Carbon black dispersion, method for preparing same, electrode slurry composition comprising same, electrode comprising same, and secondary battery comprising same
The carbon black dispersion, utilizing amide and hydroxyl/carboxyl group-containing dispersants with sulfur, addresses the challenge of uniform dispersion and aggregation, enhancing battery performance by improving conductive networks and reducing internal resistance.
Patent Information
- Application Number
- PCT/KR2024/003456
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-30
- Filing Date
- 2024-03-20
- Publication Date
- 2024-10-03
AI Technical Summary
Carbon black's strong cohesive forces make it difficult to disperse uniformly in electrode slurry, leading to inadequate conductive networks, increased internal resistance, and reduced battery performance, especially when repeated charging and discharging cause interfacial adhesion deterioration.
A carbon black dispersion is created using a first dispersant with an amide group and a second dispersant with hydroxyl or carboxyl groups, both forming hydrogen bonds to reduce viscosity, with the inclusion of sulfur to prevent excessive bonding and maintain low viscosity, enhancing dispersibility and coating properties.
The carbon black dispersion achieves improved dispersibility and conductivity, minimizing aggregation and maintaining low viscosity, which improves electrode processability and battery performance.
Smart Images

Figure KR2024003456_03102024_PF_FP_ABST
Abstract
Description
Carbon black dispersion, method for producing the same, electrode slurry composition containing the same, electrode containing the same, and secondary battery containing the same
[0001] This application claims the benefit of patent application number 10-2023-0042155 filed with the Korean Intellectual Property Office on March 30, 2023, the contents of which are incorporated herein by reference.
[0002] The present specification relates to a carbon black dispersion, a method for producing the same, an electrode slurry composition comprising the same, an electrode comprising the same, and a secondary battery comprising the same.
[0003] Secondary batteries are batteries that can be used repeatedly through a discharge process in which chemical energy is converted into electrical energy and a charge process in the reverse direction. Secondary batteries are composed of a positive electrode, a negative electrode, an electrolyte, and a separator. The positive and negative electrodes are generally composed of an electrode current collector and an electrode active material layer formed on the electrode current collector. The electrode active material layer is manufactured by applying an electrode slurry composition containing an electrode active material, a conductive material, a binder, etc., onto the electrode current collector, drying it, and then rolling it.
[0004] Carbon black is used as a material for coloring, shading, or conductive purposes in various technical fields, and to meet the requirements of various applications, it has become important to finely disperse carbon black in a solvent.
[0005] Meanwhile, there has been a growing demand for small, lightweight, and high-capacity batteries for electronic devices. Furthermore, there is a continued demand for improved performance of large-capacity secondary batteries for automotive applications. To meet this demand, the development of secondary batteries is actively underway. Typically, secondary battery electrodes are formed by applying a slurry containing electrode active materials, binder resin, and conductive agents to the surface of a current collector. Carbon black may be added as a conductive agent.
[0006] Carbon black has a large specific surface area, so it has strong cohesion and is difficult to uniformly disperse within the slurry for forming an electrode. If the carbon black dispersibility is insufficient, a uniform conductive network cannot be formed, which not only fails to sufficiently reduce the internal resistance of the electrode, but also causes partial cohesion to cause a resistance distribution within the electrode, which may cause the current to concentrate during battery use, resulting in partial heat generation or deterioration. In addition, when charging and discharging are repeated, the interfacial adhesion between the current collector and the electrode layer, or between the active material and the carbon black, may deteriorate, which may deteriorate battery performance. If the carbon black dispersibility is insufficient, the deterioration of the interfacial adhesion as described above may become even more severe.
[0007] Various additives, such as surfactants and pigment dispersion resins, have been attempted to disperse carbon black. However, while surfactants are advantageous for dispersion in aqueous systems, they are not suitable for dispersion in organic solvents. Even when pigment dispersion resins are used, carbon black readily re-agglomerates or stability deteriorates over time. Furthermore, when manufacturing battery electrodes, if the amount of surfactant or pigment dispersion resin added is reduced, sufficient dispersibility cannot be achieved. On the other hand, if the amount of surfactant or pigment dispersion resin added is increased to achieve sufficient dispersibility, the content of electrode active material may decrease, which may result in a decrease in battery capacity.
[0008] A method of introducing acidic functional groups onto the particle surface by oxidizing carbon black in a gaseous or liquid phase has been attempted, but gaseous oxidation such as plasma or ozone treatment has problems such as low treatment efficiency or expensive treatment equipment, and liquid treatment has problems such as work safety because strong acids such as acetic acid or hydrogen peroxide are used.
[0009] Polyvinylpyrrolidone (PVP), a dispersant having an amide group, is a polymer surfactant used as a dispersant, emulsifier, thickener, etc. in various dispersion systems, and is known to be effective as a dispersant (Patent Document 1).
[0010] Polyacrylic acid and tannic acid, which are polyacids containing carboxyl groups, are also known to be effective as dispersants.
[0011] In summary of the above-mentioned information, it can be assumed that a better dispersion effect can be obtained by mixing polyvinylpyrrolidone and polyacid. However, in reality, when these substances are mixed, an excessively strong bond is generated between the two substances, forming insoluble substances or aggregates, which causes the dispersibility of the dispersion to decrease.
[0012]
[0013] [Prior Art Literature]
[0014] [Patent Document]
[0015] KR No. 10-2011-0118460
[0016] [Non-patent literature]
[0017] Toxicol. Res., 2015,4, 160-168
[0018]
[0019] The present invention relates to a carbon black dispersion having improved dispersibility of carbon black, a method for producing the same, an electrode slurry composition comprising the same, an electrode comprising the same, and a secondary battery comprising the same.
