Cathode active material for lithium secondary battery, manufacturing method for same, and lithium secondary battery comprising same

The development of a single-particle nickel-containing layered lithium transition metal oxide with a medium particle size and bimodal distribution addresses the limitations of small particle size cathode materials, enhancing energy density and lifespan through a two-stage firing process and strategic element addition, resulting in improved electrochemical performance.

WO2024205103A1PCT designated stage expired Publication Date: 2024-10-03POSCO HLDG INC +1

Patent Information

Application Number
PCT/KR2024/003421
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-19
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Lithium-ion batteries face limitations in electrode energy density and lifespan due to the small particle size of single-particle cathode active materials, which results in poor electrochemical properties and capacity retention, as larger particle sizes compromise lithium ion movement and structural stability.

Method used

A single-particle nickel-containing layered lithium transition metal oxide with a medium volume-based average particle diameter of 5 to 8 μm, comprising both small-diameter single particles and medium-diameter quasi-single particles, optimized through a two-stage firing process and incorporating grain growth promoting elements and a coating layer to enhance tap density and electrochemical performance.

Benefits of technology

The solution significantly improves electrode energy density, charge/discharge efficiency, and lifespan characteristics by balancing particle size and structure, while maintaining high nickel content and incorporating elements like Zr, Al, or B to promote grain growth and stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2024003421_03102024_PF_FP_ABST
    Figure KR2024003421_03102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to a cathode active material for a lithium secondary battery, the cathode active material being a single particle-based nickel-containing layered lithium transition metal oxide which has a volume-based average particle diameter (Dv50) of 5-8 μm, comprises a small-particle-diameter single particle formed from one primary particle, and a medium-particle-diameter quasi-single particle formed from a plurality of primary particles, and, in a number-based particle size distribution curve analysis, has maximum peaks in the particle diameter ranges of 0.7-1.2 μm and 2.5-4.0 μm.
Need to check novelty before this filing date? Find Prior Art

Description

Positive electrode active material for lithium secondary batteries, method for producing the same, and lithium secondary batteries comprising the same

[0001] The present invention relates to a positive electrode active material for a lithium secondary battery, a method for producing the same, and a lithium secondary battery comprising the same, and more specifically, to a positive electrode active material for a single-particle lithium secondary battery, a method for producing the same, and a lithium secondary battery comprising the same.

[0002]

[0003] As electric vehicles expand to achieve carbon neutrality and demand for energy storage devices such as ESS for renewable energy sources surges, lithium-ion batteries are becoming an irreplaceable, core energy storage device. In particular, the characteristics of lithium-ion batteries are significantly influenced by their cathode materials, making cathode material research a significant part of lithium-ion battery research.

[0004] Among cathode materials, active research is being conducted on NCM cathode materials, which substitute cobalt and manganese for nickel-based cathode active materials with a layered structure. Previously, much research has focused on secondary particle active materials formed by agglomeration of primary particles. However, these secondary particle active materials have large surface areas and low particle strength, leading to problems such as cracking and reduced lifespan due to gas generation. Therefore, development is underway on single-particle cathode materials composed of a single primary particle. These are primarily produced for small-particle cathode materials with an average particle diameter of approximately 3 to 5 μm in bimodal cathode materials.

[0005] The above-mentioned small-diameter single particles possess excellent mechanical particle strength characteristics, resulting in excellent lifespan and stability. However, the small particle size results in a low tap density, which limits the ability to increase electrode energy density.

[0006] To solve this problem, there were attempts to increase the tap density by increasing the particle size of a single particle, but as the particle size of a single particle increases, the lithium ion movement distance increases, which resulted in a problem of decreased electrochemical characteristics (i.e., capacity, charge / discharge efficiency, output characteristics, etc.) related to lithium diffusion.

[0007]

[0008] Accordingly, one object of the present invention is to provide a cathode active material for a lithium secondary battery, which is a single-particle series cathode active material capable of improving electrode energy density and evenly improving the capacity, charge / discharge efficiency, and lifespan characteristics of the battery, a method for producing the same, and a lithium secondary battery including the same.

[0009]

[0010] One embodiment of the present invention provides a cathode active material for a lithium secondary battery, which is a nickel-containing layered lithium transition metal oxide of a single particle series, having a volume-based average particle diameter (Dv50) of 5 to 8 μm, including a small-diameter single particle composed of one primary particle and a medium-diameter quasi-single particle composed of multiple primary particles, and having peaks in a particle diameter range of 0.7 to 1.2 μm and a particle diameter range of 2.5 to 4.0 μm when analyzing a particle size distribution curve based on number.

[0011] The above positive electrode active material may have a compressed density of 3.6 g / cc or more after applying a pressure of 9 tons.

[0012] The number ratio of the single particle and the quasi-single particle (single particle:quasi-single particle) may be 8:2 to 5:5.

[0013] The above positive electrode active material for a lithium secondary battery can satisfy the following equation 1.

[0014] [Formula 1]

[0015] Average particle size by volume (Dv50) - Average particle size by number (Dn50) ≥ 3.5 μm

[0016] The above lithium transition metal oxide may contain nickel in an amount of 60 mol% or more based on the total mole number of transition metals.

[0017] The above lithium transition metal oxide may further include a grain growth promoting element such as Zr, Al, B or a combination thereof.

[0018] The content of the above-mentioned growth promoting element may be 0.1 to 1 mol% based on the total mole number of transition metals.

[0019] The above positive electrode active material may further include a coating layer including Co, Al or a combination thereof on the lithium transition metal oxide.

[0020] The above lithium transition metal oxide can be represented by the following chemical formula 1.

[0021] [Chemical Formula 1]

[0022] Li a [Ni x Co y Mn z M1 w1 M2 w2 ]O2

[0023] In the above chemical formula 1, 0.8≤a≤1.2, 0.60≤x<1, 0≤y≤0.4, 0≤z≤0.4, 0≤w1≤0.01, 0≤w2≤0.2, x+y+z+w1+w2=1, M1 is Zr, Al, B or a combination thereof, and M2 is Y, Mg, Ti, Nb, W, Sc, Si, V, Fe, Y, Mo, Ce, Hf, Ta, La, Sr or a combination thereof.

[0024]

[0025] Another embodiment of the present invention provides a positive electrode for a lithium secondary battery comprising the positive electrode active material described above.

[0026] Another embodiment of the present invention provides a lithium secondary battery including the positive electrode for the lithium secondary battery.

[0027]

[0028] A cathode active material for a lithium secondary battery according to one embodiment of the present invention has a medium-sized particle size based on volume, and includes small-sized and medium-sized particles, thereby greatly improving electrode energy density.

[0029] In addition, the cathode active material for a lithium secondary battery according to one embodiment of the present invention can evenly improve battery capacity, charge / discharge efficiency, and life characteristics, as the small-diameter active material is a single particle composed of one primary particle, and the medium-diameter active material is a quasi-single particle composed of multiple primary particles.

