Catalyst composition for producing ethylene-based polymer applicable to high-temperature solution process, and method for producing ethylene-based polymer using same

The catalyst composition of two transition metal compounds with an aluminum or boron cocatalyst in high-temperature solution polymerization addresses the challenge of producing low-density ethylene-based polymers with wide molecular weight distribution and bimodality, enhancing both processability and physical properties while maintaining economic feasibility.

WO2024204958A1PCT designated stage expired Publication Date: 2024-10-03HANWHA TOTALENERGIES PETROCHEMICAL CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2023/020942
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-24
Filing Date
2023-12-19
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Current catalyst systems for producing ethylene-based polymers in high-temperature solution processes face challenges in achieving high activity and bimodality, particularly in producing low-density ethylene homopolymers or copolymers with wide molecular weight distribution, which is essential for both excellent physical properties and processability, while maintaining economic feasibility.

Method used

A catalyst composition comprising a mixture of two specific transition metal compounds, along with an aluminum or boron cocatalyst, is used in high-temperature solution polymerization to achieve high catalytic activity and produce low-density ethylene-based polymers with wide molecular weight distribution and bimodality.

Benefits of technology

The catalyst composition effectively produces ethylene-based polymers with excellent processability and physical properties, achieving high yield and activity, thereby addressing the limitations of existing systems and reducing production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2023020942_03102024_PF_FP_ABST
    Figure KR2023020942_03102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to a catalyst composition for producing an ethylene-based polymer, the catalyst composition being applicable to a high-temperature solution process, and a method for producing an ethylene-based polymer using same. According to the present invention, a low-density ethylene homopolymer or an ethylene-alpha-olefin copolymer having a wide molecular weight distribution and bimodality can be prepared with high activity in a solution polymerization process performed at high temperature.
Need to check novelty before this filing date? Find Prior Art

Description

Catalyst composition for producing ethylene polymer applicable to high-temperature solution process and method for producing ethylene polymer using the same

[0001] The present invention relates to a catalyst composition for producing an ethylene polymer applicable to a high-temperature solution process and a method for producing an ethylene polymer using the same.

[0002] Metallocene catalysts have been used in the production of ethylene homopolymers and copolymers with α-olefins. Metallocenes are currently used industrially, not only for polyethylene but also for polypropylene. These metallocenes are often produced using cyclopentadienyl-based catalyst systems with different substitution patterns.

[0003] Several of these metallocene catalysts have been described for use in solution polymerization to produce polyethylene homo- or copolymers.

[0004] For example, US6313240 describes a catalyst system comprising a hafnocene catalyst complex derived from (A) a biscyclopentadienyl hafnium organometallic compound having (A) 1) one or more substituted cyclopentadienyl ligands or aromatically fused and substituted pentadienyl ligands having no additional substituents on the ligands, 2) one substituted or unsubstituted aromatically fused and substituted pentadienyl ligand, and 3) a covalent bridge connecting the two cyclopentadienyl ligands.

[0005] This bridge may be a single carbon substituted with two aryl groups, each of which is substituted with a C1-C20 hydrocarbyl or hydrocarbylsilyl group.

[0006] Additionally, the catalyst system preferably comprises an activating cocatalyst which is a precursor ion compound comprising a Group 13 anion substituted with a halogenated tetraaryl.

[0007] Recently, research is being conducted to develop bimodal polymers using two types of catalysts: a low-molecular-weight catalyst with processability and a high-molecular-weight catalyst with easy property control. Because high-molecular-weight polymers can define the physical properties, and low-molecular-weight polymers can define the processability, two types of catalysts are commonly used to produce bimodal polymers. While hydrogen is also used to produce low-molecular-weight polymers, this method suffers from reduced activity. Furthermore, attempts to control bimodal polymerization by installing additional reactors increase costs. To address this, a catalyst with high activity at high temperatures and capable of producing low-molecular-weight polymers is needed, and the combination of these two catalysts can be used to control bimodal polymerization.

[0008] Additionally, low molecular weight polymers have the potential to produce ideal polyethylene waxes, increasing the importance of catalysts that can be developed independently.

[0009] Meanwhile, metallocene catalysts, in which a transition metal is linked to a cross-linked Cp-Flu ligand, have been reported as catalysts capable of producing high catalytic activity and high molecular weight polymers in ethylene homopolymerization or ethylene and alpha-olefin copolymerization under solution polymerization conditions. US6559253 presents an example of a structure in which a diphenyl-substituted bridge and an unsubstituted fluorene are linked to a cyclopentadiene ligand. In addition, US6121396 discloses the structure of a Cp-Flu ligand having a diphenyl methylene bridge and substituted with one or more electron donor groups.

[0010] While these catalysts significantly improve reactivity with alpha-olefins due to the reduced steric hindrance inherent in the catalyst itself, their commercial application for low-molecular-weight polymers remains challenging. Therefore, securing a more competitive catalyst system that meets the required characteristics of a commercial catalyst based on economic feasibility, namely the ability to produce polymers with excellent high-temperature activity and superior processability, is crucial.

[0011] In order to overcome the problems of the above-mentioned prior art, the inventors of the present invention conducted research and discovered that when two transition metal compounds of a specific structure are mixed, a low-density ethylene homopolymer or a copolymer of ethylene and alpha-olefin with a broad molecular weight distribution and bimodality can be produced with high activity in a solution polymerization process carried out at high temperatures.

[0012] Accordingly, the purpose of the present invention is to provide a catalyst composition for producing an ethylene polymer capable of producing a low-density ethylene homopolymer or a copolymer of ethylene and alpha-olefin with a broad molecular weight distribution and bimodality with high activity in a solution polymerization process carried out at high temperature, and a method for producing an ethylene polymer using the same.

[0013] One aspect of the present invention provides a catalyst composition for producing an ethylene polymer, comprising: a first transition metal compound represented by the following chemical formula 1; a second transition metal compound represented by the following chemical formula 2; and a cocatalyst selected from an aluminum compound, a boron compound, or a mixture thereof.