[0020] One embodiment of the present invention comprises carbon black;
[0021] A first dispersant having an amide group;
[0022] A second dispersant having at least one functional group selected from the group consisting of a hydroxyl group and a carboxyl group; and
[0023] A carbon black dispersion containing a sulfur element is provided.
[0024] In addition, another embodiment of the present invention provides a method for producing the above-described carbon black dispersion, comprising the step of mixing carbon black, a first dispersant having an amide group, and a second dispersant having at least one functional group selected from the group consisting of a hydroxyl group and a carboxyl group.
[0025] In addition, another embodiment of the present invention provides an electrode slurry composition comprising the above-described carbon black dispersion, a silicon-based electrode active material, and a binder.
[0026] In addition, another embodiment of the present invention provides an electrode including an electrode active material layer formed by the electrode slurry composition described above.
[0027] In addition, another embodiment of the present invention provides a secondary battery including the above-described electrode.
[0028] A carbon black dispersion according to one embodiment of the present invention has a significantly low viscosity and has the effect of improving the dispersibility of carbon black within the dispersion.
[0029] A carbon black dispersion according to one embodiment of the present invention has excellent coating properties and processability when used in electrode manufacturing.
[0030] Figures 1 to 3 show the results of confirming whether the first dispersant used in the examples and comparative examples contains sulfur.
[0031] Hereinafter, the present invention will be described in detail.
[0032] A carbon black dispersion according to one embodiment of the present invention refers to a dispersion containing carbon black. Specifically, it refers to a dispersion in which carbon black is dispersed and does not aggregate with each other.
[0033] One embodiment of the present invention provides a carbon black dispersion comprising carbon black; a first dispersant having an amide group; a second dispersant having at least one functional group selected from the group consisting of a hydroxyl group and a carboxyl group; and sulfur element.
[0034] It has been known that a first dispersant having an amide group is effective in dispersing carbon black (Patent Document 1), and a second dispersant having at least one functional group selected from the group consisting of a hydroxyl group and a carboxyl group is known to lower the viscosity of the dispersion liquid due to the effect of the functional group (Non-patent Document 1).
[0035] In addition, the oxygen of the amide group contained in the first dispersant and the functional group (hydroxyl group or carboxyl group) of the second dispersant form hydrogen bonds with each other, which contributes to reducing the viscosity of the dispersion. However, there is a problem that the above hydrogen bond is too strong, so insoluble substances or aggregates (complexes) are formed. In this case, there are many restrictions on the selection of dispersants, such as having to adjust the contents of the first and second dispersants, or having to use only specific types of the first and / or second dispersants.
[0036] The inventors of the present invention discovered that the agglomeration phenomenon of the first and second dispersants described above is improved when the dispersion contains elemental sulfur, and thus completed the present invention. In this case, the viscosity of the dispersion is maintained low even when containing carbon black with a large specific surface area. The improvement in agglomeration can be confirmed by preparing a carbon black dispersion containing the above substances, allowing it to stand for a certain period of time, and then visually observing for agglomeration.
[0037] A carbon black dispersion according to one embodiment of the present invention comprises carbon black with excellent conductivity, while also having improved dispersibility of the carbon black, thereby minimizing the phenomenon of carbon black agglomeration. This characteristic can be confirmed by the significantly low viscosity of the dispersion.
[0038] A carbon black dispersion according to one embodiment of the present invention is characterized by containing elemental sulfur. The elemental sulfur may be present in the dispersion in the form of a compound, an element, or an ion. For example, the elemental sulfur may be derived from a compound containing sulfur, and these compounds will be described below. The presence and content of the elemental sulfur can be confirmed by elemental analysis.
[0039] In one embodiment of the present invention, the content of elemental sulfur may be 0.01 wt% or more and 10 wt% or less based on solid content. Preferably, it may be 0.05 wt% or more and 8 wt% or less, or 0.1 wt% or more and 5 wt% or less. The content of elemental sulfur may be achieved by a method for controlling the content of a compound containing sulfur. The content of elemental sulfur may be measured and calculated using an elemental analyzer (EA), and a specific method will be described later.
[0040] In one embodiment of the present invention, the content of sulfur element may be 0.01% or more and 20% or less based on the total content of oxygen (O) and nitrogen (N) elements on a solid basis. Preferably, it may be 0.1% or more and 10% or less, or 1% or more and 5% or less. When the above numerical range is satisfied, by controlling the ratio of the content of oxygen and nitrogen elements involved in hydrogen bonding and the content of sulfur element, the dispersant can be prevented from agglomerating with each other, and the dispersibility of carbon black can be improved. The content of the above elements can be measured and calculated using an elemental analyzer (EA), and a specific method will be described later.
[0041] In one embodiment of the present invention, part or all of the first dispersant may be substituted with sulfur. If part of the first dispersant is substituted with sulfur, the remainder of the first dispersant may not be substituted with sulfur. For example, a sulfur-substituted first dispersant and a non-sulfur-substituted first dispersant may be used together.
[0042] In one embodiment of the present invention, the proportion of the sulfur-substituted first dispersant among the first dispersants may be 10 mol% to 100 mol%. Preferably, it may be 20 mol% to 80 mol% or 40 mol% to 60 mol%.
[0043] In one embodiment of the present invention, the first dispersant has a wavelength of 1,110 cm on a Fourier-transform infrared (FTIR) spectrum. -1 1,050 cm inland -1 First peak, 1,140 cm -1 1180 cm inland -1 The second peak at 1,180 cm; and -1 1220 cm inland -1 It may include one or more peaks selected from the group consisting of the first to third peaks. The first to third peaks indicate the presence of an S=0 bond in the dispersant, and when the peaks appear, it can be confirmed that the first dispersant is substituted with sulfur.
