Coating composition, fruit and vegetable with coating film and method for keeping freshness of fruit and vegetable
A sugar-based surfactant and glycerin fatty acid ester coating composition forms a film on fruits and vegetables, addressing the challenges of existing freshness preservation methods by enhancing water and oxygen barrier properties, thus maintaining freshness and stability.
Patent Information
- Application Number
- PCT/JP2024/013461
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2024-03-27
- Filing Date
- 2024-04-01
- Publication Date
- 2024-10-03
AI Technical Summary
Existing methods for preserving the freshness of fruits and vegetables, such as Modified Atmosphere packaging and direct application of quality preserving agents, face challenges including safety concerns, short freshness retention periods, and difficulties in handling and applicability, with existing compositions not effectively preventing pericarp damage and maintaining freshness.
A coating composition comprising a sugar-based surfactant and a glycerin fatty acid ester, with specific mass ratios and properties, is used to form a film on fruits and vegetables, providing a water vapor and oxygen barrier without the need for packaging materials, enhancing freshness retention.
The coating composition effectively suppresses water and oxygen transmission, maintaining the freshness of fruits and vegetables for a longer period, improving storage stability and handling, while being safe for human consumption.
Smart Images

Figure JPOXMLDOC01-APPB-M000001 
Figure JPOXMLDOC01-APPB-M000002 
Figure JPOXMLDOC01-APPB-T000003
Abstract
Description
Coating composition, coated fruits and vegetables, and method for preserving the freshness of fruits and vegetables
[0001] The present invention relates to a coating composition, fruits and vegetables coated with the composition, and a method for preserving the freshness of fruits and vegetables.
[0002] In recent years, packaging materials capable of preserving the freshness of food during distribution or storage, such as modified atmosphere (MA) packaging, have attracted attention. For example, a technology for preserving the freshness of food by providing a layer with a freshness-preserving effect on a film for packaging food has been proposed (see Patent Document 1). Another technology for preserving the freshness of food by directly applying a quality preservative to food, such as fruits and vegetables, has also been proposed (see Patent Documents 2 and 3). In particular, Patent Documents 4 and 5 disclose compositions containing glycerin fatty acid esters as compositions that can be used to form protective coatings on substrates, and state that they can be used to protect substrates, such as food and / or agricultural products, from quality deterioration and / or decomposition due to factors such as moisture loss, oxidation, mechanical degradation, photodegradation, and mold growth.
[0003] JP 2001-171058 JP JP 2018-134115 JP 2005-530502 JP JP 2018-534912 JP JP 2021-536457 JP 8-056564
[0004] In the technology disclosed in Patent Document 1, food may come into contact with the packaging film during distribution or storage, so it is preferable that the layer having a freshness-preserving effect is also highly safe for humans. Furthermore, the methods disclosed in Patent Documents 2 and 3 have a short freshness-preserving period and are not necessarily sufficient for achieving freshness-preserving performance. Furthermore, the compositions disclosed in Patent Documents 4 and 5 have a freshness-preserving effect, but they are not necessarily easy to apply and are difficult to handle. Patent Document 6 describes an agent for preventing skin damage to fruits and vegetables, containing a surfactant with an HLB of 5 or less as an active ingredient. This agent aims to prevent water penetration through the skin of fruits and vegetables, effectively preventing skin damage while avoiding the adverse effects of oil-based coatings. Patent Document 6 overcomes the difficulty of dispersing and dissolving surfactants alone in water by using an emulsifier. The method for producing this agent for preventing skin damage involves adding a heated, melted surfactant to a heated, dissolved emulsifier. Although the method of Patent Document 6 prevents damage to the fruit skin to some extent, it is believed that further improvement can be made in terms of maintaining freshness.
[0005] An object of the present invention is to provide a coating composition capable of directly forming a coating having a freshness-preserving function without using a packaging material, coated fruits and vegetables using the composition, and a method for preserving the freshness of fruits and vegetables.
[0006] As a result of extensive research, the present inventors have found that the above-mentioned problems can be solved by using a composition containing at least two specific fatty acid esters. The present invention was completed based on this finding.
[0007] That is, the present invention has the following aspects: [1] A coating composition containing a sugar-based surfactant and a glycerin fatty acid ester, wherein the mass ratio (solid content) of the sugar-based surfactant to the total mass of the sugar-based surfactant and the glycerin fatty acid ester is 1% or more but less than 100%, and the glycerin fatty acid ester having three fatty acid ester groups accounts for 50% by mass or less. [2] A coating composition containing a sugar-based surfactant and a glycerin fatty acid ester having three fatty acid ester groups at a shear rate of 1 s-1 [1] The coating composition according to the above [1], wherein the shear viscosity at 1000 kJ / min is 0.1 to 8000 mPa·s. [3] The coating composition according to the above [1] or [2], wherein the sugar-based surfactant is a sucrose fatty acid ester. [4] The coating composition according to any one of the above [1] to [3], further comprising an aqueous solvent. [5] The coating composition according to the above [4], wherein the aqueous solvent comprises water or a mixed solvent of water and a water-soluble organic solvent. [6] The coating composition according to any one of the above [1] to [5], wherein the non-volatile component concentration is 0.1% by mass or more and 60% by mass or less. [7] In differential scanning calorimetry at a measurement temperature range of -80°C or more, the total exothermic peak area A 3 The total area A of the endothermic peaks between 0 ° C and 80 ° C 2
[10] A method for preserving the freshness of fruits and vegetables, comprising the step of covering fruits and vegetables with the coating composition according to any one of [1] to [7] above.
[11] The method for preserving the freshness of fruits and vegetables according to
[10] above, wherein the step of covering fruits and vegetables with the coating composition is a step of immersing the fruits and vegetables in the composition, or applying or spraying the composition onto the fruits and vegetables.
[0008] According to the present invention, it is possible to propose a coating composition that can directly form a coating having a freshness-preserving function without using a packaging material, coated fruits and vegetables using said composition, and a method for preserving the freshness of fruits and vegetables.
[0009] [Coating composition] The coating composition of the present invention (hereinafter sometimes referred to as "the composition") contains a sugar-based surfactant and a glycerin fatty acid ester, in which the mass ratio (solid content) of the sugar-based surfactant to the total mass of the sugar-based surfactant and the glycerin fatty acid ester is 1% or more but less than 100%, and the glycerin fatty acid ester (triester) having three fatty acid ester groups is 50% by mass or less. The coating composition of the present invention can be suitably used for fruits and vegetables.
[0010] <Sugar-based surfactants> Sugar-based surfactants are surfactants that contain a sugar, such as a monosaccharide, disaccharide, trisaccharide, tetrasaccharide, polysaccharide, sugar alcohol, or other oligosaccharide, as the hydrophilic group. Examples of sugar-based surfactants include sugar fatty acid esters formed by an ester bond between a sugar and a fatty acid, and alkyl glycosides formed by a glycosidic bond between a sugar and a higher alcohol. Of these, sugar fatty acid esters are preferred from the viewpoint of film-forming properties.
[0011] The sugar-based surfactant is preferably crystalline from the viewpoint of suppressing stickiness of the resulting coating and enhancing the water vapor barrier property and oxygen barrier property. Furthermore, from the viewpoint of suppressing stickiness of the resulting coating, the sugar-based surfactant preferably contains 60% by mass or more, more preferably 70% by mass or more, even more preferably 80% by mass or more, and even more preferably 90% by mass or more of a component that becomes solid at room temperature (20-25°C). The sugar-based surfactant may be composed solely of components that become solid at room temperature (20-25°C), and therefore, the above ratio may be 100% by mass or less.