[0030]

[0031] Figure 1 is a SEM image of a positive electrode active material manufactured according to Example 1.

[0032] Figure 2 is an SEM image of a positive electrode active material manufactured according to Comparative Example 1.

[0033] Figure 3 is an SEM image of a positive electrode active material manufactured according to Comparative Example 2.

[0034] Figure 4 is a graph of particle size distribution curves based on the number of positive electrode active materials manufactured according to Example 1, Comparative Example 1, and Comparative Example 2.

[0035]

[0036] The terms first, second, and third, etc., are used to describe, but are not limited to, various parts, components, regions, layers, and / or sections. These terms are used only to distinguish one part, component, region, layer, or section from another part, component, region, layer, or section. Accordingly, a first part, component, region, layer, or section described below may be referred to as a second part, component, region, layer, or section without departing from the scope of the present invention.

[0037] The terminology used herein is for the purpose of describing particular embodiments only and is not intended to limit the present invention. As used herein, the singular forms "singular" and "comprising" include plural forms as well, unless the context clearly dictates otherwise. The word "comprising" as used herein specifies a particular feature, region, integer, step, operation, element, and / or component, but does not exclude the presence or addition of other features, regions, integers, steps, operations, elements, and / or components.

[0038] When a part is referred to as being "on" or "over" another part, it can be directly on or over the other part, or there may be other parts intervening. Conversely, when a part is referred to as being "directly on" another part, there are no other parts intervening.

[0039] Although not defined otherwise, all terms, including technical and scientific terms, used herein have the same meaning as commonly understood by those of ordinary skill in the technical field to which the present invention pertains. Terms defined in commonly used dictionaries are further interpreted to have meanings consistent with the relevant technical literature and the present disclosure, and are not to be construed as ideal or overly formal unless otherwise defined.

[0040] Also, unless otherwise stated, % means weight%, and 1 ppm is 0.0001 weight%.

[0041] In this specification, the term "combination(s) thereof" described in the expression in the Makushi format means one or more mixtures or combinations selected from the group consisting of the components described in the expression in the Makushi format, and means including any one or more selected from the group consisting of said components.

[0042] Hereinafter, embodiments of the present invention will be described in detail so that those skilled in the art can easily implement them. However, the present invention may be implemented in various different forms and is not limited to the embodiments described herein.

[0043]

[0044] One embodiment of the present invention provides a cathode active material for a lithium secondary battery, which is a nickel-containing layered lithium transition metal oxide of a single particle series, having a volume-based average particle diameter (Dv50) of 5 to 8 μm, including a small-diameter single particle composed of one primary particle and a medium-diameter quasi-single particle composed of multiple primary particles, and having peaks in a particle diameter range of 0.7 to 1.2 μm and a particle diameter range of 2.5 to 4.0 μm when analyzing a particle size distribution curve based on number.

[0045]

[0046] A cathode active material for a lithium secondary battery according to one embodiment of the present invention is composed of single-particle series particles.

[0047] In this specification, the term “single particle” is used to distinguish it from the secondary particle type positive electrode active material particle formed by the agglomeration of tens to hundreds of primary particles, which has been commonly used in the past, and is a concept that includes a single particle composed of one primary particle and an aggregate particle of 30 or fewer primary particles. The “secondary particle” refers to an aggregate, i.e., a secondary structure, formed by the physical or chemical bonding between primary particles without an intentional agglomeration or assembly process for the primary particles.

[0048] The above “primary particle” refers to the smallest particle unit that can be distinguished as a single lump when observing the cross-section of the positive electrode active material through a scanning electron microscope (SEM), and may be composed of a single crystal grain or multiple crystal grains.

[0049] Since the cathode active material for a lithium secondary battery according to one embodiment of the present invention is composed of single-particle series particles, the particle strength is increased, which can suppress particle breakage during rolling, and the occurrence of cracks between primary particles during repeated charging and discharging can be prevented, and the specific surface area is small, which can reduce the amount of gas generated due to side reactions with the electrolyte.

[0050]

[0051] The positive electrode active material for a lithium secondary battery according to one embodiment of the present invention may have an average particle diameter (Dv50) based on volume of 5 to 8 μm, and more specifically, 5.2 to 8 μm, 5.5 to 8 μm, or 6 to 8 μm.

[0052] In this specification, the volume-based average particle diameter (Dv50) can be defined as the particle diameter corresponding to 50% of the volume accumulation amount in the particle diameter distribution curve. The average particle diameter (Dv50) can be measured using, for example, the laser diffraction method. The laser diffraction method can generally measure particle diameters from the submicron range to several millimeters, and can obtain results with high reproducibility and high resolution.

[0053] As the average particle diameter of the positive electrode active material is sufficiently large as in the above range, the tap density can be further improved compared to conventional small-diameter single particles, and as a result, the electrode energy density can be greatly improved.

[0054]

[0055] In addition, the cathode active material for a lithium secondary battery according to one embodiment of the present invention includes both a small-diameter single particle composed of only one primary particle and a medium-diameter medium particle composed of multiple primary particles.

[0056] In this specification, “single particle” means a single particle composed of only one primary particle, and “quasi-single particle” means a single particle composed of multiple primary particles.

[0057] Since the positive electrode active material includes both small- and medium-sized particles, the effect of improving the electrode energy density can be further maximized.

[0058] The volume average particle diameter of the positive electrode active material according to the present invention is in the medium particle diameter range, but the small particle diameter particles are single particles and the medium particle diameter particles are quasi-single particles. Therefore, the capacity, charge / discharge efficiency, and life characteristics of the battery can be further improved compared to the active material composed of only single particles and the active material composed of only quasi-single particles.

[0059] Additionally, the above-mentioned suspended particles may be spherical. Accordingly, the electrochemical properties of the battery may be further improved. In this specification, the term "spherical" does not necessarily mean a spherical particle, but rather encompasses pseudo-spherical particles.

[0060]

[0061] According to one embodiment of the present invention, a positive electrode active material for a lithium secondary battery has peaks in a particle size range of 0.7 to 1.2 μm and a particle size range of 2.5 to 4.0 μm when analyzing a particle size distribution curve based on number.

[0062] In this specification, the particle size distribution curve based on the number of active materials refers to the particle size distribution curve based on the number of active materials measured using the Mastersizer 3000 equipment from Malvern. This product is the world's most widely used laser diffraction particle size analyzer. In particular, it provides particle analysis solutions down to the nanoscale, making it an analytical device suitable for active materials with numerous small particle sizes, such as those of the present invention.

[0063] At this time, most of the particles forming a peak of 0.7 to 1.2 μm may be single particles of small particle size, and most of the particles forming a peak of 2.5 to 4.0 μm may be quasi-single particles of medium particle size.

[0064] When the range of peaks on the particle size distribution curve satisfies the above range, the aforementioned electrode energy density improvement and battery electrochemical characteristic effects can be preferably implemented.

