unsaturated fatty acid having at least one carboxyl group, or a compound obtained by a chemical reaction between a saturated fatty acid and / or an unsaturated fatty acid and another compound. Examples of the (A-2) fatty acid derivative include fatty acid salts, fatty acid esters, and fatty acid amides, and it is preferable to include at least one selected from these.

[0052] Examples of fatty acid salts include fatty acid metal salts, such as lithium salts, calcium salts, magnesium salts, zinc salts, and aluminum salts of fatty acids (preferably saturated or unsaturated C8-35 fatty acids, more preferably saturated or unsaturated C10-20 fatty acids). Examples of saturated or unsaturated C8-35 fatty acids include saturated fatty acids such as lauric acid (dodecanoic acid), isodecanoic acid, tridecylic acid, myristic acid (tetradecanoic acid), pentadecylic acid, palmitic acid (hexadecanoic acid), margaric acid (heptadecanoic acid), stearic acid (octadecanoic acid), isostearic acid, tuberculostearic acid (nonadecanoic acid), 2-hydroxystearic acid, arachidic acid (icosanoic acid), behenic acid (docosanoic acid), lignoceric acid (tetradocosanoic acid), cerotic acid (hexadocosanoic acid), montanic acid (octadocosanoic acid), and melissic acid. and unsaturated fatty acids such as myristoleic acid (tetradecenoic acid), palmitoleic acid (hexadecenoic acid), oleic acid (cis-9-octadecenoic acid), elaidic acid (trans-9-octadecenoic acid), ricinoleic acid (octadecadienoic acid), vaccenic acid (cis-11-octadecenoic acid), linoleic acid (octadecadienoic acid), linolenic acid (9,11,13-octadecatrienoic acid), elestearic acid (9,11,13-octadecatrienoic acid), gadoleic acid (icosanoic acid), erucic acid (docosanoic acid), and nervonic acid (tetradocosanoic acid). These fatty acid metal salts may be used alone or in combination of two or more. Among these, from the viewpoints of cost and availability, zinc salts, calcium salts, or aluminum salts of fatty acids having less than 22 carbon atoms, such as lauric acid, myristic acid, palmitic acid, stearic acid, and oleic acid, are preferred, with calcium stearate and magnesium stearate being more preferred.

[0053] Examples of fatty acid esters include esters of aliphatic alcohols and fatty acids, with esters of polyhydric alcohols and fatty acids being preferred. Examples of polyhydric alcohols include glycol, polyglycol, glycerin, polyglycerin, propylene glycol, pentaerythritol, sorbitol, mannitol, and the like. Examples of fatty acids include saturated or unsaturated C8-35 fatty acids (preferably C10-20 fatty acids), and examples thereof include the fatty acids described above for the fatty acid metal salts. These fatty acid esters may be used alone or in combination of two or more. Among these, from the standpoints of cost and availability, esters of one or more selected from glycol, propylene glycol, and pentaerythritol with one or more fatty acids selected from fatty acids having less than 22 carbon atoms, such as lauric acid, myristic acid, palmitic acid, stearic acid, and oleic acid, are preferred, with pentaerythritol stearates such as pentaerythritol tristearate and pentaerythritol tetrastearate being more preferred.

[0054] Examples of fatty acid amides include C8-35 fatty acid amides and alkylene fatty acid amides. Examples of C8-35 fatty acid amides include oleic acid amide, stearic acid amide, erucic acid amide, behenic acid amide, ethylene bisstearic acid amide, ethylene bisoleic acid amide, ethylene biserucic acid amide, and ethylene bislauric acid amide. Examples of alkylene fatty acid amides include methylene bisstearic acid amide and ethylene bisstearic acid amide. These fatty acid amides may be used alone or in combination of two or more. Of these, ethylene bisstearic acid amide is more preferred from the viewpoints of cost and availability.

[0055] Examples of the silicone compound (A-3) include silicone oil and silicone resin. The silicone compound (A-3) may be used alone or in combination of two or more. Among these, silicone oil is more preferred from the viewpoints of cost and availability.

[0056] The inventors' research has revealed that when recycled pellets (X) containing a polyarylene sulfide resin contain an elastomer having a reactive functional group, the releasability can be further improved by selecting and using, from the above-mentioned compounds (A), a compound (A) having a high content of (A-1) an olefin resin having a melt viscosity at 140°C of 0.1 to 8.0 Pa s (or consisting of such a compound).

[0057] In one embodiment, when the recycled pellets (X) contain an elastomer having a reactive functional group (preferably the content of the elastomer having a reactive functional group is preferably 1% by mass or more, more preferably 3 to 10% by mass, relative to the total amount of the recycled pellets (X)), from the viewpoint of further improving releasability, the compound (A) preferably contains (A-1) an olefin resin having a melt viscosity of 0.1 to 8.0 Pa s at 140°C, more preferably 95% by mass or more, or 98% by mass or more, of the (A-1) olefin resin having a melt viscosity of 0.1 to 8.0 Pa s at 140°C, relative to the total amount of the compound (A), and even more preferably consists of (A-1) an olefin resin having a melt viscosity of 0.1 to 8.0 Pa s at 140°C.

