Lithium secondary battery
The lithium secondary battery design with perlithium manganese-rich oxide and a specific non-aqueous electrolyte formulation addresses gas generation and lifespan issues by forming a stable SEI layer, improving performance at high temperatures and voltages.
Patent Information
- Application Number
- PCT/KR2024/003766
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-12-15
- Filing Date
- 2024-03-26
- Publication Date
- 2024-10-03
AI Technical Summary
Lithium secondary batteries using perlithium manganese-rich oxide as a positive electrode active material face issues with increased gas generation and transition metal elution, leading to reduced lifespan and safety concerns, especially at high temperatures and high voltages, due to electrolyte side reactions and SEI film destruction.
A lithium secondary battery design incorporating a positive electrode with perlithium manganese-rich oxide, a non-aqueous electrolyte containing ethylene carbonate, diethyl carbonate, ethylmethyl carbonate, and a cyclic sulfur oxide additive, which reduces gas generation and improves lifespan performance by forming a stable SEI layer.
The solution significantly reduces gas generation and enhances the battery's lifespan and durability at high temperatures and high voltages, maintaining excellent capacity retention and reducing resistance.
Smart Images

Figure PCTKR2024003766-APPB-IMG-000001 
Figure PCTKR2024003766-APPB-IMG-000002 
Figure PCTKR2024003766-APPB-IMG-000003
Abstract
Description
lithium secondary battery
[0001] Cross-citation with related applications
[0002] This application claims the benefit of priority to Korean Patent Application No. 10-2023-0040007, filed March 27, 2023, and Korean Patent Application No. 10-2023-0183782, filed December 15, 2023, the entire contents of which are incorporated herein by reference.
[0003] Technology field
[0004] The present invention relates to a lithium secondary battery.
[0005] Recently, as the application areas of lithium secondary batteries have rapidly expanded to include not only power supply for electronic devices such as electric, electronic, communication, and computer devices, but also power storage for large-area devices such as automobiles and power storage devices, the demand for high-capacity, high-output, and high-stability secondary batteries is increasing.
[0006] The above lithium secondary battery is generally composed of a positive electrode containing a positive electrode active material, a negative electrode containing a negative electrode active material, an electrolyte that serves as a medium for transferring lithium ions, and a separator. At this time, carbon-based active materials, silicon-based active materials, etc. can be used as the negative electrode active material. In addition, lithium transition metal oxides such as lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), and lithium nickel-cobalt-manganese composite oxide can be used as the positive electrode active material.
[0007] Meanwhile, improvements are being made to the characteristics of each of the positive electrode, negative electrode, electrolyte, and separator to form a high-capacity secondary battery.
[0008] One object of the present invention is to provide a lithium secondary battery comprising a lithium manganese-rich oxide as a cathode active material, which reduces the amount of gas generated at the cathode interface during high voltage or high temperature operation, reduces gas generation during initial activation and charge / discharge, and suppresses the elution of transition metals from the cathode active material, thereby simultaneously improving the lifespan, resistance reduction, durability improvement, and gas generation prevention effects at high temperatures.
[0009] The present invention provides a lithium secondary battery comprising: a positive electrode; a negative electrode; a separator interposed between the positive electrode and the negative electrode; and a non-aqueous electrolyte; wherein the positive electrode comprises a positive electrode active material, the positive electrode active material comprises a perlithium manganese-rich oxide comprising Mn in an amount of about 50 mol% or more among all metals excluding lithium, and a molar ratio of lithium to transition metal exceeding about 1; and the non-aqueous electrolyte comprises a lithium salt, an organic solvent, and an additive, the organic solvent comprises a first organic solvent and a second organic solvent, the first organic solvent comprises ethylene carbonate, the second organic solvent comprises diethyl carbonate and ethylmethyl carbonate, and the additive comprises a compound represented by the following chemical formula 1.
[0010] [Chemical Formula 1]
[0011]
[0012] In the above chemical formula 1, n is 1 or 2, L1 and L2 are each independently a direct bond or a substituted or unsubstituted alkylene group having 1 to 6 carbon atoms, R1 and R2 are each independently selected from a substituent represented by the following chemical formula 2, an alkyl group having 1 to 10 carbon atoms, an alkyl group having 1 to 10 carbon atoms substituted with at least one fluorine, an alkenyl group having 2 to 10 carbon atoms, an alkynyl group having 2 to 10 carbon atoms, a phosphate group, and a nitrile group, and at least one of R1 and R2 is a substituent represented by the following chemical formula 2,
[0013] [Chemical Formula 2]
[0014]
[0015] In the above chemical formula 2, m is 1 or 2, X1 and X2 are each independently -O- or -C(R 31 )(R 32 )-, but at least one of the above X1 and X2 is -O-, and R 31 Inland R 36 are each independently hydrogen, an alkyl group having 1 to 6 carbon atoms, -C(=O)-R4 or -R5-OC(=O)-R6, wherein R4 and R6 are each independently a substituted or unsubstituted alkyl group having 1 to 6 carbon atoms, an alkenyl group having 2 to 20 carbon atoms, an alkynyl group having 2 to 20 carbon atoms, or a substituted or unsubstituted aryl group having 6 to 20 carbon atoms, wherein R5 is a substituted or unsubstituted alkylene group having 1 to 6 carbon atoms, and the substituents of L1, L2, R4, R5 and R6 are each independently at least one selected from the group consisting of deuterium, -F, -Cl, -Br, -I, -CN, -NO2 and -SO3, and * is a position bonded to L1 or L2, but when both L1 and L2 are direct bonds, R1 and R2 are not CS-7 at the same time, and L1 and L2 are When both are methylene groups and n is 2, R1 and R2 are not CS-2 at the same time.
[0016] .
[0017] The lithium secondary battery of the present invention uses a perlithium manganese-rich oxide as a positive electrode active material, and is characterized in that the non-aqueous electrolyte includes a lithium salt, an organic solvent, and an additive, wherein the organic solvent includes ethylene carbonate, diethyl carbonate, and ethylmethyl carbonate, and the additive includes a cyclic sulfur oxide represented by a specific chemical formula. According to the present invention, the combination of the above-described organic solvents significantly reduces the amount of gas generated at the positive electrode interface including the perlithium manganese-rich oxide, improves the life performance of the negative electrode, and as a result, it is possible to realize a lithium secondary battery having excellent capacity retention rate and gas generation reduction performance. For example, since the cyclic sulfur oxide included as the additive has a low consumption rate within the secondary battery, it can continuously improve long-term durability during operation of the secondary battery. Therefore, the lithium secondary battery of the present invention can simultaneously improve the lifespan, resistance reduction, durability improvement, and gas generation prevention effects, especially at high temperatures and high voltages.
[0018] Terms or words used in this specification and claims should not be interpreted as limited to their usual or dictionary meanings, but should be interpreted as meanings and concepts that conform to the technical spirit of the present invention, based on the principle that the inventor can appropriately define the concept of the term to explain his or her own invention in the best possible manner.
[0019] It should be understood that the terms “include,” “comprising,” or “having” used in this specification are intended to specify the presence of a feature, number, step, component, or combination thereof, but do not preclude the possibility of the presence or addition of one or more other features, numbers, steps, components, or combinations thereof.
[0020] In this specification, the average particle diameter (D 50) can be defined as the particle size corresponding to 50% of the volume accumulation in the particle size distribution curve. The average particle size (D 50 ) can be measured, for example, using a laser diffraction method. The laser diffraction method can generally measure particle diameters from the submicron range to several mm, and can obtain results with high reproducibility and high resolution.
[0021] As used herein, the terms "about," "approximately," and "substantially" are used to mean a range or approximation of a numerical value or degree, taking into account inherent manufacturing and material tolerances, and are used to prevent infringers from unfairly exploiting the disclosure, which includes precise or absolute numerical values provided to aid understanding of the present invention.
[0022] Lithium manganese-rich oxides (LiMnO) are attracting attention as next-generation cathode active materials for high-capacity batteries. LiMnO is relatively inexpensive and contains a high amount of abundant manganese (Mn), and lithium secondary batteries using it have the advantage of high capacity. However, when using LiMnO, there is a problem that the amount of gas emissions such as CO2 increases significantly due to electrolyte side reactions at the cathode interface when operated at high voltages (e.g., 4.35 V or higher) or high temperatures. Furthermore, in the case of LiMnO, the decomposition of the electrolyte is aggravated by reactive oxygen generated by the phase transformation of the cathode active material during activation (formation) and charge / discharge processes, which significantly increases the amount of gas emissions such as CO2. In addition, the use of LiMnO is limited by the problem that transition metals eluted from the cathode active material are deposited on the cathode, destroying the solid electrolyte interphase (SEI) film of the cathode.
[0023] The present invention provides a lithium secondary battery that overcomes the aforementioned gas generation problem and SEI film destruction problem of the negative electrode while applying lithium manganese-rich oxide as a positive electrode active material of the lithium secondary battery.
[0024] Hereinafter, the present invention will be described in more detail.
[0025]
[0026] lithium secondary battery
[0027] The present invention relates to a lithium secondary battery.
[0028] The present invention provides a lithium secondary battery comprising: a positive electrode; an negative electrode; a separator interposed between the positive electrode and the negative electrode; and a non-aqueous electrolyte; wherein the positive electrode comprises a positive electrode active material, and the positive electrode active material comprises a perlithium manganese-rich oxide containing Mn of about 50 mol% or more among all metals excluding lithium and a molar ratio of lithium to transition metal exceeding about 1; and the non-aqueous electrolyte comprises a lithium salt, an organic solvent, and an additive, and the organic solvent comprises a first organic solvent and a second organic solvent, the first organic solvent comprises ethylene carbonate, the second organic solvent comprises diethyl carbonate and ethylmethyl carbonate, and the additive comprises a compound represented by the following chemical formula 1.