[0014] [Chemical Formula 1]

[0015]

[0016] [Chemical Formula 2]

[0017]

[0018] In the above chemical formulas 1 and 2,

[0019] M1 is a transition metal in group 4 of the periodic table;

[0020] R 1 Inland R 4 are each independently C1-C20 alkyl or C6-C20 aryl;

[0021] R 5 , R 6 , R 15 and R 16 are each independently C6-C20 aryl, and the above R 5 , R 6 , R 15 and R 16 The aryl of may be further substituted with C1-C20 alkyl;

[0022] R 11 and R 12 are each independently hydrogen or C1-C20 alkyl;

[0023] X 1 , X 2 , X 11 and X 12 are each independently halogen, C1-C20 alkyl, C3-C20 cycloalkyl, C6-C20 aryl, C6-C20 arylC1-C20 alkyl, (C1-C20 alkylC6-C20 aryl)C1-C20 alkyl, C1-C20 alkoxy, C6-C20 aryloxy, C1-C20 alkylC6-C20 aryloxy, C1-C20 alkoxyC6-C20 aryloxy, -OSiR a R b R c , -SR d , -NR e R f , -PR g R h or C1-C20 alkylidene;

[0024] R a Inland R d are independently C1-C20 alkyl, C6-C20 aryl, C6-C20 arylC1-C20 alkyl, C1-C20 alkylC6-C20 aryl or C3-C20 cycloalkyl;

[0025] R e Inland R hare independently C1-C20 alkyl, C6-C20 aryl, C6-C20 arylC1-C20 alkyl, C1-C20 alkylC6-C20 aryl or C3-C20 cycloalkyl;

[0026] X 1 and X 2 If one of them is C1-C20 alkylidene, the other is absent;

[0027] X 11 and X 12 If one of them is C1-C20 alkylidene, the other is absent.

[0028] In addition, another aspect of the present invention provides a method for producing an ethylene polymer by polymerizing an ethylene monomer in the presence of the catalyst composition for producing an ethylene polymer.

[0029] The catalyst composition according to the present invention maintains high catalytic activity by mixing two transition metal compounds of specific structures in high-temperature solution polymerization, and can produce low-density polymers with good copolymerization reactivity with other olefins and a broad molecular weight distribution in high yield. In addition, the catalyst composition according to the present invention can produce low-density ethylene polymers with a broad molecular weight distribution and bimodality, and the produced ethylene polymers can secure excellent processability. Therefore, the catalyst composition according to the present invention can be usefully used in the production of ethylene homopolymers or copolymers with alpha-olefins having various physical properties.

[0030] Figure 1 - GPC graph of the copolymer prepared in Example 2

[0031] The present invention will be described in more detail. Unless otherwise defined, the technical and scientific terms used herein have the meanings commonly understood by those of ordinary skill in the art to which this invention pertains. In the following description, descriptions of well-known functions and configurations that may unnecessarily obscure the gist of the present invention will be omitted.

[0032] As used herein, the singular forms may be intended to include the plural forms as well, unless the context clearly indicates otherwise.

[0033] The term "includes" as used herein is an open-ended description equivalent to expressions such as "comprises," "contains," "has," or "characterizes," and does not exclude additional elements, materials, or processes not listed herein.

[0034] As used herein, “alkyl” means a monovalent straight-chain or branched saturated hydrocarbon radical composed solely of carbon and hydrogen atoms, examples of which include, but are not limited to, methyl, ethyl, propyl, isopropyl, butyl, isobutyl, t-butyl, pentyl, hexyl, octyl, nonyl, and the like.

[0035] The term "aryl" as used herein refers to an organic radical derived from an aromatic hydrocarbon by the removal of one hydrogen, including single or fused ring systems, each ring suitably containing 4 to 7, preferably 5 or 6, ring atoms, and even including a form in which multiple aryls are connected by single bonds. The fused ring system may include an aliphatic ring, such as a saturated or partially saturated ring, and necessarily contains at least one aromatic ring. In addition, the aliphatic ring may contain nitrogen, oxygen, sulfur, carbonyl, etc. within the ring. Specific examples of the aryl radical include, but are not limited to, phenyl, naphthyl, biphenyl, indenyl, fluorenyl, phenanthrenyl, anthracenyl, triphenylenyl, pyrenyl, chrysenyl, naphthacenyl, 9,10-dihydroanthracenyl, and the like.

[0036] As used herein, "cycloalkyl" refers to a monovalent saturated carbocyclic radical consisting of one or more rings. Examples of cycloalkyl radicals include, but are not limited to, cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, cycloheptyl, and the like.

[0037] As used herein, “halo” or “halogen” means a fluorine, chlorine, bromine or iodine atom.

[0038] As used herein, “alkoxy” means -O-(alkyl) including -OCH3, -OCH2CH3, -O(CH2)2CH3, -O(CH2)3CH3, -O(CH2)4CH3, -O(CH2)5CH3 and the like, wherein alkyl is as defined above.

[0039] As used herein, “aryloxy” refers to an -O-aryl radical, where “aryl” is as defined above.

[0040] As used herein, “alkylidene” means a straight or branched chain saturated divalent hydrocarbon group having a valence of 2 on one common carbon atom.

[0041] In this specification, (co)polymer means both a homopolymer and a copolymer.

[0042] Unless otherwise defined herein, “copolymerization” may mean block copolymerization, random copolymerization, graft copolymerization or alternating copolymerization, and “copolymer” may mean block copolymer, random copolymer, graft copolymer or alternating copolymer.

[0043] Hereinafter, the present invention will be described in detail.

[0044] One aspect of the present invention provides a catalyst composition for producing an ethylene polymer in a high-temperature solution process, wherein the catalyst composition for producing an ethylene polymer according to one aspect comprises: a first transition metal compound represented by the following chemical formula 1; a second transition metal compound represented by the following chemical formula 2; and a cocatalyst selected from an aluminum compound, a boron compound, or a mixture thereof.

[0045] [Chemical Formula 1]

[0046]

[0047] [Chemical Formula 2]

[0048]

[0049] In the above chemical formulas 1 and 2

[0050] M 1 is a transition metal in group 4 of the periodic table;

[0051] R 1 Inland R 4 are each independently C1-C20 alkyl or C6-C20 aryl;

[0052] R 5 , R 6 , R 15 and R 16 are each independently C6-C20 aryl, and the above R 5 , R 6 , R 15 and R 16 The aryl of may be further substituted with C1-C20 alkyl;

[0053] R 11 and R 12 are each independently hydrogen or C1-C20 alkyl;

[0054] X 1 , X 2 , X 11 and X 12are each independently halogen, C1-C20 alkyl, C3-C20 cycloalkyl, C6-C20 aryl, C6-C20 arylC1-C20 alkyl, (C1-C20 alkylC6-C20 aryl)C1-C20 alkyl, C1-C20 alkoxy, C6-C20 aryloxy, C1-C20 alkylC6-C20 aryloxy, C1-C20 alkoxyC6-C20 aryloxy, -OSiR a R b R c , -SR d , -NR e R f , -PR g R h or C1-C20 alkylidene;

[0055] R a Inland R d are independently C1-C20 alkyl, C6-C20 aryl, C6-C20 arylC1-C20 alkyl, C1-C20 alkylC6-C20 aryl or C3-C20 cycloalkyl;

[0056] R e Inland R h are independently C1-C20 alkyl, C6-C20 aryl, C6-C20 arylC1-C20 alkyl, C1-C20 alkylC6-C20 aryl or C3-C20 cycloalkyl;

[0057] X 1 and X 2 If one of them is C1-C20 alkylidene, the other is absent;

[0058] X 11 and X 12 If one of them is C1-C20 alkylidene, the other is absent.