[0058] In one embodiment, when the recycled pellets (X) contain an elastomer having a reactive functional group (preferably the content of the elastomer having a reactive functional group is preferably 1% by mass or more, more preferably 3 to 10% by mass, relative to the total amount of the recycled pellets (X)), it is preferable that the compound (A) contains (A-1) an olefin resin having a melt viscosity of 0.1 to 8.0 Pa s at 140°C in an amount of 95% by mass or more, relative to the total amount of the compound (A), and does not contain (A-2) a fatty acid derivative or (A-3) a silicone-based compound, or the contents of the (A-2) fatty acid derivative and the (A-3) silicone-based compound are less than 5% by mass in total, relative to the total amount of the compound (A).

[0059] In one embodiment, the recycled pellets (X) comprise an elastomer containing structural units derived from an α-olefin and structural units derived from a glycidyl ester of an α,β-unsaturated acid, and the compound (A) contains 95% by mass or more (preferably 98% by mass or more, and more preferably 98% by mass or more, of an olefin resin (A-1) having a melt viscosity at 140°C of 0.1 to 8.0 Pa s) relative to the total amount of the compound (A).

[0060] In another embodiment, when the recycled pellets (X) do not contain an elastomer having a reactive functional group, or the content of the elastomer having a reactive functional group is less than 1 mass%, preferably less than 0.8 mass%, relative to the total amount of the recycled pellets (X), the compound (A) may contain one or more selected from the above-mentioned (A-1) olefin resin having a melt viscosity at 140°C of 0.1 to 8.0 Pa·s, (A-2) fatty acid derivative, and (A-3) silicone-based compound, and from the viewpoint of easier improvement of releasability, it preferably contains one or more selected from (A-1) olefin resin having a melt viscosity at 140°C of 0.1 to 8.0 Pa·s, and (A-2) fatty acid ester.

[0061] (Coating Amount) The total coating amount of compound (A) is 0.04 to 3.0 parts by mass relative to 100 parts by mass of recycled pellets (X), preferably 0.07 to 2.5 parts by mass, more preferably 0.1 to 2.0 parts by mass, even more preferably 0.1 to 1.0 parts by mass, and particularly preferably 0.1 to 0.5 parts by mass. By making the amount 0.04 parts by mass or more relative to 100 parts by mass of recycled pellets (X), the releasability from the mold when molding the coated recycled pellets (Y) can be improved. By making the amount 3.0 parts by mass or less, the occurrence of mold deposits (MD) can be suppressed. The total coating amount of compound (A) may be 0.1 parts by mass, 0.2 parts by mass, or 0.3 parts by mass within the range of 0.04 to 3.0 parts by mass relative to 100 parts by mass of recycled pellets (X), and these may be the upper and / or lower limits.

[0062] (Other Additives) The coated recycled pellets (Y) may contain additives as needed. Examples of the additives include the same components as those that may be contained in the above-mentioned recycled pellets (X).

[0063] In the coated recycled pellets (Y), at least a portion of the surface of the recycled pellets (X) is coated with the compound (A), so that the compound (A) is uniformly dispersed in the aggregate of the coated recycled pellets (Y), and excellent releasability can be realized. In one embodiment, the coated recycled pellets (Y) have a release resistance value (R Y ) of the uncoated recycled pellet (X) not coated with the compound (A) X ) to the ratio value [R Y / R X ] is preferably less than 0.98, and more preferably 0.95 or less.

[0064] (Release resistance) Release resistance value (R Y ), (R X ) is the double cylinder demolding resistance value, which means the resistance when the double cylindrical molded product shown in Figure 1 is demolded from the mold. Figure 1(a) is a top view of the double cylindrical molded product, Figure 1(b) is a bottom view of the double cylindrical molded product, Figure 1(c) is a perspective view of the double cylindrical molded product, and Figure 1(d) is a dimensional diagram of the double cylindrical molded product, with the dimensions in Figures 1(a) and 1(d) being in mm. The gate size of the double cylindrical molded product is 5 mm x 2.5 mm.

[0065] The double cylindrical molded product shown in Figure 1 has a double cylindrical shape with a first cylinder 1 on the inside and a second cylinder 2 on the outside, and the first cylinder 1 and the second cylinder 2 are connected at four points by a 4 mm axis. The first cylinder 1 has a height of 20 mm, an outer diameter of 18 mm, and an inner diameter of 9 mm, while the second cylinder 2 has a height of 40 mm, an outer diameter of 40 mm, and an inner diameter of 30 mm. The thickness of the side surface of the first cylinder 1 is 4.5 mm, and the thickness of the bottom and side surfaces of the second cylinder 2 is 5 mm. The second cylinder 2 is a bottomed cylinder, but has an opening at the portion of the first cylinder 1.

[0066] (Mold Adhesion) In one embodiment, the coated recycled pellets (Y) preferably have a mold adhesivity of 100 μg or less, more preferably 90 μg or less, and even more preferably 80 μg or less, measured under the following conditions. A molded article having the dimensions and shape shown in FIG. 2 is continuously molded for 4 hours (1,000 times) using the injection molding machine and conditions described below. The total weight of the vent portion and cavity portion removed from the mold is measured before and after continuous molding. The change in the total weight of the vent portion and cavity portion before and after continuous molding is calculated as the weight (μg) of the adhesivity to the mold. Injection molding machine: FANUC ROBOSHOT S2000i30A Cylinder temperature: 340°C Injection time: 2 seconds Cooling time: 10 seconds Mold temperature: 140°C

[0067] (Uses) The coated recycled pellets (Y) can be suitably used as resin pellets for injection molding or resin pellets for extrusion molding.

