Solar cell and method for manufacturing same

The integration of a plasma damage prevention layer between the semiconductor and transparent conductive layers in solar cells, formed using ALD, addresses defects and efficiency losses, enhancing the quality and performance of solar cells by preventing damage and using CVD for electrode formation.

WO2024205123A1PCT designated stage expired Publication Date: 2024-10-03JUSUNG ENG
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2024/003541
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2024-03-19
Filing Date
2024-03-21
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Solar cells face efficiency decreases due to defects in the silicon semiconductor layer caused by the sputtering process for depositing transparent electrodes, and the use of oxygen can form oxide films that deteriorate electrical and optical properties.

Method used

Incorporating a thin film plasma damage prevention layer made of AZO, ITO, or IZO between the semiconductor layer and the transparent conductive layer, formed using atomic layer deposition (ALD) to prevent defects and improve film quality, and using chemical vapor deposition (CVD) for electrode formation instead of sputtering.

Benefits of technology

Prevents defects in the semiconductor layer during transparent electrode deposition, enhances film quality, and improves solar cell efficiency by using a plasma damage prevention layer and alternative deposition methods.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2024003541_03102024_PF_FP_ABST
    Figure KR2024003541_03102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to a solar cell and a method for manufacturing same, the solar cell comprising: a first semiconductor layer; a second semiconductor layer formed on one surface of the first semiconductor layer; a third semiconductor layer formed on the other surface of the first semiconductor layer; a first transparent conductive layer formed on the second semiconductor layer; and a second transparent conductive layer formed on the lower surface of the third semiconductor layer, wherein a first plasma damage prevention layer is provided between the second semiconductor layer and the first transparent conductive layer, and a second plasma damage prevention layer is provided between the third semiconductor layer and the second transparent conductive layer. According to the present invention, the formation of defects in a semiconductor layer can be prevented by a plasma damage prevention layer even when a step for forming a transparent conductive layer is performed.
Need to check novelty before this filing date? Find Prior Art

Description

Solar cell and manufacturing method thereof

[0001] The present invention relates to a solar cell.

[0002] A solar cell is a device that converts light energy into electrical energy by utilizing the properties of semiconductors.

[0003] A solar cell has a PN junction structure that joins a P (positive) type semiconductor and an N (negative) type semiconductor, and when sunlight is incident on a solar cell of this structure, holes and electrons are generated within the semiconductor due to the energy of the incident sunlight, and at this time, the holes (+) move toward the P-type semiconductor and the electrons (-) move toward the N-type semiconductor due to the electric field generated at the PN junction, so that a potential is generated, thereby generating electricity.

[0004] Solar cells of this type can generally be divided into substrate-type solar cells and thin-film solar cells.

[0005] The above substrate-type solar cell is a solar cell manufactured using a semiconductor material such as silicon as a substrate, and the above thin-film solar cell is a solar cell manufactured by forming a semiconductor in the form of a thin film on a substrate such as glass.

[0006] The above substrate-type solar cell has the advantage of being somewhat more efficient than the above thin-film solar cell, and the above thin-film solar cell has the advantage of having a reduced manufacturing cost compared to the above substrate-type solar cell.

[0007] When a solar cell is formed by including a silicon layer, a transparent electrode may be provided on the upper surface of the silicon layer. At this time, the transparent electrode may be deposited through a sputtering process using plasma. When the transparent electrode is deposited using the sputtering process, a portion of the semiconductor layer including silicon (Si) provided under the transparent electrode may be crystallized or damaged, resulting in a defect. At this time, there is a problem that the efficiency of the solar cell may be reduced due to the defect.

[0008] In addition, when depositing the transparent electrode using a sputtering process, if oxygen (O2) is used, there is a problem that an oxide film may be formed on the surface of the semiconductor layer, thereby deteriorating the electrical and optical characteristics of the solar cell.

[0009] The present invention has been designed to overcome the disadvantages of the aforementioned solar cell, and the purpose of the present invention is to provide a solar cell including a thin film-type plasma damage prevention layer on a silicon semiconductor layer to prevent defects from occurring in the silicon semiconductor layer, and a method for manufacturing the same.

[0010] In order to achieve the above object, the present invention provides a solar cell comprising: a first semiconductor layer; a second semiconductor layer provided on one surface of the first semiconductor layer; a first transparent conductive layer provided on the second semiconductor layer; and a first plasma damage prevention layer provided between the second semiconductor layer and the first transparent conductive layer.

[0011] The above first plasma damage prevention layer may be formed of an oxide selected from the group consisting of AZO, ITO, and IZO.

[0012] The thickness of the first plasma damage prevention layer may be thinner than that of the first transparent conductive layer.

[0013] It may further include a third semiconductor layer provided on the other surface of the first semiconductor layer; a second transparent conductive layer provided on the third semiconductor layer; and a second plasma damage prevention layer provided between the third semiconductor layer and the second transparent conductive layer.

[0014] The second plasma damage prevention layer may be formed of an oxide selected from the group consisting of AZO, ITO, and IZO.

[0015] The thickness of the second plasma damage prevention layer may be thinner than that of the second transparent conductive layer.

[0016] It may further include a first electrode provided on the first transparent conductive layer; and a second electrode provided on the second transparent conductive layer.

[0017] It may further include a fourth semiconductor layer provided between the first semiconductor layer and the second semiconductor layer; and a fifth semiconductor layer provided between the first semiconductor layer and the third semiconductor layer.

[0018] The fourth semiconductor layer may be formed of an intrinsic semiconductor layer or a semiconductor layer doped at a relatively low concentration compared to the second semiconductor layer, and the fifth semiconductor layer may be formed of an intrinsic semiconductor layer or a semiconductor layer doped at a relatively low concentration compared to the third semiconductor layer.

[0019] The present invention also provides a method for manufacturing a solar cell, comprising: forming a second semiconductor layer on one surface of a first semiconductor layer made of a semiconductor wafer; forming a first plasma damage prevention layer on the second semiconductor layer; and forming a first transparent conductive layer on the first plasma damage prevention layer, wherein the first plasma damage prevention layer is formed using atomic layer deposition (ALD) and the first transparent conductive layer is formed using sputtering or chemical vapor deposition (CVD).

[0020] The step of forming the first plasma damage prevention layer may include a step of injecting a first source material; a step of injecting a second source material; a step of injecting a first purge gas; a step of injecting a first reactant material; and a step of injecting a second purge gas.

[0021] The first source material may be an aluminum (Al) series material, the second source material may be a zinc (Zn) series material, and the first reactant material may be either oxygen (O2) or ozone (O3).

[0022] The first source material may be an indium (In) series material, the second source material may be any one of zinc (Zn) and tin (Sn) series materials, and the first reactant material may be any one of oxygen (O2) and ozone (O3).

[0023] The first source material may be a zinc (Zn) series material, the second source material may be any one of aluminum (Al) and indium (In) series materials, and the first reactant material may be any one of oxygen (O2) and ozone (O3).

[0024] The first source material may be a tin (Sn) series material, the second source material may be an indium (In) series material, and the first reactant material may be either oxygen (O2) or ozone (O3).

[0025] The above first plasma damage prevention layer may be formed of an oxide selected from the group consisting of AZO, ITO, and IZO.

[0026] The method further comprises: forming a third semiconductor layer on the other surface of the first semiconductor layer; forming a second plasma damage prevention layer on the third semiconductor layer; and forming a second transparent conductive layer on the second plasma damage prevention layer, wherein the second plasma damage prevention layer is formed using atomic layer deposition (ALD), and the second transparent conductive layer can be formed using sputtering or chemical vapor deposition (CVD).

[0027] Furthermore, the present invention provides a method for manufacturing a solar cell, comprising the steps of: bringing a substrate having a second semiconductor layer formed on one surface of a first semiconductor layer into a chamber; and forming a first plasma damage prevention layer on the second semiconductor layer, wherein the first plasma damage prevention layer is formed using an atomic layer deposition (ALD) method.

[0028] Furthermore, the present invention provides a method for manufacturing a solar cell, wherein the first plasma damage prevention layer is made of an oxide selected from the group consisting of AZO, ITO, and IZO.

[0029] Furthermore, the present invention provides a method for manufacturing a solar cell, which further includes a step of forming a first transparent conductive layer on the first plasma damage prevention layer after the step of forming the first plasma damage layer, wherein the first transparent conductive layer is formed using a chemical vapor deposition (CVD) method or a plasma-enhanced chemical vapor deposition (PECVD) method.