[0065]

[0066]

[0067] In particular, the cathode active material for the lithium secondary battery may have an average particle diameter (Dn50) based on the number of particles of 1.5 μm or less.

[0068] In this specification, the average particle diameter based on number (Dn50) can be defined as the particle diameter corresponding to 50% of the accumulated number amount in the particle diameter distribution curve. The average particle diameter based on number (Dn50) can be measured using, for example, the laser diffraction method.

[0069] That is, in the positive electrode active material according to one embodiment, the average particle diameter (Dn50) based on the number of particles in the above range may have a value that is considerably smaller than the average particle diameter (Dv50) based on the volume of the medium particle size range mentioned above. This means that the number of small particle size active materials is large, and as a result, since there are many small particle sizes with excellent particle strength, the small particle sizes effectively fill the gaps between the medium particle sizes, thereby dramatically improving the rolling density, and due to the short diffusion distance of the small particle sizes, the capacity and efficiency of the positive electrode active material may also be improved.

[0070] More specifically, the positive electrode active material for the lithium secondary battery can satisfy the following equation 1.

[0071] [Formula 1]

[0072] Average particle size by volume (Dv50) - Average particle size by number (Dn50) ≥ 3.5 μm

[0073] The technical significance of the positive electrode active material satisfying Equation 1 is the same as described above.

[0074]

[0075] In addition, the cathode active material for the lithium secondary battery may have a particle size (Dn10) based on the number of particles of 1.0 μm or less. In addition, the cathode active material for the lithium secondary battery may have a particle size (Dn90) based on the number of particles of 4 to 5.8 μm.

[0076] In this specification, the particle size based on number (Dn10) and the particle size based on number (Dn90) can be defined as particle sizes corresponding to 10% and 90% of the number accumulation amount, respectively, in the particle size distribution curve of the particles.

[0077]

[0078] When the number-based particle diameter (Dn10) and number-based particle diameter (Dn90) of the positive electrode active material satisfy the above range, the battery electrochemical characteristics can be more preferably implemented.

[0079]

[0080] In addition, the positive electrode active material for a lithium secondary battery according to one embodiment of the present invention may have a compression density of 3.6 g / cc or more after applying 9 tons of pressure. The above physical property corresponds to the rolling density of the active material during electrode manufacturing, and thus, having such a high compression density can improve the electrode energy density.

[0081] In this specification, the compression density after applying 9 tons of pressure to the active material can be measured by loading 3g of the active material sample into a pellet with a diameter of 13mm, applying 9 tons of pressure using a hydraulic press from Caver, and then measuring the change in height of the pellet before and after applying the pressure. The specific calculation formula is as follows.

[0082] [Calculation Formula 1]

[0083] Density after applying 9 tons of pressure = Weight of active material sample (3g) / (Φ*(1.3cm / 2) 2 *(Height change before and after pressure application)

[0084] In the above calculation formula 1, Φ represents pi.

[0085]

[0086] Meanwhile, the average number of primary particles in the quasi-single particle may be 20 or less, and more specifically, 15 or less. If the average number of primary particles in the quasi-single particle becomes too large, the particle may have a polycrystalline nature, weakening the particle strength and increasing the specific surface area, which may deteriorate the life characteristics of the battery.

[0087]

[0088] In addition, the number ratio of the single particles and the quasi-single particles (single particles: quasi-single particles) may be 8:2 to 5:5. In the present specification, the number ratio of the single particles and the quasi-single particles can be derived by measuring the number of single particles and quasi-single particles produced by image software in a (25 μm) × (20 μm) 2D image observed in a SEM (scanning electron microscope) image at a magnification of 5,000 times. When the number ratio of the single particles and the quasi-single particles satisfies the above range, the aforementioned effects of improving electrode energy density and improving battery electrochemical characteristics can be more preferably implemented.

[0089]

[0090] Meanwhile, the lithium transition metal oxide may contain nickel in an amount of 60 mol% or more, and more specifically, 70, 80, or 90 mol% or more, based on the total moles of transition metals. With such a high nickel content, high-capacity characteristics can be realized.

[0091] The lithium transition metal oxide may further include a grain growth promoting element composed of Zr, Al, B, or a combination thereof. By further including the grain growth promoting element in the lithium transition metal oxide, the sintering temperature for forming the lithium transition metal oxide can be lowered, thereby preventing crystal defects such as an increase in the cation mixing ratio due to high-temperature sintering, and the average particle diameter of single particles can be efficiently increased during the sintering process.

[0092] The content of the above grain growth promoting element may be 0.1 to 1 mol% based on the total mole number of transition metals, and more specifically, 0.3 to 1 mol%. More specifically, the content of Zr may be 0.1 to 0.3 mol% based on the total mole number of transition metals. In addition, the content of Al may be 0.2 to 1 mol% based on the total mole number of transition metals. In addition, the content of B may be 0.1 to 1 mol% based on the total mole number of transition metals.

[0093] When the content of the growth-promoting element satisfies the above range, the effect of adding the growth-promoting element described above and the effect of preventing deterioration of electrochemical properties due to excessive addition can be equally implemented.

[0094]

[0095] The above-described positive electrode active material may further include a coating layer comprising Co, Al, or a combination thereof on the lithium transition metal oxide. By further including a coating layer having the above-described composition, the positive electrode active material can suppress side reactions with the electrolyte, improve the structural stability of the active material, and further improve battery life characteristics.

[0096]

[0097] The lithium transition metal oxide according to the present invention can be more specifically represented by the following chemical formula 1.

[0098] [Chemical Formula 1]

[0099] Li a [Ni x Co y Mn z M1 w1 M2 W2 ]O2

[0100] In the above chemical formula 1, 0.8≤a≤1.2, 0.60≤x<1, 0≤y≤0.4, 0≤z≤0.4, 0≤w1≤0.01, 0≤w2≤0.2, x+y+z+w1+w2=1, M1 is Zr, Al, B or a combination thereof, and M2 is Y, Mg, Ti, Nb, W, Sc, Si, V, Fe, Y, Mo, Ce, Hf, Ta, La, Sr or a combination thereof.

[0101] In the lithium transition metal oxide of the above chemical formula 1, lithium may be included in a content corresponding to a, that is, 0.8≤a≤1.2. If a is too small, the capacity may be reduced, and if a is too large, the strength of the sintered positive electrode active material may be increased, making pulverization difficult, and the amount of gas generated may increase due to an increase in lithium byproducts. Considering the effect of improving the capacity characteristics of the positive electrode active material according to the control of the lithium content and the sinterability balance during the production of the active material, the lithium may be included in a content of 0.9≤a≤1.1 more preferably.