[0068] [Fourth embodiment: manufacturing method of coated recycled pellets (Y)] The manufacturing method of coated recycled pellets (Y) according to this embodiment includes coating at least a portion of the surface of recycled pellets (X) with compound (A) (hereinafter also referred to as the "coating step"), and the total amount of compound (A) blended is 0.04 to 3.0 parts by mass per 100 parts by mass of recycled pellets (X). The above descriptions regarding the recycled pellets (X), compound (A) and additives, and their blending amounts also apply here.

[0069] The total amount of compound (A) is 0.04 to 3.0 parts by mass relative to 100 parts by mass of recycled pellets (X), preferably 0.07 to 2.5 parts by mass, more preferably 0.1 to 2.0 parts by mass, even more preferably 0.1 to 1.0 parts by mass, and particularly preferably 0.1 to 0.5 parts by mass. By incorporating 0.04 parts by mass or more relative to 100 parts by mass of recycled pellets (X), the releasability from the mold when molding the coated recycled pellets (Y) can be improved. By incorporating 3.0 parts by mass or less, the occurrence of mold deposits can be suppressed. The type of compound (A) is as described above. In one embodiment, compound (A) preferably includes one or more selected from (A-1) an olefin resin having a melt viscosity of 0.1 to 8.0 Pa·s at 140°C, (A-2) a fatty acid derivative, and (A-3) a silicone-based compound.

[0070] (Coating Step) In the coating step, at least a portion of the surface of the recycled pellets (X) is coated with the compound (A). Examples of the coating method include a method of contacting the recycled pellets (X) with a solid or liquid compound (A) at a temperature equal to or higher than the melting point of the compound (A) (hereinafter referred to as "coating method (1)"), and a method of contacting the recycled pellets (X) with a liquid compound (A) (hereinafter referred to as "coating method (2)").

[0071] (Coating method (1)) Coating method (1) is a method of contacting recycled pellets (X) with compound (A) at a temperature equal to or higher than the melting point of compound (A). In one embodiment, coating method (1) is preferably a method of contacting recycled pellets (X) with solid or liquid compound (A) at a temperature equal to or higher than the melting point of compound (A) and equal to or lower than the melting point (Tm1) (°C) of the polyarylene sulfide resin contained in recycled pellets (X). In the present disclosure, the melting point of compound (A) is a value measured according to the DSC method (method described in JIS K7121). The melting point of the polyarylene sulfide resin contained in recycled pellets (X) is the melting point Tm1 measured with a differential scanning calorimeter, and is the peak top temperature of the endothermic peak observed when heated (1st RUN) from room temperature at a heating rate of 10°C / min according to a method based on JIS K7121. In one embodiment, from the viewpoint of facilitating coating, the melting point of the compound (A) is preferably 50 to 135° C., more preferably 55 to 130° C., even more preferably 70 to 125° C., and most preferably 90 to 120° C. The melting point is a value measured according to a DSC method (the method described in JIS K7121).

[0072] In the coating method (1), the temperature at which the recycled pellets (X) are brought into contact with the compound (A) may be, for example, 80 to 160° C., or 100 to 140° C. The contact time is not limited and may be, for example, 5 minutes or more, or 3 to 8 hours.

[0073] The contacting method is not limited, and the recycled pellets (X) and the compound (A) can be contacted with each other in a known dryer such as an air circulation dryer, while heating or after heating, preferably with stirring. In one embodiment, the contacting may be mixing the recycled pellets (X) and the compound (A).

[0074] Generally, when producing a molded product using resin pellets, a step of drying the raw material resin pellets is often included. In one embodiment, the coating step can be carried out by coating method (1) in a step of drying the recycled pellets (X) at a temperature equal to or higher than the melting point of the compound (A), or immediately after the drying step, in a state where the temperature of the recycled pellets (X) is equal to or higher than the melting point (°C) of the compound (A). By carrying out the coating step in the step of drying the recycled pellets (X) (or immediately after the drying step), the heat from the drying step can be effectively utilized to coat the recycled pellets (X).

[0075] The compound (A) used in the coating method (1) may be solid or liquid at room temperature (20 to 25°C), and is preferably solid. When the compound (A) is solid, it is easier to handle. Even when the compound (A) is solid, it is brought into contact with the recycled pellets (X) at a temperature equal to or higher than the melting point of the compound (A), so that the compound (A) melts and can wet and spread over at least a portion of the surface of the recycled pellets (X). As a result, at least a portion of the surface of the recycled pellets (X) can be coated. In one embodiment, the compound (A) is preferably in a powder, flake, or granular form.

[0076] In one embodiment, the method for producing the coated recycled pellets (Y) can be configured so that the compound (A) is in a powder, flake, or granular form, and includes contacting the recycled pellets (X) with the compound (A) at a temperature equal to or higher than the melting point of the compound (A).