[0059] According to one embodiment, a catalyst composition for producing an ethylene polymer can produce an ethylene polymer having a bimodal structure with high activity in a solution polymerization process carried out at high temperatures by satisfying a combination of a first transition metal compound, a second transition metal compound, and a cocatalyst having a specific structure. In addition, according to one embodiment, a catalyst composition for producing an ethylene polymer can produce a low-density ethylene polymer having high activity and a broad molecular weight distribution by satisfying the above-described combination of components. In addition, according to one embodiment, a catalyst composition for producing an ethylene polymer can produce a low-density ethylene polymer having bimodality and a broad molecular weight distribution under polymerization conditions of high temperature and high pressure by satisfying the above-described combination of components.

[0060] The transition metals of the above group 4 include titanium (Ti), zirconium (Zr), hafnium (Hf), etc., and specifically, zirconium (Zr) or hafnium (Hf).

[0061] In the above chemical formula 1, M 1 is Zr or Hf; R 1 Inland R 4 are each independently C1-C20 alkyl or C6-C20 aryl; R 5 and R 6 are each independently C6-C20 aryl, and the above R 5 and R 6 The aryl of may be further substituted with C1-C20 alkyl; X 1 and X 2 Each may independently be halogen, C1-C20 alkyl, C6-C20 aryl or C6-C20 arylC1-C20 alkyl.

[0062] Specifically, in the above chemical formula 1, the M 1 is Hf; R 1 Inland R 4 are each independently C1-C10 alkyl or C6-C12 aryl; R 5 and R 6are each independently C6-C12 aryl, and the above R 5 and R 6 The aryl of may be further substituted with C1-C10 alkyl; X 1 and X 2 can each independently be halogen, C1-C10 alkyl, C6-C12 aryl or C6-C12 arylC1-C10 alkyl.

[0063] In the above chemical formula 2, R 11 and R 12 are each independently hydrogen or C1-C20 alkyl; R 15 and R 16 are each independently C6-C20 aryl, and the above R 15 and R 16 The aryl of may be further substituted with C1-C20 alkyl; X 11 and X 12 Each may independently be halogen, C1-C20 alkyl, C6-C20 aryl or C6-C20 arylC1-C20 alkyl.

[0064] Specifically, in the above chemical formula 2, R 11 and R 12 are each independently hydrogen or C1-C10 alkyl; R 15 and R 16 are each independently C6-C12 aryl, and the above R 15 and R 16 The aryl of may be further substituted with C1-C10 alkyl; X 11 and X 12 can each independently be halogen, C1-C10 alkyl, C6-C12 aryl or C6-C12 arylC1-C10 alkyl.

[0065] More specifically, in the above chemical formula 1, M 1 is Hf; R 1 Inland R 4 are identical to each other and are C1-C10 alkyl or C6-C12 aryl; R 5 and R 6 are each independently and R 21is C1-C10 alkyl; a is an integer from 0 to 5; X 1 and X 2 can each independently be halogen, C1-C6 alkyl, C6-C12 aryl or C6-C12 arylC1-C6 alkyl.

[0066] More specifically, in the above chemical formula 2, R 11 and R 12 are identical to each other and are hydrogen or C1-C10 alkyl; R 15 and R 16 are each independently and R 21 is C1-C10 alkyl; a is an integer from 0 to 5; X 11 and X 12 can each independently be halogen, C1-C6 alkyl, C6-C12 aryl or C6-C12 arylC1-C6 alkyl.

[0067] The first transition metal compound is [1-(η5-cyclopentadien-1-yl)-1-(η5-2,7-di-dimethylaminefluorenyl)-1,1-diphenyl methane]hafnium dichloro, [1-(η5-cyclopentadien-1-yl)-1-(η5-2,7-di-dimethylaminefluorenyl)-1,1-diphenyl methane]hafnium dibenzyl, or [1-(η5-cyclopentadien-1-yl)-1-(η5-2,7-di-dimethylaminefluorenyl)-1,1-diphenyl methane]hafnium dimethyl;

[0068] The second transition metal compound is [1-(η5-cyclopentadien-1-yl)-1-(η5-fluorenyl)-1,1-diphenyl methane]hafnium dichloro, [1-(η5-cyclopentadien-1-yl)-1-(η5-fluorenyl)-1,1-diphenyl methane]hafnium dibenzyl, [1-(η5-cyclopentadien-1-yl)-1-(η5-fluorenyl)-1,1-diphenyl methane]hafnium dimethyl, [1-(η5-cyclopentadien-1-yl)-1-(η5-2,7-di-tertbutylfluorenyl)-1,1-diphenyl methane]hafnium dichloro, [1-(η5-cyclopentadien-1-yl)-1-(η5-2,7-di-tertbutylfluorenyl)-1,1-diphenyl methane]hafnium dibenzyl, or [1-(η5-cyclopentadien-1-yl)-1-(η5-2,7-di-tertbutylfluorenyl)-1,1-diphenyl methane]hafnium dimethyl.

[0069] The first transition metal compound of the above chemical formula 1 has a group 4 transition metal as a central metal and a fluorene ligand with an amine substituent having a large electron-donating effect introduced at positions 2 and 7, which are far from the active site, so that it has high activity in high-temperature solution polymerization and can be useful as a catalyst capable of producing a low-molecular-weight ethylene polymer.

[0070] The first transition metal compound of the above chemical formula 1, when combined with the second transition metal compound of the above chemical formula 2, which produces a high molecular weight polymer, has high activity in high-temperature solution polymerization, has a wide molecular weight distribution, and has bimodality, so that a low-density ethylene polymer having excellent physical properties as well as excellent processability can be produced.

[0071] In order to produce a low-density ethylene polymer having a broad molecular weight distribution and bimodality, the first transition metal compound of the above formula 1 and the second transition metal compound of the above formula 2 may be used in a molar ratio of 1:0.2 to 1:1.5. More specifically, the first transition metal compound of the above formula 1 and the second transition metal compound of the above formula 2 may be mixed in a molar ratio of 1:0.5 to 1:1.5, or 1:0.5 to 1:1.