[0044] In one embodiment of the present invention, the first dispersant has an amide group, and thus can form a hydrogen bond with a hydroxyl group or carboxyl group of the second dispersant described below.
[0045] In one embodiment of the present invention, the first dispersant may include at least one selected from the group consisting of polyvinylpyrrolidone, polyester amide, polycarboxylic amide, polyamido amine, thioamido amine, and water-soluble nylon. Since the first dispersant has an amide group, it can exhibit a further enhanced viscosity improvement effect and an effect of suppressing changes in viscosity over time.
[0046] In one embodiment of the present invention, the weight average molecular weight of the first dispersant may be 1,000 to 100,000 g / mol. Preferably, it may be 2,000 to 80,000 g / mol, 2,000 to 30,000 g / mol, or 2,000 to 15,000 g / mol. When the weight average molecular weight of the first dispersant is less than 1,000 g / mol, the carbon black dispersing performance may be reduced, and a problem of the first dispersant being eluted during electrode manufacture may occur. When it exceeds 100,000 g / mol, the viscosity of the carbon black dispersion may increase, which may deteriorate the coatability and processability. Therefore, it is preferable to adjust it within the above range.
[0047] In one embodiment of the present invention, the second dispersant has a hydroxyl group or a carboxyl group, and thus can form a hydrogen bond with the amide group of the first dispersant described above.
[0048] In one embodiment of the present invention, the second dispersant may include an aromatic ring. In this case, the complex structure of the second dispersant can effectively reduce the viscosity of the dispersion.
[0049] In one embodiment of the present invention, the second dispersant may include two or more aromatic rings. For example, the second dispersant may be at least one selected from the group consisting of baicalin, luteolin, taxifolin, myricetin, quercetin, rutin, catechin, epigallocatechin gallate, butein, piceatenol, and tannic acid, and preferably tannic acid, quercetin, epigallocatechin gallate, or a combination thereof.
[0050] In one embodiment of the present invention, the second dispersant may be a phenol-based compound. The phenol-based compound may include at least one structure selected from the group consisting of a phenol structure, a catechol structure, a galol structure, and a naphthol structure, at least one of the aromatic rings. The phenol structure is a structure in which one hydroxyl group is bonded to a benzene ring, the catechol structure is a structure in which two hydroxyl groups are bonded to a benzene ring, the galol structure is a structure in which three hydroxyl groups are bonded to a benzene ring, and the naphthol structure is a structure in which one hydroxyl group is bonded to naphthalene.
[0051] In one embodiment of the present invention, the second dispersant may be a polyacrylic acid compound. The polyacrylic acid compound refers to an acrylic acid compound containing two or more acidic hydrogen atoms.
[0052] In one embodiment of the present invention, the polyacrylic acid compound may be polyacrylic acid (PAA) or a polyacrylic acid derivative. The polyacrylic acid derivative may be a polyacrylic acid-maleic acid copolymer (PAAMA).
[0053] In one embodiment of the present invention, the second dispersant may include at least one selected from the group consisting of compounds containing an aromatic ring and polyacrylic acid compounds. The compounds containing an aromatic ring and the polyacrylic acid compounds are as described above.
[0054] In one embodiment of the present invention, the weight ratio of the first dispersant and the second dispersant may be 1:10 to 10:1. Preferably, it may be 1:5 to 5:1, or 1:3 to 3:1. When the above range is satisfied, the dispersing effect of carbon black is improved, and the viscosity of the dispersion can be maintained low.
[0055] In one embodiment of the present invention, the content of the first dispersant may be 0.01 wt% to 10 wt% based on the total weight of the dispersion. Preferably, it may be 0.01 wt% to 5 wt%, or 0.1 wt% to 3 wt%.
[0056] In one embodiment of the present invention, the content of the second dispersant may be 0.01 wt% to 10 wt% based on the total weight of the dispersion. Preferably, it may be 0.01 wt% to 5 wt%, or 0.1 wt% to 3 wt%.
[0057] In one embodiment of the present invention, various carbon blacks, such as commercially available furnace black, channel black, thermal black, acetylene black, and Ketjen black, can be used. In addition, hollow carbon black can also be used.
[0058] In one embodiment of the present invention, the carbon black may include two or more carbon black units.
[0059] In one embodiment of the present invention, the diameter of the carbon black unit may be 1 nm or more and 200 nm or less, 1 nm or more and 150 nm or less, or 1 nm or more and 100 nm or less.
[0060] In the above numerical range, the dispersibility of carbon black can be improved and resistance can be prevented from increasing when applied to an electrode.
[0061] In one embodiment of the present invention, the length of the carbon black unit may be 0.1 μm or more and 200 μm or less. Preferably, it may be 0.1 μm or more and 150 μm or less or 0.5 μm or more and 100 μm or less. Within the above numerical range, the dispersibility of the carbon black can be improved and resistance can be prevented from increasing when applied to an electrode.
[0062] In one embodiment of the present invention, the aspect ratio (length / diameter) of the carbon black may be 5 to 50,000, or 10 to 15,000. Within the above numerical range, the dispersibility of the carbon black can be improved, and resistance can be prevented from increasing when applied to an electrode.
[0063] In one embodiment of the present invention, the average particle diameter (D50) of the carbon black may be 0.1 ㎛ to 20 ㎛. Preferably, it may be 0.1 ㎛ to 15 ㎛, 0.1 ㎛ to 10 ㎛, or 0.1 ㎛ to 5 ㎛. The average particle diameter (D50) refers to a particle diameter corresponding to 50% of the accumulated number amount in the particle diameter distribution curve of the carbon black. The average particle diameter (D50) can be measured using, for example, a laser diffraction method. In the above range, the carbon black does not aggregate with each other, and dispersibility can be improved.