[0077] (Coating method (2)) Coating method (2) is a method in which a liquid compound (A) is brought into contact with the recycled pellets (X). The liquid compound (A) may be a compound (A) that is liquid at room temperature (20 to 25°C), or may be a liquid compound (A) obtained by heating a compound (A) that is solid at room temperature (20 to 25°C) to a temperature equal to or higher than its melting point. Alternatively, it may be a liquid compound (A) obtained by dissolving a compound (A) that is solid at room temperature (20 to 25°C) in a solvent. By using a liquid compound (A), it is not necessary to heat the recycled pellets (X) in the coating step.

[0078] The contact method is not limited, and examples thereof include a method of applying the liquid compound (A) to the surface of the recycled pellets (X) by coating, spraying, etc., and a method of stirring and mixing the recycled pellets (X) and the liquid compound (A).

[0079] After the coating step, the obtained coated recycled pellets (Y) are preferably cooled to room temperature (e.g., 25°C) to 80°C, more preferably room temperature to 40°C, to fix the surface coating layer (or coated portion). Fixing the coating layer makes it possible to maintain a uniformly dispersed state of the compound, thereby improving stable mold releasability. The cooling method is not limited, and may be allowed to stand, blow air, or the like.

[0080] (Step of selecting compound (A)) The method for producing coated recycled pellets (Y) may include selecting a compound (A) prior to coating. As described above, when the recycled pellets (X) contain an elastomer having a reactive functional group, the compound (A) can be selected and used to further improve releasability by selecting (A-1) a compound (A) having a high content of (or consisting of) an olefin resin having a melt viscosity of 0.1 to 8.0 Pa s at 140°C.

[0081] In one embodiment, the selection of compound (A) includes: (A-1) selecting a compound (A) containing an olefin resin having a melt viscosity of 0.1 to 8.0 Pa s at 140°C, preferably a C1-4 olefin resin such as a polyethylene resin, an ethylene copolymer, or a polypropylene resin, when the recycled pellets (X) contain an elastomer having a reactive functional group in an amount of 1% by mass or more (preferably 2% by mass or more, more preferably 3 to 10% by mass) relative to the total amount of the recycled pellets (X); When the recycled pellets (X) do not contain an elastomer having a reactive functional group, or the content of the elastomer having a reactive functional group is less than 1 mass%, preferably less than 0.8 mass%, of the total amount of the recycled pellets (X), a compound (A) is selected that contains one or more selected from (A-1) an olefin resin having a melt viscosity at 140°C of 0.1 to 8.0 Pa·s, (A-2) a fatty acid derivative, and (A-3) a silicone-based compound in a total amount of 95 mass% or more relative to the total amount of the compound (A) (preferably consisting of one or more selected from these), preferably a compound (A) containing one or more selected from (A-1) an olefin resin having a melt viscosity at 140°C of 0.1 to 8.0 Pa·s and (A-2) a fatty acid ester, more preferably a compound (A) containing one or more selected from a C1-4 olefin-based resin such as a polyethylene resin, an ethylene copolymer, or a polypropylene resin; and a C8-35 fatty acid ester such as pentaerythritol tristearate or pentaerythritol tetrastearate.

[0082] [Fifth embodiment: Manufacturing method for molded articles containing coated recycled pellets (Y)] The coated recycled pellets (Y) can be molded and processed by known methods such as injection molding, profile / solidification extrusion, press molding, and spinning. The coated recycled pellets (Y) have excellent mold releasability, so the number of times a mold release agent needs to be applied to the mold during molding can be reduced. Furthermore, even when producing molded articles with a large contact area with the mold, the excellent mold releasability from the mold allows for a wider range of part shape options.

[0083] In one embodiment, a method for producing a molded article containing the coated recycled pellets (Y) includes continuously injecting or extruding the above-described coated recycled pellets (Y) into a mold together with other thermoplastic resins and additives as necessary, and applying a release agent to the mold, and the number of times the release agent is applied to the mold may be once for every 10 or more injections or extrusions. The release agent to be applied to the mold is not limited, and can be selected from known release agents.

[0084] The coated recycled pellets (Y) have excellent releasability from a mold, so even when injection molding or extrusion molding a molded product with a large contact area with the mold, the number of times a mold release agent needs to be applied to the mold can be reduced.

[0085] [Sixth embodiment: Polyarylene sulfide resin composition (Z)] The coated recycled pellets (Y) described above can be mixed with other thermoplastic resins as needed to be used as a molding material. Examples of the other thermoplastic resins include virgin pellets containing polyarylene sulfide resins, and preferably virgin pellets containing polyarylene sulfide resins.

[0086] In one embodiment, the polyarylene sulfide resin composition (Z) preferably contains coated recycled pellets (Y) and virgin pellets (V) containing a polyarylene sulfide resin (hereinafter also simply referred to as "virgin pellets (V)"). By containing the coated recycled pellets (Y), it is possible to effectively utilize the recycled material and obtain a resin composition with excellent mold releasability. By containing the virgin pellets (V), it is possible to reinforce the excellent physical properties of the polyarylene sulfide resin.

[0087] The content of the coated recycled pellets (Y) is preferably 50% by mass or more, more preferably 50 to 99.99% by mass, and even more preferably 60 to 100% by mass, of the total amount of the coated recycled pellets (Y) and the virgin pellets (V) containing the polyarylene sulfide resin. The polyarylene sulfide resin composition (Z) has excellent releasability from a mold even when the content of the coated recycled pellets (Y) is high.