[0029] [Chemical Formula 1]
[0030]
[0031] In the above chemical formula 1, n is 1 or 2, L1 and L2 are each independently a direct bond or a substituted or unsubstituted alkylene group having 1 to 6 carbon atoms, R1 and R2 are each independently selected from a substituent represented by the following chemical formula 2, an alkyl group having 1 to 10 carbon atoms, an alkyl group having 1 to 10 carbon atoms substituted with at least one fluorine, an alkenyl group having 2 to 10 carbon atoms, an alkynyl group having 2 to 10 carbon atoms, a phosphate group, and a nitrile group, and at least one of R1 and R2 is a substituent represented by the following chemical formula 2,
[0032] [Chemical Formula 2]
[0033]
[0034] In the above chemical formula 2, m is 1 or 2, X1 and X2 are each independently -O- or -C(R 31 )(R 32 )-, but at least one of the above X1 and X2 is -O-, and R 31 Inland R 36 are each independently hydrogen, an alkyl group having 1 to 6 carbon atoms, -C(=O)-R4 or -R5-OC(=O)-R6, wherein R4 and R6 are each independently a substituted or unsubstituted alkyl group having 1 to 6 carbon atoms, an alkenyl group having 2 to 20 carbon atoms, an alkynyl group having 2 to 20 carbon atoms, or a substituted or unsubstituted aryl group having 6 to 20 carbon atoms, wherein R5 is a substituted or unsubstituted alkylene group having 1 to 6 carbon atoms, and the substituents of L1, L2, R4, R5 and R6 are each independently at least one selected from the group consisting of deuterium, -F, -Cl, -Br, -I, -CN, -NO2 and -SO3, and * is a position bonded to L1 or L2, but when both L1 and L2 are direct bonds, R1 and R2 are not CS-7 at the same time, and L1 and L2 are When both are methylene groups and n is 2, R1 and R2 are not CS-2 at the same time.
[0035] .
[0036]
[0037] The lithium secondary battery includes a positive electrode; a negative electrode; a separator; and a non-aqueous electrolyte. For example, the lithium secondary battery includes a positive electrode; a negative electrode facing the positive electrode; a separator interposed between the positive electrode and the negative electrode; and a non-aqueous electrolyte. The lithium secondary battery can be manufactured by housing an electrode assembly including the positive electrode; a negative electrode facing the positive electrode; and a separator interposed between the positive electrode and the negative electrode in a battery case, and then injecting a non-aqueous electrolyte.
[0038]
[0039] (1) Bipolar
[0040] The above positive electrode includes a positive electrode active material.
[0041] In one embodiment, the cathode active material comprises a lithium manganese-rich oxide. The lithium manganese-rich oxide comprises manganese in an amount of about 50 mol% or more among all metals excluding lithium, and the molar ratio of lithium to transition metal may exceed about 1.
[0042] Although the above-mentioned perlithium manganese-rich oxide is attracting attention as a next-generation high-capacity cathode active material, its use is limited due to the structural deterioration unique to the material. For example, when perlithium manganese-rich oxide is used as a cathode active material, there is a problem that an electrolyte side reaction occurs at the cathode interface, which significantly increases the amount of gas generated, such as carbon dioxide (CO2). In addition, during the initial activation of a lithium secondary battery containing perlithium manganese-rich oxide, the reactive oxygen decomposes and consumes the organic solvent (such as ethylene carbonate) contained in the non-aqueous electrolyte, thereby generating gaseous byproducts, which causes problems such as reduced life performance, increased resistance, and reduced safety. In addition, there is also a problem that manganese (Mn) is eluted to maintain the charge balance as reactive oxygen is decomposed during the charge / discharge process of a lithium secondary battery containing perlithium manganese-rich oxide. At this time, the eluted manganese is deposited on the negative electrode, causing the problem of destroying the SEI (Solid Electrolyte Interphase) film, and the reactive oxygen desorbed during the charge / discharge process continuously decomposes and consumes the organic solvent of the non-aqueous electrolyte, increasing the generation of gaseous by-products. This consumption of the non-aqueous electrolyte, structural collapse of the lithium manganese-rich oxide, and increase in gaseous by-products significantly reduce the life performance, resistance characteristics, and safety of lithium secondary batteries. Furthermore, these problems are further aggravated under high temperature and high voltage conditions.
[0043] In order to solve these problems, the lithium secondary battery according to the present invention is characterized in that, as described below, it includes ethylene carbonate, diethyl carbonate and ethyl methyl carbonate as organic solvents of a non-aqueous electrolyte, and the additive includes a compound represented by the above chemical formula 1. According to the present invention, by the combination of components of the above-described non-aqueous electrolyte, the amount of gas generated at the positive electrode interface including the perlithium manganese-rich oxide is significantly reduced, and the life performance of the negative electrode is improved, so that as a result, it is possible to implement a lithium secondary battery having superior capacity retention rate and gas generation reduction performance compared to a conventional lithium secondary battery. The lithium secondary battery of the present invention can have superior life performance and gas reduction performance, especially at high temperatures and high voltages.
[0044]
[0045] The above lithium manganese-rich oxide may include a compound represented by the following chemical formula X.
[0046] [chemical formula X]
[0047] Li 1+s [Ni t Co u Mn v M 1 w ]O 2+z
[0048] In the above chemical formula X, M 1is at least one selected from W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B and Mo, and 0.05≤s≤1, 0≤t≤0.5, 0≤u≤0.3, 0.5≤v<1.0, 0≤w≤0.2, 0≤z≤1. For example, in the chemical formula X, 0.05≤s≤1.0, 0.1≤t≤0.5, 0≤u≤0.1, 0.5≤v<1.0, 0≤w≤0.2, 0≤z≤1. Alternatively, in the chemical formula X, 0.10≤s≤0.50, 0.1≤t≤0.5, 0≤u≤0.1, 0.6≤v<1.0, 0≤w≤0.1, 0≤z≤0.50 may be satisfied.
[0049] In one embodiment, the lithium manganese-rich oxide may comprise a compound represented by the following chemical formula Y.
[0050] [Chemical formula Y]
[0051] X Li2MnO3·(1-X)Li[Ni 1-y-z-w Mn y Co z M 1 w ]O2
[0052] In the above chemical formula Y, M 1 is at least one selected from W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B, and Mo. In addition, in the chemical formula Y, 0.1≤X≤0.5, 0.5≤y<1, 0≤z≤0.3, 0≤w≤0.2 may be satisfied, for example, 0.2≤X≤0.5, 0.5≤y<1, 0≤z≤0.1, 0≤w≤0.2, or 0.3≤X≤0.5, 0.6≤y<1, 0≤z≤0.1, 0≤w≤0.2.
[0053]
[0054] The positive electrode may include a positive electrode current collector; and a positive electrode active material layer disposed on at least one surface of the positive electrode current collector. In this case, the positive electrode active material may be included in the positive electrode active material layer.
[0055] The positive electrode current collector is not particularly limited as long as it has high conductivity without causing chemical changes in the battery. For example, the positive electrode current collector may include at least one selected from the group consisting of copper, stainless steel, aluminum, nickel, titanium, calcined carbon, and an aluminum-cadmium alloy, or may include aluminum according to one embodiment.
[0056] The thickness of the above positive electrode collector may typically have a thickness of about 3 ㎛ to 500 ㎛.
[0057] The above-described positive electrode current collector may also form fine irregularities on its surface to enhance the bonding strength of the positive electrode active material. For example, the above-described positive electrode current collector may be used in various forms, such as a film, sheet, foil, net, porous body, foam, or non-woven fabric.
[0058]
[0059] The positive electrode active material layer may be disposed on at least one surface of the positive electrode current collector, for example, one surface or both surfaces of the positive electrode current collector.
[0060] The above-mentioned positive electrode active material may be included in the positive electrode active material layer at about 80 wt% to 99 wt%, for example, about 92 wt% to 98.5 wt%, taking into account sufficient capacity of the positive electrode active material.
[0061] Description of other positive electrode active materials is omitted as it has been described above.
[0062] The above positive electrode active material layer may further include a binder and / or a conductive material together with the positive electrode active material.
[0063] The above binder is a component that assists in the binding of the active material and the conductive material and the binding to the current collector, and includes at least one selected from the group consisting of, for example, polyvinylidene fluoride, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene terpolymer (EPDM), sulfonated EPDM, styrene-butadiene rubber, and fluororubber, or may include polyvinylidene fluoride according to one embodiment.
[0064] The above binder may be included in the positive electrode active material layer at about 1 wt% to 20 wt%, for example, about 1.2 wt% to 10 wt%, in order to sufficiently secure binding force between components such as the positive electrode active material.
[0065] The conductive material may be used to assist and improve conductivity in a secondary battery, and is not particularly limited as long as it has conductivity without causing chemical changes. For example, the positive electrode conductive material may include at least one selected from the group consisting of graphite such as natural graphite or artificial graphite; carbon black such as carbon black, acetylene black, Ketjen black, channel black, paneth black, lamp black, thermal black, etc.; conductive fibers such as carbon fibers or metal fibers; conductive tubes such as carbon nanotubes; fluorocarbons; metal powders such as aluminum or nickel powder; conductive whiskers such as zinc oxide or potassium titanate; conductive metal oxides such as titanium oxide; and polyphenylene derivatives, and according to one embodiment, in terms of improving conductivity, the positive electrode conductive material may include carbon nanotubes.