[0030] Furthermore, the present invention provides a method for manufacturing a solar cell, wherein the step of forming the first plasma damage prevention layer and the step of forming the first transparent conductive layer are performed in-situ within the chamber.

[0031] Furthermore, the present invention provides a method for manufacturing a solar cell, comprising the steps of: bringing a substrate having a first semiconductor layer and a second semiconductor layer formed thereon into a chamber; forming a first plasma damage prevention layer on the second semiconductor layer; and forming a first transparent conductive layer on the first plasma damage prevention layer, wherein the first plasma damage prevention layer is formed using atomic layer deposition (ALD), and the first transparent conductive layer is formed using any one of sputtering, chemical vapor deposition (CVD), and plasma-enhanced chemical vapor deposition (PECVD).

[0032] According to the present invention with the above configuration, the following effects are achieved.

[0033] According to the present invention, by forming a plasma damage prevention layer between a semiconductor layer and a transparent electrode, it is possible to prevent defects from occurring in the semiconductor layer during the process of depositing the transparent electrode through a sputtering process.

[0034] According to the present invention, by depositing the plasma damage prevention layer through atomic layer deposition (ALD), the thickness of the plasma damage prevention layer can be finely controlled, the composition ratio according to the thickness can be freely controlled, and further, a high-density thin film can be deposited compared to physical vapor deposition (PVD) or chemical vapor deposition (CVD), so that a film of superior quality can be realized.

[0035] According to the present invention, by depositing the transparent electrode through a chemical vapor deposition (CVD) method rather than a sputtering process, it is possible to prevent defects from occurring in the semiconductor layer.

[0036] According to the present invention, by depositing the transparent electrode through the chemical vapor deposition (CVD) method rather than the sputtering process, the quality of the thin film can be improved, thereby improving the efficiency of the solar cell.

[0037] FIG. 1 is a schematic cross-sectional view of a solar cell according to one embodiment of the present invention.

[0038] Figure 2 is a schematic cross-sectional view of a solar cell according to another embodiment of the present invention.

[0039] Figure 3 is a flow chart for forming a plasma damage prevention layer according to one embodiment of the present invention.

[0040] FIGS. 4A to 4G are schematic process cross-sectional views illustrating a manufacturing process of a solar cell according to one embodiment of the present invention.

[0041] FIGS. 5A to 5G are schematic process cross-sectional views illustrating a manufacturing process of a solar cell according to another embodiment of the present invention.

[0042] FIG. 6 is a schematic cross-sectional view of a substrate processing device for forming a plasma damage prevention layer according to the present invention.

[0043] FIG. 7 is a schematic cross-sectional view of the third electrode and the fourth electrode in a substrate processing device for forming a plasma damage prevention layer according to the present invention.

[0044] FIG. 8 is a schematic cross-sectional view of the third electrode and the fourth electrode in a substrate processing device for forming a plasma damage prevention layer according to the present invention.

[0045] FIG. 9 is a conceptual side view illustrating a modified embodiment of the positions of the first injection portion and the second injection portion in a substrate processing device for forming a plasma damage prevention layer according to the present invention.

[0046] The advantages and features of the present invention, and the methods for achieving them, will become clearer with reference to the embodiments described in detail below together with the accompanying drawings. However, the present invention is not limited to the embodiments disclosed below, but may be implemented in various different forms. These embodiments are provided solely to ensure that the disclosure of the present invention is complete and to fully inform those skilled in the art of the scope of the invention, and the present invention is defined solely by the scope of the claims.

[0047] The shapes, sizes, ratios, angles, numbers, etc. disclosed in the drawings for explaining embodiments of the present invention are illustrative and are not limited to the matters illustrated in the drawings. Like reference numerals refer to like components throughout the specification. In addition, in describing the present invention, if a detailed description of a related known technology is judged to unnecessarily obscure the gist of the present invention, the detailed description thereof will be omitted. When the terms “includes,” “has,” and “consists of” are used in this specification, other parts may be added unless “only” is used. When a component is expressed in the singular, it includes a case where the plural is included unless there is a specifically explicit description.

[0048] When interpreting a component, it is interpreted as including the error range even if there is no separate explicit description.

[0049] When describing a positional relationship, for example, when the positional relationship between two parts is described as 'on top of', 'upper part of', 'lower part of', 'next to', etc., one or more other parts may be located between the two parts, unless 'right away' or 'directly' is used.

[0050] When describing a temporal relationship, for example, when the temporal continuity is described as 'after', 'following', 'next to', 'before', etc., it can also include cases where it is not continuous, as long as 'right away' or 'directly' is not used.

[0051] While terms like "first" and "second" are used to describe various components, these components are not limited by these terms. These terms are merely used to distinguish one component from another. Therefore, a "first" component referred to below may also be a "second" component within the technical scope of the present invention.

[0052] The individual features of the various embodiments of the present invention can be partially or wholly combined or combined with each other, and various technical linkages and operations are possible, and each embodiment can be implemented independently of each other or implemented together in a related relationship.

[0053] Hereinafter, a preferred embodiment of the present invention will be described in detail with reference to the drawings.

[0054] FIG. 1 is a schematic cross-sectional view of a solar cell according to one embodiment of the present invention.

[0055] As can be seen in FIG. 1, a solar cell according to one embodiment of the present invention includes a first semiconductor layer (110), a second semiconductor layer (120a), a third semiconductor layer (120b), a first plasma damage prevention layer (200a), a second plasma damage prevention layer (200b), a first transparent conductive layer (300a), a second transparent conductive layer (300b), a first electrode (400a), and a second electrode (400b).

[0056] The first semiconductor layer (110) may be formed of a semiconductor wafer, for example, a silicon wafer, and specifically, may be formed of an N-type silicon wafer or a P-type silicon wafer. The first semiconductor layer (110) has the same polarity as one of the second semiconductor layer (120a) and the third semiconductor layer (120b).

[0057] Although not shown, a rough structure may be formed on at least one of the upper or lower surfaces of the first semiconductor layer (110). When the rough structure is formed on the upper and lower surfaces of the first semiconductor layer (110), the rough structure may also be formed on the surfaces of the second semiconductor layer (120a), the third semiconductor layer (120b), the first plasma damage prevention layer (200a), the second plasma damage prevention layer (200b), the first transparent conductive layer (300a), and the second transparent conductive layer (300b).

[0058] The second semiconductor layer (120a) is formed in the form of a thin film on the upper surface of the first semiconductor layer (110) made of the semiconductor wafer. The second semiconductor layer (120a) can form a PN junction together with the first semiconductor layer (110). Therefore, when the first semiconductor layer (110) is made of an N-type silicon wafer, the second semiconductor layer (120a) can be made of a P-type semiconductor layer. In particular, the second semiconductor layer (120a) can be made of P-type amorphous silicon doped with a Group III element such as boron (B).

[0059] In general, since the drift mobility of holes is lower than that of electrons, it is desirable to form a P-type semiconductor layer close to the light-receiving surface in order to maximize the efficiency of collecting holes by incident light, and therefore, it is desirable for the second semiconductor layer (120a) close to the light-receiving surface to be formed of a P-type semiconductor layer.

[0060] The first plasma damage prevention layer (200a) is formed in the form of a thin film on the upper surface of the second semiconductor layer (120a). The first plasma damage prevention layer (200a) is provided between the second semiconductor layer (120a) and the first transparent conductive layer (300a), and can prevent defects from occurring in the second semiconductor layer (120a) during the step of forming the first transparent conductive layer (300a).

[0061] Specifically, the first transparent conductive layer (300a) may be formed through a sputtering process. However, since the sputtering process is performed using plasma having high energy, defects may be formed in the second semiconductor layer (120a) provided beneath the first transparent conductive layer (300a).

[0062] For example, when the second semiconductor layer (120a) is formed by including amorphous silicon (Si), a portion of the second semiconductor layer (120a) including the amorphous silicon may be crystallized or damaged, thereby forming a defect in the second semiconductor layer (120a).

[0063] According to one embodiment of the present invention, the first plasma damage prevention layer (200a) is formed in the form of a thin film on the upper surface of the second semiconductor layer (120a), thereby protecting the second semiconductor layer (120a) during the process of forming the first transparent conductive layer (300a). Therefore, even if the step of forming the first transparent conductive layer (300a) is performed by the first plasma damage prevention layer (200a), a defect may not be formed in the second semiconductor layer (120a).