[0088] Examples of the polyarylene sulfide resin contained in the virgin pellets (V) include those described in the section on recycled pellets (X) above. From the viewpoint of quality control, etc., it is preferable that the virgin pellets (V) have the same composition as the polyarylene sulfide resin in the recycled pellets (X). The term "virgin pellets (V)" may include virgin polyarylene sulfide resins and compositions thereof. Like the recycled pellets (X), the virgin pellets (V) may contain other components such as elastomers, organic or inorganic fillers, mold release agents, and other additives commonly added to thermoplastic resins (e.g., flame retardants, colorants such as dyes and pigments, stabilizers such as antioxidants and UV absorbers, lubricants, crystallization accelerators, crystal nucleating agents, etc.). Details of the other components are as described above. In one embodiment, from the viewpoint of quality control, etc., it is preferable that the virgin pellets (V) have the same composition as the recycled pellets (X) with respect to components other than the polyarylene sulfide resin (e.g., the same type and content of additives). In one embodiment, if the recycled pellets (X) do not contain an elastomer having a reactive functional group, it is preferable that the virgin pellets (V) also do not contain an elastomer having a reactive functional group. In this case, the compound (A) may or may not be contained. If the compound (A) is contained, the type of compound (A) is not limited. In another embodiment, if the recycled pellets (X) contain an elastomer having a reactive functional group, it is preferable that the virgin pellets (V) also contain an elastomer having a reactive functional group, and it is more preferable that the type and content of the elastomer are the same. In this case, it is preferable that the virgin pellets (V) contain the compound (A), and it is more preferable to select an olefin resin (A-1) having a melt viscosity at 140°C of 0.1 to 8.0 Pa·s.

[0089] The melt viscosity of the virgin pellets (V) is not particularly limited as long as it is within a range that does not impair the effects of the present disclosure. However, from the viewpoint of the balance between mechanical properties and fluidity, it is preferable to use a melt viscosity of 310°C and a shear rate of 1200 sec. -1 The melt viscosity measured by is preferably 300 Pa·s or less, more preferably 250 Pa·s or less.

[0090] The method for producing the polyarylene sulfide resin composition (Z) is not limited, and the coated recycled pellets (Y) and another thermoplastic resin (preferably virgin pellets containing a polyarylene sulfide resin) may be dry-blended, or may be melt-kneaded using a conventionally known melt-kneading device such as a single-screw or twin-screw extruder, or may be mixed in the hopper (material supply member) of an injection molding machine.

[0091] The method for producing a molded article containing the polyarylene sulfide resin composition (Z) can be carried out in the same manner as the method for producing a molded article containing the coated recycled pellets (Y) described above.

[0092] (Uses) The polyarylene sulfide resin composition (Z) can be suitably used as a resin composition for injection molding or a resin composition for extrusion molding.

[0093] The present invention will be explained in more detail below by showing examples, but the interpretation of the present invention is not limited to these examples.

[0094] [Materials] (Recycled PPS pellets (X1)) An injection-molded product of a resin composition containing 65 mass% polyphenylene sulfide resin (manufactured by Kureha Corporation, Fortron (registered trademark) KPS), 30 mass% glass fiber, and 4 mass% elastomer (composition: E-GMA-MA (glycidyl methacrylate content: 3 mass%)), with the remainder being additives, was pulverized using a mechanical pulverizer to obtain a pulverized product. The pulverized product was melt-kneaded and extruded at 320°C using a twin-screw extruder to obtain recycled PPS pellets (X1).

[0095] (Recycled PPS pellets (X2)) An injection-molded product of a resin composition (containing no elastomer component) containing 69 mass% polyphenylene sulfide resin (manufactured by Kureha Corporation, Fortron (registered trademark) KPS), 30 mass% glass fiber, and the remainder additives was pulverized using a mechanical pulverizer to obtain a pulverized product, which was melt-kneaded and extruded at 320°C using a twin-screw extruder to obtain recycled PPS pellets (X2).

[0096] (PPS virgin pellets (X3)) Pellets of a resin composition (virgin material having the same composition as the resin composition used in the PPS recycled pellets (X1)) containing 65 mass % of polyphenylene sulfide resin (Fortron (registered trademark) KPS, manufactured by Kureha Corporation), 30 mass % of glass fiber, and 4 mass % of elastomer (composition: E-GMA-MA (glycidyl methacrylate content: 3 mass %)), with the remainder being additives, were used as PPS virgin pellets (X3).

[0097] Compound (A1): polyethylene resin (Sanyo Chemical Industries, Ltd., "SANWAX 161-P", granular, melting point 103°C, melt viscosity at 140°C 4.3 Pa s) Compound (A2): pentaerythritol stearate (NOF Corporation, "UNISTAR H476", melting point 63°C) The melting points of compound (A1) and compound (A2) and the melt viscosity at 140°C of compound (A1) were measured by the following method. (Melting Point) Using a DSC device (TA Instrument, differential scanning calorimeter, DSC-Q1000), the melting point (Tm) was measured by the DSC method (method described in JIS K7121) under conditions of a nitrogen atmosphere and a heating rate of 10°C / min. (Viscosity at 140°C) The viscosity was measured at 140°C using a Brookfield viscometer (RB-80H manufactured by Toki Sangyo Co., Ltd.) in accordance with JIS K7117 (1999).