[0066] The above-mentioned conductive material may be included in the positive electrode active material layer in an amount of about 1 wt% to 20 wt%, for example, about 1.2 wt% to 10 wt%, in order to sufficiently secure electrical conductivity.
[0067] The thickness of the positive electrode active material layer may be about 30 µm to 400 µm, for example, about 40 µm to 110 µm.
[0068] The above positive electrode can be manufactured by coating a positive electrode slurry containing a positive electrode active material and optionally a binder, a conductive material, and a solvent for forming a positive electrode slurry on the positive electrode current collector, and then drying and rolling.
[0069] The solvent for forming the positive electrode slurry may include an organic solvent such as NMP (N-methyl-2-pyrrolidone). The solid content of the positive electrode slurry may be about 40 wt% to 90 wt%, for example, about 50 wt% to 80 wt%.
[0070]
[0071] (2) Cathode
[0072] The above cathode may be opposite to the above anode.
[0073] The above negative electrode includes a negative electrode active material.
[0074] The above negative electrode active material is a material capable of reversibly inserting / de-inserting lithium ions, and may include at least one selected from the group consisting of carbon-based active materials, (semi)metal-based active materials, and lithium metal, and for example, may include at least one selected from among carbon-based active materials and (semi)metal-based active materials.
[0075] The above carbon-based active material may include at least one selected from the group consisting of artificial graphite, natural graphite, hard carbon, soft carbon, carbon black, graphene, and fibrous carbon, and may include, for example, at least one selected from the group consisting of artificial graphite and natural graphite.
[0076] The average particle diameter (D) of the above carbon-based active material 50 ) may be about 10㎛ to 30㎛, for example, about 15㎛ to 25㎛, in order to ensure structural stability during charging and discharging and reduce side reactions with the electrolyte.
[0077] For example, the (semi)metal-based active material may include at least one selected from the group consisting of a (semi)metal, an alloy of a (semi)metal and lithium, an oxide of a (semi)metal, lithium titanium oxide (LTO), and lithium vanadium oxide.
[0078] The above (semi)metal may include at least one selected from the group consisting of Cu, Ni, Na, K, Rb, Cs, Fr, Be, Mg, Ca, Sr, Si, Sb, Pb, In, Zn, Ba, Ra, Ge, Al, V, Ti, and Sn.
[0079] The alloy of the above (semi-)metal and lithium may include an alloy of lithium and at least one (semi-)metal selected from the group consisting of Cu, Ni, Na, K, Rb, Cs, Fr, Be, Mg, Ca, Sr, Si, Sb, Pb, In, Zn, Ba, Ra, Ge, Al, V, Ti, and Sn.
[0080] The oxide of the above (semi-)metal may include at least one selected from the group consisting of Cu, Ni, Na, K, Rb, Cs, Fr, Be, Mg, Ca, Sr, Si, Sb, Pb, In, Zn, Ba, Ra, Ge, Al, V, Ti, and Sn.
[0081] In one embodiment, the (semi)metal-based active material may include a silicon-based active material.
[0082] The above silicon-based active material is SiO x It may include a compound represented by (0≤x<2). In the case of SiO2, since it does not react with lithium ions and thus cannot store lithium, x is selected to be within the above range not including 2, and according to one embodiment, the silicon-based active material may be SiO.
[0083] The average particle diameter (D) of the above silicon-based active material 50) may be about 1㎛ to 30㎛, for example, about 2㎛ to 15㎛, in order to reduce side reactions with the electrolyte while ensuring structural stability during charge and discharge.
[0084]
[0085] The above negative electrode may include a negative electrode current collector; and a negative electrode active material layer disposed on at least one surface of the negative electrode current collector. In this case, the negative electrode active material may be included in the negative electrode active material layer.
[0086] The above negative electrode current collector is not particularly limited as long as it has high conductivity without causing chemical changes in the battery. For example, the negative electrode current collector may be made of copper, stainless steel, aluminum, nickel, titanium, calcined carbon, copper or stainless steel surface-treated with carbon, nickel, titanium, silver, etc., or an aluminum-cadmium alloy.
[0087] The above negative electrode current collector may typically have a thickness of about 3 μm to 500 μm.
[0088] The above-described negative electrode current collector may have fine irregularities formed on its surface to enhance the bonding strength of the negative electrode active material. For example, the above-described negative electrode current collector may be used in various forms, such as a film, sheet, foil, net, porous body, foam, or non-woven fabric.
[0089]
[0090] The negative electrode active material layer may be disposed on at least one side of the negative electrode current collector, for example, one side or both sides of the negative electrode current collector.
[0091] The above negative active material may be included in the negative active material layer at about 60 wt% to 99 wt%, for example, about 75 wt% to 95 wt%.
[0092] Description of other positive electrode active materials is omitted as it has been described above.
[0093] The above negative electrode active material layer may further include a binder and / or a conductive material together with the negative electrode active material.
[0094] The above binder is used to improve the performance of the battery by improving the adhesion between the negative electrode active material layer and the negative electrode current collector, and may include, for example, at least one selected from the group consisting of polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinylidene fluoride (PVDF), polyacrylonitrile, polymethylmethacrylate, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, polyacrylic acid, ethylene-propylene-diene monomer (EPDM), sulfonated EPDM, styrene butadiene rubber (SBR), fluororubber, and materials in which hydrogens of these are substituted with Li, Na, Ca, etc., and may also include various copolymers thereof. May include.
[0095] The above binder may be included in the negative electrode active material layer in an amount of about 0.5 wt% to 10 wt%, for example, about 1 wt% to 5 wt%.
[0096] The conductive material is not particularly limited as long as it is conductive and does not cause a chemical change in the battery, and examples thereof include graphite such as natural graphite or artificial graphite; carbon black such as carbon black, acetylene black, Ketjen black, channel black, paneth black, lamp black, thermal black, and the like; conductive fibers such as carbon fibers or metal fibers; conductive tubes such as carbon nanotubes; fluorocarbons; metal powders such as aluminum or nickel powder; conductive whiskers such as zinc oxide or potassium titanate; conductive metal oxides such as titanium oxide; and conductive materials such as polyphenylene derivatives.
[0097] The above conductive material may be included in the negative electrode active material layer in an amount of about 0.5 wt% to 10 wt%, for example, about 1 wt% to 5 wt%.
[0098] The thickness of the negative electrode active material layer may be about 10 µm to 200 µm, for example, about 20 µm to 150 µm.
[0099] The above negative electrode can be manufactured by coating a negative electrode slurry including a negative electrode active material, a binder, a conductive material, and / or a solvent for forming a negative electrode slurry on at least one surface of a negative electrode current collector, and then drying and rolling.
[0100] The solvent for forming the negative electrode slurry may include at least one selected from the group consisting of distilled water, NMP (N-methyl-2-pyrrolidone), ethanol, methanol, and isopropyl alcohol, or may include distilled water according to one embodiment, in order to facilitate dispersion of the negative electrode active material, binder, and / or conductive material, for example. The solid content of the negative electrode slurry may be about 30 wt% to 80 wt%, for example, about 40 wt% to 70 wt%.
[0101]
[0102] (3) Membrane
[0103] The above separator may be interposed between the positive electrode and the negative electrode.
[0104] In addition, as the separator, a conventional porous polymer film that has been conventionally used as a separator, for example, a porous polymer film made of a polyolefin polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, and an ethylene / methacrylate copolymer, may be used alone or in a laminated manner, or a conventional porous nonwoven fabric, for example, a nonwoven fabric made of high-melting-point glass fiber, polyethylene terephthalate fiber, etc. may be used, but is not limited thereto. In addition, a coated separator containing a ceramic component or a polymer material may be used to secure heat resistance or mechanical strength, and may optionally be used in a single-layer or multi-layer structure.
[0105]
[0106] (4) Non-aqueous electrolyte
[0107] The above non-aqueous electrolyte comprises a lithium salt and an organic solvent.
[0108]
[0109] 1) Lithium salt
[0110] As the lithium salt used in the present invention, various lithium salts commonly used in non-aqueous electrolytes for lithium secondary batteries can be used without limitation. For example, the lithium salt may be Li as a cation. + , and the anion is F - , Cl - , Br - , I - , NO3 - , N(CN)2 - , BF4 - , ClO4 - , AlO4 - , AlCl4 - , PF6 - , SbF6 - , AsF6 - , B 10 Cl 10 - , BF2C2O4 -, BC4O8 - , PF4C2O4 - , PF2C4O8 - , (CF3)2PF4 - , (CF3)3PF3 - , (CF3)4PF2 - , (CF3)5PF - , (CF3)6P - , CF3SO3 - , C4F9SO3 - , CF3CF2SO3 - , (FSO2)2N - , CF3CF2(CF3)2CO - , (CF3SO2)2CH - , CH3SO3 - , CF3(CF2)7SO3 - , CF3CO2 - , CH3CO2 - , SCN - and (CF3CF2SO2)2N - It may include at least one selected from the group consisting of .
[0111] For example, the lithium salts include LiCl, LiBr, LiI, LiBF4, LiClO4, LiAlO4, LiAlCl4, LiPF6, LiSbF6, LiAsF6, LiB 10 Cl 10 , LiBOB (LiB(C2O4)2), LiCF3SO3, LiFSI (LiN(SO2F)2), LiCH3SO3, LiCF3CO2, LiCH3CO2, and LiBETI (LiN(SO2CF2CF3)2). For example, the lithium salt may include at least one selected from the group consisting of LiBF4, LiClO4, LiPF6, LiBOB (LiB(C2O4)2), LiCF3SO3, LiTFSI (LiN(SO2CF3)2), LiFSI ((LiN(SO2F)2), and LiBETI (LiN(SO2CF2CF3)2).