[0064] The thickness of the first plasma damage prevention layer (200a) is formed thinner than the thickness of the first transparent conductive layer (300a) formed on the upper surface of the first plasma damage prevention layer (200a).

[0065] The first plasma damage prevention layer (200a) may be formed by including at least one of IZO (Indium Zinc Oxide), AZO (Aluminum Zinc Oxide), and ITO (Indium Tin Oxide). In this case, the first plasma damage prevention layer (200a) may be formed by using an atomic layer deposition method, for example, a thermal atomic layer deposition method (Thermal ALD) or a plasma-enhanced atomic layer deposition method (Physical Enhanced ALD; PEALD) containing oxygen.

[0066] When the first plasma damage prevention layer (200a) is formed through the atomic layer deposition (ALD) method, the thickness of the first plasma damage prevention layer (200a) can be finely controlled, and accordingly, the composition ratio of the first plasma damage prevention layer (200a) according to the thickness can be easily controlled. Furthermore, when the first plasma damage prevention layer (200a) is formed using the atomic layer deposition (ALD) method, a high-density thin film can be deposited compared to when the first plasma damage prevention layer (200a) is formed using the physical vapor deposition (PVD) method or the chemical vapor deposition (CVD) method under the same conditions, and thus the first plasma damage prevention layer (200a) having a relatively superior film quality can be implemented.

[0067] The step of forming the first plasma damage prevention layer (200a) will be described in detail below with reference to FIG. 3.

[0068] The first transparent conductive layer (300a) is provided on the upper surface of the first plasma damage prevention layer (200a), and can be formed in situ with the first plasma damage prevention layer (200a) within one chamber.

[0069] The first transparent conductive layer (300a) is formed in the form of a thin film on the upper surface of the first plasma damage prevention layer (200a). The first transparent conductive layer (300a) collects carriers, for example, holes, generated in the first semiconductor layer (110) and moves the collected carriers to the first electrode (400a).

[0070] The first transparent conductive layer (300a) may be made of a transparent conductive material such as ITO (Indium Tin Oxide), ZnOH, ZnO:B, ZnO:Al, SnO2, SnO2:F, etc., and among them, ITO may be selected.

[0071] The above first transparent conductive layer (300a) may be formed by a sputtering process, a chemical vapor deposition (CVD) process, or a plasma-enhanced chemical vapor deposition (PECVD) process.

[0072] The first electrode (400a) is formed on the first transparent conductive layer (300a) to form the front surface of the solar cell. Accordingly, the first electrode (400a) is patterned in a predetermined shape so that sunlight can penetrate into the interior of the solar cell.

[0073] The first electrode (400a) may be made of any one metal selected from the group consisting of Ag, Cu, Al, Mo, and W. Meanwhile, the first electrode (400a) is not limited thereto and may be formed into one or more multilayer structures.

[0074] The third semiconductor layer (120b) is formed in the form of a thin film on the lower surface of the first semiconductor layer (110) formed of the semiconductor wafer. The third semiconductor layer (120b) is formed to have a different polarity from the second semiconductor layer (120a). When the second semiconductor layer (120a) is formed of a P-type semiconductor layer doped with a Group 3 element such as boron (B), the third semiconductor layer (120b) is formed of an N-type semiconductor layer doped with a Group 5 element such as phosphorus (P). In particular, the third semiconductor layer (120b) may be formed of N-type amorphous silicon.

[0075] The second plasma damage prevention layer (200b) is formed in the form of a thin film on the lower surface of the third semiconductor layer (120b).

[0076] The second plasma damage prevention layer (200b) is provided between the third semiconductor layer (120b) and the second transparent conductive layer (300b), and can prevent defects from occurring in the third semiconductor layer (120b) during the step of forming the second transparent conductive layer (300b).

[0077] Specifically, the second transparent conductive layer (300b) may be formed through a sputtering process. However, since the sputtering process is performed using plasma having high energy, defects may be formed in the third semiconductor layer (120b) provided on the second transparent conductive layer (300b).

[0078] For example, when the third semiconductor layer (120b) is formed of amorphous silicon (Si), a portion of the third semiconductor layer (120b) containing the amorphous silicon may be crystallized or damaged during the sputtering process, thereby forming a defect in the third semiconductor layer (120b).

[0079] According to one embodiment of the present invention, the second plasma damage prevention layer (200b) is formed in the form of a thin film on the lower surface of the third semiconductor layer (120b), thereby protecting the third semiconductor layer (120b) during the process of forming the second transparent conductive layer (300b). Therefore, even if the step of forming the second transparent conductive layer (300b) is performed by the second plasma damage prevention layer (200b), a defect may not be formed in the third semiconductor layer (120b).

[0080] The thickness of the second plasma damage prevention layer (200b) is formed thinner than the thickness of the second transparent conductive layer (300b) formed on the lower surface of the second plasma damage prevention layer (200b).

[0081] The second plasma damage prevention layer (200b) may be formed by including at least one of IZO (Indium Zinc Oxide), AZO (Aluminum Zinc Oxide), and ITO (Indium Tin Oxide). In this case, the second plasma damage prevention layer (200b) may be formed by using an atomic layer deposition (ALD) method, for example, a thermal atomic layer deposition (Thermal ALD) method or an oxygen-containing plasma enhanced atomic layer deposition (Plasma Enhanced ALD (PEALD) method.

[0082] When the second plasma damage prevention layer (200b) is formed through the atomic layer deposition (ALD) method, the thickness of the second plasma damage prevention layer (200b) can be finely controlled, and accordingly, the composition ratio of the second plasma damage prevention layer (200b) according to the thickness can be easily controlled. Furthermore, when the second plasma damage prevention layer (200b) is formed using the atomic layer deposition (ALD) method, a high-density thin film can be deposited compared to when the second plasma damage prevention layer (200b) is formed using the physical vapor deposition (PVD) method or the chemical vapor deposition (CVD) method under the same conditions, and thus the second plasma damage prevention layer (200b) having relatively superior film quality can be implemented.

[0083] The step of forming the second plasma damage prevention layer (200b) will be described in detail below with reference to FIG. 3.

[0084] The second transparent conductive layer (300b) is formed in the form of a thin film on the lower surface of the second plasma damage prevention layer (200b), and can be formed in situ with the second plasma damage prevention layer (200b) within one chamber.

[0085] The second transparent conductive layer (300b) serves to collect carriers, for example, electrons, generated in the first semiconductor layer (110) and move the collected carriers to the second electrode (400b).

[0086] The second transparent conductive layer (300b) may be made of a transparent conductive material such as ITO (Indium Tin Oxide), ZnOH, ZnO:B, ZnO:Al, SnO2, SnO2:F, etc., and among them, ITO may be selected.

[0087] The above second transparent conductive layer (300b) may be formed by a sputtering process, a chemical vapor deposition (CVD) process, or a plasma-enhanced chemical vapor deposition (PECVD) process.

[0088] The second electrode (400b) is formed on the lower surface of the second transparent conductive layer (300b). Since the second electrode (400b) is formed on the very back surface of the solar cell, it may be formed on the entire lower surface of the second transparent conductive layer (300b). However, as illustrated, it may be patterned so that reflected sunlight can be incident through the back surface of the solar cell.

[0089] The second electrode (400b) is pattern-formed on the lower surface of the second transparent conductive layer (300b). The second electrode (400b) may be formed of any one metal selected from the group consisting of Ag, Cu, Al, Mo, and W. Meanwhile, the second electrode (400b) is not limited thereto and may be formed in a multilayer structure of one or more layers.

[0090] FIG. 2 is a schematic cross-sectional view of a solar cell according to another embodiment of the present invention, which is identical to the solar cell illustrated in FIG. 1 described above, except that a fourth semiconductor layer (130a) is additionally formed between the first semiconductor layer (110) and the second semiconductor layer (120a), and a fifth semiconductor layer (130b) is additionally formed between the first semiconductor layer (110) and the third semiconductor layer (130b). Therefore, identical components are given the same reference numerals, and a repeated description of the identical components will be omitted.

[0091] When a second semiconductor layer (120a) or a third semiconductor layer (120b) is formed on the surface of the first semiconductor layer (110) using a high concentration of dopant gas, a defect may occur on the surface of the first semiconductor layer (110) due to the high concentration of dopant gas.