[0098] [Examples 1 to 4] 3 kg of ground PPS recycled pellets (X1) or (X2) listed in Table 1 was placed in a metal container (30 cm x 60 cm x 15 cm), and compound (A1) was added in the proportions listed in Table 1. The mixture was dried at 140°C for 3 hours in a blower dryer and then cooled to room temperature. The mixture was then stirred (dispersed) in a mixer to obtain coated recycled pellets. Compound (A1) was dissolved and added during the drying process. In the obtained coated recycled pellets, at least a portion of the surface of the PPS recycled pellets (X1) or (X2) was coated with compound (A1).

[0099] Example 5: 3 kg of ground PPS recycled pellets (X1) were placed in a metal container (30 cm x 60 cm x 15 cm), and compound (A2) was added in the proportions shown in Table 2. The mixture was dried in a fan dryer at 140°C for 3 hours and then cooled to room temperature. The mixture was then stirred (dispersed) in a mixer to obtain coated recycled pellets. Compound (A2) was dissolved and added during the drying process. In the obtained coated recycled pellets, at least a portion of the surface of the PPS recycled pellets (X1) was coated with compound (A2).

[0100] Example 6 3 kg of virgin PPS pellets (X3) were placed in a metal container (30 cm x 60 cm x 15 cm), and 6 g of compound (A1) was added. The mixture was dried in a fan dryer at 140°C for 3 hours and then cooled to room temperature. The mixture was then stirred (dispersed) in a mixer to obtain coated pellets. Compound (A1) was dissolved and added during the drying process. In the obtained coated pellets, at least a portion of the surface of the virgin PPS pellets (X3) was coated with compound (A1). An injection-molded product of the obtained coated pellets was pulverized using a mechanical pulverizer, and the pulverized material was melt-kneaded and extruded at 320°C using a twin-screw extruder to obtain recycled PPS pellets (X3).

[0101] Comparative Example 1 Recycled PPS pellets (X1) were used without being coated with compound (A).

[0102] Comparative Example 2 Recycled PPS pellets (X2) were used without being coated with compound (A).

[0103] Comparative Examples 3 to 5: 3 kg of ground PPS recycled pellets (X1) or (X2) listed in Table 1 was placed in a metal container (30 cm x 60 cm x 15 cm), dried in a fan dryer at 140°C for 3 hours, and then cooled to room temperature. Compound (A1) was added in the proportion listed in Table 1, and then the mixture was stirred (dispersed) in a mixer. In this method, compound (A1) was added in a solid state. Visual inspection of the pellet surface revealed that compound (A) was not attached to the pellet surface.

[0104] [Comparative Examples 6 and 7] 3 kg of ground PPS recycled pellets (X1) were placed in a metal container (30 cm x 60 cm x 15 cm), and compound (A1) was added in the proportions shown in Table 2. The mixture was dried in a fan dryer at 140°C for 3 hours and then cooled to room temperature. The mixture was then stirred (dispersed) in a mixer to obtain coated recycled pellets. Compound (A1) was dissolved and added during the drying process. In the obtained coated recycled pellets, at least a portion of the surface of the PPS recycled pellets (X1) was coated with compound (A1).

[0105] [Mold Release Resistance] Using the pellets of the Examples and Comparative Examples, the mold release resistance was measured by the following method. The results are shown in Table 1. Using an injection molding machine, a double cylindrical molded article as shown in FIG. 1 was molded under the following conditions, and the force when the molded piece (test piece) was extruded from the mold was measured, and the measured value was taken as the mold release resistance value. During injection molding, the hopper capacity amount was supplied to the hopper (i.e., the amount supplied in one go without replenishment), and the mold release resistance was measured when 80% by mass was consumed. Pressure sensor: "Indirect type in-mold sensor" (model: 9221A) manufactured by Nippon Kistler Co., Ltd. Injection molding machine: "EC60Ni1.5A" manufactured by Toshiba Machine Co., Ltd. Cylinder temperature: 320°C Injection time: 12 seconds Cooling time: 45 seconds Mold temperature: 150°C

[0106] The release resistance values ​​of Examples 1 to 3 and Comparative Examples 3 and 4 are shown as R Y The release resistance value of Comparative Example 1 is R X As R X R against Y The ratio value [R Y / R X Similarly, the release resistance values ​​of Example 4 and Comparative Example 5 were calculated as R Y The release resistance value of Comparative Example 2 is R X As R X R against Y The ratio value [R Y / R X The results are shown in Table 1. Y / R X When [R Y / R XWhen the value of R is 0.98 or more, the mold release properties are still insufficient. Y The release resistance value of Comparative Example 1 is R X As R X R against Y The ratio value [R Y / R X The results are shown in Table 2.

[0107] [Evaluation of Mold Adhesion] Using the pellets of the Examples and Comparative Examples, mold adhesion was measured by the following method. The results are shown in Tables 1 and 2. A nested mold with detachable vent and cavity sections was used. Using each re-pellet material, molded articles having the dimensions and shape shown in Figure 2 were continuously molded (1,000 times) for 4 hours using the injection molding machine and conditions below. The total weight of the vent and cavity sections removed from the mold was measured before and after continuous molding. The change in the total weight of the vent and cavity sections before and after continuous molding was calculated as the weight (μg) of adhesion to the mold. Injection molding machine: FANUC ROBOSHOT S2000i30A Cylinder temperature: 340°C Injection time: 2 seconds Cooling time: 10 seconds Mold temperature: 140°C When the amount of mold adhesion is 100 μg or less, there is an effect of suppressing mold deposits, when it is 90 μg or less there is an excellent effect of suppressing mold deposits, and when it is 80 μg or less there is an even better effect of suppressing mold deposits.