[0072] The above cocatalyst can act as a scavenger that activates the transition metal compound while removing impurities that act as catalyst poisons.

[0073] The aluminum compound used as the above cocatalyst may be one or more selected from an aluminoxane compound and an organoaluminum compound, and the aluminoxane compound may be represented by the following chemical formula A or B, and the organoaluminum compound may be represented by the following chemical formula C.

[0074] [Chemical Formula A]

[0075] (R a )2Al-(-O(R a )-) p -(R a )2

[0076] [Chemical Formula B]

[0077] (-Al(R a )-O-) q

[0078] [Chemical Formula C]

[0079] (R b ) r Al(E) 3-r

[0080] In the above chemical formulas A to C,

[0081] R a is C1-C20 alkyl; p and q are each independently an integer from 5 to 20; R bis C1-C20 alkyl; E is hydrogen or halogen; r is an integer from 1 to 3.

[0082] In the above chemical formulas A and B, R a It can be methyl or isobutyl.

[0083] Examples of the above aluminoxane compounds include methylaluminoxane, modified methylaluminoxane, tetraisobutylaluminoxane, etc.; Examples of the above organoaluminum compounds include trialkylaluminum including trimethylaluminum, triethylaluminum, tripropylaluminum, triisobutylaluminum, trihexylaluminum, and trioctylaluminum, dialkylaluminum chloride including dimethylaluminum chloride, diethylaluminum chloride, dipropylaluminum chloride, diisobutylaluminum chloride, and dihexylaluminum chloride, alkylaluminum dichlorides including methylaluminum dichloride, ethylaluminum dichloride, propylaluminum dichloride, isobutylaluminum dichloride, and hexylaluminum dichloride, dimethylaluminum hydride, diethylaluminum hydride, dipropylaluminum hydride, diisobutylaluminum hydride, and dihexylaluminum hydride. Examples include dialkyl aluminum hydrides, etc.

[0084] Preferably, the aluminum compound may be one or two or more selected from methylaluminoxane, modified methylaluminoxane, tetraisobutylaluminoxane, trimethylaluminium, triethylaluminium, trioctylaluminium and triisobutylaluminium.

[0085] The boron compound used as the above cocatalyst may be selected from boron compounds represented by the following chemical formulas D to F.

[0086] [Chemical Formula D]

[0087] B(R c )3

[0088] [Chemical Formula E]

[0089] [R d ] + [B(Rc )4] -

[0090] [Chemical formula F]

[0091] [(R e ) s ZH] + [B(R c )4] -

[0092] In the above chemical formulas D to F,

[0093] B is a boron atom; R c is phenyl, wherein said phenyl may be further substituted with 3 to 5 substituents selected from fluorine atom, C1-C20 alkyl substituted or unsubstituted by fluorine atom, and C1-C20 alkoxy substituted or unsubstituted by fluorine atom; R d is a C5-C7 aromatic radical or a C1-C20 alkylC6-C20 aryl radical, a C6-C20 arylC1-C20 alkyl radical, for example, a triphenylmethylium radical; Z is a nitrogen or phosphorus atom; R e is a C1-C20 alkyl radical or anilinium radical substituted with two C1-C10 alkyls together with a nitrogen atom; s is an integer of 2 or 3.

[0094] Examples of the above boron compounds include dimethylphenylammonium tetra(phenyl)borate, trityl tetra(phenyl)borate, dimethylphenylammonium tetra(pentafluorophenyl)borate, trityl tetrakis(pentafluorophenyl)borate, trimethylammonium tetra(phenyl)borate, triethylammonium tetra(phenyl)borate, tripropylammonium tetra(phenyl)borate, tributylammonium tetra(phenyl)borate, trimethylammonium tetrakis(pentafluorophenyl)borate, triethylammonium tetrakis(pentafluorophenyl)borate, tripropylammonium tetrakis(pentafluorophenyl)borate, tributylammonium tetrakis(pentafluorophenyl)borate, anilinium tetra(phenyl)borate, anilinium tetrakis(pentafluorophenyl)borate, pyridinium tetrakis(pentafluorophenyl)borate, etc.

[0095] The above-mentioned cocatalyst may specifically be a combination of an organoaluminum compound and a boron compound.

[0096] More specifically, the above cocatalyst may be a combination of an organoaluminum compound of the above chemical formula C and a boron compound of the above chemical formula E or F.

[0097] The above cocatalyst is one or more trialkylaluminum selected from trimethylaluminum, triethylaluminum, tripropylaluminum, triisobutylaluminum, trihexylaluminum and trioctylaluminum and dimethylphenylammonium tetra(phenyl)borate, trityl tetra(phenyl)borate, dimethylphenylammonium tetra(pentafluorophenyl)borate, trityl tetrakis(pentafluorophenyl)borate, trimethylammonium tetra(phenyl)borate, triethylammonium tetra(phenyl)borate, tripropylammonium tetra(phenyl)borate, tributylammonium tetra(phenyl)borate, trimethylammonium tetrakis(pentafluorophenyl)borate, triethylammonium tetrakis(pentafluorophenyl)borate, tripropylammonium tetrakis(pentafluorophenyl)borate, tributylammonium It may be a combination of one or more boron compounds selected from tetrakis(pentafluorophenyl)borate, anilinium tetra(phenyl)borate, anilinium tetrakis(pentafluorophenyl)borate and pyridinium tetrakis(pentafluorophenyl)borate.

[0098] The above cocatalyst can be used in an appropriate amount so that the activation of the first transition metal compound of the above chemical formula 1 and the second transition metal compound of the above chemical formula 2 can proceed sufficiently.

[0099] For example, when the aluminum compound and the boron compound are used simultaneously as a cocatalyst, a preferable range of the ratio between the total transition metal compound (first transition metal compound + second transition metal compound) included in the catalyst composition and the cocatalyst may be a molar ratio of transition metal (M): aluminum atom (Al): boron atom (B) of 1: (10 to 3,000): (1 to 100), and more preferably, a range of 1: (100 to 1,000): (3 to 10).

[0100] If the ratio between the entire transition metal compound and the cocatalyst is outside the above range, the amount of cocatalyst may be relatively small, so that the transition metal compound may not be fully activated, resulting in insufficient catalytic activity of the transition metal compound, or excessive cocatalyst may be used, resulting in a significant increase in production costs. Within the above range, excellent catalytic activity for producing ethylene polymers is exhibited, and the range of the ratio varies depending on the purity of the reaction.

[0101] The above catalyst composition may further include one or more C5-C12 aliphatic hydrocarbon solvents selected from pentane, hexane, heptane, octane, isooctane, nonane, decane, dodecane, cyclohexane and methylcyclohexane as a reaction solvent.