[0012] The HLB of the sugar-based surfactant is not particularly limited, but from the viewpoint of being able to form a coating using an aqueous solvent described below, it is preferably 5 or more, more preferably 7 or more, and even more preferably 9 or more. The upper limit of the HLB is usually 20, and more preferably 18 or less.
[0013] <Sugar fatty acid ester> The sugar surfactant of the present invention may contain a sugar fatty acid ester. The sugar fatty acid ester is formed by an ester bond between a sugar and a fatty acid.
[0014] The sugar in the sugar fatty acid ester may be any of monosaccharides, disaccharides, trisaccharides, tetrasaccharides, polysaccharides, sugar alcohols, and other oligosaccharides. Examples of monosaccharides include pentoses such as ribulose, xylulose, ribose, arabinose, xylose, lyxose, and deoxyribose; and hexoses such as psicose, fructose, sorbose, tagatose, allose, altrose, glucose, mannose, gulose, idose, galactose, talose, fucose, fuculose, and rhamnose.
[0015] The fatty acids constituting the sugar fatty acid ester may be the same as the constituent fatty acids of the sucrose fatty acid ester described below. The constituent fatty acids of the sugar fatty acid ester do not all need to be the same, as long as 60% by mass or more of the constituent fatty acids in the sugar fatty acid ester are suitable constituent fatty acids described below. From the viewpoint of suppressing stickiness of the resulting coating, this ratio is preferably 70% by mass or more, more preferably 80% by mass or more, and even more preferably 90% by mass or more. There is no particular upper limit, but it is sufficient as long as it is 100% by mass or less. The constituent fatty acid composition of the sugar fatty acid ester can be measured by isolating the sugar fatty acid ester from the composition, derivatizing it, and then analyzing it by gas chromatography.
[0016] The number of fatty acid ester groups in a sugar fatty acid ester varies depending on the number of ester-bondable hydroxyl groups in the molecular structure of the sugar, which is the hydrophilic group; for example, 1 to 8 for sucrose fatty acid esters and 1 to 4 for sorbitan fatty acid esters. From the viewpoint of being dispersible or soluble in aqueous solvents, the sugar surfactant preferably contains 50% by mass or more of sugar fatty acid esters (monoesters, diesters, or triesters) having three or fewer fatty acid ester groups, when the total amount of the sugar surfactant is taken as 100% by mass, more preferably 60% by mass or more, and even more preferably 70% by mass or more. The upper limit is not particularly limited, but it is sufficient as long as it is 100% by mass or less. From the same viewpoint, the sugar surfactant preferably contains 30% by mass or less of sugar fatty acid esters having six or more fatty acid ester groups (hexaesters, heptaesters, octaesters, or more) when the total amount of the sugar surfactant is taken as 100% by mass, more preferably 20% by mass or less, and even more preferably 10% by mass or less. Sugar fatty acid esters having 6 or more fatty acid ester groups may not be contained, and the content thereof may be 0% by mass or more. The content ratio by number of fatty acid ester groups can be measured by the same method as the measurement method described in the section on sucrose fatty acid esters below.
[0017] The sugar fatty acid ester is not particularly limited as long as it is usable for food products, but examples include sucrose fatty acid esters, sorbitan fatty acid esters, glucose esters, etc., with sucrose fatty acid esters being preferred from the viewpoint of easy availability. The sugar-based surfactant may be used alone or in combination of two or more. When two or more types are combined, it is preferable that sucrose fatty acid esters account for 60% by mass or more of the total amount of sugar-based surfactants, taken as 100% by mass. This ratio is more preferably 70% by mass or more, even more preferably 80% by mass or more, and even more preferably 90% by mass or more, from the viewpoint of suppressing stickiness of the resulting coating and enhancing the water vapor barrier property and oxygen barrier property. The sugar-based surfactant may be sucrose fatty acid ester alone, and therefore the above ratio may be 100% by mass or less.
[0018] <Sucrose fatty acid ester> Any known sucrose fatty acid ester can be used as the sucrose fatty acid ester used in the present composition, as long as at least one of the eight hydroxyl groups of sucrose forms an ester structure with a fatty acid.
[0019] The constituent fatty acid of the sucrose fatty acid ester is preferably an edible oil or fat. The number of carbon atoms of the constituent fatty acid of the sucrose fatty acid ester is not particularly limited, but is preferably 12 to 22, more preferably 12 to 18, and even more preferably 14 to 18. Having the carbon number within the above range reduces the stickiness of the resulting coating. The constituent fatty acid of the sucrose fatty acid ester may be a saturated or unsaturated fatty acid, but saturated fatty acids are preferred because they tend to solidify at room temperature (20 to 25°C) and reduce the stickiness of the resulting coating. More specific examples include lauric acid, myristic acid, pentadecylic acid, palmitic acid, palmitoleic acid, margaric acid, stearic acid, oleic acid, etc., and among these, saturated fatty acids having 12 to 18 carbon atoms, such as lauric acid, myristic acid, palmitic acid, and stearic acid, are preferred, and saturated fatty acids having 14 to 18 carbon atoms, such as myristic acid, palmitic acid, and stearic acid, are more preferred. These saturated fatty acids may be used alone or in combination of two or more. The constituent fatty acids of the sugar fatty acid ester do not all need to be the same, as long as 60% by mass or more of the constituent fatty acids in the sucrose fatty acid ester are the above-mentioned suitable constituent fatty acids. From the viewpoint of suppressing the stickiness of the resulting coating, this ratio is preferably 70% by mass or more, more preferably 80% by mass or more, and even more preferably 90% by mass or more. There is no particular upper limit, but it is sufficient as long as it is 100% by mass or less. The constituent fatty acid composition of the sucrose fatty acid ester can be measured by isolating the sucrose fatty acid ester from the composition, derivatizing it, and then gas chromatography.
[0020] The number of fatty acid ester groups in the sucrose fatty acid ester is 1 to 8. From the viewpoint of being able to form a coating using an aqueous solvent, when the total amount of sucrose fatty acid esters is taken as 100% by mass, it is preferable that the sucrose fatty acid esters contain 50% by mass or more of sucrose fatty acid esters (monoesters, diesters, or triesters) having 3 or fewer fatty acid ester groups, more preferably 60% by mass or more, and even more preferably 70% by mass or more. The upper limit is not particularly limited, but it is sufficient that it is 100% by mass or less. From the same viewpoint, when the total amount of sucrose fatty acid esters is taken as 100% by mass, it is preferable that the sucrose fatty acid esters contain 30% by mass or less of sucrose fatty acid esters having 6 or more fatty acid ester groups (hexaesters, heptaesters, octaesters, or more) more preferably 20% by mass or less, and even more preferably 10% by mass or less. Sucrose fatty acid esters having 6 or more fatty acid ester groups may not be contained, and their content may be 0% by mass or more.
[0021] The content ratio by number of fatty acid ester groups can be measured after isolating the sugar fatty acid ester from the composition according to the method of assay described in the Residue Monograph prepared by the meeting of the Joint FAO / WHO Expert Committee on Food Additives (JECFA), 84th meeting 2017, "Sucrose Esters of Fatty Acids," and in the FAO JECFA Monographs 7 (2009), "Sucrose Oligoesters Type I" and "Sucrose Oligoesters Type II," prepared at the 71st JECFA meeting (2009) and published in FAO JECFA Monographs 7 (2009).