[0064] In one embodiment of the present invention, the content of the carbon black may be 0.01 wt% to 20 wt% based on the total weight of the carbon black dispersion. Preferably, it may be 1 wt% to 8 wt%. In the above numerical range, it is possible to prevent a decrease in the loading amount during electrode manufacturing, thereby increasing the process cost, and to prevent problems such as binder migration occurring during electrode drying, which reduces the adhesive strength, or increases the viscosity of the carbon black dispersion.
[0065] In one embodiment of the present invention, the BET specific surface area of the carbon black is 30 m 2 / g to 1,300 m 2 / g may be. Preferably, 30 m 2 / g to 900 m 2 / g, 30 to 500 m 2 / g, or 30 to 300 m 2 / g. In the above numerical range, the electrical conductivity of carbon black is excellent and the agglomeration phenomenon can be controlled.
[0066] In one embodiment of the present invention, the carbon black dispersion is heated at 25°C and 2.5 sec. -1 The viscosity at a shear rate of may be 800 cPs or less. The viscosity may be 500 cPs or less, 400 cPs or less, 140 cPs or less, or 100 cPs or less. Considering the purpose of the present invention, the lower the viscosity, the better, so the lower limit is not particularly limited, but may be 1 cPs or more, 3 cPs or more, or 5 cPs or more. When the viscosity range is satisfied, the carbon black of the carbon black dispersion does not aggregate with each other, and the processability is improved when used in electrode manufacturing.
[0067] In one embodiment of the present invention, the carbon black dispersion is heated at 25°C and 15 sec. -1 The viscosity at a shear rate of may be 300 cPs or less. The viscosity may be 190 cPs or less, 180 cPs or less, 60 cPs or less, 50 cPs or less, or 30 cPs or less. Considering the purpose of the present invention, the lower the viscosity, the better, so the lower limit is not particularly limited, but may be 1 cPs or more, 3 cPs or more, or 5 cPs or more. When the viscosity range is satisfied, the carbon black of the carbon black dispersion does not aggregate with each other, and the processability is improved when used in electrode manufacturing.
[0068] The viscosity of the carbon black dispersion can be measured using a method commonly used in the field of this technology. For example, it can be measured using a Brookfield DVNextCP Rheometer at a measurement temperature of 25°C and the shear rate described above. For more accurate measurement, the prepared carbon black dispersion can be stored at 25°C for one week before being measured.
[0069] In one embodiment of the present invention, the value expressed by the following formula 2 of the carbon black dispersion may be 1 to 10. Preferably, it may be 1 to 6, or 1 to 4. The value expressed by the following formula 2 is a shear fluidization index of the dispersion, which means the ratio of viscosities measured at different shear rates. When the above range is satisfied, uniform mixing is possible during electrode manufacturing by preventing the viscosity from becoming too high in a stationary state and reducing fluidity. In addition, sedimentation of carbon black particles can be prevented, thereby improving storage stability.
[0070] [Formula 2]
[0071] Shear Thinning Index (STI) = V low / V high
[0072] In the above equation 2,
[0073] V low is 25℃ and 15 sec -1 is the viscosity of the dispersion measured at the shear rate,
[0074] V high is 25℃ and 150 sec -1 is the viscosity of the dispersion measured at a shear rate of .
[0075] In one embodiment of the present invention, the value calculated from the following Equation 3 of the carbon black dispersion may be 1 to 10. Preferably, it may be 1 to 8 or 2 to 6. The value calculated from the following Equation 3 represents the relationship between the shear thinning index (STI) characteristics of the above-described dispersion and the average particle diameter of the carbon black contained in the dispersion. In general, if the carbon black particle diameter (D50) is too small, the carbon black tends to aggregate with each other, thereby increasing the shear thinning index (STI) of the dispersion. In addition, if the carbon black particle diameter (D50) is too large, the carbon black is not sufficiently dispersed, so the carbon black forms a network structure, and the overall viscosity and shear thinning index (STI) of the dispersion tend to increase.
[0076] However, the carbon black dispersion according to one embodiment of the present invention has the effect of improving the viscosity stability of the entire dispersion over time even if the particle size of the carbon black is small by adjusting the value calculated by Equation 3 below to the above numerical range.
[0077] [Formula 3]
[0078]
[0079] In the above equation 3,
[0080] STI is the shear thinning index of the dispersion,
[0081] D50 is the average particle diameter (D50) of the above carbon black.
[0082] In one embodiment of the present invention, the carbon black dispersion may contain an alkali metal element. The form of the alkali metal is not particularly limited, but may exist in the form of an alkali metal salt containing the alkali metal.
[0083] The carbon black dispersion of the present invention can improve the dispersibility of the substances contained in the dispersion by including the alkali metal element. Specifically, the first dispersant and the second dispersant contained in the dispersion can form a complex with each other. However, such a complex has low solubility in a solvent such as water, which increases the viscosity of the dispersion. However, the alkali metal contained in the carbon black dispersion of the present invention can resolve the above problem by disintegrating the complex.
[0084] In one embodiment of the present invention, the content of the alkali metal element may be 1 ppm or more and 300 ppm or less based on the entire carbon black dispersion. Preferably, it may be 5 ppm or more and 200 ppm or less, or 5 ppm or more and 150 ppm or less.
[0085] In one embodiment of the present invention, the carbon black dispersion may include one or more alkali metal salts selected from the group consisting of KOH, NaOH, LiOH, K2CO3, Na2CO3, and LiCO3.
[0086] In one embodiment of the present invention, when the first dispersant is a polyvinylpyrrolidone resin, the molar ratio of the alkali metal salt may be 60 mol or less based on 100 mol of vinylpyrrolidone units. Preferably, it may be 30 mol or less, or 25 mol or less. The lower limit of the content is not particularly limited, but may be 0.1 mol or more, 1 mol or more, or 2 mol or more. When the above range is satisfied, the viscosity of the carbon black dispersion can be lowered.