[0092] Accordingly, in another embodiment of the present invention illustrated in FIG. 2, a fourth semiconductor layer (130a) is formed on the upper surface of the first semiconductor layer (110), and then the second semiconductor layer (120a) is formed on the fourth semiconductor layer (130a), thereby preventing the occurrence of defects on the upper surface of the first semiconductor layer (110). In addition, a fifth semiconductor layer (130b) is formed on the lower surface of the first semiconductor layer (110), and then the third semiconductor layer (120b) is formed on the fifth semiconductor layer (130b), thereby preventing the occurrence of defects on the lower surface of the first semiconductor layer (110).

[0093] Meanwhile, although FIG. 2 illustrates a state in which both the fourth semiconductor layer (130a) and the fifth semiconductor layer (130b) are formed, only one semiconductor layer among the fourth semiconductor layer (130a) and the fifth semiconductor layer (130b) may be formed.

[0094] According to an embodiment of the present invention, the fourth semiconductor layer (130a) and the fifth semiconductor layer (130b) may each be formed of an intrinsic semiconductor layer, or the fourth semiconductor layer (130a) and the fifth semiconductor layer (130b) may each be a semiconductor layer doped at a lower concentration than the second semiconductor layer (120a) and the third semiconductor layer (120b).

[0095] For example, the fourth semiconductor layer (130a) may be formed of an intrinsic semiconductor layer, and the fifth semiconductor layer (130b) may be formed of an intrinsic semiconductor layer.

[0096] Since the fourth semiconductor layer (130a) is formed of an intrinsic semiconductor layer and the fifth semiconductor layer (130b) is formed of an intrinsic semiconductor layer, a defect may not occur on the upper surface of the first semiconductor layer (110) in the process of forming the second semiconductor layer (120a) on the first semiconductor layer (110), and a defect may not occur on the lower surface of the first semiconductor layer (110) in the process of forming the third semiconductor layer (120b) on the first semiconductor layer (110).

[0097] For another example, the fourth semiconductor layer (130a) may be a semiconductor layer doped at a relatively lower concentration than the second semiconductor layer (120a), and the fifth semiconductor layer (130b) may be a semiconductor layer doped at a relatively lower concentration than the third semiconductor layer (120b).

[0098] The dopant doped into the fourth semiconductor layer (130a) and the dopant doped into the second semiconductor layer (120a) may be of the same type, for example, the same P type. In addition, the dopant doped into the fifth semiconductor layer (130b) and the dopant doped into the third semiconductor layer (120b) may be of the same type, for example, the same N type.

[0099] By forming the fourth semiconductor layer (130a) between the first semiconductor layer (110) and the second semiconductor layer (120a), the occurrence of defects on the upper surface of the first semiconductor layer (110) can be prevented, and by forming the fifth semiconductor layer (130b) between the first semiconductor layer (110) and the third semiconductor layer (120b), the occurrence of defects on the lower surface of the first semiconductor layer (110) can be prevented.

[0100] At this time, it is preferable that the dopant concentration of the low-concentration doped fourth semiconductor layer (130a) and the fifth semiconductor layer (130b) be controlled to such an extent that no defects occur on the surface of the first semiconductor layer (110).

[0101] When the dopant concentration of the fourth semiconductor layer (130a) is formed relatively lower than the dopant concentration of the second semiconductor layer (120a), and the dopant concentration of the fifth semiconductor layer (130b) is formed relatively lower than the dopant concentration of the third semiconductor layer (120b), the second semiconductor layer (120a) and the fourth semiconductor layer (130a) can be continuously performed in one chamber, and also the third semiconductor layer (120b) and the fifth semiconductor layer (130b) can be continuously performed in one chamber, so that separate deposition equipment or processes may not be added, and as a result, the solar cell of the present invention has the advantage of excellent productivity.

[0102] FIG. 3 is a flowchart illustrating a method for forming a plasma damage prevention layer included in a solar cell according to one embodiment of the present invention.

[0103] As can be seen in FIG. 3, a method for forming a plasma damage prevention layer according to an embodiment of the present invention includes a step of injecting a first source material (S110), a step of injecting a second source material (S120), a step of injecting a first purge gas (S130), a step of injecting a first reactant material (S140), and a step of injecting a second purge gas (S150). At this time, through the step of injecting the first source material (S110) to the step of injecting the second purge gas (S150), a first plasma damage prevention layer (200a) and a second plasma damage prevention layer (200b) included in a solar cell according to an embodiment of the present invention according to FIG. 1 or 2 described above can be formed.

[0104] According to one embodiment of the present invention, the step of forming the plasma damage prevention layer may utilize atomic layer deposition (ALD). In this case, the atomic layer deposition (ALD) may be, for example, thermal atomic layer deposition (Thermal ALD) or plasma enhanced atomic layer deposition (PELAD).

[0105] Therefore, the step of spraying the first source material (S110) to the step of spraying the second purge gas (S150) can be performed in a vacuum chamber, and specifically, the substrate is placed on a susceptor provided at the bottom of the vacuum chamber, and the first source material, the second source material, and the first reactant are sprayed through a gas spray port provided at the top of the vacuum chamber to form the first plasma damage prevention layer (200a) on the upper surface of the second semiconductor layer (120a), or the second plasma damage prevention layer (200b) can be formed on the lower surface of the third semiconductor layer (120b).

[0106] When the above-described atomic layer deposition (ALD) method is used, the steps of spraying the first source material on the second semiconductor layer (120a), spraying the second source material, processing the first purge gas, spraying the first reactant, and then processing the second purge gas can be repeated in one cycle. Furthermore, the steps of spraying the first source material under the third semiconductor layer (120b), spraying the second source material, processing the first purge gas, spraying the first reactant, and then processing the second purge gas can be repeated in one cycle.

[0107] The step of spraying the first source material (S110) and the step of spraying the second source material (S120) may be performed separately or simultaneously. Specifically, after the first source material is sprayed, the second source material may be sprayed, and the first source material and the second source material may be mixed in the same gas supply pipe and supplied into the chamber, or the first source material and the second source material may be sprayed simultaneously, mixed in the same gas supply pipe, and the first source material and the second source material may be mixed in the chamber and supplied into the chamber.

[0108] In the step (S110) of spraying the first source material, the first source material may be any one of aluminum (Al), zinc (Zn), tin (Sn), and indium (In) series materials. At this time, each of the materials may be a precursor material or a gas material.

[0109] In the step (S120) of spraying the second source material, the second source material may be any one of aluminum (Al), zinc (Zn), tin (Sn), and indium (In) series materials. At this time, each of the materials may be a precursor material or a gas material.

[0110] At this time, the second source material can be selected to match the first source material.

[0111] For example, if the first source material is an aluminum (Al) series material, the second source material may be a zinc (Zn) series material.

[0112] As another example, when the first source material is an indium (In) series material, the second source material may be any one of a zinc (Zn) and tin (Sn) series material.

[0113] As another example, when the first source material is a zinc (Zn) series material, the second source material may be any one of aluminum (Al) and indium (In) series materials.

[0114] As another example, if the first source material is a tin (Sn) series material, the second source material may be an indium (In) series material.

[0115] Depending on the combination of the first source material and the second source material selected, the first plasma damage prevention layer (200a) and the second plasma damage prevention layer (200b) formed through the step of spraying the first source material (S110) or the step of spraying the second purge gas (S150) may be formed of any one of a thin film of AZO, ITO, and IZO.

[0116] After the step of injecting the first source material (S120) is performed, the step of injecting the first purge gas (S130) may be performed.

[0117] The first purge gas may utilize a non-reactive gaseous substance. For example, the first purge gas may utilize argon (Ar) gas or nitrogen (N2) gas, but is not limited thereto. The step of injecting the first purge gas (S130) may be performed by injecting the first purge gas into the chamber so that no unnecessary substances remain inside the chamber after the step of injecting the first source material (S110) and the step of injecting the second source material (S120) are performed.

[0118] After the step of injecting the first purge gas (S130) is performed, the step of injecting the first reactant (S140) may be performed.

[0119] At this time, the first reactant material may be selected to match the first source material and the second source material in the step of injecting the first source material (S110) and the step of injecting the second source material (S120).

[0120] For example, when the first source material is an indium (In) series material and the second source material is a tin (Sn) series material, the first reactant material may be either oxygen (O2) or ozone (O3). In this case, the first plasma damage prevention layer (200a) and the second plasma damage prevention layer (200b) may include ITO (InSnO).

[0121] After the step of injecting the first reactant (S140) is performed, the step of injecting the second purge gas (S150) may be performed.

[0122] After the step of injecting the first reactant (S130) is performed, the step of injecting the second purge gas (S140) may be performed.