[0112] The lithium salt may be included in the non-aqueous electrolyte at a concentration of about 0.5 M to 5 M, for example, a concentration of about 0.8 M to 4 M, or a concentration of about 0.8 M to 2.0 M. When the concentration of the lithium salt satisfies the above range, the lithium ion yield (Li + The output characteristics of the battery can be improved by improving the transference number and the degree of dissociation of lithium ions.
[0113]
[0114] 2) Organic solvent
[0115] The organic solvent includes a first organic solvent and a second organic solvent.
[0116] The first organic solvent comprises ethylene carbonate.
[0117] The above ethylene carbonate is a high viscosity organic solvent with a high dielectric constant, and can function as an organic solvent that can easily dissociate lithium salts in the electrolyte.
[0118] The first organic solvent may further include, but is not limited to, at least one selected from the group consisting of fluoroethylene carbonate (FEC), propylene carbonate (PC), 1,2-butylene carbonate, 2,3-butylene carbonate, 1,2-pentylene carbonate, 2,3-pentylene carbonate, vinylene carbonate, γ-butyrolactone, γ-valerolactone, γ-caprolactone, σ-valerolactone, and ε-caprolactone, together with the ethylene carbonate.
[0119] The second organic solvent includes diethyl carbonate and ethylmethyl carbonate.
[0120] In the case of the lithium secondary battery of the present invention, by including diethyl carbonate as the second organic solvent, the oxidation stability of the non-aqueous electrolyte is improved, thereby enhancing the effect of reducing gas generation, and thus the life performance of the lithium secondary battery including the perlithium manganese-rich oxide can be significantly improved. On the other hand, when diethyl carbonate alone is used as a linear carbonate, there are problems such as a decrease in ionic conductivity, a decrease in electrolyte impregnation due to an increase in viscosity, and an increase in initial resistance, but these disadvantages can be offset by using ethyl methyl carbonate together, which has a relatively low viscosity and excellent ionic conductivity. When ethyl methyl carbonate is used, a better effect is exhibited compared to when using a linear carbonate other than ethyl methyl carbonate, such as dimethyl carbonate.
[0121] In addition, the present invention has an excellent capacity retention rate by using the first organic solvent (containing ethylene carbonate) and the second organic solvent (containing diethyl carbonate and ethyl methyl carbonate), and at the same time, it can prevent volume expansion of the cell by reducing the amount of gas generated. Meanwhile, in the present embodiment, a combination of diethyl carbonate and ethyl methyl carbonate was used as the second organic solvent, but it is not limited thereto, and when lithium manganese-rich oxide is used as the positive electrode component, the amount of carbon dioxide (CO2) generated can be reduced, and any solvent or combination of solvents can be applied as the second organic solvent as long as it has low reactivity with reactive oxygen that can be released from lithium manganese-rich oxide.
[0122] As described above, the effects of the present invention, such as the characteristic of reducing gas generation in a lithium secondary battery, are effects that are uniquely expressed when a lithium manganese-rich oxide is used as a cathode active material, but for limited purposes, the organic solvent of the present invention can be used in combination with other cathode active materials, such as high nickel-containing lithium nickel manganese cobalt transition metal oxides (e.g., NCM-based active materials containing Ni at 80 mol% or more among transition metals) in which generation of reactive oxygen and excessive dissolution of Mn are not major problems.
[0123] Meanwhile, the second organic solvent may further include another additional organic solvent together with the diethyl carbonate at a level that does not inhibit the aforementioned effect.
[0124] For example, the second organic solvent may further include at least one selected from the group consisting of dipropyl carbonate, methylpropyl carbonate, ethylpropyl carbonate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, and butyl propionate.
[0125] The volume ratio of the first organic solvent and the second organic solvent may be about 10:90 to 50:50, for example, about 15:85 to 40:60, or about 15:85 to 35:65, and when it is in the above range, it is possible to further improve the life performance of the positive / negative electrode while achieving high ion transfer characteristics and an appropriate level of viscosity of the non-aqueous electrolyte and reducing gas generation in the above-described lithium manganese-rich oxide.
[0126] Additionally, the organic solvent may comprise about 10% to 50% by volume of the ethylene carbonate, about 5% to 80% by volume of the diethyl carbonate, and about 5% to 80% by volume of the ethylmethyl carbonate; for example, it may comprise about 15% to 40% by volume of the ethylene carbonate, about 8% to 75% by volume of the diethyl carbonate, and about 8% to 75% by volume of the ethylmethyl carbonate; for example, it may comprise about 15% to 35% by volume of the ethylene carbonate, about 8% to 50% by volume of the diethyl carbonate, and about 30% to 75% by volume of the ethylmethyl carbonate. When within the above range, the life performance of the positive / negative electrodes can be further improved while achieving high ion transfer characteristics and an appropriate level of viscosity of the non-aqueous electrolyte and reducing gas generation from the aforementioned lithium manganese-rich oxide.
[0127] Meanwhile, the organic solvent may be used without limitation by adding organic solvents commonly used in non-aqueous electrolytes as needed. For example, the organic solvent may include at least one additional organic solvent from among an ether-based organic solvent, a glyme-based solvent, and a nitrile-based organic solvent.
[0128] As the above ether solvent, any one selected from the group consisting of dimethyl ether, diethyl ether, dipropyl ether, methyl ethyl ether, methyl propyl ether, ethyl propyl ether, 1,3-dioxolane (DOL), and 2,2-bis(trifluoromethyl)-1,3-dioxolane (TFDOL) or a mixture of two or more thereof may be used, but is not limited thereto.
[0129] The above glyme-based solvent has a high dielectric constant and low surface tension compared to linear carbonate-based organic solvents, and is a solvent with low reactivity with metals, and may include at least one selected from the group consisting of dimethoxyethane (glyme, DME), diethoxyethane, diglyme, tri-glyme, and tetra-glyme (TEGDME), but is not limited thereto.
[0130] The above nitrile solvent may be at least one selected from the group consisting of acetonitrile, propionitrile, butyronitrile, valeronitrile, caprylonitrile, heptanenitrile, cyclopentane carbonitrile, cyclohexane carbonitrile, 2-fluorobenzonitrile, 4-fluorobenzonitrile, difluorobenzonitrile, trifluorobenzonitrile, phenylacetonitrile, 2-fluorophenylacetonitrile, and 4-fluorophenylacetonitrile, but is not limited thereto.
[0131]
[0132] 3) Additives
[0133] The above non-aqueous electrolyte contains an additive.
[0134] The above additive includes a compound represented by the following chemical formula 1.
[0135] [Chemical Formula 1]
[0136]
[0137] In the above chemical formula 1, n is 1 or 2, L1 and L2 are each independently a direct bond or a substituted or unsubstituted alkylene group having 1 to 6 carbon atoms, R1 and R2 are each independently selected from a substituent represented by the following chemical formula 2, an alkyl group having 1 to 10 carbon atoms, an alkyl group having 1 to 10 carbon atoms substituted with at least one fluorine, an alkenyl group having 2 to 10 carbon atoms, an alkynyl group having 2 to 10 carbon atoms, a phosphate group, and a nitrile group, and at least one of R1 and R2 is a substituent represented by the following chemical formula 2,
[0138] [Chemical Formula 2]
[0139]
[0140] In the above chemical formula 2, m is 1 or 2, X1 and X2 are each independently -O- or -C(R 31 )(R 32 )-, but at least one of the above X1 and X2 is -O-, and R 31 Inland R 36 are each independently hydrogen, an alkyl group having 1 to 6 carbon atoms, -C(=O)-R4 or -R5-OC(=O)-R6, wherein R4 and R6 are each independently a substituted or unsubstituted alkyl group having 1 to 6 carbon atoms, an alkenyl group having 2 to 20 carbon atoms, an alkynyl group having 2 to 20 carbon atoms, or a substituted or unsubstituted aryl group having 6 to 20 carbon atoms, wherein R5 is a substituted or unsubstituted alkylene group having 1 to 6 carbon atoms, and the substituents of L1, L2, R4, R5 and R6 are each independently at least one selected from the group consisting of deuterium, -F, -Cl, -Br, -I, -CN, -NO2 and -SO3, and * is a position bonded to L1 or L2, but when both L1 and L2 are direct bonds, R1 and R2 are not CS-7 at the same time, and L1 and L2 are When both are methylene groups and n is 2, R1 and R2 are not CS-2 at the same time.
[0141] .
[0142]
[0143] The compound represented by the above chemical formula 1 is characterized by including a sulfur oxide structure at the center, while at least one of both terminals has a cyclic sulfur oxide structure. By adopting this chemical structure, when applied as a non-aqueous electrolyte additive, it can induce stable formation of anions, and further, it can form a stable SEI layer. For example, since the compound represented by the above chemical formula 1 has a lower consumption rate in a secondary battery compared to other cyclic sulfur oxides (e.g., 1,3-propanesultone), it remains during the operation of the secondary battery and has the effect of continuously improving the high-temperature durability of the secondary battery.
[0144] In this respect, the compound represented by the above chemical formula 1 can continuously function to form a stable and strong film of the positive electrode when using lithium manganese-rich oxide, which generates a lot of gas at high temperature and high voltage and has an extreme degree of reactive oxygen or manganese release, as a positive electrode active material, and thus can assist in improving the high-temperature durability, gas reduction, and life performance of a secondary battery using lithium manganese-rich oxide. For example, the high-temperature life performance, durability, and gas reduction improvement effects of the secondary battery according to the present invention are realized by the combined use of the organic solvent and additive of the non-aqueous electrolyte described above.