[0102] In the lithium transition metal oxide of the above chemical formula 1, nickel may be included in an amount corresponding to x, that is, 0.6≤x<1, 0.6≤x≤0.97, 0.80≤x≤0.97, or 0.90≤x≤0.97. If the nickel amount is too low, it may be difficult to achieve high capacity of the battery, and if the nickel amount is too high, the battery life and safety may be reduced due to a decrease in the structural stability of the active material.

[0103] In the lithium transition metal oxide of the above chemical formula 1, cobalt may be included in an amount corresponding to y, i.e., 0≤y≤0.4, 0≤y≤0.2, or 0≤y≤0.1. If the cobalt amount is too low, it may be difficult to simultaneously achieve sufficient rate characteristics and high powder density of the active material. If the cobalt amount is too high, the overall cost of the raw material may increase and the reversible capacity may decrease.

[0104] In the lithium transition metal oxide of the above chemical formula 1, manganese may be included in a content corresponding to z, i.e., 0≤z≤0.4. If the manganese content is too low, the production cost may increase and the stability of the active material may decrease. If the manganese content is too high, the capacity and output characteristics of the battery may decrease.

[0105] In the lithium transition metal oxide of the above chemical formula 1, M1 may be included in a content corresponding to w1, that is, 0≤w1≤0.01. At this time, M1 is a grain growth promoting element, and is Zr, Al, B, or a combination thereof.

[0106] In the lithium transition metal oxide of the above chemical formula 1, M2 may be included in a content corresponding to w2, that is, 0≤w2≤0.2. At this time, M2 is another doping element, such as Y, Mg, Ti, Nb, W, Sc, Si, V, Fe, Y, Mo, Ce, Hf, Ta, La, Sr, or a combination thereof.

[0107]

[0108] According to another embodiment of the present invention, a method for manufacturing a cathode active material for a lithium secondary battery comprises the steps of: preparing a nickel-containing transition metal precursor; forming a mixture including the transition metal precursor and a lithium raw material and then firing the mixture to form a lithium transition metal oxide having a large number of primary particles; post-firing the lithium transition metal oxide; and pulverizing the post-firing lithium transition metal oxide to form a lithium transition metal oxide including a small-diameter single particle composed of one primary particle and a medium-diameter quasi-single particle composed of a plurality of primary particles.

[0109] Hereinafter, a method for manufacturing a positive electrode active material for a lithium secondary battery according to another embodiment of the present invention will be described step by step.

[0110]

[0111] First, a nickel-containing transition metal precursor is prepared.

[0112] The above transition metal precursor may be a transition metal hydroxide or a transition metal oxide.

[0113] The above transition metal hydroxide may be prepared by a coprecipitation reaction by adding a complexing agent-containing solution and a pH adjusting agent-containing solution to a transition metal-containing solution including, for example, a nickel raw material and optionally, a cobalt raw material or a manganese raw material, as a precursor of a positive electrode active material.

[0114] The above transition metal oxide may be manufactured by calcining a transition metal hydroxide in an oxygen or air atmosphere at a temperature of 250 to 650°C.

[0115] At this time, the average particle diameter (D50) of the transition metal precursor may be 5 μm or more. When the average particle diameter of the transition metal precursor satisfies the above range, a single-particle lithium transition metal oxide having a medium particle diameter as targeted by the present invention can be easily obtained.

[0116] Next, a mixture containing the above transition metal precursor and lithium raw material is formed and then fired to form a lithium transition metal oxide with a grown number of primary particles.

[0117] More specifically, a single particle of lithium transition metal oxide composed of a plurality of primary particles can be formed through the above-described primary particle formation.

[0118] Afterwards, the grown lithium transition metal oxide is post-calcined.

[0119] The method for manufacturing an active material according to one embodiment of the present invention divides the sintering into two stages as described above.

[0120] At this time, the main firing temperature may be higher than the post-firing temperature, and the main firing time may be shorter than the post-firing time.

[0121] High-temperature, short-term primary sintering can grow the number of primary particles within a single particle to an appropriate range. Low-temperature, long-term post-sintering can induce crystal rearrangement, thereby relieving the increased internal stress during high-temperature primary sintering and reducing nickel cation mixing. Furthermore, the series of high-temperature, short-term, and low-temperature, long-term sintering can facilitate the formation of active materials comprising small-diameter single particles and medium-diameter quasi-particles.

[0122] More specifically, as a conventional method for manufacturing single particles, a single-stage firing method using high-temperature, long-term firing had problems in that nickel cation mixing occurred and rock salt impurity phases were generated. On the other hand, a manufacturing method according to one embodiment of the present invention can prevent the above problems through high-temperature, short-term main firing and low-temperature, long-term post-firing, and can induce the final active material to include a medium-sized single particle composed of a small-sized single particle and a plurality of primary particles by appropriately growing the number of primary particles within the single particle.

[0123] At this time, the main firing temperature may be 850 to 900°C, and the main firing time may be 5 to 9 hours. In addition, the post-firing temperature may be 760 to 820°C, and the post-firing time may be 9 to 12 hours. When the main firing temperature and time, and the post-firing temperature and time satisfy the above ranges, the active material composition and properties targeted by the present invention can be more easily achieved.

[0124] The lithium raw material may be lithium-containing sulfate, nitrate, acetate, carbonate, oxalate, citrate, halide, hydroxide, or oxyhydroxide, and is not particularly limited as long as it can be dissolved in water. Specifically, the lithium raw material may be, but is not limited to, Li2CO3, LiNO3, LiNO2, LiOH, LiOHㆍH2O, LiH, LiF, LiCl, LiBr, LiI, CH3COOLi, Li2O, Li2SO4, CH3COOLi, Li3C6H5O7, or a combination thereof.

[0125] The above firing can be performed under an oxygen or air atmosphere. When firing under the above atmosphere, the local oxygen partial pressure increases, which can improve the crystallinity of the positive electrode active material.

[0126] Meanwhile, other doping elements can be doped during the lithium transition metal oxide formation stage. In this case, other doping raw materials can be added during the formation of the mixture and then calcined to dope other doping elements into the lithium transition metal oxide.

[0127]

[0128] Meanwhile, the transition metal precursor prepared in the step of preparing the transition metal precursor or the lithium transition metal oxide formed in the step of forming the lithium transition metal oxide in which the number of primary particles has grown by the main firing may further include a grain growth promoting element such as Zr, Al, B or a combination thereof. That is, the grain growth promoting element may be doped in the step of forming the transition metal precursor or may be doped in the step of forming the lithium transition metal oxide as the active material.

[0129] At this time, the content of the grain growth promoting element may be 0.1 to 1 mol% based on the total mole number of transition metals in the transition metal precursor or the lithium transition metal oxide. More specifically, the content of Zr may be 0.1 to 0.3 mol% based on the total mole number of transition metals in the transition metal precursor or the lithium transition metal oxide. In addition, the content of Al may be 0.3 to 0.8 mol% based on the total mole number of transition metals in the transition metal precursor or the lithium transition metal oxide. In addition, the content of B may be 0.1 to 1 mol% based on the total mole number of transition metals.