[0102] Since the above catalyst composition exists in a uniform form within a polymerization reactor, it is preferable to apply it to a high-temperature solution polymerization process of 110°C or higher.

[0103] Another aspect of the present invention provides a method for producing an ethylene polymer by polymerizing an ethylene monomer in the presence of the catalyst composition for producing an ethylene polymer.

[0104] The above ethylene monomer is ethylene or α-olefin; specifically, when producing an ethylene homopolymer, ethylene is used alone as a monomer, and when producing a copolymer of ethylene and α-olefin, one or more selected from among (C3~C18) α-olefin, (C5~C20) cycloolefin, styrene, and derivatives of styrene may be used as a comonomer copolymerized with ethylene. Preferred examples of the (C3~C18)α-olefin may be selected from the group consisting of propylene, 1-butene, 1-pentene, 4-methyl-1-pentene, 1-hexene, 1-heptene, 1-octene, 1-decene, 1-undecene, 1-dodecene, 1-tetradecene, 1-hexadecene and 1-octadecene, and preferred examples of the (C5~C20)cycloolefin may be selected from the group consisting of cyclopentene, cyclohexene, norbonene and phenylnorbornene, and styrene and its derivatives may be selected from styrene, α-methylstyrene, p-methylstyrene and 3-chloromethylstyrene. More preferably, the α-olefin may be one or more selected from 1-butene, 1-hexene, 1-octene and 1-decene.

[0105] The above manufacturing method can be carried out by contacting the catalyst composition for manufacturing an ethylene polymer according to one embodiment with ethylene or, if necessary, a comonomer in the presence of a suitable organic solvent. At this time, the first transition metal compound, the second transition metal compound, and the cocatalyst component can be separately introduced into the reactor, or each component can be mixed in advance and introduced into the reactor. There are no particular restrictions on the mixing conditions such as the order of introduction, temperature, or concentration.

[0106] The above polymerization reaction can be carried out at a temperature of 110°C to 170°C, specifically 120°C to 160°C, and under a pressure of 10 to 100 bar, and more specifically 130°C to 150°C, and under a pressure of 15 to 50 bar.

[0107] In addition, the above manufacturing method can be performed in a C5-C12 aliphatic hydrocarbon solvent, and specifically, the C5-C12 aliphatic hydrocarbon solvent can be one or two or more selected from pentane, hexane, heptane, octane, isooctane, nonane, decane, dodecane, cyclohexane and methylcyclohexane, and preferably hexane, cyclohexane or a mixture thereof.

[0108] The manufacturing method according to one embodiment does not use toluene, a common solvent commonly used in the manufacture of existing copolymers, and thus the toluene solvent removal step in the manufacturing process is reduced, making it a more economical manufacturing method.

[0109] The ethylene polymer prepared according to one embodiment may be an ethylene homopolymer.

[0110] In one embodiment, the ethylene polymer manufactured may be a copolymer of ethylene and an α-olefin. The copolymer of ethylene and an α-olefin contains 50 wt% or more of ethylene, preferably 60 wt% or more of ethylene, and more preferably 60 to 99 wt% of ethylene. The density of the copolymer of ethylene and an α-olefin may be 0.900 g / cm3 or less, specifically 0.850 g / cm3 to 0.900 g / cm3, and the molecular weight distribution (Mw / Mn) may be 4 or more, specifically 4.5 to 8.0, and may have bimodality.

[0111] Generally, a wider molecular weight distribution leads to lower viscosity as shear stress (shear rate) decreases, improving processability but also compromising physical properties such as strength. However, bimodality and a wide molecular weight distribution can improve processability while potentially enhancing physical properties, depending on the catalyst type.

[0112] The present invention is specifically described through the following examples, but the scope of the present invention is not limited by the following examples.

[0113] [Materials and Analytical Equipment]

[0114] All synthetic reactions were carried out under an inert atmosphere such as nitrogen or argon, using standard Schlenk and glove box techniques. Synthetic solvents such as tetrahydrofuran (THF), n-hexane, n-pentane, diethyl ether, and methylene chloride (CH2Cl2) were used after removing moisture by passing through an activated alumina column and storing on activated molecular sieves. Most reagents were purchased from Sigma-Aldrich, TCI, Alfa, and Strem unless otherwise stated. Synthetic ligands and catalysts 1 H NMR analysis was performed at room temperature using a Bruker 500 MHz.

[0115] [Measurement of physical properties]

[0116] The polymerized polymer was analyzed by the method described below.

[0117] 1. Polymerization activity

[0118] Polymerization activity (kg / g cat) was calculated as the weight ratio of polymer produced per amount of catalyst used.

[0119] 2. Melt Flow Index (MI)

[0120] Measured at 190°C under a load of 2.16 kg according to ASTM D1238.

[0121] 3. Density

[0122] Measured in a Density Gradient Column according to the ASTM D1505 method.

[0123] 4. Molecular weight distribution

[0124] Molecular weight distribution was measured using GPC (Gel Permeation Chromatography) at 150°C using 1,2,4-trichlorobenzene as a solvent, and the weight average molecular weight (Mw) and number average molecular weight (Mn) were calculated by dividing the measured Mw by Mn.

[0125] [Catalyst Preparation Example 1] Preparation of [1-(η5-cyclopentadien-1-yl)-1-(η5-fluorenyl)-1,1-diphenyl methane]hafnium dichloro (CAT-1)

[0126] [1-(η5-Cyclopentadien-1-yl)-1-(η5-fluorenyl)-1,1-diphenyl methane]hafnium dichloro (CAT-1) was synthesized by the procedure described in the literature [A. Razavi, JL Atwood, J. Organometallic. Chen, 459 (1993), 117-123].

[0127] 1 H NMR (500 MHz, Chloroform-d) δ 8.19 (d,J= 8.5 Hz, 2H), 7.95 (d,J= 8.3 Hz, 2H), 7.88 (d,J= 8.5 Hz, 2H), 7.55 (t,J= 8.0 Hz, 2H), 7.44 (t,J= 8.2 Hz, 2H), 7.31 (m, 4H), 7.01 (t,J= 8.1 Hz, 2H), 6.47 (d,J= 7.1 Hz, 2H), 6.33 (s, 2H), 5.75 (s, 2H)

[0128] [Catalyst Preparation Example 2] Preparation of [1-(η5-cyclopentadien-1-yl)-1-(η5-2,7-di-tertbutylfluorenyl)-1,1-diphenyl methane]hafnium dichloro (CAT-2)

[0129] Step 1: Preparation of 1-(cyclopentadien-1-yl)-1-(2,7-di-tertbutylfluorenyl)-1,1-diphenyl methane (a1)

[0130]

[0131] 2,7-Di-tertbutylfluorene (12 g, 43.1 mmol) was dissolved in THF (87 mL), n-BuLi (1.6 M in Hex, 27.1 mL, 43.1 mmol) was added, and the mixture was stirred at room temperature. After 3 h, 6,6-Diphenylfulvene (10 g, 43.1 mmol) was added. The reaction solution was stirred for 16 h, and then NH4Cl aqueous solution (40 mL) was poured to quench the reaction. The product was extracted into the organic layer, dried over MgSO4, filtered, and under reduced pressure, and the resulting yellow solid was washed with ethanol to obtain ligand a1 as a white solid (20 g, yield 93%).