[0145] In addition, the effect of the present invention is an effect expressed in lithium manganese-rich oxide, and in other positive electrode active materials such as lithium nickel manganese cobalt transition metal oxide containing high nickel (for example, NCM active material containing Ni in an amount of about 80 mol% or more among transition metals), generation of reactive oxygen, excessive dissolution of Mn, etc. do not cause problems, so even if the organic solvent described above is used in combination, the intended effect is not expressed. Rather, when a non-aqueous electrolyte containing the organic solvent and additive described above is applied to a positive electrode active material other than lithium manganese-rich oxide, the non-aqueous electrolyte components may act as resistance, which may cause a problem of lowering the life performance.
[0146] In the above chemical formula 1, R1 and R2 are each independently selected from a substituent represented by the following chemical formula 2, an alkyl group having 1 to 10 carbon atoms, an alkyl group having 1 to 10 carbon atoms substituted with at least one fluorine, an alkenyl group having 2 to 10 carbon atoms, an alkynyl group having 2 to 10 carbon atoms, a phosphate group, and a nitrile group, and at least one of R1 and R2 is a substituent represented by the following chemical formula 2. For example, in the above chemical formula 1, both R1 and R2 may be substituents represented by the above chemical formula 2.
[0147] The above alkyl group having 1 to 10 carbon atoms may be selected from, for example, alkyl groups having 1 to 3 carbon atoms, i.e., a methyl group, an ethyl group, and a propyl group.
[0148] The above alkyl group having 1 to 10 carbon atoms substituted with one or more fluorines may be specifically an alkyl group having 1 to 3 carbon atoms substituted with one or more fluorines, and may be selected from, for example, *-CF3, *-CH2CF3, *-CF2CF3, *-CH2CH2CF3, *-CH2CF2CF3, and *-CF2CF2CF3. In the present invention, the symbol “*” may denote a binding site.
[0149] In addition, the substituent represented by the above chemical formula 2 may be selected from the group consisting of CS-1 to CS-15 below:
[0150]
[0151]
[0152]
[0153] _
[0154]
[0155] .
[0156]
[0157] The substituent structures CS-1 to CS-15 listed above are preferred examples of the substituents represented by Chemical Formula 2 or R1 and R2 of Chemical Formula 1, and when the substituents of CS-1 to CS-15 are applied as R1 and R2 of Chemical Formula 1, the overall compound has excellent structural stability while also being able to smoothly perform its function as a non-aqueous electrolyte additive. For example, it may be preferable in terms of structural stability and ease of synthesis that the R1 and R2 are each independently selected from the group consisting of CS-1, CS-2, CS-5, CS-8, CS-10, and CS-11.
[0158] Meanwhile, in the compound represented by the chemical formula 1 of the present invention, if both L1 and L2 are direct bonds and R1 and R2 are CS-7, or if both L1 and L2 are methylene groups and n is 2 and R1 and R2 are both CS-2, the structural stability of the compound itself is low and it can be easily decomposed, and accordingly, the synthesis of the compound itself can be difficult. For example, compounds that satisfy the above conditions have the disadvantage that the R1 and R2 structures having a ring form are easily decomposed during the synthesis process, and even if the compound is ultimately synthesized, it can be easily decomposed during the storage process, and the synthesis yield is also significantly low. Therefore, the present invention excludes compounds in which both L1 and L2 are direct bonds and R1 and R2 are CS-7, and in which n is 2 and R1 and R2 are both CS-2.
[0159] In the compound represented by the above chemical formula 1, L1 and L2 can each independently be a direct bond, a methylene group, or an ethylene group, and for example, can be a methylene group. When L1 and L2 are methylene groups, the synthesis of the compound is easy, and the decomposition of the compound after synthesis can be suppressed.
[0160] It may be particularly preferable that the compound represented by the above chemical formula 1 comprises at least one compound selected from the group consisting of compounds A to U below, for example, at least one compound selected from the group consisting of compound A, compound F, and compound J below:
[0161]
[0162]
[0163]
[0164]
[0165]
[0166]
[0167]
[0168]
[0169]
[0170]
[0171]
[0172]
[0173]
[0174]
[0175]
[0176]
[0177]
[0178]
[0179]
[0180]
[0181] .
[0182]
[0183] When the compound represented by the above chemical formula 1 has the structure described above, it has the advantage of being able to form a stable SEI layer with low resistance even with a smaller amount compared to the additives used previously.
[0184] The compound represented by the above chemical formula 1 may be included in the non-aqueous electrolyte at about 0.01 wt% to 10 wt%, for example, about 0.1 wt% to 5 wt%, about 0.2 wt% to 3 wt%, about 0.5 wt% to 2 wt%, or about 0.7 wt% to 1.5 wt%. When it is within the above range, it is preferable in that the effect of improving the high-temperature durability of the secondary battery described above is exhibited while preventing an increase in resistance due to excessive use of additives.
[0185] Meanwhile, in addition to the compound represented by the above-mentioned chemical formula 1, any material that can continuously function to form a stable and solid film of the positive electrode when using lithium manganese-rich oxide, which generates a lot of gas at high temperature and high voltage and has an extreme degree of reactive oxygen or manganese release as a positive electrode active material, and can help improve the high-temperature durability, gas reduction, and life performance of a secondary battery using lithium manganese-rich oxide, can be selected and used.
[0186] The above non-aqueous electrolyte may further include an additional additive along with the compound represented by the above chemical formula 1. The additional additive may be included in the non-aqueous electrolyte to prevent gas generation due to electrolyte side reactions by strengthening the SEI film of the positive / negative electrode, to prevent the non-aqueous electrolyte from being decomposed in a high-power environment and causing anode collapse, or to provide low-temperature high-rate discharge characteristics, high-temperature stability, overcharge prevention, and suppression of battery expansion at high temperatures.
[0187] For example, the additional additive may include at least one selected from the group consisting of a sulfate compound, a phosphate compound, a borate compound, a nitrile compound, a benzene compound, and a lithium salt compound.
[0188] The above sulfate compound may include ethylene sulfate (Esa), trimethylene sulfate (TMS), or methyl trimethylene sulfate (MTMS), and may be included in an amount of about 5 wt% or less based on the total weight of the electrolyte.
[0189] The above phosphate compound may include at least one compound selected from the group consisting of lithium difluoro(bisoxalato)phosphate, lithium difluorophosphate, tetramethyl trimethyl silyl phosphate, trimethyl silyl phosphite, tris(2,2,2-trifluoroethyl)phosphate, and tris(trifluoroethyl) phosphite, and may be included in an amount of about 5 wt% or less based on the total weight of the electrolyte.
[0190] The above borate compounds include tetraphenylborate and lithium oxalyldifluoroborate, and may be included in an amount of about 5 wt% or less based on the total weight of the electrolyte.
[0191] The above nitrile compound is a nitrile compound other than decanenitrile (DN) and 1,4-dicyano-2-butene (DCB), and representative examples thereof include at least one compound selected from the group consisting of succinonitrile, adiponitrile, acetonitrile, propionitrile, butyronitrile, valeronitrile, caprylonitrile, heptanenitrile, cyclopentane carbonitrile, cyclohexane carbonitrile, 2-fluorobenzonitrile, 4-fluorobenzonitrile, difluorobenzonitrile, trifluorobenzonitrile, phenylacetonitrile, 2-fluorophenylacetonitrile, and 4-fluorophenylacetonitrile and 1,3,6-hexanetricarbonitrile.
[0192] The nitrile compound may be present in an amount of about 5 wt% to 8 wt%, for example, about 6 wt% to 8 wt%, based on the total weight of the non-aqueous electrolyte. If the content of the nitrile compound in the electrolyte exceeds 8 wt%, the resistance may increase due to an increase in the film formed on the electrode surface, which may deteriorate battery performance.
[0193] The benzene compound may include fluorobenzene, the amine compound may include triethanolamine or ethylenediamine, and the silane compound may include tetravinylsilane.
[0194] The lithium salt-based compound is a compound different from the lithium salt included in the non-aqueous electrolyte, and may include at least one compound selected from the group consisting of LiPO2F2, LiODFB, LiBOB (lithium bisoxalatoborate (LiB(C2O4)2) and LiBF4), and may be included in an amount of about 5 wt% or less based on the total weight of the electrolyte.
[0195] For example, the additional additive may include at least one selected from the group consisting of coumarine, vinylene carbonate, vinyl ethylene carbonate, fluoroethylene carbonate, propane sultone, propene sultone, succinonitrile, adiponitrile, ethylene sulfate, lithium difluoro phosphate (LiDFP), lithium tetrafluoroborate (LiBF4), lithium difluoro(oxalato)borate (LiODFB), lithium bis-(oxalato)borate (LiBOB), 3-trimethoxysilanyl-propyl-N-aniline (TMSPa), Tris(trimethylsilyl) Phosphite (TMSPi), and a compound represented by the following chemical formula 3.
[0196] [Chemical Formula 3]
[0197]
[0198] The above additive may include, for example, at least one selected from the group consisting of vinylene carbonate, propane sultone, ethylene sulfate, LiDFP, LiBF4, and a compound represented by the above chemical formula 1.
[0199] The above additive may be included in the non-aqueous electrolyte in an amount of about 0.1 wt% to 15 wt%.
[0200] The above additional additive may be included in the non-aqueous electrolyte in an amount of about 0.1 wt% to 15 wt%.
[0201] There is no particular limitation on the external shape of the lithium secondary battery of the present invention, but it may be a cylindrical shape using a can, a square shape, a pouch shape, or a coin shape.