[0022] <<Measurement of Monoesters to Triesters and Tetraesters or Higher>> A sample is dissolved in a certain amount of tetrahydrofuran (stabilized GPC or industrial grade), and the insoluble matter is removed using a 0.5 μm membrane filter. This solution is used as a measurement sample and subjected to high performance liquid chromatography under the following conditions. The composition ratio is calculated by individually calculating the peak areas of the monoesters to triesters and the combined peak area of tetraesters or higher, and then calculating the ratio to the total peak area of all peaks detected up to 43 minutes. The peak area corresponds to the area from the start point (rising point) to the end point (falling point) of each peak. If two or more peaks are adjacent and the start and end points are unknown, the points where the data between the peaks is smallest are used as the start and end points, respectively, to calculate the area.
[0023] <Measurement conditions: monoesters to triesters and tetraesters and above> Apparatus: HLC-8320GPC Detector: differential refractometer (manufactured by Tosoh Corporation) Column: TSK-gel G1000HXL, G2000HXL, G3000HXL, G4000HXL (manufactured by Tosoh Corporation) Column temperature: 40°C Detector temperature: 40°C Eluent: tetrahydrofuran (stabilizer-containing GPC or industrial grade) Flow rate: 0.8 ml / min Injection volume: 80 μl Measurement time: 50 minutes (area ratio is calculated based on all peaks detected up to 43 minutes)
[0024] <<Measurement of Tetraesters to Octaesters>> A sample is dissolved in a fixed amount of methanol (special reagent grade) / tetrahydrofuran (stabilizer-free HPLC grade) = 20 / 80 (vol / vol), and the solution is used as a measurement sample after removing insoluble matter with a 0.45 μm membrane filter. High-performance liquid chromatography is performed under the following conditions. The composition ratio of tetraesters to octaesters is calculated by calculating the peak areas of each tetraester to octaester individually, calculating the ratio to the total peak area of tetraesters to octaesters, and then proportionally dividing the area ratio of tetraesters and higher peaks obtained in <<Measurement of Monoesters to Triesters and Tetraesters or Higher>> by the area ratio of tetraesters to octaesters.>> The peak area corresponds to the area from the start point (rising point) to the end point (falling point) of each peak. If two or more peaks are adjacent and the start and end points are unknown, the points with the smallest data between the peaks are used as the start and end points to calculate the area.
[0025] <Measurement conditions: tetraester to octaester> Equipment Degasser: DGU-20A (Shimadzu Corporation) Pump: LC-20AD (Shimadzu Corporation) Oven: CTO-20A (Shimadzu Corporation) Detector: RID-20A differential refractometer (Shimadzu Corporation) Column: 150 mm x 4.6 mm i.d.; ODS-2 (GL Sciences) Column temperature: 40°C Detector temperature: 40°C Eluent: methanol (special reagent grade) / tetrahydrofuran (stabilizer-free HPLC grade) = 70 / 30 to 50 / 50 (vol / vol) Flow rate: 0.8 ml / min Injection volume: 20 μl Measurement time: 16 minutes
[0026] Commercially available products of the sucrose fatty acid esters include "Ryoto (registered trademark) Sugar Ester S-370," "Ryoto (registered trademark) Sugar Ester S-570," "Ryoto Sugar Ester S-970," "Ryoto (registered trademark) Sugar Ester S-1170," "Ryoto (registered trademark) Sugar Ester S-1570," "Ryoto (registered trademark) Sugar Ester S-1670," "Ryoto (registered trademark) Sugar Ester P-170," "Ryoto (registered trademark) Sugar Ester P-1670," "Ryoto (registered trademark) Sugar Ester M-1695," "Ryoto (registered trademark) Sugar Ester O-170," and "Ryoto (registered trademark) Sugar Ester Examples of suitable sucrose fatty acid esters include "Ryoto (registered trademark) Sugar Ester L-1570," "Ryoto (registered trademark) Sugar Ester L-195," "Ryoto (registered trademark) Sugar Ester L-595," "Ryoto (registered trademark) Sugar Ester L-1695," "Ryoto (registered trademark) Sugar Ester B-370," "Ryoto (registered trademark) Sugar Ester ER-190," and "Ryoto (registered trademark) Sugar Ester POS-135" (all manufactured by Mitsubishi Chemical Corporation), and "DK Ester (registered trademark) F-160," "DK Ester (registered trademark) F-140," "DK Ester (registered trademark) F-110," "DK Ester (registered trademark) F-70," and "DK Ester (registered trademark) F-50" (all manufactured by Dai-ichi Kogyo Seiyaku Co., Ltd.). Among these, the use of sucrose fatty acid esters that are solid at 0°C or higher is preferred, as this broadens the range of application of the coating composition of the present invention in industrial applications. These sucrose fatty acid esters may be used alone, or two or more types may be used in combination as a mixture.
[0027] The sucrose fatty acid ester is preferably crystalline from the viewpoint of suppressing stickiness of the resulting coating and enhancing the water vapor barrier property and oxygen barrier property. Furthermore, from the viewpoint of suppressing stickiness of the resulting coating, the sucrose fatty acid ester preferably contains 60% by mass or more, more preferably 70% by mass or more, even more preferably 80% by mass or more, and even more preferably 90% by mass or more of a component that becomes solid at room temperature (20 to 25°C). The sucrose fatty acid ester may be composed solely of components that become solid at room temperature (20 to 25°C), and therefore, the above ratio may be 100% by mass or less.
[0028] The sucrose fatty acid ester is preferably crystalline from the viewpoint of suppressing stickiness of the resulting coating and enhancing water vapor barrier properties. The crystalline melting peak temperature is preferably 40°C or higher and 80°C or lower, more preferably 45°C or higher and 70°C or lower. A crystalline melting peak temperature of 40°C or higher suppresses stickiness of the resulting coating. On the other hand, a crystalline melting peak temperature of 80°C or lower allows for less heating when dissolving in an aqueous solvent, improving productivity. The crystalline melting peak temperature is the temperature at which a crystalline melting peak is detected in differential scanning calorimetry (DSC) measured by placing 1 mg of sucrose fatty acid ester in an aluminum pan and initially heating from 30°C to 100°C at a heating rate of 10°C / min. When there are multiple crystalline melting peaks, it is preferable that the sum of the peak areas within the above temperature range is 50% or more of the sum of the peak areas across the entire temperature range.
[0029] <Other Fatty Acid Esters> The composition may contain other fatty acid esters to the extent that the effects of the present invention are not impaired. The other fatty acid esters are not particularly limited as long as they are usable in foods, and examples thereof include sorbitan fatty acid esters and glucose esters.
[0030] <Glycerin fatty acid ester> Glycerin fatty acid ester is an ester bond between glycerin and a fatty acid. Examples of fatty acids constituting the glycerin fatty acid ester include the same fatty acids as those constituting the sucrose fatty acid ester.
[0031] The content of glycerin fatty acid ester (monoester) having one fatty acid ester group is usually 5% by mass or more when the total amount of glycerin fatty acid ester is taken as 100% by mass, from the viewpoints of dispersibility in aqueous solvents, viscosity of the composition, and handling. 10% by mass or more is preferred, 20% by mass or more is more preferred, 30% by mass or more is even more preferred, and 40% by mass or more is particularly preferred. 50% by mass or more is preferred, 60% by mass or more is more preferred, 70% by mass or more is even more preferred, and 80% by mass or more is particularly preferred. There is no particular upper limit, but it is sufficient as long as it is 100% by mass or less.