[0130] The technical significance of introducing the pressure growth promoting element and controlling its content as described above is omitted as it is the same as described above.

[0131]

[0132] Next, the post-calcined lithium transition metal oxide is pulverized to form a lithium transition metal oxide comprising a small-diameter single particle composed of a single primary particle and a medium-diameter quasi-single particle composed of multiple primary particles. Thus, a cathode active material according to the present invention can be obtained.

[0133] At this time, the crushing pressure during the crushing may be 2 to 4 bar.

[0134] Additionally, the stirring speed of the classifier during the above grinding can be performed at 1,500 to 3,000 rpm.

[0135] When the crushing pressure and the classifier stirring speed during crushing satisfy the above ranges, the small-diameter single particles and medium-diameter quasi-single particles having the particle size distribution and particle number targeted by the present invention mentioned above can be more easily formed.

[0136]

[0137] According to another embodiment of the present invention, a positive electrode active material for a lithium secondary battery can form bimodal single particles and quasi-single particles by obtaining a precursor in this way and through a simple process of calcination and pulverization. More specifically, a conventional method for producing a bimodal positive electrode active material involves producing a small-particle-size active material through a first calcination process for a small-particle-size precursor, and separately from the first calcination process, producing a large-particle-size active material through a second calcination process for a large-particle-size precursor, thereby requiring multiple calcination processes and a subsequent mixing process for mixing the small-particle-size active material and the large-particle-size active material. On the other hand, the positive electrode active material according to the present invention can be produced through a single calcination and pulverization process without a separate calcination process to produce small-particle-size and medium-particle-size active materials, thereby providing an advantage in process economy.

[0138]

[0139] Optionally, as needed, after the step of forming a lithium transition metal oxide including a single particle composed of the above-described one primary particle and a spherical single particle composed of a plurality of primary particles, a step of forming a coating layer including Co, Al or a combination thereof may be further included.

[0140] More specifically, a coating layer can be formed by mixing the lithium transition metal oxide of the single particle with a Co raw material, an Al raw material, or a combination thereof, and then heat-treating the mixture. The technical significance of forming the coating layer is as described above, and thus is omitted.

[0141]

[0142] Another embodiment of the present invention provides a positive electrode for a lithium secondary battery comprising the positive electrode active material described above.

[0143] Another embodiment of the present invention provides a lithium secondary battery comprising the positive electrode. More specifically, the lithium secondary battery may include a positive electrode; a negative electrode; a separator; and an electrolyte.

[0144] In addition, the lithium secondary battery may optionally further include a battery container that houses the electrode assembly of the positive electrode, the negative electrode, and the separator, and a sealing member that seals the battery container.

[0145]

[0146] Specifically, the positive electrode may include a positive electrode current collector and a positive electrode active material layer disposed on the positive electrode current collector, and including the positive electrode active material described above.

[0147] The positive electrode current collector is not particularly limited as long as it is conductive and does not cause a chemical change in the battery, and for example, stainless steel, aluminum, nickel, titanium, calcined carbon, or aluminum or stainless steel surface-treated with carbon, nickel, titanium, silver, etc. may be used. In addition, the positive electrode current collector may typically have a thickness of 3 to 500 μm, and fine unevenness may be formed on the surface of the positive electrode current collector to increase the adhesion of the positive electrode active material. For example, the positive electrode current collector may be used in various forms such as a film, sheet, foil, net, porous body, foam, or non-woven fabric.

[0148] The above-described positive electrode active material layer may include a binder and / or a conductive material together with the above-described positive electrode active material.

[0149] At this time, the binder plays a role of improving the adhesion between the positive electrode active material particles and the adhesive strength between the positive electrode active material and the positive electrode current collector. Specific examples include polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer rubber (EPDM rubber), sulfonated-EPDM, styrene butadiene rubber (SBR), fluororubber, or various copolymers thereof, and one kind alone or a mixture of two or more kinds thereof may be used, but is not limited thereto. The binder may be included in an amount of 1 to 30 wt% based on the total weight of the positive electrode active material layer.

[0150] And, the conductive material is used to provide conductivity to the electrode, and in the battery to be constructed, as long as it does not cause a chemical change and has electronic conductivity, it can be used without any special restrictions. Specific examples include graphite such as natural graphite or artificial graphite; carbon-based materials such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, summer black, and carbon fiber; metal powder or metal fiber such as copper, nickel, aluminum, and silver; conductive whiskers such as zinc oxide or potassium titanate; conductive metal oxides such as titanium oxide; or conductive polymers such as polyphenylene derivatives, and the like. One type alone or a mixture of two or more types among these may be used, but the present invention is not limited thereto. The conductive material may typically be included in an amount of 1 to 30 wt% based on the total weight of the positive electrode active material layer.

[0151] The above positive electrode can be manufactured according to a conventional positive electrode manufacturing method, except that the above positive electrode active material is used.

[0152] Specifically, the positive electrode can be manufactured by applying a composition for forming a positive electrode active material layer, including the positive electrode active material described above and optionally a binder, a conductive agent, or a solvent, on a positive electrode current collector, followed by drying and rolling. At this time, the types and contents of the positive electrode active material, binder, and conductive agent are as described above.

[0153] The solvent may be a solvent generally used in the relevant technical field, such as dimethylsulfoxide (DMSO), isopropyl alcohol, N-methylpyrrolidone (NMP), acetone, or water. One of these may be used alone or a mixture of two or more thereof may be used. The amount of the solvent used is sufficient to dissolve or disperse the positive electrode active material, conductive material, and binder, taking into account the coating thickness and manufacturing yield of the slurry, and to have a viscosity that can exhibit excellent thickness uniformity when applied thereafter for manufacturing the positive electrode.

[0154] Alternatively, the positive electrode may be manufactured by casting the composition for forming the positive electrode active material layer on a separate support, and then laminating the resulting film on a positive electrode current collector by peeling it off from the support.

[0155]

[0156] The above negative electrode may include a negative electrode current collector and a negative electrode active material layer positioned on the negative electrode current collector.

[0157] The negative electrode current collector is not particularly limited as long as it has high conductivity without causing chemical changes in the battery, and for example, copper, stainless steel, aluminum, nickel, titanium, calcined carbon, copper or stainless steel surface-treated with carbon, nickel, titanium, silver, etc., aluminum-cadmium alloy, etc. can be used. In addition, the negative electrode current collector can typically have a thickness of 3 to 500 ㎛, and like the positive electrode current collector, fine unevenness can be formed on the surface of the current collector to strengthen the bonding strength of the negative electrode active material. For example, it can be used in various forms such as a film, a sheet, a foil, a net, a porous body, a foam, a non-woven fabric, etc.