[0087] The molar ratio of the above alkali metal salt can be calculated using the molecular weight of the alkali metal salt and the vinylidone unit and the weight % of the alkali metal salt and polyvinylidene. Specifically, it can be calculated using the following equation 1.
[0088] [Formula 1]
[0089] Molar ratio of alkali metal salt = {(weight % of alkali metal salt) / (molecular weight of alkali metal salt)} / {(weight % of polyvinylidene) / (molecular weight of vinylidone unit)}*100
[0090] For example, if the contents of polyvinylpyrrolidone and alkali metal salt (LiOH) are 0.6 wt% and 0.01 wt%, respectively, based on the total weight of the dispersion, the molecular weight of the alkali metal salt (LiOH) is 24 g / mol, and the molecular weight of the vinylidone unit is 111.14 g / mol, the molar ratio of the alkali metal salt is calculated as 7.7 mol based on 100 mol of the vinylpyrrolidone unit [7.7 = {(0.01) / (24)} / {(0.6) / (111.14)}*100]
[0091] The above vinylpyrrolidone unit refers to a unit composed of a 5-membered lactam linked to a vinyl group, and refers to a unit constituting the polyvinylpyrrolidone-based resin. Specifically, among the polyvinylpyrrolidone units represented by the following chemical formula 1, it may be a unit represented by the following chemical formula 2.
[0092] [Chemical Formula 1]
[0093]
[0094] [Chemical Formula 2]
[0095]
[0096] In one embodiment of the present invention, the carbon black dispersion may further include a solvent. The solvent is used to supply the carbon black dispersion by pre-dispersing it in order to prevent agglomeration when the carbon black is directly mixed with an electrode active material or the like to be used as an electrode slurry composition.
[0097] In one embodiment of the present invention, the solvent may be an aqueous solvent. For example, the aqueous solvent may be water. In this case, the viscosity of the dispersion can be easily controlled.
[0098] One embodiment of the present invention provides a method for producing a carbon black dispersion, comprising the step of mixing carbon black, a first dispersant having an amide group, and a second dispersant having at least one functional group selected from the group consisting of a hydroxyl group and a carboxyl group.
[0099] In one embodiment of the present invention, the step of mixing the carbon black, the first dispersant having an amide group, and the second dispersant having at least one functional group selected from the group consisting of a hydroxyl group and a carboxyl group may be performed under temperature conditions that do not change the physical properties. For example, it may be performed at a temperature of 50°C or lower, more specifically, from 5°C to 50°C.
[0100] In one embodiment of the present invention, the step of dispersing the carbon black in a dispersion liquid may be further included.
[0101] In one embodiment of the present invention, the step of dispersing the carbon black in the dispersion liquid can be performed by a method such as a ball mill, a bead mill, a disc mill, a basket mill, a high pressure homogenizer, etc., and more specifically, it can be performed by a milling method using a disc mill or a high pressure homogenizer.
[0102] When milling using the above disk mill, the size of the beads can be appropriately determined depending on the type and amount of carbon black and the type of dispersant, and specifically, the diameter of the beads can be 0.1 mm to 5 mm, more specifically, 0.5 mm to 4 mm. In addition, the bead milling process can be performed at a speed of 2,000 rpm to 10,000 rpm, and more specifically, can be performed at a speed of 5,000 rpm to 9,000 rpm.
[0103] In one embodiment of the present invention, the step of dispersing the carbon black in the dispersion liquid may be performed for 10 to 120 minutes, more specifically, for 20 to 90 minutes, so that the carbon black can be sufficiently dispersed.
[0104] One embodiment of the present invention provides an electrode slurry composition comprising the above-described carbon black dispersion, electrode active material, and binder.
[0105] In one embodiment of the present invention, the electrode active material includes a silicon-based electrode active material. The silicon-based electrode active material includes metal silicon (Si), silicon oxide (SiOx, where 0 <x<2) 실리콘 탄화물(SiC) 및 Si-Y 합금(상기 Y는 알칼리 금속, 알칼리 토금속, 13족 원소, 14족 원소, 전이금속, 희토류 원소 및 이들의 조합으로 이루어진 군에서 선택되는 원소이며, Si은 아님)로 이루어진 군으로부터 선택된 1종 이상을 포함할 수 있다. 상기 원소 Y로는 Mg, Ca, Sr, Ba, Ra, Sc, Y, Ti, Zr, Hf, Rf, V, Nb, Ta, Db, Cr, Mo, W, Sg, Tc, Re, Bh, Fe, Pb, Ru, Os, Hs, Rh, Ir, Pd, Pt, Cu, Ag, Au, Zn, Cd, B, Al, Ga, Sn, In, Ti, Ge, P, As, Sb, Bi, S, Se, Te, Po, 및 이들의 조합으로 이루어진 군에서 선택될 수 있다.
[0106] In one embodiment of the present invention, since the silicon-based electrode active material exhibits higher capacity characteristics than the carbon-based electrode active material, when the silicon-based electrode active material is additionally included, even better capacity characteristics can be obtained. However, since the silicon-based electrode active material has a large volume change during charge and discharge, the battery characteristics deteriorate rapidly when charge and discharge are repeated, resulting in insufficient cycle characteristics, which has made commercialization difficult. However, when carbon black is used as a conductive material as in the present invention, the effect of improving cycle characteristics can be obtained when the silicon-based electrode active material is applied. Therefore, when the electrode slurry composition of the present invention, which includes the carbon black dispersion of the present invention and the silicon-based electrode active material, is used, a secondary battery having excellent capacity characteristics and cycle characteristics can be realized.