[0032] The content of the glycerin fatty acid ester (diester) having two fatty acid ester groups depends on the content of the monoester and triester, and is not particularly limited.
[0033] From the viewpoints of dispersibility in aqueous solvents, viscosity of the composition, and ease of handling, the content of glycerin fatty acid esters (triesters) having three fatty acid ester groups is preferably 50% by mass or less, more preferably 40% by mass or more, even more preferably 30% by mass or more, particularly preferably 20% by mass or more, and most preferably 10% by mass or more, when the total amount of glycerin fatty acid esters is taken as 100% by mass. The lower limit is not particularly limited, but it may not be contained (0% by mass), or may contain less than 1% by mass as an impurity, or may be 0.5% by mass or more.
[0034] From the viewpoints of dispersibility in aqueous solvents, viscosity of the composition, and ease of handling, when the total amount of glycerin fatty acid esters is taken as 100% by mass, the total amount of glycerin fatty acid esters (monoesters) having one fatty acid ester group and fatty acid esters (diesters) having two fatty acid ester groups is preferably 50% by mass or more, more preferably 60% by mass or more, and even more preferably 70% by mass or more. There are no particular limitations on the upper limit, but it is sufficient that it is 100% by mass or less. Of these, the proportion of monoesters when the monoesters and diesters are combined is preferably 20% by mass or more, more preferably 40% by mass or more, even more preferably 50% by mass or more, particularly preferably 60% by mass or more, and most preferably 80% by mass. There are no particular limitations on the upper limit, but it is sufficient that it is 100% by mass or less.
[0035] The types and amounts of fatty acids can be analyzed by column chromatography, gas chromatography, thin layer chromatography, high performance liquid chromatography, colorimetric analysis, or the like.
[0036] <Mass Ratio> The mass ratio (solids content) of the sucrose fatty acid ester to the total mass of the sucrose fatty acid ester and the glycerin fatty acid ester is preferably 1% or more, more preferably 5% or more, even more preferably 10% or more, and particularly preferably 20% or more. Furthermore, this ratio is less than 100%. Within this range, the composition exhibits good applicability, resulting in a good coating appearance after application to fruits and vegetables. From the above viewpoints, the mass ratio of the sucrose fatty acid ester to the glycerin fatty acid ester is preferably 1 / 99 to 99 / 1, more preferably 5 / 95 to 99 / 1, even more preferably 10 / 90 to 98 / 2, particularly preferably 20 / 80 to 97 / 3, and most preferably 20 / 80 to 80 / 20.
[0037] <Aqueous Solvent> The present composition may be solvent-free, but preferably contains a solvent from the viewpoint of application efficiency. The solvent preferably contains an aqueous solvent. The aqueous solvent constituting the coating composition is water or a mixed solvent of water and one or more water-soluble organic solvents. Examples of the water-soluble organic solvent include alcohols such as ethanol, isopropanol, ethylene glycol, and glycerin. From the viewpoint of being able to be applied to food, an aqueous composition using water as the solvent is preferred. However, from the viewpoint of stability and application property, an organic solvent such as the above-mentioned alcohol may be contained in addition to water as the solvent. The content of the organic solvent in the aqueous solvent is preferably 30% by mass or less, more preferably 20% by mass or less, even more preferably 10% by mass or less, and even more preferably 5% by mass or less.
[0038] <Other Components> The coating composition of the present invention may contain other components in amounts that do not impair the function of the coating composition of the present invention. Examples of other components include pH adjusters. Examples of pH adjusters that can be used include acetic acid, lactic acid, citric acid, and ammonia.
[0039] <Differential Scanning Calorimetry at 0°C or Higher> The coating composition of the present invention has a total endothermic peak area A in the range of 0°C to 40°C in differential scanning calorimetry at a measurement temperature range of 0°C or higher. 1 The total area A of the endothermic peaks between 0 ° C and 80 ° C 2 The ratio of the coating composition to the total amount of the raw material may be 50% or less. The ratio is preferably 40% or less, more preferably 30% or less, and even more preferably 20% or less. The ratio may be 0%. By being within this range, the phase change rate of the film formed on the coating composition is reduced within the practical temperature range for storing, transporting, and selling fruits and vegetables that are not stored frozen, and no phase change that affects the properties of the film occurs. For example, freshness-preserving functions such as water vapor barrier properties and oxygen barrier properties, which will be described later, can be maintained. The peak area is the area from the start point (rising point) to the end point (falling point) of each peak. In addition, A 1The temperature range when calculating is preferably 0°C or higher and 35°C or lower, more preferably 0°C or higher and 30°C or lower, and even more preferably 0°C or higher and 25°C or lower. This indicates that it is within the temperature range that is preferable for practical use as described above. By setting the measurement temperature range to 0°C or higher, it becomes possible to reflect the properties of the coating in the practical temperature range in which fruits and vegetables that are not stored frozen are stored, transported, and sold. For example, for a compound with a melting point of less than 0°C, setting the measurement range to less than 0°C makes it possible to perform measurements that reflect behaviors such as the phase change from liquid to solid, crystallization of uncrystallized components, and melting of solids. However, these behaviors are not exhibited within the practical temperature range described above, and it is difficult to say that the measurements reflect practical behavior. A 1 and A 2 Regarding the total area, there may be cases where multiple peaks exist within each temperature range for which the total area is calculated, or where only a portion of a peak falls within that temperature range. In such cases, for all peaks present within that temperature range, the total area of only the portion that falls within that temperature range is calculated. For example, if one broad peak exists between 0 and 50°C, only the portion between 0 and 40°C is used as A. 1 It is considered that the surfactant used in the coating composition of the present invention has almost no peak in the temperature range exceeding 80°C. 2 Regarding the temperature range above 80°C, it is not considered necessary to consider the temperature range above 80°C.
[0040] Differential scanning calorimetry, with a measurement temperature range of 0°C or higher, is performed under the following conditions: Measurement device: differential scanning calorimeter Measurement method: heat flux method Temperature: 25°C → 0°C → 100°C Temperature increase / decrease rate: 10°C / min Atmosphere: nitrogen Sample preparation: The coating composition is placed in an empty aluminum pan so that the dry solid content is 1 mg, and the pan is left to dry at room temperature. It is confirmed that the weight change from the previous day is 1% or less, and a measurement sample is obtained. Reference: aluminum pan Note that for a sample in which no peak is observed when the temperature is increased or decreased below 0°C, the temperature may be decreased from 25°C to below 0°C, and then increased to 100°C for measurement.