[0123] At this time, the step (S150) of injecting the second purge gas may be performed in the same manner as the step (S130) of injecting the first purge gas. Accordingly, the second purge gas may be argon (Ar) gas or nitrogen (N2) gas, but is not limited thereto. The step (S150) of injecting the second purge gas may inject the second purge gas into the chamber so that no unnecessary material remains inside the chamber after the step (S140) of injecting the first reactant.

[0124] FIGS. 4A to 4G are schematic process cross-sectional views illustrating a manufacturing process of a solar cell according to one embodiment of the present invention, which relate to the manufacturing method of the solar cell illustrated in FIG. 1 described above.

[0125] First, as can be seen in Fig. 4a, a second semiconductor layer (120a) is formed on the upper surface of a first semiconductor layer (110) made of a semiconductor wafer.

[0126] The above first semiconductor layer (110) may be formed of an N-type silicon wafer.

[0127] Although not illustrated, a texturing process may be performed prior to the step of forming the second semiconductor layer (120a) to form a rough structure on at least one of the upper or lower surfaces of the first semiconductor layer (110). The texturing process may be performed using reactive ion etching (RIE) or a wet etching method.

[0128] The step of forming the second semiconductor layer (120a) may be performed by forming a P-type semiconductor layer, for example, a P-type amorphous silicon layer, on the first semiconductor layer (110) using a PECVD (Plasma Enhanced Chemical Vapor Deposition) method.

[0129] Next, as can be seen in Fig. 4b, a first plasma damage prevention layer (200a) is formed on the second semiconductor layer (120a).

[0130] The step of forming the first plasma damage prevention layer (200a) may be performed by forming a material layer such as ITO (Indium Tin Oxide), IZO (Indium Zinc Oxide), and AZO (Aluminum Zinc Oxide) using atomic layer deposition (ALD).

[0131] At this time, the atomic layer deposition (ALD) method may use, for example, thermal atomic layer deposition (Thermal ALD) or plasma enhanced atomic layer deposition (Plasma Enhanced ALD; PEALD).

[0132] The step of forming the first plasma damage prevention layer (200a) is the same as that described in FIG. 3 above, so a repeated description will be omitted.

[0133] Next, as can be seen in Fig. 4c, a first transparent conductive layer (300a) is formed on the first plasma damage prevention layer (200a).

[0134] The step of forming the first transparent conductive layer (300a) may be performed by forming a transparent conductive material layer such as ITO (Indium Tin Oxide), ZnOH, ZnO:B, ZnO:Al, SnO2, SnO2:F, etc. using sputtering or MOCVD (Metal Organic Chemical Vapor Deposition) method.

[0135] In the case where the first transparent conductive layer (300a) is formed through the sputtering process, the sputtering process may be performed in a separate chamber different from the chamber in which the first plasma damage prevention layer (200a) is formed in FIG. 4b.

[0136] A target material to be deposited on the upper surface of the first plasma damage prevention layer (200a) can be prepared within the chamber. For example, when the first transparent conductive layer (300a) is formed of ITO (Indium Tin Oxide), the target material may be an ITO sputtering target material.

[0137] After preparing the target material, a carrier material may be injected into the chamber. The carrier material may be, for example, argon (Ar) gas.

[0138] After injecting the carrier material, a cathode (-) can be connected to the target material, and an anode (+) can be connected to a location where the target material is to be formed, for example, a location where the first plasma damage prevention layer (200a) is formed. At this time, when power is applied to form plasma, the carrier material accelerated by the plasma collides with the target material, so that the target material can be formed as a film on the plasma damage prevention layer (200a).

[0139] When the first transparent conductive layer (300a) is formed through the metal organic chemical vapor deposition (MOCVD), it may be formed in the same chamber as the chamber in which the first plasma damage prevention layer (200a) is formed in FIG. 4b, or it may be formed in a different chamber. By simultaneously spraying the source material and the reactant material for forming the first transparent conductive layer (300a) onto the first plasma damage prevention layer (200a), the first transparent conductive film (300a) can be formed through the metal organic chemical vapor deposition (MOCVD).

[0140] Next, as can be seen in FIG. 4d, a third semiconductor layer (120b) is formed on the lower surface of the first semiconductor layer (110).

[0141] The step of forming the third semiconductor layer (120b) may be performed by forming an N-type semiconductor layer, for example, an N-type amorphous silicon layer, on the first semiconductor layer (110) using a PECVD (Plasma Enhanced Chemical Vapor Deposition) method.

[0142] Next, as can be seen in FIG. 4e, a second plasma damage prevention layer (200b) is formed on the third semiconductor layer (120b).

[0143] The step of forming the second plasma damage prevention layer (200b) may be performed by forming a material layer such as ITO (Indium Tin Oxide), IZO (Indium Zinc Oxide), and AZO (Aluminum Zinc Oxide) using atomic layer deposition (ALD).

[0144] At this time, the atomic layer deposition (ALD) method may use, for example, thermal atomic layer deposition (Thermal ALD) or plasma enhanced atomic layer deposition (Plasma Enhanced ALD; PEALD).

[0145] The step of forming the second plasma damage prevention layer (200b) is the same as that described in FIG. 3 above, so a repeated description will be omitted.

[0146] Next, as can be seen in FIG. 4f, a second transparent conductive layer (300b) is formed on the second plasma damage prevention layer (200b).

[0147] The step of forming the second transparent conductive layer (300b) may be performed by forming a transparent conductive material layer such as ITO (Indium Tin Oxide), ZnOH, ZnO:B, ZnO:Al, SnO2, SnO2:F, etc. using sputtering or MOCVD (Metal Organic Chemical Vapor Deposition) method.

[0148] The second transparent conductive layer (300b) can be formed in the same manner as the first transparent conductive layer (300a) in FIG. 4c, and since this is the same as the content described above and in FIG. 4c, detailed descriptions are omitted.

[0149] Next, as can be seen in FIG. 4g, a first electrode (400a) is formed on the first transparent conductive layer (300a), and a second electrode (400b) is formed on the second transparent conductive layer (300b).

[0150] The first electrode (400a) and the second electrode (400b) can be formed through screen printing. At this time, the first electrode (400a) is formed on the upper surface of the first transparent conductive layer (300a), and the second electrode (400b) is formed on the lower surface of the second transparent conductive layer (300b).

[0151] FIGS. 5A to 5G are schematic process cross-sectional views illustrating a manufacturing process of a solar cell according to another embodiment of the present invention, which relates to the manufacturing method of the solar cell illustrated in FIG. 2 described above. In this case, FIGS. 5A to 5F are identical to FIGS. 4A to 4F except for the addition of the configuration of the fourth semiconductor layer and the fifth semiconductor layer, and therefore, the following description will focus on the different configurations.

[0152] First, as can be seen in Fig. 5a, a fourth semiconductor layer (130a) is formed on the upper surface of a first semiconductor layer (110) made of a semiconductor wafer, and a second semiconductor layer (120a) is formed on the upper surface of the fourth semiconductor layer (130a). Meanwhile, the description of the first semiconductor layer (110) is the same as in Fig. 4a, and thus will be omitted.

[0153] The fourth semiconductor layer (130a) may be formed as an I (intrinsic) type amorphous silicon layer using a PECVD (Plasma Enhanced Chemical Vaporization Deposition) method, or the fourth semiconductor layer (130a) may be formed to be doped at a relatively lower concentration than the second semiconductor layer (120a).

[0154] When the fourth semiconductor layer (130a) is doped at a lower concentration than the second semiconductor layer (120a), the steps of forming the fourth semiconductor layer (130a) doped at a lower concentration and the second semiconductor layer (120a) doped at a higher concentration can be performed continuously in one chamber. That is, the fourth semiconductor layer (130a) doped at a lower concentration and the second semiconductor layer (120a) doped at a higher concentration can be formed continuously while controlling the amount of dopant gas of a Group III element such as boron (B) in one PECVD (Plasma Enhanced Chemical Vaporization Deposition) chamber.

[0155] Next, as can be seen in Fig. 5b, a first plasma damage prevention layer (200a) is formed on the second semiconductor layer (120a). At this time, the method of forming the first plasma damage prevention layer (200a) is the same as in Fig. 4b, so a detailed description thereof will be omitted.

[0156] Next, as can be seen in Fig. 5c, a first transparent conductive layer (300a) is formed on the first plasma damage prevention layer (200a). At this time, the method for forming the first transparent conductive layer (300a) is the same as in Fig. 4c, so a detailed description thereof will be omitted.