[0158] The negative electrode active material layer may optionally include a binder and a conductive material together with the negative electrode active material. As an example, the negative electrode active material layer may be manufactured by applying a composition for forming a negative electrode active material layer comprising the negative electrode active material and optionally a binder and a conductive material onto a negative electrode current collector and drying the composition, or by casting the negative electrode forming composition onto a separate support and then laminating the resulting film onto a negative electrode current collector by peeling the film off from the support.

[0159] As the negative electrode active material, a compound capable of reversible intercalation and deintercalation of lithium may be used. Specific examples thereof include carbonaceous materials such as artificial graphite, natural graphite, graphitized carbon fiber, and amorphous carbon; metallic compounds capable of alloying with lithium, such as Si, Al, Sn, Pb, Zn, Bi, In, Mg, Ga, Cd, Si alloy, Sn alloy, and Al alloy; metallic oxides capable of doping and dedoping lithium, such as SiOβ (0 < β < 2), SnO2, vanadium oxide, and lithium vanadium oxide; or composites comprising the metallic compounds and carbonaceous materials, such as Si-C composites or Sn-C composites, and any one or a mixture of two or more of these may be used. In addition, a metallic lithium thin film may be used as the negative electrode active material. In addition, both low-crystalline carbon and high-crystalline carbon may be used as the carbonaceous material. Representative examples of low-crystalline carbon include soft carbon and hard carbon, and representative examples of high-crystalline carbon include natural graphite or artificial graphite in the form of amorphous, plate-like, flaky, spherical, or fiber-like forms, Kish graphite, pyrolytic carbon, mesophase pitch-based carbon fiber, meso-carbon microbeads, mesophase pitches, and high-temperature calcined carbon such as petroleum or coal tar pitch derived cokes.

[0160] The above binder and conductive material may be the same as those described above for the positive electrode.

[0161]

[0162] The above separator separates the negative electrode and the positive electrode and provides a passage for lithium ions to move. Any separator commonly used as a separator in lithium secondary batteries can be used without any particular restrictions. In particular, a separator having low resistance to ion movement of the electrolyte and excellent electrolyte moisture absorption capacity is preferable. Specifically, a porous polymer film, for example, a porous polymer film made of a polyolefin polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, and an ethylene / methacrylate copolymer, or a laminated structure of two or more layers thereof, may be used. In addition, a conventional porous nonwoven fabric, for example, a nonwoven fabric made of high-melting-point glass fiber, polyethylene terephthalate fiber, etc. may be used. In addition, a coated separator containing a ceramic component or a polymer material to secure heat resistance or mechanical strength may be used, and may optionally be used in a single-layer or multi-layer structure.

[0163]

[0164] The above electrolyte may include, but is not limited to, organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel-type polymer electrolytes, solid inorganic electrolytes, and molten inorganic electrolytes that can be used in the manufacture of lithium secondary batteries.

[0165] Specifically, the organic liquid electrolyte may include an organic solvent and a lithium salt.

[0166] The organic solvent may be used without any particular limitation as long as it can serve as a medium through which ions involved in the electrochemical reaction of the battery can move. Specifically, the organic solvent may include ester solvents such as methyl acetate, ethyl acetate, γ-butyrolactone, and ε-caprolactone; ether solvents such as dibutyl ether or tetrahydrofuran; ketone solvents such as cyclohexanone; aromatic hydrocarbon solvents such as benzene and fluorobenzene; Carbonate solvents such as dimethylcarbonate (DMC), diethylcarbonate (DEC), methylethylcarbonate (MEC), ethylmethylcarbonate (EMC), ethylene carbonate (EC), and propylene carbonate (PC); alcohol solvents such as ethyl alcohol and isopropyl alcohol; nitriles such as R-CN (wherein R is a C2 to C20 linear, branched, or cyclic hydrocarbon group, and may include a double-bonded aromatic ring or an ether bond); amides such as dimethylformamide; dioxolanes such as 1,3-dioxolane; or sulfolanes can be used. Among these, a carbonate solvent is preferable, and a mixture of a cyclic carbonate (e.g., ethylene carbonate or propylene carbonate, etc.) having high ionic conductivity and high dielectric constant that can improve the charge / discharge performance of the battery and a linear carbonate compound having low viscosity (e.g., ethyl methyl carbonate, dimethyl carbonate, or diethyl carbonate, etc.) is more preferable.In this case, the performance of the electrolyte may be improved when the cyclic carbonate and the chain carbonate are mixed and used in a volume ratio of about 1:1 to about 1:9.

[0167] The lithium salt may be used without any particular limitation as long as it is a compound capable of providing lithium ions used in a lithium secondary battery. Specifically, the lithium salt may be LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAl04, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2)2. LiCl, LiI, or LiB(C2O4)2. It is preferable that the concentration of the lithium salt be used within the range of 0.1 to 2.0 M. When the concentration of the lithium salt is within the above range, the electrolyte can exhibit excellent electrolyte performance because it has appropriate conductivity and viscosity, and lithium ions can move effectively.

[0168] In addition to the electrolyte components, the electrolyte may further include one or more additives, such as haloalkylene carbonate compounds such as difluoroethylene carbonate, pyridine, triethylphosphite, triethanolamine, cyclic ethers, ethylene diamine, n-glyme, hexamethylphosphoric acid triamide, nitrobenzene derivatives, sulfur, quinone imine dyes, N-substituted oxazolidinones, N,N-substituted imidazolidines, ethylene glycol dialkyl ethers, ammonium salts, pyrrole, 2-methoxyethanol, or aluminum trichloride, for the purpose of improving the life characteristics of the battery, suppressing battery capacity decrease, and improving the discharge capacity of the battery. At this time, the additives may be included in an amount of 0.1 to 5 wt% based on the total weight of the electrolyte.

[0169]

[0170] Another embodiment of the present invention provides a battery module including the lithium secondary battery as a unit cell and a battery pack including the same.

[0171] The above battery module or battery pack can be used as a power source for one or more medium- to large-sized devices, such as power tools; electric vehicles including electric vehicles (EVs), hybrid electric vehicles, and plug-in hybrid electric vehicles (PHEVs); or power storage systems.

[0172]

[0173] Hereinafter, embodiments of the present invention will be described in more detail through examples. However, the following examples are merely preferred embodiments of the present invention, and the present invention is not limited to the following examples.

[0174]

[0175] Example 1

[0176] (1) Manufacturing of positive electrode active material

[0177] (Preparation of transition metal hydroxide) According to the general coprecipitation method, (Ni) with an average particle size (D50) of 7 μm 0.96 Co 0.03 Mn 0.01 )(OH)2 composition hydroxide was prepared.

[0178] (Sintering) After mixing 200 g of the above transition metal hydroxide, 90.556 g of LiOH·H2O as a lithium raw material, 0.403 g of ZrO2 and 30.850 g of Al(OH) as a grain growth accelerator, main firing was performed at a temperature of 860°C for 3.8 hours, and post-sintering was performed at a temperature of 790°C for 9.8 hours.