[0107] In one embodiment of the present invention, the electrode active material may further include another type of electrode active material together with the silicon-based electrode active material. Examples of the other types of electrode active materials include carbonaceous materials such as artificial graphite, natural graphite, graphitized carbon fiber, and amorphous carbon; metallic compounds capable of alloying with lithium such as Al, Sn, Pb, Zn, Bi, In, Mg, Ga, Cd, Si alloy, Sn alloy, or Al alloy; metallic oxides capable of doping and dedoping lithium such as SnO2, vanadium oxide, and lithium vanadium oxide; or composites containing the metallic compounds and carbonaceous materials such as Sn-C composites, and among these, carbonaceous materials are particularly preferred.
[0108] In one embodiment of the present invention, the total amount of the electrode active material, which is the combination of the silicon-based electrode active material and another type of electrode active material, may be 70 to 99 wt%, preferably 80 to 98 wt%, based on the total solid content in the electrode slurry composition. When the content of the electrode active material satisfies the above range, excellent capacity characteristics can be realized.
[0109] In one embodiment of the present invention, the binder is used to secure adhesion between active materials or between the active materials and the current collector, and general binders used in the relevant technical field can be used, and the type thereof is not particularly limited. Examples of the binder include polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated-EPDM, styrene-butadiene rubber (SBR), fluororubber, or various copolymers thereof, and one type alone or a mixture of two or more types thereof may be used.
[0110] In one embodiment of the present invention, the binder may be included in an amount of 5 wt% or less, and preferably 1 to 3 wt%, based on the total solid content in the electrode slurry composition. When the binder content satisfies the above range, excellent electrode adhesion can be achieved while minimizing an increase in electrode resistance.
[0111] In one embodiment of the present invention, the electrode slurry composition may further include a solvent, if necessary, for viscosity control, etc. In this case, the solvent may be water, an organic solvent, or a mixture thereof. Examples of the organic solvent include amide-based polar organic solvents such as dimethylformamide (DMF), diethyl formamide, dimethyl acetamide (DMAc), N-methyl pyrrolidone (NMP); alcohols such as methanol, ethanol, 1-propanol, 2-propanol (isopropyl alcohol), 1-butanol (n-butanol), 2-methyl-1-propanol (isobutanol), 2-butanol (sec-butanol), 1-methyl-2-propanol (tert-butanol), pentanol, hexanol, heptanol, or octanol; Glycols such as ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, 1,3-propanediol, 1,3-butanediol, 1,5-pentanediol, or hexylene glycol; polyhydric alcohols such as glycerin, trimethylolpropane, pentaerythritol, or sorbitol; glycol ethers such as ethylene glycol monomethyl ether, diethylene glycol monomethyl ether, triethylene glycol monomethyl ether, tetraethylene glycol monomethyl ether, ethylene glycol monoethyl ether, diethylene glycol monoethyl ether, triethylene glycol monoethyl ether, tetraethylene glycol monoethyl ether, ethylene glycol monobutyl ether, diethylene glycol monobutyl ether, triethylene glycol monobutyl ether, or tetraethylene glycol monobutyl ether; Examples thereof include ketones such as acetone, methyl ethyl ketone, methyl propyl ketone, or cyclopentanone; esters such as ethyl acetate, γ-butyl lactone, and ε-propiolactone; and any one or a mixture of two or more of these may be used, but is not limited thereto.
[0112] In one embodiment of the present invention, the electrode slurry composition may additionally include additives such as a viscosity modifier, a filler, etc., as needed.
[0113] One embodiment of the present invention provides an electrode comprising an electrode active material layer formed by the electrode slurry composition described above. Specifically, the electrode can be manufactured by applying the electrode slurry composition of the present invention described above and drying it to form an electrode active material layer. More specifically, the electrode active material layer can be formed by applying the electrode slurry composition on an electrode current collector and then drying it, or by applying the electrode slurry composition on a separate support and then peeling it from the support, and laminating the obtained film on an electrode current collector. If necessary, a rolling process can be additionally performed after forming the electrode active material layer through the above method. At this time, drying and rolling can be performed under appropriate conditions considering the physical properties of the electrode to be manufactured, and there are no particular limitations.
[0114] In one embodiment of the present invention, the electrode current collector is not particularly limited as long as it is a material that is conductive and does not cause a chemical change in the battery, and for example, copper, stainless steel, aluminum, nickel, titanium, alloys thereof, those surface-treated with carbon, nickel, titanium, silver, etc., or calcined carbon, etc. can be used.
[0115] In one embodiment of the present invention, the electrode current collector may typically have a thickness of 3 μm to 500 μm, and may form fine irregularities on the surface of the current collector to enhance the bonding strength of the electrode active material. In addition, the electrode current collector may be used in various forms, such as a film, sheet, foil, net, porous body, foam, or non-woven fabric.
[0116] In one embodiment of the present invention, the electrode may be a cathode.
[0117] One embodiment of the present invention provides a secondary battery including the above-described electrode.
[0118] One embodiment of the present invention provides a secondary battery comprising a positive electrode; a negative electrode; and a separator and an electrolyte provided between the positive electrode and the negative electrode, wherein at least one of the positive electrode and the negative electrode is the electrode described above.
[0119] In one embodiment of the present invention, the secondary battery may be a lithium secondary battery.
[0120] In one embodiment of the present invention, the separator separates the negative electrode and the positive electrode and provides a passage for lithium ions, and can be used without any particular limitation as long as it is commonly used as a separator in secondary batteries. Specifically, the separator may be a porous polymer film, for example, a porous polymer film made of a polyolefin polymer such as ethylene homopolymer, propylene homopolymer, ethylene / butene copolymer, ethylene / hexene copolymer, and ethylene / methacrylate copolymer, or a laminated structure of two or more layers thereof. In addition, a conventional porous nonwoven fabric, for example, a nonwoven fabric made of high-melting-point glass fiber, polyethylene terephthalate fiber, etc. may also be used. In addition, a coated separator containing a ceramic component or a polymer material to secure heat resistance or mechanical strength may be used, and may optionally be used in a single-layer or multi-layer structure.