[0041] <Differential Scanning Calorimetry at −80° C. or Higher> The coating composition of the present invention has a total exothermic peak area A 3 The total area A of the endothermic peaks between 0 ° C and 80 ° C 2 The ratio of the coating composition to the total surface area of the coating composition may be 50% or less. By being within this range, the stickiness of the coating formed from the coating composition can be reduced within the temperature range in which fruits and vegetables that are not stored frozen are stored, transported, and sold, improving handleability, and further improving freshness-retaining properties such as water vapor barrier property and oxygen barrier property, which will be described later. The peak area is the area from the start point (rising point) to the end point (falling point) of each peak. The exothermic peak is thought to indicate the phase change behavior in which a component that was not solid becomes solid, or the crystallization behavior of a component that was not crystallized. On the other hand, the endothermic peak observed at 0°C or higher is thought to be a peak resulting from the phase change behavior of all components in the coating formed from the coating composition that can become solid, for example, the behavior in which all crystallizable components of the coating crystallize. Therefore, the total exothermic peak area A 3 The total area A of the endothermic peaks between 0 ° C and 80 ° C 2 The ratio of A to B is considered to indicate the ratio of components in the coating film formed from the coating composition that are not solid at temperatures above 0°C, e.g., not crystallized. From the viewpoint of enhancing the above-mentioned effect, this ratio is preferably 40% or less, more preferably 30% or less, and even more preferably 20% or less. Note that the exothermic peak observed by the measurement method described below may be observed during temperature rise. This is considered to indicate the behavior of components that have been in a supercooled state becoming solid, e.g., crystallizing. A 2 and A 3 Regarding the temperature ranges for which the total area is calculated, there may be cases where multiple peaks exist within the respective temperature ranges. In such cases, the total area of only the parts of all peaks within the temperature range is calculated. Although unlikely, it is also possible that one peak exists within a temperature range that includes 0°C. In such cases, the peak area is calculated as A depending on whether it is an endothermic peak or an exothermic peak.2 and A 3 It is considered that the surfactant used in the coating composition of the present invention has almost no peaks in the temperature range below -80°C or above 80°C. 2 and A 3 Regarding the temperature range, it is not considered necessary to consider the range below -80°C and above 80°C.
[0042] Differential scanning calorimetry with a measurement temperature range of -80°C or higher is carried out under the following conditions. Measurement device: differential scanning calorimeter Measurement method: heat flux method Temperature: 25°C → -80°C → 100°C Temperature increase / decrease rate: 10°C / min Atmosphere: nitrogen Sample preparation: The coating composition is placed in an empty aluminum pan so that the dry solid content is 1 mg, and the pan is left to dry at room temperature. It is confirmed that the weight change from the previous day is 1% or less, and a measurement sample is obtained. Reference: aluminum pan
[0043] <Viscosity> The viscosity of the present composition at a shear rate of 1 s -1 The shear viscosity at 2000 mPa·s is preferably 8000 mPa·s or less. It is more preferably 4000 mPa·s or less, even more preferably 2000 mPa·s or less, particularly preferably 1000 mPa·s or less, and most preferably 500 mPa·s or less. By having the shear viscosity at or below this upper limit, the composition can be applied uniformly. The lower limit of the shear viscosity is preferably 0.1 mPa·s or more. It is more preferably 1 mPa·s or more, even more preferably 5 mPa·s or more, particularly preferably 10 mPa·s or more, and most preferably 50 mPa·s or more. Of these, 80 mPa·s or more is more preferable, and 100 mPa·s or more is even more preferable. By having the shear viscosity at or above this lower limit, when the composition is applied, dripping can be prevented and the appearance can be improved, and it is easy to ensure a certain film thickness or more, thereby maintaining good storage stability of fruits and vegetables.
[0044] <Viscosity measurement conditions> Apparatus: Rotational rheometer (model: Kinexus pro+) Plate: Cone-plate type, diameter 40 mm, cone angle 2 degrees Measurement temperature: 25°C Shear rate history and measurement range: Shear rate 0 to 1000 (s -1 ), then again to 0(s -1 ) when it is returned to 1 (s -1 ) shear viscosity
[0045] <Non-volatile component concentration> The non-volatile component concentration in the present composition is not particularly limited, but is typically 0.1% by mass or more. It is preferably 0.2% by mass or more, more preferably 0.3% by mass or more, even more preferably 0.5% by mass or more, particularly preferably 1% by mass or more, and preferably 2% by mass or more. It is more preferably 2.5% by mass or more, even more preferably 3.0% by mass or more, particularly preferably 3.5% by mass or more, and most preferably 4.0% by mass or more. In particular, a concentration of 1% by mass or more ensures a sufficient film thickness when a coating is formed, making it easier to exhibit gas barrier properties against water vapor, oxygen, etc., and ensuring sufficient storage stability for fruits and vegetables. The upper limit of the non-volatile component concentration in the present composition is also not particularly limited, but is typically 60% by mass or less. It is preferably 50% by mass or less, more preferably 40% by mass or less, even more preferably 30% by mass or less, more particularly preferably 20% by mass or less, and most preferably 10% by mass or less. By setting the nonvolatile component concentration within the above range, it becomes easier to form a coating film with a suitable thickness while properly dissolving or dispersing the sucrose fatty acid ester and glycerin fatty acid ester in the aqueous solvent. This improves the appearance of the fruits and vegetables on which the coating is formed and increases their storage stability. Note that the "nonvolatile component concentration" in the present invention refers to the concentration of nonvolatile components excluding the solvent contained in the composition.
[0046] <pH of the Present Composition> The pH of the present composition is preferably 4 or more and 10 or less, more preferably 4 or more and 8 or less, from the viewpoint of safe application to food.
[0047] [Method for producing coating liquid composition] The coating liquid composition of the present invention is preferably produced by mixing a sugar-based surfactant, a glycerin fatty acid ester, and a solvent, heating the mixture, and then cooling. This method is thought to increase the uniformity of the mixed state of the sugar-based surfactant and the glycerin fatty acid ester in the aggregate formed by the sugar-based surfactant and the glycerin fatty acid ester, thereby forming a dense film and further reducing gas permeability. In addition to the above-mentioned production method, the uniformity of the coating liquid composition can be improved by using a composition that combines a sugar fatty acid ester and a glycerin fatty acid ester.
[0048] [Coated Fruits and Vegetables] The coated fruits and vegetables of the present invention are fruits and vegetables that have been coated with the coating composition to form a coating. The coating suppresses respiration and evaporation of water from the fruits and vegetables, thereby maintaining the freshness of the fruits and vegetables.
[0049] <Fruits and Vegetables> Fruits and vegetables to which the composition is applied refer to vegetables, fruit trees, etc., and specifically include citrus fruits such as oranges, grapefruits, and mandarins; pome fruits such as quince, pears, loquats, and apples; stone fruits such as peaches, apricots, plums, plums, and cherry blossoms; small fruits such as berries including blackberries, raspberries, blueberries, and grapes; root vegetables such as daikon radish, carrots, ginger, and burdock; potatoes such as sweet potatoes, taro, and potatoes; onions, chives, garlic, and rakki. These include bulb vegetables such as onions and leeks; cucumbers such as cucumbers, zucchini, bitter melon, pumpkin, melon, and watermelon; Solanaceae fruit vegetables such as tomatoes, cherry tomatoes, eggplants, bell peppers, and chili peppers; Brassica vegetables such as broccoli, cauliflower, and pickled mustard greens; leafy vegetables such as bok choy, takana, cabbage, Chinese cabbage, lettuce, and chrysanthemum; stem vegetables such as butterbur, asparagus, bracken, fern, and butterbur; and mushrooms such as shiitake mushrooms, king oyster mushrooms, buna-shimeji mushrooms, enoki mushrooms, and maitake mushrooms.
[0050] <Coating> The coating of the present invention is formed by volatilizing the solvent from the composition, and therefore the types and composition ratios of the sugar-based surfactant and the glycerin fatty acid ester in the coating, as well as the preferred content of the non-volatile component concentration, are the same as those described above. From the viewpoint of preserving the freshness of fruits and vegetables, the coating of the present invention preferably has water vapor barrier properties and / or oxygen barrier properties to suppress respiration and evaporation of moisture. Furthermore, from the viewpoint of safety when used in food, the coating is preferably edible.