[0157] Next, as can be seen in FIG. 5d, a fifth semiconductor layer (130b) is formed on the lower surface of the first semiconductor layer (110), and a third semiconductor layer (120b) is formed on the lower surface of the fifth semiconductor layer (130b).

[0158] The fifth semiconductor layer (130b) may be formed as an I (intrinsic) type amorphous silicon layer using a PECVD (Plasma Enhanced Chemical Vaporization Deposition) method, or the fifth semiconductor layer (130b) may be formed to be doped at a relatively lower concentration than the third semiconductor layer (120b).

[0159] When the fifth semiconductor layer (130b) is doped at a lower concentration than the third semiconductor layer (120b), the steps of forming the fifth semiconductor layer (130b) doped at a lower concentration and the third semiconductor layer (120b) doped at a higher concentration can be performed continuously in one chamber. That is, the fifth semiconductor layer (130b) doped at a lower concentration and the third semiconductor layer (120b) doped at a higher concentration can be formed continuously in one PECVD (Plasma Enhanced Chemical Vaporization Deposition) chamber while controlling the amount of dopant gas of a Group III element such as boron (B).

[0160] Next, as can be seen in FIG. 5e, a second plasma damage prevention layer (200b) is formed on the third semiconductor layer (120b). At this time, the method of forming the second plasma damage prevention layer (200b) is the same as in FIG. 4e, so a detailed description thereof will be omitted.

[0161] Next, as can be seen in FIG. 5f, a second transparent conductive layer (300b) is formed on the second plasma damage prevention layer (200b).

[0162] At this time, the second transparent conductive layer (300b) can be formed in the same manner as forming the second transparent conductive layer (300b) in FIG. 4f, and since this is the same as the description in FIG. 4c, a detailed description will be omitted.

[0163] Next, as can be seen in FIG. 5g, a first electrode (400a) is formed on the first transparent conductive layer (300a), and a second electrode (400b) is formed on the second transparent conductive layer (300b). The first electrode (400a) is formed on the upper surface, and the second electrode (400b) is formed on the lower surface of the second transparent conductive layer (300b). At this time, the method of forming the second transparent conductive layer (300b), the first electrode (400a), and the second electrode (400b) is the same as in FIG. 4f, so a detailed description thereof will be omitted.

[0164] Below, a substrate processing device for forming a plasma damage prevention layer according to the present invention will be described with reference to FIGS. 6 to 9.

[0165] Referring to FIGS. 6 and 7, the substrate processing device (1) performs a processing process on a substrate (20). For example, the substrate processing device (1) can perform a deposition process for depositing a thin film on the substrate (20). For example, the substrate processing device (1) can perform a deposition process such as CVD (Chemical Vapor Depostion), ALD (Atomic Layer Deposition), etc. The substrate processing device (1) includes a mounting table (2), a third electrode (3), a fourth electrode (4), a first injection unit (5), a second injection unit (6), a first injection unit (7), and a second injection unit (8).

[0166] Referring to Fig. 6, the mounting stand (2) supports the substrate (20). The substrate (20) can be mounted on the mounting stand (2). The mounting stand (2) can be placed below the fourth electrode (4). In this case, the substrate (20) can be mounted on the upper surface of the mounting stand (2). The substrate (20) can be a semiconductor substrate, a wafer, or the like. The mounting stand (2) can also support a plurality of substrates (20).

[0167] The above-mentioned mounting plate (2) can be coupled to a chamber (50). The chamber (50) provides a processing space where the processing process takes place. The mounting plate (2) can be placed inside the chamber (50). The mounting plate (2) can also be rotatably coupled to the chamber (50). In this case, the mounting plate (2) can be connected to a rotating part that provides rotating force. The rotating part can rotate the substrate (20) supported on the mounting plate (2) by rotating the mounting plate (2).

[0168] Referring to Fig. 6, the third electrode (3) is positioned on the upper side of the mounting plate (2). The third electrode (3) may be positioned on the upper side of the fourth electrode (4). The third electrode (3) may be positioned so as to be spaced a predetermined distance upward from the fourth electrode (4). The third electrode (3) may be positioned inside the chamber (50). The third electrode (3) may be coupled to the chamber (50) so as to be positioned on the upper side of the chamber (50). The third electrode (3) may be formed in an overall square plate shape, but is not limited thereto and may be formed in other shapes such as a disc shape.

[0169] Referring to Fig. 6, the fourth electrode (4) is positioned between the third electrode (3) and the mounting plate (3). The fourth electrode (4) may be positioned below the third electrode (3) and above the mounting plate (3). The fourth electrode (4) may be positioned so as to be spaced a predetermined distance upward from the mounting plate (3). The fourth electrode (4) may be positioned inside the chamber (50). The fourth electrode (4) may be formed in an overall square plate shape, but is not limited thereto and may be formed in other shapes such as a disc shape.

[0170] The fourth electrode (4) and the third electrode (3) can be used to generate plasma. One of the fourth electrode (4) and the third electrode (3) can be applied with RF (Radio Frequency) power, and the other can be grounded. Accordingly, a discharge can be generated by an electric field applied between the fourth electrode (4) and the third electrode (3), thereby generating plasma. RF power can be applied to the fourth electrode (4), and the third electrode (3) can be grounded. The fourth electrode (4) can also be grounded, and RF power can be applied to the third electrode (3).

[0171] An opening (41) may be formed in the fourth electrode (4). The opening (41) may be formed to penetrate the fourth electrode (4). The opening (41) may be formed to penetrate the upper and lower surfaces of the fourth electrode (4). The opening (41) may be formed in an overall cylindrical shape, but is not limited thereto and may be formed in other shapes, such as a rectangular parallelepiped shape.

[0172] When the opening (41) is formed in the fourth electrode (4), a protruding electrode (31) may be coupled to the third electrode (3). The protruding electrode (31) may be coupled to the third electrode (3) so as to protrude toward the mounting plate (2). The protruding electrode (31) may protrude from the lower surface of the third electrode (3). The protruding electrode (31) and the third electrode (3) may be formed integrally. When the third electrode (3) is grounded, the protruding electrode (31) may be grounded through the third electrode (3). When RF power is applied to the third electrode (3), RF power may be applied to the protruding electrode (31) through the third electrode (3).

[0173] The fourth electrode (4) may have a plurality of openings (41). The openings (41) may be positioned at positions spaced apart from each other. In this case, the third electrode (3) may be coupled with a plurality of protruding electrodes (31). The protruding electrodes (31) may be positioned at positions spaced apart from each other. The openings (41) may be positioned at positions corresponding to the protruding electrodes (31). Accordingly, the protruding electrodes (31) may protrude toward the openings (41). The protruding electrodes (31) may protrude to a length that allows them to be inserted into the openings (41). Although not shown, the protruding electrodes (31) may also protrude to a length that does not allow them to be inserted into the openings (41). In this case, the protruding electrodes (31) may be positioned above the openings (41).

[0174] Referring to FIGS. 6 and 7, the first injection unit (5) injects a first gas. At this time, the first gas may be any one of the first source material or the second source material described in FIG. 3. Accordingly, as described above, the first gas may include any one of materials including at least one of aluminum (Al), indium (In), tin (Sn), and zinc (Zn) series materials.

[0175] The first gas may be a gas for performing a processing process on the substrate (20). The first gas may be a mixed gas in which a gas for performing a processing process on the substrate (20) and a gas for generating plasma are mixed.

[0176] The first injection unit (5) can inject the first gas into the first injection unit (7). The first gas injected into the first injection unit (7) can flow along the first injection unit (7) so as to be injected toward the entire front surface of the substrate (20) and then be injected toward the mounting plate (2) through the third electrode (3). The entire front surface of the substrate (20) may correspond to the entire upper surface of the substrate (20). The upper surface of the substrate (20) is a surface arranged to face the fourth electrode (4). The first injection unit (5) can be coupled to the chamber (50).

[0177] Referring to FIGS. 6 to 8, the second injection unit (6) injects a second gas. At this time, the second gas may be the first reactant described in FIG. 3. Accordingly, as described above, the second gas may include any one of substances including oxygen (O2) and ozone (O3).

[0178] The second gas may be a gas for performing a processing process on the substrate (20). The second gas may be a mixed gas in which a gas for performing a processing process on the substrate (20) and a gas for generating plasma are mixed. The second gas and the first gas may be composed of different components.