[0202] Hereinafter, the present invention will be described in more detail through examples. However, the following examples are merely illustrative and serve to aid understanding of the present invention and do not limit its scope. It will be apparent to those skilled in the art that various modifications and variations are possible within the scope and technical spirit of this disclosure, and such modifications and variations are naturally within the scope of the appended claims.
[0203]
[0204] Examples and Comparative Examples
[0205] Example 1
[0206] (Manufacture of non-aqueous electrolyte)
[0207] As an organic solvent, a mixture of ethylene carbonate, diethyl carbonate, and ethyl methyl carbonate in a volume ratio of 20:10:70 was used.
[0208] A non-aqueous electrolyte was prepared by adding LiPF6 as a lithium salt to the organic solvent, the compound A as an additive, propane sultone (PS), ethylene sulfate (ESa), LiDFP, LiBF4 as additional additives, and the compound represented by the chemical formula 3.
[0209] The above LiPF6 was included in the non-aqueous electrolyte at a molar concentration of 1.2 M.
[0210] The above compound A was included in the non-aqueous electrolyte at a content of 1 wt%.
[0211] Additionally, the non-aqueous electrolyte contained 0.5 wt% of vinylene carbonate, 0.8 wt% of propane sultone, 1.0 wt% of ethylene sulfate, 1.0 wt% of LiDFP, 0.5 wt% of LiBF4, and 0.1 wt% of the compound represented by the chemical formula 1.
[0212]
[0213] (Lithium secondary battery manufacturing)
[0214] Cathode active material (Li 1.3 [Ni 0.35 Mn 0.65 ]O 2.33 , lithium manganese-rich oxide): conductive material (carbon nanotube): binder (PVdF) were added to the solvent N-methyl-2-pyrrolidone (NMP) in a weight ratio of 97.4:0.6:2.0 to prepare a positive electrode mixture slurry (solid content 48 wt%). The positive electrode mixture slurry was applied to one surface of a positive electrode current collector (Al thin film) having a thickness of 12 μm, and dried and roll pressed to prepare a positive electrode.
[0215] A negative electrode mixture slurry (solid content 70 wt%) was prepared by adding a negative electrode active material (mixture of artificial graphite, natural graphite, and SiO), a conductive agent (carbon black), and a binder (PVdF) to distilled water as a solvent in a weight ratio of 95.7:1.0:3.3. The negative electrode mixture slurry was applied to one surface of an 8 μm thick negative electrode current collector (Cu thin film), and drying and roll pressing were performed to prepare a negative electrode.
[0216] A polyethylene porous film separator was interposed between the positive and negative electrodes manufactured above in a dry room, and then the non-aqueous electrolyte manufactured above was injected to manufacture a secondary battery.
[0217]
[0218] Example 2
[0219] A lithium secondary battery was manufactured in the same manner as in Example 1, except that the compound A was added to the non-aqueous electrolyte in an amount of 0.5 wt% instead of 1 wt%. That is, in the case of Example 2, a lithium secondary battery was manufactured using ethylene carbonate, diethyl carbonate, and ethyl methyl carbonate as organic solvents and using a different amount of the compound A used as an additive from Example 1.
[0220]
[0221] Example 3
[0222] A lithium secondary battery was manufactured in the same manner as in Example 1, except that the compound A was added to the non-aqueous electrolyte in an amount of 2.0 wt% instead of 1 wt%. That is, in Example 3, a lithium secondary battery was manufactured using ethylene carbonate, diethyl carbonate, and ethyl methyl carbonate as organic solvents and using a different amount of the compound A as an additive from Examples 1 and 2.
[0223]
[0224] Example 4
[0225] A lithium secondary battery was manufactured in the same manner as in Example 1, except that Compound S was used instead of Compound A. That is, in Example 4, a lithium secondary battery was manufactured using ethylene carbonate, diethyl carbonate, and ethyl methyl carbonate as organic solvents and Compound S instead of Compound A of Example 1 as an additive.
[0226]
[0227] Comparative Example 1
[0228] A lithium secondary battery was manufactured in the same manner as in Example 1, except that the compound A was not added to the non-aqueous electrolyte. That is, in the case of Example 1, the compound A was used as an additive in addition to ethylene carbonate, diethyl carbonate, and ethyl methyl carbonate as organic solvents, whereas in the case of Comparative Example 1, a lithium secondary battery was manufactured without using any additives other than these three organic solvents.
[0229]
[0230] Comparative Example 2
[0231] A lithium secondary battery was manufactured in the same manner as in Example 1, except that 1,3-propane sultone (PS) was used instead of the compound A in the non-aqueous electrolyte. That is, in the case of Comparative Example 2, in addition to using ethylene carbonate, diethyl carbonate, and ethyl methyl carbonate as organic solvents, a lithium secondary battery was manufactured using 1,3-propane sultone (PS) as an additive instead of the compound A.
[0232]
[0233] Comparative Example 3
[0234] A lithium secondary battery was manufactured in the same manner as in Example 1, except that a mixture of ethylene carbonate and ethyl methyl carbonate in a volume ratio of 20:80 was used as the organic solvent of the non-aqueous electrolyte. That is, in the case of Comparative Example 3, a lithium secondary battery was manufactured using only two types of organic solvents, ethylene carbonate and ethyl methyl carbonate, and the compound A as an additive.
[0235]
[0236] Comparative Example 4
[0237] A lithium secondary battery was manufactured in the same manner as in Example 1, except that a mixture of ethylene carbonate and diethyl carbonate in a volume ratio of 20:80 was used as the organic solvent of the non-aqueous electrolyte. That is, in the case of Comparative Example 4, a lithium secondary battery was manufactured using only two types of organic solvents, ethylene carbonate and diethyl carbonate, and the compound A as an additive.
[0238]
[0239] Comparative Example 5
[0240] A lithium secondary battery was manufactured in the same manner as in Example 1, except that a mixture of ethylene carbonate, dimethyl carbonate, and ethyl methyl carbonate in a volume ratio of 20:10:70 was used as the organic solvent of the non-aqueous electrolyte. That is, in the case of Comparative Example 5, a lithium secondary battery was manufactured using dimethyl carbonate instead of diethyl carbonate among the three organic solvents of Example 1.
[0241]
[0242] Experimental example
[0243] Experimental Example 1: Evaluation of High-Temperature Cycle Charge-Discharge Performance
[0244] The lithium secondary batteries manufactured in Examples 1 to 4 and Comparative Examples 1 to 5 above were charged to 4.35 V, 1 / 40 C using an electrochemical charger / discharger at 45°C under CC / CV, 0.33 C conditions, and then discharged to 2.0 V under CC, 0.33 C conditions, which constituted one cycle, and 200 cycles of charge and discharge were performed.
[0245]
[0246] Experimental Example 1-A: Capacity Retention Rate Evaluation
[0247] The capacity retention rate is calculated using the formula below, and the results are shown in Table 1 below.
[0248]
[0249] Capacity retention rate (%) = {(discharge capacity after 200 cycles / discharge capacity after 1 cycle)} × 100
[0250]
[0251] Experimental Example 1-B: Resistance Increase Rate Evaluation
[0252] At this time, after one cycle of charge and discharge, the discharge capacity after one cycle was measured using an electrochemical charger and discharger, the SOC (State of Charge) was adjusted to 50%, and then a 2.5C pulse was applied for 10 seconds, and the initial resistance was calculated through the difference between the voltage before and after the pulse was applied.
[0253] After 200 cycles of charge and discharge, the resistance after 200 cycles was calculated using the same method as above, and the resistance increase rate was calculated using the equation below, and the results are shown in Table 1 below.
[0254]
[0255] Resistance increase rate (%) = (Resistance after 200 cycles - Initial resistance) / Initial resistance × 100
[0256]
[0257] Experimental Example 1-A Experimental Example 1-B Capacity retention rate (%, 45℃, 200 th Cycle) Resistance increase rate (%, 45℃, 200 th Cycle) Example 189.670.1 Example 289.871.9 Example 388.473.6 Example 488.573.6 Comparative Example 187.781.4 Comparative Example 288.177.5 Comparative Example 388.275.8 Comparative Example 487.378.6 Comparative Example 586.983.3
[0258]
[0259] Referring to Table 1, it can be confirmed that the lithium secondary batteries of Examples 1 to 4, which are lithium secondary batteries in which a non-aqueous electrolyte according to the present invention and a positive electrode including a lithium manganese-rich oxide are combined, have a higher capacity retention rate and a lower resistance increase rate during high-temperature cycle charge and discharge than the lithium secondary batteries of Comparative Examples 1 to 5, which do not have such a combination.
[0260]
[0261] Experimental Example 2: Evaluation of High-Temperature Storage Performance
[0262] The lithium secondary batteries manufactured in Examples 1 to 5 and Comparative Examples 1 to 5 above were charged to 4.35 V, 1 / 40 C under CC / CV, 0.33 C conditions at 25°C, and then discharged to 2.0 V under CC, 0.33 C conditions to perform initial charge / discharge. Afterwards, they were charged to 4.35 V, 1 / 40 C under CC / CV, 0.33 C conditions at 25°C, and then stored at 60°C for 8 weeks.
[0263]
[0264] Experimental Example 2-A: Capacity Retention Rate Evaluation
[0265] After 8 weeks of storage, the lithium secondary battery was charged to 4.35 V, 1 / 40 C under CC / CV, 0.33 C conditions at 25°C, and then discharged to 2.0 V under CC, 0.33 C conditions to measure the capacity at discharge.
[0266] The capacity retention rate was evaluated according to the following formula, and the results are shown in Table 2 below.