[0051] <Water Vapor Barrier Properties> The coating film formed by the coating liquid composition of the present invention has a water vapor permeability of 0.1 g / (m 2 ·day·atm) or more, and 2 ·day·atm) or more, and 1.0 g / (m 2 ·day·atm) or more is more preferable. 2 ·day·atm) or less, and 2 ·day·atm) or less, and 2 ·day·atm) or less, and more preferably 40 g / (m 2 ·day·atm) or less is particularly preferable. 2 ·day·atm) or less, and 2 ·day·atm) or less, and more preferably 15 g / (m 2 It is even more preferable that the water vapor transmission rate is equal to or less than 1 / 2 day / atm. When the water vapor transmission rate is within the above range, evaporation from vegetables or fruits can be suppressed, enabling freshness to be maintained. The water vapor transmission rate (WVTR) can be measured by a differential pressure method using a water vapor transmission rate measuring device DELTAPERM in accordance with JIS K7129-5. More specifically, the water vapor transmission rate measured when the film is coated on a polyethylene terephthalate film with a thickness of 50 μm under conditions of 30°C and 80% RH is converted into transmission rate per μm using the following formula:
[0052]
[0053] <Oxygen Barrier Property> The coating film formed by the coating liquid composition of the present invention has an oxygen permeability per 1 μm at 25° C. and 50% RH of 0.1 cc / (m 2 ·day·atm) or more is preferable, and 0.5 cc / (m 2 ·day·atm) or more is more preferable, and 1.0 cc / (m 2 ·day·atm) or more is more preferable. 2 ·day·atm) or less, and 300cc / (m 2 ·day·atm) or less is more preferable, and 250cc / (m 2 ·day·atm) or less is more preferable, and 200 cc / (m 2 ·day·atm) or less is particularly preferable. 2 ·day·atm) or less is more preferable, and 90cc / (m 2 ·day·atm) or less is more preferable, and 50 cc / (m 2 ·day·atm) or less is particularly preferred. When the oxygen permeability is within the above range, aging of vegetables or fruits due to respiration can be suppressed, and freshness can be better maintained. The oxygen permeability (OTR) can be measured by the isobaric method using an oxygen permeability measuring device OX-TRAN 2 / 21 (manufactured by MOCON) based on JIS K7126-2. More specifically, the measured oxygen permeability when coated on a polyethylene terephthalate film with a thickness of 50 μm under conditions of 25°C and 50% RH is converted into permeability per μm using the following formula.
[0054]
[0055] <Edible> Edible means that a substance can be used for food. From the viewpoint of safety, it is preferable that a compound approved as a food additive be used in a dosage that satisfies the required amount to be edible.
[0056] <Crystallization> The coating of the present invention preferably has crystallinity from the viewpoint of suppressing stickiness and enhancing water vapor barrier properties. The crystalline melting peak temperature of the coating of the present invention is preferably 40°C or higher and 80°C or lower, more preferably 45°C or higher and 70°C or lower. A crystalline melting peak temperature of 40°C or higher reduces stickiness of the resulting coating. The crystalline melting peak temperature is the temperature at which a crystalline melting peak is detected during the initial temperature rise from 30°C to 100°C in differential scanning calorimetry (DSC) measured at a heating rate of 10°C / min. When there are multiple crystalline melting peaks, the sum of the peak areas within the above temperature range is preferably 50% or more of the sum of the peak areas across the entire temperature range. For measurement, the coating may be formed on any substrate, or only the coating may be measured. Examples of substrates include polyethylene terephthalate films and glass plates.
[0057] <Average Film Thickness> The average film thickness of the coated fruit or vegetable is preferably 0.1 μm or more and 10 μm or less, more preferably 0.5 μm or more and 5 μm or less. An average film thickness of 0.1 μm or more sufficiently suppresses the respiration of the fruit or vegetable and the evaporation of water. On the other hand, an average film thickness of 10 μm or less allows the film to be formed while maintaining the texture of the fruit or vegetable as a food. In the present invention, the thickness of the film does not need to be uniform over the entire food. The average film thickness can be determined by observing the cross section of the coated fruit or vegetable under a microscope and measuring the thickness at 10 or more randomly selected points.
[0058] [Method for preserving the freshness of fruits and vegetables] The method for preserving the freshness of fruits and vegetables of the present invention includes a step of covering fruits and vegetables with the present composition. The step of covering fruits and vegetables with the present composition is not particularly limited as long as it is a step of covering fruits and vegetables with the present composition, and examples thereof include direct application methods such as brush coating and curtain coating; immersion methods such as impregnation coating; and spraying methods such as spray coating. Of these, the immersion method and spraying method are preferred from the viewpoint of being able to relatively uniformly cover fruits and vegetables having a three-dimensional shape and from the viewpoint of productivity.
[0059] When covering fruits or vegetables with the composition, the composition may be applied to only a portion of the fruit or vegetable, or to the entire fruit or vegetable. Applying the composition to the entire fruit or vegetable effectively preserves the freshness of the fruit or vegetable. On the other hand, from the viewpoint of shortening the drying time of the composition and increasing the efficiency of the coating process, the composition may be applied to only a portion of the fruit or vegetable. In this case, the application area is preferably 10% or more of the surface area of the fruit or vegetable, more preferably 25% or more, even more preferably 40% or more, and even more preferably 50% or more. Furthermore, a portion of the applied composition may be removed. While the removal method is not particularly limited, examples include removal by wind pressure using an air dryer. This removal can prevent poor drying of the excess applied portion. An example of the application method is described in "Coating Method," Maki Shoten, by Harasaki Yuji, published in 1979.
[0060] After applying the present composition to fruits and vegetables, the coating may be dried for the purpose of removing the aqueous solvent, etc. Drying methods include, for example, static drying, air drying, and heat drying, but from the viewpoint of maintaining the freshness of fruits and vegetables, a method of drying by leaving the composition to stand at room temperature (20 to 25°C) or a method of air drying at room temperature is preferred.
[0061] The present invention will now be described in more detail with reference to examples, although the present invention is not limited to the examples described below.
[0062] [Evaluation Method] 1. Coating Liquid (Coating Composition) (State of Coating Liquid) To evaluate the stability of the coating liquid, the state of the coating liquid was evaluated according to the following criteria. <Evaluation Criteria> A: The liquid is uniform and has fluidity. B: The liquid is uniform but has no fluidity. C: The liquid is non-uniform, with precipitation or separation.
[0063] (Viscosity of Coating Liquid) The shear viscosity of the liquid prepared in each Example and Comparative Example was measured under the following conditions. -1 The shear viscosity at this temperature was taken as the viscosity of the coating liquid. <Conditions for measuring viscosity> Apparatus: Rotational rheometer (model: Kinexus pro+) Plate: Cone-plate type, diameter 40 mm, cone angle 2 degrees Measurement temperature: 25°C Shear rate history and measurement range: Shear rate 0 to 1000 (s -1), then again to 0(s -1 ) when it is returned to 1 (s -1 ) shear viscosity
[0064] (State of coating film) <Differential scanning calorimetry at 0°C or higher> Differential scanning calorimetry was carried out under the following conditions. If no peak is observed below 0°C, the temperature may be changed from 25°C to -80°C to 100°C. Measuring device: NETZSCH DSC 204F1 Measurement method: heat flux method Temperature: 25°C → 0°C → 100°C Temperature increase / decrease rate: 10°C / min Atmosphere: nitrogen Sample preparation: The coating composition was placed in an empty aluminum pan so that the dry solid content was 1 mg, and the pan was left to dry at room temperature. It was confirmed that the weight change from the previous day was 1% or less, and a measurement sample was obtained. Reference: Aluminum pan
[0065] <Differential scanning calorimetry at -80°C or higher> Differential scanning calorimetry with a measurement temperature range of -80°C or higher was carried out under the following conditions. Measurement device: NETZSCH DSC 204F1 Measurement method: heat flux method Temperature: 25°C → -80°C → 100°C Temperature increase / decrease rate: 10°C / min Atmosphere: nitrogen Sample preparation: The coating composition was placed in an empty aluminum pan so that the dry solid content was 1 mg, and the pan was left to dry at room temperature. It was confirmed that the weight change from the previous day was 1% or less, and a measurement sample was obtained. Reference: aluminum pan
[0066] 2. Evaluation of Freshness Retention Avocados were used as fruits and vegetables, and the coating solutions prepared in each of the Examples and Comparative Examples were applied to them by dipping, and the coating appearance, weight retention rate, and skin color were evaluated.