[0179] The second injection unit (6) can inject the second gas into the second injection unit (8). The second gas injected into the second injection unit (8) can flow along the second injection unit (8) so as to be injected toward the entire surface of the substrate (20) and then be injected toward the mounting plate (2) through the third electrode (3). The second injection unit (6) can be coupled to the chamber (50). The second gas injected by the second injection unit (6) and the first gas injected by the first injection unit (5) can be used to perform a processing process on the substrate (20) by being injected toward the substrate (20) supported on the mounting plate (2). Therefore, the first gas and the second gas can be injected separately by the gas injection unit.

[0180] The second injection unit (6) and the first injection unit (5) may be respectively positioned on the same side with respect to the third electrode (3). The second injection unit (6) and the first injection unit (5) may inject the second gas and the first gas into the second injection unit (8) and the first injection unit (7), respectively.

[0181] Next, as illustrated in FIG. 7, the embodiment may be such that the second injection portion (6) is disposed on one side (3a) of the third electrode (3) and the first injection portion (5) is disposed on one side (3a) of the third electrode (3). That is, the embodiment may be such that the second injection portion (6) and the first injection portion (5) are disposed on the same side with respect to the third electrode (3).

[0182] The second gas injected into the second injection unit (8) by the second injection unit (6) flows from one side (3a) of the third electrode (3) toward the other side (3c). Accordingly, the second gas is injected from one side (21) to the other side (22) of the substrate (20). The dotted arrow in Fig. 7 indicates the second gas.

[0183] The first gas injected into the first injection unit (7) by the first injection unit (5) flows from one side (3a) of the third electrode (3) toward the other side (3c). Accordingly, the more it flows from one side (21) of the substrate (20) toward the other side (22), the more it is injected toward the substrate (20). The solid arrow in Fig. 7 indicates the first gas.

[0184] In Fig. 7, it is described that both the second injection part (6) and the first injection part (5) are arranged on one side (3a) of the third electrode (3), but this is not limited thereto, and the second injection part (6) and the first injection part (5) may be implemented differently if they are arranged on the same side with respect to the third electrode (3).

[0185] For example, both the second injection part (6) and the first injection part (5) may be placed on the other side (3c) of the third electrode (3).

[0186] For example, as illustrated in FIG. 9, both the second injection unit (6) and the first injection unit (5) may be arranged to inject the second gas and the first gas through the central portion of the third electrode (3) from the upper side (3b) of the third electrode (3).

[0187] Referring to FIGS. 7 and 8, the first injection unit (7) injects the first gas through the third electrode (3). The first injection unit (7) can be connected to the first injection unit (5). The first gas injected into the first injection unit (7) by the first injection unit (5) can flow along the first injection unit (7) and be injected toward the mounting plate (2).

[0188] The above first injection unit (7) may include a first injection member (71).

[0189] The first injection member (71) is disposed inside the third electrode (3). The first injection member (71) can function as a passage for flowing the first gas injected from the first injection portion (5). The first injection member (71) can be formed to extend along the first axial direction (X-axis direction). Accordingly, the first gas injected into the first injection member (71) can flow in the first axial direction (X-axis direction) along the first injection member (71). The first injection member (71) can be implemented as a pipe, a tube, or the like. In this case, the first injection member (71) can be coupled to the third electrode (3) so as to be disposed inside the third electrode (3). The first injection member (71) may be implemented to be placed inside the third electrode (3) by forming a groove inside the third electrode (3). The first injection unit (7) may include a first injection hole (72).

[0190] The first injection hole (72) is for injecting the first gas toward the mounting plate (2). The first injection hole (72) may be connected to the first injection member (71). Accordingly, the first gas flowing along the first injection member (71) may be injected toward the mounting plate (2) through the first injection hole (72). The first injection hole (72) may be formed such that one end is connected to the first injection member (71) and the other end penetrates the third electrode (3). When the first injection member (71) is formed parallel to the first axial direction (X-axis direction), the first injection hole (72) may be formed parallel to the up-down direction (Z-axis direction).

[0191] The first injection unit (7) may include a plurality of first injection holes (72). The first injection holes (72) may be arranged to be spaced apart from each other along the first axial direction (X-axis direction). Accordingly, the first injection holes (72) may inject the first gas to different parts of the substrate (20) supported on the mounting plate (2). The first injection holes (72) may be respectively connected to different parts of the first injection member (71). Accordingly, the first gas may flow along the first injection member (71) in the first axial direction (X-axis direction) and be injected toward the mounting plate (2) through the first injection holes (72).

[0192] As the first injection holes (72) are provided in multiple numbers, the first injection unit (7) can be implemented to inject the first gas entirely toward the substrate (20) based on the first axial direction (X-axis direction). In order to inject the first gas entirely toward the substrate (20) based on the second axial direction (Y-axis direction) perpendicular to the first axial direction (X-axis direction), the first injection unit (7) can include a plurality of first injection members (71).

[0193] The first injection members (71) may be arranged at positions spaced apart from each other along the second axial direction (Y-axis direction). The second axial direction (Y-axis direction) and the first axial direction (X-axis direction) are axial directions that are arranged perpendicular to each other on one plane. A plurality of first injection holes (72) may be connected to each of the first injection members (71). Accordingly, the first injection members (71) may inject the first gas toward the mounting plate (2) through the first injection holes (72). Therefore, the substrate processing device (1) according to the present invention may inject the first gas as a whole toward the substrate (20) based on the first axial direction (X-axis direction) as well as inject the first gas as a whole toward the substrate (20) based on the second axial direction (Y-axis direction). Accordingly, the substrate processing device (1) according to the present invention is implemented so as to be able to inject the first gas toward the entire surface of the substrate (20) placed on the mounting plate (2). The first injection holes (72) may be formed to penetrate the protruding electrode (31). In this case, the first gas may be injected toward the opening (41) through the first injection holes (72) and then flow toward the mounting plate (2) through the opening (41).

[0194] Referring to FIGS. 7 and 8, the second injection unit (8) injects the second gas through the third electrode (3). The second injection unit (8) can be connected to the second injection unit (6). The second gas injected into the second injection unit (8) by the second injection unit (6) can flow along the second injection unit (8) and be injected toward the mounting plate (2).

[0195] The above second injection unit (8) may include a second injection member (81).

[0196] The second injection member (81) is disposed inside the third electrode (3). The second injection member (81) can function as a passage for flowing the second gas injected from the second injection portion (6). The second injection member (81) can be formed to extend along the first axial direction (X-axis direction). Accordingly, the second gas injected into the second injection member (81) can flow in the first axial direction (X-axis direction) along the second injection member (81). The second injection member (81) can be implemented as a pipe, a tube, or the like. In this case, the second injection member (81) can be coupled to the third electrode (3) so as to be disposed inside the third electrode (3). The second injection member (81) may be implemented to be placed inside the third electrode (3) by forming a groove inside the third electrode (3). In this case, when the substrate processing device (1) needs to control the temperature of the second gas flowing along the second injection member (81), the temperature of the third electrode (3) can be controlled to directly control the temperature of the second gas. Accordingly, the substrate processing device (1) can improve the ease and accuracy of the task of controlling the temperature of the second gas.

[0197] The above second injection unit (8) may include a second injection hole (82).

[0198] The second injection hole (82) is for injecting the second gas toward the mounting plate (2). The second injection hole (82) may be connected to the second injection member (81). Accordingly, the second gas flowing along the second injection member (81) may be injected toward the mounting plate (2) through the second injection hole (82). The second injection hole (82) may be formed such that one end is connected to the second injection member (81) and the other end penetrates the third electrode (3). When the second injection member (81) is formed parallel to the first axial direction (X-axis direction), the second injection hole (82) may be formed parallel to the up-down direction (Z-axis direction).

[0199] The second injection unit (8) may include a plurality of second injection holes (82). The second injection holes (82) may be arranged to be spaced apart from each other along the first axial direction (X-axis direction). Accordingly, the second injection holes (82) may inject the second gas to different parts of the substrate (20) supported on the mounting plate (2). The second injection holes (82) may be respectively connected to different parts of the second injection member (81). Accordingly, the second gas may flow along the second injection member (81) in the first axial direction (X-axis direction) and be injected toward the mounting plate (2) through the second injection holes (82). As illustrated in FIG. 7, the second injection holes (82) and the first injection holes (72) may be arranged alternately in a plurality of directions based on the first axial direction (X-axis direction).