[0132] 1 H NMR (500 MHz, Chloroform-d) δ 6.21~7.35 (m, 20H), 5.45 (s, 1H), 3.01 (m, 1H), 1.14 (s, 18H)

[0133] Step 2: Preparation of [1-(η5-cyclopentadien-1-yl)-1-(η5-2,7-di-tertbutylfluorenyl)-1,1-diphenyl methane]hafnium dichloro (CAT-2)

[0134]

[0135] 1-(Cyclopentadien-1-yl)-1-(2,7-di-tertbutylfluorenyl)-1,1-diphenyl methane (a1, 5 g, 9.82 mmol) is dissolved in 60 mL of ether, n-BuLi (1.6 M in Hex, 13.5 mL, 21.6 mmol) is added, and the mixture is stirred for 16 hours. After the reaction is complete, ether is removed by vacuum drying, n-hexane is added, and the mixture is depressurized by decantation. In a glove box, the lithiated intermediate a2 (5.1 g, 9.79 mmol) and HfCl4 (3.13 g, 9.79 mmol) are dissolved in 80 mL of ether in small portions. After stirring at room temperature for 16 hours, ether was removed by vacuum drying, 80 mL of toluene was added, and the mixture was heated at 50°C for 2 hours. The produced LiCl was precipitated and filtered. The filtrate was vacuum dried and then crystallized to obtain 4.4 g of yellow crystals of CAT-2 (recrystallized from toluene, yield 60%).

[0136] [Catalyst Preparation Example 3] Preparation of [1-(η5-cyclopentadien-1-yl)-1-(η5-2,7-di-dimethylaminefluorenyl)-1,1-diphenyl methane]hafnium dichloro (CAT-3)

[0137] Step 1: Preparation of 2,7-di-dimethylaminefluorene (b1)

[0138]

[0139] In a Schlenk flask, add NaBH4 (7.7 g, 203.8 mmol) and 2,7-DiaminoFluorene (5 g, 25.4 mmol), and maintain at 0℃. Add ethanol (50 mL), acetic acid (7.27 mL, 127 mmol), and paraformaldehyde (11.5 g, 382 mmol). After 16 h, extract three times with saturated NHCO3 aqueous solution and ether. The organic layer was collected, dried over MgSO4, filtered, and reduced pressure. After recrystallization using hexane, 2,7-di-dimethylaminefluorene (b1) was obtained as a yellow solid (5.1 g, 80%).

[0140] 1 H NMR (500 MHz, Chloroform-d) δ 7.50 (d,J= 8.5 Hz, 2H), 6.93 (d,J= 2.0 Hz, 2H), 6.76 (d,J= 7.7 Hz, 2H), 3.81 (s, 2H), 2.98 (s, 12H).

[0141] Step 2: Preparation of 1-(cyclopentadien-1-yl)-1-(2,7-di-n-butylfluorenyl)-1,1-diphenyl methane (b2)

[0142]

[0143] 2,7-Di-dimethylaminefluorene (b1, 12 g, 43.1 mmol) was dissolved in THF (87 mL), n-BuLi (1.6 M in Hex, 27.1 mL, 43.1 mmol) was added, and the mixture was stirred at room temperature. After 3 h, 6,6-Diphenylfulvene (10 g, 43.1 mmol) was added. The reaction solution was stirred for 16 h, and then NH4Cl aqueous solution (40 mL) was poured to quench the reaction. The product was extracted into the organic layer, dried over MgSO4, filtered, and under reduced pressure, and the resulting yellow solid was washed with ethanol to obtain brown solid ligand b2 (20 g, yield 91%).

[0144] Step 3: Preparation of [1-(η5-cyclopentadien-1-yl)-1-(η5-2,7-di-dimethylaminefluorenyl)-1,1-diphenylmethane]hafnium dichloro (CAT-3)

[0145]

[0146] 1-(Cyclopentadien-1-yl)-1-(2,7-di-dimethylaminebutylfluorenyl)-1,1-diphenylmethane (b2, 5 g, 9.82 mmol) is dissolved in 60 mL of ether, n-BuLi (1.6 M in Hex, 13.5 mL, 21.6 mmol) is added, and the mixture is stirred for 16 h. After the reaction is complete, ether is removed by vacuum drying, and n-hexane is added, decant, and the pressure is reduced. In a glove box, the lithiated intermediate b3 (5.1 g, 9.79 mmol) and HfCl4 (3.13 g, 9.79 mmol) are dissolved in 80 mL of ether in small portions. After stirring at room temperature for 16 hours, ether was removed by vacuum drying, 80 mL of toluene was added, and the mixture was heated at 50°C for 2 hours. The produced LiCl was precipitated and filtered. The filtrate was vacuum dried and then crystallized to obtain 4.5 g of yellow crystals of CAT-3 (recrystallized from toluene, yield 60%).

[0147] Example 1: Preparation of copolymer of ethylene and 1-octene

[0148] At room temperature, 1 L of hexane and 2 mL of triisobutyl aluminum (TIBA) (1 M in Hex) were injected into a 4 L reactor, followed by 100 mL of 1-octene. In a glove box, catalysts CAT-1 (3.9 μmol) and CAT-3 (3.9 μmol) were weighed and mixed with 2 mL of TIBA (0.1 M in Hex), and 5 mL of toluene was additionally added and injected into the reactor inlet. In the glove box, 19.5 μmol of trityl tetrakis(pentafluorophenyl)borate was mixed with 5 mL of toluene and injected into the reactor inlet. After raising the reactor temperature to 140°C, the solution in the inlet was forced into the reactor using high-pressure nitrogen. Ethylene injection was performed at 21 bar for 15 minutes, and it was shown that the initial temperature increased in proportion to the activity. After polymerization, the reactor temperature was cooled to 30°C, and the ethylene pressure inside the reactor was slowly exhausted to remove it. The reaction product was washed with ethanol and acetone, filtered, and vacuum-dried. The physical properties of the obtained polymer are listed in Table 1.