[0179] (After crushing), the above-mentioned calcined material was crushed at a crushing pressure of 2 to 4 bar and a stirring speed of the classifier of 1,500 to 3,000 rpm to form a lithium transition metal oxide of single particles. At this time, the molar numbers of lithium (Li), zirconium (Zr), and aluminum (Al) per 1 mol of transition metal in the lithium transition metal oxide correspond to 1.00, 0.0015, and 0.005 mol, respectively.

[0180] (Coating) After that, 130 g of the above lithium transition metal oxide was mixed with 0.560 g of LiOH·H2O, 22.504 g of Co(OH), and 30.189 g of Al(OH) to prepare a mixture, and then heat-treated at 650 to 700°C for 15 hours to prepare a positive electrode active material having a coating layer containing 2 mol% of Co and 0.2 mol% of Al formed on the surface.

[0181] (2) Lithium secondary battery manufacturing

[0182] The slurry for manufacturing the electrode plate was mixed with the above-mentioned positive electrode active material: conductive material (carbon black, Denka black): binder (PVDF, KF1100) = 96.5:1.5:2 wt%, and the viscosity was adjusted so that the solid content was approximately 30% by adding NMP (N-Methyl-2-pyrrolidone). The manufactured slurry was coated on a 15 μm thick Al foil using a doctor blade, and then dried and rolled. The electrode loading was 15.0 mg / cm 2 and the rolling density (25 ℃, 20 kN) was 3.6 g / cm 3 It was.

[0183] The electrolyte was 1M LiPF6in EC:DMC:EMC=3:4:3 (vol%), with 3.0 vol% VC added to the total amount of the electrolyte, and a coin cell was manufactured using a PP separator and a lithium negative electrode (200 μm, Honzo metal).

[0184]

[0185] Comparative Example 1

[0186] A positive electrode active material and a lithium secondary battery were manufactured in the same manner as in Example 1, except that the crushing step was not performed.

[0187]

[0188] Comparative Example 2

[0189] (1) Manufacturing of positive electrode active material

[0190] (Preparation of transition metal hydroxide) According to the general coprecipitation method, (Ni) with an average particle size (D50) of 3.5 μm 0.96 Co 0.03 Mn 0.01 )(OH)2 composition hydroxide was prepared.

[0191] (Sintering) After mixing 200 g of the above transition metal hydroxide, 90.556 g of LiOH·H2O as a lithium raw material, 0.403 g of ZrO2 as a grain growth accelerator, and 30.850 g of Al(OH), the main firing was performed at a temperature of 830°C for 3.8 hours, and then post-sintering was performed at a temperature of 750°C for 9.8 hours.

[0192] (After crushing), the above-mentioned calcined material was crushed at a crushing pressure of 1 to 4 bar and a stirring speed of 3,000 to 5,000 rpm of a classifier to form a lithium transition metal oxide of single particles. At this time, the molar numbers of lithium (Li), zirconium (Zr), and aluminum (Al) per 1 mol of transition metal in the lithium transition metal oxide correspond to 1.00, 0.0015, and 0.005 mol, respectively.

[0193] (Coating) After that, 130 g of the above lithium transition metal oxide was mixed with 0.560 g of LiOH·H2O, 22.504 g of Co(OH), and 30.189 g of Al(OH) to prepare a mixture, and then heat-treated at 650 to 700°C for 15 hours to prepare a positive electrode active material having a coating layer containing 2 mol% of Co and 0.2 mol% of Al formed on the surface.

[0194] Afterwards, a lithium secondary battery was manufactured in the same manner as in Example 1.

[0195]

[0196] Experimental Example 1: Observation of SEM images of active materials

[0197] SEM (scanning electron microscope) images of the positive electrode active materials manufactured according to the examples and comparative examples were observed, and these are shown in Figs. 1 to 3 in the order of Example 1 and Comparative Examples 1 to 2, respectively.

[0198] Referring to FIGS. 1 to 3, it was confirmed that Example 1 included both single particles composed of only one primary particle and quasi-single particles composed of only multiple primary particles. In addition, it was confirmed that single particles had a smaller particle size than quasi-single particles. In addition, it was confirmed that the intermediate particles had an approximately spherical shape, and the single particles had an angular polyhedral shape.

[0199]

[0200] On the other hand, in the case of Comparative Example 2, which did not undergo a crushing process, it was confirmed that it consisted only of medium particles.

[0201] Additionally, in the case of Comparative Example 3, it was confirmed that the particle size was small and consisted of only single particles.

[0202]

[0203] Experimental Example 2: Evaluation of Active Material Properties

[0204] Various properties of the positive electrode active materials manufactured according to the examples and comparative examples were evaluated, and the results are summarized in Table 1 below.

[0205] (1) Evaluation of particle size distribution curve based on number of particles

[0206] For the active material powder, the particle size distribution curve based on number of particles was evaluated using the laser diffraction method, and the particle sizes corresponding to the maximum peaks of small and medium particle sizes were measured. The results are shown in Fig. 4 and Table 1, respectively.

[0207] (2) Evaluation of average particle size by volume (Dv50)

[0208] For the active material powder, the particle size corresponding to 50% of the cumulative volume was measured using the laser diffraction method.

[0209] (3) Evaluation of particle size (Dn10, Dn50, Dn90) based on number of particles

[0210] For the active material powder, the particle sizes corresponding to 10%, 50%, and 90% of the accumulated number were measured using the laser diffraction method.

[0211] (4) Evaluation of Equation 1

[0212] Through the above results, the value of Equation 1, which is defined as the average particle diameter by volume (Dv50) - the average particle diameter by number (Dn50), was calculated.

[0213] (5) Evaluation of compression density (9 tons)

[0214] Density was evaluated after applying 9 tons of pressure. Specifically, 3 g of active material sample was loaded onto a pellet with a diameter of 13 mm, and then 9 tons of pressure was applied using a hydraulic press from Caver. The change in height of the pellet before and after applying the pressure was measured, and the specific calculation formula is as follows.

[0215] [Calculation Formula 1]

[0216] Density after applying 9 tons of pressure = Weight of active material sample (3g) / (Φ*(1.3cm / 2) 2 *(Height change before and after pressure application)

[0217] In the above calculation formula 1, Φ represents pi.

[0218] Particle size distribution curve Peak particle size (μm) Dv50 (μm) Dn10 (μm) Dn50 (μm) Dn90 (μm) Formula 1 (μm) Compressed density (9 ton, g / cc) Example 10.872, 3.125.670.8221.355.24.323.68 Comparative example 13.555.772.824.16.411.673.55 Comparative example 21.883.081.352.023.291.063.50

[0219] Referring to Table 1, Example 1, which is bimodal and satisfies other conditions, has a large compression density, which is expected to improve electrode energy density. However, Comparative Examples 1 and 2, which are composed of only single particles or only medium particles, were confirmed to have small compression densities. In addition, Example 1 was confirmed to have an appropriate peak particle size on the particle size distribution curve, and other properties were properly obtained.