[0108]

[0109] As shown in Table 1, the pellets of Examples 1 to 3, in which at least a portion of the surface of the recycled PPS pellets (X1) was coated with the compound (A1), had a lower release resistance than the recycled PPS pellets (X1) of Comparative Example 1, and the release resistance value (R X ) to the ratio of the release resistance value [R Y / R XThe pellets of Example 4, in which at least a portion of the surface of the recycled PPS pellets (X2) is coated with compound (A1), have a lower mold release resistance than the recycled PPS pellets (X2) of Comparative Example 2, and the mold release resistance (R X ) to the ratio of the release resistance value [R Y / R X ] is less than 0.98, and the mold releasability is improved. As shown in Examples 1 to 4, by contacting the PPS recycled pellets (X1) or (X2) with the compound (A1) at a temperature equal to or higher than the melting point of the compound (A1), at least a portion of the surface of the PPS recycled pellets (X1) or (X2) is coated with the compound (A). The obtained coated recycled pellets have a mold release resistance (R X ) to the ratio of the release resistance value [R Y / R X As shown in Comparative Examples 3 to 5, even when compound (A) is added during molding, if compound (A) is not attached to the surface of the PPS recycled pellets, compound (A) segregates during molding, and the effect of improving mold releasability is not sufficiently achieved.

[0110] As shown in Table 2, the pellets of Example 5, in which at least a portion of the surface of the recycled PPS pellets (X1) is coated with the compound (A2), have a lower release resistance than the recycled PPS pellets (X1) of Comparative Example 1, and the release resistance value (R X ) to the ratio of the release resistance value [R Y / R X] is less than 0.98, and the mold releasability from the mold is improved. Furthermore, the PPS recycled pellets (X3) of Example 6, which were produced from pellets in which at least a portion of the surface of the PPS virgin pellets (X3) was coated with compound (A1), had a lower mold release resistance than the PPS recycled pellets (X1) of Comparative Example 1, even though the recycled pellets were not coated with compound (A1) during production. Furthermore, the mold release resistance value (R X ) to the ratio of the release resistance value [R Y / R X ] is less than 0.98, and the mold releasability from the mold is improved. Comparing Example 2 with Example 5, when the recycled material (X1) containing the elastomer having a reactive functional group is used, by using the compound (A) containing the olefin resin having a melt viscosity at 140°C of 0.1 to 8.0 Pa s as the compound (A), the ratio of the mold release resistance values ​​[R Y / R X As shown in Comparative Example 6, even when the compound (A1) is attached to the surface of the PPS recycled pellets, if the compound (A1) is added in a small amount, the release resistance value (R X ) to the ratio of the release resistance value [R Y / R X ] exceeds 0.98, and the mold releasability from the mold is insufficient.

[0111] As shown in Tables 1 and 2, the recycled PPS pellets of Examples had a mold deposit of 80 g or less, and were more effective in suppressing mold deposits. In contrast, the recycled PPS pellets of Comparative Example 7 had a mold deposit of more than 100 g, resulting in the generation of large amounts of mold deposits.

[0112] The method for improving the mold releasability of recycled pellets according to the present disclosure can improve mold releasability when using recycled pellets for molding, thereby increasing productivity and having industrial applicability. The coated recycled pellets according to the present disclosure have excellent mold releasability, so they can be suitably used as resin pellets for injection molding or extrusion molding, and have industrial applicability.

Claims

1. A method for improving the releasability of recycled pellets containing a polyarylene sulfide resin, comprising coating at least a portion of the surface of pellets (Q) containing a polyarylene sulfide resin with a compound (A) containing one or more selected from (A-1) an olefin resin having a melt viscosity of 0.1 to 8.0 Pa·s at 140°C, (A-2) a fatty acid derivative, and (A-3) a silicone-based compound, wherein the total amount of coating with compound (A) is 0.04 to 3.0 parts by mass per 100 parts by mass of pellets (Q) containing a polyarylene sulfide resin.

2. The method according to claim 1, wherein the pellets (Q) containing the polyarylene sulfide resin are recycled pellets (Q2) of an article containing a polyarylene sulfide resin.

3. Use of compound (A) for improving the releasability of recycled pellets containing a polyarylene sulfide resin, comprising coating at least a portion of the surface of pellets (Q) containing a polyarylene sulfide resin with compound (A) containing one or more selected from (A-1) an olefin resin having a melt viscosity of 0.1 to 8.0 Pa·s at 140°C, (A-2) a fatty acid derivative, and (A-3) a silicone-based compound, wherein the total coating amount of compound (A) is 0.04 to 3.0 parts by mass per 100 parts by mass of pellets (Q) containing a polyarylene sulfide resin.

4. The use according to claim 3, wherein the pellets (Q) containing a polyarylene sulfide resin are recycled pellets (Q2) of an article containing a polyarylene sulfide resin.