[0149] Example 2

[0150] Polymerization was performed by following the same procedure as in Example 1, except that CAT-2 was used instead of CAT-1 in Example 1, and the properties of the obtained polymer are shown in Table 1 below.

[0151] Comparative Example 1

[0152] Polymerization was performed in the same manner as in Example 1, except that the catalyst Ph2C(Cp)(Flu)ZrCl2(diphenylmethylidene(cyclopentadienyl)(9-fluorenyl)zirconium dichloride) was used instead of CAT-1 in Example 1, and the properties of the obtained polymer are shown in Table 1 below.

[0153] Comparative Example 2

[0154] Polymerization was performed in the same manner as in Example 1, except that Et(IND)2ZrCl2 (ethylenebis(indenyl)zirconium dichloride) catalyst was used instead of CAT-1 in Example 1, and the properties of the obtained polymer are shown in Table 1 below.

[0155] Comparative Example 3

[0156] Polymerization was performed in the same manner as in Example 1, except that Et(THI)2ZrCl2(ethylenebis(tetrahydroindenyl)zirconium Dichloride) catalyst was used instead of CAT-1 in Example 1, and the properties of the obtained polymer are shown in Table 1 below.

[0157] Comparative Example 4

[0158] Polymerization was performed in the same manner as in Example 1, except that CAT-3 was not used and only the catalyst CAT-1 (7.8 μmol) was used, and the properties of the obtained polymer are shown in Table 1 below.

[0159] Comparative Example 5

[0160] Polymerization was performed in the same manner as in Example 1, except that CAT-3 and CAT-1 were not used and only the catalyst CAT-2 (7.8 μmol) was used, and the properties of the obtained polymer are shown in Table 1 below.

[0161] Comparative Example 6

[0162] Polymerization was performed in the same manner as in Example 1, except that CAT-1 was not used and only the catalyst CAT-3 (7.8 μmol) was used, and the properties of the obtained polymer are shown in Table 1 below.

[0163] Polymerization transition metal catalyst activity (Kg / g cat) MI (2.16 Kg / 10min) Density (g / cm) 3)Molecular weight distribution (Mw / Mn)Example 1CAT-1CAT-310.50.770.8834.8Example 2CAT-2CAT-327.31.20.8727.8Comparison 1Ph2C(Cp)(Flu)ZrCl2CAT-315.623.20.9103.2Comparison Example 2Et(IND)2ZrCl2CAT-317.817.20.9212.4Comparison 3Et(THI)2ZrCl2CAT-312.815.10.9022.7Comparison Example 4CAT-11.80.91420.86032.32Comparison Example 5CAT-210.50.22910.86782.09Comparison Example 6CAT-37.210.2910.89482.57CAT-1: CAT-2: CAT-3: Ph2C(Cp)(Flu)ZrCl2 : Et(IND)2ZrCl2 : Et(THI)2ZrCl2 :

[0164] As shown in Table 1 above, as can be seen from the ethylene / 1-octene copolymerization results of Examples 1 and 2, it can be confirmed that the polymers produced by the novel catalyst system according to the present invention, i.e., the combination of CAT-3 and CAT-1 (Example 1) and the combination of CAT-3 and CAT-2 (Example 2), have a wide molecular weight distribution of 4 or more and a low density of 0.9 or less.

[0165] In Comparative Examples 4 to 6 using CAT-1, CAT-2, and CAT-3 alone, the molecular weight distribution is narrow, and the combination of Ph2C(Cp)(Flu)ZrCl2 and CAT-3 (Comparative Example 1), the combination of Et(IND)2ZrCl2 and CAT-3 (Comparative Example 2), and the combination of Et(THI)2ZrCl2 and CAT-3 (Comparative Example 3) show narrow molecular weight distribution and high density of 0.9 or higher.

[0166] GPC data of Example 2 using CAT-3 and CAT-2 as polymerization catalysts is shown in Fig. 1. As in Examples 1 and 2 of the present invention, when CAT-3, which produces a low molecular weight polymer, and CAT-1 and CAT-2, which produce high molecular weight polymers, are combined and used as a polymerization catalyst, a bimodal polymer is produced, as shown in Fig. 1.

[0167] That is, it can be seen that the novel catalyst system according to the present invention is a catalyst system capable of obtaining a low-density polymer with a broad molecular weight distribution and bimodality under high-temperature and high-pressure polymerization conditions.

[0168] While the embodiments of the present invention have been described in detail above, those skilled in the art will appreciate that various modifications and variations can be made to the present invention without departing from the scope of the invention as defined in the appended claims. Therefore, modifications to future embodiments of the present invention will not depart from the scope of the invention.

Claims

1. A first transition metal compound represented by the following chemical formula 1; A second transition metal compound represented by the following chemical formula 2; and A catalyst composition for producing an ethylene polymer, comprising a cocatalyst selected from an aluminum compound, a boron compound or a mixture thereof. [Chemical Formula 1] [Chemical Formula 2] In the above chemical formulas 1 and 2 M 1 is a transition metal in group 4 of the periodic table; R 1 Inland R 4 are each independently C1-C20 alkyl or C6-C20 aryl; R 5 , R 6 , R 15 and R 16 are each independently C6-C20 aryl, and the above R 5 , R 6 , R 15 and R 16 The aryl of may be further substituted with C1-C20 alkyl; R 11 and R 12 are each independently hydrogen or C1-C20 alkyl; X 1 , X 2 , X 11 and X 12 are each independently halogen, C1-C20 alkyl, C3-C20 cycloalkyl, C6-C20 aryl, C6-C20 arylC1-C20 alkyl, (C1-C20 alkylC6-C20 aryl)C1-C20 alkyl, C1-C20 alkoxy, C6-C20 aryloxy, C1-C20 alkylC6-C20 aryloxy, C1-C20 alkoxyC6-C20 aryloxy, -OSiR a R b R c , -SR d , -NR e R f , -PR g R h or C1-C20 alkylidene; R a Inland R d are independently C1-C20 alkyl, C6-C20 aryl, C6-C20 arylC1-C20 alkyl, C1-C20 alkylC6-C20 aryl or C3-C20 cycloalkyl; R e Inland R h are independently C1-C20 alkyl, C6-C20 aryl, C6-C20 arylC1-C20 alkyl, C1-C20 alkylC6-C20 aryl or C3-C20 cycloalkyl; X 1 and X 2 If one of them is C1-C20 alkylidene, the other is absent; X 11 and X 12 If one of them is C1-C20 alkylidene, the other is absent.