[0220]

[0221] Experimental Example 3: Evaluation of Battery Electrochemical Characteristics

[0222] The electrochemical characteristics of lithium secondary batteries manufactured according to the examples and comparative examples were evaluated, and the results are shown in Table 2 below. The specific experimental methods are as follows.

[0223] (1) Initial charge and discharge capacity, initial efficiency evaluation

[0224] After fabricating half-cells of lithium secondary batteries, they were aged at 25°C for 12 hours and then subjected to charge-discharge tests. To evaluate the initial capacity, 200 mAh / g was used as the reference capacity, and the cells were charged to 4.25 V at a constant current of 0.1 C. After switching to constant voltage, the cells were charged until the end current reached 0.05 C. After a 10-minute rest period, the cells were discharged to 2.5 V at a constant current of 0.1 C, using 200 mAh / g as the reference capacity.

[0225] (2) Evaluation of high temperature lifespan (45℃, 50 cycles)

[0226] The high-temperature life retention rate was measured at 45℃, by charging to 4.25 V with a constant current of 0.5 C, then switching to a constant voltage and charging until the end current reached 0.05 C. After a 10-minute rest time after charging, the battery was discharged at a constant current of 1.0 C until the voltage reached 2.5 V. 50 charge / discharge cycles were performed under these charge / discharge conditions, and the capacity retention rate of the 50th cycle was calculated compared to the first cycle.

[0227] (3) Evaluation of high temperature resistance increase rate (45℃, 50 cycles)

[0228] The high temperature resistance increase rate was measured by charging the battery to 4.25 V at a constant current of 0.5 C at 45 °C, then switching to a constant voltage and charging until the end current reached 0.05 C. After a 10-minute rest time after charging, the battery was discharged at a constant current of 1.0 C until the voltage reached 2.5 V. 50 charge / discharge cycles were performed under these charge / discharge conditions, and the resistance increase rate of the 50th cycle compared to the first cycle was calculated.

[0229] Classification Charge capacity (mAh / g, 0.1C) Discharge capacity (mAh / g, 0.1C) Initial efficiency (%) High temperature life maintenance rate (%, 50 cycles) High temperature resistance increase rate (%, 50 cycles) Example 1244.0212.587.193.870.1 Comparative example 1242.0209.386.593.471.5 Comparative example 2243.4216.789.091.576.1

[0230] Referring to Table 2, it was confirmed that Example 1, which included small-diameter single particles and medium-diameter quasi-single particles, and had other properties such as maximum peak range, average particle diameter based on a single particle (Dn50), and Equation 1 values ​​appropriately controlled, had excellent capacity, initial efficiency, and high-temperature life characteristics.

[0231] On the other hand, in the case of Comparative Example 1, where the properties such as the average particle size (Dn50) based on the standard and the value of Equation 1 were outside the appropriate range, it was confirmed that the capacity and charge / discharge efficiency were low.

[0232] In addition, it was confirmed that the life characteristics were poor in the case of Comparative Example 2, which had a small average particle diameter by volume (Dv50) and consisted of only single particles, and had properties such as an average particle diameter by diameter (Dn50) and an equation 1 value that were outside the appropriate range.

[0233]

[0234] Although the preferred embodiments of the present invention have been described above, the present invention is not limited thereto, and various modifications can be made within the scope of the patent claims, the detailed description of the invention, and the attached drawings, and it is obvious that this also falls within the scope of the present invention.

[0235] Accordingly, the actual scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A layered lithium transition metal oxide containing nickel in the single particle series, The average particle diameter by volume (Dv50) is 5 to 8 μm, It includes a small-diameter single particle composed of one primary particle and a medium-diameter quasi-single particle composed of multiple primary particles, A cathode active material for a lithium secondary battery having peaks in the particle size range of 0.7 to 1.2 μm and the particle size range of 2.5 to 4.0 μm when analyzing a particle size distribution curve based on number of particles.

2. In paragraph 1, A cathode active material for a lithium secondary battery having an average particle diameter (Dn50) of 1.6 μm or less.

3. In paragraph 1, A cathode active material for a lithium secondary battery satisfying the following equation 1: [Formula 1] Average particle size by volume (Dv50) - Average particle size by number (Dn50) ≥ 3.5 μm 4. In paragraph 1, A cathode active material for a lithium secondary battery having a compression density of 3.6 g / cc or more after applying a pressure of 9 tons.

5. In paragraph 1, A positive electrode active material for a lithium secondary battery, wherein the number ratio of the single particle and the quasi-single particle (single particle:quasi-single particle) is 8:2 to 5:

5.

6. In paragraph 1, The above lithium transition metal oxide is a positive electrode active material for a lithium secondary battery containing nickel in an amount of 60 mol% or more based on the total mole number of transition metals.

7. In paragraph 1, The above lithium transition metal oxide is a cathode active material for a lithium secondary battery, further comprising a grain growth promoting element such as Zr, Al, B or a combination thereof.

8. In paragraph 7, A positive electrode active material for a lithium secondary battery, wherein the content of the above-mentioned growth promoting element is 0.1 to 1 mol% based on the total mole number of transition metals.

9. In paragraph 1, The positive electrode active material for a lithium secondary battery further comprises a coating layer containing Co, Al or a combination thereof on the lithium transition metal oxide.

10. In paragraph 1, The above lithium transition metal oxide is a positive electrode active material for a lithium secondary battery represented by the following chemical formula 1: [Chemical Formula 1] Li a [Ni x Co y Mr z M1 w1 M2 w2 ]O2 In the above chemical formula 1, 0.8≤a≤1.2, 0.60≤x<1, 0≤y≤0.4, 0≤z≤0.4, 0≤w1≤0.01, 0≤w2≤0.2, x+y+z+w1+w2=1, M1 is Zr, Al, B or a combination thereof, and M2 is Y, Mg, Ti, Nb, W, Sc, Si, V, Fe, Y, Mo, Ce, Hf, Ta, La, Sr or a combination thereof.

11. A positive electrode for a lithium secondary battery comprising the positive electrode active material of any one of claims 1 to 10.

12. A lithium secondary battery comprising the positive electrode for a lithium secondary battery of Article 11.

Citation Information

Patent Citations

  • Image signal encoding / decoding method and apparatus using efficient motion vector predictor

    KR1020200085667A

  • Environment learning automation method for optinizing ai image analysis and apparatus therefor

    KR1020230166356A

  • Manufacturing method for hybrid photocatalyst disinfectant and hybrid photocatalytic disinfectant prepared thereby

    KR102176682B1

  • Segment prestressed concrete girder and junction method of the same and bridge fast construction method using the same

    KR102378877B1

  • Method and apparatus for microarray spot analysis

    KR102610794B1

Cited By

  • Polycrystalline cathode active material and lithium secondary battery containing the same

    EP4738470A1