[0267]
[0268] Capacity retention rate (%) = (Discharge capacity after 8 weeks of storage / Initial discharge capacity) × 100
[0269]
[0270] Experimental Example 2-B: Resistance Increase Rate Evaluation
[0271] After the initial charge and discharge above, the capacity was checked at room temperature, and then charged to 50% of SOC based on the discharge capacity, discharged for 10 seconds with a current of 2.5 C, and the resistance was measured based on the difference in voltage drop at this time, which was used as the initial resistance. After 8 weeks of storage at 60°C, the resistance was measured using the same method, which was used as the final resistance, and the resistance increase rate was calculated using the following formula. The results are shown in Table 2 below.
[0272]
[0273] Resistance increase rate (%) = (final resistance - initial resistance) / (initial resistance) × 100
[0274]
[0275] Experimental Example 2-A Experimental Example 2-B Capacity retention rate (%, 60℃, 8 weeks storage) Resistance increase rate (%, 60℃, 8 weeks storage) Example 191.7 4.3 Example 290.4 8.9 Example 392.2 3.1 Example 488.4 16.4 Comparative Example 166.7 58.3 Comparative Example 282.8 27.5 Comparative Example 381.2 36.0 Comparative Example 483.5 38.7 Comparative Example 573.4 4.8
[0276]
[0277] Referring to Table 2, it can be confirmed that the lithium secondary batteries of Examples 1 to 4, which are lithium secondary batteries in which a non-aqueous electrolyte according to the present invention and a positive electrode including a lithium manganese-rich oxide are combined, have a higher capacity retention rate and a lower resistance increase rate during high-temperature cycle charge and discharge than the lithium secondary batteries of Comparative Examples 1 to 5, which do not have such a combination.
[0278]
[0279] Reference example
[0280] Reference Example 1
[0281] (1) Preparation of non-aqueous electrolyte
[0282] A non-aqueous electrolyte was prepared using the same method as in Example 1.
[0283]
[0284] (2) Manufacturing of lithium secondary batteries
[0285] Cathode active material (LiNi) 0.85 Co 0.05 Mn 0.07 Al 0.03 O2): Conductive agent (carbon nanotube): Binder (polyvinylidene fluoride) was added to N-methyl-2-pyrrolidone (NMP) as a solvent in a weight ratio of 98.0:0.7:1.3 to prepare a positive electrode mixture slurry (solid content 76.5 wt%). The positive electrode mixture slurry was applied to one surface of a positive electrode current collector (Al thin film) having a thickness of 12 ㎛, and dried and roll pressed to prepare a positive electrode. That is, in Reference Example 1, a positive electrode was prepared using a different type of positive electrode active material from the aforementioned Example 1, for example, a high-nickel-containing lithium nickel cobalt manganese oxide, as a positive electrode active material.
[0286] A negative electrode mixture slurry (solid content 50 wt%) was prepared by adding a negative electrode active material (artificial graphite), a conductive agent (carbon black), and a binder (styrene-butadiene rubber) to distilled water as a solvent in a weight ratio of 96.5:1.5:2.0. The negative electrode mixture slurry was applied to one surface of an 8 ㎛ thick negative electrode current collector (Cu thin film), and drying and roll pressing were performed to prepare a negative electrode.
[0287] A polyethylene porous film separator was interposed between the positive and negative electrodes manufactured above in a dry room, and then the non-aqueous electrolyte manufactured above was injected to manufacture a secondary battery.
[0288]
[0289] Reference Example 2
[0290] A lithium secondary battery was manufactured in the same manner as in Reference Example 1, except that the non-aqueous electrolyte manufactured in Comparative Example 1 was used instead of the non-aqueous electrolyte manufactured in Example 1.
[0291]
[0292] Reference Experimental Example 1: Evaluation of High-Temperature Cycle Charge-Discharge Performance
[0293] The lithium secondary batteries of Reference Examples 1 and 2 manufactured above were charged to 4.2 V, 1 / 40 C using an electrochemical charger / discharger at 45°C under CC / CV, 0.33 C conditions, and discharged to 2.5 V at 0.33 C, which constituted one cycle, and 200 cycles of charge / discharge were performed.
[0294]
[0295] Reference Experimental Example 1-A: Capacity Retention Rate Evaluation
[0296] The capacity retention rate is calculated using the formula below, and the results are shown in Table 3 below.
[0297]
[0298] Capacity retention rate (%) = {(discharge capacity after 200 cycles / discharge capacity after 1 cycle)} × 100
[0299]
[0300] Reference Experimental Example 1-B: Resistance Increase Rate Evaluation
[0301] At this time, after one cycle of charge and discharge, the discharge capacity after one cycle was measured using an electrochemical charger and discharger, the SOC was adjusted to 50%, and then a 2.5C pulse was applied for 10 seconds, and the initial resistance was calculated through the difference between the voltage before and after the pulse was applied.
[0302] After 200 cycles of charge and discharge, the resistance after 200 cycles was calculated using the same method as above, and the resistance increase rate was calculated using the equation below, and the results are shown in Table 3 below.
[0303]
[0304] Resistance increase rate (%) = (Resistance after 200 cycles - Initial resistance) / Initial resistance × 100
[0305]
[0306] Reference Experimental Example 1-A Reference Experimental Example 1-B Capacity retention rate (%, 45℃, 200 th Cycle) Resistance increase rate (%, 45℃, 200 th Cycle) Reference Example 194.18.7 Reference Example 294.37.5
[0307]
[0308] Referring to Table 3, in the case of Reference Example 1 using a high-nickel lithium nickel cobalt manganese oxide rather than a perlithium manganese-rich oxide, it can be seen that the effect of improving the cycle charge / discharge performance at high temperatures is limited even when the same non-aqueous electrolyte as the non-aqueous electrolyte according to Example 1 is used. Rather, in the case of Reference Example 1, since Compound A was used as a non-aqueous electrolyte additive, problems such as a decrease in capacity retention and an increase in resistance occurred compared to Reference Example 2 where Compound A was not used. Through this, it can be understood that the non-aqueous electrolyte according to the present invention exhibits a unique effect when a perlithium manganese-rich oxide is used as a positive electrode active material.
[0309]
[0310] Reference Experimental Example 2: Evaluation of High-Temperature Storage Performance
[0311] The lithium secondary batteries of Reference Examples 1 and 2 manufactured above were charged to 4.2 V, 1 / 40 C using an electrochemical charger / discharger at 25°C under CC / CV, 0.33C conditions, and discharged to 2.5 V at 0.33C to perform initial charging / discharging. Afterwards, they were charged to 4.2 V, 1 / 40 C under CC / CV, 0.33C conditions at 25°C, and then stored at 60°C for 8 weeks.
[0312]
[0313] Reference Experimental Example 2-A: Capacity Retention Rate Evaluation
[0314] After 8 weeks of storage, the lithium secondary battery was charged to 4.2 V, 1 / 40 C under CC / CV, 0.33 C conditions at 25°C, and discharged to 2.5 V at 0.33 C to measure the capacity at discharge.
[0315] The capacity retention rate was evaluated according to the following formula, and the results are shown in Table 4 below.
[0316]
[0317] Capacity retention rate (%) = (Discharge capacity after 8 weeks of storage / Initial discharge capacity) × 100
[0318]
[0319] Reference Experimental Example 2-B: Resistance Increase Rate Evaluation
[0320] After the initial charge and discharge above, the capacity was checked at room temperature, and then charged to 50% of SOC based on the discharge capacity, discharged for 10 seconds with a current of 2.5 C, and the resistance was measured based on the difference in voltage drop at this time, which was used as the initial resistance. After 8 weeks of storage at 60°C, the resistance was measured using the same method, which was used as the final resistance, and the resistance increase rate was calculated using the following formula. The results are shown in Table 4 below.
[0321]
[0322] Resistance increase rate (%) = (final resistance - initial resistance) / (initial resistance) × 100
[0323]
[0324] Reference Experimental Example 2-A Reference Experimental Example 2-B Capacity Retention Rate (%, 60℃, 8 weeks storage) Resistance Increase Rate (%, 60℃, 8 weeks storage) Reference Example 196.85.2 Reference Example 296.84.6
[0325]
[0326] Referring to Table 4, in the case of Reference Example 1, which used a high-nickel-containing lithium nickel cobalt manganese oxide rather than a lithium manganese-rich oxide, it can be seen that the effect of improving the high-temperature storage performance was limited even when the same non-aqueous electrolyte as the non-aqueous electrolyte according to Example 1 was used. Rather, in the case of Reference Example 1, the use of Compound A as a non-aqueous electrolyte additive resulted in a problem of increased resistance compared to Reference Example 2, which did not use it. Through this, it can be understood that the non-aqueous electrolyte according to the present invention exhibits a unique effect when a lithium manganese-rich oxide is used as a positive electrode active material.
[0327] While the present invention has been described above with reference to preferred embodiments, it will be understood by those skilled in the art or those with ordinary knowledge in the art that various modifications and changes can be made to the present invention without departing from the spirit and technical scope of the present invention as set forth in the claims below. Accordingly, the technical scope of the present invention should not be limited to the contents described in the detailed description of the specification, but should be defined by the claims.