5. Coated recycled pellets (Y), in which at least a portion of the surface of recycled pellets (X) containing a polyarylene sulfide resin is coated with a compound (A) containing one or more selected from (A-1) an olefin resin having a melt viscosity of 0.1 to 8.0 Pa·s at 140°C, (A-2) a fatty acid derivative, and (A-3) a silicone-based compound, and the total coating amount of compound (A) is 0.04 to 3.0 parts by mass per 100 parts by mass of the recycled pellets (X).

6. Release resistance value of coated recycled pellets (Y) (R Y ) of the regenerated pellet (X) containing an uncoated polyarylene sulfide resin that is not coated with the compound (A) (R X ) to the ratio value [R Y / R X 6. The coated recycled pellet (Y) according to claim 5, wherein the value of is less than 0.

98.

7. The coated recycled pellet (Y) according to claim 5 or 6, wherein the recycled pellet (X) containing a polyarylene sulfide resin contains an elastomer having a reactive functional group in an amount of 1 mass% or more based on the total amount of the recycled pellet (X) containing a polyarylene sulfide resin.

8. The coated recycled pellets (Y) according to claim 5 or 6, wherein the recycled pellets (X) containing a polyarylene sulfide resin contain an elastomer containing a structural unit derived from an α-olefin and a structural unit derived from a glycidyl ester of an α,β-unsaturated acid.

9. The coated recycled pellets (Y) according to claim 5 or 6, wherein the recycled pellets (X) containing a polyarylene sulfide resin contain an elastomer having a reactive functional group, and the compound (A) contains (A-1) an olefin resin having a melt viscosity of 0.1 to 8.0 Pa·s at 140°C in an amount of 95 mass% or more based on the total amount of the compound (A).

10. The coated recycled pellets (Y) according to claim 5 or 6, wherein the recycled pellets (X) containing a polyarylene sulfide resin do not contain an elastomer having a reactive functional group, or the content of the elastomer having a reactive functional group is less than 1 mass% based on the total amount of the recycled pellets (X) containing a polyarylene sulfide resin.

11. A method for producing coated recycled pellets (Y), comprising coating at least a portion of the surface of recycled pellets (X) containing a polyarylene sulfide resin with a compound (A) containing one or more selected from (A-1) an olefin resin having a melt viscosity of 0.1 to 8.0 Pa·s at 140°C, (A-2) a fatty acid derivative, and (A-3) a silicone-based compound, wherein the total amount of compound (A) is 0.04 to 3.0 parts by mass per 100 parts by mass of the recycled pellets (X).

12. The method for producing coated recycled pellets (Y) according to claim 11, wherein the compound (A) is in the form of a powder, flake or granule, and the coating step comprises contacting the recycled pellets (X) containing a polyarylene sulfide resin with the compound (A) at a temperature equal to or higher than the melting point of the compound (A).

13. The method for producing coated recycled pellets (Y) according to claim 11, wherein the coating step comprises contacting recycled pellets (X) containing a polyarylene sulfide resin with a liquid compound (A).

14. The method includes selecting a compound (A) prior to coating, and selecting the compound (A) includes selecting (A-1) a compound (A) containing an olefin resin having a melt viscosity of 0.1 to 8.0 Pa·s at 140°C in a total amount of 95 mass% or more relative to the total amount of the compound (A) when the recycled pellets (X) containing a polyarylene sulfide resin contain an elastomer having a reactive functional group in an amount of 1 mass% or more relative to the total amount of the recycled pellets (X) containing a polyarylene sulfide resin, In the case where the recycled pellets (X) containing a polyarylene sulfide resin do not contain an elastomer having a reactive functional group, or the content of the elastomer having a reactive functional group is less than 1 mass% relative to the total amount of the recycled pellets (X) containing a polyarylene sulfide resin, the method for producing coated recycled pellets (Y) according to any one of claims 11 to 13 is selected from (A-1) an olefin resin having a melt viscosity at 140 ° C. of 0.1 to 8.0 Pa · s, (A-2) a fatty acid derivative, and (A-3) a silicone-based compound, and the compound (A) contains one or more of these in total at 95 mass % or more relative to the total amount of the compound (A).

15. A polyarylene sulfide resin composition (Z) comprising the coated recycled pellets (Y) according to claim 5 or 6 and virgin pellets (V) containing a polyarylene sulfide resin.

16. The polyarylene sulfide resin composition (Z) according to claim 15, wherein the content of the coated recycled pellets (Y) is 50 mass% or more based on the total amount of the coated recycled pellets (Y) and the virgin pellets (V) containing the polyarylene sulfide resin.

Citation Information

Patent Citations

  • Thermoplastic resin molding material and its production

    JP1992353524A

  • Manufacturing method of thermoplastic resin pellet containing additive

    JP2004169027A

  • Preparation process of polyphenylenesulfide resin composition

    JP2006022326A

  • Self-adhesion preventive agent

    JP2016188327A

  • Gasket for lithium-ion battery

    JP2022165484A

Cited By

  • Method for producing recycled polyarylene sulfide resin composition, and recycled polyarylene sulfide resin composition

    JPWO2025094875A1

  • Method for producing recycled polyarylene sulfide resin composition, and recycled polyarylene sulfide resin composition

    WO2025094875A1