[0121] In one embodiment of the present invention, the electrolyte may include, but is not limited to, an organic liquid electrolyte, an inorganic liquid electrolyte, a solid polymer electrolyte, a gel-type polymer electrolyte, a solid inorganic electrolyte, a molten inorganic electrolyte, etc. that can be used in the manufacture of a secondary battery.
[0122]
[0123] Hereinafter, the present invention will be described in more detail through examples.
[0124] <Preparation of the first dispersion agent>
[0125] Ar gas is introduced into the reactor to stabilize the atmosphere. The monomer N-vinylpyrrolidone and potassium sulfite are dissolved in water to prepare a mixed solution. The mixed solution is stirred for 24 hours under an Ar atmosphere at a temperature of 40°C and allowed to react, then slowly cooled to room temperature. A certain amount of water is evaporated to make it concentrated. PVP-1 containing S is obtained through a process of precipitation, filtration, and drying using acetone. In addition, PVP-2 purchased from Aldrich and PVP-3 provided by Ashland were prepared.
[0126] The presence of sulfur in the first dispersant was verified using the attenuated total reflection (ATR) method. For PVP-1, it was 1,030 cm -1 , 1,160 cm -1 , 1,200 cm -1 A peak was confirmed at the position (Fig. 1), but no peak was confirmed at the position for PVP-2 (Fig. 2) and PVP-3 (Fig. 3). From the above results, it was confirmed that the first dispersant of PVP-1 was substituted with sulfur.
[0127]
[0128] <Preparation of the second dispersion agent>
[0129] Tannic acid (TA) obtained from Aldrich and polyacrylic acid (PAA, weight average molecular weight 2,000) obtained from Thermo Scientific were prepared.
[0130]
[0131] <Preparation of dispersion>
[0132] Example 1
[0133] A carbon black dispersion was prepared by mixing 15 wt% of CB1 as carbon black, 1.13 wt% of PVP-1 as a first dispersant, 0.38 wt% of TA as a second dispersant, and distilled water as a solvent, and treating the mixture with a high-pressure homogenizer.
[0134] Examples and Comparative Examples
[0135] For the remaining examples and comparative examples, dispersions were prepared by changing the weight and type of each material as shown in Tables 1 and 2 below, and the physical properties were tested.
[0136] The composition of the dispersions prepared in the above examples and comparative examples and the results of each experimental example are shown in Table 1 below. The content of each component is based on the total weight of the dispersion.
[0137]
[0138] Experimental Example 1: Confirmation of dispersant coagulation
[0139] A test solution was prepared in the same manner as in the examples and comparative examples described above, except that carbon black was not added. The test solution was mixed at room temperature using a vortex mixer and left for 6 hours to observe coagulation and sedimentation.
[0140] The test solution of the example did not exhibit coagulation or precipitation, but the test solution of the comparative example exhibited a phenomenon in which the dispersants coagulated with each other and even precipitated.
[0141]
[0142] Experimental Example 2: Viscosity Measurement
[0143] Brookfield's DVNextCP Rheometer was used, and the shear rate was 2.5 sec at 25℃. -1 and 15 sec -1 Each was measured by changing it to .
[0144]
[0145] Experimental Example 3: Measurement of average particle size
[0146] The laser diffraction method was used, and a commercially available laser diffraction particle size measuring device (Malvern Mastersizer3000) was used. The average particle diameter (D50) at 50% of the particle size distribution was calculated from the measuring device. Meanwhile, D10 and D90 refer to particle sizes at 10% and 90% of the particle size distribution, respectively.
[0147]
[0148] Experimental Example 4: Measurement of elemental sulfur content
[0149] -Sample production
[0150] The dispersions prepared in the examples and comparative examples were dried in a convection oven at 90°C for 3 days and then ground using a mixer grinder to prepare powder samples.
[0151] -Measurement of sulfur element content
[0152] It was measured using an elemental analyzer (EA).
[0153] Organic samples are oxidized to CO2, H2O, NO2, and SO2 using a catalyst at high temperatures (approximately 1,000°C), and the resulting gases are separated using a GC column (packed column). Detection is performed using a TCD (Thermal conductive detector), and calibration curves for each C, H, N, and S are drawn using standard substances in advance, and the content of each element is quantified in % from the GC chromatogram.