[0200] As the second injection holes (82) are provided in multiple numbers, the second injection unit (8) can be implemented to inject the second gas entirely toward the substrate (20) based on the first axial direction (X-axis direction). In order to inject the second gas entirely toward the substrate (20) based on the second axial direction (Y-axis direction) perpendicular to the first axial direction (X-axis direction), the second injection unit (8) can include a plurality of second injection members (81).

[0201] The second injection members (81) may be arranged at positions spaced apart from each other along the second axial direction (Y-axis direction). A plurality of second injection holes (82) may be connected to each of the second injection members (81). Accordingly, the second injection members (81) may inject the second gas toward the mounting plate (2) through the second injection holes (82). Accordingly, the substrate processing device (1) according to the present invention may not only inject the second gas toward the entire substrate (20) based on the first axial direction (X-axis direction), but may also inject the second gas toward the entire substrate (20) based on the second axial direction (Y-axis direction). Accordingly, the substrate processing device (1) according to the present invention is implemented so as to inject the second gas toward the entire surface of the substrate (20) placed on the mounting plate (2). The second injection holes (82) may be arranged above the fourth electrode (4). In this case, the second gas may be injected between the third electrode (3) and the fourth electrode (4) through the second injection holes (82), and then flow toward the mounting plate (2) through the opening (41).

[0202] Although the embodiments of the present invention have been described in more detail with reference to the attached drawings, the present invention is not necessarily limited to these embodiments, and various modifications may be implemented without departing from the technical spirit of the present invention. Therefore, the embodiments disclosed in the present invention are not intended to limit the technical spirit of the present invention, but to explain it, and the scope of the technical spirit of the present invention is not limited by these embodiments. Therefore, it should be understood that the embodiments described above are illustrative in all aspects and not restrictive. The protection scope of the present invention should be interpreted by the claims, and all technical ideas within a scope equivalent thereto should be interpreted as being included in the scope of the rights of the present invention.

Claims

1. First semiconductor layer; A second semiconductor layer provided on one surface of the first semiconductor layer; A first transparent conductive layer provided on the second semiconductor layer; and Including a first plasma damage prevention layer provided between the second semiconductor layer and the first transparent conductive layer, The above first plasma damage prevention layer is a solar cell formed using atomic layer deposition (ALD).

2. In paragraph 1, A solar cell in which the first plasma damage prevention layer is formed using a plasma-enhanced atomic layer deposition (PEALD) method containing oxygen.

3. In paragraph 1, A solar cell wherein the first plasma damage prevention layer is made of an oxide selected from the group consisting of AZO, ITO, and IZO.

4. In paragraph 1, A solar cell in which the thickness of the first plasma damage prevention layer is thinner than that of the first transparent conductive layer.

5. In paragraph 1, A third semiconductor layer provided on the other surface of the first semiconductor layer; A second transparent conductive layer provided on the third semiconductor layer; and A solar cell further comprising a second plasma damage prevention layer provided between the third semiconductor layer and the second transparent conductive layer.

6. In paragraph 5, A solar cell wherein the second plasma damage prevention layer is made of an oxide selected from the group consisting of AZO, ITO, and IZO.

7. In paragraph 5, A solar cell in which the thickness of the second plasma damage prevention layer is thinner than that of the second transparent conductive layer.

8. In paragraph 5, A first electrode provided on the first transparent conductive layer; and A solar cell further comprising a second electrode provided on the second transparent conductive layer.

9. In paragraph 1, A fourth semiconductor layer provided between the first semiconductor layer and the second semiconductor layer; and A solar cell further comprising a fifth semiconductor layer provided between the first semiconductor layer and the third semiconductor layer.

10. In paragraph 9, The fourth semiconductor layer is formed of an intrinsic semiconductor layer or a semiconductor layer doped at a relatively low concentration compared to the second semiconductor layer, A solar cell in which the fifth semiconductor layer is formed of an intrinsic semiconductor layer or a semiconductor layer doped at a relatively low concentration compared to the third semiconductor layer.

11. A step of forming a second semiconductor layer on one surface of a first semiconductor layer made of a semiconductor wafer; A step of forming a first plasma damage prevention layer on the second semiconductor layer; and Comprising a step of forming a first transparent conductive layer on the first plasma damage prevention layer, The above first plasma damage prevention layer is formed using atomic layer deposition (ALD), A method for manufacturing a solar cell in which the first transparent conductive layer is formed using a sputtering method, a chemical vapor deposition method (CVD), and a plasma-enhanced chemical vapor deposition method (PECVD).

12. In paragraph 10, A method for manufacturing a solar cell in which the first plasma damage prevention layer is formed using a plasma-enhanced atomic layer deposition (PEALD) method containing oxygen.

13. In paragraph 11, The step of forming the first plasma damage prevention layer is A step of spraying a first source material; Step of spraying the second source material; Step of injecting the first purge gas; a step of injecting a first reactant; and A method for manufacturing a solar cell, comprising a step of injecting a second purge gas.

14. In paragraph 13, A method for manufacturing a solar cell, wherein the first source material is an aluminum (Al) series material, the second source material is a zinc (Zn) series material, and the first reactant material is one of oxygen (O2) and ozone (O3).

15. In paragraph 13, A method for manufacturing a solar cell, wherein the first source material is an indium (In) series material, the second source material is any one of zinc (Zn) and tin (Sn) series materials, and the first reactant material is any one of oxygen (O2) and ozone (O3).

16. In paragraph 13, A method for manufacturing a solar cell, wherein the first source material is a zinc (Zn) series material, the second source material is any one of aluminum (Al) and indium (In) series materials, and the first reactant material is any one of oxygen (O2) and ozone (O3).

17. In paragraph 13, A method for manufacturing a solar cell, wherein the first source material is a tin (Sn) series material, the second source material is an indium (In) series material, and the first reactant material is one of oxygen (O2) and ozone (O3).

18. In paragraph 11, A method for manufacturing a solar cell, wherein the first plasma damage prevention layer is made of an oxide selected from the group consisting of AZO, ITO, and IZO.

19. In paragraph 11, A step of forming a third semiconductor layer on the other surface of the first semiconductor layer; A step of forming a second plasma damage prevention layer on the third semiconductor layer; and It further includes a step of forming a second transparent conductive layer on the second plasma damage prevention layer, The above second plasma damage prevention layer is formed using atomic layer deposition (ALD), A method for manufacturing a solar cell in which the second transparent conductive layer is formed using a sputtering method, a chemical vapor deposition method (CVD), and a plasma-enhanced chemical vapor deposition method (PECVD).

20. A step of bringing a substrate having a second semiconductor layer formed on one surface of a first semiconductor layer into a chamber; and A step of forming a first plasma damage prevention layer on the second semiconductor layer is included, A method for manufacturing a solar cell in which the first plasma damage prevention layer is formed using an atomic layer deposition (ALD) method.

21. In paragraph 20, A method for manufacturing a solar cell, wherein the first plasma damage prevention layer is made of an oxide selected from the group consisting of AZO, ITO, and IZO.

22. In paragraph 20, After the step of forming the first plasma damage prevention layer, the step of forming a first transparent conductive layer on the first plasma damage prevention layer is additionally included. A method for manufacturing a solar cell in which the first transparent conductive layer is formed using a chemical vapor deposition (CVD) method or a plasma-enhanced chemical vapor deposition (PECVD) method.

23. In paragraph 22, A method for manufacturing a solar cell, wherein the step of forming the first plasma damage prevention layer and the step of forming the first transparent conductive layer are performed in-situ within the chamber.

24. A step of bringing a substrate on which a first semiconductor layer and a second semiconductor layer are formed into a chamber; A step of forming a first plasma damage prevention layer on the second semiconductor layer; and Comprising a step of forming a first transparent conductive layer on the first plasma damage prevention layer, The first plasma damage prevention layer is formed using atomic layer deposition (ALD), A method for manufacturing a solar cell, wherein the first transparent conductive layer is formed using any one of sputtering, chemical vapor deposition (CVD), and plasma-enhanced chemical vapor deposition (PECVD).

Citation Information

Patent Citations

  • Selective layer formation using deposition and removal

    JP7146690B2

  • Flexible Organic Solar Cell and Fabricating Apparatus and Method Thereof

    KR101455514B1

  • Passivation film and method for the same, and display apparatus having the passivation film

    KR101827854B1

  • Smart aluminum processing methods, devices and systems

    KR102534084B1

  • Semiconductor device with advanced pad structure resistant to plasma damage and metnod for forming same

    US20160315058A1