Claims
1. Containing a positive electrode; a negative electrode; a separator interposed between the positive electrode and the negative electrode; and a non-aqueous electrolyte; The above positive electrode includes a positive electrode active material, The above cathode active material comprises a lithium manganese-rich oxide containing Mn at 50 mol% or more among all metals excluding lithium, and a molar ratio of lithium to transition metal exceeding 1, The above non-aqueous electrolyte comprises a lithium salt, an organic solvent and an additive, The organic solvent comprises a first organic solvent and a second organic solvent, The first organic solvent comprises ethylene carbonate, The second organic solvent comprises diethyl carbonate and ethyl methyl carbonate, The above additive is a lithium secondary battery comprising a compound represented by the following chemical formula 1: [Chemical Formula 1] In the above chemical formula 1, n is 1 or 2, L1 and L2 are each independently a direct bond or a substituted or unsubstituted alkylene group having 1 to 6 carbon atoms, R1 and R2 are each independently selected from a substituent represented by the following chemical formula 2, an alkyl group having 1 to 10 carbon atoms, an alkyl group having 1 to 10 carbon atoms substituted with at least one fluorine, an alkenyl group having 2 to 10 carbon atoms, an alkynyl group having 2 to 10 carbon atoms, a phosphate group, and a nitrile group, At least one of R1 and R2 is a substituent represented by the following chemical formula 2, [Chemical Formula 2] In the above chemical formula 2, m is 1 or 2, X1 and X2 are each independently -O- or -C(R 31 )(R 32 )-but at least one of the above X1 and X2 is -O-, R 31 Inland R 36 are each independently hydrogen, an alkyl group having 1 to 6 carbon atoms, -C(=O)-R4 or -R5-OC(=O)-R6, The above R4 and R6 are each independently a substituted or unsubstituted alkyl group having 1 to 6 carbon atoms, an alkenyl group having 2 to 20 carbon atoms, an alkynyl group having 2 to 20 carbon atoms, or a substituted or unsubstituted aryl group having 6 to 20 carbon atoms, The above R5 is a substituted or unsubstituted alkylene group having 1 to 6 carbon atoms, The substituents of the above L1, L2, R4, R5 and R6 are each independently at least one selected from the group consisting of deuterium, -F, -Cl, -Br, -I, -CN, -NO2 and -SO3, * is the position where it binds to L1 or L2, If both L1 and L2 are direct bonds, then R1 and R2 are not CS-7 at the same time, When L1 and L2 are both methylene groups and n is 2, R1 and R2 are not CS-2 at the same time. .
2. In claim 1, The lithium manganese-rich oxide is a lithium secondary battery having a compound represented by the following chemical formula X: [chemical formula X] Li 1+s [Ni t Co u Mr v M 1 w ]O 2+z In the above chemical formula X, M 1 is at least one selected from W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B and Mo, 0.05≤s≤1, 0≤t≤0.5, 0≤u≤0.3, 0.5≤v<1.0, 0≤w≤0.2, 0≤z≤1.
3. In claim 1, A lithium secondary battery wherein the volume ratio of the first organic solvent and the second organic solvent is 10:90 to 50:
50.
4. In claim 1, A lithium secondary battery wherein the substituent represented by the above chemical formula 2 is selected from the group consisting of CS-1 to CS-15: _ .
5. In claim 4, A lithium secondary battery wherein the above R1 and R2 are each independently selected from the group consisting of CS-1, CS-2, CS-5, CS-8, CS-10, and CS-11.
6. In claim 1, A lithium secondary battery in which the above L1 and L2 are methylene groups.
7. In claim 1, A lithium secondary battery comprising at least one compound selected from the group consisting of compounds A to U, wherein the compound represented by the above chemical formula 1: .
8. In claim 1, A lithium secondary battery, wherein the compound represented by the above chemical formula 1 is included in the non-aqueous electrolyte at 0.01 wt% to 10 wt%.
9. In claim 1, The above lithium salts are LiCl, LiBr, LiI, LiBF4, LiClO4, LiAlO4, LiAlCl4, LiPF6, LiSbF6, LiAsF6, LiB 10 Cl 10 , LiBOB (LiB(C2O4)2), LiCF3SO3, LiFSI (LiN(SO2F)2), LiCH3SO3, LiCF3CO2, LiCH3CO2, and LiBETI (LiN(SO2CF2CF3)2).
10. In claim 1, A lithium secondary battery, wherein the lithium salt is included in the non-aqueous electrolyte at a molar concentration of 0.5 M to 5.0 M.
11. In claim 1, A lithium secondary battery comprising at least one selected from the group consisting of the additives coumarine, vinylene carbonate, vinyl ethylene carbonate, fluoroethylene carbonate, propane sultone, propene sultone, succinonitrile, adiponitrile, ethylene sulfate, LiDFP (lithium difluoro phosphate), LiBF4 (lithium tetrafluoroborate), LiODFB (lithium difluoro(oxalato)borate), LiBOB (lithium bis-(oxalato)borate), TMSPa (3-trimethoxysilanyl-propyl-N-aniline), TMSPi (Tris(trimethylsilyl) Phosphite) and compounds represented by the following chemical formula 3: [Chemical Formula 3] .
12. A step of housing an electrode assembly including a positive electrode, a negative electrode, and a separator interposed between the positive electrode and the negative electrode in a battery case; and A step of injecting a non-aqueous electrolyte into a battery case in which the electrode assembly is housed; The above positive electrode includes a positive electrode active material, The above cathode active material comprises a lithium manganese-rich oxide containing Mn at 50 mol% or more among all metals excluding lithium, and a molar ratio of lithium to transition metal exceeding 1, The above non-aqueous electrolyte comprises a lithium salt, an organic solvent and an additive, The organic solvent comprises a first organic solvent and a second organic solvent, The first organic solvent comprises ethylene carbonate, The second organic solvent comprises diethyl carbonate and ethyl methyl carbonate, A method for manufacturing a lithium secondary battery, wherein the additive comprises a compound represented by the following chemical formula 1: [Chemical Formula 1] In the above chemical formula 1, n is 1 or 2, L1 and L2 are each independently a direct bond or a substituted or unsubstituted alkylene group having 1 to 6 carbon atoms, R1 and R2 are each independently selected from a substituent represented by the following chemical formula 2, an alkyl group having 1 to 10 carbon atoms, an alkyl group having 1 to 10 carbon atoms substituted with at least one fluorine, an alkenyl group having 2 to 10 carbon atoms, an alkynyl group having 2 to 10 carbon atoms, a phosphate group, and a nitrile group, At least one of R1 and R2 is a substituent represented by the following chemical formula 2, [Chemical Formula 2] In the above chemical formula 2, m is 1 or 2, X1 and X2 are each independently -O- or -C(R 31 )(R 32 )-but at least one of the above X1 and X2 is -O-, R 31 Inland R 36 are each independently hydrogen, an alkyl group having 1 to 6 carbon atoms, -C(=O)-R4 or -R5-OC(=O)-R6, The above R4 and R6 are each independently a substituted or unsubstituted alkyl group having 1 to 6 carbon atoms, an alkenyl group having 2 to 20 carbon atoms, an alkynyl group having 2 to 20 carbon atoms, or a substituted or unsubstituted aryl group having 6 to 20 carbon atoms, The above R5 is a substituted or unsubstituted alkylene group having 1 to 6 carbon atoms, The substituents of the above L1, L2, R4, R5 and R6 are each independently at least one selected from the group consisting of deuterium, -F, -Cl, -Br, -I, -CN, -NO2 and -SO3, * is the position where it binds to L1 or L2, If both L1 and L2 are direct bonds, then R1 and R2 are not CS-7 at the same time, When L1 and L2 are both methylene groups and n is 2, R1 and R2 are not CS-2 at the same time. .
13. In claim 12, The above lithium manganese-rich oxide is a method for manufacturing a lithium secondary battery, wherein the compound is represented by the following chemical formula X: [chemical formula X] Li 1+s [Ni t Co u Mr v M 1 w ]O 2+z In the above chemical formula X, M 1 is at least one selected from W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B and Mo, 0.05≤s≤1, 0≤t≤0.5, 0≤u≤0.3, 0.5≤v<1.0, 0≤w≤0.2, 0≤z≤1.
14. In claim 12, A method for manufacturing a lithium secondary battery, wherein the volume ratio of the first organic solvent and the second organic solvent is 10:90 to 50:
50.
15. In claim 12, A method for manufacturing a lithium secondary battery, wherein the substituent represented by the above chemical formula 2 is selected from the group consisting of CS-1 to CS-15: _ .
16. In claim 15, A method for manufacturing a lithium secondary battery, wherein the above R1 and R2 are each independently selected from the group consisting of CS-1, CS-2, CS-5, CS-8, CS-10, and CS-11.
17. In claim 12, A method for manufacturing a lithium secondary battery, wherein the above L1 and L2 are methylene groups.
18. In claim 12, A method for manufacturing a lithium secondary battery comprising at least one compound selected from the group consisting of compounds A to U, wherein the compound represented by the above chemical formula 1 is: .
19. In claim 12, A method for manufacturing a lithium secondary battery, wherein the compound represented by the above chemical formula 1 is included in the non-aqueous electrolyte at 0.01 wt% to 10 wt%.
20. In claim 12, The above lithium salts are LiCl, LiBr, LiI, LiBF4, LiClO4, LiAlO4, LiAlCl4, LiPF6, LiSbF6, LiAsF6, LiB 10 Cl 10 , a method for manufacturing a lithium secondary battery comprising at least one selected from the group consisting of LiBOB (LiB(C2O4)2), LiCF3SO3, LiFSI (LiN(SO2F)2), LiCH3SO3, LiCF3CO2, LiCH3CO2, and LiBETI (LiN(SO2CF2CF3)2).
Citation Information
Patent Citations
Lithium secondary battery
KR102788465B1
Methdo for training neural networks for covid-19 diagnosis, system therefor, and covid-19 diagnosis apparatus using neural networks trained by the method
KR1020240052440A
Circuit board
KR1020240122012A
Nonaqueous electrolyte secondary battery and method for producing nonaqueous electrolyte secondary battery
US20150270575A1
KR20220135208A