2. In paragraph 1, Above M 1 is Zr or Hf; R 1 Inland R 4 are each independently C1-C20 alkyl or C6-C20 aryl; R 5 , R 6 , R 15 and R 16 are each independently C6-C20 aryl, and the above R 5 , R 6 , R 15 and R 16 The aryl of may be further substituted with C1-C20 alkyl; R 11 and R 12 are each independently hydrogen or C1-C20 alkyl; X 1 , X 2 , X 11 and X 12 A catalyst composition for producing an ethylene polymer, wherein each independently represents halogen, C1-C20 alkyl, C6-C20 aryl or C6-C20 arylC1-C20 alkyl.

3. In paragraph 1, Above M 1 is Hf; R 1 Inland R 4 are each independently C1-C10 alkyl or C6-C12 aryl; R 5 , R 6 , R 15 and R 16 are each independently C6-C12 aryl, and the above R 5 , R 6 , R 15 and R 16 The aryl of may be further substituted with C1-C10 alkyl; R 11 and R 12 are each independently hydrogen or C1-C10 alkyl; X 1 , X 2 , X 11 and X 12 A catalyst composition for producing an ethylene polymer, wherein each independently represents halogen, C1-C10 alkyl, C6-C12 aryl or C6-C12 arylC1-C10 alkyl.

4. In paragraph 1, Above M 1 is Hf; R 1 Inland R 4 are identical to each other and are C1-C10 alkyl or C6-C12 aryl; R 5 , R 6 , R 15 and R 16 are each independently and R 21 is C1-C10 alkyl; a is an integer from 0 to 5; R 11 and R 12 are identical to each other and are hydrogen or C1-C10 alkyl; X 1 , X 2 , X 11 and X 12 A catalyst composition for producing an ethylene polymer, wherein each independently represents halogen, C1-C6 alkyl, C6-C12 aryl or C6-C12 arylC1-C6 alkyl.

5. In paragraph 1, The first transition metal compound is [1-(η5-cyclopentadien-1-yl)-1-(η5-2,7-di-dimethylaminefluorenyl)-1,1-diphenyl methane]hafnium dichloro, [1-(η5-cyclopentadien-1-yl)-1-(η5-2,7-di-dimethylaminefluorenyl)-1,1-diphenyl methane]hafnium dibenzyl, or [1-(η5-cyclopentadien-1-yl)-1-(η5-2,7-di-dimethylaminefluorenyl)-1,1-diphenyl methane]hafnium dimethyl; The second transition metal compound is [1-(η5-cyclopentadien-1-yl)-1-(η5-fluorenyl)-1,1-diphenyl methane]hafnium dichloro, [1-(η5-cyclopentadien-1-yl)-1-(η5-fluorenyl)-1,1-diphenyl methane]hafnium dibenzyl, [1-(η5-cyclopentadien-1-yl)-1-(η5-fluorenyl)-1,1-diphenyl methane]hafnium dimethyl, [1-(η5-cyclopentadien-1-yl)-1-(η5-2,7-di-tertbutylfluorenyl)-1,1-diphenyl methane]hafnium dichloro, A catalyst composition for producing an ethylene polymer, comprising [1-(η5-cyclopentadien-1-yl)-1-(η5-2,7-di-tertbutylfluorenyl)-1,1-diphenyl methane]hafnium dibenzyl or [1-(η5-cyclopentadien-1-yl)-1-(η5-2,7-di-tertbutylfluorenyl)-1,1-diphenyl methane]hafnium dimethyl.

6. In paragraph 1, A catalyst composition for producing an ethylene polymer, wherein the aluminum compound is one or more selected from an aluminoxane compound and an organoaluminum compound.

7. In paragraph 1, The above aluminum compound is selected from methylaluminoxane, modified methylaluminoxane, tetraisobutylaluminoxane, trimethylaluminium, triethylaluminium, triisobutylaluminium, trihexylaluminium and trioctylaluminium, alone or in a mixture thereof, a catalyst composition for producing an ethylene polymer.

8. In paragraph 1, A catalyst composition for producing an ethylene polymer, wherein the boron compound is one or more selected from dimethylphenylammonium tetraphenylborate, trityl tetraphenylborate, dimethylphenylammonium tetra(pentafluorophenyl)borate, trityl tetrakis(pentafluorophenyl)borate, trimethylammonium tetraphenylborate, triethylammonium tetraphenylborate, tripropylammonium tetraphenylborate, tributylammonium tetraphenylborate, trimethylammonium tetrakis(pentafluorophenyl)borate, triethylammonium tetrakis(pentafluorophenyl)borate, tripropylammonium tetrakis(pentafluorophenyl)borate, tributylammonium tetrakis(pentafluorophenyl)borate, anilinium tetraphenylborate, anilinium tetrakis(pentafluorophenyl)borate, and pyridinium tetrakis(pentafluorophenyl)borate.

9. A method for producing an ethylene polymer by polymerizing an ethylene monomer in the presence of a catalyst composition for producing an ethylene polymer according to any one of claims 1 to 8.

10. In paragraph 9, A manufacturing method wherein the above ethylene polymer is an ethylene homopolymer or a copolymer of ethylene and α-olefin.

11. In paragraph 10, The above ethylene monomer is ethylene or α-olefin; A manufacturing method, wherein the α-olefin copolymerized with the above ethylene is one or more selected from propylene, 1-butene, 1-pentene, 4-methyl-1-pentene, 1-hexene, 1-heptene, 1-octene, 1-decene, 1-undecene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-octadecene, cyclopentene, cyclohexene, norbonene, phenylnorbornene, 1,4-butadiene, 1,5-pentadiene, 1,6-hexadiene, styrene, alpha-methylstyrene, p-methylstyrene, divinylbenzene, and 3-chloromethylstyrene.

12. In paragraph 9, A manufacturing method wherein the above polymerization reaction is performed at a temperature of 120 to 160°C and a pressure of 10 to 100 bar.

13. In paragraph 9, A manufacturing method wherein the above polymerization reaction is carried out in a C5-C12 aliphatic hydrocarbon solvent.

Citation Information

Patent Citations

  • Continuous preparation method of novel polyethylene

    CN114591458A

  • Polyolefins for catalyst compositions and extrusion coating applications

    JP2007520597A

  • Catalyst for production of polyethylene and method for producing polyethylene

    JP2018162384A

  • Catalyst for producing ultrahigh molecular weight polyethylene-based copolymer and method for producing ultrahigh molecular weight polyethylene-based copolymer using the same

    JP2019167430A

  • Dual Metallocene Catalyst Copolymer Compositions

    US20190169322A1