[0067] (Coating Appearance) The coating solution prepared in each Example and Comparative Example was applied to an avocado by dipping, and after drying, the coating solution remaining on the avocado skin was visually evaluated for appearance defects resulting from the coating solution, according to the following criteria: <Evaluation Criteria> A: The area with poor appearance was less than 5% of the avocado skin surface, B: The area with poor appearance was 5% or more but less than 50% of the avocado skin surface, C: The area with poor appearance was 50% or more but less than 100% of the avocado skin surface.
[0068] (Weight retention rate) Using the weight of the avocado before storage (day 0) as the reference, the weight retention rate ((weight after storage / weight on day 0) x 100(%)) after storage for 3, 4 and 5 days at 25°C and 50% RH was calculated. (Weight loss rate) Using the weight of the avocado before storage (day 0) as the reference, the weight loss rate (100-(weight after storage / weight on day 0) x 100(%)) after storage for 4 days at 25°C and 50% RH was calculated.
[0069] (Skin Color) As avocados ripen, their skin color changes from green to dark purple. This change is easily noticeable, and consumers commonly evaluate the freshness of avocados by their color. Therefore, a coating was formed on the surface of each avocado, and the freshness-preserving effect was confirmed by the color change. Five avocados were prepared, and the color change was evaluated according to the following criteria. The color change was evaluated according to the following criteria before storage (day 0) and after storage at 25°C and 50% RH for 3, 4, and 5 days. <Evaluation Criteria> A: Either none (0%) or less than 50% of the samples had a completely dark purple surface. B: 50% or more but less than 100% of the samples had a completely dark purple surface. C: All samples had a completely dark purple surface (100%).
[0070] (Fruit Firmness) The load (N) was measured when a cylindrical plunger with a diameter of 5 mm was pressed 3 mm into an avocado at a speed of 60 mm / min. Three avocados stored at 25°C and 50% RH for 4 days were used for the measurement, and measurements were taken at three different locations near the equator for each avocado. The arithmetic mean of the obtained values was taken as the fruit firmness.
[0071] (Feel of the fruit surface after coating) Five avocados were prepared before storage (day 0) after the coating treatment, and the feel of the fruit surface after coating was evaluated by hand according to the following criteria. The evaluation was based on the results of a discussion between three experienced experts. <Evaluation criteria> A: None of the samples felt sticky (0%) or less than 50%. B: More than 50% of the samples felt sticky, or the surface of all the samples felt sticky (100%).
[0072] The materials used are as follows: S-1170: sucrose stearate, manufactured by Mitsubishi Chemical Corporation, "Ryoto (registered trademark) Sugar Ester S-1170", HLB: approximately 11, monoester content: approximately 55%, bound fatty acid purity: approximately 70%. S-1670: sucrose stearate, manufactured by Mitsubishi Chemical Corporation, "Ryoto (registered trademark) Sugar Ester S-1670", HLB: approximately 16, monoester content: approximately 75%, bound fatty acid purity: approximately 70%. S-570: sucrose stearate, manufactured by Mitsubishi Chemical Corporation, "Ryoto (registered trademark) Sugar Ester S-570", HLB: approximately 5, monoester content: approximately 30%, bound fatty acid purity: approximately 70%. F-110: sucrose stearate, manufactured by Dai-ichi Kogyo Seiyaku Co., Ltd., "DK Ester (registered trademark) F-110", HLB: 11. S-100P: Glycerin fatty acid ester, Riken Vitamin Co., Ltd. "Rikemal (registered trademark) S-100P", main ingredient: glycerin monostearate, HLB: 4.3, melting point 63-68°C, monoester content: 95% or more. M-100: Glycerin fatty acid ester, Riken Vitamin Co., Ltd. "Poem (registered trademark) M-100", main ingredient: glycerin monocaprylate, HLB: 7.0, melting point approximately 31°C, monoester content: 85% or more. M-1695: Sucrose myristate ester, Mitsubishi Chemical Corporation "Ryoto (registered trademark) Sugar Ester M-1695", HLB: approximately 16, monoester content: approximately 80%, bound fatty acid purity: approximately 20%. MCT oil: Medium-chain fatty acid triacylglycerol (tri(caprylic / capric)glyceryl)), Nisshin Oillio Group, Inc. Tannic acid: Fujifilm Wako Pure Chemical Industries, Ltd.
[0073] Example 1 (Method of Preparing Coating Liquid) A coating liquid (coating composition) was prepared by dispersing glycerin fatty acid ester (S-100P) and sucrose fatty acid ester (S-1170) in a water solvent (ion-exchanged water) at 73°C for 30 minutes, leaving the dispersion at room temperature of 20°C, and then cooling it to 25°C. The content of each material is as shown in Table 1. The evaluation results are shown in Table 1.
[0074] Examples 2 to 5 Coating solutions were prepared in the same manner as in Example 1, except that the contents of glycerin fatty acid ester and sucrose fatty acid ester were changed as shown in Table 1. The evaluation results are shown in Table 1.
[0075] Comparative Example 1 A coating solution was prepared in the same manner as in Example 1, except that Rikemal (registered trademark) S-100P was used as the glycerin fatty acid ester and no sucrose fatty acid ester was added. The coating solution separated from the solvent. Subsequent evaluations could not be measured.
[0076] Comparative Example 2 The above evaluation was carried out on an avocado that had not been coated with the coating liquid. The results are shown in Table 1.
[0077]
[0078] The results shown in Table 1 indicate that avocados coated with the coating composition of the present invention exhibited good coating appearance upon application, and showed good results in both weight retention and peel color after 5 days of storage. On the other hand, in Example 5, where the mass ratio of sucrose fatty acid ester to glycerin fatty acid ester was outside the range of the present invention, the coating appearance was poor, but the freshness-preserving effect was still exhibited without any problems. Furthermore, when a coating solution without sucrose fatty acid ester was used, the viscosity was high, as shown in Comparative Example 1, making it impossible to measure shear rate. Therefore, a coating film could not be formed on the avocado. Furthermore, in Comparative Example 2, where no coating was formed, weight loss was observed over time and peel color deteriorated, indicating a clear decrease in freshness retention. These effects are speculatively attributed to the crystallization of the fatty acid ester moieties of the glycerin fatty acid ester and sugar fatty acid ester contained in the composition, resulting in a denser coating, which exhibited gas barrier properties, and the change in the structure of the aggregate formed by the glycerin fatty acid ester and sugar fatty acid ester, which improved applicability by mixing the sugar fatty acid ester with the glycerin fatty acid ester.