[0154] Classification Example 1 Example 2 Example 3 Example 4 Example 5 Example 6 Example 7 Carbon black product CB1CB1CB1CB1CB2CB3CB1 Specific surface area (m / 2)626262628001,27062Content151515155415Type 1 dispersantPVP-1PVP-1PVP-1PVP-1 + PVP-2PVP-1PVP-1PVP-2Content1.131.131.130.56+0.560.750.61.13Type 2 dispersantTAPAATA+PAATATAPAATAContent0.380.380.19+0.190.380.250.20.38Type of additive(content)Sodium sulfite (0.056)Experimental example 2 Viscosity (cP@2.5 / s) 25.4 27.23 4.12 6.8 35.13 6 36 Viscosity (cP@15 / s) 9.8 18.2 18 19 13.3 11.9 15 Experimental Example 3 Particle Size (D50, ㎛) 0.45 0.46 0.55 0.47 0.55 0.51 0.53 Experimental Example 4O(%)2.252.282.272.174.144.181.97N(%)0.810.810.810.801.491.490.80C(%)96.2396.1596.1996.3593.0892.9396 .41H(%)0.620.680.650.621.131.240.61S(%)0.090.090.090.040.160.160.09S / (O+N)*100(%)2.92.92.91.32.82.83.2
[0155]
[0156] Classification Comparison Example 1 Comparison Example 2 Comparison Example 3 Comparison Example 4 Carbon Black Product CB1 CB1 CB2 CB3 Specific Surface Area (m / 2 )62628001,270Content151554Type of first dispersantPVP-2PVP-3PVP-2PVP-2Content1.131.130.750.6Type of second dispersantTATATAPAAContent0.380.380.250.2Type of additive(content)----Experimental example 2Viscosity(cP@2.5 / s)139146595487Viscosity(cP@15 / s)5762.7186.6199.5Experimental example 3Particle size(D50, ㎛)1.281.331.51.45Experimental example 4O(%)2.092.253.843.89N(%)0.800.791.461.46C(%)96.4896.3493.5493.38H(%)0.630.621.161.26S(%)Not detectedNot detectedNot detectedNot detectedS / (O+N)*100(%)0000
[0157]
[0158] In Tables 1 and 2, CB1 is Super P from Imerys, CB2 is ECP from LION, and CB3 is ECP600JD from LION.
[0159] From the above results, it was confirmed that when the dispersion did not contain elemental sulfur (Comparative Examples 1 to 4), the viscosity of the dispersion became too high. This was because the first dispersant and the second dispersant coagulated with each other, increasing the viscosity of the dispersion.
[0160] Example 1 includes a first dispersant and a second dispersant that can form hydrogen bonds with each other, but since the first dispersant is substituted with sulfur, hydrogen bonding between the first dispersant and the second dispersant is suppressed, and the phenomenon of the dispersants agglomerating with each other occurs less frequently.
[0161] On the other hand, Comparative Examples 1 to 4 had the same composition as Example 1 except that PVP not substituted with sulfur was used as the first dispersant, but there was a problem that the viscosity of the dispersion increased due to the occurrence of a large amount of hydrogen bonding between the first dispersant and the second dispersant.
[0162] Comparative Example 3 was the same as Example 5 except that PVP-2 was used as the first dispersant. However, a problem occurred in which the viscosity of the dispersion increased by about 20 times or more due to the occurrence of a large amount of hydrogen bonding between the first and second dispersants (@2.5 / s).
[0163] Methods for adding elemental sulfur to a dispersion include methods using sulfur-substituted PVP (Examples 1 to 6) and methods adding sulfur salts (Example 7). Both methods were able to significantly reduce the viscosity of the dispersion. However, it was confirmed that the method using sulfur-substituted PVP was able to further reduce the viscosity.
[0164] The carbon black dispersion according to the present invention, the electrode slurry composition containing the same, and the electrode containing the same are useful for manufacturing a high-performance secondary battery.
Claims
1. Carbon black; A first dispersant having an amide group; A second dispersant having at least one functional group selected from the group consisting of a hydroxyl group and a carboxyl group; and Carbon black dispersion containing sulfur element.
2. In claim 1, A carbon black dispersion having a sulfur element content of 0.01 wt% or more and 10 wt% or less based on solid content.
3. In claim 1, A carbon black dispersion having a sulfur element content of 0.01% or more and 20% or less based on the total content of oxygen (O) and nitrogen (N) elements on a solid basis.
4. In claim 1, A carbon black dispersion in which part or all of the first dispersant is substituted with sulfur.
5. In claim 4, A carbon black dispersion, wherein the proportion of the first dispersant substituted with sulfur among the first dispersants is 10 mol% to 100 mol%.
6. In claim 1, The first dispersant has a Fourier-transform infrared (FTIR) spectrum at 1,110 cm -1 1,050 cm inland -1 First peak, 1,140 cm -1 1180 cm inland -1 The second peak at 1,180 cm; and -1 1220 cm inland -1 A carbon black dispersion comprising at least one peak selected from the group consisting of the third peak.
7. In claim 1, A carbon black dispersion, wherein the first dispersant comprises at least one selected from the group consisting of polyvinylpyrrolidone, polyester amide, polycarboxylic amide, polyamido amine, thioamido amine, and water soluble nylon.
8. In claim 1, A carbon black dispersion wherein the second dispersant contains an aromatic ring.
9. In claim 1, A carbon black dispersion having a weight ratio of the first dispersant and the second dispersant of 1:10 to 10:
1.
10. In claim 1, The BET surface area of the above carbon black is 30 m 2 / g to 1,300 m 2 Carbon black dispersion having a mass of / g.
11. In claim 1, A carbon black dispersion having an average particle diameter (D50) of 0.1 ㎛ to 20 ㎛.
12. A step of mixing carbon black, a first dispersant having an amide group, and a second dispersant having at least one functional group selected from the group consisting of a hydroxyl group and a carboxyl group. A method for producing a carbon black dispersion according to any one of claims 1 to 11.
13. An electrode slurry composition comprising a carbon black dispersion according to any one of claims 1 to 11, an electrode active material, and a binder.
14. An electrode comprising an electrode active material layer formed by an electrode slurry composition according to claim 13.
15. In claim 14, The above electrode is a cathode electrode.
16. A secondary battery comprising an electrode according to claim 14.
Citation Information
Patent Citations
Conductive agent dispersion liquid, electrode slurry, electrode, battery, and preparation methods thereof
CN101752548A
Manufacturing method of highly electrically conductive carbon nanotube-metal composite
KR1020110033652A
Manufacturing method for highly concentrated and dispersed carbon NANO tube dispersion solution
KR1020130053015A
Method for preparation of high concentrated carbon nanotube / graphene dispersion
KR1020160133711A
Safe route area indication system for ship's coastal navigation
KR102522957B1