[0079] Examples 6 to 11 and Comparative Examples 2 to 4 Coating solutions were prepared in the same manner as in Example 1, except that the sugar fatty acid ester and glycerin fatty acid ester were made to have the ingredients and compositions shown in Table 2. The state of the coating solution, the viscosity of the coating solution, the state of the coating film, and the freshness retention of the coated avocado were evaluated, and the results are shown in Table 2.
[0080] In the differential scanning calorimetry of Example 6 at temperatures above -80°C, there was no peak when the temperature was lowered, but there was an exothermic peak of 85.39 J / g in the range of 62°C to 68°C with a peak top at 65.7°C when the temperature was raised. 1 / A 2 = A 3 / A 2 =0%.
[0081] The aqueous coating composition in Example 8 was changed from S-1170 to the equivalent F-110. 3 / A 2 =49%.
[0082] In Example 10, differential scanning calorimetry at temperatures above -80 ° C. showed an exothermic peak of 4.885 J / g with a peak top at 1.1 ° C. in the range of 2 ° C. to -1 ° C. during cooling, and two exothermic peaks of 32.9 J / g with a peak top at -29.6 ° C. in the range of -29 ° C. to -32 ° C. during heating, and an exothermic peak of 32.07 J / g with a peak top at -27.1 ° C. in the range of -27 ° C. to -25 ° C. during heating. In addition, there was an endothermic peak of 59.91 J / g with a peak top at 20.8 ° C. in the range of 5 ° C. to 24 ° C., and an endothermic peak of 25.2 J / g with a peak top at 27.6 ° C. in the range of 24 ° C. to 30 ° C. At this time, A 3 / A 2 =82%.
[0083] In Example 11, differential scanning calorimetry at temperatures above -80 ° C. showed an exothermic peak of 4.358 J / g with a peak top at 1.8 ° C. in the range of 2 ° C. to -2 ° C. during cooling, and two exothermic peaks of 30.58 J / g with a peak top at -29.7 ° C. in the range of -29 ° C. to -32 ° C. during heating, and an exothermic peak of 28.11 J / g with a peak top at -26.4 ° C. in the range of -29 ° C. to -24 ° C. during heating. In addition, an endothermic peak of 57.56 J / g with a peak top at 21.0 ° C. in the range of 2 ° C. to 24 ° C. and an endothermic peak of 23.3 J / g with a peak top at 27.2 ° C. in the range of 24 ° C. to 30 ° C. were observed. At this time, A 3 / A 2 =78%.
[0084]
[0085] The results shown in Table 2 indicate that the coating composition of the present invention is homogeneous and free from precipitation or separation, allowing for stable coating. Avocados coated with the coating composition of the present invention exhibited a favorable coating appearance upon application, and exhibited favorable results in weight retention, skin color, and fruit firmness after four days of storage. The results of Examples 1 to 11 and Comparative Examples 3 and 4 demonstrate that a low proportion of triester in the coating composition resulted in a stable coating composition. While the coating compositions of Examples 6, 7, 9, and 10 were fluid and homogeneous, the coating composition of Comparative Example 1 lacked fluidity and was in a heterogeneous state. This indicates that by blending a certain amount of sucrose fatty acid ester with a glycerin fatty acid ester, the coating composition exhibits physical properties suitable for use in coating. This is believed to be due to the fact that the glycerin fatty acid ester, which alone would not form a stable coating solution, was transformed into a usable coating solution by mixing it with a certain amount of sucrose fatty acid ester, which has a similar structure and a fatty acid ester structure. In particular, it was found that when the ratio of sucrose fatty acid ester to glycerin fatty acid ester in the coating liquid composition is 10% by mass or more, the effect of suppressing ripening such as changes in the skin color and a decrease in hardness of avocados is enhanced. 3 / A 2 The smaller the value, the higher the freshness preservation effect. 3 / A 2 Example 10, in which the % α value was 82.1%, was found to have suppressed weight loss, changes in skin color, and softening of the fruit compared to Comparative Example 2, which was not subjected to coating treatment. 3 / A 2 In Example 11, where A = 78.0%, the change in skin color and softening of the fruit were further suppressed. 3 / A 2 In Example 8, where the content of A is 49.2%, the change in skin color and softening of the fruit are further suppressed. 3 / A 2In Example 6, where the content was 0%, weight loss was further suppressed. This is because, in differential scanning calorimetry, an exothermic peak appears when a liquid component changes to a solid component upon temperature change, and the ratio of the exothermic peak to the endothermic peak is thought to be one aspect that indicates the amount of liquid component. The film formed on the fruit surface inhibits the permeation of oxygen gas and water vapor, thereby inhibiting the progression of ripening and weight loss. As the liquid component in the material that makes up the film increases, the permeation of gas components increases. Therefore, from the perspective of maintaining freshness, a smaller ratio of the exothermic peak to the endothermic peak, which represents the liquid component, is considered more desirable. From the above, it has been demonstrated that the coating composition of the present invention is particularly suitable for use on fruits and vegetables.
[0086] According to the present invention, by covering fruits and vegetables with a coating that is highly safe and has a high water vapor barrier property, it is possible to suppress evaporation of moisture from the fruits and vegetables and maintain their freshness for a long period of time. In other words, since the freshness of fruits and vegetables is maintained for a long period of time, there is no need for farmers and others to ship fruits and vegetables earlier than necessary when harvesting them, and there is also the advantage that consumers can obtain fruits and vegetables that are extremely fresh, making this a technology with great industrial value.
Claims
1. A coating composition containing a sugar-based surfactant and a glycerin fatty acid ester, wherein the mass ratio (solid content) of the sugar-based surfactant to the total mass of the sugar-based surfactant and the glycerin fatty acid ester is 30% or more and less than 100%, and the glycerin fatty acid ester having three fatty acid ester groups accounts for 50% or less by mass.
2. Shear rate 1s -1 2. The coating composition according to claim 1, having a shear viscosity of 0.1 to 8000 mPa·s.
3. The coating composition according to claim 1, wherein the sugar-based surfactant is a sucrose fatty acid ester.
4. The coating composition of claim 1, further comprising an aqueous solvent.
5. The coating composition according to claim 4, wherein the water-based solvent comprises water or a mixture of a water-soluble organic solvent and water.
6. The coating composition according to claim 1, wherein the concentration of non-volatile components is 0.1% by mass or more and 60% by mass or less.
7. In differential scanning calorimetry with a measurement temperature range of -80°C or higher, the total area A of exothermic peaks 3 The total area A of endothermic peaks at 0°C to 80°C 2 2. The coating composition of claim 1, wherein the ratio of 8. Fruit or vegetable coated with the coating composition according to any one of claims 1 to 7.
9. The coated fruit or vegetable according to claim 8, wherein the average thickness of the coating is from 0.1 μm to 10 μm.
10. A method for preserving the freshness of fruits and vegetables, comprising the step of covering the fruits and vegetables with the coating composition according to any one of claims 1 to 7.
11. The method for preserving the freshness of fruits and vegetables according to claim 10, wherein the step of covering the fruits and vegetables with the coating composition is a step of immersing the fruits and vegetables in the composition, or applying or spraying the composition onto the fruits and vegetables.
Citation Information
Patent Citations
Anti-fogging surface-treatment agent and Anti-fogging resin sheet
JP2010037387A
Food Coating
JP2020506988A
Coated agricultural products and corresponding methods
WO2021178553A1
Composition, coated food product, coated food product manufacturing method, coating formation method, and food product shipping method
WO2022080444A1